Method for permanently bonding wafers

By forming a reservoir on one substrate surface and using plasma activation to enhance hydrophilicity and smoothness, the method addresses reproducibility and temperature issues in substrate bonding, achieving a strong, irreversible bond with reduced mechanical stress and contamination.

JP7592118B2Active Publication Date: 2024-11-29EV GRP E THALLNER GMBH
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2023061728
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-04-05
Publication Date
2024-11-29
Estimated Expiration
2031-01-25

AI Technical Summary

Technical Problem

Existing methods for bonding substrates are not reproducible, require high temperatures, and can damage active components on the substrate, leading to high energy consumption and mechanical stress, while also failing to ensure low pollution and mutual compatibility during the bonding process.

Method used

A method involving the formation of a reservoir on one substrate surface, filled with a raw material that reacts with the other substrate to form a permanent bond, using plasma activation to enhance hydrophilicity and smoothness, allowing for a controlled reaction at low temperatures to increase bonding strength.

Benefits of technology

The method achieves a strong, irreversible bond with increased bonding force, reducing mechanical stress and temperature requirements, while maintaining compatibility with existing components and minimizing contamination.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007592118000004
    Figure 0007592118000004
  • Figure 0007592118000005
    Figure 0007592118000005
  • Figure 0007592118000006
    Figure 0007592118000006
Patent Text Reader

Abstract

To find out a method of carefully providing permanent bonding having bonding strength which is as high as possible.SOLUTION: A method comprises a step of forming a storage portion (5) in a surface layer (6) on a first contact surface (3), a step of at least partially filling the storage portion (5) with a first raw material or a first raw material group, a step of bringing the first contact surface (3) into contact with the second contact surface (4) to form temporary bonding connection, and a step that forms permanent bonding between the first contact surface (3) and the second contact surface (4) and reacts the first raw material with a second raw material contained in a reaction layer (7) of the second substrate (2) to at least partially strengthen the permanent bonding, thereby bonding the first contact surface (3) of the first substrate (1) to the second contact surface (4) of the second substrate (2).SELECTED DRAWING: Figure 5
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method of bonding a first contact surface of a first substrate to a second contact surface of a second substrate according to embodiment 1. [Background technology]

[0002] The aim in the permanent or irreversible bonding of substrates is to produce an interconnection between the two contact surfaces of the substrates that is as strong as possible and in particular irreversible, and thus a high bonding force. In the prior art there are various techniques and manufacturing methods for such bonding.

[0003] Known manufacturing methods and techniques practiced to date are often not reproducible or not sufficiently reproducible and are hardly applicable, especially when conditions change, especially in the manufacturing methods currently used, which often involve high temperatures, especially above 400° C., to ensure reproducible results.

[0004] Technical problems such as high energy consumption and possible destruction of structures present on the substrate are partly a result of the high temperatures, much higher than 300°C, that have been required to date for high bonding strength. A method for low-temperature bonding is shown in the following Patent Document 1. Further bonding methods are shown in the following Patent Documents 1 to 8.

[0005] Other requirements include: - Front-end-of-line compatibility It is defined as the compatibility of processes during the manufacture of electrically active components. The bonding process must therefore be designed in such a way that active components, such as transistors, already present on the structure wafer are not adversely affected or damaged during processing. Compatibility criteria include (mainly for CMOS structures) mainly purity of chemical elements and mechanical load capacity, mainly due to thermal stresses. - Low pollution - No force applied

[0006] A reduced bond strength requires more careful handling of the structural wafer, thus reducing the probability of failure due to direct mechanical loading. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] International Publication No. 01 / 61743 Brochure [Patent Document 2] US Patent Application Publication No. 2003 / 0089950 [Patent Document 3] US Patent Application Publication No. 2002 / 0048900 [Patent Document 4] US Patent Application Publication No. 2008 / 0006369 [Patent Document 5] U.S. Pat. No. 5,451,547 [Patent Document 6] European Patent Application Publication No. 0584778 [Patent Document 7] U.S. Pat. No. 5,427,638 [Patent Document 8] Japanese Patent Application Publication No. 5-166690 Summary of the Invention [Problem to be solved by the invention]

[0008] It is therefore an object of the present invention to devise a method for deliberately producing a permanent bond having the highest possible bond strength. [Means for solving the problem]

[0009] This object is achieved by the features described in embodiment 1. Advantageous developments of the invention are described in the dependent embodiments. Any combination of at least two of the features described in the description, the claims and at least one of the drawings also falls within the framework of the invention. In the given value ranges, values ​​that are within the indicated limits are also disclosed as boundary values ​​and are claimed in any combination.

[0010] The idea behind the invention is to come up with a reservoir on at least one of the substrates for holding a first raw material, which reacts after contact or temporary bonding between the substrates with a second raw material present in the other substrate, thereby forming an irreversible or permanent bond between the substrates. Before or after forming the reservoir in a surface layer on the first contact surface, the substrate is generally cleaned, in particular by a flushing step. This cleaning must generally ensure that there are no particles on the surface, which would result in non-bonding spots. The reservoir and the raw material contained therein provide the technical possibility of inducing a reaction that strengthens the permanent bond and increases the bonding rate in a controlled manner directly on the contact surface after forming the temporary or reversible bond, in particular by deforming at least one of the contact surfaces, preferably the contact surface facing the reservoir, with said reaction.

[0011] There are various possibilities for creating a weak interaction between the contacting surfaces of the substrates as a temporary bonding step to form a temporary or reversible bond between the substrates. The strength of the temporary bond is lower than the strength of the permanent bond, at least 2 to 3 times lower, in particular 5 times lower, preferably 15 times lower and even more preferably 25 times lower. As a guideline, the temporary bond strength of pure non-activated hydrophilized silicone is about 100 mJ / m 2 The temporary bonding strength of pure plasma-activated hydrophilic silicon is about 200-300 mJ / m 2Temporary bonding between molecule-wetted substrates is achieved by van der Waals interactions between molecules on different sides of the substrates. Therefore, molecules with primarily permanent dipole moments are suitable to enable temporary bonding between wafers. The following chemical compounds are mentioned by way of example as interconnecting agents, but are not limited to them: - water - Thiol - AP3000 - Silane, and / or -Silanol

[0012] Suitable substrates according to the invention are those whose materials, as raw materials, can react with separately supplied raw materials to form products with higher molar volumes, so that a growth layer is formed on the substrate. The following combinations are particularly advantageous, in which to the left of the arrow the raw materials are listed, and to the right of the arrow the products are listed, without separately listing the supplied raw materials or by-products that react with the listed raw materials: - Si → SiO2, Si3N4, SiN x O y - Ge → GeO2, Ge3N4 - α-Sn → SnO2 - B → B2O3, BN - Se → SeO2 - Te → TeO2, TeO3 - Mg → MgO, Mg3N2 - Al → Al2O3, AlN - Ti → TiO2, TiN - V→V2O5 - Mn→MnO, MnO2, Mn2O3, Mn2O7, Mn3O4 - Fe → FeO, Fe2O3, Fe3O4 - Co → CoO, Co3O4 - Ni → NiO, Ni2O3 - Cu → CuO, Cu2O, Cu3N - Zn → ZnO - Cr → CrN, Cr 23C6, Cr3C, Cr7C3, Cr3C2 - Mo→Mo3C2 - Ti → TiC - Nb → Nb4C3 - Ta → Ta4C3 - Zr → ZrC - Hf→HfC - V → V4C3, VC - W→W2C, WC - Fe → Fe3C, Fe7C3, Fe2C

[0013] As substrates, mixed types of the following semiconductors are also conceivable: - III-V: GaP, GaAs, InP, InSb, InAs, GaSb, GaN, AlN, InN, Al x Ga 1-x As, In x Ga 1-x N - IV-IV: SiC, SiGe - III-IV: InAlP - Nonlinear optical system: LiNbO3, LiTaO3, KDP(KH2PO4) - Solar cells: CdS, CdSe, CdTe, CuInSe2, CuInGaSe2, CuInS2, CuInGaS2 - Conductive oxide: In 2-x Sn x O 3-y

[0014] As claimed in the present invention, on at least one of the wafers and directly on the respective contact surface there is a reservoir capable of storing in a quantity at least one of the raw materials supplied for the volume expansion reaction. The raw materials can thus be, for example, O2, O3, H2O, N2, NH3, H2O2, etc. Based on the tendency of the reaction partners to reduce the energy of the system, especially due to the expansion caused by the oxide growth, possible gaps, holes and cavities between the contact surfaces are minimized, thus increasing the bonding force by narrowing the distance between the substrates in these areas. In the best possible case, existing gaps, holes and cavities are completely closed, resulting in an increase in the overall bonding area and a corresponding increase in the bonding force as claimed in the present invention.

[0015] The contact surfaces typically exhibit a root mean square roughness (Rq) of 0.2 nm, which corresponds to a surface peak-to-peak value in the range of 1 nm. These empirical values ​​were determined using atomic force microscopy (AFM).

[0016] The reaction claimed in this invention is suitable for enabling the growth of a growth layer of only 0.1 to 0.3 nm on the wafer surface of a conventional circular wafer with a diameter of 200 to 300 mm and having one monolayer (ML) of water.

[0017] Thus, as claimed in the present invention, in particular at least 2 ML, preferably at least 5 ML, more preferably at least 10 ML of fluid, in particular water, is stored in the reservoir.

[0018] It is particularly preferred to form the reservoir by plasma exposure, because the plasma exposure additionally results in a synergistic effect of smoothing and hydrophilizing the contact surface. The surface is smoothed by plasma activation, mainly due to the viscous flow of the material in the surface layer. The increase in hydrophilicity is caused in particular by an increase in silicon hydroxyl bonds, preferably by the decomposition of Si-O bonds present on the surface, such as Si-O-Si, in particular according to the reaction shown in the following chemical formula (1):

[0019] [ka]

[0020] Another side effect, which is obtained as a result of the above mentioned effects in particular, is that the temporary bond strength is increased, in particular by a factor of 2 to 3.

[0021] The reservoirs in the surface layer on the first contact surface of the first substrate are formed by plasma activation of the first substrate, for example coated with thermal oxide. The plasma activation is carried out in a vacuum chamber so that the conditions required for the plasma can be adjusted. As claimed in the present invention, N2, O2 or argon gas is used as the plasma discharge with an ion energy in the range of 0 to 2000 eV, so that the reservoirs are formed to a depth of up to 20 nm, preferably up to 15 nm, more preferably up to 10 nm, most preferably up to 5 nm in the treatment surface, in this case the first contact surface. As claimed in the present invention, at least one of the respective particle types, atoms and molecules suitable for forming the reservoirs can be used. Preferably, atoms or molecules or both are used that can form the reservoirs with the required properties. The relevant properties are mainly the pore size, pore distribution and pore density. Alternatively, as claimed in the present invention, a mixture of gases can be used, such as air or a forming gas consisting of 95% Ar and 5% H2. Depending on the gas used, N, among others, may be present in the reservoir during plasma processing. + , N2 + , O + , O2 + , Ar + ions are present. The first raw material can be accommodated in the unoccupied free space.

[0022] The reservoirs are formed based on the following considerations: The pore size is less than 10 nm, preferably less than 5 nm, more preferably less than 1 nm, even more preferably less than 0.5 nm, and most preferably less than 0.2 nm.

[0023] The pore density is preferably directly proportional to the density of the particles which produce the pores by the impact action, and most preferably can be varied by the partial pressure of the impacting species, and also depending on the treatment time and in particular the parameters of the plasma system used.

[0024] The pore distribution preferably has at least one region of highest pore density below the surface, which, by varying the parameters of several such regions, overlaps and preferably becomes a flat-shaped region (see FIG. 7). The pore distribution decreases to zero with increasing thickness. The region near the surface during the bombardment has approximately the same pore density as the pore density near the surface. After the plasma treatment is completed, the pore density on the surface may be reduced as a result of stress relaxation mechanisms. The pore distribution through the thickness has steep flanks towards the surface and rather flatter, but continuously decreasing, flanks towards the bulk (see FIG. 7).

[0025] Similar considerations regarding pore size, pore distribution, and pore density apply to any method not performed with a plasma.

[0026] The reservoir can be designed by controlling and combining the process parameters. Figure 7 shows the concentration of nitrogen atoms implanted by the plasma as a function of the penetration depth into the silicon oxide layer. By varying the physical parameters, it was possible to obtain two profiles. The first profile 11 is formed by faster accelerated atoms penetrating deeper into the silicon oxide, whereas profile 12 is formed after changing the process parameters to a lower density. The superposition of the two profiles results in a sum of curves 13, which is characteristic of the reservoir. The relationship between the concentrations of the implanted atomic and / or molecular species is clear. A higher concentration indicates an area with a more defective structure and therefore more space to accommodate the subsequent feedstock. A dedicated control of the process parameters during plasma activation allows to achieve a reservoir in which the added ions are distributed as uniformly as possible over the depth, by successively changing them.

[0027] As a reservoir or instead of a reservoir formed by plasma, it is conceivable to use, on at least one of the substrates, at least the first substrate, a TEOS (tetraethyl orthosilicate) oxide layer. This oxide is generally less dense than a thermal oxide and for this reason is advantageous to compress as claimed in the present invention. The compression is carried out by a thermal treatment with the aim of adjusting the reservoir to a defined porosity.

[0028] According to one embodiment of the invention, the filling of the reservoir can be carried out simultaneously with the formation of the reservoir, particularly advantageously by applying the reservoir as a coating to the first substrate, the coating already comprising the first raw material.

[0029] The reservoir may be considered as a porous layer with a porosity in the nanometer range or as a layer having channels with a channel width of less than 10 nm, more preferably less than 5 nm, even more preferably less than 2 nm, most preferably less than 1 nm, and most preferably of all less than 0.5 nm.

[0030] With regard to the step of filling the reservoir with the first ingredient or first group of ingredients, the following embodiments, or combinations thereof, are contemplated as claimed in the present invention. - exposing the reservoir to the ambient atmosphere; - especially the flushing step with deionized water - flushing with a fluid containing or consisting of a raw material, in particular H2O, H2O2, NH4OH; - exposing the reservoir to any gas atmosphere, in particular atomic, molecular or mixed gases; - exposing the reservoir to an atmosphere containing water vapor or hydrogen peroxide vapor; and - depositing a reservoir already filled with the raw material as a surface layer on a first substrate;

[0031] At least one of the compounds O2, O3, N2, NH3, H2O, H2O2, and NH4OH may be considered as raw materials.

[0032] The use of hydrogen peroxide vapor as mentioned above is considered a preferred version in addition to the use of water. Hydrogen peroxide has the additional advantage of having a higher oxygen to hydrogen ratio. Moreover, hydrogen peroxide dissociates into hydrogen and oxygen above a certain temperature and / or when using high frequency electromagnetic fields in the MHz range.

[0033] According to an advantageous embodiment of the invention, the formation of the growth layer and the strengthening of the irreversible bond are achieved by diffusion of the first source material into the reaction layer.

[0034] According to another advantageous embodiment of the invention, it is intended that the formation of the irreversible bond typically takes place at less than 300° C., advantageously less than 200° C., more preferably less than 150° C., even more preferably less than 100° C., most preferably at room temperature, in particular for a period of up to 12 days, more preferably up to 1 day, even more preferably up to 1 hour, most preferably up to 15 minutes.

[0035] In this specification, irreversible bonding is defined as 1.5 J / m 2 Ultra, especially 2J / m 2 More than 2.5 J / m 2 It is particularly advantageous for the adhesive to have a bond strength of greater than 1000 MPa.

[0036] The bonding strength can be particularly advantageously increased by forming, during the reaction, a product in the reaction layer having a molar volume greater than the molar volume of the second raw material, as claimed in the present invention. In this way, growth is caused on the second substrate, so that the gap between the contacting surfaces can be closed by a chemical reaction, as claimed in the present invention. As a result, the distance between the contacting surfaces, and therefore the average distance, is reduced and the dead space is minimized.

[0037] The formation of the reservoir is achieved by plasma activation, in particular with an activation frequency between 10 and 600 kHz and / or a current of 0.075 to 0.2 Watts / cm 2 As long as the application is performed with a power density between 0.1 and 0.6 mbar and / or with a pressure between 0.1 and 0.6 mbar, additional effects such as smoothing of the contact surface and even a clear increase in the hydrophilicity of the contact surface are obtained.

[0038] Alternatively, the formation of the claimed reservoirs can be achieved by using a tetraethoxysilane oxide layer as a surface layer, specifically compressed in a controlled manner to a certain porosity.

[0039] According to another advantageous embodiment of the invention, it is provided that the surface layer consists mainly, in particular essentially completely, in particular of amorphous, in particular of silicon dioxide produced by thermal oxidation, and the reaction layer consists mainly, preferably essentially completely, of an oxidizable material, in particular of Si, Ge, InP, GaP or GaN. A particularly stable reaction, which closes existing gaps particularly effectively, is made possible by oxidation.

[0040] It is particularly advantageous here if there is a growth layer, in particular mainly of native silicon dioxide, between the second contact surface and the reaction layer, as claimed in the present invention. This growth layer undergoes a growth caused by the reaction claimed in the present invention. This growth proceeds from the transition Si-SiO2 (7) by reformation of amorphous SiO2, which leads to a deformation, in particular a bulge, of the growth layer, in particular on its interface with the reaction layer and in particular in the gap region between the first and second contact surfaces. This reduces the distance between the two contact surfaces or reduces the dead space, which results in an increased bonding strength between the two substrates. Temperatures between 200 and 400°C, preferably between about 200°C and 150°C, more preferably between 150°C and 100°C, most preferably between 100°C and room temperature, are particularly advantageous.

[0041] It is particularly advantageous here if the growth layer has an average thickness A between 0.1 nm and 5 nm before forming an irreversible bond. The thinner the growth layer, the faster and easier the reaction between the first and second feedstocks through the growth layer takes place, in particular by diffusion of the first feedstock through the growth layer into the reaction layer.

[0042] According to an embodiment of the invention, the formation of the reservoir is advantageously carried out in vacuum, thus making it possible to avoid contamination of the reservoir with undesired materials or compounds.

[0043] In another embodiment of the invention, the filling of the reservoir comprises: - exposing the first contact surface to the atmosphere to charge the reservoir with atmospheric moisture or oxygen contained in air, or both; - exposing the first contact surface to a fluid which in particular consists mainly, preferably almost entirely, of deionized H2O or H2O2 or both, - exposing the first contact surface to at least one of N2 gas, O2 gas, Ar gas, and forming gas, particularly forming gas consisting of 95% Ar and 5% H2, particularly with an ion energy in the range of 0 to 2000 eV; - vaporizing any of the ingredients named above to fill the reservoir; The method is carried out by one or more steps of:

[0044] It is particularly advantageous for the process sequence if the reservoir is formed with a thickness R of between 0.1 nm and 25 nm, more preferably between 0.1 nm and 15 nm, even more preferably between 0.1 nm and 10 nm, and most preferably between 0.1 nm and 5 nm. Furthermore, according to one embodiment of the invention, it is advantageous if the average distance B between the reservoir and the reaction layer just prior to forming the irreversible bond is between 0.1 nm and 15 nm, in particular between 0.5 nm and 5 nm, and preferably between 0.5 nm and 3 nm.

[0045] The apparatus for carrying out the method claimed in the present invention is formed of a chamber for forming the reservoir, a specially provided separate chamber for filling the reservoir, and a specially provided separate chamber for forming the temporary bond, all of which are directly connected to each other via a vacuum system.

[0046] In another embodiment, the filling of the reservoir can also be done directly with the atmosphere and therefore in a chamber that can be open to the atmosphere, or simply on a structure that does not have an enclosure but can handle wafers semi-automatically and / or fully automatically.

[0047] Other advantages, features and details of the present invention will become apparent from the following description of exemplary preferred embodiments and by use of the drawings. [Brief description of the drawings]

[0048] [Figure 1] FIG. 2 illustrates the first step of the method claimed in the present invention, immediately after contacting a first substrate with a second substrate. [Figure 2a] 4A-4C illustrate other steps of the method claimed in the present invention to create a higher bond strength. [Figure 2b] 4A-4C illustrate other steps of the method claimed in the present invention to create a higher bond strength. [Diagram 3] FIG. 2 shows another step of the method claimed in the present invention, following the steps shown in FIGS. 1, 2a and 2b, in which the contact surfaces of the substrates are brought into contact. [Figure 4] FIG. 1 illustrates the steps claimed in the present invention for forming an irreversible / permanent bond between substrates. [Diagram 5] FIG. 5 is a close-up view of the chemical / physical processes taking place on two contacting surfaces during the steps described in FIGS. 3 and 4. [Figure 6] FIG. 5 is another close-up view of the chemical / physical processes taking place on the interface between two contacting surfaces during the steps described in FIGS. 3 and 4. [Figure 7] 1 is a graph showing the manufacture of a reservoir as claimed in the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0049] In the figures, identical components / features, and components / features having identical functions, are identified with the same reference numbers.

[0050] The situation shown in Figure 1 shows only a part of the chemical reaction taking place between the first contact surface 3 of the first substrate 1 and the second contact surface 4 of the second substrate 2 during or immediately after the temporary bonding step. This surface is terminated with polar OH groups and is therefore hydrophilic. The first substrate 1 and the second substrate 2 are held together by hydrogen bonding attractions between the OH groups present on the surface and H2O molecules, and between H2O molecules alone. The hydrophilicity of at least the first contact surface 3 has been increased by the plasma treatment of the first contact surface 3 in a preceding step.

[0051] Reservoirs 5 in a surface layer 6 of thermal silicon dioxide are formed by plasma treatment as claimed in the present invention. By plasma treatment with O2 ions and ion energies ranging from 0 to 2000 eV, the average thickness R of the reservoirs 5 is about 15 nm, and the ions form channels or pores in the surface layer 6.

[0052] Similarly, reservoir 5 is filled with HO as a first feedstock prior to the step shown in Figure 1 and after plasma treatment. Ionic reducing species present during the plasma process, particularly O, N, H, Ar, can also be located within the reservoir.

[0053] Thus, the contact surfaces 3, 4 still have a relatively large gap, which is occupied in particular by the water present between the contact surfaces 3 and 4. The existing bond strength is therefore relatively small, about 100 mJ / cm 2 to 300 mJ / cm 2 Especially between 200mJ / cm 2 In this respect the prior plasma activation plays a decisive role, in particular because the hydrophilicity of the first contact surface 3 is increased by the plasma activation and because a smoothing effect is obtained by the plasma activation.

[0054] The process shown in Figure 1, called temporary bonding, can proceed preferably at ambient temperature or up to 50°C. Figures 2a and 2b show hydrophilic bonding, where Si-O-Si bridges result from the desorption of water by -OH terminated surfaces. The process of Figures 2a and 2b lasts for about 300 hours at room temperature; at 50°C it lasts for about 60 hours. The state of Figure 2b occurs without the production of a reservoir at the indicated temperatures.

[0055] Between the contact surfaces 3 and 4, HO molecules are formed and, as long as there is still free space, at least a part of them is provided to further fill the reservoir 5. The other HO molecules are removed. In the step described in FIG. 1, about 3 to 5 individual OH groups or HO layers are present, and in the steps described in FIG. 1 to FIG. 2a, 1 to 3 HO monolayers are removed or accommodated in the reservoir 5.

[0056] In the step shown in Fig. 2a, hydrogen bridge bonds are formed directly between the siloxane groups, resulting in a higher bonding force, which causes the contact surfaces 3, 4 to be attracted to each other more strongly and reduces the distance between the contact surfaces 3 and 4. Therefore, there are only 1 to 2 individual OH group layers between the contact surfaces 3 and 4.

[0057] In the step shown in FIG. 2b, a covalent bond in the form of a silanol group is formed between contact surfaces 3 and 4 by the separation of the HO molecules according to the reaction shown in the following chemical formula (2), which results in a much stronger bonding force and requires less space, thus further reducing the distance between contact surfaces 3 and 4, and finally reaching the minimum distance shown in FIG. 3 where contact surfaces 3 and 4 are in contact with each other.

[0058] [ka]

[0059] Up to step 3, since the reservoir 5 has been formed, there is no need to increase the temperature excessively, but rather the process can be carried out at room temperature. In this way, the process steps described in Figures 1 to 3 can be carried out particularly carefully.

[0060] In the method steps shown in Figure 4, the temperature is increased to preferably up to 500°C, more preferably up to 300°C, even more preferably up to 200°C, most preferably up to 100°C, and most preferably not above room temperature in order to form an irreversible or permanent bond between the first and second contact surfaces. These temperatures are relatively low, unlike the prior art, and are only possible if the reservoir 5 contains a first raw material for the reaction shown in Figures 5 and 6, as shown in chemical equation (3) below:

[0061] [ka]

[0062] Due to the above-mentioned slight temperature increase, H2O molecules diffuse as a first source from the reservoir 5 into the reaction layer 7. This diffusion can take place by direct contact of the surface layer 6 formed as an oxide layer with the growth layer, or through or from the gaps 9 present between the oxide layers. Silicon dioxide, i.e. a chemical compound having a molar volume greater than pure silicon, is formed there from the reaction layer 7 as a reaction product 10 of the above-mentioned reaction. This silicon dioxide grows at the interface between the reaction layer 7 and the growth layer 8, thus deforming the layer of the growth layer 8 formed as a native oxide in the direction of the gaps 9. Here again, H2O molecules from the reservoir are required.

[0063] Due to the presence of gaps in the nanometer range, the native oxide layer 8 can bulge, which reduces the stress on the contact surfaces 3, 4. In this way, the distance between the contact surfaces 3 and 4 is reduced, which further increases the effective contact surface and therefore the bond strength. In a welded connection made in this way, unlike the partially unwelded products of the prior art, all pores are closed and a welded connection is formed over the entire wafer, which therefore essentially contributes to an increase in the bond strength. The type of bond between the two amorphous silicon oxide surfaces that are welded together is a mixed form of covalent and ionic bonds.

[0064] The above-mentioned reaction between the first raw material (H2O) and the second raw material (Si) in the reaction layer 7 takes place particularly quickly or at the lowest possible temperature if the average distance B between the first contact surface 3 and the reaction layer 7 is as small as possible.

[0065] Therefore, the pretreatment of the first substrate 1 and the choice of the second substrate 2, consisting of a reaction layer 7 of silicon and a native oxide layer as thin as possible as growth layer 8, are decisive. The native oxide layer as thin as possible, as claimed in the present invention, is provided for two reasons: the growth layer 8 is so thin that the reaction products 10 newly formed on the reaction layer 7 can cause the growth layer 8 to bulge towards the surface layer 6 formed as an oxide layer of the opposing substrate 1, and mainly in the region of the nano-gaps 9. Furthermore, in order to achieve the desired effect as quickly as possible and at the lowest possible temperature, a diffusion path as short as possible is desirable. The first substrate 1 likewise consists of a silicon layer and an oxide layer formed thereon as a surface layer 6, in which the reservoirs 5 are formed at least partially or completely.

[0066] Thus, the reservoir 5 claimed in the present invention is filled with at least the amount of first raw material necessary to close the nanogaps 9, and thus the growth layer 8 can be optimally grown to close the nanogaps 9 in the shortest possible time and / or at the lowest possible temperature.

[0067] An embodiment of the present invention is described below. Aspect 1 A method for bonding a first contact surface (3) of a first substrate (1) to a second contact surface (4) of a second substrate (2), comprising the steps of: forming a reservoir (5) in a surface layer (6) on said first contact surface (3); at least partially filling the reservoir (5) with a first ingredient or a first batch of ingredients; bringing said first contact surface (3) into contact with said second contact surface (4) to form a temporary bonded connection; forming a permanent bond between the first contact surface (3) and the second contact surface (4), at least partially strengthening the permanent bond by reacting the first feedstock with a second feedstock contained in a reaction layer (7) of the second substrate (2); particularly in the above order. Aspect 2 2. The method of claim 1, wherein the permanent bond is formed or strengthened, or both, by diffusion of the first feedstock into the reaction layer (7). Aspect 3 3. The method of claim 1 or 2, wherein the formation of the permanent bond is carried out at a temperature between room temperature and 200° C., in particular for up to 12 days, more preferably for up to 1 day, even more preferably for up to 1 hour, and most preferably for up to 15 minutes. Aspect 4 The irreversible junction is 1.5J / m 2 Larger, especially 2 J / m 2 Greater than 2.5 J / m 2 4. The method of any one of claims 1 to 3, wherein the bonding strength is greater. Aspect 5 5. The method of any one of the preceding aspects, wherein during the reaction, a reaction product (10) is formed in the reaction bed (7) having a molar volume greater than a molar volume of the second feedstock. Aspect 6 6. The method of any one of the preceding aspects, wherein the reservoir (5) is formed by plasma activation. Aspect 7 7. The method according to any of the preceding aspects, wherein the formation of the reservoir (5) is carried out in particular using a compressed tetraethoxysilane oxide layer as the surface layer (6). Aspect 8 8. The method according to any of the preceding aspects 1 to 7, wherein the surface layer (6) consists mainly, in particular essentially completely, of an amorphous material, in particular silicon dioxide produced by thermal oxidation, and the reaction layer (7) consists mainly, in particular essentially completely, of an oxidizable material, in particular Si, Ge, InP, GaP, or GaN. Aspect 9 9. The method according to any of the preceding aspects, wherein between the second contact surface (4) and the reaction layer (7) there is a grown layer (8), in particular of mainly native silicon dioxide. Aspect 10 10. The method of claim 9, wherein prior to forming a permanent bond, the growth layer (8) has an average thickness A between 1 Angstrom and 10 nm. Aspect 11 11. The method of any one of the preceding claims, wherein the reservoir is formed in a vacuum. Aspect 12 The storage section, exposing said first contact surface (3) to an atmosphere, in particular having a high content of oxygen or water or both, - exposing said first contact surface (3) to a fluid, in particular consisting mainly, preferably almost completely, of deionized H2O or H2O2 or both, exposing the first contact surface (3) to at least one of N2 gas, O2 gas, Ar gas, and forming gas, in particular forming gas consisting of 95% Ar and 5% H2, in particular with an ion energy in the range of 0 to 2000 eV; 12. The method of any one of claims 1 to 11, wherein the filling is performed by one or more steps of: Aspect 13 13. The method according to any of the preceding aspects, wherein the reservoir (5) is formed with an average thickness (R) of between 0.1 nm and 25 nm, in particular between 0.1 nm and 20 nm. Aspect 14 14. The method according to any of the preceding aspects, wherein the average distance (B) between the reservoir (5) and the reaction layer (7) immediately prior to forming the permanent bond is between 0.1 nm and 15 nm, in particular between 0.5 nm and 5 nm, preferably between 0.5 nm and 3 nm. Aspect 15 15. The method of any one of the preceding aspects, wherein the irreversible bond has a bond strength that is 2 times, preferably 4 times, more preferably 10 times, and most preferably 25 times the strength of the temporary bond. [Explanation of symbols]

[0068] 1 First Substrate 2 Second Board 3 First Contact Surface 4 Second Contact Surface 5. Storage section 6 Surface layer 7 Reaction Layer 8 growth layer 9 Nano gap 10 Reaction Products 11 First Profile 12 Second Profile 13 Sum of curves A Average thickness B Average distance R Average thickness

Claims

1. 1. A method of bonding a first contact surface of a first substrate to a second contact surface of a second substrate, comprising the steps of: forming reservoirs in a surface layer on the first contact surface, the reservoirs being formed with an average thickness (R) between 0.1 nm and 25 nm; at least partially filling the reservoir with a first ingredient or a first batch of ingredients; contacting the first contact surface with the second contact surface to form a temporary bonded connection; forming a permanent bond between the first contact surface and the second contact surface, the permanent bond being at least partially strengthened by reacting the first feedstock with a second feedstock contained in a reaction layer of the second substrate; wherein forming the permanent bond is performed at a temperature between room temperature and 200° C. for up to 1 hour.

2. The method of claim 1 , wherein the permanent bond is formed or strengthened, or both, by diffusing the first feedstock into the reaction layer.

3. The permanent bond is 1.5 J / m 2 The method of claim 1 or 2, having a greater bond strength.

4. 4. The method of claim 1, wherein during the reaction, a reaction product is formed in the reaction bed having a molar volume greater than a molar volume of the second feedstock.

5. 5. A method according to any one of claims 1 to 4, wherein the reservoir is formed by plasma activation, and reduced species of ions present during the plasma process are located within the reservoir.

6. The method according to claim 5, wherein the reducing species is O 2 ions, N 2 ions, H 2 ions, or Ar ions.

7. 7. The method of claim 1, wherein the surface layer is made of an amorphous material and the reactive layer is made of an oxidizable material.

8. 8. The method of claim 1, wherein there is a grown layer of native silicon dioxide between the second contact surface and the reaction layer.

9. The method of claim 8 , wherein, prior to forming a permanent bond, the grown layer has an average thickness A between 1 Angstrom and 10 nm.

10. The method of claim 1 , wherein the reservoir is formed in a vacuum.

11. 11. The method of claim 1, wherein the reservoirs are formed with an average thickness (R) of between 0.1 nm and 20 nm.

12. 12. The method of claim 1, wherein the average distance (B) between the reservoir and the reaction layer just prior to forming the permanent bond is between 0.1 nm and 15 nm.

13. 13. The method of claim 1, wherein the permanent bond has a bond strength that is twice as strong as the temporary bond.

Citation Information

Patent Citations

  • Semiconductor substrate and method for preparing it

    EP0584778A2

  • Method for joining silicon substrate

    JP1993082404A

  • Manufacturing method of composite substrate

    JP2007201429A

  • Room temperature common combination method

    JP2007515779A

  • A method of bonding two wafers made of a material selected from semiconductor materials

    JP2008535230A