Method for regenerating bed material used in a fluidized bed combustion furnace

By polishing fluidized media with aids like water, acid, or abrasive, and separating deposits, the method enhances regeneration efficiency and reduces waste in fluidized bed combustion furnaces.

JP7591368B2Active Publication Date: 2024-11-28ASAHI YUKIZAI KOGYO CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020139647
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-08-20
Publication Date
2024-11-28
Estimated Expiration
2040-08-20

AI Technical Summary

Technical Problem

Existing methods struggle to efficiently remove low melting point compounds adhering to fluidized media in fluidized bed combustion furnaces, making it difficult to regenerate and reuse the media.

Method used

A method involving polishing of the used fluidized medium with the addition of polishing aids such as water, acid, surfactant, or abrasive, followed by a separation and removal step to enhance the detachment and removal of deposits.

Benefits of technology

The method significantly improves polishing efficiency, allowing for effective removal of adhering deposits and regeneration of the fluidized medium, reducing waste and maintaining furnace efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591368000001
    Figure 0007591368000001
  • Figure 0007591368000002
    Figure 0007591368000002
Patent Text Reader

Abstract

To improve polishing efficiency of a polishing treatment step for polishing a used bed material to separate deposits that adheres to the surface of the bed material during use, in a regeneration method of the bed material used in a fluidized bed combustion furnace for biomass power generation.SOLUTION: In a polishing treatment step, a polishing aid substance containing at least one selected from a group consisting of water, acid, surfactant, and abrasive is added.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for regenerating a fluidized bed medium used in a fluidized bed combustion furnace. [Background technology]

[0002] There is a demand for the operation of fluidized bed combustion furnaces using biomass fuel. A sand-like fluidized medium is fluidized inside the combustion furnace to improve combustion efficiency (heat retention effect). However, as combustion continues, the biomass fuel contains a lot of alkaline components (ash), and these alkaline components produce compounds with low melting points. These low melting point compounds can adhere to the fluidized medium and cause poor fluidity, so the fluidized medium must be replaced periodically. Conventionally, used bedrock removed from a combustion furnace during replacement has been discarded, but if it were possible to remove the adhering matter from the used bedrock to which ash has adhered and regenerate the bedrock, it would be possible to reuse the bedrock. For example, Patent Document 1 discloses a technique for regenerating a used fluid medium by removing deposits from the fluid medium through physical polishing. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 8-278018 Summary of the Invention [Problem to be solved by the invention]

[0004] However, it was found that if low-melting point compounds are firmly attached to the used fluid medium, they are difficult to remove by physical polishing alone. An object of the present invention is to improve the efficiency of removing ash (alkaline components) adhering to a used fluidized medium by a polishing treatment. [Means for solving the problem]

[0005] The present inventors have found that the polishing efficiency can be improved by adding a polishing aid (water, acid, surfactant or abrasive) during the polishing treatment step of the used fluid medium, and have completed the present invention.

[0006] The present invention relates to a method for regenerating a fluidized bed used in a fluidized bed combustion furnace, the method comprising: a polishing process step of polishing the used fluidized bed to remove any deposits that have adhered to the surface of the fluidized bed during use; and a flaking matter separation and removal process step of separating and removing the flaking matter that has been removed in the polishing process, the method being characterized in that a polishing auxiliary agent containing at least one selected from the group consisting of water, acid, surfactants and abrasives is added in the polishing process.

[0007] The present invention includes the following embodiments. [1] A method for regenerating a fluidized bed used in a fluidized bed combustion furnace, the method comprising: a polishing process for polishing the used fluidized bed to remove any deposits that have adhered to the surface of the fluidized bed during use; and a peeled matter separation and removal process for separating and removing the peeled matter that has been removed in the polishing process, the method being characterized in that a polishing auxiliary agent containing at least one selected from the group consisting of water, acid, surfactants and abrasives is added in the polishing process. [2] The method according to [1], wherein the fluidized medium is spherical refractory particles. [3] The method according to [1] or [2], wherein the polishing process is a dry polishing process in which the fluid media used are brought into contact or collided with each other. [4] The method according to any one of [1] to [3], wherein the peeled material separating and removing step is a step of feeding air into the fluidized medium after the polishing treatment step to cause it to flow, and collecting the peeled material discharged along with the exhaust air. Effect of the Invention

[0008] The method for regenerating a fluid medium of the present invention has high polishing efficiency in the polishing treatment for removing deposits that have adhered to the surface of the fluid medium due to use. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The present invention relates to a method for regenerating a bed material used in a fluidized bed combustion furnace. In particular, the present invention relates to a method for regenerating a bed material used in a fluidized bed combustion furnace mainly used for biomass power generation. Biomass power generation is a system that uses biomass fuel such as construction waste, green wood, wood chips, PKS (coconut shells), EFB (empty fruit bunches), and wood pellets as fuel, burns the biomass fuel, and generates electricity, for example, with a steam turbine, using the generated heat. A fluidized bed combustion furnace for biomass power generation is a fluidized bed or circulating fluidized bed combustion furnace used to burn biomass fuel in biomass power generation. A fluidized bed combustion furnace is filled with a sand-like bed material, and air is pumped in from the bottom of the fluidized bed combustion furnace and ejected upward, so that the force of the air acting on the bed material and gravity are balanced, and the bed material is suspended and suspended in the air, resulting in a fluidized state in which the bed material behaves as if it were a fluid.

[0010] As the bed material, natural sand or artificial sand is used. Natural sand includes naturally occurring silica sand, such as river sand, sea sand, and mountain sand. Artificial sand includes artificially produced refractory particles. Among them, the preferred bed material is artificially produced spherical refractory particles, and more preferably artificially produced spherical aluminosilicate particles with a smooth surface. By using spherical refractory particles with a smooth surface, the smoothness makes it easier to remove adhesions, improving the polishing efficiency and improving the heat retention effect of the fluidized bed combustion furnace. The average particle size of the fluidized medium is not limited as long as a fluidized state can be achieved in the fluidized bed combustion furnace, but is preferably 50 to 2000 μm, more preferably 100 to 1500 μm, and further preferably 150 to 1000 μm, where the average particle size of the fluidized medium is the average particle size measured by a laser diffraction / scattering method.

[0011] The method for regenerating a fluid medium of the present invention includes a polishing step and a peeled material separating and removing step.

[0012] The polishing treatment process is a process in which a fluidized bed material used in a fluidized bed combustion furnace (hereinafter also simply referred to as "used fluidized bed material") is polished to remove any deposits that have adhered to the surface of the fluidized bed material during use. Ash generated by the combustion of biomass adheres to the bed material while it is being used in a fluidized bed combustion furnace for biomass power generation. The ash includes, for example, alkali metal oxides such as sodium oxide and potassium oxide, alkaline earth metal oxides such as calcium oxide and magnesium oxide, other metal oxides, and other inorganic substances. The polishing process is a process in which the ash adhered to the surface of the bed material (hereinafter simply referred to as "adherent material") is removed from the surface of the bed material by polishing.

[0013] The polishing method is not limited as long as it can remove the deposits from the surface of the fluid medium, and any polishing machine may be used. Wet polishing methods include, for example, rotary type (a method in which a fluid medium immersed in water is agitated by a rotating blade to remove deposits), water jet type (a method in which a fluid medium is impacted by a jet of water to remove deposits), ultrasonic vibration type (a method in which a fluid medium immersed in water is subjected to ultrasonic vibration to remove deposits), and other devices. Dry polishing methods include, for example, jet type (a method in which a fluid medium is blown away by high-speed air to remove deposits by applying impact and friction), vertical axis rotation type and horizontal axis rotation type (a method in which a fluid medium is splashed or agitated by a rotating body or blade, or further, a method in which a rotor is applied to apply impact and friction between the fluid medium to remove deposits), and vibration type (a method in which a fluid medium is agitated by vibration force to remove deposits mainly by friction), and these methods are appropriately adopted. The polishing process may be a batch type or a continuous type. Furthermore, the polishing conditions such as the polishing time in this polishing process are appropriately selected depending on the state of adhesion of the deposits on the surface of the recovered fluid medium. Among these, the polishing process is preferably a dry polishing process in which used fluidized media are brought into contact or collided with each other, and more preferably, from the viewpoint of easily fluidizing the used fluidized media, a polishing process using a vertical axis rotation type, horizontal axis rotation type, or vibration type device, and among these, a polishing process using a vertical axis rotation type device is preferred.

[0014] The present invention is characterized in that a polishing aid is added in the polishing process. The polishing aid contains at least one selected from the group consisting of water, an acid, a surfactant, and an abrasive. Ash adhering to used fluidized media usually contains alkali such as sodium oxide or potassium oxide, but adding water or acid dissolves some of the alkali, creating voids in the adhering material, making it easier to remove the adhering material. In addition, fluidized media may bond to each other during use due to sintering or through ash adhering to the surface, forming coarse particles, but adding water or acid makes it easier to break up the bonded fluidized media. In addition, adding a surfactant or water to used fluidized media can remove static electricity and prevent fine powder from re-adhering to the fluidized media, improving the polishing efficiency. In addition, adding an abrasive can increase frictional resistance, improving the polishing efficiency in the polishing process.

[0015] The type of acid used as the polishing aid is not limited as long as it improves the polishing efficiency. Both inorganic and organic acids can be used. Examples of inorganic acids include sulfuric acid, phosphoric acid, hydrochloric acid, and their ammonium salts, or acid salts such as sodium hydrogen sulfate, sodium hydrogen phosphate, and potassium hydrogen phosphate. Among these inorganic acids, phosphoric acid is preferred because it has little effect on the fluid medium, such as corrosion. These inorganic acids may be used alone or in combination of two or more. Examples of organic acids include sulfonic acids and acids having a carboxyl group. Examples of sulfonic acids include xylenesulfonic acid, paratoluenesulfonic acid, benzenesulfonic acid, methanesulfonic acid, and ammonium salts thereof. Examples of acids having a carboxyl group include formic acid, acetic acid, oxalic acid, lactic acid, maleic acid, malic acid, citric acid, stearic acid, lauric acid, palmitic acid, linoleic acid, oleic acid, and ammonium salts thereof. Among these organic acids, xylenesulfonic acid, paratoluenesulfonic acid, benzenesulfonic acid, methanesulfonic acid, formic acid, acetic acid, oxalic acid, lactic acid, maleic acid, malic acid, and citric acid are preferred. These organic acids may be used alone or in combination of two or more. These organic acids may also be used in combination with the inorganic acids described above. The acid may be either liquid or solid at room temperature, but an acid that is liquid at the temperature during use is more preferable because it will more easily penetrate into the deposits to be removed.

[0016] Examples of the polishing aid containing acid include the acid itself and an acid solution. The solvent of the acid solution may be water or an organic solvent. A specific example of an acid dissolved in an organic solvent is an ethanol solution of citric acid. When an acid solution is used as a polishing aid, the concentration and amount of the acid solution are not limited as long as the polishing efficiency is improved. However, since there is a risk of the fluid medium becoming wet due to corrosion of the device or an increase in the amount of water, which may result in a decrease in the polishing efficiency, it is better to titrate the fluid medium with an acid solution of a predetermined concentration in advance and measure the amount of neutralization to determine the optimal concentration and amount of addition. The measurement method is to put 50g of sample into 100mL of distilled water and stir for 1 hour, then add a stir bar and indicator (methyl red) and stir, then titrate with 0.1N-HCL until neutralized, and calculate the amount of alkali dissolved in distilled water per 1g of sample. This determines the concentration and amount of acid to be used. Among them, the concentration of the acid solution is not limited as long as the polishing efficiency is improved, but is preferably 0.5 to 20 mass %, more preferably 1 to 10 mass %, and further preferably 2 to 8 mass %. The amount of acid solution added is not limited as long as the polishing efficiency is improved, but is preferably 0.1 to 20 parts by mass, more preferably 0.5 to 15 parts by mass, and even more preferably 1 to 10 parts by mass, per 100 parts by mass of used fluid medium.

[0017] The type of surfactant used as the polishing aid is not limited as long as it improves the polishing efficiency. Any of cationic surfactants, anionic surfactants, amphoteric surfactants, nonionic surfactants, silicone surfactants and fluorine surfactants can be used.

[0018] Specific examples of cationic surfactants include aliphatic amine salts, aliphatic quaternary ammonium salts, benzalkonium salts, benzethonium chloride, pyridinium salts, and imidazolinium salts. Examples of anionic surfactants include fatty acid soaps, N-acyl-N-methylglycine salts, N-acyl-N-methyl-β-alanine salts, N-acylglutamates, alkyl ether carboxylates, acylated peptides, alkyl sulfonates, alkylbenzene sulfonates, alkylnaphthalene sulfonates, dialkyl sulfosuccinates, alkyl sulfoacetates, α-olefin sulfonates, N-acylmethyltaurines, sulfated oils, higher alcohol sulfates, secondary higher alcohol sulfates, alkyl ether sulfates, secondary higher alcohol ethoxy sulfates, polyoxyethylene alkylphenyl ether sulfates, monoglycerates, fatty acid alkylolamide sulfates, alkyl ether phosphates, and alkyl phosphates. Furthermore, examples of amphoteric surfactants include carboxybetaine type, sulfobetaine type, aminocarboxylate, imidazolinium betaine, and the like. In addition, nonionic surfactants include polyoxyethylene alkyl ethers, polyoxyethylene secondary alcohol ethers, polyoxyethylene alkylphenyl ethers (e.g., Emulgen (registered trademark) 911), polyoxyethylene sterol ethers, polyoxyethylene lanolin derivatives, polyoxyethylene polyoxypropylene alkyl ethers (e.g., Nupol (registered trademark) PE-62), polyoxyethylene glycerin fatty acid esters, polyoxyethylene castor oil, hydrogenated castor oil, polyoxyethylene sorbitan fatty acid esters, polyoxyethylene sorbitol fatty acid esters, polyethylene glycol fatty acid esters, fatty acid monoglycerides, polyglycerin fatty acid esters, sorbitan fatty acid esters, propylene glycol fatty acid esters, sucrose fatty acid esters, fatty acid alkanolamides, polyoxyethylene fatty acid amides, polyoxyethylene alkylamines, alkylamine oxides, acetylene glycol, acetylene alcohols, and the like.

[0019] Among various surfactants, those having a siloxane structure as a non-polar site are called silicone surfactants, and those having a perfluoroalkyl group are called fluorine surfactants. Examples of silicone surfactants include polyester-modified silicone, acrylic-terminated polyester-modified silicone, polyether-modified silicone, acrylic-terminated polyether-modified silicone, polyglycerin-modified silicone, and aminopropyl-modified silicone. Examples of the fluorine-based surfactant include perfluoroalkyl sulfonates, perfluoroalkyl carboxylates, perfluoroalkyl phosphates, perfluoroalkyl trimethylammonium salts, perfluoroalkyl ethylene oxide adducts, and perfluoroalkyl group-containing oligomers.

[0020] In the present invention, the various surfactants as described above can be used alone or in combination of two or more kinds. The surfactant may be either liquid or solid at room temperature, but it is more preferable that the surfactant be liquid at the temperature during use, since this makes it easier to disperse uniformly.

[0021] Examples of the polishing aid containing a surfactant include the surfactant itself and a surfactant solution. The solvent of the surfactant solution may be water or an organic solvent. When using a surfactant solution as a polishing aid, the concentration of the surfactant solution is not limited as long as the polishing efficiency is improved, but is preferably 0.001 to 15 mass%, more preferably 0.01 to 10 mass%, and even more preferably 0.1 to 5 mass%. The amount of surfactant solution added is not limited as long as the polishing efficiency is improved, but is preferably 0.1 to 20 parts by mass, more preferably 0.5 to 15 parts by mass, and even more preferably 1 to 10 parts by mass, relative to 100 parts by mass of used fluid medium.

[0022] When the polishing aid consists of only water (water that does not contain any acid, surfactant, or abrasive, i.e., pure water), the amount of water added is not limited as long as the polishing efficiency is improved, but is preferably 0.1 to 20 parts by mass, more preferably 0.5 to 15 parts by mass, and even more preferably 1 to 10 parts by mass relative to 100 parts by mass of used fluid medium.

[0023] The polishing aid preferably contains a volatile organic solvent. Among them, alcohol is more preferable from the viewpoint of safety, etc. By containing alcohol in the polishing aid, it is possible to easily dry the fluid medium after adding the polishing aid. Examples of the alcohol include methanol, ethanol, propanol, etc. When the polishing aid contains an alcohol, the concentration of the alcohol in the polishing aid is preferably 1 to 90 mass%, more preferably 3 to 70 mass%, and further preferably 5 to 50 mass%.

[0024] The type of abrasive used as a polishing aid is not limited as long as the polishing efficiency is improved, but examples of the abrasive include silica sand, zircon sand, chromite sand, olivine sand, and metal particles mainly composed of iron.

[0025] The average particle size of the abrasive is preferably 5 to 100 μm, more preferably 7 to 70 μm, and further preferably 10 to 50 μm. However, the average particle size of the abrasive is the average particle size measured by a laser diffraction / scattering method. If the average particle size is too small, the frictional resistance of the fluid medium does not increase during polishing unless a large amount of the abrasive is added, which is inefficient and uneconomical. On the other hand, if the average particle size is too large, the particle size of the fluid medium and the particle size of the abrasive are close to each other, so that the abrasive does not easily penetrate into the gaps between the fluid media, and as a result, the effect of increasing the frictional resistance is reduced.

[0026] The amount of the abrasive added is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 8 parts by mass, and even more preferably 1 to 5 parts by mass, relative to 100 parts by mass of the used fluid medium. If the amount added is too small, the effect of adding the abrasive cannot be obtained, and if the amount added is too large, further increase in the amount added does not increase the effect, which is uneconomical.

[0027] The abrasive is added to increase the frictional resistance, and therefore preferably has a large dynamic friction coefficient or a polygonal shape. When an abrasive is used, the abrasive is separated from the fluid medium after the polishing process. The separation can be performed by classification, but the method of separation is not limited.

[0028] The polishing aid contains at least one selected from the group consisting of water, acid, surfactant, and abrasive. The polishing aid may contain only one selected from the group consisting of water, acid, surfactant, and abrasive, may contain any two selected from the group consisting of water, acid, surfactant, and abrasive, may contain any three selected from the group consisting of water, acid, surfactant, and abrasive, or may contain all four selected from the group consisting of water, acid, surfactant, and abrasive.

[0029] The method of adding the polishing aid to the polishing process is not particularly limited, but can be, for example, spraying, dripping, gravity drop, screw feeder, air transport, immersion, etc., and preferably, when the polishing aid is a liquid, it is added by spraying or dripping, and when the polishing aid is a solid, it is added by gravity drop, screw feeder or air transport.

[0030] The timing of adding the grinding aid is not particularly limited as long as it is during the grinding process. The grinding process may be started by putting the used fluid medium and the grinding aid into the grinder, the grinding aid may be added immediately after the start of the grinding process, the grinding aid may be added during the grinding process, or the grinding aid may be added in two or more portions during the grinding process. The polishing process may be carried out by first polishing for a certain time without adding a polishing aid, and then polishing for an additional time with the addition of a polishing aid. That is, the polishing process may be carried out in a stepwise manner consisting of polishing without adding a polishing aid (rough polishing) and polishing with adding a polishing aid (main polishing).

[0031] The method of the present invention includes a peeling separation and removal step after the polishing process. The peeling separation and removal step is a step of separating and removing the peelings peeled off in the polishing process. By removing the peelings after the polishing process, the attached ash and fine powder are removed, and only the regenerated fluidized medium is taken out so that it can be used again as a fluidized medium. The method of separating and removing the peelings is not limited as long as it can separate and remove the peelings, but for example, it can be carried out by a step of feeding air into the fluidized medium after the polishing process to make it fluid, and collecting the peelings discharged along with the exhaust air. More specifically, the fluidized medium after the polishing process is placed in a container, and air is fed from the bottom of the container and ejected upward, so that the fluidized medium is suspended in the air, i.e., in a fluidized state, and the air flowing upward between the fluidized medium is discharged from the container along with the peelings, and the peelings discharged along with the exhaust air are collected by a dust collector or the like.

[0032] By regenerating bed media that have conventionally been discarded using the method of the present invention, the bed media can be reused. In the method for regenerating a fluid medium of the present invention, a polishing auxiliary is added in the polishing treatment step, so that the polishing efficiency is high and the polishing treatment time can be shortened. According to the method for regenerating a bed material of the present invention, ash and fine powder adhering to a used bed material can be effectively removed. In the regeneration method of the fluid medium of the present invention, the polishing auxiliary agent can be added even during the polishing process, so the polishing process time is not increased. In the regeneration method of the fluid medium of the present invention, the polishing auxiliary agent is added during the polishing process, not in the pretreatment process, so the total time of all the processes of the regeneration method is not increased. According to the method for regenerating a fluid medium of the present invention, sintering between fluid media can be reduced, and therefore the fluidity of the fluid medium can be maintained. According to the method for regenerating a bed material of the present invention, instead of disposing of both the ash and bed material as in the conventional method, only the ash is disposed of, which leads to a significant reduction in the amount of industrial waste.

[0033] It should be understood that the method for regenerating a fluid medium according to the present invention should not be interpreted in any way as being limited by the specific description of the above exemplary embodiments, and that the present invention can be embodied in various forms with various changes, modifications, improvements, etc. based on the knowledge of those skilled in the art, and that all such embodiments fall within the scope of the present invention as long as they do not deviate from the spirit of the present invention. EXAMPLES

[0034] The present invention will be explained in more detail below using several test examples, but it should be understood that the present invention is not to be interpreted in any limited manner by the description of such test examples. In the following test examples, "%" and "parts" are all expressed by mass unless otherwise specified.

[0035] [raw materials] The raw materials used in the following examples and comparative examples are as follows. (fluid medium) Silica sand: Flattery sand manufactured by Mitsubishi Corporation Building Materials Co., Ltd. (average particle size: 249.8 μm) Spherical particles (spherical refractory particles): Lunamos (registered trademark) manufactured by Kao Quaker Co., Ltd. (average particle size: 205.3 μm) (Polishing aid) 3% sulfuric acid: Sulfuric acid diluted with distilled water to a concentration of 3% by mass 5% phosphoric acid: Phosphoric acid diluted with distilled water to a concentration of 5% by mass 5% citric acid: Citric acid dissolved in distilled water to a concentration of 5% by mass. 5% citric acid ethanol solution: Citric acid dissolved in a 1:1 mixture of distilled water and ethanol to a concentration of 5% by mass. 5% paratoluenesulfonic acid: Paratoluenesulfonic acid dissolved in distilled water to a concentration of 5% by mass. 1% surfactant aqueous solution: Takemoto Yushi Co., Ltd.'s Paionin A-40 dissolved in distilled water to a concentration of 1% by mass. Abrasive: Alumina abrasive (average particle size: 30 μm)

[0036] [Example 1] Silica sand was used as a bed material, and the bed material was prepared from a used bed material in a fluidized bed combustion furnace for biomass power generation. 500 parts by mass of the used bed material and 3 parts by mass of 3% sulfuric acid as a polishing aid were placed in a cylindrical container together with ceramic balls, and the container was placed on a pot mill rotating table manufactured by Nitto Kagaku Co., Ltd. and treated at a rotation speed of 58 rpm for 30 minutes (polishing treatment step). The bed material after the polishing process was placed in a cylindrical tube with a dust collector attached to the top and a 280 mesh screen attached to the bottom, and the peeling removal process was carried out. The peeling removal process was carried out by feeding air from the bottom at a flow rate of 30 L / min to make the bed material flow, discharging the peeling material contained in the used bed material with the air, and guiding the discharged air containing the peeling material to the dust collector to collect the peeling material. The peeling removal process was carried out for 30 minutes. The adhesion removal rate (mass%) was calculated from the mass W0 of the bed material before the polishing treatment and the mass W1 of the bed material after the peeled material was separated and removed, using the following formula. The results are shown in Table 1. Deposit removal rate=(W0-W1) / W0×100

[0037] [Example 2] The same procedure as in Example 1 was carried out except that 5% phosphoric acid was used instead of 3% sulfuric acid in Example 1, and the rate of deposit removal was calculated. The results are shown in Table 1.

[0038] [Example 3] The same procedure as in Example 1 was carried out except that 5% citric acid was used instead of 3% sulfuric acid in Example 1, and the rate of deposit removal was calculated. The results are shown in Table 1.

[0039] [Example 4] The same procedure as in Example 1 was carried out except that a 5% ethanol solution of citric acid was used instead of the 3% sulfuric acid in Example 1, and the rate of deposit removal was calculated. The results are shown in Table 1.

[0040] [Example 5] The same procedure as in Example 1 was carried out except that 5% paratoluenesulfonic acid was used instead of 3% sulfuric acid in Example 1, and the rate of deposit removal was calculated. The results are shown in Table 1.

[0041] [Example 6] The same procedure as in Example 1 was carried out except that water (distilled water) was used instead of the 3% sulfuric acid in Example 1, and the rate of deposit removal was calculated. The results are shown in Table 1.

[0042] [Example 7] The same procedure as in Example 1 was carried out except that a 1% aqueous surfactant solution was used instead of the 3% sulfuric acid in Example 1, and the rate of deposit removal was calculated. The results are shown in Table 1.

[0043] [Example 8] The same procedure as in Example 1 was carried out, except that 10 parts by mass of abrasive was used instead of 3 parts by mass of 3% sulfuric acid in Example 1, and the adhesion removal rate was calculated. The results are shown in Table 2. Note that the abrasive is separated and removed in the peeled material separating and removing step, and is included in the peeled material collected by the dust collector, but the numerical value of the adhesion removal rate in Table 2 is a numerical value after subtracting the amount of the abrasive.

[0044] [Example 9] The same procedure as in Example 1 was carried out except that the amount of 3% sulfuric acid was changed from 3 parts by mass to 7 parts by mass in Example 1, and the rate of deposit removal was calculated. The results are shown in Table 2.

[0045] [Example 10] The same procedure as in Example 1 was carried out, except that 3 parts by mass of 3% sulfuric acid and 10 parts by mass of abrasive were used as the polishing aid, and the adhesion removal rate was calculated. The results are shown in Table 2. Note that the abrasive is separated and removed in the peeled material separating and removing step, and is included in the peeled material collected by the dust collector, but the numerical value of the adhesion removal rate in Table 2 is a numerical value after subtracting the amount of the abrasive.

[0046] [Example 11] The same procedure was carried out as in Example 1, except that 3 parts by mass of 3% sulfuric acid and 3 parts by mass of a 1% aqueous surfactant solution were used as the polishing aids, and the rate of deposit removal was calculated. The results are shown in Table 2.

[0047] [Example 12] The same procedure as in Example 1 was carried out except that spherical particles were used as the fluidized medium instead of the silica sand, and the rate of deposit removal was calculated. The results are shown in Table 2.

[0048] [Comparative Example 1] The same procedure as in Example 1 was carried out except that no polishing aid was used, and the rate of deposit removal was calculated. The results are shown in Table 2.

[0049] [Sintering experiment] The recycled fluid media obtained in the examples and comparative examples were placed in a magnetic crucible and then treated at 800°C for 12 hours to observe whether the fluid media were bonded together by sintering. The results are shown in Tables 1, 2, and 3. In the tables, "Yes" indicates a case where sintering (bonding) was observed, and "No" indicates a case where sintering (bonding) was not observed. It is preferable not to sinter.

[0050] [Table 1]

[0051] [Table 2] [Industrial Applicability]

[0052] The method of the present invention can be suitably used for regenerating a fluidized bed medium used in a fluidized bed combustion furnace for biomass power generation.

Claims

1. A method for regenerating a fluidized medium used in a fluidized bed combustion furnace, the method comprising: a polishing process step of polishing the used fluidized medium to remove any deposits that have adhered to the surface of the fluidized medium during use; and a flaking material separating and removing process step of separating and removing the flaking material that has been flaked in the polishing process; the method being characterized in that after the start of the polishing process, a polishing auxiliary agent containing at least one type selected from the group consisting of an acid and an abrasive is added, the abrasive being at least one type selected from the group consisting of silica sand, zircon sand, chromite sand, olivine sand, and metal grains mainly composed of iron, and the average particle size of the abrasive being 5 to 100 μm.

2. The method of claim 1 , wherein the fluidizing medium is spherical refractory particles.

3. 3. The method according to claim 1, wherein the polishing step is a polishing step in which the fluid media used are brought into contact or collided with each other.

4. The method according to any one of claims 1 to 3, wherein the peeled material separating and removing step is a step of feeding air into the fluidized medium after the polishing step to cause it to flow, and collecting the peeled material discharged along with the exhaust air.

Citation Information

Patent Citations

  • Fluid medium regenerator

    JP1981117016A

  • Regenerative method and device for fluidized medium

    JP1981160513A

  • Fluidized medium dry regenerating device

    JP1996278018A

  • Surface treatment method

    JP2012152872A

  • Casting sand regeneration process, and polishing device

    JP2016147287A