Solid polymer electrolytes containing polyalkene carbonates

A polymer matrix of polyalkene carbonate and a second polymer forms a free-standing electrolyte film, addressing conductivity and stability issues in solid-state batteries, enabling scalable and efficient production.

JP7592065B2Active Publication Date: 2024-11-29TOTALENERGIES ONETECH +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2022503778
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-19
Filing Date
2020-07-17
Publication Date
2024-11-29
Estimated Expiration
2040-07-17

AI Technical Summary

Technical Problem

Existing solid electrolytes for lithium-ion batteries face challenges in achieving high ionic conductivity at temperatures below 60°C, mechanical stability, and industrial scalability, particularly in the context of solid-state storage batteries.

Method used

A polymer matrix comprising polyalkene carbonate and a second polymer, which is soluble and partially decomposed to form a free-standing electrolyte film without a substrate, ensuring ionic conductivity and mechanical resilience.

Benefits of technology

The solution provides a solid polymer electrolyte with improved ionic conductivity at room temperature, enhanced mechanical stability, and a simple, cost-effective production method, suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007592065000007
    Figure 0007592065000007
  • Figure 0007592065000008
    Figure 0007592065000008
  • Figure 0007592065000009
    Figure 0007592065000009
Patent Text Reader

Abstract

The present invention relates to a solid polymer electrolyte comprising a polymer matrix containing at least one ionic salt, the polymer matrix comprising at least one polyalkene carbonate, at least one second polymer different from the polyalkene carbonate, and at least one alkene carbonate derived from decomposition of the polyalkene carbonate. The present invention also relates to a method for producing the solid polymer electrolyte, and to electrodes and storage batteries containing the solid polymer electrolyte.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of electrolytes, in particular for storage batteries.

[0002] The invention particularly relates to the field of electrolytes for solid-state batteries. [Background technology]

[0003] The commercialization of lithium-ion batteries since the 90s has been a real innovation in the field of energy storage. Thanks to the constant improvement of their performance, this technology is growing exponentially. The capacity of accumulators in particular makes it possible to develop even further the continuous operating capacity of portable electronic systems. The capacity of accumulators has today reached a threshold that allows their integration into hybrid or purely electric vehicles. The car of the future will be electric. Since then, an ever more intense race for the performance of accumulators has begun in order to maximize their energy density and thus achieve the highest possible continuous operating capacity for electric vehicles.

[0004] Moreover, as the energy density of energy storage systems installed inside vehicles increases, their safety becomes more important. It is fundamentally important that the electrochemical energy of the accumulator is not released as heat in the event of an accident. This is a problem posed in the case of conventional lithium-ion batteries, which have a flammable organic electrolyte that can lead to thermal runaway of the accumulator in the event of a strong temperature rise, which can even lead to an explosion. Lithium-ion battery packs today are thus equipped with complex thermal management systems that normally make it possible to prevent critical developments of this type and approach zero risk of occurrence.

[0005] In this context, intensive research efforts have been identified aimed at developing storage batteries, called "all-solid-state batteries". The basic idea is to replace the liquid electrolyte with an ionically conductive solid electrolyte. Such a material prevents the electrolyte from evaporating and catching fire in case of overheating, which in effect prevents thermal runaway. This may allow for a simplified or less critical (in mass and volume) thermal management. Moreover, the use of solid materials as electrolytes may make it possible to obtain different and even enlarged electrochemical stability regions compared to conventional solvents (mainly cyclic or linear carbonates). In particular, it may be envisaged to have a stable solid electrolyte for lithium metal, as in the case of polyethylene oxide (PEO), thus suppressing / slowing down the dendrite growth compared to that occurring in liquid media. The use of lithium metal, the most reducible element, as the negative electrode may thus allow for an increase in the operating voltage of the electrochemical cell and therefore an increase in its energy density.

[0006] A number of technological approaches have been explored to fabricate solid electrolytes.

[0007] Among them, polymer solid electrolytes can be mentioned. Among them, PEO is today the most reliable technical solution, but it requires high temperatures (above 60 °C) to function effectively. The ether functional groups of PEO make it possible to dissociate lithium salts (typically LiTFSi), and the chain mobility obtained at high temperatures (70-80 °C) then dissociates the cation Li inside the polymer matrix. + PEO has a viscosity of 10 at 80°C. -3 It exhibits a maximum conductivity of 1.0 S / cm. In particular, a wide range of polymers were tested to achieve better conductivity at room temperature compared to that exhibited by PEO.

[0008] In this respect, various past and current efforts are concerned with the development of gelled electrolytes, which are polymer systems in which a liquid electrolyte is trapped, which allows to favor ionic mobility. However, even if the materials display better conductivity (especially at room temperature), they exhibit serious disadvantages, especially a significant loss of mechanical resistance. Moreover, there is a real risk of electrolyte loss when the system is heated. In other words, the increase in ionic conductivity manifests itself in a loss of safety properties for the accumulator.

[0009] In addition to the polymer approach, many Li + Conductive inorganic phases (ceramics and glasses) are being explored. Among them, the commercially available Li7La3Zr2O 12 (LLZO) or substitution composition [garnet structure], Li 1+x Al x Ti 2-x (PO4)3(LATP) [Nasiconic structure] or Li 0.05-3x La 0.5+x TiO3(LLTO) [perovskite structure]. LLZO has Ti in the structure. 4+ Unlike LATP and LLTO, which are subject to the presence of lithium metal, these products have the great advantage of being stable against lithium metal. These products have promising "intragranular" conductivity (10 at room temperature). -4 ~10 -3 The real problem comes from the grain boundaries, where it is essential to limit the resistance contribution at the interfaces between the grains. These materials are therefore conventionally formed by sintering. The resulting ceramic plates then have a significant brittleness that would be a fatal flaw for minimizing their thickness and therefore for integration in cells of several ampere hours. Summary of the Invention [Problem to be solved by the invention]

[0010] The present invention aims to solve the technical problem of providing an ion-conducting electrolyte that increases the storage safety of a storage battery.

[0011] The present invention aims inter alia to solve the technical problem of providing an ionically conductive solid electrolyte, in particular for solid-state storage batteries.

[0012] The present invention aims to solve the technical problem of providing an ionically conductive solid electrolyte at temperatures below 60°C.

[0013] The present invention relates to Li + The object is to solve the technical problem of providing an ion-conducting solid electrolyte.

[0014] The present invention also aims to solve the technical problem, which consists in providing an industrial or industrializable process for the production of an ion-conducting electrolyte, and in particular a process which is easily industrializable and simple to implement.

[0015] The present invention also aims to solve the cited technical problems at limited cost. [Means for solving the problem]

[0016] Surprisingly, it has been found that at least one and preferably all of the above mentioned technical problems can be solved by providing a solid polymer electrolyte comprising a polymer matrix containing at least one ionic salt, said polymer matrix comprising at least one polyalkene carbonate, at least one second polymer different from the polyalkene carbonate, and at least an alkene carbonate resulting from decomposition of the polyalkene carbonate.

[0017] Among the solutions proposed according to the prior art utilizing polyalkene carbonates, the use of a substrate supporting a solid electrolyte is found. Among others, one can cite Adv. Ener. Mater. 2015, 5, 1501082, J. Zhang et al., which uses a nonwoven cellulose membrane as a receiving part for polyalkene carbonate (PPC). PPC and LiTFSI salt are dissolved in acetonitrile. The homogeneous solution is poured onto a cellulose nonwoven substrate and then evaporated in vacuum (100°C-24h). The PPC / cellulose system thus has improved mechanical resistance compared to PPC alone, and also good conductivity at room temperature and above (3.0 x 10 at 20°C). -4 S / cm). However, this solution has the technical drawback that to obtain interesting results, the polyalkene carbonate must be deposited on a substrate. Similarly, in Electro.Comm. 66 (2016) 46-48, K. Kimura et al. report the preparation of a poly(ethylene carbonate) (PEC) system with a very high salt content, i.e., 80% LiTFSI. As this system alone does not have good mechanical resistance, a polyimide matrix is ​​used as a porous substrate supporting the solid electrolyte. PEC and LiTFSI salt are dissolved in acetonitrile. The solution is poured on top of the polyimide matrix and then evaporated in vacuum (60 °C-24 h). The ionic conductivity of the material is 10 at 30 °C. -5 Here too, the polyalkene carbonates are deposited on a substrate to obtain interesting results, which is not an industrially simple enough process.

[0018] These prior art solutions are therefore unsatisfactory.

[0019] The present invention also relates to a method for preparing a solid polymer electrolyte according to the present invention, said method comprising mixing a polyalkene carbonate and a second polymer, both of which are soluble, by means of a solvent or by melting, and partially decomposing the polyalkene carbonate to an alkene carbonate, to obtain a solid polymer electrolyte according to the present invention.

[0020] Advantageously, the matrix according to the invention is capable of absorbing ions, typically ions Li, at room temperature (typically 20° C.) or above. + The present invention therefore makes it possible to overcome the technical problem of the prior art, which consists in supporting the polyalkene carbonates by a substrate.

[0021] Advantageously, the matrix according to the invention comprises at least one second polymer which is an amorphous polymer.

[0022] Advantageously, the matrix according to the invention comprises a liquid fraction within the matrix due to the degradation of the polymer.

[0023] Advantageously, the matrix according to the invention has a unique morphology which exhibits very good ionic conductivity.

[0024] According to the invention, the matrix may contain one or more polymers other than the polyalkene carbonate, thus the matrix may contain one or more polymers of the second polymer type according to the invention.

[0025] According to one embodiment, the matrix comprises as the second polymer one or more polymers selected from the following: polyolefins, polycarbonates, halogenated polymers, acrylic polymers, acrylate polymers, methacrylate polymers, vinyl acetate polymers, polyethers, polyesters, polyamides, aromatic polymers, elastomeric polymers such as HNBR, polyisoprene, rubbery polymers, and any mixtures thereof.

[0026] Preferably, the second polymer is an elastomer.

[0027] Typically, the matrix comprises at least two polymeric phases, one comprising at least one polyalkene carbonate that can be decomposed or split into alkene carbonates, and one comprising at least one second polymer.

[0028] Typically, the matrix comprises at least 10 ppm of acene carbonate relative to the total mass of the matrix. According to one variant, the matrix comprises at least 100 ppm, or even at least 1000 ppm, of acene carbonate relative to the total mass of the matrix.

[0029] Typically, the alkene polycarbonate is degraded to at most 99% by weight, preferably at most 70% by weight and even more preferably at most 50% by weight, relative to the initial weight of the alkene polycarbonate. According to one variant, the matrix comprises less than 50% of acene carbonate relative to the total weight of the matrix.

[0030] According to one variant, the alkene carbonate is in monomeric form.

[0031] Advantageously, according to the invention, the matrix does not contain a macro-separation between the phase comprising the polyalkene carbonate and the phase comprising the second polymer.

[0032] Thus, the second polymer is selected to avoid macrophase separation. Absence of macrophase separation means that the pure phase of undispersed polymer with dimensions greater than a few hundred microns is hardly detectable. Macrophase separation can be looked for by nanoscale Fourier transform infrared spectroscopy. Macrophase separation can also be looked for by scanning electron microscopy techniques.

[0033] More generally, any polymeric base can be associated with the polyalkene carbonate, provided that the morphology does not result in macrophase separation as defined above.

[0034] Generally, an amount of polyalkene carbonate relative to the total amount of polymer, in the presence of at most 80% (w / w), makes it possible to obtain sufficient mechanical properties in electrochemical cycles or in contact with lithium metal and thus to produce a satisfactory solid electrolyte.

[0035] According to one embodiment, the polyalkene carbonate is present in an amount ranging from 5 to 80% by weight, preferably from 10 to 70% by weight, relative to the total polymer weight of the matrix.

[0036] According to one embodiment, an amount of polyalkene carbonate between 10 and 70% (w / w) is preferred. Generally, an amount of polyalkene carbonate between 15 and 60% (w / w) is more preferred. More preferably, the amount of polyalkene carbonate ranges between 20 and 50% (w / w).

[0037] The polyalkene carbonate does not have a specific molar mass: it could be used alone or as a mixture of various molar masses.

[0038] Advantageously, the polymer matrix comprises polyalkene carbonates having a high molar mass and polyalkene carbonates having a low molar mass relative to one another.

[0039] Thus, the oligomers with low molar mass (less than 15000 g / mol) make it possible to flow the mixture by plasticizing the polymers with high molar mass (greater than 15000 g / mol). This embodiment advantageously makes it possible to adapt the final viscosity of the mixture in relation to the selected process with or without solvent, or in relation to the final formulation with or without filler, or even in relation to a thicker or thinner final product. Thus, the proportion of polyalkene carbonates with low molar mass relative to the total amount of polyalkene carbonates typically varies between 0.1 and 99.9%, preferably between 5 and 90% and even more preferably between 10 and 80%.

[0040] By way of example, mention may be made of PPC polyols such as Converge 212-10 as low molar mass polyalkene carbonates and QPac® 40 as high molar mass polyalkene carbonates.

[0041] According to one embodiment, the ionic salts are chosen from among the salts of metal ions of metals belonging to group 1 of the periodic table.

[0042] Thus, the ionic salt or salts are at least partially dissociated in at least one of the polymeric phases.

[0043] In one embodiment, the ionic salt is selected from the group consisting of LiBETI, LiC2F5SO3, LiC4F9SO3, LiCF3SO3, NaI, NaSCN, NaBr, KI, KBr, LiClO4, LiBF4, LiAsF6, LiPF6, LiNO3, Li(CF3SO2)2N, Li(CF3SO2)3C, LiN(SO2C2F5)2, lithium alkylfluorophosphates, lithium difluoro(oxalato)borate, lithium bis(oxalato)borate, MTFSiLi, STFSiLi, and any mixture thereof.

[0044] According to one embodiment, the matrix comprises an inorganic or organic solid filler.

[0045] Thus, according to one embodiment, the matrix contains inorganic or organic solid fillers to provide various properties such as mechanical reinforcement, assistance with ionic conductivity, or assistance with the insertion and desorption of metal ions.

[0046] By way of example, solid fillers that can improve conductivity are: inert fillers, such as Al2O3, SiO2, cellulose, starch, which are not cation-conducting but can improve the transfer of ions through surface interactions of the fillers, or -capacitive cationically conductive filler (e.g. ceramic or glass) It is.

[0047] According to one embodiment, the matrix contains a solid filler that allows for the insertion and desorption of metal salts, called "active". An example is C-LiFePO4, but other examples include positive electrode active materials (e.g., LiCoO2, LiMnO4, LiNi 1 / 3 Mn 1 / 3 Co 1 / 3 O2, etc.) or negative electrode active material (e.g. Li4Ti5O 12 All active materials known to those skilled in the art, such as graphite, graphite, etc., should also be considered.

[0048] According to one embodiment, the matrix comprises an electrically conductive filler, which may include, for example, conductive carbon black, but also graphite, graphene, carbon nanofibers and carbon nanotubes, or mixtures thereof.

[0049] According to one embodiment, the solid polymer electrolyte is in the form of a film less than 1 mm thick.

[0050] The film according to the present invention typically has a thickness of from 10 to 500 micrometers, for example from 80 to 300 micrometers and typically from 90 to 200 micrometers.

[0051] Typically, the manufacturing method according to the present invention involves mixing of a polymer, including a polyalkene carbonate and a second polymer, either by a dry process, a "polymer in the molten state" (also called the melt process) or by a solvent process (also called the wet process).

[0052] According to one embodiment, the method includes heating during mixing of the polyalkene carbonate and the second polymer.

[0053] Advantageously, according to one embodiment, melt mixing is carried out completely or partially or followed by heating at a temperature sufficient for partial decomposition of the polyalkene carbonate to an alkene carbonate.

[0054] According to one variant, the melt mixing is effected entirely at a temperature sufficient for partial decomposition of the polyalkene carbonate to an alkene carbonate.

[0055] According to one variant, the melt mixing is effected partially, preferably at the end of the mixing, at a temperature sufficient for partial decomposition of the polyalkene carbonate to an alkene carbonate.

[0056] According to one embodiment, mixing by the solvent method is accomplished at room temperature (typically 20° C.), and the mixture is then dried at a temperature sufficient to remove the solvent and partially decompose the polyalkene carbonate to an alkene carbonate.

[0057] In the liquid process, preferably a solvent is used whose boiling temperature does not reach the decomposition temperature of the polyalkene carbonate.

[0058] According to one embodiment, the method includes melt blending a polyalkene carbonate with a second polymer, the blending being achieved in at least partial contact with an inorganic filler that promotes partial decomposition of the polyalkene carbonate to an alkene carbonate.

[0059] According to one embodiment, the method includes, after drying, the addition of a reducing metal, for example lithium, under conditions to partially decompose the polyalkene carbonate to an alkene carbonate. Advantageously, in the presence of such a metal, no heating is required to obtain the partial decomposition of the polyalkene carbonate to an alkene carbonate.

[0060] Preferably, the mixture is then cast into the form of a film and then dried.

[0061] Advantageously, the mixture of polymers makes it possible to obtain a film that does not require a substrate, unlike the prior art mentioned above.

[0062] Preferably, the mixture is dried during the drying step.

[0063] Typically, drying of the mixture is carried out for a sufficient time to achieve the desired dryness, for example at least 1 hour under vacuum at 60° C. The vacuum is achieved according to conditions known to those skilled in the art, for example using a vacuum pump.

[0064] Preferably, according to one variant, at the end of the mixing in the melt process or after drying in the liquid process, the material is heated to a temperature which releases in situ part of the alkene carbonate inside the polymer matrix. Thus, according to one variant, the method comprises heating at a temperature sufficient to partially decompose the polyalkene carbonate into alkene carbonate, also called the conditioning temperature.

[0065] Advantageously, the conditioning temperature can be lowered, for example for the production of a solid electrolyte in contact with a metal, e.g., lithium metal, anode, in the presence of a metal that promotes partial decomposition of the polyalkene carbonate to an alkene carbonate. Advantageously, according to one embodiment, heating at the conditioning temperature is performed on a storage battery comprising a solid polymer electrolyte, e.g., before commercialization or use.

[0066] According to one embodiment, the method includes heating the solid polymer electrolyte after mixing at a conditioning temperature.

[0067] The conditioning temperature is for example greater than 80°C, such as greater than 100°C, and further for example greater than 120°C.

[0068] According to one embodiment, the conditioning temperature is above 150°C, such as above 170°C.

[0069] Thus, advantageously, according to one variant of the method according to the invention, the mixture obtained is treated at the conditioning temperature for a time sufficient to improve its ionic conductivity (typically between 1 and 30 minutes) and then returned to room temperature.

[0070] According to one variant, the method comprises the addition to the polymer mixture of specific additives to improve and / or optimize the production process of the solid polymer electrolyte.

[0071] According to one variant, the method comprises crosslinking of the second polymer or polymers, preferably during mixing with the polyalkene carbonate, which crosslinking can take place exclusively with the second polymer or polymers (other than the polyalkene carbonate) or with the polyalkene carbonate in so far as this does not prevent the in situ generation of the corresponding alkene carbonate.

[0072] According to one variant, the method comprises the addition of one or more compounds forming crosslinkers for one or more second polymers mixed with the polyalkene carbonate.

[0073] According to one variant, the method includes the addition of one or more auxiliary agents that aid in the crosslinking and its homogenization. For example, mention may be made of organic peroxides as crosslinking agents or triallyl cyanurate as auxiliary. But it is equally possible to use all compounds that allow the crosslinking of the second polymer, such as photoinitiators or sulfur compounds specific for the crosslinking of rubber. It is also possible to take advantage of the chemical reaction of bifunctional compounds on the pendant molecular chains (if present) of the second polymer, such as maleic anhydride, epoxide or also acid, alcohol, amine, amide or ester functional groups, taking into account that the reaction on the pendant functional groups leads to the formation of bridges between the polymer chains and thus to the crosslinking of the system. Advantageously, the crosslinking increases the cohesion of the matrix. Thus, the use of crosslinking agents, and possibly auxiliary agents, is therefore useful but not essential for the invention, entirely depending on the intended application and the envisaged method.

[0074] The present invention also relates to an electrode comprising at least one solid polymer electrolyte according to the present invention or obtainable by the method according to the present invention.

[0075] The present invention also relates to a storage battery comprising at least one solid polymer electrolyte according to the invention or obtainable by the method according to the invention.

[0076] According to one variant, the accumulator is a lithium battery with solid polymer electrolyte.

[0077] In particular, solid polymer electrolytes in the form of films can be used as the membrane of energy storage batteries, which are typically inserted between the two electrodes of the battery. [Brief description of the drawings]

[0078] [Figure 1] 4 shows the voltage (in volts, expressed in V) as a function of time (h) for a system with a solid polymer electrolyte according to example 2b between two lithium metals at 60° C. [Diagram 2] 1 shows a system using a polymer solid electrolyte according to Example 4 between two metallic lithium electrodes at 60° C., where a short circuit occurs within 30 minutes of use. [Diagram 3] 1 shows the initial discharge of an electrode having the composition described in Example 5. [Figure 4] FIG. 1 shows the cycling stability of half-cells using a C-LFP electrode (Example 5) vs. Li metal. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0079] Percentages are expressed by weight relative to the total weight of the composition under consideration, unless otherwise indicated.

[0080] Temperatures are room temperature (20° C.) unless otherwise indicated. Pressures are atmospheric (101325 Pa) unless otherwise indicated.

[0081] Electrochemical analysis was performed using electrochemical impedance spectroscopy (MTZ-35 instrument, BioLogic) with a temperature control attachment (ITS instrument, BioLogic). Morphology was obtained by scanning electron microscopy (SEM).

[0082] Example 1: Solid electrolyte produced by melt process (or dry process) A mixture was made by combining 10.1 g HNBR (zetpol 2010), 5.5 g PPC (QPac40), 5.3 g PPC polyol (Converge 212-10) and 8.5 g LiTFSI in an internal mixer. After the materials were added, they were mixed for 5 minutes at 85±10°C.

[0083] [Table 1]

[0084] The final mixture was cast into films approximately 100 μm thick by rolling using Dr Collin's Teachline CR72T. The films were then dried at 60° C. for at least 12 hours under vacuum provided by an Edwards RV12 pump.

[0085] 1.b. A film of the same composition was conditioned at 190° C. for 1 hour.

[0086] Conductivity measurements were performed on various films and the results are summarized in Table 5.

[0087] Example 2: Solid electrolyte produced by melt process A mixture was made by combining 13.4g HNBR (zetpol 2010), 2.7g PPC (QPac40), 2.8g PPC polyol (Converge 212-10) and 8.2g LiTFSI in an internal mixer. After the materials were added, they were mixed for 5 minutes at 85±10°C.

[0088] [Table 2]

[0089] The final mixture was cast into films approximately 100 μm thick by rolling using Dr Collin's Teachline CR72T. The films were then dried at 60° C. for at least 12 hours under vacuum provided by an Edwards RV12 pump.

[0090] 2.b. A film of the same composition was conditioned at 190° C. for 1 hour.

[0091] Finally, conductivity measurements of the various films were performed and the results are summarized in Table 5. The polarization behavior of the conditioned films was tested between two electrodes of metallic lithium subjected to different current densities (Figure 1).

[0092] Example 3: Solid electrolyte produced by melt process A mixture was made by combining 8.4g HNBR (zetpol 0020), 5.6g PPC (QPac40), 5.3g PPC polyol (Converge 212-10) and 8.4g LiTFSI in an internal mixer. After the materials were added, they were mixed for 5 minutes at 85±10°C.

[0093] [Table 3]

[0094] The final mixture was cast into films approximately 100 μm thick by rolling using Dr Collin's Teachline CR72T. The films were then dried at 60° C. for at least 12 hours under vacuum provided by an Edwards RV12 pump.

[0095] 3.b. A film of the same composition was conditioned at 190° C. for 1 hour.

[0096] Finally, conductivity measurements were performed on the various films, and the results are summarized in Table 5.

[0097] Example 4: Comparative Example A mixture was made by combining 12.2g of PPC (QPac40) and 11.6g of PPC polyol (Converge 212-10) and 10.2g of LiTFSI in a 30ml internal mixer. After the materials were added, they were mixed for 5 minutes at 65±5°C.

[0098] [Table 4]

[0099] Conductivity measurements were taken for the various films and the results are summarized in Table 5. The polarization behavior of the conditioned films was evaluated at 0.1 mA / cm 2 The test was performed between two electrodes of metallic lithium subjected to a thermal shock (Figure 2).

[0100] [Table 5]

[0101] Example 5: Electrodes containing polymer solid electrolyte produced by melt processing Into a 30 ml internal mixer were added 4.8 g HNBR (zetpol 2010), 3.0 g PPC (QPac40), 2.9 g PPC polyol (Converge 212-10), 4.6 g LiTFSI, 33.5 g LiFePO4 (Lifepower P2) and 2.6 g carbon black (Timcal C65). After the materials were added, they were mixed for 5 minutes at 85±10°C.

[0102] The final mixture has the following composition:

[0103] [Table 6]

[0104] The final mixture was cast into films approximately 50 μm thick by rolling using Dr Collin's Teachline CR72T. The films were then attached to current collectors and dried at 60° C. for at least 12 hours under vacuum provided by an Edwards RV12 pump.

[0105] The electrodes thus obtained were assembled into button cells using the mixture of Example 1 with a thickness of approximately 75 μm as separator and lithium metal as anode. The two films were conditioned at 190° C. for 1 h before assembly into a button cell type accumulator. A capacity of LFP 164 mAh / g at 60° C. during the first discharge at a rate of C / 20 (FIG. 3) and stable over at least 12 cycles (FIG. 4) is obtained. [Prior art documents] [Non-patent literature]

[0106] [Non-Patent Document 1] Adv.Ener.Mater.2015,5,1501082,J.Zhang et al. [Non-Patent Document 2] Electro.Comm.66(2016)46-48, K. Kimura et al.

Claims

1. 1. A solid polymer electrolyte comprising a polymer matrix including at least one ionic salt, the polymer matrix comprising at least one polyalkene carbonate, at least one second polymer that is an elastomeric polymer, and at least an alkene carbonate derived from decomposition of the polyalkene carbonate.

2. 2. The solid polymer electrolyte according to claim 1, characterized in that the polyalkene carbonate is present in an amount of 5 to 80% by weight, based on the total polymer weight of the matrix.

3. 3. The solid polymer electrolyte according to claim 1, wherein the polymer matrix comprises polyalkene carbonates having a relatively high molar mass and polyalkene carbonates having a relatively low molar mass.

4. 4. A solid polymer electrolyte according to claim 1, characterized in that the ionic salt is chosen from among the salts of metal ions of metals belonging to group 1 of the periodic table.

5. The ionic salts are LiBETI, LiC 2 F 5 SO 3 , LiC 4 F 9 SO 3 , LiCF 3 SO 3 , NaI, NaSCN, NaBr, KI, KBr, LiClO 4 , LiBF 4 , LiAsF 6 , LiPF 6 , LiNO 3 , Li(CF 3 SO 2 ) 2 N, Li(CF 3 SO 2 ) 3 C, LiN(SO 2 C 2 F 5 ) 2 5. The solid polymer electrolyte according to claim 1, wherein the lithium phosphate is selected from the group consisting of lithium alkylfluorophosphate, lithium difluoro(oxalato)borate, lithium bis(oxalato)borate, MTFSiLi, STFSiLi, and any mixture thereof.

6. 6. The solid polymer electrolyte according to claim 1, wherein the second polymer is selected from HNBR, polyisoprene, rubbery polymers, and any mixture thereof.

7. 7. A solid polymer electrolyte according to claim 1, characterized in that the matrix does not contain a macro-separation between a phase comprising the polyalkene carbonate and a phase comprising the second polymer.

8. 8. The solid polymer electrolyte according to claim 1, characterized in that the matrix contains an inorganic or organic solid filler.

9. 9. A solid polymer electrolyte according to claim 1, characterized in that the solid polymer electrolyte is in the form of a film with a thickness of less than 1 mm.

10. 10. A solid polymer electrolyte according to claim 1, characterized in that the polymer matrix is ​​obtained by mixing the polyalkene carbonate and the second polymer, both of which are soluble, by means of a solvent or by melting.

11. 11. A method for producing a solid polymer electrolyte according to any one of claims 1 to 10, the method comprising mixing the polyalkene carbonate and the second polymer, both of which are soluble, by means of a solvent or by melting, and partially decomposing the polyalkene carbonate to an alkene carbonate, to obtain a solid polymer electrolyte according to any one of claims 1 to 10.

12. 12. The method of claim 11, wherein the method includes heating the solid polymer electrolyte.

13. 13. An electrode comprising at least one solid polymer electrolyte according to any one of claims 1 to 10 or obtainable by the method according to claim 11 or 12.

14. Storage battery comprising at least one solid polymer electrolyte according to any one of claims 1 to 10 or obtainable by the method according to claim 11 or 12.

15. 15. The accumulator according to claim 14, characterized in that it is a lithium battery with a solid polymer electrolyte.

Citation Information

Patent Citations

  • Multilayer polymer solid electrolyte and all-solid-state battery comprising same

    EP3457486A1

  • Polymeric Electrolyte, Method for Production Thereof, and Electrochemical Element

    US20090065730A1

  • Process for preparing an electrode composition or composition with magnetic properties, mixture and composition obtained by means of said process and said electrode

    US20160340476A1

  • All solid state secondary-battery additive, all-solid-state secondary battery, and method for producing same

    WO2017030127A1