Production method of non-oriented silicon steel

Optimizing the chemical composition and process steps for non-oriented silicon steel production allows for relaxed sulfur content limits, achieving cost-effective and high-performance silicon steel production.

JP7591341B2Active Publication Date: 2024-11-28INST OF RES OF IRON & STEEL JIANGSU PROVINCE +2
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023519304
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-09-27
Filing Date
2021-08-04
Publication Date
2024-11-28
Estimated Expiration
2041-08-04

AI Technical Summary

Technical Problem

The production of non-oriented silicon steel is hindered by the need for ultra-low sulfur content, which increases production costs and complicates processes like hot metal desulfurization and RH refining, leading to erosion of equipment and high costs.

Method used

A method for producing non-oriented silicon steel with relaxed sulfur content limits of up to 0.008% by optimizing the chemical composition and process steps, including hot metal desulfurization, converter smelting, RH refining, continuous casting, hot rolling, pickling continuous rolling, annealing, and finishing, while controlling elements like Si, Mn, and P to maintain magnetic performance.

Benefits of technology

The method produces silicon steel with excellent magnetic performance and reduced production costs, stabilizing yield and avoiding equipment damage, thus promoting smooth production processes and lowering costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591341000004
    Figure 0007591341000004
  • Figure 0007591341000005
    Figure 0007591341000005
  • Figure 0007591341000006
    Figure 0007591341000006
Patent Text Reader

Abstract

The present invention discloses a non-oriented silicon steel and a method for producing the same. The non-oriented silicon steel is produced by hot metal desulfurization, converter smelting, RH refining, continuous casting, hot rolling, pickling and continuous rolling, annealing, painting, and finishing, and its chemical composition is, in mass percent, C≦0.003%, S≦0.008%, Si: 0.35%+Δ1, Mn: 0.15-0.25%, P: 0.04-0.06%, Sn: 0.015%+Δ2, Nb≦0.004%, V≦0.004%, Ti≦0.005%, Mo≦0.004%, Cr≦0.03%, Ni≦0.03%, Cu≦0.03%, N≦0.003%, and the balance is Fe and unavoidable impurities. When the thickness of the non-oriented silicon steel is 0.5 mm, P 1.5 / 50 ≦5.5W / kg, B 5000 ≧1.75, and desulfurization treatment is not required in RH refining.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing non-oriented silicon steel, which is a technical field related to the production of steel materials. Regarding do. [Background technology]

[0002] Non-oriented silicon steel is the core material of the rotor of electric motors and generators that operate in a rotating magnetic field, and good magnetic performance is required. Usually, the chemical composition is very strictly controlled to ensure the magnetic performance of non-oriented silicon steel. However, during the production and manufacturing of non-oriented silicon steel, the S element forms a solid solution and precipitates in MnS in the steel, which inhibits the growth of crystal grains during annealing, and further affects the magnetic performance of the manufactured product, specifically, the magnetic flux density decreases and the iron loss increases. Therefore, in the conventional technology, it is common to aim at realizing ultra-low S control in the chemical composition design and production process of non-oriented silicon steel.

[0003] In addition, for the ultra-low S chemical composition design of non-oriented silicon steel, the steps of hot metal desulfurization, converter smelting, RH refining and other steps in the production process need to be strictly controlled accordingly, which results in high production costs and ultimately affects the smooth progress of the work situation.

[0004] For example, in the RH refining step, it is necessary to desulfurize the molten steel with a desulfurization agent. As the molten steel circulates, the desulfurization agent comes into contact with the immersion tube of the RH refining furnace, and the CaF2 in the desulfurization agent reacts with CaO and Al2O3 in the castable lining of the immersion tube to produce a low-melting point material, 11CaO. · 7Al2O3 · This produces CaF2, which is corroded by molten steel and peels off in the molten steel, that is, the immersion tube of the RH refining furnace is severely corroded during the desulfurization treatment in the RH refining process, which increases the production cost and is very unfavorable to the smooth progress of the work situation.

[0005] Therefore, developing a chemical composition design plan for non-oriented silicon steel, relaxing the requirements for S content, and enabling the magnetic performance of low-grade products to be satisfied is of great value in the industrial production of non-oriented silicon steel.

Summary of the Invention

[0006] In order to solve the technical problem of high production cost caused by the ultra-low S chemical composition design plan of non-oriented silicon steel in the prior art, an object of the present invention is to provide a production method of non-oriented silicon steel do.

[0007] In order to achieve the above object of the invention, an embodiment of the present invention includes the steps of hot metal desulfurization, converter steelmaking, RH refining, continuous casting, hot rolling, pickling continuous rolling, annealing, coating and finishing, By mass percentage, C≦0.003%, S≦0.008%, Si: 0.35%+Δ1, Mn: 0.15~0.25%, P: 0.04~0.06%, Sn: 0.015%+Δ2, Nb≦0.004%, V≦0.004%, Ti≦0.005%, Mo≦0.004%, Cr≦0.03%, Ni≦0.03%, Cu≦0.03%, N≦0.003%, and the balance is Fe and inevitable impurities, to produce a non-oriented silicon steel product that meets the chemical composition design plan, When the molten steel reaches RH refining and S≦0.0030%, Δ1=Δ2=0, When the molten steel reaches RH refining and 0.0030%<S≦0.0045%, Δ1=0.05% and Δ2=0.005%, When the molten steel reaches RH refining and 0.0045%<S≦0.060%, Δ1=0.15% and Δ2=0.010%, When the molten steel reaches RH refining and 0.0060%<S≦0.0075%, Δ1=0.25% and Δ2=0.020%, to provide a production method of non-oriented silicon steel.

[0008] Preferably, the thickness of the non-oriented silicon steel product is 0.500±0.005mm, and its iron loss is P 1.5 / 50 ≦5.5W / kg, and the magnetic flux density is B5000 ≧1.75.

[0009] Preferably, in the case of a hot metal desulfurization process, The temperature of the molten pig iron before desulfurization is controlled to ≧1350°C and the chemical components are controlled to satisfy, in mass percent, Si: 0.20-0.70%, S≦0.05%, Nb≦0.005%, V≦0.04%, Ti≦0.06%, Mo≦0.001%, Cr≦0.03%, Ni≦0.03%, and Cu≦0.03%. The molten pig iron before desulfurization is desulfurized, and the temperature of the molten pig iron after desulfurization is controlled to ≧1320°C and the S content, in mass percent, is ≦0.0015%. In the case of converter smelting process, The desulfurized molten iron is mixed with steel scrap and smelted in a converter. During tapping, a sufficient amount of tin ingot is added to the tapping molten steel according to the basic chemical composition plan of Δ1=Δ2=0 in the chemical composition design plan. After tapping is completed, a slag surface deoxidizer is added to the molten steel. In the case of RH refining process, The mass percentage of S contained in the molten steel when it reaches the RH refining is detected, and the values ​​of Δ1 and Δ2 in the chemical composition design plan are determined to obtain a final chemical composition plan. The molten steel is decarbonized in a pre-evacuated RH refining furnace, and then ultra-low titanium silicon iron, tin ingot, low titanium phosphorus iron and manganese metal are added to the molten steel according to the final chemical composition plan, and the molten steel is washed and circulated for more than 7 minutes before being tapped out. No desulfurization agent is added in the RH refining process.

[0010] In the case of the hot metal desulfurization process, the slag removal rate of the hot metal after desulfurization is preferably controlled to ≧98%.

[0011] Preferably, in the case of the converter smelting process, the amount of added steel scrap accounts for 20-25% of the total of the steel scrap and the molten iron, and lime is added first during tapping, and then tin ingot is added.

[0012] Preferably, in the hot rolling process, the continuously cast slab is successively subjected to continuous cast slab heating, intermediate slab rolling, finish rolling and coiling to produce a hot roll, in which the heating temperature of the continuously cast slab is 1130-1160°C and the heat retention time is ≧180 minutes, the thickness of the intermediate slab is 35-40 mm, the final rolling temperature is 865±15°C, the coiling temperature is 680°C±20°C and the thickness of the hot roll is 2.70±0.1 mm.

[0013] Preferably, in the case of the pickling continuous rolling process, the hot roll obtained by hot rolling is pickled with HCl, rinsed and dried, and then cold rolled to produce a hard rolling roll, in which the cold rolling reduction is 80-83%, and the hard rolling thickness is 0.501±0.005 mm.

[0014] Preferably, three-stage pickling is performed with HCl, where the concentration of the first-stage acid is 50 to 80 g / L and the Fe content in the acid is 1.0 to 1.0 g / L. 2+ The concentration of the second acid solution is 90-120g / L and the Fe concentration in the acid solution is ≦130g / L. 2+ The concentration of the acid in the third stage is 140-160g / L and the Fe concentration in the acid is less than 90g / L. 2+ The concentration is ≦50 g / L, During each pickling step, the acid temperature is 75-85°C, and the weight percentage of the silicon steel pickling accelerator in the acid solution is 0.05-0.10%. The temperature of the rinsing water is 45-55℃, and the pickling and rinsing speed is controlled at 100-180mpm.

[0015] Preferably, in the annealing process, the cold hard rolled steel strip is annealed in a continuous annealing furnace in a mixed atmosphere of H2 and N2, the annealing temperature is 850±5°C, the annealing time is 60±5 seconds, and the annealed steel strip is cooled by three-stage cooling; However, the first cooling stage is a high-temperature slow cooling stage, in which the steel strip is cooled from the annealing temperature to 800°C at a cooling rate of ≦5°C / s, The second stage cooling is controlled by circulating gas injection, and the steel strip is continuously cooled to below 300°C at a cooling rate of ≦15°C / s. The cooling in the third stage is cooling by circulating water injection, and the steel strip is continuously cooled to 100°C or lower.

[0016] Preferably, in the case of the painting and finishing process, painting and finishing are performed on the steel strip cooled to 100°C or lower in annealing to obtain a non-oriented silicon steel product with a thickness of 0.500 ± 0.005 mm.

[0017] One embodiment is manufactured using the processes of hot metal desulfurization, converter steelmaking, RH refining, continuous casting, hot rolling, pickling continuous rolling, annealing, painting, and finishing. In mass percentage, C ≦ 0.003%, S ≦ 0.008%, Si: 0.35% + Δ1, Mn: 0.15 - 0.25%, P: 0.04 - 0.06%, Sn: 0.015% + Δ2, Nb ≦ 0.004%, V ≦ 0.004%, Ti ≦ 0.005%, Mo ≦ 0.004%, Cr ≦ 0.03%, Ni ≦ 0.03%, Cu ≦ 0.03%, N ≦ 0.003%, and the balance is Fe and unavoidable impurities as the chemical composition. When S ≦ 0.0030% when the molten steel reaches RH refining, Δ1 = Δ2 = 0. When 0.0030% < S ≦ 0.0045% when the molten steel reaches RH refining, Δ1 = 0.05% and Δ2 = 0.005%. When 0.0045% < S ≦ 0.060% when the molten steel reaches RH refining, Δ1 = 0.15% and Δ2 = 0.010%. When 0.0060% < S ≦ 0.0075% when the molten steel reaches RH refining, Δ1 = 0.25% and Δ2 = 0.020%, and a non-oriented silicon steel is further provided.

[0018] To achieve the object of the above invention, one embodiment of the present invention provides a non-oriented silicon steel and a production method of the non-oriented silicon steel. The production method manufactures a non-oriented silicon steel product with a thickness of 0.5 ± 0.005 mm through the processes of hot metal desulfurization, converter steelmaking, RH refining, continuous casting, hot rolling, pickling continuous rolling, annealing, painting, and finishing. The iron loss of the non-oriented silicon steel product is P 1.5 / 50 ≦ 5.5 W / kg, and the magnetic flux density is B 5000 ≧ 1.75. However, in the hot metal desulfurization process, The temperature of the molten pig iron before desulfurization is controlled to ≧1350°C and the chemical components are controlled to satisfy, in mass percent, Si: 0.20-0.70%, S≦0.05%, Nb≦0.005%, V≦0.04%, Ti≦0.06%, Mo≦0.001%, Cr≦0.03%, Ni≦0.03%, and Cu≦0.03%. The molten pig iron before desulfurization is desulfurized, and the temperature of the molten pig iron after desulfurization is controlled to ≧1320°C and the S content, in mass percent, is ≦0.0015%. In the converter smelting process, The desulfurized molten iron is mixed with steel scrap and smelted in a converter, a sufficient amount of tin ingot is added to the tapped molten steel according to a basic chemical composition plan during tapping, and a slag surface deoxidizer is added to the molten steel after tapping is completed, the basic chemical composition plan being, in mass percent, C≦0.003%, S≦0.008%, Si:0.35%, Mn:0.15-0.25%, P:0.04-0.06%, Sn:0.015%, Nb≦0.004%, V≦0.004%, Ti≦0.005%, Mo≦0.004%, Cr≦0.03%, Ni≦0.03%, Cu≦0.03%, N≦0.003%, the balance being Fe and unavoidable impurities; In the RH refining process, The molten steel is decarbonized in a pre-evacuated RH refining furnace. Subsequently, alloying treatment is carried out based on the mass percentage of S contained in the molten steel when reaching RH refining. When S ≤ 0.0030% when the molten steel reaches RH refining, ultra-low titanium silicon iron, low titanium phosphorus iron and metallic manganese are added to the molten steel according to the basic chemical composition plan. When 0.0030% < S ≤ 0.0045% when the molten steel reaches RH refining, Si and Sn in the basic chemical composition plan are adjusted to Si: 0.40% and Sn: 0.020% respectively. When 0.0045% < S ≤ 0.060% when the molten steel reaches RH refining, Si and Sn in the basic chemical composition plan are adjusted to Si: 0.50% and Sn: 0.025% respectively. When 0.0060% < S ≤ 0.0075% when the molten steel reaches RH refining, Si and Sn in the basic chemical composition plan are adjusted to Si: 0.60% and Sn: 0.035% respectively, and ultra-low titanium silicon iron, tin ingot, low titanium phosphorus iron and metallic manganese are added to the molten steel according to the adjusted chemical composition plan. Then, it is washed and circulated for 7 minutes or more and then tapped, and no desulfurizing agent is added in the RH refining process.

[0019] Compared with the prior art, the beneficial effects of the present invention are as follows.

[0020] (1) The non-oriented silicon steel product with a thickness of 0.500 ± 0.005 mm manufactured by using the production method has an iron loss of P 1.5 / 50 ≤ 5.5 W / kg and a magnetic flux density of B 5000 ≥ 1.75, has excellent magnetic properties, can meet the demand for low-standard non-oriented silicon steel for small and medium-sized motors, has a low production cost, and promotes the smooth progress of the working situation. (2) By controlling the contents of elements such as C, Nb, V, Ti, Mo, Cr, Ni, Cu, N, etc. and optimizing the corresponding relationship between the contents of Si, Sn and S, the upper limit of the S content can be relaxed to 0.0080%, that is, it can be controlled to satisfy S ≤ 0.008%. Under the condition of S ≤ 0.008%, it is further possible that S > 0.0050% to ≥ 0.0060%. The stabilization of the magnetic properties of the non-oriented silicon steel is guaranteed, and the increase in the S content does not cause the destabilization of the magnetic properties, and the stabilization of the yield is realized. (3) Magnetic properties are guaranteed, and by correspondingly designing the content of elements such as Mn and P, the strength and weldability of non-oriented silicon steel are both achieved. (4) In the above production method, the requirement for S content is reduced, and accordingly the difficulty of S control in processes such as hot metal desulfurization, converter smelting, and RH refining is reduced, the requirement for steel scrap in converter smelting is reduced, and costs are reduced. The RH refining process does not require desulfurization treatment, and the problem of erosion of the RH refining furnace immersion tube caused by desulfurization agents in the prior art is solved, the service life of the RH refining furnace immersion tube is improved, production costs are reduced, and the impact of equipment damage on the smooth progress of work is avoided. [Brief description of the drawings]

[0021] [Figure 1] 1 is a metallographic micrograph of a non-oriented silicon steel product sample in Example 1 of the present invention. [Diagram 2] 1 is a metallographic micrograph of a non-oriented silicon steel product sample in Example 2 of the present invention. [Diagram 3] 1 is a metallographic micrograph of a non-oriented silicon steel product sample in Example 3 of the present invention. [Figure 4] 1 is a metallographic micrograph of a non-oriented silicon steel product sample in Example 4 of the present invention. [Diagram 5] 1 is a metallographic micrograph of a non-oriented silicon steel product sample in Comparative Example 1 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] One embodiment of the present invention provides a method for producing non-oriented silicon steel. The method includes sequentially carrying out the steps of hot metal desulfurization, converter smelting, RH refining, continuous casting, hot rolling, pickling continuous rolling, annealing, painting, and finishing. The present embodiment further provides a non-oriented silicon steel produced using the method. That is, the non-oriented silicon steel is produced through the steps of hot metal desulfurization, converter smelting, RH refining, continuous casting, hot rolling, pickling continuous rolling, annealing, painting, and finishing.

[0023] Here, the chemical composition design plan of the non-oriented silicon steel is, by mass percentage, C ≤ 0.003%, S ≤ 0.008%, Si: 0.35% + Δ1, Mn: 0.15 - 0.25%, P: 0.04 - 0.06%, Sn: 0.015% + Δ2, Nb ≤ 0.004%, V ≤ 0.004%, Ti ≤ 0.005%, Mo ≤ 0.004%, Cr ≤ 0.03%, Ni ≤ 0.03%, Cu ≤ 0.03%, N ≤ 0.003%, and the balance is Fe and inevitable impurities.

[0024] However, when S ≤ 0.0030% when the molten steel reaches RH refining, Δ1 = Δ2 = 0; when 0.0030% < S ≤ 0.0045% when the molten steel reaches RH refining, Δ1 = 0.05% and Δ2 = 0.005%; when 0.0045% < S ≤ 0.060% when the molten steel reaches RH refining, Δ1 = 0.15% and Δ2 = 0.010%; when 0.0060% < S ≤ 0.0075% when the molten steel reaches RH refining, Δ1 = 0.25% and Δ2 = 0.020%.

[0025] That is, in the production method of the present invention, in the entire steelmaking process from the hot metal desulfurization process, through the converter steelmaking process and the RH refining process, to the continuous casting process, the content of each element is controlled according to the above chemical composition design plan, and further, a continuous casting slab and non-oriented silicon steel that meet the above chemical composition design plan are manufactured.

[0026] Here, based on the mass percentage of S contained in the molten steel when it reaches RH refining (that is, when it reaches RH refining, that is, when the molten steel has just entered the RH refining furnace and the RH refining process has not yet started), according to the correspondence relationship between Δ1, Δ2 and the S content in the molten steel, the mass percentages of Si and Sn in the chemical composition design plan are adjusted, and further, the content of each element is precisely controlled.

[0027] Using the above production method, a non-oriented silicon steel product with a thickness of 0.500 ± 0.005 mm is manufactured. By detection, the iron loss of the non-oriented silicon steel product is P 1.5 / 50 ≤ 5.5 W / kg, and the magnetic flux density is B 5000≧1.75, has excellent magnetic performance, can meet the demand for low-specification non-oriented silicon steel of small and medium-sized electric machines, and has low production costs to promote the smooth progress of work.

[0028] Each element in the chemical composition design proposal is explained as follows.

[0029] As for C, Nb, V, Ti, Mo, Cr, Ni, Cu, and N, the higher the content of these elements, the more disadvantageous it is for the growth of crystal grains during the annealing process, and further deteriorate the magnetic performance of the non-oriented silicon steel, resulting in increased iron loss and reduced magnetic flux density. Therefore, the lower the content is within a controllable range, the better, for example, C≦0.003%, Nb≦0.004%, V≦0.004%, Ti≦0.005%, Mo≦0.004%, Cr≦0.03%, Ni≦0.03%, Cu≦0.03%, N≦0.003%.

[0030] As mentioned in the Background Art, S dissolves and precipitates in the steel in the form of MnS, inhibits the growth of crystal grains during annealing, and further affects the magnetic properties of the manufactured product, so that in the conventional technology, it is common to aim for ultra-low S control, for example, to 0.0050% or less. On the other hand, in the present invention, by optimizing the corresponding relationship between the contents of Si and Sn and S, the upper limit of the S content can be relaxed to 0.0080%, that is, it is sufficient to control so as to satisfy S≦0.008%, and under the condition of S≦0.008%, S>0.0050% to ≧0.0060% is also possible, as shown in Examples 3 and 4 described later.

[0031] The Si content is controlled to 0.35 to 0.60%, and if the content is increased, the resistivity can be increased and the core loss can be effectively reduced.

[0032] The content of Sn is controlled to 0.015-0.035%, which is a grain boundary segregation element. In the non-oriented silicon steel of the present invention, the increase in the content of Sn can significantly reduce the proportion of unfavorable {111} texture and increase the magnetic flux density of the product.

[0033] The Mn content is controlled to 0.15 to 0.25% to ensure magnetic performance and suppress hot brittleness caused by S.

[0034] Regarding P, the content is controlled to 0.04-0.06%, which can effectively increase the strength of the non-oriented silicon steel and improve the punchability, and also ensure good welding performance. In particular, for the medium and low specification non-oriented silicon steel of the present invention, the Si content is relatively low, and the strengthening effect of P ensures sufficient strength.

[0035] In general, the present invention controls the contents of elements such as C, Nb, V, Ti, Mo, Cr, Ni, Cu, and N in the chemical composition design plan, and also designs the contents of elements such as Si, Sn, Mn, and P, thereby intentionally breaking away from the conventional technology and relaxing the upper limit of S content to 0.0080%, which not only ensures the magnetic properties, strength and weldability of non-oriented silicon steel, but also solves the problem of high production costs and poor workability caused by the strict control of ultra-low S in the existing method, thereby reducing production costs and promoting the smooth workability.

[0036] Specifically, each step of the production method described in one embodiment will be described in detail below.

[0037] (1)Hot metal desulfurization process Molten iron is desulfurized using KR desulfurization technology.

[0038] Here, the temperature of the molten iron before desulfurization is controlled to be ≧1350°C, and the chemical components of the molten iron before desulfurization are controlled to satisfy, in mass percent, Si: 0.20~0.70%, S≦0.05%, Nb≦0.005%, V≦0.04%, Ti≦0.06%, Mo≦0.001%, Cr≦0.03%, Ni≦0.03%, and Cu≦0.03%.

[0039] The temperature of the molten iron after desulfurization is controlled to ≧1320° C. and the S content, by mass percent, is ≦0.0015%. That is, after the molten iron desulfurization process, the S content in the molten iron is controlled to ≦0.0015% by mass.

[0040] Preferably, the slag removal rate of the molten iron after desulfurization is controlled to ≧98%.

[0041] (2) Converter smelting process The steel tapped in the hot metal desulfurization process (i.e., the hot metal after desulfurization) is transferred to a converter, and steel scrap is mixed in the converter, and the hot metal after desulfurization and the steel scrap are both smelted in the converter to obtain molten steel. Here, the steel scrap may preferably be clean steel scrap, and the amount of the steel scrap added accounts for 20 to 25% of the total of the steel scrap and the hot metal.

[0042] During tapping, a sufficient amount of tin ingot is added to the tapping molten steel according to the basic chemical composition plan of Δ1=Δ2=0 in the chemical composition design plan. Specifically, the chemical composition in the case of Δ1=Δ2=0 in the chemical composition design plan may be regarded as one basic chemical composition plan. Specifically, in mass percent, C≦0.003%, S≦0.008%, Si:0.35%, Mn:0.15-0.25%, P:0.04-0.06%, Sn:0.015%, Nb≦0.004%, V≦0.004%, Ti≦0.005%, Mo≦0.004%, Cr≦0.03%, Ni≦0.03%, Cu≦0.03%, N≦0.003%, the balance being Fe and unavoidable impurities. According to the basic chemical composition plan, the Sn content in the final non-oriented silicon steel product is assumed to be 0.015%, and the weight of the tin ingot to be added is calculated and added to the molten steel in its entirety.

[0043] Here, a method for determining the weight of a tin ingot will be described with an example. Assuming that the total amount of molten steel in the converter smelting process is M1, the weight of the tin ingot added in the converter smelting process is M2, and the weights of the ultra-low titanium silicon ferrous, low titanium phosphorus ferrous, and metal manganese further added in the next RH refining process are M3, M4, and M5 according to the basic design plan of Δ1=Δ2=0, the total amount of molten steel is set to (M1+M2+M3+M4+M5), the weight of the tin ingot M2 is calculated assuming that the mass percentage of Sn in the total amount of molten steel is 0.015%, the weight of the ultra-low titanium silicon ferrous is calculated assuming that the mass percentage of Si in the total amount of molten steel is 0.35%, the weight of the low titanium phosphorus ferrous is calculated assuming that P in the total amount of molten steel is 0.04-0.06%, and the weight of the ultra-low titanium silicon ferrous is calculated assuming that Mn in the total amount of molten steel is 0.15-0.25%. In the calculation process, M3, M4 and M5 are also roughly calculated according to the basic design plan, and are only provisional data to assist in determining M2, and are understood to be not the actual amounts added in the next RH refining step under certain conditions (e.g., when S>0.0030% when reaching the subsequent RH refining).

[0044] Preferably, the lime is added first during tapping and then a sufficient amount of the tin ingot is added, i.e., the lime is added before the tin ingot is added.

[0045] After tapping is completed, a slag surface deoxidizer is added to the molten steel.

[0046] (3) RH refining process This step is carried out in an RH refining furnace, adopting a decarburization treatment mode, and the treatment is carried out in the order of pre-evacuation, decarburization, alloying, cleaning circulation, and vacuum break.

[0047] Here, in order to facilitate the control of the amount of the corresponding alloy added in alloying, the mass percentage of S contained in the molten steel when it reaches the RH refining is detected, and the values ​​of Δ1 and Δ2 in the chemical composition design plan are determined to obtain the final chemical composition plan.

[0048] Specifically, when the molten steel reaches RH refining, S ≤ 0.0075%, and as described above, when S ≤ 0.0030% when the molten steel reaches RH refining, Δ1 = Δ2 = 0. In this case, it corresponds to the basic chemical composition plan, that is, the continuous casting slab finally cast from the molten steel and the final non-oriented silicon steel product satisfy the basic chemical composition plan.

[0049] When 0.0030% < S ≤ 0.0045% when the molten steel reaches RH refining, Δ1 = 0.05% and Δ2 = 0.005%. In this case, it corresponds to the first design plan after adjustment with Si: 0.40% and Sn: 0.020%. When 0.0045% < S ≤ 0.060% when the molten steel reaches RH refining, Δ1 = 0.15% and Δ2 = 0.010%. In this case, it corresponds to the second design plan after adjustment with Si: 0.50% and Sn: 0.025%. When 0.0060% < S ≤ 0.0075% when the molten steel reaches RH refining, Δ1 = 0.25% and Δ2 = 0.020%. In this case, it corresponds to the third design plan after adjustment with Si: 0.60% and Sn: 0.035%. Here, the first design plan, the second design plan, and the third design plan are all the final chemical composition plans obtained by adjusting Si and Sn in the basic chemical composition plan. That is, the continuous casting slab finally cast from the molten steel and the final non-oriented silicon steel product satisfy the final chemical composition plan.

[0050] In a preliminarily evacuated RH refining furnace, decarburize the molten steel to control the mass percentage of C contained therein.

[0051] After reaching RH refining, the molten steel is alloyed according to the final chemical composition plan based on the mass percentage of S contained in the molten steel. Specifically, when S ≤ 0.0030% when the molten steel reaches RH refining, ultra-low titanium silicon iron, low titanium phosphorus iron, and metallic manganese are added to the molten steel according to the basic chemical composition plan, that is, added with M3, M4, and M5 calculated in the converter steelmaking step. When 0.0030% < S ≤ 0.0045% when the molten steel reaches RH refining, according to the adjusted first design plan, ultra-low titanium silicon iron, tin ingot, low titanium phosphorus iron, and metallic manganese are added to the molten steel. When 0.0045% < S ≤ 0.060% when the molten steel reaches RH refining, according to the adjusted second design plan, ultra-low titanium silicon iron, tin ingot, low titanium phosphorus iron, and metallic manganese are added to the molten steel. When 0.0060% < S ≤ 0.0075% when the molten steel reaches RH refining, according to the adjusted third design plan, ultra-low titanium silicon iron, tin ingot, low titanium phosphorus iron, and metallic manganese are added to the molten steel.

[0052] For the first design plan, the second design plan, and the third design plan mentioned above, based on the basic chemical composition plan, the addition amount of ultra-low titanium silicon iron is further increased, and tin ingot is added. Regarding the determination method of the addition amounts of ultra-low titanium silicon iron, tin ingot, low titanium phosphorus iron, and metallic manganese in these three design plans, here, taking the first design plan as an example, it is described as follows.

[0053] As described above, assuming that the total amount of molten steel in the converter smelting step is M1, the weight of the tin ingot added in the converter smelting step is M2, and further, the weights of the extra-low titanium silicon iron, the tin ingot, the low titanium phosphorus iron, and the metal manganese further added in the RH refining step according to the first design plan are M3', M2', M4', and M5', respectively, the total amount of molten steel is (M1+M2+M3'+M2'+M4'+M5') and the mass percentage of Sn in the total amount of molten steel is 0.020% (i.e., Sn in the non-oriented silicon steel product: 0.020%). In this case, the weight M2' of the tin ingot to be added is calculated, the weight M3' of the ultra-low titanium silicon iron is calculated assuming that the mass percentage of Si in the total amount of the molten steel is 0.40% (i.e., Si in the non-oriented silicon steel product: 0.40%), the weight M4' of the low titanium phosphorus iron is calculated assuming that the mass percentage of P in the total amount of the molten steel is 0.04-0.06% (i.e., P in the non-oriented silicon steel product: 0.04-0.06%), and the weight M5' of the ultra-low titanium silicon iron is calculated assuming that the mass percentage of Mn in the total amount of the molten steel is 0.15-0.25% (i.e., Mn in the non-oriented silicon steel product: 0.15-0.25%). Then, according to the calculation results, sufficient amounts of ultra-low titanium silicon iron, tin ingot, low titanium phosphorus iron, and metal manganese are added to the molten steel.

[0054] After alloying, the steel is washed and circulated for at least 7 minutes before being tapped.

[0055] In the present invention, no desulfurization agent is added in the RH refining process, that is, the desulfurization treatment in the RH refining process of the prior art is omitted. From this, it can be seen that the present invention, by combining the design of chemical components with the improvement of production methods, breaks through the prior art and relaxes the upper limit requirement of S content to 0.0080%, not only ensuring the magnetic properties, strength and welding performance of non-oriented silicon steel, but also reducing the difficulty of S control in the processes of hot metal desulfurization, converter smelting, RH refining and the like. In particular, desulfurization treatment is not required in the RH refining process, solving the erosion of the RH refining furnace immersion tube caused by the desulfurization agent in the prior art, improving the service life of the RH refining furnace immersion tube, reducing production costs, and avoiding the impact of equipment damage on the smooth progress of the work situation.

[0056] (4) Continuous casting process The steel tapped in the RH refining process (i.e., the final molten steel obtained by smelting) is produced as a continuously cast slab in a continuous casting facility. The specific operation of the continuous casting process can be realized by using a conventional and feasible continuous casting technology, and therefore a detailed description thereof will be omitted.

[0057] (5) Hot rolling process The continuously cast slab is subjected to the steps of continuous cast slab heating, intermediate slab rolling, finish rolling, and coiling to produce hot rolls.

[0058] Here, the heating temperature of the continuous casting slab is 1130-1160℃, the heat retention time is ≥180min, and the thickness of the intermediate slab is 35-40mm. In this way, the extension of the heating time, the increase of the rolling force, the increase of the production difficulty, the decrease of the production efficiency, and the increase of the production cost caused by the low-temperature rolling can be avoided, and at the same time, the low-temperature rolling can prevent the precipitates such as MnS in the steel from dissolving during the heating process, thereby further ensuring the magnetic performance of the non-oriented silicon steel product.

[0059] The final rolling temperature is 865±15°C. When the Si content is less than 1.7%, there will be austenite-ferrite phase transition during hot rolling. Usually, when the Si content is 0.35%, the phase transition temperature is 880-910°C, and with the increase of Si content, the phase transition temperature increases. Due to the heat loss during rolling, the final rolling temperature is generally controlled between 800-920°C. For high silicon steel, the phase transition temperature is high, and the final rolling is performed between 800-920°C. Both are rolled in the ferrite region, so in order to obtain coarse grains, the higher the final rolling temperature, the better. However, for the non-oriented silicon steel of the present invention, the final rolling temperature is controlled at 865±15°C, which can avoid the final rolling pass being in the austenite region, and further avoid the deterioration of magnetic performance caused by the phase transformation to obtain fine crystal grains after rolling, and ensure that the final rolling pass is rolled in the two-phase region or ferrite region, thereby ensuring the formation of coarse crystal grains and optimizing magnetic performance.

[0060] The winding temperature is 680°C±20°C, which is favorable for the growth of crystal grains during the winding process, improves the magnetic properties, and avoids the formation of iron oxide skin, which is difficult to pickle.

[0061] The thickness of the hot roll is 2.70±0.1mm. The hot rolling thickness affects the deformation amount of cold rolling. The thinner the hot rolling thickness, the smaller the deformation amount of cold rolling, and the larger the crystal grains obtained.

[0062] (6) Pickling and continuous rolling process The hot roll obtained by hot rolling is pickled with HCl, rinsed and dried, and then cold rolled to produce a hard roll, in which the cold rolling reduction is 80-83% and the hard rolled thickness is 0.501±0.005 mm.

[0063] Preferably, three-stage pickling is performed with HCl, where the concentration of the first-stage acid is 50 to 80 g / L and the Fe content in the acid is 1.0 to 1.0 g / L. 2+ The concentration of the second acid solution is 90-120g / L and the Fe concentration in the acid solution is ≦130g / L. 2+ The concentration of the acid in the third stage is 140-160g / L and the Fe concentration in the acid is less than 90g / L. 2+ The concentration is ≦50 g / L,

[0064] During each pickling step, the acid temperature is 75-85°C, and the weight percentage of the silicon steel pickling accelerator in the acid solution is 0.05-0.10%.

[0065] The temperature of the rinsing water is 45-55℃, and the pickling and rinsing speed is controlled at 100-180mpm.

[0066] (7) Annealing process The cold hard roll steel strip is annealed in a continuous annealing furnace in a mixed atmosphere of H2 and N2, the annealing temperature is 850±5℃, the annealing time is 60±5 seconds, and the annealed steel strip is cooled by three-stage cooling, where the first stage is high-temperature slow cooling, the steel strip is cooled from the annealing temperature to 800℃ at a cooling rate of ≦5℃ / sec. The second stage is circulating gas injection controlled cooling, the steel strip after the first stage cooling is continuously cooled to ≦300℃ at a cooling rate of ≦15℃ / sec. The third stage is circulating water injection cooling, the steel strip after the second stage cooling is continuously cooled to ≦100℃.

[0067] The slower the cooling rate of the steel strip, the more advantageous it is for reducing the stress during cooling of the steel plate. However, if the cooling period is too long, the production costs will increase significantly. By controlling the above three-stage cooling method, the residual stress of the steel plate can be effectively controlled to ≦50MPa at low cost, which is advantageous for controlling the plate shape.

[0068] (8) Painting and finishing processes The steel strip cooled to below 100°C during annealing is then painted and finished. The specific operations can be realized using conventional and feasible painting and finishing techniques, and detailed descriptions are omitted. Finally, a non-oriented silicon steel product with a thickness of 0.500±0.005mm is obtained. Here, the stability of magnetic performance is improved by precise control over the hot roll thickness, hard rolled thickness (i.e., thickness after pickling and continuous rolling), and product thickness.

[0069] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0070] (1) The non-oriented silicon steel product having a thickness of 0.500±0.005 mm manufactured using the above production method has an iron loss of P 1.5 / 50 ≦5.5W / kg, magnetic flux density is B 5000 ≧1.75, has excellent magnetic performance, can meet the demand for low-specification non-oriented silicon steel of small and medium-sized electric machines, and has low production costs to promote the smooth progress of work. (2) By controlling the contents of elements such as C, Nb, V, Ti, Mo, Cr, Ni, Cu, and N, and optimizing the relationship between the contents of Si and Sn and S, the upper limit of the S content can be relaxed to 0.0080%. In other words, it is sufficient to control so that S≦0.008% is satisfied. As shown in Examples 3 and 4 described below, under the condition of S≦0.008%, S>0.0050% to ≧0.0060% is also possible. This ensures the stabilization of the magnetic properties of the non-oriented silicon steel, and an increase in the S content does not lead to instability in the magnetic properties, thereby realizing stabilization of the yield. (3) In addition to ensuring magnetic properties, the content of elements such as Mn and P is correspondingly designed to achieve both the strength and weldability of non-oriented silicon steel. (4) In the above production method, the requirement for S content is reduced, and accordingly the difficulty of S control in processes such as hot metal desulfurization, converter smelting, and RH refining is reduced, the requirement for steel scrap in converter smelting is reduced, and costs are reduced. The RH refining process does not require desulfurization treatment, and the problem of erosion of the RH refining furnace immersion tube caused by desulfurization agents in the prior art is solved, the service life of the RH refining furnace immersion tube is improved, production costs are reduced, and the impact of equipment damage on the smooth progress of work is avoided.

[0071] The detailed descriptions recited above are merely specific descriptions of possible embodiments of the present invention, and are not intended to limit the protection scope of the present invention; any equivalent embodiments or modifications that do not depart from the technical spirit of the present invention shall be included in the protection scope of the present invention.

[0072] Below, four examples according to this embodiment and one comparative example not according to this embodiment are selected to further illustrate the excellent progress of this embodiment, and of course, these four examples are only a part, not all, of the many modified examples included in this embodiment.

[0073] Specifically, four examples and one comparative example all provide non-oriented silicon steel, and the production methods thereof all include sequentially carrying out the steps of hot metal desulfurization, converter smelting, RH refining, continuous casting, hot rolling, pickling continuous rolling, annealing, painting and finishing.

[0074] Here, the chemical compositions of the non-oriented silicon steels in the four examples and one comparative example (i.e., the chemical composition of the molten steel tapped from RH refining / the chemical composition of the continuously cast slab) are expressed in mass percent, and the results of sampling and detection are shown in Table 1. Also, in the production processes of the four examples and one comparative example, the mass percent of S contained in the molten steel when it reaches the RH refining is also shown in Table 1. [Table 1]

[0075] Furthermore, the thickness, core loss, and magnetic flux density of the non-oriented silicon steel products manufactured in Examples 1 to 4 and Comparative Example 1 are shown in Table 2, and the metallographic micrographs of the non-oriented silicon steel are shown in Figures 1 to 5, respectively. [Table 2]

[0076] Comparing Examples 1 to 4 with Comparative Example 1, in one embodiment of the present invention, the chemical composition is designed based on the S content when the molten steel reaches the RH refining, and the ultra-low titanium silicon iron and tin ingot are supplemented during the alloying of the RH refining. The crystal grains in the metallographic structure of the obtained non-oriented silicon steel are relatively coarse, and the iron loss is P when the thickness is 0.5 mm. 1.5 / 50 ≦5.5W / kg, magnetic flux density is B 5000 ≧1.75, and it is clear that the magnetic performance is superior to that of Comparative Example 1.

[0077] Specifically, the production processes of Examples 1 to 4 and Comparative Example 1 are as follows.

[0078] (1)Hot metal desulfurization process In Examples 1 to 4 and Comparative Example 1, the hot metal desulfurization step is as follows: The temperature of the hot metal before desulfurization is controlled to ≧1350°C, and the chemical components of the hot metal before desulfurization are controlled to satisfy, in mass percent, Si: 0.20 to 0.70%, S≦0.05%, Nb≦0.005%, V≦0.04%, Ti≦0.06%, Mo≦0.001%, Cr≦0.03%, Ni≦0.03%, and Cu≦0.03%. The temperature of the hot metal after desulfurization is controlled to ≧1320°C, and the S content, in mass percent, is controlled to ≦0.0015%. The slag removal rate is controlled to ≧98%.

[0079] (2) Converter smelting process In Examples 1 to 4 and Comparative Example 1, the converter smelting step is as follows: The steel tapped in the hot metal desulfurization step (i.e., hot metal after desulfurization) is transferred to a converter and mixed with clean steel scrap in the converter, and the amount of steel scrap added is 20 to 25% of the total of the steel scrap and hot metal, and the hot metal after desulfurization and the steel scrap are smelted together in the converter to obtain molten steel. During tapping, lime is first added, and further, a sufficient amount of tin ingot is added to the tapped molten steel so that the final non-oriented silicon steel product contains Sn: 0.015%. After tapping is completed, a slag surface deoxidizer is added to the molten steel.

[0080] (3) RH refining process In Examples 1 to 4 and Comparative Example 1, the RH refining process is as follows: A decarbonization mode is adopted, and the processes are performed in the order of preliminary vacuum evacuation, decarbonization, alloying, cleaning circulation, and vacuum break. After alloying, cleaning circulation is performed for 7 minutes or more, and steel is tapped. In addition, no desulfurization agent is added in the RH refining process, i.e., no desulfurization treatment is performed.

[0081] Here, Examples 1 to 4 and Comparative Example 1 differ from each other only in the following respects regarding the converter smelting process.

[0082] In Example 1, as shown in Table 1, when the molten steel reached RH refining, S ≤ 0.0030%, and ultra-low titanium silicon iron, low titanium ferrophosphorus, and metallic manganese were added to the molten steel so that in the final non-oriented silicon steel product, Si: 0.35%, P: 0.04 - 0.06%, Mn: 0.15 - 0.25%. Refer to Table 1 for the mass percentages of the actual chemical components of the molten steel tapped from the RH refining.

[0083] In Example 2, as shown in Table 1, when the molten steel reached RH refining, 0.0030% < S ≤ 0.0045%, and ultra-low titanium silicon iron, tin ingot, low titanium ferrophosphorus, and metallic manganese were added to the molten steel so that in the final non-oriented silicon steel product, Si: 0.40%, Sn: 0.020%, P: 0.04 - 0.06%, Mn: 0.15 - 0.25%. Refer to Table 1 for the mass percentages of the actual chemical components of the molten steel tapped from the RH refining.

[0084] In Example 3, as shown in Table 1, when the molten steel reached RH refining, 0.0045% < S ≤ 0.060%, and ultra-low titanium silicon iron, tin ingot, low titanium ferrophosphorus, and metallic manganese were added to the molten steel so that in the final non-oriented silicon steel product, Si: 0.50%, Sn: 0.025%, P: 0.04 - 0.06%, Mn: 0.15 - 0.25%. Refer to Table 1 for the mass percentages of the actual chemical components of the molten steel tapped from the RH refining.

[0085] In Example 4, when the molten steel reached RH refining, 0.0060% < S ≤ 0.0075%, and ultra-low titanium silicon iron, tin ingot, low titanium ferrophosphorus, and metallic manganese were added to the molten steel so that in the final non-oriented silicon steel product, Si: 0.60%, Sn: 0.035%, P: 0.04 - 0.06%, Mn: 0.15 - 0.25%. Refer to Table 1 for the mass percentages of the actual chemical components of the molten steel tapped from the RH refining.

[0086] On the one hand, in Comparative Example 1, when the molten steel reached RH refining, 0.0060% < S ≤ 0.0075%, but still, as in the final non-oriented silicon steel product with Si: 0.35%, P: 0.04 - 0.06%, Mn: 0.15 - 0.25%, ultra-low titanium silicon iron, low titanium ferrophosphorus and metallic manganese were added to the molten steel. Refer to Table 1 for the actual chemical composition mass percentages of the molten steel after tapping from the RH refining. (4) Continuous casting process In Examples 1 - 4 and Comparative Example 1, in each case, the continuous casting process manufactures the molten steel tapped from the RH refining process into continuous casting slabs using continuous casting equipment.

[0087] (5) Hot rolling process In Examples 1 - 4 and Comparative Example 1, in each case, the hot rolling process manufactures hot rolls from the continuous casting slabs through continuous casting slab heating, intermediate slab rolling, finish rolling, and coiling in sequence.

[0088] Here, the specific values such as the heating temperature, holding time, intermediate slab thickness, final rolling temperature, coiling temperature, and hot roll thickness of the continuous casting slabs in Examples 1 - 4 and Comparative Example 1 are as shown in Table 3.

[0089] (6) Pickling and continuous rolling process In Examples 1 - 4 and Comparative Example 1, the pickling and continuous rolling process is as follows in each case.

[0090] The hot roll obtained by hot rolling is subjected to three-stage pickling with HCl. Here, the acid concentration in the first stage is 50 - 80 g / L and the Fe concentration in the acid solution ≤ 130 g / L, the acid concentration in the second stage is 90 - 120 g / L and the Fe concentration in the acid solution ≤ 90 g / L, and the acid concentration in the third stage is 140 - 160 g / L and the Fe concentration in the acid solution ≤ 50 g / L. During pickling at each stage, the acid solution temperature is 75 - 85°C, and a silicon steel pickling accelerator is added to the acid solution such that the weight percentage of the silicon steel pickling accelerator in the acid solution is 0.05 - 0.10%. 2+ concentration ≤ 130 g / L, the acid concentration in the second stage is 90 - 120 g / L and the Fe concentration in the acid solution ≤ 90 g / L, 2+ concentration ≤ 90 g / L, the acid concentration in the third stage is 140 - 160 g / L and the Fe concentration in the acid solution ≤ 50 g / L. 2+ During pickling at each stage, the acid solution temperature is 75 - 85°C, and a silicon steel pickling accelerator is added to the acid solution such that the weight percentage of the silicon steel pickling accelerator in the acid solution is 0.05 - 0.10%.

[0091] After rinsing and drying, cold rolling is performed to manufacture a hard roll. Here, the rinsing water temperature is 45-55°C, the pickling and rinsing speeds are controlled to 100-180mpm, and the cold rolling reduction and hard rolling thickness of Examples 1-4 and Comparative Example 1 are shown in Table 3.

[0092] (7) Annealing process In Examples 1 to 4 and Comparative Example 1, the annealing process is as follows: the steel strip of the cold hard roll is annealed in a mixed atmosphere of H2 and N2 in a continuous annealing furnace, the annealing temperature and the annealing time are as shown in Table 3, and the steel strip after annealing is cooled by three-stage cooling, where the first stage cooling is a high-temperature stage slow cooling, and the steel strip is cooled from the annealing temperature to 800°C at a cooling rate of ≦5°C / sec. The second stage cooling is circulating gas injection control cooling, and the steel strip after the first stage cooling is continuously cooled to 300°C or less at a cooling rate of ≦15°C / sec. The third stage cooling is circulating water injection cooling, and the steel strip after the second stage cooling is continuously cooled to 100°C or less. [Table 3]

[0093] (8) Painting and finishing processes In Examples 1 to 4 and Comparative Example 1, the painting and finishing steps are all as follows. The steel strip cooled to 100°C or less during annealing was painted and finished, and the thickness of the finally obtained non-oriented silicon steel product is as shown in Table 2.

[0094] As can be seen from the above, by comparing Examples 1 to 4 with Comparative Example 1, the iron loss of the non-oriented silicon steel product having a thickness of 0.500±0.005 mm manufactured using the production method described in this embodiment is P 1.5 / 50 ≦5.5W / kg, magnetic flux density is B 5000 ≧1.75, excellent magnetic performance, no desulfurization treatment is required in the RH refining process, the erosion of the RH refining furnace immersion tube caused by the desulfurization agent in the prior art is solved, the service life of the RH refining furnace immersion tube is improved, production costs are reduced, and the impact of equipment damage on the smooth progress of the work situation is avoided.

[0095] It should be noted that the experimental examples 1 to 4 are merely examples of the present embodiment, and the present embodiment does not have to be carried out in accordance with the experimental examples 1 to 4. As long as they do not deviate from the technical spirit of the present embodiment, any other embodiment different from the experimental examples is included in the scope of protection of the present invention.

Claims

1. A method for producing non-oriented silicon steel, comprising the steps of hot metal desulfurization, converter smelting, RH refining, continuous casting, hot rolling, pickling continuous rolling, annealing, painting and finishing, In the hot metal desulfurization process, the temperature of the molten pig iron before desulfurization is controlled to be ≧1350°C and the chemical components satisfy, in mass percent, Si: 0.20-0.70%, S≦0.05%, Nb≦0.005%, V≦0.04%, Ti≦0.06%, Mo≦0.001%, Cr≦0.03%, Ni≦0.03%, and Cu≦0.03%; the molten pig iron before desulfurization is desulfurized, and the temperature of the molten pig iron after desulfurization is controlled to be ≧1320°C and the S content, in mass percent, is ≦0.0015%; In the converter smelting process, The desulfurized molten iron is mixed with steel scrap and smelted in a converter, a sufficient amount of tin ingot is added to the tapped molten steel according to a basic chemical composition plan during tapping, and a slag surface deoxidizer is added to the molten steel after tapping is completed, the basic chemical composition plan being, in mass percent, C≦0.003%, S≦0.008%, Si: 0.35%+Δ1, Mn: 0.15-0.25%, P: 0.04-0.06%, Sn: 0.015%+Δ2, Nb≦0.004%, V≦0.004%, Ti≦0.005%, Mo≦0.004%, Cr≦0.03%, Ni≦0.03%, Cu≦0.03%, N≦0.003%, the balance being Fe and unavoidable impurities, and Δ1=Δ2=0, In the RH refining process, The mass percentage of S contained in the molten steel when it reaches the RH refining is detected, and the values ​​of Δ1 and Δ2 determined based on the detection results are applied to the formula of the basic chemical composition plan to obtain a final chemical composition plan, and the final chemical composition plan is When the molten steel reaches the RH refining stage, if S≦0.0030%, then Δ1=Δ2=0. When the molten steel reaches the RH refining stage, 0.0030%<S≦0.0045%, then Δ1=0.05% and Δ2=0.005%; When the molten steel reaches the RH refining stage, 0.0045%<S≦0.060%, then Δ1=0.15% and Δ2=0.010%; When the molten steel reaches the RH refining stage, 0.0060%<S≦0.0075%, then Δ1=0.25% and Δ2=0.020%; a decarbonization treatment of molten steel in a pre-evacuated RH refining furnace; then, in accordance with the final proposed chemical composition, adding ultra-low titanium silicon ferroconductive steel, low titanium ferrophosphorus and metallic manganese to the molten steel if S≦0.0030% when the molten steel reaches the RH refining; adding ultra-low titanium silicon ferroconductive steel, tin ingot, low titanium ferrophosphorus and metallic manganese to the molten steel if S≦0.0030%<S≦0.0075% when the molten steel reaches the RH refining; cleaning and circulating for 7 minutes or more before tapping out; and wherein no desulfurization agent is added in the RH refining process.

2. The thickness of the non-oriented silicon steel product is 0.500±0.005 mm, and its core loss is P 1.5/50 ≦5.5W / kg, magnetic flux density is B 5000 2. The method for producing non-oriented silicon steel according to claim 1, characterized in that the tensile strength is ≧1.

75.

3. 2. The method for producing non-oriented silicon steel according to claim 1, wherein in the hot metal desulfurization process, the slag removal rate of the hot metal after desulfurization is controlled to be ≧98%.

4. The method for producing non-oriented silicon steel as claimed in claim 1, characterized in that in the converter smelting process, the amount of added steel scrap accounts for 20-25% of the total of the steel scrap and the molten iron, and lime is added first during tapping, and tin ingot is further added.

5. 2. The method for producing non-oriented silicon steel according to claim 1, characterized in that in the hot rolling process, the continuously cast slab is successively subjected to continuous cast slab heating, intermediate slab rolling, finish rolling and coiling to produce a hot roll, wherein the heating temperature of the continuously cast slab is 1130-1160°C and the heat retention time is ≧180 minutes, the thickness of the intermediate slab is 35-40 mm, the final rolling temperature is 865±15°C, the coiling temperature is 680°C±20°C and the thickness of the hot roll is 2.70±0.1 mm.

6. The method for producing non-oriented silicon steel according to claim 1, characterized in that in the pickling continuous rolling process, the hot roll obtained by hot rolling is pickled with HCl, rinsed and dried, and then cold rolled to produce a hard roll, wherein the cold rolling reduction is 80-83%, and the hard rolled thickness is 0.501±0.005 mm.

7. The acid concentration in the first stage is 50 to 80 g / L, and the Fe content in the acid solution is 100%. 2+ The concentration of the acid solution in the second stage is 90 to 120 g / L and the Fe content in the acid solution is 2+ The concentration of the acid solution in the third stage is 140 to 160 g / L and the Fe content in the acid solution is 2+ The concentration is ≦50 g / L, During each pickling step, the acid temperature is 75-85°C, and the weight percentage of the silicon steel pickling accelerator in the acid solution is 0.05-0.10%. The method for producing non-oriented silicon steel as claimed in claim 6, characterized in that the temperature of the rinsing water is 45-55°C, and the pickling and rinsing speed is controlled at 100-180 mpm.

8. In the annealing process, the steel strip on the cold hard roll is fed into the H 2 and N 2 The annealing temperature is 850±5°C, the annealing time is 60±5 seconds, and the annealed steel strip is cooled by three-stage cooling. The first cooling stage is a high-temperature slow cooling stage, in which the steel strip is cooled from the annealing temperature to 800° C. at a cooling rate of ≦5° C. / s; The second stage of cooling is a circulating gas injection controlled cooling, in which the steel strip is subsequently cooled to below 300°C at a cooling rate of ≦15°C / s; 2. The method for producing non-oriented silicon steel according to claim 1, wherein the third cooling step is circulating water jet cooling, and the steel strip is subsequently cooled to below 100°C.

9. The method for producing non-oriented silicon steel according to claim 1, characterized in that in the painting and finishing process, the steel strip cooled to 100°C or less in the annealing is painted and finished to obtain a non-oriented silicon steel product with a thickness of 0.500±0.005 mm.

10. Through the processes of hot metal desulfurization, converter smelting, RH refining, continuous casting, hot rolling, pickling continuous rolling, annealing, painting and finishing, a non-oriented silicon steel product with a thickness of 0.5±0.005 mm is manufactured, and the core loss of the non-oriented silicon steel product is P 1.5/50 ≦5.5W / kg, magnetic flux density is B 5000 ≧1.75, In the hot metal desulfurization process, the temperature of the molten pig iron before desulfurization is controlled to be ≧1350°C and the chemical components satisfy, in mass percent, Si: 0.20-0.70%, S≦0.05%, Nb≦0.005%, V≦0.04%, Ti≦0.06%, Mo≦0.001%, Cr≦0.03%, Ni≦0.03%, and Cu≦0.03%; the molten pig iron before desulfurization is desulfurized, and the temperature of the molten pig iron after desulfurization is controlled to be ≧1320°C and the S content, in mass percent, is ≦0.0015%; In the converter smelting process, The desulfurized molten iron is mixed with steel scrap and smelted in a converter, a sufficient amount of tin ingot is added to the tapped molten steel during tapping according to a basic chemical composition plan, and after tapping is completed, a slag surface deoxidizer is added to the molten steel, the basic chemical composition plan being, in mass percent, C≦0.003%, S≦0.008%, Si: 0.35%, Mn: 0.15-0.25%, P: 0.04-0.06%, Sn: 0.015%, Nb≦0.004%, V≦0.004%, Ti≦0.005%, Mo≦0.004%, Cr≦0.03%, Ni≦0.03%, Cu≦0.03%, N≦0.003%, the balance being Fe and unavoidable impurities, In the RH refining process, The molten steel is decarbonized in a pre-evacuated RH refining furnace. Next, alloying is performed based on the mass percent of S contained in the molten steel when it reaches the RH refining. If S≦0.0030% when the molten steel reaches the RH refining, ultra-low titanium silicon iron, low titanium phosphorus iron, and metal manganese are added to the molten steel according to the basic chemical composition plan. If 0.0030%<S≦0.0045% when the molten steel reaches the RH refining, Si and Sn in the basic chemical composition plan are adjusted to Si: 0.40% and Sn: 0.020%, respectively. If 0.0045%<S≦0.060% when the molten steel reaches the RH refining stage, adjust Si and Sn in the basic chemical composition plan to Si:0.50% and Sn:0.025%, respectively; if 0.0060%<S≦0.0075% when the molten steel reaches the RH refining stage, adjust Si and Sn in the basic chemical composition plan to Si:0.60% and Sn:0.035%, respectively; and add ultra-low titanium silicon iron, tin ingot, low titanium phosphorus iron, and metal manganese to the molten steel according to the adjusted chemical composition plan; The method for producing non-oriented silicon steel is characterized in that the steel is then washed and circulated for 7 minutes or more before being tapped, and no desulfurization agent is added in the RH refining process.

Citation Information

Patent Citations

  • Semi-process cold-rolling non-oriented electrical steel and production process thereof

    CN103060680A

  • Production method of non-oriented electrical steel 50w800 with blueing coating

    CN106048140A

  • Steelmaking method of non-oriented silicon steel

    CN110592460A

  • Method for producing non-oriented silicon steel sheet

    JP2005002401A