Method for recovering valuable metals from waste secondary batteries

The method addresses inefficiencies in existing metal recovery from waste secondary batteries by using a chlorinating agent to convert lithium into lithium chloride and separate nickel and cobalt from slag, enhancing recovery efficiency and reducing environmental impact.

JP7592194B2Active Publication Date: 2024-11-29KOREA ZINC CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023568505
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-09-05
Filing Date
2023-07-04
Publication Date
2024-11-29
Estimated Expiration
2043-07-04

AI Technical Summary

Technical Problem

Existing methods for recovering valuable metals from waste secondary batteries, such as nickel, cobalt, copper, and lithium, face inefficiencies, particularly in the dry method where lithium recovery requires additional processes and the wet method generates significant wastewater.

Method used

A method involving a pretreatment step followed by a melting process with a chlorinating agent, such as CaCl2, CuCl2, NaCl, or KCl, to convert lithium into lithium chloride (LiCl) and separate nickel, cobalt, and copper from slag, using a three-phase slag composition of CaO-SiO2-Al2O3, with controlled heating and flux addition.

Benefits of technology

Enables efficient recovery of nickel, cobalt, and copper directly from slag and converts lithium into lithium chloride without additional processing, improving recovery rates and reducing environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007592194000005
    Figure 0007592194000005
  • Figure 0007592194000006
    Figure 0007592194000006
  • Figure 0007592194000001
    Figure 0007592194000001
Patent Text Reader

Abstract

A method for recovering valuable metals from used secondary batteries according to an embodiment of the present invention includes a pretreatment process for pretreating used secondary batteries, a melting process for heating the pretreated used secondary batteries to generate a molten liquid, and a recovery process for recovering valuable metals from the molten liquid. A chlorinating agent is added in the melting process, and lithium is recovered in the form of lithium dust in the recovery process.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for recovering valuable metals from waste secondary batteries. [Background technology]

[0002] In recent years, the electric vehicle market has grown rapidly, and the demand for secondary batteries (e.g., lithium secondary batteries) used as power sources for electric vehicles has also increased sharply. Secondary batteries for electric vehicles contain large amounts of valuable metals such as nickel, cobalt, copper, and lithium, and as a result, various research efforts have been conducted recently on methods for recovering and recycling valuable metals from secondary batteries for electric vehicles that have been discarded after use.

[0003] Methods for recovering valuable metals from used secondary batteries of electric vehicles can be divided into a dry method, in which the used secondary batteries of electric vehicles are melted in a furnace and the valuable metals are separated / concentrated from the slag and recovered, and a wet method, in which the valuable metals are leached with acid and refined.

[0004] The dry process is suitable for treating a large amount of used secondary batteries for electric vehicles, and has the advantage that nickel, cobalt, and copper can be quickly separated and recovered from the slag. However, since most of the lithium is discharged as slag, it has the disadvantage that an additional process for leaching lithium from the slag and large-scale additional equipment for this purpose are required to recover it.

[0005] The wet method has the disadvantages of generating a large amount of wastewater due to the use of highly concentrated acid and neutralizing agents, and of being limited in its ability to process a large amount of used secondary batteries for electric vehicles since the treatment is performed without removing aluminum, iron, carbon, etc. Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to provide a method for easily recovering valuable metals such as nickel, cobalt, copper, and lithium from waste secondary batteries. [Means for solving the problem]

[0007] In order to solve the above problems, a method for recovering valuable metals from used secondary batteries according to an embodiment of the present invention includes a pretreatment process for pretreating used secondary batteries, a melting process for heating the pretreated used secondary batteries to generate a molten solution, and a recovery process for recovering valuable metals from the molten solution. A chlorinating agent is added in the melting process, and lithium is recovered in the form of lithium dust in the recovery process.

[0008] According to one embodiment of the present invention, the chlorinating agent includes at least one of CaCl2, CuCl2, NaCl, KCl, and CuCl.

[0009] According to one embodiment of the present invention, the chlorinating agent includes CaCl2 or CuCl2.

[0010] According to an embodiment of the present invention, the chlorinating agent is added so that the equivalent of chlorine to lithium contained in the pretreated waste secondary battery is 1.2 or more.

[0011] According to an embodiment of the present invention, the pretreated waste secondary batteries are heated to a temperature of 1500° C. or more in the melting process.

[0012] According to one embodiment of the present invention, the lithium dust is LiCl.

[0013] According to one embodiment of the present invention, the slag produced in the melting process is a CaO-SiO2-Al2O3 three-phase slag.

[0014] According to one embodiment of the present invention, the composition of the slag is 21-28% CaO, 55-63% SiO2, and 12-17% Al2O3.

[0015] According to one embodiment of the present invention, the method further includes a composition analysis step of analyzing the composition of the pretreated waste secondary battery, and based on the composition analysis result of the pretreated waste secondary battery, the amount of flux added is adjusted so that the composition of the slag is 1-28% CaO, 55-63% SiO, and 12-17% AlO.

[0016] According to one embodiment of the present invention, a slag composition analysis process is performed to analyze the composition of the slag generated during the melting process, and based on the composition analysis result of the slag, the amount of flux added is adjusted so that the composition of the slag becomes 1-28% CaO, 55-63% SiO, and 12-17% AlO.

[0017] According to one embodiment of the present invention, the pre-treatment process includes a discharging process for discharging the used secondary batteries, a dismantling process for dismantling the used secondary batteries from packs into modules, a shredding / crushing process for crushing and pulverizing the dismantled used secondary batteries, and a drying process for drying the shredded / crushed used secondary batteries. Effect of the Invention

[0018] According to the present invention, nickel, cobalt and copper can be reduced in the melting process and separated from the slag for recovery.

[0019] According to the present invention, lithium can be converted into lithium chloride in the melting process by adding a chlorinating agent, and thus lithium can be recovered in the form of lithium dust without an additional process of recovering lithium from the slag. [Brief description of the drawings]

[0020] [Figure 1] FIG. 2 is a process diagram of a method for recovering valuable metals from waste secondary batteries according to an embodiment of the present invention. [Diagram 2] A phase equilibrium diagram of CaO-SiO2-Al2O3 three-phase slag. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] The present invention will now be described with reference to the drawings.

[0022] FIG. 1 is a process diagram showing a method for recovering valuable metals from waste secondary batteries according to one embodiment of the present invention.

[0023] Referring to FIG. 1, a method for recovering valuable metals from waste secondary batteries according to an embodiment of the present invention includes a pretreatment process (S100), a melting process (S200), and a recovery process (S300).

[0024] [Pretreatment process (S100)] The pretreatment step (S100) is a step carried out before melting the waste secondary batteries, and may include a discharging step (S10), a dismantling step (S20), a breaking / crushing step (S30), and a drying step (S40).

[0025] [Discharge process (S10)] The discharging process (S10) is a process of discharging the power stored in the used secondary battery to prevent the used secondary battery from exploding during subsequent processes. The discharging process (S10) may be performed by discharging using a discharger or by discharging using salt water. For example, the charging rate of the used secondary battery may be reduced to 20% or less through the discharging process (S10).

[0026] [Demolition process (S20)] The dismantling process (S20) is a process of dismantling the used secondary batteries in the form of a pack into modules or cells. According to one embodiment, as shown in FIG. 1, the dismantling process (S20) may be performed after the discharging process (S10). However, the present invention is not limited thereto, and according to another embodiment, unlike that shown in FIG. 1, the dismantling process (S20) may be performed first and then the discharging process (S10). The dismantling process (S20) may be performed, for example, using automated dismantling equipment.

[0027] [Break / Crush process (S30)] The crushing / pulverizing process (S30) is a process of crushing and pulverizing the disassembled waste secondary batteries into a crushed form. The crushing / pulverizing process (S30) may be performed by spraying water in a nitrogen atmosphere to prevent sparks and explosions. After the crushing and pulverizing process, the sprayed water and electrolyte flowing out from the waste secondary batteries may be removed. For example, the water and electrolyte may be removed by a centrifugation method through a rotary barrel.

[0028] [Drying process (S40)] The drying step (S40) is a step for removing water and electrolytes remaining after the crushing / grinding step (S30). For example, the drying step (S40) can be performed by adding nitrogen gas heated to about 50° C. or higher to a dryer in which the crushed material is placed.

[0029] [Composition analysis process (S150)] According to one embodiment of the present invention, a composition analysis step (S150) may be performed to analyze the composition of the waste secondary battery (hereinafter, "pretreated waste secondary battery") that has been subjected to the pretreatment step (S100). The composition analysis result of the pretreated waste secondary battery is used to determine the components and content of the flux to be added in the melting step (S200) described below. In contrast, according to another embodiment of the present invention (e.g., when the composition of the pretreated waste secondary battery is already known), the composition analysis step (S150) may be omitted.

[0030] [Melting process (S200)] The melting step (S200) is a step of heating and melting the pretreated waste secondary battery. Specifically, in the melting step (S200), the pretreated waste secondary battery is mixed with a flux and a chlorinating agent and melted. Preferably, this can be performed by heating at 1,500°C or higher for about 3 to 5 hours. During the heating, air, preferably air mixed with oxygen, more preferably oxygen, can be introduced, thereby oxidizing the carbon, aluminum, manganese, iron, and other associated substances contained in the pretreated waste secondary battery. Carbon can be oxidized to carbon dioxide or carbon monoxide and discharged as gas, and oxides of aluminum, manganese, iron, and residual carbon can be contained in slag as described below. If the heating temperature in the melting step (S200) is less than 1,500°C, sufficient reactivity cannot be ensured, and the recovery rate of lithium in the subsequent steps can be reduced.

[0031] The flux contains SiO2 and CaCO3, and thus a three-phase slag of CaO-SiO2-Al2O3 is generated together with the aluminum oxide (Al2O3) contained in the waste secondary batteries. In addition, the slag may contain the auxiliary substances contained in the pretreated waste secondary batteries, such as manganese, iron, carbon, etc., and may also contain some of nickel, cobalt, copper, and lithium.

[0032] The composition of the three-phase slag generated during the melting step (S200) is preferably 1-28% CaO2, 55-63% SiO2, and 12-17% Al2O3, and the amount of flux (components and content of the flux to be added) can be adjusted to achieve this. In this case, the melting point of the slag is about 1,200°C (see FIG. 2). The amount of flux to be added can be determined based on the composition analysis results of the pretreated waste secondary batteries obtained in the composition analysis step (S150). Specifically, the amounts of SiO2 and CaCO3 added can be adjusted based on the composition of the pretreated waste secondary batteries so that the composition of the three-phase slag is 1-28% CaO2, 55-63% SiO2, and 12-17% Al2O3.

[0033] Also, a step of analyzing the composition of the slag generated during the melting step (S200) may be performed. In this case, based on the composition analysis result of the generated slag, the amount of flux input during the melting step (S200) may be adjusted so that the composition of the three-phase slag is preferably 1-28% CaO2, 55-63% SiO2, and 12-17% Al2O3. Specifically, based on the composition of the generated slag, the amounts of SiO2 and CaCO3 additionally input may be adjusted so that the composition of the three-phase slag is 1-28% CaO2, 55-63% SiO2, and 12-17% Al2O3.

[0034] The chlorinating agent may include at least one of CaCl2, CuCl2, NaCl, KCl, and CuCl, and may be added so that the chlorine equivalent to the lithium contained in the pretreated waste secondary battery is preferably 1.2 or more. If the chlorinating agent has an equivalent of less than 1.2, the chlorination reaction of lithium may not be sufficiently carried out, which may result in a low recovery rate of lithium in the subsequent process.

[0035] During the melting process (S200), nickel, cobalt, and copper contained in the pretreated waste secondary batteries are reduced from their oxides. The related reaction formula is as follows (Formula 1).

[0036] MO + C = CO + M (M=Ni,Co,Cu) …(Formula 1)

[0037] The reduced nickel, cobalt, and copper are melted and exist in the form of a molten liquid, and are separated and exist below the slag due to the difference in specific gravity between them and the slag.

[0038] The lithium contained in the waste secondary batteries pretreated in the melting process (S200) is chlorinated by the chlorinating agent to form lithium chloride (LiCl), as shown in the following reaction formulas (2), (3), and (4).

[0039] Li2O + SiO2+ MCl2= 2LiCl + MSiO3(M=Ca,Cu) …(Formula 2)

[0040] Li2O + 2SiO2+ Al2O3+ MCl2= 2LiCl + MAl2Si2O8(M=Ca,Cu) …(Formula 3)

[0041] Li2O + 6SiO2+ Al2O3+ 2MCl = 2LiCl + 2MAlSi3O8(M=Na,K,Cu) …(Formula 4)

[0042] Specifically, when CaCl2 or CuCl2 is used as a chlorinating agent, lithium chloride can be produced through the reaction formulas (2) and (3), and when NaCl, KCl, or CuCl is used, lithium chloride can be produced through the reaction formula (4).

[0043] [Recovery process (S300)] The recovery step (S300) is a step of recovering nickel, cobalt, copper, and lithium chloride (LiCl).

[0044] The molten nickel, cobalt, and copper produced by reduction in the melting step (S200) has a higher specific gravity than the slag, and therefore exists separately below the slag. This allows the nickel, cobalt, and copper to be separated and recovered from the slag.

[0045] The boiling point of the lithium chloride (LiCl) produced in the melting step (S200) is about 1,382° C., and therefore, it may be vaporized during the melting step (S200) and become a dust form. The dust form of lithium chloride (LiCl) may be collected through a dust collector, for example, an electrostatic precipitator or a back filter dust collector.

[0046] Hereinafter, the present invention will be described in detail through examples and comparative examples. In the examples, valuable metals nickel, cobalt, copper, and lithium were recovered from waste secondary batteries through the above-mentioned process, and the recovery rates were measured. Meanwhile, in the comparative example, the melting process (S200) was performed without adding a chlorinating agent, and then the recovery rates of valuable metals nickel, cobalt, copper, and lithium were measured. The recovery rates of nickel, cobalt, copper, and lithium were calculated by subtracting the amount discharged as slag from the amount added. The components of the crushed waste secondary batteries (pretreated waste secondary batteries) used in the examples and comparative examples are as shown in Table 1 below.

[0047] [Table 1]

[0048] [Comparative Example] In a comparative example, without adding a chlorinating agent, 100 g of crushed waste secondary batteries was mixed with 82.2 g of SiO2 and 57.0 g of CaCO3 as fluxes, and the mixture was melted at 1,500°C for 3 hours while adding oxygen.

[0049] [Examples 1 to 5] In Examples 1 to 5, the recovery rate of valuable metals depending on the temperature in the melting step (S200) was confirmed.

[0050] Specifically, 100 g of crushed waste secondary batteries were mixed with 82.2 g of SiO2 and 21.3 g of CaCO3 as fluxes, and 39.6 g of CaCl2 (equivalent of chlorine to lithium: 1.5) as a chlorinating agent, and then oxygen was added for 3 hours to carry out a melting process. The melting temperatures were 1300°C in Example 1, 1350°C in Example 2, 1400°C in Example 3, 1450°C in Example 4, and 1500°C in Example 5.

[0051] The experimental conditions and recovery rates of valuable metals in Examples 1 to 5 and the Comparative Example are shown in Table 2.

[0052] [Table 2]

[0053] As can be seen from Table 2, in Examples 1 to 5, lithium could be recovered without any additional process for the slag. Also, in Examples 1 to 5, the higher the temperature in the melting process, the higher the recovery rate of valuable metals, especially the recovery rate of lithium, and Example 5, in which the temperature in the melting process was 1,500°C, showed a high lithium recovery rate of 91.5%.

[0054] On the other hand, in the comparative example in which the chlorinating agent was not added during the melting process, most of the lithium was discharged into the slag, and therefore lithium could not be recovered without an additional process for the slag.

[0055] [Examples 6 to 10] In Examples 6 to 10, the recovery rate of valuable metals based on the equivalent amount of the chlorinating agent was confirmed.

[0056] Specifically, 100 g of crushed waste secondary batteries was mixed with SiO2 and CaCO3 as flux, and CaCl2 was mixed as a chlorinating agent, and then the melting process was carried out by feeding oxygen for 3 hours at 1,500°C. The amount of CaCl2 fed was 26.4 g (equivalent of chlorine to lithium: 1.0) in Example 6, 31.7 g (equivalent of chlorine to lithium: 1.2) in Example 7, 39.6 g (equivalent of chlorine to lithium: 1.5) in Example 8, 47.5 g (equivalent of chlorine to lithium: 1.8) in Example 9, and 52.8 g (equivalent of chlorine to lithium: 2.0) in Example 10.

[0057] SiO2 was added in an amount of 82.2 g in all of Examples 6 to 10, and CaCO3 was added in an amount of 33.2 g in Example 6, 28.4 g in Example 7, 21.3 g in Example 8, 14.2 g in Example 9, and 9.4 g in Example 10, in accordance with the amount of CaCl2 (chlorinating agent) added.

[0058] The experimental conditions and recovery rates of valuable metals in each example are shown in Table 3.

[0059] [Table 3]

[0060] As can be seen from Table 3, in Examples 6 to 10, lithium could be recovered without an additional process for the slag. Also, the lithium recovery rate increased as the amount of CaCl2 (chlorinating agent) added increased. In particular, Examples 2 to 5, in which the amount of CaCl2 added was 31.7 g (equivalent of chlorine to lithium: 1.2) or more, showed a high lithium recovery rate of 90% or more.

[0061] [Examples 5, 11 to 14] In Examples 5 and 11 to 14, the recovery rate of valuable metals depending on the type of chlorinating agent was confirmed.

[0062] Specifically, 100 g of crushed waste secondary batteries was mixed with SiO2 and CaCO3 as flux, and a chlorinating agent was added so that the chlorine equivalent to lithium was 1.5, and then a melting process was carried out by introducing oxygen for 3 hours at 1,500°C. In Example 5, 39.6 g of CaCl2 was mixed, in Example 11, 47.9 g of CuCl2, in Example 12, 41.7 g of NaCl, in Example 13, 53.2 g of KCl, and in Example 14, 70.6 g of CuCl were mixed.

[0063] SiO2 was added in an amount of 82.2 g in all of Examples 5 and 11 to 14, and CaCO3 was added in an amount of 21.3 g in Example 5 and 57.0 g in Examples 11 to 14 in accordance with the amount of the chlorinating agent added.

[0064] The experimental conditions and recovery rates of valuable metals in each example are shown in Table 4.

[0065] [Table 4]

[0066] As can be seen in Table 4, lithium was recovered without any additional process for slag in Examples 5, 11 to 14. In addition, the lithium recovery rate differed depending on the type of chlorinating agent, and in particular, Examples 5 and 11, in which CaCl2 and CuCl2 were added, showed high lithium recovery rates.

Claims

1. A pretreatment step of pretreating waste secondary batteries; A melting step of heating the pretreated waste secondary batteries to generate a molten liquid; and A recovery step of recovering valuable metals from the molten liquid, In the melting step, a flux and a chlorinating agent are added, In the recovery step, lithium is recovered in the form of lithium dust, In the melting process, the flux is added so as to produce a three-phase slag of CaO-SiO 2 -Al 2 O 3 containing 21-28% CaO, 55-63% SiO 2 and 12-17% Al 2 O 3 ; A slag composition analysis step is performed to analyze the composition of the slag generated during the melting step; Based on the composition analysis result of the slag, the amount of flux added is adjusted so that the slag contains 21-28% CaO, 55-63% SiO 2 , and 12-17% Al 2 O 3 . A method for recovering valuable metals from discarded secondary batteries.

2. The chlorinating agent is CaCl 2 , CuCl 2 2. The method for recovering valuable metals from waste secondary batteries according to claim 1, wherein the metal comprises at least one of NaCl, KCl, and CuCl.

3. The chlorinating agent is CaCl 2 or CuCl 2 The method for recovering valuable metals from waste secondary batteries according to claim 2, comprising:

4. 2. The method for recovering valuable metals from waste secondary batteries according to claim 1, wherein the chlorinating agent is added so that a molar equivalent of chlorine relative to lithium contained in the pretreated waste secondary batteries is 1.2 or more.

5. The method for recovering valuable metals from waste secondary batteries according to claim 1 , wherein the waste secondary batteries pretreated in the melting step are heated at a temperature of 1500° C. or higher.

6. 2. The method for recovering valuable metals from waste secondary batteries according to claim 1, wherein the lithium dust is LiCl.

7. The method further includes a composition analysis step of analyzing the composition of the pretreated waste secondary battery, Based on the composition analysis results of the pretreated waste secondary battery, the slag contains 21 to 28% CaO, SiO 2 55-63%, Al 2 O 3 The method for recovering valuable metals from waste secondary batteries according to claim 1, wherein the amount of flux added is adjusted to contain 12 to 17%.

8. The pretreatment step includes: a discharging step of discharging the used secondary battery; a dismantling step of dismantling the waste secondary batteries from packs into modules; A crushing / pulverizing step of crushing and pulverizing the disassembled waste secondary batteries; and The method for recovering valuable metals from waste secondary batteries according to claim 1 , further comprising a drying step of drying the shattered / pulverized waste secondary batteries.

Citation Information

Patent Citations

  • Method for recycling lithium in waste lithium battery slags through chloridizing roasting and evaporation

    CN107964593A

  • Recycling method and battery processing equipment for processing used batteries, especially rechargeable batteries

    JP2022016471A

  • Process for the recovery of lithium

    JP2022507413A

  • Method of recovering valuable metal including lithium from waste lithium battery

    KR1020210131258A