Support sheet, composite sheet for forming resin film, kit, and method for producing chip with resin film

The support sheet addresses sheet loosening issues during resin film formation by maintaining chip position stability, improving chip recognition in the manufacturing process.

JP7591453B2Active Publication Date: 2024-11-28LINTEC CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021062255
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-31
Publication Date
2024-11-28
Estimated Expiration
2041-03-31

AI Technical Summary

Technical Problem

Conventional composite sheets for resin film formation experience issues with sheet loosening due to heating and cooling, leading to poor recognition of chips during the pickup process, especially with larger semiconductor wafers and smaller chip sizes.

Method used

A support sheet with specific thermomechanical properties, including displacement limits and average displacement values, is used to minimize sheet loosening and improve chip recognition during the manufacturing process.

Benefits of technology

The support sheet effectively reduces the influence of heating and cooling-induced slack, enhancing the recognition of chips by the pickup device, even with larger workpieces and smaller chips.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591453000002
    Figure 0007591453000002
  • Figure 0007591453000003
    Figure 0007591453000003
  • Figure 0007591453000004
    Figure 0007591453000004
Patent Text Reader

Abstract

To provide a support sheet capable of eliminating the influence of slackness of a manufacturing processing sheet due to heating and cooling and improving the recognition of a chip of a pickup device, a composite sheet for resin film formation and a kit including the support sheet and a resin film forming layer, and a manufacturing method of a chip with a resin film.SOLUTION: A support sheet (10) is used for heating a workpiece or chips obtained by dividing the workpiece. In the support sheet (10), when a support sheet (10) having a sample size: 20 mm long and 5 mm wide is subjected to a thermo-mechanical analysis (TMA) in a tensile mode in either a machine direction (MD) or perpendicular direction (CD), an amount of displacement (A130) at 130°C is 500 μm or less, and an average displacement (A23→130) per 1°C when the temperature is raised from 23°C to 130°C is smaller than an absolute value (|B130→50|) of an average displacement amount per 1°C at slow cooling from 130°C to 50°C.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a support sheet, a composite sheet and kit for resin film formation that include the support sheet and a resin film forming layer, and a method for producing a chip with a resin film. [Background technology]

[0002] Some workpieces, such as semiconductor wafers, insulator wafers, and semiconductor device panels, have circuits formed on one surface (circuit surface) and further have protruding electrodes such as bumps on that surface (circuit surface). The workpieces are attached to a support sheet (e.g., a dicing sheet) to obtain a laminate. The laminate is heated and then cooled with the peripheral portion of the support sheet attached to a fixing jig such as a ring frame. The workpieces attached to the support sheet are divided to obtain chips. The chips are then sometimes picked up from the support sheet (see Patent Document 1).

[0003] In a manufacturing process of a semiconductor device using a mounting method called the face-down method, a protective film-forming film is used to protect the back surface of a chip formed by dicing the workpiece, and a protective film-forming composite sheet in which a protective film-forming film and a support sheet are combined is used. Also, a film-like adhesive is used to bond the back surface of the chip to a lead frame or an organic substrate, and a dicing die bonding sheet in which a film-like adhesive and a support sheet are combined is also used when dicing the workpiece. The protective film-forming film and the film-like adhesive are attached to the back surface of the workpiece.

[0004] Hereinafter, in this specification, the protective film-forming film or the film-like adhesive is referred to as a resin film-forming layer, and the composite sheet for protective film formation or the dicing die bonding sheet is referred to as a composite sheet for resin film formation. The protective film formed by the protective film-forming film or the bonding film formed by the film-like adhesive is referred to as a resin film.

[0005] In the manufacturing process of a chip with a resin film, a resin film forming layer for forming a protective film or a bonding film is attached to the back surface of a workpiece. The resin film forming layer may be attached to the back surface of the workpiece in the form of a composite sheet for resin film formation in which the resin film forming layer is laminated on a support sheet. The resin film forming layer may be attached to the back surface of the workpiece without being laminated on a support sheet, and then attached to the support sheet.

[0006] The resin film forming layer attached to the back surface of the workpiece is thermally cured on the support sheet as necessary to form a resin film. When the resin film forming layer attached to the back surface of the workpiece is thermally cured on the support sheet, a first laminated composite sheet, which is composed of the support sheet, the resin film forming layer, and the workpiece stacked in this order in the thickness direction, is heated and then cooled with the peripheral portion of the sheet attached to a ring frame. Thereafter, in a dicing process on the support sheet, the workpiece is divided, the resin film is cut, and the chips with the resin film are picked up (see Patent Document 2).

[0007] Alternatively, the resin film forming layer attached to the back surface of the workpiece is subjected to a dicing process on the support sheet, in which the workpiece is divided and the resin film is cut to form chips with the resin film forming layer, and then the resin film forming layer is thermally cured on the support sheet to form the chips with the resin film. When the resin film forming layer attached to the back surface of the chip is thermally cured on the support sheet, a fourth laminated composite sheet, which is composed of the support sheet, the resin film forming layer, and the chip stacked in this order in the thickness direction, is heated and cooled with the peripheral portion of the sheet attached to the ring frame. Then, the chips with the resin film are picked up. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] International Publication No. 2015 / 190230 [Patent Document 2] International Publication No. 2015 / 178346 Summary of the Invention [Problem to be solved by the invention]

[0009] For example, the semiconductor wafer described in Patent Documents 1 and 2 has a diameter of 8 inches, a thickness of 100 μm, and a mass of approximately 7.4 g. It is described that the semiconductor wafer is diced into chips having a chip size of 9 mm×9 mm.

[0010] In the manufacturing process of resin-coated chips, semiconductor wafers with larger diameters are used and the number and size of protruding electrodes on the semiconductor wafers are increasing, so that the load on the support sheet, the peripheral edge of which is supported by a ring frame, tends to become greater and, conversely, the chip size tends to become smaller.

[0011] When a conventional resin film-forming composite sheet or a support sheet is used, when the manufacturing processing sheet such as the first laminated composite sheet or the fourth laminated composite sheet is heated with the peripheral portion of the manufacturing processing sheet attached to a ring frame, the manufacturing processing sheet may slacken due to the load of a work such as a semiconductor wafer or the load of multiple chips, causing the position of the resin film-coated chip to shift. In addition, during the dicing process after the manufacturing processing sheet is heated, the position of the resin film-coated chip may shift. As a result, when the chip size is smaller, the problem of poor recognition of the resin film-coated chip during pick-up may occur.

[0012] The present invention aims to provide a support sheet that can eliminate the effects of sagging of manufacturing processing sheets due to heating and cooling and improve the recognition of chips by a pick-up device, a composite sheet and kit for resin film formation that includes the support sheet and a resin film forming layer, and a method for manufacturing chips with a resin film. [Means for solving the problem]

[0013] The present invention provides the following support sheet, composite sheet and kit for forming a resin film, and method for producing a chip with a resin film.

[0014] [1] A support sheet used for heating a workpiece or a chip obtained by dividing a workpiece, When the support sheet was subjected to thermomechanical analysis (TMA) in tensile mode in either the machine direction (MD) or the cross direction (CD) under the following conditions, Displacement at 130℃ (A 130 ) is 500 μm or less, Average displacement per degree when the temperature is increased from 23°C to 130°C (A 23→130 ) is the absolute value of the average displacement per degree Celsius when slowly cooled from 130°C to 50°C (|B 130→50 |) smaller than the support sheet.

[0015] <Thermo-mechanical analysis (TMA) conditions> Sample size: length 20mm, width 5mm Chuck spacing: 15mm The temperature is raised from 23°C to 130°C with a load of 0.8g and a heating rate of 10°C / min, and held for 30 minutes.Then, the temperature is cooled from 130°C to 50°C with a load of 0.8g and a cooling rate of 1°C / min.The displacement [μm] during this period is measured.

[0016] [2] When the support sheet was subjected to thermomechanical analysis (TMA) in a tensile mode in the machine direction (MD) and a tensile mode in the transverse direction (CD) under the above conditions, Displacement at 130℃ (A 130 ) are all 500 μm or less, Average displacement per degree when the temperature is increased from 23°C to 130°C (A 23→130 ) is the absolute value of the average displacement per degree Celsius when slowly cooled from 130°C to 50°C (|B 130→50 |), both of which are smaller than the support sheet described in [1].

[0017] [3] When the support sheet is subjected to thermomechanical analysis (TMA) in a tensile mode in either the machine direction (MD) or the cross direction (CD) under the above conditions, Average displacement per degree when the temperature is increased from 23°C to 130°C (A 23→130) is a positive value. [4] When the support sheet is subjected to thermomechanical analysis (TMA) in a tensile mode in the machine direction (MD) and a tensile mode in the transverse direction (CD) under the above conditions, Average displacement per degree when the temperature is increased from 23°C to 130°C (A 23→130 ) are all positive values.

[0018] [5] When the support sheet is subjected to thermomechanical analysis (TMA) in a tensile mode in either the machine direction (MD) or the cross direction (CD) under the above conditions, Average displacement per degree when the temperature is increased from 23°C to 130°C (A 23→130 ) for the average displacement per degree Celsius when the temperature is increased from 60°C to 130°C (A 60→130 The support sheet according to [3] or [4], wherein the ratio of the above is less than 1. [6] When the support sheet was subjected to thermomechanical analysis (TMA) in a tensile mode in the machine direction (MD) and a tensile mode in the transverse direction (CD) under the above conditions, Average displacement per degree when the temperature is increased from 23°C to 130°C (A 23→130 ) for the average displacement per degree Celsius when the temperature is increased from 60°C to 130°C (A 60→130 ) are all less than 1.

[0019] [7] The support sheet described in any one of [1] to [6], wherein the support sheet consists of only a substrate, or comprises a substrate and a pressure-sensitive adhesive layer provided on one side of the substrate, and the constituent material of the substrate contains a polyolefin resin. [8] The support sheet described in any one of [1] to [7], wherein the support sheet consists of only a substrate, or comprises a substrate and a pressure-sensitive adhesive layer provided on one side of the substrate, and the substrate is a stretched film. [9] The support sheet according to any one of [1] to [8], wherein the support sheet is in a roll form.

[0020]

[10] A composite sheet for resin film formation, comprising: a support sheet according to any one of [1] to [8]; and a resin film forming layer provided on one surface of the support sheet.

[11] The composite sheet for resin film formation described in

[10] , wherein the resin film forming layer is a protective film forming film.

[12] The composite sheet for resin film formation described in

[10] or

[11] , wherein the composite sheet for resin film formation is in a roll form.

[0021]

[13] A kit comprising a first laminate in which a first release film, a resin film forming layer and a second release film are laminated in this order, and a support sheet described in any one of [1] to [9], which is used to support a workpiece to which the resin film forming layer is to be attached and the resin film forming layer.

[14] The kit described in

[13] , wherein the resin film forming layer is a protective film forming film.

[15] The kit described in

[13] or

[14] , wherein the first laminate is in a roll form.

[0022]

[16] A method for manufacturing a resin-film-coated chip comprising: a chip; and a resin film provided on a back surface of the chip, the method comprising: A process of attaching a resin film forming layer in a composite sheet for resin film formation described in any one of

[10] to

[12] to the back surface of a workpiece, or attaching a resin film forming layer in a kit described in any one of

[13] to

[15] to the back surface of a workpiece, thereby producing a first laminated film in which the resin film forming layer and the workpiece are laminated in their thickness direction, and further attaching a support sheet in the kit to the resin film forming layer in the first laminated film, thereby producing a first laminated composite sheet in which the resin film forming layer and the workpiece are laminated in this order in their thickness direction on the support sheet; a step of heating the first laminated composite sheet while the peripheral portion of the first laminated composite sheet is attached to a fixing jig, hardening the resin film forming layer, and forming the resin film, thereby producing a second laminated composite sheet in which the resin film and the work are laminated in this order in the thickness direction on the support sheet; cooling the second laminated composite sheet, and then dividing the work in the second laminated composite sheet on the support sheet and cutting the resin film to produce a third laminated composite sheet in which a plurality of chips with a resin film are fixed on the support sheet; and picking up the resin-film-coated chip in the third laminated composite sheet by separating it from the support sheet.

[0023]

[17] A method for manufacturing a resin-film-coated chip comprising: a chip; and a resin film provided on a back surface of the chip, the method comprising: A process of attaching a resin film forming layer in a composite sheet for resin film formation described in any one of

[10] to

[12] to the back surface of a workpiece, or attaching a resin film forming layer in a kit described in any one of

[13] to

[15] to the back surface of a workpiece, thereby producing a first laminated film in which the resin film forming layer and the workpiece are laminated in their thickness direction, and further attaching a support sheet in the kit to the resin film forming layer in the first laminated film, thereby producing a first laminated composite sheet in which the resin film forming layer and the workpiece are laminated in this order in their thickness direction on the support sheet; A step of dividing the work in the first laminated composite sheet on the support sheet and cutting the resin film forming layer to produce a fourth laminated composite sheet in which a plurality of chips with a resin film forming layer are fixed on the support sheet; a step of heating and cooling the fourth laminated composite sheet while the peripheral portion of the fourth laminated composite sheet is attached to a fixing jig, thereby hardening the resin film forming layer in the fourth laminated composite sheet and forming the resin film, thereby producing a third laminated composite sheet on the support sheet in which a plurality of resin film-coated chips are fixed on the support sheet; and picking up the resin-film-coated chip in the third laminated composite sheet by separating it from the support sheet. Effect of the Invention

[0024] According to the present invention, there is provided a support sheet that can eliminate the effects of sagging of the manufacturing processing sheet due to heating and cooling and prevent the pickup device from failing to recognize the chip, a composite sheet and kit for resin film formation that includes the support sheet and a resin film forming layer, and a method for manufacturing chips with a resin film. [Brief description of the drawings]

[0025] [Figure 1] FIG. 1 is a cross-sectional view illustrating an example of a support sheet according to an embodiment of the present invention. [Diagram 2] FIG. 1 is a cross-sectional view showing a schematic example of a composite sheet for resin film formation according to an embodiment of the present invention. [Diagram 3] FIG. 2 is a cross-sectional view showing a schematic diagram of another example of the composite sheet for resin film formation according to the embodiment of the present invention. [Figure 4] FIG. 2 is a cross-sectional view showing a schematic diagram of still another example of the composite sheet for resin film formation according to an embodiment of the present invention. [Diagram 5] FIG. 2 is a cross-sectional view showing a schematic diagram of still another example of the composite sheet for resin film formation according to an embodiment of the present invention. [Figure 6] FIG. 1 is a cross-sectional view showing a schematic example of a kit according to an embodiment of the present invention. [Figure 7A] 1A to 1C are cross-sectional views for illustrating a schematic view of a part of an example of a method for manufacturing a resin-film-coated chip according to an embodiment of the present invention. [Figure 7B]1A to 1C are cross-sectional views for illustrating a schematic view of a part of an example of a method for manufacturing a resin-film-coated chip according to an embodiment of the present invention. [Figure 7C] 1A to 1C are cross-sectional views for illustrating a schematic view of a part of an example of a method for manufacturing a resin-film-coated chip according to an embodiment of the present invention. [Figure 7D] 1A to 1C are cross-sectional views for illustrating a schematic view of a part of an example of a method for manufacturing a resin-film-coated chip according to an embodiment of the present invention. [Figure 7E] 1A to 1C are cross-sectional views for illustrating a schematic view of a part of an example of a method for manufacturing a resin-film-coated chip according to an embodiment of the present invention. [Figure 8] 10A to 10C are cross-sectional views for illustrating a schematic view of a part of another example of a method for manufacturing a resin-film-coated chip according to an embodiment of the present invention. [Figure 9A] 10A to 10C are cross-sectional views for illustrating a schematic view of a part of another example of a method for manufacturing a resin-film-coated chip according to an embodiment of the present invention. [Figure 9B] 10A to 10C are cross-sectional views for illustrating a schematic view of a part of another example of a method for manufacturing a resin-film-coated chip according to an embodiment of the present invention. [Figure 9C] 10A to 10C are cross-sectional views for illustrating a schematic view of a part of another example of a method for manufacturing a resin-film-coated chip according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] <<Support sheet>> The support sheet according to an embodiment of the present invention is a support sheet used for heating a workpiece or a chip obtained by dividing a workpiece, When the support sheet was subjected to thermomechanical analysis (TMA) in tensile mode in either the machine direction (MD) or the cross direction (CD) under the following conditions, Displacement at 130℃ (A 130 ) is 500 μm or less, Average displacement per degree when the temperature is increased from 23°C to 130°C (A 23→130 ) is the absolute value of the average displacement per degree Celsius when slowly cooled from 130°C to 50°C (|B 130→50 Less than |).

[0027] <Thermo-mechanical analysis (TMA) conditions> Sample size: length 20mm, width 5mm Chuck spacing: 15mm The temperature is raised from 23°C to 130°C with a load of 0.8g and a heating rate of 10°C / min, and held for 30 minutes.Then, the temperature is cooled from 130°C to 50°C with a load of 0.8g and a cooling rate of 1°C / min.The displacement [μm] during this period is measured.

[0028] When the amount of displacement in the thermomechanical analysis (TMA) is a positive value, it means that the support sheet has expanded, and when the amount of displacement is a negative value, it means that the support sheet has contracted.

[0029] The support sheet according to this embodiment has a displacement (A 130 ) is 500 μm or less. Here, the displacement (A 130 ) was measured when the temperature was raised from 23°C to 130°C and reached 130°C. Displacement at 130℃ (A 130 By keeping the thickness of the support sheet at 500 μm or less, the slack of the support sheet during heating can be reduced. 130 The displacement (A) at 130° C. is preferably 450 μm or less, more preferably 400 μm or less, and even more preferably 360 μm or less. 130 ) is preferably greater than -50 μm, more preferably greater than 0 μm, even more preferably greater than 21 μm, even more preferably greater than 43 μm, and particularly preferably greater than 64 μm.

[0030] For example, the displacement amount (A 130In the case of a support sheet that has a negative value and has the property of shrinking significantly, the adhesive strength between the jig and the fixing jig, such as the adhesive layer for the jig, weakens at high temperatures, and the weight of the workpiece may cause the support sheet to peel off and fall off from the fixing jig. However, at low temperatures, the adhesive strength between the jig and the fixing jig, such as the adhesive layer for the jig, is restored, so the absolute value of the average displacement per degree Celsius when slowly cooled from 130°C to 50°C (|B 130→50 |) can be large. Therefore, the average displacement (A) per degree Celsius when the temperature is increased from 23°C to 130°C 23→130 ) is the absolute value of the average displacement per degree Celsius when slowly cooled from 130°C to 50°C (|B 130→50 |) is preferable.

[0031] Here, the average displacement per degree Celsius when the temperature is increased from 23°C to 130°C (A 23→130 ) can be calculated using the following formula: A 23→130 =(A 130 -A 23 ) / 107=A 130 / 107[μm / ℃]

[0032] Displacement at 23°C (A 23 )=0μm Displacement at 130℃ (A 130 ) [μm]

[0033] Here, the average displacement per degree Celsius when slowly cooling from 130°C to 50°C (B 130→50 ) can be calculated using the following formula: B 130→50 =(B 50 -B 130 ) / 80[μm / ℃] In addition, since it is not expected that the support sheet will expand when cooled slowly, B 130→50 is a negative value.

[0034] Here, the absolute value of the average displacement per degree Celsius when slowly cooling from 130°C to 50°C (|B 130→50 |) can be calculated using the following formula: |B 130→50|=|B 50 -B 130 | / 80[μm / ℃]

[0035] Displacement after holding at 130℃ for 30 minutes (B 130 ) [μm] Displacement at 50℃ after slow cooling (B 50 ) [μm]

[0036] The average displacement (A 23→130 ) is the absolute value of the average displacement (|B 130→50 By making the distance smaller than the distance (|), the change in position of the chip on the support sheet due to heating and cooling can be reduced, and the pick-up device can eliminate the failure to recognize the chip.

[0037] When the support sheet is subjected to a thermomechanical analysis (TMA) in a tensile mode in either the machine direction (MD) or the cross direction (CD) under the following conditions, the average displacement (A 23→130 ) from the absolute value of the average displacement (|B 130→50 |) minus [(A 23→130 )-|B 130→50 |] is a negative value, and is preferably -0.10 to -5 µm / °C, more preferably -0.40 to -4 µm / °C, and further preferably -0.75 to -3 µm / °C.

[0038] When the temperature is increased to 130°C and the support sheet is held in a constant state without any temperature change, the support sheet slowly expands due to the same load (load of the workpiece) being applied to the base material of the support sheet for a long time. This is due to the average displacement (A 23→130 ) to the absolute value of the average displacement (|B 130→50 |) minus [(A 23→130 )-|B 130→50|] is important. This is because when the first laminated composite sheet or the fourth laminated composite sheet is actually held at 130°C, the resin film forming layer, the adhesive layer, and the jig adhesive layer in the first laminated composite sheet or the fourth laminated composite sheet have viscosity at high temperatures, so the phenomenon in which the support sheet slowly stretches is unlikely to affect slackening because stress is relaxed in the entire first laminated composite sheet or the fourth laminated composite sheet.

[0039] Here, "in the flow direction (MD) [(A 23→130 )-|B 130→50 |] value in the vertical direction (CD) 23→130 )-|B 130→50 The absolute value of the value obtained by subtracting the "value of |" from the "MD and CD balance evaluation value" can be obtained. The balance evaluation value of MD and CD is preferably 3.0 or less, more preferably 2.5 or less, even more preferably 2.0 or less, and particularly preferably 1.8 or less. When the balance evaluation value of MD and CD is greater than the upper limit, in a situation where the shrinkage behavior of the support sheet is restricted by a fixing jig such as a ring frame, a force that tends to excessively shrink only in one direction, either MD or CD, occurs in the support sheet after heating and cooling, and wrinkles (a wavy shape of the support sheet) are likely to form in the support sheet near the fixing jig. When the wrinkles are formed, a force is generated in the direction in which the support sheet or the composite sheet for resin film formation peels off the fixing jig (i.e., in a direction perpendicular to the plane of the fixing jig such as a ring frame), so that the support sheet or the composite sheet for resin film formation peels off the fixing jig and there is an increased risk of it falling off starting from this peeling point. However, it is considered that this risk can be further reduced by having the balance evaluation value of MD and CD be equal to or less than the upper limit.

[0040] When the support sheet is subjected to thermomechanical analysis (TMA) under the above conditions in a tensile mode in either the machine direction (MD) or the cross direction (CD), the above requirements need to be met.

[0041] When the support sheet is subjected to thermomechanical analysis (TMA) under the above conditions in a tensile mode in the machine direction (MD) and a tensile mode in the cross direction (CD), it is preferable that both of the above requirements are satisfied.

[0042] That is, when the support sheet was subjected to a thermomechanical analysis (TMA) in a tensile mode in the machine direction (MD) under the above conditions, the displacement (A 130 ) is 500μm or less, and when thermal mechanical analysis (TMA) is performed in the tensile mode in the perpendicular direction (CD), the displacement (A 130 ) is preferably 500 μm or less. When the support sheet is subjected to a thermomechanical analysis (TMA) in a tensile mode in the machine direction (MD) under the above conditions, the average displacement (A 23→130 ) is the absolute value of the average displacement (|B 130→50 |) and when subjected to thermomechanical analysis (TMA) in the tensile mode in the transverse direction (CD), the average displacement (A 23→130 ) is the absolute value of the average displacement (|B 130→50 |) is preferable.

[0043] Typically, the machine direction (MD) of a support sheet refers to the direction in which the resin flows when the support sheet is molded. The cross direction (CD) of a support sheet refers to the direction perpendicular to the machine direction (MD) of the support sheet. When the support sheet is in roll form, the machine direction (MD) is the long direction of the support sheet, and the cross direction (CD) of the support sheet is the cross direction of the support sheet, regardless of whether the support sheet is stretched or not. Even when the support sheet is in the form of a single sheet, the flow directions of the resin can be distinguished from one another by optical analysis, such as analysis of two-dimensional X-ray diffraction images.

[0044] When the support sheet comprises a substrate and an adhesive layer, the amount of displacement when the support sheet is subjected to thermomechanical analysis (TMA) is greatly influenced by the characteristics of the substrate, and therefore the machine direction (MD) of the support sheet is the machine direction (MD) of the substrate, and the vertical direction (CD) of the support sheet is the vertical direction (CD) of the substrate.

[0045] When the support sheet of this embodiment is subjected to a thermomechanical analysis (TMA) in a tensile mode in either the machine direction (MD) or the perpendicular direction (CD) under the above conditions, the average displacement (A) per degree Celsius when the temperature is increased from 23° C. to 130° C. 23→130 ) is preferably a positive value. The adhesive strength with the fixing jig is weak at high temperatures. 23→130 If the average displacement (A) is a negative value, the support sheet will shrink, and the weight of the workpiece or chip at high temperatures may cause the support sheet to peel off from the fixing jig and fall off. 23→130 ) is a positive value, it is possible to eliminate the risk of the support sheet peeling off and falling off the fixing jig.

[0046] Here, the average displacement per degree Celsius when the temperature is increased from 23°C to 130°C (A 23→130 ) is represented by the formula (A 23→130 =A 130 / 107[μm / ℃]).

[0047] The average displacement (A 23→130 ) is more preferably 0.20 μm / ° C. or more, even more preferably 0.40 μm / ° C. or more, and particularly preferably 0.60 μm / ° C. or more.

[0048] When the support sheet is subjected to a thermomechanical analysis (TMA) in a tensile mode in either the machine direction (MD) or the perpendicular direction (CD) under the above conditions, the average displacement (A 23→130 ) should be a positive value.

[0049] When the support sheet is subjected to a thermomechanical analysis (TMA) in a tensile mode in the machine direction (MD) and a tensile mode in the perpendicular direction (CD) under the above conditions, the average displacement (A 23→130 ) are preferably positive values.

[0050] When the support sheet is subjected to a thermomechanical analysis (TMA) in a tensile mode in the machine direction (MD) and a tensile mode in the perpendicular direction (CD) under the above conditions, the average displacement (A 23→130) is more preferably 0.20 μm / ° C. or more, further preferably 0.40 μm / ° C. or more, and particularly preferably 0.60 μm / ° C. or more.

[0051] When the support sheet was subjected to thermomechanical analysis (TMA) in a tensile mode in either the machine direction (MD) or the perpendicular direction (CD) under the above conditions, the average displacement (A) per degree Celsius when the temperature was increased from 23°C to 130°C was 23→130 ) for the average displacement per degree Celsius when the temperature is increased from 60°C to 130°C (A 60→130 ) is preferably less than 1. After 60° C. during the temperature rise, the support sheet tends to become flexible as a material. The average displacement (A 23→130 ) to the average displacement (A 60→130 ) is less than 1, the elongation behavior of the support sheet is suppressed after the temperature rise reaches 60° C., and sagging after final cooling is likely to be suppressed.

[0052] Average displacement per degree when the temperature is increased from 23°C to 130°C (A 23→130 ) can be calculated using the following formula: A 23→130 =(A 130 -A 23 ) / 107=A 130 / 107[μm / ℃]

[0053] Displacement at 23°C (A 23 )=0μm Displacement at 130℃ (A 130 ) [μm]

[0054] Here, the average displacement per degree Celsius when the temperature is increased from 60°C to 130°C (A 60→130 ) can be calculated using the following formula: A 60→130 =(A 130 -A 60 ) / 70[μm / ℃]

[0055] Displacement at 60°C (A60 ) [μm] Displacement at 130℃ (A 130 ) [μm]

[0056] Therefore, the average displacement per degree Celsius when the temperature is increased from 23°C to 130°C (A 23→130 ) for the average displacement per degree Celsius when the temperature is increased from 60°C to 130°C (A 60→130 ) ratio [(A 60→130 ) / (A 23→130 )] can be calculated from these formulas.

[0057] The average displacement (A 23→130 ) to the average displacement (A 60→130 ) ratio [(A 60→130 ) / (A 23→130 The average displacement (A 23→130 ) to the average displacement (A 60→130 ) ratio [(A 60→130 ) / (A 23→130 )] is preferably 0.10 or more, more preferably 0.20 or more, even more preferably 0.30 or more, and particularly preferably 0.90 or more.

[0058] When the temperature is increased to 130°C and the support sheet is held in a constant state without any temperature change, the support sheet slowly expands due to the same load (load of the workpiece) being applied to the base material of the support sheet for a long time. This is due to the average displacement (A 23→130 ) to the average displacement (A 60→130 ) ratio [(A 60→130 ) / (A 23→130)] is important. This is because when the first laminated composite sheet or the fourth laminated composite sheet is actually held at 130°C, the resin film forming layer, the adhesive layer, and the jig adhesive layer in the first laminated composite sheet or the fourth laminated composite sheet have viscosity at high temperatures, so the phenomenon in which the support sheet slowly stretches is less likely to affect slackening because stress is relaxed in the entire first laminated composite sheet or the fourth laminated composite sheet.

[0059] When the support sheet is subjected to a thermomechanical analysis (TMA) in a tensile mode in the machine direction (MD) and a tensile mode in the perpendicular direction (CD) under the above conditions, the average displacement (A 23→130 ) to the average displacement (A 60→130 ) is preferably less than 1.

[0060] When the support sheet is subjected to a thermomechanical analysis (TMA) in a tensile mode in the machine direction (MD) and a tensile mode in the perpendicular direction (CD) under the above conditions, the average displacement (A 23→130 ) to the average displacement (A 60→130 ) ratio [(A 60→130 ) / (A 23→130 Each of the average displacements (A 23→130 ) to the average displacement (A 60→130 ) ratio [(A 60→130 ) / (A 23→130 )] are preferably all 0.10 or more, more preferably all 0.20 or more, and even more preferably all 0.30 or more.

[0061] The support sheet of this embodiment can be suitably used in a method for manufacturing a resin film-coated chip, in which a resin film forming layer is attached to the back surface of a workpiece, and a first laminated composite sheet is formed by stacking the resin film forming layer and the workpiece in this order in the thickness direction on the support sheet, and with the peripheral portion of the first laminated composite sheet attached to a fixing jig, the first laminated composite sheet is heated to form a second laminated composite sheet on the support sheet in which the resin film and the workpiece are stacked in this order in the thickness direction, the second laminated composite sheet is cooled, and then the workpiece is divided on the support sheet, the resin film is cut, and a third laminated composite sheet is formed on the support sheet with a plurality of resin film-coated chips fixed thereon, and the resin film-coated chips in the third laminated composite sheet are picked up. Since the support sheet according to an embodiment of the present invention has the above-mentioned configuration, even if the first laminated composite sheet is heated while its peripheral portion is attached to a fixing jig and then the second laminated composite sheet is cooled, the effect of slackness of the third laminated composite sheet is eliminated and the recognition ability of the chip by the pickup device can be improved.

[0062] In addition, the support sheet of this embodiment can be suitably used in a method for manufacturing a resin film-coated chip, in which a resin film forming layer is attached to the back surface of a workpiece, and the resin film forming layer and the workpiece are stacked in this order in the thickness direction on the support sheet, the workpiece is divided in a first laminated composite sheet, the resin film forming layer is cut, and a fourth laminated composite sheet is formed in which a plurality of chips with a resin film forming layer are fixed on the support sheet, the fourth laminated composite sheet is heated while the peripheral portion of the fourth laminated composite sheet is attached to a fixing jig to form a third laminated composite sheet in which a plurality of chips with a resin film are fixed on the support sheet, the third laminated composite sheet is cooled, and then the resin film-coated chips in the third laminated composite sheet are picked up. Since the support sheet according to an embodiment of the present invention has the above-mentioned configuration, even if the fourth laminate composite sheet is heated while its peripheral portion is attached to a fixing jig and then the third laminate composite sheet is cooled, the effect of slackness of the third laminate composite sheet is eliminated and the recognition ability of the chip by the pickup device can be improved.

[0063] Since the support sheet according to an embodiment of the present invention has the above-mentioned configuration, it can improve the chip recognition ability of the pickup device even when the workpiece has a mass of 20 g or more, it can improve the chip recognition ability of the pickup device even when the workpiece has a mass of 30 g or more, and it can improve the chip recognition ability of the pickup device even when the workpiece has a mass of 40 g or more.

[0064] In this specification, the term "workpiece" refers to a wafer or a semiconductor device panel. Examples of "wafers" include semiconductor wafers made of elemental semiconductors such as silicon, germanium, and selenium, and compound semiconductors such as GaAs, GaP, InP, CdTe, ZnSe, and SiC; and insulator wafers made of insulators such as sapphire, glass, lithium niobate, and lithium tantalate. The term "semiconductor device panel" refers to an assembly in which a plurality of semiconductor devices, each of which has at least one electronic component sealed with a sealing resin layer, are arranged side by side in a plane. A circuit is formed on one surface of each of these workpieces, and in this specification, the surface of the workpiece on which the circuit is formed is referred to as the "circuit surface," and the surface of the workpiece opposite to the circuit surface is referred to as the "rear surface." The work is divided into chips by dicing or other means. In this specification, as in the case of the work, the surface of the chip on which the circuit is formed is referred to as the "circuit surface," and the surface of the chip opposite the circuit surface is referred to as the "back surface." Both the circuit surface of the workpiece and the circuit surface of the chip are provided with protruding electrodes such as bumps, pillars, etc. The protruding electrodes are preferably made of solder.

[0065] The support sheet may be one layer (single layer) or two or more layers. When the support sheet is made of multiple layers, the constituent materials and thicknesses of the multiple layers may be the same or different, and the combination of the multiple layers is not particularly limited as long as it does not impair the effects of the present invention.

[0066] The support sheet is preferably transparent, and may be colored depending on the purpose. When the resin film forming layer has energy ray curing properties, the support sheet is preferably one that transmits energy rays.

[0067] Examples of the support sheet include a sheet having a substrate and a pressure-sensitive adhesive layer provided on one side of the substrate, a sheet consisting of only the substrate, etc. When the support sheet has a pressure-sensitive adhesive layer, the pressure-sensitive adhesive layer is disposed between the substrate and the resin film-forming layer in the composite sheet for resin film formation.

[0068] When a support sheet having a substrate and a pressure-sensitive adhesive layer is used, the adhesion and peelability between the support sheet and the resin film forming layer in the composite sheet for resin film formation can be easily adjusted. When a support sheet consisting of only a substrate is used, a composite sheet for resin film formation can be produced at low cost.

[0069] An example of the support sheet of this embodiment will be described below with reference to the drawings.

[0070] Fig. 1 is a cross-sectional view showing an example of the support sheet of the present embodiment. In the drawings used in the following description, in order to make the features of the present invention easier to understand, the main parts may be enlarged for convenience, and the dimensional ratios of each component may not necessarily be the same as the actual ones.

[0071] The support sheet 10 shown in FIG. 1 has a pressure-sensitive adhesive layer 12 provided on one surface 11a (sometimes referred to as "first surface 11a" in this specification) of a substrate 11.

[0072] Next, each layer constituting the support sheet 10 will be described in more detail.

[0073] ○Base material The substrate is in the form of a sheet or film, and examples of the constituent materials thereof include various resins. Examples of the resin include polyethylenes such as low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), and high-density polyethylene (HDPE); polyolefins other than polyethylene such as polypropylene, polybutene, polybutadiene, polymethylpentene, and norbornene resin; ethylene-based copolymers (copolymers obtained by using ethylene as a monomer) such as ethylene-vinyl acetate copolymer, ethylene-(meth)acrylic acid copolymer, ethylene-(meth)acrylic acid ester copolymer, and ethylene-norbornene copolymer; vinyl chloride-based resins (copolymers obtained by using vinyl chloride as a monomer) such as polyvinyl chloride and vinyl chloride copolymer. resins having aromatic ring groups); polystyrene; polycycloolefins; polyesters such as polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, polyethylene isophthalate, polyethylene-2,6-naphthalenedicarboxylate, and wholly aromatic polyesters in which all constituent units have aromatic cyclic groups; copolymers of two or more of the above polyesters; poly(meth)acrylic acid esters; polyurethanes; polyurethane acrylates; polyimides; polyamides; polycarbonates; fluororesins; polyacetals; modified polyphenylene oxides; polyphenylene sulfides; polysulfones; and polyether ketones.

[0074] The material constituting the substrate preferably contains a polyolefin resin, and among these, polyolefins other than polyethylene are preferred, and polypropylene is more preferred.

[0075] The resin may also be a polymer alloy such as a mixture of the polyester and another resin. The polymer alloy of the polyester and another resin is preferably one in which the amount of the resin other than the polyester is relatively small. Examples of the resin include crosslinked resins in which one or more of the resins exemplified above are crosslinked; and modified resins such as ionomers using one or more of the resins exemplified above.

[0076] The resin constituting the substrate may be of only one type, or of two or more types. When two or more types are used, the combination and ratio thereof can be selected arbitrarily.

[0077] The substrate may consist of one layer (single layer), or may consist of two or more layers. When the substrate consists of multiple layers, the multiple layers may be the same or different, and the combination of the multiple layers is not particularly limited.

[0078] The thickness of the substrate is preferably 50 to 300 μm, more preferably 60 to 100 μm. By setting the thickness of the substrate within such a range, the flexibility of the support sheet and the composite sheet for resin film formation and the suitability for attachment to a workpiece are further improved. Here, the "thickness of the substrate" means the thickness of the entire substrate. For example, the thickness of a substrate consisting of multiple layers means the total thickness of all layers constituting the substrate.

[0079] The substrate may contain, in addition to the main constituent materials such as the resin, various known additives such as fillers, colorants, antioxidants, organic lubricants, catalysts, softeners (plasticizers), and the like.

[0080] The substrate is preferably transparent, and may be colored according to the purpose, or other layers may be vapor-deposited thereon.

[0081] In order to adjust the adhesion to the pressure-sensitive adhesive layer or resin film-forming layer provided thereon, the surface of the substrate may be subjected to roughening treatment such as sandblasting or solvent treatment, oxidation treatment such as corona discharge treatment, electron beam irradiation treatment, plasma treatment, ozone / ultraviolet radiation treatment, flame treatment, chromic acid treatment, or hot air treatment, lipophilic treatment, hydrophilic treatment, etc. The surface of the substrate may be treated with a primer.

[0082] The substrate may have adhesiveness on at least one surface thereof by containing a specific range of components (for example, a resin, etc.).

[0083] ○Method of manufacturing the substrate The substrate can be produced by a known method. For example, a substrate containing a resin can be produced by molding a resin composition containing the resin.

[0084] The substrate is preferably a stretched film. The stretching direction of the substrate may be only the machine direction (MD) of the substrate, or only the perpendicular direction (CD) of the substrate, and more preferably the substrate is biaxially stretched in the machine direction (MD) and the perpendicular direction (CD).

[0085] By using a stretched film as the base material, the residual stress of the stretched film is reduced by the average displacement (A 23→130 ) and the average displacement (A 60→130 In particular, the residual stress of the stretched film can be reduced by reducing the average displacement (A 60→130 ) is highly effective in reducing the amount of displacement (A 130 ) and the ratio [(A 60→130 ) / (A 23→130 )] can be made smaller.

[0086] The substrate is preferably stretched under heating conditions. The heating temperature conditions are adjusted depending on the constituent material of the substrate. For example, when the constituent material of the substrate is polypropylene, the heating temperature conditions are preferably 100 to 140°C, more preferably 105 to 135°C, and even more preferably 110 to 130°C.

[0087] The heating time condition is preferably from 15 to 120 s, more preferably from 30 to 100 s, and further preferably from 45 to 80 s.

[0088] The tension in the stretching is preferably from 1.0 to 6.0 N / m, more preferably from 1.3 to 5.0 N / m, and further preferably from 1.6 to 4.0 N / m.

[0089] Adhesive layer The pressure-sensitive adhesive layer is in the form of a sheet or film, and contains an adhesive resin. Examples of the adhesive resin include acrylic resin, urethane resin, rubber-based resin, silicone resin, epoxy-based resin, polyvinyl ether, polycarbonate, ester-based resin, etc. Among them, acrylic resin is preferable from the viewpoint of adjusting the adhesion with the resin film forming layer and the resin film.

[0090] The adhesive layer may consist of one layer (single layer), or may consist of two or more layers. If it consists of multiple layers, these multiple layers may be the same or different, and the combination of these multiple layers is not particularly limited.

[0091] The thickness of the adhesive layer is not particularly limited, but since this makes it easier to adjust the adhesion to the resin film-forming layer and the resin film, it is preferably 1 to 100 μm, more preferably 1 to 60 μm, even more preferably 1 to 30 μm, even more preferably 1 to 15 μm, and particularly preferably 1 to 9 μm. Here, "the thickness of the adhesive layer" means the thickness of the entire adhesive layer. For example, the thickness of an adhesive layer consisting of multiple layers means the total thickness of all layers that make up the adhesive layer.

[0092] The pressure-sensitive adhesive layer is preferably transparent, and may be colored depending on the purpose. When the resin film forming layer has energy ray curing properties, the pressure-sensitive adhesive layer is preferably one that transmits energy rays.

[0093] The adhesive layer may be either energy ray curable or non-energy ray curable. The energy ray curable adhesive layer can adjust its physical properties before and after curing. For example, before picking up the chip with the resin film described below, the energy ray curable adhesive layer can be cured to make it easier to pick up the chip with the resin film.

[0094] In this specification, the term "energy rays" refers to electromagnetic waves or charged particle beams that have an energy quantum. Examples of energy rays include ultraviolet rays, radiation, and electron beams. Ultraviolet rays can be irradiated by using, for example, a high-pressure mercury lamp, a fusion lamp, a xenon lamp, a black light, or an LED lamp as an ultraviolet ray source. Electron beams can be irradiated by generating them using an electron beam accelerator or the like. In this specification, "energy ray curable" means a property that is cured by irradiation with energy rays, and "non-energy ray curable" means a property that is not cured even when irradiated with energy rays. Moreover, the term "non-curable" means a property that does not cure by any means such as heating or irradiation with energy rays.

[0095] When the adhesive layer is energy ray curable, examples of the energy ray curable adhesive composition include an adhesive composition (I-1) containing a non-energy ray curable adhesive acrylic resin (I-1a) (hereinafter may be abbreviated as "adhesive resin (I-1a)") having a functional group such as a hydroxyl group and a non-energy ray curable adhesive compound, and an energy ray curable compound; an adhesive composition (I-2) containing an energy ray curable adhesive resin (I-2a) (hereinafter may be abbreviated as "adhesive resin (I-2a)") in which an unsaturated group has been introduced into the side chain of the non-energy ray curable adhesive resin (I-1a); an adhesive composition (I-3) containing the adhesive resin (I-2a) and a energy ray curable compound, and the like.

[0096] When the adhesive layer is non-energy ray curable, examples of the non-energy ray curable adhesive composition include an adhesive composition (I-4) containing the non-energy ray curable adhesive resin (I-1a).

[0097] [Non-energy ray curable adhesive resin (I-1a)] The adhesive resin (I-1a) is an adhesive acrylic resin having a functional group such as a hydroxyl group. Examples of the acrylic resin include acrylic polymers having a structural unit derived from a hydroxyl group-containing monomer and a structural unit derived from an alkyl (meth)acrylate ester. The (meth)acrylic acid alkyl ester may, for example, be one in which the alkyl group constituting the alkyl ester has 1 to 20 carbon atoms, and the alkyl group is preferably linear or branched.

[0098] The acrylic resin is a resin containing structural units derived from a (meth)acrylic acid ester monomer. Here, "derived from" means that the monomer has undergone a structural change necessary for polymerization. In this specification, the term "(meth)acrylic acid" is a concept that encompasses both "acrylic acid" and "methacrylic acid." The same applies to terms similar to (meth)acrylic acid.

[0099] The acrylic polymer may further contain, in addition to the constituent units derived from hydroxyl group-containing monomers and the constituent units derived from alkyl (meth)acrylates, constituent units derived from functional group-containing monomers other than hydroxyl group-containing monomers. Examples of the functional group-containing monomer include those in which the functional group reacts with a crosslinking agent described below to become a crosslinking starting point, and those in which the functional group reacts with a functional group such as an isocyanate group or a glycidyl group in an unsaturated group-containing compound described below to enable the introduction of an unsaturated group into a side chain of an acrylic polymer.

[0100] Examples of the functional group-containing monomer include, in addition to hydroxyl group-containing monomers, carboxy group-containing monomers, amino group-containing monomers, and epoxy group-containing monomers.

[0101] The acrylic polymer may further contain a constituent unit derived from another monomer, in addition to the constituent unit derived from the (meth)acrylic acid alkyl ester and the constituent unit derived from the functional group-containing monomer. The other monomer is not particularly limited as long as it is copolymerizable with the (meth)acrylic acid alkyl ester and the like. Examples of the other monomers include styrene, α-methylstyrene, vinyl toluene, vinyl formate, vinyl acetate, acrylonitrile, and acrylamide.

[0102] In the pressure-sensitive adhesive composition (I-1), pressure-sensitive adhesive composition (I-2), pressure-sensitive adhesive composition (I-3) and pressure-sensitive adhesive composition (I-4) (hereinafter, these pressure-sensitive adhesive compositions are collectively abbreviated as "pressure-sensitive adhesive compositions (I-1) to (I-4)"), the structural unit possessed by the acrylic resin such as the acrylic polymer may be of only one type or of two or more types, and when there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0103] In the acrylic polymer, the proportion of the amount of the structural units derived from functional group-containing monomers relative to the total amount of the structural units is preferably 1 to 35% by mass.

[0104] The adhesive resin (I-1a) contained in the adhesive composition (I-1) or the adhesive composition (I-4) may be one type or two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0105] In the pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive composition (I-1) or the pressure-sensitive adhesive composition (I-4), the content of the pressure-sensitive adhesive resin (I-1a) relative to the total mass of the pressure-sensitive adhesive layer is preferably 5 to 99 mass%, and may be, for example, any one of 25 to 98 mass%, 45 to 97 mass%, and 65 to 96 mass%.

[0106] [Energy ray curable adhesive resin (I-2a)] The adhesive resin (I-2a) can be obtained, for example, by reacting a functional group in the adhesive resin (I-1a) with an unsaturated group-containing compound having an energy ray-polymerizable unsaturated group.

[0107] The unsaturated group-containing compound is a compound that, in addition to the energy ray-polymerizable unsaturated group, further has a group that can bond to the adhesive resin (I-1a) by reacting with a functional group in the adhesive resin (I-1a). Examples of the energy ray-polymerizable unsaturated group include a (meth)acryloyl group, a vinyl group (ethenyl group), and an allyl group (2-propenyl group), and the like, with a (meth)acryloyl group being preferred. Examples of groups capable of bonding to functional groups in the adhesive resin (I-1a) include isocyanate groups and glycidyl groups capable of bonding to hydroxyl groups or amino groups, and hydroxyl groups and amino groups capable of bonding to carboxy groups or epoxy groups.

[0108] Examples of the unsaturated group-containing compound include (meth)acryloyloxyethyl isocyanate, (meth)acryloyl isocyanate, and glycidyl (meth)acrylate.

[0109] The adhesive resin (I-2a) contained in the adhesive composition (I-2) or (I-3) may be one type or two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0110] In the pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive composition (I-2) or (I-3), the content of the pressure-sensitive adhesive resin (I-2a) relative to the total mass of the pressure-sensitive adhesive layer is preferably 5 to 99 mass %.

[0111] [Energy ray curable compounds] The energy ray-curable compound contained in the pressure-sensitive adhesive composition (I-1) or (I-3) includes a monomer or oligomer having an energy ray-polymerizable unsaturated group and capable of being cured by irradiation with energy rays.

[0112] Among the energy ray-curable compounds, examples of the monomer include polyvalent (meth)acrylates such as trimethylolpropane tri(meth)acrylate, pentaerythritol (meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,4-butylene glycol di(meth)acrylate, and 1,6-hexanediol (meth)acrylate; urethane (meth)acrylate; polyester (meth)acrylate; polyether (meth)acrylate; and epoxy (meth)acrylate. Among the energy ray-curable compounds, examples of the oligomer include oligomers which are polymers of the monomers exemplified above.

[0113] The pressure-sensitive adhesive composition (I-1) or (I-3) may contain only one type of energy ray-curable compound, or two or more types. When two or more types are contained, the combination and ratio thereof can be selected arbitrarily.

[0114] In the pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive composition (I-1) or (I-3), the content of the energy ray-curable compound relative to the total mass of the pressure-sensitive adhesive layer is preferably 1 to 95 mass %.

[0115] [Crosslinking agent] The pressure-sensitive adhesive compositions (I-1) to (I-4) preferably further contain an isocyanate-based crosslinking agent.

[0116] The crosslinking agent reacts with the hydroxyl groups to crosslink the adhesive resins (I-1a) together or the adhesive resins (I-2a) together.

[0117] In the pressure-sensitive adhesive compositions (I-1) to (I-4), the content of the crosslinking agent is preferably 0.01 to 50 parts by mass relative to 100 parts by mass of the pressure-sensitive adhesive resin (I-1a), and may be, for example, any one of 1 to 40 parts by mass, 5 to 35 parts by mass, and 10 to 30 parts by mass. Examples of the crosslinking agent include the same ones as the "(crosslinking agent)" exemplified in the composition for forming a protective film (III-1) described later.

[0118] [Photopolymerization initiator] The pressure-sensitive adhesive compositions (I-1), (I-2) and (I-3) (hereinafter collectively referred to as "pressure-sensitive adhesive compositions (I-1) to (I-3)") may further contain a photopolymerization initiator. The pressure-sensitive adhesive compositions (I-1) to (I-3) containing a photopolymerization initiator sufficiently undergo a curing reaction even when irradiated with relatively low-energy energy rays such as ultraviolet rays.

[0119] Examples of the photopolymerization initiator include the same ones as the "(photopolymerization initiator)" exemplified in the composition for forming a protective film (III-1) described later.

[0120] The photopolymerization initiator contained in the pressure-sensitive adhesive compositions (I-1) to (I-3) may be only one type, or may be two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0121] In the pressure-sensitive adhesive composition (I-1), the content of the photopolymerization initiator is preferably 0.01 to 20 parts by mass relative to 100 parts by mass of the content of the energy ray-curable compound. In the pressure-sensitive adhesive composition (I-2), the content of the photopolymerization initiator is preferably 0.01 to 20 parts by mass per 100 parts by mass of the pressure-sensitive adhesive resin (I-2a). In the pressure-sensitive adhesive composition (I-3), the content of the photopolymerization initiator is preferably 0.01 to 20 parts by mass per 100 parts by mass of the total content of the pressure-sensitive adhesive resin (I-2a) and the energy ray-curable compound.

[0122] [Other additives] The pressure-sensitive adhesive compositions (I-1) to (I-4) may contain other additives that do not fall into any of the above-mentioned components, as long as the effects of the present invention are not impaired. Examples of the other additives include known additives such as antistatic agents, antioxidants, softeners (plasticizers), fillers, rust inhibitors, colorants (pigments, dyes), sensitizers, tackifiers, reaction retarders, and crosslinking accelerators (catalysts). The reaction retarder is, for example, a component that suppresses the progress of unintended crosslinking reactions in the pressure-sensitive adhesive compositions (I-1) to (I-4) during storage due to the action of a catalyst mixed in the pressure-sensitive adhesive compositions (I-1) to (I-4). Examples of the reaction retarder include those that form a chelate complex by chelating with the catalyst, and more specifically, those that have two or more carbonyl groups (-C(=O)-) in one molecule.

[0123] The other additives contained in the pressure-sensitive adhesive compositions (I-1) to (I-4) may be of only one type, or of two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0124] The content of other additives in the pressure-sensitive adhesive compositions (I-1) to (I-4) is not particularly limited and may be appropriately selected depending on the type of additive.

[0125] [solvent] The pressure-sensitive adhesive compositions (I-1) to (I-4) may contain a solvent. By containing a solvent, the pressure-sensitive adhesive compositions (I-1) to (I-4) have improved suitability for application to a surface to be coated.

[0126] The solvent is preferably an organic solvent, and examples of the organic solvent include ketones such as methyl ethyl ketone and acetone; esters (carboxylates) such as ethyl acetate; ethers such as tetrahydrofuran and dioxane; aliphatic hydrocarbons such as cyclohexane and n-hexane; aromatic hydrocarbons such as toluene and xylene; and alcohols such as 1-propanol and 2-propanol.

[0127] The pressure-sensitive adhesive compositions (I-1) to (I-4) may contain only one type of solvent, or two or more types. When two or more types are contained, the combination and ratio thereof can be selected arbitrarily.

[0128] The content of the solvent in each of the pressure-sensitive adhesive compositions (I-1) to (I-4) is not particularly limited and may be appropriately adjusted.

[0129] Method for producing pressure-sensitive adhesive composition The adhesive compositions such as the adhesive compositions (I-1) to (I-4) can be obtained by blending the adhesive resin and, if necessary, components other than the adhesive resin, which are components for constituting the adhesive composition. The order of addition of the components when blending is not particularly limited, and two or more components may be added simultaneously. The method for mixing the components during blending is not particularly limited, and may be appropriately selected from known methods such as a method of mixing by rotating a stirrer or stirring blade, a method of mixing using a mixer, a method of mixing by adding ultrasound, etc. The temperature and time during addition and mixing of each component are not particularly limited as long as the components do not deteriorate, and may be adjusted appropriately. A temperature of 15 to 30°C is preferred.

[0130] Method for producing pressure-sensitive adhesive layer The pressure-sensitive adhesive layer can be formed using a pressure-sensitive adhesive composition containing a pressure-sensitive adhesive resin. For example, the pressure-sensitive adhesive composition is applied to the surface on which the pressure-sensitive adhesive layer is to be formed, and then dried as necessary to form the pressure-sensitive adhesive layer at the desired location. The ratio of the contents of the components that do not vaporize at room temperature in the pressure-sensitive adhesive composition is usually the same as the ratio of the contents of the components in the pressure-sensitive adhesive layer.

[0131] The pressure-sensitive adhesive composition may be applied by a known method, for example, a method using various coaters such as an air knife coater, a blade coater, a bar coater, a gravure coater, a roll coater, a roll knife coater, a curtain coater, a die coater, a knife coater, a screen coater, a Mayer bar coater, or a kiss coater.

[0132] The drying conditions for the adhesive composition are not particularly limited. However, when the adhesive composition contains a solvent, it is preferable to heat-dry it. And, the adhesive composition containing the solvent is preferably heat-dried under conditions of, for example, 70 to 130°C and 10 seconds to 5 minutes.

[0133] ◇ Manufacturing method of support sheet When providing a pressure-sensitive adhesive layer on a substrate, for example, a pressure-sensitive adhesive composition may be applied to the substrate and dried as necessary. Also, for example, a pressure-sensitive adhesive composition may be applied to a release film and dried as necessary to form a pressure-sensitive adhesive layer on the release film, and the exposed surface of the pressure-sensitive adhesive layer may be attached to one surface of the substrate to laminate the pressure-sensitive adhesive layer on the substrate. In this case, the release film may be removed at any timing during the manufacturing process or use process of the composite sheet for resin film formation.

[0134] The support sheet 10 is preferably in the form of a roll. When support sheet 10 is in a roll form, the longitudinal direction of support sheet 10 is the machine direction (MD) and the cross direction of support sheet 10 is the cross direction (CD), regardless of whether support sheet 10 is stretched.

[0135] <<Composite sheet for forming resin film>> The composite sheet for resin film formation according to the embodiment of the present invention comprises the support sheet 10 according to the embodiment of the present invention described above, and a resin film formation layer provided on one surface of the support sheet 10. An example of the composite sheet for resin film formation of this embodiment will be described below with reference to the drawings.

[0136] FIG. 2 is a cross-sectional view that illustrates an example of the composite sheet for resin film formation of the present embodiment. In FIG. 2 and subsequent figures, the same components as those shown in the figures already described are given the same reference numerals as in the figures already described, and detailed description thereof will be omitted.

[0137] The composite sheet 101 for forming a resin film shown here is composed of a support sheet 10 and a resin film forming layer 13 provided on one side 10a (sometimes referred to as the "first side" in this specification) of the support sheet 10. The support sheet 10 is configured to include a base material 11 and an adhesive layer 12 provided on one surface (first surface) 11a of the base material 11. In the composite sheet 101 for resin film formation, the adhesive layer 12 is disposed between the base material 11 and the resin film formation layer 13.

[0138] That is, the composite sheet for resin film formation 101 is configured by laminating a substrate 11, a pressure-sensitive adhesive layer 12, and a resin film formation layer 13 in this order in the thickness direction. The first surface 10a of the support sheet 10 is the same as the surface 12a of the pressure-sensitive adhesive layer 12 opposite the substrate 11 side (sometimes referred to as the "first surface" in this specification).

[0139] The composite sheet for resin film formation 101 further includes a jig adhesive layer 16 and a release film 15 on the resin film formation layer 13 . In the composite sheet 101 for resin film formation, the resin film forming layer 13 is laminated on the entire or almost entire surface of the first surface 12a of the adhesive layer 12, and the jig adhesive layer 16 is laminated on a part of the surface 13a of the resin film forming layer 13 opposite to the adhesive layer 12 side (sometimes referred to as the "first surface" in this specification), i.e., on a region near the periphery. Furthermore, a release film 15 is laminated on the region of the first surface 13a of the resin film forming layer 13 where the jig adhesive layer 16 is not laminated, and on the surface 16a of the jig adhesive layer 16 opposite to the resin film forming layer 13 side (sometimes referred to as the "first surface" in this specification). A support sheet 10 is provided on the surface 13b of the resin film forming layer 13 opposite to the first surface 13a (sometimes referred to as the "second surface" in this specification).

[0140] Not only in the case of the composite sheet 101 for forming a resin film, but also in the composite sheet for forming a resin film of this embodiment, the release film is of an optional configuration, and the composite sheet for forming a resin film of this embodiment may or may not have a release film.

[0141] The adhesive layer 16 for a jig is used to fix the composite sheet 101 for resin film formation to a fixing jig 18 such as a ring frame. The jig adhesive layer 16 may have, for example, a single layer structure containing an adhesive component, or may have a multi-layer structure including a core sheet and layers containing an adhesive component provided on both sides of the core sheet.

[0142] The adhesive constituting the jig adhesive layer 16 is preferably one having the desired adhesive strength and removability, and for example, an acrylic adhesive, a rubber adhesive, a silicone adhesive, a urethane adhesive, a polyester adhesive, a polyvinyl ether adhesive, etc. can be used. Among these, an acrylic adhesive is preferred because it has high adhesion to the fixing jig 18 such as a ring frame and can effectively prevent the composite sheet for forming a protective film from peeling off from the fixing jig 18 such as a ring frame during a dicing process, etc. In addition, a substrate as a core material may be interposed in the middle of the thickness direction of the jig adhesive layer.

[0143] The pressure-sensitive adhesive layer for a jig can be formed using a pressure-sensitive adhesive composition for a jig containing an adhesive resin. For example, the pressure-sensitive adhesive composition for a jig can be applied to a surface on which the pressure-sensitive adhesive layer for a jig is to be formed, and then dried to form the pressure-sensitive adhesive layer for a jig at a desired location. Examples of the pressure-sensitive adhesive composition for a jig include compositions similar to the pressure-sensitive adhesive compositions (I-1) to (I-4). The ratio of the contents of the components that do not vaporize at room temperature in the pressure-sensitive adhesive composition for a jig is usually the same as the ratio of the contents of the components in the pressure-sensitive adhesive layer for a jig.

[0144] On the other hand, the thickness of the jig pressure-sensitive adhesive layer is preferably 5 to 200 μm, particularly preferably 10 to 100 μm, from the viewpoint of adhesiveness to the fixing jig 18 such as a ring frame.

[0145] The composite sheet 101 for resin film formation is used by removing the release film 15, attaching the back surface of a workpiece to the first surface 13a of the resin film formation layer 13, and further attaching the first surface 16a of the jig adhesive layer 16 to a fixing jig 18 such as a ring frame.

[0146] FIG. 3 is a cross-sectional view that illustrates a schematic diagram of another example of the composite sheet for resin film formation according to the present embodiment. The composite sheet 102 for resin film formation shown here is the same as the composite sheet 101 for resin film formation shown in Figure 2, except that the shape and size of the resin film formation layer are different and the adhesive layer for the jig is laminated on the first side of the adhesive layer rather than the first side of the resin film formation layer.

[0147] More specifically, in the composite sheet 102 for resin film formation, the resin film forming layer 23 is laminated in a part of the region of the first surface 12a of the adhesive layer 12, that is, in the central region in the width direction (left and right direction in FIG. 3) of the adhesive layer 12. Furthermore, in the region of the first surface 12a of the adhesive layer 12 where the resin film forming layer 23 is not laminated, the jig adhesive layer 16 is laminated so as to surround the resin film forming layer 23 from the outside in the width direction without contact. A release film 15 is laminated on the surface (sometimes referred to as the "first surface" in this specification) 23a of the resin film forming layer 23 opposite to the adhesive layer 12 side and the first surface 16a of the jig adhesive layer 16. A support sheet 10 is provided on the surface (sometimes referred to as the "second surface" in this specification) 23b of the resin film forming layer 23 opposite to the first surface 23a.

[0148] FIG. 4 is a cross-sectional view that illustrates a schematic diagram of still another example of the composite sheet for resin film formation of the present embodiment. The composite sheet for resin film formation 103 shown here is the same as the composite sheet for resin film formation 102 shown in FIG.

[0149] FIG. 5 is a cross-sectional view that illustrates a schematic diagram of still another example of the composite sheet for resin film formation of the present embodiment. The composite sheet 104 for resin film formation shown here is the same as the composite sheet 101 for resin film formation shown in FIG.

[0150] The support sheet 20 is made of only a substrate 11 . That is, the composite sheet for resin film formation 104 is configured by laminating the base material 11 and the resin film formation layer 13 in the thickness direction. The surface (first surface) 20 a of the support sheet 20 on the side of the resin film formation layer 13 is the same as the first surface 11 a of the substrate 11 . The substrate 11 has adhesiveness at least on the first surface 11a thereof.

[0151] The composite sheet for forming a resin film of this embodiment is not limited to that shown in Figures 2 to 5, and may be one in which some of the configurations shown in Figures 2 to 5 have been changed or deleted, or other configurations may be added to those described above, within the scope that does not impair the effects of the present invention.

[0152] ○Resin film forming layer The resin film forming layer is attached to the back surface of a workpiece in the method for producing a resin-coated chip. The resin film forming layer is preferably a protective film forming film used to protect the back surface of the workpiece or the chip obtained by dividing the workpiece.

[0153] By using the composite sheet for resin film formation or the kit comprising the support sheet and the resin film forming layer, a chip with a resin film can be manufactured by the manufacturing method for a chip with a resin film described below, which comprises a chip and a resin film provided on the back surface of the chip.

[0154] When the resin film forming layer is a protective film forming film, by using the protective film forming composite sheet or kit comprising the support sheet and the protective film forming film, a chip with a protective film can be manufactured by the resin film-coated chip manufacturing method described below, which comprises a chip and a protective film provided on the back surface of the chip.

[0155] Furthermore, by using the chip with the resin film, a substrate device can be manufactured. In this specification, the term "substrate device" refers to a device in which a resin-coated chip is flip-chip connected to a connection pad on a circuit board at a protruding electrode on the circuit surface of the chip. For example, when a semiconductor wafer is used as the wafer, a semiconductor device is an example of the substrate device.

[0156] The resin film forming layer is preferably thermosetting. The resin film forming layer can be formed using a resin film forming composition, and in particular, when the resin film forming layer is a thermosetting protective film forming film, the protective film forming film can be formed using the protective film forming composition (III-1) described below.

[0157] <Protective film forming composition (III-1)> Examples of compositions for forming resin films include a composition for forming a protective film (III-1) (sometimes abbreviated as "composition for forming a protective film (III-1)" in this specification) containing a polymer component (A) and a thermosetting component (B).

[0158] [Polymer component (A)] The polymer component (A) is a polymer compound for imparting film-forming properties, flexibility, and the like to the thermosetting protective film-forming film. The polymer component (A) contained in the protective film-forming composition (III-1) and the thermosetting protective film-forming film may be one type or two or more types, and if there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0159] The polymer component may also be considered as a curable component. In this specification, when the protective film-forming composition contains a component that corresponds to both a polymer component and a curable component, the protective film-forming composition is considered to contain a polymer component and a curable component.

[0160] As the polymer component, it is possible to use acrylic resin, urethane resin, phenoxy resin, silicone resin, saturated polyester resin, etc. As the polymer component, it is preferable to use acrylic resin.

[0161] The weight average molecular weight (Mw) of the polymer component is preferably 10,000 to 2,000,000, and more preferably 100,000 to 1,200,000. If the weight average molecular weight of the polymer component is equal to or greater than the lower limit, the adhesion to the support sheet 10 tends to decrease, and the adhesion between the support sheet and the protective film can be reduced. If the weight average molecular weight of the polymer component is equal to or less than the upper limit, the adhesion between the support sheet and the protective film-forming film can be improved.

[0162] The glass transition temperature (Tg) of the polymer component is preferably in the range of -60 to 50°C, more preferably -50 to 40°C, and particularly preferably -40 to 30°C. When the glass transition temperature of the polymer component is equal to or higher than the lower limit, the adhesion between the support sheet and the protective film can be reduced. When the glass transition temperature of the polymer component is equal to or lower than the upper limit, the adhesion between the support sheet and the protective film-forming film can be improved, and the risk of cracking (cracking) when the protective film-forming film is bent in a roll is reduced.

[0163] From the viewpoints of adhesion, adhesiveness and film-forming properties, the content of the polymer component is preferably 5 to 50 parts by mass, 10 to 45 parts by mass, 14 to 40 parts by mass, or 18 to 35 parts by mass relative to 100 parts by total weight of the protective film-forming film.

[0164] The glass transition temperature (Tg) of the resin constituting the polymer component can be calculated using the Fox formula shown below. 1 / Tg=(W1 / Tg1)+(W2 / Tg2)+...+(Wm / Tgm) (wherein Tg is the glass transition temperature of the resin constituting the polymer component, Tg1, Tg2,...Tgm are the glass transition temperatures of the homopolymers of the monomers that are the raw materials of the resin constituting the polymer component, and W1, W2,...Wm are the mass fractions of the monomers. However, W1+W2+...+Wm=1.) The glass transition temperature of the homopolymer of each monomer in the Fox formula can be the value described in the Polymer Data Handbook, the Adhesive Handbook, the Polymer Handbook, etc. For example, the glass transition temperatures of homopolymers are 10°C for methyl acrylate, 105°C for methyl methacrylate, -54°C for n-butyl acrylate, -70°C for 2-ethylhexyl acrylate, 41°C for glycidyl methacrylate, and -15°C for 2-hydroxyethyl acrylate.

[0165] Examples of monomers constituting the acrylic resin include (meth)acrylic acid ester monomers or derivatives thereof. For example, alkyl (meth)acrylates having an alkyl group with 1 to 18 carbon atoms, specifically methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, etc., can be mentioned. In addition, (meth)acrylates having a cyclic skeleton, specifically cyclohexyl (meth)acrylate, benzyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, imide (meth)acrylate, etc. can be mentioned. Furthermore, examples of functional group-containing monomers include hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, etc. having a hydroxyl group; and glycidyl (meth)acrylate, etc. having an epoxy group. The acrylic resin is preferably an acrylic polymer containing a structural unit having a hydroxyl group, since it has good compatibility with the curable component described later. The acrylic polymer may be copolymerized with acrylic acid, methacrylic acid, itaconic acid, vinyl acetate, acrylonitrile, styrene, or the like.

[0166] (curable component) As the curable component, for example, a thermosetting component (B) is used, which can make the protective film-forming film thermosetting.

[0167] By using a thermosetting protective film-forming film, the protective film-forming film can be easily thermally cured even if it is made thick, so that the protective film-forming film can be made thick with good protective performance. In the heat curing process, multiple workpieces can be cured at once.

[0168] The thermosetting component may be a thermosetting resin or a thermosetting agent. The thermosetting resin is preferably, for example, an epoxy resin.

[0169] As the epoxy resin, a conventionally known epoxy resin can be used. Specific examples of the epoxy resin include polyfunctional epoxy resins, biphenyl compounds, bisphenol A diglycidyl ether and its hydrogenated products, orthocresol novolac epoxy resins, dicyclopentadiene type epoxy resins, biphenyl type epoxy resins, bisphenol A type epoxy resins, bisphenol F type epoxy resins, and phenylene skeleton type epoxy resins, and other epoxy compounds having two or more functional groups in the molecule. These can be used alone or in combination of two or more.

[0170] The preferred content of the thermosetting component is 1 to 75 parts by mass, more preferably 2 to 60 parts by mass, and even more preferably 3 to 50 parts by mass, relative to the total weight of the protective film-forming film (100), and may be, for example, 4 to 40 parts by mass, 5 to 35 parts by mass, or 6 to 30 parts by mass. When the content of the thermosetting resin is equal to or more than the lower limit, the protective film can have sufficient adhesion to the workpiece, and the protective film has excellent performance in protecting the workpiece. When the content of the thermosetting resin is equal to or less than the upper limit, the protective film has excellent storage stability when stored as a roll.

[0171] The thermosetting agent functions as a curing agent for thermosetting resins, particularly epoxy resins. A preferred thermosetting agent is a compound having two or more functional groups in one molecule that can react with an epoxy group. The functional groups include phenolic hydroxyl groups, alcoholic hydroxyl groups, amino groups, carboxyl groups, and acid anhydrides. Of these, preferred are phenolic hydroxyl groups, amino groups, and acid anhydrides, and more preferred are phenolic hydroxyl groups and amino groups.

[0172] Specific examples of phenol-based hardeners include polyfunctional phenol resins, biphenols, novolac-type phenol resins, dicyclopentadiene-based phenol resins, xylok-type phenol resins, and aralkyl phenol resins.Specific examples of amine-based hardeners include DICY (dicyandiamide).These can be used alone or in combination of two or more.

[0173] The content of the thermosetting agent is preferably 0.1 to 500 parts by mass, and more preferably 1 to 200 parts by mass, relative to 100 parts by mass of the thermosetting resin. When the content of the thermosetting agent is equal to or more than the lower limit, the thermosetting agent is sufficiently cured and adhesiveness is obtained, and when the content is equal to or less than the upper limit, the moisture absorption rate of the protective film is suppressed, improving the adhesive reliability between the workpiece and the protective film.

[0174] The protective film-forming composition (III-1) may contain an energy ray-curable component. As the energy ray-curable component, a low molecular weight compound (energy ray-polymerizable compound) that contains an energy ray-polymerizable group and is polymerized and cured when irradiated with energy rays such as ultraviolet rays and electron beams can be used. Specific examples of such energy ray-curable components include trimethylolpropane triacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, dipentaerythritol monohydroxypentaacrylate, dipentaerythritol hexaacrylate, or acrylate-based compounds such as 1,4-butylene glycol diacrylate, 1,6-hexanediol diacrylate, polyethylene glycol diacrylate, oligoester acrylate, urethane acrylate-based oligomer, epoxy-modified acrylate, polyether acrylate, and itaconic acid oligomer. Such compounds have at least one polymerizable double bond in the molecule, and usually have a weight average molecular weight of 100 to 30,000, preferably about 300 to 10,000. The content of the energy ray curable component is preferably 1 to 30 parts by mass, and more preferably 5 to 25 parts by mass, based on 100 parts by total weight of the protective film-forming film.

[0175] In addition, as the energy ray curable component, an energy ray curable polymer having an energy ray polymerizable group bonded to the main chain or side chain of a polymer component may be used. Such an energy ray curable polymer has both a function as a polymer component and a function as a curable component.

[0176] The main skeleton of the energy ray curable polymer is not particularly limited, and may be an acrylic polymer, which is widely used as a polymer component, or may be polyester, polyether, or the like. However, it is particularly preferable to use an acrylic polymer as the main skeleton because of ease of synthesis and control of physical properties.

[0177] The energy ray-polymerizable group bonded to the main chain or side chain of the energy ray-curable polymer is, for example, a group containing an energy ray-polymerizable carbon-carbon double bond, and specific examples thereof include a (meth)acryloyl group, etc. The energy ray-polymerizable group may be bonded to the energy ray-curable polymer via an alkylene group, an alkyleneoxy group, or a polyalkyleneoxy group.

[0178] The weight average molecular weight (Mw) of the energy ray curable polymer is preferably 10,000 to 2,000,000, and more preferably 100,000 to 1,500,000. The glass transition temperature (Tg) of the energy ray curable polymer is preferably in the range of -60 to 50°C, more preferably -50 to 40°C, and particularly preferably -40 to 30°C.

[0179] The energy beam curable polymer is obtained by reacting an acrylic resin containing a functional group such as a hydroxyl group, a carboxyl group, an amino group, a substituted amino group, or an epoxy group with a polymerizable group-containing compound having a substituent reactive with the functional group and 1 to 5 energy beam polymerizable carbon-carbon double bonds per molecule. Examples of the substituent reactive with the functional group include an isocyanate group, a glycidyl group, and a carboxyl group.

[0180] Examples of the polymerizable group-containing compound include (meth)acryloyloxyethyl isocyanate, meta-isopropenyl-α,α-dimethylbenzyl isocyanate, (meth)acryloyl isocyanate, allyl isocyanate, glycidyl (meth)acrylate; (meth)acrylic acid; and the like.

[0181] The acrylic resin is preferably a copolymer consisting of a (meth)acrylic monomer having a functional group such as a hydroxyl group, a carboxyl group, an amino group, a substituted amino group, an epoxy group, or the like, or a derivative thereof, and another (meth)acrylic acid ester monomer copolymerizable therewith, or a derivative thereof.

[0182] Examples of (meth)acrylic monomers or derivatives thereof having a functional group such as a hydroxyl group, a carboxyl group, an amino group, a substituted amino group, or an epoxy group include 2-hydroxyethyl (meth)acrylate and 2-hydroxypropyl (meth)acrylate having a hydroxyl group; acrylic acid, methacrylic acid, and itaconic acid having a carboxyl group; and glycidyl methacrylate and glycidyl acrylate having an epoxy group.

[0183] Examples of other (meth)acrylic acid ester monomers or derivatives thereof that can be copolymerized with the above monomers include alkyl (meth)acrylates having an alkyl group with 1 to 18 carbon atoms, specifically methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, etc.; and (meth)acrylates having a cyclic skeleton, specifically cyclohexyl (meth)acrylate, benzyl (meth)acrylate, isobornyl acrylate, dicyclopentanyl acrylate, dicyclopentenyl acrylate, dicyclopentenyloxyethyl acrylate, imide acrylate, etc. In addition, the above acrylic resins may be copolymerized with vinyl acetate, acrylonitrile, styrene, etc.

[0184] Even when an energy ray curable polymer is used, the above-mentioned energy ray polymerizable compound may be used in combination, or a polymer component may be used in combination.

[0185] The protective film-forming film may contain the following components in addition to the above polymer component and curable component.

[0186] (Coloring agent) The protective film-forming film preferably contains a colorant. By blending a colorant in the protective film-forming film, when the semiconductor device is incorporated into an apparatus, infrared rays and the like generated from the surrounding devices can be shielded, and malfunction of the semiconductor device due to them can be prevented. In a semiconductor device or semiconductor chip on which a protective film is formed, a product number and the like are usually printed on the surface of the protective film by a laser marking method, but when the protective film contains a colorant, a sufficient contrast difference is obtained between the part of the protective film marked by the laser light and the part that is not, and visibility is improved. As the colorant, organic or inorganic pigments and dyes are used. Pigments are preferred from the viewpoint of heat resistance and the like. As the pigment, carbon black, iron oxide, manganese dioxide, aniline black, activated carbon, etc. are used, but are not limited to these. Among them, carbon black is particularly preferred from the viewpoint of handling and dispersibility. The colorant may be used alone or in combination of two or more kinds.

[0187] The content of the colorant is preferably 0.05 to 35 parts by mass, more preferably 0.1 to 25 parts by mass, and particularly preferably 0.2 to 15 parts by mass, based on 100 parts by mass of the total solid content constituting the protective film-forming film.

[0188] (Cure accelerator) The curing accelerator is used to adjust the curing speed of the protective film-forming film, and is preferably used particularly when an epoxy resin and a heat curing agent are used in combination in the heat curable component (B).

[0189] Preferred curing accelerators include tertiary amines such as triethylenediamine, benzyldimethylamine, triethanolamine, dimethylaminoethanol, and tris(dimethylaminomethyl)phenol; imidazoles such as 2-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, and 2-phenyl-4-methyl-5-hydroxymethylimidazole; organic phosphines such as tributylphosphine, diphenylphosphine, and triphenylphosphine; and tetraphenylboron salts such as tetraphenylphosphonium tetraphenylborate and triphenylphosphine tetraphenylborate. These may be used alone or in combination of two or more.

[0190] The curing accelerator is preferably contained in an amount of 0.01 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, based on 100 parts by mass of the curable component. By containing the curing accelerator in the amount within the above range, the adhesive has excellent adhesive properties even when exposed to high temperature and high humidity, and can achieve high adhesive reliability even when exposed to severe reflow conditions.

[0191] (Coupling Agent) The coupling agent may be used to improve the adhesive reliability of the protective film to the workpiece. In addition, by using the coupling agent, the water resistance of the protective film obtained by curing the protective film-forming film can be improved without impairing the heat resistance of the protective film.

[0192] As the coupling agent, a compound having a group that reacts with a functional group possessed by the polymer component, the curable component, etc. is preferably used. As the coupling agent, a silane coupling agent is preferable. Examples of such coupling agents include γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-(methacryloxypropyl)trimethoxysilane, γ-aminopropyltrimethoxysilane, N-6-(aminoethyl)-γ-aminopropyltrimethoxysilane, N-6-(aminoethyl)-γ-aminopropylmethyldiethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, γ-ureidopropyltriethoxysilane, γ-mercaptopropyltrimethoxysilane, γ-mercaptopropylmethyldimethoxysilane, bis(3-triethoxysilylpropyl)tetrasulfane, methyltrimethoxysilane, methyltriethoxysilane, vinyltrimethoxysilane, vinyltriacetoxysilane, imidazolesilane, etc. These can be used alone or in combination of two or more.

[0193] The coupling agent is usually contained in an amount of 0.1 to 20 parts by mass, preferably 0.2 to 10 parts by mass, and more preferably 0.3 to 5 parts by mass, based on 100 parts by mass of the polymer component and the curable component combined. If the content of the coupling agent is less than 0.1 part by mass, the above effect may not be obtained, and if it exceeds 20 parts by mass, it may cause outgassing.

[0194] (filling material) By blending the filler into the protective film-forming film, it becomes possible to adjust the thermal expansion coefficient of the protective film after curing, and by optimizing the thermal expansion coefficient of the protective film after curing with respect to the semiconductor chip, it is possible to improve the adhesion reliability between the workpiece and the protective film. As the filler, an inorganic filler is preferable. It is also possible to reduce the moisture absorption rate of the protective film after curing.

[0195] Preferred inorganic fillers include silica, alumina, talc, calcium carbonate, titanium oxide, iron oxide, silicon carbide, boron nitride, and the like powders, beads obtained by shaping these into spheres, single crystal fibers, and glass fibers. Among these, silica filler and alumina filler are preferred. The inorganic fillers can be used alone or in combination of two or more. The content of the inorganic filler can be 1 to 85 parts by mass, 5 to 80 parts by mass, 10 to 75 parts by mass, 20 to 70 parts by mass, or 30 to 66 parts by mass, relative to 100 parts by mass of the total solid content constituting the protective film-forming film. By making the content of the inorganic filler below the above upper limit value, the risk of cracks (fissures) occurring when the protective film-forming film is bent when rolled can be reduced, and by making the content above the above lower limit value, the heat resistance of the protective film can be improved.

[0196] (Photopolymerization initiator) When the protective film-forming film contains an energy ray-curable component, the protective film-forming film is irradiated with energy rays such as ultraviolet rays during use to cure the energy ray-curable component. In this case, by including a photopolymerization initiator in the composition, the polymerization and curing time and the amount of light irradiation can be reduced.

[0197] Specific examples of such photopolymerization initiators include benzophenone, acetophenone, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin isobutyl ether, benzoin benzoic acid, benzoin methyl benzoate, benzoin dimethyl ketal, 2,4-diethylthioxanthone, α-hydroxycyclohexyl phenyl ketone, benzyl diphenyl sulfide, tetramethylthiuram monosulfide, azobisisobutyronitrile, benzyl, dibenzyl, diacetyl, 1,2-diphenylmethane, 2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, and β-chloroanthraquinone. The photopolymerization initiators can be used alone or in combination of two or more.

[0198] The blending ratio of the photopolymerization initiator is preferably 0.1 to 10 parts by mass, more preferably 1 to 5 parts by mass, per 100 parts by mass of the energy ray curable component. If it is equal to or more than the lower limit, photopolymerization can be performed to obtain satisfactory protective performance, and if it is equal to or less than the upper limit, generation of residues that do not contribute to photopolymerization can be suppressed, and the curability of the protective film-forming film can be sufficient.

[0199] (Crosslinking agent) In order to adjust the adhesive strength and cohesiveness of the protective film-forming film with the workpiece, a crosslinking agent may be added. Examples of the crosslinking agent include an organic polyvalent isocyanate compound and an organic polyvalent imine compound.

[0200] Examples of the organic polyisocyanate compound include aromatic polyisocyanate compounds, aliphatic polyisocyanate compounds, alicyclic polyisocyanate compounds, and trimers of these organic polyisocyanate compounds, as well as isocyanate-terminated urethane prepolymers obtained by reacting these organic polyisocyanate compounds with polyol compounds.

[0201] Examples of the organic polyisocyanate compound include 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 1,3-xylylene diisocyanate, 1,4-xylylene diisocyanate, diphenylmethane-4,4'-diisocyanate, diphenylmethane-2,4'-diisocyanate, 3-methyldiphenylmethane diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, dicyclohexylmethane-2,4'-diisocyanate, trimethylolpropane adduct tolylene diisocyanate, and lysine isocyanate.

[0202] Examples of the organic polyvalent imine compound include N,N'-diphenylmethane-4,4'-bis(1-aziridinecarboxamide), trimethylolpropane-tri-β-aziridinylpropionate, tetramethylolmethane-tri-β-aziridinylpropionate, and N,N'-toluene-2,4-bis(1-aziridinecarboxamide)triethylenemelamine.

[0203] The crosslinking agent is usually used in a ratio of 0.01 to 20 parts by mass, preferably 0.1 to 10 parts by mass, and more preferably 0.5 to 5 parts by mass, per 100 parts by mass of the total amount of the polymer component and the energy ray curable polymer.

[0204] (General purpose additive) In addition to the above, various additives may be blended into the protective film-forming film as necessary. Examples of the various additives include tackifiers, leveling agents, plasticizers, antistatic agents, antioxidants, ion trapping agents, gettering agents, and chain transfer agents.

[0205] (solvent) The protective film-forming composition preferably further contains a solvent. A protective film-forming composition containing a solvent has good handleability. The solvent is not particularly limited, but preferred examples include hydrocarbons such as toluene and xylene; alcohols such as methanol, ethanol, 2-propanol, isobutyl alcohol (2-methylpropan-1-ol), and 1-butanol; esters such as ethyl acetate; ketones such as acetone and methyl ethyl ketone; ethers such as tetrahydrofuran; and amides (compounds having an amide bond) such as dimethylformamide and N-methylpyrrolidone. The protective film-forming composition may contain only one type of solvent, or two or more types. When two or more types are contained, the combination and ratio of the solvents can be selected arbitrarily.

[0206] The solvent contained in the protective film-forming composition is preferably methyl ethyl ketone or the like, since this allows the components contained in the composition to be mixed more uniformly.

[0207] The protective film-forming film obtained by applying and drying the protective film-forming composition composed of the above-mentioned components has adhesion and curability, and is pressed onto a workpiece in an uncured state. The protective film-forming film may be heated during pressing. After curing, a protective film with high impact resistance can be finally obtained, and the film has excellent adhesion and can maintain sufficient protective function even under severe high temperature and high humidity conditions. The protective film-forming film may have a single layer structure, or may have a multilayer structure as long as it contains at least one layer containing the above-mentioned components.

[0208] The thickness of the protective film-forming film is not particularly limited, but can be 3 to 300 μm, 3 to 200 μm, 5 to 100 μm, 7 to 80 μm, 10 to 70 μm, 12 to 60 μm, 15 to 50 μm, 18 to 40 μm, or 20 to 30 μm. When the thickness of the protective film-forming film is equal to or greater than the above lower limit, the protective performance of the protective film can be made sufficient, and when the thickness is equal to or less than the above upper limit, the cost can be reduced.

[0209] Method for producing resin film-forming composition A resin film-forming composition such as the protective film-forming composition (III-1) can be obtained by blending the respective components constituting the composition. The order of addition of the components when blending is not particularly limited, and two or more components may be added simultaneously. When a solvent is used, the solvent may be used by mixing it with any of the other ingredients to pre-dilute the ingredients, or the solvent may be used by mixing it with any of the other ingredients without pre-diluting the ingredients. The method for mixing the components during blending is not particularly limited, and may be appropriately selected from known methods such as a method of mixing by rotating a stirrer or stirring blades, a method of mixing using a mixer, a method of mixing by adding ultrasound, etc. The temperature and time during addition and mixing of each component may be appropriately adjusted taking into consideration conditions under which each blended component is unlikely to deteriorate, but a temperature of 15 to 30°C is preferable.

[0210] ◇Manufacturing method of composite sheet for resin film formation The composite sheet for resin film formation can be produced by laminating the above-mentioned layers so as to have a corresponding positional relationship, and adjusting the shape of some or all of the layers as necessary. The method for forming each layer is as described above.

[0211] It is possible to directly form a resin film-forming layer by applying a resin film-forming composition on the pressure-sensitive adhesive layer already laminated on the substrate. In this way, when forming a new layer (hereinafter abbreviated as "second layer") on any layer (hereinafter abbreviated as "first layer") already laminated on the substrate to form a continuous two-layer laminate structure (in other words, a laminate structure of the first layer and the second layer), a method of applying a composition for forming the second layer on the first layer and drying it as necessary can be applied. However, it is preferable to form the second layer in advance on a release film using a composition for forming the second layer, and then bond the exposed surface of the second layer opposite to the side in contact with the release film to the exposed surface of the first layer to form a continuous two-layer laminate structure. In this case, it is preferable to coat the composition on the release-treated surface of the release film. The release film can be removed as necessary after the laminate structure is formed. Here, we have given an example of laminating a resin film-forming layer onto an adhesive layer, but the target laminate structure can be selected arbitrarily, for example, when laminating a layer (film) other than the resin film-forming layer onto the adhesive layer.

[0212] In this way, all layers other than the substrate that constitute the composite sheet for forming a resin film can be formed in advance on a release film and laminated by bonding it to the surface of the desired layer, so the composite sheet for forming a resin film can be manufactured by appropriately selecting the layers that will undergo such a process as necessary.

[0213] The composite sheet for resin film formation is usually stored in a state where a release film is attached to the surface of the outermost layer (for example, the resin film-forming layer) on the opposite side to the support sheet. Therefore, the composition for resin film formation is applied onto this release film (preferably its release-treated surface) and dried as necessary to form a resin film-forming layer on the release film, and the remaining layers are laminated on the exposed surface opposite to the side in contact with the release film of this resin film-forming layer by any of the above-mentioned methods, and the release film is not removed and the laminated state is left as it is, thereby obtaining a composite sheet for resin film formation with a release film.

[0214] When the resin film forming layer is a protective film forming film, the composite sheet for forming a protective film is obtained, which comprises the support sheet and the protective film forming film.

[0215] The composite sheet for resin film formation may be in the form of a sheet, and is preferably in the form of a roll.

[0216] <<Kit>> A kit according to an embodiment of the present invention comprises a first laminate in which a first release film, a resin film forming layer and a second release film are laminated in this order, and a support sheet used to support a workpiece to which the resin film forming layer is to be attached and the resin film forming layer. An example of the kit 1 of this embodiment will now be described with reference to the drawings.

[0217] FIG. 6 is a cross-sectional view that illustrates an example of the kit 1 of the present embodiment. The kit 1 of this embodiment comprises a first laminate 5 in which a first release film 151, a resin film forming layer 13 and a second release film 152 are laminated in this order, and a support sheet 10 used to support the workpiece to which the resin film forming layer 13 is to be attached and the resin film forming layer 13, and the support sheet 10 is the support sheet relating to the embodiment of the present invention described above.

[0218] The resin film forming layer 13 shown here has a first release film 151 on one of its surfaces (sometimes referred to as the "first surface" in this specification) 13a, and a second release film 152 on the other surface (sometimes referred to as the "second surface" in this specification) 13b opposite the first surface 13a.

[0219] When the resin film forming layer is a protective film forming film, by using a kit 1 including the support sheet 10 and the protective film forming film, a chip with a protective film can be manufactured by the manufacturing method for a chip with a resin film described below, which includes a chip and a protective film provided on the back surface of the chip.

[0220] Such a resin film forming layer 13 is suitable for storage, for example, in a roll form. That is, the first laminate is preferably in a roll form.

[0221] The resin film forming layer 13 can be formed using the above-mentioned resin film forming composition.

[0222] Both the first release film 151 and the second release film 152 may be of known types. The first release film 151 and the second release film 152 may be the same as each other, or may be different from each other, for example, in that the peeling forces required to peel them from the resin film formation layer 13 are different from each other.

[0223] 6, one of the first release film 151 and the second release film 152 is removed, and the resulting exposed surface becomes the surface to be attached to the back surface of the work (not shown). Then, the remaining other of the first release film 151 and the second release film 152 is removed, and the resulting exposed surface becomes the surface to be attached to the back surface of the support sheet.

[0224] Figure 6 shows an example in which a release film is provided on both sides (first side 13a and second side 13b) of the resin film-forming layer 13, but the release film may be provided on only one side of the resin film-forming layer 13, i.e., only the first side 13a or only the second side 13b.

[0225] In the kit 1 of this embodiment, by using the resin film formation layer 13 and the support sheet 10 in combination, both the application of the resin film formation layer to the work and the subsequent application of the support sheet can be performed in an in-line process. Here, "in-line process" refers to a process "performed in a device in which multiple (multiple) devices performing one or multiple steps are connected together, or in the same device, including multiple steps and the transport connecting the steps, in which the work is transported one by one between one step and the next step."

[0226] <<Method of manufacturing chips with resin coating>> The support sheet according to the above-mentioned embodiment of the present invention, the composite sheet for forming a resin film comprising the support sheet, and the kit 1 comprising the support sheet can be used in a method for manufacturing a chip with a resin film comprising a chip and a resin film provided on the back surface of the chip.

[0227] <Manufacturing method 1> The manufacturing method according to the first embodiment is a method for manufacturing a resin film-coated chip including a chip and a resin film provided on a back surface of the chip, The method for producing the resin-film-coated chip includes the steps of: attaching a resin film-forming layer in the composite sheet for resin film formation according to the embodiment of the present invention described above to the back surface of a workpiece, thereby producing a first laminated composite sheet in which the resin film-forming layer and the workpiece are laminated in this order in the thickness direction on the support sheet; a step of heating the first laminated composite sheet while the peripheral portion of the first laminated composite sheet is attached to a fixing jig, hardening the resin film forming layer, and forming the resin film, thereby producing a second laminated composite sheet in which the resin film and the work are laminated in this order in the thickness direction on the support sheet; cooling the second laminated composite sheet, and then dividing the work in the second laminated composite sheet on the support sheet and cutting the resin film to produce a third laminated composite sheet in which a plurality of chips with a resin film are fixed on the support sheet; and picking up the resin-film-attached chip in the third laminated composite sheet by separating it from the support sheet. Hereinafter, the manufacturing method according to the first embodiment may be referred to as "manufacturing method 1" in this specification.

[0228] 7A to 7E are cross-sectional views for typically explaining manufacturing method 1. Here, manufacturing method 1 will be explained by taking as an example a case where a composite sheet 101 for resin film formation in FIG. 2 having a support sheet 10 shown in FIG. 1 is used.

[0229] In the step of producing the first laminated composite sheet in manufacturing method 1, as shown in Fig. 7A, the resin film forming layer 13 in the composite sheet 101 for resin film formation is attached to the back surface 9b of the work 9 to produce a first laminated composite sheet 501 in which the resin film forming layer 13 and the work 9 are laminated in this order in the thickness direction on the support sheet 10. The first surface 13a of the resin film forming layer 13 in the composite sheet 101 for resin film formation is attached to the back surface 9b of the work 9.

[0230] The resin film forming layer 13 in the composite sheet for resin film formation 101 can be attached to the workpiece 9 by a known method. For example, the resin film forming layer 13 may be attached to the workpiece 9 while being heated.

[0231] Next, in the step of producing the second laminated composite sheet of manufacturing method 1, the first laminated composite sheet 501 is heated in a state where the peripheral portion of the first laminated composite sheet 501 is attached to a fixing jig 18 such as a ring frame via the jig adhesive layer 16 (FIG. 7B). This causes the resin film forming layer 13 to harden and form a resin film 13', thereby producing a second laminated composite sheet 502 in which the support sheet 10, the resin film 13' and the workpiece 9 are laminated in this order in the thickness direction, as shown in FIG. 7C.

[0232] Reference numeral 13a' denotes a surface of the resin film 13' that was the first surface 13a of the resin film-formed layer 13 (sometimes referred to as the "first surface" in this specification). Reference numeral 13b' denotes a surface of the resin film 13' that was the second surface 13b of the resin film-formed layer 13 (sometimes referred to as the "second surface" in this specification).

[0233] When the resin film forming layer 13 is thermosetting, the resin film forming layer 13 can be cured by heating the resin film forming layer 13 .

[0234] When the resin film forming layer 13 is a protective film forming film, the resin film forming layer 13 shown in Figure 7A may be laser marked by irradiating it with a laser through the support sheet 10 (through the support sheet 10), or the resin film 13' shown in Figure 7C may be laser marked by irradiating it with a laser through the support sheet 10 (through the support sheet 10).

[0235] Next, in the step of producing the third laminated composite sheet of manufacturing method 1, the second laminated composite sheet 502 is cooled, and then, as shown in Fig. 7D, the work 9 in the second laminated composite sheet 502 is divided on the support sheet 10, and the resin film 13' is cut. The work 9 is divided into individual pieces into a plurality of chips 90.

[0236] The division of the workpiece 9 and the cutting of the resin film 13' may be performed by a known method. For example, the division of the workpiece 9 and the cutting of the resin film 13' can be performed successively by dicing such as blade dicing, laser dicing by irradiating a laser, or water dicing by spraying water containing an abrasive. The resin film 13' is cut along the outer periphery of the chip 90, regardless of the cutting method.

[0237] In this manner, by dividing the workpiece 9 and cutting the resin film 13', a plurality of chips 901 with resin film are obtained, each chip 90 having a resin film (sometimes simply referred to as "resin film" in this specification) 130' after cutting provided on the back surface 90b of the chip 90. Reference numeral 130b' denotes a surface of the resin film 130' after cutting that was the second surface 13b' of the resin film 13' (sometimes referred to as "second surface" in this specification).

[0238] In the step of producing the third laminated composite sheet in manufacturing method 1, the third laminated composite sheet 503 in which the plurality of resin-film-coated chips 901 are fixed on the support sheet 10 is produced as described above.

[0239] Next, in the picking up step of manufacturing method 1, chip 901 with resin film in third laminated composite sheet 503 is picked up by being pulled away from support sheet 10 as shown in FIG. 7E.

[0240] In manufacturing method 1 according to an embodiment of the present invention, since support sheet 10 has the above-described configuration, even if the peripheral portion of first laminated composite sheet 501 is heated while attached to a fixing jig and then second laminated composite sheet 502 is cooled, the effect of slackness of third laminated composite sheet 503 is eliminated and the recognition ability of the chip by the pickup device can be improved.

[0241] In the picking up step, peeling occurs between second surface 130b' of resin film 130' in resin-film-coated chip 901 and first surface 12a of adhesive layer 12 in support sheet 10.

[0242] Here, a case is shown in which a separating means 7 such as a vacuum collet is used to separate the resin film-coated chip 901 in the direction of arrow P. Note that a cross-sectional view of the separating means 7 is omitted here. The resin film-coated chip 901 can be picked up by a known method.

[0243] When the adhesive layer 12 is energy ray curable, in the picking up step, the adhesive layer 12 may be cured by irradiating it with energy rays to form a cured product (not shown), and then the resin film-coated chip 901 may be separated from the support sheet 10. In this case, in the picking up step, peeling occurs between the resin film 130' in the resin film-coated chip 901 and the cured product of the adhesive layer 12 in the support sheet 10. In this case, the adhesive strength between the cured product of the adhesive layer 12 and the resin film 130' is smaller than the adhesive strength between the cured product of the adhesive layer 12 and the substrate 11, so that the resin film-attached chip 901 can be easily picked up.

[0244] In this specification, even after the energy ray-curable pressure-sensitive adhesive layer is cured with energy rays, as long as the laminated structure of the substrate and the cured product of the energy ray-curable pressure-sensitive adhesive layer is maintained, this laminated structure is referred to as a "support sheet."

[0245] On the other hand, if the adhesive layer 12 is non-energy ray curable, the resin film-coated chip 901 can be simply pulled away from the adhesive layer 12, and since there is no need to harden the adhesive layer 12, the resin film-coated chip 901 can be picked up in a simplified process.

[0246] In the picking up step, such picking up of the resin film-coated chips 901 is performed for all of the intended resin film-coated chips 901 .

[0247] In the manufacturing method 1, the intended chip 901 with a resin film is obtained by carrying out the steps up to the picking up step.

[0248] The explanation of manufacturing method 1 so far has been given for the case where a composite sheet 101 for forming a resin film having a support sheet 10 shown in FIG. 2 is used. However, in manufacturing method 1, a composite sheet for forming a resin film of this embodiment other than the composite sheet 101 for forming a resin film, such as the composite sheet 102 for forming a resin film, the composite sheet 103 for forming a resin film or the composite sheet 104 for forming a resin film shown in FIGS. 3 to 5 may also be used.

[0249] <Manufacturing method 2> The manufacturing method according to the second embodiment is a method for manufacturing a resin film-coated chip including a chip and a resin film provided on a back surface of the chip, A process of attaching a resin film forming layer in the kit 1 according to the embodiment of the present invention described above to the back surface of a workpiece to produce a first laminate film in which the resin film forming layer and the workpiece are laminated in their thickness direction, and further attaching an adhesive layer of a support sheet in the kit 1 to the resin film forming layer in the first laminate film to produce a first laminated composite sheet in which the resin film forming layer and the workpiece are laminated in this order in their thickness direction on the support sheet; a step of heating the first laminated composite sheet while the peripheral portion of the first laminated composite sheet is attached to a fixing jig, hardening the resin film forming layer, and forming the resin film, thereby producing a second laminated composite sheet in which the resin film and the work are laminated in this order in the thickness direction on the support sheet; cooling the second laminated composite sheet, and then dividing the work in the second laminated composite sheet on the support sheet and cutting the resin film to produce a third laminated composite sheet in which a plurality of chips with a resin film are fixed on the support sheet; and picking up the resin-film-attached chip in the third laminated composite sheet by separating it from the support sheet. Hereinafter, the production method according to the second embodiment may be referred to as "production method 2" in this specification.

[0250] 8 and 7A to 7E are cross-sectional views for typically explaining manufacturing method 2. Here, manufacturing method 2 will be explained by taking as an example a case where kit 1 in Fig. 6 including support sheet 10 shown in Fig. 1 is used.

[0251] In the step of producing the first laminated composite sheet in manufacturing method 2, first, the resin film-formed layer 13 in the kit 1 is attached to the back surface 9b of the work 9 to produce a first laminated film 601 in which the resin film-formed layer 13 and the work 9 are laminated in their thickness direction, as shown in Fig. 8. In this case, as in manufacturing method 1, the first surface 13a of the resin film-formed layer 13 in the first laminate 5 is attached to the back surface 9b of the work 9.

[0252] Here, the first release film 151 is removed from the first laminate 5 of the kit 1 shown in Fig. 6, and the first surface 13a of the resin film-formed layer 13 is attached to the back surface 9b of the work 9, but the second release film 152 may be removed from the resin film-formed layer 13 of the kit 1 shown in Fig. 6, and the second surface 13b of the resin film-formed layer 13 may be attached to the back surface 9b of the work 9. A circular punching blade may be applied to the first laminate 5 of the kit 1 shown in Fig. 6 from the side of the first release film 151 to peel off the first release film 151, and the circular outer side of the resin film-formed layer 13 may be removed together with the first release film 151, and the resulting circular first surface 13a of the resin film-formed layer 13 may be attached to the back surface 9b of the work 9.

[0253] The resin film forming layer 13 can be attached to the workpiece 9 by a known method. For example, the resin film forming layer 13 may be attached to the workpiece 9 while being heated.

[0254] Next, the adhesive layer 12 of the support sheet 10 in the kit 1 is attached to the resin film forming layer 13 in the first laminate film 601 to produce a first laminated composite sheet 501 in which the resin film forming layer 13 and the workpiece 9 are laminated in this order in the thickness direction on the support sheet 10.

[0255] The second release film 152 is removed from the resin film-formed layer 13 in the first laminate film 601. Then, one surface 10a of the support sheet 10 is attached to the newly exposed second surface 13b of the resin film-formed layer 13, as shown in Fig. 7A. The jig adhesive layer 16 may be provided thereafter. The support sheet 10 shown here is configured to include a base material 11 and an adhesive layer 12 provided on one surface 11a of the base material 11, and the adhesive layer 12 in the support sheet 10 is attached to a resin film-forming layer 13. A first surface 12a of the adhesive layer 12 on the resin film-forming layer 13 side is the same as the first surface 10a of the support sheet 10.

[0256] In the manufacturing method 2, the first laminated composite sheet 501 is the same as the first laminated composite sheet 501 in the manufacturing method 1.

[0257] In the manufacturing method 2, the step of preparing the second laminated composite sheet can be carried out in the same manner as in the step of preparing the second laminated composite sheet in the manufacturing method 1.

[0258] In the manufacturing method 2, the step of preparing the third laminated composite sheet can be carried out in the same manner as in the step of preparing the third laminated composite sheet in the manufacturing method 1.

[0259] In the manufacturing method 2, the picking up step can be performed in the same manner as the picking up step in the manufacturing method 1.

[0260] In manufacturing method 2 according to an embodiment of the present invention, since support sheet 10 has the above-described configuration, even if the peripheral portion of first laminated composite sheet 501 is heated while attached to a fixing jig and then second laminated composite sheet 502 is cooled, the effect of slackness of third laminated composite sheet 503 is eliminated, and the recognition ability of the chip by the pickup device can be improved.

[0261] <Manufacturing method 3> A manufacturing method according to a third embodiment is a method for manufacturing a resin film-coated chip including a chip and a resin film provided on a back surface of the chip, A process of attaching a resin film forming layer in a composite sheet for resin film formation according to the embodiment of the present invention described above to the back side of a workpiece, or attaching a resin film forming layer in kit 1 according to the embodiment of the present invention to the back side of a workpiece to produce a first laminate film in which the resin film forming layer and the workpiece are laminated in their thickness direction, and further attaching an adhesive layer of a support sheet in kit 1 to the resin film forming layer in the first laminate film to produce a first laminate composite sheet in which the resin film forming layer and the workpiece are laminated in this order in their thickness direction on the support sheet; A step of dividing the work in the first laminated composite sheet on the support sheet and cutting the resin film forming layer to produce a fourth laminated composite sheet in which a plurality of chips with a resin film forming layer are fixed on the support sheet; a step of heating and cooling the fourth laminated composite sheet while the peripheral portion of the fourth laminated composite sheet is attached to a fixing jig, thereby hardening the resin film forming layer in the fourth laminated composite sheet and forming the resin film, thereby producing a third laminated composite sheet on the support sheet in which a plurality of resin film-coated chips are fixed on the support sheet; and picking up the resin-film-attached chip in the third laminated composite sheet by separating it from the support sheet. Hereinafter, the manufacturing method according to the third embodiment may be referred to as "manufacturing method 3" in this specification.

[0262] 9A to 9C and 7D to 7E are cross-sectional views for typically explaining manufacturing method 3. Here, manufacturing method 3 will be explained by taking as an example a case where a composite sheet 101 for resin film formation in FIG. 2 having a support sheet 10 shown in FIG. 1 is used.

[0263] In the step of producing the first laminated composite sheet in manufacturing method 3, as shown in FIG. 9A, the resin film forming layer 13 in the composite sheet for resin film formation 101 is attached to the rear surface 9b of the workpiece 9 to produce a first laminated composite sheet 501 in which the resin film forming layer 13 and the workpiece 9 are laminated in this order in the thickness direction on the support sheet 10. The first laminated composite sheet 501 in FIG. 9A is the same as the first laminated composite sheet 501 in FIG. 7A.

[0264] Next, in the step of producing the fourth laminated composite sheet of manufacturing method 3, as shown in Fig. 9B, the work 9 in the first laminated composite sheet 501 is divided on the support sheet 10, and the resin film forming layer 13 is cut. The work 9 is divided into individual pieces into a plurality of chips 90.

[0265] The division of the work 9 and the cutting of the resin film-formed layer 13 may be performed by a known method. For example, the division of the work 9 and the cutting of the resin film-formed layer 13 are performed along the outer periphery of the chip 90 by dicing such as blade dicing, laser dicing by laser irradiation, or water dicing by spraying water containing an abrasive, regardless of the cutting method.

[0266] In this manner, by dividing the workpiece 9 and cutting the resin film-formed layer 13, a plurality of chips 902 with a resin film-formed layer are obtained, each chip 90 including a resin film-formed layer (sometimes simply referred to as a "resin film-formed layer" in this specification) 130 after cutting provided on the back surface 90b of the chip 90. Reference numeral 130b indicates the surface of the resin film-formed layer 130 after cutting that was the second surface 13b of the resin film-formed layer 13 (sometimes referred to as a "second surface" in this specification).

[0267] In the step of producing the fourth laminated composite sheet in manufacturing method 3, a fourth laminated composite sheet 504 in which a plurality of chips 902 with a resin film forming layer are fixed on the support sheet 10 is produced as described above.

[0268] Next, in the process of producing the third laminated composite sheet in manufacturing method 3, as shown in FIG. 9C, the peripheral portion of the fourth laminated composite sheet 504 is attached to a fixing jig 18 such as a ring frame, and the fourth laminated composite sheet 504 is heated and cooled to harden the resin film forming layer 130 in the fourth laminated composite sheet 504 and form the resin film 130', as shown in FIG. 7D.

[0269] In the manufacturing method 3, the third laminated composite sheet 503 is the same as the third laminated composite sheet 503 in the manufacturing method 1.

[0270] In the manufacturing method 3, the picking up step can be performed in the same manner as the picking up step in the manufacturing method 1.

[0271] In manufacturing method 3 according to an embodiment of the present invention, since support sheet 10 has the above-described configuration, even if the peripheral portion of fourth laminated composite sheet 504 is heated while attached to fixing jig 18 such as a ring frame, and then third laminated composite sheet 503 is cooled, the effect of slackness of third laminated composite sheet 503 is eliminated, and the recognition ability of the chip by the pickup device can be improved.

[0272] The explanation of manufacturing method 3 so far has been given for the case where a composite sheet 101 for forming a resin film having a support sheet 10 shown in FIG. 2 is used. However, in manufacturing method 3, a composite sheet for forming a resin film of this embodiment other than the composite sheet 101 for forming a resin film, such as the composite sheet 102 for forming a resin film, the composite sheet 103 for forming a resin film or the composite sheet 104 for forming a resin film shown in FIGS. 3 to 5 may also be used.

[0273] In the step of producing the first laminated composite sheet in manufacturing method 3, kit 1 shown in FIG. 6 is used, and resin film forming layer 13 in kit 1 is attached to the back surface 9b of work 9 to produce a first laminated film 601 in which the resin film forming layer 13 and work 9 are laminated in their thickness direction as shown in FIG. 8, and further, adhesive layer 12 of support sheet 10 in kit 1 is attached to the resin film forming layer 13 in the first laminated film 601 to produce a first laminated composite sheet 501.

[0274] ◇ Manufacturing method of substrate device (method of using chip with resin film) After the chip with a resin film is obtained by the above-mentioned manufacturing method, a substrate device can be manufactured in the same manner as the conventional substrate device manufacturing method, except that this chip with a resin film is used instead of the conventional substrate device.

[0275] For example, when the resin film forming layer is a protective film forming film and the resin film-coated chip is a protective film-coated chip, a manufacturing method can be mentioned that includes a flip chip connection step in which the protective film-coated chip obtained using the protective film-coated film is picked up from a support sheet, and the protruding electrode on the resin film-coated chip is brought into contact with a connection pad on a circuit board, thereby electrically connecting the protruding electrode and the connection pad on the circuit board.

[0276] In the case where the resin film forming layer is a film-like adhesive and the chip with resin film is a chip with a film-like adhesive, a manufacturing method can be mentioned which has a connection step in which a chip with a resin film forming layer obtained using the film-like adhesive is picked up from a support sheet, and the chip with a resin film is attached to a circuit board via the film-like adhesive. EXAMPLES

[0277] The present invention will be described in more detail below with reference to specific examples, although the present invention is not limited to the following examples.

[0278] [Example 1] In Example 1, the support sheet 10 shown in FIG. 1 and the composite sheet for resin film formation 101 shown in FIG. 2 in which the resin film formation layer is a protective film-forming film were produced as follows.

[0279] (1) Preparation of a first laminate including a protective film-forming film The following components (a) to (g) were mixed and diluted with methyl ethyl ketone to a solids concentration of 50 mass %, to prepare a composition for forming a protective film.

[0280] (a) Polymer component: (meth)acrylic acid ester copolymer (a copolymer obtained by copolymerizing 10 parts by mass of n-butyl acrylate, 70 parts by mass of methyl acrylate, 5 parts by mass of glycidyl methacrylate, and 15 parts by mass of 2-hydroxyethyl acrylate, weight average molecular weight: 800,000, glass transition temperature: -1°C) 120 parts by mass (solid content equivalent, the same below) (b-1) Thermosetting component: 60 parts by mass of bisphenol A type epoxy resin (manufactured by Mitsubishi Chemical Corporation, product name "jER828", epoxy equivalent 184 to 194 g / eq) (b-2) Thermosetting component: 10 parts by mass of bisphenol A type epoxy resin (manufactured by Mitsubishi Chemical Corporation, product name "jER1055", epoxy equivalent 800 to 900 g / eq) (b-3) Thermosetting component: 30 parts by mass of dicyclopentadiene type epoxy resin (manufactured by Dainippon Ink and Chemicals, Inc., product name "Epicron HP-7200HH", epoxy equivalent 255 to 260 g / eq) (c) Heat-activated latent epoxy resin curing agent: dicyandiamide (ADEKA Corporation: ADEKA Hardener EH3636AS, active hydrogen content 21 g / eq) 3 parts by mass (d) Curing accelerator: 2-phenyl-4,5-dihydroxymethylimidazole (manufactured by Shikoku Chemical Industry Co., Ltd., product name "Curesol 2PHZ") 3 parts by mass (e) Filler: Silica filler (manufactured by Admatechs Co., Ltd., product name "SC2050MA", average particle size: 0.5 μm) 290 parts by mass (f) Colorant: Carbon black (manufactured by Mitsubishi Chemical Corporation, product name "#MA650", average particle size: 28 nm) 1.2 parts by mass (g) Silane coupling agent: (manufactured by Shin-Etsu Chemical Co., Ltd., product name "KBM-403") 2 parts by mass

[0281] A first release film (manufactured by Lintec Corporation, product name "SP-PET381031") consisting of a 38 μm-thick polyethylene terephthalate (PET) film with a silicone-based release agent layer formed on one side, and a second release film (manufactured by Lintec Corporation, product name "SP-PET381130") consisting of a 38 μm-thick PET film with a silicone-based release agent layer formed on one side were prepared.

[0282] First, the above-mentioned protective film-forming composition was applied to the release surface of the first release film by a knife coater, and dried to form a protective film-forming film having a thickness of 25 μm. Then, the release surface of the second release film was placed on the protective film-forming film and the two were bonded together to obtain a laminate consisting of the first release film, the protective film-forming film (thickness: 25 μm), and the second release film. This laminate was long and was wound up into a roll-shaped wound body.

[0283] (2) Preparation of a second laminate including a support sheet The following components (h) and (i) were mixed and diluted with methyl ethyl ketone to a solids concentration of 25 mass % to prepare a pressure-sensitive adhesive composition.

[0284] (h) Adhesive base: (meth)acrylic acid ester copolymer (a copolymer obtained by copolymerizing 60 parts by mass of 2-ethylhexyl acrylate, 30 parts by mass of methyl methacrylate, and 10 parts by mass of 2-hydroxyethyl acrylate, weight average molecular weight: 600,000) 100 parts by mass (i) Crosslinking agent: 20 parts by mass of a xylene diisocyanate adduct of trimethylolpropane (manufactured by Mitsui Takeda Chemicals, Inc., product name "Takenate D110N")

[0285] As the release film, a release film (manufactured by Lintec Corporation, product name "SP-PET381031") was prepared, which was made by forming a silicone-based release agent layer on one side of a PET film having a thickness of 38 μm.

[0286] As a material for the substrate of the support sheet, a polypropylene film 1 (thickness: 80 μm) was prepared, which has a no-load stretch rate of 99% in the MD direction / 99% in the CD direction, a tensile modulus of 370 MPa in the MD direction / 350 MPa in the CD direction, and a melting point of 138° C. The polypropylene film 1 was stretched only in the MD direction at a temperature of 120° C. for 1 minute with a tension of 2 N / m to produce a substrate. The no-load stretch rate, tensile modulus, and melting point were measured as shown in the test examples described later (same below).

[0287] First, the above-mentioned adhesive composition was applied to the release surface of the release film using a knife coater, and dried at 100°C for 1 minute to form an adhesive layer having a thickness of 5 μm. Then, the above-mentioned substrate was attached to the adhesive layer to obtain a second laminate consisting of the support sheet of Example 1 consisting of the substrate and the adhesive layer, and the release film. This laminate was long. Then, the laminate was wound up into a roll-shaped roll.

[0288] (3) Preparation of a third laminate including a pressure-sensitive adhesive layer 16 for a jig The following components (j) and (k) were mixed and diluted with toluene to a solids concentration of 15 mass % to prepare a pressure-sensitive adhesive composition for use as a jig.

[0289] (j) Adhesive base: (meth)acrylic acid ester copolymer (a copolymer obtained by copolymerizing 69.5 parts by mass of butyl acrylate, 30 parts by mass of methyl acrylate, and 0.5 parts by mass of 2-hydroxyethyl acrylate, weight average molecular weight: 500,000) 100 parts by mass (k) Crosslinking agent: 5 parts by mass of tolylene diisocyanate crosslinking agent (Tosoh Corporation, Coronate L)

[0290] We prepared first and second release films (manufactured by Lintec Corporation, product name "SP-PET381031") consisting of a 38 μm thick PET film with a silicone-based release agent layer formed on one side, and a polyvinyl chloride film (manufactured by Okamoto Corporation, thickness: 50 μm) as a core material.

[0291] First, the above-mentioned adhesive composition for the jig was applied to the release surface of the first release film by a knife coater and dried to form a first adhesive layer having a thickness of 5 μm. Then, the above-mentioned core material was attached to the first adhesive layer to obtain a laminate A consisting of the core material, the first adhesive layer, and the first release film. This laminate A was long and was wound up into a roll-shaped wound body.

[0292] Next, the above-mentioned adhesive composition for the jig was applied to the release surface of the second release film using a knife coater and dried to form a second adhesive layer having a thickness of 5 μm. After that, the exposed surface of the core material in the laminate A was attached to the second adhesive layer to obtain a third laminate consisting of the first release film / first adhesive layer / core material / second adhesive layer / second release film. This laminate was long and was wound up into a roll-shaped wound body.

[0293] (4) Preparation of the fourth laminate The second release film was peeled off from the first laminate obtained in (1) above to expose the protective film-forming film. Meanwhile, the release film was peeled off from the second laminate obtained in (2) above to expose the adhesive layer. The first laminate and the second laminate were bonded together so that the protective film-forming film was in contact with the adhesive layer, and a fourth laminate was obtained in which a support sheet consisting of a base material and an adhesive layer, a protective film-forming film, and a first release film were laminated. The fourth laminate was long and was wound up into a roll-shaped wound body.

[0294] (5) Preparation of composite sheet for forming protective film The second release film was peeled off from the third laminate obtained in (3) above, leaving the first release film, and the inner peripheral edge of the jig pressure-sensitive adhesive layer was half-cut to remove the inner circular portion, so that the diameter of the inner peripheral edge of the jig pressure-sensitive adhesive layer was 345 mm.

[0295] The first release film was peeled off from the fourth laminate obtained in (4) above, and the exposed protective film-forming film and the jig adhesive layer exposed in the third laminate were superimposed and pressed together. Thereafter, the outer peripheral edge of the composite sheet for forming a protective film was half-cut to remove the outer portion, leaving the first release film in the third laminate. At this time, the diameter of the outer peripheral edge of the composite sheet for forming a protective film was 370 mm.

[0296] In this way, a composite sheet for forming a protective film of Example 1 was obtained, which was composed of a support sheet in which an adhesive layer (thickness: 5 μm) was laminated on a substrate, a protective film-forming film laminated on the adhesive layer side of the support sheet, a ring-shaped adhesive layer for a jig laminated on the peripheral portion of the protective film-forming film on the side opposite the support sheet, and a release film laminated on the adhesive layer for a jig on the side opposite the protective film-forming film. The release film in the composite sheet for forming a protective film was a continuous long piece, and the composite sheet for forming a protective film was wound up in a roll using the release film as a support to form a roll.

[0297] [Examples 2 to 6, Comparative Example 1] The polypropylene film 1 (thickness: 80 μm) was prepared as the material of the substrate of the support sheet. Then, the polypropylene film 1 was stretched in the direction, temperature, time, and tension shown in Table 1. Except for this, the substrates were prepared in the same manner as in Example 1, and the support sheet and the composite sheet for forming a protective film were manufactured.

[0298] [Comparative Example 2] As a material for the substrate of the support sheet, a polypropylene film 2 (thickness: 80 μm) was prepared, which had a load-free stretch rate of 100% in the MD direction and 100% in the CD direction, a tensile modulus of 450 MPa in the MD direction and 440 MPa in the CD direction, and a melting point of 155° C. The substrate was produced in the same manner as in Example 1, except that the polypropylene film 2 was stretched only in the MD direction at a temperature of 120° C. for 1 minute with a tension of 1 N / m, and a support sheet and a composite sheet for forming a protective film were manufactured.

[0299] [Test Example 1] <Measurement of expansion rate without load> The polypropylene film 1 and the polypropylene film 2 used in the examples and comparative examples were cut to a size of 22 mm on the short side and 110 mm on the long side so that the short side was in the CD direction and the long side was in the MD direction, respectively, to prepare a test piece in the MD direction. Of the 110 mm length, 100 mm from the center in the length direction was marked on the test piece as the measurement distance, and a clip with a mass of 2.2 g was attached to one end of the test piece in the length direction (5 mm from the end).

[0300] The test piece was hung in an oven using a clip. After heating in the oven at 130°C and 30% RH for 2 hours, the test piece was removed from the oven and cooled to 23°C. The distance between the marked areas on the test piece was then measured again, and the no-load expansion rate (%) of the substrate was calculated based on the following formula. Elongation rate without load (%) = (measurement distance after heating / measurement distance before heating) x 100

[0301] The polypropylene film 1 and the polypropylene film 2 used in the examples and comparative examples were cut into a size of 22 mm on the short side and 110 mm on the long side so that the short side was in the MD direction and the long side was in the CD direction, respectively, to prepare a test piece in the CD direction. The no-load stretch rate (%) of the test piece in the CD direction was calculated in the same manner as above.

[0302] [Test Example 2] <Tensile elastic modulus measurement> The polypropylene film 1 and the polypropylene film 2 used in the examples and comparative examples were each cut into a test piece of 15 mm x 140 mm, and the tensile modulus (Young's modulus) at 23°C was measured in accordance with JIS K7127:1999. Specifically, the test piece was subjected to a tensile test at a speed of 200 mm / min using a tensile tester (manufactured by Shimadzu Corporation, product name "Autograph AG-IS 500N") with a chuck distance set to 100 mm, and the tensile modulus (MPa) was measured. The tensile modulus was measured in both the MD and CD directions of the substrate.

[0303] [Test Example 3] <Melt point measurement> The melting points of the polypropylene film 1 and the polypropylene film 2 used in the examples and comparative examples were measured using a thermogravimetric measuring device (manufactured by PerkinElmer, product name "Pyris1"). Specifically, the substrate was heated from 50°C to 250°C at 10°C per minute, and DSC (differential scanning calorimetry) measurement was performed, and the temperature at which an endothermic peak was observed was determined as the melting point.

[0304] [Test Example 4] <Loosening evaluation> The release film was peeled off from the composite sheet for forming a protective film produced in the examples and comparative examples, and the obtained composite sheet for forming a protective film was attached to a silicon wafer (#6000 polishing, diameter: 12 inches, thickness: 300 μm, mass: 50 g) and a ring frame (made of stainless steel, inner diameter 350 mm) as shown in Fig. 7A. In this state, the ring frame alone was held so that the silicon wafer surface was horizontal, and the protective film-forming film was hardened by heating in an environment of 130°C for 2 hours to form a protective film, and then cooled to room temperature.

[0305] The difference in height between the lower end face of the composite sheet for forming a protective film located under the ring frame and the lower end face of the composite sheet for forming a protective film located under the silicon wafer (amount of sinking; mm) was measured and evaluated as slack. The evaluation criteria are as follows. The results are shown in Table 1. A (Excellent): Less than 1.2 mm B (Good): 1.2mm or more, less than 3.0mm C (defective): 3.0mm or more

[0306] As a result of the above, the composite sheets for forming a protective film of Examples 1 to 6 were evaluated as A (excellent), and the composite sheets for forming a protective film of Comparative Examples 1 and 2 were evaluated as B (good).

[0307] [Test Example 5] <Thermo-mechanical analysis (TMA)> A rectangular test piece 20 mm long and 5 mm wide was cut out from the support sheet of each of the examples and comparative examples with the MD direction as the long side direction. Using a thermomechanical analyzer (Bruker AXS, "TMA-4000SA"), the temperature was raised from 23°C to 130°C with a chuck distance of 15 mm, load of 0.8 g, and heating rate of 10°C / min, and held for 30 minutes. After that, the temperature was cooled from 130°C to 50°C with a load of 0.8 g and a cooling rate of 1°C / min. The displacement [μm] during this period was recorded at a sampling rate of 1 s -1 was measured.

[0308] A rectangular test piece 20 mm long and 5 mm wide was cut out from the support sheet of each of the examples and comparative examples with the CD direction as the long side direction. Similarly, using a thermomechanical analyzer ("TMA-4000SA" manufactured by Bruker AXS Co., Ltd.), the temperature was raised from 23°C to 130°C with a chuck distance of 15 mm, a load of 0.8 g, and a heating rate of 10°C / min, and held for 30 minutes. Thereafter, the temperature was cooled from 130°C to 50°C with a load of 0.8 g and a cooling rate of 1°C / min. The displacement [μm] during this period was recorded at a sampling rate of 1 s -1 was measured.

[0309] Average displacement per degree when the temperature is increased from 23°C to 130°C (A 23→130 ) for the average displacement per degree Celsius when the temperature is increased from 60°C to 130°C (A 60→130 ) ratio [(A 60→130 ) / (A 23→130 )] was calculated using the following procedure.

[0310] Average displacement per degree when the temperature is increased from 23°C to 130°C (A 23→130 ) was calculated using the following formula: A 23→130 =(A 130 -A 23 ) / 107=A 130 / 107[μm / ℃]

[0311] Average displacement per degree when the temperature is increased from 60°C to 130°C (A 60→130 ) was calculated using the following formula: A 60→130 =(A 130 -A 60 ) / 70[μm / ℃]

[0312] Displacement at 23°C (A 23 )=0μm Displacement at 60°C (A 60 ) [μm] Displacement at 130℃ (A 130 ) [μm]

[0313] Average displacement per degree when cooled slowly from 130℃ to 50℃ (B130→50 ) was calculated using the following formula: B 130→50 =(B 50 -B 130 ) / 80[μm / ℃]

[0314] The absolute value of the average displacement per degree Celsius when slowly cooling from 130°C to 50°C (|B 130→50 |) was calculated using the following formula: |B 130→50 |=|B 50 -B 130 | / 80[μm / ℃]

[0315] Displacement after holding at 130℃ for 30 minutes (B 130 ) [μm] Displacement at 50℃ after slow cooling (B 50 ) [μm]

[0316] The average displacement (A 23→130 ) from the absolute value of the average displacement (|B 130→50 |) minus [(A 23→130 )-|B 130→50 |] was requested.

[0317] The results of the above thermomechanical analysis (TMA) are shown in Table 1.

[0318] Here, "in the flow direction (MD) [(A 23→130 )-|B 130→50 |] value in the vertical direction (CD) 23→130 )-|B 130→50 The absolute value of the difference between the "value of |" and the "balance evaluation value of MD and CD" was calculated. The calculation results are shown in Table 1. The balance evaluation value of MD and CD is preferably 3.0 or less, more preferably 2.5 or less, even more preferably 2.0 or less, and particularly preferably 1.8 or less. By having a small balance evaluation value of MD and CD, it is possible to reduce the risk that the support sheet or the composite sheet for resin film formation peels off from the fixing jig after heating and cooling, and falls off starting from this.

[0319] [Test Example 6] <Evaluation of chip recognition> (Manufacturing semiconductor chips with protective film) The protective film-forming film side of the protective film-forming composite sheet was attached to the polished surface of a silicon wafer (#6000 polishing, diameter: 12 inches, thickness: 300 μm, mass: 50 g) using a tape mounter (manufactured by Lintec Corporation, product name: Adwill (registered trademark) RAD2500), and a first laminated composite sheet was formed on the support sheet by laminating the protective film-forming film and the silicon wafer in this order in the thickness direction, and the peripheral portion of the first laminated composite sheet was fixed to a ring frame (made of stainless steel, inner diameter 350 mm) for wafer dicing (FIG. 7A). Next, the ring frame alone was held so that the silicon wafer surface was horizontal, and the sheet was heated in an oven manufactured by ESPEC Corporation at 130° C. for 2 hours (FIG. 7B), and the protective film-forming film was hardened to form a second laminated composite sheet on the support sheet by laminating the protective film and the silicon wafer in this order in the thickness direction, and the second laminated composite sheet was cooled to 23° C. (FIG. 7C).

[0320] Next, using a dicing device (DISCO Corporation, DFD6361), the silicon wafer and protective film were diced into chips of 3 mm x 3 mm on the support sheet at a cutting speed of 30 mm / s and a rotation speed of 40,000 rpm to form a third laminated composite sheet in which multiple chips with protective film were fixed on the support sheet (Figure 7D). The cutting depth during dicing was set to 20 μm into the support sheet. The dicing blade used was ZH05-SD2000-D1-90 CC, manufactured by DISCO Corporation. Using a pick-up die bonding device (Canon Machinery's "BESTEM D-510"), 500 chips were recognized using the auto trace function, and the chips that could be recognized were rated as A (excellent), and the chips that could be recognized less than 500 were rated as B (poor). The results are shown in Table 1.

[0321] Similarly, using a dicing device (DISCO Corporation, DFD6361), the silicon wafer and protective film were diced into chips of 3 mm x 1.5 mm on the support sheet at a cutting speed of 30 mm / s and a rotation speed of 40,000 rpm to form a third laminated composite sheet in which multiple chips with protective film were fixed on the support sheet (Figure 7D). The cutting depth during dicing was set to 20 μm into the support sheet. Similarly, using a pick-up die bonding device (Canon Machinery's "BESTEM D-510"), 500 chips were recognized using the auto trace function, and the chips that could be recognized were rated as A (excellent), and the chips that could be recognized less than 500 were rated as B (poor). The results are shown in Table 1.

[0322] [Table 1]

[0323] When the chips were diced to a chip size of 3 mm x 3 mm and the chip recognizability was evaluated, in Comparative Examples 1 and 2, the number of recognizable chips was less than 500 in all cases, resulting in a grade of B (poor), whereas in Examples 1 to 6, the number of recognizable chips was 500 in all cases, resulting in a grade of A (excellent).

[0324] When the chips were diced to a chip size of 3 mm x 1.5 mm and the chip recognizability was evaluated, in Comparative Examples 1 and 2, the number of recognizable chips was less than 500 in all cases, resulting in a grade of B (poor), whereas in Examples 2, and 4 to 6, the number of recognizable chips was 500 in all cases, resulting in a grade of A (excellent). [Industrial Applicability]

[0325] The present invention can be used in the manufacture of various substrate devices, including semiconductor devices. [Explanation of symbols]

[0326] 1... kit, 5... first laminate, 10, 20... Support sheet, 10a... One side (first side) of the support sheet, 11...base material, 12...adhesive layer, 13, 23 ... resin film forming layer, 13' ... resin film, 13b' ... other surface (second surface) of the resin film, 130 ... resin film forming layer after cutting, 130' ... resin film after cutting, 101, 102, 103, 104 ... Composite sheet for forming resin film, 501...first laminated composite sheet, 502...second laminated composite sheet, 503...third laminated composite sheet, 504...fourth laminated composite sheet, 16...adhesive layer for jig, 15...release film, 15...release film, 151...first release film, 152...second release film, 18...fixing jig, 601...first laminated film, 9... workpiece, 9b... back surface of workpiece, 90... chip, 90b... back surface of chip, 901... chip with resin film, 902... chip with resin film forming layer

Claims

1. A support sheet used for heating a workpiece or a chip obtained by dividing the workpiece, When the support sheet was subjected to thermomechanical analysis (TMA) in a tensile mode in either the machine direction (MD) or the cross direction (CD) under the following conditions, Displacement at 130°C (A 130 ) is 500 μm or less, Average displacement per degree Celsius when the temperature is increased from 23° C. to 130° C. (A 23→130 ) is the absolute value of the average displacement per 1°C when slowly cooled from 130°C to 50°C (|B 130→50 |) A support sheet that is smaller than the original. <Thermo-mechanical analysis (TMA) conditions> Sample size: length 20 mm, width 5 mm Chuck distance: 15 mm The temperature is raised from 23° C. to 130° C. with a load of 0.8 g and a heating rate of 10° C. / min, and maintained at that temperature for 30 minutes. Thereafter, the temperature is cooled from 130° C. to 50° C. with a load of 0.8 g and a cooling rate of 1° C. / min. The displacement [μm] during this period is measured.

2. When the support sheet was subjected to thermomechanical analysis (TMA) in a tensile mode in the machine direction (MD) and a tensile mode in the cross direction (CD) under the above conditions, Displacement at 130°C (A 130 ) are all 500 μm or less, Average displacement per degree Celsius when the temperature is increased from 23° C. to 130° C. (A 23→130 ) is the absolute value of the average displacement per 1°C when slowly cooled from 130°C to 50°C (|B 130→50 The support sheet according to claim 1, wherein each of the above is smaller than |.

3. When the support sheet was subjected to thermomechanical analysis (TMA) in a tensile mode in either the machine direction (MD) or the cross direction (CD) under the above conditions, Average displacement per degree Celsius when the temperature is increased from 23° C. to 130° C. (A 23→130 3. The support sheet according to claim 1 or 2, wherein the value of is a positive value.

4. When the support sheet was subjected to thermomechanical analysis (TMA) in a tensile mode in the machine direction (MD) and a tensile mode in the cross direction (CD) under the above conditions, Average displacement per degree Celsius when the temperature is increased from 23° C. to 130° C. (A 23→130 4. The support sheet according to claim 3, wherein all of the above are positive values.

5. When the support sheet was subjected to thermomechanical analysis (TMA) in a tensile mode in either the machine direction (MD) or the cross direction (CD) under the above conditions, Average displacement per degree Celsius when the temperature is increased from 23° C. to 130° C. (A 23→130 ) relative to the average displacement (A 60→130 5. The support sheet according to claim 3 or 4, wherein the ratio of

6. When the support sheet was subjected to thermomechanical analysis (TMA) in a tensile mode in the machine direction (MD) and a tensile mode in the cross direction (CD) under the above conditions, Average displacement per degree Celsius when the temperature is increased from 23° C. to 130° C. (A 23→130 ) relative to the average displacement (A 60→130 6. The support sheet of claim 5, wherein the ratios of are all less than 1.

7. The support sheet according to any one of claims 1 to 6, wherein the support sheet is made of only a substrate, or comprises a substrate and an adhesive layer provided on one side of the substrate, and the constituent material of the substrate contains a polyolefin resin.

8. The support sheet according to any one of claims 1 to 7, wherein the support sheet is composed of only a substrate, or comprises a substrate and a pressure-sensitive adhesive layer provided on one surface of the substrate, and the substrate is a stretched film.

9. The support sheet according to any one of claims 1 to 8, wherein the support sheet is in a roll form.

10. A composite sheet for resin film formation, comprising: a support sheet according to any one of claims 1 to 8; and a resin film forming layer provided on one surface of the support sheet.

11. The composite sheet for resin film formation according to claim 10 , wherein the resin film forming layer is a protective film forming film.

12. The composite sheet for resin film formation according to claim 10 or 11, which is in a roll form.

13. A kit comprising a first laminate in which a first release film, a resin film forming layer and a second release film are laminated in this order, and a support sheet described in any one of claims 1 to 9, which is used to support a workpiece to which the resin film forming layer is to be attached and the resin film forming layer.

14. The kit according to claim 13 , wherein the resin film forming layer is a protective film forming film.

15. The kit of claim 13 or 14, wherein the first laminate is in roll form.

16. A method for manufacturing a resin-film-coated chip comprising: a chip; and a resin film provided on a back surface of the chip, the method comprising: A process of attaching a resin film forming layer in a composite sheet for resin film formation according to any one of claims 10 to 12 to the back surface of a workpiece, or attaching a resin film forming layer in a kit according to any one of claims 13 to 15 to the back surface of a workpiece to produce a first laminate film in which the resin film forming layer and the workpiece are laminated in their thickness direction, and further attaching a support sheet in the kit to the resin film forming layer in the first laminate film to produce a first laminate composite sheet in which the resin film forming layer and the workpiece are laminated in this order in their thickness direction on the support sheet; a step of heating the first laminated composite sheet while the peripheral portion of the first laminated composite sheet is attached to a fixing jig, hardening the resin film forming layer, and forming the resin film, thereby producing a second laminated composite sheet in which the resin film and the workpiece are laminated in this order in the thickness direction on the support sheet; cooling the second laminated composite sheet, and then dividing the work in the second laminated composite sheet on the support sheet and cutting the resin film to produce a third laminated composite sheet having a plurality of resin-film-coated chips fixed on the support sheet; and picking up the resin-film-coated chip in the third laminated composite sheet by separating it from the support sheet.

17. A method for manufacturing a resin-film-coated chip comprising: a chip; and a resin film provided on a back surface of the chip, the method comprising: A process of attaching a resin film forming layer in a composite sheet for resin film formation according to any one of claims 10 to 12 to the back surface of a workpiece, or attaching a resin film forming layer in a kit according to any one of claims 13 to 15 to the back surface of a workpiece to produce a first laminate film in which the resin film forming layer and the workpiece are laminated in their thickness direction, and further attaching a support sheet in the kit to the resin film forming layer in the first laminate film to produce a first laminate composite sheet in which the resin film forming layer and the workpiece are laminated in this order in their thickness direction on the support sheet; A step of dividing the work in the first laminated composite sheet on the support sheet and cutting the resin film forming layer to produce a fourth laminated composite sheet in which a plurality of chips with a resin film forming layer are fixed on the support sheet; a step of heating and cooling the fourth laminated composite sheet while the peripheral portion of the fourth laminated composite sheet is attached to a fixing jig, thereby hardening the resin film forming layer in the fourth laminated composite sheet and forming the resin film, thereby producing a third laminated composite sheet on the support sheet in which a plurality of chips with a resin film are fixed on the support sheet; and picking up the resin-film-coated chip in the third laminated composite sheet by separating it from the support sheet.

Citation Information

Patent Citations

  • Polyester film and its production

    JP2000141472A

  • Composite sheet for protection film formation

    JP2016015456A

  • Heat-resistant pressure-sensitive adhesive tape for production of semiconductor device and method for producing semiconductor device using the tape

    US20130244377A1

  • Composite sheet for forming protective film

    WO2015178346A1

  • Dicing sheet

    WO2015190230A1