Resin sheets, decorative sheets and decorative panels
The resin sheet with a phosphate ester flame retardant and fumed silica in a transparent resin layer addresses fire resistance and pattern clarity issues, enhancing flame retardancy and transparency while avoiding environmental hazards.
Patent Information
- Application Number
- JP2020158760
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-27
- Filing Date
- 2020-09-23
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-09-23
AI Technical Summary
Conventional resin sheets used as decorative materials face challenges in achieving fire resistance, preventing fire spread, maintaining transparency and pattern clarity, and avoiding environmental hazards from halogen and antimony-based flame retardants, while phosphate ester flame retardants cause discoloration and printing issues.
A resin sheet comprising a transparent resin layer with a phosphate ester flame retardant and fumed silica, combined with polyolefin or polyester resins, enhances flame retardancy, pattern clarity, and suppresses discoloration, using a specific composition and layer structure to improve dispersibility and compatibility.
The resin sheet effectively prevents fire spread, maintains high sharpness and pattern clarity, and avoids environmental issues, ensuring excellent flame retardancy and transparency.
Smart Images

Figure 0007593021000003 
Figure 0007593021000004 
Figure 0007593021000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin sheet, a decorative sheet, and a decorative board. [Background technology]
[0002] 2. Description of the Related Art Conventionally, resin sheets have been used in various articles, and they are required to be flame-resistant in the event of a fire.
[0003] For example, resin sheets are laminated as decorative sheets on the surfaces of various articles to impart design features. The decorative sheets are laminated on substrates and used as decorative panels for the floor surfaces of buildings.
[0004] Since such decorative sheets are laminated on the surface of buildings, they may be required to meet the requirements for obtaining a non-combustible certification, which indicates that they are difficult to burn in the event of a fire. Here, the non-combustible certification requirements are the specified requirements for the total heat generation, maximum heat generation rate, and occurrence of cracks and holes in the heat generation test in accordance with ISO5660-1, as stipulated in Article 2, Paragraph 9 of the Building Standards Act of Japan.
[0005] As a sheet exhibiting the above-mentioned flame retardancy, a flame-retardant nonwoven fabric pressure-sensitive adhesive sheet has been proposed in which a pressure-sensitive adhesive layer is provided on at least one side of a flame-retardant nonwoven fabric containing a flame retardant (see, for example, Patent Document 1).
[0006] However, in the sheet described in Patent Document 1, the non-halogen flame retardant is imparted flame retardancy to the nonwoven fabric by binding it to the nonwoven fabric using a binder resin, or by dispersing it in the fibers that make up the nonwoven fabric, or by bonding it to the fibers. Since a nonwoven fabric is used, there is a problem that the sheet cannot be used in cases where transparency is required.
[0007] Furthermore, the sheet described in Patent Document 1 does not consider the difficulty of fire spreading in the decorative sheet on the substrate in the event of a fire. In components that are applied to horizontal surfaces, such as decorative floor materials, flame retardancy, which limits the area of the decorative sheet burning in the event of a fire and makes it difficult for the fire to spread, is also an important performance in terms of ensuring evacuation time.
[0008] Flame retardants are useful for imparting flame retardancy to decorative sheets, and examples of such flame retardants include halogen-based flame retardants, antimony-based flame retardants, metal hydroxide-based flame retardants, phosphate-based flame retardants, etc. However, there is a problem that halogen-based flame retardants and antimony-based flame retardants are not preferable from the environmental viewpoint.
[0009] When a metal hydroxide-based flame retardant is used as the flame retardant, it is necessary to add a large amount. Also, a phosphate-based flame retardant forms combustion char during combustion to suppress combustion. When the phosphate-based flame retardant is used, it is necessary to add a large amount in order to form combustion char and obtain a flame retardant effect. Therefore, when these flame retardants are used, the transparency of the layer containing the flame retardant is impaired and coloring may occur, resulting in a problem of reduced sharpness of the pattern of the decorative sheet.
[0010] In addition, since the particle size of the phosphate ester flame retardant is large, when the resin sheet is used as a printing sheet, it becomes a surface foreign matter, which causes a problem of easily causing printing defects. When the phosphate ester flame retardant is added to a transparent resin layer containing an olefin resin, it is poorly compatible with the olefin resin and difficult to disperse uniformly. Therefore, there is a problem that the sharpness of the decorative sheet is reduced and the flame retardancy is also reduced.
[0011] Therefore, there is a demand for the development of resin sheets, decorative sheets and decorative panels which are difficult for fire to spread, have excellent flame retardancy, and have patterns which are clearly visible and which are inhibited from discoloring, resulting in excellent sharpness. [Prior art documents] [Patent documents]
[0012] [Patent Document 1] JP 2002-69403 A Summary of the Invention [Problem to be solved by the invention]
[0013] To provide a resin sheet, a decorative sheet and a decorative board which are difficult for fire to spread, have excellent flame retardancy, and have excellent sharpness, in which patterns are clearly visible and discoloration is suppressed. [Means for solving the problem]
[0014] As a result of extensive research, the inventors have discovered that the above object can be achieved by configuring a resin sheet having a transparent resin layer so that the transparent resin layer contains a phosphate ester-based flame retardant and fumed silica, and also contains at least one resin selected from the group consisting of polyolefin-based resins and polyester-based resins, and have thus completed the present invention.
[0015] That is, the present invention relates to the following resin sheet, decorative sheet, and decorative board. 1. A resin sheet having at least a transparent resin layer, (1) The transparent resin layer contains a phosphate ester-based flame retardant and fumed silica, (2) The transparent resin layer contains at least one resin selected from the group consisting of polyolefin-based resins and polyester-based resins. A resin sheet comprising: 2. The resin sheet according to item 1, wherein the content of the phosphate ester-based flame retardant is 7.0% by mass or more, based on 100% by mass of the transparent resin layer. 3. The resin sheet according to item 1 or 2, wherein the fumed silica is hydrophilic fumed silica. 4. The resin sheet according to any one of items 1 to 3, wherein the content of the fumed silica is 4.0% by mass or more, based on 100% by mass of the transparent resin layer. 5. The resin sheet according to any one of items 1 to 4, comprising the transparent resin layer and a base sheet. 6. The resin sheet according to any one of items 1 to 4, comprising at least a picture pattern layer and the transparent resin layer in this order on a base sheet. 7. The resin sheet according to any one of items 1 to 4, comprising at least a picture pattern layer, the transparent resin layer, and a surface protective layer on a base sheet in this order. 8. The resin sheet according to item 7, wherein the surface protective layer contains an antiviral agent. 9. The resin sheet according to any one of items 5 to 8, wherein the transparent resin layer side has an embossed shape. 10. A decorative sheet which is the resin sheet according to any one of items 1 to 9. 11. A decorative board having the decorative sheet according to item 10 on a substrate. Effect of the Invention
[0016] The resin sheet and decorative sheet of the present invention are flame retardant, flame retardant, and have a clear pattern, are inhibited from discoloring, and exhibit high sharpness. The decorative plate of the present invention has the decorative sheet on a substrate, and therefore has flame retardant and high sharpness. [Brief description of the drawings]
[0017] [Figure 1] FIG. 1 is a schematic diagram showing an example of the layer structure of a decorative sheet of the present invention. [Diagram 2] FIG. 1 is a schematic diagram showing an example of the layer structure of a decorative sheet of the present invention. [Diagram 3] FIG. 1 is a schematic diagram showing an example of the layer structure of a decorative sheet of the present invention. [Figure 4] FIG. 1 is a schematic diagram showing an example of the layer structure of a decorative sheet of the present invention. [Diagram 5] FIG. 2 is a schematic diagram showing an example of a layer structure of a substrate constituting the decorative board of the present invention. [Figure 6] FIG. 2 is a schematic diagram showing an example of a layer structure of the decorative board of the present invention. [Figure 7]FIG. 2 is a schematic diagram showing an example of a layer structure of the decorative board of the present invention. [Figure 8] FIG. 2 is a schematic diagram showing an example of a layer structure of the decorative board of the present invention. [Figure 9] FIG. 2 is a schematic diagram showing an example of a layer structure of the decorative board of the present invention. [Figure 10] FIG. 1 is a schematic diagram showing a test method for fire spread resistance. [Figure 11] FIG. 1 is a schematic diagram showing a test method for fire spread resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The resin sheet, decorative sheet, and decorative board of the present invention will be described in detail below. In addition, the resin sheet and decorative sheet of the present invention have a surface opposite to the side of the resin sheet and decorative sheet laminated with the substrate, which is the so-called "front surface", and is the surface that is visible when applied to a floor or the like. Therefore, in this specification, the direction of the surface opposite to the side of the resin sheet and decorative sheet laminated with the substrate is referred to as "upper", and the opposite side, i.e., the surface direction of the side laminated with the substrate, is referred to as "rear" or "lower". Similarly, in this specification, the direction of the surface of the decorative board facing the resin sheet and decorative sheet is referred to as "upper", and the opposite side, i.e., the surface direction of the substrate side, is referred to as "rear" or "lower".
[0019] 1. Resin sheets and decorative sheets The resin sheet of the present invention is a resin sheet having at least a transparent resin layer, characterized in that (1) the transparent resin layer contains a phosphate ester-based flame retardant and fumed silica, and (2) the transparent resin layer contains at least one resin selected from the group consisting of polyolefin-based resins and polyester-based resins. The resin sheet of the present invention having the above characteristics is characterized in that (1) the transparent resin layer contains a phosphate ester-based flame retardant and fumed silica, and (2) the transparent resin layer contains at least one resin selected from the group consisting of polyolefin-based resins and polyester-based resins, so that even without adding a large amount of flame retardant, the fire is unlikely to spread and flame retardancy can be exhibited, and the pattern shown by the decorative sheet is clearly visible, discoloration is suppressed, and high sharpness can be exhibited. The resin sheet of the present invention is particularly excellent in sharpness and flame retardancy because the transparent resin layer contains both a phosphate ester-based flame retardant and fumed silica. This is believed to be because the polar portion of the phosphate flame retardant is attracted to the polar groups on the surface of the fumed silica, and the presence of the phosphate flame retardant on the surface improves dispersibility.
[0020] The resin sheet of the present invention has at least a transparent resin layer, and the layer structure is not limited as long as it satisfies the above requirements (1) and (2). The resin sheet of the present invention can also be used as a decorative sheet. That is, the decorative sheet is also one aspect of the present invention, and the resin sheet of the present invention is also the decorative sheet of the present invention.
[0021] Examples of the layer structure of the resin sheet and decorative sheet of the present invention include a structure having a transparent resin layer and a base sheet, and a layer structure having at least a picture pattern layer and a transparent resin layer on the base sheet in this order. Also, as shown in FIG. 1, a layer structure having a synthetic resin backer layer 11, a base sheet 12, a picture pattern layer 13 (solid ink layer and / or pattern ink layer), an adhesive layer (not shown), a transparent resin layer 14, a primer layer (not shown), and a surface protective layer 15 in this order (a doubling-type decorative sheet having a synthetic resin backer layer). Also, as shown in FIG. 2, the decorative sheet of the present invention may have a layer structure having a base sheet 12, a picture pattern layer 13 (solid ink layer and / or pattern ink layer), an adhesive layer (not shown), a transparent resin layer 14, and a surface protective layer 15 in this order (a doubling-type decorative sheet). The decorative sheet of the present invention may have a layer structure having, in order, a base sheet 12, a picture pattern layer 13 (solid ink layer and / or pattern ink layer), a primer layer (not shown), and a surface protective layer 15 (single-layer decorative sheet) as shown in Fig. 3. Furthermore, the decorative sheet of the present invention may have a layer structure having, in order, a picture pattern layer 13 (solid ink layer and / or pattern ink layer), an adhesive layer (not shown), a transparent resin layer 14, a primer layer (not shown), and a surface protective layer 15 (back-printed decorative sheet) as shown in Fig. 4. A decorative sheet having such a layer structure will be specifically described below as a representative example.
[0022] (Transparent resin layer) The transparent resin layer contains a phosphate ester-based flame retardant and fumed silica.
[0023] Phosphate ester flame retardants The phosphoric acid ester-based flame retardant is not particularly limited as long as it is a phosphoric acid ester-based compound that has been conventionally used as a flame retardant, and examples thereof include bisphenol A bisphosphate, bisphenol A bis(diphenyl phosphate), resorcinol bisphosphate, resorcinol(diphenyl phosphate), resorcinol bis(diphenyl phosphate), resorcinol bis[di(2,6-dimethylphenyl)phosphate], resorcinol bis(dixylenyl phosphate), 2,2-bis{4-[bis(phenoxy)phosphoryloxy]phenyl}propane, 2,2-bis{4-[bis(methylphenoxy)phosphoryloxy]phenyl}propane, hydroquinone bisphosphate, etc. Among these, resorcinol bis(dixylenyl phosphate) is preferred in that it further improves the flame retardancy of the resin sheet and decorative sheet.
[0024] As the phosphate ester-based flame retardant, commercially available products can be used. Examples of such commercially available products include CR741, CR733S, PX200, and PX202 manufactured by Daihachi Chemical Industry Co., Ltd.; FP600, FP700, and FP800 manufactured by ADEKA Corporation.
[0025] The above phosphate ester-based flame retardants may be used alone or in combination of two or more.
[0026] The content of the phosphate ester-based flame retardant is preferably 7.0% by mass or more, more preferably 7.7% by mass or more, and even more preferably 8% by mass or more, based on 100% by mass of the transparent resin layer. By setting the lower limit of the content of the phosphate ester-based flame retardant within the above range, the flame retardancy of the resin sheet and the decorative sheet is further improved. In addition, the content of the phosphate ester-based flame retardant is preferably 20% by mass or less, more preferably 15% by mass or less, and preferably 10% by mass or less, based on 100% by mass of the total mass of the transparent resin layer. By setting the upper limit of the content of the phosphate ester-based flame retardant within the above range, the sharpness of the resin sheet and the decorative sheet is further improved.
[0027] The content of the phosphate ester-based flame retardant is preferably 3 parts by mass or more, more preferably 5 parts by mass or more, and even more preferably 7 parts by mass or more, based on 100 parts by mass of the resin in the transparent resin layer. By setting the lower limit of the content of the phosphate ester-based flame retardant within the above range, the flame retardancy of the resin sheet and the decorative sheet is further improved. In addition, the content of the phosphate ester-based flame retardant is preferably 20 parts by mass or less, more preferably 17 parts by mass or less, and even more preferably 15 parts by mass or less, based on 100 parts by mass of the resin in the transparent resin layer. By setting the upper limit of the content of the phosphate ester-based flame retardant within the above range, the sharpness of the resin sheet and the decorative sheet is further improved.
[0028] The resin sheet and decorative sheet of the present invention preferably have a configuration in which the above-mentioned phosphate ester-based flame retardant is contained in a transparent resin layer, and at least one thermoplastic resin layer selected from the group consisting of the transparent resin layer, the base sheet described below, and a synthetic resin backer layer contains a phosphate ester-based flame retardant.
[0029] When only the uppermost thermoplastic resin layer, i.e., the transparent resin layer, of the thermoplastic resin layers contains a phosphate ester-based flame retardant, the content of the phosphate ester-based flame retardant is preferably 3% by mass or more, more preferably 4.4% by mass or more, based on 100% by mass of the total mass of the thermoplastic resin layers. In addition, when the above-mentioned configuration is adopted, the content of the phosphate ester-based flame retardant is preferably 20% by mass or less, more preferably 15% by mass or less, based on 100% by mass of the total mass of the thermoplastic resin layers. By setting the lower limit of the content of the phosphate ester-based flame retardant within the above range, the flame retardancy of the resin sheet and the decorative sheet is further improved. In addition, by setting the upper limit of the content of the phosphate ester-based flame retardant within the above range, the sharpness of the resin sheet and the decorative sheet is further improved.
[0030] Fumed Silica The fumed silica is not particularly limited as long as it exhibits hydrophilicity and does not impair the transparency of the transparent resin layer, and fumed silica exhibiting an average particle size equal to or smaller than the wavelength of visible light is preferred in terms of further improving the sharpness of the decorative sheet. Examples of fumed silica include hydrophilic fumed silica.
[0031] An example of the hydrophilic fumed silica is fumed silica having hydroxyl groups such as silanol groups on the surface.
[0032] Fumed silica may be either a natural product or a synthetic product, and may be either crystalline or amorphous. Synthetic amorphous fumed silica may be prepared by either a wet method or a dry method. The method for preparing synthetic wet-method fumed silica prepared by a wet method is not particularly limited, and includes a precipitation method, a gel method, etc. The method for preparing synthetic dry-method fumed silica prepared by a dry method is not particularly limited, and includes a combustion method, an arc method, etc.
[0033] The BET specific surface area of fumed silica, such as hydrophilic fumed silica, is 50m 2 / g or more is preferable, and 130m 2 / g or more is more preferable, and 200m 2 / g or more is more preferable. By setting the lower limit of the BET specific surface area of the fumed silica within the above range, the average particle size is small, and in the case of hydrophilic fumed silica, the amount of silanol increases, so that the decrease in transparency of the transparent resin layer caused by adding fumed silica is further suppressed, and the dispersibility of the phosphate ester-based flame retardant is further improved, and the sharpness and flame retardancy of the resin sheet and decorative sheet are further improved. In addition, by setting the lower limit of the BET specific surface area of the fumed silica within the above range, the flame retardancy of the resin sheet and decorative sheet is improved, and the content of the phosphate ester-based flame retardant can be reduced.
[0034] In this specification, the BET specific surface area is a BET specific surface area measured by a nitrogen adsorption method in accordance with DIN66131.
[0035] The fumed silica may be a commercially available product, such as AEROSIL 50, AEROSIL 130, AEROSIL 200, AEROSIL 300, or AEROSIL 380 manufactured by Nippon Aerosil Co., Ltd.
[0036] The content of fumed silica in the transparent resin layer is preferably 4.0% by mass or more, more preferably 4.3% by mass or more, even more preferably 8.0% by mass or more, and particularly preferably 8.3% by mass or more, based on 100% by mass of the transparent resin layer. By setting the lower limit of the content of fumed silica in the transparent resin layer within the above range, the sharpness of the resin sheet and the decorative sheet is further improved. In addition, the content of fumed silica in the transparent resin layer is preferably 20% by mass or less, more preferably 18.5% by mass or less, even more preferably 17% by mass or less, and particularly preferably 15.4% by mass or less.
[0037] The content of fumed silica in the transparent resin layer is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, based on 100 parts by mass of the resin in the transparent resin layer. By setting the lower limit of the content of fumed silica in the transparent resin layer within the above range, the sharpness of the resin sheet and the decorative sheet is further improved. In addition, the content of fumed silica in the transparent resin layer is preferably 25 parts by mass or less, more preferably 20 parts by mass or less.
[0038] resin The transparent resin layer contains at least one resin selected from the group consisting of polyolefin-based resins and polyester-based resins.
[0039] Examples of the polyolefin-based thermoplastic resin include polyethylene, ethylene-α-olefin copolymer, polypropylene, polymethylpentene, polybutene, ethylene-propylene copolymer, propylene-butene copolymer, ethylene-vinyl acetate copolymer, saponified ethylene-vinyl acetate copolymer, ethylene-(meth)acrylic acid copolymer, ethylene-(meth)acrylic acid ester copolymer, etc. Among these, polypropylene is preferred.
[0040] As the polyester resin, a polyester thermoplastic resin can be used, and examples thereof include polyethylene terephthalate, highly heat-resistant polyalkylene terephthalate (for example, polyethylene terephthalate in which part of ethylene glycol is replaced with 1,4-cyclohexanedimethanol or diethylene glycol, so-called product name PET-G (manufactured by Eastman Chemical Company)), polybutylene terephthalate, polyethylene naphthalate, polyethylene naphthalate-isophthalate copolymer, etc. Among these, highly heat-resistant polyalkylene terephthalate is preferred.
[0041] The transparent resin layer may be colored as long as it has transparency. In this case, a colorant may be added to the resin. As the colorant, the pigment or dye used in the picture pattern layer may be used.
[0042] The transparent resin layer may contain various additives such as a matting agent, a foaming agent, a lubricant, an antistatic agent, an antioxidant, an ultraviolet absorber, a light stabilizer, a radical scavenger, and a soft component (for example, rubber).
[0043] The thickness of the transparent resin layer is preferably 60 μm or more, more preferably 80 μm or more. The thickness of the transparent resin layer is preferably 300 μm or less, more preferably 200 μm or less. By setting the lower limit of the thickness of the transparent resin layer within the above range, the scratch resistance and abrasion resistance of the resin sheet and the decorative sheet are further improved. By setting the upper limit of the thickness of the transparent resin layer within the above range, the resistance of the resin sheet and the decorative sheet to the spread of fire is further improved.
[0044] If necessary, the surface of the transparent resin layer may be subjected to a surface treatment such as a corona discharge treatment, an ozone treatment, a plasma treatment, an ionizing radiation treatment, a dichromate treatment, etc. The surface treatment may be performed according to a conventional method for each treatment.
[0045] A primer layer (a primer layer for facilitating the formation of a surface protective layer) may be formed on the surface of the transparent resin layer.
[0046] The primer layer can be formed by applying a known primer agent to the transparent resin layer. Examples of the primer agent include a urethane resin-based primer agent made of an acrylic-modified urethane resin, and a resin-based primer agent made of an acrylic-urethane block copolymer.
[0047] The thickness of the primer layer is not particularly limited, but is usually about 0.1 to 10 μm, and preferably about 1 to 5 μm.
[0048] (Base sheet) The substrate sheet is preferably a layer containing at least one resin selected from the group consisting of polyolefin-based resins and polyester-based resins.
[0049] As the polyolefin resin, a polyolefin thermoplastic resin can be used, and examples thereof include polyethylene, ethylene-α-olefin copolymer, polypropylene, polymethylpentene, polybutene, ethylene-propylene copolymer, propylene-butene copolymer, ethylene-vinyl acetate copolymer, saponified ethylene-vinyl acetate copolymer, ethylene-(meth)acrylic acid copolymer, ethylene-(meth)acrylic acid ester copolymer, etc. Among these, polypropylene is preferred.
[0050] As the polyester resin, a polyester thermoplastic resin can be used, and examples thereof include polyethylene terephthalate, highly heat-resistant polyalkylene terephthalate (for example, polyethylene terephthalate in which part of ethylene glycol is replaced with 1,4-cyclohexanedimethanol or diethylene glycol, so-called product name PET-G (manufactured by Eastman Chemical Company)), polybutylene terephthalate, polyethylene naphthalate, polyethylene naphthalate-isophthalate copolymer, etc. Among these, highly heat-resistant polyalkylene terephthalate is preferred.
[0051] The thickness of the substrate sheet is preferably 20 to 300 μm, more preferably 40 to 200 μm. The substrate sheet may be colored as necessary. In addition, the surface may be subjected to a surface treatment such as a corona discharge treatment, a plasma treatment, an ozone treatment, or the like, or may be coated with a primer, which is a base paint, for improving adhesion with adjacent layers.
[0052] (Pattern layer) The picture pattern layer is composed of a pattern ink layer and / or a solid ink layer. The picture pattern layer can be formed by a printing method such as gravure printing, offset printing, silk screen printing, inkjet printing, etc. Examples of the pattern of the pattern ink layer include wood grain patterns, stone grain patterns, fabric patterns, leather patterns, geometric patterns, letters, symbols, line drawings, various abstract patterns, etc. The solid ink layer is obtained by solid printing of colored inks. The picture pattern layer is composed of one or both of a pattern ink layer and a solid ink layer.
[0053] The ink used for the picture pattern layer may be one which uses as a vehicle one or more of chlorinated polyolefins such as chlorinated polyethylene and chlorinated polypropylene, polyester, polyurethane consisting of isocyanate and polyol, polyacrylic, polyvinyl acetate, polyvinyl chloride, vinyl chloride-vinyl acetate copolymer, cellulose resin, polyamide resin, etc., mixed together to which pigments, solvents, various auxiliary agents, etc. are added to make an ink. Among these, from the viewpoints of environmental issues, adhesion to the printed surface, etc., one or more mixtures of polyester, polyurethane consisting of isocyanate and polyol, polyacrylic, polyamide resin, etc. are preferred.
[0054] (Transparent adhesive layer) The transparent adhesive layer is provided between the picture pattern layer and the transparent resin layer as required. The transparent adhesive layer can be obtained, for example, by applying and drying a known adhesive for dry lamination, such as a two-component curing urethane resin.
[0055] The transparent adhesive layer preferably has a thickness after drying of about 0.1 to 30 μm, more preferably about 1 to 5 μm.
[0056] (Surface protective layer) The surface protective layer (transparent surface protective layer) is provided to impart surface properties such as scratch resistance, abrasion resistance, water resistance, and contamination resistance required for the decorative sheet. The resin forming this surface protective layer preferably contains at least one type of curable resin such as a thermosetting resin or an ionizing radiation curable resin. In particular, an ionizing radiation curable resin is preferred from the viewpoints of high surface hardness, productivity, and the like. Furthermore, an electron beam curable resin is most preferred from the viewpoint of further improving weather resistance.
[0057] Examples of thermosetting resins include unsaturated polyester resins, polyurethane resins (including two-component curing polyurethanes), epoxy resins, aminoalkyd resins, phenolic resins, urea resins, diallyl phthalate resins, melamine resins, guanamine resins, melamine-urea co-condensation resins, silicon resins, and polysiloxane resins.
[0058] A crosslinking agent, a curing agent such as a polymerization initiator, and a polymerization accelerator can be added to the resin. For example, as a curing agent, isocyanate, organic sulfonate, etc. can be added to unsaturated polyester resin or polyurethane resin, etc., organic amine, etc. can be added to epoxy resin, and peroxide such as methyl ethyl ketone peroxide, radical initiator such as azoisobutylnitrile, etc. can be added to unsaturated polyester resin.
[0059] Examples of methods for forming a surface protective layer using a thermosetting resin include a method in which a solution of a thermosetting resin is applied by a coating method such as roll coating or gravure coating, and then dried and cured. The amount of solution applied is about 5 to 50 μm, preferably about 5 to 40 μm, in terms of solid content.
[0060] The ionizing radiation curable resin is not limited as long as it undergoes a crosslinking polymerization reaction by irradiation with ionizing radiation and changes into a three-dimensional polymer structure. For example, one or more of prepolymers, oligomers, and monomers having polymerizable unsaturated bonds or epoxy groups in the molecule that can be crosslinked by irradiation with ionizing radiation can be used. For example, acrylate resins such as urethane acrylate, polyester acrylate, and epoxy acrylate; silicon resins such as siloxane; polyester resins; and epoxy resins can be mentioned.
[0061] Ionizing radiation includes visible light, ultraviolet light (near ultraviolet light, vacuum ultraviolet light, etc.), X-rays, electron beams, ion beams, etc., of which ultraviolet light and electron beams are preferred, and electron beams are more preferred.
[0062] As the ultraviolet light source, light sources such as ultra-high pressure mercury lamps, high pressure mercury lamps, low pressure mercury lamps, carbon arc lamps, black light fluorescent lamps, and metal halide lamps can be used. The wavelength of the ultraviolet light is about 190 to 380 nm.
[0063] As the electron beam source, various electron beam accelerators such as Cockcroft-Wald type, Van de Graff type, resonant transformer type, insulating core transformer type, linear type, dynamitron type, high frequency type, etc. can be used. The energy of the electron beam is preferably about 100 to 1000 keV, more preferably about 100 to 300 keV. The dose of the electron beam is preferably about 2 to 15 Mrad.
[0064] Ionizing radiation curable resins are sufficiently cured when irradiated with electron beams, but when curing is performed by irradiating with ultraviolet rays, it is preferable to add a photopolymerization initiator (sensitizer).
[0065] In the case of a resin system having a radical polymerizable unsaturated group, the photopolymerization initiator may be, for example, at least one of acetophenones, benzophenones, thioxanthones, benzoin, benzoin methyl ether, Michler's benzoyl benzoate, Michler's ketone, diphenyl sulfide, dibenzyl disulfide, diethyl oxide, triphenyl biimidazole, isopropyl-N,N-dimethylaminobenzoate, etc. In the case of a resin system having a cationic polymerizable functional group, for example, at least one of aromatic diazonium salts, aromatic sulfonium salts, metallocene compounds, benzoin sulfonate esters, furyloxysulfoxonium diallyliodosyl salts, etc. may be used.
[0066] The amount of the photopolymerization initiator added is not particularly limited, but is generally about 0.1 to 10 parts by mass per 100 parts by mass of the ionizing radiation curable resin.
[0067] The method for forming a protective layer using an ionizing radiation curable resin may be, for example, to apply a solution of the ionizing radiation curable resin by a coating method such as gravure coating, roll coating, etc. The amount of the solution to be applied is about 10 to 50 μm, preferably about 15 to 40 μm, in terms of solid content.
[0068] The thickness of the surface protective layer is preferably 4 μm or more, more preferably 8 μm or more, even more preferably 10 μm or more, and particularly preferably 12 μm or more. The thickness of the surface protective layer is preferably 50 μm or less, more preferably 40 μm or less, even more preferably 30 μm or less, particularly preferably 20 μm or less, and most preferably 15 μm or less. By setting the lower limit of the thickness of the surface protective layer within the above range, the scratch resistance and abrasion resistance of the decorative sheet are further improved. By setting the upper limit of the thickness of the surface protective layer within the above range, the decorative sheet is further improved in terms of the resistance to fire spread.
[0069] In this specification, when the fine particles 16 protrude from the surface of the surface protective layer as shown by ts in Figures 1 to 4, the thickness of the surface protective layer is measured at a location other than the protruding fine particles 16. When an uneven pattern is formed on the decorative sheet by embossing as shown in Figures 1 to 4, the thickness of the surface protective layer is measured at a location other than the uneven pattern.
[0070] In order to further impart scratch resistance and abrasion resistance to the surface protective layer or to reduce gloss, fine particles 16 may be blended as shown in Figs. 1 to 4. Examples of the fine particles include inorganic fillers. Examples of the inorganic fillers include powdered aluminum oxide, silicon carbide, silicon dioxide, calcium titanate, barium titanate, magnesium pyroborate, zinc oxide, silicon nitride, zirconium oxide, chromium oxide, iron oxide, boron nitride, diamond, emerythritol, glass fiber, and the like.
[0071] The average particle size of the fine particles is not particularly limited, and in the case where scratch resistance and abrasion resistance are further imparted to the surface protective layer, it is preferable that the average particle size is larger than the thickness of the surface protective layer. By having the average particle size of the fine particles larger than the thickness of the surface protective layer, the scratch resistance and abrasion resistance of the decorative sheet are further improved. The average particle size of the fine particles for further imparting scratch resistance and abrasion resistance to the surface protective layer is preferably more than 15 μm and 50 μm or less, more preferably 16 to 35 μm, and most preferably 16 to 20 μm.
[0072] The average particle size of the fine particles used as a matting agent for reducing the gloss of the surface protective layer is preferably 3 to 15 μm, more preferably 4 to 15 μm, and most preferably 8 to 15 μm. When the average particle size of the fine particles used as a matting agent is within the above range, the gloss of the surface protective layer can be further reduced.
[0073] Furthermore, when the surface protective layer is to be provided with scratch resistance, fine particles having an even smaller average particle size may be used. The average particle size of the fine particles for providing scratch resistance to the surface protective layer is preferably 1 to 5 μm, more preferably 3 to 5 μm, and even more preferably 3 to 4 μm. When the average particle size of the fine particles for providing scratch resistance to the surface protective layer is within the above range, the scratch resistance of the surface protective layer is further improved.
[0074] In this specification, the average particle size of the fine particles is the mode diameter. Note that the mode diameter is the particle size that shows the maximum value in the particle size distribution and is the particle size that occurs most frequently.
[0075] The amount of inorganic filler added is about 1 to 80 parts by mass with respect to 100 parts by mass of the ionizing radiation curable resin.
[0076] The surface protective layer may contain additives other than the inorganic fillers as necessary, such as fillers such as calcium carbonate and clay, flame retardants such as magnesium hydroxide, antioxidants, lubricants, foaming agents, ultraviolet absorbers, light stabilizers, deodorants, antibacterial agents, antiviral agents, antiallergen agents, and antifungal agents.
[0077] The surface protective layer preferably contains an antiviral agent. Antiviral agents can generally be broadly divided into organic and inorganic types. Examples of organic antiviral agents include quaternary ammonium salt-based, quaternary phosphonium salt-based, pyridine-based, pyrithione-based, benzimidazole-based, organic iodine-based, isothiazolin-based, and anion-based antiviral agents. Examples of inorganic antiviral agents include antiviral agents in which metal ions such as silver, copper, and zinc are supported on zeolite, apatite, zirconia, and glass.
[0078] Among the above organic antiviral agents, benzimidazole antiviral agents or anionic antiviral agents, which are antiviral agents that maintain a particle shape, are preferably used. The antiviral agent maintains a particle shape means that the antiviral agent does not dissolve in the composition for forming the surface protective layer (ink before curing) and exists in the form of particles in the cured surface protective layer. Therefore, in the process of forming the surface protective layer, the particles of the antiviral agent tend to float up, and the particles of the antiviral agent can be easily unevenly distributed on the outermost surface side of the surface protective layer. By unevenly distributing the particles of the antiviral agent on the outermost surface side of the surface protective layer, the amount of the antiviral agent required to obtain a predetermined antiviral property can be suppressed, and therefore, the deterioration of the scratch resistance of the surface protective layer can be easily suppressed.
[0079] The anionic antiviral agent preferably contains, for example, a styrene polymer derivative compound and an unsaturated carboxylic acid derivative compound. The styrene polymer derivative compound and the unsaturated carboxylic acid derivative compound preferably contain at least one structure selected from the structures of styrene, sodium sulfonate, acrylic acid, maleic acid, and fumaric acid, and more preferably contain all of these structures. This is because there are two types of viruses, enveloped and unenveloped, and it is believed that the structures of antiviral agents that can effectively inhibit the activity of each type are different.
[0080] As the inorganic antiviral agent, a silver-based antiviral agent is preferable from the viewpoint of lack of biotoxicity and excellent safety, and among them, a phosphate glass-supported silver compound or a silver zeolite compound is more preferable because it exhibits antiviral performance even in a small amount, and therefore the amount added can be reduced.
[0081] The above antiviral agents may be used alone or in combination of two or more.
[0082] (Synthetic resin backing layer) The resin sheet and decorative sheet of the present invention may have a synthetic resin backing layer. By having a synthetic resin backing layer, the impact resistance of the resin sheet and decorative sheet of the present invention is further improved.
[0083] Examples of resins constituting the synthetic resin backer layer include polypropylene, ethylene-vinyl alcohol copolymer, polymethylene, polymethylpentene, polyethylene terephthalate, highly heat-resistant polyalkylene terephthalate (e.g., polyethylene terephthalate in which part of ethylene glycol is replaced with 1,4-cyclohexanedimethanol or diethylene glycol, so-called trade name PET-G (manufactured by Eastman Chemical Company)), polybutylene terephthalate, polyethylene naphthalate, polyethylene naphthalate-isophthalate copolymer, polycarbonate, polyarylate, polyimide, polystyrene, polyamide, ABS, etc. These resins can be used alone or in combination of two or more kinds.
[0084] The thickness of the synthetic resin backing layer is preferably 0.1 to 0.6 mm, more preferably 0.15 to 0.45 mm, and even more preferably 0.20 to 0.40 mm. By setting the lower limit of the thickness of the synthetic resin backing layer within the above range, the impact resistance of the resin sheet and the decorative sheet is further improved. Also, by setting the upper limit of the thickness of the synthetic resin backing layer within the above range, the warping of the resin sheet and the decorative sheet is further suppressed.
[0085] The layers described above can be laminated, for example, by forming a picture pattern layer (solid ink layer, pattern ink layer) on one side of a base sheet by printing, laminating a transparent resin layer on the picture pattern layer via a known dry lamination adhesive such as a two-component curing urethane resin by dry lamination, T-die extrusion, or the like, and further forming a surface protective layer to produce an intermediate body, and then laminating a synthetic resin layer backer layer produced by T-die extrusion, or the like, and the base sheet side of the intermediate body by thermal lamination.
[0086] The total thickness of the resin sheet and the decorative sheet is preferably 110 μm or more, more preferably 120 μm or more. The total thickness of the resin sheet and the decorative sheet is preferably 600 μm or less, more preferably 400 μm or less. By setting the lower limit of the total thickness of the resin sheet and the decorative sheet within the above range, the scratch resistance and abrasion resistance of the resin sheet and the decorative sheet are further improved. By setting the upper limit of the total thickness of the resin sheet and the decorative sheet within the above range, the resistance of the resin sheet and the decorative sheet to the spread of fire is further improved.
[0087] In this specification, the total thickness of the resin sheet and the decorative sheet is measured at the surface of the decorative sheet other than the exposed particles 16 when the particles 16 protrude from the surface of the surface protective layer as shown as td in Figures 1 to 4. Also, when an uneven pattern is formed on the resin sheet and the decorative sheet by embossing as shown in Figures 1 to 4, the total thickness of the resin sheet and the decorative sheet is measured at the area other than the uneven pattern.
[0088] The resin sheet and the decorative sheet may be embossed from the transparent resin layer side or the surface protective layer side (the upper side of the resin sheet and the decorative sheet) to form a concave-convex pattern. The concave-convex pattern can be formed by heat pressing, hairline processing, etc. Examples of the concave-convex pattern include vessel grooves, stone slab surface unevenness, cloth surface texture, matte finish, sand grain, hairline, and stripe grooves.
[0089] In this specification, the layer thicknesses such as the total thickness of the resin sheet and the decorative sheet are values measured at a location where the uneven pattern is not formed.
[0090] The various additives (such as the fine particles contained in the surface protective layer and the phosphate ester-based flame retardant contained in the transparent resin layer) added to the above-mentioned layers of the resin sheet and decorative sheet of the present invention are preferably vesiculated. The method for vesiculating the various additives is not particularly limited, and they can be vesiculated by known methods, among which supercritical reverse phase evaporation is preferred.
[0091] The supercritical reverse phase evaporation method will be described in detail below. The supercritical reverse phase evaporation method is a method in which a mixture in which a substance forming the outer membrane of a vesicle is uniformly dissolved in carbon dioxide in a supercritical state or at a temperature or pressure condition above the supercritical point is added with an aqueous phase containing various additives as water-soluble or hydrophilic encapsulation substances to form a capsule-like vesicle containing various additives as encapsulation substances in a single layer of membrane. Note that carbon dioxide in a supercritical state means carbon dioxide in a supercritical state at a critical temperature (30.98°C) and a critical pressure (7.3773±0.0030MPa) or higher, and carbon dioxide under a temperature or pressure condition above the critical point means carbon dioxide under a condition in which only the critical temperature or only the critical pressure exceeds the critical condition. This method can obtain unilamellar vesicles with a diameter of 50 to 800 nm. In general, a vesicle is a general term for a vesicle having a membrane structure closed in a spherical shell shape and containing a liquid phase inside, and in particular, a vesicle whose outer membrane is composed of biological lipids such as phospholipids is called a liposome.
[0092] Examples of the above-mentioned phospholipids include glycerophospholipids such as phosphatidylcholine, phosphatidylethanolamine, phosphatidylserine, phosphatidic acid, phosphatidylglycerol, phosphatidylinositol, cardiolipin, yolk egg lecithin, hydrogenated yolk egg lecithin, soybean lecithin, and hydrogenated soybean lecithin; and sphingophospholipids such as sphingomyelin, ceramide phosphorylethanolamine, and ceramide phosphorylglycerol.
[0093] As the substance constituting the outer membrane, a dispersant such as a nonionic surfactant or a mixture of this with cholesterol or triacylglycerol can also be used.
[0094] As the nonionic surfactant, one or more of polyglycerin ether, dialkyl glycerin, polyoxyethylene hydrogenated castor oil, polyoxyethylene alkyl ether, polyoxyethylene sorbitan fatty acid ester, sorbitan fatty acid ester, polyoxyethylene polyoxypropylene copolymer, polybutadiene-polyoxyethylene copolymer, polybutadiene-poly2-vinylpyridine, polystyrene-polyacrylic acid copolymer, polyethylene oxide-polyethylethylene copolymer, polyoxyethylene-polycaprolactam copolymer, etc. can be used.
[0095] As the cholesterols, one or more of cholesterol, α-cholestanol, β-cholestanol, cholestane, desmosterol (5,24-cholestadiene-3β-ol), sodium cholate, cholecalciferol, and the like can be used.
[0096] The outer membrane of the liposome may be formed from a mixture of a phospholipid and a dispersant. In the decorative sheet of the present invention, by using a liposome having an outer membrane formed from a phospholipid, it is possible to improve the compatibility between the resin composition, which is the main component of each layer, and various additives.
[0097] Since the resin sheet and decorative sheet of the present invention have the above-mentioned configuration, fire does not spread easily even when laminated on a substrate with low thermal conductivity. Therefore, they can be used as resin sheets and decorative sheets to be laminated on substrates with thermal conductivity of less than 0.1 W / (m·K), and fire does not spread easily even when laminated on the substrate. Therefore, the resin sheet and decorative sheet of the present invention can be suitably used as decorative sheets for interior materials, in particular decorative sheets for floors.
[0098] 2. Decorative panels The decorative board of the present invention is a decorative board having the above-mentioned decorative sheet on a substrate.
[0099] (decorative sheet) As the decorative sheet constituting the decorative board of the present invention, the decorative sheet of the present invention explained above can be used.
[0100] (base material) The material of the substrate is not particularly limited, and for example, as shown in FIG. 5, a wooden substrate may be used in which a surface material 22 having a thermal conductivity within the above range is laminated on a wooden board 21 that is usually used for decorative boards such as floor decorative boards. Also, FIGS. 6 to 9 show an example of the layer structure of the decorative board of the present invention using the substrate of FIG. 5. In FIG. 6, the surface material 22 of the substrate 2 and the synthetic resin backer layer 11 of the decorative sheet 1 are bonded together, and the decorative sheet 1 is laminated on the substrate 2 to form a decorative board. Also, in FIGS. 7 and 8, the surface material 22 of the substrate 2 and the substrate sheet 12 of the decorative sheet 1 are bonded together, and the decorative sheet 1 is laminated on the substrate 2 to form a decorative board. Also, in FIG. 9, the surface material 22 of the substrate 2 and the picture pattern layer 13 (solid ink layer and / or pattern ink layer) side of the decorative sheet 1 are bonded together, and the decorative sheet 1 is laminated on the substrate 2 to form a decorative board.
[0101] The surface material is not particularly limited, and examples thereof include cork, paulownia, medium density fiberboard (MDF), high density fiberboard (HDF), etc., and these may also be used in combination. Among these, cork is preferably used because it can impart heat retention and cushioning properties to the decorative board. In other words, it is preferable that the above-mentioned substrate has a cork layer on the decorative sheet side.
[0102] The thickness of the surface material is not particularly limited, but is preferably 1.0 to 5.0 mm, and more preferably 1.0 to 2.5 mm.
[0103] The wood board is not particularly limited, and examples thereof include medium density fiberboard (MDF), high density fiberboard (HDF), plywood, etc. Among these, plywood is preferably used.
[0104] The thickness of the wood board is not particularly limited, but is preferably 4.0 to 15.0 mm, and more preferably 5.0 to 10.0 mm.
[0105] The method for laminating the surface material and the wood board is not particularly limited, and lamination can be performed by a conventionally known method, such as lamination using an adhesive. The adhesive is not particularly limited, and a wide variety of known woodworking adhesives can be used. Examples of adhesives include adhesives containing polyvinyl acetate, polyvinyl chloride, urethane, acrylic, acrylic urethane, vinyl chloride-vinyl acetate copolymer, ethylene-acrylic acid copolymer, ionomer, butadiene-acrylonitrile rubber, neoprene rubber, natural rubber, etc. as active ingredients. Examples of thermosetting adhesives include melamine-based, phenol-based, and urea-based (vinyl acetate-urea, etc.) adhesives.
[0106] The substrate constituting the decorative board of the present invention may have a thermal conductivity of less than 0.1 W / (m K) on the side to which the decorative sheet is attached. In this specification, the thermal conductivity of the substrate is the thermal conductivity measured by the following measurement method.
[0107] (Method for measuring the thermal conductivity of substrate) The material that forms the layer of the substrate on which the decorative sheet is attached is cut into a circle with a diameter of 40 mm to prepare a measurement sample. The measurement samples are stacked in the thickness direction, and an even number of sheets are stacked so that the thickness exceeds 15 mm. Next, a sensor is placed between half of the stacked measurement samples, and the thermal conductivity is measured by the hot disk method in accordance with ISO 22007-2:2008. Note that when the measurement samples are stacked, the air gap between adjacent measurement samples can be ignored.
[0108] Here is an example of how to measure thermal conductivity. A cork with a diameter of 40 mm and a thickness of 1.5 mm is prepared as the measurement sample. 30 sheets of the measurement samples are stacked so that the total thickness exceeds 15 mm when stacked. This results in a 45 mm stack. Next, a sensor is placed between the 15th and 16th measurement samples (at the 22.5 mm position), which is halfway through the thickness of the stack, and the thermal conductivity is measured using the hot disk method in accordance with ISO 22007-2:2008.
[0109] Furthermore, if the measurement sample is a cork with a thickness of 2.0 mm, stacking 20 sheets will result in a laminated body with a thickness of 40 mm, so the sensor can be placed between the 10th and 20th measurement samples.
[0110] In addition, if the measurement sample is a cork with a thickness of 1.0 mm, stacking 40 sheets will result in a laminated body with a thickness of 40 mm, so the sensor can be placed between the 20th and 21st measurement samples.
[0111] The method for laminating the decorative sheet on the front surface of the substrate is not particularly limited, and the decorative sheet can be laminated by a conventionally known method, such as forming an adhesive layer on the front surface of the substrate and laminating the decorative sheet thereon.
[0112] The thickness of the adhesive layer is not particularly limited, and the thickness after drying is preferably 0.1 to 100 μm, more preferably 0.1 to 30 μm, and even more preferably 1 to 20 μm.
[0113] Examples of adhesives used in the adhesive layer include water-soluble emulsion adhesives, polyester adhesives, acrylic adhesives, urethane adhesives, etc. The adhesives may be used alone or in combination of two or more.
[0114] The decorative board of the present invention has the above-mentioned configuration, and therefore has excellent flame retardancy and can exhibit high sharpness. Therefore, the decorative board of the present invention can be suitably used as a decorative board for interior materials, in particular, as a decorative board for floors. EXAMPLES
[0115] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.
[0116] Example 1 (Manufacturing decorative sheets (resin sheets)) As the substrate sheet, an opaque colored polypropylene film with a thickness of 60 μm was prepared. Next, after subjecting both sides of the substrate sheet to a corona discharge treatment, a primer layer (thickness 2 μm) of a two-component curing urethane resin was formed on the back surface of the substrate sheet, and a picture pattern layer was formed on the front surface of the substrate sheet by a gravure printing method using a curing printing ink containing an acrylic urethane resin. Furthermore, a transparent adhesive layer was formed by applying an adhesive of a two-component curing urethane resin on the picture pattern layer. Furthermore, a transparent polypropylene resin containing the following phosphate ester flame retardant was hot-melted and extruded on the adhesive layer with a T-die extruder to form a thermoplastic transparent resin layer (thickness 100 μm).
[0117] Transparent polypropylene resin: 100 parts by weight Phosphate ester flame retardant (product name: PX-200 (manufactured by Daihachi Chemical Industry Co., Ltd.); phosphate ester): 10 parts by weight Fumed silica (product name: AEROSIL 300 (manufactured by Nippon Aerosil Co., Ltd.); hydrophilic fumed silica; BET specific surface area 300 m 2 / g):20 parts by mass
[0118] Next, the surface of the transparent resin layer was subjected to a corona discharge treatment, and then a primer layer (thickness 2 μm) of a two-component curing urethane resin was formed on the transparent resin layer. Furthermore, an electron beam curing resin composition containing a urethane (meth)acrylate oligomer was applied to the primer layer by a gravure coating method, and dried. Then, an electron beam was irradiated under conditions of an acceleration voltage of 165 keV and 30 kGy to form a surface protection layer having a thickness of 15 μm.
[0119] Next, the surface protective layer side was heated with an infrared non-contact heater to soften the base sheet and the transparent resin layer, and then immediately embossed from the surface protective layer side by heat and pressure to form a concave-convex pattern. The decorative sheet (resin sheet) of Example 1 was produced by the above-mentioned manufacturing method.
[0120] The total thickness of the transparent resin layer and the base sheet of the decorative sheet of Example 1 was 160 μm. The content of the phosphate ester-based flame retardant was 7.7 mass% based on 100 mass% of the transparent resin layer. The content of the phosphate ester-based flame retardant was 5.0 mass% based on 100 mass% of the total mass of the transparent resin layer and the base sheet.
[0121] (Manufacturing decorative panels) A cork sheet having a thickness of 1.5 mm was attached to a plywood having a thickness of 7.5 mm using an adhesive to prepare a wood substrate.
[0122] Next, the surface of the decorative sheet facing the base sheet was attached to the surface of the cork sheet of the wood base material via a two-part curing water-soluble emulsion adhesive. The amount of the two-part curing water-soluble emulsion adhesive applied was 130 g / m 2 It was.
[0123] The water-soluble emulsion adhesive used was as follows: Water-soluble emulsion adhesive Base material: "BA-10L" manufactured by Japan Coating Resin Co., Ltd., modified ethylene vinyl acetate type Hardener: "BA-11B" manufactured by Japan Coating Resin Co., Ltd., isocyanate type. Mixing ratio: Base agent: Hardener = 100:2.5 (mass ratio)
[0124] Then, 25°C, 10 kg / m 2 The laminate was then cured for three days under pressure to produce a decorative panel.
[0125] Example 2 A decorative sheet and a decorative board were manufactured in the same manner as in Example 1, except that the content of fumed silica in the transparent resin layer was 10 parts by mass, and the composition of the transparent polypropylene resin containing a phosphate-based flame retardant was changed as follows. The content of the phosphate-based flame retardant was 8.3% by mass, with the transparent resin layer being 100% by mass. The content of the phosphate-based flame retardant was 5.3% by mass, with the total mass of the transparent resin layer and the base sheet being 100% by mass.
[0126] Transparent polypropylene resin: 100 parts by weight Phosphate ester flame retardant (product name: PX-200 (manufactured by Daihachi Chemical Industry Co., Ltd.); phosphate ester): 10 parts by weight Fumed silica (product name: AEROSIL 300 (manufactured by Nippon Aerosil Co., Ltd.); hydrophilic fumed silica; BET specific surface area 300 m 2 / g):10 parts by mass
[0127] Example 3 A decorative sheet and a decorative board were manufactured in the same manner as in Example 1, except that the content of fumed silica in the transparent resin layer was 15 parts by mass, and the composition of the transparent polypropylene resin containing a phosphate-based flame retardant was changed as follows. The content of the phosphate-based flame retardant was 8.0% by mass, with the transparent resin layer being 100% by mass. The content of the phosphate-based flame retardant was 5.2% by mass, with the total mass of the transparent resin layer and the base sheet being 100% by mass.
[0128] Transparent polypropylene resin: 100 parts by weight Phosphate ester flame retardant (product name: PX-200 (manufactured by Daihachi Chemical Industry Co., Ltd.); phosphate ester): 10 parts by weight Fumed silica (product name: AEROSIL 300 (manufactured by Nippon Aerosil Co., Ltd.); hydrophilic fumed silica; BET specific surface area 300 m 2 / g):15 parts by mass
[0129] Comparative Example 1 A decorative sheet and a decorative board were manufactured in the same manner as in Example 1, except that the content of the phosphate ester-based flame retardant in the transparent resin layer was 15 parts by mass, the composition was made to contain no fumed silica, and the composition of the transparent polypropylene resin containing the phosphate ester-based flame retardant was changed as follows. The content of the phosphate ester-based flame retardant was 13.0% by mass, with the transparent resin layer being 100% by mass. The content of the phosphate ester-based flame retardant was 8.2% by mass, with the total mass of the transparent resin layer and the base sheet being 100% by mass.
[0130] Transparent polypropylene resin: 100 parts by weight Phosphate ester flame retardant (product name: PX-200 (manufactured by Daihachi Chemical Industry Co., Ltd.); phosphate ester): 15 parts by weight
[0131] Reference example 1 A decorative sheet and a decorative board were produced in the same manner as in Example 1, except that the transparent resin layer did not contain a phosphate-based flame retardant and fumed silica.
[0132] (evaluation) The decorative sheets and decorative boards of the Examples and Comparative Examples produced as described above were evaluated by the following methods.
[0133] (1) Horizontal combustion (flame retardancy: difficulty in spreading fire) The decorative board was cut into a size of 9 cm x 30 cm to prepare a test specimen. As shown in Figs. 10 and 11, a rectangular metal stand 103 was placed on a stand 102 of a commercially available household heater 101 (Zaiguru Handsome SJ-100 (trade name)), and a test specimen 105 was placed in a metal frame 104 installed on the stand, and a test for fire spread resistance was performed under conditions of a heater angle of 45° and a heater output dial of 4. In detail, the test specimen was preheated for 2 minutes using the household heater. Next, as shown in Fig. 10, the end 106 on the heater side in the longitudinal direction of the test specimen was heated with a lighter 107 for 1 minute to ignite, and the fire was spread in the longitudinal direction of the test specimen 105 as shown in Fig. 11. Next, the fire spread was visually observed, and the burning distance (L1) and burning duration were evaluated as follows.
[0134] [Burn Distance (L1)] The test piece was ignited, the flame from the lighter was removed, and the fire spread distance (L1) was measured and evaluated according to the following evaluation criteria. A rating of + or higher is considered to be satisfactory for practical use. ++: L1 is less than 5 cm +: L1 is 5cm or more but less than 10cm -: L1 is 10cm or more
[0135] [Burning duration] The test piece was ignited, the lighter flame was removed, and the duration of burning from the initial ignition to self-extinguishing was measured and rated according to the following criteria. A rating of + or higher is considered to be satisfactory for practical use. +++: Burning duration is less than 100 seconds or does not ignite ++: Burning duration is between 100 and 300 seconds +: Burning duration is between 300 and 600 seconds -: Burning duration is 600 seconds or more (does not self-extinguish within 600 seconds)
[0136] (2) Sharpness [Hayes] Only the transparent resin layer of each decorative sheet was placed in the device and the haze value was measured using a direct reading haze meter manufactured by Toyo Seiki Seisakusho Co., Ltd. If the haze value is 90.0 or less, it is evaluated as being suitable for practical use.
[0137] [exterior] The appearance of the decorative sheet was visually observed from the transparent resin layer side (surface protective layer side) of the decorative sheet and evaluated according to the following evaluation criteria. Note that a rating of + or higher is evaluated as being satisfactory for practical use. ++: The design of the pattern layer is clearly visible +: The design of the pattern layer appears slightly cloudy. -: The design of the pattern layer appears discolored or cloudy.
[0138] The results are shown in Tables 1 and 2.
[0139] [Table 1]
[0140] [Table 2]
[0141] Table 2 shows the effect of the amount of fumed silica (hydrophilic fumed silica) on sharpness. It is generally believed that the greater the amount of fumed silica in the transparent resin layer, the higher the haze value and the poorer the sharpness. However, the results in Table 2 show that the greater the amount of fumed silica (hydrophilic fumed silica) contained in the transparent resin layer containing a phosphate ester flame retardant, the lower the haze value and the further improved the sharpness. [Explanation of symbols]
[0142] 1. Decorative sheet 11. Synthetic resin backing layer 12. Base sheet 13.Pattern layer 14.Transparent resin layer 15.Surface protection layer 16. Fine particles 2. Base material 21. Wood board 22.Surface material 101. Home heater 102. Household heater stand 103. Metal rectangular stand 104. Metal Frame 105. Test Pieces 106. Heater side end of the test piece in the longitudinal direction 107. Writer L1. Burning distance
Claims
1. A resin sheet having at least a transparent resin layer, (1) The transparent resin layer contains a phosphate ester-based flame retardant and fumed silica prepared by a dry method, (2) The transparent resin layer contains at least one resin selected from the group consisting of polyolefin-based resins and polyester-based resins. A resin sheet characterized by:
2. The resin sheet according to claim 1 , wherein the content of the phosphate-based flame retardant is 7.0% by mass or more, based on 100% by mass of the transparent resin layer.
3. The resin sheet according to claim 1 or 2, wherein the fumed silica is hydrophilic fumed silica.
4. The resin sheet according to any one of claims 1 to 3, wherein the content of the fumed silica is 4.0% by mass or more, based on 100% by mass of the transparent resin layer.
5. The resin sheet according to any one of claims 1 to 4, comprising the transparent resin layer and a base sheet.
6. The resin sheet according to any one of claims 1 to 4, comprising at least a picture pattern layer and the transparent resin layer in this order on a base sheet.
7. The resin sheet according to any one of claims 1 to 4, comprising at least a picture pattern layer, the transparent resin layer, and a surface protective layer in this order on a base sheet.
8. The resin sheet according to claim 7 , wherein the surface protective layer contains an antiviral agent.
9. The resin sheet according to any one of claims 5 to 8, having an embossed shape on the transparent resin layer side.
10. A decorative sheet which is the resin sheet according to any one of claims 1 to 9.
11. A decorative board having the decorative sheet according to claim 10 on a substrate.
Citation Information
Patent Citations
Fire-retardant non-halogen type floor material
JP1995089014A
Fire-resistant non-woven adhesive sheet
JP2002069403A
Biaxially oriented polyester film
JP2004339495A
Decorative sheet and production method thereof
JP2017124624A
Decorative laminate film and method for producing the same
JP2018012215A