Material system and method for making the material system
The material system with alternating aluminum, glass composite, and carbon composite layers, bonded by thermoplastic resins, addresses the need for improved resistance and reduced weight in industries by enhancing structural support and stability.
Patent Information
- Application Number
- JP2022167351
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2016-12-14
- Filing Date
- 2022-10-19
- Publication Date
- 2024-11-28
- Estimated Expiration
- 2037-12-12
AI Technical Summary
Existing material systems, such as fiber metal laminates (FML), do not adequately address the need for improved resistance to corrosion, fatigue, fire, impact, and reduced weight in industries like aerospace, automotive, and rail transportation.
A material system comprising alternating layers of aluminum, glass composite, and carbon composite, bonded by thermoplastic resins like PEEK or PEKK, with integrated thermoplastic prepreg plies to soften the aluminum layers, enhancing structural support and reducing weight.
The system provides enhanced resistance to corrosion, fatigue, and impact while maintaining reduced weight, offering improved structural strength and stability through the use of thermoplastic bonding and layer integration processes.
Smart Images

Figure 0007591544000005 
Figure 0007591544000006 
Figure 0007591544000007
Abstract
Description
[Technical field]
[0001] The subject matter described herein generally relates to material systems and / or methods of making material systems. More specifically, the subject matter described herein relates to material systems including aluminum, glass composite, and / or carbon composite layers and / or methods of making material systems including aluminum, glass composite, and / or carbon composite layers. [Background technology]
[0002] Material systems may include aluminum, glass composite, and / or carbon composite layers. Such material systems may be classified, for example, as fiber metal laminates (FML). Compared to simple metal structures, FML materials may exhibit unique advantages. Such advantages may include, for example, improved resistance to corrosion, fatigue, fire, and / or impact. Additionally or alternatively, such advantages may include, for example, specialized strength properties and / or reduced weight for a given volume.
[0003] Many industries, such as aerospace, automotive, and rail transportation, are continually being challenged to push the boundaries of conventional technology in material systems and methods for manufacturing such systems, and therefore there is a need for improved material systems and methods for manufacturing such systems. Summary of the Invention
[0004] The present disclosure is directed to a material system. In some examples, the material system may include a first aluminum layer, a first glass composite layer adjacent to the first aluminum layer, and / or a first carbon composite layer adjacent to the first glass composite layer and opposite the first aluminum layer. The first glass composite layer may include a first thermoplastic resin. The first thermoplastic resin may bond the first aluminum layer and the first glass composite layer.
[0005] In some embodiments, the first thermoplastic resin can bond the first glass composite layer and the first carbon composite layer.
[0006] In some examples, the first thermoplastic resin may include polyetheretherketone ("PEEK") or polyetherketoneketone ("PEKK").
[0007] In some embodiments, the first carbon composite layer can include a second thermoplastic resin.
[0008] In some examples, the second thermoplastic resin may include polyetheretherketone ("PEEK") or polyetherketoneketone ("PEKK").
[0009] In some embodiments, the first thermoplastic resin may be the same as the second thermoplastic resin.
[0010] In some embodiments, the first thermoplastic resin can be different from the second thermoplastic resin.
[0011] In some embodiments, the system may further include a second glass composite layer adjacent to the first carbon composite layer and on an opposite side to the first glass composite layer.
[0012] In some embodiments, the system may further include a second aluminum layer adjacent to the second glass composite layer and opposite the first carbon composite layer.
[0013] In some embodiments, the system may further include a second carbon composite layer adjacent to the second glass composite layer and opposite the first carbon composite layer.
[0014] In some embodiments, the first aluminum layer may include multiple first aluminum sub-layers.
[0015] In some embodiments, the first glass composite layer may include multiple first glass composite sub-layers.
[0016] In some embodiments, the first carbon composite layer may include multiple first carbon composite sub-layers.
[0017] In some embodiments, the first glass composite layer can include woven glass, the strength of which can vary depending on the orientation of the woven glass.
[0018] The present disclosure is further directed to methods of making the material system. In some examples, the method of making the material system may include laminating an aluminum layer, a glass composite layer including one or more thermoplastic prepreg plies, and a carbon composite layer such that the aluminum layer is adjacent to the glass composite layer in the laminate and the glass composite layer is adjacent to the carbon composite layer in the laminate, and / or consolidating the one or more thermoplastic prepreg plies at a temperature sufficient to soften the aluminum layer.
[0019] In some embodiments, one or more thermoplastic prepreg plies may include polyetheretherketone ("PEEK") or polyetherketoneketone ("PEKK").
[0020] In some examples, consolidating one or more thermoplastic prepreg plies may include raising the temperature of the one or more thermoplastic prepreg plies to 600° F. or greater.
[0021] In some examples, consolidating one or more thermoplastic prepreg plies may include raising the temperature of the laminate to 600° F. or higher.
[0022] The present disclosure is further directed to methods of making the material system, which in some exemplary embodiments may include stacking an aluminum layer, a glass composite layer with a thermoplastic resin, and a carbon composite layer such that the glass composite layer is between the aluminum layer and the carbon composite layer in the stack, and / or adjusting the temperature and pressure of the stack to consolidate the stack.
[0023] In some examples, the thermoplastic resin may include polyetheretherketone ("PEEK") or polyetherketoneketone ("PEKK").
[0024] It is to be understood that both the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present disclosure, as claimed. [Brief description of the drawings]
[0025] The above and / or other aspects and advantages will become more apparent and will be more readily understood from the following detailed description of the embodiments taken in conjunction with the accompanying drawings.
[0026] [Figure 1A] 1 illustrates a material system according to some embodiments of the disclosed material system. [Figure 1B] 1 illustrates a material system according to some embodiments of the disclosed material system. [Figure 1C] 1 illustrates a material system according to some embodiments of the disclosed material system. [Figure 1D] 1 illustrates a material system according to some embodiments of the disclosed material system. [Figure 1E] 1 illustrates a material system according to some embodiments of the disclosed material system. [Figure 2A] 1 illustrates a material system according to some embodiments of the disclosed material system. [Figure 2B] 1 illustrates a material system according to some embodiments of the disclosed material system. [Figure 2C] 1 illustrates a material system according to some embodiments of the disclosed material system. [Figure 2D] 1 illustrates a material system according to some embodiments of the disclosed material system. [Figure 2E] 1 illustrates a material system according to some embodiments of the disclosed material system. [Figure 3A] 1 illustrates the laying up of a first layer onto a forming tool according to some embodiments of the disclosed material system. [Figure 3B] 3B illustrates laying up a second layer onto the first layer of FIG. 3A according to some embodiments of the disclosed material system. [Figure 3C] 3C illustrates laying up a third layer onto the second layer of FIG. 3B, according to some embodiments of the disclosed material system. [Figure 3D] 1 illustrates a laminate including a first carbon composite layer, a first glass composite layer, a second carbon composite layer, a second glass composite layer, and / or an aluminum layer according to several embodiments of the disclosed material system. [Figure 4A] FIG. 1 shows temperature versus time profiles for consolidating one or more thermoplastic prepreg plies at a temperature sufficient to soften the aluminum layer or for adjusting the temperature and pressure of the laminate according to several embodiments of the disclosed material system. [Figure 4B] FIG. 1 shows pressure versus time profiles for consolidating one or more thermoplastic prepreg plies at a temperature sufficient to soften the aluminum layer or for adjusting the temperature and pressure of a laminate according to several embodiments of the disclosed material system. [Figure 4C] FIG. 1 shows temperature and pressure versus time profiles for consolidating one or more thermoplastic prepreg plies at a temperature sufficient to soften the aluminum layer or for adjusting the temperature and pressure of a laminate according to several embodiments of the disclosed material system. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] Exemplary aspects will now be described more fully with reference to the accompanying drawings. However, the embodiments of the present disclosure may be embodied in many different forms and should not be construed as being limited to the embodiments set forth herein. Rather, these embodiments are presented so that this disclosure will be thorough and complete, and will fully convey the scope to those skilled in the art. In the drawings, some details may be simplified and / or illustrated to facilitate understanding, rather than maintaining strict structural accuracy, detail, and / or scale. For example, thicknesses of layers and regions may be exaggerated for clarity.
[0028] When an element is described as being "on," "connected to," "electrically connected to," or "coupled to" another element, it is understood that the element may be directly on, electrically connected to, or coupled to the other element, or there may be intervening components. In contrast, when an element is described as being "directly on," "directly connected to," "directly electrically connected to," or "directly coupled to" another element, there are no intervening components. As used herein, the term "and / or" includes any and all combinations of one or more of the associated listed items.
[0029] Terms such as first, second, third, etc. may be used herein to describe various elements, components, regions, layers, and / or sections, but it should be understood that these elements, components, regions, layers, and / or sections should not be limited to these terms. These terms are used only to distinguish one element, component, region, layer, and / or section from another element, component, region, layer, and / or section. For example, a first element, component, region, layer, and / or section may be referred to as a second element, component, region, layer, and / or section without departing from the teachings of the embodiment.
[0030] Spatial terms such as "beneath," "below," "lower," "above," "upper," and the like may be used herein for ease of description to describe the relationship of one component and / or feature to another component and / or feature, or to one or more other components and / or features. Spatial terms are intended to encompass various orientations of the device in use or operation in addition to the orientation shown in the drawings.
[0031] The terms used herein are for the purpose of describing particular embodiments only and are not intended to limit the embodiments. As used herein, the singular forms "a," "an," and "the" are intended to include the plural unless the context clearly indicates otherwise. Furthermore, it will be understood that the terms "comprises," "comprising," "includes," and / or "including," when used herein, specify the presence of stated features, integers, steps, operations, elements, and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components, and / or groups thereof.
[0032] Unless otherwise defined, all terms used herein (including technical and scientific terms) have the same meaning as commonly understood by those skilled in the art to which the examples belong. Furthermore, it will be understood that terms as defined in commonly used dictionaries should be interpreted to have a meaning consistent with the meaning in the context of the relevant art, and should not be interpreted as an idealized or overly formal meaning unless expressly defined herein.
[0033] The present disclosure is directed to material systems and / or methods of manufacturing the material systems. FIG. 1A illustrates a material system 100A in accordance with some embodiments of the disclosed material systems. As shown in FIG. 1A, the material system 100A includes an aluminum layer 102A, a glass composite layer 104A adjacent to the aluminum layer 102A, and a carbon composite layer 106A adjacent to the glass composite layer 104A and opposite the aluminum layer 102A. The glass composite layer 104A can include a first thermoplastic resin. The first thermoplastic resin can bond the aluminum layer 102A and the glass composite layer 104A.
[0034] Material system 100A can provide, for example, a reduction in weight for a given volume compared to simple metal structures.
[0035] The aluminum layer 102A, the glass composite layer 104A, and the carbon composite layer 106A may have the same thickness or may have different thicknesses.
[0036] The aluminum layer 102A may or may not have an aluminum sub-layer, the glass composite layer 104A may or may not have a glass composite sub-layer, and / or the carbon composite layer 106A may or may not have a carbon composite sub-layer.
[0037] As used herein, the term "aluminum" refers to the metallic element having atomic number 13 and includes any isotope thereof.
[0038] As used herein, the term "alloy" means a solid or liquid mixture of two or more metals, or one or more metals with one or more non-metallic elements, such as carbon steel.
[0039] The term "layer" as used herein means a material of a constant thickness deposited, formed, or spread on a surface, body, or a portion of a surface or body. A layer may cover a surface, body, or a portion of a surface or body, or may form an overlapping portion or segment on a material covering a surface, body, or a portion of a surface or body. A layer may have a constant or variable thickness.
[0040] The term "aluminum layer" as used herein means a layer that includes aluminum. The aluminum layer may include, for example, pure aluminum, an aluminum alloy, or any other material that includes aluminum. The aluminum layer may include, for example, 1100 series aluminum (e.g., commercially available pure aluminum alloys such as 1100-O, 1100-H12, 1100-H14, 1100-H16, 1100-H18, 1100-H22, 1100-H24, 1100-H26, 1100-H28, 1100-H112, or 1100-H113 aluminum according to the International Alloy Designation System (IADS)).More generally, the aluminum layer may be, for example, a 1000 series aluminum alloy (e.g., aluminum alloys 1050, 1060, 1100, 1145, 1199, 1200, 1230, or 1350 according to the IADS), a 2000 series aluminum alloy (e.g., aluminum alloys 2008, 2011, 2014, 2017, 2018, 2024, 2025, 2036, 2048, 2090, 2117, 2120, 2130, 2140, 2150, 2160, 2170, 2180, 2190, 2200, 2219, 2221, 2230, 2240, 2250, 2260, 2270, 2280, 2290, 2300, 2310, 2320, 2330, 2340, 2350, 2360, 2370, 2380, 2390, 2400, 2410, 2420, 2430, 2440, 2450, 2460, 2470, 2480, 2490, 2500, 2510, 2520, 2530, 2540, 2550, 2560, 2570, 2580, 2590, 2610, 2620, 2630, 2640, 2650, 2660, 2670, 2680, 2690, , 2124, 2127, 2195, 2218, 2219, 2224, 2319, 2324, 2524, or 2618), 3000 series aluminum alloys (e.g. aluminum alloys 3003, 3004, 3005, 3102, or 3105 according to the IADS), 5000 series aluminum alloys (e.g. aluminum alloys 5005, 5050, 5052, 5056, 5059, 5083, 5086, 5090, 5091, 5092, 5093, 5094, 5095, 5096, 5097, 5098, 5099, 5000, 5001, 5002, 5003, 5004, 5005, 5006, 5007, 5008, 5009 ...10, 5011, 5012, 5013, 5014, 5015, 5016, 5017, 5018, 5019, 5020, 5021, 5022, 5023, 5024, 5025, 5026, 5027, 5028, 5029, 5030, 5031, 5032, 5033, 5034, 5035, 5036 154, 5182, 5183, 5252, 5254, 5356, 5357, 5454, 5456, 5457, 5554, 5556, 5652, 5654, 5657, or 5754), 6000 series aluminum alloys (e.g. 6003, 6005, 6005A, 6009, 6010, 6013, 6016, 6053, 6060, 6061, 6062, 6063, 6066, 6070, 6082, 6101, 61 05, 6111, 6151, 6162, 6201, 6205, 6253, 6262, 6351, 6463, or 6951), 7000 series aluminum alloys (e.g., 7001, 7005, 7008, 7022, 7039, 7049, 7050, 7055, 7068, 7072, 7075, 7076, 7079, 7108, 7116, 7129, 7150, 7175, 7178, or 7475 according to the IADS).
[0041] Pure aluminum, aluminum alloys, and / or other aluminum-containing materials described above are compatible with high temperature processing (e.g., temperatures required for thermoplastic processing or consolidation, but below the melting temperature of the pure aluminum, aluminum alloys, and / or other aluminum-containing materials, such as ≧600° F., ≧650° F., ≧675° F., or ≧700° F.). For example, pure aluminum, aluminum alloys, and / or other aluminum-containing materials described above may have low yield strengths (e.g., ≦7.2×103 pounds per square inch gauge (psig), ≦5.8×103 psig, ≦5.1×103 psig, or ≦4.3×103 psig), which reduces residual thermal stresses in other layers during and / or after cooling. Other factors may also facilitate reducing residual thermal stresses in other layers during and / or after cooling. These other factors include the thickness of the pure aluminum, aluminum alloys, and / or other aluminum containing materials, the presence and number of sublayers of pure aluminum, aluminum alloys, and / or other aluminum containing materials, and / or whether the pure aluminum, aluminum alloys, and / or other aluminum containing materials are in direct contact with a particular adjacent layer (e.g., a glass composite layer).
[0042] The surface of the aluminum layer may be subjected to a surface treatment such as alkaline degreasing, chromic acid anodizing or other anodizing, priming (e.g., with BR127 anti-corrosive primer), sol-gel, and / or acid washing in chromic-sulfuric acid. The surface may also be roughened, for example, by polishing. Such surface treatments may enhance the bond between the aluminum layer or layers and other layers.
[0043] The aluminum layer or layers may be relied upon to provide significant structural support. Typically, in this case, the number and / or thickness of the aluminum layer or layers is greater than if the aluminum layer or layers were not relied upon to provide significant structural support. Whether or not the aluminum layer or layers are relied upon to provide significant structural support, the thickness of the aluminum layer or layers may be, for example, ≧0.005 inches and ≦0.020 inches (e.g., 0.005 inches, 0.010 inches, 0.015 inches, or 0.020 inches). If relied upon to provide significant structural support, the thickness of the aluminum layer or layers may be greater than 0.0020 inches.
[0044] As used herein, the term "composite" refers to a macro-scale mixture or mechanical combination of two or more materials that are solid in their finished state, are incompatible with each other, and have different chemical properties.
[0045] As used herein, the term "tenacity" means the strength per weight of a fiber, typically expressed in grams per denier.
[0046] The term "fiber" as used herein refers to the fundamental form of a (usually crystalline) solid. The solid is characterized by a relatively high viscosity and an extremely high length to diameter ratio (e.g., several hundred to one or more). Semi-synthetic fibers include inorganic materials, for example, using carbon or glass, extruded into fibers. Semi-synthetic fibers include materials, for example, using high polymers, extruded into fibers.
[0047] The term "glass" as used herein means a non-crystalline, amorphous solid. Glass may include, for example, ceramic materials including mixtures of silica, soda ash, and lime. Glass may include, for example, one or more of C-glass, E-glass, S-glass, or T-glass. Glass may be, for example, in the form of glass fibers (e.g., fiberglass). Glass may include, for example, S-2 glass (e.g., S-2 glass fiber).
[0048] The glass fibers may be woven or non-woven (e.g., chopped, tiled, randomly oriented). The strength of woven fibers may vary with the type of weave and / or orientation of the woven fibers (e.g., if the woven fibers are oriented parallel, the strength of the woven fibers as a group should be higher in the direction parallel to the orientation). The type of weave may be, for example, a plain weave (e.g., 1×1), twill (e.g., 2×2), sapphire weave, fish weave, harness weave, leno weave, satin weave, or unidirectional weave.
[0049] As used herein, the term "matrix" means the substance that holds together the strength members of a composite, which substance is one of two or more materials in the composite.
[0050] As used herein, the term "resin" means a semi-solid or solid complex amorphous mixture of organic compounds.
[0051] As used herein, the term "monomer" refers to a molecule or compound that typically contains carbon, has a relatively low molecular weight, and is structurally simple.
[0052] As used herein, the term "polymer" refers to a macromolecule formed by the chemical union of five or more identical monomers. A polymer may be, for example, inorganic or organic. An organic polymer may be, for example, natural or synthetic (e.g., man-made). A synthetic organic polymer may be, for example, inorganic or organic.
[0053] As used herein, the term "polymer" means an organic polymer having a molecular weight of ≧5000 grams / mole.
[0054] The term "thermoplastic" as used herein means a polymer, as defined above, that softens when exposed to heat and returns to its original state when cooled to room temperature. The thermoplastic polymer may be, for example, amorphous or semi-crystalline. The thermoplastic polymer may include, for example, one or more of polyaryletherketone (PAEK), polyetherimide (PEI), or polyphenylene sulfide (PPS). The polyaryletherketone may include, for example, one or more of polyetherketone (PEK), polyetheretherketone (PEEK), polyetherketoneketone (PEKK), polyetheretherketoneketone (PEEKK), or polyetherketoneetherketoneketone (PEKEKK).
[0055] As used herein, the term "thermoset polymer" means a polymer, as defined above, that crosslinks and irreversibly solidifies or "sets" upon the application of heat.
[0056] As used herein, the term "glass composite layer" refers to a layer that includes a composite that includes glass. The glass may be in the form of, for example, glass fibers. The glass fibers in a glass composite layer may have no particular orientation (omnidirectional) or may be oriented in one or more directions (e.g., unidirectional, bidirectional, or multidirectional). The glass fibers may be aligned, continuous, and / or unidirectional.
[0057] The glass composite layer may, for example, include a matrix. The matrix may, for example, include a resin. The resin may, for example, include a thermoplastic polymer. The thermoplastic polymer may, for example, include one or more of PEEK (PEEK has a relatively high glass transition temperature (about 290° F.) and melting temperature (about 650° F.) and is capable of high heat processing), PEKK (PEKK has a relatively high glass transition temperature (about 315° F.) and melting temperature (about 640° F.) and is capable of high heat processing), or other thermoplastic polymers. The glass composite layer may, for example, include one or more glass fiber reinforced polymers. The glass composite layer may, for example, include one or more glass fiber reinforced thermoplastics.
[0058] The term "prepreg" as used herein is an abbreviation for "pre-impregnated" composite fibers, where the matrix material, such as a thermoplastic resin, is already present in the fiber reinforcement prior to molding. Prepreg manufacturing techniques can be used to manufacture composite parts for a variety of commercial applications, including, for example, aircraft and / or spacecraft manufacturing. Composite part manufacturing using prepreg manufacturing methods can be rate limiting in the fabrication of composite products.
[0059] As used herein, the term "prepreg ply" includes both prepreg fabric and prepreg tape.
[0060] The thermoplastic resin of the one or more glass fiber reinforced thermoplastic prepreg plies provides bonding for the glass fibers. The thermoplastic resin may exhibit a sufficiently high glass transition temperature, continued use temperature, and / or crystallite melting point to allow the one or more aluminum layers (e.g., aluminum layer 102A) to be softened for molding, shaping, and / or other processes related to the manufacturing of the material system.
[0061] One or more glass composite layers may be relied upon to provide significant structural support, typically in a greater number and / or thickness than would be the case if the glass composite layer or layers were not relied upon to provide significant structural support.
[0062] Whether or not relied upon to provide significant structural support, the glass composite layer or layers may have a thickness of, for example, ≧0.0020 inches and ≦0.0080 inches (e.g., 0.0020 inches, 0.0025 inches, 0.0030 inches, 0.0035 inches, 0.0040 inches, 0.0045 inches, 0.0050 inches, 0.0055 inches, 0.0060 inches, 0.0065 inches, 0.0070 inches, 0.0075 inches, or 0.0080 inches). If relied upon to provide significant structural support, the glass composite layer or layers may have a thickness greater than 0.0080 inches.
[0063] Whether or not relied upon to provide significant structural support, the thickness of one or more of the glass composite layer sublayers may be, for example, ≧0.0020 inches and ≦0.0040 inches (e.g., 0.0020 inches, 0.0025 inches, 0.0030 inches, 0.0035 inches, or 0.0040 inches). If relied upon to provide significant structural support, the thickness of one or more of the glass composite sublayers may be greater than 0.0040 inches.
[0064] As used herein, the term "adjacent" means "near or in direct contact."
[0065] The resin of the glass composite layer can directly bond the aluminum layer and the glass composite layer (e.g., aluminum layer 102A and glass composite layer 104A), where glass composite layer 104A can be adjacent to aluminum layer 102A or can be in direct contact with aluminum layer 102A.
[0066] An additional layer (not shown) may be between the aluminum layer 102A and the glass composite layer 104A. In this case, the glass composite layer 104A may be adjacent to the aluminum layer 102A, but may not be in direct contact with the aluminum layer 102A. The additional layer may improve the bond between the aluminum layer 102A and the glass composite layer 104A. The additional layer may at least partially mitigate effects (e.g., thermal contraction, thermal expansion, distortion, or stress) associated with the bond between the aluminum layer 102A and the glass composite layer 104A.
[0067] The additional layer may be, for example, an adhesive layer. Care should be taken when selecting materials for such additional layers because, for example, some adhesives contain silver or other elements or compounds that may interact with the aluminum layer 102A and / or the glass composite layer 104A via one or more interaction mechanisms (e.g., galvanic corrosion).
[0068] As used herein, the term "carbon" means the nonmetallic element having atomic number 6 and includes any isotopes thereof.
[0069] As used herein, the term "carbon composite layer" refers to a layer that includes a composite that includes carbon. The carbon may be in the form of, for example, carbon fibers. The carbon fibers in a carbon composite layer may have no particular orientation (omnidirectional) or may be oriented in one or more directions (e.g., unidirectional, bidirectional, or multidirectional). The carbon fibers may be aligned, continuous, and / or unidirectional.
[0070] The carbon fibers may be woven. The strength of the woven fibers may vary depending on the type of weave and / or orientation of the woven fibers (e.g., if the woven fibers are oriented parallel, the strength of the woven fibers as a group should be higher in the direction parallel to the orientation). The type of weave may be, for example, a plain weave (e.g., 1×1), twill weave (e.g., 2×2), seven-ply weave, fish weave, harness weave, leno weave, satin weave, or unidirectional weave.
[0071] The carbon composite layer may, for example, include a matrix. The matrix may, for example, include a resin. The resin may, for example, include a thermoplastic polymer. The thermoplastic polymer may, for example, include one or more of PEEK, PEKK, or other thermoplastic polymers. The carbon composite layer may, for example, include one or more carbon fiber reinforced polymers. The carbon composite layer may, for example, include one or more carbon fiber reinforced thermoplastics.
[0072] The thermoplastic resin of the one or more carbon fiber reinforced thermoplastic prepreg plies provides bonding for the carbon fibers. The thermoplastic resin may exhibit a sufficiently high glass transition temperature, continued use temperature, and / or crystallite melting point to allow the one or more aluminum layers (e.g., aluminum layer 102A) to be softened for molding, shaping, and / or other processes related to the manufacturing of the material system.
[0073] One or more carbon composite layers may be relied upon to provide significant structural support, typically in a greater number and / or thickness than would be the case if one or more carbon composite layers were not relied upon to provide significant structural support.
[0074] Whether or not relied upon to provide significant structural support, the carbon composite layer or layers may have a thickness of, for example, ≧0.0400 inches and ≦0.0800 inches (e.g., 0.0400 inches, 0.0432 inches, 0.0440 inches, 0.0450 inches, 0.0500 inches, 0.0550 inches, 0.0600 inches, 0.0650 inches, 0.0700 inches, 0.0750 inches, or 0.0800 inches). If relied upon to provide significant structural support, the carbon composite layer or layers may have a thickness greater than 0.0800 inches.
[0075] Whether or not relied upon to provide significant structural support, the thickness of one or more of the carbon composite layer sub-layers may be, for example, ≧0.0040 inches and ≦0.0080 inches (e.g., 0.0040 inches, 0.0044 inches, 0.0045 inches, 0.0050 inches, 0.0054 inches, 0.0055 inches, 0.0060 inches, 0.0065 inches, 0.0070 inches, 0.0075 inches, or 0.0080 inches). If relied upon to provide significant structural support, the thickness of one or more of the carbon composite sub-layers may be greater than 0.0080 inches.
[0076] The first glass composite layer and / or one or more glass fiber reinforced thermoplastic prepreg plies may comprise a first thermoplastic resin, and the first carbon composite layer and / or one or more carbon fiber reinforced thermoplastic prepreg plies may comprise a second thermoplastic resin, and the first thermoplastic resin may be the same as the second thermoplastic resin. If the first thermoplastic resin is the same as the second thermoplastic resin, the manufacturing of the material system can be simplified. The bond between the first glass composite layer and / or one or more glass fiber reinforced thermoplastic prepreg plies and the first carbon composite layer and / or one or more carbon fiber reinforced thermoplastic prepreg plies may be more uniform and / or more stable over time due to the compatibility of the first thermoplastic resin with the second thermoplastic resin.
[0077] The first glass composite layer and / or one or more glass fiber reinforced thermoplastic prepreg plies may comprise a first thermoplastic resin, and the first carbon composite layer and / or one or more carbon fiber reinforced thermoplastic prepreg plies may comprise a second thermoplastic resin, and the first thermoplastic resin may be different from the second thermoplastic resin. If the first thermoplastic resin is different from the second thermoplastic resin, more design options may be available during the manufacture of the material system. The bond between the first glass composite layer and / or one or more glass fiber reinforced thermoplastic prepreg plies and the first carbon composite layer and / or one or more carbon fiber reinforced thermoplastic prepreg plies may be stronger initially and / or over time, especially if the first thermoplastic resin and the second thermoplastic resin are selected with mutual chemical compatibility in mind.
[0078] The one or more glass composite layers may be configured to prevent (e.g., direct) interaction between the aluminum layer and the carbon composite layer (e.g., glass composite layer 104A may be configured to prevent interaction between aluminum layer 102A and carbon composite layer 106A). The one or more glass composite layers may be configured to prevent galvanic corrosion resulting from interaction (e.g., direct or indirect) between the aluminum layer and the carbon composite layer (e.g., glass composite layer 104A may be configured to prevent galvanic corrosion resulting from interaction between aluminum layer 102A and carbon composite layer 106A).
[0079] One or more glass composite layers may be configured to reduce thermal stresses due to differences in thermal contraction between the aluminum layer and the carbon composite layer during cooling (e.g., during the consolidation process) by at least partially mitigating the effects of thermal contraction in the aluminum and carbon composite layers and / or through effects associated with the orientation of the glass fibers within the one or more glass composite layers (e.g., glass composite layer 104A may be configured to reduce thermal stresses due to differences in thermal contraction between aluminum layer 102A and carbon composite layer 106A during cooling). The one or more glass composite layers may be configured to reduce residual thermal stresses due to differences in thermal contraction during cooling between the aluminum layer and the carbon composite layer after cooling (e.g., after the consolidation process) by at least partially mitigating the effects of thermal contraction in the aluminum and carbon composite layers and / or through effects associated with the orientation of the glass fibers within the one or more glass composite layers (e.g., glass composite layer 104A may be configured to reduce residual thermal stresses due to differences in thermal contraction during cooling between the aluminum layer 102A and the carbon composite layer 106A after cooling).
[0080] One or more glass composite layers may be configured to act as a conformal layer to reduce thermal stresses both during and after cooling, helping to prevent adjacent layers from separating due to stress buildup near, at, or across the boundaries between adjacent layers.
[0081] The resin of the glass composite layer can directly bond the glass composite layer and the carbon composite layer (e.g., glass composite layer 104A and carbon composite layer 106A), where glass composite layer 104A can be adjacent to or in direct contact with carbon composite layer 106A.
[0082] The resin of the carbon composite layer can directly bond the glass composite layer and the carbon composite layer (e.g., glass composite layer 104A and carbon composite layer 106A), where glass composite layer 104A can be adjacent to or in direct contact with carbon composite layer 106A.
[0083] The resins of the glass and carbon composite layers can directly bond the glass and carbon composite layers (e.g., glass composite layer 104A and carbon composite layer 106A), where glass composite layer 104A can be adjacent to or in direct contact with carbon composite layer 106A.
[0084] An additional layer (not shown) may be between the glass composite layer 104A and the carbon composite layer 106A. In this case, the glass composite layer 104A may be adjacent to the carbon composite layer 106A, but may not be in direct contact with the carbon composite layer 106A. The additional layer may improve the bond between the glass composite layer 104A and the carbon composite layer 106A. The additional layer may at least partially mitigate effects (e.g., thermal contraction, thermal expansion, distortion, or stress) associated with the bond between the glass composite layer 104A and the carbon composite layer 106A.
[0085] The additional layer may be, for example, an adhesive layer. Care should be taken when selecting materials for such additional layers because, for example, some adhesives contain elements or compounds that may interact with the glass composite layer 104A and / or the carbon composite layer 106A via one or more interaction mechanisms.
[0086] One or more layers may be between a given aluminum layer and a given carbon composite layer. The one or more layers may include, for example, one or more glass composite layers and / or one or more adhesive layers. The one or more layers may be configured to prevent (e.g., direct) interaction between the one or more aluminum layers and the one or more carbon composite layers (e.g., configured to prevent interaction between the aluminum layer 102A and the carbon composite layer 106A). The one or more layers may be configured to prevent galvanic corrosion resulting from interaction (e.g., direct or indirect) between the one or more aluminum layers and the one or more carbon composite layers (e.g., configured to prevent galvanic corrosion resulting from interaction between the aluminum layer 102A and the carbon composite layer 106A).
[0087] 1B illustrates a material system 100B in accordance with some embodiments of the disclosed material systems. As shown in FIG. 1B, material system 100B includes an aluminum layer 102B, a glass composite layer 104B adjacent to aluminum layer 102B, and a carbon composite layer 106B adjacent to glass composite layer 104B and opposite aluminum layer 102B. Aluminum layer 102B can include multiple aluminum sublayers 102B1, 102B2, 102B3, 102B4 (e.g., 102B1, 102B2, ... 102Bn). The number of aluminum sublayers (n) can be, for example, 2, 3, 4, 5, 6 or more sublayers.
[0088] The aluminum layer 102B, the glass composite layer 104B, and the carbon composite layer 106B may have the same or different thicknesses. Similarly, the aluminum sub-layers 102B1, 102B2, 102B3, 102B4 may have the same or different thicknesses.
[0089] 1C illustrates a material system 100C according to some embodiments of the disclosed material system. As shown in FIG. 1C, the material system 100C includes an aluminum layer 102C, a glass composite layer 104C adjacent to the aluminum layer 102C, and a carbon composite layer 106C adjacent to the glass composite layer 104C and opposite the aluminum layer 102C. The glass composite layer 104C can include multiple glass composite sublayers 104C1, 104C2, 104C3, 104C4 (e.g., 104C1, 104C2, ... 104Cn). The number of glass composite sublayers (n) can be, for example, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12 or more sublayers.
[0090] The aluminum layer 102C, the glass composite layer 104C, and the carbon composite layer 106C may have the same or different thicknesses. Similarly, the glass composite sub-layers 104C1, 104C2, 104C3, 104C4 may have the same or different thicknesses.
[0091] FIG 1D illustrates a material system 100D in accordance with some embodiments of the disclosed material systems. As shown in FIG 1D, material system 100D includes an aluminum layer 102D, a glass composite layer 104D adjacent to aluminum layer 102D, and a carbon composite layer 106D adjacent to glass composite layer 104D and opposite aluminum layer 102D. Carbon composite layer 106D can include multiple carbon composite sub-layers 106D1, 106D2, 106D3, 106D4 (e.g., 106D1, 106D2, ... 106Dn). The number (n) of carbon composite sublayers can be, for example, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32 or more sublayers (e.g., 8, 16, 24, 32, 40, or 64 sublayers).
[0092] The aluminum layer 102D, the glass composite layer 104D, and the carbon composite layer 106D may have the same or different thicknesses. Similarly, the carbon composite sub-layers 106D1, 106D2, 106D3, 106D4 may have the same or different thicknesses.
[0093] FIG. 1E illustrates a material system 100E according to some embodiments of the disclosed material system. As shown in FIG. 1E, the material system 100E includes an aluminum layer 102E, a glass composite layer 104E adjacent to the aluminum layer 102E, and a carbon composite layer 106E adjacent to the glass composite layer 104E and opposite the aluminum layer 102E. The aluminum layer 102E may include multiple aluminum sublayers 102E1, 102E2 (e.g., 102E1, 102E2, ... 102En). The number of aluminum sublayers (n) may be, for example, 2, 3, 4, 5, 6 or more sublayers. The glass composite layer 104E may include multiple glass composite sublayers 104E1, 104E2, 104E3, 104E4 (e.g., 104E1, 104E2, ... 104Eo). The number of glass composite sublayers (o) can be, for example, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12 or more sublayers. The carbon composite layer 106E can include multiple carbon composite sublayers 106E1, 106E2, 106E3 (e.g., 106E1, 106E2, ... 106Ep). The number of carbon composite sublayers (p) can be, for example, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32 or more sublayers (e.g., 8, 16, 24, 32, 40, or 64 sublayers).
[0094] The number of aluminum sublayers may be the same as or different from the number of glass composite sublayers. The number of aluminum sublayers may be the same as or different from the number of carbon composite sublayers. The number of glass composite sublayers may be the same as or different from the number of carbon composite sublayers.
[0095] The aluminum layer 102E, the glass composite layer 104E, and the carbon composite layer 106E may have the same thickness or different thicknesses. The aluminum sub-layers 102E1, 102E2 may have the same thickness or different thicknesses. The glass composite sub-layers 104E1, 104E2, 104E3, 104E4 may have the same thickness or different thicknesses. The carbon composite sub-layers 106E1, 106E2, 106E3 may have the same thickness or different thicknesses.
[0096] The glass composite layers (e.g., glass composite layers 104A, 104B, 104C, 104D, 104E) may include a first thermoplastic resin. The first thermoplastic resin may include PEEK. The first thermoplastic resin may include PEKK. The first thermoplastic resin may include one or more of PAEK, PEI, or PPS. The first thermoplastic resin may include, for example, one or more of PAEK, PEEK, PEEKK, PEI, PEK, PEKEKK, PEKK, or PPS. The carbon composite layers (e.g., carbon composite layers 106A, 106B, 106C, 106D, 106E) may include a second thermoplastic resin. The second thermoplastic resin may include PEEK. The second thermoplastic resin may include PEKK. The second thermoplastic resin may include one or more of PAEK, PEI, or PPS. The second thermoplastic resin may include, for example, one or more of PAEK, PEEK, PEEKK, PEI, PEK, PEKEKK, PEKK, or PPS. The first thermoplastic resin may be the same as the second thermoplastic resin. The first thermoplastic resin may be different from the second thermoplastic resin.
[0097] The first thermoplastic resin can bond the glass composite layer and the carbon composite layer (e.g., glass composite layer 104A and carbon composite layer 106A). The second thermoplastic resin can bond the glass composite layer and the carbon composite layer (e.g., glass composite layer 104A and carbon composite layer 106A). The first and second thermoplastic resins can bond the glass composite layer and the carbon composite layer (e.g., glass composite layer 104A and carbon composite layer 106A).
[0098] Figure 2A illustrates a material system 200A in accordance with some embodiments of the disclosed material systems. As shown in Figure 2A, material system 200A includes a first aluminum layer 202A, a first glass composite layer 204A adjacent to first aluminum layer 202A, a first carbon composite layer 206A adjacent to first glass composite layer 204A and on an opposite side to first aluminum layer 202A, and a second glass composite layer 208A adjacent to first carbon composite layer 206A and on an opposite side to first glass composite layer 204A.
[0099] The second glass composite layer 208A may include multiple second glass composite sub-layers (not shown). The number of second glass composite sub-layers may be, for example, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12 or more sub-layers. The sub-layers may each or all include one or more glass fiber reinforced thermoplastic prepreg plies.
[0100] The first glass composite layer 204A may include one or more first glass fiber reinforced thermoplastic prepreg plies, which may include a first thermoplastic resin. The first carbon composite layer 206A may include one or more first carbon fiber reinforced thermoplastic prepreg plies, which may include a second thermoplastic resin. The second glass composite layer 208A may include one or more second glass fiber reinforced thermoplastic prepreg plies, which may include a third thermoplastic resin. The first thermoplastic resin may be the same as or different from the second thermoplastic resin. The first thermoplastic resin may be the same as or different from the third thermoplastic resin. The second thermoplastic resin may be the same as or different from the third thermoplastic resin.
[0101] The first thermoplastic resin may include PEEK. The first thermoplastic resin may include PEKK. The first thermoplastic resin may include one or more of PAEK, PEI, or PPS. The first thermoplastic resin may include, for example, one or more of PAEK, PEEK, PEEKK, PEI, PEK, PEKEKK, PEKK, or PPS. The second thermoplastic resin may include PEEK. The second thermoplastic resin may include PEKK. The second thermoplastic resin may include one or more of PAEK, PEI, or PPS. The second thermoplastic resin may include, for example, one or more of PAEK, PEEK, PEEKK, PEI, PEK, PEKEKK, PEKK, or PPS. The third thermoplastic resin may include PEEK. The third thermoplastic resin may include PEKK. The third thermoplastic resin may include one or more of PAEK, PEI, or PPS. The third thermoplastic resin may include, for example, one or more of PAEK, PEEK, PEEKK, PEI, PEK, PEKEKK, PEKK, or PPS.
[0102] Figure 2B illustrates a material system 200B in accordance with some embodiments of the disclosed material systems. As shown in Figure 2B, material system 200B includes a first aluminum layer 202B, a first glass composite layer 204B adjacent to first aluminum layer 202B, a first carbon composite layer 206B adjacent to first glass composite layer 204B and on an opposite side to first aluminum layer 202B, a second glass composite layer 208B adjacent to first carbon composite layer 206B and on an opposite side to first glass composite layer 204B, and a second aluminum layer 210B adjacent to second glass composite layer 208B and on an opposite side to first carbon composite layer 206B.
[0103] The second aluminum layer 210B may include multiple second aluminum sub-layers (not shown). The number of second aluminum sub-layers may be, for example, 2, 3, 4, 5, 6 or more sub-layers.
[0104] Figure 2C illustrates a material system 200C in accordance with some embodiments of the disclosed material systems. As shown in Figure 2C, material system 200C includes a first aluminum layer 202C, a first glass composite layer 204C adjacent to first aluminum layer 202C, a first carbon composite layer 206C adjacent to first glass composite layer 204C and on an opposite side to first aluminum layer 202C, a second glass composite layer 208C adjacent to first carbon composite layer 206C and on an opposite side to first glass composite layer 204C, and a second carbon composite layer 212C adjacent to second glass composite layer 208C and on an opposite side to first carbon composite layer 206C.
[0105] The second carbon composite layer 212C may include multiple second carbon composite sub-layers (not shown). The number of second carbon composite sub-layers may be, for example, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32 or more sub-layers (e.g., 8, 16, 24, 32, 40, or 64 sub-layers). Each or all of the sub-layers may include one or more carbon fiber reinforced thermoplastic prepreg plies.
[0106] The first glass composite layer 204C may include one or more first glass fiber reinforced thermoplastic prepreg plies, which may include a first thermoplastic resin. The first carbon composite layer 206C may include one or more first carbon fiber reinforced thermoplastic prepreg plies, which may include a second thermoplastic resin. The second glass composite layer 208C may include one or more second glass fiber reinforced thermoplastic prepreg plies, which may include a third thermoplastic resin. The second carbon composite layer 212C may include one or more second carbon fiber reinforced thermoplastic prepreg plies, which may include a fourth thermoplastic resin. The first thermoplastic resin may be the same as or different from the second thermoplastic resin. The first thermoplastic resin may be the same as or different from the third thermoplastic resin. The first thermoplastic resin may be the same as or different from the fourth thermoplastic resin. The second thermoplastic resin may be the same as or different from the third thermoplastic resin. The second thermoplastic resin may be the same as or different from the fourth thermoplastic resin. The third thermoplastic resin may be the same as or different from the fourth thermoplastic resin.
[0107] The first thermoplastic resin may include PEEK. The first thermoplastic resin may include PEKK. The first thermoplastic resin may include one or more of PAEK, PEI, or PPS. The first thermoplastic resin may include, for example, one or more of PAEK, PEEK, PEEKK, PEI, PEK, PEKEKK, PEKK, or PPS. The second thermoplastic resin may include PEEK. The second thermoplastic resin may include PEKK. The second thermoplastic resin may include one or more of PAEK, PEI, or PPS. The second thermoplastic resin may include, for example, one or more of PAEK, PEEK, PEEKK, PEI, PEK, PEKEKK, PEKK, or PPS. The third thermoplastic resin may include PEEK. The third thermoplastic resin may include PEKK. The third thermoplastic resin may include one or more of PAEK, PEI, or PPS. The third thermoplastic resin may include, for example, one or more of PAEK, PEEK, PEEKK, PEI, PEK, PEKEKK, PEKK, or PPS. The fourth thermoplastic resin may include PEEK. The fourth thermoplastic resin may include PEKK. The fourth thermoplastic resin may include one or more of PAEK, PEI, or PPS. The fourth thermoplastic resin may include, for example, one or more of PAEK, PEEK, PEEKK, PEI, PEK, PEKEKK, PEKK, or PPS.
[0108] 2D illustrates a material system 200D in accordance with some embodiments of the disclosed material systems. As shown in FIG. 2D, material system 200D includes a first aluminum layer 202D, a first glass composite layer 204D adjacent to first aluminum layer 202D, a first carbon composite layer 206D adjacent to first glass composite layer 204D and on an opposite side to first aluminum layer 202D, a second glass composite layer 208D adjacent to first carbon composite layer 206D and on an opposite side to first glass composite layer 204D, a second aluminum layer 210 adjacent to second glass composite layer 208D and on an opposite side to first carbon composite layer 206D. 2D, a third glass composite layer 214D adjacent to the second aluminum layer 210D and opposite the second glass composite layer 208D, a second carbon composite layer 216D adjacent to the third glass composite layer 214D and opposite the second aluminum layer 210D, a fourth glass composite layer 218D adjacent to the second carbon composite layer 216D and opposite the third glass composite layer 214D, and / or a third aluminum layer 220D adjacent to the fourth glass composite layer 218D and opposite the second carbon composite layer 216D.
[0109] Each aluminum layer may include multiple aluminum sublayers (not shown). The number of aluminum sublayers may be, for example, 2, 3, 4, 5, 6 or more sublayers. Each glass composite layer may include multiple glass composite sublayers (not shown). The number of glass composite sublayers may be, for example, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12 or more sublayers. Each carbon composite layer may include multiple carbon composite sublayers (not shown). The number of carbon composite sublayers may be, for example, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32 or more sublayers (e.g., 8, 16, 24, 32, 40, or 64 sublayers).
[0110] Each or all of the glass composite layers may include one or more first glass fiber reinforced thermoplastic prepreg plies, which may include a first thermoplastic resin. The first thermoplastic resin may include PEEK. The first thermoplastic resin may include PEKK. The first thermoplastic resin may include one or more of PAEK, PEI, or PPS. The first thermoplastic resin may include one or more of PAEK, PEEK, PEEKK, PEI, PEK, PEKEKK, PEKK, or PPS. The first thermoplastic resin may be the same or different as the thermoplastic resin in any other glass composite layer or carbon composite layer.
[0111] Each or all of the carbon composite layers may include one or more carbon fiber reinforced thermoplastic prepreg plies, which may include a second thermoplastic resin. In each or all of the carbon composite layers, the second thermoplastic resin may include PEEK. In each or all of the carbon composite layers, the second thermoplastic resin may include PEKK. In each or all of the carbon composite layers, the second thermoplastic resin may include one or more of PAEK, PEI, or PPS. In each or all of the carbon composite layers, the second thermoplastic resin may include one or more of PAEK, PEEK, PEEKK, PEI, PEK, PEKEKK, PEKK, or PPS. In each of the carbon composite layers, the second thermoplastic resin may be the same or different from the thermoplastic resin in any other carbon composite layer or glass composite layer.
[0112] 2E illustrates a material system 200E in accordance with some embodiments of the disclosed material systems. As shown in FIG. 2E, material system 200E includes a first aluminum layer 202E, a first glass composite layer 204E adjacent to first aluminum layer 202E, a first carbon composite layer 206E adjacent to first glass composite layer 204E and on an opposite side to first aluminum layer 202E, a second glass composite layer 208E adjacent to first carbon composite layer 206E and on an opposite side to first glass composite layer 204E, a first carbon composite layer 208E adjacent to second glass composite layer 208E and on an opposite side to first glass composite layer 204E, and a second carbon composite layer 208E adjacent to second glass composite layer 208E. The laminate includes a second aluminum layer 212E opposite the base composite layer 206E, a third glass composite layer 222E adjacent to the second aluminum layer 212E and opposite the second glass composite layer 208E, a third carbon composite layer 224E adjacent to the third glass composite layer 222E and opposite the second aluminum layer 212E, and / or a fourth glass composite layer 226E adjacent to the third carbon composite layer 224E and opposite the third glass composite layer 222E.
[0113] The first aluminum layer 202E may include multiple first aluminum sublayers (not shown). The number of first aluminum sublayers may be, for example, 2, 3, 4, 5, 6 or more sublayers. Each glass composite layer may include multiple glass composite sublayers (not shown). The number of glass composite sublayers may be, for example, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12 or more sublayers. Each carbon composite layer may include multiple carbon composite sublayers (not shown). The number of carbon composite sublayers can be, for example, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32 or more sublayers (e.g., 8, 16, 24, 32, 40, or 64 sublayers).
[0114] Each or all of the glass composite layers may include one or more glass fiber reinforced thermoplastic prepreg plies, which may include a first thermoplastic resin. In each or all of the glass composite layers, the first thermoplastic resin may include PEEK. In each or all of the glass composite layers, the first thermoplastic resin may include PEKK. In each or all of the glass composite layers, the first thermoplastic resin may include one or more of PAEK, PEI, or PPS. In each or all of the glass composite layers, the first thermoplastic resin may include one or more of PAEK, PEEK, PEEKK, PEI, PEK, PEKEKK, PEKK, or PPS. In each of the glass composite layers, the first thermoplastic resin may be the same or different from the thermoplastic resin in any other glass composite layer or carbon composite layer.
[0115] Each or all of the carbon composite layers may include one or more carbon fiber reinforced thermoplastic prepreg plies, which may include a second thermoplastic resin. In each or all of the carbon composite layers, the second thermoplastic resin may include PEEK. In each or all of the carbon composite layers, the second thermoplastic resin may include PEKK. In each or all of the carbon composite layers, the second thermoplastic resin may include one or more of PAEK, PEI, or PPS. In each or all of the carbon composite layers, the second thermoplastic resin may include one or more of PAEK, PEEK, PEEKK, PEI, PEK, PEKEKK, PEKK, or PPS. In each of the carbon composite layers, the second thermoplastic resin may be the same or different from the thermoplastic resin in any other carbon composite layer or glass composite layer.
[0116] FIG. 3A illustrates laying up a first layer on a forming tool (e.g., a mandrel) according to some embodiments of the disclosed material system. As shown in FIG. 3A, a first layer 302 may be laid up on a forming tool 300. The forming tool 300 may be of virtually any shape. The first layer 302 may include, for example, an aluminum layer, a glass composite layer, or a carbon composite layer. A separator or the like may be used between the forming tool 300 and the first layer 302 to facilitate subsequent removal of the material system from the forming tool 300. The first layer 302 may include two or more sublayers (not shown).
[0117] FIG. 3B illustrates laying up a second layer on the first layer of FIG. 3A according to some embodiments of the disclosed material system. As shown in FIG. 3B, a second layer 304 can be laid up on the first layer 302 to form a first portion of a stack 318 (see FIG. 3D). The second layer 304 can include, for example, an aluminum layer, a glass composite layer, or a carbon composite layer, so long as the aluminum layer does not directly contact the carbon composite layer (due to concerns about galvanic corrosion). The second layer 304 can include two or more sublayers (not shown). The shape of the second layer 304 can be the same as or different from the shape of the first layer 302. The thickness of the second layer 304 can be the same as or different from the thickness of the first layer 302.
[0118] The stack 318 may include an additional layer (not shown) between the first layer 302 and the second layer 304. The additional layer may improve the bonding between the first layer 302 and the second layer 304. The additional layer may be, for example, an adhesive layer. In this case, the second layer 304 may be adjacent to the first layer 302 but may not be in direct contact with the first layer 302. Care should be taken when selecting materials for such additional layers because, for example, some materials contain elements or compounds that may interact with the first layer 302 and / or the second layer 304 via one or more interaction mechanisms.
[0119] FIG. 3C illustrates laying up a third layer on the second layer of FIG. 3B according to some embodiments of the disclosed material system. As shown in FIG. 3C, a third layer 306 can be laid up on the second layer 304 to form a second portion of the stack 318. The third layer 306 can include, for example, an aluminum layer, a glass composite layer, or a carbon composite layer, so long as the aluminum layer does not directly contact the carbon composite layer (due to concerns about galvanic corrosion). The third layer 306 can include two or more sublayers (not shown). The shape of the third layer 306 can be the same as or different from the shape of the first layer 302. The thickness of the third layer 306 can be the same as or different from the thickness of the first layer 302. The shape of the third layer 306 can be the same as or different from the shape of the second layer 304. The thickness of the third layer 306 can be the same as or different from the thickness of the second layer 304.
[0120] The stack 318 may include an additional layer (not shown) between the second layer 304 and the third layer 306. The additional layer may improve the bonding between the second layer 304 and the third layer 306. The additional layer may be, for example, an adhesive layer. In this case, the third layer 306 may be adjacent to the second layer 304 but may not be in direct contact with the second layer 304. Care should be taken when selecting materials for such additional layers because, for example, some materials contain elements or compounds that may interact with the second layer 304 and / or the third layer 306 via one or more interaction mechanisms.
[0121] In addition to addressing concerns about galvanic corrosion, the glass composite layer may act as a conforming layer to reduce strain in and / or stress between layers adjacent to the glass composite layer (e.g., an aluminum layer on one side and a carbon fiber layer on the other side). Such a conforming layer may at least partially mitigate effects (e.g., thermal contraction, thermal expansion, strain, or stress) associated with the layers adjacent to the glass composite layer and / or reduce strain and / or stress between layers through effects associated with the orientation of the glass fibers within the glass composite layer.
[0122] Addition of layers may continue until the desired ply stack is achieved. The layup may be performed manually and / or automatically.
[0123] The surface of the aluminum layer may be subjected to a surface treatment such as alkaline degreasing, chromic acid anodization or other anodizing, priming (e.g., with BR127 anti-corrosive primer), sol-gel, and / or acid washing in chromic sulfuric acid. The surface may also be roughened, for example, by polishing.
[0124] The laminate 318 may be bagged (eg, with a vacuum bag) on a forming tool (eg, a mandrel).
[0125] The lamination and consolidation may use stationary compression molding (eg, in an autoclave) or continuous compression molding (eg, outside of an autoclave or using vacuum bags only).
[0126] 3D illustrates a laminate 318 including a first carbon composite layer, a first glass composite layer, a second carbon composite layer, a second glass composite layer, and / or an aluminum layer according to some embodiments of the disclosed material system. As shown in FIG. 3D, to obtain the laminate 318, a first carbon composite layer 308 may be laid up on the forming tool 300, a first glass composite layer 310 may be laid up on the first carbon composite layer 308, a second carbon composite layer 312 may be laid up on the first glass composite layer 310, a second glass composite layer 314 may be laid up on the second carbon composite layer 312, and / or an aluminum layer 316 may be laid up on the second glass composite layer 314.
[0127] A first glass composite layer 310 may be adjacent to the first carbon composite layer 308, a second carbon composite layer 312 may be adjacent to the first glass composite layer 310, a second glass composite layer 314 may be adjacent to the second carbon composite layer 312, and / or an aluminum layer 316 may be adjacent to the second glass composite layer 314.
[0128] One or more of the first carbon composite layer 308, the first glass composite layer 310, the second carbon composite layer 312, the second glass composite layer 314, or the aluminum layer 316 may include two or more sublayers (not shown).
[0129] The laminate 318 may include additional layers (not shown) between the first carbon composite layer 308 and the first glass composite layer 310, between the first glass composite layer 310 and the second carbon composite layer 312, between the second carbon composite layer 312 and the second glass composite layer 314, and / or between the second glass composite layer 314 and the aluminum layer 316. The additional layers may improve the bonding between the associated adjacent layers. The additional layers may be, for example, adhesive layers. In this case, the layers may be adjacent to each other but may not be in direct contact. Care should be taken when selecting materials for such additional layers because, for example, some materials include elements or compounds that may interact with other layers via one or more interaction mechanisms.
[0130] Either or both of the first glass composite layer 310 or the second glass composite layer 314 may include one or more thermoplastic prepreg plies. The one or more thermoplastic prepreg plies may be consolidated at a temperature sufficient to soften the aluminum layer 316. Consolidating the one or more thermoplastic prepreg plies may be performed, for example, in an autoclave.
[0131] Consolidating one or more thermoplastic prepreg plies of either or both of the first glass composite layer 310 or the second glass composite layer 314 includes raising the temperature of the one or more thermoplastic prepreg plies to ≧600°F, ≧650°F, ≧675°F, or ≧700°F (e.g., 707°F±9°F or 710°F±10°F), raising the pressure of the one or more thermoplastic prepreg plies to ≧50 psig, ≧100 psig, ≧150 psig, ≧200 psig, ≧250 psig, or ≦300 psig (e.g., 100 psig±5 psig or minimum 290 psig), and / or holding the temperature and pressure for ≧5 minutes, ≧10 minutes, ≧15 minutes, or ≧20 minutes (e.g., 20 minutes +15 minutes / −5 minutes). For example, the temperature of one or more thermoplastic prepreg plies may be raised to 710°F ± 10°F, the pressure adjusted to 100 psig ± 5 psig, and then the temperature and pressure held within those ranges for 20 minutes + 15 minutes / - 5 minutes. For example, the temperature of one or more thermoplastic prepreg plies may be raised to 707°F ± 9°F, the pressure adjusted to a minimum of 290 psig, and then the temperature and pressure held within those temperature and pressure ranges for a minimum of 6 minutes.
[0132] Consolidating one or more thermoplastic prepreg plies of either or both of the first glass composite layer 310 or the second glass composite layer 314 includes raising the temperature of the laminate 318 to ≧600°F, ≧650°F, ≧675°F, or ≧700°F (e.g., 707°F±9°F or 710°F±10°F), raising the pressure of the laminate 318 to ≧50 psig, ≧100 psig, ≧150 psig, ≧200 psig, ≧250 psig, or ≦300 psig (e.g., 100 psig±5 psig or minimum 290 psig), and / or holding the temperature and pressure for ≧5 minutes, ≧10 minutes, ≧15 minutes, or ≧20 minutes (e.g., 20 minutes +15 minutes / −5 minutes). For example, the temperature of the stack 318 may be raised to 710°F ± 10°F, the pressure adjusted to 100 psig ± 5 psig, and then the temperature and pressure may be held within those temperature and pressure ranges for 20 minutes + 15 minutes / - 5 minutes. For example, the temperature of the stack 318 may be raised to 707°F ± 9°F, the pressure adjusted to a minimum of 290 psig, and then the temperature and pressure may be held within those temperature and pressure ranges for a minimum of 6 minutes.
[0133] Either or both of the first carbon composite layer 308 or the second carbon composite layer 312 may include one or more thermoplastic prepreg plies. The one or more thermoplastic prepreg plies may be consolidated at a temperature sufficient to soften the aluminum layer 316. Consolidating the one or more thermoplastic prepreg plies may be performed, for example, in an autoclave.
[0134] Consolidating one or more thermoplastic prepreg plies of either or both of the first carbon composite layer 308 or the second carbon composite layer 312 may include raising the temperature of the one or more thermoplastic prepreg plies to ≥ 600°F, ≥ 650°F, ≥ 675°F, or ≥ 700°F (e.g., 707°F ± 9°F or 710°F ± 10°F), raising the pressure of the one or more thermoplastic prepreg plies to ≥ 50 pounds per square inch gauge (psig), ≥ 100 psig, ≥ 150 psig, ≥ 200 psig, ≥ 250 psig, or ≤ 300 psig (e.g., 100 psig ± 5 psig or minimum 290 psig), and / or holding the temperature and pressure for ≥ 5 minutes, ≥ 10 minutes, ≥ 15 minutes, or ≥ 20 minutes (e.g., 20 minutes + 15 minutes / - 5 minutes). For example, the temperature of one or more thermoplastic prepreg plies may be raised to 710°F ± 10°F, the pressure adjusted to 100 psig ± 5 psig, and then the temperature and pressure held within those ranges for 20 minutes + 15 minutes / - 5 minutes. For example, the temperature of one or more thermoplastic prepreg plies may be raised to 707°F ± 9°F, the pressure adjusted to a minimum of 290 psig, and then the temperature and pressure held within those temperature and pressure ranges for a minimum of 6 minutes.
[0135] Consolidating one or more thermoplastic prepreg plies of either or both of the first carbon composite layer 308 or the second carbon composite layer 312 includes raising the temperature of the laminate 318 to ≧600°F, ≧650°F, ≧675°F, or ≧700°F (e.g., 707°F±9°F or 710°F±10°F), raising the pressure of the laminate 318 to ≧50 psig, ≧100 psig, ≧150 psig, ≧200 psig, ≧250 psig, or ≦300 psig (e.g., 100 psig±5 psig or minimum 290 psig), and / or holding the temperature and pressure for ≧5 minutes, ≧10 minutes, ≧15 minutes, or ≧20 minutes (e.g., 20 minutes +15 minutes / −5 minutes). For example, the temperature of the stack 318 may be raised to 710°F ± 10°F, the pressure adjusted to 100 psig ± 5 psig, and then the temperature and pressure may be held within those temperature and pressure ranges for 20 minutes + 15 minutes / - 5 minutes. For example, the temperature of the stack 318 may be raised to 707°F ± 9°F, the pressure adjusted to a minimum of 290 psig, and then the temperature and pressure may be held within those temperature and pressure ranges for a minimum of 6 minutes.
[0136] Such thermoplastic prepreg plies can be pre-produced and stored, for example, on rolls together with a paper backing. Prepreg tapes for thermoplastic prepreg plies, if unidirectional, can be produced, for example, by extrusion or drawing.
[0137] The thermoplastic prepreg plies may be dried (e.g., in an oven) before consolidation. For example, the thermoplastic prepreg plies may be dried at 250° F. for a minimum of 10 minutes before consolidation.
[0138] Either or both of the first glass composite layer 310 or the second glass composite layer 314 may comprise a first thermoplastic resin. The temperature and pressure of the laminate 318 may be adjusted to consolidate the laminate 318 in manufacturing the material system. Regulating the temperature and pressure of the laminate 318 may include increasing the temperature of the first thermoplastic to ≧600°F, ≧650°F, ≧675°F, or ≧700°F (e.g., 707°F±9°F or 710°F±10°F), increasing the pressure of the first thermoplastic to ≧50 psig, ≧100 psig, ≧150 psig, ≧200 psig, ≧250 psig, or ≦300 psig (e.g., 100 psig±5 psig or minimum 290 psig), and / or holding the temperature and pressure for ≧5 minutes, ≧10 minutes, ≧15 minutes, or ≧20 minutes (e.g., 20 minutes +15 minutes / −5 minutes). For example, the temperature of the first thermoplastic may be raised to 710°F ± 10°F, the pressure adjusted to 100 psig ± 5 psig, and then the temperature and pressure held within those ranges for 20 minutes + 15 minutes / - 5 minutes. For example, the temperature of the first thermoplastic may be raised to 707°F ± 9°F, the pressure adjusted to a minimum of 290 psig, and then the temperature and pressure held within those temperature and pressure ranges for a minimum of 6 minutes.
[0139] Either or both of the first carbon composite layer 308 or the second carbon composite layer 312 may include a second thermoplastic resin, the temperature and pressure of which may be adjusted to consolidate the laminate 318 in manufacturing the material system. Regulating the temperature and pressure of the laminate 318 may include increasing the temperature of the second thermoplastic to ≧600°F, ≧650°F, ≧675°F, or ≧700°F (e.g., 707°F±9°F or 710°F±10°F), increasing the pressure of the second thermoplastic to ≧50 psig, ≧100 psig, ≧150 psig, ≧200 psig, ≧250 psig, or ≦300 psig (e.g., 100 psig±5 psig or minimum 290 psig), and / or holding the temperature and pressure for ≧5 minutes, ≧10 minutes, ≧15 minutes, or ≧20 minutes (e.g., 20 minutes +15 minutes / −5 minutes). For example, the temperature of the second thermoplastic may be increased to 710°F ± 10°F, the pressure adjusted to 100 psig ± 5 psig, and then the temperature and pressure held within those ranges for 20 minutes + 15 minutes / - 5 minutes. For example, the temperature of the second thermoplastic may be increased to 707°F ± 9°F, the pressure adjusted to a minimum of 290 psig, and then the temperature and pressure held within those temperature and pressure ranges for a minimum of 6 minutes.
[0140] The temperature versus time profile for consolidating one or more thermoplastic prepreg plies at a temperature sufficient to soften the aluminum layer 316, or for adjusting the temperature and pressure of the laminate 318 to consolidate the laminate 318, has three phases: a heating phase (generally a positive slope), a holding phase (generally a zero slope), and a cooling phase (generally a negative slope). In the heating phase, the heating rate can be nearly any value (e.g., F° / min). In the holding phase, the temperature and pressure can be held substantially constant within a given band or beyond a given minimum value. In the cooling phase, the heating rate (e.g., F° / min) may be limited, for example, by concerns about thermally induced stresses, crystallinity issues, and equipment limitations. Additionally or alternatively, the pressure band may need to be maintained until the temperature has dropped significantly.
[0141] 4A shows a temperature versus time profile for consolidating one or more thermoplastic prepreg plies at a temperature sufficient to soften the aluminum layer or for adjusting the temperature and pressure of the laminate to consolidate the laminate in fabricating the material system, according to some embodiments of the disclosed material system. As shown in FIG. 4A, in the heating phase, the temperature increase rate can be almost any value, in the holding phase, the temperature (e.g., the cure temperature) can be held substantially constant within a predetermined band (e.g., 707°F±9°F or 710°F±10°F), and in the cooling phase, the temperature decrease rate can be limited (e.g., ≦100°F / min) until the temperature is significantly reduced (e.g., until the temperature is ≦250°F).
[0142] 4B shows a pressure versus time profile for consolidating one or more thermoplastic prepreg plies at a temperature sufficient to soften the aluminum layer or for adjusting the temperature and pressure of the laminate to consolidate the laminate in fabricating the material system, according to some embodiments of the disclosed material system. As shown in FIG. 4B, in the heating phase, the pressure is low, in the holding phase, the pressure may be held substantially constant within a predetermined band (e.g., 100 psig ± 5 psig for 20 min + 15 min / - 5 min or minimum 290 psig for minimum 6 min), and in the cooling phase, the pressure band may have to be maintained until the temperature is significantly reduced (e.g., 100 psig ± 5 psig or minimum 290 psig until the temperature is ≦ 250°F).
[0143] 4B, the pressure increase to and / or decrease from the adjusted pressure may be relatively quick. The pressure increase to and / or decrease from the adjusted pressure may be relatively slower, such that the leading and / or trailing ends of the pressure graph have a more gradual slope. The pressure increase to and / or decrease from the adjusted pressure may be done in a series of smaller steps.
[0144] 4C shows temperature and pressure versus time profiles for consolidating one or more thermoplastic prepreg plies at a temperature sufficient to soften the aluminum layer or for adjusting the temperature and pressure of a laminate according to some embodiments of the disclosed material system. As shown in FIG. 4C, in the heating phase, the heating rate can be almost any value, in the holding phase, the temperature (e.g., cure temperature) and pressure can be held substantially constant in a predetermined band or at a predetermined minimum (e.g., 707°F±9°F and at least 290 psig for at least 6 minutes), and in the cooling phase, the heating rate can be limited (e.g., ≦108°F / min) until the temperature is significantly reduced (e.g., until the temperature is ≦410°F), and / or a minimum pressure may have to be maintained until the temperature is significantly reduced (e.g., at least 290 psig until the temperature is ≦248°F).
[0145] During the heating phase, heating may be paused to allow the temperature to stabilize and / or standardize, and then heating may be continued (e.g., effectively creating a soak or pre-consolidation step in the heating profile with a dwell temperature; not shown). Similarly, during the cooling phase, cooling may be paused to allow the temperature to stabilize and / or standardize, and then cooling may be continued (e.g., effectively creating a soak or post-consolidation step in the cooling profile; not shown).
[0146] Material systems can be produced having a variety of component cross-sectional shapes. Material systems may have cross-sections that are, for example, circular and solid (e.g., rods), circular and hollow (e.g., tubes), square and solid, or square and hollow. Material systems may have cross-sections that resemble, for example, a blade, a hat, and / or a capital letter C, I, L, T, U, or Z.
[0147] Example 1 The four-ply laminate may include an aluminum layer (layer 1), two glass composite layers (sublayers 2-3, and 12-13), and a carbon composite layer (sublayers 4-11). The carbon composite layers may exhibit quasi-isotropic strength properties. In the table below, each glass composite layer includes two sublayers and the carbon composite layer includes eight sublayers.
[0148] TIFF0007591544000001.tif109170
[0149] Example 2 The four-ply laminate may include an aluminum layer (layer 1), two glass composite layers (sublayers 2-3, and 20-21), and a carbon composite layer (sublayers 4-19). The carbon composite layers may exhibit quasi-isotropic strength properties. In the table below, each glass composite layer includes two sublayers, and the carbon composite layer includes 16 sublayers.
[0150] TIFF0007591544000002.tif160170
[0151] Example 3 The four-ply laminate may include an aluminum layer (layer 1), two glass composite layers (sublayers 2-3, and 12-13), and a carbon composite layer (sublayers 4-11). The carbon composite layers may exhibit quasi-isotropic strength properties. In the table below, each glass composite layer includes two sublayers and the carbon composite layer includes eight sublayers.
[0152] TIFF0007591544000003.tif109170
[0153] Example 4 The four-ply laminate may include an aluminum layer (layer 1), two glass composite layers (layers 2 and 11), and a carbon composite layer (sublayers 3-10). The carbon composite layers may exhibit quasi-isotropic strength properties. In the table below, each glass composite layer includes one layer and the carbon composite layer includes eight sublayers.
[0154] TIFF0007591544000004.tif95170
[0155] For example, E-glass, S-glass, and / or S-2 glass fibers (eg, 933 S-2 glass fibers) for the glass composite layers are available from AGY of Aiken, South Carolina under the trade name S-2 Glass®.
[0156] For example, carbon fibers for the carbon composite layers (eg, AS4D 4000 carbon fibers) are available from Hexcel Corporation of Stamford, Connecticut under the trade name HexTow®.
[0157] Additionally, the present disclosure includes embodiments according to the following clauses:
[0158] Clause 1 1. A material system comprising: a first aluminum layer; a first glass composite layer adjacent to the first aluminum layer; and a first carbon composite layer adjacent to the first glass composite layer and opposite the first aluminum layer, wherein the first glass composite layer comprises a first thermoplastic resin, and wherein the first thermoplastic resin bonds the first aluminum layer and the first glass composite layer.
[0159] Clause 2 2. The system of claim 1, wherein the first thermoplastic resin bonds the first glass composite layer and the first carbon composite layer.
[0160] Clause 3 3. The system of claim 1 or 2, wherein the first thermoplastic resin comprises polyetheretherketone (PEEK) or polyetherketoneketone (PEKK).
[0161] Clause 4 4. The system of any one of clauses 1 to 3, wherein the first carbon composite layer comprises a second thermoplastic resin.
[0162] Clause 5 5. The system of claim 4, wherein the second thermoplastic resin comprises polyetheretherketone (PEEK) or polyetherketoneketone (PEKK).
[0163] Clause 6 5. The system of claim 4, wherein the first thermoplastic resin is the same as the second thermoplastic resin.
[0164] Clause 7 5. The system of claim 4, wherein the first thermoplastic resin is different from the second thermoplastic resin.
[0165] Clause 8 8. The system of any one of clauses 1 to 7, further comprising a second glass composite layer adjacent to the first carbon composite layer and opposite the first glass composite layer.
[0166] Clause 9 9. The system of claim 8, further comprising a second aluminum layer adjacent to the second glass composite layer and opposite the first carbon composite layer.
[0167] Clause 10 10. The system of any one of clauses 8-9, further comprising a second carbon composite layer adjacent to the second glass composite layer and opposite the first carbon composite layer.
[0168] Clause 11 11. The system of any one of clauses 1 to 10, wherein the first aluminum layer comprises a plurality of first aluminum sublayers.
[0169] Clause 12 12. The system of any one of clauses 1 to 11, wherein the first glass composite layer comprises a plurality of first glass composite sub-layers.
[0170] Clause 13 13. The system of any one of clauses 1 to 12, wherein the first carbon composite layer comprises a plurality of first carbon composite sub-layers.
[0171] Clause 14 14. The system of any one of clauses 1-13, wherein the first glass composite layer comprises woven glass and the strength of the first glass composite layer varies with the orientation of the woven glass.
[0172] Clause 15 1. A method of making a material system, comprising: laminating an aluminum layer, a glass composite layer including one or more thermoplastic prepreg plies, and a carbon composite layer such that an aluminum layer is adjacent to a glass composite layer in the laminate and such that the glass composite layer is adjacent to a carbon composite layer in the laminate; and consolidating the one or more thermoplastic prepreg plies at a temperature sufficient to soften the aluminum layer.
[0173] Clause 16 16. The method of claim 15, wherein the one or more thermoplastic prepreg plies comprise polyetheretherketone (PEEK) or polyetherketoneketone (PEKK).
[0174] Clause 17 17. The method of any one of clauses 15 to 16, wherein consolidating the one or more thermoplastic prepreg plies includes raising a temperature of the one or more thermoplastic prepreg plies to 600° F. or greater.
[0175] Clause 18 17. The method of claim 15 or 16, wherein consolidating the one or more thermoplastic prepreg plies includes raising a temperature of the laminate to 600° F. or greater.
[0176] Clause 19 1. A method of manufacturing a material system, comprising stacking an aluminum layer, a glass composite layer including a thermoplastic resin, and a carbon composite layer such that the glass composite layer is between the aluminum layer and the carbon composite layer in the stack, and adjusting the temperature and pressure of the stack to consolidate the stack.
[0177] Clause 20 20. The method of claim 19, wherein the thermoplastic resin comprises polyetheretherketone (PEEK) or polyetherketoneketone (PEKK).
[0178] While embodiments have been illustrated and described herein and in the accompanying drawings, it should be understood that changes can be made to the illustrated and / or described embodiments without departing from the principles and spirit thereof. The scope of the present disclosure is defined by the following claims and their equivalents.
Claims
1. 1. A method of making a materials system, comprising: laminating the first aluminum layer (202A), the first glass composite layer (204A) comprising one or more first thermoplastic prepreg plies, the first carbon composite layer (206A), and the second glass composite layer (208A) such that a first aluminum layer is adjacent to a first glass composite layer in the laminate, the first glass composite layer is adjacent to a first carbon composite layer in the laminate, and the first carbon composite layer is adjacent to a second glass composite layer in the laminate; consolidating the one or more first thermoplastic prepreg plies to soften the first aluminum layer; Including, the consolidating the one or more first thermoplastic prepreg plies comprises raising a temperature of the one or more first thermoplastic prepreg plies or a temperature of the laminate to a temperature of 600° F. or greater.
2. The method of claim 1 , wherein the first carbon composite layer comprises one or more first carbon fiber reinforced thermoplastic prepreg plies.
3. laminating the second aluminum layer (210B) such that the second glass composite layer is adjacent to the second aluminum layer in the laminate; The method of claim 1 or 2, further comprising:
4. The method of claim 3 , wherein the second aluminum layer (210B) comprises a plurality of second aluminum sub-layers.
5. stacking the third glass composite layer (214D), the second carbon composite layer (216D), the fourth glass composite layer (218D) and the third aluminum layer (220D) such that the second aluminum layer is adjacent to the third glass composite layer in the stack, the third glass composite layer is adjacent to the second carbon composite layer in the stack, the second carbon composite layer is adjacent to the fourth glass composite layer in the stack, and the fourth glass composite layer is adjacent to the third aluminum layer in the stack; The method of claim 3 or 4, further comprising:
6. laminating the second carbon composite layer (212C) such that the second glass composite layer is adjacent to the second carbon composite layer in the stack; The method of claim 1 further comprising:
7. The method of claim 6, wherein the second carbon composite layer (212C) comprises one or more second carbon fiber reinforced thermoplastic prepreg plies.
8. stacking the third glass composite layer (222E), the third carbon composite layer (224E), and the fourth glass composite layer (226E) such that the second carbon composite layer is adjacent to the third glass composite layer in the stack, the third glass composite layer is adjacent to the third carbon composite layer in the stack, and the third carbon composite layer is adjacent to the fourth glass composite layer in the stack; The method of claim 6 or 7, further comprising:
9. 9. The method of any one of claims 1 to 8, wherein the second glass composite layer (208A) comprises one or more second thermoplastic prepreg plies.
10. 10. The method of claim 9, wherein the one or more first thermoplastic prepreg plies comprise a first thermoplastic resin and the one or more second thermoplastic prepreg plies comprise a second thermoplastic resin.
11. The method of claim 10 , wherein the first thermoplastic resin is the same as the second thermoplastic resin.
12. The method of claim 10 , wherein the first thermoplastic resin is different from the second thermoplastic resin.
13. 13. The method of claim 10, wherein the first thermoplastic resin comprises polyetheretherketone (PEEK) or polyetherketoneketone (PEKK).
14. 14. The method of any one of claims 10 to 13, wherein the second thermoplastic resin comprises polyetheretherketone (PEEK) or polyetherketoneketone (PEKK).
Citation Information
Patent Citations
Laminated sheet material and reed of loom produced therefrom
JP1996309926A
Heat-radiation substrate and module substrate for lighting each having hybrid layer
JP2010241101A
Preform and fiber-reinforced resin molding using the same
JP2013249441A
Metal matrix composite used as heating element
JP2014195990A
Dissimilar material joined body and method of manufacturing the same
JP2016036955A