Particulate material, its manufacturing method and use

A composite particulate material of metal acid hydroxide and spinel-type metal oxide agglomerates addresses the challenge of simultaneous high activity in OER and ORR, improving the efficiency of zinc-air secondary batteries.

JP7591256B2Active Publication Date: 2024-11-28HOKKAIDO UNIVERSITY
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020187522
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-10
Publication Date
2024-11-28
Estimated Expiration
2040-11-10

AI Technical Summary

Technical Problem

Existing catalyst materials for zinc-air secondary batteries fail to exhibit high activity for both oxygen evolution reaction (OER) and oxygen reduction reaction (ORR) simultaneously, necessitating the development of a bifunctional air electrode catalyst with composite materials in the nano-sized region.

Method used

A particulate material comprising metal acid hydroxide and spinel-type metal oxide agglomerates, each with specific compositions and sizes, is synthesized by firing a precursor containing layered double hydroxides and metal hydroxides, allowing for high activity in both OER and ORR reactions.

Benefits of technology

The composite catalyst achieves high activity in both OER and ORR reactions, enhancing the performance of air electrodes and metal-air secondary batteries by reducing overvoltages and improving efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591256000004
    Figure 0007591256000004
  • Figure 0007591256000005
    Figure 0007591256000005
  • Figure 0007591256000006
    Figure 0007591256000006
Patent Text Reader

Abstract

To provide a material having an oxy-hydroxide and a spinel-type oxide differing in crystal structure which are combined in a nanosize area, and also to provide an air electrode catalyst, a metal-air secondary battery air electrode, and a metal-air secondary battery which use the material.SOLUTION: A particulate material comprises in one particle: a metal-oxy-hydroxide particle mass containing Co, Ni, and Fe having a particle diameter within a range of 1 to 100nm; and a spinel-type metal-oxide particle mass containing Co, Ni, and Fe having a particle diameter within a range of 1 to 100nm. A production method of a particulate material comprises firing a precursor containing a layered double hydroxide containing Co, Ni, and Fe and containing a metal hydroxide containing Co, Ni, and Fe to obtain the particulate material. An air electrode catalyst and a metal-air secondary battery air electrode comprise the particulate material. A metal-air secondary battery comprises: an air electrode containing the particulate material; a negative electrode containing a negative electrode active material; and an electrolyte interposed between the air electrode and the negative electrode.SELECTED DRAWING: Figure 13-1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a particulate material, a method for producing the same, and use of the same. In particular, the present invention relates to a particulate material containing a metal oxide hydroxide particle agglomerate and a spinel-type metal oxide particle agglomerate in each particle, a method for producing the same, and use of the same as an air electrode catalyst, etc. [Background technology]

[0002] Zinc-air secondary batteries have a theoretical capacity five times that of currently practical lithium-ion batteries, and are attracting attention as the next generation of secondary batteries. There are many challenges to overcome before zinc-air secondary batteries can be put to practical use. In particular, the large overpotentials of the oxygen evolution reaction (OER) and oxygen reduction reaction (ORR) at the air electrode significantly reduce efficiency, so there is a demand for the development of a bifunctional air electrode catalyst that exhibits high activity in both reactions. However, to date, no single catalyst material that exhibits high activity in both reactions has been reported. The only known example is a catalyst that combines CoMn2O4 and MnOOH and is active in both the OER and ORR (Non-Patent Document 1).

[0003] From the viewpoint of metal price and production amount, catalysts made of transition metals of the fourth period have attracted attention, and it has been reported that metal oxide hydroxides show high activity as OER catalysts (e.g., Patent Document 1 and Non-Patent Document 2). It has been reported that metal oxides with a spinel crystal structure show high activity as ORR catalysts (e.g., Non-Patent Document 3). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] WO2020 / 006022 [Non-patent literature]

[0005] [Non-Patent Document 1] Chem. Commun., 2018, 54, 4005 [Non-Patent Document 2] Angew.chem.Int.Ed.2018,57,2672-2676 [Non-Patent Document 3] Adv. Mater. 2014, 26, 2408-2412 Summary of the Invention [Problem to be solved by the invention]

[0006] However, simply mixing these catalysts has not been enough to achieve high activity for both reactions simultaneously as a bifunctional air catalyst, and in order to develop a high-performance air electrode catalyst, it is necessary to synthesize a composite catalyst material in the nano-sized region. However, a method for developing a material in which an oxyhydroxide and a spinel-type oxide, which have different crystal structures, are composited in the nano-sized region has not yet been established.

[0007] Therefore, an object of the present invention is to provide a material in which an oxyhydroxide and a spinel-type oxide having different crystal structures are composited in the nano-sized region, and further to provide an air electrode catalyst, an air electrode for a metal-air secondary battery, and a metal-air secondary battery using this material. [Means for solving the problem]

[0008] The present invention is as follows. [1] A particulate material containing, in each particle, a metal oxide hydroxide particle agglomerate containing Co, Ni and Fe, the particle size of which is in the range of 1 to 100 nm, and a spinel-type metal oxide particle agglomerate containing Co, Ni and Fe, the particle size of which is in the range of 1 to 100 nm. [2] The particulate material according to [1], wherein at least a portion of the metal oxide hydroxide particle agglomerates and the spinel-type metal oxide particle agglomerates are present on the surface of the particulate material. [3] The particulate material contains 60 to 95 mol % of Co atoms, 1 to 25 mol % of Ni atoms, and 1 to 20 mol % of Fe atoms, and the total content of Ni atoms and Fe atoms is 5 mol % or more, with the proviso that the total of Co atoms, Ni atoms, and Fe atoms is 100 mol %. [4] The particulate material according to [3], wherein the particulate material has a Co atom content of 70 to 90 mol %, a Ni atom content of 4 to 25 mol %, and an Fe atom content of 2 to 14 mol %. [5] the metal oxide hydroxide particle agglomerates contain 60 to 95 mol % of Co atoms, 1 to 25 mol % of Ni atoms, and 1 to 20 mol % of Fe atoms, the total content of Ni atoms and Fe atoms being 5 mol % or more; The particulate material according to any one of [1] to [4], wherein the spinel-type metal oxide particle agglomerates contain 60 to 95 mol % Co atoms, 1 to 25 mol % Ni atoms, and 1 to 20 mol % Fe atoms, with the total content of Ni atoms and Fe atoms being 5 mol % or more, provided that in each case, the total of Co atoms, Ni atoms, and Fe atoms is 100 mol %. [6] The particulate material according to any one of [1] to [5], wherein the metal oxide hydroxide particle agglomerates have a particle diameter in the range of 1 to 20 nm, and the spinel-type metal oxide particle agglomerates have a particle diameter in the range of 1 to 20 nm. [7] The particulate material according to any one of [1] to [6], wherein the particle diameter of at least a part of the particulate material is in the range of 0.01 to 50 μm. [8] A method for producing a particulate material, comprising calcining a precursor containing a layered double hydroxide containing Co, Ni, and Fe, and a metal hydroxide containing Co, Ni, and Fe, to obtain a particulate material containing, in each particle, a metal oxide hydroxide particle agglomerate containing Co, Ni, and Fe, having a particle size in the range of 1 to 100 nm, and a spinel-type metal oxide particle agglomerate containing Co, Ni, and Fe, having a particle size in the range of 1 to 100 nm. [9] The precursor is Co 2+ 70 to 98 mol%, Ni 2+ 1 to 20 mol% and Fe3+ The method according to [8], further comprising adding an alkali to an aqueous solution containing 1 to 10 mol % of the compound.

[10] The method according to [8] or [9], wherein the calcination is carried out at a temperature in the range of 110 to 190°C.

[11] A catalyst for an air electrode, comprising the particulate material according to any one of [1] to [7].

[12] An air electrode for a metal-air secondary battery, comprising the particulate material according to any one of [1] to [7].

[13] [1]. A metal-air secondary battery comprising: an air electrode containing the particulate material according to any one of [1] to [7]; a negative electrode containing a negative electrode active material; and an electrolyte interposed between the air electrode and the negative electrode. Effect of the Invention

[0009] According to the present invention, a material can be provided in which an oxyhydroxide and a spinel-type oxide having different crystal structures are composited in the nano-sized region, and this material can be a catalyst with high activity in both OER and ORR. Furthermore, it is possible to provide an air electrode catalyst, an air electrode for a metal-air secondary battery, and a metal-air secondary battery using this material. [Brief description of the drawings]

[0010] [Figure 1] 1 shows XRD patterns of the precursor and the catalysts calcined at 100, 150, and 200° C. in Example 1 (Co73Ni13Fe14 sample). [Diagram 2] FIG. 1 shows (a) ORR and (b) OER activity evaluations of the precursor and samples calcined at various temperatures in Example 1 (Co73Ni13Fe14 sample). [Diagram 3] 1 shows XRD patterns of the precursor and the catalysts calcined at 100 and 150° C. in Example 2 (Co80Ni6Fe14 sample). [Figure 4] FIG. 1 shows (a) ORR and (b) OER activity evaluations of the precursor and samples calcined at various temperatures in Example 2 (Co80Ni6Fe14 sample). [Diagram 5]1 shows XRD patterns of a precursor and a catalyst calcined at 150° C. in Example 3 (Co84Ni12Fe4 sample). [Figure 6] FIG. 1 shows (a) ORR and (b) OER activity evaluations of the precursor and the sample calcined at 150° C. in Example 3 (Co84Ni12Fe4 sample). [Figure 7] 1 shows XRD patterns of the precursor and the catalysts calcined at 100° C. and 150° C. in Reference Example 1 (Co72Ni6Fe22 sample). [Figure 8] FIG. 1 shows (a) ORR and (b) OER activity evaluations of the precursor in Reference Example 1 (Co72Ni6Fe22 sample) and the samples calcined at each temperature. [Figure 9] 1 shows XRD patterns of a precursor and a catalyst calcined at 150° C. in Reference Example 2 (Co65Ni20Fe15 sample). [Figure 10] FIG. 1 shows (a) ORR and (b) OER activity evaluations of the precursor and the sample calcined at 150° C. in Reference Example 2 (Co65Ni20Fe15 sample). [Figure 11] 1 shows XRD patterns of the precursor and the catalysts calcined at 100 and 150° C. in Reference Example 3 (Co50Ni36Fe14 sample). [Figure 12] FIG. 1 shows (a) ORR and (b) OER activity evaluations of the precursor and samples calcined at various temperatures in Reference Example 3 (Co50Ni36Fe14 sample). [Figure 13-1] TEM images of the Co73Ni13Fe14 sample sintered at 150° C. in Example 1 (a) low-magnification image, and (b) high-magnification image of the red portion. [Figure 13-2] 1 shows the results of TEM-EDX analysis of a Co73Ni13Fe14 sample sintered at 150° C. in Example 1. [Figure 14-1] In Example 2, STEM images of a Co80Ni6Fe14 sample sintered at 150°C are shown: (a) a low-magnification image, and (b) a high-magnification image of the red portion. [Figure 14-2] 1 shows the results of STEM-EDX analysis of a Co80Ni6Fe14 sample sintered at 150° C. in Example 1. [Figure 15]1 shows the results of a cathode durability test when CFCO and a 150° C.-sintered Co73Ni13Fe14 sample (Example 1) were used. [Figure 16] 1 shows an example of the configuration of a metal-air secondary battery of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] [Particulate material] The present invention relates to a particulate material containing, in each particle, a metal oxide hydroxide particle agglomerate containing Co, Ni and Fe and having a particle size in the range of 1 to 100 nm, and a spinel-type metal oxide particle agglomerate containing Co, Ni and Fe and having a particle size in the range of 1 to 100 nm.

[0012] A metal oxide hydroxide is a compound represented by the formula MOOH (M: trivalent metal), and the trivalent metal represented by M can be composed of two or more trivalent metals. For example, when it contains three types of metals, M, M', and M'', M x M' y M'' (1-x-y) In the formula, x, y, and z represent the numbers of M, M', and M'', and are values ​​of 1 or less. For example, when M, M', and M'' are Co, Ni, and Fe, and the numbers are 0.6, 0.3, and 0.1, respectively, Co 0.6 Ni 0.3 Fe 0.1 It is written as OOH. Metal oxide hydroxides can maintain their structure even if the composition ratio of the anions changes slightly. For example, CoO(OH) 0.99 The composition ratio of MO(OH) is also possible. p In the formula, p may be less than 1 or more than 1 as long as the crystal structure of the oxide hydroxide is maintained. The metal oxide hydroxide in the present invention is an oxide hydroxide containing Co, Ni, and Fe as metals, and has the same crystal structure as the β-CoOOH type crystal structure. Identification of whether or not it is a metal oxide hydroxide can be performed by comparing with the β-CoOOH type crystal in XRD data. When the particulate material of the present invention is used as a catalyst for the air electrode of a metal-air secondary battery, the metal oxide hydroxide mainly exhibits OER activity.

[0013] Spinel-type metal oxides are represented by the formula AB2O4 (A: divalent metal, B: trivalent metal), and two or more metals can coexist in both A and B. For example, (Ni 0.1 Co 0.9 )(Fe 0.4 Co 1.6 However, the spinel structure can be maintained even if the ratio of elements is slightly different, so for example, NiCo2O 3.99 There are also reports of spinel oxides with composition ratios such as the above. The spinel metal oxide of the present invention is an oxide containing Co, Ni, and Fe as metals and has a spinel crystal structure. Identification of whether or not a spinel metal oxide is a spinel metal oxide can be performed by comparing XRD data with Co3O4 crystals.

[0014] The particulate material of the present invention contains a metal oxide hydroxide particle agglomerate containing Co, Ni and Fe having a particle diameter in the range of 1 to 100 nm and a spinel-type metal oxide particle agglomerate containing Co, Ni and Fe having a particle diameter in the range of 1 to 100 nm in one particle. The inclusion of a metal oxide hydroxide particle agglomerate and a spinel-type metal oxide particle agglomerate in one particle can be determined by observing a TEM image. The particulate material of the present invention contains the above-mentioned metal oxide hydroxide particle agglomerate and a spinel-type metal oxide particle agglomerate in one particle, thereby obtaining a catalyst having high activity in both OER and ORR. The metal oxide hydroxide particle agglomerate has a particle diameter in the range of 1 to 100 nm, preferably in the range of 1 to 50 nm, more preferably in the range of 1 to 20 nm. The spinel-type metal oxide particle agglomerate has a particle diameter in the range of 1 to 100 nm, preferably in the range of 1 to 50 nm, more preferably in the range of 1 to 20 nm. When the particulate material of the present invention is used as a catalyst for an air electrode of a metal-air secondary battery, the spinel-type metal oxide mainly exhibits ORR activity.

[0015] In the particulate material of the present invention, preferably, at least a portion of the metal oxide hydroxide particle agglomerates and the spinel type metal oxide particle agglomerates are present on the surface of the particulate material. The presence of at least a portion of the metal oxide hydroxide particle agglomerates and the spinel type metal oxide particle agglomerates on the surface of the particulate material can be determined by observing a TEM image. Since it is considered that the OER activity occurs mainly in the metal oxide hydroxide particle agglomerates and the ORR activity occurs mainly in the spinel type metal oxide particle agglomerates, a catalyst having high activity in both OER and ORR can be obtained by having at least a portion of both of them present on the surface of the particulate material.

[0016] The particulate material of the present invention contains Co atoms, Ni atoms and Fe atoms, and the contents of Co atoms, Ni atoms and Fe atoms are, for example, 60 to 95 mol%, 1 to 25 mol%, and 1 to 20 mol%, respectively, and the total content of Ni atoms and Fe atoms is suitably 5 mol% or more. However, the total of Co atoms, Ni atoms and Fe atoms is 100 mol%. When the particulate material has this content, a catalyst having high activity in both OER and ORR can be obtained. From the viewpoint of a catalyst having high activity in both OER and ORR, the contents of Co atoms, Ni atoms and Fe atoms in the particulate material are preferably 70 to 95 mol%, 4 to 25 mol%, and 2 to 20 mol%, respectively, and more preferably 70 to 85 mol%, 5 to 15 mol%, and 3 to 15 mol%. The total content of Ni atoms and Fe atoms is preferably in the range of 10 to 35 mol%, more preferably 15 to 30 mol%. The particulate material of the present invention may unavoidably contain metal atoms other than Co, Ni, and Fe as impurities. Alternatively, the particulate material of the present invention may contain metal atoms other than Co, Ni, and Fe, such as atoms of Si, Na, Mg, Ca, Zn, Al, Pb, Cu, Mn, etc., within a range that does not impair the effects of the present invention. However, even when the particulate material contains metal atoms other than Co, Ni, and Fe, the content (in mol%) of Co atoms, Ni atoms, and Fe atoms in the particulate material is defined as 100 mol% of the total of Co atoms, Ni atoms, and Fe atoms.

[0017] The contents of Co atoms, Ni atoms and Fe atoms in the metal oxide hydroxide particle agglomerate and the spinel metal oxide particle agglomerate are almost the same as the contents of Co atoms, Ni atoms and Fe atoms (expressed in mol%) in the particulate material. The contents of Co atoms, Ni atoms and Fe atoms in the metal oxide hydroxide particle agglomerate are, for example, 60 to 95 mol%, 1 to 25 mol%, and 1 to 20 mol%, respectively, and the total content of Ni atoms and Fe atoms is 5 mol% or more. The contents of Co atoms, Ni atoms and Fe atoms in the spinel metal oxide particle agglomerate are, for example, in the ranges of 60 to 95 mol%, 1 to 25 mol%, and 1 to 20 mol%, respectively, and the total content of Ni atoms and Fe atoms is suitably 5 mol% or more. Either or both of the metal oxide hydroxide particle mass and the spinel type metal oxide particle mass may contain metal atoms other than Co, Ni and Fe, such as atoms of Si, Na, Mg, Ca, Zn, Al, Pb, Cu, Mn, etc., as unavoidable impurities or as additives within a range that does not impair the effects of the present invention. In this case, as in the case of the particulate material, the contents (expressed in mol%) of Co atoms, Ni atoms and Fe atoms are defined as 100 mol% of the total of Co atoms, Ni atoms and Fe atoms.

[0018] In the particulate material of the present invention, the particle size of at least a part of the particulate material may be, for example, in the range of 0.01 to 50 μm, preferably in the range of 0.01 to 20 μm, and more preferably in the range of 0.01 to 10 μm. However, the particle size of the particulate material can be appropriately adjusted by pulverization or classification.

[0019] TEM and STEM images of an example of the particulate material of the present invention are shown in Figures 13-1 and 14-1. The TEM image shown in Figure 13-1 is a TEM image of a Co73Ni13Fe14 sample prepared in Example 1 and calcined at 150 ° C. The STEM image shown in Figure 14-1 is a STEM image of a Co80Ni6Fe14 sample prepared in Example 2 and calcined at 150 ° C. As can be seen from these images, the particulate material of the present invention contains a spinel-type metal oxide particle mass and an oxyhydroxide particle mass in one particle. TEM-EDX analysis and STEM-EDX analysis of these particles showed that the spinel-type metal oxide contains Co, Ni, and Fe as metals, and the metal oxyhydroxide also contains Co, Ni, and Fe as metals, as shown in Figures 13-2 and 14-2.

[0020] Furthermore, it is clear from the TEM and STEM images shown in Figs. 13-1 and 14-1 that the spinel-type oxide particle agglomerates and the oxyhydroxide particle agglomerates are present on the surface of the particulate material in at least some regions.

[0021] [Method of manufacturing particulate material] The present invention includes a method for producing a particulate material, which comprises calcining a precursor containing a layered double hydroxide containing Co, Ni, and Fe and a metal hydroxide containing Co, Ni, and Fe to obtain a particulate material containing a metal oxide hydroxide particle mass containing Co, Ni, and Fe and a spinel-type metal oxide particle mass containing Co, Ni, and Fe in each particle. The particulate material of the present invention can be produced by this method.

[0022] The precursors used in the manufacturing method of the present invention include layered double hydroxides containing Co, Ni and Fe, and metal hydroxides containing Co, Ni and Fe.

[0023] Metal hydroxides are represented by the formula M(OH)2 (M: divalent metal), where M can be composed of multiple divalent metals. Metal hydroxides containing Co, Ni, and Fe contain Co, Ni, and Fe as metals, so Co x Ni y Fe (1-x-y)The composition is (OH)2, where x, y, and z vary depending on the ratio of Co, Ni, and Fe in the raw materials used to prepare the precursor. The structure can be maintained even if the composition ratio of the anions varies slightly. Metal hydroxides can be specified by the hexagonal cadmium hydroxide type structure (cadmium iodide structure) or brucite type crystal structure.

[0024] Layered double hydroxides are 1-x M' x (OH)2][A x / n M is a monovalent or divalent metal, and M' is a trivalent or tetravalent metal. Two or more metals can coexist in M ​​and M'. Layered double hydroxides containing Co, Ni, and Fe have a composition of [Co yH2O] when x=0.2. 0.6 Ni 0.2 Co 0.1 Fe 0.1 (OH)2][(CO3) 0.2 ·0.5H2O]. The combination of valences of M and M' can be M-M'=1-3, 2-3, or 2-4, but in most cases M-M'=2-3. A is a monovalent or divalent anion. Generally, x=0.2-0.33, and n is the valence of the anion. M 1-x M' x It has a layered structure in which anion A and water molecules are inserted between the sheet layers composed of (OH)2.

[0025] The precursor may be, for example, Co. 2+ 70 to 98 mol%, Ni 2+ 1 to 20 mol% and Fe 3+The compound can be produced by adding an alkali to an aqueous solution containing 1 to 10 mol % of Co. By adding an alkali to an aqueous solution containing metal ions of this composition, a precursor containing both a layered double hydroxide containing Co, Ni, and Fe and a metal hydroxide containing Co, Ni, and Fe is precipitated. The raw materials of Co, Ni, and Fe can be salts of these metals, such as nitrates, acetates, citrates, etc. The alkali is not particularly limited, and can be, for example, an alkali metal hydroxide, ammonia water, etc., and potassium hydroxide can be used as the alkali metal hydroxide. The precipitate is separated into solid and liquid by a conventional method, and the obtained solid can be washed and dried appropriately. It is preferable to wash the precipitate with water and alcohol (e.g., ethanol) to remove the raw materials and alkali, and then dry it.

[0026] The precursor contains both a layered double hydroxide and a metal hydroxide, and the layered double hydroxide becomes a spinel-type metal oxide and the metal hydroxide becomes a metal oxyhydroxide by the calcination described later. 2+ 70 to 98 mol%, Ni 2+ and Fe 3+ By adding an alkali to an aqueous solution containing 1 to 10 mol % of Co, a precursor containing appropriate amounts of both layered double hydroxide and metal hydroxide can be obtained. 2+ , Ni 2+ and Fe 3+ The composition ratio can be appropriately adjusted so that both the layered double hydroxide and the metal hydroxide are contained in appropriate amounts. The precursor produced by this method has, for example, Co atom, Ni atom and Fe atom contents in the ranges of 60 to 95 mol%, 1 to 25 mol% and 1 to 20 mol%, respectively. The contents of Co atom, Ni atom and Fe atom in the precursor (expressed in mol%) are calculated based on the total of Co atom, Ni atom and Fe atom being 100 mol%.

[0027] The calcination of the precursor is suitably carried out at a temperature in the range of, for example, 110 to 190°C, depending on the ratio of Co, Ni and Fe in the precursor, from the viewpoint of obtaining a particulate material containing a metal oxide hydroxide particle agglomerate and a spinel type metal oxide particle agglomerate in one particle. The calcination of the precursor is preferably carried out in the range of 120 to 180°C, more preferably in the range of 130 to 170°C. The calcination time of the precursor is not particularly limited as long as the particulate material obtained by calcination contains a metal oxide hydroxide particle agglomerate and a spinel type metal oxide particle agglomerate, and although it varies depending on the temperature, it can be, for example, 1 hour to 24 hours. The atmosphere for the calcination may be an oxygen-containing atmosphere, and it is suitable to carry out the calcination in the air from the viewpoint of easy operation. The particulate material obtained by calcination can be used as it is, or after appropriate crushing and classification, as a catalyst.

[0028] <Catalyst for electrode> The present invention includes a cathode catalyst comprising the particulate material of the present invention.

[0029] The air electrode catalyst and the water electrolysis anode catalyst containing the particulate material of the present invention have a surface area of, for example, 1 to 100 m 2 / g, preferably 10 to 100 m 2 / g, but is not intended to be limited to this range.

[0030] INDUSTRIAL APPLICABILITY The particulate material of the present invention is extremely useful for air electrodes, and is extremely promising for hydrogen production by photochemical water splitting, and for use as air electrodes in metal-air secondary batteries, which are expected to be the next-generation high-capacity secondary batteries.

[0031] The particulate material of the present invention also has excellent catalytic activity against the ORR reaction, which is represented by the following reaction formula: O2+4H + +4e - →2H2O (neutral to acidic) O2+2H2O+4e - →4OH - (Basic) The particulate material of the present invention has excellent both OER activity and ORR activity and is extremely useful as an air electrode in a secondary battery.

[0032] <Air electrode> The air electrode functions as a positive electrode. The air electrode usually has a porous structure and contains an oxygen reaction catalyst as well as a conductive material. The air electrode may also contain a binder, etc., as necessary. The air electrode may contain an OER catalyst or an ORR catalyst, or both, other than the particulate material of the present invention. The air electrode in a secondary battery is required to have OER catalytic activity as a function during charging and ORR catalytic activity as a function during discharging. The catalyst of the present invention is a catalyst for both OER and ORR, so it can be used alone as a catalyst for the air electrode. The chemical formulas of the air electrode during charging and discharging are shown below.

[0033] [ka]

[0034] The content of the catalyst of the present invention in the air electrode is not particularly limited, but from the viewpoint of improving the oxygen reaction performance and oxygen reduction performance of the air electrode, it is preferably, for example, 1 to 90 mass %, particularly preferably 10 to 80 mass %, and more preferably 30 to 60 mass %.

[0035] The OER catalyst other than the particulate material of the present invention is not particularly limited. The OER catalyst can be, for example, the Brownmillerite transition metal oxide described in WO2015 / 115592. However, it is not intended to be limited thereto.

[0036] Examples of ORR catalysts other than the particulate material of the present invention are not particularly limited, but include, for example, Pt or Pt-based materials (e.g., PtCo, PtCoCr, Pt-W2C, Pt-RuOx, etc.), Pd-based materials (e.g., PdTi, PdCr, PdCo, ​​PdCoAu, etc.), metal oxides (e.g., ZrO 2-x , TiO x ,TaN x O y, IrMO x etc.), complexes (Co-porphyrin complexes), others (PtMoRuSeO x , RuSe, etc. Further examples include LaNiO3 (Nat. Chem. 3, 546 (2011)), which has been reported by Suntivich et al. as being highly active, and CoO / N-doped CNT (Nat. Commun. 4, 1805 (2013)), which has been reported by Li et al. However, it is not intended to be limited to these. Also, multiple catalysts can be used in combination, taking into consideration the performance and properties of each catalyst. Furthermore, the above catalysts can be used in combination with a promoter (for example, TiO x , RuO2, SnO2, etc.) can also be used in combination. The content when using an additional ORR catalyst can be appropriately determined taking into consideration the type and catalytic activity of the ORR catalyst, and can be, for example, 1 to 90 mass %. However, it is not intended to be limited to this numerical range.

[0037] The conductive material is not particularly limited, and may be any material that can be generally used as a conductive assistant, but a suitable example is conductive carbon. Specific examples include mesoporous carbon, graphite, acetylene black, carbon nanotubes, and carbon fibers. As the conductive material, a conductive assistant for oxygen generating electrodes containing pCNF (loop edge-pCNF (lpe-pCNF)) having a platelet structure of a carbon hexagonal mesh surface described in WO2019 / 039538, in which at least a part of the edge of the carbon hexagonal mesh surface exposed on the side surface of the fiber has a loop structure between the edge of the adjacent carbon hexagonal mesh surface, can also be used. Since it provides many reaction fields at the air electrode, conductive carbon with a large specific surface area is preferred. Specifically, a specific surface area of ​​1 to 3000 m 2 / g, especially 500~1500m 2 The catalyst for the air electrode may be supported on a conductive material.

[0038] The content of the conductive material in the air electrode is not particularly limited, but from the viewpoint of increasing the discharge capacity, it is preferably, for example, 10 to 99 mass %, particularly preferably 20 to 80 mass %, and more preferably 20 to 60 mass %.

[0039] By incorporating a binder in the air electrode, the catalyst and conductive material can be immobilized, and the cycle characteristics of the battery can be improved. The binder is not particularly limited, and examples thereof include polyvinylidene fluoride (PVDF) and its copolymers, polytetrafluoroethylene (PTFE) and its copolymers, and styrene butadiene rubber (SBR). The content of the binder in the air electrode is not particularly limited, but from the viewpoint of the binding strength between the carbon (conductive material) and the catalyst, it is preferably, for example, 1 to 40 mass%, particularly preferably 5 to 35 mass%, and more preferably 10 to 35 mass%.

[0040] The air electrode can be formed, for example, by dispersing the air electrode constituent material in a suitable solvent to prepare a slurry, which is then applied to a substrate and dried. The solvent is not particularly limited, and examples thereof include acetone, N,N-dimethylformamide, and N-methyl-2-pyrrolidone (NMP). The air electrode constituent material and the solvent are usually mixed for 3 hours or more, preferably 4 hours. The mixing method is not particularly limited, and a general method can be used.

[0041] The substrate to which the slurry is applied is not particularly limited, and examples thereof include a glass plate, a Teflon (registered trademark) plate, and the like. These substrates are peeled off from the obtained air electrode after the slurry is dried. Alternatively, the current collector of the air electrode or the solid electrolyte layer can be treated as the substrate. In this case, the substrate is not peeled off and is used as it is as a component of the metal-air secondary battery.

[0042] The method for applying and drying the slurry is not particularly limited, and a common method can be used. For example, a spray method, a doctor blade method, a gravure printing method, or the like can be used as the application method, and a drying method such as a heat drying method or a reduced pressure drying method can be used.

[0043] The thickness of the air electrode is not particularly limited and may be appropriately set depending on the application of the metal-air secondary battery, but is usually preferably 5 to 100 μm, 10 to 80 μm, and particularly preferably 20 to 70 μm.

[0044] An air electrode current collector that collects current from the air electrode is usually connected to the air electrode. The material and shape of the air electrode current collector are not particularly limited. Examples of materials for the air electrode current collector include stainless steel, aluminum, iron, nickel, titanium, and carbon. Examples of the shape of the air electrode current collector include foil, plate, mesh (grid), and fiber, and among these, a porous shape such as a mesh is preferable. This is because a porous current collector has excellent oxygen supply efficiency to the air electrode.

[0045] <Metal-air secondary battery> The metal-air secondary battery of the present invention has an air electrode containing a catalyst including the particulate material of the present invention, a negative electrode containing a negative electrode active material, and an electrolyte interposed between the air electrode and the negative electrode. The air electrode of the metal-air secondary battery of the present invention contains a catalyst including the particulate material of the present invention, and this catalyst exhibits excellent OER catalyst and ORR catalyst properties. Therefore, by using an air electrode using this catalyst, the overvoltage required for charging can be reduced, the electromotive force of the battery during discharge can be improved, and high efficiency can be achieved, so that the metal-air secondary battery of the present invention has excellent charge and discharge voltages.

[0046] As described above, the air electrode can also contain a catalyst having OER catalytic activity or a catalyst having ORR catalytic activity.

[0047] An example of the configuration of the metal-air secondary battery of the present invention will be described below. The metal-air secondary battery of the present invention is not limited to the following configuration. FIG. 16 is a cross-sectional view showing an example of the metal-air secondary battery of the present invention. The metal-air secondary battery 1 comprises an air electrode 2, which is a positive electrode using oxygen as an active material, a negative electrode 3 containing a negative electrode active material, an electrolyte 4 which is responsible for ion conduction between the air electrode 2 and the negative electrode 3, an air electrode current collector 5 which collects the current of the air electrode 2, and a negative electrode current collector 6 which collects the current of the negative electrode 3, and these are housed in a battery case (not shown). The air electrode 2 is electrically connected to the air electrode current collector 5 which collects the current of the air electrode 2, and the air electrode current collector 5 has a porous structure capable of supplying oxygen to the air electrode 2. The negative electrode 3 is electrically connected to the negative electrode current collector 6 which collects the current of the negative electrode 3, and one of the ends of the air electrode current collector 5 and the negative electrode current collector 6 protrudes from the battery case. They function as a positive electrode terminal (not shown) and a negative electrode terminal (not shown), respectively.

[0048] (Negative electrode) The negative electrode contains a negative electrode active material. The negative electrode active material may be a general air battery negative electrode active material, and is not particularly limited. The negative electrode active material is usually capable of absorbing and releasing metal ions. Specific examples of the negative electrode active material include metals such as Li, Na, K, Mg, Ca, Zn, Al, and Fe, alloys, oxides, and nitrides of these metals, and carbon materials.

[0049] Among them, zinc-air secondary batteries are expected to be the next generation secondary batteries because of their superior safety. From the viewpoint of high voltage and high output, lithium-air secondary batteries and magnesium-air secondary batteries are promising. An example of a zinc-air secondary battery is described below. The reaction formula is as follows: [ka]

[0050] In the zinc-air secondary battery of the present invention, a material capable of absorbing and releasing zinc ions is used as the negative electrode. In addition to metallic zinc, a zinc alloy can also be used as such a negative electrode. Examples of the zinc alloy include zinc alloys containing one or more elements selected from aluminum, indium, magnesium, tin, titanium, and copper.

[0051] Examples of the negative electrode active material for the lithium-air secondary battery include metallic lithium; lithium alloys such as lithium aluminum alloys, lithium tin alloys, lithium lead alloys, and lithium silicon alloys; metal oxides such as tin oxide, silicon oxide, lithium titanium oxide, niobium oxide, and tungsten oxide; metal sulfides such as tin sulfide and titanium sulfide; metal nitrides such as lithium cobalt nitride, lithium iron nitride, and lithium manganese nitride; and carbon materials such as graphite. Of these, metallic lithium is preferred.

[0052] Furthermore, a material capable of absorbing and releasing magnesium ions is used as the negative electrode active material of the magnesium-air secondary battery. In addition to metallic magnesium, magnesium alloys such as magnesium aluminum, magnesium silicon, and magnesium gallium can be used as the negative electrode.

[0053] When a foil- or plate-shaped metal, alloy, or the like is used as the negative electrode active material, the foil- or plate-shaped negative electrode active material can be used as the negative electrode itself.

[0054] The negative electrode may contain at least a negative electrode active material, and may contain a binder to fix the negative electrode active material, if necessary. The type and amount of the binder are the same as those of the air electrode described above, and therefore will not be described here.

[0055] A negative electrode current collector that collects current from the negative electrode is usually connected to the negative electrode. The material and shape of the negative electrode current collector are not particularly limited. Examples of the material of the negative electrode current collector include stainless steel, copper, nickel, etc. In addition, examples of the shape of the negative electrode current collector include foil, plate, mesh (grid), etc.

[0056] (electrolyte) The electrolyte is disposed between the air electrode and the negative electrode. Metal ion conduction between the negative electrode and the air electrode occurs via the electrolyte. The form of the electrolyte is not particularly limited, and examples thereof include a liquid electrolyte, a gel electrolyte, and a solid electrolyte.

[0057] For example, when the negative electrode is zinc or an alloy thereof, the electrolyte may be an alkaline aqueous solution such as an aqueous potassium hydroxide solution or an aqueous sodium hydroxide solution containing zinc oxide, an aqueous solution containing zinc chloride or zinc perchlorate, or a non-aqueous solvent containing zinc perchlorate or a non-aqueous solvent containing zinc bis(trifluoromethylsulfonyl)imide. For example, when the negative electrode is magnesium or an alloy thereof, a non-aqueous solvent containing magnesium perchlorate or magnesium bis(trifluoromethylsulfonyl)imide may be used. Here, examples of the non-aqueous solvent include organic solvents used in conventional secondary batteries and capacitors, such as ethylene carbonate (EC), propylene carbonate (PC), γ-butyrolactone (γ-BL), diethyl carbonate (DEC), and dimethyl carbonate (DMC). These may be used alone or in combination. Alternatively, an ionic liquid such as N,N-diethyl-N-methyl-N-(2-methoxyethyl)ammonium bis(trifluoromethylsulfonyl)imide (am) can be used.

[0058] In the secondary battery of the present invention, the electrolyte preferably contains a dendrite formation inhibitor. It is believed that the dendrite formation inhibitor is adsorbed to the negative electrode surface during charging to reduce the energy difference between crystal planes and prevent preferred orientation, thereby suppressing the generation of dendrites. The dendrite formation inhibitor is not particularly limited, and may be, for example, at least one selected from the group consisting of polyalkyleneimines, polyallylamines, and asymmetric dialkylsulfones (see, for example, JP 2009-93983 A). The amount of the dendrite formation inhibitor used is not particularly limited, and may be, for example, an amount sufficient to saturate the electrolyte at room temperature and normal pressure, or may be used as a solvent.

[0059] In the case of a lithium-air secondary battery, the liquid electrolyte having lithium ion conductivity is usually a non-aqueous electrolyte solution containing a lithium salt and a non-aqueous solvent. Examples of the lithium salt include inorganic lithium salts such as LiPF6, LiBF4, LiClO4, and LiAsF6; and organic lithium salts such as LiCF3SO3, LiN(CF3SO2)2, LiN(C2F5SO2)2, and LiC(CF3SO2)3.

[0060] Examples of the non-aqueous solvent include ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), butylene carbonate, γ-butyrolactone, sulfolane, acetonitrile, 1,2-dimethoxymethane, 1,3-dimethoxypropane, diethyl ether, tetrahydrofuran, 2-methyltetrahydrofuran, and mixtures thereof. Ionic liquids can also be used as the non-aqueous solvent.

[0061] The concentration of the lithium salt in the non-aqueous electrolyte is not particularly limited, but is preferably within the range of, for example, 0.1 mol / L to 3 mol / L, and is preferably 1 mol / L. In the present invention, a low-volatility liquid such as an ionic liquid may be used as the non-aqueous electrolyte.

[0062] A gel electrolyte having lithium ion conductivity can be obtained, for example, by adding a polymer to the non-aqueous electrolyte solution and gelling it. Specifically, the gelling can be achieved by adding a polymer such as polyethylene oxide (PEO), polyvinylidene fluoride (PVDF, Kynar, manufactured by Arkema, etc.), polyacrylonitrile (PAN), or polymethyl methacrylate (PMMA) to the non-aqueous electrolyte solution.

[0063] The solid electrolyte having lithium ion conductivity is not particularly limited, and a general solid electrolyte that can be used in a lithium metal air secondary battery can be used. For example, Li 1.5 Al 0.5 Ge 1.5 Examples of the solid electrolyte include oxide solid electrolytes such as (PO4)3, and sulfide solid electrolytes such as Li2S-P2S5 compounds, Li2S-SiS2 compounds, and Li2S-GeS2 compounds.

[0064] The thickness of the electrolyte varies greatly depending on the configuration of the battery, but is preferably within the range of 10 μm to 5000 μm, for example.

[0065] (Included configuration) In the metal-air secondary battery of the present invention, a separator is preferably disposed between the air electrode and the negative electrode in order to ensure electrical insulation between these electrodes. The separator is not particularly limited as long as it has a structure that can ensure electrical insulation between the air electrode and the negative electrode and allows an electrolyte to be interposed between the air electrode and the negative electrode.

[0066] Examples of the separator include porous membranes such as polyethylene, polypropylene, cellulose, polyvinylidene fluoride, and glass ceramics; and nonwoven fabrics such as resin nonwoven fabrics and glass fiber nonwoven fabrics. Among these, separators made of glass ceramics are preferred.

[0067] In addition, a battery case for a general metal-air secondary battery can be used as the battery case for housing the metal-air secondary battery. The shape of the battery case is not particularly limited as long as it can hold the air electrode, the negative electrode, and the electrolyte described above, but specific examples include a coin type, a flat type, a cylindrical type, a laminate type, and the like.

[0068] The metal-air secondary battery of the present invention can discharge by supplying oxygen, which is an active material, to the air electrode. Examples of the oxygen supply source include air and oxygen gas, and oxygen gas is preferred. The pressure of the air or oxygen gas to be supplied is not particularly limited and may be set appropriately. EXAMPLES

[0069] The present invention will be described in more detail below with reference to examples. However, the examples are merely illustrative of the present invention and are not intended to limit the present invention.

[0070] (1) Synthesis of particulate materials A precursor was synthesized by adding 15 ml of 1 M potassium hydroxide aqueous solution to 150 ml of an aqueous solution (total metal concentration 0.1 M) in which nitrates of iron group metals (Fe, Co, Ni) were dissolved in the specified molar ratios shown in Table 1. The precursor was calcined in an O2 atmosphere at 100, 150, and 200°C for 12 hours to synthesize a catalyst.

[0071] (2) Electrochemical measurements The obtained powder sample was dispersed in ethanol with acetylene black (AB) and Nafion in a weight ratio of sample:AB:Nafion = 5:1:1, and the oxide catalyst amount was 10 mg cm on a glassy carbon (GC) electrode. -2 Electrochemical measurements were performed using a VersaStat4 (manufactured by AMETEC) and a rotating ring disk electrode device (manufactured by Pine Research) in a 4M KOH aqueous solution with a Hg / HgO electrode as the reference electrode and a Pt wire as the counter electrode.

[0072] Carbon black powder (TB300) manufactured by Tokai Carbon and a PTFE dispersion were mixed in a ratio of carbon:PTFE = 70:30 and rolled into a sheet with a thickness of approximately 0.3 mm using a roll press. The obtained sheet was cut into a circle with a diameter of 12 mm and heat-treated at 335°C in a nitrogen atmosphere to produce a gas diffusion layer. The catalyst sample was dispersed in a solvent of ultrapure water:isopropanol = 1:1 with a carbon conductive assistant (TB3800 or carbon nanochips) and Nafion so that the weight ratio of sample:carbon:Nafion = 3:1:1, and the amount of oxide catalyst was 10 mg cm to form the catalyst layer. -2 The gas diffusion layer was coated with the catalyst layer so that the catalyst layer was applied to the gas diffusion layer. The gas diffusion layer with the catalyst layer applied was hot pressed together with a nickel mesh at 130°C and 0.7t to produce an air electrode. The air electrode was placed in a PFA cell, and the air electrode was evaluated at 40°C using a 4M KOH aqueous solution as the electrolyte.

[0073] (3) Element ratios in raw materials and products The feed ratios during synthesis of the catalyst samples and the obtained samples (calcined at 150°C) were analyzed by SEM-EDX (Sigma-500, Carl Zeiss), and the content of each metal atom is shown in Table 1. In all samples, the content ratios of Fe and Ni were greater than the feed ratios. Hereafter, the names of the samples (calcined products) will be expressed as CoxNiyFez, using the numerical values ​​(x, y, z) of the ratios of each element.

[0074] [Table 1]

[0075] Example 1 Figure 1 shows the XRD patterns of the precursor and catalysts calcined at 100°C, 150°C, or 200°C for the Co73Ni13Fe14 sample. The precursor showed peaks derived from LDH (layered double hydroxide) and hydroxide, indicating that it was a composite of particles with these crystal structures. The catalyst calcined from the precursor at 100°C showed the disappearance of the hydroxide peak and the appearance of LDH and oxyhydroxide peaks. The catalyst calcined at 150°C showed the disappearance of the LDH peak and the appearance of oxyhydroxide and spinel oxide peaks. The catalyst calcined at 200°C showed the disappearance of the oxyhydroxide peak and the appearance of only the spinel oxide peak.

[0076] The results of ORR and OER activity evaluation of the precursor and samples calcined at each temperature for the Co73Ni13Fe14 sample are shown in Figure 2. The precursor showed ORR activity equivalent to that of CFCO and OER activity higher than that of CFCO. CFCO is Ca2FeCoO5 prepared in Example 1 of WO2015 / 115592. The 100°C calcined catalyst also showed activity equivalent to that of the precursor. The LDH, hydroxide, and oxyhydroxide, which are the crystal structures of the precursor and the 100°C sample, are known as materials that show low ORR activity but high OER activity, and it is considered that this sample also showed low ORR activity and high OER activity. The 150°C calcined sample showed improved ORR activity compared to the 100°C calcined sample and showed higher ORR activity than CFCO. The OER activity was also lower than that of the 100°C calcined sample, and showed the same level of OER activity as CFCO. The 200°C sample had higher ORR activity than the 150°C calcined sample, but its OER activity was significantly lower. The spinel-type oxides found in the samples calcined at 150°C or higher are generally known to be highly active in ORR, but their OER activity is lower than that of LDHs, hydroxides, and oxyhydroxides. In this sample, the LDHs and oxyhydroxides found in the 100°C calcined sample were partially converted to spinel-type oxides at 150°C, which is thought to have improved the ORR activity and reduced the OER activity. At 200°C, the entire sample was converted to a spinel structure, which is thought to have improved the ORR activity but significantly reduced the OER activity. From the above, the optimal temperature for a bifunctional catalyst is thought to be, for example, around 125-175°C.

[0077] Example 2 The XRD patterns of the precursor and the catalysts calcined at 100°C or 150°C for the Co80Ni6Fe14 sample are shown in Figure 3. The Co80Ni6Fe14 sample showed similar changes in crystal structure to the Co73Ni13Fe14 sample, i.e., the precursor showed LDH and hydroxide peaks, the catalyst calcined at 100°C showed LDH and oxyhydroxide peaks with the disappearance of the hydroxide peak, and the catalyst calcined at 150°C showed oxyhydroxide and spinel-type oxide peaks with the disappearance of the LDH peak.

[0078] Figure 4 shows the results of ORR and OER activity evaluation of the Co80Ni6Fe14 precursor and samples calcined at various temperatures. The Co80Ni6Fe14 sample showed a similar tendency to the Co73Ni13Fe14 sample. The precursor and the sample calcined at 100°C showed ORR and OER activity comparable to that of CFCO. The 150°C sample showed an improvement in ORR activity and a decrease in OER activity.

[0079] Example 3 The XRD patterns of the precursor and 150 °C calcined catalyst for the Co84Ni12Fe4 sample are shown in Figure 5. The Co84Ni12Fe4 sample showed a change in crystal structure similar to that of the Co73Ni13Fe14 sample, i.e., the precursor showed LDH and hydroxide peaks, and the catalyst calcined at 150 °C showed oxyhydroxide and spinel oxide peaks.

[0080] The results of ORR and OER activity evaluation of the precursor and samples calcined at each temperature for the Co84Ni12Fe4 sample are shown in Figure 6. The precursor sample showed ORR activity similar to that of CFCO, but lower OER activity than CFCO. The 150°C sample showed improved ORR activity and almost the same OER activity.

[0081] Reference example 1 Figure 7 shows the XRD patterns of the precursor and the catalysts calcined at 100°C or 150°C for the Co72Ni6Fe22 sample. The precursor showed peaks of LDH and hydroxide. In the sample calcined at 100°C, the hydroxide peak disappeared and peaks due to oxyhydroxide and spinel-type oxide were shown. In the sample calcined at 150°C, the LDH and oxyhydroxide peaks disappeared and only the peak of spinel-type oxide was shown.

[0082] Figure 8 shows the results of ORR and OER activity evaluation of the precursor and samples calcined at each temperature for the Co72Ni6Fe22 sample. The precursor and the sample calcined at 100°C showed low ORR activity similar to that of CFCO, and higher OER activity than CFCO. The 150°C sample showed a slight improvement in ORR activity, but showed lower ORR activity than the 150°C calcined Co73Ni13Fe14 sample and the 150°C calcined Co80Ni6Fe14 sample. The OER activity of the 150°C sample was lower than that of the precursor and the 100°C calcined sample, and showed the same level of OER activity as CFCO.

[0083] The 150°C calcined Co72Ni6Fe22 sample is expected to show high ORR activity because it only exhibits a spinel structure, but in fact it showed low ORR activity. In addition, when comparing the ORR activity of the catalysts calcined at 150°C for the above four compositions, the samples with higher Fe content showed lower ORR activity. From this, it is thought that the ORR activity of spinel-type oxides decreases as the Fe ratio increases. On the other hand, it was found that the OER activity increases as the Fe ratio increases.

[0084] Reference example 2 The XRD patterns of the precursor and the catalyst calcined at 150°C for the Co65Ni20Fe15 sample are shown in Figure 9. For the Co65Ni20Fe15 sample, the precursor showed a peak only for LDH, and the catalyst calcined at 150°C showed a peak only for spinel-type oxide.

[0085] Figure 10 shows the results of ORR and OER activity evaluation of the precursor and samples calcined at each temperature for the Co65Ni20Fe15 sample. The precursor sample showed ORR and OER activity comparable to that of CFCO. The 150°C sample showed a slight improvement in ORR activity, but showed lower ORR activity than the 150°C calcined Co73Ni13Fe14 sample, the 150°C calcined Co80Ni6Fe14 sample, and the 150°C calcined Co84Ni12Fe4 sample. The OER activity was lower than that of the precursor.

[0086] Reference example 3 The XRD patterns of the precursor and the 100°C or 150°C calcined catalyst for the Co50Ni36Fe14 sample are shown in Figure 11. Both the precursor and the calcined sample of the Co50Ni36Fe14 sample showed only the LDH peak.

[0087] The results of ORR and OER activity evaluation of the precursor and samples calcined at each temperature for the Co50Ni36Fe14 sample are shown in Figure 12. For the Co65Ni5Fe10 sample, both the precursor and calcined sample showed almost the same activity, with low ORR activity similar to that of CFCO and higher OER activity than CFCO. LDH is a material that shows high activity in OER, and since the crystal structure was the same even after calcination, it is thought to have shown almost the same activity.

[0088] [TEM image] FIG. 13-1 shows a TEM image of the Co73Ni13Fe14 sample sintered at 150°C in Example 1. The TEM was a JEM-2000FX (JEOL Ltd.). It was found that the sample was in a state of secondary particles with a particle size of several hundred nm, which were formed by agglomeration of primary particles with a particle size of about 10 nm. When the crystal structure was identified from the lattice spacing of the primary particles (metal oxide hydroxide particle agglomerates and spinel-type metal oxide particle agglomerates) observed by high-magnification TEM, it was found that the particulate material, which was a secondary particle, was in a state in which spinel-type metal oxide particle agglomerates, which were primary particles of spinel oxide, and metal oxide hydroxide particle agglomerates, which were primary particles of oxide hydroxide, were highly dispersed and composited. The average particle size of the spinel-type oxide particle agglomerates was 5.1 nm, and the average particle size of the oxide hydroxide particle agglomerates was 4.9 nm. In addition, TEM-EDX analysis revealed that the metal content in the spinel oxide was 60-85 mol% Co atoms, 7-20 mol% Ni atoms, and 3-18 mol% Fe atoms, while the metal content in the oxyhydroxide was 64-85 mol% Co atoms, 8-24 mol% Ni atoms, and 5-20 mol% Fe atoms, indicating that all nanoparticles contained all three metal elements with similar ratios. The results of the TEM-EDX analysis are shown in Figure 13-2.

[0089] [STEM image] FIG. 14-1 shows a STEM image of the Co80Ni6Fe14 sample sintered at 150°C in Example 2. The STEM was a JEM-ARM200F (JEOL Ltd.). As in Example 1, the sample was found to be a particle agglomerate with a particle size of several hundred nm, which was formed by agglomeration of primary particles with a particle size of about 10 nm. When the crystal structure was identified from the lattice spacing of the primary particles by high-magnification STEM observation, it was found that the particle agglomerate was in a highly dispersed composite state of primary particles of spinel oxide and oxyhydroxide. It was found that the average particle size of the spinel oxide particle agglomerates was 6.3 nm, and that of the oxyhydroxide particle agglomerates was 5.9 nm. In addition, STEM-EDX analysis showed that the metal contents in the spinel oxide were Co: 71-87 mol%, Ni: 4-13 mol%, Fe: 6-20 mol%, and the metal contents in the oxyhydroxide were Co: 69-90 mol%, Ni: 5-16 mol%, Fe: 6-18 mol%, indicating that all nanoparticles contained all three metal elements with similar ratios. The results of the STEM-EDX analysis are shown in Figure 14-2.

[0090] [Relationship between composition ratio and ORR, OER activity] When the composition ratios of the samples synthesized in Examples 1 to 3 and Reference Examples 1 to 3 and the tendency of the ORR activity and OER activity were examined, it was found that the higher the content ratios of Ni atoms and Fe atoms (in mol%), the higher the OER activity. On the other hand, when the crystal structure of a spinel-type oxide is present, it was found that the higher the Ni atom content ratio and the lower the Fe content ratio, the higher the ORR activity. When the correlation between the composition ratios and the crystal structure of the synthesized samples was examined, it was found that when the Ni atom content was more than 25 mol%, no hydroxide was generated in the precursor and only LDH was generated, and after calcination, no oxyhydroxide was generated and only spinel-type oxide was generated, or the crystal structure of LDH remained unchanged. From the above results, it was found that a bifunctional catalyst in which oxyhydroxide and spinel-type oxide coexist was obtained by calcination treatment when the Co atom content was 60 to 95, the Ni atom content was 1 to 25 mol%, and the Fe content was 1 to 20 mol%. In particular, it was found that the Co73Ni13Fe14 sample calcined at 150°C exhibited the highest activity as a bifunctional catalyst among the materials obtained in the examples.

[0091] [Air electrode durability test results] The Co73Ni13Fe14 sample (Example 1) sintered at 150°C was applied to a gas diffusion electrode and subjected to a cycle durability test as an air electrode. -2 Figure 15 shows the electrode potential over the number of cycles when OER and ORR were performed for 1 hour each per cycle under constant current conditions. The OER activity was almost constant and stable during the test, and the ORR activity gradually improved with the increase in the number of cycles. The overall overpotential decreased with the increase in the number of cycles. The Co73Ni13Fe14 sample calcined at 150°C showed good bifunctional performance and was found to have high durability of 450 cycles (1.5 months) as an air electrode catalyst. [Industrial Applicability]

[0092] INDUSTRIAL APPLICABILITY The present invention is useful in the field of secondary batteries, particularly metal-air secondary batteries which are expected to become next-generation high-capacity secondary batteries. [Explanation of symbols]

[0093] 1. Metal-air secondary battery 2 Air electrode 3 Negative electrode 4 electrolyte 4 5. Air cathode current collector 6 Negative electrode current collector 6

Claims

1. The metal oxide hydroxide particle agglomerate containing Co, Ni and Fe and having a particle size in the range of 1 to 100 nm, and a spinel-type metal oxide particle agglomerate containing Co, Ni and Fe and having a particle size in the range of 1 to 100 nm are contained in one particle, A particulate material containing 70 to 95 mol % Co atoms, 1 to 25 mol % Ni atoms, and 1 to 20 mol % Fe atoms, with the total content of Ni atoms and Fe atoms being 5 mol % or more, with the proviso that the total of Co atoms, Ni atoms, and Fe atoms is 100 mol %, and peaks of the metal oxide hydroxide and the spinel metal oxide are detected by XRD measurement.

2. 2. The particulate material of claim 1, wherein at least a portion of the metal oxide hydroxide particle agglomerates and the metal spinel type oxide particle agglomerates are each present on a surface of the particulate material.

3. 2. The particulate material according to claim 1, wherein the particulate material has a Co atomic content of 70-90 mol%, a Ni atomic content of 4-25 mol% and a Fe atomic content of 2-14 mol%.

4. the metal oxide hydroxide particle agglomerates contain 70 to 95 mol % Co atoms, 1 to 25 mol % Ni atoms, and 1 to 20 mol % Fe atoms, the total content of Ni atoms and Fe atoms being 5 mol % or more; The particulate material according to any one of claims 1 to 3, wherein the spinel-type metal oxide particle agglomerates contain 70 to 95 mol % Co atoms, 1 to 25 mol % Ni atoms, and 1 to 20 mol % Fe atoms, with the total content of Ni atoms and Fe atoms being 5 mol % or more, provided that in each case, the total of Co atoms, Ni atoms, and Fe atoms is 100 mol %.

5. 5. The particulate material according to claim 1, wherein the metal oxide hydroxide particle agglomerates have a particle size in the range of 1 to 20 nm and the spinel type metal oxide particle agglomerates have a particle size in the range of 1 to 20 nm.

6. A particulate material according to any one of the preceding claims, wherein at least a portion of the particulate material has a particle size in the range 0.01 to 50 μm.

7. a precursor containing a layered double hydroxide containing Co, Ni and Fe and a metal hydroxide containing Co, Ni and Fe is fired at a temperature in the range of 110 to 190°C to produce a metal oxide hydroxide particle agglomerate containing Co, Ni and Fe having a particle size in the range of 1 to 100 nm and a spinel type metal oxide particle agglomerate containing Co, Ni and Fe having a particle size in the range of 1 to 100 nm, A method for producing a particulate material comprising obtaining a particulate material containing 70 to 95 mol % Co atoms, 1 to 25 mol % Ni atoms, and 1 to 20 mol % Fe atoms, with the total content of Ni atoms and Fe atoms being 5 mol % or more, with the proviso that the total of Co atoms, Ni atoms, and Fe atoms is 100 mol %, and in which peaks of the metal oxide hydroxide and the spinel metal oxide are detected by XRD measurement.

8. The precursor is Co 2+ 70 to 98 mol %, Ni 2+ 1 to 20 mol % and Fe 3+ The method according to claim 7, wherein the compound is produced by adding an alkali to an aqueous solution containing 1 to 10 mol % of the compound.

9. A catalyst for an air electrode comprising the particulate material according to any one of claims 1 to 6.

10. A metal-air secondary battery air electrode comprising the particulate material according to any one of claims 1 to 6.

11. A metal-air secondary battery comprising an air electrode containing the particulate material according to any one of claims 1 to 6, a negative electrode containing a negative electrode active material, and an electrolyte interposed between the air electrode and the negative electrode.

Citation Information

Patent Citations

  • Ferromagnetic metallic particle and manufacture thereof

    JP1991293703A

  • Nickel-manganese composite oxide, method of producing the same, and application thereof

    JP2015110509A

  • Textile inkjet printing ink

    WO2020006022A1

  • Material for oxygen evolution (OER) electrode catalyst, and use thereof

    WO2020096022A1