Positive electrode active material for lithium ion secondary battery and lithium ion secondary battery

The development of a lithium ion secondary battery with a 0.2 μm to 1.0 μm pore diameter positive electrode active material addresses the inadequate contact area issue, improving charge/discharge capacity and efficiency by optimizing electrolyte interaction and structural stability.

JP7592963B2Active Publication Date: 2024-12-03SUMITOMO METAL MINING CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2021546941
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-17
Filing Date
2020-09-16
Publication Date
2024-12-03
Estimated Expiration
2040-09-16

AI Technical Summary

Technical Problem

Existing lithium ion secondary batteries do not achieve sufficient capacity and efficiency due to inadequate contact area between the positive electrode active material and the electrolyte, despite using materials like lithium cobalt composite oxide, necessitating improved porous structures for enhanced performance.

Method used

A positive electrode active material with an average pore diameter of 0.2 μm to 1.0 μm, optimized to allow electrolyte penetration and maintain structural integrity, is developed, featuring a specific surface area distribution that enhances charge/discharge capacity and efficiency.

Benefits of technology

The optimized pore structure improves charge/discharge capacity and efficiency of lithium ion secondary batteries by increasing the effective contact area with the electrolyte, stabilizing pore size, and reducing deformation, thereby enhancing battery characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007592963000004
    Figure 0007592963000004
  • Figure 0007592963000001
    Figure 0007592963000001
  • Figure 0007592963000002
    Figure 0007592963000002
Patent Text Reader

Abstract

A positive electrode active material for lithium ion secondary batteries according to the present invention has an average pore diameter of from 0.2 μm to 1.0 μm as determined within the pore diameter range of from 0.0036 μm to 400 μm.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a positive electrode active material for a lithium ion secondary battery and a lithium ion secondary battery. [Background technology]

[0002] In recent years, with the widespread use of portable electronic devices such as mobile phones and notebook computers, there has been a strong demand for the development of small, lightweight non-aqueous electrolyte secondary batteries with high energy density, as well as secondary batteries with excellent output characteristics and charge / discharge cycle characteristics for use in electric vehicles, including hybrid vehicles.

[0003] Lithium ion secondary batteries are a type of secondary battery that meets these requirements. Lithium ion secondary batteries are composed of a positive electrode, a negative electrode, an electrolyte, and the like, and use materials capable of desorbing and inserting lithium as the positive electrode active material, the negative electrode active material, and the negative electrode active material.

[0004] Currently, research and development of such lithium-ion secondary batteries is being actively conducted. In particular, lithium-ion secondary batteries using layered or spinel-type lithium composite oxides as the positive electrode material can obtain a high voltage of about 4 V, and therefore are being put to practical use as batteries with high energy density.

[0005] Lithium cobalt oxide (LiCoO) is used as a positive electrode material for lithium-ion secondary batteries. 2 ) and lithium nickel composite oxide (LiNiO 2 ), lithium nickel cobalt manganese composite oxide (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 ), and manganese-based lithium manganese oxide (LiMn 2 O 4 ), lithium nickel manganese composite oxide (LiNi 0.5 Mn 0.5 O 2 ), lithium-excess nickel-cobalt-manganese composite oxide (Li 2 MnO3 -LiNi x Mn y Co z O 2 Lithium composite oxides such as

[0006] In the future, especially when used in electric vehicles and the like, there will be a demand for even higher capacity positive electrode materials in order to extend the driving range.

[0007] As a method for increasing the capacity of a positive electrode material, controlling the structure of the positive electrode material has been studied. For example, Patent Document 1 discloses a nonaqueous electrolyte battery that has a positive electrode active material with a pore volume in the range of 0.001 cc / g to 0.01 cc / g and thus achieves both high discharge capacity and excellent cycle characteristics. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Japanese Patent Publication No. 2002-203552 Summary of the Invention [Problem to be solved by the invention]

[0009] During the charge and discharge reaction of a lithium ion secondary battery, lithium ions move between the positive electrode active material and the electrolyte. Therefore, in order to improve the battery characteristics of the lithium ion secondary battery, such as increasing the output power, it is effective to maximize the contact area between the positive electrode active material and the electrolyte and to use porous particles of the positive electrode active material having uniform pores on the surface.

[0010] However, the capacity of the obtained nonaqueous electrolyte battery is not sufficient even if the positive electrode active material of Patent Document 1 is used. In order to further increase the capacity of lithium ion secondary batteries, a positive electrode active material that can further increase the capacity of lithium ion secondary batteries is required.

[0011] In view of the problems associated with the above-described conventional techniques, an object of one aspect of the present invention is to provide a positive electrode active material for a lithium ion secondary battery that can improve the battery characteristics when used in the lithium ion secondary battery. [Means for solving the problem]

[0012] In order to solve the above problems, one embodiment of the positive electrode active material for a lithium ion secondary battery according to the present invention has an average pore diameter of 0.2 μm to 1.0 μm when measured in a pore diameter range of 0.0036 μm to 400 μm. Effect of the Invention

[0013] One embodiment of the positive electrode active material for a lithium ion secondary battery according to the present invention can improve the battery characteristics when used in a lithium ion secondary battery. [Brief description of the drawings]

[0014] [Figure 1] FIG. 2 is an explanatory diagram of a cross-sectional configuration of a coin battery produced in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, the embodiments of the present invention will be described in detail. Note that the embodiments are not limited by the following description, and can be modified as appropriate without departing from the gist of the present invention. Note that in this specification, a tilde "~" indicating a numerical range means that the numerical values ​​before and after it are included as the lower and upper limits, unless otherwise specified.

[0016] [Positive electrode active material for lithium-ion secondary batteries] The positive electrode active material for a lithium ion secondary battery according to this embodiment (hereinafter, also simply referred to as "positive electrode active material") can contain particles of a lithium composite oxide.

[0017] The positive electrode active material according to this embodiment has an average pore diameter of 0.2 μm to 1.0 μm, preferably 0.2 μm to 0.75 μm, more preferably 0.25 μm to 0.65 μm, and even more preferably 0.3 μm to 0.55 μm, when measured within a pore diameter range of 0.0036 μm to 400 μm.

[0018] In this embodiment, the pore size can be a value measured using a fully automatic pore size distribution measuring device (mercury porosimeter (PoreMaster 60-GT, manufactured by Quantachrome)). The average pore size is the average pore diameter of a plurality of pores, and the average value of the diameters of the individual pores can be used.

[0019] In general, when a positive electrode active material is used in a lithium ion secondary battery, the capacity of the positive electrode active material is affected by the contact area between the positive electrode active material and the electrolyte, so the larger the specific surface area of ​​the positive electrode active material, the higher the capacity of the lithium ion secondary battery tends to be. However, even if the specific surface area of ​​the positive electrode active material is large, the capacity of the lithium ion secondary battery may not increase, but may decrease. This is because the specific surface area of ​​the positive electrode active material is measured using a gas adsorption method in which gas is adsorbed into the pores, so that the surface of the pores is also included in the measurement of the specific surface area of ​​the positive electrode active material. However, if the pore diameter of the pores is too small, the electrolyte cannot enter the pores due to its surface tension, and it is considered that it cannot be effectively used to measure the specific surface area of ​​the positive electrode active material.

[0020] Therefore, the positive electrode active material according to the present embodiment has an average pore diameter of 0.2 μm to 1.0 μm when measured in a range of 0.0036 μm to 400 μm. If the average pore diameter is 0.2 μm or more when measured in a range of 0.0036 μm to 400 μm, the electrolyte can easily penetrate into the pores. This can reduce the amount of pores into which the electrolyte cannot penetrate, and can increase the contact area with the electrolyte. Therefore, if the positive electrode active material is used in a lithium ion secondary battery, the charge and discharge capacity of the lithium ion secondary battery can be improved. On the other hand, if the average pore diameter is 1.0 μm or less when measured in a range of 0.0036 μm to 400 μm, the strength of the positive electrode active material can be maintained. Therefore, by preventing deformation of the positive electrode active material, the size of the pores can be reduced from fluctuating, and the size of the pores can be easily maintained stably. Therefore, even when the positive electrode active material is used in a lithium ion secondary battery, it becomes easier to reduce a decrease in the charge / discharge capacity of the lithium ion secondary battery.

[0021] The positive electrode active material according to this embodiment has an average pore diameter of 0.2 μm to 1.0 μm when measured in a range of pore diameters of 0.0036 μm to 400 μm, so that the particles can have a plurality of uniform pores on the surface and inside. Therefore, when the positive electrode active material according to this embodiment is used as a positive electrode of a lithium ion secondary battery, the battery characteristics of the lithium ion secondary battery, such as charge capacity, discharge capacity, and charge / discharge efficiency, can be improved.

[0022] In this embodiment, the ratio S2 / S1 of the cumulative specific surface area S2 measured in the pore diameter range of 0.0036 μm to 0.5 μm to the cumulative specific surface area S1 measured in the pore diameter range of 0.0036 μm to 400 μm is defined as the ratio of micropores, as shown in the following formula (1). At this time, the positive electrode active material according to this embodiment has a ratio of micropores of preferably 70% to 92%, more preferably 80% to 90%, and even more preferably 83% to 88%. By setting the ratio of micropores to 70% to 92%, the positive electrode active material according to this embodiment can adjust the cumulative specific surface area S2 so that it is not too high relative to the cumulative specific surface area S1. This can reduce the number of pores that are not effectively used when measuring the battery characteristics, and therefore the battery characteristics of the lithium ion secondary battery can be further improved by using the positive electrode active material according to this embodiment as the positive electrode of the lithium ion secondary battery. The cumulative specific surface area can be measured, for example, using a flow type gas adsorption method specific surface area measuring device or the like. Percentage of micropores (%) = (cumulative specific surface area S2 measured in the pore diameter range of 0.0036 μm to 0.5 μm) / (cumulative specific surface area S1 measured in the pore diameter range of 0.0036 μm to 400 μm) × 100 (1)

[0023] The lithium composite oxide is not limited in composition, and may be, for example, lithium nickel composite oxide. The lithium nickel composite oxide may contain, for example, lithium (Li), nickel (Ni), cobalt (Co), and element (also called additive element) M (M) in a ratio of substance amount of Li:Ni:Co:M=1+a:1-xy:x:y. However, it is preferable that a, x, and y in the above formula satisfy -0.05≦a≦0.50, 0≦x≦0.35, and 0≦y≦0.35, respectively. The element M may be at least one element selected from Mg, Ca, Al, Si, Fe, Cr, Mn, V, Mo, W, Nb, Ti, Zr, and Ta.

[0024] The lithium nickel composite oxide is, for example, represented by the general formula Li 1+a Ni 1-x-y Co x M y O 2+αIn addition, since a, x, and y in the above general formula have already been described, the description will be omitted here. In addition, α is preferably, for example, 0≦α≦0.10.

[0025] [Method of manufacturing positive electrode active material for lithium ion secondary batteries] A method for producing a positive electrode active material according to the present embodiment will be described. The method for producing a positive electrode active material according to the present embodiment can include a crystallization step, a mixing step, and a firing step. The method for producing a positive electrode active material according to the present embodiment can include an oxidizing roasting step between the crystallization step and the mixing step, if necessary, and the oxide obtained in the oxidizing roasting step can be used in the mixing step.

[0026] (A) Crystallization process Particles of nickel composite hydroxide containing nickel and an additive element M (nickel composite hydroxide particles) are crystallized by a crystallization method (crystallization step).

[0027] The nickel composite hydroxide is, for example, represented by the general formula: Ni 1-x-y Co x M y (OH) 2+β In the above formula, it is preferable that x and y satisfy the above-mentioned ranges. It is preferable that β satisfies, for example, −0.2≦β≦0.2.

[0028] The specific procedure of the crystallization step is not particularly limited, but for example, a mixed aqueous solution containing nickel (Ni) and an additive element M and an alkaline aqueous solution can be mixed to crystallize nickel composite hydroxide particles. Specifically, for example, it is preferable to carry out the following procedure. The mixed aqueous solution can further contain cobalt (Co).

[0029] First, water is put into the reaction tank and controlled to a predetermined atmosphere and temperature. During the crystallization process, the atmosphere in the reaction tank is not particularly limited, but can be, for example, an inert gas atmosphere such as a nitrogen atmosphere. In addition to the inert gas, an oxygen-containing gas such as air can also be supplied to adjust the dissolved oxygen concentration of the solution in the reaction tank. In addition to water, an alkaline aqueous solution or a complexing agent, which will be described later, can also be added to the reaction tank to form an initial aqueous solution.

[0030] Then, in the reaction tank, a mixed aqueous solution containing at least nickel and the additive element M and an alkaline aqueous solution are added to prepare a reaction aqueous solution. Next, the reaction aqueous solution is stirred at a constant speed to control the pH, whereby nickel composite hydroxide particles can be coprecipitated and crystallized in the reaction tank.

[0031] Alternatively, instead of supplying a mixed aqueous solution containing nickel and the additive element M to the reaction tank, a mixed aqueous solution containing some of the metals and an aqueous solution containing the remaining metals may be supplied to the reaction tank. Specifically, for example, a mixed aqueous solution containing nickel and an aqueous solution containing the additive element M may be supplied. Alternatively, aqueous solutions of each metal may be prepared separately, and the aqueous solutions containing each metal may be supplied to the reaction tank.

[0032] A mixed aqueous solution containing nickel and an additive element M can be prepared by adding salts of each metal to water, which is a solvent. The type of salt is not particularly limited, and for example, one or more types of salts selected from sulfates, nitrates, and chlorides can be used as the nickel salt. When cobalt is contained, one or more types of salts selected from sulfates, nitrates, and chlorides can be used as the cobalt salt. The types of salts of each metal may be different, but it is preferable to use the same type of salt from the viewpoint of preventing the inclusion of impurities.

[0033] As the salt containing the additive element M, for example, one or more selected from manganese sulfate, manganese chloride, titanium sulfate, tungsten oxide, molybdenum oxide, molybdenum sulfide, vanadium pentoxide, calcium chloride, aluminum sulfate, sodium aluminate, magnesium sulfate, magnesium chloride, magnesium carbonate, etc. can be used.

[0034] The alkaline aqueous solution can be prepared by adding an alkaline component to water, which is a solvent. The type of alkaline component is not particularly limited, but for example, one or more types selected from sodium hydroxide, potassium hydroxide, sodium carbonate, etc. can be used.

[0035] The composition of the metal elements contained in the mixed aqueous solution is almost the same as the composition of the metal elements contained in the obtained nickel composite hydroxide. Therefore, it is preferable to adjust the composition of the metal elements in the mixed aqueous solution so that it is the same as the composition of the metal elements in the target nickel composite hydroxide.

[0036] In the crystallization step, any component can be added to the reaction aqueous solution in addition to the aqueous solution containing the metal component (mixed aqueous solution) and the aqueous alkali solution.

[0037] For example, a complexing agent may be added to the aqueous reaction solution together with the aqueous alkaline solution.

[0038] The complexing agent is not particularly limited, and may be any agent capable of forming a complex by bonding with nickel ions or other metal ions in an aqueous solution. An example of the complexing agent is an ammonium ion donor. The ammonium ion donor is not particularly limited, and may be one or more selected from ammonia, ammonium sulfate, ammonium chloride, ammonium carbonate, ammonium fluoride, etc.

[0039] The temperature of the reaction aqueous solution in the crystallization step is not particularly limited, but for example, when no complexing agent is used, the temperature of the mixed aqueous solution is preferably in the range of more than 60°C and 80°C or less.

[0040] When a complexing agent is not used in the crystallization process, the solubility of Ni increases by setting the temperature of the reaction aqueous solution to above 60°C, which more reliably prevents the amount of Ni precipitate from deviating from the target composition and preventing coprecipitation.

[0041] In addition, by setting the temperature of the aqueous reaction solution to 80° C. or less in the crystallization step, the amount of water evaporation can be suppressed, and therefore the slurry concentration can be prevented from becoming high. By preventing the slurry concentration from becoming high, it is possible to suppress the precipitation of unintended crystals such as sodium sulfate in the aqueous reaction solution, which would otherwise cause the impurity concentration to become high.

[0042] The pH of the mixed aqueous solution in the crystallization step can be adjusted appropriately depending on the particle size of the nickel composite hydroxide, and for example, when no complexing agent is used, the pH of the reaction aqueous solution is preferably 10 to 12. Note that, unless otherwise specified, the pH of the reaction aqueous solution in this specification means the pH at the temperature of the reaction aqueous solution.

[0043] In the crystallization step, when a complexing agent is not used, the pH of the reaction aqueous solution is set to 12 or less, which can prevent the nickel composite hydroxide particles from becoming fine particles and improve filterability. In addition, spherical particles can be obtained more reliably.

[0044] By setting the pH of the reaction aqueous solution to 10 or more, the production rate of nickel composite hydroxide particles can be increased and, for example, some components such as Ni can be prevented from remaining in the filtrate, etc. Therefore, nickel composite hydroxide particles having the target composition can be obtained more reliably.

[0045] On the other hand, when an ammonium ion donor such as ammonia is used as a complexing agent in the crystallization step, the pH of the reaction solution in the crystallization step is preferably 10 to 13.5 since the solubility of Ni increases. In this case, the temperature of the reaction solution is preferably 30°C to 60°C.

[0046] When an ammonium ion donor is not used as a complexing agent in the reaction aqueous solution, the ammonia concentration in the reaction aqueous solution in the reaction tank is preferably maintained within a constant range of 3 g / L to 25 g / L.

[0047] By setting the ammonia concentration in the reaction aqueous solution to 3 g / L or more, the solubility of metal ions can be kept particularly constant, and therefore primary particles of nickel composite hydroxide with a regular shape and particle size can be formed. As a result, the spread of the particle size distribution of the obtained nickel composite hydroxide particles can be suppressed.

[0048] Furthermore, by setting the ammonia concentration in the reaction aqueous solution to 25 g / L or less, the solubility of metal ions can be prevented from becoming excessively high, and the amount of metal ions remaining in the reaction aqueous solution can be suppressed, so that nickel composite hydroxide particles having the target composition can be obtained more reliably.

[0049] In addition, since fluctuations in ammonia concentration may cause fluctuations in the solubility of metal ions and may result in failure to form uniform hydroxide particles, it is preferable to maintain the ammonia concentration within a certain range. For example, during the crystallization process, it is preferable to maintain the ammonia concentration at a desired concentration with the upper and lower limits within about 5 g / L.

[0050] After the steady state is reached, the precipitate is collected, filtered, and washed with water to obtain nickel composite hydroxide particles. Alternatively, the mixed aqueous solution, the alkaline aqueous solution, and optionally an aqueous solution containing an ammonium ion donor may be continuously supplied to the reaction tank, and the precipitate is allowed to overflow from the reaction tank, collected, filtered, and washed with water to obtain nickel composite hydroxide particles.

[0051] Note that, in order to optimize the crystallization conditions and facilitate control of the composition ratio, the additive element M can also be added by coating the surfaces of the nickel composite hydroxide particles with the additive element M. In this case, the crystallization step can further include a coating step of coating the surfaces of the obtained nickel composite hydroxide particles with the additive element M.

[0052] (Coating process) In the coating step, the method for coating the surface of the nickel composite hydroxide particles with the additive element M is not particularly limited, and various known methods can be used.

[0053] For example, nickel composite hydroxide particles are dispersed in pure water to form a slurry. A solution containing an additive element M in an amount corresponding to the target coating amount is mixed with this slurry, and an acid is dropped to a predetermined pH to adjust the pH value. The acid used in this case is not particularly limited, but it is preferable to use one or more types selected from sulfuric acid, hydrochloric acid, nitric acid, etc.

[0054] After adjusting the pH value of the mixed solution containing the slurry and the additive element M, the slurry and the mixed solution are mixed for a predetermined time. Thereafter, the mixed solution is filtered and dried, whereby a nickel composite hydroxide coated with the additive element M can be obtained.

[0055] The method for coating the surface of the nickel composite hydroxide particles with the additive element M is not limited to the above method. For example, a method of drying a solution containing a compound of the additive element M and a solution containing nickel composite hydroxide particles by spray drying, a method of impregnating nickel composite hydroxide particles with a solution containing a compound of the additive element M, etc. can also be used.

[0056] The nickel composite hydroxide particles to be subjected to the coating step may have a part of the additive element M added in advance, or may not contain the additive element M. When a part of the additive element M is added in advance, an aqueous solution containing the additive element M may be added to the mixed aqueous solution when performing crystallization, as described above. In this way, when the nickel composite hydroxide particles contain a part of the additive element M, it is preferable to adjust the amount of the additive element M added in the coating step so as to obtain a target composition.

[0057] In the crystallization step, a preliminary test may be performed in advance to calculate the relationship between the crystallization conditions such as pH or ammonia concentration of the reaction solution and the pore size of the positive electrode active material according to the present embodiment, which results in a pore size of 0.0036 μm to 400 μm, and the crystallization conditions in the crystallization step for the positive electrode active material according to the present embodiment to have a pore size of 0.0036 μm to 400 μm may be prepared. The crystallization step is preferably performed by selecting the crystallization conditions based on the results of the preliminary test prepared in advance so that the pore size of the positive electrode active material according to the present embodiment is 0.0036 μm to 400 μm.

[0058] (B) Oxidation roasting process The nickel composite hydroxide obtained in the crystallization step is calcined in an oxygen-containing atmosphere (oxidizing roasting) and then cooled to room temperature, thereby obtaining a nickel composite oxide (roasted nickel composite).

[0059] The nickel composite oxide is, for example, represented by the general formula: Ni 1-x-y Co x M y O 1+γ In the above formula, it is preferable that x and y satisfy the above-mentioned ranges. It is preferable that γ satisfies, for example, −0.2≦γ≦0.2.

[0060] In the oxidizing roasting step, the nickel composite hydroxide is calcined to reduce the moisture content, and at least a part of it can be converted into the nickel composite oxide as described above. However, in the oxidizing roasting step, it is not necessary to completely convert the nickel composite hydroxide into the nickel composite oxide, and the nickel composite oxide referred to here may contain, for example, a nickel composite hydroxide or an intermediate thereof.

[0061] The roasting conditions in the oxidation roasting step are not particularly limited, but it is preferable to roast in an oxygen-containing atmosphere, for example, in an air atmosphere, at a temperature of 350° C. to 1000° C. for 5 hours to 24 hours.

[0062] This is because the specific surface area of ​​the resulting nickel composite oxide can be prevented from becoming excessively large by setting the firing temperature to 350° C. or higher, and the specific surface area of ​​the nickel composite oxide can be prevented from becoming excessively small by setting the firing temperature to 1000° C. or lower.

[0063] By setting the calcination time to 5 hours or more, the temperature in the calcination vessel can be made particularly uniform, and the reaction can proceed uniformly. Furthermore, even if the calcination is performed for a time longer than 24 hours, no significant change is observed in the obtained nickel composite oxide, so from the viewpoint of energy efficiency, the calcination time is preferably set to 24 hours or less.

[0064] The oxygen concentration in the oxygen-containing atmosphere during the heat treatment is not particularly limited, but for example, the oxygen concentration is preferably 20% by volume or more. Since the oxygen atmosphere can be used, the upper limit of the oxygen concentration of the oxygen-containing atmosphere can be 100% by volume.

[0065] (C) Mixing process In the mixing step, a nickel composite compound and a lithium compound are mixed to obtain a raw material mixture (also called a lithium composite oxide precursor).

[0066] The nickel composite compound may be a nickel composite hydroxide obtained in the crystallization step, a nickel composite roasted product obtained in the oxidation roasting step, or a mixture of these. The nickel composite compound preferably has a composition corresponding to the target lithium composite oxide.

[0067] For example, when obtaining a lithium composite oxide having the above-mentioned composition ratio, the nickel composite compound can contain nickel (Ni), cobalt (Co), and element M (M) in a ratio of Ni:Co:M=1-xy:x:y in terms of the amount of substance. However, it is preferable that x and y in the above formula satisfy the above-mentioned range. Also, the element M can be the same as the above-mentioned element.

[0068] The mixing ratio of the lithium compound and the nickel composite compound is not particularly limited. However, the ratio (Li / Me) of the number of lithium atoms (Li) and the number of metal atoms other than lithium (Me) in the lithium composite oxide precursor hardly changes before and after the lithium composite oxide precursor is calcined. Therefore, the Li / Me in the lithium composite oxide precursor is almost the same as the Li / Me in the lithium composite oxide obtained. Therefore, it is preferable to mix so that the Li / Me in the lithium composite oxide precursor is the same as the Li / Me in the lithium composite oxide to be obtained. Note that Li / Me means the ratio of the number of lithium atoms and the number of metal atoms other than lithium contained in the lithium composite oxide precursor.

[0069] For example, it is preferable to mix so that the Li / Me ratio in the lithium composite oxide is 0.95 or more and 1.5 or less, and it is particularly preferable to mix so that the Li / Me ratio in the lithium composite oxide precursor is 1.0 or more and 1.2 or less.

[0070] The lithium compound may be one or more selected from, for example, lithium carbonate, lithium hydroxide, etc. The lithium hydroxide may contain water of hydration, and may be used as it is, but it is preferable to roast it in advance to reduce the amount of water of hydration. It is particularly preferable to use anhydrous lithium hydroxide as the lithium hydroxide.

[0071] It is preferable to adjust the particle size and the like of the nickel composite compound and the lithium compound in advance so that a desired lithium composite oxide can be obtained after the firing step.

[0072] A general mixer can be used to mix the nickel composite compound and the lithium compound, and for example, one or more types selected from a shaker mixer, a Loedige mixer, a Julia mixer, a V blender, etc. The mixing conditions in the mixing step are not particularly limited, but it is preferable to select conditions such that the raw material components are sufficiently mixed to the extent that the shells of the raw material particles, such as the nickel composite oxide, are not destroyed.

[0073] It is preferable that the lithium composite oxide precursor is thoroughly mixed in a mixing step before being subjected to the calcination step. If the mixing is insufficient, the Li / Me ratio may vary between individual particles, which may cause problems such as insufficient battery characteristics.

[0074] The nickel composite compound and the lithium compound are preferably weighed and mixed so that the lithium composite oxide precursor after mixing contains lithium (Li), nickel (Ni), cobalt (Co), and an additive element M (M) in a ratio of substance amounts of Li:Ni:Co:Zr:M=1+a:1-xy:x:y. The preferred ranges of a, x, and y in this formula can be the same as those described above, and therefore will not be described here.

[0075] This is because the content ratio of each metal hardly changes before and after the calcination step, and therefore it is preferable to mix the metals so that the content ratio of each metal in the lithium composite oxide precursor is the same as the intended content ratio of each metal in the positive electrode active material obtained by the method for producing a positive electrode active material according to this embodiment.

[0076] (D) Firing process The lithium composite oxide precursor obtained in the mixing step is calcined in an oxygen-containing atmosphere having an oxygen concentration of 80% by volume to 97% by volume at a temperature of 600° C. to 1050° C. (calcination step), thereby obtaining the positive electrode active material according to the present embodiment, which is a particulate lithium composite oxide.

[0077] The amount of the lithium composite oxide precursor to be filled in the firing vessel is not particularly limited, and is appropriately adjusted depending on the size of the firing vessel, etc.

[0078] When the lithium composite oxide precursor is filled in the firing vessel, the shape of the lithium composite oxide precursor is not particularly limited, and the shape can be selected so that it can be uniformly heated in the firing step.

[0079] The calcination temperature for calcining the lithium composite oxide precursor is not particularly limited, and can be appropriately set depending on the composition of the lithium composite oxide precursor.

[0080] By setting the firing temperature at 600°C or higher, the diffusion of the lithium component into the metal composite compound such as nickel composite oxide can be sufficiently promoted, and the characteristics of the obtained lithium composite oxide can be particularly uniform. As a result, when the obtained lithium composite oxide is used as a positive electrode active material, the battery characteristics can be particularly improved. In addition, since the reaction can be sufficiently promoted, it is possible to suppress the remaining of excess lithium and the remaining of unreacted particles.

[0081] By setting the firing temperature to 1050° C. or less, it is possible to suppress the progression of sintering between particles of the lithium composite oxide produced. In addition, by setting the firing temperature to 1050° C. or less, it is possible to suppress the occurrence of abnormal grain growth and to suppress the coarsening of particles of the lithium composite oxide produced.

[0082] Furthermore, in the process of increasing the temperature to the heat treatment temperature, it is preferable to maintain the temperature at about the melting point of the lithium compound for about 1 to 5 hours, since this allows the reaction to proceed more uniformly.

[0083] During the calcination process, the time during which the material is held at the predetermined temperature, i.e., the above-mentioned calcination temperature, is not particularly limited, but is preferably 2 hours or more, more preferably 3 hours or more. By holding the material at the calcination temperature for 2 hours or more, the production of the lithium composite oxide can be sufficiently promoted and the remaining of unreacted materials can be more reliably prevented.

[0084] The upper limit of the holding time at the firing temperature is not particularly limited, but taking into consideration productivity and the like, it is preferably 24 hours or less.

[0085] The atmosphere during firing is not particularly limited, but is preferably an oxidizing atmosphere. As the oxidizing atmosphere, an oxygen-containing gas atmosphere can be preferably used, and for example, an atmosphere with an oxygen concentration of 18 vol% to 100 vol% is more preferable.

[0086] This is because by setting the oxygen concentration in the atmosphere during firing to 18 vol % or more, the crystallinity of the lithium composite oxide can be particularly improved.

[0087] When the oxygen-containing gas atmosphere is used, the gas constituting the atmosphere can be, for example, air (atmosphere), oxygen, a mixed gas of oxygen and an inert gas, etc. In addition, when the mixed gas of oxygen and an inert gas is used as the gas constituting the oxygen-containing gas atmosphere, for example, as described above, it is preferable that the oxygen concentration in the mixed gas satisfies the above-mentioned range. In particular, the firing step is preferably carried out in an oxygen-containing gas flow, and more preferably in air or oxygen flow. In particular, in consideration of the battery characteristics, it is preferable to carry out in an oxygen flow.

[0088] The furnace used for calcination is not particularly limited, and for example, a furnace capable of calcining a precursor packing for producing a lithium composite oxide in an air or oxygen stream can be suitably used. From the viewpoint of maintaining a uniform atmosphere in the furnace, an electric furnace that does not generate gas is preferable, and either a batch type or a continuous type furnace can be used.

[0089] (Pre-firing process) In this embodiment, the raw material mixture (lithium composite oxide precursor) obtained in the mixing step may be pre-calcined before the calcination step. When the pre-calcination is performed, the pre-calcination temperature is not particularly limited, but may be a temperature lower than the calcination temperature in the calcination step. The pre-calcination temperature is, for example, preferably 250°C to 700°C, more preferably 350°C to 650°C.

[0090] The pre-firing time, that is, the holding time at the pre-firing temperature, is, for example, preferably about 1 hour to 10 hours, and more preferably 3 hours to 6 hours.

[0091] After the pre-firing, the product can be cooled once and then subjected to a firing step, or the product can be heated from the pre-firing temperature to the firing temperature and then subjected to a firing step continuously.

[0092] The atmosphere in which the pre-firing is carried out is not particularly limited, but may be, for example, the same atmosphere as that in the firing step.

[0093] By carrying out the calcination, lithium is sufficiently diffused into the metal composite compound such as nickel composite oxide, and a particularly uniform lithium composite oxide can be obtained.

[0094] [Lithium-ion secondary battery] Next, a lithium ion secondary battery (hereinafter, also referred to as a "secondary battery") using the positive electrode active material according to this embodiment will be described. The secondary battery according to this embodiment has a positive electrode using the above-mentioned positive electrode active material as a positive electrode material.

[0095] The secondary battery according to this embodiment includes, for example, a positive electrode, a negative electrode, a separator, and a non-aqueous electrolyte, and is composed of the same components as a general lithium-ion secondary battery. Note that the embodiment described below is merely an example, and the secondary battery according to this embodiment can be implemented in various forms that have been modified and improved based on the knowledge of those skilled in the art, including the following embodiment. In addition, the secondary battery is not particularly limited in its use. Below, the secondary battery according to this embodiment will be described for each component.

[0096] (positive electrode) The positive electrode of the secondary battery according to this embodiment can contain the above-mentioned positive electrode active material.

[0097] An example of a method for manufacturing a positive electrode will be described below. First, a positive electrode active material (powder), a conductive material, and a binder are mixed to prepare a positive electrode mixture, and activated carbon and a solvent for viscosity adjustment and the like are added as necessary, and the mixture is kneaded to prepare a positive electrode mixture paste.

[0098] The mixing ratio of each material in the positive electrode mixture is a factor that determines the performance of the lithium secondary battery, and can be adjusted depending on the application. The mixing ratio of the materials can be the same as that of the positive electrode of a known lithium secondary battery, and for example, when the total mass of the solid content of the positive electrode mixture excluding the solvent is taken as 100 mass%, the positive electrode active material can be contained in a ratio of 60 mass% to 95 mass%, the conductive material can be contained in a ratio of 1 mass% to 20 mass%, and the binder can be contained in a ratio of 1 mass% to 20 mass%.

[0099] The obtained positive electrode composite paste is applied to the surface of a current collector made of, for example, aluminum foil, and dried to remove the solvent, thereby producing a sheet-like positive electrode. If necessary, pressure may be applied by a roll press or the like to increase the electrode density. The sheet-like positive electrode thus obtained can be cut to an appropriate size according to the desired battery and used for the production of the battery.

[0100] As the conductive material, for example, graphite (natural graphite, artificial graphite, expanded graphite, etc.) and carbon black-based materials such as acetylene black and Ketjen Black (registered trademark) can be used.

[0101] As the binder, a material that serves to bind active material particles together can be used, such as polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), fluororubber, ethylene propylene diene rubber, styrene butadiene, cellulose-based resin, polyacrylic acid, etc.

[0102] If necessary, a solvent for dispersing the positive electrode active material, the conductive material, and the activated carbon and dissolving the binder is added to the positive electrode mixture. Specifically, an organic solvent such as N-methyl-2-pyrrolidone can be used as the solvent. Activated carbon can also be added to the positive electrode mixture to increase the electric double layer capacity.

[0103] The method for producing the positive electrode is not limited to the above-mentioned example, and other methods may be used. For example, the positive electrode may be produced by pressing a positive electrode mixture and then drying it in a vacuum atmosphere.

[0104] (Negative electrode) The negative electrode may be made of metallic lithium, a lithium alloy, etc. Alternatively, the negative electrode may be made by mixing a binder with a negative electrode active material capable of absorbing and desorbing lithium ions, adding an appropriate solvent to make a paste-like negative electrode mixture, applying the paste to the surface of a metal foil current collector such as copper, drying it, and compressing it to increase the electrode density as necessary.

[0105] As the negative electrode active material, for example, natural graphite, artificial graphite, a calcined organic compound such as phenolic resin, or a powder of a carbon material such as coke can be used. In this case, as with the positive electrode, a fluorine-containing resin such as PVDF can be used as the negative electrode binder, and as a solvent for dispersing these active materials and binders, an organic solvent such as N-methyl-2-pyrrolidone can be used.

[0106] (Separator) A separator may be sandwiched between the positive electrode and the negative electrode as necessary. The separator separates the positive electrode and the negative electrode and holds the electrolyte, and any known separator may be used, such as a thin membrane of polyethylene or polypropylene having many minute pores.

[0107] (Non-aqueous electrolyte) As the non-aqueous electrolyte, for example, a non-aqueous electrolyte solution can be used. As the non-aqueous electrolyte solution, for example, a solution in which a lithium salt as a supporting salt is dissolved in an organic solvent can be used. In addition, as the non-aqueous electrolyte solution, a solution in which a lithium salt is dissolved in an ionic liquid can be used. Note that the ionic liquid refers to a salt that is composed of cations and anions other than lithium ions and is liquid even at room temperature.

[0108] The organic solvent may be one selected from the following: cyclic carbonates such as ethylene carbonate, propylene carbonate, butylene carbonate, and trifluoropropylene carbonate; chain carbonates such as diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, and dipropyl carbonate; ether compounds such as tetrahydrofuran, 2-methyltetrahydrofuran, and dimethoxyethane; sulfur compounds such as ethyl methyl sulfone and butane sultone; and phosphorus compounds such as triethyl phosphate and trioctyl phosphate. Two or more of these organic solvents may be used alone or in combination.

[0109] The supporting salt is LiPF 6 , LiBF 4 , LiClO 4 , LiAsF 6 , LiN(CF 3 SO 2 ) 2 and their composite salts. Furthermore, the non-aqueous electrolyte may contain a radical scavenger, a surfactant, a flame retardant, and the like.

[0110] The non-aqueous electrolyte may be a solid electrolyte. The solid electrolyte has a property of being able to withstand high voltage. Examples of the solid electrolyte include inorganic solid electrolytes and organic solid electrolytes.

[0111] Examples of the inorganic solid electrolyte include oxide-based solid electrolytes and sulfide-based solid electrolytes.

[0112] The oxide-based solid electrolyte is not particularly limited, and for example, an oxide-based solid electrolyte containing oxygen (O) and having lithium ion conductivity and electronic insulation can be suitably used. For example, lithium phosphate (Li 3 PO 4 ), Li 3 PO 4 N X , LiBO 2 N X , LiNbO 3 , LiTaO 3 , Li 2 SiO3 , Li 4 SiO 4 -Li 3 PO 4 , Li 4 SiO 4 -Li 3 VO 4 , Li 2 Alumni 2 O 3 -P 2 O 5 , Li 2 O-SiO 2 , Li 2 Alumni 2 O 3 -ZnO, Li 1+X Al X Ti 2-X (PO 4 ) 3 (0≦X≦1), Li 1+X Al X Ge 2-X (PO 4 ) 3 (0≦X≦1), LiTi 2 (PO 4 ) 3 , Li 3X La 2 / 3-X TiO 3 (0≦X≦2 / 3), Li 5 La 3 Ta 2 O 12 , Li 7 La 3 Zr 2 O 12 , Li 6 Bala 2 Ta 2 O 12 , Li 3.6 S 0.6 P 0.4 O 4 One or more selected from the above can be used.

[0113] The sulfide-based solid electrolyte is not particularly limited, and for example, one that contains sulfur (S) and has lithium ion conductivity and electronic insulation properties can be suitably used. 2 SP 2 S5 , Li 2 S-SiS 2 , LiI-Li 2 S-SiS 2 , LiI-Li 2 SP 2 S 5 , LiI-Li 2 S.B. 2 S 3 , Li 3 PO 4 -Li 2 S-Si 2 S., Li 3 PO 4 -Li 2 S-SiS 2 , LiPO 4 -Li 2 S-SiS, LiI-Li 2 SP 2 O 5 , LiI-Li 3 PO 4 -P 2 S 5 One or more selected from the above can be used.

[0114] In addition, inorganic solid electrolytes other than those mentioned above may be used. For example, Li 3 N, LiI, Li 3 N-LiI-LiOH, etc. may also be used.

[0115] The organic solid electrolyte is not particularly limited as long as it is a polymer compound exhibiting ion conductivity, and examples of the organic solid electrolyte that can be used include polyethylene oxide, polypropylene oxide, and copolymers thereof. The organic solid electrolyte may also contain a supporting salt (lithium salt).

[0116] (Shape and structure of secondary battery) As described above, the lithium ion secondary battery according to the present embodiment can be formed into various shapes, such as a cylindrical shape or a laminated shape. Regardless of the shape, when the secondary battery according to the present embodiment uses a non-aqueous electrolyte solution as a non-aqueous electrolyte, the positive electrode and the negative electrode are laminated via a separator to form an electrode body. The obtained electrode body is impregnated with a non-aqueous electrolyte solution, and the positive electrode current collector and the positive electrode terminal connected to the outside and the negative electrode current collector and the negative electrode terminal connected to the outside are connected using a current collecting lead or the like, and the structure can be sealed in a battery case.

[0117] In this embodiment, the secondary battery according to the present embodiment is not limited to a form using a non-aqueous electrolyte solution as a non-aqueous electrolyte, and may be, for example, a secondary battery using a solid non-aqueous electrolyte, i.e., an all-solid-state battery. When making an all-solid-state battery, the configuration other than the positive electrode active material may be appropriately changed as necessary. EXAMPLES

[0118] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to the following examples.

[0119] The positive electrode active materials and secondary batteries used in the examples and comparative examples will be described below with reference to the manufacturing method and evaluation thereof.

[0120] <Example 1> [Preparation of positive electrode active material and secondary battery] (1) Preparation of nickel composite oxide (Crystallization process) First, the crystallization conditions (pH or ammonia concentration of the reaction solution, etc.) in the crystallization step were confirmed by a preliminary test so that the average pore diameter of the positive electrode active material would be 0.2 μm to 1.0 μm when measured in the range of 0.0036 μm to 400 μm. The crystallization conditions were selected so that the average pore diameter would be 0.00726 μm when measured in the range of 0.0036 μm to 400 μm, and nickel composite hydroxide particles with a material ratio of nickel, cobalt, and aluminum of Ni:Co:Al=92:5:3 were crystallized.

[0121] Thereafter, the recovered slurry containing the nickel composite hydroxide particles was filtered, and water-soluble impurities were removed by washing with ion-exchanged water, followed by drying.

[0122] The particle size distribution of the obtained nickel composite hydroxide particles was measured using a laser diffraction scattering type particle size distribution measuring device (Microtrac HRA, manufactured by Nikkiso Co., Ltd.). As a result, the average particle size of the nickel composite hydroxide particles was found to be median diameter D 50 The result was 14.3 μm.

[0123] (Oxidation roasting process) Next, the obtained nickel composite hydroxide particles were oxidized and roasted in an air stream (oxygen concentration: 21% by volume) at 500°C for 5 hours. As a result, nickel-cobalt composite oxide (Ni 0.92 Co 0.05 Al 0.03 O) particles (nickel-cobalt composite oxide particles) were obtained.

[0124] (2) Manufacturing of positive electrode active material (Mixing process) The obtained nickel-cobalt composite oxide particles and lithium hydroxide, a lithium compound, were thoroughly mixed using a shaker mixer (Willi & Bachofen (WAB), model: TURBULA Type T2C) to prepare a raw material mixture (lithium composite oxide precursor). At this time, each raw material was weighed and mixed so that the ratio of the number of atoms of lithium (Li) and metals other than lithium (Me) contained in the obtained lithium composite oxide precursor, Li / Me, was 1.05.

[0125] (Firing process) The lithium composite oxide precursor obtained in the mixing step was calcined at 790°C for 10 hours in an oxygen-containing atmosphere with an oxygen concentration of 90% by volume and the remainder being nitrogen. The calcined product obtained was pulverized using a pin mill at a strength sufficient to maintain the particle shape.

[0126] By the above procedure, porous lithium composite oxide particles (lithium composite oxide powder) were obtained.

[0127] (Washing / drying process) The obtained lithium composite oxide particles were mixed with 150 parts by mass of water to 100 parts by mass, and the water was stirred and then filtered by suction using a Nutsche filter to obtain a precipitate (water washing step). The obtained precipitate was placed in a SUS container, heated to 100°C using a vacuum dryer, heated at 190°C for 12 hours, and then left to dry for another 10 hours to obtain a positive electrode active material (drying step).

[0128] The composition and the heterogeneous phase of the obtained positive electrode active material were confirmed. The positive electrode active material obtained in this experiment was found to have the general formula: Li 0.98 Ni 0.92 Co 0.05 Al 0.03 O 2 It was confirmed that the active material was composed of a lithium composite oxide represented by the formula: 2 / g.

[0129] (3) Preparation of secondary batteries A coin-type battery having the structure shown in Fig. 1 was fabricated by the following procedure. As shown in Fig. 1, the coin-type battery 10 is composed of a case 11 and an electrode 12 housed in this case 11.

[0130] Case 11 has a hollow positive electrode can 111 with one end open, and a negative electrode can 112 placed in the opening of positive electrode can 111, and is configured so that when negative electrode can 112 is placed in the opening of positive electrode can 111, a space for accommodating electrode 12 is formed between negative electrode can 112 and positive electrode can 111.

[0131] Electrode 12 consists of a positive electrode 121, a separator 122, and a negative electrode 123, which are stacked in this order, and are housed in case 11 so that positive electrode 121 contacts the inner surface of positive electrode can 111 and negative electrode 123 contacts the inner surface of negative electrode can 112.

[0132] Case 11 is provided with gasket 113, which restricts relative movement between positive electrode can 111 and negative electrode can 112 and fixes them in place so as to maintain a non-contact state between them, i.e., an electrically insulated state. Gasket 113 also has the function of sealing the gap between positive electrode can 111 and negative electrode can 112 to provide an airtight and liquidtight barrier between the inside of case 11 and the outside.

[0133] This coin-type battery 10 was fabricated as follows: First, 52.5 mg of the obtained positive electrode active material, 15 mg of acetylene black, and 7.5 mg of polytetrafluoroethylene (PTFE) resin were mixed and pelletized to a diameter of 11 mm and a weight of about 75 mg to fabricate a positive electrode 121, which was then dried in a vacuum dryer at 100° C. for 12 hours.

[0134] Using the positive electrode 121, the negative electrode 123, the separator 122 and the electrolyte, a coin-type battery 10 was fabricated in a glove box in an Ar atmosphere with a dew point controlled at -60°C.

[0135] For the negative electrode 123, lithium metal punched into a disk shape with a diameter of 13 mm was used.

[0136] The separator 122 was a porous polyethylene film having a thickness of 25 μm.

[0137] The electrolyte is 1M LiClO 4 The supporting electrolyte was a 1:1 mixture of ethylene carbonate (EC) and diethyl carbonate (DEC) (manufactured by Toyama Pharmaceutical Co., Ltd.).

[0138] [Evaluation of positive electrode active material and secondary battery] (1) Evaluation of positive electrode active material The prepared positive electrode active materials were evaluated as follows.

[0139] (a) Average pore diameter The average pore size (unit: μm) of the positive electrode active material was measured using a mercury porosimeter (fully automatic pore distribution measuring device POREMASTER-60-GT). The average pore diameter was measured as the average pore size. The average pore diameter (unit: μm) of the positive electrode active material in the range of pore diameters from 0.0036 μm to 400 μm and the average pore diameter (unit: μm) in the range of pore diameters from 0.0036 μm to 0.5 μm were measured. Hereinafter, the cumulative specific surface area and cumulative pore volume were also measured within the range of the respective average particle diameters.

[0140] (b) Cumulative specific surface area The cumulative specific surface areas S1 and S2 (unit: m) of the lithium composite oxide particles were measured using a flow-type gas adsorption specific surface area measuring device (Yuasa Ionics Co., Ltd., Multisorb). 2 / g) was measured.

[0141] (c) Cumulative pore volume The cumulative pore volume (unit: cc / g) of the lithium composite oxide particles was measured using a fully automatic pore size distribution measuring device (mercury porosimeter (PoreMaster 60-GT, manufactured by Quantachrome)).

[0142] (d) Percentage of micropores Based on the following formula (1), the ratio S2 / S1 of the cumulative specific surface area S2 to the cumulative specific surface area S1 was calculated as the ratio of micropores. Percentage of micropores (%) = (cumulative specific surface area S2 of pores with diameters in the range of 0.0036 μm to 0.5 μm) / (cumulative specific surface area S1 of pores with diameters in the range of 0.0036 μm to 400 μm) × 100 (1)

[0143] These evaluation results are shown in Tables 1 and 2. Table 1 shows the results of measurements when the pores formed in the positive electrode active material had a pore diameter in the range of 0.0036 μm to 400 μm. Table 2 shows the results of measurements when the pores formed in the positive electrode active material had a pore diameter in the range of 0.0036 μm to 0.5 μm, and the proportion of fine pores.

[0144] (2) Evaluation of battery characteristics The produced coin-type battery shown in FIG. 1 was used to measure and evaluate the battery characteristics, including the charge capacity, initial discharge capacity, and charge / discharge efficiency. (a) Charge capacity, initial discharge capacity and charge / discharge efficiency The coin-type battery was left for about 12 hours after preparation, and after the open circuit voltage (OCV) had stabilized, the current density to the positive electrode was increased to 0.1 mA / cm 2 The capacity when the battery was charged up to a cutoff voltage of 4.3 V was defined as the charge capacity. After charging, the battery was left resting for 1 hour, and the capacity when the battery was discharged to a cutoff voltage of 3.0 V was defined as the initial discharge capacity. The charge / discharge efficiency, which is the ratio of the initial discharge capacity to the charge capacity, was calculated. Table 3 shows the evaluation results of the charge capacity, discharge capacity, and charge / discharge efficiency of the produced coin-type battery.

[0145] <Example 2> The same procedure as in Example 1 was carried out except that the crystallization conditions in the crystallization step were changed based on the preliminary test, and the average pore diameter was changed to 0.306 μm when preparing the positive electrode active material. The average particle diameter of the nickel composite hydroxide particles is the median diameter D 50 The BET specific surface area of ​​the positive electrode active material is 1.0 m 2 / g. The evaluation results of the average pore diameter, cumulative specific surface area, and cumulative pore volume of the positive electrode active material are shown in Tables 1 and 2. The ratio of fine pores is shown in Table 2. The evaluation results of the battery characteristics (charge capacity, initial discharge capacity, and charge / discharge efficiency) of the coin battery are shown in Table 3.

[0146] <Example 3> The same procedure as in Example 1 was repeated except that the crystallization conditions in the crystallization step were changed based on the preliminary test, the molar ratio of nickel, cobalt, and aluminum was changed to 87:5:8, and the average pore diameter was changed to 0.415 μm when the positive electrode active material was produced. 50 The BET specific surface area of ​​the positive electrode active material is 1.1 m 2 / g. The evaluation results of the average pore diameter, cumulative specific surface area, and cumulative pore volume of the positive electrode active material are shown in Tables 1 and 2. The ratio of fine pores is shown in Table 2. The evaluation results of the battery characteristics (charge capacity, initial discharge capacity, and charge / discharge efficiency) of the coin battery are shown in Table 3.

[0147] <Comparative Example 1> The same procedure as in Example 1 was carried out except that the crystallization conditions in the crystallization step were changed based on the preliminary test, and the average pore diameter was changed to 0.198 μm when the positive electrode active material was produced. The average particle diameter of the nickel composite hydroxide particles was the median diameter D 50 The BET specific surface area of ​​the positive electrode active material is about 0.7 m 2 / g. The evaluation results of the average pore diameter, cumulative specific surface area, and cumulative pore volume of the positive electrode active material are shown in Tables 1 and 2. The ratio of fine pores is shown in Table 2. The evaluation results of the battery characteristics (charge capacity, initial discharge capacity, and charge / discharge efficiency) of the coin battery are shown in Table 3.

[0148] <Comparative Example 2> The same procedure as in Example 1 was carried out except that the crystallization conditions in the crystallization step were changed based on the preliminary test, and the average pore diameter was changed to 0.127 μm when the positive electrode active material was produced. The average particle diameter of the nickel composite hydroxide particles was the median diameter D 50 The BET specific surface area of ​​the positive electrode active material is about 0.8 m 2 / g. The evaluation results of the average pore diameter, cumulative specific surface area, and cumulative pore volume of the positive electrode active material are shown in Tables 1 and 2. The ratio of fine pores is shown in Table 2. The evaluation results of the battery characteristics (charge capacity, initial discharge capacity, and charge / discharge efficiency) of the coin battery are shown in Table 3.

[0149] <Comparative Example 3> In Example 3, the crystallization conditions in the crystallization step were changed based on the preliminary test, and the positive electrode active material was produced in the same manner as in Example 3 except that the average pore diameter was changed to 0.168 μm. The average particle diameter of the nickel composite hydroxide particles is the median diameter D 50The BET specific surface area of ​​the positive electrode active material is about 0.8 m 2 / g. The evaluation results of the average pore diameter, cumulative specific surface area, and cumulative pore volume of the positive electrode active material are shown in Tables 1 and 2. The ratio of fine pores is shown in Table 2. The evaluation results of the battery characteristics (charge capacity, initial discharge capacity, and charge / discharge efficiency) of the coin battery are shown in Table 3.

[0150] [Table 1]

[0151] [Table 2]

[0152] [Table 3]

[0153] From Tables 1 and 2, the average pore diameter was 0.306 μm to 0.530 μm when measured in the pore diameter range of 0.0036 μm to 400 μm in the positive electrode active materials of Examples 1 to 3. From Table 3, the charge / discharge efficiency was 89.5% or more in the lithium ion secondary batteries produced using any of the positive electrode active materials.

[0154] On the other hand, from Tables 1 and 2, the average pore diameter was less than 0.2 μm when measured in the pore diameter range of 0.0036 μm to 400 μm in the positive electrode active materials of Comparative Examples 1 to 3. From Table 3, the charge / discharge efficiency of the lithium ion secondary batteries produced using any of the positive electrode active materials was approximately 88.5% or less.

[0155] In addition, from Table 3, when Examples 1 and 2 and Comparative Examples 1 and 2, which have the same composition, are compared, Examples 1 and 2 have larger initial discharge capacity and charge capacity than Comparative Examples 1 and 2. Similarly, when Example 3 and Comparative Example 3, which have the same composition, are compared, Example 3 has larger initial discharge capacity and charge capacity than Comparative Example 3.

[0156] Therefore, it was confirmed that when the positive electrode active material has an average pore diameter of 0.306 μm to 0.530 μm, as measured in the pore diameter range of 0.0036 μm to 400 μm, the charge amount, initial discharge amount, and charge / discharge efficiency of the lithium ion secondary battery can be increased, and the battery characteristics of the lithium ion secondary battery can be improved.

[0157] Furthermore, from Table 2, the cumulative specific surface area ratios S2 / S1 were 91% or less in the positive electrode active materials of Examples 1 to 3. On the other hand, the cumulative specific surface area ratios S2 / S1 were 93% or more in the positive electrode active materials of Comparative Examples 1 to 3. Therefore, it can be said that if the cumulative specific surface area ratios S2 / S1 of the positive electrode active material are 91% or less, the battery characteristics of the lithium ion secondary battery can be improved.

[0158] This application claims priority based on Japanese Patent Application No. 2019-168510, filed with the Japan Patent Office on September 17, 2019, the entire contents of which are incorporated herein by reference. [Explanation of symbols]

[0159] 10 Coin cell battery 11 Cases 12 electrodes 121 Positive electrode 122 Separator 123 Negative electrode

Claims

1. The average pore diameter is 0.2 μm to 1.0 μm when measured in the pore diameter range of 0.0036 μm to 400 μm, When the ratio S2 / S1 of the cumulative specific surface area S2 measured in the range of pore diameters from 0.0036 μm to 0.5 μm to the cumulative specific surface area S1 measured in the range of pore diameters from 0.0036 μm to 400 μm is defined as the ratio of fine pores, The positive electrode active material for a lithium ion secondary battery has a ratio of the micropores of 70% to 92%.

2. A lithium ion secondary battery comprising the positive electrode active material for lithium ion secondary batteries according to claim 1.

Citation Information

Patent Citations

  • Non-aqueous electrolyte battery

    JP2002203552A

  • Manufacturing method of positive electrode active material for lithium battery

    JP2008282803A