Plasma-resistant ceramic member and manufacturing method thereof

The plasma-resistant ceramic member, utilizing YAG and Y2O3 components with a thermal sprayed film, addresses the challenge of increasing member size in corrosive environments by enhancing plasma resistance and mechanical strength, enabling larger components for semiconductor devices.

JP7591425B2Active Publication Date: 2024-11-28NITERRA CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2021028145
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-25
Publication Date
2024-11-28
Estimated Expiration
2041-02-25

AI Technical Summary

Technical Problem

Existing technologies face challenges in increasing the size of plasma-resistant members due to manufacturing methods and material properties, particularly in corrosive environments like plasma processes, where gaps between small plasma-resistant components can allow corrosive gases to enter and affect the process.

Method used

A plasma-resistant ceramic member composed of a ceramic sintered body with YAG or Y2O3 components, featuring a thermal sprayed film to fill gaps between ceramic substrates, ensuring high mechanical strength and improved plasma resistance by preventing gas ingress, with specific surface roughness and porosity levels.

Benefits of technology

The solution enhances plasma resistance and mechanical strength, allowing for larger plasma-resistant ceramic members suitable for large-scale semiconductor devices, with improved surface smoothness and reduced gas penetration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591425000001
    Figure 0007591425000001
  • Figure 0007591425000002
    Figure 0007591425000002
  • Figure 0007591425000003
    Figure 0007591425000003
Patent Text Reader

Abstract

To provide a plasma-resistant ceramic member which is excellent in plasma resistance and can be applied to a large-sized structure as a member for a large-sized semiconductor device, and a method for manufacturing the same.SOLUTION: A plasma-resistant ceramic member 100 comprises: a base material 110 formed of a ceramic sintered body containing Al2O3 as a main component; a plurality of ceramic substrates 120 formed of a ceramic sintered body containing YAG as a main component and adhered to a first surface 112 of the base material 110 so as to be adjacent to each other; and a thermal spraying film 130 formed of YAG or Y2O3 formed in a gap between the adjacent ceramic substrates 120 when the plurality of ceramic substrates 120 is viewed from the stacking direction of the base material 110 and the ceramic substrates 120.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a plasma-resistant ceramic member and a method for producing the same. [Background technology]

[0002] Conventionally, Y3Al5O has been used as a material for semiconductor devices, particularly for materials used in plasma environments, due to its excellent plasma resistance. 12 (YAG) sintered bodies were used.

[0003] Patent Document 1 discloses a plasma-resistant member having at least the surface of an alumina-based substrate with a purity of 98.0% or more, the surface being exposed to plasma, formed of an yttrium aluminum garnet layer, for the purpose of providing a plasma-resistant member having reinforced mechanical strength and sufficient resistance to exposure to low-pressure, high-density plasma. It describes that low-temperature sintering is possible by adding an oxide of a group IIIA element of the periodic table, such as La2O3, as the surface layer material, and that a member having excellent mechanical properties can be obtained by bonding the alumina-based substrate and the surface layer via an intermediate layer of a composite of alumina and yttrium aluminum garnet.

[0004] Furthermore, Patent Document 2 aims to provide a large electrostatic chuck unit that can be manufactured by a simple method while suppressing factors that reduce yields due to deterioration in parallelism between the electrostatic adsorption surface and the internal electrode as the size increases and the occurrence of delamination during sintering, etc., and discloses an electrostatic chuck unit formed by bonding an electrostatic chuck to a base plate, in which the electrostatic chuck is smaller than the base plate, a recess is formed in the base plate into which the electrostatic chuck is embedded, and the adsorption surface of the electrostatic chuck is flush with the upper surface of the base plate, and an electrostatic chuck unit formed by bonding an electrostatic chuck to a base plate, in which the electrostatic chuck is smaller than the base plate and two or more electrostatic chucks are bonded to the base plate. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2004-059397 A [Patent Document 2] JP 2002-252274 A Summary of the Invention [Problem to be solved by the invention]

[0006] The dimensions of components used in semiconductor processes are becoming larger. This has resulted in a demand for larger components to be used in corrosive environments such as plasma processes. However, it has been difficult to increase the size of plasma-resistant components due to their manufacturing methods and the properties of the materials used.

[0007] On the other hand, in FPD processes and the like, when large functional components are required, if only small functional components can be manufactured, these are lined up and bonded to a substrate to be integrated (Patent Document 2). Therefore, it is conceivable to line up small plasma-resistant components to modularize them in order to meet the requirements for large components used in plasma processes. However, there is a concern that simply lining up small plasma-resistant components may allow corrosive gases to enter through the gaps between them and adversely affect the process. Therefore, there has been a demand for plasma-resistant components that can eliminate such concerns and can be made larger.

[0008] However, Patent Document 1 does not mention the enlargement of the plasma resistant member. In addition, Patent Document 2 takes into consideration the enlargement of the electrostatic chuck, but does not take into consideration the resistance to corrosive gases since the electrostatic chuck is not used in a front-end process in which a plasma process is performed in a corrosive environment.

[0009] The present invention has been made in consideration of the above circumstances, and has an object to provide a plasma-resistant ceramic member that has excellent plasma resistance and can be applied to large structures as components for large semiconductor devices, and a manufacturing method thereof. [Means for solving the problem]

[0010] (1) In order to achieve the above object, the plasma-resistant ceramic member of the present invention is a plasma-resistant ceramic member comprising: a base material formed of a ceramic sintered body mainly composed of Al2O3; a plurality of ceramic substrates formed of a ceramic sintered body mainly composed of YAG and bonded adjacent to each other on a first surface of the base material; and a thermal sprayed film made of YAG or Y2O3 formed in gaps between adjacent ceramic substrates when the plurality of ceramic substrates are viewed from the stacking direction of the base material and the ceramic substrates.

[0011] In this way, by forming a plasma-resistant surface by arranging a ceramic substrate made of a ceramic sintered body mainly composed of YAG adjacent to a predetermined surface of the plasma-resistant ceramic member and forming a thermal sprayed film of YAG or Y2O3 in the gap, it is possible to prevent the intrusion of corrosive gas from the gap and to increase plasma resistance. In addition, since the base material is formed of a ceramic sintered body mainly composed of Al2O3, the mechanical strength of the plasma-resistant ceramic member can be sufficiently increased. Therefore, it is also possible to increase the size of the plasma-resistant ceramic member.

[0012] (2) In the plasma-resistant ceramic member of the present invention, the surface roughness Ra of the surface including the adjacent surfaces of the ceramic substrate and the adjacent surface of the thermal sprayed film is 2 μm or less.

[0013] This allows the surface across the sprayed film to be sufficiently smooth, and the plasma resistance of the plasma-resistant surface can be further improved.

[0014] (3) Furthermore, the plasma-resistant ceramic member of the present invention is characterized in that the ceramic substrate has a porosity of 1% or less, and the thermal sprayed coating has a porosity of more than 1% and 5% or less.

[0015] By reducing the porosity of the ceramic substrate and the thermal sprayed film in this manner, the plasma resistance of the plasma-resistant surface can be improved.

[0016] (4) Furthermore, the present invention provides a method for producing a plasma-resistant ceramic member, the method comprising the steps of: preparing a base material formed of a ceramic sintered body mainly composed of Al2O3; and preparing a plurality of ceramic substrates formed of a ceramic sintered body mainly composed of YAG and bonded adjacent to each other on a first surface of the base material; and spraying a thermal spray raw material powder containing YAG or Y2O3 into gaps between adjacent ceramic substrates to form a thermal spray film.

[0017] In this way, by forming a plasma-resistant surface by arranging a ceramic substrate made of a ceramic sintered body mainly composed of YAG adjacent to a predetermined surface of the plasma-resistant ceramic member and forming a thermal sprayed film of YAG or Y2O3 in the gap, it is possible to prevent the intrusion of corrosive gas from the gap and to increase plasma resistance. In addition, since the base material is formed of a ceramic sintered body mainly composed of Al2O3, the mechanical strength of the plasma-resistant ceramic member can be sufficiently increased. Therefore, it is also possible to increase the size of the plasma-resistant ceramic member.

[0018] (5) Furthermore, the method for producing a plasma-resistant ceramic member of the present invention is characterized in that it further comprises, after the step of forming the thermal sprayed film, a step of grinding or polishing the surfaces including the ceramic substrate and the thermal sprayed film on both sides of the gap.

[0019] This allows the surface across the sprayed film to be sufficiently smooth, and the plasma resistance of the plasma-resistant surface can be further improved. Effect of the Invention

[0020] According to the present invention, it is possible to improve plasma resistance and also to sufficiently increase the mechanical strength of the plasma-resistant ceramic member, which makes it possible to realize a large-sized plasma-resistant ceramic member. [Brief description of the drawings]

[0021] [Figure 1] FIG. 1 is a perspective view showing an example of a plasma-resistant ceramic member according to an embodiment of the present invention. [Diagram 2] FIG. 11 is a perspective view showing a modified example of a plasma-resistant ceramic member according to an embodiment of the present invention. [Diagram 3] FIG. 11 is a perspective view showing a modified example of a plasma-resistant ceramic member according to an embodiment of the present invention. [Figure 4] 3(a) to 3(d) are cross-sectional views showing examples of the shape of gaps in a plasma-resistant ceramic member according to an embodiment of the present invention. [Diagram 5] 1A is a cross-sectional view showing an example of the shape of adjacent ceramic substrates and a sprayed film before grinding or polishing the plasma-resistant ceramic member according to an embodiment of the present invention, and FIG. 1B is a cross-sectional view showing an example of the shape of adjacent ceramic substrates and a sprayed film after grinding or polishing the plasma-resistant ceramic member according to an embodiment of the present invention. [Figure 6] 1 is a table showing the shapes and evaluation results of plasma-resistant ceramic members of examples and comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] Next, an embodiment of the present invention will be described with reference to the drawings. In order to facilitate understanding of the description, the same reference numerals are used for the same components in each drawing, and duplicated descriptions will be omitted. In the configuration diagrams, the size of each component is conceptually shown, and does not necessarily represent the actual dimensional ratio.

[0023] [Composition of plasma-resistant ceramic components] Fig. 1 is a perspective view showing an example of a plasma-resistant ceramic member according to an embodiment of the present invention. Fig. 2 and Fig. 3 are perspective views showing modified examples of the plasma-resistant ceramic member according to an embodiment of the present invention. The plasma-resistant ceramic member 100 of the present invention includes a base material 110, a ceramic substrate 120, and a thermal sprayed film 130.

[0024] The base material 110 is formed of a ceramic sintered body mainly composed of Al2O3. The main component of Al2O3 means that the ceramic sintered body contains 95 wt% or more of Al2O3. The shape of the base material 110 can be various shapes such as a disk, a polygonal plate, an elliptical plate, a column, a cylinder, etc., depending on the shape of the plasma-resistant ceramic member 100.

[0025] The ceramic substrate 120 is made of YAG (Y3Al5O 12 The ceramic substrate 120 is formed of a ceramic sintered body mainly composed of YAG. The ceramic sintered body forming the ceramic substrate 120 is composed of YAG at 95 wt% or more. Components other than YAG may include, for example, YAM, YAP, Y2O3, Al2O3, and other composite oxides of Y and Al, and oxides of Y and Al. Also, trace amounts of elements other than Y and Al that are inevitably contained may be included.

[0026] The ceramic substrates 120 are bonded adjacent to each other on the first surface 112 of the base material 110. The first surface 112 of the base material 110 refers to at least a part of the surface of the base material 110 set according to the design of the plasma-resistant ceramic member 100, and may be a flat surface or a curved surface. The first surface 112 may be a continuous flat surface or a curved surface, or a spaced flat surface or a curved surface. The surface of the ceramic substrate 120 and the sprayed film 130 formed on the first surface 112 is called a plasma-resistant surface. The plasma-resistant surface may be a surface that crosses a plurality of plasma-resistant ceramic members.

[0027] Any adhesive may be used to bond the base material 110 and the ceramic substrates 120 since corrosive gases do not penetrate through the gaps between the adjacent ceramic substrates 120, but it is preferable to use a silicone adhesive using a silicone resin in consideration of heat resistance, thermal conductivity, etc. The thickness of the adhesive layer 140 formed by the adhesive is preferably 10 μm or more and 1000 μm or less.

[0028] The porosity of the ceramic substrate 120 is preferably 1% or less, which can further increase the plasma resistance of the plasma-resistant surface.

[0029] The sprayed film 130 is made of YAG or Y2O3. When the ceramic substrates 120 are viewed from the stacking direction of the base material 110 and the ceramic substrates 120, the sprayed film 130 is formed in the gaps between the adjacent ceramic substrates 120.

[0030] In this case, various shapes are possible for the gap between adjacent ceramic substrates 120. Figures 4(a) to 4(d) are cross-sectional views showing examples of the shape of the gap in the plasma-resistant ceramic member according to an embodiment of the present invention.

[0031] As shown in FIG. 4(a), a vertical gap may be provided between adjacent ceramic substrates 120, and the sprayed film 130 may be provided in the gap. Also, as shown in FIG. 4(b), adjacent ceramic substrates 120 may be chamfered, and the sprayed film 130 may be formed on the chamfered portion. Also, as shown in FIG. 4(c), an oblique gap may be provided between adjacent ceramic substrates 120, and the sprayed film 130 may be provided in the gap. The gaps in the cases of FIG. 4(a) to (c) do not have to be parallel. It is sufficient that the sprayed film 130 is formed so as to block the intrusion path of the gas into the base material 110, and it is not necessary to fill all the gaps in the cross section, and a space may remain inside. Therefore, in the cases of FIG. 4(a) to (c), the sprayed film 130 does not have to be in contact with the base material 110.

[0032] 4(d), adjacent ceramic substrates 120 may be combined and the sprayed film 130 may be formed only in the gaps visible from the plasma-resistant surface. In this case, it is sufficient that the sprayed film 130 is formed to block the intrusion path of the gas into the base material 110, and it is not necessary to fill all the gaps in the cross section, and some space may remain inside. Therefore, the sprayed film 130 may not contact some of the surfaces inside the gaps of the ceramic substrates 120.

[0033] In this way, by forming a plasma-resistant surface by arranging a ceramic substrate 120 made of a ceramic sintered body mainly composed of YAG adjacent to a predetermined surface of the plasma-resistant ceramic member 100 and forming a thermal sprayed film 130 of YAG or Y2O3 in the gap, it is possible to prevent the intrusion of corrosive gas from the gap and to improve plasma resistance. In addition, since the base material 110 is formed of a ceramic sintered body mainly composed of Al2O3, it is possible to sufficiently increase the mechanical strength of the plasma-resistant ceramic member 100. Therefore, it is also possible to increase the size of the plasma-resistant ceramic member 100.

[0034] The ceramic substrate 120 made of a ceramic sintered body mainly composed of YAG is denser than a thermal sprayed film made of YAG or Y2O3, and therefore has high plasma resistance. It can also be made thicker more easily than a thermal sprayed film. Therefore, the plasma-resistant ceramic member 100 of the present invention has higher plasma resistance and a longer life than a member in which the surface of a ceramic sintered body mainly composed of Al2O3 is covered with a thermal sprayed film made of YAG or Y2O3.

[0035] In addition, by forming the ceramic substrate 120 from a sintered body mainly composed of YAG and forming the sprayed film 130 from YAG or Y2O3, the YAG sintered body and the YAG sprayed film or the YAG sintered body and Y2O3 have high affinity with each other and are easily mechanically adhered to each other. As a result, there is almost no risk of the sprayed film 130 peeling off.

[0036] The width of the sprayed film 130, i.e., the width of the gap between adjacent ceramic substrates 120 when the ceramic substrates 120 are viewed from the lamination direction of the base material 110 and the ceramic substrates 120, is preferably 0.2 mm or less, more preferably 0.1 mm or less, and even more preferably 0.05 mm or less. This allows the plasma resistance of the plasma-resistant ceramic member 100 to be sufficiently high. There is no particular need to set a lower limit for the width of the sprayed film 130, but when processing is performed to smooth the surface straddling the sprayed film 130 described below, it is preferable that the width be 10 μm or more so that the sprayed film 130 can easily enter the gap.

[0037] The porosity of the thermal sprayed film 130 is preferably greater than 1% and equal to or less than 5%, which can further increase the plasma resistance of the plasma-resistant surface.

[0038] The surface roughness Ra of the surface including the surface of the adjacent ceramic substrate 120 and the surface of the sprayed film 130 is preferably 2 μm or less. This allows the surface straddling the sprayed film 130 to be sufficiently smooth, and the plasma resistance of the plasma-resistant surface can be further improved.

[0039] 4(a) to (d) show an example in which the surface across the sprayed film 130 is ground or polished to make it smooth, but as shown in FIG. 5(a), even if the sprayed film 130 is not ground or polished after it is formed, it is sufficient if the intrusion path of the gas into the base material 110 is blocked. FIG. 5(a) is a cross-sectional view showing an example of the shape of adjacent ceramic substrates 120 and sprayed film 130 before grinding or polishing the plasma-resistant ceramic member 100 according to an embodiment of the present invention. FIG. 5(b) is a cross-sectional view showing an example of the shape of adjacent ceramic substrates 120 and sprayed film 130 after grinding or polishing the plasma-resistant ceramic member 100 according to an embodiment of the present invention. When grinding or polishing is performed, the adjacent ceramic substrates 120 may be processed so that their heights are uniform. In this case, the adjacent ceramic substrates 120 may be processed so that only the heights of the portions including the ends of the ceramic substrates 120 that contact one sprayed film 130 are uniform, rather than the entire height of the adjacent ceramic substrates 120.

[0040] The plasma-resistant ceramic member of the present invention can have high plasma resistance and can also have a sufficiently high mechanical strength, which allows the plasma-resistant ceramic member to be made large.

[0041] [Manufacturing method for plasma-resistant ceramic components] The manufacturing method of the plasma-resistant ceramic member can be divided into the following basic steps: a step of preparing a base material, a step of preparing a ceramic substrate, a step of bonding the ceramic substrate to the base material, a step of forming a thermal sprayed film in the gap between the ceramic substrates adjacent to the base material to which the ceramic substrates are bonded, and, if necessary, a step of grinding or polishing the surface including the thermal sprayed surface. Each step will be described in detail below.

[0042] (Substrate manufacturing process) A substrate with high mechanical strength is made of ceramics mainly composed of Al2O3. For ceramics mainly composed of Al2O3, for example, a fired body can be obtained by granulating Al2O3 raw material powder, forming a molded body by slip casting or CIP molding, and firing it. The substrate can be made by such a conventional manufacturing method. The fired body is prepared as a substrate by necessary machining. Ceramics mainly composed of Al2O3 have high mechanical strength, so they can be made large.

[0043] The average particle size of the Al2O3 raw material powder before granulation is preferably 0.1 μm or more and 2.0 μm or less. The purity of the Al2O3 raw material powder is preferably 99.9% or more, more preferably 99.99% or more. The firing temperature is preferably 1200°C or more and 1800°C or less. The firing time is preferably 0.1 hours or more and 24 hours or less. The firing method may be normal pressure firing or uniaxial pressure firing. The firing atmosphere is preferably an air atmosphere.

[0044] (Ceramic substrate manufacturing process) YAG is an example of a plasma-resistant material that can be used in a corrosive environment such as a plasma process. For example, a molded body of YAG can be formed by casting or CIP molding, and then fired to obtain a fired body. In this case, a raw material powder containing Al or an oxide of Al and a raw material powder containing Y or an oxide of Y can be mixed and granulated, a molded body is formed from the granulated powder, and then fired to form a ceramic substrate by reactive firing to form YAG during firing. Alternatively, a raw material powder of YAG can be granulated, a molded body is formed from the granulated powder, and then fired to form a ceramic substrate. That is, the ceramic substrate can be manufactured by a conventional manufacturing method.

[0045] The average particle size of each raw material powder before granulation is preferably 0.1 μm or more and 2.0 μm or less. The purity of each raw material powder is preferably 99.9% or more, more preferably 99.99% or more. The firing temperature is preferably 1500° C. or more and 1800° C. or less. The firing time is preferably 0.1 hours or more and 24 hours or less. The firing method may be normal pressure firing or uniaxial pressure firing. The firing atmosphere is preferably an air atmosphere.

[0046] Since ceramics whose main component is YAG have weaker mechanical strength than ceramics whose main component is Al2O3, it is difficult to produce large sintered ceramic substrates (e.g., Φ500mm or □500mm, thickness 30mm or more). Therefore, the plasma-resistant surface is divided into multiple areas, and multiple ceramic substrates, each about □250mm x 10mmt, that cover each area are sintered. After sintering, the substrates are machined if necessary to prepare multiple ceramic substrates.

[0047] The difference in thickness between multiple ceramic substrates is preferably 0.1 mm or less, and more preferably 0.05 mm or less. Here, "large" refers to a representative dimension (the dimension where the distance between any two points on the member is the maximum) of 500 mm or more, or a thickness of 20 mm or more. The ratio of the thickness of the base material in the stacking direction to the thickness of the ceramic substrate is preferably 1 / 3 to 1 / 10. This provides sufficient strength for a large member. In addition, it is preferable to manufacture the ceramic substrate so that the porosity is 1% or less.

[0048] (Adhesion process) The ceramic substrates are arranged side by side on the first surface of the base material and bonded. The bonding is preferably performed with a silicone adhesive containing a silicone resin. In this case, the gap between adjacent ceramic substrates is preferably 0.2 mm or less, more preferably 0.1 mm or less, and even more preferably 0.05 mm or less. After bonding, machining may be performed as necessary. In this case, the step in the stacking direction of the multiple ceramic substrates is preferably 0.05 mm or less, more preferably 0.02 mm or less. If the step is larger than this, it becomes difficult to cover the step with a sprayed film in the subsequent spraying process, and there is a risk of cracks occurring.

[0049] (Thermal spraying process) A base material made of a ceramic sintered body mainly composed of Al2O3 and a plurality of ceramic substrates made of a ceramic sintered body mainly composed of YAG and bonded adjacent to each other on a first surface of the base material are prepared, and then a thermal spraying raw material powder containing YAG or Y2O3 is sprayed into the gaps between the adjacent ceramic substrates to form a thermal sprayed film. This is because YAG or Y2O3 is known to have high resistance to plasma. The thermal spraying is preferably performed to such an extent that the ceramic raw material powder is filled into at least a part of the gap. The ceramic thermal spraying is preferably performed by a plasma thermal spraying method, and the raw material to be fed can be a slurry containing dry granules or wet raw material powder. At this time, it is preferable to perform the thermal spraying so that the porosity of the thermal sprayed film is greater than 1% and less than 5%.

[0050] (Grinding and polishing process) After the step of forming the sprayed film, the surfaces including the ceramic substrate and the sprayed film on both sides of the gap may be ground or polished. By machining the ceramic substrate and the sprayed film formed on the base material to be flush, plasma resistance can be improved. In this case, the surface roughness Ra of the surfaces including the surfaces of the adjacent ceramic substrate and the sprayed film is preferably 2 μm or less.

[0051] By the steps described above, the plasma-resistant ceramic member of the present invention can be manufactured.

[0052] [Examples and Comparative Examples] Example 1 (Preparation of substrate) The plasma-resistant ceramic member of Example 1 was formed by forming a base material and a ceramic substrate into the shape shown in Fig. 1. Al2O3 raw material powder (purity 99.99%, average particle size 0.5μm) was weighed, and 3wt% of binder (PVA) was added to the raw material powder, mixed, and granulated. The granulated powder was then CIP molded and fired in an air furnace at 1600℃ for 5 hours to produce a base material.

[0053] (Ceramics Substrate Preparation) Y2O3 raw powder (purity 99.9%, average particle size 1μm) and Al2O3 raw powder (purity 99.99%, average particle size 0.5μm) were weighed out so that the Y2O3 raw powder and Al2O3 raw powder were mixed in a ratio of 37.5mol%:62.5mol%. Next, 2wt% binder (PVA) was added to the weighed raw powder, mixed, and granulated. After that, it was uniaxially pressed and fired in an air furnace at 1700℃ for 2 hours to obtain a fired body. This was machined to produce multiple ceramic substrates. The dimensions of the ceramic substrate after machining were 250mm x 5mmt. The shape of the corners of the ceramic substrate was naturally formed C0.02mm. Four of these were prepared.

[0054] (adhesion) An adhesive was applied to the first surface of the base material, and the ceramic substrate was placed and bonded in a predetermined position. A thermosetting silicone adhesive containing silicone resin was used as the adhesive. The thickness of the adhesive layer after curing was 0.1 mm. The thermal conductivity of the adhesive layer after curing at 25°C was 0.9 W / mK. The gap between adjacent ceramic substrates after bonding (the distance between the substrates in the direction perpendicular to the lamination direction) was 0.05 mm.

[0055] (Thermal spraying) A sprayed film was formed in the gap between the bonded ceramic substrates. First, a high-velocity plasma sprayer was used to irradiate or spray a non-oxidizing gas plasma onto the substrate and the ceramic substrate surfaces to preheat the surfaces. A mixture of Ar gas, N2 gas, and H2 gas was used as the non-oxidizing gas. The supply of Ar gas to the nozzle of the sprayer was controlled at 100 l / min, the supply of N2 gas was controlled at 70 l / min, and the supply of H2 gas was controlled at 70 l / min.

[0056] The power supplied to the nozzle, which constitutes the high-velocity plasma spraying machine, was adjusted to 65 kW by controlling the current applied to the nozzle to 250 A. The distance between the tip of the nozzle and the surface of the ceramic substrate to be sprayed was adjusted to 75 mm. The scanning speed or displacement speed of the nozzle relative to the substrate was adjusted to 850 mm / s. This generated plasma of a mixed gas of Ar gas, N2 gas, and H2 gas, and this plasma was irradiated or sprayed from the tip of the nozzle onto the surface to be sprayed. The surface to be sprayed was preheated by irradiating or spraying the plasma for 3 minutes.

[0057] Then, the high-speed plasma spraying machine was used as it was to plasma spray the YAG slurry onto the surface of the substrate to be sprayed using a non-oxidizing gas. The slurry was prepared by mixing 300 g of YAG raw material powder with a purity of 99.9% or more and an average particle diameter D50 of 0.5 μm with 700 g of water. A mixed gas of Ar gas, N2 gas, and H2 gas was used as the non-oxidizing gas. The supply amount of Ar gas to the nozzle constituting the spraying machine was controlled to 100 l / min, the supply amount of N2 gas was controlled to 70 l / min, and the supply amount of H2 gas was controlled to 70 l / min. As a result, the spraying speed was controlled to 600 to 700 mm / s.

[0058] The power supplied to the nozzle, which constitutes the high-velocity plasma spraying machine, was adjusted to 65 kW by controlling the applied current to 250 A. The distance between the tip of the nozzle and the surface of the ceramic substrate to be sprayed was adjusted to 75 mm. The scanning speed or displacement speed of the nozzle relative to the substrate was adjusted to 850 mm / s. This generated a plasma of a mixed gas of Ar gas, N2 gas, and H2 gas, and the raw material powder melted by the plasma was sprayed from the tip of the nozzle onto the surface of the substrate to be sprayed.

[0059] (processing) After the sprayed film was formed, the surfaces of the adjacent ceramic substrates and the sprayed film were processed to be flush by grinding. The surface roughness Ra of the surface including the surfaces of the adjacent ceramic substrates and the sprayed film after processing was 1.2 μm. In this way, the plasma-resistant ceramic member of Example 1 was produced in which the gap between the adjacent ceramic substrates was covered with the YAG sprayed film. The cross-sectional shape of the gap in Example 1 is as shown in FIG. 4(a).

[0060] Example 2 The plasma-resistant ceramic member of Example 2 was produced under the same conditions and with the same shape as Example 1, except that the corners of the ceramic substrate were machined to C1 mm. The cross-sectional shape of the gap in Example 2 is as shown in Figure 4(b).

[0061] Example 3 The plasma-resistant ceramic member of Example 3 was produced under the same conditions and with the same shape as Example 1, except that the corners of the ceramic substrate were chamfered so that they joined at an angle of 45°. The cross-sectional shape of the gap in Example 3 is as shown in FIG. 4(c).

[0062] Example 4 The plasma-resistant ceramic member of Example 4 was produced under the same conditions and with the same shape as Example 1, except that the corners of the ceramic substrate were processed into a stepped shape for joining together. The cross-sectional shape of the gap in Example 4 is as shown in FIG. 4(d).

[0063] Example 5 In the plasma-resistant ceramic member of Example 5, the base material and the ceramic substrate were formed to have the shape shown in FIG. 2. More specifically, the base material was formed into a cylindrical shape with an outer diameter of 600 mm, an inner diameter of 550 mm, and a height of 500 mm. In addition, the ceramic substrate was formed into a shape in which a cylinder with an outer diameter of 550 mm, an inner diameter of 540 mm, and a height of 250 mm was cut into 1 / 3 in the circumferential direction, and six of these were prepared. Other than that, the manufacturing conditions were the same as those of Example 1. The cross-sectional shape of the gap in Example 5 is the same as that shown in FIG. 4(a).

[0064] Example 6 In the plasma-resistant ceramic member of Example 6, the base material and the ceramic substrate were formed to have the shape shown in FIG. 3. More specifically, the base material was formed into a disk shape with an outer diameter of 600 mm and a thickness of 25 mm. In addition, four ceramic substrates were prepared in a shape in which a doughnut shape with an outer diameter of 600 mm, an inner diameter of 300 mm, and a thickness of 5 mm was cut into 1 / 4 in the circumferential direction, and one ceramic substrate was prepared in a disk shape with an outer diameter of 300 mm and a thickness of 5 mm. The rest of the conditions were the same as those of Example 1. The cross-sectional shape of the gap in Example 6 is as shown in FIG. 4(a).

[0065] Example 7 The plasma-resistant ceramic member of Example 7 was fabricated under the same conditions and with the same shape as Example 1, except that the corners of the ceramic substrate were machined to C0.05 mm and the gap between adjacent ceramic substrates was set to 0.1 mm. The cross-sectional shape of the gap in Example 7 is as shown in FIG. 4(a).

[0066] Example 8 The plasma-resistant ceramic member of Example 8 was produced under the same conditions and with the same shape as Example 1, except that the corners of the ceramic substrate were machined to C0.05 mm and the gap between adjacent ceramic substrates was set to 0.2 mm. The cross-sectional shape of the gap in Example 8 is as shown in Figure 4(a).

[0067] Example 9 The plasma-resistant ceramic member of Example 9 was produced under the same conditions and with the same shape as Example 1, except that the corners of the ceramic substrate were machined to C2 mm. The cross-sectional shape of the gap of Example 9 is as shown in Figure 4(a).

[0068] Example 10 The plasma-resistant ceramic member of Example 10 was produced under the same conditions and with the same shape as Example 1, except that the material of the thermal sprayed coating was Y2O3. The cross-sectional shape of the gap of Example 10 is as shown in Figure 4(a).

[0069] (Comparative Example) The plasma-resistant ceramic member of the comparative example was produced under the same conditions and in the same shape as in Example 1, except that the thermal sprayed film was not formed.

[0070] (Evaluation method) The plasma-resistant ceramic members of Examples 1 to 10 and Comparative Example were individually placed in a chamber for performing plasma processing so that only the plasma-resistant surface was exposed to plasma, and the plasma process was performed for 10 hours. After that, in Example 1 and Comparative Example, a silicon wafer was placed on the surface of the adjacent ceramic substrate, and the number of particles of 0.2 to 5 μm attached to the silicon wafer was counted using a wafer surface inspection device (WM-10) manufactured by Topcon Corporation. In addition, the shape of the plasma-resistant surface of the plasma-resistant ceramic members of Examples and Comparative Example was confirmed with an optical microscope (×500). In addition, the particle dust generation position from the plasma-resistant ceramic member was confirmed by the attachment position of the particle transferred to the silicon wafer. FIG. 6 is a table showing the shape and evaluation results of the plasma-resistant ceramic members of Examples and Comparative Example.

[0071] Compared to Example 1 in which a sprayed film was formed, in the comparative example in which a sprayed film was not formed, the particles were counted concentrated in the area where the sprayed film was not formed, and the number of particles was very large. This is presumably because the corrosive gas that entered through the gaps in the ceramic substrate corroded the Al2O3 of the base material, and the particles generated by this were released to the outside of the plasma-resistant ceramic member. Therefore, it was confirmed that the plasma resistance of the plasma-resistant surface was improved by covering the gaps between adjacent ceramic substrates with a sprayed film made of YAG or Y2O3.

[0072] In Examples 1 to 7 and 10, the morphology of the plasma-resistant surface was good. On the other hand, in Example 8, steps were confirmed in the sprayed film. This is presumed to be because the gap distance of the ceramic substrate was too large. When a sprayed film is formed on a portion of the ceramic substrate where the gap is large or where there is a step, the step may not be covered by the sprayed film. It is considered that the strength of the sprayed film is easily reduced in such a portion, and cracks are easily generated. In addition, in Example 9, pores were confirmed in the sprayed film. This is presumed to be because the C-face was too large, so the volume of the sprayed film deposited became too large, resulting in a distribution of sparse and dense portions in the density of the sprayed film. When the porosity of the sprayed film is 5% or more, the plasma resistance of the sprayed film decreases, and the life of the plasma-resistant ceramic member may be shortened. These problems with the sprayed film can be improved to some extent by changing the spraying conditions.

[0073] From the above results, it was found that the plasma-resistant ceramic member of the present invention can have high plasma resistance and can have sufficiently high mechanical strength. It was also found that the plasma-resistant ceramic member can be made large, as shown by the fact that large members were produced in the examples. It was also found that the method of producing a plasma-resistant ceramic member of the present invention can produce such a plasma-resistant ceramic member.

[0074] The present invention is not limited to the above-described embodiment, and it goes without saying that various modifications and equivalents are included within the spirit and scope of the present invention. In addition, the structure, shape, number, position, size, etc. of the components shown in each drawing are for convenience of explanation and may be changed as appropriate. [Explanation of symbols]

[0075] 100 Plasma-resistant ceramics 110 Base material 112 First Surface 120 Ceramic Substrate 130 Thermal spray coating 140 Adhesive layer

Claims

1. A plasma-resistant ceramic member, A 2 O 3 A substrate formed of a ceramic sintered body having a main component thereof; A plurality of ceramic substrates are formed of a ceramic sintered body containing YAG as a main component and are bonded adjacent to each other on a first surface of the base material; When the ceramic substrates are viewed from the stacking direction of the base material and the ceramic substrates, YAG or YAG is formed in the gaps between the adjacent ceramic substrates. 2 O 3 and a thermal sprayed film comprising said plasma-resistant ceramic member.

2. 2. The plasma-resistant ceramic member according to claim 1, wherein a surface roughness Ra of a surface including the adjacent surfaces of the ceramic substrate and the thermal sprayed film is 2 [mu]m or less.

3. The ceramic substrate has a porosity of 1% or less, 3. The plasma-resistant ceramic member according to claim 1, wherein the porosity of the thermal sprayed coating is greater than 1% and less than or equal to 5%.

4. A method for manufacturing a plasma-resistant ceramic member, comprising: A 2 O 3 preparing a base material formed of a ceramic sintered body mainly composed of YAG, and a plurality of ceramic substrates formed of a ceramic sintered body mainly composed of YAG and bonded adjacent to each other on a first surface of the base material; A gap between adjacent ceramic substrates is filled with YAG or Y 2 O 3 and forming a sprayed film by spraying a powder of thermal spraying raw material containing the above compound.

5. 5. The method for producing a plasma-resistant ceramic member according to claim 4, further comprising the step of grinding or polishing the surfaces including the ceramic substrate and the sprayed film on both sides of the gap after the step of forming the sprayed film.

Citation Information

Patent Citations

  • Ceramic member and manufacturing method thereof

    JP2002087894A

  • Corrosion-resistant member

    JP2002192655A

  • Electrostatic chuck unit

    JP2002252274A

  • Plasma resistant member

    JP2004059397A

  • Plasma resistant member and its producing method