Oil-based offset printing paper
The use of a solvent barrier layer with polystyrene resin and styrene-olefin copolymer in oil-based offset printing papers addresses unevenness and curling issues, maintaining interlayer strength and ensuring high-quality printing.
Patent Information
- Application Number
- JP2021057601
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-30
- Publication Date
- 2024-11-28
- Estimated Expiration
- 2041-03-30
AI Technical Summary
Existing oil-based offset printing papers using synthetic materials face issues with unevenness and curling due to swelling from high-boiling petroleum solvents in quick-drying inks, and laminated films experience interlayer peeling or phase separation.
Incorporating a solvent barrier layer composed of a polystyrene resin and a copolymer of styrene monomer and olefin, with specific structural unit ratios, to prevent solvent penetration and maintain interlayer strength, optionally with a solvent absorption layer for enhanced ink drying.
The solution effectively suppresses unevenness and curling while maintaining interlayer strength, ensuring high-quality printing without defects.
Smart Images

Figure 0007591451000003 
Figure 0007591451000004 
Figure 0007591451000005
Abstract
Description
[Technical field]
[0001] The present invention relates to oil-based offset printing paper. [Background technology]
[0002] Oil-based offset printing allows for easy multi-color printing, and is therefore applied to a variety of printing media. In offset printing, there is a demand for shortening the ink drying time after printing in order to increase printing speed. For this reason, offset printing uses quick-drying inks that combine drying oil with resin and mineral oil (high boiling point petroleum-based solvent) as the offset printing ink vehicle. Table 1 and Figure 1 show examples of the composition of general-purpose quick-drying offset printing inks (hereinafter also referred to as quick-drying inks). When quick-drying offset printing inks are printed, the oxidatively polymerizable drying oil hardens and the mineral oil evaporates, causing it to dry and become a printed layer.
[0003] [Table 1]
[0004] However, when offset printing is performed on synthetic paper made of a stretched polyolefin film or a film made of polyolefin containing inorganic filler, using a normal sheet-fed ink for pulp paper as a quick-drying ink (for example, an ink containing 20 to 40 mass% of a high-boiling petroleum-based solvent), there is a problem that the polyolefin itself is swollen by the vehicle in the quick-drying ink (especially a high-boiling petroleum-based solvent such as mineral oil), causing partial unevenness on the surface of the printed synthetic paper or curling. Therefore, in some offset printing on synthetic paper, special offset inks (inks for non-paper) that do not use mineral oil are used at the expense of quick-drying properties.
[0005] On the other hand, from the viewpoint of productivity, etc., there has been a strong demand to perform offset printing on synthetic paper using sheet-fed ink in the same way as on pulp paper. For this reason, studies have been conducted on films that use amorphous resin as a base and are less likely to cause unevenness or curling even when using fast-drying ink (for example, see Patent Document 1). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2002-036470 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, although the film disclosed in Patent Document 1 has a certain effect in suppressing the occurrence of unevenness or curling, when the amorphous resin is laminated with another layer or when it is combined with another material to form a layer, peeling may occur between layers or between phases.
[0008] An object of the present invention is to provide an oil-based offset printing paper that is capable of suppressing the occurrence of unevenness or curling while suppressing a decrease in interlayer (interphase) strength. [Means for solving the problem]
[0009] As a result of extensive research, the inventors have discovered that by using a solvent blocking layer containing a polystyrene resin and a copolymer of a styrene monomer and an olefin, and by setting the amount of styrene-derived structural units in these resins within a specific range, it is possible to obtain oil-based offset printing paper that is capable of suppressing the occurrence of unevenness or curling while also suppressing a decrease in interlayer (interphase) strength, and have thus completed the present invention.
[0010] That is, the present invention is as follows. (1) An oil-based offset printing paper comprising a base layer containing a polyolefin resin and a solvent blocking layer containing a polystyrene resin and a copolymer of a styrene monomer and an olefin, wherein the amount of structural units based on styrene in the polystyrene resin is 70% by mass or more, the amount of structural units based on styrene in the copolymer is 20% by mass or more and less than 70% by mass, and the amount of structural units based on olefin in the copolymer is 20% by mass or more and 50% by mass or less. (2) The oil-based offset printing paper according to (1), wherein the mass ratio of the copolymer to the polystyrene resin is 0.01 to 0.30. (3) The oil-based offset printing paper according to (1) or (2), wherein the solvent blocking layer further contains a polyolefin resin. (4) The oil-based offset printing paper according to any one of (1) to (3), wherein the solvent blocking layer is stretched in at least one direction. (5) The oil-based offset printing paper according to any one of (1) to (4), wherein the olefin in the copolymer contains at least one linear olefin selected from the group consisting of ethylene, propylene, butylene, butadiene and isoprene. (6) The oil-based offset printing paper according to any one of (1) to (5), further comprising a solvent absorbing layer on the solvent blocking layer. Effect of the Invention
[0011] According to the present invention, it is possible to provide an oil-based offset printing paper that can suppress the occurrence of unevenness or curling while suppressing a decrease in interlayer (interphase) strength. [Brief description of the drawings]
[0012] [Figure 1] This is a phylogenetic tree showing the basic composition of offset printing ink. [Diagram 2] FIG. 1 is a cross-sectional view showing a schematic example of a layer structure of oil-based offset printing paper. [Diagram 3] FIG. 1 is a cross-sectional view showing a schematic example of a layer structure of oil-based offset printing paper. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The oil-based offset printing paper of the present invention will be described in detail below. The following is one example (representative example) of the present invention, and the present invention is not limited thereto.
[0014] In the following description, the term "(meth)acrylic" refers to both acrylic and methacrylic.
[0015] [Oil-based offset printing paper] FIG. 2 is a cross-sectional view showing an example of the layer structure of the oil-based offset printing paper of this embodiment. The oil-based offset printing paper 100 shown in FIG. 2 has at least a solvent blocking layer 10 containing a polystyrene resin and a copolymer of a styrene monomer and an olefin on either side of a substrate layer 20 containing a polyolefin resin. In addition, as shown in FIG. 3, the oil-based offset printing paper 100 of this embodiment may further have a solvent absorbing layer 30 for absorbing a vehicle in the quick-drying ink on the solvent blocking layer 10. That is, the oil-based offset printing paper 100 of this embodiment may have the solvent absorbing layer 30, the solvent blocking layer 10, and the substrate layer 20 in this order. The oil-based offset printing layer is provided on the side of the solvent blocking layer 10 in FIG. 2 or the side of the solvent absorbing layer 30 in FIG. 3.
[0016] In this specification, the term "polystyrene-based resin" refers to a homopolymer of a styrene-based monomer or a copolymer with other monomer components, in which the amount of structural units based on styrene in the polystyrene-based resin is 70 mass% or more. In this specification, the term "copolymer of a styrene-based monomer and an olefin" refers to a resin that is a copolymer of a styrene-based monomer and an olefin, and in which the amount of structural units based on styrene in the copolymer is less than 70 mass%.
[0017] (Solvent barrier layer) The solvent barrier layer is provided on the base layer and can be positioned on the outermost surface of the oil-based offset printing paper of this embodiment. The solvent barrier layer mainly blocks the vehicle (especially high-boiling petroleum solvents such as mineral oil) in the quick-drying ink during offset printing, thereby preventing the vehicle from reaching the base layer, suppressing swelling of the base layer, and suppressing the occurrence of unevenness or curling in the entire oil-based offset printing paper.
[0018] The solvent blocking layer comprises a polystyrene resin and a copolymer of a styrene monomer and an olefin, and is characterized in that the amount of structural units based on styrene in the polystyrene resin is 70% by mass or more, the amount of structural units based on styrene in the copolymer is 20% by mass or more and less than 70% by mass, and the amount of structural units based on olefin in the copolymer is 20% by mass or more and 50% by mass or less.
[0019] <Polystyrene resin> The solvent barrier layer contains a polystyrene resin. When the solvent barrier layer contains a polystyrene resin, the occurrence of unevenness or curling of the oil-based offset printing paper can be suppressed.
[0020] Polystyrene resins are polymers mainly having structural units derived from styrene, and are homopolymers of styrene monomers or copolymers with other monomer components. Examples of styrene monomers include styrene, α-methylstyrene, p-methylstyrene, p-ethylstyrene, vinyltoluene, vinylxylene, and vinylnaphthalene.
[0021] As the other monomer component in the copolymer, for example, olefins are preferably used. Examples of olefins include α-olefins, diene monomers, and other monomers such as ethylene, propylene, and cyclohexene. Specific examples of α-olefins include 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-heptene, 1-octene, 1-nonene, and 1-decene. Examples of diene monomers include butadiene, isoprene, and chloroprene. The copolymer may be a binary or ternary or higher multiple monomer system, and may be a random or block copolymer. Other monomer components that may be used in the copolymer include, for example, (meth)acrylic acid, (meth)acrylic acid esters, maleic anhydride, vinyl acetate, and acrylonitrile.
[0022] Specific examples of polystyrene resins used in the solvent barrier layer include styrene homopolymers, styrene-ethylene copolymers, styrene-propylene copolymers, styrene-butadiene copolymers, styrene-isoprene copolymers, styrene-ethylene-butylene copolymers, styrene-ethylene-propylene copolymers, styrene-butadiene-butylene copolymers, styrene-acrylonitrile copolymers, acrylonitrile-butadiene-styrene copolymers, acrylonitrile-styrene-acrylic acid ester copolymers, and methacrylic acid ester-butadiene-styrene copolymers. The copolymers may be random or block copolymers. The polystyrene resins may be hydrogenated.
[0023] In the polystyrene resin used in the solvent blocking layer, the amount of the structural unit based on styrene in the polystyrene resin is 70% by mass or more, preferably 80% by mass or more, and more preferably 90% by mass or more. When the amount of the structural unit based on styrene in the polystyrene resin is equal to or more than the lower limit, the occurrence of unevenness or curling tends to be suppressed.
[0024] When a copolymer of a styrene monomer and an olefin is used as the polystyrene resin for the solvent blocking layer, the amount of olefin-based structural units in the polystyrene resin is preferably less than 30 mass%, more preferably less than 20 mass%, and even more preferably less than 10 mass%.
[0025] The content of the polystyrene resin in the solvent blocking layer is preferably 20% by mass or more, more preferably 25% by mass or more, and even more preferably 30% by mass or more, from the viewpoint of suppressing the occurrence of unevenness or curling, while the content of the polystyrene resin is preferably 80% by mass or less, more preferably 60% by mass or less, and even more preferably 50% by mass or less, from the viewpoint of suppressing a decrease in interlayer (interphase) strength.
[0026] <Copolymer of styrene monomer and olefin> The solvent barrier layer contains a copolymer of a styrene monomer and an olefin. By containing the copolymer of a styrene monomer and an olefin in the solvent barrier layer, the compatibility between the polystyrene resin and the polyolefin resin described later is improved, and interlayer or interphase peeling of the oil-based offset printing paper can be efficiently suppressed. In addition, the copolymer of a styrene monomer and an olefin can contain one or more other structural units other than styrene and olefin, so long as it does not impair the effects of the present invention.
[0027] A copolymer of a styrene monomer and an olefin is a polymer mainly having a structural unit derived from styrene and a structural unit derived from an olefin. Examples of olefins include α-olefins; diene monomers; and other monomers such as ethylene, propylene, and cyclohexene. Specific examples of α-olefins include 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-heptene, 1-octene, 1-nonene, and 1-decene. Examples of diene monomers include butadiene, isoprene, and chloroprene.
[0028] Among these, the olefin used in the constituent units of the copolymer preferably contains at least one linear olefin selected from the group consisting of ethylene, propylene, butylene, butadiene and isoprene, and more preferably contains butadiene.
[0029] Specific examples of copolymers of styrene monomers and olefins used in the solvent barrier layer include styrene-ethylene copolymers, styrene-propylene copolymers, styrene-butadiene copolymers, styrene-butadiene-styrene copolymers, styrene-isoprene copolymers, styrene-isoprene-styrene copolymers, styrene-ethylene-butylene copolymers, styrene-ethylene-propylene copolymers, styrene-butadiene-butylene copolymers, acrylonitrile-butadiene-styrene copolymers, methacrylic acid ester-butadiene-styrene copolymers, and styrene-ethylene-butadiene-styrene copolymers. The copolymers may be random or block copolymers, but are preferably block copolymers. The copolymers may also be hydrogenated.
[0030] In the copolymer of a styrene monomer and an olefin, from the viewpoint of suppressing a decrease in interlayer (interphase) strength, the amount of structural units based on styrene in the copolymer is 20% by mass or more, preferably 30% by mass or more, more preferably 40% by mass or more, and even more preferably 50% by mass or more. On the other hand, in the copolymer of a styrene monomer and an olefin, from the viewpoint of suppressing a decrease in interlayer (interphase) strength, the amount of structural units based on styrene in the copolymer is less than 70% by mass.
[0031] In the copolymer of a styrene monomer and an olefin, the amount of structural units based on olefin in the copolymer is 20% by mass or more, preferably 30% by mass or more, from the viewpoint of suppressing interlaminar (interphase) strength reduction. On the other hand, in the copolymer of a styrene monomer and an olefin, the amount of structural units based on olefin in the copolymer is 50% by mass or less, preferably 40% by mass or less, from the viewpoint of suppressing unevenness or curling and interlaminar (interphase) strength reduction.
[0032] The content of the copolymer of a styrene monomer and an olefin in the solvent blocking layer is preferably 0.1% by mass or more, more preferably 1.0% by mass or more, and even more preferably 5.0% by mass or more, from the viewpoint of suppressing a decrease in interlayer (interphase) strength, while the content of the copolymer of a styrene monomer and an olefin is preferably 15% by mass or less, more preferably 10% by mass or less, and even more preferably 5.0% by mass or less, from the viewpoint of suppressing the occurrence of unevenness or curling.
[0033] The mass ratio of the copolymer of a styrene monomer and an olefin to the polystyrene resin (copolymer of a styrene monomer and an olefin / polystyrene resin) is preferably 0.01 or more, more preferably 0.02 or more, from the viewpoint of suppressing a decrease in interlayer (interphase) strength, while the mass ratio is preferably 0.3 or less, more preferably 0.2 or less, and even more preferably 0.1 or less, from the viewpoint of suppressing the occurrence of unevenness or curling.
[0034] <Polyolefin resin> The solvent blocking layer may be a resin film using only a polystyrene-based resin and a copolymer of a styrene-based monomer and an olefin, or a resin film containing a polyolefin-based resin other than a polystyrene-based resin and a copolymer of a styrene-based monomer and an olefin within a range that does not impair the effects of the present invention.
[0035] When the solvent barrier layer contains a polyolefin resin in addition to the polystyrene resin, a sea-island structure is formed between the polystyrene resin and the polyolefin resin. Furthermore, when the solvent barrier layer is a stretched film, each phase constituting the sea-island structure is stretched by stretching and tends to have a layered structure, which can more efficiently block the vehicle in the quick-drying ink (especially high-boiling petroleum solvents such as mineral oil) from penetrating into the base layer, and can suppress the occurrence of unevenness or curling on the paper surface after printing and storage.
[0036] Specific examples of polyolefin resins include polypropylene resins, polyethylene resins, and polymethyl-1-pentene.
[0037] The polypropylene-based resin is not particularly limited as long as propylene is used as the main monomer component. For example, an isotactic polymer or a syndiotactic polymer obtained by homopolymerizing propylene can be mentioned. In addition, a propylene-α-olefin copolymer, which is a copolymer of propylene as the main component and α-olefin such as ethylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, or 1-octene, can also be used. The copolymer may be a binary or ternary or more multiple monomer system, and may be a random copolymer or a block copolymer. In addition, a propylene homopolymer and a propylene copolymer may be used in combination.
[0038] The polyethylene resin has a density of, for example, 0.940 to 0.965 g / cm 3 High density polyethylene, density is 0.920~0.935g / cm 3 of medium density polyethylene, with a density of 0.900 g / cm 3 More than 0.920g / cm 3 Examples of such copolymers include linear low-density polyethylene having a molecular weight of less than 1000, copolymers mainly composed of ethylene and copolymerized with α-olefins such as propylene, butene, hexene, heptene, octene, and 4-methylpentene-1, maleic acid modified ethylene-vinyl acetate copolymer, ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer, ethylene-acrylic acid alkyl ester copolymer, ethylene-methacrylic acid alkyl ester copolymer, metal salts of ethylene-methacrylic acid copolymer (metals are zinc, aluminum, lithium, sodium, potassium, etc.), ethylene-cyclic olefin copolymer, and maleic acid modified polyethylene.
[0039] Examples of polyolefin resins used in the solvent barrier layer include branched polyethylene and linear polyethylene with a melt flow rate (190°C, 2.16 kg load) of 1 to 10 g / 10 min; propylene homopolymers, (4-methyl-1-pentene) homopolymers, propylene-ethylene copolymers, propylene-1-butene copolymers, propylene-ethylene-1-butene copolymers, propylene-4-methyl-1-pentene copolymers, propylene-3-methyl-1-pentene copolymers, poly(1-butene), poly(4-methyl-1-pentene), and propylene-ethylene-3-methyl-1-pentene copolymers with a melt flow rate (230°C, 2.16 kg load). Among these, it is more preferable to use at least one of a polyethylene resin containing ethylene as a raw material monomer and a polypropylene resin containing propylene as a raw material monomer, and propylene homopolymer, propylene-ethylene random copolymer, and high-density polyethylene are even more preferable because they are inexpensive and have good moldability.
[0040] The polyolefin resin used in the solvent blocking layer preferably has a melting point (peak temperature of DSC curve) of 130 to 210° C. Among them, a propylene homopolymer having a melting point (peak temperature of DSC curve) of 155 to 174° C. and a melt flow rate (JIS K7210:2014) of 0.5 to 10 g / 10 min can be preferably used. The polyolefin resin can be used alone or in combination of two or more kinds.
[0041] When the solvent blocking layer contains a polyolefin resin, the content of the polyolefin resin is preferably 5% by mass or more, more preferably 20% by mass or more, and even more preferably 40% by mass or more from the viewpoint of suppressing a decrease in interlayer (interphase) strength, while the content of the polyolefin resin is preferably 75% by mass or less, more preferably 70% by mass or less, and even more preferably 60% by mass or less from the viewpoint of suppressing the occurrence of unevenness or curling.
[0042] <Filler> The solvent blocking layer may contain a filler. Examples of the filler that can be used include inorganic fillers and organic fillers. The inorganic fillers and organic fillers preferably have an average particle size of 0.01 to 10 μm, and more preferably 0.05 to 8 μm.
[0043] <<Inorganic filler>> Examples of the inorganic filler include heavy calcium carbonate, light calcium carbonate, calcined clay, talc, titanium oxide, barium sulfate, aluminum sulfate, silica, zinc oxide, magnesium oxide, and diatomaceous earth.
[0044] <<Organic filler>> Examples of the organic filler include polyethylene terephthalate, polybutylene terephthalate, polyamide, polycarbonate, polyethylene naphthalate, polystyrene, melamine resin, polyethylene sulfite, polyimide, polyethyl ether ketone, and polyphenylene sulfite.
[0045] As the filler, the above-mentioned inorganic fillers and organic fillers can be used alone or in combination. The filler content in the solvent blocking layer (when an inorganic filler and an organic filler are used in combination, the total amount) is preferably 5 mass % or less, more preferably 3 mass % or less, and even more preferably 1 mass % or less, from the viewpoint of reducing the porosity of the solvent blocking layer.
[0046] <Other ingredients> The solvent blocking layer may contain, as necessary, an ultraviolet absorbing agent, a dispersing agent, a crosslinking agent, an antistatic agent, a fluorescent whitening agent, etc. These can be contained within a range that does not impair the effects of the present invention.
[0047] The solvent blocking layer may be a non-stretched film or a stretched film, but from the viewpoint of obtaining a higher solvent blocking effect when a polystyrene-based resin and a polyolefin-based resin are used in combination, it is preferable that the layer be a stretched film stretched in at least one direction.
[0048] <Porosity> The porosity of the solvent blocking layer is preferably 5% or less, more preferably 3% or less. The porosity of the solvent blocking layer refers to the area ratio of pores in the solvent blocking layer, determined by observing an arbitrary cross section of the printing paper with a scanning electron microscope. By making the porosity 5% or less, it is possible to prevent the vehicle in the quick-drying ink from passing through the pores and reaching the base layer, which tends to suppress swelling of the base layer and to easily suppress the occurrence of unevenness or curling of the entire printing paper.
[0049] <Thickness> The thickness of the solvent blocking layer is preferably 0.5 μm or more, more preferably 1 μm or more, from the viewpoint of sufficiently blocking the vehicle in the fast-drying ink, while the thickness of the solvent blocking layer is preferably 10 μm or less, more preferably 5 μm or less, from the viewpoint of cost reduction, etc.
[0050] (base material layer) The base layer is a resin film containing a polyolefin resin, and is provided as a support for the oil-based offset printing paper. Therefore, the cause of the occurrence of unevenness or curling of the entire oil-based offset printing paper is predominantly the presence or absence of swelling in the base layer. The base layer may be a single-layer structure, or a multi-layer structure of two or more layers.
[0051] The polyolefin resin used in the base layer may be the polyolefin resin listed in the solvent barrier layer. The base layer may be a resin film using only a polyolefin resin, or may contain a thermoplastic resin other than a polyolefin resin within a range that does not impair the effects of the present invention.
[0052] Examples of thermoplastic resins that can be used in combination with the polyolefin resins include polyamide resins such as nylon-6, nylon-6,6, nylon-6,10, and nylon-6,12; thermoplastic polyester resins such as polyethylene terephthalate and its copolymers, polyethylene naphthalate, and aliphatic polyesters; and polycarbonate resins such as aromatic polycarbonates and aliphatic polycarbonates.
[0053] The substrate layer may contain a filler. When the substrate layer contains a filler, when the substrate layer is a stretched film, pores originating from the filler are formed by stretching, forming a porous layer. When the substrate layer is a porous layer, the substrate layer and, in turn, the oil-based offset printing paper can be made lighter. Furthermore, when the substrate layer is a porous layer, a white film having the texture of paper can be easily obtained. Therefore, the whiteness or opacity of the film can be easily adjusted depending on whether or not the substrate layer contains a filler. In addition, when the substrate layer has pores, once the vehicle in the ink reaches the substrate layer, it is easy to penetrate deep into the substrate layer through the pores, and unevenness or curling is likely to occur. However, since the oil-based offset printing paper according to this embodiment has the above-mentioned solvent blocking layer, even when the substrate layer has pores, the occurrence of unevenness or curling can be suppressed.
[0054] The filler usable in the base layer may be the same as the filler exemplified in the solvent blocking layer. As the filler, an inorganic filler and an organic filler may be used alone or in combination.
[0055] The content of the polyolefin resin in the base layer is preferably 20 to 90% by mass, and the total content of the inorganic filler and / or organic filler is preferably 10 to 80% by mass.
[0056] The base layer may be a non-stretched film or a stretched film, but from the viewpoint of increasing the strength of the printing paper, it is preferable that the base layer is a stretched film stretched in at least one direction. When the base layer has a multi-layer structure, it preferably contains a stretched film stretched in at least one direction.
[0057] When the base layer is made into a uniaxially stretched film, the polyolefin resin is preferably at least one of a polyethylene resin and a polypropylene resin, and the total content of the polyethylene resin and / or the polypropylene resin is more preferably 20% by mass or more, even more preferably 25% by mass or more, and even more preferably 30% by mass or more. On the other hand, the content is more preferably 50% by mass or less. In this case, the inorganic filler and / or the organic filler is preferably 50% by mass or more in total, and is preferably 80% by mass or less, more preferably 75% by mass or less, and even more preferably 70% by mass or less.
[0058] When the base layer is a biaxially stretched film, the polyolefin resin is preferably at least one of a polyethylene resin and a polypropylene resin. The total content of the polyethylene resin and / or the polypropylene resin is preferably 55% by mass or more, more preferably 60% by mass or more, and even more preferably 65% by mass or more. On the other hand, the content is preferably 90% by mass or less. In this case, the total content of the inorganic filler and / or the organic filler is preferably 10% by mass or more, and is preferably 45% by mass or less, more preferably 40% by mass or less, and even more preferably 35% by mass or less.
[0059] <Porosity> The base layer preferably contains a large number of voids (holes). From the viewpoint of opacity and weight reduction, the porosity is preferably 1% or more, more preferably 10% or more, and even more preferably 20% or more. On the other hand, from the viewpoint of stability during stretch molding, the porosity is preferably 60% or less, more preferably 55% or less, even more preferably 50% or less, and particularly preferably 40% or less.
[0060] <Thickness> From the viewpoint of increasing the strength of the printing paper, the thickness of the base layer is preferably 30 μm or more, and more preferably 40 μm or more, while the thickness of the base layer is preferably 150 μm or less, and more preferably 130 μm or less.
[0061] (Solvent absorbing layer) The oil-based offset printing paper of this embodiment preferably further comprises a solvent absorbing layer on the solvent barrier layer for absorbing the vehicle in the fast-drying ink (particularly high-boiling petroleum-based solvents such as mineral oil). By providing a solvent absorbing layer, the drying and adhesion of the ink can be improved. Furthermore, by providing the oil-based offset printing paper with a solvent absorbing layer on the solvent barrier layer, the vehicle in the printing ink can be retained in the solvent absorbing layer, thereby reducing the amount of vehicle that reaches the solvent barrier layer. As a result, it becomes easier to achieve a higher level of suppression of the occurrence of unevenness or curling.
[0062] The solvent absorption layer is a porous layer having many pores, and the vehicle in the ink is absorbed into the pores, thereby improving the drying properties of the ink. The more interconnected the pores in the porous layer are, the better the drying properties of the ink. On the other hand, if the porous layer has a large proportion of independent pores, the amount of vehicle absorbed is reduced, and the drying properties of the ink are reduced.
[0063] The solvent absorbing layer preferably contains a thermoplastic resin and a filler from the viewpoint of forming interconnected pores. The thermoplastic resin and the filler used in the solvent absorbing layer may be the same as those listed in the base layer. The inorganic filler or the organic filler may be surface-treated with a fatty acid or the like from the viewpoint of dispersing the filler having a relatively small particle size in the resin. When the thermoplastic resin containing the filler is stretched, it becomes easy to form a large number of fine pores with the filler as a core.
[0064] The average particle size of the filler is preferably 0.01 μm or more, more preferably 0.1 μm or more, from the viewpoint of uniform dispersion in the porous layer, and is preferably 10 μm or less, more preferably 3 μm or less, even more preferably 1.5 μm or less, and particularly preferably 1.3 μm or less, from the viewpoint of facilitating separation of the pigment, binder, and other components in the ink from the solvent component and preventing color sinking or poor drying of the ink. The particle size of the filler can be determined, for example, by observing a cut surface of the film under an electron microscope, measuring the maximum diameters of at least 10 filler particles, and averaging the measured values.
[0065] The content of the filler in the solvent absorbing layer is preferably 45 parts by mass or more, more preferably 60 parts by mass or more, even more preferably 75 parts by mass or more, and particularly preferably 100 parts by mass or more, relative to 100 parts by mass of the thermoplastic resin, from the viewpoint of pore formability. On the other hand, the content of the filler in the solvent absorbing layer is preferably 250 parts by mass or less, more preferably 200 parts by mass or less, even more preferably 150 parts by mass or less, and particularly preferably 125 parts by mass or less, relative to 100 parts by mass of the thermoplastic resin, from the viewpoint of maintaining the strength of the solvent absorbing layer at a suitable level.
[0066] <Porosity> The porosity, which represents the proportion of pores in the porous layer, is preferably 10% or more, more preferably 15% or more, even more preferably 20% or more, and particularly preferably 25% or more from the viewpoint of increasing the number of continuous pores. From the viewpoint of increasing the surface strength and reducing printing defects such as picking, the porosity is preferably 50% or less, more preferably 45% or less, and even more preferably 40% or less.
[0067] <Thickness> The thickness of the solvent absorbing layer is preferably 3 μm or more, more preferably 5 μm or more, and even more preferably 7 μm or more. The thickness of the solvent absorbing layer is preferably 20 μm or less, more preferably 15 μm or less, and even more preferably 10 μm or less. If the thickness of the solvent absorbing layer is within the above range, picking is unlikely to occur, and high drying properties and a higher effect of suppressing the occurrence of unevenness or curling can be easily obtained.
[0068] [Physical properties of oil-based offset printing paper] (Surface strength) The surface strength of the oil-based offset printing paper is preferably 1.0 kg / cm or more, more preferably 1.5 kg / cm or more, and even more preferably 2.0 kg / cm or more. If the surface strength of the oil-based offset printing paper is equal to or greater than the above lower limit, the oil-based offset printing paper is less likely to undergo interlayer peeling or intralayer cohesive failure. The surface strength of oil-based offset printing paper can be determined by attaching an adhesive tape to the surface on the base layer side and measuring with an internal bond tester in accordance with TAPPI-UM403, as shown in the examples described later.
[0069] (Thickness) The thickness of oil-based offset printing paper is generally 35 to 300 μm. In this embodiment, in order to further add a paper-like feel, another layer, such as a layer of a propylene-based resin containing 8 to 55 mass% of inorganic filler, may be further formed between the solvent blocking layer and the base layer. Furthermore, this other layer may contain a small amount of a low-melting point resin such as a propylene-based copolymer, high-density polyethylene, polystyrene, or ethylene-vinyl acetate copolymer to improve stretchability.
[0070] [Manufacturing method of oil-based offset printing paper] There are no particular limitations on the method for producing the oil-based offset printing paper, and any method for producing the paper falls within the scope of the present invention as long as it satisfies the requirements of the present invention. A preferred method for producing oil-based offset printing paper will now be described.
[0071] In the present embodiment, the resin composition of the base layer is melt-kneaded in advance, extruded into a sheet, and stretched 4 to 7 times in the longitudinal direction by utilizing the difference in peripheral speed between rolls. Next, a resin composition to be a solvent blocking layer is melt-kneaded on at least one side of this longitudinally stretched film, laminated into a sheet, and stretched 4 to 12 times in the transverse direction by using a tenter at a temperature 5 to 35°C lower than the melting point of the polyolefin resin of the base layer. Then, the oil-based offset printing paper can be produced by heat treatment and cooling.
[0072] In another embodiment, the resin composition for the base layer and the resin composition for the solvent blocking layer are melt-kneaded separately, co-extruded into a sheet with the solvent blocking layer on the outside, and stretched 4 to 7 times in the machine direction at a temperature 10°C or more higher than the glass transition temperature of the amorphous resin by utilizing the difference in peripheral speed between rolls. Next, this is stretched 4 to 12 times in the cross direction using a tenter at a temperature 5 to 35°C lower than the melting point of the polyolefin resin of the base layer and 10°C or more higher than the glass transition temperature of the amorphous resin, followed by heat treatment and cooling, thereby producing oil-based offset printing paper.
[0073] In yet another embodiment, the resin composition for the base layer and the resin composition for the solvent blocking layer are melt-kneaded separately, co-extruded into a sheet with the solvent blocking layer on the outside, and stretched 4 to 7 times in the machine direction at a temperature 10°C higher than the glass transition temperature of the amorphous resin by utilizing the difference in peripheral speed between rolls. Then, the sheet is heat-treated and cooled to produce oil-based offset printing paper.
[0074] When a solvent absorbing layer is provided, an oil-based offset printing paper comprising a base layer, a solvent blocking layer and a solvent absorbing layer can be produced, for example, by the following method. The resin composition for the base layer is melt-kneaded in advance, extruded into a sheet, and stretched 4 to 7 times in the longitudinal direction by utilizing the difference in peripheral speed between the rolls. Next, the resin composition for the solvent blocking layer and the resin composition for the solvent absorbing layer are separately melt-kneaded in advance on this longitudinally stretched film, laminated into a sheet so as to have the desired layer structure, and stretched 4 to 12 times in the transverse direction at a specific temperature using a tenter. Then, oil-based offset printing paper can be obtained by heat treatment and cooling.
[0075] In addition to the above, the resin composition for the base layer, the resin composition for the solvent blocking layer, and the resin composition for the solvent absorbing layer can be melt-kneaded separately, co-extruded into a sheet so as to have a desired layer structure, and stretched 4 to 7 times in the machine direction at a specific temperature using the difference in peripheral speed of a group of rolls, and then stretched 4 to 12 times in the transverse direction at a specific temperature using a tenter, followed by heat treatment and cooling to produce the film. Alternatively, the resin composition for the base layer, the resin composition for the solvent blocking layer, and the resin composition for the solvent absorbing layer can be melt-kneaded separately, co-extruded into a sheet so as to have the desired layer structure, stretched 2 to 7 times in the longitudinal direction at a specific temperature by utilizing the difference in peripheral speed of a group of rolls, and then heat-treated and cooled to produce the film.
[0076] The surface of the oil-based offset printing paper may be subjected to an oxidation treatment. The oxidation treatment can adjust the proportion of polar groups on the film surface and the atomic concentration of oxygen atoms. As a result, it is easy to obtain a chemical bond with the ink, and it is easy to improve the adhesion between the printing paper and the ink. Examples of the oxidation treatment include corona discharge treatment, flame treatment, plasma treatment, glow discharge treatment, ozone treatment, etc., and these treatments can be combined. Among these, corona discharge treatment or flame treatment is preferred, and corona discharge treatment is more preferred.
[0077] As described above, the oil-based offset printing paper only needs to have a solvent blocking layer on either surface of the base layer, and may have solvent blocking layers on both surfaces of the base layer, for example. Also, when a solvent absorbing layer is provided as the oil-based offset printing paper, only needs to have a solvent blocking layer and a solvent absorbing layer in this order on either surface of the base layer, and may have a solvent blocking layer and a solvent absorbing layer in this order on both surfaces of the base layer, for example.
[0078] (oil-based offset printing) An oil-based offset print is obtained by performing oil-based offset printing on the surface of the solvent barrier layer or solvent absorbing layer side of the oil-based offset printing paper of the present invention. That is, the oil-based offset print comprises the above-mentioned base layer, the above-mentioned solvent barrier layer, and the oil-based offset printing layer in this order. In another embodiment, the oil-based offset print comprises the above-mentioned base layer, the above-mentioned solvent barrier layer, the above-mentioned solvent absorbing layer, and the oil-based offset printing layer in this order. The oil-based offset print obtained in this manner suppresses the occurrence of unevenness or curling while suppressing the decrease in interlayer (interphase) strength. Working Example
[0079] The present invention will be described in more detail below with reference to examples, comparative examples, and test examples. The materials, reagents, ratios, operations, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention is not limited to the specific examples shown below. In addition, in Table 2, "-" means that the raw material is not contained.
[0080] (Production example of polystyrene resin) <Production Example 1> Cyclohexane and styrene were added to a nitrogen-substituted stirrer and autoclave, and the temperature was raised to 70° C. with stirring. Tetramethylenediamine and sec-butyllithium were added thereto and polymerized to obtain a polystyrene resin of Production Example 1. The amount of structural units based on styrene in the polystyrene resin obtained in Production Example 1 was 100% by mass.
[0081] <Production Example 2> Cyclohexane and styrene were added to a nitrogen-substituted stirrer and autoclave, and the temperature was raised to 70°C while stirring. Tetramethylenediamine and sec-butyllithium were added to the mixture and polymerized. Butadiene was then added to the autoclave and polymerized. Thereafter, styrene was further added and polymerized to obtain a polystyrene-based resin of Production Example 2. The amount of structural units based on styrene in the polystyrene-based resin obtained in Production Example 2 was 80% by mass.
[0082] (Example of the production of copolymers of styrene monomers and olefins) <Production Example 3> Cyclohexane and styrene were added to a nitrogen-substituted stirrer and autoclave, and the temperature was raised to 70°C while stirring. Tetramethylenediamine and sec-butyllithium were added to this and polymerization was carried out. Ethylene and butadiene were further added to the autoclave and polymerization was carried out. Then, styrene was further added and polymerization was carried out to obtain a copolymer. The copolymer was dissolved in cyclohexane, and the solution was charged into an autoclave. Next, methyl t-butyl ether and nickel / silica-alumina catalyst were added, and a hydrogenation reaction was carried out under hydrogen pressure at a temperature of 180°C for 3 hours, to obtain a copolymer of a styrene-based monomer and an olefin in Production Example 3. The amount of structural units based on styrene in the copolymer obtained in Production Example 3 was 67% by mass.
[0083] Example 1 Process (I) A resin composition (1) for a base layer, which is a mixture of 80.0 parts by mass of polypropylene resin (trade name: Novatec PP MA3, manufactured by Japan Polypropylene Corporation), 19.5 parts by mass of heavy calcium carbonate particles (trade name: Softon 1800, manufactured by Bihoku Funka Kogyo Co., Ltd.), and 0.5 parts by mass of titanium dioxide particles (trade name: Typek CR-60, manufactured by Ishihara Sangyo Co., Ltd.), was melt-kneaded in an extruder set at 270 ° C. This was extruded into a sheet and cooled by a cooling roll to obtain an unstretched sheet. Next, this unstretched sheet was heated again to 150 ° C., and then stretched 4.8 times in the sheet flow direction using the speed difference between the rolls to obtain a longitudinally stretched resin film.
[0084] Process (II) A resin composition (2) for a solvent blocking layer, which was a mixture of 49.5 parts by mass of the polystyrene resin of Production Example 1, 1.0 part by mass of the copolymer of a styrene monomer and an olefin of Production Example 3, and 49.5 parts by mass of a polypropylene resin (product name: Novatec PP MA3, manufactured by Japan Polypropylene Corporation), was melt-kneaded in an extruder set at 270°C. On the other hand, a resin composition (3) for a solvent absorption layer, which is a mixture of 46 parts by mass of polypropylene resin (trade name: Novatec PP MA3, manufactured by Japan Polypropylene Corporation), 1 part by mass of maleic anhydride modified polypropylene resin (trade name: Modic P928, manufactured by Mitsubishi Chemical Corporation), 52.5 parts by mass of light calcium carbonate particles (particle size distribution D10-D90: 0.6 μm, D50: 0.5 μm) surface-treated with fatty acid, and 0.5 parts by mass of titanium dioxide particles (trade name: Typec CR-60, manufactured by Ishihara Sangyo Kaisha), was mixed with a high-speed mixer. Then, using a twin-screw kneading extruder with a cylinder temperature set to 210 ° C., the mixture was melt-kneaded at a rotation speed of 600 rpm while degassing through a vent hole. Next, these resin compositions were fed into a multi-layer die and laminated inside the die. This laminate was co-extruded from the die into a sheet, and laminated on one side of the longitudinally stretched resin film obtained in the above step (I) with the layer of resin composition (3) facing outward, to obtain a three-layer laminate sheet.
[0085] Process (III) The resulting three-layer laminate sheet was cooled to 60° C., reheated to 150° C., stretched 9 times in the sheet width direction using a tenter, and then annealed at 165° C. After that, it was cooled again to 60° C., and the edge was slit to obtain a three-layer laminate (number of stretching axes for each layer: biaxial stretching / uniaxial stretching / uniaxial stretching, total thickness: 110 μm, thickness of each layer: (1) / (2) / (3)=99 μm / 3 μm / 8 μm).
[0086] Process (IV) Using a high-frequency power supply (device name: AGF-B10, manufactured by Kasuga Electric Co., Ltd.), an aluminum electrode having a length of 0.8 m, and a silicone-coated roll as a treater roll, the gap between the electrode and the roll was set to 5 mm, and the thermoplastic resin film obtained in (IV) above was passed through the line at a processing speed of 25 m / min, with an applied energy density of 1800 J / m 2 (30W min / m 2 ) corona discharge treatment was performed on both surfaces of the film to obtain the oil-based offset printing paper of Example 1. In the oil-based offset printing paper of Example 1, the mass ratio of the copolymer of a styrene-based monomer and an olefin to the polystyrene-based resin in the solvent blocking layer was 0.02.
[0087] Process (V) The obtained oil-based offset printing paper was a white, opaque synthetic paper with numerous fine voids inside. When oil-based offset printing was performed under the printing conditions described below, no irregularities were observed on the printed film, and the ink dried well.
[0088] (Examples 2 to 5) In Example 1, when forming the three-layer laminate sheet in step (II), the resin composition (2) for the solvent blocking layer was changed to the blending amount shown in Table 2, and the same procedure as in Example 1 was carried out to obtain the oil-based offset printing papers of Examples 2 to 5. In the oil-based offset printing papers of Examples 2 to 5, the mass ratios of the copolymer of a styrene-based monomer and an olefin to the polystyrene-based resin in the solvent blocking layer were 0.02, 0.06, 0.11, 0.22, and 0.03, respectively. The obtained oil-based offset printing papers of Examples 2 to 5 were white, opaque synthetic papers having numerous minute voids inside. When oil-based offset printing was performed under the printing conditions described below, no irregularities were observed on the film after printing, and the ink dried well.
[0089] Example 6 In Example 1, when molding the three-layer laminate sheet in step (II), the same procedure as in Example 1 was carried out, except that in the resin composition (2) for the solvent blocking layer, the polystyrene-based resin of Production Example 2 was used instead of the polystyrene-based resin of Production Example 1, to obtain the oil-based offset printing paper of Example 6. In the oil-based offset printing paper of Example 6, the mass ratio of the copolymer of a styrene-based monomer and an olefin to the polystyrene-based resin in the solvent blocking layer was 0.02. The obtained oil-based offset printing paper of Example 6 was a white, opaque synthetic paper having numerous fine voids inside. When oil-based offset printing was performed under the printing conditions described below, no irregularities were observed on the film after printing, and the ink dried well.
[0090] Example 7 In step (II) of Example 1, the resin composition (3) was not used, and only the resin composition (2) was extruded from a die into a sheet shape, and laminated on one side of the longitudinally stretched resin film obtained in step (I) to obtain a two-layer laminate sheet instead of a three-layer laminate, but the same procedure as in Example 1 was carried out to obtain an oil-based offset printing paper of Example 7. That is, the oil-based offset printing paper of Example 7 is a two-layer laminate (number of stretching axes of each layer: biaxial stretching / uniaxial stretching, total thickness: 102 μm, thickness of each layer: (1) / (2)=99 μm / 3 μm). In the oil-based offset printing paper of Example 7, the mass ratio of the copolymer of a styrene-based monomer and an olefin to the polystyrene-based resin in the solvent blocking layer was 0.02. The oil-based offset printing paper obtained in Example 7 was a white, opaque synthetic paper having numerous minute voids inside. When oil-based offset printing was performed under the printing conditions described below, no irregularities were observed on the film after printing, and the ink dried well.
[0091] Example 8 The same procedure as in Example 7 was carried out to obtain the oil-based offset printing paper of Example 8, except that the stretching in step (III) in Example 7 was not performed so that a two-layer laminate of similar thickness was obtained. That is, the oil-based offset printing paper of Example 8 is a laminate with a two-layer structure (number of stretching axes in each layer: uniaxially stretched / unstretched, total thickness: 102 μm, thickness of each layer: (1) / (2)=99 μm / 3 μm). In the oil-based offset printing paper of Example 8, the mass ratio of the copolymer of a styrene-based monomer and an olefin to the polystyrene-based resin in the solvent blocking layer was 0.02. The obtained oil-based offset printing paper of Example 8 was a white, opaque synthetic paper with numerous fine voids inside. When oil-based offset printing was performed under the printing conditions described below, no irregularities were observed on the film after printing, and the ink dried well.
[0092] Example 9 In Example 1, when molding the three-layer laminate sheet in step (II), polypropylene resin (product name: Novatec PP MA3, manufactured by Japan Polypropylene Corporation) was not blended in the resin composition (2) for the solvent blocking layer, and the polystyrene-based resin in Production Example 1 and the copolymer of a styrene-based monomer and an olefin in Production Example 3 were changed to the blending amounts shown in Table 2. The same procedure as in Example 1 was carried out to obtain the oil-based offset printing paper of Example 9. In the oil-based offset printing paper of Example 9, the mass ratio of the copolymer of a styrene-based monomer and an olefin to the polystyrene-based resin in the solvent blocking layer was 0.25. The obtained oil-based offset printing paper of Example 9 was a white, opaque synthetic paper having numerous fine voids inside. When oil-based offset printing was performed under the printing conditions described below, no irregularities were observed on the printed film, and the ink dried well.
[0093] Comparative Example 1 In Example 1, when molding the three-layer laminate sheet in step (II), the resin composition (2) for the solvent blocking layer was not blended with the copolymer of styrene-based monomer and olefin of Production Example 3, and the polystyrene-based resin and polypropylene resin (product name: Novatec PP MA3, manufactured by Japan Polypropylene Corporation) of Production Example 1 were changed to the blending amounts shown in Table 2. The same procedure as in Example 1 was carried out to obtain the oil-based offset printing paper of Comparative Example 1. When the obtained oil-based offset printing paper was subjected to oil-based offset printing under the printing conditions described below, large irregularities were generated on the film.
[0094] Comparative Example 2 In Example 1, when molding a three-layer laminate sheet in step (II), the polystyrene resin of Production Example 1 was not blended in the resin composition (2) for the solvent blocking layer, and the copolymer of a styrene monomer and an olefin of Production Example 3 and the polypropylene resin (product name: Novatec PP MA3, manufactured by Japan Polypropylene Corporation) were changed to the blending amounts shown in Table 2. The same procedure as in Example 1 was carried out to obtain the oil-based offset printing paper of Comparative Example 1. When the obtained oil-based offset printing paper was subjected to oil-based offset printing under the printing conditions described below, large irregularities were generated on the film.
[0095] (Measurement conditions and evaluation methods) <Thickness> The overall thickness (μm) of the oil-based offset printing paper was measured using a constant pressure thickness gauge (device name: PG-01J, manufactured by Tecrock Corporation) based on JIS K7130:1999 "Plastics - Films and sheets - Thickness measurement method". In addition, the thickness (μm) of the solvent absorption layer, the thickness (μm) of the solvent blocking layer, and the thickness (μm) of the base layer in oil-based offset printing paper were determined by cooling the oil-based offset printing paper to a temperature of -60°C or lower with liquid nitrogen, placing a razor blade (product name: Proline Blade, manufactured by Schick Japan) at a right angle against the sample placed on a glass plate and cutting it to prepare a sample for cross-sectional measurement, and observing the cross-section of the obtained sample with a scanning electron microscope (instrument name: JSM-6490, manufactured by JEOL Ltd.) to determine the boundary lines of each layer from the appearance of the composition, and multiplying the total thickness by the observed layer thickness ratio.
[0096] <Porosity> The porosity of the solvent blocking layer and the solvent absorbing layer was determined from the ratio of the area occupied by pores in a certain region of the solvent blocking layer or the solvent absorbing layer in any cross section of the oil-based offset printing paper observed under an electron microscope. Specifically, an arbitrary part of the oil-based offset printing paper to be measured was cut out, embedded in epoxy resin and solidified, and then cut perpendicularly to the surface direction of the oil-based offset printing paper to be measured using a microtome, and the cut surface was attached to an observation sample stage so that it became the observation surface. Gold or gold-palladium, etc. was evaporated on the observation surface, and the cut surface of the oil-based offset printing paper was observed at an arbitrary magnification (for example, 500 times to 3000 times magnification) that is easy to observe with a scanning electron microscope, and the observed area was captured as image data. The obtained image data was processed by an image analyzer to determine the area ratio (%) of the void portion in a certain area of the solvent blocking layer or the solvent absorbing layer, and the porosity (%) was obtained. In this way, the measured values in the observation of 10 or more arbitrary points were averaged to obtain the porosity of the solvent blocking layer and the solvent absorbing layer.
[0097] <Unevenness or curl> Oil-based offset printing paper was cut into a piece of 50 mm x 20 mm to prepare a sample for measuring waviness. 180 μl of a high boiling point petroleum solvent (oil: Solvent AF6) was dropped onto this sample, and the dropped solvent was then spread evenly over the sample to coat it. The sample to which the solvent was applied was stored for one week in an atmosphere with a temperature of 23°C and a relative humidity of 50%. The waviness level of the sample was visually observed. Based on the waviness level, the unevenness or curl was evaluated according to the following criteria. The results are shown in Table 2. 5 (Best): The paper has no waviness. 4 (Good): Very slight waviness on the paper surface 3 (OK): The paper surface is slightly wavy, but not problematic for practical use. 2 (Fail): The paper surface is wavy and needs improvement. 1 (Not acceptable): The paper surface is wavy, and the defect level is severe.
[0098] <Interlaminar strength> The oil-based offset printing paper of the examples and comparative examples was stored for one day under an atmosphere of 23°C temperature and 50% relative humidity. Then, cellophane tape (manufactured by Nichiban Co., Ltd., product name: Cellotape (registered trademark) CT-18) was attached to the surface of the base layer side. Next, according to TAPPI-UM403, it was measured with an internal bond tester (manufactured by Kumagai Riki Kogyo Co., Ltd.), and the average value of the five measurement results was taken as the surface strength. In addition, after the measurement, the oil-based offset printing paper was visually observed to see whether interlayer peeling and interlayer cohesive failure were observed. Based on the surface strength and peeling mode, the interlayer strength was judged according to the following evaluation criteria. The results are shown in Table 2. 5 (best): Surface strength is 2.0 kg / cm or more, and no interlayer peeling or intralayer cohesive failure is observed. 4 (Good): Surface strength is 1.5 kg / cm or more and less than 2.0 kg / cm, and no interlayer peeling or intralayer cohesive failure is observed. 3 (Acceptable): Surface strength is 1.0 kg / cm or more and less than 1.5 kg / cm, and no interlayer delamination or intralayer cohesive failure is observed. 2 (Unacceptable): Surface strength is 1.0 kg / cm or more and less than 1.5 kg / cm, and interlayer peeling or intralayer cohesive failure is observed. 1 (Fail): Surface strength is less than 1.0 kg / cm, and delamination or intralayer cohesive failure is observed.
[0099] [Table 2]
[0100] It was found that the oil-based offset printing papers of Examples 1 to 9 could prevent the occurrence of unevenness or curling when used as printing papers in offset printing, and had excellent interlayer strength.
[0101] On the other hand, the oil-based offset printing paper of Comparative Example 1, which does not contain a copolymer of a styrene monomer and an olefin in the solvent barrier layer, is able to prevent the occurrence of unevenness or curling, but has low interlayer strength. Also, the oil-based offset printing paper of Comparative Example 2, which does not contain a polystyrene resin in the solvent barrier layer, has good interlayer strength but is unable to prevent the occurrence of unevenness or curling. [Industrial Applicability]
[0102] The oil-based offset printing paper of the present invention can suppress the occurrence of unevenness or curling caused by the vehicle in the offset ink during offset printing, while suppressing the decrease in interlayer (interphase) strength, making it extremely useful as a material for poster paper, wrapping paper, labels, etc. [Explanation of symbols]
[0103] 100···Oil-based offset printing paper, 10···Solvent blocking layer, 20···Base layer, 30···Solvent absorbing layer
Claims
1. A base layer containing a polyolefin resin; a solvent blocking layer including a polystyrene-based resin and a copolymer of a styrene-based monomer and an olefin; Equipped with The amount of structural units based on styrene in the polystyrene-based resin is 70% by mass or more, The amount of structural units based on styrene in the copolymer is 20% by mass or more and less than 70% by mass, The amount of structural units based on olefin in the copolymer is 20% by mass or more and 50% by mass or less. Oil-based offset printing paper.
2. 2. The oil-based offset printing paper according to claim 1, wherein a mass ratio of said copolymer to said polystyrene resin is 0.01 to 0.
30.
3. The oil-based offset printing paper according to claim 1 or 2, wherein the solvent barrier layer further comprises a polyolefin resin.
4. 4. The oil-based offset printing paper according to claim 1, wherein the solvent barrier layer is stretched in at least one direction.
5. 5. The oil-based offset printing paper according to claim 1, wherein the olefin in the copolymer contains at least one linear olefin selected from the group consisting of ethylene, propylene, butylene, butadiene and isoprene.
6. The oil-based offset printing paper according to any one of claims 1 to 5, further comprising a solvent absorbing layer on the solvent barrier layer.
Citation Information
Patent Citations
Thermoplastic film with excellent printability
JP1995216117A
Multilayered resin stretched film
JP2002036470A
Resin composition and its use
JP2003138079A
Film, synthetic paper and label
JP2003138080A
Recording sheet
JP2003291521A