Organopolysiloxane, ultraviolet-curable silicone composition and cured product

The UV-curable silicone composition with a specific organopolysiloxane and photoinitiator ensures complete curing in oxygen-rich environments, improving productivity and workability for applications such as 3D printing and adhesives.

JP7591863B2Active Publication Date: 2024-11-29SHIN ETSU CHEMICAL CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2019050681
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-03-19
Publication Date
2024-11-29
Estimated Expiration
2039-03-19

AI Technical Summary

Technical Problem

Existing ultraviolet curable silicone compositions face surface curing inhibition when cured in the presence of oxygen, leading to incomplete curing and the need for additional cleaning steps.

Method used

A UV-curable silicone composition comprising a specific organopolysiloxane component with acryloyl or methacryloyl groups, a photoinitiator, and optional (meth)acrylate compounds, which allows for complete curing even in the presence of oxygen.

Benefits of technology

The composition achieves complete surface curing without inhibition, enhancing productivity and workability, making it suitable for applications like 3D printing, adhesives, and microtransfers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591863000001
    Figure 0007591863000001
  • Figure 0007591863000002
    Figure 0007591863000002
  • Figure 0007591863000003
    Figure 0007591863000003
Patent Text Reader

Abstract

To provide ultraviolet curable organopolysiloxane that has excellent convenience and is prevented from causing surface curing inhibition even when the ultraviolet curable organopolysiloxane is cured in atmosphere, to provide a composition including the ultraviolet curable organopolysiloxane, and to provide a cured product from the ultraviolet curable organopolysiloxane.SOLUTION: The organopolysiloxane is represented by Formula (1), in which R1 has at least one group represented by Formula (2) in one molecule, and m is a number satisfying 1≤m≤10,000, and in which R2 is a group having at least one of acryloyl group, methacryloyl group, acryloyloxyalkyl group, and methacryloyloxyalkyl group).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an organopolysiloxane, an ultraviolet-curable silicone composition containing the same, and a cured product thereof. [Background technology]

[0002] For the curing of silicone compositions, crosslinking reactions using hydrosilylation reactions, heat curing reactions using peroxide as an initiator, and condensation crosslinking reactions using moisture in the air have long been used. In recent years, as energy saving and process shortening are increasingly required, ultraviolet curing reactions that can be cured in a short time at room temperature have attracted attention. Among ultraviolet curing reactions, the reaction system of ultraviolet curing radical polymerization reactions in particular can be made into a one-liquid system, and has excellent storage stability if stored without light irradiation (Patent Documents 1 and 2). However, when existing ultraviolet curing silicone compositions are cured in the atmosphere, there is a problem that curing inhibition occurs due to oxygen, and the surface layer of the cured product does not cure. If an existing ultraviolet curing silicone composition is sandwiched between transparent members and irradiated with ultraviolet light, curing inhibition does not occur, but the protruding parts of the composition are subject to oxygen curing inhibition, so it is necessary to wipe off the protruding parts or wash them. Therefore, an ultraviolet curing silicone composition that solves this problem has been earnestly desired. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2017-171734 A [Patent Document 2] International Publication No. WO2018 / 003381 Summary of the Invention [Problem to be solved by the invention]

[0004] Therefore, an object of the present invention is to provide a UV-curable organopolysiloxane that is highly convenient and does not cause surface curing inhibition even when cured in the atmosphere, a composition containing the same, and a cured product thereof. [Means for solving the problem]

[0005] As a result of extensive research conducted in order to achieve the above object, the present inventors have discovered that by using a specific ultraviolet-curable organopolysiloxane component, it is possible to provide an ultraviolet-curable silicone composition that exhibits excellent surface curing properties even in the atmosphere, and have thus completed the present invention.

[0006] The present invention provides the following ultraviolet-curable organopolysiloxane, a silicone composition containing the same, and a cured product thereof. [1] Organopolysiloxane represented by the following formula (1): [ka] (In formula (1), R 1 are each independently a monovalent aliphatic hydrocarbon group having 1 to 10 carbon atoms or a group represented by the following formula (2), and each molecule has at least one group represented by the following formula (2), and m is a number satisfying 1≦m≦10,000. [ka] (In formula (2), R 2 R is a group having at least one acryloyl group, methacryloyl group, acryloyloxyalkyl group, or methacryloyloxyalkyl group. 3 is a divalent hydrocarbon group having 1 to 20 carbon atoms. [2] (A) 100 parts by mass of an organopolysiloxane represented by the following formula (1): [ka] (In formula (1), R 1are each independently a monovalent aliphatic hydrocarbon group having 1 to 10 carbon atoms or a group represented by the following formula (2), and each molecule has at least one group represented by the following formula (2), and m is a number satisfying 1≦m≦10,000. [ka] (In formula (2), R 2 R is a group having at least one acryloyl group, methacryloyl group, acryloyloxyalkyl group, or methacryloyloxyalkyl group. 3 is a divalent hydrocarbon group having 1 to 20 carbon atoms. and (B) Photopolymerization initiator: 0.1 to 20 parts by mass 1. An ultraviolet-curable silicone composition comprising: [3] The ultraviolet-curable silicone composition according to [2], further comprising either or both of (C) a monofunctional (meth)acrylate compound not containing a siloxane structure and (D) a polyfunctional (meth)acrylate compound not containing a siloxane structure, in an amount of 1 to 500 parts by mass in total of the components (C) and (D) per 100 parts by mass of the component (A). [4] Furthermore, (E)(a)R 4 3SiO 1 / 2 Units (wherein R 4 each independently represents a monovalent hydrocarbon group having 1 to 10 carbon atoms.) and (b) SiO 4 / 2 The ultraviolet-curable silicone composition according to [2] or [3], characterized in that it contains 1 to 1,000 parts by mass of an organopolysiloxane resin consisting of (a) units:(b) units in a molar ratio of 0.4 to 1.2:1 per 100 parts by mass of component (A). [5] Furthermore, (F)(c) the following formula (3) [ka] (In the formula, R 5 each independently represents a monovalent hydrocarbon group having 1 to 20 carbon atoms; R 6represents an oxygen atom or an alkylene group having 1 to 20 carbon atoms, R 7 each independently represents an acryloyloxyalkyl group, a methacryloyloxyalkyl group, an acryloyloxyalkyloxy group, or a methacryloyloxyalkyloxy group, n represents a number satisfying 0≦n≦10, and a represents a number satisfying 1≦a≦3. 4 3SiO 1 / 2 Units (wherein R 4 each independently represents a monovalent hydrocarbon group having 1 to 10 carbon atoms.) and (e) SiO 4 / 2 The ultraviolet-curable silicone composition according to any one of [2] to [4], characterized in that it contains 1 to 1,000 parts by mass of a crosslinkable organopolysiloxane resin comprising (c) units and (d) units, and in which the molar ratio of the sum of the (c) units and the (d) units to the (e) units is in the range of 0.4 to 1.2:1, per 100 parts by mass of component (A). [6] A composition for 3D printers, comprising the ultraviolet-curable silicone composition according to any one of [2] to [5]. [7] A cured product of the ultraviolet-curable silicone composition according to any one of [2] to [5]. Effect of the Invention

[0007] The organopolysiloxane of the present invention and the ultraviolet-curable silicone composition containing it are not inhibited from curing on the surface even in the atmosphere where oxygen is present.Therefore, the ultraviolet-curable silicone composition can be cured by ultraviolet irradiation without any problems even in the presence of oxygen, so the composition has excellent productivity and workability, and is particularly useful as a material for 3D printers, adhesives, pressure sensitive adhesives, and microtransfer printing materials. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The present invention will now be described in more detail.

[0009] Organopolysiloxane The organopolysiloxane of the present invention is an organopolysiloxane represented by the following formula (1). [ka]

[0010] R in the above formula (1) 1 are each independently a monovalent hydrocarbon group having 1 to 10 carbon atoms or a group represented by the following formula (2). The monovalent hydrocarbon group may be linear, branched, or cyclic, and examples thereof include alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-hexyl, cyclohexyl, n-octyl, 2-ethylhexyl, and n-decyl groups; alkenyl groups such as vinyl, allyl (2-propenyl), 1-propenyl, isopropenyl, and butenyl groups; aryl groups such as phenyl, tolyl, xylyl, and naphthyl groups; and aralkyl groups such as benzyl, phenylethyl, and phenylpropyl groups. Some or all of the hydrogen atoms bonded to carbon atoms of these monovalent hydrocarbon groups may be substituted with a substituent, specific examples of which include halogen-substituted hydrocarbon groups such as chloromethyl, bromoethyl, and trifluoropropyl groups; and cyano-substituted hydrocarbon groups such as cyanoethyl groups. Among these monovalent hydrocarbon groups, alkyl groups and aryl groups having 1 to 6 carbon atoms are preferred, with methyl groups, ethyl groups, and phenyl groups being more preferred.

[0011] In addition, R in the above formula (1) 1 At least one of the above is a group represented by the following formula (2). [ka] R in the above formula (2) 2is a group having at least one acryloyl group, methacryloyl group, acryloyloxy group or methacryloyloxy group, and among such groups, a monovalent hydrocarbon group having 1 to 20 carbon atoms in which at least one hydrogen atom is substituted with an acryloyl group, methacryloyl group, acryloyloxyalkyl group or methacryloyloxyalkyl group is preferred, and a linear or branched alkyl group having 1 to 4 carbon atoms in which at least one hydrogen atom is substituted with an acryloyl group, methacryloyl group, acryloyloxyalkyl group or methacryloyloxyalkyl group is more preferred.

[0012] R in the above formula (2) 3 is a divalent hydrocarbon group having 1 to 20 carbon atoms, which may be linear, branched, or cyclic, and specific examples thereof include alkylene groups such as methylene, ethylene, propylene, trimethylene, tetramethylene, isobutylene, pentamethylene, hexamethylene, heptamethylene, octamethylene, nonamethylene, and decamethylene. 3 As the alkyl group, methylene, ethylene and trimethylene groups are preferred, and a trimethylene group is more preferred.

[0013] m is a number that satisfies 1≦m≦10,000, and preferably 50≦m≦5,000. If m exceeds 10,000, the viscosity becomes too high, which may result in poor workability. The value of m is, for example, 29 It can be calculated as an average value by Si-NMR measurement or the like, and can also be determined from the number average molecular weight converted into polystyrene by gel permeation chromatography (GPC) analysis.

[0014] Examples of such organopolysiloxanes include compounds represented by the following formulas (4) to (9). [ka] (In formula (4), R 8are each independently a methyl group, an ethyl group, or a phenyl group, and the siloxane units in the two parentheses may be arranged in any order, either in blocks or randomly. p and q are numbers that satisfy p≧1, q≧0, and 1≦p+q≦10,000. [ka] (In formula (5), R 8 has the same meaning as above, and r is a number satisfying 1≦r≦10,000.) [ka] (In formula (6), R 8 has the same meaning as above, and s is a number satisfying 1≦s≦10,000.) [ka] (In formula (7), the siloxane units in the two parentheses may be arranged in any order, and may be arranged in blocks or randomly.) [ka] [ka]

[0015] These organopolysiloxanes can be obtained, for example, by reacting a polysiloxane having an amino group, such as side-chain amino-modified dimethyl silicone oil (KF-864 manufactured by Shin-Etsu Chemical Co., Ltd.) and both-end amino-modified dimethyl silicone oil (KF-8008 manufactured by Shin-Etsu Chemical Co., Ltd.), with a compound such as 2-(acryloyloxy)ethyl isocyanate (Karenz AOI manufactured by Showa Denko K.K.) and 1,1-(bisacryloyloxymethyl)ethyl isocyanate (Karenz BEI manufactured by Showa Denko K.K.).

[0016] UV-curable silicone composition (A) Organopolysiloxane Component (A) of the UV-curable silicone composition of the present invention is the same as the organopolysiloxane represented by formula (1) above. The composition of the present invention contains the component (A) in an amount of preferably 5 to 99.9 mass %, more preferably 20 to 99 mass %, and even more preferably 30 to 99 mass %. The viscosity of the organopolysiloxane of component (A) at 25°C is preferably 0.01 to 100,000 Pa s, and more preferably 0.1 to 50,000 Pa s, in order to further improve the workability of the composition and the mechanical properties of the cured product. The viscosity can be measured using a rotational viscometer (for example, BL type, BH type, BS type, cone-plate type, rheometer, etc.).

[0017] (B) Photopolymerization initiator Examples of the photopolymerization initiator (B) include 2,2-diethoxyacetophenone, 2,2-dimethoxy-1,2-diphenylethan-1-one (Irgacure 651 manufactured by BASF), 1-hydroxy-cyclohexyl-phenyl-ketone (Irgacure 184 manufactured by BASF), 2-hydroxy-2-methyl-1-phenyl-propan-1-one (Irgacure 1173 manufactured by BASF), 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]-phenyl}-2-methyl-propan-1-one (Irgacure 127 manufactured by BASF), phenylglyoxylic acid methyl ester (Irgacure MBF manufactured by BASF), 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one (Irgacure 133 manufactured by BASF), and the like. 907), 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-1-butanone (Irgacure 369 manufactured by BASF), bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (Irgacure 819 manufactured by BASF), 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide (Irgacure TPO manufactured by BASF), and mixtures thereof.

[0018] Of the above-mentioned (B) components, from the viewpoint of compatibility with the (A) component, 2,2-diethoxyacetophenone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one (Irgacure 1173 manufactured by BASF), bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (Irgacure 819 manufactured by BASF), and 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide (Irgacure TPO manufactured by BASF) are preferred.

[0019] The amount of the photopolymerization initiator added is within the range of 0.1 to 20 parts by mass relative to 100 parts by mass of (A). If the amount is less than 0.1 part by mass, the curability is insufficient, and if the amount is more than 20 parts by mass, the curability in deep areas is deteriorated.

[0020] In addition to the above essential components, the UV-curable silicone composition of the present invention may optionally further contain, as component (C) and component (D), either or both of a monofunctional (meth)acrylate compound and a polyfunctional (meth)acrylate compound not containing a siloxane structure.

[0021] (C) Monofunctional (meth)acrylate compound not containing a siloxane structure Examples of the monofunctional (meth)acrylate compound (C) not containing a siloxane structure include isoamyl acrylate, lauryl acrylate, stearyl acrylate, ethoxy-diethylene glycol acrylate, methoxy-triethylene glycol acrylate, 2-ethylhexyl-diglycol acrylate, phenoxyethyl acrylate, phenoxydiethylene glycol acrylate, tetrahydrofurfuryl acrylate, isobornyl acrylate, and mixtures thereof, with isobornyl acrylate being particularly preferred.

[0022] (D) Polyfunctional (meth)acrylate compound not containing a siloxane structure Examples of the polyfunctional (meth)acrylate compound (D) not containing a siloxane structure include triethylene glycol diacrylate, polytetramethylene glycol diacrylate, neopentyl glycol diacrylate, 1,6-hexanediol diacrylate, dimethylol-tricyclodecane diacrylate, trimethylolpropane triacrylate, pentaerythritol tetraacrylate, and mixtures thereof, with dimethylol-tricyclodecane diacrylate being particularly preferred.

[0023] When the (meth)acrylate compounds of the (C) and / or (D) components are used, the total amount of the (C) and (D) components is preferably in the range of 1 to 500 parts by mass, more preferably 10 to 100 parts by mass, per 100 parts by mass of the (A) component, from the viewpoint of the rubber properties of the resulting cured product. When the (C) and / or (D) components are used in combination with the highly viscous (A) component, the viscosity of the entire composition can be reduced by increasing the amount of the (C) and / or (D) components added.

[0024] Furthermore, the UV-curable silicone composition of the present invention may optionally further contain either or both of organopolysiloxane resins as component (E) and component (F).

[0025] (E) Organopolysiloxane resin Component (E) is (a)R 4 3SiO 1 / 2 Units (wherein R 4 are each independently a monovalent hydrocarbon group having 1 to 10 carbon atoms) and (b) SiO 4 / 2 The organopolysiloxane resin is composed of units, and the molar ratio of units (a) to units (b) is in the range of 0.4 to 1.2:1. R 4 Specific examples of the monovalent hydrocarbon group having 1 to 10 carbon atoms in the above-mentioned R 1Among the groups exemplified in 1 above, those having 1 to 10 carbon atoms can be mentioned, and among these, preferred are alkyl groups having 1 to 6 carbon atoms, such as methyl, ethyl, n-propyl, and n-butyl groups; aryl groups having 6 to 10 carbon atoms, such as phenyl and tolyl groups; aralkyl groups having 7 to 10 carbon atoms, such as benzyl groups; and alkenyl groups having 2 to 6 carbon atoms, such as vinyl groups, allyl groups, and butenyl groups. In addition, the above R 4 In the monovalent hydrocarbon group, some or all of the hydrogen atoms bonded to carbon atoms may be substituted with the above-mentioned substituents. In order to set the adhesive strength and mechanical properties of the composition in a more appropriate range, the component (E) is (a)R 4 3SiO 1 / 2 Units (M units) and (b) SiO 4 / 2 The molar ratio of units (Q units) is preferably M units:Q units=0.4 to 1.2:1, and more preferably M units:Q units=0.6 to 1.2:1. When an organopolysiloxane resin of component (E) is used, the amount added is preferably within a range from 1 to 1,000 parts by mass, more preferably from 10 to 800 parts by mass, and even more preferably from 20 to 500 parts by mass, per 100 parts by mass of component (A). There are no particular limitations on the number average molecular weight of component (E), but the number average molecular weight calculated using polystyrene standards as determined by gel permeation chromatography (GPC) is preferably 500 to 10,000, particularly preferably 1,000 to 8,000, and even more preferably 1,000 to 7,000.

[0026] (F) Crosslinkable organopolysiloxane resin The component (F) is (c) a unit represented by the following formula (3) (hereinafter, M A (d) R 4 3SiO 1 / 2 Units (M units) and (e) SiO 4 / 2 It is an organopolysiloxane resin having a (meth)acryloyloxy-containing group consisting of units (Q units). 4 has the same meaning as above. [ka] R in the above formula (3) 5 are each independently a monovalent hydrocarbon group having 1 to 20 carbon atoms, which may be linear, branched, or cyclic. Specific examples thereof include alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-hexyl, cyclohexyl, n-octyl, 2-ethylhexyl, and n-decyl; alkenyl groups such as vinyl, allyl (2-propenyl), 1-propenyl, isopropenyl, and butenyl; aryl groups such as phenyl, tolyl, xylyl, and naphthyl; and aralkyl groups such as benzyl, phenylethyl, and phenylpropyl.

[0027] In addition, some or all of the hydrogen atoms bonded to the carbon atoms of these monovalent hydrocarbon groups may be substituted with a substituent, specific examples of which include halogen-substituted hydrocarbon groups such as chloromethyl, bromoethyl, trifluoropropyl, and cyanoethyl groups; and cyano-substituted hydrocarbon groups.

[0028] Among these, R 5 As the alkyl group, an alkyl group having 1 to 5 carbon atoms and an aryl group are preferable, and a methyl group, an ethyl group and a phenyl group are more preferable.

[0029] R in the above formula (3) 6 represents an oxygen atom or an alkylene group having 1 to 20 carbon atoms, which may be linear, branched, or cyclic, and specific examples thereof include methylene, ethylene, propylene, trimethylene, tetramethylene, isobutylene, pentamethylene, hexamethylene, heptamethylene, octamethylene, nonamethylene, and decylene groups.

[0030] Among these, R 6 is preferably an oxygen atom, a methylene, an ethylene or a trimethylene group, and more preferably an oxygen atom or an ethylene group.

[0031] R in the above formula (3) 7are each independently an acryloyloxyalkyl group, a methacryloyloxyalkyl group, an acryloyloxyalkyloxy group, or a methacryloyloxyalkyloxy group, and the number of carbon atoms in the alkyl (alkylene) group in these groups is not particularly limited, but is preferably 1 to 10, and more preferably 1 to 5. Specific examples of these alkyl groups include the above-mentioned R 1 Among the groups exemplified above, those having 1 to 10 carbon atoms are included.

[0032] In the above formula (3), n is a number that satisfies 0≦n≦10, but is preferably 0 or 1, and a is a number that satisfies 1≦a≦3, but is preferably 1 or 2.

[0033] In consideration of the viscosity of the composition and the mechanical properties of the cured product, the component (F) is preferably a unit represented by the above formula (3) (M A units), (d) R 4 3SiO 1 / 2 Units (M units) and (e) SiO 4 / 2 The molar ratio of units (Q units) is (M A It is preferable that (M unit + M unit):Q unit = 0.4 to 1.2:1, A It is more preferable that the ratio of M unit+Q unit) is 0.6-1.2:1. Also, M A The rubber properties of the cured product can be adjusted by the molar ratio of M units to M units. A Unit: M unit = 0.01 to 1:1 is preferred, M A It is more preferable that the unit:M unit=0.05 to 0.5:1.

[0034] When using a crosslinkable organopolysiloxane resin as component (F), the amount added is preferably within a range from 1 to 1,000 parts by mass, more preferably from 10 to 800 parts by mass, and even more preferably from 20 to 500 parts by mass, per 100 parts by mass of (A). There are no particular limitations on the number average molecular weight of component (F), but the number average molecular weight calculated using polystyrene standards as determined by gel permeation chromatography (GPC) is preferably 1,000 to 10,000, particularly preferably 2,000 to 8,000, and even more preferably 2,500 to 7,000.

[0035] Other Ingredients The composition of the present invention may contain additives such as coloring materials (pigments or dyes), silane coupling agents, adhesion aids, polymerization inhibitors, antioxidants, ultraviolet absorbers which are light resistance stabilizers, and light stabilizers, within the scope of not impairing the effects of the present invention. The composition of the present invention can also be used by appropriately mixing it with other resin compositions.

[0036] Manufacturing method The ultraviolet-curable silicone composition of the present invention can be obtained by mixing the above-mentioned components (A) and (B), and, if necessary, the components (C) to (F) and other components, in any order, followed by stirring, etc. There are no particular limitations on the equipment used for operations such as stirring, but examples of equipment that can be used include a crusher, a three-roll mill, a ball mill, a planetary mixer, etc. These equipment can also be used in combination as appropriate.

[0037] From the standpoint of shape retention and workability during application, the viscosity of the UV-curable silicone composition of the present invention, as measured at 25°C using a rotational viscometer, is preferably no more than 5,000 Pa s, more preferably no more than 3,000 Pa s, and even more preferably no more than 1,500 Pa s.

[0038] A cured product of the ultraviolet-curable silicone composition of the present invention can be rapidly obtained by irradiating it with ultraviolet light. In this case, examples of the light source of the ultraviolet light to be irradiated to the composition of the present invention include UV LED lamps, high pressure mercury lamps, ultra-high pressure mercury lamps, metal halide lamps, carbon arc lamps, xenon lamps, and the like. The amount of ultraviolet light (accumulated light amount) is preferably 1 to 10,000 mJ / cm for a sheet formed from the composition of the present invention to a thickness of about 2.0 mm. 2 and more preferably 10 to 8,000 mJ / cm 2 That is, the illuminance is 100mW / cm 2 When ultraviolet light is used, irradiation with ultraviolet light may be performed for about 0.01 to 100 seconds.

[0039] Furthermore, in order for the cured product of the UV-curable silicone composition of the present invention to exhibit excellent rubber physical properties, the hardness after curing is preferably 20 or more (Type A), and more preferably 30 or more (Type A). These values ​​are measured according to JIS K 6249:2003. The hardness after curing can be adjusted by increasing or decreasing the amounts of components (C) and (D) added. EXAMPLES

[0040] EXAMPLES The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0041] [Example 1] 1,000 g of side-chain amino-modified dimethyl silicone oil (KF-864, manufactured by Shin-Etsu Chemical Co., Ltd.) and 41.3 g of 2-(acryloyloxy)ethyl isocyanate (Karenz AOI, manufactured by Showa Denko K.K.) were weighed into a flask and stirred at 25°C for 24 hours to obtain organopolysiloxane (A-1) with a viscosity of 46.3 Pa s and represented by the average structural formula below. [ka] (In formula (A-1), the arrangement of the siloxane units in the two parentheses is block or random.)

[0042] [Example 2] 1,000 g of dimethyl silicone oil modified with amino at both ends (KF-8008 manufactured by Shin-Etsu Chemical Co., Ltd.) and 49.4 g of 1,1-(bisacryloyloxymethyl)ethyl isocyanate (Karenzu BEI manufactured by Showa Denko K.K.) were weighed into a flask and stirred at 25°C for 24 hours to obtain organopolysiloxane (A-2) with a viscosity of 13.0 Pa s and represented by the average structural formula below. [ka]

[0043] [Example 3] 1,000 g of dimethyl silicone oil modified with amino at both ends (KF-8008 manufactured by Shin-Etsu Chemical Co., Ltd.) and 29.1 g of 2-(acryloyloxy)ethyl isocyanate (Karenz AOI manufactured by Showa Denko K.K.) were weighed into a flask and stirred at 25°C for 24 hours to obtain organopolysiloxane (A-3) with a viscosity of 7.8 Pa s and represented by the average structural formula below. [ka]

[0044] [Examples 4 to 10 and Comparative Examples 1 and 2] Evaluations were carried out on silicone compositions prepared according to the formulations shown in Table 1. In the following examples, the viscosity values ​​were measured at 25°C using a rotational viscometer.

[0045] The hardness of the cured product was measured in accordance with JIS K 6249: 2003. Surface curability was evaluated by touching with the fingers. Those without an uncured layer were rated as "completely cured" and those with an uncured layer were rated as "incompletely cured."

[0046] The above components (A) to (F) were mixed in the compositions (parts by mass) shown in Table 1, and the toluene was distilled off at 100° C. under reduced pressure to prepare each of the silicone compositions shown in Table 1.

[0047] Each silicone composition thus prepared was irradiated with ultraviolet light having a wavelength of 365 nm at a dose of 4,000 mJ / cm in air at room temperature (25°C) using an Eye UV electronic control device (model UBX0601-01) manufactured by Eye Graphics Co., Ltd. 2 The resin was irradiated with ultraviolet light so as to cure.

[0048] The compounds of the respective components used in Examples 4 to 10 and Comparative Examples 1 and 2 are as follows.

[0049] Component (A) (A-1) Organopolysiloxane obtained in Example 1 (A-2) Organopolysiloxane obtained in Example 2 (A-3) Organopolysiloxane obtained in Example 3 (A-4) (For comparison) Organopolysiloxane (viscosity 3.4 Pa s) represented by the following average structural formula [ka] (In formula (A-4), the arrangement of the siloxane units in the two parentheses is block or random.) (A-5) (For comparison) Organopolysiloxane (viscosity 0.2 Pa s) represented by the following average structural formula [ka]

[0050] (B) Component (B-1) 2-Hydroxy-2-methyl-1-phenyl-propan-1-one (Irgacure 1173 manufactured by BASF) (B-2) 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide (Irgacure TPO manufactured by BASF)

[0051] (C) Component (C-1) Isobornyl acrylate (Light Acrylate IB-XA, manufactured by Kyoeisha Chemical Co., Ltd.)

[0052] (D) Component (D-1) Dimethylol-tricyclodecane diacrylate (Light Acrylate DCP-A, manufactured by Kyoeisha Chemical Co., Ltd.)

[0053] (E) Component (E-1)Me3SiO 1 / 2 Units and SiO 4 / 2 It contains units, (MeSiO 1 / 2 Unit) / (SiO 4 / 2 A 60% by mass toluene solution of an organopolysiloxane resin (number average molecular weight 3,500) with a molar ratio of 0.85

[0054] Ingredient (F) (F-1) A methacryloyloxy group-containing unit represented by the following formula: ViMe2SiO 1 / 2 Units, Me3SiO 1 / 2 Units and SiO 4 / 2 units, and 1 / 2 Unit) / (Me3SiO 1 / 2 Unit) / (SiO 4 / 2 A 50% by mass xylene solution of organopolysiloxane resin (number average molecular weight 5,700) with a molar ratio of 0.07 / 0.10 / 0.67 / 1.00. [ka]

[0055] [Table 1]

[0056] The ultraviolet-curable silicone compositions of the present invention (Examples 4 to 10) have good surface curability even when cured in the atmosphere, and are useful as silicone materials for modeling applications such as 3D printers, etc. On the other hand, the surface curability of Comparative Examples 1 and 2 was insufficient.

Claims

1. (A) 100 parts by mass of an organopolysiloxane represented by the following formula (4): 【Chemistry 1】 (In formula (4), R 8 is independently a methyl group, an ethyl group, or a phenyl group, and the siloxane units in the two parentheses may be arranged in any order, either in blocks or randomly. p and q are numbers satisfying p≧1, q≧0, and 1≦p+q≦10,000.) and (B) Photopolymerization initiator: 0.1 to 20 parts by mass and wherein the content of component (A) in the composition is 30 to 99 mass %.

2. The ultraviolet-curable silicone composition according to claim 1, further comprising either one or both of (C) a monofunctional (meth)acrylate compound not containing a siloxane structure and (D) a polyfunctional (meth)acrylate compound not containing a siloxane structure, in an amount of 1 to 500 parts by mass in total of components (C) and (D) per 100 parts by mass of component (A).

3. Furthermore, (E)(a)R 4 3 SiO 1 / 2 Units (wherein R 4 each independently represents a monovalent hydrocarbon group having 1 to 10 carbon atoms; and (b) SiO 4 / 2 3. The ultraviolet-curable silicone composition according to claim 1, characterized in that it contains 1 to 1,000 parts by mass of an organopolysiloxane resin consisting of (a) units:(b) units in a molar ratio of (a) units:(b) units in the range of 0.4 to 1.2:1 per 100 parts by mass of component (A).

4. Furthermore, (F) (c) the following formula (3) 【Chemistry 2】 (In the formula, R 5 each independently represents a monovalent hydrocarbon group having 1 to 20 carbon atoms; R 6 represents an oxygen atom or an alkylene group having 1 to 20 carbon atoms; R 7 each independently represents an acryloyloxyalkyl group, a methacryloyloxyalkyl group, an acryloyloxyalkyloxy group, or a methacryloyloxyalkyloxy group, n represents a number satisfying 0≦n≦10, and a represents a number satisfying 1≦a≦3. 4 3 SiO 1 / 2 Units (wherein R 4 each independently represents a monovalent hydrocarbon group having 1 to 10 carbon atoms; and (e) SiO 4 / 2 4. The ultraviolet-curable silicone composition according to claim 1, wherein the composition contains 1 to 1,000 parts by mass of a crosslinkable organopolysiloxane resin consisting of (c) units and (d) units, and the molar ratio of the sum of the (c) units and the (d) units to the (e) units is in the range of 0.4 to 1.2:1, per 100 parts by mass of component (A).

5. A composition for 3D printers, comprising the ultraviolet-curable silicone composition according to any one of claims 1 to 4.

6. A cured product of the ultraviolet-curable silicone composition according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Bi-component addition type silicon rubber and preparation method thereof

    CN108752936A

  • Radiation Curable Acrylate / Silicone Permanent Removable Pressure Sensitive Adhesives

    JP1996507563A

  • Photocurable silicone composition for hardly adherable material

    JP2002302664A

  • Photocurable organopolysiloxane composition

    JP2008031307A

  • Colored curable composition, color filter, and solid-state image pickup device

    JP2009288703A