Leather-like sheet and decorative molding
The leather-like sheet with a polymeric elastomer resin layer and fiber base material enhances grip by maintaining contact with convex portions, addressing the issue of articles sliding off, with improved static friction resistance.
Patent Information
- Application Number
- JP2021036032
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-08
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2041-03-08
AI Technical Summary
Leather-like sheets often lack sufficient grip, causing articles to slide off when placed on their surface, particularly in dynamic environments like vehicles or aircraft.
A leather-like sheet design featuring a resin layer composed of a polymeric elastomer on a fiber base material with specific strength and surface roughness parameters, including a maximum 20% strength of 4 kg/2.5 cm or more and an embossed uneven surface with 80% of the area corresponding to 25-65% of the total surface roughness, enhancing static friction resistance.
The design significantly improves the grip of articles on the leather-like sheet by maintaining contact with convex portions, reducing bending, and ensuring high static friction coefficients, preventing articles from slipping.
Smart Images

Figure 0007591948000002 
Figure 0007591948000003 
Figure 0007591948000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a leather-like sheet that has excellent gripping properties for articles. [Background technology]
[0002] Leather-like sheets are used as interior materials for bags, clothing, vehicles, aircraft, etc., exterior materials for the housings of mobile phones, mobile devices, and home appliances, and exterior materials for building materials, furniture, miscellaneous goods, sporting goods, etc. Also known is a decorative molded article in which such a leather-like sheet is disposed on the surface of a resin molded article.
[0003] For example, the following Patent Document 1 discloses an artificial leather comprising a fiber fabric, a grain surface layer containing a polymeric elastomer laminated on the fiber fabric, and a skin layer covering the grain surface layer, the skin layer being a film having an average thickness of 0.1 to 5 μm containing a polyurethane component containing 30 to 80 mass % of polyurethane having a 100% modulus of 1 MPa or less, and hollow nanosilica particles having an average primary particle diameter of 200 to 300 nm. It is also disclosed that such an artificial leather has dimples on the surface on which the grain surface layer and the skin layer are formed. It is also described that such an artificial leather has excellent grip properties in wet conditions and also remarkably excellent grip properties in dry conditions, and is preferably used as a skin material for balls.
[0004] Furthermore, although not a leather-like sheet, the following Patent Document 2 discloses an anti-slip sheet material in which a base sheet made of a nonwoven fabric or the like has been treated in advance by impregnation, coating or spraying with a resin water repellent compound containing a spreading agent such as an acrylic ester resin, and a resin emulsion composition such as an acrylic resin, polyurethane resin, or ethylene vinyl acetate resin is distributed at intervals on at least one side of the base sheet, and protruding resin bodies of relatively uniform convex height are dotted and protruded. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2015-101802 A [Patent Document 2] Japanese Patent Application Publication No. 7-178855 Summary of the Invention [Problem to be solved by the invention]
[0006] If the surface of the leather-like sheet does not have sufficient gripping ability for an object, there is a concern that the object may slip off when placed on the surface of the leather-like sheet. In such a case, for example, if the leather-like sheet is used as an interior material for a vehicle or an aircraft, and an object such as a mobile terminal device is placed on the surface of the leather-like sheet, it is expected that the object may slip off the surface of the leather-like sheet when the vehicle starts moving or the aircraft takes off.
[0007] An object of the present invention is to provide a leather-like sheet that has excellent gripping properties for articles, taking into consideration the concern that articles may slip off the surface of the leather-like sheet. [Means for solving the problem]
[0008] The present inventors have intensively studied factors that make it easy for an article to slip off when placed on the surface of a resin layer having an embossed uneven surface like grain that forms a leather-like sheet, and have found one of those factors. This factor will be explained with reference to FIG. 4. In FIG. 4, 20 is a conventional leather-like sheet having an embossed uneven surface on one side of a fiber substrate 11 and a resin layer 12 mainly made of a polymeric elastomer, and M is an article placed on the embossed uneven surface of the resin layer 12. As shown in FIG. 4(a), when the article M is placed on the embossed uneven surface of the resin layer 12 of the leather-like sheet 20, the article M adheres to the convex parts of the embossed uneven surface. In such a case, as shown in FIG. 4(b), when a force is applied to the article M in the horizontal direction indicated by the arrow, the frictional force between the article M and the convex parts of the embossed uneven surface causes the leather-like sheet 20 to bend, generating convex parts that do not come into contact with the article M, and thus forming voids v. They then discovered that the occurrence of convex portions that do not come into contact with the article M results in a decrease in gripping ability due to the article M coming into contact with the convex portions. They also discovered that such bending of the leather-like sheet 20 is more likely to occur the more flexible and soft the fiber base material 11 is. The present inventors conducted extensive research based on this knowledge and came up with the present invention.
[0009] That is, one aspect of the present invention is a leather-like sheet in which a resin layer mainly composed of a polymeric elastomer is applied to one surface of a fiber substrate, the maximum 20% strength T1 at 20°C being 4 kg / 2.5 cm or more, the surface of the resin layer having an embossed uneven surface, and the area of a region corresponding to a portion of 80% or more of the maximum height Sz in a surface roughness measurement according to ISO 25178 being 25 to 65% of the total area. According to such a leather-like sheet, since the area of the region corresponding to the convex parts of the embossed uneven surface is appropriate, the static friction resistance against an article by the embossed uneven surface is increased, improving the gripping ability of the article. In addition, since the maximum 20% strength T1 of the leather-like sheet at 20°C is 4 kg / 2.5 cm or more, the leather-like sheet is less likely to bend when an article placed on the embossed uneven surface receives a force in the horizontal direction and starts to move, so the contact area between the article and the convex parts of the embossed uneven surface is less likely to become small. As a result, a leather-like sheet with excellent gripping ability against an article is obtained.
[0010] As the polymeric elastomer, for example, polyurethane is preferably used.
[0011] In addition, the static friction coefficient of the surface of the resin layer is preferably 0.55 or more, since this allows for sufficient gripping properties for general articles such as smartphones.
[0012] Furthermore, it is preferable that the maximum height Sz of the embossed uneven surface is 30 to 100 μm, since this allows the surface design to be maintained while providing sufficient gripping properties for general articles.
[0013] Furthermore, it is preferable that the fiber base material has a maximum 20% strength T2 of 2.5 kg / 2.5 cm or more at 20° C., since this makes it easier to form a leather-like sheet that is less likely to bend.
[0014] In addition, it is preferable that the ratio T2 / T1 of the maximum 20% strength T2 of the fiber base material to the maximum 20% strength T1 of the leather-like sheet is 0.5 to 2.0, since this makes it easier to obtain the leather-like sheet described above by relatively increasing the rigidity of the fiber base material.
[0015] Another aspect of the present invention is a decorative molded body comprising a resin molded body and a decorative layer attached to the surface of the resin molded body, the decorative layer being any one of the above-mentioned leather-like sheets. Such a decorative molded body is preferable because the fiber base material is less likely to sink when an object is placed on the surface, and therefore the above-mentioned gripping property is easily exhibited. Effect of the Invention
[0016] According to the present invention, a leather-like sheet having excellent gripping properties for objects can be obtained. [Brief description of the drawings]
[0017] [Figure 1] FIG. 1 is a schematic cross-sectional view of a leather-like sheet 10 according to an embodiment. [Diagram 2] FIG. 2 is a schematic cross-sectional view illustrating each step of forming a decorative formed body using the leather-like sheet 10. As shown in FIG. [Diagram 3] FIG. 3 is a diagram showing the surface properties used in calculating the area of the region corresponding to 80% or more of the maximum height Sz of the embossed uneven surface 2a of the leather-like sheet obtained in Example 1. As shown in FIG. [Figure 4] FIG. 4 is an explanatory diagram for explaining the reason why an article tends to slip off when placed on the embossed uneven surface of the conventional leather-like sheet 20. As shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Hereinafter, the leather-like sheet of this embodiment will be described in detail with reference to the drawings.
[0019] Fig. 1 is a schematic cross-sectional view of a leather-like sheet 10 of this embodiment. As shown in Fig. 1, the leather-like sheet 10 is a leather-like sheet such as artificial leather or synthetic leather, in which a resin layer 2 mainly made of a polymeric elastomer is coated on one surface of a fiber substrate 1. The resin layer 2 has an embossed uneven surface 2a on its surface.
[0020] As described below, the leather-like sheet 10 has a maximum 20% strength T1 of 4 kg / 2.5 cm or more at 20°C, and the embossed uneven surface 2a has an uneven surface in which the area of a region corresponding to a portion of 80% or more of the maximum height Sz in a surface roughness measurement according to ISO 25178 is 25 to 65% of the total area.
[0021] The fiber substrate includes a nonwoven fabric, a woven fabric, a knitted fabric, or a fiber-entangled product that is a combination thereof, and preferably includes a polymeric elastomer impregnated into the fiber-entangled product. Among these, a fiber substrate obtained by impregnating a nonwoven fabric of ultrafine fibers with a polymeric elastomer as described below is particularly preferred, since it provides a fiber substrate with excellent solidity and a maximum 20% strength T1 at 20°C of 4 kg / 2.5 cm or more.
[0022] The type of fiber forming the fiber entanglement is not particularly limited. Specific examples of the resin forming the fiber include aromatic polyester resins such as polyethylene terephthalate (PET), modified polyethylene terephthalate, polybutylene terephthalate (PBT), polytrimethylene terephthalate (PTT), polytriethylene terephthalate, polyhexamethylene terephthalate, polypropylene terephthalate, and polyethylene naphthalate; aliphatic polyester resins such as polylactic acid, polyethylene succinate, polybutylene succinate, polybutylene succinate adipate, and polyhydroxybutyrate-polyhydroxyvalerate copolymer; nylon resins such as nylon 6, nylon 66, nylon 610, nylon 10, nylon 11, nylon 12, and nylon 6-12; polyolefin resins such as polypropylene, polyethylene, polybutene, polymethylpentene, chlorine-based polyolefin, ethylene-vinyl acetate copolymer, and styrene-ethylene copolymer.
[0023] In addition, the fineness of the fibers forming the fiber-entangled body is not particularly limited, but it is preferable to include ultrafine fibers having a fineness of 1 dtex or less, further 0.001 to 0.8 dtex, particularly 0.001 to 0.1 dtex, since this provides a supple texture with a sense of fullness and makes it easy to obtain a fiber base material having a maximum 20% strength T1 of 4 kg / 2.5 cm or more at 20° C. The ultrafine fibers may be present as fiber bundles formed by bundling a plurality of ultrafine fibers, such as ultrafine fiber-forming fibers such as islands-in-sea composite fibers.
[0024] The fiber substrate preferably contains a polymeric elastomer impregnated into the fiber-entangled body. Specific examples of the polymeric elastomer impregnated into the fiber-entangled body include polyurethane, acrylonitrile elastomer, olefin elastomer, polyester elastomer, polyamide elastomer, and acrylic elastomer. Among these, polyurethane, and further crosslinked water-based polyurethane obtained by solidifying water-based polyurethane emulsion, and particularly crosslinked water-based polyurethane containing polycarbonate / ether polyurethane, are preferred because they are easy to obtain a leather-like sheet having a 20% strength maximum value T1 of 4 kg / 2.5 cm or more at 20°C.
[0025] The content of the polymeric elastomer in the fiber substrate is not particularly limited, but is preferably 5 to 60 mass %, more preferably 8 to 40 mass %. The thickness of the fiber substrate is not particularly limited, but is preferably 250 to 750 μm, more preferably 300 to 500 μm.
[0026] The fiber substrate is preferably a highly rigid fiber substrate, specifically, for example, a hard fiber substrate having a maximum 20% strength T2 of 2.5 kg / 2.5 cm or more at 20° C., or more preferably 2.5 to 15 kg / 2.5 cm. By using such a hard fiber substrate, a leather-like sheet that is not easily bent is easily formed. As a result, a leather-like sheet that maintains high gripping properties is easily obtained. If the maximum 20% strength T2 of the fiber substrate at 20° C. is too low, as described above, when an article placed on the surface of the resin layer starts to move, the fiber substrate is easily bent and the surface of the resin layer is easily sunk, and as a result, the adhesion between the article and the convex portion of the resin layer tends to decrease.
[0027] Here, the maximum 20% strength at 20°C refers to the 20% strength of the leather-like sheet or fiber substrate at 20°C measured as described below. Usually, the maximum value is the 20% strength in the MD direction (longitudinal direction) parallel to the running direction of the production line of the leather-like sheet or fiber substrate. That is, the leather-like sheet or fiber substrate is produced while being pulled with tension applied in the running direction of the production line, so the fibers are stretched the most in the MD direction, and so the maximum value of the 20% strength is in the MD direction.
[0028] The 20% strength of the fiber base material at 20°C is adjusted by adjusting the fineness, type and strength of the fibers forming the fiber base material, the entanglement structure of the entangled fiber body, the degree of entanglement adjusted by needle punching, etc., the apparent density, basis weight, thickness, etc. That is, when the fiber strength is high, when the degree of entanglement is high, when the apparent density is high, when the fiber is thick, or when the basis weight is high, the 20% strength is high.
[0029] The apparent density of the fiber substrate is not particularly limited, but is preferably 0.20 to 1.00 g / cm 3 , especially 0.30~1.00g / cm 3 It is preferable that:
[0030] A leather-like sheet can be obtained by forming a resin layer mainly made of a polymeric elastomer on one surface of such a fiber substrate.
[0031] Examples of the polymeric elastomer that is the main component of the resin layer include polyurethanes such as polyether-polyester polyurethane, polycarbonate polyurethane, silicone-modified polycarbonate polyurethane, polyether polyurethane, and polyester polyurethane, which have been conventionally used to form grain-finish resin layers in leather-like sheets; acrylic elastomers; polyurethane-acrylic composite elastomers; silicone elastomers; polyvinyl chloride elastomers; and synthetic rubber. Among these, polyurethane is preferred because it has an excellent balance between the abrasion resistance and scratch resistance of the surface and the gripping properties.
[0032] The resin layer is mainly made of a polymeric elastomer, and may contain additives such as colorants such as pigments and dyes, softeners, antifouling agents, hydrophilizing agents, lubricants, deterioration inhibitors, ultraviolet absorbers, flame retardants, etc. Here, "mainly made of a polymeric elastomer" means that the resin layer contains 50% by mass or more, preferably 80% by mass or more, and more preferably 90% by mass or more of the polymeric elastomer.
[0033] The 100% modulus of such a resin layer at 20° C. is preferably 2 to 100 MPa, more preferably 25 to 50 MPa, from the viewpoint of a good balance between the resistance to bending of the uneven surface and the soft elasticity of the surface.
[0034] The storage modulus of the resin layer is preferably 2 to 80 MPa, more preferably 25 to 50 MPa, from the viewpoint of achieving an excellent balance between the resistance to bending of the uneven surface and the soft elasticity of the surface.
[0035] The thickness of the resin layer is not particularly limited, but is preferably 30 to 500 μm, more preferably 50 to 200 μm, from the viewpoints of easily forming an embossed uneven surface and of being able to sufficiently impart soft surface cushioning and a silver-finish design to the leather-like sheet.
[0036] Such a resin layer may be a homogeneous single layer, or may have a laminated structure in which a plurality of layers are laminated, such as an adhesive layer, an intermediate layer, and a surface layer.
[0037] The resin layer laminated on the leather-like sheet has an embossed uneven surface 2a having an uneven surface in which the area of a region corresponding to a portion of 80% or more of the maximum height Sz in surface roughness measurement according to ISO 25178 is 25 to 65% of the total area.
[0038] Here, surface roughness measurement according to ISO 25178 is a measurement method that measures the three-dimensional surface texture of an object surface by projecting a special stripe pattern onto the surface of the object, receiving the reflected light with a CMOS sensor, and forming an image representing the surface texture by mathematically calculating the surface texture from the result of the received light, and is measured with a non-contact surface roughness and shape measuring instrument. Then, based on the measured three-dimensional surface texture of the object surface, three-dimensional surface roughness parameters such as maximum height Sz, arithmetic mean height Sa, root mean square height Sq, skewness (deviation) Ssk, kurtosis (pointedness) Sku, maximum peak height Sp, maximum valley depth Sv, etc. can be calculated.
[0039] The maximum height Sz in surface roughness measurements based on ISO 25178 represents the distance from the highest point to the lowest point of the embossed uneven surface. The area of the region corresponding to 80% or more of the maximum height Sz can be calculated by generating a height contour diagram from an image showing the three-dimensional surface texture including information on the height difference of the surface, and then binarizing the height contour diagram using image processing software with the contour line corresponding to 80% or more of the maximum height Sz as the threshold.
[0040] The resin layer laminated on the leather-like sheet preferably has an embossed uneven surface having an uneven surface where the area of the region corresponding to 50% or more of the maximum height Sz is 60 to 90% of the total area. By having such an uneven surface, an article tends to adhere more closely to the protrusions of the uneven surface, and a high static friction coefficient can be maintained.
[0041] The resin layer laminated on the leather-like sheet has an embossed uneven surface with an area of a region corresponding to 80% or more of the maximum height Sz being 25 to 65% of the total area, preferably 25 to 60%. By having such an uneven surface, an article can be adhered to the convex parts of the uneven surface, and a high static friction coefficient can be maintained. If the area of the region corresponding to 80% or more of the maximum height Sz is less than 25% of the total area, the adhesion area between the uneven surface and the article becomes small, and if it exceeds 65%, the unevenness is small and the resistance force accompanying the bending of the convex parts generated when the article starts to move becomes small, making it difficult to maintain a high static friction coefficient.
[0042] In addition, in the surface roughness measurement of the leather-like sheet according to ISO 25178, the parameters of arithmetic mean height Sa, root mean square height Sq, skewness Ssk, kurtosis Sku, maximum peak height Sp, and maximum valley depth Sv are not particularly limited, but are preferably in the following ranges, for example: Sa is preferably 5 to 15 μm, Sq is 5 to 15 μm, Sku is 1 to 5, Ssk is -2 to -0.4, Sp is 10 to 25 μm, and Sv is 15 to 60 μm.
[0043] As a method for forming an embossed uneven surface on the surface of the resin layer of the leather-like sheet, for example, a method using a release paper having an uneven surface designed to form a resin film having an uneven surface in which the area of the region corresponding to 80% or more of the maximum height Sz is 25 to 65% of the total area by transferring the uneven surface to the surface of the resin film can be mentioned. Specifically, a resin liquid for forming a resin film mainly made of a polymeric elastomer is applied to the surface of such a release paper, and the resin film having an embossed uneven surface is formed by solidifying it.
[0044] Then, an adhesive for forming an adhesive layer is applied to the surface of the resin film formed on the release paper having the uneven surface as described above, and the resin film is attached to the surface of the fiber substrate, and if necessary, pressed to adhere, and then the release paper is peeled off. In this manner, the leather-like sheet as described above can be produced.
[0045] The release paper for forming the embossed uneven surface as described above is composed of, for example, a base paper and a release layer for transferring the embossed uneven surface. Types of paper include semi-bleached, wood-free, glassine, etc., and silicone resin is used for the release layer. The uneven surface of the release layer is adjusted by pressing a master with a different uneven surface shape into silicone resin and curing it in that shape. The release layer has a suitable adhesion to the resin layer of the leather-like sheet and has the ability to be peeled off after curing.
[0046] The release paper used is appropriately selected in consideration of the unevenness transferability of the resin layer used, and for example, a release paper having an uneven surface with Sz (μm) of about 35 to 100 and Sa (μm) of about 6 to 15 is preferably used.
[0047] As described above, the leather-like sheet of this embodiment is a leather-like sheet in which a resin layer mainly composed of a polymer elastomer is applied to one side of a fiber substrate, the maximum 20% strength T1 at 20°C being 4 kg / 2.5 cm or more, the surface of the resin layer having an embossed uneven surface, and the area of a region corresponding to a portion of 80% or more of the maximum height Sz in a surface roughness measurement in accordance with ISO 25178 being 25 to 65% of the total area.
[0048] The leather-like sheet of this embodiment is a relatively hard leather-like sheet having a maximum 20% strength T1 at 20°C of 4 kg / 2.5 cm or more, preferably 4 to 25 kg / 2.5 cm, and particularly preferably 4 to 15 kg / 2.5 cm. Such a hard leather-like sheet is less likely to bend when an article placed on the surface starts to move, and as a result, maintains high grip. If the maximum 20% strength T1 of the leather-like sheet at 20°C is less than 4 kg / 2.5 cm, as described above, the leather-like sheet will bend when an article placed on the surface of the resin layer starts to move, and the surface of the resin layer will be easily submerged, resulting in a decrease in adhesion between the article and the convex parts of the resin layer. In addition, if the maximum 20% strength T1 of the leather-like sheet at 20°C is too high, the leather-like sheet will tend to lose its supple texture.
[0049] In addition, the leather-like sheet of this embodiment has a ratio T2 / T1 of the maximum 20% strength T2 of the fiber substrate to the maximum 20% strength T1 of the leather-like sheet of 0.5 to 2.0, and preferably 0.5 to 1.0, since the rigidity of the fiber substrate is relatively high, and the leather-like sheet as described above is easily obtained. If T2 / T1 is too small, the leather-like sheet is likely to bend, resulting in the generation of convex parts that do not come into contact with the article, leading to a decrease in gripping properties, and if T2 / T1 is too large, the resin layer becomes soft relative to the fiber substrate, so that the embossed uneven surface of the resin layer is likely to deform when the article is placed on it, and the article does not obtain sufficient static friction resistance from the uneven surface, which tends to decrease gripping properties.
[0050] The thickness of the leather-like sheet is preferably 300 to 1500 μm, more preferably 400 to 1000 μm, since this makes it easier to form a resin layer having an embossed uneven surface and also makes it easier to form a leather-like sheet that is less likely to bend.
[0051] In the leather-like sheet of this embodiment, the static friction coefficient of the resin layer surface, measured as described below, is preferably 0.55 or more, more preferably 0.6 or more, and particularly preferably 0.6 to 0.9, in order to provide sufficient gripping properties to prevent articles from slipping off the surface. Also, the kinetic friction coefficient of the resin layer surface, measured as described below, is preferably 0.3 or more, more preferably 0.4 or more, and particularly preferably 0.4 to 0.9, in order to provide sufficient gripping properties to stop slipping even when the sheet starts to move.
[0052] The leather-like sheet described above can be used for any of the conventionally known applications of leather-like sheets without any particular limitation, but is particularly preferably used for applications where items are placed on the surface and are required to be less likely to slip off, such as interior materials for vehicles and aircraft, housings for mobile phones, mobile devices, and home appliances, exterior materials for building materials, furniture, miscellaneous goods, sporting goods, etc. In addition, for such applications, it is particularly preferably used as a leather-like sheet formed into a decorative molded body that decorates the surface that forms a housing.
[0053] The decorative molding of the present embodiment is a decorative molding in which a decorative layer is applied to the surface of a resin molding, and the above-mentioned leather-like sheet is used as the decorative layer. Such a decorative molding can have a leather-like surface with high gripping properties for an article.
[0054] Such decorated molded bodies are produced by trimming a leather-like sheet to fit the shape of the surface of a resin molded body to be attached and then adhering the trimmed leather-like sheet to the surface with an adhesive, or by using in-mold molding in which the leather-like sheet is integrated with the surface of a resin molded body formed by injection molding at the same time as the injection molding.
[0055] Referring to Figure 2, a process for forming a decorated molded body having a decorative surface that is a leather-like surface with a three-dimensional embossed uneven surface by performing in-mold decorative molding using a leather-like sheet 10 as a decorative layer through injection molding will be described.
[0056] 2(a), the mold 17 includes a movable mold 17a having a cavity C, and a fixed mold 17b. First, the leather-like sheet 10 having an embossed uneven surface is placed on the surface of the movable mold 17a that forms the cavity C, with the resin layer 2 facing the surface.
[0057] The leather-like sheet 10 is preferably molded into a preform molded body by heat press molding, vacuum molding, vacuum pressure molding, or the like, which is molded in advance to fit the shape of the cavity C of the mold 17 used for in-mold molding.
[0058] 2(b), molten resin 30a is injected by injection molding into the side of the fiber substrate 1 on the back side of the surface of the leather-like sheet 10 in the mold 17 opposite to the surface on which the resin layer 2 is arranged, thereby forming an in-mold molded body with the leather-like sheet 10 integrated on the surface. In detail, the movable mold 17a and the fixed mold 17b are clamped together, the cylinder 18 of the injection molding machine 7 is advanced until the nozzle 16 contacts the sprue bush 17f of the fixed mold 17b, and the molten resin 30a melted in the cylinder 18 of the injection molding machine is injected by the screw 19 into the mold 17 to perform injection molding. The injected molten resin 30a flows through the resin flow path R in the mold 17 and flows into the cavity C to fill it. In this case, when the leather-like sheet 10 is a leather-like sheet having a resin layer 2 laminated to a fiber base material 1, the molten resin 30a penetrates the fiber base material 1 moderately, so that the injection-molded body 30 formed by injection molding is integrated with the leather-like sheet 10 so as to maintain high adhesion due to the anchoring effect.
[0059] The resin injected in the injection molding may be any of a variety of thermoplastic resins, including, without particular limitation, ABS resins, polycarbonate resins, polyolefin resins such as polypropylene, polyester resins such as polyethylene terephthalate (PET) and polybutylene terephthalate (PBT), and various polyamide resins.
[0060] The injection molding conditions are appropriately selected according to the melting point and melt viscosity of the injected resin, the shape of the molded body, and the resin thickness, so that the resin can flow to the end of the flow path (resin temperature, mold temperature, injection pressure, injection speed, holding pressure after injection, and cooling time).
[0061] After the injection is completed, the molten resin 30a is cooled to form the injection molded body 30 as shown in Fig. 2(c), and the in-mold molded body 31 integrated with the leather-like sheet 10 is molded. Then, as shown in Fig. 2(d), the mold 17 is opened to separate the movable mold 17a and the fixed mold 17b, and the in-mold molded body 31 having the runner 32 is taken out. Then, the runner 32 is removed to obtain the decorated molded body 40 as shown in Fig. 2(e). EXAMPLES
[0062] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples.
[0063] First, the evaluation methods used in the present examples will be summarized below.
[0064] (Measurement of surface texture according to ISO 25178) The surface quality of the resin layer of the leather-like sheet was measured in accordance with ISO 25178 using a non-contact surface roughness and shape measuring instrument, "Digital Macroscope VHX-6000" (manufactured by Keyence Corporation). Specifically, a distorted fringe projection image was taken at 100x magnification with a 4 megapixel monochrome C-MOS camera using structured illumination light irradiated from a high-brightness LED over an area of 18mm x 24mm on the surface of the resin layer of the leather-like sheet. The obtained image was then analyzed and processed to determine the maximum height Sz. In addition, the arithmetic mean height Sa, root-mean-square height Sq, skewness (degree of deviation) Ssk, kurtosis (degree of sharpness) Sku, maximum peak height Sp, and maximum valley depth Sv were determined. Measurements were performed three times, and the average values were used for each value. The area of the region corresponding to 80% or more of the maximum height Sz and the area of the region corresponding to 50% or more of the maximum height Sz were calculated by generating a height contour map from the observed image and binarizing the height contour map with image processing software. The height contour map and the binarized image of the surface of the resin layer of the leather-like sheet obtained in Example 1 are shown in Figure 3.
[0065] (20% stronger) The leather-like sheet was left in a constant temperature and humidity environment of 20°C and 65 RH% for 20 hours. Then, a stress-strain curve was obtained according to JIS L 1096, 8.12.1 "Tensile strength test" using a universal material testing machine (Instron 5566, manufactured by Instron, USA) and a 2.5 cm x 16 cm test piece cut from the leather-like sheet. The stress at 20% elongation was read from the stress-strain curve to determine the 20% strength. In addition, since the test was maximum in the MD direction along the direction of progress of the manufacturing process of the leather-like sheet, three test pieces in the MD direction were measured, and the average value was taken as the 20% strength. The tensile speed was 200 mm / min.
[0066] (Thickness of leather-like sheet, resin layer and fiber substrate) The thicknesses of the leather-like sheet, the resin layer and the fiber substrate were measured using a "dial thickness gauge" (Peacock, model: H, manufactured by Ozaki Seisakusho Co., Ltd.) The measurement was carried out five times, and the average value was calculated.
[0067] (100% modulus of resin layer) A film of about 400 μm in thickness of the polyurethane composition forming the resin layer used in each Example and Comparative Example was prepared, and cut into a 2.5 cm width to measure the strength and elongation using a universal material testing machine (Instron 5566, manufactured by Instron Corporation, USA). The tensile speed was 200 mm / min. The strength at 100% elongation of the obtained SS curve was read and divided by the cross-sectional area obtained from the film thickness and 2.5 cm width to obtain the 100% modulus (MPa).
[0068] (storage modulus of resin layer) A film of about 120 μm in thickness was prepared from the polyurethane composition forming the resin layer used in each Example and Comparative Example, and a test piece cut to 5×10 mm was used to measure the storage modulus at room temperature (27° C.) with a dynamic viscoelasticity measuring device (Rheogel-E400, manufactured by UBM Co., Ltd.) The measurement conditions were frequency 11 Hz, sample size: 5×10 mm, thickness: 0.12 mm, measurement temperature: 0 to 240° C., heating rate: 3° C. / min., measurement mode: tension, and waveform: sine wave.
[0069] (friction coefficient) A test piece measuring 100mm x 200mm was cut out from the leather-like sheet. Then, using a friction and wear tester (HEIDON Tripo Gear TYPE:18L manufactured by Shinto Scientific Co., Ltd.), the static friction coefficient (μS) and dynamic friction coefficient (μD) were calculated with reference to JIS K 7125. The contact was made of aluminum and had a square flat contact measuring 30mm x 30mm. The load was 200g.
[0070] The fiber base material used in the present examples will be described below. Fiber base material A: A fiber bundle (average 25 fibers / bundle) of PET ultrafine fibers with a single fiber fineness of 0.08 dtex obtained by removing the sea component from a nonwoven fabric of islands-in-the-sea type composite fibers of long fibers was entangled, and the apparent density was 0.45 g / cm. 3A 370 μm thick fiber substrate was formed by impregnating a nonwoven fabric with crosslinked polycarbonate / ether-based polyurethane. The mass ratio of polyurethane / nonwoven fabric in the fiber substrate was 22 / 78. Fiber substrate B: A fiber bundle (average 25 fibers / bundle) of PET ultrafine fibers with a single fiber fineness of 0.08 dtex obtained by removing the sea component from a nonwoven fabric of islands-in-the-sea type composite fibers of long fibers was entangled, and the apparent density was 0.53 g / cm. 3 A 470 μm thick fiber substrate was formed by impregnating a nonwoven fabric with crosslinked polycarbonate / ether-based polyurethane. The mass ratio of polyurethane / nonwoven fabric in the fiber substrate was 22 / 78. Fiber base material C: A fiber bundle (average 25 fibers / bundle) of ultrafine fibers of nylon 6 (Tg 47°C) with a single fiber fineness of 0.003 dtex obtained by removing the sea component from a nonwoven fabric of islands-in-the-sea type composite fibers of long fibers was entangled. The apparent density was 0.36 g / cm. 3 A 450 μm thick fiber substrate was formed by impregnating a nonwoven fabric with crosslinked polycarbonate / ether-based polyurethane. The mass ratio of polyurethane / nonwoven fabric in the fiber substrate was 39 / 61. Fiber base material D: Fiber base material C that has been softened by immersing in a solvent and kneading.
[0071] The textured release paper used in this example has a base material of high-quality paper and a release layer of silicone resin, has a leather-like texture, and has the following maximum height Sz (μm) and arithmetic mean height Sa (μm), which are the three-dimensional surface properties of the release layer surface: Textured release paper E: Sz=38.83, Sa=6.56 Textured release paper F: Sz=90.15, Sa=12.86 Textured release paper G: Sz=78.23, Sa=13.31 Textured release paper H: Sz=51.19, Sa=7.87 Textured release paper I: Sz=49.35, Sa=8.72 Textured release paper J: Sz=57.05, Sa=8.18 Textured release paper K: Sz=47.82, Sa=7.29 Textured release paper L: Sz=73.71, Sa=6.76
[0072] The polyurethane solution used to form the resin layer in this example will be described below. Polyurethane solution M: A polyurethane solution in which polyether-polyester polyurethane resin is dissolved in a mixed solvent of ethyl acetate and N,N-dimethylformamide (DMF) and a pigment is added. Polyurethane N: Polyurethane solution in which polycarbonate-based polyurethane resin is dissolved in DMF, a solvent, and pigment is added.
[0073] [Example 1] Polyurethane solution M was applied to the surface of the embossed release paper E, and dried at 80°C for 10 minutes to form a polyurethane surface layer with a thickness of 30 μm. Next, a layer corresponding to a 30 μm thick intermediate layer was formed on the polyurethane surface layer in the same manner. Then, a polyether-ester type non-yellowing one-component curing polyurethane solution that would become an adhesive layer was further applied to the surface of the formed polyurethane surface layer / intermediate layer, and dried at 50°C for 3 minutes to form an adhesive layer with a thickness of 40 μm. In this way, a resin layer with a thickness of about 100 μm was formed. The 100% modulus of the resin layer was 27 MPa.
[0074] Then, the adhesive layer of the resin layer formed on the surface of the embossed release paper E was attached to one side of the fiber substrate A, and heated at 80°C for 2 minutes. In this way, a leather-like sheet was obtained, which is an artificial leather having a thickness of 446 μm and a grained resin layer. The obtained leather-like sheet was evaluated according to the above evaluation method. The results are shown in Table 1.
[0075] [Table 1]
[0076] [Examples 2 to 9, Comparative Examples 1 to 4] A leather-like sheet was obtained and evaluated in the same manner as in Example 1, except that the fiber substrate A and the textured release paper E in Example 1 were replaced with the fiber substrates and the textured release papers shown in Table 1. The results are shown in Table 1.
[0077] Referring to Table 1, the leather-like sheets of Examples 1 to 9, in which the maximum value T1 of 20% strength was 4 kg / 2.5 cm or more and the area of the top of the region corresponding to 80% or more of the maximum height Sz of the surface of the resin layer was in the range of 25 to 65% of the total area, all showed a static friction coefficient of 0.55 or more on the surface of the resin layer, and showed high frictional resistance. On the other hand, the leather-like sheets obtained in Comparative Examples 1 to 3, in which the area of the top of the region corresponding to 80% or more of the maximum height Sz was 25% or less of the total area, all had a static friction coefficient of less than 0.55 on the surface of the resin layer, and had low frictional resistance, even though the maximum value T1 was 4 kg / 2.5 cm or more. In addition, the leather-like sheet obtained in Comparative Example 4, in which the area of the top of the region corresponding to 80% or more of the maximum height Sz was 25% or more of the total area, but the maximum value T1 was less than 4 kg / 2.5 cm, also had a static friction coefficient of less than 0.55 on the surface of the resin layer, and had low frictional resistance. [Explanation of symbols]
[0078] 1. Fiber base material 2 Resin layer 2a Embossed textured surface 10 Leather-like sheet (decorative layer) 40 Decorative molding
Claims
1. A leather-like sheet in which a resin layer mainly made of a polymeric elastomer is coated on one side of a fiber substrate, The maximum 20% strength T1 at 20°C is 4 kg / 2.5 cm or more; The surface of the resin layer has an embossed uneven surface, and the area of a region corresponding to a portion having a maximum height Sz of 80% or more in a surface roughness measurement according to ISO 25178 is 25 to 65% of the total area.
2. 2. The leather-like sheet according to claim 1, wherein the polymeric elastomer is polyurethane.
3. 3. The leather-like sheet according to claim 1, wherein the static friction coefficient of the surface of the resin layer is 0.55 or more.
4. The leather-like sheet according to any one of claims 1 to 3, wherein the maximum height Sz of the embossed uneven surface is 30 to 100 µm.
5. 5. The leather-like sheet according to claim 1, wherein the fiber substrate has a maximum 20% strength T2 at 20° C. of 2.5 kg / 2.5 cm or more.
6. 6. The leather-like sheet according to claim 1, wherein the ratio T2 / T1 of the maximum 20% strength T2 of said fiber base material to the maximum 20% strength T1 of said leather-like sheet is 0.5 to 2.
0.
7. A decorated molded body comprising a resin molded body and a decorative layer attached to a surface of the resin molded body, A decorative molding, wherein the decorative layer is the leather-like sheet according to any one of claims 1 to 6.
Citation Information
Patent Citations
Antislipping working globe and its production
JP1993051804A
Anti-slip sheet material of production thereof
JP1995178855A
Leather-like sheet and method for producing the same
JP2009001946A
Sheet material having excellent fitting property and slip-preventing property
JP2012213471A
Grained artificial leather, decorative molded body and method for manufacturing grained artificial leather
JP2014181414A