Antifouling laminated sheet

The laminated sheet with an alcohol non-swelling urethane resin layer and antifouling fluororesin layer addresses the issue of alcohol resistance and flexibility loss in conventional stain-resistant materials, ensuring durability and effective stain resistance.

JP7591943B2Active Publication Date: 2024-11-29SEIREN CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021028583
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-25
Publication Date
2024-11-29
Estimated Expiration
2041-02-25

AI Technical Summary

Technical Problem

Conventional stain-resistant synthetic leathers used in hospitals and nursing care facilities lack alcohol resistance and flexibility, leading to potential degradation when exposed to alcohol-based disinfection, and do not maintain stretch recovery properties.

Method used

A laminated sheet structure comprising an alcohol non-swelling layer made of urethane resin and an antifouling layer made of fluororesin, acrylic resin, and a crosslinking agent, with specific formulations to ensure minimal alcohol swelling and excellent stretch recovery.

Benefits of technology

The laminated sheet maintains flexibility and stretch recovery properties even after exposure to alcohol, preventing functional deterioration and maintaining effective stain resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591943000002
    Figure 0007591943000002
  • Figure 0007591943000001
    Figure 0007591943000001
Patent Text Reader

Abstract

To provide an antifouling laminated sheet that is used to cover a mattress or the like, particularly a mattress or the like for a nursing home or a hospital, features excellent recovery after stretched and excellent alcohol resistance without sacrificing its softness.SOLUTION: An antifouling laminated sheet has an alcohol non-swollen layer and an antifouling layer, which are provided on one side of a substrate in this order, the alcohol non-swollen layer being composed of urethane resin, and the antifouling layer being composed of fluorine-based resin, acrylic resin and crosslinker.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a stain-resistant laminate sheet for use in mattresses and the like, and more particularly to a stain-resistant laminate sheet for use in covering mattresses and the like for use in nursing facilities and hospitals. [Background technology]

[0002] Conventionally, sheet materials are used to cover mattresses such as beds and wheelchair cushions in hospitals and nursing facilities. In particular, hospitals and nursing facilities are in need of stain-resistant sheet materials that are easy to remove sweat and dirt. The applicant has proposed synthetic leather for interior use and the like that has excellent stain resistance and does not impair the feel (Patent Document 1).

[0003] However, such synthetic leather does not take into consideration alcohol resistance, and there is a risk that repeated alcohol disinfection will result in a decrease in stain resistance and a decrease in stretch recovery. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2015-214773 A Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention has been made to solve the above-mentioned problems, and has an object to provide a stain-resistant laminate sheet that has excellent elongation recovery and alcohol resistance without losing its flexibility even when used to cover a mattress or the like. [Means for solving the problem]

[0006] The present invention provides an antifouling laminate sheet having an alcohol non-swelling layer and an antifouling layer sequentially provided on one surface of a substrate, the alcohol non-swelling layer being made of a urethane resin, The alcohol swelling rate measured by the following method is 5% or less,The stain-resistant layer is an stain-resistant laminate sheet made of a fluorine-based resin, an acrylic resin, and a crosslinking agent. Method for measuring alcohol swelling ratio: A square sample with sides of 70 mm is immersed in a 70% aqueous solution of isopropyl alcohol for 8.6 hours. The diagonal distance of the sample is measured before and after immersion and is calculated using the following formula. Equation 1: Alcohol swelling rate (%) = (BA) / A × 100 (In Equation 1, A represents the diagonal distance before immersion, and B represents the diagonal distance after immersion.)

[0007] The acrylic resin preferably contains an acrylic rubber. Effect of the Invention

[0008] According to the present invention, it is possible to provide a stain-resistant laminate sheet which does not lose its flexibility even when used to cover a mattress or the like and which has excellent elongation recovery and alcohol resistance. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an antifouling laminate sheet according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS An embodiment of the present invention will now be described in detail with reference to the drawings. An example of the antifouling laminate sheet 1 of the present invention is shown in Fig. 1. As shown in Fig. 1, the antifouling laminate sheet 1 has an alcohol non-swelling layer 3 and an antifouling layer 4 provided in this order on one surface of a substrate 2.

[0011] The substrate 2 is not particularly limited, and examples thereof include fabrics such as woven fabrics, knitted fabrics, and nonwoven fabrics. Fabrics can also be used that have been coated or impregnated with a conventionally known solvent-based or water-based polymer compound and then dry- or wet-coagulated. Among these, knitted fabrics are preferred from the viewpoint of elasticity. Examples of knitted fabrics include circular knitting, warp knitting, and weft knitting, and circular knitting is preferred from the viewpoint of elasticity in the lateral direction.

[0012] As the knitting structure of the circular knit, a conventionally known knitting structure can be used. Among the circular knits, double-sided knitting is preferable because it is dense, heavy, stretchable, elastic, and the ends of the fabric are less likely to curl. Examples of the double-sided knitting structure of the circular knit include brushed, mock rody, smooth (interlock), ponte roma, ripple, Milano rib, and jacquard. Among these, smooth is preferable from the viewpoints of economy and smoothness. In addition, one or both sides of the base material 2 may be a raised surface.

[0013] The type of fiber used for the base material 2 is not particularly limited, and may be any conventionally known fiber such as natural fiber, regenerated fiber, semi-synthetic fiber, or synthetic fiber, or may be a combination of two or more of these. Among these, synthetic fiber, particularly polyester fiber, is preferably used in terms of strength and processability. The base material 2 may be colored with a dye or pigment. The dye or pigment used for coloring is not particularly limited.

[0014] The form of the yarn used for the substrate 2 is not particularly limited, and may be either a filament yarn (long fiber yarn) or a spun yarn (short fiber yarn), or may be a long-short composite spun yarn combining long fibers and short fibers. The filament yarn may be twisted as necessary, or may be imparted with elasticity or bulkiness by false twisting or fluid disturbance treatment.

[0015] The fineness of the yarn used in the base material 2 is not particularly limited, but is preferably 56 to 330 dtex, and more preferably 75 to 250 dtex. When the fineness is 56 dtex or more, sewing strength and tear strength are easily obtained. When the fineness is 330 dtex or less, a soft texture is easily obtained. The single yarn fineness of the yarn used in the base material 2 is not particularly limited, but is preferably 0.1 to 20 dtex in terms of sewing strength.

[0016] The basis weight (mass per unit area) of the substrate 2 is not particularly limited, but is, for example, 150 to 600 g / m 2and more preferably 200 to 400 g / m 2 The basis weight is 200g / m 2 By having a weight of 600g / m or more, it is easy to obtain sewing strength and burst strength. 2 By satisfying the above condition, it is easy to obtain a soft texture.

[0017] The thickness of the substrate 2 is not particularly limited, but is preferably 0.4 to 0.8 mm, and more preferably 0.5 to 0.6 mm. When the thickness is 0.4 mm or more, burst strength is easily obtained. When the thickness is 0.8 mm or less, flexibility is easily obtained.

[0018] The alcohol non-swelling layer 3 is a layer that does not swell in alcohol, and specifically has an alcohol swelling rate of 5% or less. In addition, it is preferable that the alcohol swelling rate is 3% or less. The alcohol swelling rate is measured by immersing a square sample with sides of 70 mm in an aqueous solution of 70% isopropyl alcohol for 8.6 hours. The diagonal distance of the sample before and after immersion is measured, and the result is calculated using the following formula. Equation 1: Alcohol swelling rate (%) = (BA) / A × 100 In the formula, A represents the diagonal distance before immersion, and B represents the diagonal distance after immersion.

[0019] The resin used to form the alcohol non-swelling layer 3 is a urethane resin. Any urethane resin that does not swell in alcohol may be used, such as polyether polyurethane resin, polyester polyurethane resin, polycarbonate polyurethane resin, etc. These may be used alone or in combination of two or more. Among them, polycarbonate polyurethane resin is preferred from the viewpoints of light resistance and durability.

[0020] The alcohol non-swelling layer 3 preferably has a thickness of 10 to 50 μm, and more preferably 15 to 40 μm. When the thickness is 10 μm or more, abrasion resistance is easily obtained. When the thickness is 50 μm or less, flexibility is easily obtained.

[0021] The lamination method of the substrate 2 and the alcohol non-swelling layer 3 may be by bonding using an adhesive, heat fusion, or heat compression, but using an adhesive is preferable in terms of strength. The adhesive to be used is not particularly limited, but examples thereof include urethane resins, acrylic resins, and epoxy resins, and urethane resins are preferred because of their compatibility with the alcohol non-swelling layer 3. In addition, the method of applying the adhesive can employ various known methods, and is not particularly limited, but examples thereof include methods using a reverse roll coater, spray coater, roll coater, gravure coater, kiss roll coater, knife coater, and comma coater. Among these, the method using a comma coater is preferred because it can be applied easily and peel strength is easily maintained.

[0022] On the alcohol-non-swelling layer 3, an antifouling layer 4 is laminated. The stain-proof layer 4 is a layer made of a fluorine-based resin, an acrylic resin, and a crosslinking agent. Examples of the fluorine-based resin used to form the antifouling layer 4 include fluorinated acrylates, partially fluorinated resins, and fluorinated copolymers. Examples of the fluorinated acrylates include, but are not limited to, a (homo)polymer of a perfluoroalkyl group-containing methacrylate, or a copolymer of a perfluoroalkyl group-containing methacrylate with one or more of alkyl methacrylate, vinyl chloride, styrene, N-methylol methacrylamide, an aminimide group-containing monomer, and aziridinyl methacrylate. Examples of the partially fluorinated resins include polychlorotrifluoroethylene (trifluoride), polyvinylidene fluoride (difluoride), and polyvinyl fluoride. Examples of the fluorinated copolymers include tetrafluoroethylene-hexafluoropropylene copolymer, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, ethylene-tetrafluoroethylene copolymer, and ethylene-chlorotrifluoroethylene copolymer. These can be used alone or in combination of two or more. Among them, fluorinated acrylates are preferred from the viewpoint of economy.

[0023] Examples of the acrylic resin used to form the stain-resistant layer 4 include polymers and copolymers obtained from acrylic acid, methacrylic acid, or derivatives thereof, or modified products thereof. Examples of the monomer derivatives include alkyl acrylates such as methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, isobutyl acrylate, and 2-ethylhexyl acrylate, alkyl methacrylates such as methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, isobutyl methacrylate, and 2-ethylhexyl methacrylate, hydroxyl-containing acrylates such as 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, and 4-hydroxybutyl acrylate, 2-hydroxyethyl methacrylate, and 2-hydroxypropyl methacrylate. and polyfunctional methacrylic acid esters such as ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, polyethylene glycol dimethacrylate, neopentyl glycol dimethacrylate, dipropylene glycol dimethacrylate, polypropylene glycol dimethacrylate, 1,3-butanediol dimethacrylate, trimethylolethane trimethacrylate, trimethylolpropane trimethacrylate, and tetramethylolmethane tetramethacrylate. These may be used alone or in combination of two or more.

[0024] The acrylic resin used to form the stain-resistant layer 4 preferably contains acrylic rubber from the viewpoint of elongation recovery.

[0025] Examples of acrylic rubber include polymers that use one or more monomers such as methyl acrylate, ethyl acrylate, butyl acrylate, methyl methacrylate, and styrene and have a number average molecular weight of 400,000 or more. In terms of flexibility and elongation recovery, butyl acrylate polymers are preferred. In addition, those with an average molecular weight of 700,000 or more are preferred in terms of obtaining higher elongation recovery.

[0026] The crosslinking agent used in forming the antifouling layer 4 is not particularly limited, and any known crosslinking agent may be used. From the viewpoints of improving the strength of film formation and adhesion, however, epoxy compounds and isocyanate compounds are preferred.

[0027] The epoxy compound may be a compound containing two or more glycidyl groups in the molecule, such as ethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, glycerol polyglycidyl ether, diglycerol polyglycidyl ether, sorbitol polyglycidyl ether, polyethylene glycol diglycidyl ether, tripropylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, neopentyl glycol diglycidyl ether, 1,6 hexydiol diglycidyl ether, glycerin polyglycidyl ether, diglycerin polyglycidyl ether, trimethylolpropane polyglycidyl ether, spiroglycol diglycidyl ether, etc. Examples of the isocyanate compound include 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, m-phenylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 2,2'-diphenylmethane diisocyanate, 3,3'-dimethyl-4,4'-biphenylene diisocyanate, and 3,3'-dimethoxy-4,4'-biphenylene diisocyanate. , 1,5-naphthalene diisocyanate, 1,5-tetrahydronaphthalene diisocyanate, tetramethylene diisocyanate, 1,6-hexamethylene diisocyanate, dodecamethylene diisocyanate, trimethylhexamethylene diisocyanate, 1,3-cyclohexylene diisocyanate, 1,4-cyclohexylene diisocyanate, xylylene diisocyanate, tetramethylxylylene diisocyanate, and the like. These may be used alone or in combination of two or more. Among these, isocyanate compounds are preferred because of the simplicity of the crosslinking reaction and ease of production.

[0028] The stain-proof laminate sheet 1 has an elongation at break according to JIS L1096 in the longitudinal direction of preferably 20 to 60%, more preferably 30 to 50%, and in the transverse direction of preferably 50 to 100%, more preferably 60 to 80%. EXAMPLES

[0029] The stain-resistant laminate sheet of the present invention will be specifically described below, but the present invention is not limited thereto. Measurement and evaluation of physical properties in the examples and comparative examples were carried out by the following methods.

[0030] <Test Method> [Stain resistance] According to JIS L1919 8.3 C method (drop wiping method), the stain resistance test was performed using an artificial contaminant (lipophilic contaminant 3) and evaluated initially and after immersion in alcohol. The condition of the test piece before and after the stain was attached was graded using the stain gray scale according to JIS L0805.

[0031] [Alcohol resistance] A test piece 300 mm long and 200 mm wide was immersed in a 70% aqueous solution of isopropyl alcohol for 8.6 hours, then washed with overflowing water and hung to dry. The surface condition of the dried sample was observed and judged, and the antifouling properties were evaluated. The evaluation criteria for the surface condition are as follows: ○: No change on the surface △: Slight distortion is observed on the surface ×: Floating or distortion is clearly observed on the surface.

[0032] [Stretch recovery] A test piece measuring 120 mm in length and 30 mm in width was taken and stretched 10% 10 times using a tensile tester, after which the surface condition was observed and judged. The stretch test was carried out in both the course direction and the well direction of the substrate. ○: No residual distortion on the surface △: Some residual distortion is observed on the surface. ×: Residual distortion is clearly observed on the surface

[0033] [Elongation recovery after immersion in alcohol] A test piece measuring 120 mm in length and 30 mm in width was immersed in a 70% aqueous solution of isopropyl alcohol for 8.6 hours, then washed with overflowing water and hung to dry. After that, in the same manner as in the elongation recovery test, it was stretched 10% ten times using a tensile tester, and the surface condition was observed and judged.

[0034] [Example 1] [Formation of alcohol non-swelling layer] 40 parts by weight of dimethylformamide was added to 100 parts by weight of polycarbonate-based polyurethane resin (alcohol swelling rate 2%), and the mixture was applied to a release paper with a comma coater to a coating thickness of 200 μm, and then treated in a dryer at 130° C. for 2 minutes to form an alcohol non-swelling layer. The thickness of the alcohol non-swelling layer was 20 μm.

[0035] [Adhesion between substrate and alcohol non-swelling layer] To 100 parts by weight of polyether polyurethane resin, 50 parts by weight of dimethylformamide, 12 parts by weight of crosslinking agent, and 1 part by weight of crosslinking accelerator were added to prepare an adhesive solution. The adhesive solution was applied onto the alcohol non-swelling layer with a comma coater to a coating thickness of 150 μm, and dried in a dryer at 100°C for 1 minute. After drying, the adhesive-coated surface and the substrate (polyester smooth knitted fabric, yarn fineness: 75 dtex, single yarn fineness: 2 dtex, basis weight: 350 g / m 2 The release paper was then peeled off.

[0036] [Formation of anti-fouling layer] The antifouling layer mixture prepared according to Formulation 1 was applied to the alcohol non-swelling layer surface using a bar coater in a wet coating amount of 20 g / m 2 The coating was then dried in a dryer at 120° C. for 1 minute to obtain an antifouling laminate sheet. The antifouling layer had a thickness of 10 μm. The solid content is the mass fraction of the dried residue. [Formulation 1] Fluorine-based resin (perfluoroalkyl group-containing methacrylate polymer) solid content 15% 50 parts by weight Acrylic resin (2-hydroxyethyl methacrylate polymer) Solid content 15% 50 parts by weight Acrylic rubber (butyl acrylate polymer, number average molecular weight 700,000) Solid content 19% 25 parts by weight Crosslinking agent (1,6-hexamethylene diisocyanate) Solid content 100% 12 parts by weight Solvent (DMF / MEK (50 / 50)) 100 parts by weight (DMF: dimethylformamide, MEK: methyl ethyl ketone)

[0037] [Example 2] A stain-resistant laminate sheet was produced in the same manner as in Example 1, except that the alcohol non-swelling layer was produced as follows. 40 parts by weight of dimethylformamide was added to 100 parts by weight of polycarbonate-based polyurethane resin (alcohol swelling rate 4%), and the mixture was applied to a release paper with a comma coater to a coating thickness of 200 μm, and then treated in a dryer at 130° C. for 2 minutes to form an alcohol non-swelling layer. The thickness of the alcohol non-swelling layer was 20 μm.

[0038] [Example 3] The preparation was carried out in the same manner as in Example 1, except that the following formulation 2 was used to form the antifouling layer. [Formulation 2] Fluorine-based resin (perfluoroalkyl group-containing methacrylate polymer) solid content 15% 50 parts by weight Acrylic resin (2-hydroxyethyl methacrylate polymer) Solid content 15% 50 parts by weight Acrylic rubber (butyl acrylate polymer, number average molecular weight 400,000) Solid content 19% 25 parts by weight Crosslinking agent (1,6-hexamethylene diisocyanate) Solid content 100% 12 parts by weight Solvent (DMF / MEK (50 / 50)) 100 parts by weight

[0039] [Comparative Example 1] A stain-resistant laminate sheet was produced in the same manner as in Example 1, except that the alcohol non-swelling layer was produced as follows. 40 parts by weight of dimethylformamide was added to 100 parts by weight of polyester polyurethane resin (alcohol swelling rate 10%), and the mixture was applied to a release paper with a comma coater to a coating thickness of 200 μm, and then treated in a dryer at 130° C. for 2 minutes to form an alcohol non-swelling layer. The thickness of the alcohol non-swelling layer was 20 μm.

[0040] [Table 1]

[0041] As shown in Table 1, the antifouling laminate sheets according to the examples were excellent in elongation recovery and alcohol resistance, and no deterioration in function was observed due to alcohol immersion. In contrast, the antifouling laminate sheets according to the comparative examples had poor alcohol resistance, and deterioration in antifouling properties and elongation recovery was observed after alcohol immersion. [Explanation of symbols]

[0042] 1. Antifouling laminate sheet 2 Base material 3. Alcohol non-swelling layer 4. Antifouling layer

Claims

1. An antifouling laminate sheet comprising a substrate and an alcohol non-swelling layer and an antifouling layer provided in this order on one surface of the substrate, the alcohol non-swelling layer is made of a urethane resin and has an alcohol swelling rate of 5% or less as measured by the following method; The stain-resistant laminate sheet, wherein the stain-resistant layer comprises a fluorine-based resin, an acrylic resin, and a crosslinking agent. Alcohol swelling ratio measurement method: A square sample with sides of 70 mm is immersed in a 70% aqueous solution of isopropyl alcohol for 8.6 hours. The diagonal distance of the sample is measured before and after immersion and is calculated using the following formula. Formula 1: Alcohol swelling rate (%) = (B - A) / A x 100 (In formula 1, A represents the diagonal distance before immersion, and B represents the diagonal distance after immersion.)

2. The stain-resistant laminate sheet according to claim 1 , wherein the acrylic resin contains an acrylic rubber.

Citation Information

Patent Citations

  • Decorative sheet excellent in low staining properties

    JP2002326325A

  • Photocatalyst-containing actinic-radiation-curable coating composition capable of forming coating film lowly susceptible to contamination, its coating film, base material coated with the film, and method for preventing contamination

    JP2003165929A

  • Unadhesive sheet

    JP2008188989A

  • Leather-like sheet having excellent alcohol resistance and method for producing the same

    JP2011052336A

  • Antifouling synthetic leather

    JP2015214773A