Sheet for molding and molding
A sheet for molded bodies with a base material of organic fibers and a thermoplastic resin, combined with a high-elongation surface layer, addresses moldability and biodegradability issues, enabling complex shapes and reduced environmental impact.
Patent Information
- Application Number
- JP2020121439
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-15
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-07-15
AI Technical Summary
Existing paper molded products face challenges in achieving sufficient moldability, particularly when deep drawing is required, and there is a need for improved biodegradability and reduced environmental impact.
A sheet for molded bodies comprising a base material made of reinforcing fibers derived from organic resources and a thermoplastic resin, with a surface layer having an elongation rate of 30% or more in any direction, which can be laminated on one or both sides, enhancing moldability and biodegradability.
The solution provides a sheet with excellent moldability, allowing for complex shapes and deep drawing without tearing, while being highly biodegradable and reducing environmental load.
Smart Images

Figure 0007592996000002 
Figure 0007592996000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a sheet for forming a molded body and a molded body. [Background technology]
[0002] Plastics are useful substances that bring convenience and benefits to our lives, but if they are disposed of improperly, they will remain in the natural environment for a long time. In particular, plastic waste that has flowed into the ocean is a cause for concern as it will have a negative impact on ecosystems, living environments, fisheries, tourism, and other areas due to global environmental pollution.
[0003] For this reason, in recent years, the replacement of plastic products with paper products has been considered. For example, Patent Document 1 discloses a molded paper container that has oil resistance, releasability, heat resistance, moderate gas permeability, and high molding flexibility. It is said that various containers can be manufactured by molding a base paper for molded containers that satisfies the specified physical properties. In addition, Patent Document 2 discloses a packaging tray formed from a laminated product that is extrusion laminated with paper as a base.
[0004] Furthermore, Patent Document 3 discloses a molded article containing fibers derived from organic resources such as pulp fibers and a thermoplastic resin, the molded article having resin regions on both sides. Patent Document 3 studies the provision of a molded article that is highly biodegradable and also has excellent water resistance and design properties. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2007-314246 A [Patent Document 2] Special Publication No. 2002-524359 [Patent Document 3] International Publication No. 2017 / 094851 Summary of the Invention [Problem to be solved by the invention]
[0006] The molded article disclosed in Patent Document 3 is endowed with water resistance and designability that are considered difficult to achieve with paper molded articles, but its moldability is insufficient and there is room for improvement. In particular, the molding substrate is required to exhibit excellent moldability even when deep drawing molding or the like is performed.
[0007] Therefore, in order to solve such problems of the conventional techniques, the present inventors have carried out studies with the aim of providing a sheet for forming a molded body having excellent moldability. [Means for solving the problem]
[0008] As a result of intensive research to solve the above problems, the inventors have found that in a sheet for molding having a substrate containing reinforcing fibers derived from organic resources and a thermoplastic resin, and a surface layer, a sheet for molding having excellent moldability can be obtained by setting the elongation rate of the surface layer to a predetermined value or more. Specifically, the present invention has the following configuration.
[0009] [1] A substrate comprising reinforcing fibers derived from organic resources and a thermoplastic resin; A sheet for forming a molded body having a surface layer laminated on at least one surface of a substrate, A sheet for molding, the surface layer of which has an elongation rate of 30% or more in any one direction. [2] The sheet for forming a molded body according to [1], wherein the surface layers are laminated on both sides of the substrate. [3] The sheet for forming a molded body according to [1] or [2], wherein the surface layer is a nonwoven fabric. [4] The surface layer has a basis weight of 15 to 100 g / m 2 The sheet for forming a molded body according to any one of [1] to [3], [5] The sheet for forming a molded body according to any one of [1] to [4], wherein the surface layer contains at least one kind selected from cellulose fibers and regenerated cellulose fibers. [6] The sheet for forming a molding according to any one of [1] to [5], wherein the surface layer contains rayon fibers. [7] The sheet for molding according to any one of [1] to [6], wherein the content of the reinforcing fibers derived from organic resources is 30 mass % or more based on the total mass of the base material. [8] The sheet for forming a molded body according to any one of [1] to [7], wherein the reinforcing fibers derived from organic resources are cellulose fibers. [9] The sheet for forming a molded body according to any one of [1] to [8], wherein the thermoplastic resin is a biodegradable resin.
[10] Density: 0.10 to 1.30 g / cm 3 The sheet for forming a molded body according to any one of [1] to [9],
[11] A molded product obtained by heating and pressurizing the sheet for molding according to any one of [1] to
[10] . Effect of the Invention
[0010] According to the present invention, a sheet for molding having excellent moldability can be obtained. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a cross-sectional view illustrating the configuration of the sheet for forming a molded body of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention will be described in detail below. The following description of the constituent elements may be based on representative embodiments or specific examples, but the present invention is not limited to such embodiments. In this specification, a numerical range expressed using "~" means a range including the numerical values before and after "~" as the lower and upper limits.
[0013] (Sheet for molding) The present invention relates to a sheet for molding, comprising a substrate containing reinforcing fibers derived from organic resources and a thermoplastic resin, and a surface layer laminated on at least one surface of the substrate, wherein the surface layer has an elongation rate of 30% or more in any one direction.
[0014] Fig. 1 is a cross-sectional view illustrating the configuration of the sheet for forming a molded body of the present invention. As shown in Fig. 1, the sheet for forming a molded body 100 has a substrate 10 and a surface layer 20 on at least one surface of the substrate 10. The surface layer 20 may be provided only on one surface of the substrate 10, but as shown in Fig. 1, it is preferable that the surface layer 20 is laminated on both surfaces of the substrate 10.
[0015] The sheet for molded body of the present invention has a surface layer with an elongation rate of 30% or more in any one direction, and therefore has excellent moldability. For example, when a molded body is molded from the sheet for molded body, the sheet for molded body has good elongation characteristics, and the sheet for molded body easily follows the shape of a mold or the like even when deep drawing or molding into a complex shape. This allows a molded body with good moldability to be obtained. In addition, after molding a molded body from the sheet for molded body of the present invention, it is preferable that there is no see-through or tear on the surface of the molded body. It is preferable that there is no tear on the surface of the molded body, and if there is see-through, the area of the see-through part is preferably 10% or less of the total area of the molded body, more preferably 5% or less, and even more preferably 1% or less.
[0016] In addition, since the sheet for molding of the present invention uses reinforcing fibers derived from organic resources, it is highly biodegradable after landfill and can reduce the load during incineration. Thus, the molded body molded from the sheet for molding of the present invention is a molded body with reduced load on the environment.
[0017] Furthermore, since the sheet for molding of the present invention has a surface layer, it is possible to appropriately impart the design and texture of the molded body. For example, by forming the surface layer from a nonwoven fabric, it is possible to impart a texture that is pleasant to the touch. This makes it possible to manufacture a molded body with a luxurious feel. Such a molded body is also preferably used as a packaging material. For example, by forming the sheet for molding according to the outer shape of cosmetics or food, it is preferably used as an inner box, cushioning material, or partition material. In addition, by using a material that exhibits water resistance and oil resistance for the surface layer, it is also possible to mold a molded body having various functions such as water resistance and oil resistance.
[0018] The total thickness of the sheet for forming a molded body in this embodiment is preferably 0.5 mm or more, more preferably 0.7 mm or more, and even more preferably 0.9 mm or more. The total thickness of the sheet for forming a molded body is preferably 3.0 mm or less, more preferably 2.5 mm or less, and even more preferably 2.0 mm or less. By setting the thickness of the sheet for forming a molded body within the above range, the moldability can be more effectively improved.
[0019] The total basis weight of the sheet for forming a molded body in this embodiment is 50 g / m 2 It is preferable that the thickness is 100 g / m or more. 2 More preferably, it is 150 g / m or more. 2 The total basis weight of the sheet for forming a body is more preferably 4000 g / m or more. 2 It is preferable that the thickness is less than 3000 g / m 2 By setting the basis weight of the sheet for forming a molded body within the above range, moldability can be more effectively improved.
[0020] The overall density of the sheet for forming a molded body in this embodiment is 0.05 g / cm 3 It is preferable that the concentration is 0.10 g / cm or more. 3 More preferably, it is 0.15 g / cm or more. 3 More preferably, it is 0.25 g / cm or more. 3It is particularly preferable that the overall density of the sheet for forming a body is 1.30 g / cm or more. 3 It is preferable that the concentration is 1.00 g / cm or less. 3 More preferably, it is 0.80 g / cm or less. 3 By setting the density of the sheet for forming a molded body within the above range, moldability can be more effectively improved.
[0021] In this embodiment, the resin ratio of the sheet for forming a molded body is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 20% by mass or more, based on the total mass of the sheet for forming a molded body. The resin ratio of the sheet for forming a molded body is preferably 70% by mass or less, more preferably 60% by mass or less, and even more preferably 50% by mass or less. By setting the resin ratio of the sheet for forming a molded body within the above range, a molded body with high rigidity and excellent biodegradability can be formed.
[0022] <Base material> The sheet for forming a molded body includes a substrate containing reinforcing fibers derived from organic resources and a thermoplastic resin.
[0023] The content of the reinforcing fibers derived from organic resources in the substrate is preferably 30% by mass or more, more preferably 40% by mass or more, even more preferably 45% by mass or more, and particularly preferably 50% by mass or more, based on the total mass of the substrate. The content of the reinforcing fibers derived from organic resources is preferably 95% by mass or less, more preferably 90% by mass or less, based on the total mass of the substrate. By setting the content of the reinforcing fibers derived from organic resources within the above range, the biodegradability and incinerability of the resulting molded body can be improved. Furthermore, by setting the content of the reinforcing fibers derived from organic resources within the above range, the strength of the entire molded body can be increased.
[0024] The content of the thermoplastic resin in the substrate is preferably 5% by mass or more, more preferably 10% by mass or more, based on the total mass of the substrate. The content of the thermoplastic resin is preferably 70% by mass or less, more preferably 60% by mass or less, even more preferably 55% by mass or less, and particularly preferably 50% by mass or less, based on the total mass of the substrate. By setting the content of the thermoplastic resin within the above range, the moldability of the sheet for molding can be more effectively improved.
[0025] The thickness of the substrate is preferably 0.5 mm or more, more preferably 0.7 mm or more, and even more preferably 0.9 mm or more. The thickness of the substrate is preferably 3.0 mm or less, more preferably 2.5 mm or less, and even more preferably 2.0 mm or less. By making the thickness of the substrate within the above range, the sheet is sufficiently heated during molding, and the moldability can be more effectively improved.
[0026] The basis weight of the base material is 50 g / m 2 It is preferable that the thickness is 75 g / m or more. 2 More preferably, it is 100 g / m or more. 2 It is more preferable that the basis weight of the substrate is 1000 g / m or more. 2 It is preferable that the thickness is less than 900 g / m 2 More preferably, it is 800 g / m or less. 2 By setting the basis weight of the substrate within the above range, the moldability can be more effectively improved.
[0027] The density of the substrate is 0.05 g / cm 3 It is preferable that the concentration is 0.10 g / cm or more. 3 More preferably, it is 0.15 g / cm or more. 3 It is more preferable that the density of the substrate is 1.30 g / cm or more. 3 It is preferable that the concentration is 1.00 g / cm or less. 3 More preferably, it is 0.80 g / cm or less.3 By setting the density of the base material within the above range, the moldability can be more effectively improved.
[0028] <Reinforced fiber derived from organic resources> The substrate contains reinforcing fibers derived from organic resources. Examples of reinforcing fibers derived from organic resources include pulp fibers, cotton, kenaf, bamboo, hemp, silk, and wool. The substrate may contain components other than the reinforcing fibers derived from organic resources, such as organic resource-derived powders such as wood flour, glass fibers, ceramic fibers, and carbon fibers.
[0029] The reinforcing fiber derived from organic resources is preferably pulp fiber, and particularly preferably cellulose fiber. The pulp constituting the pulp fiber is not particularly limited in its manufacturing method and type. For example, chemical pulp such as kraft pulp (KP) of hardwood or softwood, mechanical pulp such as SGP, RGP, BCTMP and CTMP, waste paper pulp such as deinked pulp, and non-wood pulp such as kenaf, jute, bagasse, bamboo, straw, and hemp can be used. In addition, chlorine-free pulp such as ECF pulp and TCF pulp can be used as the pulp.
[0030] The freeness of the reinforcing fiber derived from organic resources is preferably 800 ml or less, more preferably 700 ml or less, even more preferably 600 ml or less, and particularly preferably 500 ml or less, in terms of the Canadian Standard Freeness as defined in JIS P 8121-2:2 Pulp-Freeness Test Method-Part 2: Canadian Standard Freeness Method. The freeness is preferably 300 ml or more. By setting the freeness of the reinforcing fiber derived from organic resources within the above range, the thermoplastic resin can be well retained during hot molding, and the outflow of the molten resin can be prevented.
[0031] The mass average fiber length of the reinforcing fiber derived from an organic resource is preferably 0.1 mm or more and 15 mm or less, more preferably 0.5 mm or more and 10 mm or less, and even more preferably 1 mm or more and 5 mm or less. By setting the fiber length of the reinforcing fiber derived from an organic resource within the above range, it is possible to suppress the reinforcing fiber derived from an organic resource from falling off from the substrate when forming a molded body, and it is possible to form a molded body with excellent strength. In addition, by setting the fiber length of the reinforcing fiber derived from an organic resource within the above range, it is possible to improve the dispersibility of the reinforcing fiber derived from an organic resource. In this specification, the mass average fiber length is the average value of the fiber lengths measured for 100 fibers.
[0032] <Thermoplastic resin> The melting point of the thermoplastic resin is preferably 200° C. or less. The melting point of the thermoplastic resin is more preferably 195° C. or less, and more preferably 180° C. or less. The melting point of the thermoplastic resin is preferably 80° C. or more, more preferably 90° C. or more, and even more preferably 100° C. or more. By setting the melting point of the thermoplastic resin within the above range, it is possible to suppress deterioration of the reinforcing fibers derived from organic resources used in combination, and to improve the water resistance, designability, and strength of the molded body.
[0033] Examples of thermoplastic resins that can be used in the present invention include polyesters such as polyolefin resins, polystyrene, polyethylene terephthalate (e.g., amorphous PET, low melting point PET), acrylonitrile-styrene copolymers, ABS, polyvinyl chloride, poly(meth)acrylic acid alkyl esters, polyvinylidene fluoride, polyvinyl chloride, nylon 12, polyacetal, polycarbonate, ethylene vinyl alcohol copolymers (EVOH), polylactic acid (PLA), polybutylene succinate (PBS), etc. Among these, the thermoplastic resin is preferably a biodegradable resin, and polylactic acid (PLA), polybutylene succinate (PBS), and polyhydroxybutyric acid (PHBH) are particularly preferably used. By using a biodegradable resin as the thermoplastic resin, the biodegradability of the molded body molded from the sheet for molding can be further increased.
[0034] The thermoplastic resin contained in the substrate is preferably a thermoplastic resin fiber, and particularly preferably a biodegradable resin fiber. The mass average fiber length of the biodegradable resin fiber is preferably 1 mm or more, more preferably 2 mm or more. The mass average fiber length of the biodegradable resin fiber is preferably 10 mm or less, more preferably 7 mm or less. The fiber diameter of the biodegradable resin fiber is preferably 0.1 μm or more and 500 μm or less. By using such biodegradable resin fiber, it is easy to disperse the fibers and form a sheet for molding with high uniformity.
[0035] The substrate included in the sheet for forming a molded body of the present invention is preferably an airlaid layer. That is, the substrate is preferably a layer produced by an airlaid method. Here, in the airlaid method, thermoplastic resin fibers defibrated in the air and reinforcing fibers derived from organic resources are uniformly mixed in an airflow, and the resulting airflow containing the raw material fibers and the like is discharged onto a mesh-like endless belt equipped with a suction box on the lower side to form an airlaid web. By making the substrate an airlaid layer, the moldability of the sheet for forming a molded body can be more effectively improved. In addition to improving the feel and visual effect of the obtained molded body, it is also possible to impart design properties.
[0036] <Other ingredients> The substrate may contain a binder component as another component. When the substrate contains a binder component, the content of the binder component is preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 10% by mass or less, based on the total mass of the substrate. By setting the content of the binder component within the above range, the handleability and the like can be improved when producing a molded product.
[0037] Examples of binder components that can be used include various starches, casein, sodium alginate, hydroxyethyl cellulose, carboxymethyl cellulose, polyester resins such as polyethylene terephthalate and modified polyethylene terephthalate, and binder fibers having a core-sheath structure (core-sheath PET) that combine these, acrylic resin, styrene-(meth)acrylic acid ester copolymer resin, urethane resin, polyvinyl alcohol (PVA) resin, various starches, cellulose derivatives, sodium polyacrylate, polyacrylamide, polyvinylpyrrolidone, acrylamide-acrylic acid ester-methacrylic acid ester copolymer, styrene-maleic anhydride copolymer alkali salt, isobutylene-maleic anhydride copolymer alkali salt, polyvinyl acetate resin, styrene-butadiene copolymer, vinyl chloride-vinyl acetate copolymer, ethylene-vinyl acetate copolymer, styrene-butadiene-(meth)acrylic acid ester copolymer, and the like.
[0038] The substrate may further contain fillers and paper-making chemicals, such as mineral pigments, such as kaolin, calcined kaolin, calcium carbonate, calcium sulfate, barium sulfate, titanium dioxide, talc, zinc oxide, alumina, magnesium carbonate, magnesium oxide, silica, white carbon, bentonite, zeolite, sericite, and smectite, and organic pigments, such as polystyrene resins, urea resins, melamine resins, acrylic resins, and vinylidene chloride resins.
[0039] Examples of papermaking chemicals include paper strength enhancers, retention improvers, drainage improvers, dyes, fluorescent whitening agents, pH adjusters, defoamers, pitch control agents, slime control agents, etc. Examples of paper strength enhancers include polyacrylamide, etc. Furthermore, wet strength enhancers can also be used in combination, such as polyamide resins, melamine-formaldehyde resins, urea-formaldehyde resins, polyamide-polyamine-epichlorohydrin resins, and polyethyleneimine resins.
[0040] <Surface layer> The sheet for forming a molded body includes a surface layer laminated on at least one surface of a substrate. The surface layer may be provided on only one surface of the substrate, but is preferably provided on both surfaces of the substrate.
[0041] In the sheet for forming a molded body, the elongation rate in either direction of the surface layer may be 30% or more, preferably 35% or more, more preferably 40% or more, even more preferably 45% or more, and particularly preferably 50% or more. The elongation rate in either direction of the surface layer is preferably 200% or less. Here, the elongation rate of the surface layer is a value measured according to the JIS P 8113 test method for tensile properties of paper board, except that the width of the test piece is changed to 50 mm. Here, the elongation rate is a value obtained by calculating the tensile breaking elongation (the distance extended from the initial test length to just before the test piece breaks) as a percentage of the initial test length (the length between the gripping lines when the test piece is fixed with two gripping tools) in the JIS P 8113 test method for tensile properties of paper board. Note that the measurement is performed in an environment of 23°C and relative humidity 50%. The elongation rate in either direction is the elongation rate in either the longitudinal direction (length direction) or the lateral direction (width direction) of the surface layer. When measuring the elongation percentage of the surface layer, the elongation percentages of the surface layer in the longitudinal direction (length direction) and transverse direction (width direction) are measured.
[0042] In the sheet for forming a body, the extensibility of the surface layer in both directions is more preferably within the above ranges, i.e., the extensibility of the surface layer in both the longitudinal direction (length direction) and the lateral direction (width direction) is preferably 30% or more, more preferably 35% or more, even more preferably 40% or more, still more preferably 45% or more, and particularly preferably 50% or more.
[0043] In the sheet for molding, the average value of the elongation in both directions of the surface layer is also preferably within the above range. That is, the average value of the elongation in both the longitudinal direction (length direction) and the lateral direction (width direction) of the surface layer is preferably 30% or more, more preferably 35% or more, even more preferably 40% or more, still more preferably 45% or more, and particularly preferably 50% or more.
[0044] In the sheet for forming a molded body, the surface layer is preferably a layer made of a nonwoven fabric or a mesh sheet, more preferably a layer made of a nonwoven fabric. Furthermore, the surface layer preferably contains at least one selected from cellulose fibers and regenerated cellulose fibers, more preferably a layer containing regenerated cellulose fibers. Among them, the surface layer preferably contains rayon fibers, and it is particularly preferable that the surface layer is a layer made of a nonwoven fabric of rayon fibers. By configuring the surface layer as described above, the moldability of the sheet for forming a molded body can be more effectively improved.
[0045] The surface layer may be a resin layer. In this case, examples of the resin constituting the resin layer include polyolefin resins, polystyrene, polyesters such as polyethylene terephthalate (e.g., amorphous PET), acrylonitrile-styrene copolymers, ABS, polyvinyl chloride, poly(meth)acrylic acid alkyl esters, polyvinylidene fluoride, nylon 12, polyacetal, polycarbonate, ethylene-vinyl alcohol copolymers, and polylactic acid.
[0046] The thickness of the surface layer is preferably 0.1 mm or more, more preferably 0.2 mm or more, and even more preferably 0.3 mm or more. The thickness of the surface layer is preferably 2 mm or less, more preferably 1.5 mm or less, and even more preferably 1.0 mm or less. By setting the thickness of the surface layer within the above range, it is possible to suppress the surface layer from breaking, and as a result, a sheet for molding with good moldability can be obtained.
[0047] The surface layer has a basis weight of 10g / m 2 It is preferable that the weight is 15 g / m or more. 2 More preferably, it is 20 g / m or more. 2 It is more preferable that the surface layer has a basis weight of 100 g / m or more. 2 It is preferable that the thickness is less than 90 g / m 2 More preferably, it is 80 g / m or less. 2 By setting the basis weight of the surface layer within the above range, it is possible to suppress tearing of the surface layer, and as a result, it is possible to obtain a sheet for forming a molded body having good moldability.
[0048] The surface layer may be provided with a function by using an agent such as a flame retardant, a deodorant, an antibacterial agent, an aromatic agent, a moisturizing agent, a moisture absorbing agent, a water absorbing agent, an adsorbent, a coloring agent, a hydrophilic agent, a water repellent agent, or a coupling agent, if necessary. As a method for providing a function, for example, one or more of these agents may be mixed in the form of a powder into the surface layer. Alternatively, the above-mentioned agent may be sprayed or impregnated in a liquid state.
[0049] <Other layers> For example, an adhesive layer may be provided between the substrate and the surface layer. The adhesive constituting the adhesive layer is not particularly limited as long as it is a material that follows during molding, but is preferably a hot melt adhesive using a thermoplastic resin. Examples of such thermoplastic resins include olefin-based, polyamide-based, rubber-based, and polyester-based resins such as ethylene-vinyl acetate copolymer and polypropylene. It is preferable that the hot melt adhesive is heated to a temperature above the melting point and applied. A known method can be used for the application method.
[0050] (Method of manufacturing sheet for molding) The manufacturing method of the sheet for molding includes a step of forming a substrate on the surface layer, or a step of laminating a substrate sheet. When the manufacturing method of the sheet for molding includes a step of forming a substrate on the surface layer, the substrate is preferably formed by a dry papermaking method. In the substrate manufactured by the dry papermaking method, each fiber constituting the substrate is three-dimensionally oriented randomly in the longitudinal direction, width direction, and thickness direction. This can more effectively improve the moldability of the sheet for molding.
[0051] In the process of producing the sheet for molding, it is preferable to control the direction in which the elongation rate of the surface layer is large so as to be the direction that follows the uneven shape, etc. For example, when the elongation rate of the surface layer in the lateral direction (width direction) is large in the vertical direction (length direction) and the uneven shape is continuous in the left-right direction, it is preferable to produce the sheet for molding so that the lateral direction (width direction) of the surface layer follows the uneven shape in the left-right direction.
[0052] When forming a substrate on a surface layer using a dry papermaking method, a method of forming a web in a dry manner, such as a carding method or an airlaid method, can be used. The carding method is a method of forming a uniform sheet-like web while mechanically combing a fiber mass. The airlaid method is a method of forming an airlaid web by discharging an airflow containing raw fibers, which are a mixture of thermoplastic resin fibers and pulp fibers defibrated in the air and uniformly mixed in the airflow, onto a mesh-like endless belt equipped with a suction box on the lower side.
[0053] The web formed by the dry method may be subjected to a fiber bonding treatment by a needle punch method, a thermal bond method, etc., as necessary. The needle punch method is a method of forming a sheet by entangling thermoplastic resin fibers or reinforcing fibers with each other by passing needles perpendicularly through the web surface. The thermal bond method is a method of bonding raw material fibers by fusing a heat-fusible adhesive compounded in the web.
[0054] When manufacturing a substrate sheet using a wet papermaking method, thermoplastic resin fibers, reinforcing fibers derived from organic resources, and optionally binder components, fillers, papermaking chemicals, etc. are dispersed in a solvent such as water, and the solvent is then removed to form a web.
[0055] When manufacturing a substrate sheet using a wet papermaking method, an acidic papermaking method, a neutral papermaking method, etc. can be adopted. As a papermaking machine, a Fourdrinier papermaking machine, a twin wire papermaking machine, a cylinder papermaking machine, an inclined wire papermaking machine, a single wire papermaking machine, a Yankee papermaking machine, etc. can be appropriately used. In particular, by using a multi-layer papermaking machine such as a cylinder papermaking machine or a single wire papermaking machine, a substrate sheet with a large basis weight can be obtained. In addition, by using a multi-layer papermaking machine, the formulation of each layer can be changed, and a substrate sheet having different functions depending on the depth method can be obtained.
[0056] After forming the substrate using a wet papermaking method or a dry papermaking method, a calendar treatment may be performed as necessary to improve the smoothness and control the density. In the calendar treatment, the density of the substrate can be controlled as desired by applying pressure with a metal roll or a resin roll. In addition, a highly smooth and high-density substrate can be obtained by setting the roll for the calendar treatment to a desired temperature and heating and pressurizing the substrate.
[0057] When the sheet for forming a molded body has surface layers on both sides of the substrate, it is preferable to provide a step of laminating the other surface layer after forming the substrate. When laminating the surface layer and the substrate, an adhesive may be applied to the surface of the substrate or the surface layer, or the surface layer and the substrate may be bonded via an adhesive layer.
[0058] (Molded body) The present invention also relates to a molded body obtained by molding the above-mentioned sheet for molding. The molded body of the present invention is obtained by molding the above-mentioned sheet for molding, and the molding process is preferably a hot-press molding process. That is, it is preferable that the molded body of the present invention is a press-molded product of the sheet for molding. Through such a molding process, the substrate and the surface layer are more firmly bonded and integrally molded.
[0059] The thickness of the molded body is preferably 0.3 mm or more, more preferably 0.5 mm or more, and even more preferably 0.7 mm or more. The thickness of the molded body is preferably 3.0 mm or less, more preferably 2.5 mm or less, and even more preferably 2.0 mm or less. By making the thickness of the molded body within the above range, the strength of the molded body can be increased, and the shape of the molded body can be easily maintained.
[0060] The density of the compact is 0.10 g / cm 3 It is preferable that the concentration is 0.15 g / cm or more. 3 More preferably, it is 0.20 g / cm or more. 3 It is more preferable that the density of the substrate is 1.30 g / cm or more. 3 It is preferable that the concentration is 1.00 g / cm or less. 3 More preferably, it is 0.80 g / cm or less. 3 By setting the density of the base material within the above range, the moldability can be more effectively improved.
[0061] (Method of Manufacturing Molded Product) The method for producing a molded body preferably includes at least one step selected from a step of press molding, a step of vacuum molding, and a step of pressure molding of a sheet for molding. In addition, these molding steps may be combined, or a plurality of steps may be simultaneously performed as one step.
[0062] The molding step is preferably a press molding step. By performing press molding, the thermoplastic resin contained in the sheet for molding melts, and a molded body having excellent strength can be obtained. In this case, the press molding step is preferably a hot and pressure molding step.
[0063] In the step of hot-press molding, the sheet for molding is preferably heated to 100°C or higher and pressed to 2MPa or higher. The heating temperature in the step of hot-press molding is preferably 100°C or higher, but is preferably adjusted appropriately depending on the type of thermoplastic resin contained in the substrate. Specifically, it is preferable to heat within a range of ±20°C of the melting point of the thermoplastic resin contained in the sheet for molding. When polylactic acid is used as the thermoplastic resin, the heating temperature is preferably 150°C or higher and 180°C or lower, and more preferably 160°C or higher and 180°C or lower. By performing hot-press molding within such a temperature range, it is possible to suppress the thermal decomposition (decomposition of hemicellulose) of the reinforcing fibers derived from organic resources contained in the substrate, and a molded body having superior strength can be obtained.
[0064] The pressure conditions in the hot and press molding step are preferably 2 MPa to 25 MPa. The heating rate until the desired holding temperature is reached is preferably 3°C / min to 30°C / min, the holding time under the desired hot and press conditions is preferably 1 min to 30 min, and thereafter, the cooling rate is preferably 3°C / min to 20°C / min while maintaining the pressure, down to the temperature at which the molded body is removed (200°C or less).
[0065] Among the various existing press molding methods, the autoclave method, which is often used when producing molded body members for large aircraft, and the mold pressing method, which has a relatively simple process, are preferred as the method of hot pressing. From the viewpoint of obtaining a high-quality molded body with few voids, the autoclave method is preferred. On the other hand, from the viewpoint of the energy consumption in the equipment and molding process, the simplification of the molding jigs and auxiliary materials used, and the degree of freedom in molding pressure and temperature, it is preferred to use the mold pressing method, which uses a metal mold for molding, and these can be selected according to the application.
[0066] In the hot and pressurized molding step, hot and pressurized molding may be performed multiple times in order to prevent defects such as breakage due to insufficient elongation of the reinforcing fibers derived from organic resources and the thermoplastic resin. This makes it possible to obtain a molded body with better strength and design.
[0067] The press molding step may be a stamping molding step. The stamping molding method is a method in which a sheet for molding is heated in advance, the thermoplastic resin is melted and softened, and then placed inside a mold, the mold is closed to clamp, and then pressure-cooled. For heating, a heating device such as a far-infrared heater, a heating plate, a high-temperature oven, or a dielectric heater can be used. In addition, when the temperature during molding is relatively low, such as when obtaining a low-density molded body, a hot press method can also be used.
[0068] The molding step may be a vacuum molding step. In vacuum molding, the space between the sheet for molding and the mold is made vacuum, thereby increasing the adhesion between the sheet and the mold and improving moldability. In vacuum molding, only a part of the thermoplastic resin contained in the sheet for molding can be melted by controlling the heating temperature, heating time, and the heated portion, and in such a case, a molded body with excellent breathability can be obtained. The vacuum molding is preferably performed in the mold clamping step of the stamping molding step described above. Specifically, the sheet for molding is heated in advance, the thermoplastic resin is melted and softened, and the sheet is placed inside the mold, and then the mold is closed to perform mold clamping, in which vacuum molding is performed. In vacuum molding, vacuum suction is performed from the mold side. The molding pressure in vacuum molding is usually 1.0 kg / cm. 2 The molding is performed in the range of 0.1 to 60 seconds as described below. By employing a vacuum molding process in the molding process, it becomes easy to perform, for example, deep drawing and molding of complex shapes.
[0069] The molding step may be a pressure molding step. In pressure molding, compressed air is blown onto the sheet for molding to make it adhere to the mold, thereby increasing the adhesion between the sheet and the mold. Pressure molding is preferably performed in the mold clamping step of the stamping molding step described above. Specifically, the sheet for molding is heated in advance, and in a state in which the thermoplastic resin is melted and softened, it is placed in the mold, and then compressed air is blown onto the sheet side to perform molding. Pressure molding is performed at a pressure of 3 kg / cm. 2 More than 8kg / cm 2 This is often done with the following compressed air pressure, and molding is done for about 0.1 to 60 seconds. By adopting the compressed air molding process in the molding process, it becomes easy to perform, for example, deep drawing and molding of complex shapes.
[0070] (Application) The molded article of the present invention is preferably used for electrical / electronic devices, office automation equipment, telephone equipment, civil engineering / construction, automobiles, aircraft parts, structural parts and housings, containers (e.g., food containers, drug packaging containers), packaging containers, packaging materials, furniture, daily necessities (e.g., volatilizers for impregnating and volatilizing aromatics, attractants, bait agents, etc., and container-integrated volatilizers, filters), medical tools (e.g., trays, cisterns), etc. In particular, the molded article of the present invention is preferably used for containers and packaging materials having deep-drawn or complex shapes. EXAMPLES
[0071] The features of the present invention will be described in more detail below with reference to examples and comparative examples. The materials, amounts used, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the specific examples shown below.
[0072] <Example 1> (Preparation of Sheet (A) for Molding) On a moving endless mesh conveyor, a basis weight of 28g / m 2 Rayon spunlace (product name: Shinwa 7128) was paid out. The raw fiber was dropped and piled on top of it with the air flow by an airlaid type web forming machine to obtain a web of 300 g / m 2 The raw fiber used was a mixture of pulp (NBKP) and polylactic acid fiber (product name: PL01, melting point 170°C, fiber thickness 15 μm, fiber length: 5 mm, manufactured by Unitika Ltd.) in a mass ratio of 50:50, which was mixed uniformly in air. Next, a 28 g / m2 basis weight was applied to the formed web. 2 Rayon spunlace (product name: Shinwa 7128) was unwound to obtain a web having rayon spunlace on both sides. The web having rayon spunlace on both sides was passed through a through air dryer at a temperature of 160°C to obtain a web having an overall basis weight of 356 g / m 2 The thickness of the sheet for molding (A1) was 1.0 mm and the density was 0.36 g / cm. 3 It was.
[0073] (molding process) One sheet of the sheet for molding (A1) obtained above was fixed to the frame of the molding device of a molding machine consisting of a heating zone and a molding zone. Next, the temperature setting of the far-infrared heating device in the heating zone was set to 400°C (so that the surface temperature of the sheet was 160°C), and the sheet for molding (A1) was heated for 15 seconds, and then the sheet for molding was sandwiched and held in the molding zone using a dome-shaped uneven mold with a height of 3 cm from the bottom and a diameter of 10 cm, and molding was performed. In this way, a sheet with a thickness of 0.5 mm and a density of 0.71 g / cm 3 A dome-shaped molded body of 100 mm was obtained.
[0074] <Example 2> In the production of the molded body sheet, the basis weight of the spunlace on the front and back sides was 28 g / m 2 From 40 g / m 2 A sheet for molding (A2) and a dome-shaped molded product were obtained in the same manner as in Example 1, except that the thickness and density of the sheet for molding (A2) were 1.0 mm and 0.38 g / cm3, respectively. 3 The obtained dome-shaped molded body had a thickness of 0.5 mm and a density of 0.76 g / cm 3 It was.
[0075] <Example 3> In the production of sheets for molding, the raw fiber is dropped and piled up with an air flow to a thickness of 500 g / m 2 A web of 1.5 mm was formed, and a sheet for forming a molded body (A3) and a dome-shaped molded body were obtained in the same manner as in Example 1, except that the basis weight of the substrate was changed. The sheet for forming a molded body (A3) had a thickness of 1.5 mm and a density of 0.37 g / cm. 3 The obtained dome-shaped molded body had a thickness of 1.0 mm and a density of 0.56 g / cm 3 It was.
[0076] <Example 4> In the preparation of the sheet for molding, except that the blending ratio of the raw fibers was changed to 30:70 (polylactic acid fiber:pulp), the sheet for molding (A4) and the dome-shaped molded body were obtained in the same manner as in Example 3. The thickness of the sheet for molding (A4) was 1.5 mm and the density was 0.37 g / cm.3 The obtained dome-shaped molded body had a thickness of 1.0 mm and a density of 0.56 g / cm 3 It was.
[0077] <Comparative Example 1> In the production of the sheet for molding, the rayon spunlace on the front and back sides was replaced with dry airlaid nonwoven fabric 40 g / m 2 A sheet for forming a compact (A5) and a dome-shaped compact were obtained in the same manner as in Example 1, except that the sheet for forming a compact (A5) was changed to KS-40 (product name: Oji Kinocloth). The thickness of the sheet for forming a compact (A5) was 1.0 mm and the density was 0.38 g / cm. 3 The obtained dome-shaped molded body had a thickness of 0.5 mm and a density of 0.76 g / cm 3 It was.
[0078] <Comparative Example 2> In the production of the sheet for molding, the rayon spunlace on the front and back sides was replaced with spunbond nonwoven fabric 15 g / m 2 A sheet for molding (A6) and a dome-shaped molded product were obtained in the same manner as in Example 1, except that the molding sheet (A6) was changed to Ekure (product name: Toyobo Co., Ltd.). The thickness of the sheet for molding (A6) was 1.0 mm and the density was 0.33 g / cm 3 The obtained dome-shaped molded body had a thickness of 0.5 mm and a density of 0.66 g / cm 3 It was.
[0079] (Measurement of surface layer elongation rate) The elongation was measured according to the JIS P 8113 test method for tensile properties of paper and paperboard. The test piece was 50 mm wide and measured in an environment of 23°C and 50% relative humidity. The elongation was calculated as a percentage of the tensile breaking elongation (the distance extended from the initial test length to just before the test piece breaks) to the initial test length (the length between the gripping lines when the test piece is fixed with two grips) in the JIS P 8113 test method for tensile properties of paper and paperboard.
[0080] (Moldability evaluation) The obtained molded article was visually observed and evaluated according to the following criteria. ◯: The sheet for forming a molded body is sufficiently stretched and molded, and there is almost no transparency (local density reduction in the surface layer or base layer) or tearing. Δ: The molded article was molded, but transparency and tears occurred at a low frequency. ×: The molded article was not molded, or transparency or tears frequently occurred.
[0081] [Table 1]
[0082] The moldability was better in the examples than in the comparative examples. [Explanation of symbols]
[0083] 10 Base material 20 Surface layer 100 Sheet for molding
Claims
1. A substrate comprising reinforcing fibers derived from organic resources and a thermoplastic resin; A sheet for forming a molded body having a surface layer laminated on at least one surface of the substrate, The reinforcing fiber derived from an organic resource is at least one selected from pulp fiber, cotton, kenaf, bamboo, hemp, silk, and wool, The surface layer contains rayon fibers, The sheet for forming a molded body has an elongation rate of 30% or more in any one direction of the surface layer.
2. A sheet for molded bodies as described in claim 1, wherein the thermoplastic resin is a biodegradable resin.
3. A substrate comprising reinforcing fibers derived from organic resources and a thermoplastic resin; A sheet for forming a molded body having a surface layer laminated on at least one surface of the substrate, The reinforcing fiber derived from an organic resource is at least one selected from pulp fiber, cotton, kenaf, bamboo, hemp, silk, and wool, The thermoplastic resin is a biodegradable resin, The sheet for forming a molded body has an elongation rate of 30% or more in any one direction of the surface layer.
4. The sheet for forming a molded body according to any one of claims 1 to 3, wherein the surface layer is laminated on both sides of the base material.
5. The sheet for forming a molded body according to any one of claims 1 to 4, wherein the surface layer is a nonwoven fabric.
6. The surface layer has a basis weight of 15 to 100 g / m 2 The sheet for molding according to any one of claims 1 to 5,
7. The sheet for molding according to any one of claims 1 to 6, wherein the content of the reinforcing fibers derived from organic resources is 30 mass% or more based on the total mass of the base material.
8. The sheet for forming a molded body according to any one of claims 1 to 7, wherein the reinforcing fibers derived from organic resources are cellulose fibers.
9. Density: 0.10 to 1.30 g / cm 3 The sheet for molding according to any one of claims 1 to 8,
10. A molded product obtained by hot pressing the sheet for molding according to any one of claims 1 to 9.
Citation Information
Patent Citations
Molding laminated sheet
JP1988162238A
Packaging tray and its method of manufacture and use
JP2002524359A
Base paper for molded container, and paper-made molded container
JP2007314246A
Laminated nonwoven fabric and method for production of the same
JP2009121014A
Multilayered fiber structure
JP2013241718A