Lithium-ion secondary battery
A stable positive electrode active material with a layered rock salt type crystal structure and additive elements like magnesium and fluorine enhances the charge/discharge capacity and safety of lithium ion secondary batteries by maintaining structural integrity during repeated charging and discharging.
Patent Information
- Application Number
- JP2022169346
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-03-22
- Filing Date
- 2022-10-21
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2041-10-26
AI Technical Summary
Lithium ion secondary batteries exhibit low charge/discharge capacity, cycle characteristics, and are prone to structural collapse during repeated charging and discharging, posing challenges in performance, reliability, safety, and cost.
A positive electrode active material with a broad peak around 4.55V in the dQ/dV curve, characterized by a layered rock salt type crystal structure, is developed, which maintains stability even at high charging depths by suppressing shear and volume changes, using a composite oxide with specific additives like magnesium and fluorine to enhance structural integrity.
The solution provides a secondary battery with improved charge/discharge capacity, reliability, and safety by preventing the collapse of the crystal structure during repeated cycles, ensuring high performance and safety even at high charging voltages.
Smart Images

Figure 0007592058000008 
Figure 0007592058000009 
Figure 0007592058000010
Abstract
Description
[Technical field]
[0001] One aspect of the present invention relates to an article, a method, or a manufacturing method. Alternatively, the present invention relates to a process, Pertaining to a machine, manufacture, or composition of matter. One embodiment of the present invention is a semiconductor device, a display device, a light-emitting device, a power storage device, a lighting device, an electronic device, or or a method for producing the same.
[0002] In this specification, the term "electronic device" refers to any device having a power storage device. Electro-optical devices having a power storage device, and information terminal devices having a power storage device are all electronic devices. [Background technology]
[0003] In recent years, lithium-ion secondary batteries, lithium-ion capacitors, air batteries, all-solid-state batteries, etc. The development of various types of electricity storage devices is currently underway. In particular, lithium-ion batteries, which have high output and capacity, are Demand for secondary batteries has expanded rapidly along with the development of the semiconductor industry, and the number of rechargeable energy sources has increased. As a source of supply, it has become indispensable in today's information society.
[0004] In particular, secondary batteries for mobile electronic devices have a large discharge capacity per unit weight and are highly durable. There is a high demand for secondary batteries with excellent thermal characteristics. There has been much progress in improving positive electrode active materials (for example, Patent Documents 1 to 3). Research on the crystal structure of positive electrode active materials is also being conducted (Non-Patent Documents 1 to 3). .
[0005] X-ray diffraction (XRD) is one of the techniques used to analyze the crystal structure of positive electrode active materials. ICSD (Inorganic Crystal Stabilizer) introduced in Non-Patent Document 4 By using the Structure Database, XRD data can be analyzed. This can be done. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2019-179758 A [Patent Document 2] WO2020 / 026078 Brochure [Patent Document 3] JP 2020-140954 A [Non-patent literature]
[0007] [Non-Patent Document 1] Toyoki Okumura et al, “Correlation of lithium ion distribution and X-ray absorption near-edge structure in O3-and O2-lithium cobalt oxides from first-principle calculation”, Journal of Materials Chemistry, 2012, 22, p.17340-17348 [Non-Patent Document 2] Motohashi, T. et al, “Electronic phase diagram of the layered cobalt oxide system LixCoO2 (0.0≦x≦1.0)”, Physical Review B, 80(16);165114 [Non-Patent Document 3] Zhaohui Chen et al, “Staging Phase Transitions in LixCoO2”, Journal of The Electrochemical Society, 2002, 149(12) A1604-A1609 [Non-Patent Document 4] Belsky, A. et al., “New developments in the Inorganic Crystal Structure Database (ICSD): accessibility in support of materials research and design”, Acta Cryst., (2002) B58 364-369. [Non-Patent Document 5] Rasband, WS, ImageJ, US National Institutes of Health, Bethesda, Maryland, USA, http: / / rsb.info.nih.gov / ij / , 1997-2012. [Non-Patent Document 6] Schneider, CA, Rasband, WS, Eliceiri, KW ``NIH Image to ImageJ: 25 years of image analysis''. Nature Methods 9, 671-675, 2012. [Non-Patent Document 7] Abramoff, MD, Magelhaes, PJ, Ram, SJ ``Image Processing with ImageJ''. Biophotonics International, volume 11, issue 7, pp.36-42, 2004. Summary of the Invention [Problem to be solved by the invention]
[0008] Lithium ion secondary batteries and the positive electrode active materials used therein have excellent charge / discharge capacity, cycle characteristics, and There is still room for improvement in various areas, such as speed, reliability, safety, and cost.
[0009] One embodiment of the present invention can be used in a lithium ion secondary battery, and can reduce the charge-discharge cycle One of the objectives of the present invention is to provide a positive electrode active material or a composite oxide in which the decrease in charge / discharge capacity is suppressed. Alternatively, the positive electrode active material or composite oxide has a crystal structure that does not easily collapse even after repeated charging and discharging. Another object of the present invention is to provide a positive electrode active material or a composite having a large charge / discharge capacity. Another object of the present invention is to provide a safe and highly reliable secondary battery. One of our goals is to provide
[0010] Another embodiment of the present invention provides a positive electrode active material, a composite oxide, a power storage device, or a manufacturing method thereof. One of our goals is to provide
[0011] The description of these problems does not preclude the existence of other problems. It is not necessary for the embodiment to solve all of these problems. It is possible to extract problems other than those mentioned above from the description of the claim. [Means for solving the problem]
[0012] In order to solve the above problem, one aspect of the present invention is to reduce the dQ / dVv To provide a positive electrode active material having a broad peak at about 4.55 V in the sV curve. The broadness of this peak indicates that the required temperature for lithium extraction in this vicinity is This indicates that there is little change in energy and little change in crystal structure. A positive electrode active material that is less susceptible to displacement and volume change and is relatively stable even at high charge depths It can be said that:
[0013] Alternatively, in one embodiment of the present invention, the charging voltage is 4.6 V or more and 4.8 V or less, and the charging depth is 0.8 or less. Even if the value is less than 0.9, the H1-3 type crystal structure is not formed, and the displacement of the CoO2 layer is suppressed. The present invention aims to provide a positive electrode active material capable of maintaining a good crystal structure.
[0014] More specifically, one embodiment of the present invention is a secondary battery having a positive electrode, The negative electrode is made of lithium metal, and the negative electrode is made of 1 mol / L lithium hexafluorophosphate and ethylene carbonate. Carbonate (EC) and diethyl carbonate (DEC) were mixed in a volume ratio of 3:7. ) and a mixture containing 2 wt% vinylene carbonate as the electrolyte, The capacity was measured when the battery was charged to 4.9 V at 10 mA / g in a 25°C environment. The dQ / dV vs V curve obtained by differentiating quantity (Q) with voltage (V) (dQ / dV) is , the peak is in the range of 4.5V to 4.6V, and the full width at half maximum of the peak is 0.10 or more. It is a secondary battery.
[0015] Another embodiment of the present invention is a secondary battery having a positive electrode, The negative electrode is made of lithium metal, and 1 mol / L of lithium hexafluorophosphate and ethylene carbonate are mixed. (EC) and diethyl carbonate (DEC) in a volume ratio of 3:7, vinyl When a battery was fabricated using a mixture containing 2 wt% of ethylene carbonate as the electrolyte, the battery The capacity (Q) was measured when charging at 10 mA / g up to 4.9 V in a 5°C environment. The dQ / dV vs V curve obtained by differentiating (dQ / dV) with respect to voltage (V) is 4.5V. A first peak is in the range of 4.15V to 4.25V. A second peak is present, and the ratio P1 / P2 of the intensity of the first peak P1 to the intensity of the second peak P2 is 2 is 0.8 or less.
[0016] Another embodiment of the present invention is a secondary battery having a positive electrode, The negative electrode is made of lithium metal, and 1 mol / L of lithium hexafluorophosphate and ethylene carbonate are mixed. (EC) and diethyl carbonate (DEC) in a volume ratio of 3:7, vinyl When a battery was fabricated using a mixture containing 2 wt% of ethylene carbonate as the electrolyte, the battery After charging at a constant current of 10 mA / g up to 4.75 V in a 5°C environment, the battery was placed in an argon atmosphere. When the positive electrode of the battery was analyzed by powder X-ray diffraction using CuKα1 radiation, the XRD pattern The axial alignment was at least 2θ = 19.47 ± 0.10° and 2θ = 45.62 ± 0.05°. It is a secondary battery having a diffraction peak.
[0017] Another embodiment of the present invention is a secondary battery having a positive electrode, The negative electrode is made of lithium metal, and 1 mol / L of lithium hexafluorophosphate and ethylene carbonate are mixed. (EC) and diethyl carbonate (DEC) in a volume ratio of 3:7, vinyl When a battery was fabricated using a mixture containing 2 wt% of ethylene carbonate as the electrolyte, the battery At 5℃, charge at a constant current of 100mA / g up to 4.8V, then charge at 10mA / g The charge is performed by charging at a constant voltage until the battery reaches 2.5 V, and the discharge is performed by discharging at a constant current of 100 mA / g until the battery reaches 2.5 V. After repeating this process four times, the batteries were charged at a constant current of 10 mA / g up to 4.8 V, and then placed in an argon atmosphere. When the positive electrode of the battery was analyzed by powder X-ray diffraction using CuKα1 radiation in an ambient atmosphere, The patterns are at least 2θ=19.47±0.10° and 2θ=45.62±0.0 This is a secondary battery that has a diffraction peak at 5°.
[0018] In addition, one aspect of the present invention is a method for measuring the response of a battery measured by a current rest method at an early stage of a charge / discharge cycle. The resistance component R (0.1s) that responds faster is n times faster than the nth discharge (n is a natural number greater than 1). The discharge capacity of the n+1th discharge is low, and the discharge capacity of the n+1th discharge is higher than the discharge capacity of the nth discharge. It is a pond.
[0019] In one embodiment of the present invention, a constant current discharge of 100 mA / g is performed during the charge / discharge cycle. The first step is 5 minutes and the second step is 2 minutes of rest without charging or discharging. The voltage 0.1 seconds after the start of the second step and the voltage at the end of the first step are When the difference between the pressure and the current is divided by the current value, the resistance component R (0.1s) with a fast response is The resistance component R(0.1s) has a minimum value before the 10th discharge from the second discharge onwards. This is a secondary battery that has the highest discharge capacity before the 10th discharge.
[0020] In the above, the positive electrode active material of the positive electrode preferably has a layered rock salt type crystal structure.
[0021] In the above, the transition metal M contained in the positive electrode active material of the positive electrode is 90 atomic % or more of cobalt. It is preferable that:
[0022] Another embodiment of the present invention is an electronic device including the above-described secondary battery, a display unit, and a sensor. It is a vessel. Effect of the Invention
[0023] According to one embodiment of the present invention, the present invention can be used in a lithium ion secondary battery, and can be used in a charge / discharge cycle. It is possible to provide a positive electrode active material or a composite oxide in which the decrease in charge / discharge capacity during charging / discharging is suppressed. Alternatively, a positive electrode active material or a composite oxide whose crystal structure is not easily destroyed even after repeated charging and discharging is used. Alternatively, a positive electrode active material or a composite oxide having a large charge / discharge capacity can be provided. Alternatively, a secondary battery with high safety or reliability can be provided.
[0024] According to another embodiment of the present invention, a positive electrode active material, a power storage device, or a manufacturing method thereof can be provided. This can be done.
[0025] The description of these effects does not preclude the existence of other effects. An embodiment does not necessarily have to have all of these effects. Effects other than these may also be included. The above is self-evident from the description, drawings, claims, etc. Other effects can be extracted from the claims and other descriptions. [Brief description of the drawings]
[0026] [Figure 1] FIG. 1 is a diagram illustrating a method for producing a positive electrode active material. [Diagram 2] FIG. 2 is a diagram illustrating a method for producing a positive electrode active material. [Diagram 3] 3A to 3C are diagrams illustrating a method for manufacturing a positive electrode active material. [Figure 4] FIG. 4A is a cross-sectional view of a positive electrode active material, and FIGS. 4B1 to 4C2 are a part of the cross-sectional view of the positive electrode active material. [Diagram 5] 5(A1) to 5(B) show the results of calculations regarding the magnesium distribution and crystal planes. [Figure 6] 6(A) and 6(B) are cross-sectional views of the positive electrode active material, and FIGS. 6(C1) and 6(C2) are partial cross-sectional views of the positive electrode active material. [Figure 7] FIG. 7 is a cross-sectional view of the positive electrode active material. [Figure 8] FIG. 8 is a cross-sectional view of the positive electrode active material. [Figure 9] FIG. 9 is a diagram illustrating the charge depth and the crystal structure of the positive electrode active material. [Figure 10] FIG. 10 shows an XRD pattern calculated from the crystal structure. [Figure 11] FIG. 11 is a diagram illustrating the charge depth and the crystal structure of the positive electrode active material of the comparative example. [Figure 12] FIG. 12 shows an XRD pattern calculated from the crystal structure. [Figure 13] 13(A) and 13(B) are diagrams showing XRD patterns calculated from the crystal structure. [Figure 14] 14(A) to 14(C) show the lattice constants calculated from XRD. [Figure 15] 15(A) to 15(C) show the lattice constants calculated from XRD. [Figure 16] FIG. 16 is an example of a TEM image in which the crystal orientations are roughly consistent. [Figure 17] Figure 17(A) is an example of a STEM image in which the crystal orientations are roughly consistent, Figure 17(B) is an FFT pattern of a region of rock-salt-type crystal RS, and Figure 17(C) is an FFT pattern of a region of layered rock-salt-type crystal LRS. [Figure 18] 18(A) and 18(B) are cross-sectional views of an active material layer in which a graphene compound is used as the conductive material. [Figure 19] 19(A) and 19(B) are diagrams illustrating an example of a secondary battery. [Figure 20] 20A to 20C are diagrams illustrating an example of a secondary battery. [Figure 21] 21(A) and 21(B) are diagrams illustrating an example of a secondary battery. [Figure 22] 22A to 22C are diagrams illustrating a coin-type secondary battery. [Diagram 23]23(A) to 23(D) are diagrams illustrating a cylindrical secondary battery. [Figure 24] 24(A) and 24(B) are diagrams illustrating an example of a secondary battery. [Diagram 25] 25(A) to 25(D) are diagrams illustrating an example of a secondary battery. [Figure 26] 26(A) and 26(B) are diagrams illustrating an example of a secondary battery. [Figure 27] FIG. 27 is a diagram illustrating an example of a secondary battery. [Figure 28] 28(A) to 28(C) are diagrams illustrating a laminate type secondary battery. [Figure 29] 29(A) and 29(B) are diagrams illustrating a laminate type secondary battery. [Diagram 30] FIG. 30 is a diagram showing the external appearance of a secondary battery. [Diagram 31] FIG. 31 is a diagram showing the appearance of a secondary battery. [Diagram 32] 32A to 32C are diagrams illustrating a method for manufacturing a secondary battery. [Diagram 33] 33A to 33H are diagrams illustrating examples of electronic devices. [Diagram 34] 34A to 34C are diagrams illustrating examples of electronic devices. [Diagram 35] FIG. 35 is a diagram illustrating an example of an electronic device. [Diagram 36] 36A to 36D are diagrams illustrating examples of electronic devices. [Figure 37] 37A to 37C are diagrams showing examples of electronic devices. [Figure 38] 38(A) to 38(C) are diagrams illustrating an example of a vehicle. [Figure 39] 39(A) to 39(F) are SEM images of the surface of the positive electrode active material. [Diagram 40] 40(A) to 40(H) are SEM images of the surface of the positive electrode active material. [Diagram 41]41(A), 41(B) and 41(D) are cross-sectional STEM images of the positive electrode active material, and FIG. 41(C) and 41(E) are FFT patterns. [Diagram 42] FIG. 42(A) is a cross-sectional STEM image of the positive electrode active material, and FIGS. 42(B1) to 42(D2) are EDX mapping images. [Diagram 43] Figures 43(A1) to 43(A3), 43(B1) to 43(B3), 43(C1), 43(C2-1), 43(C3-1), 43(C2-2), and 43(C3-2) are cross-sectional STEM images of the positive electrode active material. Figures 43(A4) to 43(A6), 43(B4) to 43(B6), 43(C4-1) to 43(C6-1), and 43(C4-2) to 43(C6-2) are EDX mapping images. [Diagram 44] Figures 44(A1) to 44(A3), 44(B1) to 44(B3), 44(C1), 44(C2-1), 44(C3-1), 44(C2-2), and 44(C3-2) are cross-sectional STEM images of the positive electrode active material. Figures 44(A4) to 44(A6), 44(B4) to 44(B6), 44(C4-1) to 44(C6-1), and 44(C4-2) to 44(C6-2) are EDX mapping images. [Diagram 45] 45(A) and 45(B) show the measurement results of the particle size distribution of the positive electrode active material. [Figure 46] 46(A) to 46(C) are SEM images of the surface of the positive electrode active material. [Figure 47] 47(A) to 47(C) are graphs showing the distribution of grayscale values of the positive electrode active material. [Figure 48] 48(A) to 48(C) are luminance histograms of the positive electrode active material. [Figure 49] 49(A) to 49(D) are graphs showing cycle characteristics of a secondary battery. [Figure 50] 50(A) to 50(D) are graphs showing cycle characteristics of a secondary battery. [Figure 51] 51(A) to 51(D) are graphs showing cycle characteristics of a secondary battery. [Figure 52] 52(A) to 52(D) are graphs showing cycle characteristics of a secondary battery. [Diagram 53] 53(A) and 53(B) are graphs showing cycle characteristics of a secondary battery. [Figure 54] Figure 54(A) is a photograph of the LCO pellet. Figure 54(B) and Figure 54(C) are SEM images of the surface of the positive electrode active material. [Figure 55] FIG. 55(A) is a surface SEM image of the positive electrode active material, and FIG. 55(B) is a cross-sectional STEM image of the positive electrode active material. [Figure 56] Figures 56(A1) and 56(B1) are cross-sectional HAADF-STEM images of the positive electrode active material. Figures 56(A2) to 56(A4) and 56(B2) to 56(B4) are EDX mapping images. [Figure 57] FIG. 57 shows the dQ / dV vs V curve of a secondary battery. [Figure 58] FIG. 58 shows the dQ / dV vs V curve of a secondary battery. [Figure 59] FIG. 59 shows the dQ / dV vs V curve of a secondary battery. [Figure 60] FIG. 60 is the XRD pattern of the positive electrode. [Figure 61] 61(A) and 61(B) are XRD patterns showing enlarged portions of FIG. [Figure 62] FIG. 62 is the XRD pattern of the positive electrode. [Figure 63] 63(A) and 63(B) are XRD patterns showing enlarged portions of FIG. 62. [Figure 64] Figure 64 is the XRD pattern of the positive electrode. [Figure 65] 65(A) and 65(B) are XRD patterns showing enlarged portions of FIG. 64. [Figure 66] Figure 66 is the XRD pattern of the positive electrode. [Figure 67] 67(A) and 67(B) are XRD patterns showing enlarged portions of FIG. 66. [Figure 68]Figure 68 is the XRD pattern of the positive electrode. [Figure 69] 69(A) and 69(B) are XRD patterns showing enlarged portions of FIG. 68. [Figure 70] FIG. 70 shows the XRD pattern of the positive electrode. [Figure 71] 71(A) and 71(B) are XRD patterns showing enlarged portions of FIG. [Figure 72] FIG. 72 is the XRD pattern of the positive electrode. [Figure 73] 73(A) and 73(B) are XRD patterns showing enlarged portions of FIG. [Figure 74] FIG. 74 is the XRD pattern of the positive electrode. [Figure 75] 75(A) and 75(B) are XRD patterns showing enlarged portions of FIG. 74. [Figure 76] FIG. 76 shows the XRD pattern of the positive electrode. [Figure 77] 77(A) and 77(B) are XRD patterns showing enlarged portions of FIG. [Figure 78] FIG. 78 is a diagram relating to powder resistivity measurement. [Figure 79] FIG. 79 is a graph showing a discharge curve measured by the current rest method. [Figure 80] FIG. 80 shows a method for analyzing current resting method measurements. [Figure 81] 81(A) and 81(B) are diagrams showing the analysis results of the current rest method measurement. [Figure 82] FIG. 82 shows the analysis results of the current rest method measurement. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] In the following, an embodiment of the present invention will be described with reference to the drawings. The present invention should not be construed as being limited to the following exemplary embodiments. It is possible to change the mode of carrying out the invention.
[0028] In this specification, crystal planes and crystal directions are expressed using Miller indices. The notation of crystal planes, crystal directions, and space groups is based on the numerical notation used in crystallography. However, due to formatting restrictions, in this specification, instead of putting a bar above the number, It may be expressed by putting a minus sign (-) before the character.
[0029] In this specification, the theoretical capacity of the positive electrode active material is the capacity of the positive electrode active material that can be inserted and removed. This refers to the amount of electricity when all the lithium is removed. For example, the theoretical capacity of LiCoO2 is 274m Ah / g, the theoretical capacity of LiNiO2 is 274mAh / g, and the theoretical capacity of LiMn2O4 is 1 It is 48mAh / g.
[0030] In this specification, the depth of charge refers to the degree of capacity based on the theoretical capacity of the positive electrode active material. The charged state, in other words, how much lithium has been removed from the positive electrode active material For example, lithium cobalt oxide (LiCoO2) and nickel-cobalt Lithium manganate (LiNi x Co y Mn z O2(x+y+z=1)) In the case of a positive electrode active material with a rock salt structure, the theoretical capacity of 274mAh / g is used as the standard. When the charge depth is 0, lithium has not been released from the positive electrode. When the charge depth is 0.5, This refers to a state in which lithium equivalent to 137mAh / g is released from the positive electrode active material, and the charge depth is In the case of 0.8, lithium equivalent to 219.2mAh / g is released from the positive electrode active material. Also, Li a When expressed as CoO2(0≦a≦1), if the charge depth is 0, When the charge depth is 0.5, a is written as LiCoO2 with a of 0.5. 0. If the charge depth is 0.8, then a is 0.2. 0.2 CoO2 and It is written.
[0031] In this specification, a value close to a certain value A is a value between 0.9×A and 1.1×A. The value is referred to as the
[0032] In this specification and the like, a secondary battery using a positive electrode and a positive electrode active material of one embodiment of the present invention is In some cases, lithium metal is used as the counter electrode. However, the negative electrode may be made of other materials, such as graphite, lithium titanate, etc. The positive electrode and positive electrode active material according to the present invention have a crystal structure that is resistant to collapse even after repeated charging and discharging, and have good The properties of the battery, such as good cycle characteristics, are not affected by the material of the negative electrode. For secondary batteries, the charging voltage is about 4.7V for lithium electrodes, which is higher than the general charging voltage. Although examples of charging and discharging at a high voltage are shown, charging and discharging at a lower voltage may also be performed. When charging and discharging at a low voltage, the cycle characteristics are even better than those shown in this specification. is expected.
[0033] In this specification, unless otherwise specified, the charge voltage and discharge voltage are those of the lithium counter electrode. However, even with the same positive electrode, the voltage of the secondary battery varies depending on the material used for the negative electrode. The charge and discharge voltage changes. For example, the potential of graphite is about 0.1V (vs Li / Li + ) Therefore, the charge / discharge voltage is about 0.1 V lower in the case of a graphite anode than in the case of a lithium counter electrode. In this specification, even if the charging voltage of the secondary battery is, for example, 4.7 V or higher, The plateau region of the discharge voltage does not need to be 4.7V or higher.
[0034] (Embodiment 1) In this embodiment, a method for producing a positive electrode active material according to one embodiment of the present invention will be described. do.
[0035] <<Method 1 for preparing positive electrode active material>> <Step S11> In step S11 shown in FIG. 1(A), lithium and transition metal materials as starting materials are Then, a lithium source (Li source) and a transition metal M source (M source) are prepared.
[0036] As the lithium source, it is preferable to use a compound containing lithium, for example, lithium carbonate. Lithium hydroxide, lithium nitrate, lithium fluoride, etc. can be used. The hydrogen source preferably has a high purity, for example, a material with a purity of 99.99% or more.
[0037] The transition metal M can be selected from the elements in groups 4 to 13 of the periodic table, e.g. For example, at least one of manganese, cobalt, and nickel is used. When only cobalt is used, when only nickel is used, and when cobalt and manganese are used, When using two types of cobalt and nickel, or when using cobalt and manganese In some cases, three types of cobalt are used: nickel and cobalt. When only cobalt is used, the resulting positive electrode active material It has lithium cobalt oxide (LCO) and uses three types of cobalt, manganese, and nickel. In this case, the resulting positive electrode active material is nickel-cobalt-manganese oxide (NCM). Yes.
[0038] As the source of the transition metal M, it is preferable to use a compound having the above-mentioned transition metal M. For example, The transition metal M may be an oxide of the metal exemplified above or a hydroxide of the metal exemplified above. As the cobalt source, cobalt oxide, cobalt hydroxide, etc. can be used. As the manganese source, manganese oxide, manganese hydroxide, etc. can be used. Nickel As the source of aluminum, nickel oxide, nickel hydroxide, etc. can be used. If available, aluminum oxide, aluminum hydroxide, etc. can be used.
[0039] The transition metal M source is preferably of high purity, for example, 3N (99.9%) or higher, preferably More preferably, the content is 4N (99.99%) or more, more preferably 4N5 (99.995%) or more, and even more preferably It is preferable to use materials with a purity of 5N (99.999%) or higher. Use high purity materials. As a result, the capacity of the secondary battery is increased, and the amount of impurities in the positive electrode active material can be controlled. And / or the reliability of the secondary battery is improved.
[0040] In addition, the transition metal source preferably has high crystallinity, for example, single crystal grains. The crystallinity of the metal source was evaluated using TEM (transmission electron microscope) images and STEM (scanning transmission electron microscope) images. High-angle annular dark-field scanning transmission electron microscope (HAADF-STEM) image, ABF -Evaluation using STEM (annular bright-field scanning transmission electron microscope) images, etc., or X-ray diffraction (XRD ), electron diffraction, neutron diffraction, etc. can be applied to the evaluation of crystallinity of not only transition metal sources but also other sources.
[0041] In addition, when two or more transition metal sources are used, the two or more transition metal sources are preferably arranged in a layered rock salt type crystal structure. It is preferable to prepare them in a ratio (mixture ratio) that allows for the desired structure.
[0042] <Step S12> Next, in step S12 shown in FIG. 1(A), the lithium source and the transition metal source are crushed and mixed. The mixture is mixed to produce a mixed material. The grinding and mixing can be carried out in a dry or wet manner. The wet method is preferable because it can be crushed into smaller pieces. If the wet method is used, a solvent must be prepared. Solvents include ketones such as acetone, alcohols such as ethanol and isopropanol, Ether, dioxane, acetonitrile, N-methyl-2-pyrrolidone (NMP), etc. It is better to use an aprotic solvent that does not react easily with lithium. In the present embodiment, dehydrated acetone with a purity of 99.5% or more is used. The water content is reduced to 10 ppm or less, and the purity is 99.5% or more. It is preferable to mix the lithium source and the transition metal source, and then grind and mix them. By using dehydrated acetone at a high temperature, it is possible to reduce impurities that may be present.
[0043] A ball mill, a bead mill, or the like can be used as a means for pulverizing and mixing. When using a mill, use aluminum oxide balls or zirconium oxide balls as grinding media. It is recommended to use balls. Zirconium oxide balls are preferable because they emit less impurities. When using a ball mill or bead mill, contamination from the media must be avoided. In order to suppress this, the peripheral speed is preferably set to 100 mm / s or more and 2000 mm / s or less. In this embodiment, the peripheral speed is 838 mm / s (rotation speed 400 rpm, ball mill diameter 40 mm). This will be implemented as follows.
[0044] <Step S13> Next, in step S13 shown in FIG. 1(A), the mixed material is heated. It is preferable to carry out the treatment at a temperature between 0°C and 1100°C, and more preferably between 900°C and 1000°C. If the temperature is too low, the lithium source and the transition metal If the temperature is too high, the decomposition and melting of the transition metal source may be insufficient. Lithium evaporation from the source and / or excessive reduction of the metal used as the transition metal source Such defects may occur due to, for example, transition When cobalt is used as a transition metal, excessive reduction causes cobalt to change from trivalent to divalent. This can lead to oxygen defects and other problems.
[0045] The heating time should be between 1 and 100 hours, and between 2 and 20 hours. is more preferred.
[0046] The rate of temperature rise depends on the heating temperature to be reached, but is preferably 80° C. / h or more and 250° C. / h or less. For example, when heating at 1000°C for 10 hours, the temperature rise rate should be 200°C / h.
[0047] Heating is preferably performed in an atmosphere with little moisture, such as dry air. For example, the dew point is -50°C or lower. Preferably, the dew point is -80° C. or less. Heating is performed in an atmosphere of -93℃. In addition, to suppress impurities that may be mixed into the material, In order to achieve this, the impurity concentrations of CH4, CO, CO2, and H2 in the heating atmosphere must be It is recommended that each be kept below 5 ppb (parts per billion).
[0048] The heating atmosphere is preferably an atmosphere containing oxygen. For example, dry air is continuously introduced into the reaction chamber. In this case, the flow rate of the dry air is preferably 10 L / min. Oxygen is continuously introduced into the reaction chamber, and the manner in which oxygen flows through the reaction chamber is called flow.
[0049] When the heating atmosphere is an atmosphere containing oxygen, a method without flow may be used. For example, The reaction chamber is depressurized and then filled with oxygen (or purged). It is also possible to use a method that prevents the air from leaving the chamber or from entering from the outside. The pressure can be reduced to -970hPa and then oxygen can be added to 50hPa.
[0050] After heating, the product may be cooled naturally, but the time required for the product to cool from the specified temperature to room temperature must be 10 hours or more or 50 minutes or more. However, cooling to room temperature is not necessarily required, and the next step It is sufficient to cool the material to a temperature that is acceptable to the apparatus.
[0051] The heating in this step may be performed using a rotary kiln or a roller hearth kiln. Heating with a rotary kiln involves stirring the material whether it is a continuous or batch type. It is possible.
[0052] The sheath (which can also be called a container or crucible) used during heating is preferably made of aluminum oxide. The aluminum oxide sheath is a material that is free of impurities. For heating, use a 99.9% pure aluminum oxide sheath. The sheath is covered with a lid. This is preferable because it can prevent the material from volatilizing.
[0053] After the heating is completed, the material may be crushed and sieved as necessary. When recovering the material, it may be transferred from the crucible to a mortar and then recovered. It is preferable to use an aluminum oxide mortar. Aluminum oxide mortars are prone to impurities. Specifically, it is a material with a purity of 90% or more, preferably an oxide with a purity of 99% or more. An aluminum mortar is used. Note that in the heating process other than step S13, which will be described later, , heating conditions equivalent to those in step S13 can be applied.
[0054] <Step S14> Through the above steps, a composite oxide having a transition metal (L The composite oxide can be obtained by using the lithium composite oxide represented by LiMO2. It is sufficient that the crystal structure of the material is Li:M:O=1:1:2. When cobalt is used as the transition metal, it is called a composite oxide containing cobalt. It is expressed as LiCoO2. The composition is strictly limited to Li:Co:O=1:1:2. It is not something that is done.
[0055] An example of producing a composite oxide by a solid phase method as shown in steps S11 to S14 has been shown. Alternatively, the composite oxide may be prepared by a coprecipitation method or a hydrothermal method.
[0056] <Step S15> Next, in step S15 shown in FIG. 1(A), the composite oxide is heated. Since this is the first heating for the substrate, the heating in step S15 is sometimes called the initial heating. When heated, the surface of the composite oxide becomes smooth. A smooth surface means that there are few irregularities. This refers to the state in which the composite oxide is generally rounded, with the corners also rounded. A state in which there is little foreign matter adhering to the surface is called smooth. Foreign matter is thought to be the cause of unevenness on the surface. It is preferable that it does not adhere to the surface.
[0057] The initial heating is carried out after the composite oxide is completed. They performed initial heating to smooth the surface, reducing deterioration after charging and discharging. In the initial heating step to smooth the surface, the lithium compound You don’t need to prepare a resource.
[0058] Alternatively, in the initial heating step to smooth the surface, no additional element source is required. stomach.
[0059] Or, in the initial heating process to smooth the surface, no flux is required. good.
[0060] The initial heating is heating before step S20 described below, and is called preheating or pretreatment. It is sometimes called.
[0061] The lithium source and / or the transition metal source prepared in step S11, etc. may contain impurities. In step S14, impurities may be reduced from the completed composite oxide. , this is possible by initial heating.
[0062] The heating conditions in this step may be any conditions that make the surface of the composite oxide smooth. For example, The heating conditions can be selected from those described in step S13. In addition, the heating temperature in this process is set at a temperature of 100° C. to maintain the crystal structure of the composite oxide. The heating time in this step is preferably set lower than that in step S13. In order to maintain the temperature, the time should be shorter than that of step S13. It is recommended to heat the mixture at a temperature of 0.5 °C or less for at least 2 hours.
[0063] The composite oxide is heated in step S13 to generate a temperature difference between the surface and the inside of the composite oxide. Temperature differences can induce differential shrinkage. It is also thought that the difference in fluidity between the surface and the interior of the concrete causes the difference in shrinkage. The difference in internal stress is also called strain, and the The energy is sometimes called strain energy. The internal stress is generated during the initial heating step S15. In other words, the strain energy is homogenized by the initial heating in step S15. It is believed that the homogenization of the strain energy reduces the strain in the composite oxide. Therefore, there is a possibility that the surface of the composite oxide becomes smooth after step S15. In other words, after step S15, the shrinkage difference in the composite oxide is improved. It is believed that this reduces the stress on the surface of the composite oxide, making it smoother.
[0064] Furthermore, the difference in shrinkage can cause microscopic deviations in the composite oxide, such as deviations in crystal structure. In order to reduce the deviation, it is advisable to carry out this step. When the displacement is uniformed, the surface of the complex oxide becomes It is also said that the grain alignment has been achieved. In other words, the After passing through step S15, the crystal displacement in the composite oxide is alleviated, and the surface of the composite oxide becomes It is thought to be smoother.
[0065] When a composite oxide with a smooth surface is used as a positive electrode active material, This reduces deterioration of the positive electrode active material and prevents cracking of the positive electrode active material.
[0066] The smooth surface of the complex oxide is determined by measuring the surface roughness of a cross section of the complex oxide. When quantified based on the measurement data, it can be said to have a surface roughness of 10 nm or less. One cross section is, for example, a cross section obtained when observing with a scanning transmission electron microscope (STEM). .
[0067] In step S14, a mixture of lithium, a transition metal, and oxygen is synthesized in advance. A composite oxide may be used. In this case, steps S11 to S13 may be omitted. By carrying out step S15 on a composite oxide that has been synthesized in advance, As a result, a composite oxide with a smooth surface can be obtained.
[0068] It is possible that the lithium in the composite oxide is reduced by the initial heating. The reduced amount of lithium may make it easier for the additive elements to enter the composite oxide. There is.
[0069] <Step S20> Adding an additive element X to a complex oxide with a smooth surface within the range where a layered rock salt type crystal structure can be formed. If an additive element X is added to a composite oxide with a smooth surface, the additive element is evenly distributed. Therefore, it is preferable to add the additive element after the initial heating. The step of adding the element will be described with reference to FIG. 1(B) and FIG. 1(C).
[0070] <Step S21> In step S21 shown in FIG. 1(B), a source of an additive element to be added to the composite oxide is prepared. A lithium source may be provided in conjunction with the additive source.
[0071] The added elements are nickel, cobalt, magnesium, calcium, chlorine, fluorine, and aluminium. Aluminum, manganese, titanium, zirconium, yttrium, vanadium, iron, chromium , niobium, lanthanum, hafnium, zinc, silicon, sulfur, phosphorus, boron, and arsenic The additive element may be selected from one or more of the following: bromine, borane, and tetrabromine. However, bromine, beryllium, and As for ammonium nitrate, since it is an element that is toxic to living organisms, it is better to use the additive elements mentioned above. is preferred.
[0072] When magnesium is selected as the additive element, the additive element source can be called a magnesium source. The magnesium source may be magnesium fluoride, magnesium oxide, magnesium hydroxide, etc. The magnesium source may be sodium or magnesium carbonate. Multiple use is also possible.
[0073] When fluorine is selected as the additive element, the source of the additive element can be called a fluorine source. The sources include, for example, lithium fluoride (LiF), magnesium fluoride (MgF2), fluorine Aluminum fluoride (AlF3), titanium fluoride (TiF4), cobalt fluoride (CoF2, CoF3), Nickel Fluoride (NiF2), Zirconium Fluoride (ZrF4), Ba Fluoride Nadium (VF5), manganese fluoride, iron fluoride, chromium fluoride, niobium fluoride, fluoride Zinc (ZnF2), calcium fluoride (CaF2), sodium fluoride (NaF), fluoride Potassium fluoride (KF), barium fluoride (BaF2), cerium fluoride (CeF3, CeF 4), lanthanum fluoride (LaF3), or sodium aluminum hexafluoride (Na3Al F6) can be used. Among them, lithium fluoride has a relatively low melting point of 848°C. This is preferable because it is easy to melt in the heating step described below.
[0074] Magnesium fluoride can be used as both a fluorine source and a magnesium source. The lithium fluoride used in step S21 can also be used as a lithium source. Another possible source of lithium is lithium carbonate.
[0075] The fluorine source may also be a gas, such as fluorine (F2), fluorocarbon, sulfur fluoride, or fluoroacid. Using elements (OF2, O2F2, O3F2, O4F2, O5F2, O6F2, O2F), etc. The fluorine sources may be mixed in the atmosphere during the heating step described below. It's fine.
[0076] In this embodiment, lithium fluoride (LiF) is prepared as the fluorine source. Prepare magnesium fluoride (MgF2) as a magnesium source. Magnesium oxide, when mixed with LiF:MgF2=65:35 (molar ratio), has a lower melting point. On the other hand, if the amount of lithium fluoride is too high, the lithium becomes excessive. Therefore, lithium fluoride and magnesium fluoride are The molar ratio of LiF:MgF2 is preferably LiF:MgF2=x:1 (0≦x≦1.9), and Li F:MgF2=x:1 (0.1≦x≦0.5) is more preferable, and LiF:MgF2=x: 1 (x=near 0.33) is more preferable. In this specification, the term "near" refers to the value. The value must be greater than 0.9 and less than 1.1.
[0077] At the same time, the amount of magnesium added exceeds 0.1 atomic percent based on LiCoO2, and the three elements are % or less, more preferably 0.5 atomic % or more and 2 atomic % or less, and more preferably 0.5 atomic % or more. It is more preferable that the amount of magnesium added is 1 atomic % or less. Although the discharge capacity is high, repeated charging and discharging at a high depth of charge can cause rapid discharge. The capacity decreases. If the amount of magnesium added is more than 0.1 atomic % and is less than 3 atomic %, Even if the charge / discharge cycle is repeated to increase the depth of charge, the initial discharge characteristics and charge / discharge cycle characteristics On the other hand, when the amount of magnesium added exceeds 3 atomic %, the initial discharge capacity and charge capacity decrease. The discharge cycle characteristics also tend to deteriorate gradually.
[0078] <Step S22> Next, in step S22 shown in FIG. 1(B), the magnesium source and the fluorine source are crushed and mixed. This step is carried out under the conditions selected from the grinding and mixing conditions described in step S12. It is possible.
[0079] If necessary, a heating step may be performed after step S22. The heating conditions can be selected from those described in the above. The heating time is preferably 2 hours or more. The heating temperature is preferably 800° C. or higher and 1100° C. or lower.
[0080] <Step S23> Next, in step S23 shown in FIG. 1(B), the crushed and mixed materials are collected and added. The additive element source shown in step S23 can be obtained from a plurality of sources. and can be referred to as a mixture.
[0081] The particle size of the above mixture is D50 (median diameter) of 600 nm or more and 20 μm or less. The thickness is preferably 1 μm or more and more preferably 10 μm or less. Even when various materials are used, the D50 (median diameter) is 600 nm or more and 20 μm or less. It is preferable that the thickness is 1 μm or less, and more preferable that the thickness is 1 μm or more and 10 μm or less.
[0082] Such a finely powdered mixture (including the case where only one type of added element is added) can be mixed in the subsequent process. When mixed with the composite oxide, the mixture can be easily adhered uniformly to the surfaces of the composite oxide particles. If the mixture is uniformly attached to the surface of the composite oxide particles, the surface layer of the composite oxide will This is preferable because it is easy to distribute or diffuse fluorine and magnesium uniformly in the The area where magnesium is distributed can be called the surface layer. If there is an area that does not contain the crystalline structure, the O3'-type and O3"-type crystal structures described later will be formed in the charged state. Although fluorine was used in the explanation, chlorine may be used instead of fluorine. These can be read as including halogen.
[0083] <Step S21> A process different from that shown in FIG. 1(B) will be described with reference to FIG. 1(C). In step S21, four kinds of additive element sources to be added to the composite oxide are prepared. The type of additive element source is different from that in Figure 1(B). A lithium source is prepared in addition to the additive element source. You may do so.
[0084] The four additive element sources were magnesium source (Mg source), fluorine source (F source), nickel source ( Ni source, and aluminum source (Al source). The nickel source can be selected from the compounds described in FIG. 1(B). The aluminum source may be nickel oxide, nickel hydroxide, or the like. Aluminum, aluminum hydroxide, etc. can be used.
[0085] <Steps S22 and S23> Steps S22 and S23 shown in FIG. 1C are the same as steps S22 and S23 described in FIG. 1B. is the same as:
[0086] <Step S31> Next, in step S31 shown in FIG. 1(A), the composite oxide and an additive element source (X source) are mixed. The number of transition metal atoms in the composite oxide containing lithium, transition metal, and oxygen, M, and X The ratio of the number of magnesium atoms in the source to the number of magnesium atoms in the source is M:Mg=100:y (0.1≦y≦6 ), and more preferably M:Mg=100:y (0.3≦y≦3). I wish.
[0087] The mixing in step S31 is carried out in a manner similar to that in step S12 in order not to destroy the composite oxide particles. For example, the rotation speed is set to be milder than that of the mixing in step S12. It is preferable to use conditions with less heat or shorter time. Also, a dry method is gentler than a wet method. For mixing, a ball mill, a bead mill, etc. can be used. When using a ball mill, for example, zirconium oxide balls are used as the media. It is preferable that
[0088] In this embodiment, a ball mill using zirconium oxide balls with a diameter of 1 mm is used. The mixture is mixed at 100°C for 1 hour at 350°C for 1 hour. This will be done in a dry room below 0℃.
[0089] <Step S32> Next, in step S32 of FIG. 1(A), the mixed materials are collected and mixed 90 3 is obtained. When recovering, crushing and sieving may be carried out as necessary.
[0090] In this embodiment, lithium fluoride is used as the fluorine source and fluorine is used as the magnesium source. We will explain how to add magnesium fluoride to a composite oxide that has been initially heated. However, the present invention is not limited to the above method. At the stage of the starting material of the composite oxide, the magnesium source and the fluorine source are added to the lithium source and the transition metal source. Then, in step S13, the magnesium and fluorine are added to the metal source by heating. In this case, steps S11 to S14 are carried out. There is no need to separate the process of S14 from the process of steps S21 to S23. It can be said that this is a highly productive method.
[0091] Alternatively, lithium cobalt oxide to which magnesium and fluorine have been added may be used. If lithium cobalt oxide doped with magnesium and fluorine is used, step S1 The steps S1 to S32 and S20 can be omitted. It can be said that this is a highly reliable method.
[0092] Or, for lithium cobalt oxide to which magnesium and fluorine have been added in advance, In step S20, a magnesium source and a fluorine source, or a magnesium source and a fluorine source are further A source of Cr, a source of nickel, and a source of aluminum may also be added.
[0093] <Step S33> Next, in step S33 shown in FIG. 1(A), the mixture 903 is heated. The heating conditions can be selected from those described in the above. The heating time is preferably 2 hours or more. stomach.
[0094] Here, a supplementary note about the heating temperature will be provided. The lower limit of the heating temperature in step S33 is the temperature at which the composite oxide (L The temperature must be higher than the temperature at which the reaction between iMO2) and the added element source proceeds. The temperature may be any temperature at which mutual diffusion of elements contained in LiMO2 and the additive element source occurs. The melting temperature T m 0 .757 times (Tamman temperature T d ) solid-phase diffusion occurs. The heating temperature in step S33 may be 500° C. or higher.
[0095] Of course, if the temperature is equal to or higher than the temperature at which at least a part of the mixture 903 melts, the reaction will proceed more easily. For example, when LiF and MgF2 are used as additive element sources, Since the eutectic point is around 742°C, the lower limit of the heating temperature in step S33 is set to 742°C or higher. It is preferable to do so.
[0096] In addition, the molar ratio of LiCoO2:LiF:MgF2 was 100:0.33:1. The mixture 903 obtained by mixing had a temperature of 830°C in differential scanning calorimetry (DSC). Therefore, the lower limit of the heating temperature is more preferably 830° C. or higher.
[0097] A higher heating temperature is preferable because the reaction proceeds more easily, the heating time is shorter, and the productivity is high.
[0098] The upper limit of the heating temperature is below the decomposition temperature of LiMO2 (the decomposition temperature of LiCoO2 is 1130℃). At temperatures close to the decomposition temperature, there is concern that LiMO2 may decompose, although only in small amounts. Therefore, it is more preferable that the temperature is 1000°C or lower, and even more preferable that the temperature is 950°C or lower. It is more preferable that the temperature is 00°C or lower.
[0099] Considering these, the heating temperature in step S33 is 500°C or higher, 1130°C or higher. ° C. or less, more preferably 500° C. to 1000° C. or less, and still more preferably 500° C. to 950° C. More preferably, the temperature is 500°C or higher and 900°C or lower. The temperature is preferably 1130°C or lower, more preferably 742°C or higher and 1000°C or lower, and more preferably 742°C or higher and 1000°C or lower. The temperature is preferably from 742°C to 900°C, more preferably from 742°C to 900°C. 800°C or more and 1100°C or less, 830°C or more and 1130°C or less are preferable, and 830°C or more and 1 000°C or less is more preferable, 830°C to 950°C or less is even more preferable, and 830°C or less is The heating temperature in step S33 is preferably 900° C. or less. Higher than 13 is good.
[0100] Furthermore, when the mixture 903 is heated, the partial pressure of fluorine or fluoride originating from the fluorine source, etc. It is preferable to control it within an appropriate range.
[0101] In the manufacturing method described in this embodiment, some materials, for example, LiF, which is a fluorine source, are used as a flux. This function can increase the heating temperature to the decomposition of the complex oxide (LiMO2). The temperature can be lowered to below 742℃ or higher and 950℃ or lower, and magnesium can be added to the surface layer. By distributing additive elements such as ZnO, a positive electrode active material with excellent characteristics can be produced.
[0102] However, LiF has a lower specific gravity in gaseous state than oxygen, so LiF volatilizes when heated. If it volatilizes, the LiF in mixture 903 will decrease. Therefore, it is necessary to heat the LiF while suppressing its volatilization. Even if LiF is not used as a fluorine source, the Li and fluorine on the LiMO2 surface can be The F in the source may react to produce LiF, which may then volatilize. Even with higher fluoride content, volatilization control is still necessary.
[0103] Therefore, the mixture 903 is heated in an atmosphere containing LiF, that is, the Li It is preferable to heat the mixture 903 under a high partial pressure of F. The volatilization of LiF in the mixture 903 can be suppressed.
[0104] The heating in this step is preferably performed so that the particles of the mixture 903 do not stick to each other. When the particles of the mixture 903 adhere to each other during the addition, the contact area with the oxygen in the atmosphere decreases. By blocking the route for diffusion of added elements (e.g. fluorine), added elements (e.g. The distribution of minerals (e.g. magnesium and fluorine) may be compromised.
[0105] In addition, if the additive element (e.g. fluorine) is uniformly distributed in the surface layer, the surface becomes smooth and has few irregularities. It is believed that the electrode active material can be obtained. Therefore, in this process, the heating in step S15 is performed. In order for the surface to remain smooth or to become even smoother, the particles must adhere to each other. It's better not to.
[0106] In addition, when heating using a rotary kiln, the flow rate of the oxygen-containing atmosphere in the kiln is It is preferable to heat the mixture in a controlled manner. For example, the flow rate of the oxygen-containing atmosphere is reduced. It is preferable to purge the atmosphere and not allow the atmosphere to flow after introducing the oxygen atmosphere into the kiln. Flowing oxygen may evaporate the fluorine source, which may cause the surface to become smooth. This is not desirable for this purpose.
[0107] When heating by a roller hearth kiln, for example, the container containing the mixture 903 is covered with a lid. By disposing the LiF in the atmosphere, the mixture 903 can be heated in an atmosphere containing LiF.
[0108] Regarding the heating time, the heating time depends on the heating temperature and the amount of LiMO2 particles in step S14. It varies depending on the size and composition of the particles. When the particles are small, the A lower temperature or shorter time may be more preferable.
[0109] The median diameter (D50) of the composite oxide (LiMO2) in step S14 of FIG. 1(A) is 1 In the case of about 2 μm, the heating temperature is preferably, for example, 600° C. or more and 950° C. or less. Heating time For example, the time is preferably 3 hours or more, more preferably 10 hours or more, and even more preferably 60 hours or more. The cooling time after heating is preferably, for example, 10 hours or more and 50 hours or less. It is.
[0110] On the other hand, the median diameter (D50) of the composite oxide (LiMO2) in step S14 is about 5 μm. In the case of 100° C., the heating temperature is preferably, for example, 600° C. or more and 950° C. or less. The heating time is, for example, 1 The temperature drop time after heating is preferably from 10 hours to 10 hours, and more preferably about 2 hours. It is preferable that the time is, for example, 10 hours or more and 50 hours or less.
[0111] <Step S34> Next, in step S34 shown in FIG. 1(A), the heated material is collected and crushed as necessary. The positive electrode active material 100 is obtained by further sieving the collected particles. By the above steps, the positive electrode active material 100 according to one embodiment of the present invention can be produced. The positive electrode active material of one embodiment of the present invention has a smooth surface.
[0112] <<Preparation method 2 of positive electrode active material>> Next, a method for carrying out the present invention, which is different from the method 1 for preparing a positive electrode active material, will be described. He explains.
[0113] In FIG. 2, steps S11 to S15 are carried out in the same manner as in FIG. 1(A), and the surface is smoothed. A complex oxide (LiMO2) is prepared.
[0114] <Step S20a> It is acceptable to add an additive element X to a composite oxide as long as the layered rock salt type crystal structure can be formed. As described above, in the present production method 2, the additive element is added in two or more steps. This will be described with reference to FIG.
[0115] <Step S21> In step S21 shown in FIG. 3A, a first additive element source is prepared. The additive element X is selected from the additive elements X described in step S21 shown in FIG. For example, the additive element X1 can be magnesium, fluorine, or calcium. One or more of the following can be suitably used. When a magnesium source (Mg source) and a fluorine source (F source) are used as the additive element X1, For example:
[0116] Steps S21 to S23 shown in FIG. 3A are the same as those shown in FIG. 1B. Steps S21 to S23 can be performed under the same conditions. 23 can provide an additive element source (X1 source).
[0117] In addition, steps S31 to S33 shown in FIG. 2 are the same as step S3 shown in FIG. This can be done in the same manner as steps S1 to S33.
[0118] <Step S34a> Next, in step S33, the heated material is recovered to produce a composite oxide having the additive element X1. To distinguish it from the composite oxide in step S14, it is also called a second composite oxide.
[0119] <Step S40> In step S40 shown in FIG. 2, a second additive element source is added. ) will also be referred to for explanation.
[0120] <Step S41> In step S41 shown in FIG. 3B, a second additive element source is prepared. The additive element X is selected from the additive elements X described in step S21 shown in FIG. For example, the additive element X2 can be nickel, titanium, boron, zirconium, One or more selected from the group consisting of aluminum and aluminum can be preferably used. In FIG. 3(B), nickel and aluminum are used as the additive element X2. For example:
[0121] Steps S41 to S43 shown in FIG. 3B are the same as those shown in FIG. Steps S21 to S23 can be performed under the same conditions. At 43 you can get an additive element source (X2 source).
[0122] FIG. 3(C) shows a modified example of the step described with reference to FIG. 3(B). In step S41 shown in FIG. 1, a nickel source (Ni source) and an aluminum source (Al source) are prepared. In step S42a, each of the particles is crushed independently. As a result, in step S43, A plurality of second additive element sources (X2 sources) are prepared. The step of FIG. 3(C) is The difference from FIG. 3(B) is that the additive elements are milled independently in step S42a.
[0123] <Steps S51 to S53> Next, steps S51 to S53 shown in FIG. 2 are the same as step S3 shown in FIG. The heating step S can be performed under the same conditions as steps S1 to S34. The conditions for step S53 may be lower temperature and shorter time than those for step S33. In step S54, the positive electrode active material 100 according to one embodiment of the present invention can be produced. In one embodiment, the positive electrode active material has a smooth surface.
[0124] As shown in FIG. 2 and FIG. 3, in the preparation method 2, the additive element to the composite oxide is the additive element X1. , and additional element X2 are introduced separately. By introducing them separately, the depth direction of each additional element is For example, the additive element X1 can be made higher in the surface layer than in the interior. The concentration of the additive element X2 is higher in the inner part than in the surface layer. It is also possible to profile the
[0125] By undergoing the initial heating described in this embodiment, a positive electrode active material with a smooth surface can be obtained. .
[0126] The initial heating shown in this embodiment is performed on the composite oxide. The heating temperature is lower than that for obtaining the composite oxide, and the heating time is shorter than that for obtaining the composite oxide. When adding an additive element to a composite oxide, the addition process is performed after the initial heating. It is preferable to carry out the addition step. The addition step can be divided into two or more steps. This procedure is preferred because it maintains the surface smoothness achieved by the initial heating. When a compound has cobalt as a transition metal, it is deemed to be a composite oxide having cobalt. It is possible.
[0127] This embodiment mode can be used in combination with other embodiment modes.
[0128] (Embodiment 2) In this embodiment, a positive electrode active material of one embodiment of the present invention will be described with reference to FIGS. do.
[0129] FIG. 4A is a cross-sectional view of a positive electrode active material 100 according to one embodiment of the present invention. Enlarged views of the area around -B are shown in Fig. 4(B1) and Fig. 4(B2). Enlarged views of the vicinity are shown in Figure 4(C1) and Figure 4(C2).
[0130] As shown in FIG. 4(A) to FIG. 4(C2), the positive electrode active material 100 has a surface layer 100a and an inner layer 100b. In these figures, the boundary between the surface layer 100a and the inner portion 100b is indicated by a dashed line. In addition, part of the grain boundary 101 is shown by a dashed line in FIG.
[0131] In this specification, the region from the surface of the positive electrode active material to the inside of the material having a length of 10 nm is referred to as the surface layer. The surface layer 100a is called the surface. The surface caused by the cracks can also be called the surface. The surface layer 1 of the positive electrode active material may be called the surface-nearby region or the surface-nearby region or the shell. The area deeper than 100a is called the inner area 100b. The inner area 100b is also called the inner area or the core. It can be said that.
[0132] It is preferable that the surface layer 100a has a higher concentration of an additive element, which will be described later, than the inner portion 100b. It is preferable that the added element has a concentration gradient. In addition, when there are multiple added elements, It is preferable that the depth from the surface of the concentration peak differs depending on the added element.
[0133] For example, an added element X is shown in the gradation in Fig. 4(B1), from the inner 100b It is preferable that the concentration gradient increases from the surface to the surface. The additive element X is preferably, for example, magnesium, fluorine, titanium, silicon, lithium, etc. Examples of such elements include arsenic, boron and calcium.
[0134] Another additive element Y has a concentration gradient as shown by the gradation in FIG. 4(B2) and is an additive. It is preferable that the concentration peak is located in a region deeper than that of the element X. It may be present in the surface layer 100a or may be deeper than the surface layer 100a. It is preferable that the concentration peak is 5 nm or more from the surface to the inside. It is preferable that the concentration gradient has a peak in the region of 0.1 nm or less. Preferred examples of the additional element Y include aluminum and manganese.
[0135] In addition, due to the above-mentioned concentration gradient of the added element, the crystal grains are formed from the inside 100b toward the surface. It is preferable that the crystal structure changes continuously.
[0136] <Contained elements> The positive electrode active material 100 contains lithium, a transition metal M, oxygen, and an additive element. Although active material 100 is a composite oxide represented by LiMO2 to which additive elements have been added, However, the positive electrode active material of one embodiment of the present invention is a lithium composite oxide represented by LiMO2. It is sufficient to have a crystal structure, and the composition is strictly limited to Li:M:O=1:1:2. In addition, positive electrode active materials to which an additive element is added are also sometimes called composite oxides.
[0137] The transition metal M contained in the positive electrode active material 100 belongs to the space group R-3m together with lithium. It is preferable to use a metal capable of forming a layered rock salt type composite oxide. At least one of gallium, cobalt, and nickel can be used. The transition metal M in 100 may be cobalt alone or nickel alone. Alternatively, two types of metals, cobalt and manganese, or cobalt and nickel, may be used. Alternatively, three types of metals, cobalt, manganese, and nickel, may be used. Lithium cobalt oxide, lithium nickel oxide, and cobalt oxide in which some of the cobalt is replaced by manganese Lithium cobaltate, lithium cobalt oxide in which some of the cobalt is replaced by nickel, nickel -Having a composite oxide containing lithium and a transition metal M, such as lithium manganese-cobalt oxide The layered rock-salt complex oxide has two-dimensional diffusion paths for lithium ions. It is suitable for lithium ion insertion / extraction reactions.
[0138] In particular, the positive electrode active material 100 contains 75 atomic % or more of cobalt as the transition metal M, preferably When 90 atomic % or more, more preferably 95 atomic % or more is used, the synthesis is relatively easy and easy to handle. It has many advantages, such as being easy to use and having excellent cycle characteristics. When nickel is added to the surrounding cobalt, the layered structure of cobalt and oxygen octahedra is formed. Therefore, the crystal structure becomes more stable, especially in the charged state at high temperatures. This is preferable because it may result in a fixed
[0139] The transition metal M does not necessarily have to contain manganese. By using a positive electrode active material that does not contain any cations, the synthesis is relatively easy, it is easy to handle, and it has excellent cycling properties. In some cases, the above-mentioned advantages, such as the ability to provide a high-temperature characteristic, may become even greater. The weight of manganese contained is, for example, 600 ppm or less, more preferably 100 ppm or less. It is preferable that there is.
[0140] On the other hand, the transition metal M contained in the positive electrode active material 100 is nickel at 33 atomic % or more, preferably When 60 atomic % or more, more preferably 80 atomic % or more of cobalt is used, the The raw materials may be cheaper than conventional batteries, and the charge / discharge capacity per weight may be increased. preferable.
[0141] The transition metal M does not necessarily have to include nickel.
[0142] The additive elements contained in the positive electrode active material 100 include magnesium, fluorine, aluminum, and titanium. Titanium, zirconium, vanadium, iron, chromium, niobium, cobalt, arsenic, zinc, silicon It is preferable to use at least one of the additive elements, sulfur, phosphorus, and boron. As described later, this may further stabilize the crystal structure of the positive electrode active material 100. The positive electrode active material 100 is lithium cobalt oxide doped with magnesium and fluorine. Lithium cobalt oxide doped with magnesium, fluorine and titanium, magnesium and Lithium nickel-cobalt oxide doped with magnesium and fluorine, Lithium cobalt aluminate, lithium nickel cobalt aluminate Lithium-, magnesium-, and fluorine-doped nickel-cobalt-aluminate Lithium-, magnesium- and fluorine-doped nickel-manganese-cobalt oxide, etc. In this specification, the additive element may be a mixture, a part of a raw material, an impurity, etc. It can also be called an element.
[0143] The additive elements do not necessarily include magnesium, fluorine, aluminum, titanium, zirconium, etc. Aluminum, vanadium, iron, chromium, niobium, cobalt, arsenic, zinc, silicon, sulfur, phosphorus, or may not contain boron.
[0144] In the positive electrode active material 100 of one embodiment of the present invention, lithium is extracted from the positive electrode active material 100 upon charging. The concentration of the added element is adjusted so that the layered structure consisting of the transition metal M and oxygen octahedra is not destroyed even when the The high surface layer 100a, that is, the outer periphery of the particle, is reinforced.
[0145] In addition, the concentration gradient of the added element is similar throughout the entire surface layer 100a of the positive electrode active material 100. It is preferable that the reinforcement resulting from the high concentration of the additive element is uniform in the surface layer portion 100a. Even if a part of the surface layer portion 100a is reinforced, If there are weak areas, stress may be concentrated in those areas. When they become concentrated, defects such as cracks can form, causing the positive electrode active material to break and reducing the charge / discharge capacity. There is a risk of it leading down.
[0146] In this specification, homogeneity refers to a solid consisting of multiple elements (e.g., A, B, C). This refers to the phenomenon in which a certain element (e.g. A) is distributed with similar characteristics in a specific area. It is sufficient that the concentrations of elements in the specific regions are substantially the same. The difference in concentration should be within 10%. Examples of specific regions include the surface layer, the surface, the convex portion, Examples include recesses, interiors, etc.
[0147] However, it is not necessarily the case that the additive element is uniformly distributed throughout the entire surface layer 100a of the positive electrode active material 100. It is not necessary to have a concentration gradient. For example, the distribution of the added element X near CD in FIG. An example of the distribution of the added element Y near the CD is shown in FIG. 4(C1) and an example of the distribution of the added element Y near the CD is shown in FIG. 4(C2).
[0148] Here, the CD area has a layered rock-salt type crystal structure of R-3m, and the surface has a (001) orientation. The (001) oriented surface has a different distribution of added elements from the other surfaces. For example, the (001) oriented surface and its surface layer 100a may be formed by adding an additional element X and At least one of the distributions of the added element Y is shallower from the surface than the surface other than the (001) orientation. Alternatively, the (001) oriented surface and its surface layer 100a may remain in the (001) oriented portion. is at least one of the added element X and the added element Y compared to a surface other than the (001) orientation. Alternatively, the (001) oriented surface and its surface layer 100a may have a low concentration of dopant. The concentration of at least one of the element X and the added element Y may be below the lower detection limit.
[0149] In the layered rock-salt crystal structure of R-3m, cations are arranged parallel to the (001) plane. This is a MO2 layer consisting of a transition metal M and an oxygen octahedron, a lithium layer, and a (001) surface. It can be said that the structure is made up of parallel layers stacked alternately. The paths also lie parallel to the (001) plane.
[0150] The MO2 layer, which is composed of a transition metal M and an octahedron of oxygen, is relatively stable and can be used as a positive electrode active material. The surface of the ZnO layer is more stable if it has a (001) orientation. The diffuse pathway is not exposed.
[0151] On the other hand, the diffusion paths of lithium ions are exposed on surfaces other than the (001) orientation. Therefore, the surface and the surface layer portion 100a other than the (001) orientation maintain a diffusion path for lithium ions. This is an important area for the battery, but it is also a worrying area because it is the area where lithium ions are first desorbed. Therefore, it is necessary to reinforce the surface and the surface layer portion 100a other than the (001) orientation. This is extremely important for maintaining the crystal structure of the entire positive electrode active material 100.
[0152] Therefore, in the positive electrode active material 100 according to another embodiment of the present invention, the surface and The distribution of the additive elements in the surface layer 100a is as shown in FIG. 4(B1) or FIG. 4(B2). On the other hand, the (001) oriented surface and its surface layer 10 In 0a, as described above, the concentration of the added element is low, or the added element may be absent.
[0153] As shown in the previous embodiment, after producing high-purity LiMO2, the additive elements are added later. The method of mixing and heating the material mainly allows the added elements to spread through the diffusion pathway of lithium ions. Therefore, the distribution of the added elements in the surface other than the (001) orientation and in the surface layer 100a thereof is preferable. It is easy to adjust the range.
[0154] Using Fig. 5(A1) to Fig. 5(B), after producing high purity LiMO2, The results of calculations on the distribution of added elements when the above-mentioned materials are mixed and heated will be explained below.
[0155] FIG. 5(A1) shows the results of calculations for a (104) oriented surface and its surface layer 100a. This is the result of the classical molecular dynamics calculation. LiCoO2 (LCO) is placed at the bottom of the system. LiF and MgF2 are placed on the top of the system. The ensemble is NVT, and the density of the initial structure is 1.8 g / cm 3 The system temperature is 2000K, the elapsed time is 100psec, and the potential is LCO The crystal structure is optimized and the other atoms are UFF (Universal Force Field). ld), the number of atoms in the system is 10,000, and the charge of the system is neutral. The o and Mg atoms are shown in excerpt.
[0156] Figure 5(A2) shows the results calculated up to 200psec, and Figure 5(A3) shows the results calculated up to 1200psec. The result is.
[0157] Mg diffuses through the following process: (1) Li atoms are desorbed from LCO due to heat (not shown). (2) Mg atoms enter the Li layer of LCO and diffuse inward. (3) Li atoms from LiF enter the Li layer of LCO and complement the Li atoms that were desorbed in (1). Will be
[0158] From Figure 5(A1) after 100 psec, it is clear that Mg atoms are diffusing into the LCO. The Mg atoms diffuse along the cobalt array, and after 1200 psec In Figure 5(A3), almost all of the Mg atoms prepared at the top of the system are incorporated into LCO.
[0159] FIG. 5(B) shows the results of calculations similar to those in FIG. 5(A1), except that the orientation is (001). In 5(B), it can be seen that the Mg atoms remain on the surface of the LCO.
[0160] In this way, after producing high-purity LiMO2 as shown in the previous embodiment, the additive elements are added. The method of preparation, mixing and heating, resulted in a surface with a non-(001) orientation rather than a (001) orientation. The additive elements in the surface and the surface layer 100a can be preferably distributed. In the fabrication method that involves initial heating, lithium atoms in the surface layer are removed from LiMO2 by the initial heating. This is expected to allow for the separation of magnesium atoms and other additive elements at high concentrations. It is thought that this makes it easier for the ions to be distributed to the surface layer.
[0161] In addition, it is preferable that the surface of the positive electrode active material 100 is smooth and has few irregularities. The entire surface of the positive electrode active material 100 does not have to be such a structure. A complex oxide with a crystal structure has a plane parallel to the (001) plane, for example, a plane in which lithium is arranged. As shown in Figure 6(A), when the (001) plane is horizontal, However, by going through processes such as pressing, horizontal slip occurs as shown by the arrow in Figure 6(B). This may cause deformation.
[0162] In this case, the surface newly generated as a result of the slip and the surface layer 100a thereof contain the additive element. In some cases, the slippage is absent or the concentration is below the detection limit. This is an example of the surface and its surface layer 100a newly formed as a result of the pressing. The results are shown in Fig. 6(C1) and Fig. 6(C2). In Fig. 6(C1) and Fig. 6(C2), Unlike Fig. 4(B1) to Fig. 4(C2), the gradation of the added element X and the added element Y is Does not exist.
[0163] However, slip tends to occur parallel to the (001) plane, so the newly formed surface and its The layer 100a has a (001) orientation. The (001) plane exposes the diffusion path of lithium ions. Since it is relatively stable and does not react with added elements, it can be used even if the added elements are not present or their concentration is below the detection limit. There are very few problems.
[0164] As mentioned above, the compound acid has a layered rock salt structure with a composition of LiMO2 and a crystal structure of R-3m. In the HAADF-STE, the transition metal atoms are aligned parallel to the (001) plane. In the M image, the transition metal M, which has the largest atomic number among LiMO2, has the highest brightness. Therefore, in the HAADF-STEM image, the arrangement of atoms with high brightness is the arrangement of transition metal M atoms. The repetition of this bright arrangement can be called crystal fringes or lattice fringes. Furthermore, the crystal fringes or lattice fringes are (001) planes when the crystal structure is a layered rock salt type of R-3m. It can be considered parallel.
[0165] The positive electrode active material 100 may have recesses, cracks, dents, V-shaped cross sections, etc. is one of the defects, and repeated charging and discharging causes the elution of transition metal M and the collapse of the crystal structure. However, there is a risk that the positive electrode active material 100 may crack or oxygen may be released. If the buried portion 102 (FIG. 8) is present so as to cover the pores, the elution of the transition metal M can be suppressed. Therefore, it is possible to obtain a positive electrode active material 100 having excellent reliability and cycle characteristics. Cut.
[0166] The positive electrode active material 100 has a protrusion 103 (FIG. 8) as a region where the additive element is unevenly distributed. Good too.
[0167] As described above, if the amount of the additive element contained in the positive electrode active material 100 is excessive, lithium intercalation may occur. In addition, when the positive electrode active material 100 is used in a secondary battery, There is a risk of an increase in internal resistance and a decrease in charge / discharge capacity. On the other hand, the amount of added elements is insufficient. If the amount of the crystalline structure is too small, the crystalline structure may not be sufficiently suppressed due to the lack of distribution over the entire surface layer 100a. In this way, the additive element needs to be present at an appropriate concentration in the positive electrode active material 100. , and making the adjustment is not easy.
[0168] Therefore, if the positive electrode active material 100 has a region where the additive element is unevenly distributed, an excessive additive element A part of the atoms is removed from the interior 100b of the positive electrode active material 100, and the inside 100b is appropriately This can prevent the increase in internal resistance when used as a secondary battery. The decrease in charge / discharge capacity can be suppressed. The increase in the internal resistance of the secondary battery can be suppressed. This is a particularly favorable characteristic for high-rate charging and discharging, for example, charging and discharging at 2C or higher. It is sexuality.
[0169] In the positive electrode active material 100 having a region where the additive element is unevenly distributed, It is permissible to mix impurities in excess to some extent, which allows for a wider margin in production. This is more preferable.
[0170] In this specification, uneven distribution means that the concentration of an element in a certain region is different from that in other regions. Segregation, precipitation, non-uniformity, bias, the mixture of high concentration and low concentration areas, etc. That's a good thing.
[0171] Magnesium, one of the added elements X, is divalent and has a transition Since it is more stable at the lithium site than at the metal site, The presence of magnesium at an appropriate concentration at the lithium site of the surface layer 100a makes it possible to The presence of magnesium makes it easier to maintain the layered rock salt crystal structure. It is possible to suppress the desorption of oxygen around magnesium when the electrical depth is high. The presence of magnesium is expected to increase the density of the positive electrode active material. However, if the concentration is appropriate, it is preferable since it does not adversely affect the insertion and desorption of lithium during charging and discharging. However, excess magnesium has a negative effect on lithium insertion and extraction. Therefore, as described later, the surface layer 100a is preferably made of a material other than magnesium. A high concentration of the transition metal M is preferred.
[0172] Aluminum, one of the added elements Y, is trivalent and has a transition property in the layered rock-salt crystal structure. Aluminum can be present at metal sites. It can suppress the dissolution of surrounding cobalt. In addition, aluminum has a strong bond with oxygen, which prevents the oxygen from escaping from the aluminum. Therefore, by having aluminum as an additive element, repeated charging and discharging can be performed. Therefore, the crystal structure of the positive electrode active material 100 is not easily broken even if the positive electrode active material 100 is heated.
[0173] Fluorine is a monovalent anion, and part of the oxygen in the surface layer 100a is replaced by fluorine. This is because the lithium desorption energy is smaller when the cobalt content is increased. This is because the redox potential of the ions differs depending on whether or not there is fluorine. In the absence of lithium, the cobalt ion changes from trivalent to tetravalent upon lithium elimination. In the case of the cation exchange reaction, the cobalt ion changes from divalent to trivalent upon lithium elimination. Therefore, the surface layer 100a of the positive electrode active material 100 has a different redox potential. When some of the oxygen is replaced by fluorine, the desorption and desorption of lithium ions near the fluorine Therefore, when used in secondary batteries, the charge / discharge characteristics and This is preferable because it improves rate characteristics and the like.
[0174] Titanium oxide is known to have superhydrophilicity. By using a positive electrode active material 100 having a cation oxide, the wettability with respect to a highly polar solvent is improved. When a secondary battery is formed, the boundary between the positive electrode active material 100 and the electrolyte with high polarity may become This improves surface contact and may help prevent an increase in internal resistance.
[0175] As the charging voltage of the secondary battery increases, the voltage of the positive electrode generally increases. The electrode active material has a stable crystal structure even at high voltages. The stable crystal structure of the material suppresses the decrease in charge / discharge capacity caused by repeated charging and discharging. It is possible.
[0176] In addition, a short circuit in the secondary battery may cause malfunctions in the charging and / or discharging operations of the secondary battery. Not only does this cause problems, but it can also lead to heat generation and fire. In order to achieve this, it is preferable that the short circuit current is suppressed even at a high charging voltage. The positive electrode active material 100 of one embodiment suppresses short circuit current even at a high charging voltage. Therefore, it is possible to provide a secondary battery that achieves both high charge / discharge capacity and safety.
[0177] The concentration gradient of the added element can be measured, for example, by energy dispersive X-ray spectroscopy (EDX). Dispersive X-ray Spectroscopy, EPMA (Electron Probe The EDX measurement can be performed by scanning the area. Evaluating the area in two dimensions is called EDX area analysis. The evaluation of the distribution of atomic concentrations within the positive electrode active material particles is called line analysis. The area analysis of X may be called line analysis when data on a linear region is extracted. Measuring a given area without scanning is called point analysis.
[0178] By EDX surface analysis (e.g., element mapping), The concentration of the additive element in the portion 100b and in the vicinity of the grain boundary 101 is quantitatively analyzed. In addition, the concentration distribution and maximum value of the added elements can be analyzed by EDX line analysis. In addition, analysis of a thin sample, such as STEM-EDX, allows for the observation of the depth direction. The concentration in the depth direction from the surface to the center of a particle in a specific area is not affected by the distribution. This is more preferable since it allows the degree distribution to be analyzed.
[0179] When EDX analysis was performed on the positive electrode active material 100 containing magnesium as an added element, The peak of the magnesium concentration in the surface layer 100a increases from the surface of the positive electrode active material 100 toward the center. It is preferable that the ions are present at a depth of up to 3 nm, and more preferably at a depth of up to 1 nm. It is preferable that the thickness of the pores is less than 0.5 nm, and more preferable that the thickness of the pores is less than 0.5 nm.
[0180] In the positive electrode active material 100 having magnesium and fluorine as additive elements, the amount of fluorine is The distribution of magnesium should overlap with that of magnesium. The peak of the fluorine concentration in the surface layer 100a increases from the surface of the positive electrode active material 100 toward the center. Preferably, the surface roughness is present at a depth of up to 3 nm, more preferably at a depth of up to 1 nm. It is preferable that the depth of the pores is within 0.5 nm.
[0181] It is not necessary that all the additive elements have the same concentration distribution. When aluminum is used as an additional element, it is preferable to use magnesium and fluorine as described above. For example, when EDX analysis was performed, The magnesium concentration peak is closer to the surface than the aluminum concentration peak in 00a. For example, the peak of the aluminum concentration is preferably from the surface to the center of the positive electrode active material 100. Preferably, the depth is 0.5 nm to 50 nm, and more preferably, the depth is 5 nm to 30 nm. It is more preferable that the diameter of the slit is 0.5 nm or more and 30 nm or less. Alternatively, it is preferable that the size of the nanoparticles is 5 nm or more and 50 nm or less.
[0182] In addition, when the positive electrode active material 100 was subjected to a line analysis or a surface analysis, The ratio of the number of atoms of the additive element I to the transition metal M (I / M) is preferably 0.05 or more and 1.00 or less. Furthermore, when the added element is titanium, the ratio of the number of titanium atoms to the transition metal M (Ti / M) is The ratio is preferably 0.05 to 0.4, and more preferably 0.1 to 0.3. When the element is magnesium, the ratio of the number of atoms of magnesium to the transition metal M (Mg / M) is 0 The ratio is preferably 0.4 or more and 1.5 or less, and more preferably 0.45 or more and 1.00 or less. When the element is fluorine, the ratio of the number of fluorine atoms to the transition metal atom M (F / M) must be greater than or equal to 0.05 and less than or equal to 1. It is preferably 5 or less, and more preferably 0.3 or more and 1.00 or less.
[0183] The surface of the positive electrode active material 100 in the EDX analysis is estimated as follows, for example. An element that is uniformly present in the inside 100b of the positive electrode active material 100, for example, For example, oxygen or a transition metal M such as cobalt was detected at half the amount of the internal 100b. Let the points be the surface.
[0184] Since the positive electrode active material 100 is a composite oxide, the surface can be estimated using the detected amount of oxygen. Specifically, first, the oxygen concentration is measured from the region in the interior 100b where the amount of oxygen detected is stable. Average degree O ave At this time, chemical adsorption occurs in an area that can be clearly determined to be outside the surface. or background oxygen (O background If detected In this case, O is removed from the measurement value. background The average oxygen concentration is calculated by subtracting ave To This average value O ave That is, 1 / 2O ave The closest measurement to The indicated measurement points can be assumed to be the surface of the positive electrode active material.
[0185] The surface can also be estimated using the transition metal M contained in the positive electrode active material 100. For example, if 95% or more of the transition metals M is cobalt, the amount of cobalt detected can be used. The surface can be estimated in the same manner as above. Alternatively, the sum of the detected amounts of multiple transition metals M can be used. The amount of the transition metal M detected is less susceptible to chemical adsorption. , which is suitable for estimating surfaces.
[0186] In addition, when the positive electrode active material 100 is subjected to a line analysis or an area analysis, The ratio of the number of atoms of the additive element I to the number of atoms of the transition metal M (I / M) is preferably 0.020 or more and 0.50 or less. It is more preferable that the ratio is 0.025 or more and 0.30 or less. It is even more preferable that the ratio is 0.030 or more and 0. 20 or less is preferable. Or, 0.020 or more and 0.30 or less is preferable. Or, 0.020 Preferably, the ratio is 0.025 or more and 0.50 or less. Preferably, the ratio is 0.025 or more and 0.20 or less, or more preferably 0.030 or more and 0.50 or less. Alternatively, it is preferably 0.030 or more and 0.30 or less.
[0187] For example, when the additive element is magnesium and the transition metal M is cobalt, magnesium and The ratio of the number of cobalt atoms (Mg / Co) is preferably 0.020 or more and 0.50 or less. The range is preferably 0.025 or more and 0.30 or less, and more preferably 0.030 or more and 0.20 or less. It is preferable that the ratio is 0.020 or more and 0.30 or less. It is preferable that the ratio is 0.020 or more and 0.20 or less. or less is preferable. Or, 0.025 or more and 0.50 or less is preferable. Or, 0.025 or more Preferably, it is 0.20 or less. Or, it is preferably 0.030 or more and 0.50 or less. Or, it is preferably 0.0 A value of 30 or more and 0.30 or less is preferred.
[0188] The positive electrode active material 100 is used under conditions of high charge depth such as charging at 4.5 V or higher or high temperature. By charging and discharging at low temperatures (45°C or higher), progressive defects (also called pits) form in the positive electrode active material. In addition, cracks ( In some cases, defects such as cracks may occur. In the positive electrode active material 51, the pits are shown as holes at 54 and 58. The opening shape is not circular but has depth and is shaped like a groove. The source of the pit is a point defect. In addition, the crystal structure of LCO collapses near the pits, which is different from the layered rock salt type. When the crystal structure is broken, the lithium ions, which are carrier ions, The pits may hinder the diffusion and release of ions, and are considered to be a cause of deterioration of cycle characteristics. In the positive electrode active material 51, the cracks are indicated by 57. 55 is a cation. The crystal plane is parallel to the arrangement of the doped elements, 52 is a recess, and 53 and 56 are regions where the doped elements are present. .
[0189] The positive electrode active material of lithium-ion secondary batteries is typically LCO (lithium cobalt oxide) and and NMC (lithium nickel-manganese-cobalt oxide), which are made up of multiple metal elements (cobalt At least one of the positive electrode active materials is an alloy containing at least one The positive electrode active material has defects, and these defects may change before and after charging and discharging. When used in a battery, the positive electrode active material is chemically or chemically affected by the environmental substances (such as electrolyte) surrounding it. In some cases, the positive electrode active material may be electrochemically corroded or deteriorated. This deterioration does not occur uniformly on the surface of the positive electrode active material, but occurs locally and in a concentrated manner. Repeated charging and discharging of the battery can cause deep defects, for example, from the surface to the inside.
[0190] Pitting corrosion is a phenomenon in which defects in the positive electrode material progress and form holes. The holes generated by this phenomenon are also called pits in this specification. .
[0191] In this specification, cracks and pits are different. Cracks are present immediately after the preparation of the positive electrode active material. No pits will be present even if the battery is charged. Pits occur when the battery is at a high charge level, for example, 4.5V or higher. By charging and discharging under high voltage conditions or at high temperatures (45°C or higher), cobalt and oxygen are It can be said that the layer is missing, or that the cobalt has dissolved. The crack is caused by physical pressure. New faces that are created by the addition of 101 or grain boundaries 101 This refers to cases where cracks occur due to expansion and contraction of the positive electrode active material caused by charging and discharging. In addition, pits may occur due to cracks and / or cavities inside the positive electrode active material. There are also.
[0192] The positive electrode active material 100 may have a coating on at least a part of its surface. 1 shows an example of a positive electrode active material 100 having a first electrode 104.
[0193] The coating 104 is formed, for example, by the accumulation of decomposition products of the electrolyte during charging and discharging. In particular, when charging is repeated to a high charging depth, the surface of the positive electrode active material 100 is preferably It is expected that the charge-discharge cycle characteristics will be improved by having a coating derived from the electrolyte on the surface. This is to suppress the increase in impedance of the positive electrode active material surface or to prevent the elution of the transition metal M. The coating 104 may contain, for example, carbon, oxygen, and fluorine. It is preferable to use LiBOB and / or SUN (suberonitrile) as the electrolyte. Therefore, it is easy to obtain a good quality coating when boron, nitrogen, sulfur, fluorine, etc. are used. The coating 104 having at least one of the above may be a good quality coating and is therefore preferred. 04 does not have to cover the entire positive electrode active material 100 .
[0194] <Crystal structure> Materials with a layered rock-salt crystal structure, such as lithium cobalt oxide (LiCoO2), It has a high capacity and is known to be an excellent positive electrode active material for secondary batteries. Layered rock salt type crystal An example of a material having this structure is a composite oxide represented by LiMO2.
[0195] The Jahn-Teller effect in transition metal compounds depends on the number of electrons in the d orbitals of the transition metal. are known to vary in the strength of their effects.
[0196] In nickel-containing compounds, distortion may easily occur due to the Jahn-Teller effect. Therefore, when LiNiO2 is charged and discharged to a high degree of charge, the strain There is a concern that the crystal structure of LiCoO2 may collapse due to the stress. This suggests that the effect of the charge-discharge effect is small, and resistance may be better when the charge depth is high. This is more preferable.
[0197] The crystal structure of the positive electrode active material will be described with reference to Figs. 9 to 13. The case where cobalt is used as the transition metal M in the positive electrode active material will be described.
[0198] <Conventional positive electrode active materials> The positive electrode active material shown in FIG. 11 is made by the method described below to which fluorine and magnesium are added. The lithium cobalt oxide shown in Figure 11 is lithium cobalt oxide (LiCoO2). As described in Non-Patent Documents 1 and 2, the crystal structure changes depending on the charge depth. changes.
[0199] As shown in Figure 11, the charge depth is 0 (discharge state). Lithium cobalt oxide, which is almost 100% pure, has a crystal structure of the space group R-3m. The lithium ions occupy octahedral sites, and the unit There are three CoO2 layers in the tococell. Therefore, this crystal structure is called the O3 type crystal structure. In addition, the CoO2 layer is an octahedral structure in which cobalt is coordinated with six oxygen atoms, with edge-sharing. This term refers to a structure that is continuous on a plane in this state.
[0200] At a charge depth of 1, the crystal structure has the space group P-3m1, and there is CoO There is one 2-layer structure. Therefore, this crystal structure is sometimes called the O1-type crystal structure.
[0201] In addition, when the charge depth is about 0.8, lithium cobalt oxide has a crystal structure of the space group R-3m. This structure is similar to the structure of CoO2, such as P-3m1(O1), and R-3m(O3). The structure of LiCoO2 is like that of LiCoO2, and the structure of LiCoO2 is like that of LiCoO2. The structure is sometimes called the H1-3 crystal structure. In reality, the H1-3 crystal structure is The number of cobalt atoms per unit cell is twice that of the other structures. In this specification, the c-axis of the H1-3 crystal structure is defined as It will be shown in a diagram that is half of a unit cell.
[0202] As an example of the H1-3 type crystal structure, as described in Non-Patent Document 3, in the unit cell The coordinates of cobalt and oxygen in the (0,0,0.27671±0.00045), O2(0,0,0.11535±0.0 0045), where O1 and O2 are oxygen atoms. The H1-3 crystal structure is a unit cell with one cobalt atom and two oxygen atoms. On the other hand, as described below, the O3′-type and O3″-type bonds according to one embodiment of the present invention are The crystal structure preferably has a unit cell with one cobalt atom and one oxygen atom. This is because the cobalt and the oxide are different in the O3' structure and the H1-3 structure. The symmetry of the O3' structure is different from that of the H1-3 structure. The change in the crystal structure of the positive electrode active material is small. The choice of which is more preferable to represent, for example, in the Rietveld analysis of the XRD pattern. GOF (goodness of fit) value should be smaller. stomach.
[0203] High-voltage charging where the charging voltage is 4.6V or higher based on the redox potential of lithium metal Or, if you repeatedly charge and discharge to a deep depth of charge of 0.8 or more, Lithium cobalt oxide has a H1-3 type crystal structure and a discharged R-3m(O3) structure. The crystal structure changes (i.e., non-equilibrium phase changes) occur repeatedly between these two states.
[0204] However, these two crystal structures have a large misalignment of the CoO2 layers. As shown by the arrows and the lines in the figure, in the H1-3 crystal structure, the CoO2 layer is separated from the R-3m(O3) by a large Such dynamic structural changes adversely affect the stability of the crystal structure. Yes.
[0205] Furthermore, the difference in volume is also large. When comparing per the same number of cobalt atoms, the H1-3 crystal structure The difference in volume between the O3-type crystal structure and the discharged state is more than 3.0%.
[0206] In addition, the H1-3 type crystal structure has continuous CoO2 layers like P-3m1(O1). The resulting structure is likely to be unstable.
[0207] Therefore, when the charge / discharge cycle is repeated to increase the depth of charge, the crystal structure of the lithium cobalt oxide The breakdown of the crystal structure causes the deterioration of cycle characteristics. The collapse of the bond reduces the number of sites where lithium can exist stably, and the insertion and desorption of lithium becomes difficult. This is thought to be because it becomes more difficult to separate.
[0208] <Positive Electrode Active Material of One Embodiment of the Present Invention> <Crystal structure> The positive electrode active material 100 according to one embodiment of the present invention exhibits excellent electrical conductivity even when repeatedly charged and discharged to increase the depth of charge. By doing so, the displacement of the CoO2 layer can be reduced. Furthermore, the change in volume can be reduced. Therefore, the positive electrode active material of one embodiment of the present invention can achieve excellent cycle characteristics. In addition, the positive electrode active material according to one embodiment of the present invention is stable at a high depth of charge. Therefore, the positive electrode active material of one embodiment of the present invention can maintain a high state of charge. In such cases, it is safer to use a short circuit. This is preferable because it improves the
[0209] In the positive electrode active material according to one embodiment of the present invention, the charge-discharge current is The change in crystal structure and the difference in volume per the same number of transition metal M atoms are small. stomach.
[0210] When the charge depth is 0 and when the charge depth is as high as about 0.8, the inside of the positive electrode active material 100 The crystal structure of the inner portion 100b is shown in FIG. This accounts for half of the total volume of the CoO2 layer and contributes greatly to charging and discharging. This is arguably the most problematic part.
[0211] The positive electrode active material 100 is a composite acid having lithium, cobalt as a transition metal M, and oxygen. In addition to the above, the inner portion 100b may have magnesium as an added element. It is preferable that the transition metal M contains nickel in addition to cobalt. The surface layer 100a preferably contains fluorine as an additive element, and aluminum and / or More preferably, the surface layer 100a contains nickel. Details of the surface layer 100a will be described later.
[0212] The crystal structure at charge depth 0 (discharged state) in FIG. 9 is R-3m(O3), the same as in FIG. 11. On the other hand, the inside 100b of the positive electrode active material 100 is H1-3 type when the charge depth is sufficiently high. The structure of this compound is assigned to the space group R-3m, and the structure of the compound is different from that of the cobalt compound. The ions of Zn, Mg, etc. occupy the 6-coordinated oxygen sites. The properties are the same as those of the O3 type. Therefore, this structure is referred to as the O3' type crystal structure in this specification. In both the O3 and O3' crystal structures, the interlayers of the CoO2 layers, i.e., the ribs, It is preferable that magnesium is present in a dilute amount at the lithium site. It is preferred that the fluorine be present randomly and dilutely.
[0213] In addition, in the O3' type crystal structure, light elements such as lithium may occupy the oxygen tetracoordination position. Possible.
[0214] In addition, in O3' in Figure 9, lithium exists at all lithium sites with a probability of 1 / 5. However, the positive electrode active material 100 according to one embodiment of the present invention is not limited to this. For example, Li, which belongs to the space group P2 / m, 0.5 Similar to CoO2 The lithium distribution may be, for example, It can be analyzed by neutron diffraction.
[0215] The O3' type crystal structure has random lithium between layers, but the CdCl2 type has no interlayer structure. It can be said that the crystal structure is similar to that of the CdCl2 type. The structure is that when lithium nickel oxide is charged to a charge depth of 0.94 (Li 0.06 NiO 2) It has a similar crystal structure to pure lithium cobalt oxide, or a layered rock containing a large amount of cobalt. It is known that salt-type positive electrode active materials do not usually have this crystal structure.
[0216] In the positive electrode active material 100 according to one embodiment of the present invention, when the charge depth is high, that is, when a large amount of lithium is present, The change in the crystal structure when the metal is desorbed is suppressed more than in conventional positive electrode active materials. For example, As shown by the dotted lines in Fig. 9, there is almost no misalignment of the CoO2 layers in these crystal structures.
[0217] More specifically, the positive electrode active material 100 according to one embodiment of the present invention has a high charge depth. The crystal structure is highly stable. For example, conventional positive electrode active materials have an H1-3 type crystal structure. For example, even at a charging voltage of about 4.6 V based on the potential of lithium metal, There exists a region of charging voltage where the crystal structure of 3m(O3) can be maintained, and the charging voltage was further increased. For example, in the region where the potential of lithium metal is between 4.65V and 4.7V Even at high voltages, there is still a region where the O3' type crystal structure can be formed. In some cases, the H1-3 crystal structure is observed. For example, the charging voltage may be 4.5 V or more and less than 4.6 V based on the potential of lithium metal. The positive electrode active material 100 according to one embodiment may have an O3' type crystal structure.
[0218] Therefore, in the positive electrode active material 100 according to one embodiment of the present invention, charging is performed so as to increase the depth of charge. The crystal structure does not easily collapse even after repeated discharge.
[0219] The space group of the crystal structure is identified by XRD, electron diffraction, neutron diffraction, etc. Therefore, in this specification and the like, belonging to a certain space group or being a certain space group means , which can be rephrased as being assigned to a certain space group.
[0220] In addition, when graphite is used as the negative electrode active material in the secondary battery, the graphite The voltage of the secondary battery drops by the amount of the potential of the graphite. For example, a secondary battery using graphite as the negative electrode active material has a voltage of about 0.05 V to 0.2 V. Even when the battery voltage is 4.3 V or more and 4.5 V or less, the positive electrode active material 100 according to one embodiment of the present invention has R -3m(O3) crystal structure can be maintained, and the charging voltage can be increased, for example, in secondary batteries. The O3' type crystal structure can be formed even when the voltage is greater than 4.5 V and is equal to or less than 4.6 V. If the charging voltage is lower, for example if the voltage of the secondary battery is between 4.2V and 4.3V, The positive electrode active material 100 according to one embodiment of the invention may have an O3' type crystal structure.
[0221] In the O3' type crystal structure, the coordinates of cobalt and oxygen in the unit cell are Co(0, 0,0.5), O(0,0,x), and can be shown within the range of 0.20≦x≦0.25. The lattice constants of the unit cell are typically a = 2.817 (Å) and c = 13.781 ( Å). Note that 1Å=10 -10 m.
[0222] Additive elements that exist randomly and dilutely between the CoO2 layers, i.e., at the lithium sites, e.g. Magnesium has the effect of suppressing the shift of the CoO2 layer when the charge depth is high. Therefore, when magnesium exists between the CoO2 layers, the O3' type crystal structure tends to be formed. Therefore, magnesium is preferably distributed throughout the particles of the positive electrode active material 100 of one embodiment of the present invention. In order to distribute magnesium throughout the particles, it is preferable to use a positive electrode active material according to one embodiment of the present invention. In the manufacturing process of 100, a heat treatment is preferably performed.
[0223] However, if the heat treatment temperature is too high, cation mixing occurs, and the added elements, For example, magnesium is more likely to enter the cobalt site. Magnesium is ineffective in preserving the structure of R-3m at high charge depths. If the temperature of the process is too high, cobalt will be reduced to divalent and lithium will evaporate. There are also concerns about other adverse effects.
[0224] Therefore, prior to the heat treatment to distribute magnesium throughout the particles, the lithium cobaltate was It is preferable to add a fluorine compound to cobalt. The melting point of lithium tritate is lowered. By lowering the melting point, cation mixing occurs. At high temperatures, it becomes easier to distribute magnesium throughout the particles. It is expected that the presence of this substance will improve corrosion resistance against hydrofluoric acid produced by the decomposition of the electrolyte. Cut.
[0225] Furthermore, by carrying out the above-mentioned initial heating, additives such as magnesium and aluminum are This allows for better distribution of the charge element, which allows for higher charging voltages, e.g. Even if the charge voltage is between 4.6V and 4.8V, and the charge depth is between 0.8 and 0.9, The 1-3 type crystal structure is not formed, and the crystal structure in which the displacement of the CoO2 layer is suppressed can be maintained. The crystal structure has the same symmetry as the O3' type crystal structure, but the lattice constant is O This structure is different from the 3'-type crystal structure. Therefore, this structure is referred to as the O3"-type crystal structure in this specification. The O3" type crystal structure has a layered structure. The O3" type also has a similar structure to the CdCl2 type crystal structure. This can be called a crystal structure.
[0226] If the magnesium concentration is made higher than the desired value, the effect of stabilizing the crystal structure is small. In some cases, magnesium may occupy the cobalt site in addition to the lithium site. In addition, the lithium site and the cobalt site The positive electrode active material is not substituted with unnecessary magnesium compounds (e.g. oxides, fluorides, etc.). The magnesium oxide contained in the positive electrode active material according to one embodiment of the present invention may be unevenly distributed on the surface or the like and may become a resistance component. The number of nesium atoms is preferably 0.001 to 0.1 times the number of transition metal M atoms, More preferably, the ratio is greater than 0.01 and less than 0.04, and even more preferably, about 0.02. Or, it is preferably 0.001 times or more and less than 0.04 times. Or, it is preferably 0.01 times or more and 0.1 times or less. The magnesium concentration shown here is preferably determined by, for example, GD-MS (glow discharge mass spectrometry). The whole particle of the positive electrode active material was analyzed using a spectrometer (electrochemical analyzer), an inductively coupled plasma mass spectrometer (ICP-MS), etc. The value may be a value obtained by elemental analysis of the positive electrode active material, or the value may be a value obtained by mixing the raw materials in the process of producing the positive electrode active material. It may be based on value.
[0227] Nickel and other transition metals, as well as aluminum, are present on the cobalt site. However, some of it may be present at the lithium site. It is preferable that oxygen is present in the .mu.site. The oxygen may be partially substituted with fluorine.
[0228] As the magnesium concentration of the positive electrode active material of one embodiment of the present invention increases, the charging and discharging properties of the positive electrode active material also increase. The capacitance may decrease. For example, magnesium may be present at the lithium site. The amount of lithium that contributes to charging and discharging decreases when excess In some cases, magnesium may generate magnesium compounds that do not contribute to charging and discharging. In one embodiment of the positive electrode active material, in addition to magnesium, nickel is included as the metal Z. This may increase the charge / discharge capacity per weight and per volume. The positive electrode active material according to one embodiment of the present invention has aluminum as the metal Z in addition to magnesium. By doing so, it may be possible to increase the charge / discharge capacity per weight and per volume. In addition, the positive electrode active material according to one embodiment of the present invention contains nickel and aluminum in addition to magnesium. By having a gyro, it is possible to increase the charge / discharge capacity per weight and per volume. There are cases.
[0229] The concentrations of elements such as magnesium and metal Z contained in the positive electrode active material of one embodiment of the present invention are shown below. , expressed using the number of atoms.
[0230] The number of nickel atoms in the positive electrode active material 100 according to one embodiment of the present invention is 0.1% of the number of cobalt atoms. %, preferably 7.5% or less, more preferably 0.05% to 4%, more preferably 0.1% or more 2% or less is preferable, 0.2% or more and 1% or less is more preferable, or more than 0% and 4% or less is more preferable. or less than 0% is preferable; or more than 0% and less than 2% is preferable; or 0.05% to 7.5% or less. Or, 0.05% or more and 2% or less. Or, 0.1% or more and 7.5% or less. % or less, or 0.1% to 4% or less. For example, elemental analysis of the entire particles of the positive electrode active material was performed using GD-MS, ICP-MS, etc. It may be a value based on the composition of the raw materials in the process of producing the positive electrode active material. stomach.
[0231] Nickel contained in the above concentration is easily dissolved uniformly throughout the positive electrode active material 100, and therefore In addition, the presence of divalent nickel in the inner portion 100b contributes to stabilizing the crystal structure of the inner portion 100b. When the lithium site is present, divalent dopants are present randomly and dilutely at the lithium site nearby. For example, magnesium may be more stable, which may result in a higher charge depth. Therefore, even if the battery is subjected to a charge-discharge cycle, the elution of magnesium can be suppressed. In this way, the effect of nickel in the inner portion 100b and the effect of nickel in the surface layer portion 100a can be improved. The effects of magnesium, aluminum, titanium, fluorine, etc. in the It is extremely effective in stabilizing the crystal structure at high electrical depths.
[0232] The number of aluminum atoms in the positive electrode active material of one embodiment of the present invention is 0. 0.5% or more and 4% or less are preferable, 0.1% or more and 2% or less are preferable, and 0.3% or more and 1.5% or less are preferable. % or less is more preferable. Alternatively, 0.05% to 2% is more preferable. Alternatively, 0.1% or more is more preferable. The aluminum concentration shown here is preferably 4% or less. The value may be obtained by performing elemental analysis of the entire particles of the positive electrode active material using S or the like, or the positive electrode active material It may be based on the value of the raw material composition in the manufacturing process.
[0233] The positive electrode active material of one embodiment of the present invention preferably further contains phosphorus as an additional element. In addition, the positive electrode active material of one embodiment of the present invention preferably contains a compound containing phosphorus and oxygen. stomach.
[0234] By including a compound containing phosphorus in the positive electrode active material of one embodiment of the present invention, the positive electrode active material can be used at a high depth of charge. When the above-mentioned state is maintained, it may be possible to suppress a short circuit.
[0235] In the case where the positive electrode active material according to one embodiment of the present invention contains phosphorus, the fluorine generated by the decomposition of the electrolyte is There is a possibility that hydrogen fluoride and phosphorus will react, resulting in a decrease in the hydrogen fluoride concentration in the electrolyte.
[0236] When the electrolyte contains LiPF6, hydrogen fluoride may be generated due to hydrolysis. In addition, hydrogen fluoride is produced by the reaction of PVDF, which is used as a component of the positive electrode, with alkali. A decrease in the hydrogen fluoride concentration in the electrolyte may cause corrosion of the current collector and In some cases, the gelation of PVDF and / or peeling of the coating 104 can be suppressed. In some cases, it may be possible to suppress the decrease in adhesiveness due to insolubilization.
[0237] When the positive electrode active material according to one embodiment of the present invention contains phosphorus in addition to magnesium, the positive electrode active material has a high degree of charge. In the case of phosphorus, the number of phosphorus atoms is 1 / 1 that of cobalt atoms. Preferably, 1% to 20% of the number, more preferably 2% to 10% and even more preferably 3% to 8% More preferably, the ratio is 1% or more and 10% or less. Or, the ratio is 1% or more and 8% or less. is preferable. Alternatively, 2% or more and 20% or less is preferable. Alternatively, 2% or more and 8% or less is preferable. Alternatively, 3% or more and 20% or less are preferable. Alternatively, 3% or more and 10% or less are preferable. The number of magnesium atoms is preferably 0.1% to 10% of the number of cobalt atoms, and 0. More preferably, the ratio is 5% or more and 5% or less, and even more preferably, 0.7% or more and 4% or less. % or more and 5% or less is preferable. Or 0.1% or more and 4% or less is preferable. Or 0.5% or less Preferably between 0.5% and 4%. Or preferably between 0.7% and 10%. Preferably, the phosphorus and phosphorus content is 10% or less, or more preferably 0.7% to 5%. The magnesium concentration was measured by elemental analysis of the entire particles of the positive electrode active material using ICP-MS, for example. The value may be based on the value of the raw material composition in the process of producing the positive electrode active material. This is also fine.
[0238] The positive electrode active material may have cracks. The area adjacent to the crack, for example, the buried portion The presence of phosphorus, more specifically, compounds containing phosphorus and oxygen, in 102 may The progression of the rack may be restricted.
[0239] ≪Surface layer≫ Magnesium is preferably distributed throughout the particles of the positive electrode active material 100 of one embodiment of the present invention. In addition, the magnesium concentration in the surface layer 100a is higher than the average of the whole particle. Alternatively, it is preferable that the magnesium concentration in the surface layer 100a is higher than that in the interior 100b. For example, the magnesium content of the surface layer 100a measured by XPS or the like is preferably higher than that of the surface layer 100a. The concentration is higher than the average magnesium concentration of the whole particle as measured by ICP-MS, etc. Alternatively, the magnesium concentration of the surface layer 100a measured by EDX surface analysis or the like is preferably , preferably higher than the magnesium concentration in the interior 100b.
[0240] In addition, the positive electrode active material 100 according to one embodiment of the present invention may contain an additive element such as aluminum or manganese. In the case where the alloy contains one or more metals selected from the group consisting of iron and chromium, the surface layer of the added element It is preferable that the concentration of the metal in 100a is higher than the average of the whole particle. It is preferable that the concentration in the surface layer 100a is higher than that in the inside 100b. For example, XP The concentration of additive elements other than cobalt in the surface layer 100a measured by S, etc., is measured by ICP-MS, etc. Preferably, the concentration of the element is greater than the average concentration of the whole particle being measured. The concentration of additive elements other than cobalt in the surface layer 100a measured by DX surface analysis etc. is It is preferable that the concentration of the additive element other than cobalt in 0b is higher than that of the additive element other than cobalt in 0b.
[0241] The surface layer 100a is in a state where bonds are broken, unlike the inner portion 100b where the crystal structure is maintained. In addition, when charging, lithium is removed from the surface, so the lithium concentration is lower than inside. Therefore, it is the part that is easily unstable and the crystal structure is easily destroyed. If the magnesium concentration in the surface layer 100a is high, the change in the crystal structure is more effectively suppressed. In addition, if the magnesium concentration in the surface layer 100a is high, the electrolyte may decompose and produce It is also expected that the corrosion resistance to hydrofluoric acid will be improved.
[0242] In addition, the concentration of fluorine in the surface layer 100a of the positive electrode active material 100 according to one embodiment of the present invention is higher than that in the entire particle. Alternatively, it is preferable that the fluorine concentration in the surface layer 100a is higher than the average of the fluorine concentration in the inner layer 100. It is preferable that the concentration of fluorine is higher than that of b. The presence of can effectively improve corrosion resistance to hydrofluoric acid.
[0243] In this way, the surface layer 100a of the positive electrode active material 100 according to one embodiment of the present invention is more porous than the inner portion 100b. A composition different from that of the inner portion 100b, which has a high concentration of additive elements such as magnesium and fluorine. It is preferable that the composition has a stable crystal structure at room temperature (25°C). Therefore, even if the surface layer 100a has a crystal structure different from that of the inner portion 100b, For example, at least a part of the surface layer 100a of the positive electrode active material 100 according to one embodiment of the present invention may be The surface layer 100a and the inner portion 100b may have different crystal structures. In the case where the crystal structure is a crystalline structure, the crystal orientation of the surface layer portion 100a and the inner portion 100b are approximately the same. is preferred.
[0244] Layered rock salt crystals and the anions of rock salt crystals have a cubic close-packed structure (face-centered cubic lattice structure) In the O3' type crystal, the anions are also assumed to form a cubic close-packed structure.
[0245] In this specification, the anions are stacked in three layers, shifted from each other, like ABCABC. structure, we call it a cubic close-packed structure. Therefore, the anions are strictly cubic lattice At the same time, since real crystals always have defects, analytical results do not necessarily match the theory. For example, FFT (Fast Fourier Transform) of electron beam diffraction patterns or TEM images can be used. d) In the transformed pattern, spots may appear in positions slightly different from their theoretical positions. For example, if the orientation with respect to the theoretical position is less than 5 degrees or less than 2.5 degrees, the cubic close-packed structure It can be said that this structure is
[0246] When layered rock salt crystals come into contact with each other, a cubic close-packed structure is formed by anions. There are crystal planes where the directions are aligned.
[0247] Alternatively, it can be explained as follows: On the (111) plane of the cubic crystal structure The anions have a triangular lattice. The layered rock salt type has the space group R-3m and a rhombohedral structure. However, to make it easier to understand the structure, it is generally represented as a complex hexagonal lattice, and the layered rock salt type (000 The (111) plane of the cubic crystal has a hexagonal lattice. The (0001) plane of the layered rock salt type has a triangular lattice. The atomic arrangement is the same as that of the hexagonal lattice ... It can be said that the orientation of the packing structure is aligned.
[0248] However, the space group of the layered rock salt crystal and the O3' crystal is R-3m, and the space group of the rock salt crystal is Since this is different from the space group Fm-3m (the space group of typical rock salt crystals), the above conditions are met. The Miller indices of the crystal planes are different between the layered rock salt crystal and the O3' type crystal, and the rock salt type crystal. In the fine print, in layered rock salt crystals, O3' and O3" type crystals, and rock salt crystals, When the orientation of the cubic close-packed structure formed by the anions is aligned, the crystal orientation is roughly the same. It is sometimes said that.
[0249] The crystal orientation of the two regions roughly coincides, as confirmed by TEM (Transmission Emission) lectron microscope, transmission electron microscope) image, STEM (Scanni ng Transmission Electron Microscope, Scanning Transmission Electron microscope) image, HAADF-STEM (High-angle Annular Da rk Field Scanning TEM, High Angle Scattering Annular Dark Field Scanning Transmission Electron Microscope ) statue, ABF-STEM (Annular Bright-Field Scannin g Transmission Electron Microscope, annular bright field Judging from scanning transmission electron microscope (STEM) images, electron beam diffraction patterns, FFT patterns of TEM images, etc. XRD (X-ray Diffraction), neutron X-ray diffraction etc. can also be used as a basis for judgment.
[0250] Figure 16 shows a TEM image in which the orientation of the layered rock salt crystal LRS and the rock salt crystal RS roughly coincides. Examples are shown below. For TEM images, STEM images, HAADF-STEM images, ABF-STEM images, etc. , an image reflecting the crystal structure is obtained.
[0251] For example, in high-resolution TEM images, contrast due to crystal planes can be obtained. For example, the electron beam is directed perpendicular to the c-axis of a layered rock-salt type composite hexagonal lattice due to diffraction and interference. When the incident light enters the (0003) plane, a bright strip of contrast appears. This is why the TEM image shows a repetition of bright and dark bands (dark strips). Repeated dark and light lines are observed, and the bright lines (for example, the L shown in Figure 16) RS and L LRS ) corner If the difference is less than 5 degrees, or less than 2.5 degrees, the crystal faces are roughly coincident, i.e. Similarly, the angle between the dark lines is less than 5 degrees. Even if the difference is less than 2.5 degrees, the crystal orientation can be judged to be roughly the same. can.
[0252] In addition, in the HAADF-STEM image, contrast according to the atomic number is obtained, The larger the element, the brighter it is observed. For example, cobalt, which belongs to the layered rocksalt space group R-3m, In the case of lithium tritate, cobalt (atomic number 27) has the highest atomic number, so cobalt The electron beam is strongly scattered at the atomic positions, and the arrangement of cobalt atoms appears as bright lines or points of strong brightness. Therefore, lithium cobalt oxide with a layered rock-salt crystal structure is When observed perpendicular to the axis, the arrangement of cobalt atoms perpendicular to the c axis appears as bright lines or points of strong brightness. The arrangement of lithium and oxygen atoms is observed as dark lines or low brightness areas. The lithium cobalt oxide is doped with fluorine (atomic number 9) and magnesium. The same is true when it contains nesium (atomic number 12).
[0253] Therefore, in the HAADF-STEM image, bright and dark lines appear in two regions with different crystal structures. If repetition is observed and the angle between the bright lines is less than 5 degrees or less than 2.5 degrees, the atom It can be determined that the arrangement of the crystals is roughly the same, that is, the crystal orientation is roughly the same. Similarly, when the angle between the dark lines is less than 5 degrees, or less than 2.5 degrees, the crystal alignment is also poor. It can be determined that the directions are roughly the same.
[0254] In ABF-STEM, elements with smaller atomic numbers are observed brighter. The contrast obtained is similar to that of HAADF-STEM, so -The crystal orientation can be determined in the same way as with STEM images.
[0255] FIG. 17(A) shows a STE in which the orientations of the layered rock-salt crystal LRS and the rock-salt crystal RS are roughly the same. The FFT pattern of the rock salt crystal RS region is shown in Fig. 17(B), and the layered rock salt crystal RS region is shown in Fig. 17(C). The FFT pattern of the region of the crystalline LRS is shown in FIG. 17(C). C) On the left are the composition, JCPDS card number, and the d value and angle calculated from this. The degrees are shown. The actual measured values are shown on the right. The spot marked with O is the zeroth order diffraction.
[0256] The spot marked A in FIG. 17(B) is due to the 11-1 reflection of a cubic crystal. The spot marked A in 7(C) is due to the 0003 reflection of the layered salt type. 7(B) and 17(C), the 11-1 reflection orientation of the cubic crystal and the 000 reflection of the layered salt type are It can be seen that the direction of the reflection is roughly the same as that of the reflection in Fig. 17(B). It can be seen that the line and the line passing through AO in FIG. 17(C) are approximately parallel. "Approximately coincident" and "approximately parallel" refer to angles of 5 degrees or less, and 2.5 degrees or less.
[0257] Thus, the FFT patterns and electron diffraction patterns show that the layered rock salt crystals and the rock salt crystals are oriented in the same direction. If they roughly match, the layered rock salt type has a 〈0003〉 orientation, and the rock salt type has a 〈11-1〉 orientation. In this case, these reciprocal lattice points are spot-like. It is preferable that the reciprocal lattice points are not continuous with other reciprocal lattice points. The lack of contiguous dots indicates high crystallinity.
[0258] As mentioned above, the 11-1 reflection of the cubic crystal and the 0003 reflection of the layered rock salt crystal are , are roughly the same, depending on the incident direction of the electron beam, the layered rock salt type 0003 reflection Spots that are not due to the layered salt type 0003 reflection are observed in the reciprocal space with a different orientation. For example, the spot marked B in Fig. 17(C) is a layered rock salt type 1014 This is due to the reciprocal lattice point (Figure 17) from the 0003 reflection of the layered rock salt type. (C) From the direction of A), the angle is 52° or more and 56° or less (i.e., ∠AOB is 52°). 0° to 56°), and d is observed in the area where d is 0.19 nm to 0.21 nm. Note that this index is just an example and does not necessarily have to match the actual index. For example, the reciprocal lattice points equivalent to 0003 and 1014 may be used.
[0259] Similarly, the 11-1 reflection of the cubic crystal is observed in a different reciprocal lattice space from that in which the 11-1 reflection of the cubic crystal is observed. A spot that is not due to a single reflection may be observed. For example, the spot marked with B in Figure 17(B) The spot is due to the 200 reflection of the cubic crystal. This is due to the 11-1 reflection of the cubic crystal. The angle is between 54° and 56° from the direction of the reflection (A in Figure 17(B)). Diffraction spots may be observed where the AOB angle is between 54° and 56°. Note that this index is just an example and does not necessarily have to match the actual index. For example, 11- Reciprocal lattice points equivalent to 1 and 200 may also be used.
[0260] In addition, the layered rock salt type positive electrode active material, including lithium cobalt oxide, has a (0003) plane and The (10-14) plane and its equivalents, as well as the (10-14) plane and its equivalents, appear as crystal faces. Therefore, when the shape of the positive electrode active material is observed carefully using a SEM, In order to make it easier to observe the (0003) plane, for example, in a TEM, the electron beam is focused on [12-1 It is possible to process the observation sample into a thin slice using FIB or other methods so that the incident light is 0. When determining whether the orientation is consistent, the (0003) plane of the layered rock salt type is easy to observe. Exfoliation is preferred.
[0261] However, the surface layer 100a is only MgO or only a structure in which MgO and CoO(II) are solid-solved. Therefore, the surface layer 100a is at least It contains cobalt, and in the discharged state, it also contains lithium, and has a route for lithium insertion and removal. It is also preferable that the concentration of cobalt is higher than that of magnesium.
[0262] In addition, the additive element X is located in the surface layer portion 100a of the positive electrode active material 100 according to one embodiment of the present invention. For example, the positive electrode active material 100 according to one embodiment of the present invention includes a coating 10 having an additive element X. 4 may be covered.
[0263] ≪Grain boundary≫ The additive elements contained in the positive electrode active material 100 according to one embodiment of the present invention are distributed as described above. It is more preferable that the portion is unevenly distributed in the grain boundary 101 and its vicinity as shown in FIG. I wish.
[0264] More specifically, the magnesium concentration at and near the grain boundary 101 of the positive electrode active material 100 It is preferable that the grain boundary 101 and the other regions of the inner portion 100b are higher than those of the other regions of the inner portion 100b. The fluorine concentration in the vicinity is also preferably higher than in other regions of the interior 100b.
[0265] The grain boundary 101 is one of the planar defects. Therefore, like the grain surface, it is easily unstable and the crystal Therefore, the magnesium concentration at the grain boundary 101 and its vicinity is increased. The higher the concentration, the more effectively the change in the crystal structure can be suppressed.
[0266] In addition, when the magnesium concentration and fluorine concentration at and near the grain boundary 101 are high, Even if a crack occurs along the grain boundary 101 of the positive electrode active material 100 according to an embodiment of the present invention, The magnesium and fluorine concentrations are high near the surface where the cracks are generated. Therefore, it is possible to improve the corrosion resistance of the positive electrode active material against hydrofluoric acid even after cracks have occurred. can.
[0267] In this specification, the vicinity of the grain boundary 101 refers to a region within about 10 nm from the grain boundary. The grain boundary 101 refers to a surface where there is a change in the arrangement of atoms. It can be observed under a microscope. Specifically, it can be seen in an electron microscope image as a repetition of bright and dark lines. This refers to a point where the angle exceeds 5 degrees or where the crystal structure can no longer be observed.
[0268] ≪Particle size≫ If the particle size of the positive electrode active material 100 according to one embodiment of the present invention is too large, it becomes difficult for lithium to diffuse. However, when the active material is applied to the current collector, the surface of the active material layer becomes too rough. If it is too thin, it will be difficult to support the active material layer when it is applied to the current collector, and excessive reaction with the electrolyte may occur. Therefore, the median diameter (D50) is set to 1 μm or more and 100 μm or less. Preferably, the thickness is 2 μm or more and 40 μm or less, more preferably, 5 μm or more and 30 μm or less. It is more preferable that the thickness is 1 μm or less, or 1 μm or more and 40 μm or less. 30 μm or less is preferable. Or 2 μm or more and 100 μm or less is preferable. Or 2 μm or less Preferably, the thickness is 30 μm or less. Or, preferably, the thickness is 5 μm or more and 100 μm or less. Or, preferably, the thickness is 5 μm or more and 100 μm or less. It is preferable that the thickness is 40 μm or more.
[0269] <Analysis method> The present invention relates to a method for producing a positive electrode active material that exhibits an O3'-type or O3"-type crystal structure when the charge depth is high. Whether the positive electrode active material 100 is one embodiment of the positive electrode active material 100 or not can be determined by using a positive electrode having a positive electrode active material with a high depth of charge. , XRD, electron diffraction, neutron diffraction, electron spin resonance (ESR), nuclear magnetic resonance (NMR) In particular, XRD can be used to analyze the cobalt, etc., contained in the positive electrode active material. The symmetry of transition metals can be analyzed with high resolution, and the degree of crystallinity and crystal orientation can be compared. It is possible to analyze the periodic distortion of the lattice and the crystallite size. This is preferable in that sufficient accuracy can be obtained even if the poles are measured as they are.
[0270] As described above, the positive electrode active material 100 according to one embodiment of the present invention has a high degree of charge and a low degree of discharge. The characteristic of this battery is that the crystal structure changes little when it is in a deep charge state or discharge state. Materials with a crystal structure that exhibits large changes in charge ratios of 50 wt% or more have a high charge depth. It is not desirable because it cannot withstand discharge. It should be noted that some materials may not have the same structure as magnesium and fluorine. Although they have in common the fact that they are lithium cobalt oxides, the O3' and O4' types are and O3” type crystal structure is 60wt% or more, and H1-3 type crystal structure is 50wt% or more. % or more. At a given voltage, the crystals of O3' and O3" types The structure becomes nearly 100 wt%, and when the voltage is further increased, the H1-3 type crystal structure is formed. Therefore, when determining whether the positive electrode active material 100 is one embodiment of the present invention, To achieve this, analysis of the crystal structure, including XRD, is necessary.
[0271] However, when the positive electrode active material is in a highly charged or discharged state, the crystal structure changes when it is exposed to air. For example, the crystal structure of O3' and O3" may change to that of H1-3. Therefore, all samples were placed in an inert atmosphere such as argon. It is preferable to handle it with care.
[0272] ≪Charging method≫ A high-temperature method for determining whether a certain composite oxide is the positive electrode active material 100 of one embodiment of the present invention Voltage charging is done by using a coin cell (CR2032 type, diameter 20 mm height) with lithium as the counter electrode. 3.2mm) can be created and charged.
[0273] More specifically, for the positive electrode, a slurry containing a positive electrode active material, a conductive material, and a binder is mixed, A coating of the positive electrode current collector made of aluminum foil can be used.
[0274] The counter electrode can be made of lithium metal. However, if a material other than lithium metal is used for the counter electrode, When the secondary battery is in a charged state, the potential of the secondary battery is different from the potential of the positive electrode. Unless otherwise specified, the potential is that of the positive electrode.
[0275] The electrolyte used in the electrolytic solution is 1 mol / L lithium hexafluorophosphate (LiPF6). The electrolyte contains ethylene carbonate (EC) and diethyl carbonate (DEC). C:DEC=3:7 (volume ratio), vinylene carbonate (VC) was mixed at 2 wt%. can be used.
[0276] The separator can be a 25 μm thick porous polypropylene film.
[0277] The positive and negative electrode cans may be made of stainless steel (SUS). do.
[0278] The coin cell made under the above conditions was then charged to any voltage (e.g., 4.5V, 4.55V, 4.6 V, 4.65V, 4.7V, 4.75V or 4.8V) and current of 10mA / g(1 The battery was charged at a constant current of 0.05C when C was 200mA / g. The phase change of the positive electrode active material was observed. In order to achieve this, it is desirable to charge the battery at such a low current value. After charging in this way, the coin cell was placed in a globe with an argon atmosphere. If you disassemble it in the box and take out the positive electrode, you can obtain a positive electrode active material with a high degree of charge. When performing various analyses, the container must be sealed in an argon atmosphere to prevent reactions with external components. For example, XRD can be performed in a sealed container with an argon atmosphere. After the charging is completed, it is preferable to quickly remove the positive electrode and subject it to analysis. The time is preferably within 1 hour after the completion of the electrochemical reaction, and more preferably within 30 minutes.
[0279] In addition, when analyzing the crystal structure in the charged state after multiple charge / discharge cycles, the multiple charge / discharge cycles are The charging conditions may be different from those stated above. For example, charging can be performed at any voltage (e.g. 4.6V, 4.65V, 4.7V, 4.75V or 4.8V), current value 100mA / g (1C The battery was charged at a constant current of 0.5C (when the charge was 200mA / g), and then the current was increased to 10mA / g (1 Charge at a constant voltage until C reaches 0.05 C at 200 mA / g, and discharge at 2.5 V, 0 It can be discharged at constant current of .5C.
[0280] Furthermore, when analyzing the crystal structure in the discharged state after multiple charge / discharge cycles, for example at 2.5 V, Discharge at a constant current of 100mA / g (0.5C when 1C is 200mA / g). This can be done.
[0281] <XRD> The apparatus and conditions for the XRD measurement are not particularly limited. For example, the following apparatus and conditions are used: It can be measured by. XRD equipment: Bruker AXS, D8 ADVANCE X-ray source: CuKα1 ray Output: 40kV, 40mA Slit type: Div.Slit, 0.5° Detector: LynxEye Scan method: 2θ / θ continuous scan Measurement range (2θ): 15° to 90° Step width (2θ): 0.01° setting Counting time: 1 second / step Sample stage rotation: 15 rpm
[0282] If the sample is a powder, place it in a glass sample holder or grease it. The sample can be set up by sprinkling it on a silicon non-reflective plate. When the measurement sample is a positive electrode, the positive electrode is attached to the substrate with double-sided tape, and the positive electrode active material layer is It can be set to match the measurement surface required by the device.
[0283] The crystal structure of the O3' type and the H1-3 type crystal structure model are calculated using CuKα1 radiation. The ideal powder XRD patterns are shown in Figures 10, 12, 13(A) and 13(B). For comparison, LiCoO2(O3) at charge depth 0 and CoO2(O1) at charge depth 1 are The ideal XRD pattern calculated from the crystal structure of (A) and (B) is also shown. (B) shows the XRD patterns of the O3' type crystal structure and the H1-3 type crystal structure. FIG. 13(A) shows the region where 2θ is between 18° and 21°, and FIG. 13(B) shows the region where 2θ is between 18° and 21°. The area of the LiCoO2(O 3) and CoO2(O1) patterns are ICSD (Inorganic Crystal The crystal structure was obtained from the NMR Structure Database (see Non-Patent Document 4). It is one of the modules of Materials Studio (BIOVIA) The data was created using Reflex Powder Diffraction. The range is 15° to 75°, Step size=0.01, wavelength λ1=1.54056 2×10 -10 m and λ2 were not set, and Monochromator was set to single. The pattern of the H1-3 type crystal structure was similarly created from the crystal structure information described in Non-Patent Document 3. The pattern of the O3' type crystal structure was obtained from the XRD pattern of the positive electrode active material according to one embodiment of the present invention. The crystal structure was estimated and analyzed using TOPAS ver.3 (crystal structure analysis software manufactured by Bruker). (a) was used for fitting and the XRD pattern was created in the same manner as the others.
[0284] As shown in Figures 10 and 13, in the O3' type crystal structure, 2θ = 19.30 ± 0.2 0° (19.10° to 19.50°), and 2θ=45.55±0.10° (4 Diffraction peaks appear at angles between 2θ 5.45° and 45.65°. = 19.30 ± 0.10° (between 19.20° and 19.40°), and 2θ = 45. A sharp diffraction peak appears at 55±0.05° (45.50° or more and 45.60° or less). However, as shown in Figures 12 and 13, the H1-3 type crystal structure and CoO2(P-3m 1, O1), no peaks appear at these positions. Therefore, at high charge depths, Peaks appear at θ=19.30±0.20° and 2θ=45.55±0.10°. This can be said to be a feature of the positive electrode active material 100 of one embodiment of the present invention.
[0285] This is the XRD diffraction peak of the crystal structure at 0 charge depth and the crystal structure at a high charge depth. More specifically, the positions of the main diffraction peaks of both are close to each other. The difference in the positions at which the peaks appear in two or more of the above, more preferably three or more of the above, is 2θ= It can be said that the angle is 0.7 or less, and more preferably 2θ=0.5 or less.
[0286] Although not shown, in the O3″ type crystal structure, 2θ=19.47±0.10° (19.37 ° or more and 19.57° or less), and 2θ=45.62±0.05° (45.57° or more and 4 Diffraction peaks appear at 5.67° or less. H1-3 type crystal structure and CoO2(P-3 m1, O1), no peaks appear at these positions. Therefore, the higher charge depth Peaks appeared at 2θ=19.47±0.10° and 2θ=45.62±0.05°. This is a feature of the positive electrode active material 100 according to one embodiment of the present invention that is produced through initial heating. A higher charging depth is, for example, a charging voltage of 4.8V or higher. State of charge and / or charge depth is greater than 0.8 and less than or equal to 0.88, more specifically charge depth is This refers to a state between 0.83 and 0.85.
[0287] In addition, the positive electrode active material 100 according to one embodiment of the present invention is an O3′ type or an O3″ type when the charge depth is high. However, not all of the particles need to have the O3' or O3" type crystal structure. It may contain other crystal structures or may be partially amorphous. However, XRD When the pattern was subjected to Rietveld refinement, the crystal structures of O3' and O3" were identified. It is preferably 50% or more, more preferably 60% or more, and more preferably 66% or more. It is more preferable that the O3' type and O3" type crystal structures are 50% or more. If the ratio is 60% or more, and more preferably 66% or more, the positive electrode exhibits sufficiently excellent cycle characteristics. It can be used as an electrode active material.
[0288] In addition, even after more than 100 charge / discharge cycles from the start of the measurements, Rietveld analysis showed that The O3' and O3" crystal structures preferably account for 35% or more, and more preferably 40% or more. It is more preferable that the ratio is 43% or more, and further preferably 43% or more.
[0289] In addition, the sharpness of the diffraction peaks in the XRD pattern indicates high crystallinity. Each diffraction peak is preferably sharp, i.e., the half-width, for example, the full width at half maximum, is preferably narrow. Even if the peaks originate from the same crystalline phase, they may differ depending on the XRD measurement conditions and / or 2θ value. In the case of the measurement conditions described above, the peak observed at 2θ=43° to 46° is In the case of the saturation angle, the full width at half maximum is preferably 0.2° or less, and more preferably 0.15° or less. It is more preferable that the angle is 0.12° or less. However, not all peaks necessarily meet this requirement. If some peaks satisfy this requirement, the crystallinity of the crystal phase is high. Such high crystallinity contributes to stabilization of the crystal structure after charging.
[0290] In addition, the crystallite size of the O3' type crystal structure of the positive electrode active material particles is The charge / discharge current is reduced to only about 1 / 10 of that of CoO2(O3). Even under the XRD measurement conditions, a clear peak of the O3' type crystal structure was observed at high charge depths. On the other hand, in simple LiCoO2, some of the structures are similar to the O3' type crystal structure. Even if it is possible, the crystallite size will be small and the peak will be broad and small. The size can be determined from the half-width of the XRD peak.
[0291] As described above, in the positive electrode active material according to one embodiment of the present invention, the influence of the Jahn-Teller effect is small. The positive electrode active material according to one embodiment of the present invention has a layered rock salt type crystal structure and a transition It is preferable that the metal is mainly cobalt. In terms of quality, if the influence of the Jahn-Teller effect is small, other than cobalt, It may have a solid metal Z.
[0292] In the positive electrode active material, it was estimated using XRD analysis that the influence of the Jahn-Teller effect is small. We consider the range of lattice constants that can be determined.
[0293] FIG. 14 shows a positive electrode active material according to one embodiment of the present invention having a layered rock-salt crystal structure and containing cobalt and nickel. The lattice constants of the a-axis and c-axis were calculated using XRD for the case with a lattice Fig. 14(A) shows the results for the a-axis, and Fig. 14(B) shows the results for the c-axis. The XRD pattern shown is of the powder after the synthesis of the positive electrode active material, and before it was incorporated into the positive electrode. The nickel concentration on the horizontal axis is calculated by taking the sum of the number of cobalt and nickel atoms as 100%. The positive electrode active material was prepared in the same manner as in Figure 2, except that no aluminum source was used. It was prepared according to the method.
[0294] FIG. 15 shows a positive electrode active material according to one embodiment of the present invention having a layered rock-salt crystal structure and including cobalt and manganese. The lattice constants of the a-axis and c-axis were estimated using XRD in the case of The results are shown in Fig. 15(A) for the a-axis and Fig. 15(B) for the c-axis. The lattice constant was measured for the powder after synthesis of the positive electrode active material, before it was incorporated into the positive electrode. The manganese concentration on the horizontal axis is calculated by dividing the sum of the number of cobalt and manganese atoms by 10 The manganese concentration is shown when the positive electrode active material is a manganese source instead of a nickel source. The method was similar to that shown in FIG. 2 except that no aluminum source was used.
[0295] FIG. 14(C) shows the results of the lattice constant of the positive electrode active material shown in FIG. 14(A) and FIG. 14(B). The lattice constant of the a-axis divided by the lattice constant of the c-axis (a-axis / c-axis) is shown in Fig. 15. (C) shows the results of the lattice constants of the positive electrode active materials shown in Figs. 15(A) and 15(B). In this figure, the lattice constant of the a-axis is divided by the lattice constant of the c-axis (a-axis / c-axis).
[0296] From Figure 14(C), it is clear that the a-axis / c-axis tends to change significantly when the nickel concentration is 5% and 7.5%. At a nickel concentration of 7.5%, the distortion of the a-axis is large. At nickel concentrations below 7.5%, the Jahn-Teller distortion may be observed. This suggests that an excellent positive electrode active material with small strain can be obtained.
[0297] Next, from FIG. 15(A), when the manganese concentration is 5% or more, the behavior of the change in the lattice constant is This suggests that the Vegard's law is not followed. This suggests that the crystal structure is different. Therefore, the manganese concentration is preferably, for example, 4% or less. It is nice.
[0298] The above-mentioned ranges of nickel concentration and manganese concentration are necessarily set in the surface layer portion 100a. That is, the concentration in the surface layer 100a may be higher than the above concentration. There are cases where this is the case.
[0299] From the above, a preferable range of the lattice constant was considered, and it was found that the positive electrode In the active material, the state without charging / discharging or the discharged state that can be estimated from the XRD pattern In the layered rock-salt crystal structure of the positive electrode active material particles in this state, the lattice constant of the a-axis is 2. 814×10 -10 m or larger, 2.817×10 -10 Smaller than m and c-axis lattice The constant is 14.05 x 10 -10 m or larger, 14.07×10 -10 It is smaller than m The state in which no charging or discharging is performed is, for example, when preparing a positive electrode for a secondary battery. It may be in the form of a powder.
[0300] Alternatively, the layered rock salt type positive electrode active material in a state where no charge / discharge is performed or in a discharged state In the crystal structure, the lattice constant of the a-axis divided by the lattice constant of the c-axis (a-axis / c-axis) is 0.2 Preferably it is greater than 0000 and less than 0.20049.
[0301] Alternatively, the layered rock salt type positive electrode active material in a state where no charge / discharge is performed or in a discharged state In the crystal structure, when XRD analysis was performed, 2θ was 18.50° or more and 19.30° or less. A first peak is observed, and a second peak is observed at 2θ between 38.00° and 38.80°. may be observed.
[0302] The peak appearing in the powder XRD pattern occupies most of the volume of the positive electrode active material 100. This reflects the crystal structure of the inside 100b of the positive electrode active material 100. The crystal structure of the grain boundaries 101 and the like can be analyzed by electron beam diffraction or the like of a cross section of the positive electrode active material 100. can.
[0303] <Charging curve and dQ / dVvsV curve> The positive electrode active material 100 according to one embodiment of the present invention exhibits a characteristic voltage change as the charge depth increases. The change in voltage can be calculated by differentiating the capacity (Q) of the charging curve with the voltage (V) (dQ / d V) can be read from the dQ / dV vs V curve obtained by calculating the dQ Before and after the peak in the / dV vs V curve, a non-equilibrium phase change occurs, and the crystal structure changes significantly. In this specification, a non-equilibrium phase change refers to a change in a physical quantity. This refers to a phenomenon that causes a linear change.
[0304] The positive electrode active material 100 according to one embodiment of the present invention has a dQ / dV vs. V curve of approximately 4.55 V. The peak near 4.55 V is due to the O3 crystal structure. This reflects the change in voltage when the phase changes from the O3' type crystal structure to the O3' type crystal structure. The broad peak indicates that more energy is required to extract lithium than if the peak were sharp. This means that there is little change in the energy, i.e., little change in the crystal structure. The less the oxidation, the less the influence of the displacement of the CoO2 layer and the change in volume is, and therefore, preferable.
[0305] More specifically, in the dQ / dV vs V curve of the charging curve, 4.5 V or more and 4.6 V or less When the maximum value that appears on the first peak is taken as the first peak, the full width at half maximum of the first peak must be 0.10 V or more. In this specification, the half value of the first peak is preferably set to 1. The first minimum value of the overall width is the minimum value of the dQ / dV value that appears between 4.3V and 4.5V. The average value HWHM1 of the first peak and the first minimum value when the The first peak and the second minimum when the minimum value of the dQ / dV value that appears below is the second minimum value. The difference between the average value HWHM2 and
[0306] The charge for obtaining the dQ / dV vs V curve is, for example, 10mA / g (1C It can be charged at a constant current of 0.05C when the charge current is 200mA / g. When obtaining the dQ / dV value of the charge, discharge the battery to 2.5V at 0.5C before measuring. It is preferable to start the charging.
[0307] The data acquisition interval during charging can be set to, for example, 1 second intervals or 1 mV voltage fluctuation. The voltage and current at the time of the measurement can be set to be acquired. The current value and the time are integrated. is the charging capacity.
[0308] The difference between the nth and n+1th data of the charge capacity data is the nth data of the capacity change dQ. Similarly, the difference between the nth and n+1th data of the voltage data is the voltage change Let this be the nth value of dV.
[0309] However, when using the above data, the influence of minute noise is large, so the voltage and charging capacity For the difference, the dQ / dV value may be calculated from the moving average of a certain number of intervals. For example, it can be 500.
[0310] Specifically, calculate the average value of dQ from the nth to the n+500th, and similarly, calculate the average value of dV from the nth Calculate the average value from the th to n+500th. dQ(average of 500) / dV(average of 500) The average of the two values can be used as the dQ / dV value. Similarly, the moving average value of 500 intervals can be used for pressure.
[0311] In addition, when analyzing the dQ / dV vs V curve after multiple charge / discharge cycles, the multiple charge / discharge conditions The charging conditions may differ from those listed above. For example, charging can be done at any voltage (e.g. 4.6V , 4.65V, 4.7V, 4.75V or 4.8V), 0.5C (1C is 200mA / g) constant current charging, then constant voltage charging until the current value becomes 0.05C, and discharging is 2.5 V, constant current discharge at 0.5C.
[0312] In addition, at around 4.55V, the phase changes from O3 type crystal structure to O3' type crystal structure. At this time, the charge depth of the O3 type crystal structure is about 0.7. This is the charge depth explained in Figure 11. It has the same symmetry as the O3 type crystal structure at depth 0, but the distance between the CoO2 layers is slightly different. When distinguishing between O3 type crystal structures with different charge depths in the specification, etc., O3 The O3 type crystal structure is O3(2θ=18.85), and the O3 type crystal structure with a charge depth of about 0.7 is O3( 2θ=18.57) This is because 2θ is around 19° in the XRD measurement. This is because the position of the peak that appears corresponds to the CoO2 interlayer distance.
[0313] <Discharge curve and dQ / dVvsV curve> In addition, the positive electrode active material 100 according to one embodiment of the present invention can be charged at a high voltage, for example, at a current of 0.2 C or less. When discharging at the lower rates below, a characteristic voltage change may appear near the end of discharge. This change appears around 3.9V in the dQ / dV vs V curve obtained from the discharge curve. At least one peak must be present at a voltage lower than the peak voltage and up to 3.5 V. It can be clearly confirmed by.
[0314] ≪Current pause method≫ Additives such as magnesium contained in the surface layer of the positive electrode active material 100 according to one embodiment of the present invention The distribution of the additive elements may change slightly during repeated charging and discharging. Therefore, the electronic conductivity may be improved and the electronic resistance may be reduced in the early stage of the charge / discharge cycle. The electrical resistance at .1s) may drop.
[0315] For example, when comparing the nth (n is a natural number greater than 1) charge with the n+1th charge, The resistance component R(0.1s) with a fast response measured by the current rest method is n+1 As a result, the discharge capacity of the n+1th discharge may be lower than the nth discharge. When n is 1, that is, when comparing the first charge and the second charge, 2 The increase in the charge capacity of the third charger is possible even for positive electrode active materials that do not contain additive elements. Therefore, n is preferably, for example, 2 or more and 10 or less. However, in the initial stage of the charge / discharge cycle, This is not limited to this. The charge / discharge capacity is approximately the same as the rated capacity, for example, 97% or more of the rated capacity. It can be said that the charge / discharge cycle is in its early stage when the charge / discharge cycle has a value of 0.01.
[0316] <XPS> X-ray photoelectron spectroscopy (XPS) measures the surface to a depth of about 2 to 8 nm (usually 5 nm or less). Since it is possible to analyze the area at about half the depth of the surface layer 100a, In addition, narrow scan analysis can be used to quantitatively analyze the concentration of each element. The quantitative accuracy of XPS is usually about ±1 atomic percent. The detection limit is approximately 1 atomic %, depending on the element.
[0317] When the positive electrode active material 100 according to one embodiment of the present invention was subjected to XPS analysis, the number of atoms of the added element was The number of atoms of the transition metal M is preferably 1.6 times or more and 6.0 times or less, and more preferably 1.8 times or more and less than 4.0 times. More preferably, when the additive element is magnesium and the transition metal M is cobalt, The number of sodium atoms is preferably 1.6 to 6.0 times the number of cobalt atoms, and more preferably 1.8 to 6.0 times the number of cobalt atoms. The number of halogen atoms such as fluorine is preferably at least 4.0 times that of the transition metal M. The number is preferably 0.2 to 6.0 times, and more preferably 1.2 to 4.0 times.
[0318] When performing XPS analysis, for example, monochromatic aluminum Kα radiation should be used as the X-ray source. The take-off angle can be set to, for example, 45°. For example, with the following equipment and conditions: It can be measured. Measurement equipment: PHI Quantera II X-ray source: Monochromatic Al Kα (1486.6eV) Detection area: 100μmφ Detection depth: Approx. 4 to 5 nm (take-off angle 45°) Measurement spectrum: Wide scan, narrow scan of each detected element
[0319] In addition, when the positive electrode active material 100 according to one embodiment of the present invention was analyzed by XPS, fluorine and other elements were The peak showing the bond energy of the element is preferably 682 eV or more and less than 685 eV. More preferably, the bond energy of lithium fluoride is about 684.3 eV. The energy of 685 eV, and the binding energy of magnesium fluoride, 686 eV In other words, the positive electrode active material 100 according to one embodiment of the present invention contains fluorine. If present, it is preferred that the bond be other than lithium fluoride and magnesium fluoride.
[0320] Furthermore, when the positive electrode active material 100 according to one embodiment of the present invention was subjected to XPS analysis, magnesium The peak showing the bond energy of Zn with other elements is between 1302 eV and 1304 eV. It is preferable that the energy is about 1303 eV, and more preferable that the energy is about 1303 eV. This is a different value from the 1305 eV bond energy of sodium, and the bond energy of magnesium oxide In other words, the positive electrode active material 100 according to one embodiment of the present invention is magnesium When the bond has a structure other than that of magnesium fluoride, it is preferable that the bond is other than that of magnesium fluoride.
[0321] The additive elements preferably present in large amounts in the surface layer portion 100a include, for example, magnesium and arsenic. The concentration of aluminum measured by XPS etc. is different from that measured by ICP-MS (inductively coupled plasma mass spectrometry). ), or GD-MS (glow discharge mass spectrometry), etc. preferable.
[0322] Magnesium and aluminum were processed to expose their cross sections, and the cross sections were examined using TEM-E When analyzing using DX, the concentration of the surface layer 100a is higher than the concentration of the inside 100b. For example, in TEM-EDX analysis, the concentration of magnesium is It is preferable that the peak intensity is attenuated to 60% or less at a point 1 nm deep from the top. It is preferable that the peak intensity is attenuated to 30% or less at a depth of 2 nm from the top. For example, this can be done by using a FIB (Focused Ion Beam).
[0323] In XPS (X-ray photoelectron spectroscopy) analysis, the number of magnesium atoms is 1 / 1 the number of cobalt atoms. The preferable range is 0.4 to 1.5 times. The ratio of the number of sodium atoms, Mg / Co, is preferably 0.001 or more and 0.06 or less.
[0324] On the other hand, nickel contained in the transition metal M is not unevenly distributed in the surface layer portion 100a, and It is preferable that the additive elements are distributed throughout the entire grain. However, there may be regions where the additive elements are unevenly distributed. This does not apply if:
[0325] <ESR> As described above, in the positive electrode active material of one embodiment of the present invention, cobalt and nickel are used as the transition metal M. It is preferable that the alloy contains Co as an additive element and magnesium as an additive element. 3+ Ni 3+ and some Li + Mg 2+ It is preferred that the substituent is substituted with Li + Mg 2+ With the replacement of Ni 3+ is reduced to Ni 2+ Become In addition, some Li + Mg 2+ and with that, Mg 2+ Nearby Co 3+ is reduced to Co 2+ In addition, some Co 3+ Mg 2+ Replaced by As a result, Mg 2+ Nearby Co 3+ is oxidized to Co 4+ This may be the case.
[0326] Therefore, the positive electrode active material according to one embodiment of the present invention is Ni 2+ , Ni 3+ , Co 2+ and C o 4+ It is preferable that the positive electrode active material has at least one of the following: 2+ , Ni 3+ , Co 2+ and Co 4+ The spin density due to one or more of the following: 2. 0×10 17 spins / g or more 1.0×10 21 It is preferable that the ratio is less than spins / g. By using a positive electrode active material having the above-mentioned spin density, the crystal structure, especially in the charged state, This is preferable because it is stable. However, if the magnesium concentration is too high, Ni 2+ , Ni 3+ , Co 2+ and Co 4+ The spin density may be reduced due to one or more of the above.
[0327] The spin density in the positive electrode active material can be measured, for example, by the electron spin resonance (ESR) method. The analysis can be performed using techniques such as NMR (Spin Resonance).
[0328] EPMA EPMA (Electron Probe Microanalysis) allows for quantitative analysis of elements. The distribution of can be analyzed.
[0329] EPMA analyzes the area from the surface to a depth of about 1 μm. The results may differ from those obtained by other analytical methods. When performing XPS analysis, the concentration of the added element in the surface layer may be lower than the result of XPS. The concentration of the added elements present in the surface layer was also determined based on the results of ICP-MS or the positive electrode active material. This may be higher than the value determined by the raw material composition during the manufacturing process.
[0330] When a cross section of the positive electrode active material 100 according to one embodiment of the present invention was analyzed by EPMA, It is preferable that the concentration of the fluorine-containing compound has a concentration gradient in which the concentration of the fluorine-containing compound increases from the inside toward the surface layer. As shown in Figure 4(B1), magnesium, fluorine, titanium, and silicon are distributed from the inside to the surface. It is preferable that the concentration gradient increases toward the It is preferred that aluminum has a concentration peak in a region deeper than the concentration peaks of the above elements. The peak of aluminum concentration may be present in the surface layer or may be deeper than the surface layer. .
[0331] In addition, the surface and the surface layer of the positive electrode active material according to one embodiment of the present invention are chemically adsorbed after the preparation of the positive electrode active material. The electrolyte attached to the surface of the positive electrode active material does not include carbonates, hydroxyl groups, etc. The term "positive electrode active material" does not include the binder, conductive material, or compounds derived from these. When quantitatively analyzing the elements contained in a material, surface analysis such as XPS and EPMA is used. Corrections may be made to remove excess carbon, hydrogen, excess oxygen, excess fluorine, etc. that may be present. For example, XPS can separate the types of bonds by analysis, and CF bonds derived from binders can be A correction may be made to exclude such cases.
[0332] Furthermore, before being subjected to various analyses, the electrolyte, binder, conductive material, and In order to remove compounds derived from these, samples of the positive electrode active material and the positive electrode active material layer, etc. In this case, lithium may be dissolved in the solvent used for washing. However, even in this case, the added elements are difficult to dissolve, so the atomic ratio of the added elements It doesn't have any impact.
[0333] <Surface roughness and specific surface area> The positive electrode active material 100 of one embodiment of the present invention preferably has a smooth surface with few irregularities. The fact that the surface is smooth and has few irregularities indicates that the distribution of the additive elements in the surface layer portion 100a is good. This is one element that indicates something.
[0334] The surface is smooth and has few irregularities, for example, as seen in a cross-sectional SEM image of the positive electrode active material 100 or This can be determined from a cross-sectional TEM image, the specific surface area of the positive electrode active material 100, and the like.
[0335] For example, the surface smoothness of 100 positive electrode active material was quantified from a cross-sectional SEM image as shown below. It is possible.
[0336] First, the positive electrode active material 100 is processed by FIB or the like to expose a cross section. It is preferable to cover the positive electrode active material 100 with a protective agent or the like. Take an SEM image of the interface. Then, use image processing software to remove noise from the SEM image. For example, After Gaussian blurring (σ=2), the image is binarized. The interface is then extracted using image processing software. Further, an automatic selection tool or the like is used to select the interface line between the protective film or the like and the positive electrode active material 100, Extract the data into a spreadsheet program, etc. Use the functions of the spreadsheet program, etc. to create a regression curve (second-order After the slope correction, the roughness calculation parameters are obtained from the data, and the standard deviation The root mean square (RMS) surface roughness is calculated. The material has a surface roughness of at least 400 nm around the periphery of the particle.
[0337] In the particle surface of the positive electrode active material 100 of the present embodiment, the root mean square, which is an index of roughness, The root mean square (RMS) surface roughness is less than 3 nm, preferably less than 1 nm, and more preferably less than 0. A root mean square (RMS) surface roughness of less than 5 nm is preferred.
[0338] There is no particular restriction on the image processing software used for noise processing, boundary extraction, etc. For example, "ImageJ" described in Non-Patent Documents 5 to 7 can be used.
[0339] For example, the actual specific surface area A measured by the constant volume gas adsorption method R And the ideal ratio surface area A i The surface smoothness of the positive electrode active material 100 can also be quantified from the ratio of do.
[0340] Ideal specific surface area A i is that all particles have the same diameter as D50 and have the same weight The shape is calculated assuming an ideal sphere.
[0341] The median diameter D50 should be measured using a particle size distribution meter that uses the laser diffraction / scattering method. The specific surface area can be measured, for example, using a specific surface area measuring device that uses a constant volume gas adsorption method. Therefore, it can be measured.
[0342] The positive electrode active material 100 according to one embodiment of the present invention has an ideal specific surface area calculated from the median diameter D50. A i and the actual specific surface area A R Ratio of A R / A i It is preferable that the ratio is 2.1 or less.
[0343] Alternatively, the smoothness of the surface of the positive electrode active material 100 can be confirmed from a cross-sectional SEM image by the following method. The volume can be quantified.
[0344] First, a surface SEM image of the positive electrode active material 100 is obtained. The observation surface is preferably perpendicular to the electron beam. When comparing, the measurement conditions and observation area should be the same.
[0345] Next, the above SEM image is processed using image processing software (e.g., "ImageJ"), for example, The image converted to bits (called a grayscale image) is obtained. Grayscale Images contain luminance (brightness information). For example, in an 8-bit grayscale image, Brightness can be expressed in 2 to the power of 8 = 256 gradations. Dark areas have a lower number of gradations, and bright areas have a lower number of gradations. The number of gradations is higher in the part. The luminance change can be quantified in relation to the number of gradations. The numerical value is called the grayscale value. By obtaining the grayscale value, the unevenness of the positive electrode active material can be identified. It can be evaluated as a numerical value.
[0346] Furthermore, it is possible to express the luminance change of the target area as a histogram. It is also called a brightness histogram. By obtaining a totogram, it is possible to visually evaluate the unevenness of the positive electrode active material in an easily understandable manner. It becomes Noh.
[0347] In the positive electrode active material 100 according to one embodiment of the present invention, the difference between the maximum and minimum values of the gray scale is It is preferably 120 or less, more preferably 115 or less, and more preferably 70 to 11 It is more preferable that the standard deviation of the gray scale value is 11 or less. It is preferable that the number of the sieving ratios is 8 or less, more preferable that the number of the sieving ratios is 4 or more and 8 or less. preferable.
[0348] This embodiment mode can be used in combination with other embodiment modes.
[0349] (Embodiment 3) In this embodiment, an example of a secondary battery according to an aspect of the present invention will be described with reference to FIGS. 18 to 21.
[0350] <Example 1 of the Configuration of a Secondary Battery> Hereinafter, a secondary battery in which a positive electrode, a negative electrode, and an electrolytic solution are wrapped in an exterior body will be described as an example.
[0351] [Positive Electrode] The positive electrode has a positive electrode active material layer and a positive electrode current collector. The positive electrode active material layer has a positive electrode active material and may have a conductive material (which may also be referred to as a conductive assistant) and a binder. As the positive electrode active material, the positive electrode active material produced by the production method described in the previous embodiment is used.
[0352] Also, the positive electrode active material described in the previous embodiment may be mixed with other positive electrode active materials and used.
[0353] Examples of other positive electrode active materials include composite oxides having an olivine-type crystal structure, a layered rock salt-type crystal structure, or a spinel-type crystal structure. For example, compounds such as LiFePO4, LiFeO2, LiNiO2, LiMn2O4, V2O5, Cr2O5, and MnO2 can be mentioned.
[0354] Also, as another positive electrode active material, a lithium-containing material having a spinel-type crystal structure containing manganese such as LiMn2O4 is preferably mixed with lithium nickelate (LiNiO2 or LiNiMO2 (0 < x < 1) (M = Co, Al, etc.)). With this configuration, the characteristics of the secondary battery can be improved. 1-x M x
[0355] Also, as another positive electrode active material, a composition formula Lia Mn b M c O d Lithium can be expressed as A manganese composite oxide can be used. Here, element M is any element other than lithium and manganese. It is preferable to use a metal element selected from the group consisting of silicon and phosphorus, and nickel is preferable. It is more preferable that the measurement is performed on the whole particle of the lithium manganese composite oxide. 0 <a / (b+c)<2、かつc>0 during discharge, and 0.26≦(b+c) / d<0.5 It is preferable that the metal, silicon, and other components of the lithium manganese composite oxide particles are The composition of phosphorus, etc. is measured using, for example, an ICP-MS (inductively coupled plasma mass spectrometer). The oxygen composition of the entire lithium manganese composite oxide particle can be, for example, It can be measured using EDX (energy dispersive X-ray analysis). Combined with P-MS analysis, fusion gas analysis and XAFS (X-ray absorption fine structure) analysis for charge evaluation The lithium manganese composite oxide is at least Also refers to oxides containing lithium and manganese, and oxides containing chromium, cobalt, aluminum, nickel, etc. Ru, iron, magnesium, molybdenum, zinc, indium, gallium, copper, titanium, niobium , silicon, and phosphorus, Good too.
[0356] As an example, the active material layer 200 is formed by adding graphene or a graphene compound as a conductive material. An example of a cross-sectional configuration when used will be described.
[0357] 18A shows a vertical cross-sectional view of the active material layer 200. The active material layer 200 is made of granular positive electrode active material. The conductive material 100 is a graphene or graphene compound 201 as a conductive material, and a binder (Figure (not shown) and
[0358] In this specification and the like, the graphene compound 201 refers to multi-layer graphene, multi-graphene, Graphene oxide, multi-layer graphene oxide, multi-graphene oxide, reduced graphene oxide Graphene, reduced multi-layer graphene oxide, reduced multi-graphene oxide, graphene quantum Graphene compounds include those that have carbon and have a shape such as a plate or sheet. The term refers to a two-dimensional structure formed by a six-membered carbon ring. The two-dimensional structure may be referred to as a carbon sheet. The graphene compound may have a functional group. The graphene compound preferably has a curved shape. It may also be curled up into a shape similar to carbon nanofiber.
[0359] In this specification and the like, graphene oxide refers to a material that contains carbon and oxygen and has a sheet-like shape. This refers to those having functional groups, particularly epoxy groups, carboxy groups, or hydroxy groups.
[0360] In this specification and the like, reduced graphene oxide refers to a graphene oxide having carbon and oxygen and having a sheet-like shape. It has a two-dimensional structure formed by six-membered carbon rings. Although a single sheet of reduced graphene oxide can function, multiple sheets can also be stacked. Reduced graphene oxide has a carbon concentration greater than 80 atomic % and oxygen It is preferable that the concentration of the fluorine-containing compound is 2 atomic % or more and 15 atomic % or less. By setting the carbon and oxygen concentrations in this range, even a small amount of the material can be used as a highly conductive material. In addition, reduced graphene oxide exhibits a Raman spectrum It is preferable that the intensity ratio G / D of the G band to the D band is 1 or more. A certain type of reduced graphene oxide can function as a highly conductive material even in small amounts. Cut.
[0361] Graphene compounds have excellent electrical properties, such as high electrical conductivity, as well as high flexibility and In addition, graphene may have excellent physical properties such as high mechanical strength. The compound has a sheet-like shape. The graphene compound may have curved surfaces, and the bonding In addition, even if it is thin, it can have very high conductivity, so it is difficult to Therefore, a conductive path can be efficiently formed in the active material layer with a small amount of By using the compound as a conductive material, it is possible to increase the contact area between the active material and the conductive material. It is preferable that the graphene compound covers 80% or more of the area of the active material. It is preferable that the phene compound is attached to at least a part of the active material particles. It is preferable that the laphene compound overlaps at least a part of the active material particles. It is preferable that the shape of the laphene compound at least partially coincides with the shape of the active material particles. The shape of the active material particles may be, for example, the unevenness of a single active material particle or the unevenness of a plurality of active material particles. The graphene compound is at least part of the active material particles. It is preferable that the graphene compound surrounds at least a part of the graphene. In addition, the graphene compound may have holes.
[0362] When using active material particles with a small particle size, for example, active material particles with a particle size of 1 μm or less, The specific surface area of the active material particles is large, and more conductive paths are required to connect the active material particles together. In such cases, a graphene compound that can efficiently form a conductive path even in a small amount is used. It is preferable to use it.
[0363] Due to the above-mentioned properties, the grade is used for secondary batteries that require rapid charging and rapid discharging. It is particularly effective to use laphene compounds as conductive materials. Dual-purpose secondary batteries, secondary batteries for drones, etc., require rapid charging and rapid discharging characteristics In addition, there are cases where rapid charging characteristics are required for mobile electronic devices. And rapid discharge can be referred to as high rate charging and high rate discharging. For example, 1C , 2C, or 5C or higher charging and discharging.
[0364] In the vertical cross section of the active material layer 200, as shown in FIG. 18(B), In the graphene or graphene compound 201, the sheet-like graphene or graphene compound 201 is dispersed almost uniformly. In FIG. 18(B), graphene or a graphene compound 201 is shown in bold. Although it is said to be a thin film, it is actually a single or multiple layer of carbon molecules. Alternatively, the graphene compound 201 is arranged so as to partially cover the plurality of granular positive electrode active materials 100. Since the positive electrode active material 100 is formed so as to be attached to the surface of the positive electrode active material 100, the positive electrode active material 100 is formed so as to be attached to the surface of the positive electrode active material 100. There is surface contact.
[0365] Here, a plurality of graphenes or graphene compounds are bonded to each other to form a mesh-like structure. Graphene compound sheet (hereinafter referred to as graphene compound net or graphene net) When the active material is covered with a graphene net, the graphene net The binder can also function as a binder that binds the active materials together. This allows the amount of electrode to be reduced or eliminated, thus reducing the electrode volume and weight. In other words, the charge and discharge capacity of the secondary battery can be increased. can be increased.
[0366] Here, graphene oxide is used as the graphene or graphene compound 201, and the active material It is preferable to mix the above to form a layer that will become the active material layer 200, and then reduce the layer. The active material layer preferably comprises reduced graphene oxide. To form the graphene compound 201, graphene oxide, which has extremely high dispersibility in polar solvents, is used. As a result, the graphene or graphene compound 201 is formed inside the active material layer 200. From the dispersion medium containing uniformly dispersed graphene oxide, The solvent is removed by volatilization and the graphene oxide is reduced, so that the graphene remaining in the active material layer 200 is The ene or graphene compound 201 is dispersed to such an extent that it partially overlaps and is in surface contact with each other. By using the graphene oxide as a conductive layer, a three-dimensional conductive path can be formed. The reduction may be carried out, for example, by heat treatment or by using a reducing agent.
[0367] Therefore, unlike granular conductive materials such as acetylene black, which make point contact with the active material, graphene In addition, since the graphene compound 201 enables surface contact with low contact resistance, A granular positive electrode active material 100 and graphene or graphene compound 2 are used in a smaller amount than ordinary conductive materials. Therefore, the electrical conductivity between the active material layer 2 of the positive electrode active material 100 and the active material layer 2 of the positive electrode active material 100 can be improved. 00. This increases the discharge capacity of the secondary battery. It is possible to do so.
[0368] In addition, the entire surface of the active material is covered with a conductive material in advance by using a spray dryer. The graphene compound is formed as a coating, and the active material is further conductively connected to the graphene compound. You can also create a path.
[0369] In addition, the graphene compound is mixed with the materials used to form the graphene compound to form an active material. It may be used in the material layer 200. For example, it may be used as a catalyst in forming a graphene compound. The particles of the graphene compound may be mixed with the graphene compound. Examples of the catalyst include silicon oxide (SiO2, SiO x (x<2)), aluminum oxide Particles having iron, nickel, ruthenium, iridium, platinum, copper, germanium, etc. The particles preferably have a median diameter (D50) of 1 μm or less, and It is more preferable that the thickness is less than or equal to nm.
[0370] [Binder] Examples of binders include styrene-butadiene rubber (SBR) and styrene-isoprene. Acrylonitrile-styrene rubber, butadiene rubber, ethylene-styrene rubber, acrylonitrile-butadiene rubber, butadiene rubber, It is preferable to use a rubber material such as a propylene-diene copolymer. Fluorine rubber can be used.
[0371] As the binder, it is preferable to use, for example, a water-soluble polymer. As the molecule, for example, polysaccharides can be used. CMC, methyl cellulose, ethyl cellulose, hydroxypropyl cellulose Cellulose derivatives such as cellulose, diacetyl cellulose, and regenerated cellulose; starch, etc. One or more of these can be used. In addition, these water-soluble polymers can be used in combination with the above-mentioned rubber material. It is more preferable to use them in combination.
[0372] Alternatively, the binder may be polystyrene, polymethyl acrylate, or polymethyl methacrylate. (Polymethylmethacrylate, PMMA), Sodium polyacrylate, Polyvinyl Alcohol (PVA), polyethylene oxide (PEO), polypropylene oxide, Polyimide, polyvinyl chloride, polytetrafluoroethylene, polyethylene, polypropylene Polyisobutylene, Polyethylene terephthalate, Nylon, Polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), ethylene propylene diene polymer, It is preferable to use materials such as polyvinyl acetate and nitrocellulose.
[0373] The binder may be used in combination of two or more of the above.
[0374] For example, a material having a particularly excellent viscosity adjusting effect may be used in combination with other materials. For example, rubber materials have excellent adhesive strength and / or elasticity, but when mixed with a solvent, they have high viscosity. In such cases, it may be difficult to adjust the viscosity. It is preferable to mix them. Examples of materials that have a particularly excellent viscosity adjusting effect include water-soluble polymers. In addition, the above-mentioned polysaccharides are water-soluble polymers that are particularly effective in adjusting viscosity. , such as carboxymethylcellulose (CMC), methylcellulose, ethylcellulose cellulose, hydroxypropyl cellulose, diacetyl cellulose, regenerated cellulose, etc. For example, cellulose derivatives, starch, etc. can be used.
[0375] In addition, cellulose derivatives such as carboxymethyl cellulose are, for example, carboxymethyl The solubility of cellulose is increased by making it into a salt such as sodium salt or ammonium salt. This makes it easier for the agent to exert its effect as a viscosity adjuster. It is also possible to improve the dispersibility of the active material and other components when preparing a slurry. In the specification, cellulose and cellulose derivatives used as binders for electrodes are In the above cases, the term also includes salts thereof.
[0376] The water-soluble polymer stabilizes the viscosity by dissolving in water, and also acts as an active material and a binder. Other materials that are combined with it, such as styrene butadiene rubber, are stable in aqueous solution. In addition, since it has functional groups, it is easy to stably adsorb onto the surface of the active material. It is expected that cellulose derivatives such as carboxymethyl cellulose can be used. Many of the materials have functional groups, such as hydroxyl groups and carboxyl groups. Therefore, it is expected that the polymers will interact with each other and widely cover the surface of the active material.
[0377] When the binder that covers or contacts the surface of the active material forms a film, it is called a passive film. It is expected that the passive film will also play a role in preventing the decomposition of the electrolyte. A film with no electrical conductivity or extremely low electrical conductivity is used. For example, When a dynamic membrane is formed, it is possible to suppress the decomposition of the electrolyte at the battery reaction potential. In addition, the passive film suppresses electrical conductivity while allowing lithium ions to conduct. And even more desirable.
[0378] [Positive electrode current collector] The positive electrode current collector may be made of metals such as stainless steel, gold, platinum, aluminum, titanium, or the like. In addition, the material used for the positive electrode current collector can be an alloy of these materials, which has high electrical conductivity. It is preferable that the material does not dissolve at the potential of the positive electrode. Aluminum alloys containing elements such as indium and molybdenum that improve heat resistance are used. It can also be formed from a metal element that reacts with silicon to form a silicide. Metal elements that react with silicon to form silicide include zirconium, titanium, and Tantalum, hafnium, vanadium, niobium, tantalum, chromium, molybdenum, tungsten , cobalt, nickel, etc. The positive electrode current collector is available in foil, plate, sheet, mesh, punch, etc. The positive electrode current collector may be in the form of a metal, an expanded metal, or the like. It is advisable to use a thickness of 5 μm or more and 30 μm or less.
[0379] [Negative electrode] The negative electrode has a negative electrode active material layer and a negative electrode current collector. The negative electrode active material layer includes a conductive material and It may contain a binder.
[0380] [Negative electrode active material] As the negative electrode active material, for example, an alloy-based material and / or a carbon-based material can be used. do.
[0381] As a negative electrode active material, it is possible to carry out charge / discharge reactions by alloying / de-alloying reactions with lithium. For example, silicon, tin, gallium, aluminum, and Rumanium, lead, antimony, bismuth, silver, zinc, cadmium, indium, etc. Materials containing at least one of these elements can be used. These elements have a higher charge / discharge capacity than carbon. The amount of silicon is large, and silicon in particular has a high theoretical capacity of 4200mAh / g. It is preferable to use silicon as the material. Compounds containing these elements may also be used. For example, SiO, Mg2Si, Mg2Ge, SnO, SnO2, Mg2Sn, SnS 2, V2Sn3, FeSn2, CoSn2, Ni3Sn2, Cu6Sn5, Ag3Sn, Ag3Sb, Ni2MnSb, CeSb3, LaSn3, La3Co2Sn7, CoSb 3. InSb, SbSn, etc. Here, charging occurs by alloying and dealloying reactions with lithium. Elements capable of undergoing a discharge reaction and compounds containing such elements are called alloy materials. There is a match.
[0382] In this specification, SiO refers to, for example, silicon monoxide. Alternatively, SiO x Here, it is preferable that x has a value close to 1. For example, x is 0 It is preferably 0.2 or more and 1.5 or less, and more preferably 0.3 or more and 1.2 or less. The ratio is preferably from 0.3 to 1.5.
[0383] Carbon-based materials include graphite, graphitizable carbon (soft carbon), and non-graphitizable carbon (hard carbon). Carbon nanotubes, graphene, carbon black, etc. may be used. .
[0384] Examples of graphite include artificial graphite and natural graphite. Examples of artificial graphite include Mesocar Examples include Bonn Microbeads (MCMB), coke-based artificial graphite, and pitch-based artificial graphite. Here, as the artificial graphite, spherical graphite having a spherical shape can be used. For example, The MCMB may have a spherical shape, which is preferred. The MCMB also has a surface area of It is relatively easy to make the particles smaller, which may be preferable. Examples of the graphite include flake graphite and spherical natural graphite.
[0385] When lithium ions are inserted into graphite (the formation of lithium-graphite intercalation compounds), It shows a low potential similar to that of lithium metal (0.05V to 0.3V vs. Li / Li + This allows the lithium-ion secondary battery to exhibit a high operating voltage. In addition, graphite has a relatively high charge / discharge capacity per unit volume, a relatively small volume expansion, and is stable. Since it has the advantages of being highly valenced and being safer than lithium metal, it is preferred.
[0386] In addition, titanium dioxide (TiO2) and lithium titanium oxide (Li4T i5O 12 ), lithium-graphite intercalation compound (Li x C6), niobium pentoxide (Nb2O5) Oxides such as tungsten oxide (WO2) and molybdenum oxide (MoO2) can be used. can.
[0387] In addition, the negative electrode active material is a composite nitride of lithium and transition metals, which has a Li3N structure. Li 3-x M x N (M=Co, Ni, Cu) can be used. For example, Li 2.6 Co 0.4 N3 has a large charge / discharge capacity (900mAh / g, 1890mAh / cm 3 ) And preferable.
[0388] When a composite nitride of lithium and transition metals is used, the negative electrode active material contains lithium ions, The positive electrode active material is made of V2O5, Cr3O8, etc., which do not contain lithium ions. It is preferable that the positive electrode active material contains lithium ions. The lithium ions contained in the positive electrode active material are first removed to form the negative electrode active material. A complex nitride of lithium and a transition metal can be used.
[0389] In addition, a material that undergoes a conversion reaction can also be used as the negative electrode active material. For example, Lithium oxide (LiO), cobalt oxide (CoO), nickel oxide (NiO), iron oxide (FeO), etc. A transition metal oxide that does not form an alloy with the negative electrode active material may be used. Further materials that are produced include Fe2O3, CuO, Cu2O, RuO2, Cr2O3, etc. oxide, CoS 0.89 , NiS, CuS and other sulfides, Zn3N2, Cu3N, Ge3 Nitrides such as N4, phosphides such as NiP2, FeP2, CoP3, FeF3, BiF3, etc. It also occurs with fluoride.
[0390] The conductive material and binder that can be contained in the negative electrode active material layer can be the same as those that can be contained in the positive electrode active material layer. The same conductive materials and binders that can be used can be used.
[0391] [Negative electrode current collector] The negative electrode current collector can be made of the same material as the positive electrode current collector. It is preferable to use a material that does not alloy with carrier ions such as lithium.
[0392] [Electrolyte] The electrolytic solution contains a solvent and an electrolyte. The solvent for the electrolytic solution is preferably an aprotic organic solvent. For example, ethylene carbonate (EC), propylene carbonate (PC), ethylene carbonate, chloroethylene carbonate, vinylene carbonate, gamma-butyrolactone lactone, γ-valerolactone, dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), methyl formate, methyl acetate, ethyl acetate ethyl propionate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, 1 ,3-dioxane, 1,4-dioxane, dimethoxyethane (DME), dimethylsulfur oxide, diethyl ether, methyl diglyme, acetonitrile, benzonitrile, tetrahydrofuran One of trihydrofuran, sulfolane, sultone, etc., or two or more of these Combinations and ratios may be used.
[0393] In addition, a flame-retardant and non-volatile ionic liquid (room-temperature molten salt) is used as the solvent for the electrolyte. By using one or more, the internal temperature of the secondary battery increases due to an internal short circuit or overcharging. Even if the battery is heated, it is possible to prevent the secondary battery from exploding and / or catching fire. The organic cations used in the electrolyte are composed of ions and anions. The cations used are quaternary ammonium cations, tertiary sulfonium cations, and quaternary phosphonium cations. Aliphatic onium cations such as nium cations, imidazolium cations and pyridinium The anions used in the electrolyte include aromatic cations such as cations. Amide anions, monovalent methide anions, fluorosulfonate anions, perfluor perfluoroalkylsulfonate anion, tetrafluoroborate anion, perfluoroalkyl Fluorophosphate anion, perfluoroalkane anion, xylphosphate anion and the like.
[0394] The electrolyte to be dissolved in the above solvent is, for example, LiPF6, LiClO4, Li AsF6, LiBF4, LiAlCl4, LiSCN, LiBr, LiI, Li2SO4 , Li2B 10 Cl 10 , Li2B 12 Cl 12 , LiCF3SO3, LiC4F9SO 3, LiC(CF3SO2)3, LiC(C2F5SO2)3, LiN(CF3SO2) 2. Lithium such as LiN(C4F9SO2)(CF3SO2) and LiN(C2F5SO2)2 Use one or more of these salts in any combination and ratio. can be done.
[0395] The electrolyte used in secondary batteries is made of granular waste or elements other than the constituent elements of the electrolyte (hereinafter simply referred to as It is preferable to use a highly purified electrolyte solution with a low content of "impurities." Specifically, the weight ratio of impurities to the electrolyte is 1% or less, preferably 0.1% or less, more preferably 1% or less. It is more preferable that the content is 0.01% or less.
[0396] In addition, vinylene carbonate, propane sultone (PS), and tert-butyl ether were used in the electrolyte. Benzene (TBB), Fluoroethylene carbonate (FEC), Lithium bis(oxalate) Lithium borate (LiBOB), as well as dinitriles such as succinonitrile and adiponitrile Additives such as compounds may be added. The concentration of the added material is, for example, The content should be between 0.1wt% and 5wt%. VC or LiBOB forms a good coating. This is particularly preferable.
[0397] Alternatively, a polymer gel electrolyte may be used in which a polymer is swollen with an electrolytic solution.
[0398] By using a polymer gel electrolyte, safety against leakage etc. is improved. It is possible to reduce the thickness and weight of the device.
[0399] The polymers that can be gelled include silicone gel, acrylic gel, acrylonitrile gel, Polyethylene oxide gel, polypropylene oxide gel, fluorine-based polymer A gel or the like can be used.
[0400] Examples of the polymer include polyalkylene oxides such as polyethylene oxide (PEO). Polymers with a fluororesin structure, PVDF, polyacrylonitrile, etc., and materials containing them For example, a copolymer of PVDF and hexafluoropropylene (HF The copolymer PVDF-HFP can be used. The substrate may have a porous shape.
[0401] In addition, a solid electrolyte having an inorganic material such as a sulfide or oxide instead of an electrolytic solution, It is possible to use solid electrolytes containing polymer materials such as PEO (polyethylene oxide) If a solid electrolyte is used, the installation of a separator and / or spacer is not required. In addition, since the entire battery can be solidified, there is no risk of leakage, and safety is greatly improved. Improve.
[0402] [Separator] The secondary battery preferably has a separator. The separator may be, for example, a paper. , nonwoven fabric, glass fiber, ceramics, or nylon (polyamide), vinylon (poly Vinyl alcohol fiber), polyester, acrylic, polyolefin, polyurethane The separator can be made of synthetic fibers or the like. It is preferable that the separator is processed into a shape such that it envelops either the positive electrode or the negative electrode.
[0403] The separator may be a multi-layer structure. For example, the separator may be made of an organic material such as polypropylene or polyethylene. The material film is made of ceramic, fluorine, polyamide, or a mixture of these materials. The ceramic material can be, for example, aluminum oxide. Examples of the fluorine-based material include fluorine particles, silicon oxide particles, etc. PVDF, polytetrafluoroethylene, etc. can be used. For example, nylon, aramid (meta-aramid, para-aramid), etc. can be used. can.
[0404] Coating with ceramic materials improves oxidation resistance, making it ideal for separators during high-voltage charging and discharging. This suppresses the deterioration of the capacitor and improves the reliability of the secondary battery. By coating the electrode, the separator and the electrode are more easily adhered to each other, improving the output characteristics. Coating polyamide materials, especially aramid, improves heat resistance, which contributes to the safety of secondary batteries. This can improve safety.
[0405] For example, a polypropylene film is coated on both sides with a mixture of aluminum oxide and aramid. Alternatively, aluminum oxide may be applied to the surface of the polypropylene film that comes into contact with the positive electrode. Alternatively, the surface in contact with the negative electrode may be coated with a mixed material of carbon and aramid, and then coated with a fluorine-based material.
[0406] By using a multi-layered separator, the safety of the secondary battery can be ensured even if the overall thickness of the separator is thin. Since the charge / discharge capacity per unit volume of the secondary battery can be increased, the charge / discharge capacity per unit volume of the secondary battery can be increased.
[0407] [Exterior body] The exterior body of the secondary battery is made of, for example, a metal material such as aluminum and / or a resin. A resin material can be used. A film-like outer casing can also be used. Examples of the polymers include polyethylene, polypropylene, polycarbonate, ionomer, Flexible materials such as aluminum, stainless steel, copper, and nickel are applied to a film made of a material such as polyamide. A thin metal film having excellent thermal conductivity is then applied on the thin metal film, and a polyamide resin is applied on the outer surface of the exterior body. In addition, a three-layer film having an insulating synthetic resin film such as a polyester resin may be used. can.
[0408] <Secondary battery configuration example 2> As an example of the configuration of a secondary battery, the configuration of a secondary battery using a solid electrolyte layer will be described below. Reveal.
[0409] As shown in FIG. 19A, a secondary battery 400 of one embodiment of the present invention includes a positive electrode 410, a solid electrolyte The positive electrode 430 has a porous layer 420 and a negative electrode 430 .
[0410] The positive electrode 410 includes a positive electrode current collector 413 and a positive electrode active material layer 414. The positive electrode active material 411 and the solid electrolyte 421 are the same as those in the previous embodiment. The positive electrode active material layer 41 is made of the positive electrode active material prepared by the method described above. 4 may include a conductive material and a binder.
[0411] The solid electrolyte layer 420 includes a solid electrolyte 421. The solid electrolyte layer 420 includes a positive electrode 410 and The negative electrode 430 is located between the positive electrode 411 and the negative electrode 431. It is an area.
[0412] The negative electrode 430 includes a negative electrode current collector 433 and a negative electrode active material layer 434. The negative electrode active material layer 434 has a conductive material and a solid electrolyte 421. In addition, when lithium metal is used for the negative electrode 430, 19(B), a negative electrode 430 not including a solid electrolyte 421 can be obtained. When lithium metal is used for the negative electrode 430, the energy density of the secondary battery 400 can be improved. This is preferable.
[0413] The solid electrolyte 421 of the solid electrolyte layer 420 may be, for example, a sulfide-based solid electrolyte, an acid A nitride-based solid electrolyte, a halide-based solid electrolyte, or the like can be used.
[0414] Sulfide-based solid electrolytes include thiolithium-based (Li 10 GeP2S 12 , Li 3.25 Ge 0.25 P 0.75 S4, etc.), sulfide glass (70Li2S・30P2S5, 30Li2 S·26B2S3·44LiI, 63Li2S·36SiS2·1Li3PO4, 57L i2S・38SiS2・5Li4SiO4, 50Li2S・50GeS2, etc.), sulfide crystals Crystallized glass (Li7P3S 11 , Li3.25 P 0.95 S4, etc.) are included. Solid electrolytes are materials with high conductivity, can be synthesized at low temperatures, and are relatively soft. This has the advantage that the conductive path is easily maintained even after charging and discharging.
[0415] Oxide-based solid electrolytes include materials with a perovskite crystal structure (La 2 / 3-x Li 3x TiO3, etc.), materials with NASICON type crystal structure (Li 1-x Al x Ti 2- x (PO4)3, etc.), materials with garnet-type crystal structure (Li7La3Zr2O 12 etc. ), materials with LISICON-type crystal structure (Li 14 ZnGeO 16 etc.), LLZO (Li7La3Zr2O 12 ), oxide glass (Li3PO4-Li4SiO4, 50L i4SiO4·50Li3BO3, etc.), oxide crystallized glass (Li 1.07 Al 0.69 Ti 1.46 (PO4)3, Li 1.5 Al 0.5 Ge 1.5 (PO4)3 etc. Oxide-based solid electrolytes have the advantage of being stable in the air.
[0416] Halide solid electrolytes include LiAlCl4, Li3InBr6, LiF, and LiCl These halide-based solid electrolytes are also used as porous electrolytes. Composite materials containing aluminum oxide and / or porous silica filled into the pores are also solidified. It can be used as a body electrolyte.
[0417] Further, different solid electrolytes may be mixed and used.
[0418] Among them, Li having a NASICON-type crystal structure 1+x Al x Ti 2-x (PO4)3( 0 < x < 1) (hereinafter referred to as LATP) contains aluminum and titanium, which are elements that the positive electrode active material used in the secondary battery 400 of one aspect of the present invention may have. Therefore, a synergistic effect can be expected with respect to the improvement of cycle characteristics, which is preferable. Further, an improvement in productivity due to the reduction of processes can also be expected. In the present specification and the like, the NASICON-type crystal structure is a compound represented by M2(XO4)3 (M: transition metal, X: S, P, As, Mo, W, etc.), and has a structure in which MO6 octahedrons and XO4 tetrahedrons share vertices and are three-dimensionally arranged. [Shape of the exterior body and the secondary battery] For the exterior body of the secondary battery 400 of one aspect of the present invention, those of various materials and shapes can be used, but it preferably has a function of pressing the positive electrode, the solid electrolyte layer, and the negative electrode.
[0419] For example, FIG. 20 is an example of a cell for evaluating the materials of an all-solid-state battery.
[0420]
[0421] FIG. 20(A) is a schematic cross-sectional view of the evaluation cell. The evaluation cell has a lower member 761, an upper member 762, and fixing screws or wing nuts 764 for fixing them. By rotating the pressing screw 763, the electrode plate 753 is pressed to fix the evaluation material. An insulator 766 is provided between the lower member 761 and the upper member 762, which are made of stainless steel. An O-ring 765 for sealing is provided between the upper member 762 and the pressing screw 763.
[0422] The evaluation material is placed on an electrode plate 751 and surrounded by an insulating tube 752. The electrode plate 753 is in a pressed state. The figure is FIG. 20(B).
[0423] As an example of the evaluation material, a laminate of a positive electrode 750a, a solid electrolyte layer 750b, and a negative electrode 750c is shown. The cross-sectional view is shown in FIG. 20(C). The same reference numerals are used for the same parts.
[0424] The electrode plate 751 and the lower member 761 electrically connected to the positive electrode 750a It can be said that the electrode plate is equivalent to a terminal. The electrode plate 753 and the upper member 762 can be said to correspond to a negative terminal. The material to be evaluated is subjected to pressure via the electrode plate 751 and the electrode plate 753 while measuring the electrical resistance, etc. can be measured.
[0425] In addition, a package having excellent airtightness is used for the exterior body of the secondary battery according to one embodiment of the present invention. For example, it is preferable to use a ceramic package and / or a resin package. In addition, when sealing the exterior body, the outside air is blocked and the device is placed in a sealed atmosphere, for example, It is preferably carried out in a lobe box.
[0426] FIG. 21A shows a secondary battery according to one embodiment of the present invention having an exterior body and a shape different from those in FIG. The secondary battery in FIG. 21(A) has external electrodes 771 and 772 and is made up of a plurality of packages. It is sealed with an exterior body having a cage member.
[0427] An example of a cross section taken along the dashed line in FIG. 21(A) is shown in FIG. 21(B). The laminate having the solid electrolyte layer 750b and the negative electrode 750c has an electrode layer 773a provided on a flat plate. The package member 770a is a frame-shaped package member 770b, and the electrode layer 7 The package member 770c in which the semiconductor device 73b is provided is enclosed and sealed. The package members 770a, 770b, and 770c are made of an insulating material, such as a resin material and and / or ceramics may be used.
[0428] The external electrode 771 is electrically connected to the positive electrode 750a via the electrode layer 773a, and serves as a positive electrode terminal The external electrode 772 is electrically connected to the negative electrode 750c via the electrode layer 773b. It is connected directly to the positive terminal and functions as the negative terminal.
[0429] This embodiment mode can be implemented in appropriate combination with other embodiment modes.
[0430] (Embodiment 4) In this embodiment, an example of the shape of the secondary battery having the positive electrode described in the previous embodiment will be described. The materials used in the secondary battery described in this embodiment are the same as those described in the previous embodiment. I can pour drinks.
[0431] <Coin-type secondary battery> First, an example of a coin-type secondary battery will be described. FIG. 22(A) shows a coin-type (single-layer flat type) 22(A) is a cross-sectional view of the secondary battery shown in FIG. 22(A).
[0432] The coin-type secondary battery 300 has a positive electrode can 301 that also serves as a positive electrode terminal and a negative electrode can 302 that also serves as a negative electrode terminal. 302 is insulated and sealed by a gasket 303 made of polypropylene or the like. The positive electrode 304 is composed of a positive electrode current collector 305 and a positive electrode active material layer 306 provided in contact with the positive electrode current collector 305. The negative electrode 307 is formed by contacting a negative electrode current collector 308. The negative electrode active material layer 309 is formed by bonding the negative electrode active material layer 309 to the negative electrode.
[0433] The positive electrode 304 and the negative electrode 307 used in the coin-type secondary battery 300 are each an active material. The barrier layer need only be formed on one side.
[0434] The positive electrode can 301 and the negative electrode can 302 are made of nickel or aluminum, which is resistant to corrosion by the electrolyte. , titanium, or alloys thereof and / or alloys thereof with other metals (e.g. Stainless steel, etc.) can be used. In addition, nickel is used to prevent corrosion by the electrolyte. and / or aluminum. The positive electrode can 301 is connected to the positive electrode 304. , and the negative electrode can 302 are electrically connected to the negative electrode 307 .
[0435] The negative electrode 307, the positive electrode 304, and the separator 310 are impregnated with an electrolyte, and the negative electrode 307, the positive electrode 304, and the separator 310 are impregnated with an electrolyte. As shown in FIG. 1, the positive electrode can 301 is placed downward, and the positive electrode 304, the separator 310, the negative electrode 307, The positive electrode can 301 and the negative electrode can 302 are stacked in this order, and the positive electrode can 301 and the negative electrode can 302 are secured together with a gasket 303 interposed therebetween. Then, the laminate is pressed to manufacture a coin-type secondary battery 300.
[0436] By using the positive electrode active material described in the above embodiment for the positive electrode 304, the charge and discharge capacity is high. The coin-type secondary battery 300 can have excellent cycle characteristics.
[0437] Here, the flow of current during charging of a secondary battery will be explained with reference to FIG. When a secondary battery is considered as a closed circuit, the movement of lithium ions and the flow of electric current are in the same direction. In secondary batteries that use lithium, the anode and cathode are connected by charging and discharging. The cathode (cathode) is switched, and the oxidation and reduction reactions are switched, so the reaction potential The electrode with the higher reaction potential is called the positive electrode, and the electrode with the lower reaction potential is called the negative electrode. In this case, the charge / discharge current is always the same whether the battery is charging or discharging or a reverse pulse current is applied. Even when an electric current flows through the positive electrode, it is called the "positive electrode" or "+ electrode (plus electrode)" and the negative electrode The negative electrode is called the "negative electrode" or "-electrode (minus electrode)". The related terms anode and cathode are used during charging and discharging. At times, the anode is the opposite, which can be confusing. The terms cathode and cathode are not used in this specification. When using the terms node (anode) and cathode (negative electrode), it is important to consider whether the Also indicate whether it corresponds to a positive electrode (plus electrode) or a negative electrode (minus electrode). It is decided.
[0438] A charger is connected to the two terminals shown in FIG. 22(C) to charge the secondary battery 300. As the charging of the secondary battery 300 progresses, the potential difference between the electrodes increases.
[0439] <Cylindrical secondary battery> Next, an example of a cylindrical secondary battery will be described with reference to FIG. FIG. 23(A) shows an external view of the cylindrical secondary battery 600. FIG. 23(B) shows a schematic cross section of the cylindrical secondary battery 600. As shown in FIG. 23(B), the cylindrical secondary battery 600 has a positive electrode on the upper surface. It has a polar cap (battery lid) 601 and a battery can (outer can) 602 on the side and bottom. The positive electrode cap 601 and the battery can (outer can) 602 are connected by a gasket (insulating packing). It is insulated by 610 copper.
[0440] Inside a hollow cylindrical battery can 602, a strip-shaped positive electrode 604 and a strip-shaped negative electrode 606 are sandwiched between a separator 6 The battery element is wound around the sensor. The battery can 602 is wound around a turbopin. One end is closed and the other end is open. The battery can 602 is made of nickel, aluminum, titanium, or other material that is resistant to corrosion by the electrolyte. metals, or their alloys and / or alloys with other metals (e.g., stainless steel In addition, nickel and / or stainless steel can be used to prevent corrosion by the electrolyte. Alternatively, it is preferable to coat the battery can 602 with aluminum or the like. In the battery element, the positive electrode, the negative electrode, and the separator are wound, and the battery element is sandwiched between a pair of opposing insulating plates 6. The inside of the battery can 602 in which the battery element is provided is A non-aqueous electrolyte (not shown) is injected. The non-aqueous electrolyte is the same as that of a coin-type secondary battery. can be used.
[0441] The positive and negative electrodes used in cylindrical storage batteries are wound, so active materials are formed on both sides of the current collector. A positive electrode terminal (positive electrode current collector lead) 603 is connected to the positive electrode 604, and a negative electrode A negative electrode terminal (negative electrode current collecting lead) 607 is connected to the positive electrode terminal 603 and the negative electrode The terminal 607 may be made of a metal material such as aluminum. 3 is resistance welded to the safety valve mechanism 612, and the negative terminal 607 is resistance welded to the bottom of the battery can 602. The safety valve mechanism 612 is a PTC (Positive Temperature Coupling) element. The positive electrode cap 601 is electrically connected to the positive electrode cap 601 via a positive electrode cap 611. When the internal pressure of the battery increases beyond a certain threshold, the valve mechanism 612 closes the positive electrode cap 601 and the The PTC element 611 cuts off the electrical connection with the positive electrode 604. This is a thermal resistance element whose resistance increases when the temperature rises. The increase in resistance limits the amount of current and prevents abnormal It prevents heat generation. The PTC element is made of barium titanate (BaTiO3) based semiconductor. Conductive ceramics or the like can be used.
[0442] 23(C), a plurality of secondary batteries 600 are mounted on a conductive plate 613 and a conductive plate 614. The secondary batteries 600 may be sandwiched between the secondary batteries 600 to form a module 615. They may be connected in series or in parallel and then in series. By configuring a module 615 having a plurality of secondary batteries 600, It is possible to extract a large amount of power.
[0443] FIG. 23(D) is a top view of module 615. For clarity of illustration, conductive plate 613 is As shown in FIG. 23(D), the module 615 includes a plurality of secondary batteries 600. The device may have a conductive wire 616 for electrical connection. A conductive plate is provided on the conductive wire 616. In addition, a temperature control device 617 may be provided between the multiple secondary batteries 600. When the secondary battery 600 is overheated, the temperature control device 617 cools the secondary battery 600. If the temperature controller 617 is too cold, it can be heated. The performance of the module 615 is less affected by the outside temperature. The medium is preferably insulating and non-flammable.
[0444] By using the positive electrode active material described in the above embodiment for the positive electrode 604, the charge and discharge capacity is high. The cylindrical secondary battery 600 can be provided with excellent cycle characteristics.
[0445] <Structure example of secondary battery> Another structural example of the secondary battery will be described with reference to FIGS.
[0446] 24(A) and 24(B) are diagrams showing the external appearance of a battery pack. The battery includes a secondary battery 913 and a circuit board 900. The secondary battery 913 is The secondary battery 913 is connected to an antenna 914 via a label 910. Furthermore, as shown in FIG. 24(B), the secondary battery 913 has a terminal 951 and The circuit board 900 is connected to a terminal 952. The circuit board 900 is fixed with a seal 915. do.
[0447] The circuit board 900 includes a terminal 911 and a circuit 912. The terminal 911 is connected to a terminal 951. , a terminal 952, an antenna 914, and a circuit 912. Each of the multiple terminals 911 may be used as a control signal input terminal, a power supply terminal, etc. .
[0448] The circuit 912 may be provided on the back surface of the circuit board 900. The antenna 914 is The shape of the antenna is not limited to a coil shape, and may be, for example, a wire shape or a plate shape. Antennas such as surface antennas, traveling wave antennas, EH antennas, magnetic field antennas, and dielectric antennas Alternatively, the antenna 914 may be a flat conductor. The capacitor can function as one of the conductors for electric field coupling. The antenna 914 may function as one of the two conductors. Electric power can be exchanged not only using electromagnetic fields and magnetic fields, but also using electric fields.
[0449] The battery pack has a layer 916 between the antenna 914 and the secondary battery 913. The layer 916 has a function of blocking an electromagnetic field generated by, for example, the secondary battery 913. For example, a magnetic material can be used as the material.
[0450] The structure of the battery pack is not limited to that shown in FIG.
[0451] For example, as shown in Figs. 25(A) and 25(B), In the secondary battery 913 shown in FIG. FIG. 25(A) is an external view showing one of the pair of surfaces, and FIG. 25(B) is an external view showing the pair of surfaces. 24(A) and 24(B) are the same as those in the secondary battery shown in FIG. For the same parts, the explanation of the secondary battery shown in FIG. 24(A) and FIG. 24(B) can be appropriately cited. Cut.
[0452] As shown in FIG. 25(A), a layer 916 is sandwiched between one of a pair of surfaces of a secondary battery 913 and an antenna. As shown in FIG. 25(B), a layer 914 is provided on the other of the pair of surfaces of the secondary battery 913. An antenna 918 is provided on both sides of the layer 917. The layer 917 is, for example, a secondary battery 913. The layer 917 has a function of shielding electromagnetic fields. For example, a magnetic material is used. It is possible.
[0453] By adopting the above structure, the size of both the antenna 914 and the antenna 918 can be increased. The antenna 918 can perform data communication with an external device, for example. The antenna 918 has a shape that can be applied to the antenna 914, for example. A communication method between the secondary battery and other devices via the antenna 918. Examples of such technologies include NFC (near field communication), which can be used between secondary batteries and other devices. It is possible to apply a response method that allows
[0454] Alternatively, as shown in FIG. 25(C), the secondary battery 913 shown in FIG. 24(A) and FIG. 24(B) may be used. A display device 920 may be provided in the display device 920. The display device 920 is electrically connected to the terminal 911. It is not necessary to provide the label 910 in the portion where the display device 920 is provided. The same parts as those of the secondary battery shown in FIG. 24(A) and FIG. 24(B) are shown in FIG. The description of the secondary battery shown in 24(B) can be used as appropriate.
[0455] The display device 920 displays, for example, an image indicating whether charging is in progress, an image indicating the amount of stored power, etc. The display device 920 may be, for example, an electronic paper, a liquid crystal display device, an electrophotographic display device, or the like. For example, an electroluminescence (EL) display device can be used. By using the par, the power consumption of the display device 920 can be reduced.
[0456] 25(D), the secondary battery 913 shown in FIG. 24(A) and FIG. 24(B) The sensor 921 may be electrically connected to the terminal 911 via a terminal 922. The same parts as those of the secondary battery shown in FIG. 24(A) and FIG. 24(B) are For this purpose, the description of the secondary battery shown in FIGS. 24(A) and 24(B) can be appropriately applied.
[0457] The sensor 921 may be, for example, a sensor for detecting displacement, position, speed, acceleration, angular velocity, number of rotations, distance, light, etc. , liquid, magnetic, temperature, chemical, sound, time, hardness, electric field, current, voltage, power, radiation, flow It is sufficient if the device has the function of measuring the amount, humidity, gradient, vibration, odor, or infrared rays. By providing the sensor 921, for example, data indicating the environment in which the secondary battery is placed can be obtained. It is also possible to detect a signal (such as temperature) and store it in memory within the circuit 912.
[0458] Further, a structural example of the secondary battery 913 will be described with reference to FIGS.
[0459] The secondary battery 913 shown in FIG. 26(A) has a terminal 951 and a terminal 952 provided inside a housing 930. The winding body 950 is impregnated with an electrolyte inside the housing 930. The terminal 952 is in contact with the housing 930, and the terminal 951 is in contact with the housing by using an insulating material or the like. In FIG. 26(A), the housing 930 is not in contact with the sensor. 9, in reality, the winding body 950 is covered by the housing 930, and the terminals 951 and 95 2 extends outside the housing 930. The housing 930 is made of a metal material (e.g., aluminum). Materials such as rubber or resin materials can be used.
[0460] As shown in FIG. 26B, the housing 930 shown in FIG. 26A is made of a plurality of materials. For example, the secondary battery 913 shown in FIG. The wound body 930b is attached to the housing 930a. 50 are provided.
[0461] The housing 930a can be made of an insulating material such as an organic resin. By using a material such as organic resin on the surface on which the secondary battery 913 is formed, If the shielding of the electric field by the housing 930a is small, the shielding of the housing 930a can be suppressed. An antenna such as antenna 914 may be provided inside the housing 930b. Metallic materials can be used.
[0462] Further, the structure of the wound body 950 is shown in FIG. The winding body 950 has a pole 932 and a separator 933. The negative electrode 931 and the positive electrode 932 are stacked on top of each other, and the laminated sheet is wound to form a wound body. The negative electrode 931, the positive electrode 932, and the separator 933 are laminated together. You can stack several of them.
[0463] The negative electrode 931 is connected to the terminal 911 shown in FIG. 24 via one of the terminals 951 and 952. The positive electrode 932 is connected to the terminal 91 shown in FIG. Connected to 1.
[0464] By using the positive electrode active material described in the above embodiment for the positive electrode 932, the charge and discharge capacity is high. The secondary battery 913 can have excellent cycle characteristics.
[0465] <Laminated secondary battery> Next, an example of a laminated secondary battery will be described with reference to FIGS. 28 to 32(A). If the laminated secondary battery is made flexible, the flexible portion can be reduced. If the battery is mounted on at least some electronic devices, the secondary battery will bend in accordance with the deformation of the electronic device. It is also possible.
[0466] A laminated secondary battery 980 will be described with reference to FIG. The battery 980 has a wound body 993 shown in FIG. 27, a positive electrode 995, and a separator 996. Similar to the wound body 950, a negative electrode 994 and a positive electrode 995 are stacked with a separator 996 interposed therebetween. The laminated sheet is then wound.
[0467] The number of layers of the negative electrode 994, the positive electrode 995, and the separator 996 is determined as required. The negative electrode 994 is connected to the lead electrode 997 and The positive electrode 995 is connected to a negative electrode collector (not shown) via one of the positive and negative lead electrodes 998. The positive electrode 997 is connected to a positive electrode collector (not shown) via the other of the lead electrode 998. can be.
[0468] As shown in FIG. 28B, a film 981 that serves as an exterior body and a film 98 having a recess are 2 are bonded together by thermocompression or the like to form a space in which the above-mentioned wound body 993 is housed. In this way, a secondary battery 980 can be manufactured as shown in FIG. 3 has a lead electrode 997 and a lead electrode 998, a film 981, and a recessed portion. The inside of the film 982 is impregnated with an electrolyte.
[0469] The film 981 and the film 982 having the recesses are made of a metal material such as aluminum. and / or resin material can be used. If resin is used as the material for Film 982, the film 98 will deform when external force is applied. 1, the film 982 having the recesses can be deformed, and a flexible storage battery can be created. It can be manufactured.
[0470] In addition, although Fig. 28(B) and Fig. 28(C) show an example in which two films are used, A space is formed by folding one sheet of film, and the above-mentioned wound body 99 is inserted into the space. It may also accommodate 3.
[0471] By using the positive electrode active material described in the above embodiment for the positive electrode 995, the charge / discharge capacity is high. The secondary battery 980 can have excellent cycle characteristics.
[0472] In addition, in FIG. 28, a secondary battery 9 having a wound body in a space formed by a film serving as an exterior body is shown. We have explained the example of 80, but for example, as shown in Figure 29, The space defined by the positive electrode layer may be a space defined by a separator and a negative electrode. stomach.
[0473] The laminated secondary battery 500 shown in FIG. 29(A) includes a positive electrode current collector 501 and a positive electrode active material. A positive electrode 503 having a positive electrode active material layer 502, a negative electrode current collector 504 and a negative electrode active material layer 505. The battery includes a negative electrode 506, a separator 507, an electrolyte 508, and an exterior body 509. A separator 507 is provided between a positive electrode 503 and a negative electrode 506 provided in a body 509. The exterior body 509 is filled with an electrolyte 508. The electrolyte solution shown in the third embodiment can be used.
[0474] In the laminated secondary battery 500 shown in FIG. 29(A), a positive electrode current collector 501 and a negative electrode current collector The positive electrode current collector 504 also serves as a terminal for obtaining electrical contact with the outside. A part of the current collector 501 and the negative electrode current collector 504 is exposed to the outside from the exterior body 509. In addition, the positive electrode current collector 501 and the negative electrode current collector 504 may be arranged in a manner similar to that described above. Instead of exposing it to the outside, a lead electrode is used to connect the lead electrode to the positive electrode current collector 501 or the negative electrode The lead electrode may be exposed to the outside by ultrasonic bonding to the current collector 504 .
[0475] In the laminated secondary battery 500, the exterior body 509 is made of, for example, polyethylene, poly A film made of propylene, polycarbonate, ionomer, polyamide, etc. is coated with a A thin metal film with excellent flexibility, such as aluminum, stainless steel, copper, or nickel, is applied. On the metallic thin film, an insulating synthetic resin such as polyamide resin or polyester resin is applied as the outer surface of the exterior body. A laminate film having a three-layer structure with an oil film can be used.
[0476] An example of the cross-sectional structure of a laminated secondary battery 500 is shown in FIG. For simplicity, in A), an example consisting of two current collectors is shown, but in reality, As shown in FIG. 1, it is composed of multiple electrode layers.
[0477] In FIG. 29(B), as an example, the number of electrode layers is 16. However, the secondary battery 500 has flexibility. In FIG. 29(B), the negative electrode current collector 504 has eight layers. The positive electrode current collector 501 has a structure of 8 layers, totaling 16 layers. The cross section of the extraction part is shown, and eight layers of negative electrode current collector 504 are ultrasonically bonded. The number of electrode layers is not limited to 16, and may be more or less. In addition, the number of electrode layers can be reduced, resulting in a secondary battery having a larger charge / discharge capacity. In the absence of such a conductive layer, the secondary battery can be made thin and has excellent flexibility.
[0478] An example of an external view of a laminated secondary battery 500 is shown in FIGS. 30 and 31. 31 shows a positive electrode 503, a negative electrode 506, a separator 507, an outer casing 509, a positive electrode lead The positive electrode 510 and the negative electrode 511 are connected to each other.
[0479] FIG. 32A shows an external view of a positive electrode 503 and a negative electrode 506. The positive electrode 503 is connected to a positive electrode current collector 50 1, and the positive electrode active material layer 502 is formed on the surface of the positive electrode current collector 501. 503 has a region where the positive electrode current collector 501 is partially exposed (hereinafter referred to as a tab region). 506 has a negative electrode current collector 504, and a negative electrode active material layer 505 is formed on the surface of the negative electrode current collector 504. In addition, the negative electrode 506 has a region where the negative electrode current collector 504 is partially exposed, that is, a tab region. The area and shape of the tab regions of the positive electrode and the negative electrode are the same as those shown in FIG. Not limited to.
[0480] <Method of manufacturing laminated secondary battery> Here, an example of a method for producing a laminated secondary battery shown in FIG. 30 will be described with reference to FIG. This will be explained using (B) and (C).
[0481] First, the negative electrode 506, the separator 507, and the positive electrode 503 are laminated. The negative electrode 506, the separator 507, and the positive electrode 503 are shown. Next, the bonding of the tab regions of the positive electrode 503 and the bonding of the tabs of the positive electrode on the outermost surface are shown. The positive electrode lead electrode 510 is bonded to the region. For example, ultrasonic welding or the like may be used for bonding. Similarly, the bonding between the tab regions of the negative electrodes 506 and the bonding of the negative electrode leads to the tab region of the outermost negative electrode are preferably performed. Then, the metal layer 511 is bonded.
[0482] Next, the negative electrode 506 , the separator 507 and the positive electrode 503 are placed on the exterior body 509 .
[0483] Next, as shown in FIG. 32(C), the exterior body 509 is folded at the portion indicated by the dashed line. After that, the outer periphery of the exterior body 509 is bonded. For example, thermocompression bonding may be used for bonding. 509, so that the electrolyte 508 can be poured in later. An area that is not joined (hereinafter referred to as an inlet) is provided.
[0484] Next, electrolyte 508 (not shown) is introduced into exterior body 509 through an inlet. The electrolyte 508 is introduced into the inside of the electrode 509 under a reduced pressure atmosphere or an inert atmosphere. Finally, the inlet is bonded. In this way, the laminated mold is The secondary battery 500 can be manufactured.
[0485] By using the positive electrode active material described in the above embodiment for the positive electrode 503, the charge and discharge capacity is high. The secondary battery 500 can have excellent cycle characteristics.
[0486] In solid-state batteries, a certain amount of pressure is applied in the stacking direction of the stacked positive and negative electrodes. In this way, the contact state of the internal interfaces can be maintained in a good condition. By applying a certain pressure, expansion in the layer direction caused by charging and discharging of the all-solid-state battery is suppressed. This makes it possible to improve the reliability of the all-solid-state battery.
[0487] This embodiment mode can be implemented in appropriate combination with other embodiment modes.
[0488] (Embodiment 5) In this embodiment, an example in which a secondary battery according to one embodiment of the present invention is mounted on an electronic device will be described. do.
[0489] First, an example in which a bendable secondary battery described in the above embodiment is mounted on an electronic device will be described. 33(A) to 33(G) show electronic devices using bendable secondary batteries. Examples of devices include television sets (also called televisions or television receivers); Computer monitors, digital cameras, digital video cameras, digital photos Frame, mobile phone (also called mobile phone or mobile phone device), portable game machine, portable information Examples include terminals, audio playback devices, and large game machines such as pachinko machines.
[0490] In addition, the secondary battery having a flexible shape can be mounted on the inner or outer walls of houses and buildings, automobiles, etc. It is also possible to incorporate it along the curved surfaces of the interior or exterior of the vehicle.
[0491] FIG. 33A shows an example of a mobile phone. A mobile phone 7400 includes a housing 7401. In addition to the display unit 7402, operation buttons 7403, an external connection port 7404, The mobile phone 7400 is equipped with a speaker 7405, a microphone 7406, etc. The secondary battery 7407 is a secondary battery of one embodiment of the present invention. This makes it possible to provide a lightweight mobile phone with a long life.
[0492] FIG. 33B shows the mobile phone 7400 in a curved state. When the battery is deformed by applying an external force to the battery, the secondary battery installed inside the battery is released. The secondary battery 7407 is also bent. At this time, the state of the bent secondary battery 7407 is shown in FIG. The secondary battery 7407 is a thin storage battery. The secondary battery 7407 is in a bent state. The secondary battery 7407 is fixed in place by a lead electrode electrically connected to the current collector. For example, the current collector is made of copper foil, and some of it is alloyed with gallium to form a layer in contact with the current collector. The adhesiveness between the active material layer and the secondary battery 7407 is improved, and the secondary battery 7407 has a highly reliable structure when bent. It has become a success.
[0493] FIG. 33D shows an example of a bangle-type display device. The portable display device 7100 is The device includes a housing 7101 , a display unit 7102 , operation buttons 7103 , and a secondary battery 7104 . FIG. 33(E) shows the bent state of the secondary battery 7104. When the device is attached to the user's arm, the housing may deform and cause damage to part of the secondary battery 7104 or The total curvature changes. Note that the degree of curvature at any point on the curve is expressed as the radius of the corresponding circle. The value expressed is called the radius of curvature, and the inverse of the radius of curvature is called the curvature. Within the range of 40 mm to 150 mm, a part of the main surface of the case or the secondary battery 7104 The radius of curvature of the main surface of the secondary battery 7104 is 40 mm or more and 150 mm or less. If the thickness is within the range of 1 mm or less, high reliability can be maintained. By using the secondary battery of one embodiment, a lightweight, long-life portable display device can be provided.
[0494] FIG. 33(F) shows an example of a wristwatch-type portable information terminal. The portable information terminal 7200 is , a housing 7201, a display unit 7202, a band 7203, a buckle 7204, and an operation button 72 05, input / output terminal 7206, etc.
[0495] The portable information terminal 7200 is capable of carrying out mobile telephone calls, e-mails, viewing and creating documents, playing music, and using the Internet. - It can run various applications such as internet communication and computer games. do.
[0496] The display unit 7202 has a curved display surface, and displays images along the curved display surface. The display portion 7202 is provided with a touch sensor, and a screen can be changed by touching it with a finger or a stylus. For example, the icon displayed on the display unit 7202 can be operated by touching the screen. By touching 7207, you can launch an application.
[0497] The operation button 7205 is used to set the time, turn the power on and off, and turn wireless communication on and off. It has various functions such as operation, silent mode activation and deactivation, power saving mode activation and deactivation, etc. For example, an operating system installed in the portable information terminal 7200 can The function of the operation button 7205 can also be freely set using the stem.
[0498] In addition, the mobile information terminal 7200 is capable of performing short-distance wireless communication according to a communication standard. For example, by communicating with a wireless headset, You can also make calls.
[0499] The portable information terminal 7200 also includes an input / output terminal 7206, and can communicate with other information terminals via connectors. It is also possible to charge the device via the input / output terminal 7206. The charging operation can be performed by wireless power supply without going through the input / output terminal 7206. This is also fine.
[0500] A display portion 7202 of a portable information terminal 7200 includes a secondary battery of one embodiment of the present invention. By using the secondary battery of one embodiment of the present invention, a lightweight portable information terminal with a long life can be provided. For example, the secondary battery 7104 shown in FIG. 33E is curved inside the housing 7201. or may be incorporated in a bendable state inside the band 7203.
[0501] The portable information terminal 7200 preferably has a sensor. For example, a fingerprint sensor may be used as the sensor. Sensors for measuring body temperature, pulse rate, touch, pressure, and acceleration , etc. are preferably installed.
[0502] FIG. 33G shows an example of a wristband-type display device. The display device 7300 includes a display unit 7 The display device 7300 includes a display 304 and a secondary battery of one embodiment of the present invention. The display unit 7304 may be equipped with a touch sensor, and may function as a portable information terminal. It is also possible.
[0503] The display surface of the display unit 7304 is curved, and the display can be performed along the curved display surface. In addition, the display device 7300 can display a display state by short-distance wireless communication according to a communication standard. The situation can be changed.
[0504] The display device 7300 also has an input / output terminal, and can directly exchange data with other information terminals via a connector. It is also possible to charge the device via the input / output terminals. The charging operation may be performed by wireless power supply without going through the input / output terminal.
[0505] By using the secondary battery of one embodiment of the present invention as the secondary battery included in the display device 7300, It is possible to provide a display device with a long life and low cost.
[0506] FIG. 1 shows an example in which the secondary battery having excellent cycle characteristics shown in the above embodiment is mounted on an electronic device. 33(H), FIG. 34 and FIG. 35.
[0507] By using the secondary battery of one embodiment of the present invention as a secondary battery in everyday electronic devices, the device can be lightweight and have a long life. For example, we can provide a wide range of products for daily electronic devices, such as electric toothbrushes, electric shavers, These include mobile beauty devices, and the secondary batteries for these products are designed to be easy for users to carry. Therefore, a secondary battery that is stick-shaped, small, lightweight, and has a large charge / discharge capacity is desired. is.
[0508] FIG. 33(H) is a perspective view of a device also called a tobacco-containing smoking device (electronic cigarette). In 33(H), the electronic cigarette 7500 is an atomizer 7501 including a heating element and an atomizer A secondary battery 7504 for supplying power to the myser, a liquid supply bottle, a camera including a sensor, etc. The secondary battery 7504 is composed of a cartridge 7502. To enhance safety, the secondary battery 7504 is prevented from being overcharged. And / or a protection circuit to prevent over-discharge may be electrically connected to the secondary battery 7504. The secondary battery 7504 shown in 33(H) has an external terminal so that it can be connected to a charging device. The secondary battery 7504 is at the tip when held, so the total length is short, and The secondary battery according to one embodiment of the present invention has a high charge / discharge capacity and is excellent in It has cycle characteristics, so it is small and lightweight and can be used for a long period of time. We can provide 7500 e-cigarettes in quantity.
[0509] Next, FIG. 34(A) and FIG. 34(B) show an example of a foldable tablet terminal. The tablet terminal 9600 shown in FIG. 34(A) and FIG. 34(B) includes a housing 9630. a, housing 9630b, a movable part 9640 connecting the housing 9630a and the housing 9630b, A display unit 9631 having a display unit 9631a and a display unit 9631b, a switch 9625 to a switch The display unit 9631 has a switch 9627, a fastener 9629, and an operation switch 9628. By using a flexible panel, it is possible to create a tablet terminal with a larger display area. FIG. 34(A) shows a tablet terminal 9600 in an open state, and FIG. 9B) shows the tablet terminal 9600 in a closed state.
[0510] The tablet terminal 9600 also includes a battery storage device inside the housing 9630a and the housing 9630b. The power storage unit 9635 is connected to the housing 9630a through the movable portion 9640. It is located across 9630b.
[0511] The display unit 9631 can be entirely or partially used as a touch panel. By touching images, text, input forms, etc., including icons displayed in the area, data For example, a keyboard is provided on the entire surface of the display portion 9631a on the housing 9630a side. The button is displayed to display information such as text and images on the display unit 9631b on the housing 9630b. may be displayed and used.
[0512] In addition, a keyboard is displayed on the display unit 9631b on the housing 9630b side. The display unit 9631a on the side of the camera may be used to display information such as text and images. The 9631 is equipped with a touch panel keyboard display switch button. Touch the button with your finger or a stylus to display the keyboard on the display 9631. You can do so.
[0513] In addition, the touch panel area of the display unit 9631a on the housing 9630a side and the touch panel area of the display unit 9631b on the housing 9630b side Simultaneous touch input can also be made to the touch panel area of the display portion 9631b.
[0514] Switches 9625 to 9627 are used to operate the tablet terminal 9600. It is not only an interface for the For example, at least one of the switches 9625 to 9627 may be It functions as a switch to turn the power of the tablet terminal 9600 on and off. Also, for example, at least one of the switches 9625 to 9627 may be The ability to switch between horizontal and vertical display orientation, or between black and white and color display In addition, for example, at least one of the switches 9625 to 9627 may have a function of The display portion 9631 may have a function of adjusting the luminance of the display portion 9631. The brightness of the tablet terminal 9600 is determined by the external light during use detected by a light sensor built into the tablet terminal 9600. The tablet device can be optimized according to the amount of light. It is not limited to the gyro, but has other detection devices such as a gyro, acceleration sensor, etc. that detect the inclination. This may be allowed.
[0515] In FIG. 34A, a display portion 9631a on the housing 9630a side and a display portion 9631b on the housing 9630b side are 9 shows an example in which the display area of the display unit 9631a and the display unit 9631b are substantially the same. The display area of each of 631b is not particularly limited, and one size may be different from the other. The display quality may be different, e.g. one with higher resolution than the other. The display panel may also be capable of displaying images.
[0516] FIG. 34(B) shows a state in which the tablet terminal 9600 is folded in half. The terminal 9600 includes a housing 9630, a solar cell 9633, and a DC-DC converter 9636. A charge and discharge control circuit 9634 including a power storage unit 9635 is also provided. A secondary battery is used.
[0517] As mentioned above, the tablet terminal 9600 can be folded in half, so when not in use The housing 9630a and the housing 9630b can be folded so as to overlap each other. By folding the tablet terminal 9600, the display portion 9631 can be protected, and therefore the durability of the tablet terminal 9600 can be improved. In addition, the power storage unit 9635 using the secondary battery of one embodiment of the present invention can improve rechargeability. It has a high discharge capacity and good cycle characteristics, so it can be used for a long period of time. It is possible to provide a tablet terminal 9600.
[0518] In addition, the tablet terminal 9600 shown in FIG. 34(A) and FIG. 34(B) , the ability to display various information (still images, videos, text images, etc.), calendars, dates, or The function to display the time, etc. on the display, and to operate or edit the information displayed on the display by touch input touch input function, function to control processing by various software (programs), etc. may have the following structure:
[0519] The tablet terminal 9600 is equipped with a solar cell 9633 on its surface, which provides power to the touch screen. The solar cell 963 can supply the solar cell 963 with the panel, the display unit, or the image signal processing unit. 3 can be provided on one or both sides of the housing 9630, and can efficiently charge the power storage unit 9635. The power storage unit 9635 can be a lithium ion battery. The use of such a structure has the advantage of enabling miniaturization.
[0520] The configuration and operation of the charge / discharge control circuit 9634 shown in FIG. A block diagram is shown in FIG. 34(C) and will be described. In FIG. 34(C), a solar cell 9633 and a power storage unit 963 5, DC-DC converter 9636, converter 9637, switches SW1 to SW3, table The display unit 9631 is shown, which includes a storage battery 9635, a DC-DC converter 9636, and a The inverter 9637 and the switches SW1 to SW3 are connected to the charge / discharge control circuit 96 shown in FIG. This corresponds to 34.
[0521] First, an example of operation in which power is generated by the solar cell 9633 using external light will be described. The power generated by the solar cell is converted to a voltage for charging the storage battery 9635 by the DCDC controller. The voltage is increased or decreased by a inverter 9636. When power from the 9633 is used, switch SW1 is turned on and the converter 9637 The voltage is increased or decreased to a voltage required for the display unit 9631. When not displaying the battery status, turn SW1 off and SW2 on to charge the battery 9635. The configuration may be such that the power supply is electrically connected to the power source.
[0522] The solar cell 9633 is shown as an example of a power generating means, but is not limited thereto. Other power generation methods such as piezoelectric elements and thermoelectric elements For example, the power storage unit 9635 may be configured to transmit and receive power wirelessly (contactlessly). A non-contact power transmission module that charges by transmitting power, and a configuration that combines other charging methods It is also possible to use the following.
[0523] FIG. 35 shows another example of electronic equipment. In FIG. 35, a display device 8000 according to one embodiment of the present invention is 8 is an example of an electronic device using a secondary battery 8004 according to an embodiment. 8000 corresponds to a display device for receiving TV broadcasts, and includes a housing 8001, a display unit 8002, and a speaker unit. The secondary battery 8004 according to one embodiment of the present invention includes a housing. The display device 8000 is provided inside a body 8001. The display device 8000 receives power from a commercial power source. Alternatively, the power stored in the secondary battery 8004 can be used. Even when power cannot be supplied from a commercial power source due to a power outage or the like, the present invention according to one embodiment of the present invention can be used. By using the secondary battery 8004 as an uninterruptible power supply, the display device 8000 can be used. do.
[0524] The display unit 8002 may be a liquid crystal display device, an emitting device having light emitting elements such as organic EL elements in each pixel, or the like. Device, electrophoretic display device, DMD (Digital Micromirror Devi ce), PDP (Plasma Display Panel), FED (Field A semiconductor display device such as a 3D Emission Display can be used.
[0525] In addition, display devices are used for TV broadcast reception, personal computers, advertising displays, etc. , all display devices for displaying information are included.
[0526] In FIG. 35, a stationary lighting device 8100 includes a secondary battery 81 according to one embodiment of the present invention. 8101, a light source 8102, and a light source 8103 are used. In FIG. 35, the secondary battery 8103 is mounted in the housing 81. 8102 is installed inside a ceiling 8104. However, the secondary battery 8103 may be provided inside the housing 8101. The device 8100 can receive power from a commercial power source, or store power in a secondary battery 8103. Therefore, when the power supply from the commercial power source is cut off due to a power outage, Even when the electricity cannot be received, the secondary battery 8103 according to one embodiment of the present invention is used as an uninterruptible power source. This enables the lighting device 8100 to be used.
[0527] In addition, FIG. 35 illustrates a lighting device 8100 that is installed on a ceiling 8104. However, in the secondary battery according to one embodiment of the present invention, in addition to the ceiling 8104, for example, the side wall 8105, the floor 8106, 106, the window 8107, etc., can be used as a fixed lighting device, or a tabletop lighting device. The present invention can also be used in lighting devices of this type.
[0528] In addition, the light source 8102 may be an artificial light source that artificially obtains light using electricity. Specifically, incandescent lamps, fluorescent lamps and other discharge lamps, LEDs and organic EL elements, etc. A light-emitting element is one example of the artificial light source.
[0529] In FIG. 35, an air conditioner having an indoor unit 8200 and an outdoor unit 8204 is as follows: 8 is an example of an electronic device using a secondary battery 8203 according to one embodiment of the present invention. The device 8200 includes a housing 8201, an air outlet 8202, a secondary battery 8203, and the like. 8 illustrates an example in which the secondary battery 8203 is provided in the indoor unit 8200. The battery 8203 may be provided in the outdoor unit 8204. A secondary battery 8203 may be provided in both the power source 8202 and the power source 8204. The power supply can be provided from a commercial power source, or the power stored in the secondary battery 8203 can be used. In particular, a secondary battery 82 is provided in both the indoor unit 8200 and the outdoor unit 8204. If 03 is installed, when power cannot be supplied from the commercial power source due to a power outage, etc. In addition, by using the secondary battery 8203 according to one embodiment of the present invention as an uninterruptible power supply, The conditioner can be used.
[0530] In addition, in Figure 35, a separate type air conditioner consisting of an indoor unit and an outdoor unit is shown. As an example, an all-in-one air conditioner that has both indoor and outdoor unit functions in a single housing. The secondary battery according to one embodiment of the present invention can also be used for the conditioner.
[0531] In FIG. 35, an electric refrigerator-freezer 8300 includes a secondary battery 8304 according to one embodiment of the present invention. Specifically, an electric refrigerator-freezer 8300 includes a housing 8301, a refrigerator It has a storage compartment door 8302, a freezer compartment door 8303, a secondary battery 8304, etc. A secondary battery 8304 is provided inside the housing 8301. The electric refrigerator-freezer 8300 is It can receive power from a commercial power source, or use the power stored in the secondary battery 8304. Therefore, when power cannot be supplied from commercial power sources due to a power outage, etc. However, by using the secondary battery 8304 according to one embodiment of the present invention as an uninterruptible power supply, It will be possible to use the 8300 freezer refrigerator.
[0532] Among the above-mentioned electronic devices, high-frequency heating devices such as microwave ovens, electric rice cookers, etc. The equipment requires high power for a short period of time. Therefore, the equipment supplements the power that cannot be supplied by commercial power sources. By using a secondary battery according to one embodiment of the present invention as an auxiliary power source for It can prevent the commercial power breaker from tripping during use.
[0533] In addition, during periods when electronic devices are not in use, especially during periods when the total amount of power that can be supplied by commercial power suppliers is low, During periods when the ratio of electricity actually used (called the electricity usage rate) is low, By storing power in the battery, it is possible to prevent high power usage outside of the above time periods. For example, in the case of the electric refrigerator-freezer 8300, when the temperature is low, the refrigerator compartment door 830 2. During the night when the freezer door 8303 is not opened or closed, the secondary battery 8304 stores electricity. Then, as the temperature rises, the refrigerator door 8302 and the freezer door 8303 are opened and closed. During the daytime, when the vehicle is turned on, the secondary battery 8304 is used as an auxiliary power source, and the daytime power usage rate is can be kept low.
[0534] According to one embodiment of the present invention, the cycle characteristics of a secondary battery are improved, and the reliability is improved. Moreover, according to one aspect of the present invention, a secondary battery having a high charge / discharge capacity can be obtained. Therefore, the characteristics of the secondary battery can be improved, and the secondary battery itself can be made smaller and lighter. Therefore, the secondary battery according to one embodiment of the present invention can be used as the battery described in this embodiment. By installing it in a child device, the electronic device can have a longer life and be lighter.
[0535] This embodiment mode can be implemented in appropriate combination with other embodiment modes.
[0536] (Embodiment 6) In this embodiment, an example of an electronic device using the secondary battery described in the previous embodiment is shown. This will be explained using Figures 36(A) to 37(C).
[0537] FIG. 36(A) shows an example of a wearable device. It uses a secondary battery as a power source. In addition, when the user uses it at home or outdoors, In order to improve splash and water resistance or dust resistance, the connector part to be connected is exposed. There is a demand for wearable devices that can be charged wirelessly as well as via a wired connection.
[0538] For example, a secondary lens according to one embodiment of the present invention is applied to a glasses-type device 4000 as shown in FIG. The glasses-type device 4000 includes a frame 4000a and a display. A secondary battery is mounted on the temple portion of the curved frame 4000a. This allows for a lightweight, well-balanced eyeglasses-type device that can be used continuously for a long time. By providing the secondary battery according to one embodiment of the present invention, the size of the housing can be reduced. It is possible to realize a configuration that can accommodate space saving associated with mold design.
[0539] In addition, the headset device 4001 may be equipped with a secondary battery according to one embodiment of the present invention. The headset type device 4001 includes at least a microphone unit 4001a and a frame. The flexible pipe 4001b and the earphone section 4001c are provided. A secondary battery may be provided within the earphone unit 4001b and / or within the earphone unit 4001c. By including a secondary battery according to one embodiment of the present invention, space can be saved by making the housing smaller. It is possible to realize a configuration in which
[0540] In addition, a secondary battery according to one embodiment of the present invention is installed in a device 4002 that can be directly attached to the body. The device 4002 can be mounted with a secondary battery 400 in a thin housing 4002a. By providing the secondary battery according to one embodiment of the present invention, the size of the housing can be reduced. It is possible to realize a configuration that can accommodate space saving associated with the increase in size.
[0541] In addition, a secondary battery according to one embodiment of the present invention is mounted on a device 4003 that can be attached to clothing. The device 4003 has a thin housing 4003a and a secondary battery 4003b in the housing 4003a. By providing the secondary battery according to one embodiment of the present invention, the size of the housing can be reduced. It is possible to realize a configuration that can accommodate the space saving that accompanies the above.
[0542] In addition, the belt-type device 4006 can be equipped with a secondary battery according to one embodiment of the present invention. The belt type device 4006 includes a belt part 4006a and a wireless power receiving part 4006b. 06b, and a secondary battery can be mounted inside the belt portion 4006a. By providing a secondary battery, which is one aspect of the above, it is possible to reduce space required for a smaller housing. The configuration can be realized.
[0543] In addition, the secondary battery according to one embodiment of the present invention can be mounted on the wristwatch device 4005. The wristwatch type device 4005 has a display unit 4005a and a belt unit 4005b. A secondary battery can be provided in the display unit 4005a or the belt unit 4005b. By providing a secondary battery, which is one aspect of the present invention, the structure can accommodate space saving associated with a smaller housing. This makes it possible to achieve this.
[0544] The display unit 4005a displays not only the time but also various information such as incoming mail and phone calls. It is possible.
[0545] The wristwatch type device 4005 is a wearable device that is worn directly on the arm. Therefore, sensors for measuring the user's pulse, blood pressure, etc. may be installed. It is also possible to accumulate health-related data and manage one's health.
[0546] FIG. 36(B) shows a perspective view of the wristwatch type device 4005 removed from the wrist.
[0547] A side view is shown in FIG. 36(C). In FIG. 36(C), a secondary battery 913 is built in. The secondary battery 913 is the secondary battery shown in the fourth embodiment. The battery 913 is provided at a position overlapping the display unit 4005a, and is small and lightweight. .
[0548] FIG. 36(D) shows an example of a wireless earphone. Here, a pair of main bodies 4100a and Although the wireless earphones having a main body 4100b and a main body 4100b are illustrated, they do not necessarily have to be a pair. good.
[0549] The main bodies 4100a and 4100b include a driver unit 4101, an antenna 4102, and a The device may also include a display unit 4104. It is preferable that the device has a substrate on which the sensor is mounted, a charging terminal, etc. Also, the device may have a microphone.
[0550] The case 4110 has a secondary battery 4111. Also, circuits such as a wireless IC and a charge control IC are included. It is preferable that the device has a board on which the device is mounted and a charging terminal. It also has a display unit, buttons, etc. Good too.
[0551] The main units 4100a and 4100b communicate wirelessly with other electronic devices such as smartphones. This allows the main body 4100a and the main body 4100b to receive audio data and the like sent from other electronic devices. The main units 4100a and 4100b can play the audio. If this is done, the sound picked up by the microphone can be sent to another electronic device, and the sound after processing by that electronic device can be The data can be sent back to the main units 4100a and 4100b and played back. For example, it can be used as a translation device.
[0552] Also, the secondary battery 4111 in the case 4100 is connected to the secondary battery 4112 in the main body 4100a. The secondary battery 4111 and the secondary battery 4103 can be charged. The coin-type secondary battery, cylindrical secondary battery, etc., according to the embodiment of the present invention can be used. A secondary battery using the positive electrode active material 100 obtained in 1 as a positive electrode has a high energy density and is By using it for the battery 4103 and the secondary battery 4111, the wireless earphones will become smaller. It is possible to realize a configuration that can save space.
[0553] FIG. 37A shows an example of a cleaning robot. The cleaning robot 6300 is a housing 63 01 A display unit 6302 arranged on the top surface, multiple cameras 6303 arranged on the side, and a brush 6304, an operation button 6305, a secondary battery 6306, various sensors, etc. Although not shown, the cleaning robot 6300 is equipped with tires, a suction port, etc. The robot 6300 moves by itself, detects the dirt 6310, and sucks it out from the suction port on its bottom. It can suck up mi.
[0554] For example, the cleaning robot 6300 analyzes the image captured by the camera 6303 and detects walls, furniture, etc. It can also use image analysis to detect the presence of obstacles such as wiring. When an object that is likely to get entangled in the brush 6304 is detected, the rotation of the brush 6304 is stopped. The cleaning robot 6300 includes a secondary battery 630 according to one embodiment of the present invention. 6 and a semiconductor device or electronic component. By using it in the cleaning robot 6300, the cleaning robot 6300 can be operated for a long time and with high reliability. It is possible to make the electronic device more convenient.
[0555] FIG. 37(B) shows an example of a robot. The robot 6400 shown in FIG. 37(B) is , secondary battery 6409, illuminance sensor 6401, microphone 6402, upper camera 640 3, speaker 6404, display unit 6405, lower camera 6406 and obstacle sensor 640 7. Equipped with a moving mechanism 6408, a computing device, etc.
[0556] The microphone 6402 has a function of detecting the user's voice and environmental sounds. The speaker 6404 has a function of emitting sound. The user can communicate with the computer using the computer 6402 and the speaker 6404. It is possible.
[0557] The display unit 6405 has a function of displaying various information. The display unit 6405 can display desired information. The display unit 6405 may be a removable information terminal. By placing it in a fixed position on the robot 6400, charging and data transfer can be performed. It is possible.
[0558] The upper camera 6403 and the lower camera 6406 are functions for capturing images of the surroundings of the robot 6400. The obstacle sensor 6407 detects the obstacles of the robot 640 using the moving mechanism 6408. Robot 64 can detect the presence or absence of obstacles in its path as it moves forward. 00 uses an upper camera 6403, a lower camera 6406, and an obstacle sensor 6407. It is possible for the robot to recognize its surrounding environment and move around safely.
[0559] The robot 6400 includes a secondary battery 6409 according to one embodiment of the present invention and a semiconductor device. The secondary battery according to one embodiment of the present invention is used in a robot 6400. This allows the robot 6400 to be an electronic device with long operating time and high reliability.
[0560] FIG. 37(C) shows an example of an aircraft. The aircraft 6500 shown in FIG. 37(C) is a It has a rotor blade 6501, a camera 6502, and a secondary battery 6503, and flies autonomously. It has the function of
[0561] For example, image data captured by the camera 6502 is stored in the electronic component 6504. Part 6504 can analyze image data and detect the presence or absence of obstacles when moving. Also, the electronic component 6504 can detect the change in the storage capacity of the secondary battery 6503. The remaining amount of the battery can be estimated. The secondary battery 6503 is provided. This allows the Aircraft 6500 to have electronic devices with long operating times and high reliability.
[0562] This embodiment mode can be implemented in appropriate combination with other embodiment modes.
[0563] (Embodiment 7) In this embodiment, an example in which a secondary battery according to one embodiment of the present invention is mounted on a vehicle will be described.
[0564] When a secondary battery is installed in a vehicle, it becomes a hybrid vehicle (HV), electric vehicle (EV), or plastic vehicle (PV). This will make it possible to realize next-generation clean energy vehicles such as powertrain hybrid vehicles (PHVs).
[0565] FIG. 38 illustrates an example of a vehicle using a secondary battery according to one embodiment of the present invention. The automobile 8400 shown in FIG. 1 is an electric automobile that uses an electric motor as a power source for driving. Alternatively, an electric motor and an engine can be selected as the power source for driving. By using one embodiment of the present invention, the cruising distance can be extended. In addition, the automobile 8400 has a secondary battery. 23(C) and 23(D) are mounted on the floor of the vehicle. In addition, a battery pack consisting of multiple secondary batteries as shown in FIG. The secondary battery may be installed on the floor of the vehicle. In addition, it also supplies power to light-emitting devices such as headlights 8401 and room lights (not shown). can be supplied.
[0566] In addition, the secondary battery is used for the display of the speedometer, tachometer, etc. of the automobile 8400. The secondary battery can supply power to the navigation device of the automobile 8400. The present invention can provide power to semiconductor devices such as power distribution systems.
[0567] The automobile 8500 shown in FIG. 38(B) is a secondary battery that is plugged in. The device receives power from an external charging facility using a contactless power supply method or other methods to charge the device. FIG. 38B shows a case where a charging device 8021 is installed on the ground and a vehicle 8500 is charged. The secondary battery 8024 mounted on the device is being charged via a cable 8022. When charging, the charging method and connector specifications are CHAdeMO (registered trademark) or The charging device 8021 may be installed in a commercial facility. This can be a charging station or a home power source. For example, plug-in technology Therefore, the secondary battery 8024 mounted on the automobile 8500 is charged by an external power supply. Charging is done by converting AC power to DC power via a conversion device such as an ACDC converter. This can be done by converting it into electricity.
[0568] Although not shown, a power receiving device is mounted on the vehicle and receives power from a ground power transmitting device in a non-contact manner. In this case, the road and / or the exterior wall can be used as a charging station. By incorporating a power transmission device, charging can be performed not only when the vehicle is stopped but also while the vehicle is moving. The above-mentioned contactless power supply method may be used to transmit and receive power between vehicles. Solar cells are installed on both exteriors, and the secondary battery can be charged while the vehicle is stopped and / or running. Such contactless power supply can be achieved by using electromagnetic induction and / or magnetic resonance. can be used.
[0569] FIG 38(C) shows an example of a two-wheeled vehicle using the secondary battery of one embodiment of the present invention. The scooter 8600 shown in (C) has a secondary battery 8602, side mirrors 8601, and a turn signal. The secondary battery 8602 can supply electricity to the direction indicator light 8603. can.
[0570] In addition, the scooter 8600 shown in FIG. 38(C) has a secondary battery 860 in the storage space under the seat 8604. 2 can be stored. The secondary battery 8602 can be stored in the under-seat storage 8604 even if it is small. The secondary battery 8602 can be removed and stored in the under-seat storage 8604. When charging, the secondary battery 8602 is brought indoors, charged, and stored before driving. Just do that.
[0571] According to one aspect of the present invention, the cycle characteristics of the secondary battery are improved, and the charge / discharge capacity of the secondary battery is improved. Therefore, the secondary battery itself can be made smaller and lighter. If the battery itself can be made smaller and lighter, it will contribute to reducing the weight of the vehicle, thereby improving the driving range. In addition, the secondary battery installed in the vehicle can be used as a power supply source for other purposes. In this case, for example, it is possible to avoid using commercial power sources during peak power demand periods. If we can avoid using commercial power sources during peak power demand periods, we can save energy and This can contribute to reducing CO2 emissions. This allows secondary batteries to be used for a long period of time, reducing the use of rare metals such as cobalt. It can be reduced.
[0572] This embodiment mode can be implemented in appropriate combination with other embodiment modes. EXAMPLES
[0573] In this example, a positive electrode active material 100 according to one embodiment of the present invention was produced and its characteristics were analyzed.
[0574] <Preparation of positive electrode active material> The sample produced in this example will be described with reference to the production method shown in FIGS. 2 and 3. do.
[0575] In step S14 of FIG. 2, LiMO2 is used, which has cobalt as the transition metal M and an additive element A commercially available lithium cobalt oxide (Cellseed C-1, manufactured by Nippon Chemical Industry Co., Ltd.) that does not have any particular In the initial heating step S15, the lithium cobalt oxide was placed in a crucible. The mixture was placed in a muffle furnace, covered with a lid, and heated at 850°C for 2 hours. The inside of the muffle furnace was kept in an oxygen atmosphere. After the initial heating, the weight did not flow (O2 purging). It was found that the weight was slightly decreased. It is possible that the weight was decreased due to the removal of impurities from the LCO. It is possible.
[0576] According to steps S21 and S41 shown in FIG. 3(A) and FIG. 3(B), As additional elements, Mg, F, Ni, and Al were added separately. Step S2 shown in FIG. According to the method described in 1, LiF was prepared as the F source and MgF2 was prepared as the Mg source. LiF and M were weighed out so that the molar ratio was 1:3. gF2 was mixed and stirred at a rotation speed of 400 rpm for 12 hours to obtain the additive element source X. A Create A ball mill was used for mixing, and zirconium oxide balls were used as the grinding media. For a mixing ball mill with a capacity of 45 mL, add 20 mL of dehydrated acetone and 20 mL of zirconium oxide ball mill. A total of about 10 g of F source and Mg source were added together with 22 g of a filter (1 mm diameter) and mixed. Sift through a sieve with 300 μm holes to obtain additive element source X with uniform particle size. A obtained.
[0577] Next, the additive element source X A The amount of the transition metal M was weighed out so that it was 1 atomic % of the transition metal M. The mixture was dry mixed with O. The mixture was stirred at a rotation speed of 150 rpm for 1 hour. Source X A The stirring conditions are gentler than those for obtaining the desired concentration. The mixture was sieved to obtain mixture A with a uniform particle size.
[0578] Next, mixture A was heated. The heating conditions were 900°C and 20 hours. A lid was placed on the crucible containing the substance A. The inside of the crucible was made to have an oxygen-containing atmosphere, and the inflow and outflow of the oxygen was controlled. The Mg and F-containing LCO (composite oxide A) was obtained by heating.
[0579] Next, the additive element source X is added to the composite oxide A. B In step S41 shown in FIG. Therefore, nickel hydroxide is prepared as the Ni source and aluminum hydroxide is prepared as the Al source. Nickel hydroxide was 0.5 atomic % of the transition metal M, and aluminum hydroxide was 0.5 atomic % of the transition metal M. The metal M was weighed out so as to be 0.5 atomic % of the metal M, and mixed with the composite oxide A in a dry state. The mixture was stirred for 1 hour at a rotation speed of 50 rpm. A ball mill was used for mixing, and Zirconium oxide balls were used for mixing. A total of about 7.5g of Ni source and Al source was added together with 22g of nickel balls (1mmφ). This is the additive element source X. A The stirring conditions are gentler than those for obtaining 30 The mixture was sieved through a sieve with 100 μm holes to obtain mixture B with a uniform particle size.
[0580] Next, mixture B was heated. The heating conditions were 850° C. and 10 hours. A lid was placed on the crucible containing the substance B. The inside of the crucible was made to have an oxygen-containing atmosphere, and the inflow and outflow of the oxygen was controlled. The heat treatment resulted in the production of LCO containing Mg, F, Ni, and Al. The resulting positive electrode active material (composite oxide) was designated as Sample 1-1.
[0581] In addition, the heating time in step S15 was set to 10 hours, and the sample was prepared in the same manner as sample 1-1. The resulting product was designated as sample 1-2.
[0582] In addition, the sample was prepared in the same manner as sample 1-1, except that the heating temperature in step S15 was set to 750°C. The resulting samples were designated as samples 1-3.
[0583] In addition, the sample was prepared in the same manner as sample 1-1, except that the heating temperature in step S15 was set to 900°C. The resulting samples were designated as samples 1-4.
[0584] In addition, the sample was prepared in the same manner as sample 1-1, except that the heating temperature in step S15 was 950°C. The resulting samples were designated as samples 1-5.
[0585] Sample 2 was prepared by not performing the heating in step S15. The heating in step S53 was performed with an oxygen flow rate of 10 L / min.
[0586] As a comparative example, lithium cobalt oxide (manufactured by Nippon Chemical Industry Co., Ltd.) was used without any special treatment. Cellseed C-10N) was used as sample 10.
[0587] In addition, lithium cobalt oxide was subjected to only the heating in step S15 and designated as sample 11. Ta.
[0588] The preparation conditions for samples 1-1, 1-2, 1-3, 1-4, 1-5, 2, 10 and 11 are shown. As is clear from Table 1, all of Samples 1-1 to 1-5 are In particular, LiCoO2 without any additive elements is initially heated, and then a magnesium source, a fluorine source, and Ni Both have in common that they are produced by adding nickel and aluminum sources and then heating them. These may all be referred to as sample 1 to distinguish them from samples that have no points.
[0589] [Table 1]
[0590] <sem> Figure 39 shows the results of SEM (Scanning Electron Microscope) observation. The SEM observation in this example was performed using a scanning electron microscope SU8030 manufactured by Hitachi High-Tech Corporation. The measurement conditions were an acceleration voltage of 5 kV and magnifications of 5,000x and 20,000x.
[0591] Figure 39(A) and...
Claims
1. A lithium ion secondary battery having a positive electrode and a negative electrode, The positive electrode has a plurality of positive electrode active material particles, the positive electrode active material particles contain magnesium, nickel, aluminum, and lithium cobalt oxide; a surface layer portion of the positive electrode active material particle contains magnesium, In the positive electrode active material particles, a magnesium concentration in a surface portion including a (001) plane is lower than a magnesium concentration in a surface portion including a plane other than the (001) plane; In an XPS analysis of the plurality of positive electrode active material particles, the number of magnesium atoms is 0.4 to 1.5 times the number of cobalt atoms, In a STEM-EDX ray analysis of the positive electrode active material particles, a peak of aluminum concentration exists at a depth of 0.5 nm to 50 nm from the surface of the positive electrode active material particles, In a grayscale image obtained by converting a surface SEM image of the positive electrode active material particle into an 8-bit image, the difference between the maximum and minimum grayscale values is 120 or less; The measurement conditions for the surface SEM image of the lithium ion secondary battery were an acceleration voltage of 5 kV and a magnification of 5000 times.
2. A lithium ion secondary battery having a positive electrode and a negative electrode, The positive electrode has a plurality of positive electrode active material particles, the positive electrode active material particles contain magnesium, nickel, aluminum, and lithium cobalt oxide; a surface layer portion of the positive electrode active material particle contains magnesium, In the positive electrode active material particles, a magnesium concentration in a surface portion including a (001) plane is lower than a magnesium concentration in a surface portion including a plane other than the (001) plane; In an XPS analysis of the plurality of positive electrode active material particles, the number of magnesium atoms is 0.4 to 1.5 times the number of cobalt atoms, In a STEM-EDX ray analysis of the positive electrode active material particles, a peak of aluminum concentration exists at a depth of 0.5 nm to 50 nm from the surface of the positive electrode active material particles, In a grayscale image obtained by converting a surface SEM image of the positive electrode active material particle into an 8-bit image, the difference between the maximum and minimum grayscale values is 115 or less; The measurement conditions for the surface SEM image of the lithium ion secondary battery were an acceleration voltage of 5 kV and a magnification of 5000 times.
3. A lithium ion secondary battery having a positive electrode and a negative electrode, The positive electrode has a plurality of positive electrode active material particles, the positive electrode active material particles contain magnesium, nickel, aluminum, and lithium cobalt oxide; a surface layer portion of the positive electrode active material particle contains magnesium, In the positive electrode active material particles, a magnesium concentration in a surface portion including a (001) plane is lower than a magnesium concentration in a surface portion including a plane other than the (001) plane; In an XPS analysis of the plurality of positive electrode active material particles, the number of magnesium atoms is 0.4 to 1.5 times the number of cobalt atoms, In a STEM-EDX ray analysis of the positive electrode active material particles, a peak of aluminum concentration exists at a depth of 0.5 nm to 50 nm from the surface of the positive electrode active material particles, a difference between a maximum value and a minimum value of the grayscale value in a grayscale image obtained by converting a surface SEM image of the positive electrode active material particle into an 8-bit image is 70 or more and 115 or less; The measurement conditions for the surface SEM image of the lithium ion secondary battery were an acceleration voltage of 5 kV and a magnification of 5000 times.
4. A lithium ion secondary battery having a positive electrode and a negative electrode, The positive electrode has a plurality of positive electrode active material particles, the positive electrode active material particles contain magnesium, nickel, aluminum, and lithium cobalt oxide; a surface layer portion of the positive electrode active material particle contains magnesium, In the positive electrode active material particles, a magnesium concentration in a surface portion including a (001) plane is lower than a magnesium concentration in a surface portion including a plane other than the (001) plane; In an XPS analysis of the plurality of positive electrode active material particles, the number of magnesium atoms is 0.4 to 1.5 times the number of cobalt atoms, In a STEM-EDX ray analysis of the positive electrode active material particles, a peak of aluminum concentration exists at a depth of 0.5 nm to 50 nm from the surface of the positive electrode active material particles, In a grayscale image obtained by converting a surface SEM image of the positive electrode active material particle into an 8-bit image, the standard deviation of the grayscale values is 11 or less, The measurement conditions for the surface SEM image of the lithium ion secondary battery were an acceleration voltage of 5 kV and a magnification of 5000 times.
5. A lithium ion secondary battery having a positive electrode and a negative electrode, The positive electrode has a plurality of positive electrode active material particles, the positive electrode active material particles contain magnesium, nickel, aluminum, and lithium cobalt oxide; a surface layer portion of the positive electrode active material particle contains magnesium, In the positive electrode active material particles, a magnesium concentration in a surface portion including a (001) plane is lower than a magnesium concentration in a surface portion including a plane other than the (001) plane; In an XPS analysis of the plurality of positive electrode active material particles, the number of magnesium atoms is 0.4 to 1.5 times the number of cobalt atoms, In a STEM-EDX ray analysis of the positive electrode active material particles, a peak of aluminum concentration exists at a depth of 0.5 nm to 50 nm from the surface of the positive electrode active material particles, In a grayscale image obtained by converting a surface SEM image of the positive electrode active material particle into an 8-bit image, the standard deviation of the grayscale values is 8 or less, The measurement conditions for the surface SEM image of the lithium ion secondary battery were an acceleration voltage of 5 kV and a magnification of 5000 times.
6. A lithium ion secondary battery having a positive electrode and a negative electrode, The positive electrode has a plurality of positive electrode active material particles, the positive electrode active material particles contain magnesium, nickel, aluminum, and lithium cobalt oxide; a surface layer portion of the positive electrode active material particle contains magnesium, In the positive electrode active material particles, a magnesium concentration in a surface portion including a (001) plane is lower than a magnesium concentration in a surface portion including a plane other than the (001) plane; In an XPS analysis of the plurality of positive electrode active material particles, the number of magnesium atoms is 0.4 to 1.5 times the number of cobalt atoms, In a STEM-EDX ray analysis of the positive electrode active material particles, a peak of aluminum concentration exists at a depth of 0.5 nm to 50 nm from the surface of the positive electrode active material particles, In a grayscale image obtained by converting a surface SEM image of the positive electrode active material particle into an 8-bit image, the standard deviation of the grayscale values is 4 or more and 8 or less, The measurement conditions for the surface SEM image of the lithium ion secondary battery were an acceleration voltage of 5 kV and a magnification of 5000 times.
7. In any one of claims 1 to 6, The grayscale image is taken from ImageJ. Lithium ion secondary battery.
8. In any one of claims 1 to 7, In the lithium ion secondary battery, in a STEM-EDX ray analysis of the positive electrode active material particles, the aluminum concentration peak is in a deeper region than the magnesium concentration peak.
Citation Information
Patent Citations
Positive electrode and non-aqueous electrolyte secondary battery
JP2019140054A
Method for manufacturing positive electrode active material
JP2019179758A
Method for preparing positive electrode active material for lithium ion secondary battery
JP2020021742A
Positive electrode active material, manufacturing method thereof, and secondary battery
JP2020140954A
Positive electrode active material and method for producing positive electrode active material
WO2020026078A1