White photosensitive resin composition, color filter and image display device produced using the same
The white photosensitive resin composition addresses efficiency and cost issues in color filters by using scattering particles and specific alkali-soluble resins to enhance blue pixel performance and reduce manufacturing costs, improving image quality and durability.
Patent Information
- Application Number
- JP2020202048
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-05
- Filing Date
- 2020-12-04
- Publication Date
- 2024-11-28
- Estimated Expiration
- 2040-12-04
Smart Images

Figure 0007591391000010 
Figure 0007591391000011 
Figure 0007591391000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a white photosensitive resin composition, a color filter produced using the same, and an image display device. [Background technology]
[0002] A color filter is a thin-film optical component that can extract the three colors red, green, and blue from white light and make them into minute pixel units, with each pixel measuring tens to hundreds of micrometers. Such color filters have a structure in which a black matrix layer formed in a predetermined pattern on a transparent substrate is stacked in order to block light from the boundary between each pixel, and pixel parts in which the three primary colors (usually red (R), green (G), and blue (B)) are arranged in a predetermined order to form each pixel.
[0003] Recently, one method for realizing color filters is the pigment dispersion method using a pigment-dispersed photosensitive resin. However, as the light emitted from the light source passes through the color filter, part of the light is absorbed by the color filter, reducing the light efficiency. In addition, problems have arisen in that color reproduction is reduced due to the characteristics of the pigments contained in the color filter.
[0004] In particular, as color filters are used in various fields including various image display devices, there is a demand for not only excellent pattern characteristics but also performance such as high brightness and high contrast ratio along with high color reproduction rate. In order to solve such problems, a method for producing a color filter using a spontaneous light-emitting photosensitive resin composition containing quantum dots has been proposed.
[0005] For example, Korean Patent Registration No. 10-1906279 discloses a photosensitive resin composition containing quantum dots, a binder resin, a photopolymerizable monomer, a photopolymerization initiator, a diffusing agent, a polymerization inhibitor, a thiol-based additive, and a solvent, as well as a technology relating to a color filter using the same.
[0006] However, in the case of a color filter including quantum dots as described in the above patent document, the performance of the color conversion panel may be somewhat degraded as the efficiency of the quantum dots, particularly the efficiency of the blue quantum dots, decreases, and in the case of blue quantum dots, they are expensive, which increases the overall manufacturing cost.
[0007] In the case of a display including a color conversion panel using a blue light source, green and red pixels use green and red quantum dots to display colors, respectively. However, as mentioned above, blue is difficult to use due to performance issues with blue quantum dots, so blue light is transmitted through the blue light source to display colors. For this reason, light scattered by quantum dots is generated in green and red, and direct light is generated in blue, making it difficult to mix colors clearly when mixing colors. To solve this problem, a technology has been developed that introduces a scattering layer for scattering into blue pixels.
[0008] Therefore, there is a demand for development of a photosensitive resin composition that can prevent a decrease in efficiency of blue pixels, prevent residues, provide excellent reliability, and reduce manufacturing costs. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Korean Patent No. 10-1906279 Summary of the Invention [Problem to be solved by the invention]
[0010] An object of the present invention is to provide a white photosensitive resin composition suitable for producing a pixel layer that can provide excellent reliability without causing residue problems while preventing a decrease in efficiency of blue pixels.
[0011] Another object of the present invention is to provide a color filter including a coating film produced using the white photosensitive resin composition, and an image display device including the color filter. [Means for solving the problem]
[0012] The present invention relates to a method for producing a light-emitting device comprising the steps of: (A) scattering particles; (B) an alkali-soluble resin; (C) a polymerizable compound; (D) a photopolymerization initiator; and (E) a solvent, The (B) alkali-soluble resin includes a unit represented by the following chemical formula 1 and a unit represented by the following chemical formula (2),
[0013] [ka]
[0014] In the above formula 1, R 1 is a direct bond or a linear or branched divalent organic group having 1 to 6 carbon atoms, * is a bond.
[0015] [ka]
[0016] In the above formula 2, R 2 is a divalent organic group having 1 to 20 carbon atoms and either a direct bond or a heteroatom, * is a bond.
[0017] The present invention also provides a color filter including a coating film prepared from the white photosensitive resin composition.
[0018] The present invention also provides an image display device comprising the above color filter. Effect of the Invention
[0019] The white photosensitive resin composition according to the present invention contains a specific alkali-soluble resin, which prevents the generation of residues in non-exposed areas during the production of a coating film, provides excellent heat resistance, prevents a decrease in efficiency of blue pixels, and reduces the production cost. In addition, when the white photosensitive resin composition according to the present invention is used, the transmission intensity can be improved.
[0020] Therefore, a color filter including a coating film produced using the above-mentioned white photosensitive resin composition and an image display device including the color filter can provide excellent effects in terms of image quality, viewing angle, durability, reliability, and the like. [Brief description of the drawings]
[0021] [Figure 1] FIG. 1 is a diagram showing the criteria for evaluating residues in the experimental examples of the present invention. [Diagram 2] FIG. 2 illustrates a color filter structure according to one implementation of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] The present invention provides a white photosensitive resin composition comprising (A) scattering particles, (B) an alkali-soluble resin, (C) a polymerizable compound, (D) a photopolymerization initiator, and (E) a solvent, wherein the alkali-soluble resin (B) comprises a structural unit represented by a specific chemical formula; and a color filter and an image display device including a coating film produced using the same.
[0023] In this specification, the term "organic group" refers to a group essentially containing a carbon atom, and can be used to encompass both saturated and unsaturated groups.
[0024] Each component constituting the white photosensitive resin composition of the present invention will be described in detail below, but the present invention is not limited to these components.
[0025] <White photosensitive resin composition> The white photosensitive resin composition according to the present invention contains scattering particles, an alkali-soluble resin, a polymerizable compound, a photopolymerization initiator and a solvent, and may further contain optional additives as necessary.
[0026] (A) Scattering particles The white photosensitive resin composition according to the present invention contains scattering particles to provide the effect of light scattering.
[0027] The white photosensitive resin composition of the present invention containing the scattering particles can be suitably used for producing blue pixels using a blue light source.
[0028] In the present invention, the scattering particles include a metal oxide. The metal oxide may include one or more oxides selected from the group consisting of Li, Be, B, Na, Mg, Al, Si, K, Ca, Sc, V, Cr, Mn, Fe, Ni, Cu, Zn, Ga, Ge, Rb, Sr, Y, Mo, Cs, Ba, La, Hf, W, Tl, Pb, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Ti, Sb, Sn, Zr, Nb, Ce, Ta, In, and combinations thereof.
[0029] For example, the metal oxide is Al 2 O 3 , SiO 2 , ZnO, ZrO 2 , BaTiO 3 , TiO 2 , Ta 2 O 5 , Ti 3 O 5 , ITO, IZO, ATO, ZnO-Al, Nb 2 O 3 The material may contain one or more selected from the group consisting of SnO, SnO, MgO, and combinations thereof, and if necessary, a material that has been surface-treated with a compound having an unsaturated bond, such as an acrylate, can also be used.
[0030] The scattering particles may have a limited average particle size and a limited content in the entire composition so as to maximize the luminous intensity of the color filter.
[0031] In the present invention, the "average particle size" may be a number-average particle size, and can be determined, for example, from an image observed with a field emission scanning electron microscope (FE-SEM) or a transmission electron microscope (TEM). Specifically, it is obtained by extracting several samples from the observed image of the FE-SEM or TEM, measuring the diameters of these samples, and arithmetically averaging the measured diameters.
[0032] For example, the metal oxide contained in the scattering particles of the present invention may have an average particle size of 30 to 500 nm, preferably 30 to 300 nm. When the average particle size of the metal oxide satisfies the above range, the scattering effect is increased, and the white photosensitive resin composition containing the scattering particles can act as a blue pixel by a blue light source, which is preferable. In addition, the phenomenon of sinking in the composition can be prevented, and a surface of uniform quality can be obtained, so the average particle size can be appropriately adjusted within the above range.
[0033] The scattering particles may be contained in an amount of 0.1 to 50 parts by weight, preferably 0.5 to 30 parts by weight, and more preferably 0.5 to 20 parts by weight, based on 100 parts by weight of the total of the photosensitive resin composition. When the scattering particles are contained within the above range, there is an advantage that a scattering pixel having excellent luminous intensity can be manufactured. Specifically, when the scattering particles are contained within the above range, there is an advantage that the desired luminous intensity can be easily secured and the deterioration of the stability of the composition can be suppressed.
[0034] Meanwhile, the white photosensitive resin composition of the present invention is used for manufacturing blue pixels through which a blue light source can transmit as is, i.e., scattering pixels. The white photosensitive resin composition of the present invention preferably does not substantially contain a colorant in order to improve the transmission efficiency of blue light. However, in consideration of other properties required for the composition, it is also possible to contain a small amount of a colorant in addition to the above-mentioned scattering particles, as necessary.
[0035] When the white photosensitive resin composition of the present invention contains a small amount of a colorant, the colorant may be a blue colorant, such as, but not limited to, CI Pigment 15:6.
[0036] (B) Alkali-soluble resin The alkali-soluble resin (B) has reactivity due to the action of light or heat and alkali solubility, and can also function as a dispersion medium for solids including scattering particles, and can be used selectively to perform the function of a binder resin.
[0037] In the present invention, the alkali-soluble resin (B) contains a unit represented by the following chemical formula 1 and a unit represented by the following chemical formula (2).
[0038] [ka]
[0039] In the above formula 1, R 1 may be a direct bond or a straight or branched divalent organic group having 1 to 6 carbon atoms, and * is a bond.
[0040] R 1 Examples of the linear or branched divalent organic group having 1 to 6 carbon atoms include alkylene groups such as a methylene group, an ethylene group, a propylene group, and a butylene group.
[0041] [ka]
[0042] In the above formula 2, R 2 may be a direct bond or a straight-chain or branched-chain divalent organic group having 1 to 20 carbon atoms which may or may not contain a heteroatom, and * is a bond.
[0043] R2 Examples of the linear or branched divalent organic group containing or not containing a heteroatom having 1 to 20 carbon atoms include alkylene groups such as methylene, ethylene, propylene, and butylene groups, and aromatic hydrocarbon groups such as phenylene and biphenylene groups, in which at least one carbon atom is substituted or not substituted with a heteroatom. In this case, the alkylene group substituted with a heteroatom refers to a group having at least 2 carbon atoms.
[0044] The alkali-soluble resin (B) according to the present invention contains a structural unit represented by the chemical formula 1 and a structural unit represented by the chemical formula (2), and thus has an advantage in terms of improving residues and ensuring reliability in terms of light resistance, durability, and heat resistance.
[0045] The unit represented by Chemical Formula 1 may be derived from N-benzylmaleimide, but is not limited thereto.
[0046] The unit represented by Chemical Formula 2 may be derived from cyclohexyl(meth)acrylate, but is not limited thereto.
[0047] The alkali-soluble resin (B) of the present invention includes a structure represented by the chemical formula 1 and a structure represented by the chemical formula (2), and may further include other copolymerizable comonomers, if necessary.
[0048] Such comonomers include unsaturated carboxyl group-containing monomers and other monomers photopolymerizable therewith.
[0049] Examples of the unsaturated carboxyl group-containing monomer include unsaturated carboxylic acids having one or more carboxyl groups in the molecule, such as unsaturated monocarboxylic acids, unsaturated dicarboxylic acids, and unsaturated tricarboxylic acids.
[0050] Examples of the unsaturated monocarboxylic acid include acrylic acid, methacrylic acid, crotonic acid, α-chloroacrylic acid, and cinnamic acid. Examples of the unsaturated dicarboxylic acid include maleic acid, fumaric acid, itaconic acid, citraconic acid, and mesaconic acid.
[0051] The unsaturated polycarboxylic acid may be an acid anhydride, and specifically, examples thereof include maleic anhydride, itaconic anhydride, and citraconic anhydride. The unsaturated polycarboxylic acid may be a mono(2-methacryloyloxyalkyl)ester thereof, and examples thereof include mono(2-acryloyloxyethyl) succinate, mono(2-methacryloyloxyethyl) succinate, mono(2-acryloyloxyethyl) phthalate, and mono(2-methacryloyloxyethyl) phthalate. The unsaturated polycarboxylic acid may be a mono(meth)acrylate of a dicarboxy polymer at both ends thereof, and examples thereof include ω-carboxypolycaprolactone monoacrylate and ω-carboxypolycaprolactone monomethacrylate.
[0052] The carboxyl group-containing monomers may be used alone or in combination of two or more.
[0053] Examples of other monomers copolymerizable with the carboxyl group-containing monomer include aromatic vinyl compounds such as styrene, α-methylstyrene, o-vinyltoluene, m-vinyltoluene, p-vinyltoluene, p-chlorostyrene, o-methoxystyrene, m-methoxystyrene, p-methoxystyrene, o-vinylbenzyl methyl ether, m-vinylbenzyl methyl ether, p-vinylbenzyl methyl ether, o-vinylbenzyl glycidyl ether, m-vinylbenzyl glycidyl ether, p-vinylbenzyl glycidyl ether, and indene;Methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, n-propyl acrylate, n-propyl methacrylate, i-propyl acrylate, i-propyl methacrylate, n-butyl acrylate, n-butyl methacrylate, i-butyl acrylate, i-butyl methacrylate, sec-butyl acrylate, sec-butyl methacrylate, t-butyl acrylate, t-butyl methacrylate, 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, 2-hydroxypropyl methacrylate, 3-hydroxypropyl acrylate, 3-hydroxypropyl methacrylate, 2-hydroxybutyl acrylate, 2-hydroxybutyl methacrylate, 3-hydroxybutyl acrylate, 3-hydroxybutyl methacrylate, 4-hydroxybutyl acrylate, 4-hydroxybutyl methacrylate, allyl acrylate, allyl methacrylate, benzyl acrylate, benzyl methacrylate unsaturated carboxylic acid esters such as methacrylate, cyclohexyl acrylate, phenyl acrylate, phenyl methacrylate, 2-methoxyethyl acrylate, 2-methoxyethyl methacrylate, 2-phenoxyethyl acrylate, 2-phenoxyethyl methacrylate, methoxydiethylene glycol acrylate, methoxydiethylene glycol methacrylate, methoxytriethylene glycol acrylate, methoxytriethylene glycol methacrylate, methoxypropylene glycol acrylate, methoxypropylene glycol methacrylate, methoxydipropylene glycol acrylate, methoxydipropylene glycol methacrylate, isobornyl acrylate, isobornyl methacrylate, dicyclopentadienyl acrylate, dicyclopentadiethyl methacrylate, 2-hydroxy-3-phenoxypropyl acrylate, 2-hydroxy-3-phenoxypropyl methacrylate, glycerol monoacrylate, and glycerol monomethacrylate;Unsaturated carboxylic acid aminoalkyl esters such as 2-aminoethyl acrylate, 2-aminoethyl methacrylate, 2-dimethylaminoethyl acrylate, 2-dimethylaminoethyl methacrylate, 2-aminopropyl acrylate, 2-aminopropyl methacrylate, 2-dimethylaminopropyl acrylate, 2-dimethylaminopropyl methacrylate, 3-aminopropyl acrylate, 3-aminopropyl methacrylate, 3-dimethylaminopropyl acrylate, and 3-dimethylaminopropyl methacrylate; unsaturated carboxylic acid glycidyl esters such as glycidyl acrylate and glycidyl methacrylate; carboxylic acid vinyl esters such as vinyl acetate, vinyl propionate, vinyl butyrate, and vinyl benzoate; vinyl methyl ether, vinyl ethyl ether, allyl glycidyl esters, etc. Examples of the monomers include unsaturated ethers such as acrylonitrile, methacrylonitrile, α-chloroacrylonitrile, vinylidene cyanide, and other vinyl cyanide compounds; unsaturated amides such as acrylamide, methacrylamide, α-chloroacrylamide, N-2-hydroxyethyl acrylamide, and N-2-hydroxyethyl methacrylamide; unsaturated imides such as maleimide, N-phenylmaleimide, and N-cyclohexylmaleimide; aliphatic conjugated dienes such as 1,3-butadiene, isoprene, and chloroprene; and macromonomers having a monoacryloyl group or monomethacryloyl group at the end of the polymer molecular chain of polystyrene, polymethyl acrylate, polymethyl methacrylate, poly-n-butyl acrylate, poly-n-butyl methacrylate, and polysiloxane. These monomers can be used alone or in combination of two or more.
[0054] The white photosensitive resin composition according to the present invention may further contain another alkali-soluble resin (B-2) in addition to the above-mentioned alkali-soluble resin (B).
[0055] There are no particular limitations on the other alkali-soluble resin (B-2) so long as it does not impair the intended effects of the present invention when used in combination with the alkali-soluble resin (B).
[0056] For example, the other alkali-soluble resin (B-2) may be a copolymer containing one or more monomers selected from vinyl toluene, methoxystyrene, 8-tricyclodecanyl methacrylate, methyl methacrylate, etc., but is not limited thereto.
[0057] When the white photosensitive resin composition of the present invention is used together with the alkali-soluble resin (B) and another alkali-soluble resin (B-2), it has the advantage of being easy to form a pattern with the same line width even if the development process in which a pattern is formed using a developer changes. However, it is more preferable that the white photosensitive resin composition of the present invention contains only the alkali-soluble resin (B) alone in order to provide not only a small change in line width during pattern formation, but also excellent effects in preventing the generation of residues, improving transmission strength, and improving heat resistance.
[0058] In the present invention, the alkali-soluble resin (B) may be contained in an amount of 20 to 70 parts by weight, preferably 25 to 65 parts by weight, and more preferably 30 to 60 parts by weight, based on 100 parts by weight of the total solid content in the white photosensitive resin composition.
[0059] When the alkali-soluble resin (B) is contained within the above range, there are advantages in that the solubility in the developer is sufficient, a cured film can be easily formed, the reduction in the film in the pixel portion of the exposed area during development is prevented, and chipping resistance in the non-pixel portion is good.
[0060] Furthermore, when the alkali-soluble resin (B) according to the present invention is contained, there is an advantage that a pattern having a uniform line width can be easily formed even if the development process in which a pattern is formed using a developer is changed.
[0061] (C) Polymerizable compound The polymerizable compound contained in the white photosensitive resin composition of the present invention is a compound that can be polymerized by light and heat, and any polymerizable compound known in this field can be selected and used without particular limitation as long as it can be polymerized by light and heat. Specific examples of the polymerizable compound include monofunctional monomers, bifunctional monomers, and other polyfunctional monomers.
[0062] The types of the monofunctional monomer, the bifunctional monomer, and the polyfunctional monomer are not particularly limited, and examples of the polyfunctional monomer that can be used include trimethylolpropane tri(meth)acrylate, ethoxylated trimethylolpropane tri(meth)acrylate, propoxylated trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, ethoxylated dipentaerythritol hexa(meth)acrylate, propoxylated dipentaerythritol hexa(meth)acrylate, and dipentaerythritol hexa(meth)acrylate.
[0063] Commercially available examples of said double bond monomers include, but are not limited to, Miramer M600 from Miwon Commercial.
[0064] The polymerizable compound may be contained in an amount of 5 to 50 parts by weight, preferably 10 to 40 parts by weight, relative to 100 parts by weight of the total solid content of the white photosensitive resin composition. When the polymerizable compound is contained within the above range, favorable advantages are obtained in terms of strength and smoothness of the pixel portion.
[0065] If the double bond monomer is contained in an amount less than the above range, the strength of the coating film may be somewhat decreased, and if the double bond monomer is contained in an amount exceeding the above range, the smoothness may be somewhat decreased, so it is preferable that the double bond monomer is contained within the above range.
[0066] (D) Photopolymerization initiator The white photosensitive resin composition according to the present invention may contain a photopolymerization initiator.
[0067] The photopolymerization initiator may be a photopolymerization initiator generally used in photosensitive resin compositions, or may be selected from photopolymerization initiators known in the art without any particular restrictions. For example, acetophenone-based, benzophenone-based, triazine-based, thioxanthone-based, oxime-based, benzoin-based, non-imidazole-based compounds, etc. may be used.
[0068] For example, as an oxime compound, o-ethoxycarbonyl-α-oxyamino-1-phenylpropan-1-one or the like may be used, and representative commercially available products include OXE-01 and OXE-02 from Ciba.
[0069] The photopolymerization initiators can be used alone or in combination of two or more. The photopolymerization initiator can be used in an amount of 0.01 to 10 parts by weight, preferably 0.01 to 5 parts by weight, based on 100 parts by weight of the total solid content of the white photosensitive resin composition. The range of the content is determined by considering the photopolymerization rate of the polymerizable compound and the physical properties of the coating film finally obtained. If the content is less than the range, the polymerization rate is low and the overall process time is long, and if the content exceeds the range, the crosslinking reaction occurs excessively due to an excessive reaction, which may deteriorate the physical properties of the coating film. Therefore, it is preferable to use the photopolymerization initiator appropriately within the range.
[0070] A photopolymerization initiation assistant can be used together with the photopolymerization initiator. When a photopolymerization initiation assistant is used together with the photopolymerization initiator, the white photosensitive resin composition has a higher sensitivity and the productivity is improved, which is preferable.
[0071] As the photopolymerization initiation aid, one or more compounds selected from the group consisting of amines and carboxylic acid compounds can be preferably used.
[0072] Such a photopolymerization initiation aid is usually used in an amount of 10 mol or less, preferably in the range of 0.01 to 5 mol, per mol of the photopolymerization initiator. When the photopolymerization initiation aid is used within the above range, the polymerization efficiency can be increased, and the effect of improving productivity can be expected.
[0073] (E) Solvent The solvent contained in the white photosensitive resin composition of the present invention is not particularly limited, and various organic solvents known in the field of photosensitive resin compositions can be used.
[0074] In terms of coatability and drying property, the solvent may be an organic solvent having a boiling point of 100° C. to 200° C., more preferably, alkylene glycol alkyl ether acetates, ketones, esters such as ethyl 3-ethoxypropionate and methyl 3-methoxypropionate, more preferably, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, cyclohexanone, ethyl 3-ethoxypropionate, methyl 3-methoxypropionate, etc. The solvents may be used alone or in combination of two or more kinds.
[0075] The content of the solvent may be usually 60 to 90 parts by weight, preferably 70 to 85 parts by weight, based on 100 parts by weight of the entire white photosensitive resin composition including them. When the content of the solvent satisfies the above range, the coating property tends to be good when the composition is coated with a coating device such as a roll coater, a spin coater, a slit and spin coater, a slit coater (sometimes called a die coater), or an inkjet, which is preferable.
[0076] Additives The white photosensitive resin composition according to one embodiment of the present invention may further contain an additive, if necessary.
[0077] The types of the additives are determined according to the needs of the user and are not particularly limited in the present invention, but examples thereof include other polymer compounds, heat curing agents, surfactants, adhesion promoters, antioxidants, anti-aggregation agents, dispersants, etc. The additives exemplified above can be used alone or in combination of two or more kinds.
[0078] Specific examples of the other polymer compounds include curable resins such as epoxy resins and maleimide resins, and thermoplastic resins such as polyvinyl alcohol, polyacrylic acid, polyethylene glycol monoalkyl ether, polyfluoroalkyl acrylate, polyester, and polyurethane.
[0079] The antioxidant may include at least one selected from the group consisting of phosphorus-based antioxidants, sulfur-based antioxidants, and phenol-based antioxidants, and in this case, it is possible to suppress discoloration that may occur at high temperatures during processing or yellowing that may be induced by a light source after the display is manufactured. The antioxidant may include at least one selected from the group consisting of phenolic compounds, phosphorus-based compounds, and sulfur-based compounds, and these may be used in combination as phenolic-phosphorus compounds, phenolic-sulfur compounds, phosphorus-sulfur compounds, or phenolic-phosphorus-sulfur compounds.
[0080] The antioxidant may be contained in an amount of 0.1 to 30 parts by weight, preferably 0.5 to 20 parts by weight, based on 100 parts by weight of the total solid content of the white photosensitive resin composition of the present invention. When the content of the antioxidant satisfies the above range, it is advantageous in terms of solving the problem of a decrease in luminescence intensity.
[0081] The dispersant is added to maintain the dispersion stability of the pigment, and any dispersant generally used in the art can be used without any restrictions.
[0082] The method for producing the white photosensitive resin composition of the present invention can be a method commonly known in the art, and is not particularly limited in the present invention. For example, the white photosensitive resin composition can be produced by the following method.
[0083] The scattering particles are mixed with a solvent in advance and dispersed using a bead mill or the like until the average particle size becomes 30 to 300 nm. At this time, if necessary, a dispersant may be further used, or a part or all of the alkali-soluble resin may be mixed. The remaining alkali-soluble resin, the polymerizable compound, the photopolymerization initiator, other components used if necessary, and an additional solvent if necessary may be further added to the obtained dispersion liquid (hereinafter sometimes referred to as a mill base) to a predetermined concentration to obtain the desired white photosensitive resin composition.
[0084] In addition, the components other than the scattering particles may be mixed to prepare a preliminary composition, and then the scattering particles may be added to the preliminary composition to prepare a white photosensitive resin composition.
[0085] <Scattered pixels> The present invention provides a scattering pixel fabricated using the above-mentioned white photosensitive resin composition.
[0086] The scattering pixel is a coating film formed by applying the above-mentioned white photosensitive resin composition on a substrate, exposing and developing it in a predetermined pattern. The white photosensitive resin composition of the present invention used to form the coating film does not contain quantum dots, and preferably does not substantially contain other colorants in addition to the above-mentioned scattering particles in order to improve the transmission efficiency of blue light. However, the white photosensitive resin composition for manufacturing the scattering pixel of the present invention may contain a small amount of colorant depending on the characteristics required for the scattering pixel.
[0087] The scattering pixel of the present invention can be suitably applied to image display devices, and can also mean a blue pixel layer that displays blue color by transmitting blue light directly from a blue light source.
[0088] The scattering pixel of the present invention is more suitable for use in a quantum dot display using a blue light source. For example, in the red and green pixel layers, quantum dots located in each pixel are converted to red and green by blue light, respectively, and an image is realized by the scattered light, while the blue pixel layer uses a blue light source as it is. In this case, the blue light source transmits direct light, making it difficult to realize the desired color, and scattered light is also required for blue, so the white photosensitive resin composition of the present invention is used to impart a scattering effect to the blue pixel layer.
[0089] The scattering pixel according to the present invention is manufactured using the above-mentioned white photosensitive resin composition, and therefore has the advantages of lowering the manufacturing cost, improving the transmitted light intensity, and providing an excellent viewing angle.
[0090] <Color filter> The present invention provides a color filter that includes the scattering pixels described above.
[0091] When the color filter of the present invention is applied to an image display device, it can achieve better light efficiency since it emits light by the light source of the display device, and since it emits light having a hue, it has better color reproducibility, and since light is emitted in all directions by photoluminescence, it has an improved viewing angle and excellent brightness characteristics.
[0092] 2, the color filter according to the present invention includes a substrate and a pixel layer formed on one surface of the substrate. The pixel layer may include a scattering pixel and a red and green pattern layer.
[0093] In the present invention, by using a light source that emits blue light, the red pattern layer or the green pattern layer can emit red light or green light, respectively, by the light source that emits blue light, and the scattering pixels can show blue color by transmitting blue light as it is without color conversion, unlike those using a conventional white light source.
[0094] The substrate may be a substrate of the color filter itself or a portion where the color filter is located in a display device, etc., and is not particularly limited. The substrate may be glass, silicon (Si), silicon oxide (SiOx), or a polymer substrate, and the polymer substrate may be polyethersulfone (PES), polycarbonate (PC), etc.
[0095] In the present invention, the scattering pixels may not contain quantum dots and the red and green pattern layers may contain quantum dots.
[0096] The pattern layer may be a coating film formed by applying a colored photosensitive resin composition known in the technical field of the present invention, exposing it to light in a predetermined pattern, developing it, and thermally curing it, or the pattern layer may be formed by carrying out a method commonly known in the art.
[0097] A light source that emits blue light can be used as a light source of an image display device including a color filter according to the present invention, in which the red pattern layer emits red light, the green pattern layer emits green light, and the scattering pixels transmit the blue light as it is, thereby showing blue color.
[0098] <Image display device> The present invention provides an image display device including the scattering layer according to the present invention.
[0099] For example, the image display device may be a liquid crystal display (liquid crystal display device; LCD), an organic electroluminescence display (organic electroluminescence display device), a quantum dot display, a liquid crystal projector, a display device for a game console, a display device for a portable terminal such as a mobile phone, a display device for a digital camera, a display device for a car navigation system, and the like. The image display device according to one embodiment of the present invention may be a quantum dot display.
[0100] The image display device may include other components that are typically included in an image display device, such as a light-emitting device such as a light source, a light guide plate, and a liquid crystal display unit including a color filter, but the present invention is not limited to these.
[0101] In the present invention, the light emitted from the light source applied to the image display device is not particularly limited, but from the viewpoint of better color reproducibility, it is preferable to use a light source that emits blue light.
[0102] The present invention will be described in more detail below based on examples, but the embodiments of the present invention disclosed below are merely illustrative, and the scope of the present invention is not limited to these embodiments. The scope of the present invention is set forth in the claims, and includes all modifications within the scope and meaning equivalent to the claims. In the following examples and comparative examples, the "%" and "parts" indicating the content are by weight unless otherwise specified. EXAMPLES
[0103] <Synthesis Example> Synthesis Example 1: Synthesis of alkali-soluble resin (B-1) A flask equipped with a stirrer, a thermometer, a reflux condenser, a dropping funnel and a nitrogen inlet tube was prepared. On the one hand, 15 parts by weight of N-benzylmaleimide, 30 parts by weight of acrylic acid, 50 parts by weight of cyclohexyl methacrylate, 5 parts by weight of methyl methacrylate, 4 parts by weight of t-butylperoxy-2-ethylhexanoate and 40 parts by weight of propylene glycol monomethyl ether acetate (hereinafter also referred to as PGMEA) were added and stirred and mixed to prepare a dropping funnel for the monomer. 6 parts by weight of n-dodecanediol and 24 parts by weight of PGMEA were added and stirred and mixed to prepare a dropping funnel for the chain transfer agent.
[0104] Thereafter, 395 parts by weight of PGMEA was introduced into the flask, the atmosphere in the flask was replaced with nitrogen from air, and the temperature of the flask was raised to 90°C while stirring. Next, the dropping of the monomer and the chain transfer agent was started from the dropping funnel. The dropping was carried out for 2 hours while maintaining the temperature at 90°C, and after 1 hour, the temperature was raised to 110°C and maintained for 3 hours, after which a gas inlet tube was introduced and bubbling of a mixed gas of oxygen / nitrogen = 5 / 95 (v / v) was started.
[0105] Next, 20 parts by weight of glycidyl methacrylate, 0.4 parts by weight of 2,2'-methylenebis(4-methyl-6-t-butylphenol), and 0.8 parts by weight of triethylamine were added to the flask, and the reaction was continued at 110°C for 6 hours. After that, the mixture was cooled to room temperature to obtain an alkali-soluble resin (B-1) having a weight average molecular weight of 3,800 and an acid value based on the solid content of 83 mgKOH / g.
[0106] Synthesis Example 2 A flask equipped with a stirrer, a thermometer, a reflux condenser, a dropping funnel and a nitrogen inlet tube was prepared. On the one hand, 5 parts by weight of N-benzylmaleimide, 50 parts by weight of acrylic acid, 40 parts by weight of cyclohexyl methacrylate, 5 parts by weight of methyl methacrylate, 4 parts by weight of t-butylperoxy-2-ethylhexanoate, and 40 parts by weight of propylene glycol monomethyl ether acetate (hereinafter also referred to as PGMEA) were added and then stirred and mixed to prepare a dropping funnel for the monomer. 6 parts by weight of n-dodecanediol and 24 parts by weight of PGMEA were added and stirred and mixed to prepare a dropping funnel for the chain transfer agent.
[0107] Thereafter, 395 parts by weight of PGMEA was introduced into the flask, the atmosphere in the flask was replaced with nitrogen from air, and the temperature of the flask was raised to 90°C while stirring. Next, the dropping of the monomer and the chain transfer agent was started from the dropping funnel. The dropping was carried out for 2 hours while maintaining the temperature at 90°C, and after 1 hour, the temperature was raised to 110°C and maintained for 3 hours, after which a gas inlet tube was introduced and bubbling of a mixed gas of oxygen / nitrogen = 5 / 95 (v / v) was started.
[0108] Next, 30 parts by weight of glycidyl methacrylate, 0.4 parts by weight of 2,2'-methylenebis(4-methyl-6-t-butylphenol), and 0.8 parts by weight of triethylamine were added to the flask, and the reaction was continued at 110°C for 8 hours. After that, the reaction was cooled to room temperature to obtain an alkali-soluble resin (B-2) having a solid content of 29.1% by weight, a weight average molecular weight of 6,700, and a solid content standard acid value of 130 mgKOH / g.
[0109] Synthesis Example 3 20 parts by weight of vinyl toluene, 5 parts by weight of methyl methacrylate, 4 parts by weight of t-butyl peroxy-2-ethylhexanoate, and 40 parts by weight of propylene glycol monomethyl ether acetate (hereinafter also referred to as PGMEA) were added, and then stirred and mixed to prepare a dropping funnel for the monomer. 6 parts by weight of n-dodecanediol and 24 parts by weight of PGMEA were added, and then stirred and mixed to prepare a dropping funnel for the chain transfer agent.
[0110] Thereafter, 395 parts by weight of PGMEA was introduced into the flask, the atmosphere in the flask was replaced with nitrogen from air, and the temperature of the flask was raised to 90°C while stirring. Next, the dropping of the monomer and the chain transfer agent was started from the dropping funnel. The dropping was carried out for 2 hours while maintaining the temperature at 90°C, and after 1 hour, the temperature was raised to 110°C and maintained for 3 hours, after which a gas inlet tube was introduced and bubbling of a mixed gas of oxygen / nitrogen = 5 / 95 (v / v) was started.
[0111] Next, 50 parts by weight of glycidyl methacrylate, 0.4 parts by weight of 2,2'-methylenebis(4-methyl-6-t-butylphenol), and 0.8 parts by weight of triethylamine were added to the flask, and the reaction was continued at 110°C for 8 hours. After that, the reaction was cooled to room temperature to obtain an alkali-soluble resin (B-3) having a solid content of 33.2% by weight, a weight average molecular weight of 8,000, and a solid content standard acid value of 135 mgKOH / g.
[0112] Synthesis Example 4 A flask equipped with a stirrer, a thermometer, a reflux condenser, a dropping funnel and a nitrogen inlet tube was prepared. On the one hand, 10 parts by weight of 8-tricyclodecanyl methacrylate, 40 parts by weight of acrylic acid, 40 parts by weight of cyclohexyl methacrylate, 10 parts by weight of methyl methacrylate, 4 parts by weight of t-butylperoxy-2-ethylhexanoate and 40 parts by weight of propylene glycol monomethyl ether acetate (hereinafter also referred to as PGMEA) were added and stirred and mixed to prepare a dropping funnel for the monomer. 6 parts by weight of n-dodecanediol and 24 parts by weight of PGMEA were added and stirred and mixed to prepare a dropping funnel for the chain transfer agent.
[0113] Thereafter, 395 parts by weight of PGMEA was introduced into the flask, the atmosphere in the flask was replaced with nitrogen from air, and the temperature of the flask was raised to 90°C while stirring. Next, the dropping of the monomer and the chain transfer agent was started from the dropping funnel. The dropping was carried out for 2 hours while maintaining the temperature at 90°C, and after 1 hour, the temperature was raised to 110°C and maintained for 3 hours, after which a gas inlet tube was introduced and bubbling of a mixed gas of oxygen / nitrogen = 5 / 95 (v / v) was started.
[0114] Next, 30 parts by weight of glycidyl methacrylate, 0.4 parts by weight of 2,2'-methylenebis(4-methyl-6-t-butylphenol), and 0.8 parts by weight of triethylamine were added to the flask, and the reaction was continued at 110°C for 8 hours. After that, the reaction was cooled to room temperature to obtain an alkali-soluble resin (B-4) having a solid content of 30.1% by weight, a weight average molecular weight of 6,900, and a solid content standard acid value of 90 mgKOH / g.
[0115] Synthesis Example 5 A flask equipped with a stirrer, a thermometer, a reflux condenser, a dropping funnel and a nitrogen inlet tube was prepared. On the one hand, 10 parts by weight of 8-tricyclodecanyl methacrylate, 40 parts by weight of acrylic acid, 30 parts by weight of vinyl toluene, 20 parts by weight of methyl methacrylate, 4 parts by weight of t-butyl peroxy-2-ethylhexanoate and 40 parts by weight of propylene glycol monomethyl ether acetate (hereinafter also referred to as PGMEA) were added and stirred and mixed to prepare a dropping funnel for the monomer. 6 parts by weight of n-dodecanediol and 24 parts by weight of PGMEA were added and stirred and mixed to prepare a dropping funnel for the chain transfer agent.
[0116] Thereafter, 395 parts by weight of PGMEA was introduced into the flask, the atmosphere in the flask was replaced with nitrogen from air, and the temperature of the flask was raised to 90°C while stirring. Next, the dropping of the monomer and the chain transfer agent was started from the dropping funnel. The dropping was carried out for 2 hours while maintaining the temperature at 90°C, and after 1 hour, the temperature was raised to 110°C and maintained for 3 hours, after which a gas inlet tube was introduced and bubbling of a mixed gas of oxygen / nitrogen = 5 / 95 (v / v) was started.
[0117] Next, 30 parts by weight of glycidyl methacrylate, 0.4 parts by weight of 2,2'-methylenebis(4-methyl-6-t-butylphenol), and 0.8 parts by weight of triethylamine were added to the flask, and the reaction was continued at 110°C for 8 hours. After that, the reaction was cooled to room temperature to obtain an alkali-soluble resin (B-5) having a solid content of 29.8% by weight, a weight average molecular weight of 6,200, and a solid content standard acid value of 90 mgKOH / g.
[0118] Preparation Examples 1 to 5: Preparation of preliminary compositions According to Table 1 below, preliminary compositions containing an alkali-soluble resin, a polymerizable compound, a photopolymerization initiator, a dispersant, an antioxidant, and an epoxy resin were produced in Production Examples 1 to 5.
[0119] [Table 1]
[0120] -Alkali-soluble resins B-1 to B-5: Synthesis examples 1 to 5 - Polymerizable compound: dipentaerythritol hexaacrylate (Kayarad DPHA, manufactured by Nippon Kagaku Co., Ltd.) -Photopolymerization initiator: Irgacure OXE01 (manufactured by Basf) -Dispersant: DISPERBYK-110 (BYK) -Antioxidant: Sumilizer GP (Sumitomo Chemical) -Epoxy resin: ESCN 195XL (Sumitomo Chemical) -Solvent: Propylene glycol monomethyl ether acetate (PGMEA) Examples 1 to 6 and Comparative Examples 1 to 3: Production of white photosensitive resin composition According to Table 2, the scattering particles and the preliminary compositions of Production Examples 1 to 5 were mixed to produce the white photosensitive resin compositions of Examples 1 to 6 and Comparative Examples 1 to 3.
[0121] [Table 2]
[0122] <Manufacturing Scattering Pixels> A scattering pixel was manufactured using the white photosensitive resin composition manufactured according to the examples and comparative examples. That is, each of the white photosensitive resin compositions was applied onto a glass substrate by spin coating, and then placed on a heating plate and maintained at 100° C. for 3 minutes to remove the solvent and form a coating film.
[0123] Next, a test photomask having a square transmission pattern of 20 mm x 20 mm and a line pattern of 1 to 100 μm was placed on the coating film, and ultraviolet rays were irradiated at a distance of 100 μm from the test photomask.
[0124] At this time, the ultraviolet light source was an ultra-high pressure mercury lamp (product name: USH-250D) manufactured by Ushio Inc., and the ultraviolet light was irradiated at 200 mJ / cm under air atmosphere. 2 The sample was irradiated with light at an exposure dose of 100 nm (based on 365 nm), and no special optical filters were used.
[0125] The coating film irradiated with UV rays was developed by immersing it in a pH 10.5 KOH aqueous solution development solution for a predetermined time (80 seconds and 160 seconds, respectively). The glass substrate on which the coating film was formed was washed with distilled water, dried by blowing in nitrogen gas, and heated in a heating oven at 230°C for 20 minutes to prepare a hardened film of a scattering pixel pattern. The thickness of the scattering pixel film prepared above was 10 μm.
[0126] <Experimental Example> Experimental example 1: Residue measurement Among the scattering pixels manufactured using the white photosensitive resin compositions manufactured according to the examples and comparative examples, the line patterned portions were measured using an optical microscope (ECLIPSE LV100POL, Nikon Corporation). Based on FIG. 1, the residue level was indicated as ◯ (no residue) or × (residue) depending on the presence or absence of the residue of the resin composition in the non-exposed portion. The criteria for the residue measurement are shown in FIG. 1, and the results are shown in Table 3.
[0127] Experimental example 2: Measurement of transmission intensity Of the scattering pixels prepared using the white photosensitive resin compositions prepared in Examples 1 to 6 and Comparative Examples 1 to 3, the photoconverted area was measured in a portion formed in a 20×20 mm square pattern using a 365 nm tube-type 4 W UV irradiator (VL-4LC, VILBER LOURMAT), and the luminescence intensity (i.e., transmission intensity) in the 450 nm region was measured using a Spectrum meter (Ocean Optics). The measurement results are shown in Table 3. At this time, the higher the measured transmission intensity value, the better the blue light transmission efficiency.
[0128] Experimental Example 3: Evaluation of heat resistance The scattering pixels prepared using the white photosensitive resin compositions prepared in Examples 1 to 6 and Comparative Examples 1 to 3 were heated in a heating oven at 230° C. for 2 hours, and the color change before and after heating was measured and calculated according to Equation (1), and the results are shown in Table 3. The larger the value calculated according to Equation (1), the larger the color change before and after heating, meaning that the pixel is unsuitable for use.
[0129] Mathematical formula (1)ΔEab*=[(ΔL*) 2 +(Δa*) 2 +(Δb*) 2 ] 1 / 2 Experimental Example 4: Measurement of line width change In the manufacture of the scattering pixels, the line width of a 100 μm line mask pattern was measured using an optical microscope (ECLIPSE LV100POL, Nikon Corporation) for a substrate that had been developed for 80 seconds and a substrate that had been developed for 160 seconds. The change in the pattern line width of the substrate that had been developed for 80 seconds and the substrate that had been developed for 160 seconds was measured, and the results are shown in Table 3 below.
[0130] [Table 3]
[0131] Referring to Table 3, it was confirmed that the scattering pixels manufactured using the white photosensitive resin compositions of Examples 1 to 6 had no residues as a whole, and exhibited excellent heat resistance effects. It was also confirmed that the scattering pixels had excellent effects in terms of line width change.
[0132] Meanwhile, it was confirmed that the scattering pixels manufactured using the white photosensitive resin compositions of Comparative Examples 1 to 3 had a relatively significant decrease in the effects of residue prevention, transmission intensity, and / or heat resistance compared to the present application's Examples 1 to 6. It was also confirmed that the change in line width was at least twice as large as that of the embodiment according to the present invention.
[0133] More specifically, it can be seen that the cured film of the scattering pixel manufactured using the white photosensitive resin composition according to Examples 1 to 6 has no resin composition residue in the unexposed area after pattern formation, no color change even in an additional heat process, and has heat resistance, as shown in the experimental result of Experimental Example 1. Thus, it can be seen that in a display device using a blue light source as a light source using the white photosensitive resin composition according to the present invention, the scattering pixel according to the present invention can exhibit uniform performance without distorting the light source.
[0134] On the other hand, it was confirmed that the cured films of the scattering pixels prepared using the white photosensitive resin compositions of Comparative Examples 1 to 3 had residual resin compositions in the unexposed areas after pattern formation, and had significant color change due to an additional heat process, distorting the light source and causing severe performance degradation due to the additional process.
Claims
1. A color filter comprising scattering pixels produced using a white photosensitive resin composition, The white photosensitive resin composition comprises (A) scattering particles, (B) an alkali-soluble resin, (C) a polymerizable compound, (D) a photopolymerization initiator, and (E) a solvent; The alkali-soluble resin (B) contains a unit represented by the following Chemical Formula 1 and a unit represented by the following Chemical Formula 2: The scattering pixel is a scattering pixel that exhibits blue color when exposed to a blue light source. A color filter (excluding those containing a colorant (F)). 【Chemistry 1】 (In the above Chemical Formula 1, R 1 is a direct bond or a linear or branched divalent organic group having 1 to 6 carbon atoms, * is a bond.) 【Chemistry 2】 (In the above Chemical Formula 2, R 2 is a directly bonded, linear or branched divalent organic group having 1 to 20 carbon atoms and containing or not containing a heteroatom, * is a bond.)
2. An image display device comprising the color filter according to claim 1.
Citation Information
Patent Citations
Patterning color conversion film and display device applying same
CN103917000A
Curable resin composition and application thereof
JP2014157265A
Curable resin composition and use therefor
JP2018009059A
Photosensitive resin composition and color filter using same
KR101906279B1
Photosensitive resin composition and color filter using same
KR1020170106791A