Negative electrode for secondary battery and non-aqueous electrolyte secondary battery
By using a first carbon material with a larger particle size and a second carbon material with a smaller particle size in a specific ratio with silicon-containing materials, the conductive path is maintained, enhancing discharge capacity and cycle characteristics in secondary batteries.
Patent Information
- Application Number
- JP2021542638
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-08-30
- Filing Date
- 2020-07-21
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2040-07-21
AI Technical Summary
The use of silicon-containing materials in negative electrodes for secondary batteries leads to significant expansion and contraction, causing isolation of silicon and disrupting the conductive path, which affects the cycle characteristics and discharge capacity.
Incorporating a first carbon material with a larger average particle size and a second carbon material with a smaller average particle size between particles of a silicon-containing material, ensuring the ratio A>C≧B, to maintain a conductive path and suppress expansion and contraction, thereby improving discharge capacity and cycle characteristics.
The solution effectively maintains a conductive path and suppresses the expansion and contraction of the silicon-containing material, leading to improved discharge capacity and cycle characteristics in secondary batteries.
Smart Images

Figure 0007591731000002 
Figure 0007591731000003 
Figure 0007591731000001
Abstract
Description
[Technical field]
[0001] The present disclosure primarily relates to improvements in secondary battery negative electrodes. [Background technology]
[0002] A non-aqueous electrolyte secondary battery, such as a lithium ion secondary battery, includes a positive electrode, a negative electrode, and a non-aqueous electrolyte. The negative electrode includes a negative electrode mixture that includes a negative electrode active material that can electrochemically absorb and release lithium ions. It has been considered to use a high-capacity silicon-containing material as the negative electrode active material.
[0003] In Patent Document 1, the negative electrode active material is a mixture of lump graphite, flake graphite, and SiO x (0.5≦x<1.6) is a mixture of silicon oxide and SiO x The present invention teaches a nonaqueous electrolyte secondary battery, characterized in that silicon oxide represented by (0.5≦x<1.6) is contained in an amount of 1 to 5 mass% based on the total graphite material, and flake graphite, in which the ratio of the average particle size (D50) of the flake graphite to the average particle size (D50) of the lump graphite is 1 / 2 to 1 / 4, is contained in an amount of 5 to 15 mass% based on the total graphite. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2014-67583 A Summary of the Invention
[0005] SiO proposed in Patent Document 1 x Since SiO expands significantly during charging and then shrinks during discharging, x In contrast, the presence of flake graphite results in poor electrical contact between the SiO xThe cycle characteristics can be improved by forming a conductive path between the silicon and the lump graphite, but this is not sufficient. In particular, if the expansion and contraction of the silicon-containing material becomes larger, the silicon becomes more likely to become isolated, making it more difficult to maintain the conductive path. The isolation of silicon occurs due to cracks caused by the expansion of silicon.
[0006] One aspect of the present disclosure relates to a negative electrode for a secondary battery, comprising a negative electrode active material capable of absorbing and releasing lithium ions, the negative electrode active material comprising a first carbon material as a main component, and comprising a second carbon material and a silicon-containing material interposed between particles of the first carbon material, wherein an average particle size A of the first carbon material, an average particle size B of the second carbon material, and an average particle size C of the silicon-containing material satisfy A>C≧B.
[0007] Another aspect of the present disclosure relates to a non-aqueous electrolyte secondary battery including the above negative electrode, a positive electrode, and a non-aqueous electrolyte.
[0008] When a silicon-containing material is used in a negative electrode for a secondary battery, excellent discharge capacity and cycle characteristics can be obtained. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a schematic perspective view, with a portion cut away, of a nonaqueous electrolyte secondary battery according to one embodiment of the present disclosure. [Diagram 2] FIG. 2 is a graph showing the relationship between the content w2 of the second carbon material in the negative electrode active material and the initial discharge capacity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The negative electrode for a secondary battery according to the embodiment of the present disclosure includes, as an essential component, a negative electrode active material capable of absorbing and releasing lithium ions. The negative electrode active material includes a first carbon material, a second carbon material, and a silicon-containing material. The second carbon material and the silicon-containing material are interposed between particles of the first carbon material. In other words, the second carbon material and the silicon-containing material are filled in the gaps between particles of the first carbon material.
[0011] The first carbon material is a main component of the negative electrode active material. The content of the first carbon material in the negative electrode active material may be, for example, 75 mass % or more, or may be 80 mass % or more.
[0012] On the other hand, the content of the second carbon material in the negative electrode active material may be, for example, 1 to 15 mass %, or 2 to 10 mass %.
[0013] The content of the silicon-containing material in the negative electrode active material may be 1 to 15 mass %, or may be 2 to 10 mass %.
[0014] Here, the average particle size A of the first carbon material, the average particle size B of the second carbon material, and the average particle size C of the silicon-containing material satisfy A>C>B. By satisfying A>C>B, the current collecting ability of the negative electrode is significantly improved, the discharge capacity is improved, and the cycle characteristics are improved.
[0015] When the negative electrode active material contains the silicon-containing material in the above ratio, the expansion and contraction of the negative electrode as a whole is easily suppressed even when the silicon-containing material repeatedly expands and contracts violently. This is believed to be because, when A>C is satisfied, the silicon-containing material can penetrate into the relatively large gaps formed by the first carbon material.
[0016] The ratio A / C of the average particle size A of the first carbon material to the average particle size C of the silicon-containing material may be, for example, not less than 1.8 and not more than 4. By setting the A / C ratio in this range, the expansion and contraction of the entire negative electrode can be more effectively suppressed.
[0017] Next, when the negative electrode active material contains the second carbon material in the above ratio, during discharge, the silicon-containing material shrinks violently. For example, even if cracks occur in the silicon-containing material, the conduction path between the first carbon material and the silicon-containing material is likely to be maintained. This is because when C≧B is satisfied, even if the silicon-containing material cracks and its particle size becomes smaller, it will not become extremely smaller than the particle size of the second carbon material with a small particle size, and it is considered that the second carbon material can easily enter between the first carbon materials together with the silicon-containing material. At this time, between the first carbon materials, the silicon-containing material and the first carbon material may coexist in a mixed state.
[0018] The ratio of the average particle size C of the silicon-containing material to the average particle size B of the second carbon material: C / B may be, for example, 1 or more and 5 or less. By setting the C / B ratio within such a range, the second carbon material can more easily enter between the first carbon materials together with the silicon-containing material, and furthermore, the silicon-containing material and the first carbon material can more easily mix between the first carbon materials. The C / B ratio may be 1 or more and 4 or less, and may also be 1.2 or more and 3.6 or less.
[0019] On the other hand, even if A>B, if C<B, when the silicon-containing material cracks and its particle size becomes smaller, the difference in particle size between the silicon-containing material with a small particle size and the second carbon material becomes even larger, and it is difficult for the silicon-containing material and the second carbon material to coexist in a mixed state between the first carbon materials.
[0020] The ratio of the average particle size A of the first carbon material to the average particle size B of the second carbon material: A / B may be, for example, 2 or more and 15 or less. By setting A / B to 2 or more, the second carbon material can more easily enter between the first carbon materials. Also, by setting A / B to 15 or less, the difference in particle size between the first carbon material and the second carbon material is not extremely different, and it becomes easy to design both to have appropriate particle sizes and surface areas. The A / B ratio may be 3 or more and 10 or less, and may also be 3.5 or more and 5 or less.
[0021] Here, the average particle size means a particle size (volume average particle size) at which the volume cumulative value is 50% in the particle size distribution measured by the laser diffraction scattering method. For example, the "LA-750" manufactured by HORIBA Co., Ltd. can be used as the measuring device. For example, when the negative electrode active material collected from the negative electrode is measured by the laser diffraction scattering method, a distribution having three peaks of the first carbon material, the silicon-containing material, and the second carbon material is obtained. By separating these peaks, the particle size distributions of the first carbon material, the silicon-containing material, and the second carbon material can be obtained. By analyzing each particle size distribution, the volume average particle size can be obtained.
[0022] The average particle size A of the first carbon material may be, for example, 10 μm or more, or 15 μm or more. The average particle size A may be, for example, 26 μm or less. By setting the average particle size A in the above range, it is easy to suppress side reactions and to obtain a high capacity.
[0023] The average particle size B of the second carbon material may be, for example, less than 10 μm or 8 μm or less. The average particle size B may be, for example, 2 μm or more. By setting the average particle size B in the above range, it becomes easier to form a good conductive path between the negative electrode active materials, and it becomes easier to obtain good discharge capacity and cycle characteristics.
[0024] The average particle size C of the silicon-containing material may be selected so as to satisfy A>C≧B, and may be, for example, 4 μm or more and 15 μm or less, 5 μm or more and 13 μm or less, or 6 μm or more and 11 μm or less. By setting the average particle size C within the above range, it is easy to relieve the stress caused by the volume change of the silicon-containing material accompanying charging and discharging, and it is easy to prevent the silicon-containing material from being isolated and obtain good cycle characteristics. The surface area of the silicon-containing material is also moderate, and the capacity decrease due to the side reaction with the electrolyte is also suppressed.
[0025] The content of the second carbon material in the negative electrode active material may be 1% by mass or more and 15% by mass or less, and may be 3% by mass or more and 12% by mass or less, or 5% by mass or more and 10% by mass or less. If the content of the second carbon material is less than 1% by mass, the conductive path formed by the second carbon material becomes small, making it difficult to obtain good discharge capacity and cycle characteristics. On the other hand, if the content of the second carbon material exceeds 15% by mass, the contribution of the second carbon material to the negative electrode active material becomes large, the specific surface area of the entire negative electrode active material becomes large, and the initial efficiency is easily reduced due to side reactions.
[0026] The content of the silicon-containing material in the negative electrode active material may be 1 to 15% by mass, and may be 3% by mass or more and 12% by mass or less, or 5% by mass or more and 10% by mass or less. If the content of the silicon-containing material is less than 1% by mass, the effect of increasing the negative electrode capacity by the silicon-containing material is not sufficiently exhibited. On the other hand, if the content of the silicon-containing material exceeds 15% by mass, the contribution of the silicon-containing material to the negative electrode active material becomes large, and the expansion and contraction of the negative electrode due to charging and discharging becomes intense, making it difficult to maintain the conductive path, and the cycle characteristics are likely to deteriorate.
[0027] The content of the first carbon material in the negative electrode active material may be, for example, 75 mass% or more, and may be 80 mass% or more. That is, the first carbon material is the main component of the negative electrode active material. By using the first carbon material having a relatively large average particle size as the main component, it is easy to suppress side reactions in the entire negative electrode and to obtain a high capacity.
[0028] The negative electrode active material may contain a material that absorbs and releases lithium ions in addition to the first carbon material, the second carbon material, and the silicon-containing material. For example, the negative electrode active material may contain another carbon material in addition to the first carbon material and the second carbon material. However, the total content of the first carbon material, the second carbon material, and the silicon-containing material in the entire negative electrode active material is preferably 90% by mass or more, more preferably 95% by mass or more. This increases the effect of promoting and stabilizing the formation of a conductive path, which is achieved by the coexistence of the first carbon material, the second carbon material, and the silicon-containing material. Similarly, the total content of the first carbon material and the second carbon material in the entire carbon material contained in the negative electrode active material is preferably 90% by mass or more, more preferably 95% by mass or more.
[0029] (First carbon material) Examples of the first carbon material include graphite materials, non-graphitizable carbon, graphitizable carbon, and amorphous carbon. These may be used alone or in combination. Among them, graphite materials are preferred. Graphite materials are a general term for carbon materials having a graphite-type crystal structure. Graphite materials have excellent charge / discharge stability and low irreversible capacity.
[0030] Here, graphite refers to a carbon material in which the average interplanar spacing d002 of the (002) plane measured by X-ray diffraction is 0.340 nm or less.
[0031] Graphite materials include natural graphite, artificial graphite, graphitized mesophase carbon particles, etc. From the viewpoint of cost, it is advantageous to use natural graphite, but from the viewpoint of performance, artificial graphite is preferable. Natural graphite and artificial graphite may be used in combination, or natural graphite and artificial graphite may be used in combination.
[0032] The graphite material used as the first carbon material may be massive graphite. Massive graphite refers to a graphite material having a smaller aspect ratio (or a larger circularity) than so-called flake graphite. The aspect ratio of the graphite material is expressed as the A / B ratio, where A is the length in the long axis direction (i.e., the maximum length) of the graphite particle, and B is the length in the short axis direction (the maximum length perpendicular to the maximum length A). The aspect ratio is at least 1, and graphite particles with an aspect ratio of less than 5 are massive graphite, and graphite particles with an aspect ratio of 5 or more are, for example, flake graphite.
[0033] The aspect ratio can be determined from a scanning electron microscope (SEM) photograph of the graphite particles. For example, the A / B ratio of 100 arbitrary graphite particles is measured, and the arithmetic mean value of these measurements is taken as the aspect ratio.
[0034] In the case of artificial graphite, for example, after granulating coke as a main raw material, the coke is calcined, crushed to a predetermined size, and sieved to obtain lump graphite. In the case of natural graphite, lump graphite can be obtained by spheroidizing flake-like natural graphite and sieving it. The lump graphite may have a surface layer of amorphous carbon. The surface layer of amorphous carbon can be formed, for example, by mixing lump graphite and petroleum pitch under heating in an inert gas atmosphere, calcining, and then pulverizing and classifying the mixture.
[0035] (Second carbon material) As the second carbon material, graphite materials, non-graphitizable carbon, graphitizable carbon, amorphous carbon, etc. can be used. These may be used alone or in combination. Among them, graphite materials are preferred.
[0036] The graphite material used as the second carbon material may be flake graphite. The aspect ratio (A / B ratio) of the flake graphite may be 5 or more. The flake graphite can be obtained by crushing natural graphite or artificial graphite into flakes, firing it as necessary, crushing it, and classifying it.
[0037] (Silicon-containing materials) The silicon-containing material may be any material containing silicon with a higher capacity than the carbon material, but silicon alone is prone to pulverization due to expansion and contraction associated with charging and discharging. Therefore, it is desirable to use a composite material of a lithium ion conductive phase and silicon particles dispersed in the lithium ion conductive phase. By dispersing the silicon particles in the lithium ion conductive phase, pulverization due to expansion and contraction of the silicon particles is significantly suppressed.
[0038] In addition, when the lithium ion conductive phase does not have electronic conductivity, at least a part of the surface of the silicon-containing material may be covered with a conductive layer. The conductive layer may be formed of a material having electronic conductivity, for example, a carbon material. By covering the surface of the silicon-containing material with a conductive layer, the conductivity can be dramatically increased. It is preferable that the conductive layer is thin enough not to substantially affect the average particle size of the silicon-containing material.
[0039] A composite material of a lithium ion conductive phase and silicon particles will be exemplified below.
[0040] (1st composite material) The first composite material has silicate as a lithium ion conductive phase. That is, the first composite material (hereinafter also referred to as LSX material) has a silicate phase and silicon particles dispersed in the silicate phase. Here, the silicate is a silicate compound containing at least one selected from the group consisting of alkali metal elements and Group 2 elements. Since silicate is formed of a salt of a metal element cation and a silicate anion, it has a small irreversible capacity and is difficult to take in lithium ions, so that it is easy to achieve excellent initial efficiency.
[0041] The first composite material is produced by compounding silicate and silicon. In this case, the mixing ratio of silicate and silicon can be determined arbitrarily. In other words, by increasing the ratio of silicon to silicate, a first composite material with a desired high capacity can be obtained. However, the higher the ratio of silicon to silicate, the more significantly the volume change caused by the expansion and contraction of silicon particles during charging and discharging becomes. In such a case, the combined use of the first carbon material and the second carbon material that satisfy A>B is insufficient to achieve good cycle characteristics, and it is particularly important to use a silicon-containing material that satisfies C≧B.
[0042] From the viewpoint of increasing capacity, the average particle size of silicon particles is usually 50 nm or more, preferably 100 nm or more, before the first charge. The LSX material can be produced, for example, by pulverizing a mixture of silicate and raw silicon using a pulverizing device such as a ball mill to produce fine particles, and then heat-treating the mixture in an inert atmosphere. The LSX material may also be produced by synthesizing fine particles of silicate and fine particles of raw silicon without using a pulverizing device, and heat-treating the mixture in an inert atmosphere. The amount and size of silicon particles dispersed in the silicate phase can be controlled by adjusting the mixing ratio of silicate and raw silicon and the particle size of the raw silicon.
[0043] From the viewpoint of suppressing cracks in the silicon particles themselves, the average particle size of the silicon particles is preferably 500 nm or less, more preferably 200 nm or less, before the first charge. After the first charge, the average particle size of the silicon particles is preferably 400 nm or less. By making the silicon particles finer, the volume change during charging and discharging is reduced, and the structural stability of the first composite material is further improved.
[0044] The average particle size of the silicon particles is measured using a SEM photograph of the cross section of the first composite material. Specifically, the maximum diameters of 100 random silicon particles are measured, and the arithmetic mean value of these measurements is taken as the average particle size of the silicon particles.
[0045] The silicon particles dispersed in the lithium ion conductive phase have a particulate phase of simple silicon (Si) and are usually composed of multiple crystallites. The crystallite size of the silicon particles is preferably 30 nm or less. When the crystallite size of the silicon particles is 30 nm or less, the amount of volume change due to the expansion and contraction of the silicon particles accompanying charging and discharging can be reduced, and the cycle characteristics can be further improved. The lower limit of the crystallite size of the silicon particles is not particularly limited, but is, for example, 1 nm or more.
[0046] The crystallite size of the silicon particles is more preferably 10 nm or more and 30 nm or less, and further preferably 15 nm or more and 25 nm or less. When the crystallite size of the silicon particles is 10 nm or more, the surface area of the silicon particles can be kept small, so that the deterioration of the silicon particles accompanied by the generation of irreversible capacity is unlikely to occur.
[0047] The crystallite size of silicon particles is calculated from the half-width of the diffraction peak assigned to the Si(111) plane in the X-ray diffraction (XRD) pattern of the silicon particles by Scherrer's formula.
[0048] From the viewpoint of increasing the capacity, the content of silicon particles in the first composite material is preferably 30% by mass or more, more preferably 35% by mass or more, and even more preferably 55% by mass or more. In this case, the diffusibility of lithium ions is good, and excellent load characteristics are easily obtained. On the other hand, from the viewpoint of improving cycle characteristics, the content of silicon particles in the first composite material is preferably 95% by mass or less, more preferably 75% by mass or less, and even more preferably 70% by mass or less. In this case, the surface of the silicon particles that is exposed without being covered with the lithium ion conductive phase is reduced, and the reaction between the electrolyte and the silicon particles is easily suppressed.
[0049] The content of silicon particles can be measured by Si-NMR. The preferable measurement conditions for Si-NMR are shown below.
[0050] Measurement equipment: Varian solid-state nuclear magnetic resonance spectrometer (INOVA-400) Probe: Varian 7mm CPMAS-2 MAS: 4.2 kHz MAS speed: 4 kHz Pulse: DD (45° pulse + signal acquisition time 1H decouple) Repetition time: 1200 sec Observation width: 100 kHz Observation center: around -100 ppm Signal acquisition time: 0.05 sec Number of integrations: 560 Sample amount: 207.6 mg The silicate phase contains at least one of an alkali metal element (Group 1 element other than hydrogen in the long-period periodic table) and a Group 2 element of the long-period periodic table. The alkali metal elements include lithium (Li), potassium (K), sodium (Na), etc. The Group 2 elements include magnesium (Mg), calcium (Ca), barium (Ba), etc. Among them, a silicate phase containing lithium (hereinafter also referred to as a lithium silicate phase) is preferable because it has a small irreversible capacity and a high initial charge-discharge efficiency. That is, the LSX material is preferably a composite material containing a lithium silicate phase and silicon particles dispersed in the lithium silicate phase.
[0051] The silicate phase is, for example, a lithium silicate phase (oxide phase) containing lithium (Li), silicon (Si), and oxygen (O). The atomic ratio of O to Si in the lithium silicate phase: O / Si is, for example, greater than 2 and less than 4. When O / Si is greater than 2 and less than 4 (z is 0 < z < 2 in the formula described later), it is advantageous in terms of stability and lithium ion conductivity. Preferably, O / Si is greater than 2 and less than 3 (z is 0 < z < 1 in the formula described later). The atomic ratio of Li to Si in the lithium silicate phase: Li / Si is, for example, greater than 0 and less than 4.
[0052] In addition to Li, Si, and O, the lithium silicate phase may contain trace amounts of other elements such as iron (Fe), chromium (Cr), nickel (Ni), manganese (Mn), copper (Cu), molybdenum (Mo), zinc (Zn), aluminum (Al), zirconium (Zr), niobium (Nb), tantalum (Ta), vanadium (V), titanium (Ti), bismuth (Bi), tin (Sn), lead (Pb), antimony (Sb), cobalt (Co), fluorine (F), boron (B), phosphorus (P), lanthanum (La), etc.
[0053] The lithium silicate phase may have a composition represented by the formula: Li 2z SiO 2+z (0 < z < 2). From the viewpoints of stability, ease of preparation, lithium ion conductivity, etc., z preferably satisfies the relationship of 0 < z < 1, and more preferably z = 1 / 2.
[0054] The lithium silicate phase has fewer sites that can react with lithium compared to the SiO x SiO2 phase. Therefore, LSX is less likely to generate an irreversible capacity associated with charge and discharge compared to SiO x . When silicon particles are dispersed in the lithium silicate phase, excellent charge and discharge efficiency can be obtained at the initial stage of charge and discharge. In addition, since the content of silicon particles can be arbitrarily changed, a high-capacity negative electrode can be designed.
[0055] The composition of the silicate phase of the first composite material can be analyzed, for example, by the following method.
[0056] The battery is disassembled, the negative electrode is removed, washed with a non-aqueous solvent such as ethylene carbonate, dried, and then the cross section of the negative electrode mixture layer is processed using a cross section polisher (CP) to obtain a sample. A backscattered electron image of the sample cross section is obtained using a field emission scanning electron microscope (FE-SEM), and the cross section of the first composite material is observed. An Auger electron spectroscopy (AES) analyzer is used to perform qualitative and quantitative elemental analysis of the silicate phase of the observed first composite material (accelerating voltage 10 kV, beam current 10 nA). For example, the composition of the lithium silicate phase is determined based on the obtained contents of lithium (Li), silicon (Si), oxygen (O), and other elements.
[0057] In the cross-sectional observation and analysis of the above samples, a carbon sample stage can be used to fix the sample in place to prevent diffusion of Li. A transfer vessel can be used to hold and transport the sample without exposing it to the atmosphere to prevent deterioration of the sample cross section.
[0058] (Second composite material) The second composite material has a SiO2 phase as a lithium ion conductive phase. x The second composite material has a SiO2 phase and silicon particles dispersed within the SiO2 phase. The overall composition of the second composite material is SiO x where x is, for example, about 0.5 or more and 1.5 or less.
[0059] The second composite material is obtained by heat treating silicon monoxide and separating it through a disproportionation reaction into a SiO2 phase and fine Si phase (silicon particles) dispersed within the SiO2 phase.
[0060] The silicon particles in the second composite material are smaller than those in the first composite material, and the average particle size of the silicon particles in the second composite material is, for example, about 5 nm. The second composite material has a smaller capacity and a larger irreversible capacity than the first composite material, but expands less during charging. Therefore, compared to the case where the first composite material is used, the improvement in cycle characteristics by setting A>C≧B is smaller.
[0061] When the negative electrode active material contains both the first composite material and the second composite material, the amount of the second composite material per 100 parts by mass of the first composite material may be, for example, 10 parts by mass or more and 100 parts by mass or less. By using both in such a ratio, it is possible to achieve a good balance between increasing the capacity of the negative electrode and improving the cycle characteristics.
[0062] In addition, the first composite material and the second composite material can be distinguished from each other in the cross section of the negative electrode sample. Usually, the average particle size of the silicon particles in the first composite material is larger than the average particle size of the silicon particles in the second composite material, and the two can be easily distinguished by observing the particle sizes.
[0063] The non-aqueous electrolyte secondary battery according to the embodiment of the present disclosure includes the above-mentioned negative electrode, a positive electrode, and a non-aqueous electrolyte. The negative electrode, the positive electrode, and the non-aqueous electrolyte will be described below.
[0064] [Negative electrode] The negative electrode includes, for example, a negative electrode current collector and a negative electrode mixture layer formed on the surface of the negative electrode current collector and containing a negative electrode active material. The negative electrode mixture layer can be formed by applying a negative electrode slurry in which the negative electrode mixture is dispersed in a dispersion medium to the surface of the negative electrode current collector and drying it. The coating film after drying may be rolled as necessary. The negative electrode mixture layer may be formed on one surface of the negative electrode current collector or on both surfaces. The negative electrode mixture contains a negative electrode active material as an essential component, and may contain a binder, a conductive agent, a thickener, etc. as optional components.
[0065] The negative electrode current collector may be, for example, a metal foil. Examples of the material of the negative electrode current collector include stainless steel, nickel, nickel alloy, copper, copper alloy, etc. The thickness of the negative electrode current collector is, for example, 5 to 20 μm.
[0066] Examples of the binder include resin materials, such as fluororesins such as polytetrafluoroethylene and polyvinylidene fluoride (PVDF), polyolefin resins such as polyethylene and polypropylene, polyamide resins such as aramid resin, polyimide and polyamideimide resins, acrylic resins such as polyacrylic acid, polymethyl acrylate, and ethylene-acrylic acid copolymers, vinyl resins such as polyacrylonitrile and polyvinyl acetate, polyvinylpyrrolidone, polyethersulfone, and rubber-like materials such as styrene-butadiene copolymer rubber (SBR). These may be used alone or in combination of two or more.
[0067] Examples of conductive agents include carbon blacks such as acetylene black; conductive fibers such as carbon fibers and metal fibers; carbon fluoride; metal powders such as aluminum; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and organic conductive materials such as phenylene derivatives. These may be used alone or in combination of two or more. Carbon blacks and carbon fibers can occlude lithium ions, but are not usually included in the negative electrode active material because of their small capacity. On the other hand, the second carbon material also functions as a conductive agent.
[0068] Examples of thickeners include carboxymethylcellulose (CMC) and its modified products (including salts such as Na salt), cellulose derivatives such as methylcellulose (cellulose ether, etc.), saponified polymers having vinyl acetate units such as polyvinyl alcohol, polyethers (polyalkylene oxides such as polyethylene oxide, etc.), etc. These may be used alone or in combination of two or more.
[0069] The dispersion medium is not particularly limited, but examples thereof include water, alcohols such as ethanol, ethers such as tetrahydrofuran, amides such as dimethylformamide, N-methyl-2-pyrrolidone (NMP), and mixed solvents thereof.
[0070] [Positive electrode] The positive electrode includes, for example, a positive electrode current collector and a positive electrode mixture layer formed on the surface of the positive electrode current collector. The positive electrode mixture layer can be formed by applying a positive electrode slurry in which a positive electrode mixture is dispersed in a dispersion medium to the surface of the positive electrode current collector and drying it. The dried coating film may be rolled if necessary. The positive electrode mixture layer may be formed on one surface of the positive electrode current collector or on both surfaces. The positive electrode mixture contains a positive electrode active material as an essential component and may contain, as optional components, a binder, a conductive agent, a thickening agent, and the like.
[0071] Examples of the positive electrode active material include lithium transition metal oxides containing transition metal elements such as Co, Mn, and Ni. Examples of the lithium transition metal oxide include, for example, Li x CoO2, Li x NiO2, Li x MnO2, Li x Co y Ni 1-y O2, Li x Co y M 1-y O z , Li x Ni 1-y M y O z , Li x Mn2O4, Li x Mn 2-y M y O4, LiMPO4, Li2MPO4F, and the like. Here, M is at least one selected from the group consisting of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, B, Nb, Si, Ti, Sn, Zr, Mo, Ta, W, K, Ba, Sr, Bi, Be, Zn, and Ca, and satisfies 0 < x ≦ 1.2, 0 < y ≦ 0.9, and 2.0 ≦ z ≦ 2.3. These may be used alone or in combination of multiple kinds.
[0072] From the viewpoint of increasing the capacity, the positive electrode active material is Li x Ni 1-y M y O z(M contains at least one selected from the group consisting of Mn, Co, and Al, 0 < x ≦ 1.2, 0 ≦ y ≦ 0.7) lithium nickel composite oxide is preferred. From the viewpoint of further increasing the capacity, it is preferably satisfied that 0 ≦ y ≦ 0.5. The a value indicating the molar ratio of lithium is the value immediately after the production of the active material and increases or decreases by charge and discharge.
[0073] As the binder, conductive agent, thickener, and dispersion medium, the same ones as those exemplified for the negative electrode can be used. As the conductive agent, graphite such as natural graphite and artificial graphite may be used.
[0074] As the positive electrode current collector, for example, a metal foil is used. Examples of the material of the positive electrode current collector include stainless steel, aluminum, aluminum alloy, titanium, and the like. The thickness of the positive electrode current collector is, for example, 5 to 20 μm.
[0075] [Non-aqueous electrolyte] The non-aqueous electrolyte contains a non-aqueous solvent and a lithium salt dissolved in the non-aqueous solvent. The concentration of the lithium salt in the non-aqueous electrolyte is, for example, 0.5 to 2 mol / L. The non-aqueous electrolyte may contain a known additive.
[0076] Examples of the non-aqueous solvent include cyclic carbonates, chain carbonates, cyclic carboxylic acid esters, and the like. Examples of the cyclic carbonate include propylene carbonate (PC), ethylene carbonate (EC), and the like. Examples of the chain carbonate include diethyl carbonate (DEC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), and the like. Examples of the cyclic carboxylic acid ester include γ-butyrolactone (GBL), γ-valerolactone (GVL), and the like. The non-aqueous solvent may be used alone or in combination of two or more.
[0077] Examples of the lithium salt include lithium salts of chlorine-containing acids (LiClO4, LiAlCl4, LiB 10 Cl 10etc.), lithium salts of fluorine-containing acids (LiPF6, LiBF4, LiSbF6, LiAsF6, LiCF3SO3, LiCF3CO2, etc.), lithium salts of fluorine-containing acid imides (LiN(CF3SO2)2, LiN(CF3SO2)(C4F9SO2), LiN(C2F5SO2)2, etc.), lithium halides (LiCl, LiBr, LiI, etc.), etc., can be used. One type of lithium salt may be used alone, or two or more types may be used in combination.
[0078] [Separator] Usually, it is desirable to interpose a separator between the positive electrode and the negative electrode. The separator has high ion permeability and has appropriate mechanical strength and insulation properties. As the separator, a microporous thin film, a woven fabric, a nonwoven fabric, etc. can be used. As the material of the separator, polyolefin such as polypropylene and polyethylene is preferable.
[0079] An example of the structure of the non-aqueous electrolyte secondary battery is a structure in which an electrode group formed by winding a positive electrode and a negative electrode with a separator interposed therebetween and a non-aqueous electrolyte are housed in an exterior body. Alternatively, instead of a wound type electrode group, other types of electrode groups may be applied, such as a stacked type electrode group formed by stacking a positive electrode and a negative electrode with a separator interposed therebetween. The non-aqueous electrolyte secondary battery may be in any form, such as a cylindrical type, a square type, a coin type, a button type, a laminate type, or the like.
[0080] FIG. 1 is a schematic perspective view, with a portion cut away, of a prismatic nonaqueous electrolyte secondary battery according to one embodiment of the present disclosure.
[0081] The battery includes a bottomed prismatic battery case 4, and an electrode group 1 and a non-aqueous electrolyte (not shown) housed within the battery case 4. The electrode group 1 includes a long strip-shaped negative electrode, a long strip-shaped positive electrode, and a separator interposed between them to prevent direct contact. The electrode group 1 is formed by winding the negative electrode, positive electrode, and separator around a flat plate-shaped winding core and then removing the winding core.
[0082] One end of the negative electrode lead 3 is attached to the negative electrode current collector of the negative electrode by welding or the like. The other end of the negative electrode lead 3 is electrically connected to a negative electrode terminal 6 provided on the sealing plate 5 via a resin insulating plate (not shown). The negative electrode terminal 6 is insulated from the sealing plate 5 by a resin gasket 7. One end of the positive electrode lead 2 is attached to the positive electrode current collector of the positive electrode by welding or the like. The other end of the positive electrode lead 2 is connected to the back surface of the sealing plate 5 via an insulating plate. That is, the positive electrode lead 2 is electrically connected to the battery case 4 which also serves as the positive electrode terminal. The insulating plate separates the electrode group 1 and the sealing plate 5, and separates the negative electrode lead 3 and the battery case 4. The periphery of the sealing plate 5 is fitted into the open end of the battery case 4, and the fitting portion is laser welded. In this way, the opening of the battery case 4 is sealed with the sealing plate 5. The electrolyte injection hole provided in sealing plate 5 is closed with a sealing plug 8 .
[0083] <Example> Hereinafter, the present disclosure will be specifically described based on examples and comparative examples, but the present disclosure is not limited to the following examples.
[0084] <Example 1> [First carbon material] We prepared lump artificial graphite with an average particle size A of 23 μm. Here, lump graphite synthesized using coke as a raw material was mixed with petroleum pitch, and then fired under an inert gas atmosphere. After that, it was crushed and classified to adjust the average particle size to 23 μm.
[0085] [Second carbon material] Flake-like natural graphite with an average particle size B of 6 μm was prepared. Here, the natural graphite was crushed and classified to adjust the average particle size to 6 μm.
[0086] [LSX material] Process (i) Silicon dioxide and lithium carbonate were mixed to an atomic ratio of Si / Li = 1, and the mixture was fired in air at 950°C for 10 hours to obtain lithium silicate represented by Li2Si2O5. The obtained lithium silicate was pulverized to an average particle size of 10 μm.
[0087] Process (ii) Powdered Li2Si2O5 (average particle size 10 μm) as lithium silicate and powdered raw silicon (3N, average particle size 10 μm) were mixed in a mass ratio of 50:50 and loaded into a pot (made of SUS, volume: 500 mL) of a planetary ball mill (manufactured by Fritsch, P-5). 24 SUS balls (diameter 20 mm) were added and the lid was closed, and the mixture was milled at 200 rpm for 50 hours in an inert atmosphere.
[0088] Next, the powder mixture was taken out in an inert atmosphere, and sintered at 600° C. for 4 hours while applying a predetermined pressure to the mixture using a hot press, to obtain a sintered body of the mixture.
[0089] Process (iii) The sintered body was then crushed and passed through a 40 μm mesh, and then mixed with coal pitch (MCP250, manufactured by JFE Chemical Corporation). The mixture was sintered in an inert atmosphere at 800°C for 5 hours to coat the surfaces of the composite particles with conductive carbon to form a conductive layer. The amount of the conductive layer was 5 mass% based on the total mass of the composite particles and the conductive layer. Then, a sieve was used to obtain an LSX material (average particle size C1 = 9 μm) having a conductive layer on its surface.
[0090] When the cross section of the LSX material was observed using a SEM, it was confirmed that Si particles with an average particle size of 50 nm were dispersed almost uniformly in a matrix made of Li2Si2O5. The XRD pattern of the LSX material showed diffraction peaks mainly due to elemental Si and Li2Si2O5, and the peak intensity was 1.0 times that of Li2Si2O5. <Siであった。
[0091] Measurement by Si-NMR confirmed that the content of Si particles in the LSX material (lithium silicate phase and Si particles) was 50 mass%.
[0092] [SiO x material] The disproportionation reaction of silicon monoxide causes the SiO2 phase and silicon particles to be separated and generated, resulting in an overall composition of SiOx SiO represented by (X=1) x The material (average particle size C2 = 6 μm) was obtained. SiO x A conductive layer similar to that of the LSX material was also formed on the surface of the material.
[0093] [Preparation of negative electrode] 86 parts by mass of the first carbon material, 5 parts by mass of the second carbon material, 5 parts by mass of an LSX material having a conductive layer on its surface, and a SiO x The material was mixed with 4 parts by mass and used as the negative electrode active material. The A / C ratio was 3, and the C / B ratio was 1.3. Here, the average particle size C was calculated as C = (C1 (9 μm) × 5 parts by mass + C2 (6 μm) × 4 parts by mass) / (5 parts by mass + 4 parts by mass) = (45 + 24) / 9 = 7.67.
[0094] The negative electrode active material, sodium carboxymethylcellulose (CMC-Na), and styrene-butadiene rubber (SBR) were mixed in a mass ratio of 97.5:1:1.5, water was added, and the mixture was stirred using a mixer to prepare a negative electrode slurry. The negative electrode slurry was then applied to the surface of a copper foil, the coating was dried, and the mixture was rolled to form a negative electrode slurry having a density of 1.5 g / cm on both sides of the copper foil. 3 Thus, a negative electrode having a negative electrode mixture layer of the above formula was fabricated.
[0095] [Preparation of positive electrode] Lithium cobalt oxide, acetylene black, and polyvinylidene fluoride were mixed in a mass ratio of 95:2.5:2.5, N-methyl-2-pyrrolidone (NMP) was added, and the mixture was stirred using a mixer to prepare a positive electrode slurry. The positive electrode slurry was then applied to the surface of an aluminum foil, the coating was dried, and the mixture was rolled to form a positive electrode slurry having a density of 3.6 g / cm on both sides of the aluminum foil. 3 A positive electrode having a positive electrode mixture layer of the above formula was fabricated.
[0096] [Preparation of non-aqueous electrolyte] A non-aqueous electrolyte was prepared by dissolving LiPF6 at a concentration of 1.0 mol / L in a mixed solvent containing ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 3:7.
[0097] [Preparation of non-aqueous electrolyte secondary battery (laminate type battery)] A tab was attached to each electrode, and the positive and negative electrodes were spirally wound with a separator interposed therebetween so that the tabs were located at the outermost periphery to produce an electrode group. The electrode group was inserted into an exterior body made of an aluminum laminate film and vacuum dried at 105°C for 2 hours, after which a nonaqueous electrolyte solution was poured in and the opening of the exterior body was sealed to obtain a nonaqueous electrolyte secondary battery A1 (design capacity: 800mAh).
[0098] <Example 2> 81 parts by mass of the first carbon material, 10 parts by mass of the second carbon material, 5 parts by mass of an LSX material having a conductive layer on its surface, and a SiO x A negative electrode was produced in the same manner as in Example 1, except that 4 parts by mass of the material was mixed and used as the negative electrode active material, and further a battery A2 was produced.
[0099] <Comparative Example 1> In this example, the second carbon material was not used. That is, the mixture was 91 parts by mass of the first carbon material, 5 parts by mass of the LSX material having a conductive layer on its surface, and SiO x A negative electrode was produced in the same manner as in Example 1, except that 4 parts by mass of the material was mixed and used as the negative electrode active material, and further a battery B1 was produced.
[0100] <Example 3> A negative electrode was prepared in the same manner as in Example 1, except that the average particle size of the LSX material was changed to 12 μm, and a battery A3 was prepared. The A / C ratio was 2.5, and the C / B ratio was 1.6. Here, the average particle size C was calculated as follows: C = (C1 (12 μm) × 5 parts by mass + C2 (6 μm) × 4 parts by mass) / (5 parts by mass + 4 parts by mass) = (60 + 24) / 9 = 9.33.
[0101] <Example 4> A negative electrode was prepared in the same manner as in Example 2, except that the average particle size of the LSX material was changed to 12 μm, and further a battery A4 was prepared.
[0102] <Comparative Example 2> A negative electrode was prepared in the same manner as in Comparative Example 1, except that the average particle size of the LSX material was changed to 12 μm, and further a battery B2 was prepared.
[0103] [Cycle characteristics] After repeating the charge-discharge cycle 100 times under the following conditions, the discharge capacity after the charge-discharge cycle was determined.
[0104] <charging> In an environment of 25° C., constant current charging was performed at a current of 400 mA until the voltage reached 4.2 V, and then constant voltage charging was performed at a voltage of 4.2 V until the current reached 40 mA. After charging, the battery was left to rest for 20 minutes in an environment of 25° C.
[0105] <Discharge> After the rest, constant current discharge was performed at a current of 800 mA in an environment of 25° C. until the voltage reached 2.5 V.
[0106] The capacity retention rate was calculated from the discharge capacities before and after the charge-discharge cycles obtained above according to the following formula.
[0107] Capacity retention rate after charge-discharge cycles (%) = (discharge capacity after charge-discharge cycles / initial discharge capacity) x 100 The evaluation results of the cycle characteristics are shown in Table 1. In Table 1, the content of the second carbon material in the negative electrode active material is shown as w2.
[0108] [Table 1]
[0109] [Initial capacity] Using the negative electrodes of Examples 1 and 2 and Comparative Example 1, single-electrode cells a1, a2 and b1 containing metallic lithium as a counter electrode were produced.
[0110] Each single-electrode cell was charged and discharged under the following conditions to determine the initial discharge capacity.
[0111] <charging> In an environment of 25° C., constant current charging was performed at a rate of 0.1 C until the voltage reached 5 mV. After charging, the battery was left to rest for 20 minutes in an environment of 25° C.
[0112] <Discharge> After the rest, constant current discharge was performed at a rate of 0.1 C in an environment of 25° C. until the voltage reached 1 V.
[0113] The relative value (Index) of each single-electrode cell was determined by setting the initial discharge capacity of the single-electrode cell using the negative electrode of Comparative Example 1 as 100. Fig. 2 shows the relationship between the content w2 of the second carbon material in the negative electrode active material and the initial discharge capacity.
[0114] The initial capacity of the battery a1 was increased compared to the battery b1, and the capacity retention rate of the battery A1 was improved compared to the battery B1. The initial capacity of the battery a2 was not significantly increased, but as shown in Table 1, the capacity retention rate of the battery A2 was remarkably improved. From these results, it can be understood that by using an appropriate amount of the second carbon material, it is possible to achieve both excellent discharge capacity and cycle characteristics. In this case, it can be understood that the content (w2) of the second carbon material in the negative electrode active material is preferably 15 mass% or less, for example, 5 mass% or more, and for example, 10 mass% or less. A similar tendency was also seen in the comparison of the batteries A3, B2, and A4.
[0115] Next, comparing batteries A1, A2, and B1 with batteries A3, A4, and B2, it can be seen that when the average particle size of the silicon-containing material is larger, the effect of improving the cycle characteristics by using the second carbon material tends to be greater. [Industrial Applicability]
[0116] The negative electrode for a secondary battery according to the present disclosure is useful for nonaqueous electrolyte secondary batteries that serve as the main power sources for mobile communication devices, portable electronic devices, and the like. [Explanation of symbols]
[0117] 1 electrode group 2 Positive Lead 3 Negative lead 4 Battery case 5 Sealing plate 6 Negative terminal 7 Gasket 8. Sealing
Claims
1. A negative electrode active material capable of absorbing and releasing lithium ions is included, the negative electrode active material contains a first carbon material as a main component, and contains a second carbon material and a silicon-containing material interposed between particles of the first carbon material; an average particle size A of the first carbon material, an average particle size B of the second carbon material, and an average particle size C of the silicon-containing material satisfy A>C≧B; a ratio A / C of an average particle size A of the first carbon material to an average particle size C of the silicon-containing material is 1.8 or more and 4 or less.
2. 2 . The negative electrode for a secondary battery according to claim 1 , wherein a ratio C / B of an average particle size C of the silicon-containing material to an average particle size B of the second carbon material is 1 or more and 5 or less.
3. A negative electrode active material capable of absorbing and releasing lithium ions is included, the negative electrode active material contains a first carbon material as a main component, and contains a second carbon material and a silicon-containing material interposed between particles of the first carbon material; an average particle size A of the first carbon material, an average particle size B of the second carbon material, and an average particle size C of the silicon-containing material satisfy A>C≧B; a ratio A / B of an average particle size A of the first carbon material to an average particle size B of the second carbon material is 2 or more and 15 or less.
4. 4. The negative electrode for a secondary battery according to claim 1, wherein the first carbon material has an average particle size A of 26 μm or less.
5. A negative electrode active material capable of absorbing and releasing lithium ions is included, the negative electrode active material contains a first carbon material as a main component, and contains a second carbon material and a silicon-containing material interposed between particles of the first carbon material; an average particle size A of the first carbon material, an average particle size B of the second carbon material, and an average particle size C of the silicon-containing material satisfy A>C≧B; The second carbon material has an average particle size B of 2 μm or more and less than 10 μm.
6. A negative electrode active material capable of absorbing and releasing lithium ions is included, the negative electrode active material contains a first carbon material as a main component, and contains a second carbon material and a silicon-containing material interposed between particles of the first carbon material; an average particle size A of the first carbon material, an average particle size B of the second carbon material, and an average particle size C of the silicon-containing material satisfy A>C≧B; The silicon-containing material comprises a lithium ion conductive phase and silicon particles dispersed within the lithium ion conductive phase.
7. The negative electrode for a secondary battery according to claim 6 , wherein the lithium ion conductive phase comprises a silicate.
8. 8. The negative electrode for a secondary battery according to claim 6, wherein the lithium ion conductive phase comprises silicon dioxide.
9. A non-aqueous electrolyte secondary battery comprising the negative electrode according to any one of claims 1 to 8, a positive electrode, and a non-aqueous electrolyte.
Citation Information
Patent Citations
Negative electrode active material for lithium ion secondary battery, negative electrode for lithium ion secondary battery, and lithium ion secondary battery
JP2004349164A
Electrode structure for lithium secondary battery and secondary battery having such electrode structure
JP2007165061A
Nonaqueous electrolyte secondary battery
JP2014067583A
Silicon-containing composite material
JP2014107013A
Silicon / carbon composite materials, methods for synthesizing them, and uses of such materials
JP2014503972A