Fibre material impregnated with a thermoplastic polymer having a thickness of less than 100 μm and method for producing same

A method using thermoplastic polymers and controlled fiber content in a fluidized bed process addresses the challenges of uniform impregnation, producing high-quality, lightweight composite materials with improved mechanical and thermal properties for diverse industrial applications.

JP7591927B2Active Publication Date: 2024-11-29ARKEMA FRANCE SA
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2020550677
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-03-23
Filing Date
2019-03-19
Publication Date
2024-11-29
Estimated Expiration
2039-03-19

AI Technical Summary

Technical Problem

Current methods for impregnating fibrous materials with thermoplastic polymers face challenges in achieving uniform and reproducible impregnation, particularly for high fiber content materials, leading to issues such as porosity, non-uniform thickness, and mechanical weakness, which affect the quality and production efficiency of composite materials.

Method used

A method involving the use of non-reactive or reactive thermoplastic polymers with controlled fiber content and thickness, combined with a fluidized bed impregnation and heating processes, ensures uniform impregnation and reduced porosity, resulting in a single-layer fiber material with a thickness of less than 100 μm, suitable for high production rates.

Benefits of technology

The method achieves a uniformly impregnated fiber material with high fiber content, reduced porosity, and improved mechanical properties, enabling the production of lightweight composite materials with enhanced mechanical and thermal properties, suitable for various industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591927000003
    Figure 0007591927000003
  • Figure 0007591927000004
    Figure 0007591927000004
  • Figure 0007591927000005
    Figure 0007591927000005
Patent Text Reader

Abstract

The present invention relates to an impregnated fibrous material comprising at least one fibrous material consisting of continuous fibers and at least one non-reactive thermoplastic polymer matrix or at least one reactive thermoplastic prepolymer, which is a precursor of said non-reactive thermoplastic polymer, optionally mixed with a chain extender, wherein the at least one non-reactive thermoplastic polymer or reactive prepolymer is an amorphous polymer or prepolymer having a glass transition temperature Tg≧80°C, in particular Tg≧100°C, in particular Tg≧120°C, in particular Tg≧140°C, or a semi-crystalline polymer or prepolymer having a melting temperature Tf≧150°C, wherein the fiber content in the pre-impregnated fibrous material is between 45 and 65% by volume, preferably between 50 and 60% by volume, in particular between 54 and 60%, and wherein the average thickness of the impregnated fibrous material is 100 μm or less, regardless of the number of fibers present in the fibrous material before impregnation. [Selection diagram] None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a fibrous material, in particular a monolayer material, impregnated with a thermoplastic polymer and having an average thickness of less than 100 μm.

[0002] More particularly, the present invention relates to a fibrous material, in particular a monolayer material, impregnated with a thermoplastic polymer, in which the fiber count of the carbon fibers is greater than or equal to 12K or the basis weight of the glass fibers is greater than or equal to 1,200 Tex, and in which the fiber content by volume of said monolayer material is particularly constant, in particular the fiber content by volume is constant and is at least 70% of the volume of the impregnated fibrous material.

[0003] The invention also relates to a method for preparing a single-ply fibre material, in particular with an average thickness of less than 100 μm, and to its use for producing composite parts, in particular by automated robotic placement or by filament winding methods.

[0004] In this disclosure, "fibrous material" refers to an assembly of individual reinforcing fibers, which, after being impregnated with resin, are provided in the form of a tape.

[0005] The term "tape" refers to a semi-finished strip of small thickness, not calibrated in width and thickness, consisting of a single roving of fiber or a thin tape consisting of one or more fiber rovings of calibrated thickness and width.

[0006] In all cases the thickness of the tape is less than 100 μm, preferably between 10 and 100 μm.

[0007] Such impregnated fiber materials have a three-dimensional structure and are particularly suitable for producing lightweight composite materials for manufacturing machine parts with good mechanical and thermal properties. If the fibers are made of carbon and / or the resin is filled with suitable additives, these fiber materials are capable of discharging electrostatic charges. By using flame-retardant resins or flame-retardant additives in non-flame-retardant resins, the impregnated fiber materials can be resistant to fire. They therefore have properties that are particularly compatible with the production of parts in the fields of machinery, aircraft, ships, automobiles, oil and gas, especially offshore, gas storage, energy, health and medicine, sports and recreation, and electronics.

[0008] Such impregnated fibrous materials are also called composite materials. They include fibrous materials composed of reinforcing fibers and a matrix composed of a polymer that impregnates the fibers. The primary role of this matrix is ​​to maintain the reinforcing fibers in a compact form and to give the desired shape to the final product. This matrix also ensures charge transfer between the fibers and therefore arranges the mechanical strength of the composite. Such a matrix also serves to protect the reinforcing fibers from friction and aggressive environments, to control the appearance of the surface, and to dissipate any charge between the fibers. The role of this matrix is ​​important for the long-term retention of the composite material, especially with regard to fatigue and creep. [Background technology]

[0009] Good quality three-dimensional composite parts produced from impregnated fibrous materials are generally subject to control of the method of impregnation of the reinforcing fibers with the thermoplastic polymer and thus the resulting impregnated fibrous material.

[0010] At present, the manufacture of tapes of fibrous material reinforced by impregnation with thermoplastic or thermosetting polymers is carried out using several methods, depending in particular on the nature of the polymers, the desired type of final composite material and its field of application, some of these methods consisting of an impregnation step, followed by a step of hot rolling or drying of the impregnated fibrous material, optionally followed by a step of melting the thermoplastic polymer.

[0011] Thus, wet impregnation techniques, or techniques using liquid precursors or precursors with very low viscosity and in situ polymerization, are often used to impregnate reinforcing fibers with thermosetting polymers, such as epoxy resins, as described, for example, in patent WO 2012 / 066241 (A2). These techniques are generally not directly applicable to impregnating thermoplastic polymers, since they rarely use liquid precursors.

[0012] The method of impregnation by crosshead die extrusion of molten polymer is only suitable for the use of low viscosity thermoplastic polymers, as thermoplastic polymers, especially those with high glass transition temperatures, have high viscosities in the molten state and therefore cannot be satisfactorily impregnated with fibers and made into good quality semi-finished or finished products.

[0013] Application US2014 / 0005331(A1) describes a method for preparing fibers impregnated with a polymer resin, the resulting tape being asymmetric, i.e. one side is rich in polymer and the opposite side is rich in fibers.

[0014] This method is carried out by molten route using equipment that only allows primary impregnation on one of its faces.

[0015] Another known method of impregnation is the continuous flow of the fibers through an aqueous polymer powder dispersion or an aqueous polymer particle dispersion or an aqueous polymer emulsion or suspension. Reference can be made, for example, to document EP 0324680. In this method, a dispersion of micrometer-sized powder is used (about 20 μm). After quenching in an aqueous solution, the fibers are impregnated with the polymer powder. The method then includes a drying step consisting of passing the impregnated fibers through a first oven in order to evaporate the water absorbed during quenching. A heat treatment step consisting of passing the impregnated and dried fibers through a second heating zone at high temperature must then melt the polymer so that it adheres to the fibers and is distributed and coats them.

[0016] The drying step of the process creates pores in the impregnated fibers due to evaporation of the water, and the resulting material is a fiber material that is coated with polymer and is therefore a multi-layer material.

[0017] The documents EP 0,406,067, jointly filed in the name of Atochem and the French Republic, and EP 0,201,367, describe a technique for impregnating polymer powders in a fluidized bed. The fibers pass through a closed fluidizing vessel, and in this case, for EP 0,406,067, they are optionally separated from one another using ridged rollers or cylinders, which acquire a static charge due to friction from these rollers or cylinders. This static charge allows the polymer powder to adhere to the surface of the fibers and thus to impregnate them.

[0018] Thus, as stated above, the resulting material is a fibrous material coated with a polymer and is therefore a multi-layer material.

[0019] International application WO2016 / 062896 describes the comminution of rovings by electrostatic methods using deliberate electric charges and the pulverization of the rovings by application of a potential difference between the tip of a spray gun or atomizing nozzle and the roving.

[0020] International application WO2015 / 121583 describes a method for producing an impregnated fibrous material, which comprises impregnating the material in a fluidized bed and then hot rolling the rovings, which allows shaping of the rovings parallel to the material.

[0021] Hot rolling, carried out downstream of the impregnation unit, makes it possible to homogenize the distribution of the polymer and to impregnate the fibers, but it is not possible to obtain a uniformly impregnated ribbon. The porosity obtained is not quantified.

[0022] The quality of the impregnated fibrous material ribbons, and therefore of the final composite material, depends not only on the uniformity and impregnation of the fibers and therefore on the control and reproducibility of the pores of the impregnated fibrous material and its monolayer appearance, but also on the dimensions, more specifically the width and thickness of the final ribbon. In fact, uniformity and control of these dimensional parameters improves the mechanical strength of the resulting composite material (from the ribbons).

[0023] The fibers that can be used in the composition of the fibrous material can have different linear basis weights or yardages or thread counts or "tex" and / or different numbers in the roving. Similarly, the most commonly used rovings are composed of 600 to 4,800 tex for glass fibers, and 3,000 (3K), 6,000 (6K), 12,000 (12K), 24,000 (24K), 48,000 (48K), 50,000 (50K) or 400,000 (400K) for carbon fibers. For example, carbon fibers generally have a diameter of approximately 7 to 8 μm, and glass fibers have a diameter of about 13, 15, 17 or 20 μm.

[0024] The most common practice of manufacturing webs is based on the assembly of rovings and resins to form a volume of composite material. This volume is however larger than the volume of the web to be produced. This volume is implemented by calendering in the form of a web with a calibrated thickness, with the desired thickness, but generally with wider and irregular edges than the final web. This web is then cut (slitting operation) to obtain the final web, also called calibrated web, with the desired width.

[0025] If it is desired to eliminate the cutting operation (slitting operation) in order to avoid material cracks, damage to the fibers or the cost of additional steps in the manufacture of the web, the step of manufacturing the web is eliminated and an assembly of rovings and resin is produced whose volume corresponds exactly to the final volume of the calibrated web to be manufactured. A major consequence of such a method is that the volume of the material will depend directly on the linear basis weight of the fibers and on the fiber content. For this reason, if the fiber content is fixed, only a discrete number of volumes of material can be produced, which are a function of the basis weight of the commercially available rovings.

[0026] In other words, the calibrated web produced without slits can have any width or thickness, only the fiber basis weight of the calibrated web can be equal to an integer multiple of the basis weight of the original roving.

[0027] Considering the demand from manufacturers, for example a demand for a 194 g / m2 composite of carbon fibre with 34 wt% resin of density 1.29, the calibrated web will typically have a thickness of about 190 μm and a width of about 300 mm, necessitating the use of 72 rovings that are 12K.

[0028] In the usual way, a web is produced by assembling dry fiber rovings, which are then impregnated with resin and the web obtained is then notched (by incision). Nevertheless, if it is desired to produce this web at high production speeds, the impregnation of a web of this thickness does not take place correctly in the core of the roving and it is not possible to obtain a uniform impregnation of the roving.

[0029] Current techniques for impregnating fibrous materials and forming such impregnated fibrous materials in the form of calibrated webs also have other drawbacks.

[0030] Since the length of the web is generally limited to a percentage of the length of a reel of dry fiber roving, slitting the web to obtain tapes involves splicing these tapes due to their weight and the handling problems this causes, resulting in additional manufacturing costs for the tapes and manufacturing defects in the final composite parts that may initiate premature failure of the tapes.

[0031] In addition to the above mentioned drawbacks, the incision of the web causes serious problems of cut fibers and exposed fibrils, which can cause dust and electrical arcs during robot placement, resulting in robot failure and / or composite defects. This potentially causes robot repair costs, production stoppages and scrapping of non-compliant products. Finally, during the incision process, a non-negligible amount of fibers is damaged, causing loss of properties, especially the mechanical strength and electrical conductivity of tapes of impregnated fibrous materials.

[0032] It is therefore necessary to have available unslit and unspliced ​​fibrous material (e.g. having approximately the length of the initial dry fibrous roving), which is sufficiently impregnated even during production at high production rates, in particular tapes in the form of strips of various widths and thicknesses, or thin tapes with calibrated widths and thicknesses, the average thickness of the strips or thin tapes being less than or equal to 100 μm, so as to ensure uniform core impregnation of the fibrous roving, regardless of the number of filaments present in the roving of the initial fibrous material before impregnation, even during production at high production rates.

[0033] It is therefore an object of the present invention to remedy at least one of the drawbacks from the prior art, in particular to produce an impregnated fibre material as defined above. Summary of the Invention

[0034] The present invention aims in particular to provide a monolayer impregnated fibrous material, the fiber number of which, in the case of carbon fibers, is in particular 12K or more, or in the case of glass fibers, the basis weight of which is 1,200 Tex or more, in particular 2,400 Tex or more, 4,800 Tex or more, and the fiber content by volume is in particular constant for at least 70% of the volume of the impregnated fibrous material, in which the impregnation of the fibers on which the performance of the final composite part depends is uniform, said material having controlled dimensions with reduced, controlled and reproducible porosity and with a uniform distribution of the fibers of said fibrous material in the impregnated fibrous material. [Brief description of the drawings]

[0035] [Figure 1] 1 shows an example of a vessel provided with a support. [Diagram 2] 1 shows an example of a vessel with a fluidized bed, where the support is a cylindrical compression roller. [Diagram 3] An embodiment is shown using a single compression roller, a vessel (30) equipped with a spray gun (31) for spraying powder (32), where a single cylindrical compression roller (33) is present and exhibits an angle α″1. [Figure 4] A schematic showing a single heating system for heating the pre-impregnated fibrous material and the use of three rollers to terminate the impregnation is shown. [Diagram 5] FIG. 1 shows a photograph of a cross-section of a SGL, 50K carbon fiber roving impregnated with PA BACT / 10T polyamide powder with D50=108 μm (D90=198 μm and D10=48.3 μm) according to Example 1 and as disclosed in WO2015 / 121583 (before calendering) taken with a scanning electron microscope. [Figure 6] FIG. 1 shows a photograph taken using a scanning electron microscope of the cross-section of a SGL, 50K carbon fiber roving impregnated with PA BACT / 10T polyamide powder (41 / 59 molar ratio) with D50=108 μm (D90=198 μm and D10=48.3 μm) according to Example 2 of the present invention (before calendering). [Figure 7] An embodiment of the process of forming and calibrating a 12.7 mm strip (obtained in FIG. 6 ) is shown, using a first notched support (diameter 13 mm, groove 12.7 mm), two non-notched supports (diameter 20 mm) and a notched support (diameter 13 mm, groove 12.7 mm) outside the infrared (IR) system, a final IR heating system and a heated calendaring machine mounted in series to obtain a 12.7 mm thin-layer tape, each of which is equipped with a 1 kW IR system, and is placed after the heated calendaring machine. [Figure 8] FIG. 1 shows a photograph taken with an optical microscope of a cross-section of a T700 12k 31E carbon fiber roving impregnated with PA11 / BACT polyamide powder (33 / 67) with D50=114 μm (D90=199 μm and D10=56 μm) according to Example 5 of the present invention (before calendaring). [Figure 9] FIG. 1 shows a photograph taken with an optical microscope of a cross-section of a T700 12k 31E carbon fiber roving impregnated with PA6I / 6T polyamide powder (45 / 55 molar ratio) with D50=136 μm (D90=225 μm and D10=75 μm) according to Example 6 of the present invention (before calendering). [Figure 10]FIG. 1 shows a photograph taken with an optical microscope of a cross-section of a T700 12k 31E carbon fiber roving impregnated with PA MPMDT / 10T polyamide powder (41 / 59 molar ratio) with D50=157 μm (D90=301 μm and D10=58 μm) according to Example 7 of the present invention (before calendering). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0036] To this end, the object of the present invention is to provide at least one fibre material consisting of continuous fibres, and at least one non-reactive thermoplastic polymer matrix, or at least one reactive thermoplastic prepolymer, i.e. a precursor of said non-reactive thermoplastic polymer, optionally mixed with a chain extender; An impregnated textile material comprising: the at least one non-reactive thermoplastic polymer or the reactive prepolymer is an amorphous polymer or prepolymer having a glass transition temperature Tg≧80° C., in particular Tg≧100° C., in particular ≧120° C., in particular ≧140° C., or a semi-crystalline polymer or prepolymer having a melting temperature Tm≧150° C., the fiber content in the impregnated fibrous material is between 45 and 65% by volume, preferably between 50 and 60% by volume, in particular between 54 and 60%, and the average thickness of the impregnated fibrous material is less than or equal to 100 μm, regardless of the number of fibers present in the fibrous material before impregnation, It is an impregnated fiber material.

[0037] Advantageously, PA6 is excluded from the definition of thermoplastic polymer or thermoplastic prepolymer.

[0038] Advantageously, the average thickness of said impregnated fibrous material is between 10 μm and 100 μm.

[0039] The measurement of the average thickness and width of the impregnated fibrous material can be carried out by laser measurement as described in WO2016 / 062896.

[0040] In this disclosure, the term "strip" is used to describe an impregnated fibrous material of uncalibrated width and thickness having an average thickness of 100 μm or less.

[0041] Throughout this disclosure, the width of a strip corresponds to the average width and the thickness of a strip corresponds to the average thickness, i.e. the average width and thickness over the entire length of the strip. This means that the width and thickness may vary along the strip, but the thickness is, on average, less than or equal to 100 μm. A way to ensure that the average thickness is less than 100 μm over the entire length of the strip is to carry out measurements on a statistically representative sample of the strip by non-destructive measurement means.

[0042] The expression "uncalibrated width" means that the width of the strip is not constant, but that its width is possibly equal to l+ / -20%, in particular l+ / -15%, in particular l+ / -10%, where l represents the average width.

[0043] The expression "uncalibrated thickness" means that the thickness of the strip is not constant over its entire length and that the thickness can be equal to e+ / -20%, in particular e+ / -15%, in particular e+ / -10%, where e represents the average thickness.

[0044] Advantageously, the expressions "uncalibrated width" and "uncalibrated thickness" mean, respectively, that the width is equal to l+ / -20% of the average width and that the thickness is equal to e+ / -20% of the average thickness.

[0045] Advantageously, the expressions "uncalibrated width" and "uncalibrated thickness" mean, respectively, that the width is equal to l+ / -20% of the average width and that the thickness is equal to e+ / -15% of the average thickness.

[0046] Advantageously, the expressions "uncalibrated width" and "uncalibrated thickness" mean, respectively, that the width is equal to l+ / -20% of the average width and that the thickness is equal to e+ / -10% of the average thickness.

[0047] Advantageously, the expressions "uncalibrated width" and "uncalibrated thickness" mean, respectively, that the width is equal to l+ / -15% of the average width and that the thickness is equal to e+ / -20% of the average thickness.

[0048] Advantageously, the expressions "uncalibrated width" and "uncalibrated thickness" mean, respectively, that the width is equal to l+ / -10% of the average width and that the thickness is equal to e+ / -20% of the average thickness.

[0049] Advantageously, the expressions "uncalibrated width" and "uncalibrated thickness" mean, respectively, that the width is equal to l+ / -15% of the average width and that the thickness is equal to e+ / -15% of the average thickness.

[0050] Advantageously, the expressions "uncalibrated width" and "uncalibrated thickness" mean, respectively, that the width is equal to l+ / -10% of the average width and that the thickness is equal to e+ / -15% of the average thickness.

[0051] Advantageously, the expressions "uncalibrated width" and "uncalibrated thickness" mean, respectively, that the width is equal to l+ / -15% of the average width and that the thickness is equal to e+ / -10% of the average thickness.

[0052] Advantageously, the expressions "uncalibrated width" and "uncalibrated thickness" mean, respectively, that the width is equal to l+ / -10% of the average width and that the thickness is equal to e+ / -10% of the average thickness.

[0053] Nevertheless, the average width of the strip depends on the number of fibers present in the roving.

[0054] The term "thin tape" is used to describe an impregnated fibrous material of calibrated width and thickness having an average thickness of 100 μm or less.

[0055] Throughout this disclosure, the width of the thin tape corresponds to the average width and the thickness of the thin tape corresponds to the average thickness, i.e. the average width and thickness over the entire length of the thin tape. This means that the width and thickness can vary along the thin tape, but the thickness is, on average, less than or equal to 100 μm. A way to ensure that the average thickness is less than 100 μm over the entire length of the strip is to carry out measurements on a statistically representative sample of the thin tape by non-destructive measuring means. The expression "calibrated width" means that the width of the thin tape is constant over its entire length, and the width can be l+ / -5%, in particular l+ / -2%, where l stands for the average width.

[0056] The expression "calibrated thickness" means that the average thickness of the thin tape is constant over its entire length, the thickness may be equal to e+ / -5%, in particular the thickness is equal to e+ / -2%, where e represents the average thickness.

[0057] Advantageously, the expressions "calibrated width" and "calibrated thickness" mean, respectively, that the width is equal to l+ / -5% of the average width and that the thickness is equal to e+ / -5% of the average thickness.

[0058] Advantageously, the expressions "calibrated width" and "calibrated thickness" mean, respectively, that the width is equal to l+ / -5% and the thickness is equal to e+ / -2% of the average width.

[0059] Advantageously, the expressions "calibrated width" and "calibrated thickness" mean, respectively, that the width is equal to l+ / -2% of the average width and that the thickness is equal to e+ / -5% of the average thickness.

[0060] Advantageously, the expressions "calibrated width" and "calibrated thickness" mean, respectively, that the width is equal to l+ / -2% of the average width and that the thickness is equal to e+ / -2% of the average thickness.

[0061] Nevertheless, the average width of the laminate tape depends on the number of fibers present in the roving.

[0062] Advantageously, the number of fibres in said fibre material is, in the case of carbon fibres, 3K or more, in particular 6K or more, in particular 12K or more.

[0063] Advantageously, the number of fibers in the fibrous material is, in the case of carbon fibers, 12K or more, in particular selected from 12K, 24K, 48K, 50K and 400K, in particular 12K, 24K, 48K and 50K, or, in the case of glass fibers, the basis weight is 1,200Tex or more, in particular 2,400Tex or more, 4,800Tex or more.

[0064] Tex means that 1000m of basic yarn weighs 1g.

[0065] Thus, the inventors have found that whatever the starting roving, i.e. in the case of high fiber contents above 45% by volume, and whatever the number of filaments or fibers in the starting roving, impregnation is carried out correctly at high production rates only if the strip or thin tape has an average thickness of 100 μm or less.

[0066] It is quite clear that if the average thickness and the desired average width are fixed (assuming negligible levels of porosity), it is possible to determine the required number of fibers present in the roving.

[0067] For example, for an average width of 50 mm with a carbon fiber content of 50% by volume and an average thickness of 100 μm (thin layer tape, e.g. polyamide), it would be necessary to use a 50K roving.

[0068] For an average width of 50 mm with a carbon fiber content of 62% by volume and an average thickness of 60 μm (thin tape, e.g. polyamide), it would be necessary to use a 48K roving.

[0069] Thus, the rovings used will be single rovings as opposed to multiple rovings, which in turn correspond to the joining of tapes or thin webs produced from each of the rovings that make up the multiple roving.

[0070] Advantageously, in the absence of reheating, the impregnated fibrous material is inflexible.

[0071] This means that the impregnated fibrous material cannot assume a complex shape at room temperature, and the impregnated fibrous material can assume a complex shape only above the Tm of the resin. In other words, the impregnated fibrous material does not have drapeability.

[0072] The fibers of the fibrous material may be sized or unsized.

[0073] "Sizing" refers to the surface treatment applied to the reinforcing fibers (fabric sizing) and fabrics (plastic sizing) exiting the nozzle.

[0074] The "weave" sizing applied to the filaments leaving the nozzle consists of the deposition of a binder that ensures the cohesion of the filaments relative to one another, reduces friction and facilitates subsequent handling (weaving), and prevents the formation of static charges. Sizing may be carried out on the surface of the fibers, for example by depositing an epoxy resin in solution on the carbon fibers.

[0075] Advantageously, the fibres of the fibre material are unsized fibres.

[0076] The term "unsized" means either that the fibers are not initially sized and therefore do not undergo any surface treatment, or that the fibers are resized prior to use.

[0077] Advantageously, the fiber content by volume is constant for at least 70% of the volume of the impregnated fibrous material, in particular for at least 80% of the volume of the impregnated fibrous material, in particular for at least 90% of the volume of the impregnated fibrous material, and especially for at least 95% of the volume of the impregnated fibrous material.

[0078] Advantageously, the distribution of the fibres is uniform over at least 95% of the volume of the impregnated fibrous material.

[0079] Fiber fraction by volume is measured locally with respect to the representative element volume (REV).

[0080] The term "constant" means that the fiber content by volume is constant within some measurement uncertainty, which is plus or minus 1%.

[0081] The expression "homogeneous" means that the impregnation is uniform and that there are no dry fibers, i.e. non-impregnated fibers, and conversely, no areas of pure resin without fibers over at least 95% of the volume of the tape of impregnated fibrous material.

[0082] Advantageously, the porosity level in said impregnated fibrous material is less than 10%, in particular less than 5%, in particular less than 2%.

[0083] Advantageously, said impregnated fibrous material is a single layer material.

[0084] The term "monolayer" means that the impregnation is carried out particularly uniformly on the core, in particular with at least one diffusion during impregnation, so that once the fibre material is impregnated, said fibre material and the polymer cannot be separated from each other and form a material composed of a single fibre and polymer based layer.

[0085] The various properties of thickness, fiber count, fiber content, sizing, fiber distribution and monolayer characteristics can be combined with those of the subject of the present invention and each with one or more others, and can be the subject of as many embodiments as possible of possible combinations forming an integral part of the present invention.

[0086] Polymer Matrix Thermoplastic resin or thermoplastic polymer refers to a material that is generally solid at room temperature, which may be semi-crystalline or amorphous, and if the material is amorphous, it may soften during heating, especially after its glass transition temperature (Tg), and flow at higher temperatures, or if semi-crystalline, it may show a sharp transition once it has passed its so-called melting temperature (Tm), becoming solid again when the temperature is reduced below its crystallization temperature (in the semi-crystalline case) or below its glass transition temperature (in the amorphous case).

[0087] Tg and Tm are determined by differential scanning calorimetry (DSC) according to standards 11357-2:2013 and 11357-3:2013, respectively.

[0088] Fiber materials spare As regards the polymer constituting the impregnated matrix, it is advantageously a thermoplastic polymer, or a mixture of thermoplastic polymers, which can be ground in powder form so that it can be used in devices such as tanks, in particular in fluidized beds or in aqueous media.

[0089] Advantageously, PA6 is excluded from the definition of thermoplastic polymers.

[0090] The vessel-type apparatus, particularly in fluidized beds, may be an open or closed system.

[0091] Optionally, the thermoplastic polymer or blend of thermoplastic polymers further comprises a carbon-based filler, in particular carbon black or carbon-based nanofillers, preferably selected from among graphene, carbon nanotubes, carbon nanofibrils or mixtures thereof, which are capable of conducting electricity and / or heat and therefore can facilitate melting of the polymer matrix when heated.

[0092] Optionally, said thermoplastic polymer comprises at least one additive selected from among, inter alia, catalysts, antioxidants, heat stabilizers, UV stabilizers, light stabilizers, lubricants, fillers, plasticizers, flame retardants, nucleating agents, chain extenders and pigments, electrical conductors, thermal conductors or mixtures thereof.

[0093] Advantageously, said additives are chosen among flame retardants, electrical conductors and thermal conductors.

[0094] According to another variant, the thermoplastic polymer or mixture of thermoplastic polymers may further comprise a liquid crystal polymer or a cyclized polybutylene terephthalate or a mixture containing a cyclized polybutylene terephthalate, such as the CBT100 resin sold by CYCLICS CORPORATION. These compounds make it possible to fluidize the polymer matrix in the molten state, in particular for good penetration into the core of the fibers. spare Depending on the nature of the polymer, or mixture of thermoplastic polymers, used to make the impregnated matrix, and in particular its melting temperature, one or the other of these compounds will be chosen.

[0095] Fiber materials spare The thermoplastic polymers contained in the composition of the impregnated matrix are: - polymers and copolymers from the family of aliphatic, cycloaliphatic or semi-aromatic polyamides (PA), also called polyphthalamides (PPA), - polyureas, in particular aromatic polyureas; - polymers and copolymers from the acrylic family, such as the polyacrylates, in particular polymethylmethacrylate (PMMA) or its derivatives; - polymers and copolymers from the family of poly(aryl ether ketones) (PAEK), such as polyether ether ketones (PEEK), or poly(aryl ether ketone ketones) (PAEKK), such as poly(ether ketone ketones) (PEKK), or derivatives thereof; - aromatic polyether-imide (PEI), - polyarylsulfides, in particular polyphenylsulfide (PPS), - polyarylsulfides, in particular polyphenylene sulfone (PPSU), - polyolefins, especially polypropylene (PP); - Polylactic acid (PLA), - Polyvinyl alcohol (PVA), - fluorinated polymers, in particular polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE) or polychlorotrifluoroethylene (PCTFE), and mixtures thereof You can choose from.

[0096] Advantageously, PA6 is excluded from the definition of aliphatic polyamides.

[0097] Advantageously, when said polymer is a mixture of two polymers P1 and P2, the proportion, on a polymerization basis, of the polymers P1 and P2 is between 1 and 99% and between 99 and 1%.

[0098] Advantageously, said thermoplastic polymer is a blend, spare If the impregnation method uses dry powders, the mixture may be spare It is in the form of a powder obtained by dry blending before introduction into the bath for impregnation, or by dry blending carried out directly in the bath, or by grinding of a mixture previously prepared in an extruder.

[0099] Advantageously, this mixture is made up of powders obtained by dry blending before being introduced into the tank or directly in the tank, such a mixture of two polymers P1 and P2 is a mixture of PEKK and PEI.

[0100] Advantageously, the PEKK / PEI mixture is from 90-10% to 60-40% by weight, in particular from 90-10% to 70-30% by weight.

[0101] The thermoplastic polymer is the final non-reactive polymer that impregnates the fibrous material, or leads to said final non-reactive polymer, which also impregnates the fibrous material, but spare After impregnation, depending on the chain ends it has, it can correspond to a reactive prepolymer which can react with itself or with another prepolymer or with a chain extender, in particular during heating in a heated calendaring machine, or also a reactive thermoplastic prepolymer, optionally partially polymerized with said chain extender, having a number-average molecular mass (Mn) ranging from 500 to 10,000, preferably from 4,000 to 8,000. Depending on the Tg and / or Tm of the polymer used, said partially polymerized reactive thermoplastic prepolymer can be led to said non-reactive final polymer by heating.

[0102] The expression "non-reactive polymer" means that the molecular weight can no longer change significantly, i.e., when used, its number average molecular weight (Mn) changes by less than 50% and therefore corresponds to the final polyamide polymer in the thermoplastic matrix.

[0103] Conversely, the expression "reactive polymer" refers to a polymer whose molecular weight changes during its implementation, since reactive prepolymers react together by condensation, substitution, or with chain extenders by polyaddition, without the release of volatile by-products, to lead to the final (non-reactive) polyamide polymer in a thermoplastic matrix.

[0104] According to a first possibility, said prepolymer may comprise or consist of at least one carrier-reactive prepolymer (polyamide) having on the same chain (i.e. on the same prepolymer) two terminal functional groups X' and Y', in particular X' and Y' being amine and carboxy, or carboxy and amine, respectively, which become co-reactive functional groups towards each other by condensation.

[0105] In this first possibility, said at least one reactive thermoplastic prepolymer, optionally partially polymerized with said chain extender, has a number average molecular weight (Mn) ranging from 500 to 10,000, preferably from 4,000 to 8,000.

[0106] According to a second possibility, said prepolymers can comprise or consist of at least two polyamide prepolymers which are reactive towards each other, each prepolymer having two identical terminal functional groups X' or Y', respectively (same in the case of the same prepolymer and different between the two prepolymers), said functional group X' of a prepolymer being capable of reacting, in particular by condensation, only with said functional group Y' of the other prepolymer, in particular X' and Y' being amine and carboxyl, respectively, or carboxyl-terminated amine.

[0107] In this second possibility, said at least one reactive thermoplastic prepolymer, optionally partially polymerized with said chain extender, has a number average molecular weight (Mn) in the range of 500 to 10,000, preferably 4,000 to 8,000.

[0108] According to a third possibility, said prepolymer may comprise or consist of at least one prepolymer of said thermoplastic polyamide polymer having n terminal reactive functional groups X selected from among: -NH2, -CO2H and -OH, preferably NH2 and -CO2H, where n is between 1 and 3, preferably between 1 and 2, more preferably 1 or 2, especially 2, and at least one chain extender Y-A'-Y, preferably having a molecular mass of less than 500, more preferably less than 400, where A' is a hydrocarbon disubstituent having two identical terminal reactive functional groups Y which are reactive by polyaddition with at least one functional group X of said prepolymer a1).

[0109] In this second possibility, said at least one reactive thermoplastic prepolymer, optionally partially polymerized with said chain extender, has a number average molecular weight (Mn) in the range of 500 to 10,000, preferably 4,000 to 8,000.

[0110] The number average molecular weight Mn of said final polymer of the thermoplastic matrix is ​​preferably in the range of 10 000 to 40 000, preferably 12 000 to 30 000. These Mn values, depending on the change of solvent (m-cresol instead of sulfuric acid, temperature of 20° C.), may correspond to an intrinsic viscosity of 0.8 or more, determined in m-cresol according to standard ISO 307:2007.

[0111] Said reactive prepolymers according to the two options given above have a number average molecular weight Mn ranging from 500 to 10,000, preferably from 500 to 6,000, in particular from 2,500 to 6,000.

[0112] The Mn is determined in particular by calculation from the terminal functional groups determined by potentiometric titration in solution and the proportion of functional groups of the prepolymer. The mass Mn can also be determined by steric exclusion chromatography or by NMR.

[0113] The nomenclature used to define polyamides is described in the ISO standard 1874-1:2011 "Plastiques - Materiaux polyamides (PA) pour moulage et extrusion - Partie 1: Designation", in particular on page 3 (Tables 1 and 2), and is well known to the person skilled in the art.

[0114] The polyamide can be a homopolyamide or a copolyamide, or a mixture thereof.

[0115] Advantageously, the prepolymers constituting the matrix are chosen among polyamides (PA), in particular chosen among aliphatic, cycloaliphatic and semi-aromatic polyamides (polyphthalamides) optionally modified with urea units and their copolymers, polymethylmethacrylate (PPMA) and its copolymers, polyetherimides (PEI), polyphenylene sulfide (PPS), polyphenylene sulfone (PPSU), PVDF, polyetherketones (PEKK), polyetheretherketones (PEEK), fluorinated polymers such as polyvinylidene fluoride (PVDF).

[0116] Advantageously, PA6 is excluded from the definition of aliphatic polyamides. As regards the fluorinated polymer, it is possible to use homopolymers of vinylidene fluoride (VDF with formula CH2=CF2) or copolymers of VDF, which contain, by weight, at least 50% by mass of VDF and at least one other monomer copolymerizable with VDF. The VDF content must be higher than 80% by mass, or even better still, 90% by mass, to ensure good mechanical and chemical resistance of the structural parts, especially when exposed to thermal and chemical stresses. The comonomer must be a fluorinated monomer, for example vinyl fluoride.

[0117] For structural parts which must be resistant to high temperatures, besides fluorinated polymers, PAEKs (polyaryletherketones), such as poly(etherketone) PEK, poly(etheretherketone) PEEK, poly(etherketoneketone) PEKK, poly(etherketoneetherketoneketone) PEKEKK, or PAs with high glass transition temperatures Tg, are advantageously used according to the invention.

[0118] Advantageously, the thermoplastic polymer is an amorphous polymer, such as a polymer having a glass transition temperature Tg≧80° C., in particular ≧100° C., in particular ≧120° C., in particular ≧140° C., or a semi-crystalline polymer, such as a polymer having a melting temperature Tm≧150° C.

[0119] Advantageously, said at least one thermoplastic prepolymer is chosen from among polyamide, PEKK, PEI and mixtures of PEKK and PEI.

[0120] Advantageously, said polyamide is chosen from aliphatic polyamides, cycloaliphatic polyamides and semi-aromatic polyamides (polyphthalamides).

[0121] Advantageously, the aliphatic polyamide prepolymer comprises: - selected from polyamide 6 (PA-6), polyamide 11 (PA-11), polyamide 12 (PA-12), polyamide 66 (PA-66), polyamide 46 (PA-46), polyamide 610 (PA-610), polyamide 612 (PA-612), polyamide 1010 (PA-1010), polyamide 1012 (PA-1012), polyamide 11 / 1010 and polyamide 12 / 1010, or mixtures thereof or copolyamides thereof, and block copolymers, in particular polyamide / polyether (PEBA), said semi-aromatic polyamides, which are semi-aromatic polyamides optionally modified by urea units, in particular PA-MXD6 and PA-MXD6; semi-aromatic polyamides of formula X / YAr as described in MXD10 or in EP 1505099, in particular semi-aromatic polyamides of formula A / XT, where A is selected from units resulting from at least one amino acid, from at least one lactam and from at least one unit corresponding to formula (Ca diamine).(Cb diacid) in which "a" represents the number of carbon atoms of the diamine and "b" represents the number of carbon atoms of the diacid, "a" and "b" each being between 4 and 36, advantageously between 9 and 18, the units (Ca diamine) being selected from linear or branched aliphatic diamines, cycloaliphatic diamines and alkylaromatic diamines and the units (Cb diacid) being selected from linear or branched aliphatic diacids, cycloaliphatic diacids and aromatic diacids, XT stands for units resulting from the polycondensation of Cx diamines and terephthalic acid, where x represents the number of carbon atoms of the Cx diamine, x being between 6 and 36, advantageously between 9 and 18, in particular polyamides with the formula A / 6T, A / 9T, A / 10T or A / 11T, where A is as defined above, in particular the polyamides PA6 / 6T, PA66 / 6T, PA6I / 6T, PA MPMDT / 6T, PA PA11 / 10T, PA11 / 6T / 10T, PA MXDT / 10T, PA MPMDT / 10T, PA BACT / 10T, PA BACT / 6T, PA11 / BACT, PA BACT / 10T / 6T.

[0122] T corresponds to terephthalic acid, MXD corresponds to m-xylylenediamine, MPMD corresponds to methylpentamethylenediamine, and BAC corresponds to bis(aminomethyl)cyclohexane.

[0123] Advantageously, the aliphatic polyamide prepolymer comprises: selected from polyamide 11 (PA-11), polyamide 12 (PA-12), polyamide 66 (PA-66), polyamide 46 (PA-46), polyamide 610 (PA-610), polyamide 612 (PA-612), polyamide 1010 (PA-1010), polyamide 1012 (PA-1012), polyamide 11 / 1010 and polyamide 12 / 1010, or mixtures thereof or copolyamides thereof, and block copolymers, in particular polyamide / polyether (PEBA), said semi-aromatic polyamides being semi-aromatic polyamides optionally modified by urea units, in particular PA-MXD6 and PA-MXD6; MXD10 or semi-aromatic polyamides of formula X / YAr as described in EP 1505099, in particular semi-aromatic polyamides of formula A / XT, where A is selected from units resulting from at least one amino acid, from at least one lactam and from at least one unit corresponding to formula (Ca diamine).(Cb diacid) where "a" represents the number of carbon atoms of the diamine and "b" represents the number of carbon atoms of the diacid, "a" and "b" each being between 4 and 36, advantageously between 9 and 18, and the units (Ca diamine) are selected from linear or branched aliphatic diamines, cycloaliphatic diamines and alkylaromatic diamines, and the units (Cb diacid) are selected from linear or branched aliphatic diacids, cycloaliphatic diacids and aromatic diacids, XT are units resulting from the polycondensation of Cx diamines and terephthalic acid, where x represents the number of carbon atoms of the Cx diamine, x being between 6 and 36, advantageously between 9 and 18, in particular polyamides having the formula A / 6T, A / 9T, A / 10T or A / 11T, where A is as defined above, in particular polyamides PA6 / 6T, PA66 / 6T, PA6I / 6T, PA MPMDT / 6T, PA PA11 / 10T, PA11 / 6T / 10T, PA MXDT / 10T, PA MPMDT / 10T, PA BACT / 10T, PA BACT / 6T, PA11 / BACT, PA BACT / 10T / 6T.

[0124] T corresponds to terephthalic acid, MXD corresponds to m-xylylenediamine, MPMD corresponds to methylpentamethylenediamine, and BAC corresponds to bis(aminomethyl)cyclohexane.

[0125] Advantageously, said polyamide is a semi-aromatic polyamide selected from PA MPMDT / 6T, PA PA11 / 10T, PA11 / BACT, PA11 / 6T / 10T, PA MXDT / 10T, PA MPMDT / 10T, PA BACT / 10T, PA BACT / 6T, PA BACT / 10T / 6T, PA11 / BACT / 6T, PA11 / MPMDT / 10T, PA11 / BACT / 10T, PA11 / MXDT / 10T.

[0126] Fiber Material: As regards the fibres constituting said fibre material, they are in particular continuous fibres of inorganic, organic or vegetable origin in the form of rovings.

[0127] Advantageously, the number of fibres in said fibre material is, in the case of carbon fibres, 3K or more, in particular 6K or more, in particular 12K or more.

[0128] Advantageously, the number of fibres in said fibre material is, in the case of carbon fibres, greater than or equal to 12K, in particular selected from 12K, 24K, 48K, 50K and 400K, in particular from 12K, 24K, 48 and 50K.

[0129] Advantageously, in the case of glass fibres, the basis weight is greater than or equal to 1,200 Tex, in particular greater than or equal to 2,400 Tex, and greater than or equal to 4,800 Tex.

[0130] Inorganic fibres include, for example, carbon fibres, glass fibres, basalt or basalt-based fibres, silica fibres or silicon carbide fibres. Organic fibres include, for example, fibres based on thermoplastic or thermosetting polymers, such as semi-aromatic polyamide fibres, aramid fibres or polyolefin fibres. Preferably, they are based on amorphous thermoplastic polymers, and when the thermoplastic polymer mixture is amorphous, spareIt has a glass transition temperature Tg higher than the glass transition temperature Tg of the polymer or thermoplastic polymer mixture that constitutes the impregnated matrix, or if the thermoplastic polymer matrix is ​​semi-crystalline, spare They have a glass transition temperature Tg higher than the Tm of the polymer constituting the impregnating matrix or of the thermoplastic polymer matrix. Advantageously, they are based on semicrystalline thermoplastic polymers, if the thermoplastic polymer mixture is amorphous. spare It has a melting temperature Tm higher than the Tg of the polymer or thermoplastic polymer mixture that constitutes the impregnated matrix, or if the thermoplastic polymer matrix is ​​semi-crystalline, spare It has a melting temperature Tm higher than that of the polymer or thermoplastic polymer matrix that constitutes the impregnation matrix. Therefore, there is no risk of melting in the case of the organic fibers that constitute the fiber material during impregnation by the thermoplastic matrix of the final composite. Plant fibers include natural flax, hemp, lignin, bamboo, silk, especially spider silk, sisal, and other cellulose fibers, especially viscose. These plant fibers can be used pure or can be treated or coated with a coating layer to facilitate adhesion and impregnation of the thermoplastic polymer matrix.

[0131] The plant fibres may also correspond to fibres comprising support threads.

[0132] These component fibers can be used alone or in a mixture. Thus, organic fibers are more easily absorbed by thermoplastic polymers. spare Mixed with impregnated inorganic fibers, spare An impregnated fibrous material can be formed.

[0133] The organic fiber roving can have several basis weights. The organic fiber roving can also have several geometric shapes.

[0134] Preferably, the fibrous material is composed of continuous carbon, glass or silicon carbide fibers or mixtures thereof, in particular carbon fibers. The fibrous material is used in the form of a roving or several rovings, which in turn consist of a single roving to which the fibers of each roving are added.

[0135] In impregnated materials, also called "ready for use", the polymer or mixture of thermoplastic impregnating polymers is distributed uniformly and homogeneously around the fibers. In this type of material, the thermoplastic impregnating polymer must be distributed as homogeneously as possible inside the fibers to obtain a minimum porosity, i.e. a minimum of empty spaces between the fibers. In fact, the presence of pores in this type of material can act as stress concentration spots, for example during mechanical tensile stresses, which in turn form crack initiation points of the impregnated fiber material, mechanically compromising it. The homogeneous distribution of the polymer or mixture of polymers therefore improves the mechanical strength and homogeneity of the composite materials formed from these impregnated fiber materials.

[0136] Thus, when the so-called impregnated material is "ready for use", spare The fibre content in the impregnated fibrous material is between 45 and 65% by volume, preferably between 50 and 60% by volume, in particular between 54 and 60% by volume.

[0137] The impregnation rate can be measured by image analysis of the cross-section of the ribbon (e.g., using a microscope or optical or digital camera equipment) by dividing the surface area of ​​the ribbon impregnated with the polymer by the total surface area of ​​the product (impregnated surface + pore surface). To obtain good quality images, a cut piece of the ribbon is preferably coated laterally with a standard polishing resin and polished according to standard protocols, making it possible to observe the sample under a microscope with a magnification of at least 6x.

[0138] Advantageously, the porosity level of said impregnated fibrous material is less than 10%, in particular less than 5%, in particular less than 2%.

[0139] It should be noted that a pore-free level is difficult to achieve, so that advantageously the porosity level is higher than 0%, but less than the levels recited above.

[0140] The porosity level corresponds to the independent porosity level and can be determined either by electron microscopy or as the relative deviation between the theoretical and experimental density of the impregnated fibrous material, as described in the Examples section of the present invention.

[0141] According to another aspect, the present invention relates to a method for preparing an impregnated fibrous material as defined above, comprising the steps of: (a) heating the fibrous material by means of at least one heating system provided with at least one support part (E); spare The present invention relates to a method comprising the steps of heating the impregnated fibrous material and terminating the impregnation, and optionally shaping and calibrating the rovings of the impregnated fibrous material or said parallel rovings.

[0142] Advantageously, the shaping and calibration steps comprise: spare This is carried out after the steps of heating the impregnated fibrous material and terminating the impregnation.

[0143] In one embodiment, spare The steps of heating the impregnated fibrous material and of terminating the impregnation are carried out using the same heating system.

[0144] In another embodiment, spare The steps of heating the impregnated fiber material and terminating the impregnation are carried out using two separate heating systems.

[0145] Advantageously, spare The steps of heating the impregnated fibrous material and terminating the impregnation include heating the fibrous material. spare This is carried out after the impregnation step.

[0146] Advantageously, the method of the invention comprises the following steps: i) spare To obtain impregnated fibrous materials, the fibrous materials can be impregnated in particular by powder deposition, by the melt route, in particular by pultrusion, by crosshead extrusion of molten polymer, by continuous flow of the fibers in an aqueous polymer powder dispersion or an aqueous polymer particle dispersion or an aqueous polymer emulsion or suspension, by a fluidized bed with or without at least one support (E'), by spraying with a nozzle or a spray gun, by the dry route in a tank with or without at least one support (E'). spare impregnating, ii) The above spare Heating the impregnated fibrous material to complete the impregnation and obtain an impregnated fibrous material consisting of a tape in the form of a strip having an average thickness of less than 100 μm, in particular between 10 μm and 100 μm. iii) optionally shaping and calibrating the rovings of the impregnated fibrous material or the parallel rovings to obtain an impregnated fibrous material consisting of a tape in the form of a calibrated thin tape having an average thickness of less than 100 μm, in particular between 10 μm and 100 μm; Includes.

[0147] Advantageously, the process according to the invention is carried out at a speed of at least 10 m / min, in particular at least 20 m / min, in particular at least 30 m / min.

[0148] Method for preparing impregnated textile material in the form of strips or thin tapes Impregnated textile materials in the form of strips, especially monolayer materials, can be processed in two processes: Polymer matrix spare A first step which is impregnation and a second heating step to complete the impregnation by means of at least one support part (E) and at least one heating system. It can be prepared by:

[0149] Impregnated textile materials in the form of thin tapes, especially monolayer materials, can be produced in three steps: Polymer matrix spare a first step being impregnation, a second heating step to complete the impregnation by means of at least one support part (E) and at least one heating system, and a third step of shaping and calibrating. It can be prepared by:

[0150] First step: spare Impregnation spare Producing impregnated textile materials spare The first step of impregnation can be carried out according to techniques well known to those skilled in the art and can in particular be chosen from those disclosed above.

[0151] They can thus be produced by powder deposition, by the melt route, in particular by pultrusion, by crosshead extrusion of the molten polymer, by continuous flow of the fibres in an aqueous polymer powder dispersion or an aqueous polymer particle dispersion or an aqueous polymer emulsion or suspension, by a fluidised bed with or without at least one support (E'), by spraying by means of a nozzle or a spray gun, by the dry route in a tank with or without at least one support (E'), spare This can be done by impregnation techniques.

[0152] The support may be a concave, convex or cylindrical compression roller, in particular cylindrical.

[0153] FIG. 1 shows an example of a vessel provided with a support, and FIG. 2 shows an example of a vessel with a fluidized bed, where the support is a cylindrical compression roller.

[0154] The same vessel can be used without the presence of a fluidized bed and equipped with a spray gun.

[0155] spare Impregnation may also be achieved by providing one or more supports (E″) upstream of said system, in particular spareIt can also be carried out using a system such as the one defined above, present before the bath in which the impregnation takes place.

[0156] It should be noted that the support portions (E) and (E") can be identical or different, irrespective of the material or shape, and their characteristics (diameter, length, width, height, etc. as a function of shape).

[0157] Melting Path: spare The impregnation process can be carried out by the melt route, in particular by pultrusion.

[0158] By melting route spare Impregnation techniques are known by those skilled in the art and are described in the references mentioned above.

[0159] spare The impregnation step is in particular carried out by cross-head extrusion of the polymer matrix, passing the roving(s) through the cross-head and then through a heated die, the cross-head being able to provide fixed or rotating supports over which the rovings pass, thus causing them to stretch and to deform. spare Impregnation is possible.

[0160] spare The impregnation can in particular be carried out as described in US 2014 / 0005331 (A1), with the difference that the resin supply is carried out on two sides of said roving and that there is no surface contact and one of the two surfaces is devoid of any part of the resin.

[0161] Advantageously, spareThe impregnation step is carried out by melt passage at high speed, ie with a passing speed of said roving of at least 10 m / min, in particular at least 20 m / min, in particular at least 30 m / min.

[0162] Fluidized bed: spare The impregnation process may be carried out in a fluidized bed.

[0163] An exemplary unit for carrying out a manufacturing method without a heating step using at least one support part is described in the international application WO2015 / 121583.

[0164] This system is spare The use of a vessel with a fluidized bed for carrying out the impregnation process has been described and can be used in the context of the present invention.

[0165] Advantageously, the vessel with the fluidized bed is provided with at least one support part (E') (Figure 1), which may be a compression roller (Figure 2).

[0166] The support portion (E') must be understood to mean any system on which the rovings can move in the tank. The support portion (E') can have any shape, as long as the rovings can pass through it.

[0167] An example of the support portion (E') is disclosed in detail in FIG. 1, without limiting the invention thereto.

[0168] The support portions (E) and (E') can be identical or different, whether in terms of material or shape, and their characteristics (diameter, length, width, height, etc., depending on the shape).

[0169] However, the supporting portion (E') does not heat and is not heated.

[0170] Fiber materials spare The impregnation step is carried out in a continuous process comprising a vessel (10) provided with at least one support part (E') and a fluidized bed (12) of said polymer matrix powder. spare This is done by passing one or more rovings through an impregnation device.

[0171] The polymer matrix or polymer powder is suspended in a gas G (e.g. air) introduced into the vessel and circulates from a hopper (11) to the vessel (10). Rovings are circulated in this fluidized bed (12).

[0172] The vessel may have any shape, in particular a cylinder or parallelepiped, in particular a rectangular prism or a cube, advantageously a rectangular prism.

[0173] The vessel (10) can be an open vessel or a closed vessel.

[0174] In the event that the vessel is sealed, then the vessel is equipped with a sealing system, so that the polymer matrix powder cannot leave the vessel.

[0175] Therefore, this spare The impregnation step is carried out by the dry route, ie the thermoplastic polymer matrix is ​​in powder form, particularly suspended in gas, particularly air, but cannot be dispersed in solvents or water.

[0176] spare Each roving to be impregnated is unwound from a device equipped with a reel under a traction force exerted by a cylinder (not shown).

[0177] Each reel is provided with a brake (not shown) to apply tension to each fiber roving. In this case, an alignment module allows the fiber rovings to be arranged parallel to each other. In this way, the fiber rovings cannot come into contact with each other, which makes it possible to avoid mechanical damage to the fibers due to friction against each other.

[0178] 2, the fiber rovings or parallel fiber rovings then enter a vessel (10) comprising a fluidized bed (12) provided with a support part (E'), which is in particular a compression roller (24). The ... and, in particular, a fluidized bed (12) provided with a support part (E'), which is in particular a compression roller (24). The fiber rovings or parallel fiber rovings then enter a fluidized bed (12) optionally after checking their residence time in the powder. spare After impregnation, the tank is left.

[0179] The expression "residence time in powder" means the time during which the rovings are in contact with said powder in the fluidized bed.

[0180] If the fibrous material, such as a glass or carbon fiber roving, has a sizing, an optional step of resizing may be performed before the fibrous material passes through the vessel.

[0181] Advantageously, the vessel used comprises a fluidized bed comprising a support, said spare The impregnation step is carried out while simultaneously stretching the roving(s) between the inlet and outlet of the vessel containing the fluidized bed.

[0182] The expression "vessel inlet" corresponds to a vertical tangent to the edge of the vessel containing the fluidized bed.

[0183] The expression "outlet of the vessel" corresponds to the vertical tangent of the other edge of the vessel comprising the fluidized bed.

[0184] Drawing consists in isolating as far as possible each of the fibers that compose the roving from the other fibers that surround it in the space nearest to it, which corresponds to stretching the roving in the transverse direction.

[0185] In other words, the lateral separation or width of the roving increases between the entrance to the vessel with the fluidized bed and the exit from the vessel with the fluidized bed, thus increasing the flow rate of the fibrous material. spare Improved impregnation is possible.

[0186] therefore, spare The use of at least one support (E'), in particular a cylindrical compression roller, in the impregnation step, in comparison with the methods from the prior art, spare This allows for improved impregnation.

[0187] The expression "compression roller" means that the passing roving is partially or completely positioned on the surface of said compression roller, which causes stretching of said roving.

[0188] Advantageously, said at least one compression roller is cylindrical and the stretching of said roving between the inlet and the outlet of said fluidized bed bath is between 1% and 1000%, preferably between 100% and 800%, preferably between 200% and 800%, preferably between 400% and 800%.

[0189] The stretch ratio is equal to 100 times the ratio of the final width of the roving to the initial width of the roving.

[0190] The diameter of the at least one compression roller is between 3 mm and 500 mm, preferably between 10 mm and 100 mm, in particular between 20 mm and 60 mm.

[0191] Below 3 mm, the deformation of the fibers caused by the compression rollers is too large.

[0192] Advantageously, the compression roller is cylindrical, has no undulations and is in particular made of metal.

[0193] If the support part (E') is at least one compression roller according to the first variant, a single compression roller is present in the fluidized bed, spare Impregnation takes place at the angle α1 formed by the roving between the entrance of the compression roller and the perpendicular tangent at the compression roller.

[0194] The angle α1 formed by the roving between the entrance of the compression roller and a perpendicular tangent to the compression roller allows the formation of a region where the powder is concentrated, thus allowing the powder to be drawn across a larger roving width with the simultaneous stretching of the roving by the compression roller. spare Impregnation, thus improving over the techniques of the background art spare A "corner effect" is created which allows for improved impregnation.

[0195] Throughout this description, all angle values ​​presented are expressed in absolute values.

[0196] Advantageously, the angle α1 is comprised between 0° and 89°, preferably between 5° and 85°, preferably between 5° and 45°, preferably between 5° and 30°.

[0197] Nevertheless, angles α1 including 0-5° may cause the risk of mechanical stresses, which may result in fiber breakage, while angles α1 including 85°-89° do not result in sufficient mechanical forces to produce a "corner effect".

[0198] The value of the angle α1 is therefore equal to 0°, corresponding to vertical fibres. It is clear that the height of the cylindrical compression roller is adjustable, thus making it possible to position the fibres vertically.

[0199] Advantageously, the inlet edge of the tank (23a) is equipped with rollers, in particular cylindrical and rotating, over which the rovings pass, thus spare Stretching is effected prior to impregnation.

[0200] The "corner effect" caused by the angle α1 is the surface area of ​​one face. spare The stretching of the roving obtained by the compression rollers also favors impregnation of the other side of the roving. spare It is clear that it is possible to impregnate the spare Impregnation is enhanced on the surface of one side of the roving(s) in the vicinity of the angle α1 formed by the roving(s) between the entrance to the at least one compression roller R1 and a perpendicular tangent to the compression roller R1, while stretching is also enhanced on the surface of the other side. spare It also allows for impregnation.

[0201] The angle α1 is as defined above.

[0202] Advantageously, the particles of the thermoplastic polymer powder have a volume diameter D90 of between 30 and 500 μm, advantageously between 80 and 300 μm.

[0203] Advantageously, the particles of the thermoplastic polymer powder have a volume diameter D10 of between 5 and 200 μm, advantageously between 15 and 100 μm.

[0204] Advantageously, the volume diameter of the particles of the thermoplastic polymer powder lies in a ratio D90 / D10 of between 1.5 and 50, advantageously between 2 and 10.

[0205] Advantageously, the particles of the thermoplastic polymer powder have a mean volume diameter D50 of between 10 and 300 μm, in particular between 30 and 200 μm, especially between 45 and 200 μm.

[0206] The volume diameters of the particles (D10, D50 and D90) are defined by the standard ISO9276:2014.

[0207] "D50" corresponds to the mean diameter by volume, ie, the particle size value that divides the tested particle population exactly in half.

[0208] "D90" corresponds to the value at 90% of the cumulative curve of the volumetric particle size distribution.

[0209] "D10" corresponds to the size of 10% of the particle volume.

[0210] According to other variants, two, three or more rollers may be present in the fluidized bed.

[0211] Spraying with a spray gun: Fiber materials spare The impregnation process can also be carried out by continuous spraying, comprising a tank equipped with one or more nozzles or one or more guns that spray the polymer powder onto the fibrous material at the inlet roller. spare This can be done by feeding one or more rovings into an apparatus for impregnation.

[0212] A polymer-based powder or polymer is sprayed onto the surface of the fibrous material in a bath, in particular by means of a nozzle or spray gun near the support of the compression roller (at the inlet). The rovings are circulated in this bath.

[0213] A non-limiting example of using a spray gun is shown in FIG.

[0214] All the features of the support, in particular the compression roller, the stretching and the angle α1 causing the corner effect, detailed for the fluidized bed are also valid for spraying with a spray gun.

[0215] According to other variants, there are two, three or more rollers, each of which has a spray gun.

[0216] In one embodiment, spare The impregnation is carried out by powder deposition, by continuous flow of the fibers in an aqueous polymer powder dispersion or an aqueous polymer particle dispersion or an aqueous polymer emulsion or suspension, by a fluidized bed with or without at least one support (E'), by spraying with a nozzle or spray gun, by dry pass in a tank with or without at least one support (E').

[0217] In another embodiment, spare The impregnation is carried out by continuous flow of the fibers in an aqueous polymer powder dispersion or aqueous polymer particle dispersion or aqueous polymer emulsion or suspension, by a fluidized bed equipped or not equipped with at least one support (E'), by spraying with a nozzle or spray gun, by dry pass in a tank equipped or not equipped with at least one support (E').

[0218] Second step: spare Heating the impregnated textile material and terminating the impregnation therefore, spare The impregnation step can be carried out by any means provided with or without at least one support (E').

[0219] The presence of the support allows the roving to stretch, spare The impregnation is improved. However, the presence of this support means that the heating system, which is provided with at least one support part (E), is unable to terminate the impregnation. spare It is not essential, as long as it is present after the impregnation step.

[0220] The expression "support part (E)" refers to any system over which the rovings can pass. The support part (E) can have any shape as long as the rovings can pass over it. The support part can be stationary or rotating.

[0221] Advantageously, heated calenders are excluded from the definition of the support part (E).

[0222] The heating system is any system that generates heat or any system that generates radiation that is capable of heating the support part (E).

[0223] The heating system can be selected from infrared lamps, UV lamps, convection heating, microwave heating, laser heating and radio frequency (HF) heating.

[0224] The supporting portion (E) is therefore electrically conductive and absorbs the thermally generated radiation.

[0225] The expression "thermally conductive support part (E)" means that the support part (E) is made of a material capable of absorbing and conducting heat.

[0226] It can also be a heating system using radio frequency, microwave or laser.

[0227] In this case, the supporting portion does not conduct heat and does not absorb radiation generated by heat.

[0228] The expression "non-thermally conductive supporting part (E)" means that the supporting part (E) is made of a material that is not capable of absorbing and conducting heat.

[0229] Said at least one support part (E) is arranged or comprised in the environment of the heating system, ie is not outside the heating system.

[0230] Advantageously, said heating system is mounted on said at least one support part (E) and has a sufficient level so that the polymer present on the roving surface can melt but does not destroy said polymer.

[0231] Nevertheless, the heating system can either only comprise the at least one support part (E) or can also comprise a part of the roving outside the support system (E), the roving part being located in front and / or behind the support system (E).

[0232] An example of the heating system and three supports (E) corresponding to R'1, R'2 and R'3 is shown in FIG. 4, but is in no way limited thereto.

[0233] It is evident that a second heating system can be present below the support, thus allowing uniform melting of the polymer on the two surfaces of the roving.

[0234] The heating system shown in Figure 4 is a horizontal system. However, the heating system can be vertically oriented, with the rovings still passing vertically through the support.

[0235] As a result, this heating step: spare During the impregnation step it is possible to complete the previously carried out impregnation of the rovings and in particular to obtain a uniform impregnation of the cores.

[0236] Effectively, spare Whatever the system used for the impregnation process, in particular spare If the impregnation step is carried out by use of a supported part (E'), such as in a fluidized bed comprising at least one support, as described above, the first stretching is carried out during said step.

[0237] As the roving passes partially or entirely over the support portion (E'), a first stretching of the roping occurs at the compression roller corresponding to the support portion (E') due to the "corner effect", and as the roving passes partially or entirely over the support portion (E), a second stretching occurs during the heating step at the compression roller corresponding to the support portion (E).

[0238] The heating system can be divided into two, thus consisting of two heating systems, a first heating system in front of said support part (E) and a second heating system with said support part. It is then quite clear that the distance between the two heating systems is sufficient for the polymer to remain in a molten state.

[0239] The two heating systems may be of the same or different nature and may be of identical or different power.

[0240] As the polymer melts on the roving surface, contraction of the roving occurs prior to this second drawing while the roving passes through a heating system prior to passing partially or completely over the support (E).

[0241] This second stretching combined with melting of the polymer matrix due to the heating system and contraction of the rovings results in spare It is possible to make the impregnation uniform, thus terminating the impregnation and thus having impregnation of the core, and to have a high fiber content by volume, in particular a constant value that is at least 70% of the volume of the tape, in particular at least 80% of the volume of the tape, in particular at least 90% of the volume of the tape, especially at least 95% of the volume of the tape, and to reduce the porosity.

[0242] therefore, spare The roving, which has a width l1 before impregnation, spare After impregnation, the width l2>l1 is melted, and the molten polymer is spareAfter the impregnated fiber material is shrunk, the width l3 <l2>Has l1.

[0243] After passing over the support portion, a second expansion of the fibrous material containing the molten polymer results in a material having an average width l4 approximately equal to l2 and an average thickness e4 of less than or equal to 100 μm.

[0244] This impregnated fibrous material then constitutes a tape in the form of a strip having an uncalibrated average width but an average thickness of no more than 100 μm.

[0245] Advantageously, the inlet of the first compression roller R'1 and the last compression roller R i The stretching ratio during the heating step between the exit of the roll and the sheet is about 0 to 300%, particularly 0 to 50%.

[0246] The various stretchings during the heating step combined with the melting of the thermoplastic polymer and the shrinkage of the rovings during said heating step make it possible to produce, after the heating step, an impregnated fibre content of 45% to 65% by volume, preferably 50 to 60% by volume, in particular 54 to 60% (fibre contents which cannot be reached by conventional techniques by the melt route), with a fibre content and fibre distribution on a volume basis which is substantially equal to the average value on one side of the mid-plane of the fibre material over the entire length of said fibre material, thus obtaining in particular a single-layer fibre material.

[0247] Below 45% fibre the reinforcement is not interesting in terms of mechanical properties.

[0248] Above 65%, the limit value of the method is reached and the mechanical properties are lost again.

[0249] It is quite clear that the average thickness e4 depends on the impregnated fibre content, the average thickness being in particular less than 100 µm for impregnated fibre contents between 45 and 65% by volume.

[0250] Advantageously, the porosity level in said impregnated fibrous material is less than 10%, in particular less than 5%, in particular less than 2%.

[0251] Forming and calibration process: Obtaining thin tapes The steps of shaping the roving or said parallel rovings and calibrating said impregnated fibrous material are carried out after it leaves the second heating system.

[0252] This step can be carried out directly after leaving the second heating system, in which case the speed of advancement of the rovings is the same in the second and third heating systems, or it can be delayed, which means that the speed of advancement of the rovings can be different between the second and third heating systems.

[0253] This step can be carried out according to one of the following embodiments: 1) Passing the strip over one or more supports (defined as (E)), at least one of which is notched (grooved), said strip having an average width less than the notched (or grooved) support.

[0254] At least one of said supports is placed under a third heating system, in particular an IR, microwave, radio frequency or laser heating system, in particular an IR heating system with a power (each tape or stack of parallel tapes) between 0.1 W and 10 kW, more preferably between 0.1 and 6 kW, more preferably between 0.1 and 3 kW, even more preferably between 0.6 and 3 kW, even more preferably between 0.6 and 1.8 kW. Advantageously, said at least one notched roller (41) is located first and is outside the third heating system (45). Advantageously, the second notched support (44) is located at the exit and outside the third heating system.

[0255] By passing over the unnotched supports (42) and (43), the strip is allowed to expand again to the width of the notched supports.

[0256] The diameter of the notched support(s) (41) and (44) is between 12 mm and 50 mm, in particular between 12 mm and 30 mm.

[0257] The diameter of the unnotched support(s) (42) and (43) is between 10 mm and 50 mm, in particular between 10 mm and 30 mm.

[0258] After passing under the third heating system, the strip is shaped at the outlet of the third heating system to the width of the notched support and passes at the level of the heated calender (46) mounted in series and each equipped with a 1 kW IR system, the power delivered being variable, outside the third heating system, to obtain a thin-layer tape with a thickness of less than 100 μm. When calibrated at a width of 12.7 mm, the theoretical thickness of the tape will be 66 μm for a fibre content of 55% by volume and 61 μm for a fibre content of 60% by volume.

[0259] FIG. 7 discloses an exemplary embodiment and is not limited to that embodiment.

[0260] Although the supports are shown in Figure 7 at the same level, they can be similar to the second heating system at different heights. The notched supports may also have the same or different diameters as the unnotched supports.

[0261] 2) Passing the strip over one or more supports (as defined in relation to (E)), at least one of which is notched (or grooved), said strip having an average width greater than the notched (or grooved) support.

[0262] The support is placed under a third heating system, in particular an IR, microwave, radio frequency or laser heating system, in particular an IR heating system having a power output (for each tape or stack of parallel tapes) between 0.1 W and 10 kW, more preferably between 0.1 and 6 kW, more preferably between 0.1 and 3 kW, even more preferably between 0.6 and 3 kW, even more preferably between 0.6 and 1.8 kW.

[0263] Advantageously, said at least one notched roller is placed first.

[0264] Passing over the first notched support, it is possible to reduce the width of the strip to less than the width of the notched groove. Advantageously, a second notched support is present outside the outlet, having a groove of a width greater than the width of the strip, and a third heating system.

[0265] After passing under the third heating system, the strip is shaped at the outlet of the third heating system to the width of the notched support and passes through heated calendaring machines mounted in series and each equipped with a 1 kW IR system, at the level of the heated calendaring machines outside the third heating system, to obtain a thin-layer tape with a thickness of less than 100 μm.

[0266] When calibrated at 12.7 mm width, the theoretical thickness of the tape would be 66 μm for a 55% volume fibre content and 61 μm for a 60% volume fibre content.

[0267] A calendering system with controlled pressure and roll gap as disclosed in WO2015 / 121583 can be used for both embodiments.

[0268] In order to gather the impregnated fibre material to the correct width, the support is in particular a fixed or rotating notched roller or can even be a counter-rotating roller, in particular a fixed roller.

[0269] The notched roller may also have rounded edges at the lateral contact points with the substrate to avoid damaging the fibers at the edges of the thin tape.

[0270] The expression "rounded edges" means that the bottom of the notch is concave or convex in shape.

[0271] The impregnated fibrous material then, after passing over a calendering system, consists of a tape in the form of a laminar tape having a final average width of less than I4.

[0272] Advantageously, the first embodiment of the shaping and calibration steps is preferred.

[0273] The thin tape has an average thickness of less than 100 μm when the content of impregnated fibers is between 45 and 65% by volume.

[0274] Advantageously, said thin tape has a final average width less than I4 and an average thickness between 10 μm and 100 μm, for a content of impregnated fibers between 45 and 65% by volume.

[0275] This therefore makes it possible to work at high travel speeds and thus reduce production costs.

[0276] Advantageously, the process according to the invention is carried out at a speed of at least 10 m / min, in particular at least 20 m / min, in particular at least 30 m / min.

[0277] According to another aspect, the invention relates to the use of an impregnated fibrous material, as defined above, for the preparation of a thermoformed sheet.

[0278] Thermoforming is carried out above the Tg for amorphous thermoplastic polymers and between the Tg and Tm for semi-crystalline thermoplastic polymers, but can also be carried out above the Tm for semi-crystalline thermoplastic polymers.

[0279] The impregnated fibrous material is pre-slit into pieces having a width equal to the initial width of the fibrous material and a length between 5 and 50 mm, in particular between 20 and 30 mm, and the pieces are randomly bonded or oriented to prepare a thermoformed sheet.

[0280] The fibrous material can be either a strip or a thin tape.

[0281] Advantageous embodiments of the method of the invention Advantageously, the fibre material is selected from carbon fibre rovings, in particular 12K or higher, in particular selected from 12K, 24K, 48, 50K and 400K, in particular 12K, 24K, 48 and 50K, and glass fibres, in particular the basis weight of which is 1,200 Tex or higher, in particular 2,400 Tex or higher, 4,800 Tex or higher.

[0282] Advantageously, the thermoplastic prepolymer used to impregnate the carbon fibres is chosen from polyamides, in particular PA11, PA12, PA11 / 1010 and PA12 / 1010, semi-aromatic polyamides, in particular aliphatic polyamides such as PA MPMDT / 6T, PA PA11 / 10T, PA11 / BACT, PA11 / 6T / 10T, PA MXDT / 10T, PA MPMDT / 10T, PA BACT / 10T, PA BACT / 6T, PA BACT / 10T / 6T, PA11 / BACT / 6T, PA11 / MPMDT / 10T, PA11 / BACT / 10T, PA11 / MXDT / 10T, PEKK, PEEK and PEI, or mixtures thereof.

[0283] Advantageously, the thermoplastic prepolymers used to impregnate the glass fibres are selected from polyamides, in particular PA11, PA12, PA11 / 1010 and PA12 / 1010, semi-aromatic polyamides, in particular aliphatic polyamides such as PA MPMDT / 6T, PA PA11 / 10T, PA11 / BACT, PA11 / 6T / 10T, PA MXDT / 10T, PA MPMDT / 10T, PA BACT / 10T, PA BACT / 6T, PA BACT / 10T / 6T, PA11 / BACT / 6T, PA11 / MPMDT / 10T, PA11 / BACT / 10T, PA11 / MXDT / 10T, PEKK, PEEK and PEI, or mixtures thereof.

[0284] Advantageously, the fibre material comprises carbon fibre rovings selected from 12K and above, in particular 12K, 24K, 48, 50K and 400K, in particular 12K, 24K, 48 and 50K, spare The thermoplastic polymers used for impregnation are selected from polyamides, in particular PA11, PA12, PA11 / 1010 and PA12 / 1010, semi-aromatic polyamides, in particular aliphatic polyamides such as PA MPMDT / 6T, PA PA11 / 10T, PA11 / BACT, PA11 / 6T / 10T, PA MXDT / 10T, PA MPMDT / 10T, PA BACT / 10T, PA BACT / 6T, PA BACT / 10T / 6T, PA11 / BACT / 6T, PA11 / MPMDT / 10T, PA11 / BACT / 10T, PA11 / MXDT / 10T, PEKK, PEEK and PEI, or mixtures thereof.

[0285] Advantageously, the fibre material is made of carbon fibre rovings selected from 12K and above, in particular 12K, 24K, 48, 50K and 400K, in particular 12K, 24K, 48 and 50K, spare The thermoplastic polymers used for impregnation are selected from polyamides, in particular PA11, PA12, PA11 / 1010 and PA12 / 1010, semi-aromatic polyamides, in particular aliphatic polyamides such as PA MPMDT / 6T, PA PA11 / 10T, PA11 / BACT, PA11 / 6T / 10T, PA MXDT / 10T, PA MPMDT / 10T, PA BACT / 10T, PA BACT / 6T, PA BACT / 10T / 6T, PA11 / BACT / 6T, PA11 / MPMDT / 10T, PA11 / BACT / 10T, PA11 / MXDT / 10T, PEKK, PEEK and PEI, or mixtures thereof.

[0286] Advantageously, the fibrous material comprises a glass fiber roving having a basis weight of at least 1,200 Tex, in particular at least 2,400 Tex, at least 4,800 Tex, spare The thermoplastic polymers used for impregnation are selected from polyamides, in particular PA11, PA12, PA11 / 1010 and PA12 / 1010, semi-aromatic polyamides, in particular aliphatic polyamides such as PA MPMDT / 6T, PA PA11 / 10T, PA11 / BACT, PA11 / 6T / 10T, PA MXDT / 10T, PA MPMDT / 10T, PA BACT / 10T, PA BACT / 6T, PA BACT / 10T / 6T, PA11 / BACT / 6T, PA11 / MPMDT / 10T, PA11 / BACT / 10T, PA11 / MXDT / 10T, PEKK, PEEK and PE, or mixtures thereof.

[0287] Advantageously, the fibrous material is made of glass fibre rovings whose basis weight is greater than or equal to 1,200 Tex, in particular greater than or equal to 2,400 Tex, and greater than or equal to 4,800 Tex, and the glass fibres spare The thermoplastic polymers used for impregnation are selected from polyamides, in particular PA11, PA12, PA11 / 1010 and PA12 / 1010, semi-aromatic polyamides, in particular aliphatic polyamides such as PA MPMDT / 6T, PA PA11 / 10T, PA11 / BACT, PA11 / 6T / 10T, PA MXDT / 10T, PA MPMDT / 10T, PA BACT / 10T, PA BACT / 6T, PA BACT / 10T / 6T, PA11 / BACT / 6T, PA11 / MPMDT / 10T, PA11 / BACT / 10T, PA11 / MXDT / 10T, PEKK, PEEK and PEI, or mixtures thereof.

[0288] Advantageously, the fibre material comprises carbon fibre rovings selected from 12K and above, in particular 12K, 24K, 48, 50K and 400K, in particular 12K, 24K, 48 and 50K, spare The thermoplastic polymers used for impregnation are selected from polyamides, in particular PA11, PA12, PA11 / 1010 and PA12 / 1010, semi-aromatic polyamides, in particular aliphatic polyamides such as PA MPMDT / 6T, PA PA11 / 10T, PA11 / BACT, PA11 / 6T / 10T, PA MXDT / 10T, PA MPMDT / 10T, PA BACT / 10T, PA BACT / 6T, PA BACT / 10T / 6T, PA11 / BACT / 6T, PA11 / MPMDT / 10T, PA11 / BACT / 10T, PA11 / MXDT / 10T, PEKK, or mixtures thereof, wherein the Tg of said thermoplastic polymers is ≧80° C., in particular ≧100° C., in particular ≧120° C., in particular ≧140° C., or the Tm is ≧150° C.

[0289] Advantageously, the fibre material consists of carbon fibre rovings selected from 12K and above, in particular 12K, 24K, 48, 50K and 400K, in particular 12K, 24K, 48 and 50K, spare The thermoplastic polymers used for impregnation are selected from polyamides, in particular PA11, PA12, PA11 / 1010 and PA12 / 1010, semi-aromatic polyamides, in particular aliphatic polyamides such as PA MPMDT / 6T, PA PA11 / 10T, PA11 / BACT, PA11 / 6T / 10T, PA MXDT / 10T, PA MPMDT / 10T, PA BACT / 10T, PA BACT / 6T, PA BACT / 10T / 6T, PA11 / BACT / 6T, PA11 / MPMDT / 10T, PA11 / BACT / 10T, PA11 / MXDT / 10T, PEKK, or mixtures thereof, wherein the Tg of said thermoplastic polymers is ≧80° C., in particular ≧100° C., in particular ≧120° C., in particular ≧140° C., or the Tm is ≧150° C.

[0290] Advantageously, the fibrous material comprises a glass fiber roving having a basis weight of at least 1,200 Tex, in particular at least 2,400 Tex, at least 4,800 Tex, spare The thermoplastic polymers used for impregnation are selected from polyamides, in particular PA11, PA12, PA11 / 1010 and PA12 / 1010, semi-aromatic polyamides, in particular aliphatic polyamides such as PA MPMDT / 6T, PA PA11 / 10T, PA11 / BACT, PA11 / 6T / 10T, PA MXDT / 10T, PA MPMDT / 10T, PA BACT / 10T, PA BACT / 6T, PA BACT / 10T / 6T, PA11 / BACT / 6T, PA11 / MPMDT / 10T, PA11 / BACT / 10T, PA11 / MXDT / 10T, PEKK, PEEK and PEI, or mixtures thereof, wherein the Tg of said thermoplastic polymers is ≧80° C., in particular ≧100° C., in particular ≧120° C., in particular ≧140° C., or the Tm is ≧150° C.

[0291] Advantageously, the fibrous material is made of glass fibre rovings whose basis weight is greater than or equal to 1,200 Tex, in particular greater than or equal to 2,400 Tex, and greater than or equal to 4,800 Tex, spare The thermoplastic polymers used for impregnation are selected from polyamides, in particular PA11, PA12, PA11 / 1010 and PA12 / 1010, semi-aromatic polyamides, in particular aliphatic polyamides such as PA MPMDT / 6T, PA PA11 / 10T, PA11 / BACT, PA11 / 6T / 10T, PA MXDT / 10T, PA MPMDT / 10T, PA BACT / 10T, PA BACT / 6T, PA BACT / 10T / 6T, PA11 / BACT / 6T, PA11 / MPMDT / 10T, PA11 / BACT / 10T, PA11 / MXDT / 10T, PEKK and PEI, or mixtures thereof, wherein the Tg of said thermoplastic polymers is ≧80° C., in particular ≧100° C., in particular ≧120° C., in particular ≧140° C., or the Tm is ≧150° C.

[0292] 1 depicts a vessel (10) with a fluidized bed (12) with supports, the height of which (22) is adjustable. The inlet edge of the vessel is equipped with rotating rollers 23a, over which the rovings 21a pass, and the outlet edge of the vessel is equipped with rotating rollers 23b, over which the rovings 21b pass.

[0293] FIG. 2 describes an embodiment using a vessel (10) with a single compression roller, fluidized bed (12), in which there is a single cylindrical compression roller (24) exhibiting an angle α1.

[0294] The fiber arrows indicate the fiber passing direction.

[0295] FIG. 3 shows an embodiment using a single compression roller, a vessel (30) with a spray gun (31) for spraying powder (32), where there is a single cylindrical compression roller (33) and exhibits an angle α″1.

[0296] The fiber arrows indicate the fiber passing direction.

[0297] Figure 4 shows spare 1 shows a schematic of a single heating system for heating the impregnated fibrous material and the use of three rollers to terminate the impregnation.

[0298] FIG. 5 shows a photograph of the cross-section of a SGL, 50K carbon fiber roving impregnated with PA BACT / 10T polyamide powder with D50=108 μm (D90=198 μm and D10=48.3 μm) according to Example 1 and as disclosed in WO2015 / 121583 (before calendering) taken with a scanning electron microscope.

[0299] The method according to WO2015 / 121583 results in a fibrous material that is too thick (181 μm), lacking uniformity in some areas of the impregnated roving and also large pores, and poor distribution of the fibers.

[0300] The diameter of the fibres represents 7 μm.

[0301] FIG. 6 shows a photograph taken using a scanning electron microscope of the cross section of a SGL, 50K carbon fiber roving impregnated with PA BACT / 10T polyamide powder (41 / 59 molar ratio) with D50=108 μm (D90=198 μm and D10=48.3 μm) according to Example 2 of the present invention (before calendering).

[0302] The diameter of the fibres represents 7 μm.

[0303] The resulting strip has an average thickness of less than 88 μm with a fiber content of 55% by volume.

[0304] FIG. 7 shows an embodiment of the process of forming and calibrating a 12.7 mm strip (obtained in FIG. 6 ) using a first notched support (diameter 13 mm, groove 12.7 mm), two non-notched supports (diameter 20 mm) and a notched support (diameter 13 mm, groove 12.7 mm) outside the infrared (IR) system, a final IR heating system and a heated calendaring machine mounted in series, each of which is placed after the heated calendaring machine equipped with a 1 kW IR system, to obtain a 12.7 mm thin-layer tape.

[0305] FIG. 8 shows a photograph taken with an optical microscope of the cross section of a T700 12k 31E carbon fiber roving impregnated with PA11 / BACT polyamide powder (33 / 67) with D50=114 μm (D90=199 μm and D10=56 μm) according to Example 5 of the present invention (before calendering).

[0306] The diameter of the fibres represents 7 μm.

[0307] FIG. 9 shows a photograph taken with an optical microscope of the cross section of a T700 12k 31E carbon fiber roving impregnated with PA6I / 6T polyamide powder (45 / 55 molar ratio) with D50=136 μm (D90=225 μm and D10=75 μm) according to Example 6 of the present invention (before calendering).

[0308] The diameter of the fibres represents 7 μm.

[0309] FIG. 10 shows a photograph taken with an optical microscope of the cross section of a T700 12k 31E carbon fiber roving impregnated with PA MPMDT / 10T polyamide powder (41 / 59 molar ratio) with D50=157 μm (D90=301 μm and D10=58 μm) according to Example 7 of the present invention (before calendering).

[0310] The diameter of the fibres represents 7 μm.

[0311] The following examples provide non-limiting illustrations of the scope of the invention.

[0312] Example 1 (Comparative Example): A 50K carbon fibre roving from SGL was impregnated with PA BACT / 10T as described in WO2015 / 121583. D50=108μm, D90=198μm and D10=48.3μm

[0313] result: These results are shown in FIG. 5 and show a lack of uniformity in some of the areas of the impregnated roving, also with large pores and poor distribution of fibers.

[0314] Example 2: Single-ply fibrous material (SGL, 50K carbon fiber) impregnated with BACT / 10T (41 / 59 molar ratio) The following steps were performed: Four cylindrical and fixed rollers with a diameter of 8 cm are present upstream of the vessel with the fluidized bed, over which the rovings move.

[0315] The rollers are spaced 54 cm apart (distance between the central axis of the first roller and the central axis of the last roller).

[0316] Fluidized bed spare Impregnation process - Cylindrical compression roller R1 in the trough (L=500mm, l=500mm, H=600mm), diameter 25mm, as shown in Figure 2 - 0.3 second dwell time on powder - Angle α1 is 25° - For BACT / 10T powder, D50=108μm (D10=48.3μm, D90=198μm). - The edge of the tub is equipped with fixed rollers.

[0317] spare Terminating the heating and impregnation of the impregnated fiber material. The heating system disclosed in FIG. 4 is used, but with eight fixed cylindrical rollers R′1 to R′8, each having a diameter of 8 mm.

[0318] The travelling speed of the roving is 10 m / min.

[0319] The infrared generator used has a total power of 25 kW, the height between the infrared generator and the upper roller is 4 cm and the height between the infrared generator and the lower roller is 9 cm.

[0320] The angles α'1 to α'8 are the same and are 25°.

[0321] The height h is 20 mm.

[0322] The length l is 1,000 mm.

[0323] These eight rollers are spaced 43mm apart from each other.

[0324] FIG. 6 shows the resulting impregnated fibre material (strip), which has a thickness of 88 μm.

[0325] The resulting fibrous material is a single layer material, which has low porosity with impregnation uniformity and very good distribution of the fibers.

[0326] Molding and calibration steps to obtain thin tapes The steps of shaping the roving or said parallel rovings and of calibrating said impregnated fibre material are carried out, for example after leaving the second heating system described in FIG. 4, by passing the 88 μm strip (obtained in the previous step) over a first notched support of 13 mm diameter (the grooves are 12.7 mm), then over two unnotched rollers of 20 mm diameter under a third heating system, in particular an IR, microwave or laser heating system, in particular an IR heating system with a power between 0.1 W and 10 kW, more preferably between 0.1 and 6 kW, more preferably between 0.1 and 3 kW, even more preferably between 0.6 and 3 kW, even more preferably between 0.6 and 1.8 kW (for each tape or stack of parallel tapes), and finally over a notched roller of the same diameter and the same groove dimensions as the first one.

[0327] After passing under the third heating system, the strip formed to 12.7 mm is passed to the level of the heated calenders mounted in series outside the third heating system, each equipped with a 1 kW IR system, to obtain a calibrated 12.7 mm thin tape with a thickness of less than 100 μm. The fiber content is 55% by volume, the porosity level is <2%, and the thickness of the thin tape is 66 μm.

[0328] FIG. 7 illustrates this exemplary embodiment.

[0329] Example 3: Determining the porosity level by image analysis Porosity was determined by image analysis on rovings of SGL 50K carbon fibre impregnated with BACT / 10T (41 / 59 molar ratio) in a fluidised bed followed by a heating process as described above.

[0330] The porosity is less than 5%.

[0331] Example 4: Determination of the relative deviation of the porosity level between theoretical and experimental density (general method) a) The data required is: - Density of the thermoplastic matrix - Fiber density - Reinforcement weight: For example, linear mass for 1 / 4 inch tape (derived from a single roving) Surface density (g / m2) for example a wider tape or fabric 2 ) b) Measurements to be taken: The number of samples should be at least 30 in order for the results to be representative of the study: The measurements taken were as follows: - Size of sample taken: ○ Length (if linear mass is known). ○ Length and width (if surface density is known). - Experimental Density of Sample Taken: 〇 Mass measurement in air and water. The measurement of the fiber level is determined, for example, in the document B. Benzler, Applikationslabor, Mettler Toledo, Giesen, UserCom1 / 2001, in accordance with ISO 1172:1999 or by thermogravimetric analysis (TGA).

[0332] Measurement of carbon fiber levels may be determined in accordance with ISO 14127:2008.

[0333] Determination of theoretical mass fiber level: a) Determination of the theoretical mass fiber level: TIFF0007591927000001.tif13170 (in the formula, m l is the linear mass of the tape, L is the length of the sample, Me air is the mass of the sample measured in air)

[0334] The variation in fiber level by mass is believed to be directly related to the variation in matrix level, without considering the variation in fiber amount in the reinforcement.

[0335] b) Determination of the theoretical density: TIFF0007591927000002.tif17170(in the formula, d m and d f are the densities of the matrix and fiber, respectively)

[0336] The theoretical density thus calculated is the density available if no pores are present in the sample.

[0337] c) Porosity assessment: Porosity is then the relative deviation between the theoretical and experimental density.

[0338] Example 5: Single layer fiber material (Toray T700 12k 31E carbon fiber) impregnated with 11 / BACT (33 / 67 molar ratio) Using the same procedure as in Example 2, a fibrous material (Toray T700 12k 31E carbon fiber with a diameter of 7 μm) was impregnated with 11 / BACT powder with D50=114 μm (D10=56 μm, D90=199 μm).

[0339] FIG. 8 shows the results obtained.

[0340] Example 6: Single layer fibrous material (Toray T700 12k 31E carbon fiber) impregnated with PA6I / 6T (45 / 55 molar ratio) Using the same procedure as in Example 2, a fibrous material (Toray T700 12k 31E carbon fiber with a diameter of 7 μm) was impregnated with PA6I / 6T powder with D50=136 μm (D90=225 μm and D10=75 μm).

[0341] FIG. 9 shows the results obtained.

[0342] Example 7: Single-ply fiber material (Toray T700 12k 31E carbon fiber) impregnated with MPMDT / 10T (41 / 59 molar ratio) Using the same procedure as in Example 2, a fibrous material (Toray T700 12k 31E carbon fiber with a diameter of 7 μm) was impregnated with PA MPMDT / 10T powder with D50=157 μm (D90=301 μm and D10=58 μm).

[0343] FIG. 10 shows the results obtained.

Claims

1. At least one fibrous material consisting of continuous fibers and at least one non-reactive thermoplastic polymer matrix, or at least one reactive thermoplastic prepolymer, which is a precursor of said non-reactive thermoplastic polymer, optionally mixed with a chain extender; An impregnated textile material comprising: characterised in that the at least one non-reactive thermoplastic polymer or the reactive prepolymer is an amorphous polymer or prepolymer having a glass transition temperature Tg≧80° C. or a semi-crystalline polymer or prepolymer having a melting temperature Tm≧150° C., the fibre content by volume is constant for at least 90% of the volume of the impregnated fibrous material, the average thickness of the impregnated fibrous material is equal to or less than 100 μm, independent of the number of fibres present in the fibrous material before impregnation, and polyamide 6 is excluded from the definition of a thermoplastic polymer or thermoplastic prepolymer. Impregnated textile materials.

2. 2. The impregnated fibre material according to claim 1, characterized in that it has an average thickness between 10 μm and 100 μm.

3. 3. The impregnated fibrous material according to claim 1, characterized in that the number of fibres in the fibrous material is 12K or more in the case of carbon fibres and the basis weight is 1,200 Tex or more in the case of glass fibres.

4. 4. Impregnated fibrous material according to claim 1, characterized in that the fibres of the fibrous material are unsized fibres.

5. 5. Impregnated fibrous material according to claim 1, characterized in that the porosity level in the impregnated fibrous material is less than 10%.

6. 6. Impregnated fibrous material according to claim 1, characterized in that the impregnated fibrous material is a single layer.

7. 7. The impregnated textile material according to claim 1, characterized in that the at least one thermoplastic polymer is chosen from polyamide, PEKK, PEI and mixtures of PEKK and PEI.

8. 8. Impregnated textile material according to claim 7, characterized in that the polyamide is chosen from aliphatic, cycloaliphatic and semi-aromatic polyamides (polyphthalamides).

9. The aliphatic polyamide is selected from polyamide 11 (PA-11), polyamide 12 (PA-12), polyamide 66 (PA-66), polyamide 46 (PA-46), polyamide 610 (PA-610), polyamide 612 (PA-612), polyamide 1010 (PA-1010), polyamide 1012 (PA-1012), polyamide 11 / 1010, polyamide 12 / 1010, or mixtures or copolyamides and block copolymers thereof, and the semi-aromatic polyamide is a semi-aromatic polyamide which may be modified by urea units or a semi-aromatic polyamide of formula A / XT, where A is a unit derived from an amino acid, a unit derived from a lactam, and a unit derived from a diamine of formula (Ca). (Cb diacids) [wherein "a" represents the number of carbon atoms in the diamine and "b" represents the number of carbon atoms in the diacid, and "a" and "b" are each between 4 and 36], the units (Ca diamines) are selected from linear or branched aliphatic diamines, cycloaliphatic diamines and alkyl aromatic diamines, and the units (Cb diacids) are selected from linear or branched aliphatic diacids, cycloaliphatic diacids and aromatic diacids, 9. The impregnated textile material according to claim 8, characterized in that T is a unit resulting from the polycondensation of a Cx diamine and terephthalic acid, where x represents the number of carbon atoms of the Cx diamine and x is between 6 and 36.

10. 10. Impregnated fibrous material according to any one of claims 1 to 9, characterized in that the fibrous material comprises continuous fibres selected from carbon, glass, silicon carbide, basalt or basalt-based silica, natural fibres, or amorphous thermoplastic fibres having a Tg higher than the glass transition temperature Tg of the polymer or of the polymer blend, or semi-crystalline thermoplastic fibres having a melting temperature Tm higher than the Tg of the polymer or of the polymer blend, or a mixture of two or more of said fibres, 1. An impregnated fibrous material, wherein the polymer mixture is amorphous.

11. 10. Impregnated fibrous material according to any one of claims 1 to 9, characterized in that the fibrous material comprises continuous fibres selected from carbon, glass, silicon carbide, basalt or basalt-based silica, natural fibres, or amorphous thermoplastic fibres having a glass transition temperature Tg higher than the Tm of the polymer or of the polymer blend, or semi-crystalline thermoplastic fibres having a Tm higher than the melting temperature Tm of the polymer or of the polymer blend, or a mixture of two or more of the said fibres, 1. An impregnated fibrous material, wherein the polymer mixture is semi-crystalline.

12. 12. The impregnated fibrous material according to any one of the preceding claims, characterized in that the thermoplastic polymer further comprises a carbon-based filler.

13. 13. The impregnated fibrous material according to claim 1, characterized in that the thermoplastic prepolymer further comprises, as an additive, a liquid crystal polymer or a cyclic poly(butylene terephthalate), or a mixture containing said liquid crystal polymer or said cyclic poly(butylene terephthalate).

14. 14. Impregnated fibre material according to any one of the preceding claims, characterized in that it corresponds to a strip.

15. 14. Impregnated fibrous material according to any one of the preceding claims, characterized in that the impregnated fibrous material corresponds to a thin tape.

16. 16. A method for preparing an impregnated fibrous material as defined in any one of claims 1 to 15, characterized in that it comprises a step of heating the pre-impregnated fibrous material by means of at least one heating system provided with at least one support part (E), a step of terminating the impregnation and, optionally, a step of shaping and calibrating the rovings or said parallel rovings of the impregnated fibrous material.

17. 17. The method of claim 16, characterized in that the shaping and calibration steps are performed after the steps of heating the pre-impregnated fibrous material and of terminating the impregnation.

18. 18. Method according to claim 16 or 17, characterized in that the steps of heating the pre-impregnated fibre material and of terminating the impregnation are carried out using the same heating system.

19. 18. Method according to claim 16 or 17, characterized in that the steps of heating the pre-impregnated fibre material and of terminating the impregnation are carried out by means of two separate heating systems.

20. 20. The method according to any one of claims 16 to 19, characterized in that the steps of heating the pre-impregnated fibrous material and of terminating the impregnation are carried out after the step of pre-impregnating the fibrous material.

21. The following steps: i) pre-impregnating a fibrous material to obtain a pre-impregnated fibrous material; ii) heating said pre-impregnated fibrous material and terminating the impregnation to obtain an impregnated fibrous material consisting of a tape in the form of a strip having an average thickness of less than or equal to 100 μm; iii) optionally shaping and calibrating the rovings of said impregnated fibrous material or said parallel rovings to obtain an impregnated fibrous material consisting of a tape in the form of a thin tape having an average thickness of less than or equal to 100 μm; 21. The method according to any one of claims 16 to 20, characterized in that it comprises:

22. 22. A method according to any one of claims 16 to 21, characterized in that it is carried out at a speed of at least 10 m / min.

23. 16. Use of an impregnated fibre material as defined in any one of claims 1 to 15 for preparing a tape suitable for producing a three-dimensional composite part by automated robotic tape placement.

24. 16. Use of an impregnated fibrous material as defined in any one of claims 1 to 15 for preparing a thermoformed sheet.

25. 25. Use according to claim 24, characterised in that the impregnated fibrous material is pre-slit into pieces, said pieces being randomly bonded or oriented to prepare a thermoformed sheet.

Citation Information

Patent Citations

  • Manufacturing device for thermoplastic resin prepreg sheet material, and its manufacturing method

    JP2003181832A

  • Thermoplastic resin reinforced sheet material, its manufacturing method, and thermoplastic-resin multilayer reinforced sheet material

    JP2008221833A

  • Carbon fiber prepreg, carbon fiber prepreg tape, carbon fiber-reinforced composite material and automobile part that uses the carbon fiber-reinforced composite material

    JP2013203941A

  • Asymmetric fiber-reinforced polymer tape

    JP2015505879A

  • Method for producing unidirectional fiber-reinforced tape-shaped composite material, production device therefor and method for producing random sheet using the tape-shaped composite material

    JP2016011403A