Manufacturing aluminum alloy parts by additive manufacturing from powder mixtures containing yttria-stabilized zirconia
A powder mixture of aluminum and yttria-stabilized zirconia in additive manufacturing addresses hot cracking issues, enabling cost-effective production of crack-free aluminum alloy parts through equiaxed solidification.
Patent Information
- Application Number
- JP2020083383
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-05-13
- Filing Date
- 2020-05-11
- Publication Date
- 2024-11-28
- Estimated Expiration
- 2040-05-11
AI Technical Summary
Aluminum alloys suffer from hot cracking during additive manufacturing due to columnar dendritic solidification, which is thermodynamically sensitive, and existing solutions like using scandium or nanoparticles are costly.
A method involving a powder mixture of aluminum particles with yttria-stabilized zirconia particles and optionally a reducing element, promoting equiaxed solidification to prevent cracking, using a process like selective laser melting or electron beam melting.
The method produces crack-free aluminum alloy parts efficiently and cost-effectively, with yttria-stabilized zirconia facilitating grain growth and reducing elements enhancing the process, suitable for various industrial applications.
Smart Images

Figure 0007591356000002 
Figure 0007591356000003 
Figure 0007591356000004
Abstract
Description
[Technical field]
[0001] The present invention relates to the general field of manufacturing aluminium alloy parts by additive manufacturing.
[0002] The present invention relates to a method for producing an aluminum alloy component from a powder mixture that includes aluminum-based particles and particles containing yttria-stabilized zirconia.
[0003] The invention also relates to an aluminium alloy part obtained by this method.
[0004] The present invention is particularly interesting since it overcomes the problem of hot cracking of aluminum alloys in additive manufacturing processes involving melting.
[0005] The invention finds applications in many industrial sectors, in particular in the automotive, aeronautical, energy sectors (for example for the manufacture of heat exchangers) or in the case of structural reinforcement with untreated particles. [Background technology]
[0006] The various methods for the production of metal alloy parts by additive manufacturing (also called 3D printing) have in common the use of raw materials in the form of powders and the shaping of the metal alloy via a process of melting these powders.
[0007] Various related additive manufacturing methods include, inter alia, Powder Bed Fusion (or PBF for "Powder Bed Fusion") and methods of depositing material under focused energy (or DED for "Directed Energy Deposition").
[0008] The PBF method consists of melting specific areas of a powder bed, for example with laser light. The DED method consists of bringing in a solid material, for example in the form of a wire or powder, melting it, for example with laser light, and depositing the molten material.
[0009] This method allows the industrial production of parts of simple and complex shapes with sufficient mechanical properties.
[0010] However, some aluminum alloys, especially for solid fractions in the range of 0.9–0.98, are subject to problems of hot cracking due to columnar dendritic solidification, which is the origin of a microstructure sensitive to thermomechanical stresses during solidification.
[0011] To overcome this drawback, various solutions have been considered.
[0012] For example, it is possible to modify the chemical composition of powder alloys, especially with Scamalloy. This is a light alloy containing aluminum, magnesium and scandium that has been specially developed for additive manufacturing. Upon solidification, Al 3 Sc primary particles precipitate from the liquid and act as germs for grain growth of the Al matrix. Thus, scandium allows for the densification of the microstructure and the progression of equiaxed dendritic solidification. However, scandium is a particularly expensive element, which significantly increases the cost of the raw material.
[0013] Another solution involves adding nanoparticles of a material called a germinating material, which is cheaper than scandium, to the aluminum powder to promote equiaxed solidification.
[0014] In the patent application JP 2003-233636, an aluminum alloy powder is mixed with nanoparticles of Zr, Ta, Nb, Ti or any of their oxides, nitrides, hydrides, borides, carbides and aluminides, and an aluminum alloy part is produced by additive manufacturing. In various exemplary embodiments described, the part is produced, for example, by selective laser melting (also described as SLM) from a mixture comprising: - Aluminum and tantalum nanoparticles (1% by volume) with a diameter of 50 nm; or - Aluminum alloy (Al7075 or Al6061) and zirconium nanoparticles (1% by volume) with diameters of 500-1500 nm.
[0015] In a paper by Zhang et al. (Non-Patent Document 1), 2 mass % of zirconium particles having an average particle size of 8.8 μm are added to densify the particles of an aluminum alloy Al-Cu-Mg.
[0016] In a paper by Martin et al. (Non-Patent Document 2), the 7075 series (bimodal distribution of 15 μm and 45 μm) and the 6061 series (d 50 Aluminum alloy powder with a diameter of 45 μm was mixed with 1% by volume of hydrogen-stabilized zirconium (ZrH 2 ) nanoparticles to overcome the hot cracking problem of aluminum alloys obtained by SLM. The nanoparticles are electrostatically accumulated on the substrate powder in order to obtain a homogeneous distribution. No information is given about the particle size of the nanoparticles used. [Prior art documents] [Patent documents]
[0017] [Patent Document 1] International Publication No. 2018 / 144323
[0018] [Non-Patent Document 1] “Effect of Zirconium addition on crack,microstructure and mechanical behavior of selective laser melted Al-Cu-Mg alloy”,Scripta Materialia 134(2017),6-10 [Non-Patent Document 2] “3D printing of high-strength aluminum alloys”,Nature 549(2017),365-369 Summary of the Invention [Problem to be solved by the invention]
[0019] The object of the present invention is to provide a method for producing crack-free aluminum alloy parts, which is easy to implement and inexpensive.
[0020] To this end, the invention provides a method for producing an aluminium alloy part by additive manufacturing comprising at least one step of melting and then solidifying a layer of a powder mixture. The powder mixture comprises: - first particles containing at least 80% by weight of aluminum and up to 20% by weight of one or more additional elements; and - second particles of yttria-stabilized zirconia; The powder mixture includes at least 1.5 volume percent of the second particles.
[0021] The present invention uses yttria-stabilized zirconia particles (ZrO 2 -Y 2 O 3 , more commonly called YSZ), which distinguishes it fundamentally from the prior art. The addition of this particle makes it possible to promote an equiaxed solidification structure and thus eliminate cracking of the final part.
[0022] Unexpectedly, yttria-stabilized zirconia reacts with aluminum to form Al according to the following reaction: 3 Grain growth of Zr particles is generated.
[0023] [ka]
[0024] In fact, zirconia (ZrO 2 ) and yttria (Y 2 O 3Even though yttria-stabilized zirconia appears to be more thermodynamically stable than alumina regardless of temperature (see the Ellingham diagrams shown in Figures 1A and 1B, which are derived from data extracted from the papers by Shen [1] and Chu et al. [2], referenced at the end of the specification), the grain growth phase Al 2 O 3 is formed during the additive manufacturing process by decomposition of yttria-stabilized zirconia. 3 It has been observed that Zr is formed.
[0025] The lifetime of the molten metal bath formed in this way is relatively short (100 microseconds to 1 millisecond); 3 It was not clear that the Zr phase (second reaction) had time to undergo grain growth. At first glance, this in situ reaction is neither thermodynamically nor kinetically favorable for the thermal conditions imposed by this method.
[0026] Advantageously, the powder mixture further comprises a reducing element, by which is meant an element that is more reducible than Zr and Al, which, when oxidized, reduces the Al content by, for example, acting as a substrate for this grain growth. 3 Promotes non-uniform grain growth of Zr.
[0027] The reducing element is preferably magnesium or one of its alloys, in particular MgAl.
[0028] The oxidation of reducing elements is Al 2 O 3 This may be due to reactions with oxygen resulting from oxidation-reduction reactions in the presence of yttria and / or dissolution of the yttria stabilized zirconia particles.
[0029] The reducing element is Al 2 O 3 In the presence of Al, a redox reaction occurs, producing Al and an oxide of a reducing element, such as an oxide of magnesium Mg (e.g., MgO) or one of its alloys (preferably MgAl 2 O 4 )) may be formed.
[0030] Alternatively, the manufacturing process for aluminum alloy parts by additive manufacturing can lead to the dissolution of secondary particles of yttria-stabilized zirconia. The oxygen thus released can combine directly with reducing elements to form a non-uniform grain growth matrix.
[0031] Advantageously, the mixture comprises at least 0.5% by weight of reducing element, for example, the mixture comprises 0.5 to 10% by weight, preferably 0.6 to 5% by weight, and even better still 0.7 to 2% by weight of reducing element.
[0032] Preferably, the reducing element is present in the first particles, i.e. one of the additional elements of the aluminium alloy is the reducing element.
[0033] For alloy grades that do not contain reducing elements, the latter can be added in particulate form to the mixture. For example, Mg metal particles can be added. Also, magnesium oxide particles can be added.
[0034] According to certain embodiments, for alloy grades containing Mg, magnesium metal can also be added to compensate for differential evaporation that may occur during the additive manufacturing process.
[0035] Advantageously, yttria stabilized zirconia is a stable oxide and is easy to handle and / or store, as compared to metallic elements that are known to be highly reducible.
[0036] Advantageously, the second particles have a larger dimension ranging from 5 nm to 600 nm, preferably from 100 nm to 400 nm, and even better from 200 nm to 300 nm.
[0037] Advantageously, the volume fraction of the second particles (YSZ) in the powder mixture is in the range 1.5% to 5%, and even better in the range 1.5% to 2.5%.
[0038] Advantageously, the first particles have a larger dimension ranging from 10 μm to 100 μm, preferably from 20 μm to 65 μm.
[0039] Advantageously, the additional elements are selected from Cu, Si, Zn, Mg, Fe, Ti, Mn, Zr, Va, Ni, Pb, Bi and Cr.
[0040] Advantageously, the aluminium alloy is alloy 7075, alloy 6061, alloy 2219 or alloy 2024.
[0041] According to a first advantageous variant embodiment, the shaping technique is selective laser melting.
[0042] According to a second advantageous variant embodiment, the shaping technique is selective electron beam melting.
[0043] Advantageously, the mixing of the powders is carried out in a 3D dynamic mixer or by mechanical synthesis (mechanosynthesis).
[0044] Advantageously, the specific surface of the mixture after mixing using the Dynamic 3D Mixer is less than 0.3 m 2 / g.
[0045] This approach has many advantages: - It is easy to carry out since only the mixing of powders is required, it is a dry process, regardless of the amount of powder, it can be carried out quickly and is easy to set up; - It is interesting from an industrial point of view because it is inexpensive. To illustrate, the material cost of aluminum alloy 6061 is about 60 euros / kg, while the material cost of a powder mixture containing aluminum alloy 6061 and yttria-stabilized zirconia (1.5% by volume) is about 61.71 euros / kg. Tantalum oxide and ZrH 2 is significantly (at least 15 times more) expensive than yttria-stabilized zirconia; - Because yttria stabilized zirconia powder is an oxide, it is easy to store / handle without the need for an inert atmosphere; - When mixing powders, the volume ratio between the powders can be easily changed; - Easily adaptable to any additive manufacturing method and to any aluminum alloy subject to hot cracking problems; - Parameters traditionally used in additive manufacturing can be used.
[0046] The present invention also relates to an aluminum alloy part (or workpiece) obtained according to the above method, said part comprising yttria stabilized zirconia, said part being free of cracks / cracking.
[0047] Advantageously, the component is a heat exchanger.
[0048] Other features and advantages of the present invention will become apparent from the further description that follows.
[0049] It should be understood that this additional description is given to illustrate the scope of the invention and should not be construed as limiting the scope of the invention in any way.
[0050] The invention will be better understood from reading the description of exemplary embodiments, given purely indicative and in no way limiting, with reference to the accompanying drawings, in which: [Brief description of the drawings]
[0051] [Figure 1] Figure 1A, which has already been described, is an Ellingham diagram showing the stability of aluminum oxide (Al2O3) and zirconium oxide (ZrO2). Figure 1B, which has already been described, is an Ellingham diagram showing the stability of aluminum oxide (Al2O3) and yttrium oxide (Y2O3). [Diagram 2] FIG. 2 shows a schematic representation of a powder mixture according to a particular embodiment of the method of the present invention. [Diagram 3]3A, 3B, 3C, and 3D are photographs obtained with a scanning electron microscope (SEM) of aluminum particles and yttria stabilized zirconia (YSZ) particles at various volume concentrations in accordance with certain embodiments of the present invention. [Figure 4] Figure 4A is a photograph taken with an optical microscope along the plane XY of a part made from aluminum alloy 6061 particles, and Figures 4B, 4C, 4D and 4E are photographs taken with an optical microscope along the plane XY of parts made from mixtures of aluminum alloy 6061 particles and YSZ particles of various volume concentrations according to various embodiments of the present invention. [Diagram 5] 5A and 5B are electron backscatter diffraction (EBSD) images along the plane XZ of a part made from aluminum particles and a part made from a mixture of aluminum alloy 6061 particles and 2 vol.% YSZ particles in accordance with certain embodiments of the present invention. [Figure 6] 6A and 6B are photographs taken using an electron backscatter scanning electron microscope along the planes XY and XZ, respectively, of a part made from a mixture of aluminum alloy 6061 particles and 2 volume percent YSZ particles in accordance with a specific embodiment of the invention. [Figure 7] FIG. 7 is a graph showing the specific surface area of a mixture according to certain embodiments of the present invention as a function of volume percent of YSZ. [Figure 8] Figure 8A is a photograph obtained by transmission electron microscopy of a portion of a workpiece manufactured in accordance with certain embodiments of the present invention, while Figures 8B, 8C, and 8D are maps of the elements Zr, O, and Mg produced within the boxes of Figure 8A.
[0052] The various parts shown in the figures are not necessarily drawn to scale, in order to make the figures easier to read.
[0053] The various possibilities (variants and embodiments) are to be understood as not mutually exclusive but as being combinable with one another. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0054] The method for producing an aluminium alloy part (or workpiece) by additive manufacturing comprises the following successive steps: a) providing a powder mixture preferably consisting of: - a first powder comprising first particles 10 of a first material containing at least 80% by weight of aluminium and up to 20% by weight of one or more additional elements; - a second powder comprising second particles 20 made of a second material, which is yttria-stabilized zirconia; b) forming a layer of the powder mixture; c) locally melting the layer of powder mixture, preferably by scanning a laser light or by scanning an electron beam, to form a plurality of melted regions; d) cooling the plurality of molten regions of step c) to form a plurality of solidified regions that constitute a first element of the part to be produced.
[0055] Advantageously, steps b), c) and d) can be repeated at least once to form at least one further solidified region on the first solidified region. The method is repeated until the final form of the part is obtained. A first layer of the powder mixture is formed on a substrate.
[0056] The addition of yttria stabilized zirconia particles 20 (YSZ) to the aluminum-based target first particles 10 can provide an equiaxed solidification structure and final aluminum alloy part without cracking.
[0057] Preferably, the first particles 10 are functionalized with second particles 20 (FIG. 2).
[0058] Preferably, the second particles 20 are made of yttria stabilized zirconia.
[0059] The yttria-stabilized zirconia advantageously contains 1-10% by weight, preferably 3-10% by weight, of yttrium oxide, and it may also contain small amounts (typically less than 3% by weight) of contaminants normally encountered in powder manufacturing processes, in particular oxides such as hafnium oxide.
[0060] The second powder of yttria stabilized zirconia is preferably at least 1.5% by volume of the powder mixture, preferably 1.5% to 5%, for example 1.5% to 2.5%.
[0061] According to an advantageous embodiment, the first particles 10 have a larger dimension in the range of 10 μm to 120 μm, and the second particles 20 have a larger dimension in the range of 5 nm to 600 nm, preferably 100 nm to 600 nm, more preferably 100 nm to 400 nm, even more preferably 200 nm to 300 nm.
[0062] The first particle 10 and the second particle 20 are elements that can be spherical, ovoid or elongated in shape. Preferably, the particles are substantially spherical, with their largest dimension being their diameter.
[0063] The first powder is formed from first particles 10 made of a first material. The first material comprises at least 80% by weight aluminium, preferably at least 90% by weight aluminium.
[0064] The first particles 10 may contain up to 20% by weight, preferably up to 10% by weight, of one or more additional elements (also called alloying elements), preferably selected from zinc, magnesium, copper, silicon, iron, manganese, titanium, vanadium, bismuth, lead, nickel, zirconium and chromium.
[0065] Preferably the alloy is aluminium alloy 7075, alloy 2024, alloy 2219 or aluminium alloy 6061.
[0066] Advantageously, the powder mixture further comprises a reducing element, preferably magnesium or one of its alloys (in particular MgAl).
[0067] Preferably, the mixture contains at least 0.5% by mass of the reducing element, for example, 0.5 to 10% by mass, preferably 0.6 to 5% by mass, and more preferably 0.7 to 2% by mass of the reducing element.
[0068] The reducing element may be present in the first particles or may be added in the form of particles to the mixture provided in step a).
[0069] The powder mixture provided in step a) is produced prior to the additive manufacturing process.
[0070] In a preferred embodiment of the invention, the first and second powders are mixed using a 3D dynamic mixer, such as a Turbula™ mixer. Alternatively, it may be by mechanosynthesis.
[0071] In step c) at least the first particles 10 are melted using a beam of sufficient energy.
[0072] The deposited layer may be locally melted or may be completely melted.
[0073] The melting step creates a molten pattern in the powder mixture layer. One or more areas of molten particles can be created to form the desired pattern. The particles 10 that form the pattern melt completely during solidification (step d) to connect to one or more areas that solidify in the aluminum alloy.
[0074] Advantageously, steps b), c) and d) can be repeated at least once to form at least one further solidified region on the first solidified region, the method being repeated until the final shape of the part is obtained.
[0075] The unsolidified powder is then removed and the final part is peeled from the substrate.
[0076] A part obtained according to one of these methods can be subjected to an annealing step (heat treatment) in order to reduce internal stresses and improve the mechanical properties.
[0077] According to a first variant embodiment, it is a laser melting on powder bed (SLM) process. In an exemplary and non-limiting manner, the parameters of the laser melting on powder bed building method are as follows: - Laser power is 50-500W; - Laser speed is 100~2000mm / s; - the distance between the two vector spaces ("hatch") is 25-120 μm; - Layer thickness: 15-60 μm.
[0078] According to another variant embodiment, it is a powder bed electron beam melting (EBM) method. In an exemplary and non-limiting aspect, the parameters of the manufacturing method by electron beam melting on a powder bed are as follows: - Electron beam 50-3000W; - Beam speed is 100-8000mm / s; - the distance between the two vector spaces is 50-150 μm; - Layer thickness: 40-60 μm.
[0079] A deposition apparatus used in additive manufacturing may, for example, comprise a powder feeder, a device for spreading and homogenizing the surface of the powder (a "roller" or "blade"), a beam (e.g., infrared laser light with a wavelength of about 1060 nm), a scanner for managing the beam, and a substrate (also called a plate) that can be lowered vertically (along an axis Z perpendicular to the powder bed).
[0080] The assembly can be housed in a thermally sealed, inert enclosure to control the atmosphere as well as to avoid powder scattering.
[0081] Although not exclusively, the invention finds particular application in the energy sector, in particular in heat exchangers, the aeronautical sector and the automotive sector. EXAMPLES
[0082] Illustrative and Non-Limiting Examples of Embodiments In this example, a cubic part with dimensions 10 mm x 10 mm x 10 mm is produced by SLM printing.
[0083] The part is obtained from a mixture of two powders: an aluminum alloy powder and a YSZ powder.
[0084] The particle size distribution of aluminum alloy powder (Al6061) is as follows: 10 = 27.5 μm, d 50 = 41.5 μm, d 90 =62.7μm.
[0085] As for the YSZ powder, its particle size distribution is as follows: diameter 120nm~600nm. This powder is sold by Innovnano Materials under the reference name "2YSZ". 2 O 3 Contains 3.5% by mass.
[0086] The aluminum powder is calcined at 180° C. for 2 hours. The mixing of the two powders is then carried out in a glove box (1200 mL of aluminum alloy powder to be densified; 24 mL of yttria stabilized zirconia powder (2% by volume of the mixture); and 250 mL of zirconia beads with a diameter of 3 mm used to homogenize the mixture). The volume of the mixing pot is 6.5 L.
[0087] The filling rate, defined as the ratio of the volume of particles 10, particles 20 and zirconia beads to the capacity of the mixing pot, is about 23%.
[0088] The mixture is placed in a 3D dynamic mixer, such as a Turbula™, for 6 hours.
[0089] Finally, the mixture is coarsely sieved (1 mm) to recover the zirconia beads.
[0090] Various powder mixtures were tested: the volume fraction of YSZ powder ranged from 0.05 to 2 vol%. The powder mixtures were observed using SEM (Figures 3A-3D). The aluminum alloy 6061 particles appear gray and the YSZ particles appear white.
[0091] This mixture is then used to 3D print the part. As an example, the SLM conditions that result in the densest cubes are as follows: laser power: 190-270 W; laser speed: 400-800 mm / s; vector space: 100 μm; layer thickness (powder bed): 20 μm.
[0092] For comparison, aluminum parts are produced without the addition of YSZ powder.
[0093] Parts made using only aluminum powder (Figure 4A) or powder mixes containing 0.05-1 vol% YSZ (Figures 4B-4D) exhibit cracks, whereas parts made using powder mixes containing 2 vol% YSZ powder are dense and crack-free (Figure 4E).
[0094] Parts fabricated without the addition of YSZ powder and with 2 vol.% YSZ have been characterized by electron backscatter diffraction (Figures 5A and 5B, respectively): the addition of 2 vol.% YSZ leads to a refinement of the microstructure.
[0095] The aluminum parts manufactured with 2 vol.% YSZ were also characterized by SEM. The grain densification is perfectly evident in the plane XZ (FIG. 6A) as well as in the plane XY (FIG. 6B). The axis Z corresponds to the build axis, i.e. the axis of stacking of the layers of the powder mixture (or the axis perpendicular to the build plate); the axes X and Y correspond to the axes of the build plate, i.e. the axes X and Y are parallel to the main faces of the build plate on which the layers of the powder mixture were deposited.
[0096] Finally, the specific surface area was measured by BET for various powder mixtures (Figure 7). To overcome the hot cracking problem, a specific surface area of at least 0.3 m 2 It has been found that a specific surface area in g / g is necessary. These measurements can form another source of characterization in terms of the amount of grain growth material to be added to avoid cracking phenomena.
[0097] Characterization by transmission electron microscopy confirmed the presence of magnesium-containing oxides (Figures 8A-8D).
[0098] References [1]Shen “Carbothermal synthesis of metal-functionalized nanostructures for energy and environmental applications”, J.Mater.Chem.A3(2015), 13114-13188. [2]Chu and al. “Sintering of aluminum nitride by using alumina crucible and MoSi 2 heating element at temperatures of 1650℃ and 1700℃”, Ceramics International 35(2009), 3455-3461.
Claims
1. 1. A method for producing an aluminum alloy part by selective laser melting or selective electron beam melting, comprising the steps of locally melting and then solidifying a layer of a powder mixture, The powder mixture comprises: - first particles (10) containing at least 80% by weight of aluminium and up to 20% by weight of one or more additional elements; and - second particles (20) made of yttria stabilized zirconia; The method of making the powder mixture comprises at least 1.5 volume percent of second particles.
2. The method of claim 1, wherein the second particles (20) have a maximum dimension in the range of 5 nm to 600 nm.
3. The method according to claim 1 or 2, wherein the volume fraction of the second particles (20) in the powder mixture is in the range of 1.5% to 2.5%.
4. A method according to any one of the preceding claims, wherein the first particles (10) have a maximum dimension in the range of 10 μm to 100 μm.
5. 5. The method according to any one of claims 1 to 4, wherein the additional elements are selected from Cu, Si, Zn, Mg, Fe, Ti, Mn, Zr, Va, Ni, Pb, Bi and Cr.
6. The method according to any one of claims 1 to 5, wherein the aluminium alloy is a 7075 alloy, a 2024 alloy, a 2219 alloy or a 6061 alloy.
7. The method according to any one of claims 1 to 6, comprising a step in which the powder mixture is obtained in a 3D dynamic mixer.
8. The specific surface area of the powder mixture after mixing using a 3D dynamic mixer is 0.3 m 2 The method according to any one of claims 1 to 7, wherein the molecular weight is greater than 1 / g.
9. The method according to any one of claims 1 to 8, wherein the powder mixture further comprises a reducing element.
10. 10. The method of claim 9, wherein the reducing element is magnesium.
11. 11. The method according to claim 9 or 10, wherein the powder mixture comprises at least 0.5% by weight of a reducing element.
12. A method according to any one of claims 9 to 11, wherein the reducing element is present in the first particles.
Citation Information
Patent Citations
Ceramic articles and methods for adding treatments to ceramic articles
JP2015517450A
Molding material to be used for powder laminate molding
JP2017113952A
Additive manufacturing of metal alloys and metal alloy matrix composites
US20180161874A1
Aluminum alloys with grain refiners, and methods for making and using the same
WO2018144323A1