Mesh sheet for industrial materials and its manufacturing method
Patent Information
- Application Number
- JP2023039448
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-03-14
- Publication Date
- 2024-11-28
- Estimated Expiration
- 2043-03-14
AI Technical Summary
【0013】 本発明により、耐折り畳み性(特に寒冷下)、及び使用時の耐展開性(特に寒冷下)に優れ、さらに耐洗濯性にも優れた産業資材用メッシュシートを得ることができるので、ビル、マンション、学校などの建設現場、改修工事現場、解体工事現場の張囲、またビルのファサード、公共施設の改修工事現場のファサード張囲、などに適して用いることができる。それ以外にも、住宅、マンション住居、店舗などの日除け、屋内天井、間仕切り、横断幕、懸垂幕、防風防雪フェンスなどにも使用できる。
Smart Images

Figure 0007591303000001 
Figure 0007591303000002 
Figure 0007591303000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a mesh sheet used for enclosing construction sites, repair and demolition sites of buildings, condominiums, schools, etc., as well as for enclosing the facades of buildings and repair sites of public facilities. [Background technology]
[0002] Architectural protection mesh sheets used to enclose construction sites, renovation sites, and demolition sites such as buildings, condominiums, and schools, or facades used to decorate the front of buildings, are mainly composite products made of coarse polyester fiber fabric impregnated and coated with soft polyvinyl chloride resin, and are classified into Class 1, which meets the safety standards of the Fire and Disaster Management Agency's fireproofing standards and the Temporary Construction Industry Association's certification, and Class 2, which only meets the Fire and Disaster Management Agency's fireproofing standards. Architectural protection mesh sheets are mainly 1.8m wide x 3.4m long, with the edges folded back and reinforced with sewing, and have connecting means such as grommets and hook-and-loop fasteners on the edges. The raw material for architectural protection mesh sheets (or facades) includes "Tarposcreen (registered trademark)" (Class 1: #1003, #1004, #1005, #1023, #1034, Class 2: #2014, #2024, #2054, #2039), and are available in white, black, gray, blue, green, etc. In addition, "Tarp Screen" and "Light Screen (registered trademark)" are used as base fabric for sunshades in houses, apartments, stores, etc., as well as for indoor ceilings, partitions, banners, hanging banners, etc., and are used in any shape and size.
[0003] Construction companies often lease architectural protection mesh sheets for each construction project. The main reason for this is that construction sites want to always use clean and normal architectural protection mesh sheets in order to maintain a healthy corporate image and improve the image of the construction site environment. Architectural protection mesh sheets (for example, 1.8m wide x 3.4m long) are stored folded at right angles in four and transported to the construction site in that state. The folded and unfolded architectural protection mesh sheets are fixed along the pipe frames of the construction scaffolding, and the architectural protection mesh sheets are connected and expanded up, down, left, and right to complete the safety enclosure of the construction site. After the construction is completed, the architectural protection mesh sheets are removed and transported to the machine cleaning site in a folded state with soot dust, paint splashes, and other dirt still attached, and after cleaning, they are stored by the leasing company and then leased to the next construction site. This process of folding at right angles in four and machine cleaning is repeated. Troubles that occur under these conditions include deterioration of the architectural protection mesh sheet due to repeated machine washing, and changes in appearance, i.e., deterioration of the soft polyvinyl chloride resin coating layer due to alkaline detergents (deterioration of the polyvinyl chloride resin, deterioration and extraction of plasticizers). In addition, when unfolding the architectural protection mesh sheet in a four-folded state in the cold of winter, the architectural protection mesh sheet becomes brittle at low temperatures, causing cracks in the soft polyvinyl chloride resin coating layer, and the texture becomes hard in the cold, making the folded sheet bulky and inconvenient for transportation, handling, and storage. When the architectural protection mesh sheet is folded in four at right angles with excessive force, low-temperature brittle cracks occur in the soft polyvinyl chloride resin coating layer. Therefore, there is a demand for architectural protection mesh sheets that are resistant to folding and unfolding in cold conditions, as well as excellent resistance to washing. There is also a demand for mesh sheets for industrial materials such as facades.
[0004] Regarding the toughening of soft polyvinyl chloride resin coating layers of mesh sheets (for architectural protection, protective netting, etc.), the applicant disclosed in paragraph
[0023] of Patent Document 1 that the soft polyvinyl chloride resin layer contains a polyol compound, and a triisocyanate compound undergoes an addition reaction with the polyol compound to generate a crosslinked urethane component in the soft polyvinyl chloride resin layer, thereby improving the abrasion resistance, heat resistance, impact resistance, etc. of the soft polyvinyl chloride resin layer. The generation of this crosslinked urethane component improves the toughness of the soft polyvinyl chloride resin layer, but the more the amount of three-dimensional mesh-like crosslinked urethane by the triisocyanate compound (trifunctional monomer) increases, the harder the texture becomes in cold weather, and the soft polyvinyl chloride resin layer is vulnerable to cracking due to dynamic stress such as repeated bending, folding, and flapping, especially below freezing. This is considered to be due to the glass transition temperature difference between the soft polyvinyl chloride resin and the crosslinked urethane, and furthermore, the compatibility is significantly deteriorated below freezing. Therefore, there was a need to improve the toughness of the soft polyvinyl chloride resin layer and to make it less susceptible to cracking even when subjected to dynamic stress below freezing. If the problem of cracking at sub-freezing temperatures could be solved, it would be possible to obtain a mesh sheet with better resistance to folding, unfolding, and washing, which would be expected to extend the service life of applications such as architectural protection mesh sheets and facades. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2015-217608 A Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention provides a mesh sheet for industrial materials used for enclosing construction sites, repair and demolition sites of buildings, condominiums, schools, etc., as well as for enclosing the facades of buildings and repair sites of public facilities, which has excellent resistance to folding after use and recovery (especially in cold weather), resistance to unfolding during use (especially in cold weather), and also has excellent resistance to washing. [Means for solving the problem]
[0007] As a result of intensive research taking into consideration these points, the inventors have found that in a mesh sheet comprising a coarse woven fabric as a base fabric and a soft vinyl chloride resin-impregnated coating layer provided over the entire surface of the base fabric, by containing rubber crosslinks throughout the entire area of the soft vinyl chloride resin-impregnated coating layer, and this rubber crosslink is a condensation product of a reactive liquid synthetic rubber and a polyisocyanate compound, it is possible to obtain a mesh sheet for industrial materials which has excellent resistance to folding and unfolding, particularly below freezing points, and also has excellent resistance to washing, and have thus completed the present invention.
[0008] The mesh sheet for industrial materials of the present invention is a mesh sheet comprising a coarse woven fabric as a base fabric and a soft vinyl chloride resin-impregnated coating layer provided on the entire surface of the base fabric, the soft vinyl chloride resin-impregnated coating layer containing rubber crosslinks over the entire area, the rubber crosslinks being a condensate of a liquid synthetic rubber having either a -COOH group or a -OH group at the molecular end and a polyisocyanate compound, the liquid synthetic rubber being preferably one or more selected from butadiene-based, isoprene-based, and farnesene-based. This composite formation of rubber crosslinks makes it possible to obtain a mesh sheet for industrial materials that is excellent in resistance to folding (especially in cold weather) after use and recovery, resistance to unfolding (especially in cold weather) during use, and also excellent in washing resistance, for use in construction sites, repair sites, and demolition sites of buildings, condominiums, schools, etc., as well as in the facades of building facades and facades of repair sites of public facilities.
[0009] In the mesh sheet for industrial materials of the present invention, the rubber crosslinking is preferably an organic-inorganic composite crosslinking that further contains silica particles and is present as a part of the rubber crosslinking. By incorporating silica particles into a part of the condensation product of liquid synthetic rubber and polyisocyanate compound and becoming a part of the rubber crosslinking, the soft polyvinyl chloride resin impregnated coating layer is strengthened, and the deterioration and appearance change of the architectural protection mesh sheet due to repeated mechanical washing, that is, the deterioration of the soft polyvinyl chloride resin coating layer due to alkaline detergent (deterioration of polyvinyl chloride resin, deterioration and extraction of plasticizer) can be alleviated.
[0010] In the mesh sheet for industrial materials of the present invention, the silica particles are preferably surface-modified particles treated with a silane coupling agent. This surface modification is achieved by bonding a hydrolyzate of the silane coupling agent to the surface of the silica particles. The functional groups of the silica particles react with the terminal functional groups of the liquid synthetic rubber, and the functional groups of the silica particles react with the polyisocyanate compound at the same time to form an organic-inorganic composite crosslink in which the silica particles are interposed as part of the rubber crosslink. This further strengthens the soft polyvinyl chloride resin-impregnated coating layer, and can mitigate the deterioration and appearance change of the architectural protection mesh sheet caused by repeated mechanical washing, that is, the deterioration of the soft polyvinyl chloride resin coating layer caused by alkaline detergent (deterioration of the polyvinyl chloride resin, deterioration and extraction of the plasticizer).
[0011] The method for producing a mesh sheet for industrial materials of the present invention, in which a soft vinyl chloride resin-impregnated coating layer is formed on the entire surface of a coarse woven fabric, preferably comprises the steps of: 1) preparing a soft vinyl chloride resin composition containing at least four components: a) vinyl chloride resin; b) plasticizer; c) liquid synthetic rubber (liquid synthetic rubber having either a -COOH group or a -OH group at the molecular end of one or more synthetic rubbers selected from butadiene-based, isoprene-based, and farnesene-based synthetic rubbers); and d) polyisocyanate compound; 2) coating the soft vinyl chloride resin composition on the coarse woven fabric to form a soft vinyl chloride resin-impregnated coating layer; and 3) converting the liquid synthetic rubber into a crosslinked rubber to form rubber crosslinks over the entire area of the soft vinyl chloride resin-impregnated coating layer. After coating, the liquid synthetic rubber molecules are present in the soft polyvinyl chloride resin-impregnated coating layer in a state entangled with the polyvinyl chloride resin main chain, and by cross-linking this liquid synthetic rubber with a polyisocyanate compound, a state in which the rubber cross-links are entangled with the polyvinyl chloride resin main chain is formed throughout the entire soft polyvinyl chloride resin-impregnated coating layer, thereby obtaining a mesh sheet for industrial materials that has excellent resistance to folding (especially in cold weather) and resistance to unfolding during use (especially in cold weather), as well as excellent washability.
[0012] In the manufacturing method of the mesh sheet for industrial materials of the present invention, the soft polyvinyl chloride resin composition further contains silica particles, and it is preferable to form an organic-inorganic composite crosslink in which the silica particles are interposed in a part of the rubber crosslink. As a result, the silanol group (Si-OH group) on the surface of the silica particles reacts with the polyisocyanate compound to become a part of the rubber crosslink, or the silica particles to which functional groups treated with a silane coupling agent are introduced react with the polyisocyanate compound to become a part of the rubber crosslink, thereby making the soft polyvinyl chloride resin coating layer tougher, and the deterioration and appearance change of the architectural protection mesh sheet due to repeated mechanical washing, that is, the deterioration of the soft polyvinyl chloride resin coating layer due to alkaline detergent (deterioration of the polyvinyl chloride resin, deterioration and extraction of the plasticizer) can be alleviated. Effect of the Invention
[0013] According to the present invention, it is possible to obtain a mesh sheet for industrial materials that is excellent in resistance to folding (particularly in cold climates), resistance to unfolding during use (particularly in cold climates), and also excellent in washing resistance, and thus can be suitably used for enclosing construction sites, repair and demolition sites of buildings, condominiums, schools, etc., as well as for enclosing building facades and facades of repair sites of public facilities, etc. In addition, it can also be used for sunshades, indoor ceilings, partitions, banners, hanging banners, wind and snow fences, etc. for houses, condominiums, stores, etc. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The mesh sheet for industrial materials of the present invention is a mesh sheet comprising a coarse woven fabric as a base fabric and a soft polyvinyl chloride resin-impregnated coating layer provided on the entire surface of the base fabric, and includes an embodiment in which the soft polyvinyl chloride resin-impregnated coating layer contains a rubber crosslink throughout the entire area, the rubber crosslink being a condensation product of a liquid synthetic rubber having either a -COOH group or an -OH group at the molecular end and a polyisocyanate compound; an embodiment in which the rubber crosslink further contains silica particles and is an organic-inorganic composite crosslink interposed as part of the rubber crosslink; and an embodiment in which the silica particles are surface-modified particles treated with a silane coupling agent.
[0015] In the present invention, the yarns constituting the coarse woven fabric are preferably multifilament yarns such as polypropylene, polyethylene, polyvinyl alcohol, nylon (6 or 6,6), polyester (polyethylene terephthalate, polybutylene terephthalate, polynaphthalene terephthalate), and mixtures thereof (mixed twisted or double twisted). These yarns are uncolored yarns (natural) or dyed yarns that are optionally colored. Polyethylene terephthalate (PET), which is particularly versatile, can be used in any type, such as recycled PET bottles, recycled PET obtained by polymerizing recycled monomers obtained by depolymerizing recovered polyethylene terephthalate, biomass PET containing at least monomers synthesized using raw materials derived from plants as starting materials, and polyalkylene furanoate (alkylene is ethylene, propylene, butylene, trimethylene, etc.). In order to prevent holes caused by construction materials such as pipes and steel beams colliding with architectural protection mesh sheets, particularly inside and outside the enclosures of construction and demolition sites, it is possible to use a coarse woven fabric in which some of the yarns constituting the coarse woven fabric are replaced with multifilament yarns such as wholly aromatic polyester, wholly aromatic polyamide, or aromatic heterocyclic polymers (polybenzimidazole, polybenzoxazole, polybenzothiazole, and copolymers thereof).
[0016] For multifilament yarn, a long fiber spun bundle (50-500 filament bundle) made by extruding thermoplastic resins such as nylon or polyester (uncolored or dyed) from a spinneret and stretching the long fiber spun yarn 3-5 times can be used, either untwisted or twisted 10-200 times / m, as yarn (uncolored or dyed) with a fineness of 125-2000 denier (139-2222 dtex). For protective mesh sheets (class 1), a coarse imitation gauze fabric with a void ratio of 12-60% using three yarns of 750 (833 dtex)-1000 denier (1111 dtex) is suitable. For the protective mesh sheet (class 2), a plain weave coarse fabric or a basket weave fabric with a void ratio of 17 to 72% using yarns of 250 (278 dtex) to 500 (555 dtex) denier is suitable. These multifilament yarns include bulky processed yarns such as taslan yarns and woolly yarns. Covering yarns in which short fibers are wound around the outer periphery of the multifilament yarn bundles can also be used. These coarse fabrics are generally made by intertwining warp and bias yarns, but they may also be triaxial coarse fabrics made of warp yarns and bias yarns, or quadriaxial coarse fabrics made of warp yarns, weft yarns, and bias yarns. These triaxial or quadriaxial coarse fabrics containing bias yarns have excellent tear resistance, and therefore have the effect of keeping small holes caused by construction materials such as pipes and steel frames colliding with the architectural protective mesh sheet inside and outside the enclosure of a construction site or demolition site.
[0017] The voids in the coarse woven fabric used in the base fabric of the present invention act as ventilation holes, as well as mitigating the effects of strong winds and improving visibility within the enclosure. The coarse woven fabric may be, for example, a plain weave fabric (for protective mesh sheet type 2) with 26 250 (278 dtex) denier warp and weft threads woven in each inch, each with a void ratio of 31%, a plain weave fabric (for protective mesh sheet type 2) with 7 500 (555 dtex) denier warp and weft threads woven in each inch, each with a void ratio of 72%, or a plain weave fabric (for protective mesh sheet type 2) with 7 500 (555 dtex) denier warp and weft threads woven in each inch, each with 3 750 (832 dtex) denier warp and weft threads woven in each inch. Examples of such imitation woven fabrics include a 32% void ratio (for protective mesh sheet type 1) in which 9 warp and weft threads of 500 (555 dtex) denier yarns are woven per inch, and a 20% void ratio (for protective mesh sheet type 1) in which 9 warp and weft threads of 500 (555 dtex) denier yarns are woven per inch, and a 32% void ratio (for protective mesh sheet type 1) in which 13 warp and weft threads of 250 (278 dtex) denier yarns are woven per inch, and a 32% void ratio (for protective mesh sheet type 1) in which 13 warp and weft threads of 250 (278 dtex) denier yarns are woven per inch. The void ratio is the total area ratio of voids in any unit area of the coarse woven fabric. The total area of voids is calculated by subtracting the total area of the yarn body parts present in the unit area from the unit area. Specifically, a digital image of a 1-inch square mesh sheet is input into a computer, and the area of the yarn body parts and void parts is calculated based on the image. Alternatively, it may be a value calculated as a theoretical value based on the design of the yarn width and the yarn arrangement density.
[0018] The mesh sheet for industrial materials of the present invention is an embodiment in which a coarse woven fabric is used as a base fabric, and a soft vinyl chloride resin impregnated coating layer is provided on the entire surface of the base fabric. The soft vinyl chloride resin impregnated coating layer is formed by coating both sides of the coarse woven fabric with a soft vinyl chloride resin composition and heat treatment gelation, or by dipping the entire surface of the coarse woven fabric and heat treatment gelation. The impregnated layer means a soft vinyl chloride resin that has permeated the gaps between the filaments of the multifilament yarn that constitutes the coarse woven fabric, and may be an embodiment in which the entire multifilament yarn is impregnated, or an embodiment in which the core of the yarn is not impregnated, as shown by the cross section of . The coating layer is a film layer (0.01 to 0.25 mm) of soft vinyl chloride resin that completely covers the multifilament yarn. The mass (basis weight 55 to 220 g / m) of the coarse woven fabric is 0.01 to 0.25 mm. 2 The mass ratio of the soft vinyl chloride resin-impregnated coating layer to the mesh sheet is 1:1 to 2:5, preferably 1:1 to 2:3. The protective mesh sheet type 2 is, for example, a plain weave fabric with a void ratio of 31%, in which 26 warp and weft threads of 250 (278 dtex) denier are woven per inch, and the soft vinyl chloride resin-impregnated coating layer is formed on the plain weave fabric with a mass of 130 g / m. 2 For example, a plain weave fabric with a void ratio of 72%, in which 7 warp and weft yarns of 500 (555 dtex) denier are woven per inch, and a soft polyvinyl chloride resin impregnated coating layer is formed on the plain weave fabric with a mass of 160 g / m 2 For example, the protective mesh type 1 is a 470g / m2 soft polyvinyl chloride resin-impregnated coating layer formed on a 32% porosity imitation fabric, which is made of warp and weft threads each having 3 denier threads of 750 (832 dtex) per inch, with 7 threads per inch for each warp and weft. 2 For example, a 500 (555 dtex) denier yarn is used for the warp and weft, each of which has three yarns per inch, and 9 yarns are woven per inch for a 20% void ratio. A soft polyvinyl chloride resin impregnated coating layer is formed on the imitation fabric, which weighs 400 g / m 2 For example, a 32% void ratio imitation fabric is made by weaving 13 warp and weft threads per inch, each of which is made of 250 (278 dtex) denier yarns, with a mass of 455 g / m2 and a soft polyvinyl chloride resin impregnated coating layer.2 Examples of specifications include a void ratio of 30%.
[0019] The soft polyvinyl chloride resin composition is a liquid paste sol that contains four essential ingredients: polyvinyl chloride resin, a plasticizer, a liquid synthetic rubber having either a -COOH group or a -OH group at the molecular end, and a polyisocyanate compound. Specifically, the soft polyvinyl chloride resin composition mainly contains a paste polyvinyl chloride resin (emulsion polymerization type) having a number average molecular weight of 1000 to 2000, 40 to 100 parts by mass of a plasticizer (adipic acid ester compound, a phthalic acid ester compound, a cyclohexane dicarboxylate ester compound, a cyclohexene dicarboxylate ester compound, a phosphate ester compound, a chlorinated paraffin compound, a polyester compound, etc.) relative to 100 parts by mass of the paste polyvinyl chloride resin, 5 to 30 parts by mass of a liquid synthetic rubber (a butadiene rubber, an isoprene rubber, etc., having either a -COOH group or a -OH group at the molecular end, which is converted into a crosslinked rubber by a reaction with a polyisocyanate compound later) relative to 100 parts by mass of the paste polyvinyl chloride resin, and 2 to 15 parts by mass of a polyisocyanate compound relative to 100 parts by mass of the paste polyvinyl chloride resin. Other compounding agents include stabilizers (barium-zinc complexes, calcium-zinc complexes, epoxidized soybean oil, etc.), flame retardants (antimony trioxide, antimony pentoxide, aluminum hydroxide, magnesium hydroxide, zinc borate, etc.), fillers (calcium carbonate, barium sulfate, silica, talc, etc.), light resistance stabilizers (benzophenone tautomers, benzotriazole tautomers, triazine tautomers, hindered amine compounds, etc.), adhesives (multifunctional isocyanate compounds, silane coupling agents, etc.), antifungal agents (imidazo Preferred are blended compositions containing any and any amounts of compounds such as aryl compounds, thiazole compounds, isothiazoline compounds, pyridine compounds, N-haloalkylthio compounds, phenoxyarsine compounds, pigments (titanium oxide, carbon black, inorganic compounds, azo compounds, phthalocyanine compounds, anthraquinone compounds, quinacridone compounds, etc.), to which known additives such as fluorescent whitening agents, antistatic agents, surfactants, lubricants, antioxidants, chemical foaming agents, insect repellents, deodorants, and heat insulating agents can be added as necessary.
[0020] The liquid synthetic rubber having either a -COOH group or a -OH group at the molecular end may be one or more selected from butadiene-based rubber, isoprene-based rubber, and farnesene-based rubber. This liquid synthetic rubber is compatible with the plasticizer contained in the soft vinyl chloride resin composition, and penetrates into the vinyl chloride resin fine particles together with the plasticizer to become a softener for the vinyl chloride resin. In this state, the soft vinyl chloride resin composition is heated and gelled to form a soft vinyl chloride resin-impregnated coating layer. After coating, the liquid synthetic rubber molecules are entangled with the vinyl chloride resin main chain in the soft vinyl chloride resin-impregnated coating layer. Next, the liquid synthetic rubber is reacted with a polyisocyanate compound to form a hybrid in which a rubber crosslinked network is entangled with the vinyl chloride resin main chain throughout the soft vinyl chloride resin-impregnated coating layer.
[0021] The butadiene liquid rubber having either -COOH or -OH at the molecular end has a molecular weight Mn of 1000 to 5000, particularly 1300 to 3500, and a viscosity of 50 to 1000 poise (25°C), particularly 200 to 500 poise (25°C). This butadiene liquid rubber contains 5 to 25% by mass of styrene and / or acrylonitrile as a block copolymer component, and 10 to 50% by mass of isoprene or hydrogenated isoprene as a copolymer component. If the butadiene liquid rubber has about 75 to 80% of 1,4-cis structure or 1,4-trans structure and about 20 to 25% of 1,2-vinyl structure, it has low viscosity and excellent rubber elasticity when rubberized. The isoprene liquid rubber having either -COOH or -OH at (both) molecular ends is preferably one having a molecular weight Mn in the range of 3000 to 25000. This isoprene liquid rubber contains 5 to 25 mass% of styrene and / or acrylonitrile as a block copolymerization component, and 10 to 50 mass% of butadiene or hydrogenated isoprene as a copolymerization component. Examples of farnesene rubber having either -COOH or -OH at (both) molecular ends include rubbers using monomers such as α-farnesene ((3E,7E)-3,7,11-trimethyl-1,3,6,10-dodecatetraene) and β-farnesene (7,11-dimethyl-3-methylene-1,6,10-dodecatriene), copolymer rubber of farnesene and styrene, and copolymer rubber of farnesene and butadiene. The Funnelsen liquid rubber preferably has a molecular weight Mn in the range of 3000 to 50000. The rubber crosslinking of these liquid synthetic rubbers can be formed by dehydration condensation of -COOH groups and -OH groups at (both) molecular terminals, but is preferably formed by reaction with a polyisocyanate compound. As a crosslinking aid, diamines, polyamines, diisocyanates, epoxy-amines, aziridines, oxazolines, etc. can also be used in combination. Alternatively, diols, polyols, dicarboxylic acids, polycarboxylic acids, etc. can also be used in combination. Furthermore, as a part of the rubber crosslinking, an organic-inorganic composite crosslinking containing silica can be used.
[0022] Polyisocyanate compounds include isocyanurate-modified triisocyanate, which is a trimer of tolylene diisocyanate (TDI), isocyanurate-modified triisocyanate, which is a trimer of 4,4-diphenylmethane diisocyanate (MDI), isocyanurate-modified triisocyanate, which is a trimer of xylylene diisocyanate (XDI), and isocyanurate-modified triisocyanate, which is a trimer of tetramethylxylylene diisocyanate (mTMXDI). isocyanurate modified triisocyanate, which is a trimer of hexamethylene diisocyanate (HDI); isocyanurate modified triisocyanate, which is a trimer of isophorone diisocyanate (IPDI); isocyanurate modified triisocyanate, which is a trimer of hydrogenated xylylene diisocyanate (H6XDI); biuret modified triisocyanate, which is a trimer of TDI; biuret modified triisocyanate, which is a trimer of MDI; XDI 21 types of trifunctional isocyanate compounds can be used alone or in any combination: biuret modified triisocyanate which is a trimer of mTMXDI, biuret modified triisocyanate which is a trimer of HDI, biuret modified triisocyanate which is a trimer of IPDI, biuret modified triisocyanate which is a trimer of H6XDI, trimethylol alkyl modified triisocyanate which is a trimer of TDI, trimethylol alkyl modified triisocyanate which is a trimer of MDI, trimethylol alkyl modified triisocyanate which is a trimer of XDI, trimethylol alkyl modified triisocyanate which is a trimer of mTMXDI, trimethylol alkyl modified triisocyanate which is a trimer of HDI, trimethylol alkyl modified triisocyanate which is a trimer of IPDI, and trimethylol alkyl modified triisocyanate which is a trimer of H6XDI. In particular, it is preferable to use one or more triisocyanates selected from nine types of HDI, IPDI, and H6XDI triisocyanates as light-resistant, non-yellowing triisocyanates. These 21 types of triisocyanate compounds are preferably used in the form of blocked isocyanate compounds to which a blocking agent has been temporarily added in order to control the reactivity of the isocyanate group.Examples of blocking agents include alcohols, phenols, active methylenes, mercaptans, acid amides, acid imides, imidazoles, ureas, oximes, amines, imides, pyridines, pyrazoles, etc. These blocked isocyanates are dissociated by heating at a specific temperature, thereby regenerating the above 12 types of triisocyanate compounds individually.
[0023] The rubber crosslinking may be an organic-inorganic composite crosslinking in which silica particles are interposed as part of the rubber crosslinking. Silica is used in an amount of 1 to 25% by weight with respect to the liquid synthetic rubber, and is made part of the rubber crosslinking by forming chemical bonds between the silanol groups on the silica surface and the -COOH and -OH groups at the molecular ends (both) of the liquid synthetic rubber. Such crosslinking is formed by dehydration condensation between the -COOH and -OH groups at the molecular ends (both) of the liquid synthetic rubber and the silanol groups on the silica surface, and at the same time, a reaction in which the functional groups of the liquid synthetic rubber and the silanol groups of the silica particles are bonded with a polyisocyanate compound (paragraph
[0022] ). As a crosslinking aid, diamines, polyamines, diisocyanates, epoxy-amines, aziridines, oxazolines, etc. can also be used in combination. Diols, polyols, dicarboxylic acids, polycarboxylic acids, etc. can also be used in combination. The rubber crosslinks are generated simultaneously with the gelling heat treatment of the soft vinyl chloride resin paste that forms the soft vinyl chloride resin-impregnated coating layer, and a homogeneous rubber crosslink is compositely formed throughout the soft vinyl chloride resin-impregnated coating layer. The composite formation of the rubber crosslinks toughens the entire soft vinyl chloride resin-impregnated coating layer, and an industrial mesh sheet that is excellent in folding resistance (particularly in cold weather) and unfolding resistance during use (particularly in cold weather) and also excellent in washing resistance can be obtained. The soft vinyl chloride resin paste composition can also contain a silane coupling agent to assist the chemical bonding between the liquid synthetic rubber and silica.
[0024] Silica has a BET specific surface area of 100 to 300 m 2Synthetic amorphous silica having a particle size of 1 to 40 μm is preferred. Synthetic amorphous silica may be either wet-process silica (precipitation method or gel method) or dry-process silica (fumed silica). The surface of the silica has silanol (Si-OH group), and the silanol group reacts with -COOH group, -OH group at (both) ends of the liquid synthetic rubber molecule, polyisocyanate compound (paragraph
[0022] ), etc., and the silica particles become part of the rubber component, thereby toughening the entire soft vinyl chloride resin impregnated coating layer, thereby obtaining a mesh sheet for industrial materials that is more excellent in folding resistance (especially in cold weather) and unfolding resistance during use (especially in cold weather), and further excellent in washing resistance. Functional groups such as amino groups, vinyl groups, epoxy groups, methacryl groups, acrylic groups, chlorine groups, mercapto groups, isocyanurate groups, and isocyanate groups may be introduced into the silica surface. The silica particles are preferably surface-modified particles treated with a silane coupling agent. The silane coupling agent is an alkoxysilane compound having two or more different reactive groups in a molecule represented by the general formula: XR-Si(Y)3, for example, X=amino group (aminosilane), vinyl group (vinylsilane), epoxy group (epoxysilane), methacryl group (methacrylsilane), acrylic group (acrylicsilane), chloro group (chlorosilane), mercapto group (mercaptosilane), isocyanurate group (isocyanuratesilane), isocyanate group (isocyanatesilane), etc. (R=alkyl chain), Y=methoxy group, ethoxy group, etc. The surface modification of silica is the -Si-R-Si(Y)3 modification of the silanol group of silica, but may also be the (-O)3Si-RX modification of the siloxane bond portion of silica. The functional groups introduced into the silica particles react with the terminal functional groups of the liquid synthetic rubber, and the functional groups introduced into the silica particles react with the polyisocyanate compound at the same time, forming an organic-inorganic composite crosslink in which the silica particles are interposed as part of the rubber crosslink. This further strengthens the soft polyvinyl chloride resin impregnated coating layer, and can mitigate the deterioration and appearance change of the architectural protection mesh sheet caused by repeated mechanical washing, that is, the deterioration of the soft polyvinyl chloride resin coating layer caused by alkaline detergents (deterioration of the polyvinyl chloride resin, deterioration and extraction of the plasticizer).
[0025] The method for producing a mesh sheet for industrial materials of the present invention, in which a soft vinyl chloride resin-impregnated coating layer is formed on the entire surface of a coarse woven fabric, comprises the steps of: 1) preparing a soft vinyl chloride resin composition containing at least four components: a) vinyl chloride resin; b) plasticizer; c) liquid synthetic rubber (liquid synthetic rubber having either a -COOH group or a -OH group at the molecular end of one or more synthetic rubbers selected from butadiene-based, isoprene-based, and farnesene-based synthetic rubbers); and d) polyisocyanate compound; 2) coating the soft vinyl chloride resin composition on the coarse woven fabric to form a soft vinyl chloride resin-impregnated coating layer; and 3) converting the liquid synthetic rubber into a crosslinked rubber to form rubber crosslinks over the entire area of the soft vinyl chloride resin-impregnated coating layer. The application of the soft vinyl chloride resin composition (paste sol) to the coarse woven fabric and the formation of the soft vinyl chloride resin impregnated coating layer can be carried out by dipping (immersion - impregnation - roll squeezing - heat treatment gelation of the paste sol) or coating (impregnation coating - heat treatment gelation of the paste sol) such as gravure coating method, comma coating method, roll coating method, reverse roll coating method, bar coating method, doctor knife coating method, etc. In order to convert the liquid synthetic rubber into a crosslinked rubber, the -COOH group or -OH group at the molecular end of the liquid synthetic rubber is reacted with a polyisocyanate compound (paragraph
[0022] ). The conversion of the liquid synthetic rubber into a crosslinked rubber can be carried out simultaneously with the gelation of the soft vinyl chloride resin composition, thereby forming a homogeneous rubber crosslink throughout the soft vinyl chloride resin impregnated coating layer. Furthermore, the soft vinyl chloride resin composition further contains silica particles, and an organic-inorganic composite crosslink in which the silica particles are interposed in a part of the rubber crosslink can be formed. This strengthens the soft polyvinyl chloride resin coating layer, and can mitigate the deterioration and appearance change of the architectural protection mesh sheet caused by repeated mechanical washing, i.e., the deterioration of the soft polyvinyl chloride resin coating layer caused by alkaline detergents (deterioration of the polyvinyl chloride resin, deterioration and extraction of the plasticizer). The reaction between the liquid synthetic rubber and the crosslinking agent is preferably an equimolar reaction, but excess liquid synthetic rubber may remain in the soft polyvinyl chloride resin-impregnated coating layer. The remaining liquid synthetic rubber is compatible with the plasticizer and has the effect of lowering the glass transition temperature of the soft polyvinyl chloride resin-impregnated coating layer, i.e., it acts as an agent that imparts cold resistance.The remaining liquid synthetic rubber is preferably 1 to 10 parts by mass per 100 parts by mass of the vinyl chloride resin.
[0026] The mesh sheet for industrial materials of the present invention may also be provided with an antifouling layer, which is preferably formed on the soft polyvinyl chloride resin impregnated coating layer and formed over the entire mesh sheet. The antifouling layer is, for example, a transparent layer containing an acrylic resin, a fluorine-based copolymer resin, an acrylic-silicone copolymer resin, an acrylic-fluorine copolymer resin, an acrylic-urethane copolymer resin, a blend of an acrylic resin and a fluorine-based copolymer resin, or these resins containing silica particles, colloidal silica, an organosilicate, a silane coupling agent, an ultraviolet absorber (benzophenone tautomer, benzotriazole tautomer, triazine tautomer, etc.). The formation of these antifouling layers can be achieved by coating these coating materials on both sides of the mesh sheet by gravure coating or the like and drying them, or by coating these water-based coating materials on the entire surface of the mesh sheet by dipping or the like and drying them.
[0027] Architectural protection mesh sheets are available in sizes such as 1.8m wide x 3.4m long, 1.8m wide x 3.6m long, 1.8m wide x 5.1m long, 1.8m wide x 5.4m long and 3.6m wide x 5.4m long, with the edges folded back and reinforced with sewing, and with connecting means such as grommets or hook-and-loop fasteners on the edges.
[0028] The present invention will now be described in more detail with reference to examples and comparative examples, but the present invention is not limited to the scope of these examples. The test methods used in the examples and comparative examples of the present invention are as follows. (1) Dematcha cold bending fatigue durability test (JIS K6301 compliant) A 50mm wide x 150mm long sample was taken from the mesh sheet and left to rest in a -10℃ environment for 24 hours, after which a 25mm wide x 150mm long folded test piece was made by folding it in half from the center 25mm of the width, and then attached to a YSS Dematcha Flexing Tester (Yasuda Seiki Seisakusho Co., Ltd.) and a simulated test of repeatedly folding and unfolding the mesh sheet in cold conditions was carried out for 100 cycles in a constant temperature room at -10℃, and the surface condition of the test piece was observed to determine the dynamic cold resistance as follows. 1: No abnormality is detected 2: Minor cracks observed in the soft polyvinyl chloride resin impregnated coating layer 3: Large cracks were found in the soft polyvinyl chloride resin impregnated coating layer. (2) Washability The wash resistance of an unused mesh sheet sewn product (1.8m wide x 3.6m long: 8 folds in the length direction x 4 folds in the width direction) was evaluated using a 450L industrial rotary washing machine. The product was washed for 300 minutes at 30 to 35°C using 500g of alkaline industrial detergent (Genbu Nice manufactured by Genbu Co., Ltd.: [ingredients] sodium linear alkylbenzene sulfonate as a surfactant, sulfate as a processing agent, silicate and carbonate as alkaline agents, aluminosilicate as a water conversion agent, and fluorescent whitening agent) and 100g of sodium metasilicate nonahydrate as an additional alkaline agent dissolved in 300L of 40°C warm water. The product was washed for 300 minutes at 30 to 35°C and its appearance was observed immediately after washing. 1: No abnormalities in the appearance of the soft polyvinyl chloride resin impregnated coating layer 2: Peeling (lifting) is observed in part of the soft polyvinyl chloride resin impregnated coating layer. 3: The soft polyvinyl chloride resin impregnated coating layer has partially fallen off
[0029] Example 1 <Coarse fabric (1)> 1) A coarse woven fabric (1) with a void ratio of 31% was used, in which 250 (278 dtex) denier multifilament yarns made of green dyed polyester (polyethylene terephthalate) fiber were used as the warp and weft yarns, with 26 yarns per inch. 2) A vinyl chloride resin composition paste composition (containing four essential components: vinyl chloride resin, plasticizer, liquid synthetic rubber, and polyisocyanate compound) for forming a soft vinyl chloride resin impregnated coating layer was prepared according to the following <Recipe 1>. 3) A coarse-grained fabric (1) was immersed (dipped) in a liquid bath of a soft polyvinyl chloride resin composition <Blend 1>, and the paste composition of <Blend 1> was impregnated into the coarse-grained fabric (1) at normal pressure. The coarse-grained fabric (1) was then pulled out of the liquid bath and simultaneously squeezed with a rubber mangle roll to remove excess paste composition, thereby forming a soft polyvinyl chloride resin-impregnated coating layer. 4) Next, a gelling heat treatment is performed for 3 minutes in a hot air oven at 180°C to form a soft polyvinyl chloride resin-impregnated coating layer of 74 g / m 2 is formed on the entire coarse woven fabric (1), with a mass of 130 g / m 2 As a result, a mesh sheet (1) with a porosity of 29% and suitable for architectural curing purposes (Class 2) was obtained. This gelation heat treatment is a process in which the vinyl chloride resin composition paste composition is converted into soft vinyl chloride resin, and at the same time, liquid synthetic rubber (having either a -COOH group or a -OH group at the molecular end) is reacted with a polyisocyanate compound to convert it into crosslinked rubber, thereby forming a hybrid in which a rubber crosslinked network is entangled with the vinyl chloride resin main chain throughout the entire area of the resulting soft vinyl chloride resin impregnated coating layer. <Formulation 1> Paste composition for forming soft polyvinyl chloride resin impregnated coating layer Paste polyvinyl chloride resin (degree of polymerization 1700) 100 parts by weight Diisononyl phthalate (DINP plasticizer) 60 parts by weight Butadiene-based liquid rubber* 10 parts by mass Isocyanurate (HDI* trimer: NCO crosslinking agent) 2 parts by weight Chlorinated paraffin (flame retardant and plasticizer) 5 parts by weight Epoxidized soybean oil (stabilizer and plasticizer) 4 parts by weight Antimony trioxide (flame retardant) 20 parts by weight Zinc stearate (stabilizer) 2 parts by weight UV absorber (triazine tautomer) 0.5 parts by weight Titanium oxide (white pigment) 1 part by weight Phthalocyanine green (green pigment) 3 parts by weight Trichloroethylene (dilution solvent) 20 parts by weight *Butadiene liquid rubber: Contains 15% by mass of styrene as a block copolymer component. Properties: Average molecular weight 3000 with -COOH groups at both ends of the molecule *HDI: Hexamethylene diisocyanate HDI trimer (isocyanurate) has three isocyanate groups
[0030] Example 2 The same procedure as in Example 1 was repeated except that the paste composition of <Composition 1> in Example 1 was changed to the paste composition of <Composition 2>, and the mass was 130 g / m 2 As a result, a mesh sheet (2) with a porosity of 29% and suitable for architectural curing purposes (Class 2) was obtained. The paste composition of <Mixture 2> is prepared by replacing 10 parts by mass of the butadiene-based liquid rubber of <Mixture 1> with 10 parts by mass of isoprene-based liquid rubber. The isoprene-based liquid rubber contains 10% by mass of acrylonitrile as a block copolymer component, has -COOH groups at both ends of the molecule, and has an average molecular weight of 2500. As in Example 1, the rubber crosslinked network is entangled with the vinyl chloride resin main chain to form a hybrid throughout the entire area of the soft polyvinyl chloride resin impregnated coating layer.
[0031] Example 3 The same procedure as in Example 1 was repeated except that the paste composition of <Composition 1> in Example 1 was changed to the paste composition of <Composition 3>, and the mass was 130 g / m 2 As a result, a mesh sheet (3) with a porosity of 29% and suitable for architectural curing Class 2 was obtained. The paste composition of <Mixture 3> is prepared by replacing 10 parts by mass of the butadiene-based liquid rubber of <Mixture 1> with 10 parts by mass of β-funnelsen-based liquid rubber. The β-funnelsen-based liquid rubber contains 10% by mass of butadiene as a block copolymer component, has -COOH groups at both ends of the molecule, and has an average molecular weight of 5,000. As in Example 1, a hybrid is formed throughout the entire area of the soft polyvinyl chloride resin-impregnated coating layer, in which a rubber cross-linked network is entangled with the polyvinyl chloride resin main chain.
[0032] Example 4 The same procedure as in Example 1 was repeated except that the paste composition of <Composition 1> in Example 1 was changed to the paste composition of <Composition 4>, and a mass of 130 g / m 2 As a result, a mesh sheet (4) with a porosity of 29% and suitable for architectural curing Class 2 was obtained. The paste composition of <Formulation 4> is obtained by adding 2 parts by mass of surface-modified silica particles to the paste composition of <Formulation 1>. The surface-modified silica particles are dry silica (gel method: average particle diameter 2 μm, BET specific surface area 300 m 2 100g) in a 5% by mass aqueous solution of N-2-(aminoethyl)-3-aminopropyltrimethoxysilane (a silane coupling agent) was stirred at 24°C for 3 hours, then separated and dried, resulting in a mixture of -Si-R-Si(OCH3)3 modifications that bond to the silanol groups of the silica and (-O)3Si-R-NH2 modifications that bond to the siloxane moieties. The amino groups introduced into the silica particles react with the terminal functional groups of the liquid synthetic rubber, and the amino groups introduced into the silica particles react with the polyisocyanate compound at the same time, forming an organic-inorganic hybrid crosslink in which the silica particles are interposed as part of the rubber crosslink.
[0033] Example 5 The same procedure as in Example 2 was repeated except that the paste composition of <Recipe 2> in Example 2 was changed to the paste composition of <Recipe 4>, and the mass was 130 g / m 2 As a result, a mesh sheet (5) with a porosity of 29% and suitable for architectural curing purposes (Class 2) was obtained.
[0034] Example 6 The same procedure as in Example 3 was repeated except that the paste composition of <Recipe 3> in Example 3 was changed to the paste composition of <Recipe 4>, and a mass of 130 g / m 2 As a result, a mesh sheet (6) with a porosity of 29% and suitable for architectural curing Class 2 was obtained.
[0035] Example 7 The same procedure as in Example 1 was repeated except that the coarse woven fabric (1) used in Example 1 was changed to the coarse woven fabric (2). A soft polyvinyl chloride resin-impregnated coating layer of 305 g / m2 is formed on the entire coarse woven fabric (2), with a mass of 470 g / m 2 As a result, a mesh sheet (7) with a void ratio of 30% and class 1 construction protection grade was obtained. <Coarse fabric (2)> A 32% porosity imitation fabric made of green solution-dyed polyester (polyethylene terephthalate) fibers, with 750 (832 dtex) denier warp and weft threads, each consisting of 3 yarns per inch.
[0036] Example 8 The same as in Example 2 except that the coarse woven fabric (1) used in Example 2 was changed to the coarse woven fabric (2), and the mass was 470 g / m 2 As a result, a mesh sheet (8) with a void ratio of 30% and class 1 construction protection grade was obtained.
[0037] Example 9 The same as in Example 3 except that the coarse woven fabric (1) used in Example 3 was changed to the coarse woven fabric (2), and the mass was 470 g / m 2 As a result, a mesh sheet (9) with a void ratio of 30% and class 1 construction curing grade was obtained.
[0038] Example 10 The same as in Example 4 except that the coarse woven fabric (1) used in Example 4 was changed to the coarse woven fabric (2), and the mass was 470 g / m 2 As a result, a mesh sheet (10) with a void ratio of 30% and class 1 construction protection grade was obtained.
[0039] Example 11 The same as in Example 5 except that the coarse woven fabric (1) used in Example 5 was changed to the coarse woven fabric (2), and the mass was 470 g / m 2 As a result, a mesh sheet (11) with a void ratio of 30% and class 1 construction protection grade was obtained.
[0040] Example 12 The same as in Example 6 except that the coarse woven fabric (1) used in Example 6 was changed to the coarse woven fabric (2), and the mass was 470 g / m 2 As a result, a mesh sheet (12) with a void ratio of 30% and class 1 construction protection grade was obtained.
[0041] [Examples 13 to 18] The fluororesin paint of [Mixture 5] below was applied to both sides of the mesh sheets (7) to (12) of Examples 7 to 12 using a 100-mesh gravure roll, and then heated and dried for 2 minutes in a hot air oven at 120°C to harden the fluororesin paint of [Mixture 5] to form an antifouling layer (8 g / m on both sides). 2 ) and weighs 478g / m 2 Thus, mesh sheets (13) to (18) with an antifouling layer having a porosity of 30% were obtained. The obtained mesh sheets (13) to (18) were used at construction sites for a cumulative period of one year, and when they were washed after accumulating dirt such as soot and dust, they had such an antifouling effect that they could be washed to an appearance close to that when they were first used, and were superior in retention of the initial appearance to the mesh sheets (7) to (12) of Examples 7 to 12. [Formulation 5] Fluorine-based resin paint (for forming anti-fouling layer) Hydroxyl-containing fluoroolefin vinyl ether copolymer (fluorine-based resin) 100 parts by mass Isocyanurate trimer of hexamethylene diisocyanate (isocyanate) 10 parts by mass Colloidal silica (antistatic) 8 parts by weight Triazine tautomer (ultraviolet absorber) 5 parts by weight Curing catalyst: Dibutyltin dilaurate (approximately 10 ppm for fluororesin) Toluene / butyl acetate (diluent with a mass ratio of 1:1) 400 parts by mass
[0042] [Table 1]
[0043] [Table 2]
[0044] In the mesh sheets (1) to (3), (7) to (9) of Examples 1 to 3 and 7 to 9, rubber crosslinks are formed in the soft vinyl chloride resin-impregnated coating layer. The formation of the rubber crosslinks is carried out by applying a soft vinyl chloride resin paste composition containing a liquid synthetic rubber having either a -COOH group or a -OH group at the molecular end and a polyisocyanate compound to a coarse woven fabric (1) or (2), and then heating and gelling the soft vinyl chloride resin paste composition. At the same time, the liquid synthetic rubber is reacted with the polyisocyanate compound to convert it into a crosslinked rubber, thereby forming a rubber crosslinked network throughout the entire soft vinyl chloride resin-impregnated coating layer. In the applied soft polyvinyl chloride resin-impregnated coating layer, liquid synthetic rubber molecules are present in a state entangled with the polyvinyl chloride resin main chain, and by crosslinking this liquid synthetic rubber, a hybrid in which a rubber crosslinked network is entangled with the polyvinyl chloride resin main chain can be formed throughout the entire soft polyvinyl chloride resin-impregnated coating layer, making it possible to obtain a mesh sheet for industrial materials that has excellent washability and bending durability (resistance to folding and resistance to unfolding during use) at temperatures below freezing. In particular, by constructing the coarse woven fabric from dyed yarn and making the hue of the soft polyvinyl chloride resin-impregnated coating layer a similar color, a concealing effect is achieved that makes damage less noticeable even if the soft polyvinyl chloride resin-impregnated coating layer is damaged when it is hit by construction materials during use at a construction site, etc.
[0045] In the mesh sheets (4) to (6), (10) to (12) of Examples 4 to 6, and 10 to 12, rubber crosslinks were formed in the soft polyvinyl chloride resin-impregnated coating layer. The formation of the rubber crosslinks was carried out by applying a soft polyvinyl chloride resin paste composition containing a liquid synthetic rubber having either a -COOH group or a -OH group at the molecular end, a polyisocyanate compound, and further containing surface-modified silica particles (functional group introduction) to a coarse woven fabric (1) or (2), and then heating and gelling the soft polyvinyl chloride resin paste composition, reacting the liquid synthetic rubber with the polyisocyanate compound, and reacting the surface-modified silica particles with the polyisocyanate compound to convert the composition into a crosslinked rubber having silica particles interposed in part of the structure, thereby forming an organic-inorganic composite crosslinked network throughout the soft polyvinyl chloride resin-impregnated coating layer. In the applied soft polyvinyl chloride resin-impregnated coating layer, liquid synthetic rubber molecules are present in a state of being entangled with the polyvinyl chloride resin main chain, and by crosslinking this liquid synthetic rubber, a hybrid in which an organic / inorganic composite crosslinked network is entangled with the polyvinyl chloride resin main chain can be formed throughout the soft polyvinyl chloride resin-impregnated coating layer, so that a mesh sheet for industrial materials can be obtained that is more excellent in washing resistance and abrasion resistance than the mesh sheets (1)-(3), (7)-(9) of Examples 1-3, 7-9, and that is less damaged even in a 500-minute washing test. In particular, by forming the coarse woven fabric from dyed yarn and making the hue of the soft polyvinyl chloride resin-impregnated coating layer a similar color, even if damage occurs to the soft polyvinyl chloride resin-impregnated coating layer when it is hit by construction materials during use at a construction site, etc., a concealing effect is achieved that makes the damage less noticeable.
[0046] [Comparative Example 1] The same procedure as in Example 1 was repeated except that the paste composition of <Composition 1> in Example 1 was changed to the paste composition of <Composition 6>, and the mass was 130 g / m 2 As a result, a mesh sheet (19) with a porosity of 29% and suitable for architectural curing, Class 2, was obtained. The paste composition of <Mixture 6> is a conventional compound that omits 10 parts by mass of the butadiene liquid rubber (having -COOH groups at both ends of the molecule and an average molecular weight of 3000). Comparative Example 1 (conventional product) was inferior in bending durability (resistance to folding and resistance to unfolding during use) below freezing, and a solution to this problem was desired. (Recent state of the art)
[0047] [Comparative Example 2] The same procedure as in Example 1 was repeated except that the paste composition of <Composition 1> in Example 1 was changed to the paste composition of <Composition 7>. 2 As a result, a mesh sheet (20) with a porosity of 29% and suitable for architectural curing Class 2 was obtained. The paste composition of <Mixture 7> is prepared by replacing 10 parts by mass of the butadiene liquid rubber (having -COOH groups at both ends of the molecule and an average molecular weight of 3000) of <Mixture 1> with 10 parts by mass of a butadiene liquid rubber having no functional groups at both ends of the molecule and an average molecular weight of 3000. The butadiene liquid rubber having no functional groups remained in liquid form in the soft polyvinyl chloride resin-impregnated coating layer, and exerted the effect of lowering the glass transition temperature of the polyvinyl chloride resin, and thus had superior bending durability (resistance to folding and resistance to unfolding during use) below freezing point compared to the mesh sheet (1) of Example 1. However, the soft polyvinyl chloride resin-impregnated coating layer became too soft and swelled during washing, causing a part of the soft polyvinyl chloride resin-impregnated coating layer to fall off from the coarse woven fabric.
[0048] [Comparative Example 3] The same procedure as in Example 1 was repeated except that the paste composition of <Composition 1> in Example 1 was changed to the paste composition of <Composition 8>, and the mass was 130 g / m 2 As a result, a mesh sheet (21) with a porosity of 29% and suitable for architectural curing Class 2 was obtained. The paste composition of <Mixture 8> is obtained by replacing 10 parts by mass of the butadiene-based liquid rubber (having -COOH groups at both ends of the molecule and an average molecular weight of 3000) of <Mixture 1> with 10 parts by mass of butadiene rubber powder (registered trademark "Kane Ace" M-711: Kaneka Corporation). Although the butadiene rubber powder (non-crosslinked) itself has excellent cold resistance, it is incompatiblely dispersed in the soft polyvinyl chloride resin-impregnated coating layer in a sea-island shape, so that the fundamental cold resistance of the soft polyvinyl chloride resin-impregnated coating layer is not improved, and the bending cold resistance at the level of the mesh sheet (1) of Example 1 is not obtained, and rather many fine cracks due to the incompatible dispersion in the sea-island shape are generated. In addition, the butadiene rubber powder swells during washing, causing parts of the soft polyvinyl chloride resin-impregnated coating layer to fall off from the coarse woven fabric.
[0049] [Comparative Example 4] The same procedure as in Example 7 was repeated except that the paste composition of <Composition 1> was changed to the paste composition of <Composition 6>, and a mass of 470 g / m 2 As a result, a mesh sheet (22) with a void ratio of 30% and class 1 construction protection grade was obtained. The paste composition of <Mixture 6> is a conventional compound that omits 10 parts by mass of the butadiene liquid rubber (having -COOH groups at both ends of the molecule and an average molecular weight of 3000). Comparative Example 4 (conventional product) is inferior in bending durability (resistance to folding and resistance to unfolding during use) below freezing, and a solution to this problem was desired. (Recent state of the art)
[0050] [Comparative Example 5] The same procedure as in Example 7 was repeated except that the paste composition of <Composition 1> was changed to the paste composition of <Composition 7>. 2 As a result, a mesh sheet (23) with a porosity of 30% and class 1 construction protection grade was obtained. The paste composition of <Mixture 7> is obtained by replacing 10 parts by mass of the butadiene-based liquid rubber (having -COOH groups at both molecular terminals and an average molecular weight of 3000) of <Mixture 1> with 10 parts by mass of a butadiene-based liquid rubber having no functional groups at both molecular terminals and an average molecular weight of 3000. The butadiene-based liquid rubber having no functional groups remained in liquid form in the soft polyvinyl chloride resin-impregnated coating layer, and exerted the effect of lowering the glass transition temperature of the polyvinyl chloride resin, and thus had superior bending durability (resistance to folding and resistance to unfolding during use) below freezing point compared to the mesh sheet (7) of Example 7. However, the soft polyvinyl chloride resin-impregnated coating layer became too soft and swelled during washing, causing a part of the soft polyvinyl chloride resin-impregnated coating layer to fall off from the coarse woven fabric.
[0051] [Comparative Example 6] The same procedure as in Example 7 was repeated except that the paste composition of <Composition 1> was changed to the paste composition of <Composition 8>, and a mass of 470 g / m 2 As a result, a mesh sheet (24) with a porosity of 30% and class 1 construction protection grade was obtained. The paste composition of <Mixture 8> is obtained by replacing 10 parts by mass of the butadiene-based liquid rubber (having -COOH groups at both ends of the molecule and an average molecular weight of 3000) of <Mixture 1> with 10 parts by mass of butadiene rubber powder (registered trademark "Kane Ace" M-711: Kaneka Corporation). Although the butadiene rubber powder (non-crosslinked) itself has excellent cold resistance, it is incompatiblely dispersed in the soft polyvinyl chloride resin-impregnated coating layer in a sea-island shape, so that the fundamental cold resistance of the soft polyvinyl chloride resin-impregnated coating layer is not improved, and the bending cold resistance at the level of the mesh sheet (7) of Example 7 is not obtained, and rather many fine cracks due to the incompatible dispersion in the sea-island shape occur. In addition, the butadiene rubber powder swells during washing, causing parts of the soft polyvinyl chloride resin-impregnated coating layer to fall off from the coarse woven fabric.
[0052] [Table 3] [Industrial Applicability]
[0053] As is clear from the above examples and comparative examples, according to the present invention, it is possible to obtain a mesh sheet for industrial materials that is excellent in resistance to folding (particularly in cold weather), resistance to unfolding during use (particularly in cold weather), and also excellent in washing resistance, and is therefore suitable for use in enclosing construction sites, repair and demolition sites for buildings, condominiums, schools, etc., as well as for enclosing building facades and facades for repair sites for public facilities, etc. In addition, it can also be used for sunshades, indoor ceilings, partitions, banners, hanging banners, wind and snow fences, etc. for houses, condominiums, stores, etc.
Claims
1. The mesh sheet for industrial materials is characterized in that it is a mesh sheet comprising a coarse woven fabric as a base fabric and a soft vinyl chloride resin-impregnated coating layer provided on the entire surface of the base fabric, the soft vinyl chloride resin-impregnated coating layer contains rubber crosslinks throughout the entire area, the rubber crosslinks being a condensation product of a liquid synthetic rubber having either a -COOH group or an -OH group at the molecular end with a polyisocyanate compound, and the liquid synthetic rubber being one or more types selected from butadiene-based, isoprene-based, and farnesene-based rubbers.
2. 2. The mesh sheet for industrial materials according to claim 1, wherein the rubber crosslink is an organic-inorganic composite crosslink that further contains silica particles and is present as a part of the rubber crosslink.
3. 3. The mesh sheet for industrial materials according to claim 2, wherein the silica particles are surface-modified particles treated with a silane coupling agent.
4. A method for producing a mesh sheet for industrial materials, comprising forming a soft vinyl chloride resin-impregnated coating layer on the entire surface of a coarse woven fabric, the method comprising the steps of: 1) preparing a soft vinyl chloride resin composition comprising at least four components: a) vinyl chloride resin; b) a plasticizer; c) liquid synthetic rubber (a liquid synthetic rubber having either a -COOH group or a -OH group at the molecular end of one or more synthetic rubbers selected from butadiene-based, isoprene-based, and farnesene-based synthetic rubbers); and d) a polyisocyanate compound; 2) coating the soft vinyl chloride resin composition on the coarse woven fabric to form a soft vinyl chloride resin-impregnated coating layer; and 3) converting the liquid synthetic rubber into a crosslinked rubber to form rubber crosslinks over the entire area of the soft vinyl chloride resin-impregnated coating layer.
5. 5. The method for producing a mesh sheet for industrial materials according to claim 4, wherein the soft polyvinyl chloride resin composition further contains silica particles, and an organic-inorganic composite crosslink is formed in which the silica particles are interposed in a part of the rubber crosslink.
Citation Information
Patent Citations
JP1974085141A
Sheet-shaped material and its manufacture
JP1984103750A
Soft vinyl chloride resin-made industrial material sheet
JP2015205428A
Soft vinyl chloride resin-made industrial material sheet
JP2015217608A
Industrial tarpaulin and film material for tent structure
JP2016022708A