Laminated Film

A laminated film with specific layer properties and manufacturing processes addresses the limitations of existing methods, achieving low retardation, high quality, and improved productivity, suitable for optical applications.

JP7593027B2Active Publication Date: 2024-12-03TORAY INDUSTRIES INC
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020159796
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-30
Filing Date
2020-09-24
Publication Date
2024-12-03
Estimated Expiration
2040-09-24

AI Technical Summary

Technical Problem

Existing methods for producing laminated films with low retardation and improved quality and productivity face limitations, such as restricted stretching and heat treatment conditions, difficulty in incorporating olefin resins, and insufficient stretching ratios, leading to issues with cost, versatility, and productivity.

Method used

A laminated film structure with layers A and B, where A has a retardation of 0.0 nm to 180 nm, B provides protection, and both layers have specific crystal melting energy differences, peel strength, and solubility parameters, allowing for coextrusion, casting, and controlled stretching to achieve low retardation and high quality.

Benefits of technology

The laminated film achieves low retardation, excellent quality, and improved productivity, with enhanced protection and optical properties, suitable for applications like polarizer protective films and transparent conductive films.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593027000001
    Figure 0007593027000001
  • Figure 0007593027000002
    Figure 0007593027000002
  • Figure 0007593027000003
    Figure 0007593027000003
Patent Text Reader

Abstract

To provide a laminated film having a low phase difference and excellent even in quality or productivity, and a method for manufacturing the same.SOLUTION: The laminated film including an A layer and a B layer having crystal melting energy ΔHm (J / g) different from each other is provided in which both surfaces of the A layer are in contact with the B layer, the retardation of the A layer is 0.0 nm or more and 180 nm or less, the surface orientation coefficient of the B layer is 0.0300 or more and 0.1700 or less, and when ΔHmA (J / g) denotes ΔHm of the A layer and ΔHmB (J / g) denotes ΔHm of the B layer, ΔHmB-ΔHmA is 5.0 (J / g) or more, and the peel strength of at least one of the B layer and the A layer is 1.0 g / 50 mm or more and 100 g / 50 mm or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate film having a low retardation layer and a protective layer. [Background technology]

[0002] In recent years, in the fields of flat panel displays and touch panels, there has been an increasing demand for various optical films with low retardation, such as polarizer protective films and transparent conductive films. In addition to having a low retardation, such optical films are usually required to have improved quality, reduced thickness unevenness, dimensional stability at high temperatures, productivity, and the like.

[0003] To date, various studies have been made on films and their manufacturing methods in order to improve the above-mentioned properties. For example, a method for manufacturing a film is known in which a laminated film of a target film layer and a protective layer is longitudinally stretched by a roll-type stretching machine, and then the protective layer is peeled off and transversely stretched or heat-treated without contact, thereby reducing scratches due to slipping on the roll (Patent Document 1). In addition, a method for manufacturing a film that combines optical properties and handleability is also known by adding gels of different sizes to a cyclic olefin resin with excellent optical properties to form a film (Patent Document 2). Furthermore, it is also known that a biaxially oriented cyclic olefin resin film with a stretching ratio of 1.1 to 1.8 times in each direction becomes an optical film with excellent heat resistance, optical properties, and dimensional stability (Patent Document 3). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2001-30351 A [Patent Document 2] JP 2009-227932 A [Patent Document 3] JP 2011-93285 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, in the technology described in Patent Document 1, the productivity is improved by forming the target film layer and the protective layer in an integrated manner, but the conditions for stretching and heat treatment are limited, so that it is difficult to apply it to the production of a low retardation film mainly composed of a cyclic olefin resin. The technology described in Patent Document 2 is excellent in that a high-quality film can be obtained, but when long-term storage or transportation is required, a process of attaching a protective layer later to prevent scratches is required, so it is inferior in terms of productivity, cost, and versatility. In addition, the film in Patent Document 3 is a biaxially oriented film, but the stretching ratio is only 3.24 times at most in terms of area ratio, which is insufficient for making a low retardation film, and specific improvements in surface properties and optical properties are not clear.

[0006] An object of the present invention is to overcome these problems of the conventional techniques and to provide a laminated film having a low retardation and excellent quality and productivity, and a method for producing the same. [Means for solving the problem]

[0007] In order to solve the above problems, the present invention employs the following means. (1) A layer and a layer B having different crystal melting energies ΔHm (J / g), both surfaces of the layer A are in contact with the layer B, the retardation of the layer A is 0.0 nm or more and 180 nm or less, the plane orientation coefficient of the layer B is 0.0300 or more and 0.1700 or less, and ΔHm of the layer A is ΔHm A (J / g), ΔHm of layer B is ΔHm B (J / g), ΔHm B -ΔHm A 5.0 (J / g) or more, and the peel strength between at least one of the B layer and the A layer is 1.0 g / 50 mm or more and 100 g / 50 mm or less. (2) The solubility parameter of the A layer is SP A (cal / cm 3 ) 1 / 2, the solubility parameter of layer B is SP B (cal / cm 3 ) 1 / 2 Then, |SP A -SP B The laminate film according to (1), characterized in that | is 0.5 or more and 4.0 or less. (3) The laminate film according to (1) or (2), characterized in that the haze is 0.5% or more and 3.0% or less. (4) The glass transition temperature (Tg A ) is greater than 100° C. and not greater than 170° C. The laminate film according to any one of (1) to (3). (5) The laminate film according to any one of (1) to (4), wherein the layer A contains an amorphous resin as a main component. (6) The laminate film according to (5), wherein the amorphous resin is at least one resin selected from the group consisting of polypropylene resins, cyclic olefin resins, polystyrene resins, polycarbonate resins, acrylic resins, polyester resins, and polyamide resins. (7) The laminate film according to any one of (1) to (6), wherein the number of flexion cycles until breakage of the layer A is 100 or more and 10,000 or less. (8) The laminate film according to any one of (1) to (7), wherein the surface roughness Ra of one or both sides of the layer A is 1 nm or more and 100 nm or less. (9) The laminate film according to any one of (1) to (8), wherein the layer B has a minor endothermic peak temperature (Tmeta) of 120° C. or higher and 220° C. or lower. (10) The laminate film according to any one of (1) to (9), wherein the B layer has a refractive index in the plane direction of 1.6000 or more and 1.6600 or less, and a refractive index in the thickness direction of the B layer of 1.4800 or more and 1.5700 or less. (11) The crystallinity parameter (ΔTcg) of the layer B is 10° C. or more and 100° C. or less, and the ΔHm B The laminate film according to any one of (1) to (10), wherein the strength is 15.0 J / g or more and 50.0 J / g or less. (12) The glass transition temperature (Tg B ) is 30° C. or more and 100° C. or less. (13) The laminate film according to any one of (1) to (12), wherein the layer B contains a crystalline resin as a main component. (14) The laminate film according to (13), wherein the crystalline resin is a polyester resin. (15) A method for producing the laminated film according to any one of (1) to (14), comprising the steps of: a coextrusion lamination step of coextruding and laminating the molten resin composition A and the molten resin composition B, the molten resin composition A being used to obtain the A layer, and the molten resin composition B being used to obtain the B layer; a casting step of cooling and solidifying the laminate obtained by the coextrusion lamination step; a stretching step of stretching the sheet obtained by the casting step in at least one direction; and a stretching step of stretching the Tg A Tg over +20℃ A A method for producing a laminated film, comprising the steps of: a) heat treating the film at a temperature of +120°C or lower; and b) heat treating the film at a temperature of +120°C or lower. (16) The method for producing a laminated film according to (15), characterized in that the crystallinity of the layer B in the casting process is controlled to be 10% or more and 30% or less. (17) The method for producing a laminated film according to (15) or (16), characterized in that in a co-extrusion lamination step, the molten resin composition B is laminated on both sides of the molten resin composition A. (18) The method for producing a laminated film according to (17), wherein the molten resin compositions B located on either side of the molten resin composition A have compositions different from each other. (19) The method for producing a film according to any one of (15) to (18), further comprising a width-spreading step of separately spreading the molten resin composition A and the molten resin composition B upstream of the co-extrusion lamination step. Effect of the Invention

[0008] According to the present invention, it is possible to provide a laminated film having a low retardation and excellent quality and productivity, and a method for producing the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The laminated film of the present invention has a layer A and a layer B having different crystal melting energies ΔHm (J / g), both surfaces of the layer A are in contact with the layer B, the retardation of the layer A is 0.0 nm or more and 180 nm or less, the plane orientation coefficient of the layer B is 0.0300 or more and 0.1700 or less, and ΔHm of the layer A is ΔHm A (J / g), ΔHm of layer B is ΔHm B (J / g), ΔHm B -ΔHm A The present invention is characterized in that the peel strength between at least one of the layers B and A is 5.0 (J / g) or more, and the peel strength between at least one of the layers B and A is 1.0 g / 50 mm or more and 100 g / 50 mm or less. The present invention will be specifically described below.

[0010] From the viewpoint of protecting the A layer, it is important that the laminated film of the present invention has the A layer and the B layer, which have different crystal melting energies ΔHm (J / g), and that both surfaces of the A layer are in contact with the B layer. ΔHm is a value indicating the degree of crystallization of the resin constituting the layer, and is an index of the hardness of the layer. In other words, the higher the ΔHm, the higher the hardness of the layer. And the measurement of ΔHm can be performed by a method conforming to JIS K-7122 (1987 edition). In addition, "both surfaces of the A layer are in contact with the B layer" means that there is at least one laminated structure in which the B layer / A layer / B layer are directly laminated in this order. In the laminated film of the present invention, the A layer is assumed to be used for optical purposes, and the B layer plays a role of protecting the A layer. In this embodiment, each of the B layers located on both sides of the A layer functions as a protective layer for the A layer, so that a film obtained by peeling and removing the B layers on both sides of the laminate film of the present invention (hereinafter sometimes referred to as the A layer film) is less susceptible to scratches and unevenness due to friction with the roll or collision with foreign objects during the winding process, etc., and can be suitably used for optical applications, etc.

[0011] The laminated structure of the laminated film of the present invention is not particularly limited as long as both surfaces of the A layer are in contact with the B layer. For example, B / A / B is the minimum laminated structure for achieving the effects of the present invention, but it may be a super multi-layer structure of 100 layers or more such as B / A / B / A / B..., or a C / B / A / B structure or a C / B / A / B / C structure in which a C layer is provided on the outside of B / A / B. The thickness ratio of the A layer to the B layer (A:B) is not particularly limited, but is preferably 1:10 to 1:100, more preferably 1:10 to 1:20, from the viewpoint of film formation stability and protective performance.

[0012] In the B / A / B structure, the thickness of each B layer may be the same or different as long as it does not impair the effects of the present invention. The thickness ratio of each layer in the B / A / B structure is not particularly limited as long as it does not impair the effects of the present invention, but is preferably 1:1:1 to 1:20:1 from the viewpoints of film formation stability and protective performance.

[0013] In the laminated film of the present invention, from the viewpoint of protecting the A layer, the ΔHm of the A layer is set to ΔHm A (J / g), ΔHm of layer B is ΔHm B (J / g), ΔHm B -ΔHm A It is important that the ΔHm of the B layer is 5.0 (J / g) or more. By having the ΔHm of the B layer higher than the ΔHm of the A layer, the B layer can exhibit high protective performance. B -ΔHm A is preferably 10.0 J / g or more and 50.0 J / g or less. B -ΔHm A As a method for making the ΔHm to be 5.0 (J / g) or more or within the above-mentioned preferable range, for example, a method for selecting the resins constituting the A layer and the B layer in consideration of the difference in ΔHm can be mentioned. More specifically, B >ΔHm A By selecting a resin that satisfies and increases the difference between the two, ΔHm B -ΔHm A can be made larger.

[0014] In the laminated film of the present invention, from the viewpoint of easily obtaining the A layer film, it is important that the peel strength between at least one of the B layer and the A layer is 1.0 g / 50 mm or more and 100 g / 50 mm or less. By adopting such an embodiment, it becomes easy to peel the A layer and the B layer. More specifically, if the peel strength between the B layer and the A layer is less than 1.0 g / 50 mm, interlayer peeling occurs with a small force, and there is a problem that peeling occurs during the conveying process or the processing process. On the other hand, if the peel strength between the B layer and the A layer exceeds 100 g / 50 mm, the adhesion between the B layer and the A layer becomes too strong, so that it becomes difficult to peel them off, and there is a problem that tearing or residue occurs during peeling. From the above viewpoint, it is preferable that the peel strength between the B layer and the A layer is 2.0 g / 50 mm or more and 50 g / 50 mm or less. From the above viewpoint, it is sufficient that the peel strength between at least one of the B layers and the A layers is 1.0 g / 50 mm or more and 100 g / 50 mm or less, or within the above-mentioned preferred range, but from the viewpoint of easily obtaining the A layer film, it is preferable that the peel strength between the B layer and the A layer on both sides is 1.0 g / 50 mm or more and 100 g / 50 mm or less, or within the above-mentioned preferred range. The peel strength between the B layer and the A layer refers to the peel strength between the B layer and the A layer when peeled at 180°, measured in accordance with JIS K 6854-2 (1999 edition).

[0015] In the laminated film of the present invention, a method for adjusting the peel strength between the B layer and the A layer to 1.0 g / 50 mm or more and 100 g / 50 mm or less, or to the above-mentioned preferable range, is to adjust the solubility parameter of the A layer to SP A (cal / cm 3 ) 1 / 2 , the solubility parameter of layer B is SP B (cal / cm 3 ) 1 / 2 When |SP A -SP B A method of adjusting the peel strength between the B layer and the A layer is preferably used. A -SP B Therefore, if you want to lower the peel strength between layers B and A, you should set |SP A -SP BSpecifically, from the viewpoint of both reducing peeling during the transport and processing steps and suppressing residues at the time of peeling, |SP A -SP B is preferably 0.5 or more and 4.0 or less, and more preferably 1.0 or more and 3.0 or less. Alternatively, the peel strength between layer B and layer A can be controlled by adjusting the heat treatment conditions after stretching or the thickness of the laminated film. More specifically, the peel strength between layer B and layer A can be increased by setting the heat treatment temperature to the glass transition temperature of layer A or higher or increasing the thickness of the laminated film.

[0016] In the present invention, the solubility parameter SP A (cal / cm 3 ) 1 / 2 , S.P. B (cal / cm 3 ) 1 / 2 The calculation of is based on the molecular structure and is relatively easy to use, using the Fedors method. In the Fedors method, the solubility is considered to change depending on the molecular cohesive energy density and molar volume, depending on the type and number of substituents, and the solubility parameter value δ (cal / cm) is calculated according to the following formula (1). 3 ) 1 / 2 is estimated, where E coh (cal / mol) is the cohesive energy and V is the molar volume (cm 3 / mol).

[0017]

number

[0018] The solubility parameter SP value of a thermoplastic resin can be estimated using Fedor's formula based on the repeating structural units of the molecular chain, so the solubility parameter SP value of a thermoplastic resin containing structural units derived from copolymer components is calculated according to the ratio of each structural unit. The solubility parameter SP value of a representative thermoplastic resin is as follows: polyethylene: 8.0 (cal / cm 3 ) 1 / 2, Polyethylene terephthalate: 10.7 (cal / cm 3 ) 1 / 2 , polystyrene: 9.4 (cal / cm 3 ) 1 / 2 , polymethyl methacrylate: 9.3 (cal / cm 3 ) 1 / 2 , Polybutylene terephthalate: 10.0 (cal / cm 3 ) 1 / 2 , Nylon 6: 12.7 (cal / cm 3 ) 1 / 2 , Polycarbonate: 9.9 (cal / cm 3 ) 1 / 2 , COP: 8.6 (cal / cm 3 ) 1 / 2 , COC: 7.8 (cal / cm 3 ) 1 / 2 , ABS resin: 10.0 (cal / cm 3 ) 1 / 2 , Polypropylene: 8.0 (cal / cm 3 ) 1 / 2 In addition, when multiple components are contained in each layer, the mass ratio of each component is multiplied by the SP value of each component, and the sum of the results is the SP A Value, SP B value.

[0019] In the laminated film of the present invention, it is important that the retardation of the A layer is 0.0 nm or more and 180 nm or less. By adopting such an embodiment, it is possible to reduce rainbow unevenness in the A layer and ensure visibility. Therefore, a film obtained by peeling and removing the B layers on both sides of the laminated film of the present invention (hereinafter, sometimes referred to as the A layer film) can be used in applications where visibility and reduction of rainbow unevenness are required at the same time, such as optical applications such as polarizer protection.

[0020] If the retardation of the A layer exceeds 180 nm, problems such as rainbow unevenness and deterioration of visibility occur in the film made of the A layer, making it difficult to use it for the above-mentioned applications. From the viewpoint of simultaneously improving the visibility of the film made of the A layer and reducing the rainbow unevenness, the retardation of the A layer is preferably 0.0 nm or more and 100 nm or less, more preferably 0.0 nm or more and 10 nm or less, and particularly preferably 0.0 nm or more and 1.0 nm or less.

[0021] The retardation of the A layer in the present invention is a value obtained by measuring the phase difference of the A layer film with a light beam having a wavelength of 548.3 nm using an automatic birefringence meter (KOBRA-21ADH) manufactured by Oji Measurement Co., Ltd.

[0022] A method for making the retardation of the A layer 0.0 nm or more and 180 nm or less or the above-mentioned preferred range includes a method in which the main component of the A layer is an amorphous resin. More specifically, the retardation of the A layer can be reduced by increasing the content ratio of the amorphous resin in the A layer or by using a resin with stronger amorphousness. The main component refers to a component that is contained in an amount of more than 50 mass% when the total components constituting the layer are taken as 100 mass%. In the case where a plurality of types of components corresponding to the amorphous resin are contained, if the total amount of the components corresponding to the amorphous resin exceeds 50 mass%, it can be interpreted as the amorphous resin being the main component. Hereinafter, the "main component" can be interpreted in the same way. In the present invention, the amorphous resin refers to a resin whose crystal melting energy ΔHm obtained from a differential scanning calorimeter DSC is less than 5.0 J / g. In addition, the strength of the amorphousness is determined by the value of ΔHm, and the lower the ΔHm, the stronger the amorphousness. That is, a resin with a ΔHm of 0.0 J / g is the most amorphous resin, and a resin with a ΔHm of 5.0 J / g is the most amorphous crystalline resin.

[0023] When the main component of the A layer is a crystalline resin, the retardation of the A layer can be adjusted to 0.0 nm or more and 180 nm or less, or to the above-mentioned preferred range, by a method of stretching at a uniform magnification in two perpendicular directions, or a method of relaxing the molecular orientation by performing heat treatment after stretching. The heat treatment is preferably performed under conditions of a crystal melting peak temperature (Tm°C) of the crystalline resin or more and Tm+80°C or less.

[0024] The resin in layer A of the laminated film of the present invention is not particularly limited as long as it does not impair the effects of the present invention, but from the viewpoint of optical quality, it is preferably at least one resin selected from polypropylene resins, cyclic olefin resins, polystyrene resins, polycarbonate resins, acrylic resins, polyester resins, and polyamide resins. Here, at least one resin refers to all of the following: a single component, a plurality of resins of the same category (e.g., a plurality of cyclic olefin resins), and a resin of different categories (e.g., a total of two or more components of cyclic olefin resins and polystyrene resins).

[0025] In the present invention, the polypropylene resin means a polymer in which the total of polypropylene-derived components (polypropylene units) is more than 50 mol% and not more than 100 mol% when the total structural units of the resin are 100 mol%. Specifically, various polypropylene resins such as polypropylene, ethylene-propylene copolymer, ethylene-propylene-butene copolymer, methylpentene polymer, etc. can be used. In addition, polymers made of α-olefin monomers such as ethylene, propylene, butene-1, pentene-1, 4-methylpentene-1, hexene-1, octene-1, etc., random copolymers made of the α-olefin monomers, block copolymers made of the α-olefin monomers, etc. can also be used.

[0026] In the present invention, the cyclic olefin resin refers to a cyclic olefin resin (hereinafter sometimes referred to as COP) or a cyclic olefin copolymer resin (hereinafter sometimes referred to as COC). The cyclic olefin resin (COP) refers to a resin in which only "repeating units containing a cyclic olefin skeleton in the main chain" (hereinafter sometimes referred to as cyclic olefin units) are polymerized, and the cyclic olefin copolymer resin (COC) refers to a resin in which a cyclic olefin unit and a "repeating unit consisting of an olefin unit not containing a cyclic olefin skeleton in the main chain" (hereinafter sometimes referred to as non-cyclic olefin unit) are copolymerized.

[0027] The cyclic olefins (cyclic olefin units) that make up COP and COC include monocyclic olefins such as cyclobutene, cyclopentene, cycloheptene, cyclooctene, cyclopentadiene, and 1,3-cyclohexadiene, bicyclo[2,2,1]hept-2-ene, 5-methyl-bicyclo[2,2,1]hept-2-ene, and 5,5-dimethyl-bicyclo[2,2,1]hept-2-ene. ene, 5-ethyl-bicyclo[2,2,1]hept-2-ene, 5-butyl-bicyclo[2,2,1]hept-2-ene, 5-ethylidene-bicyclo[2,2,1]hept-2-ene, 5-hexyl-bicyclo[2,2,1]hept-2-ene, 5-octyl-bicyclo[2,2,1]hept-2-ene, 5-octadecyl-bicyclo[2,2,1]hept-2-ene, 5-methylidene- Bicyclic olefins such as bicyclo[2,2,1]hept-2-ene, 5-vinyl-bicyclo[2,2,1]hept-2-ene, 5-propenyl-bicyclo[2,2,1]hept-2-ene, tricyclo[4,3,0,12.5]deca-3,7-diene, tricyclo[4,3,0,12.5]deca-3-ene, tricyclo[4,3,0,12.5]undeca-3,7-diene, tricyclo[4,3,0,12.5]undeca-3,8-diene, or partially hydrogenated versions of these (or adducts of cyclopentadiene and cyclohexene) tricyclic olefins such as 5-cyclopentyl-bicyclo[2,2,1]hept-2-ene, 5-cyclohexyl-bicyclo[2,2,1]hept-2-ene, 5-cyclohexenyl-bicyclo[2,2,1]hept-2-ene, and 5-phenyl-bicyclo[2,2,1]hept-2-ene; tetracyclo[4,4,0,12.5,17.10]dodec-3-ene, 8-methyltetracyclo[4 ,4,0,12.5,17.10]dodec-3-ene, 8-ethyltetracyclo〔4,4,0,12.5,17.10〕dodec-3-ene, 8-methylidenetetracyclo〔4,4,0,12.5,17.10〕dodec-3-ene, 8-ethylidenetetracyclo〔4,4,0,12.5,17.10〕dodec-3-ene, 8-vinyltetracyclo〔4,4,0,12.5,17.10〕dodec-3-ene, 8-propenyl-tetracyclo〔4,4,0,12.tetracyclic olefins such as tetracyclo[4,4,0,12.5,17.10]dodec-3-ene, 8-cyclopentyl-tetracyclo[4,4,0,12.5,17.10]dodec-3-ene, 8-cyclohexyl-tetracyclo[4,4,0,12.5,17.10]dodec-3-ene, 8-cyclohexenyl-tetracyclo[4,4,0,12.5,17.10]dodec-3-ene, 8-phenyl-cyclopentyl-tetracyclo[4,4,0,12.5,17.10]dodec-3-ene, tetracyclo[7,4,13.6,01.9,02.7]tetradec-4,9,11,13-tetraene, and tetracyclo[8,4,14.7,01. Examples of polycyclic olefins include tetramers such as pentacyclo[6,6,13.6,02.7,09.14]-4-hexadecene, pentacyclo[6,5,1,13.6,02.7,09.13]-4-pentadecene, pentacyclo[7,4,0,02.7,13.6,110.13]-4-pentadecene, heptacyclo[8,7,0,12.9,14.7,111.17,03.8,012.16]-5-eicosene, and heptacyclo[8,7,0,12.9,03.8,14.7,012.17,113.16]-14-eicosene. These cyclic olefins can be used alone or in combination of two or more.

[0028] Among the above, from the viewpoints of productivity and surface properties, tricyclic olefins having 10 carbon atoms, such as bicyclo[2,2,1]hept-2-ene (hereinafter sometimes referred to as norbornene), tricyclo[4,3,0,12.5]dec-3-ene (hereinafter sometimes referred to as tricyclodecene), tetracyclic olefins having 12 carbon atoms, such as tetracyclo[4,4,0,12.5,17.10]dodec-3-ene (hereinafter sometimes referred to as tetracyclododecene), cyclopentadiene, 1,3-cyclohexadiene, and the like, are preferably used.

[0029] Examples of methods for producing COPs include known methods such as addition polymerization or ring-opening polymerization of cyclic olefin monomers. Examples of such methods include a method of subjecting norbornene, tricyclodecene, tetracyclododecene, or derivatives thereof to ring-opening metathesis polymerization followed by hydrogenation, a method of subjecting norbornene and its derivatives to addition polymerization, and a method of subjecting cyclopentadiene or cyclohexadiene to 1,2- or 1,4-addition polymerization followed by hydrogenation.

[0030] The non-cyclic olefin (non-cyclic olefin unit) constituting the COC in the present invention may be either one that contains a cyclic olefin skeleton in the side chain or one that does not contain a cyclic olefin skeleton in the side chain, but from the viewpoint of productivity and cost, it is preferable to be a so-called chain olefin (chain olefin unit) that does not contain a cyclic olefin in the side chain.Preferred chain olefins include ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 3-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-hexene, 4,4-dimethyl-1-pentene, 4-ethyl-1-hexene, 3-ethyl-1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, 1-eicosene, etc. Among these, ethylene is particularly preferably used from the viewpoints of productivity and cost.

[0031] Methods for producing COC include known methods such as addition polymerization of cyclic olefin monomers and non-cyclic olefin monomers, and a specific example is a method of addition copolymerization of norbornene or its derivatives with ethylene.

[0032] From the viewpoint of heat resistance, the molar ratio of cyclic olefin units and non-cyclic olefin units in COC in layer A is preferably cyclic olefin units (mol%) / non-cyclic olefin units (mol%)=60 / 40 to 85 / 15, more preferably 65 / 35 to 80 / 20, when all constituent units are taken as 100 mol%. By making the molar ratio of cyclic olefin units in COC 60 mol% or more when all constituent units are taken as 100 mol%, the glass transition temperature is not excessively low and the heat resistance of layer A is improved.

[0033] When COP is used in the A layer, from the viewpoints of productivity and surface properties, the COP in the A layer is particularly preferably a resin obtained by subjecting norbornene, tricyclodecene, tetracyclododecene, or a derivative thereof to ring-opening metathesis polymerization and then hydrogenating it.When COC is used in the A layer, from the same viewpoints, the COC in the A layer is particularly preferably a copolymer of norbornene and ethylene.

[0034] The low polarity resin in the A layer, such as COC or COP, may contain a polar group from the viewpoint of improving adhesion with coating layers such as polarizers and other adhesive layers when the B layer is peeled off and used as an optical film. Examples of the polar group include a carboxyl group, an acid anhydride group, an epoxy group, an amide group, an ester group, and a hydroxyl group. These polar groups in the low polarity resin, such as COC or COP, may be one type or multiple types as long as the effect of the present invention is not impaired. In addition, a method for incorporating a polar group into a low polarity resin, such as COC or COP, may include a method of grafting and / or copolymerizing an unsaturated compound having a polar group. Examples of the unsaturated compound having a polar group include (meth)acrylic acid, maleic acid, maleic anhydride, itaconic anhydride, glycidyl (meth)acrylate, (meth)acrylic acid alkyl (carbon number 1 to 10) ester, maleic acid alkyl (carbon number 1 to 10) ester, (meth)acrylamide, and (meth)acrylic acid-2-hydroxyethyl.

[0035] In addition, when the A layer is mainly composed of a cyclic olefin resin such as COC or COP, the A layer may be composed entirely of a cyclic olefin resin or may contain other resin components. Examples of other resin components include acyclic olefin resins. The acyclic olefin resin refers to a resin in which only acyclic olefin units are polymerized.

[0036] Examples of the acyclic olefin resin include polymers of α-olefin monomers such as ethylene, propylene, butene-1, pentene-1, 4-methylpentene-1, hexene-1, and octene-1, random copolymers of the α-olefin monomers, and block copolymers of the α-olefin monomers. Specific examples include various polyethylene resins such as low-density polyethylene, medium-density polyethylene, high-density polyethylene, linear low-density polyethylene, and ethylene-α-olefin copolymers polymerized using a metallocene catalyst, various polypropylene resins such as polypropylene, ethylene-propylene copolymer, and ethylene-propylene-butene copolymer, and methylpentene polymer. When the A layer contains such an acyclic olefin resin, its brittleness can be reduced.

[0037] Among these non-cyclic olefin resins, various polyethylene resins and various polypropylene resins are preferably used from the viewpoint of compatibility with COC and COP. When layer A contains a polyethylene resin or a polypropylene resin, it is possible to reduce the shear stress in the extrusion process in addition to mitigating brittleness. Therefore, it is also possible to suppress the generation of foreign matter due to crosslinking. The polyethylene resin refers to a polymer in an embodiment in which the total of ethylene-derived components (ethylene units) is 50 mol% or more and 100 mol% or less, more preferably more than 50 mol% and 100 mol% or less, when the total constituent units of the resin are 100 mol%.

[0038] A polystyrene resin is a polymer obtained by polymerizing a styrene monomer. The polystyrene resin in layer A is preferably a styrene polymer having a syndiotactic structure (syndiotactic polystyrene resin, hereinafter sometimes referred to as SPS resin). The syndiotactic structure means a stereochemical structure in which the phenyl groups or substituted phenyl groups, which are side chains, are alternately positioned in the opposite direction to the main chain formed from carbon-carbon bonds. The degree of stereoregularity (tacticity) of an SPS resin can be quantified by a nuclear magnetic resonance method (13C-NMR method) using a carbon isotope. The tacticity of an SPS resin measured by the 13C-NMR method can be indicated by the proportion of chains consisting of several monomer units, for example, dyads in the case of two units, triads in the case of three units, and pentads in the case of five units, in which the configuration of the constituent units is reversed and syndiotactic (racemic dyads, etc.). The SPS resin in the present invention is usually a styrene polymer having a syndiotacticity of 75% or more, preferably 85% or more, in racemic diads, 60% or more, preferably 75% or more, in racemic triads, or 30% or more, preferably 50% or more, in racemic pentads. The types of styrene polymers as SPS resins include polystyrene, poly(alkylstyrene), poly(halogenated styrene), poly(halogenated alkylstyrene), poly(alkoxystyrene), poly(vinyl benzoate ester), hydrogenated polymers thereof, and mixtures thereof, or copolymers containing these as main components. Examples of poly(alkylstyrene) include poly(methylstyrene), poly(ethylstyrene), poly(isopropylstyrene), poly(tertiary butylstyrene), poly(phenylstyrene), poly(vinylnaphthalene), poly(vinylstyrene), etc. Examples of poly(halogenated styrene) include poly(chlorostyrene), poly(bromostyrene), poly(fluorostyrene), etc. Examples of the poly(halogenated alkylstyrene) include poly(chloromethylstyrene), etc. Examples of the poly(alkoxystyrene) include poly(methoxystyrene), poly(ethoxystyrene), etc.

[0039] The polycarbonate resin is a polymer obtained by reacting a dihydroxydiaryl compound with phosgene or a carbonate ester such as diphenyl carbonate. Examples of dihydroxy diaryl compounds used in polycarbonate resins include bis(hydroxyaryl)alkane compounds such as 2,2-bis(4-hydroxyphenyl)propane (commonly known as bisphenol A), bis(4-hydroxyphenyl)methane, 1,1-bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)octane, bis(4-hydroxyphenyl)phenylmethane, 2,2-bis(4-hydroxyphenyl-3-methylphenyl)propane, 1,1-bis(4-hydroxy-3-tert-butylphenyl)propane, 2,2-bis(4-hydroxy-3-bromophenyl)propane, 2,2-bis(4-hydroxy-3,5-dibromophenyl)propane, and 2,2-bis(4-hydroxy-3,5-dichlorophenyl)propane; Examples of the hydroxyl group include, but are not limited to, bis(hydroxyaryl)cycloalkane compounds such as 1,1-bis(4-hydroxyphenyl)cyclopentane and 1,1-bis(4-hydroxyphenyl)cyclohexane, dihydroxydiaryl ether compounds such as 4,4'-dihydroxydiphenyl ether and 4,4'-dihydroxy-3,3'-dimethyldiphenyl ether, dihydroxydiaryl sulfide compounds such as 4,4'-dihydroxydiphenyl sulfide, dihydroxydiaryl sulfoxide compounds such as 4,4'-dihydroxydiphenyl sulfoxide and 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfoxide, and dihydroxydiaryl sulfone compounds such as 4,4'-dihydroxydiphenyl sulfone and 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfone. These may be used alone or in combination as necessary.

[0040] In addition to the above-mentioned dihydroxydiaryl compounds, compounds having three or more phenolic hydroxyl groups may be used in the polycarbonate resin of the present invention, such as phloroglucin, 4,6-dimethyl-2,4,6-tri(4-hydroxyphenyl)-heptene, 2,4,6-dimethyl-2,4,6-tri(4-hydroxyphenyl)-heptane, 1,3,5-tri(4-hydroxyphenyl)-benzene, 1,1,1-tri(4-hydroxyphenyl)-ethane, and 2,2-bis[4,4-(4,4'-dihydroxydiphenyl)-cyclohexyl]-propane.

[0041] The polycarbonate resin of the present invention is preferably a polycarbonate resin in which the dihydroxydiaryl compound is a 2,2-bis(4-hydroxyphenyl)propane (commonly known as bisphenol A) unit as the main constituent unit from the viewpoint of heat resistance and wet heat resistance. The main constituent unit here refers to a constituent unit that occupies 80 mol% or more of 100 mol% of all dihydroxydiaryl units used in the polycarbonate resin. From the above viewpoint, it is more preferable that the bisphenol A unit is 90 mol% or more, and even more preferable that it is 95 mol% or more, out of 100 mol% of all dihydroxydiaryl units. In the present invention, the polycarbonate resin preferably has a number average molecular weight (Mn) of 10,000 or more and 50,000 or less from the viewpoint of melt extrudability. It is more preferable that it is 12,000 or more and 40,000 or less, and even more preferable that it is 15,000 or more and 30,000 or less.

[0042] The acrylic resin refers to a polymer of an acrylic acid ester or a methacrylic acid ester. The acrylic resin in the A layer is preferably a polymer mainly composed of an alkyl methacrylate. Specifically, it may be a homopolymer of an alkyl methacrylate, a copolymer using two or more kinds of alkyl methacrylate, or a copolymer of 50 mol% or more and less than 100 mol% of an alkyl methacrylate and more than 0 mol% and 50 mol% or less of a monomer other than the alkyl methacrylate. As the alkyl methacrylate, one having an alkyl group with 1 to 4 carbon atoms is usually used, and among them, methyl methacrylate is preferably used. In addition, the monomer other than the alkyl methacrylate may be a monofunctional monomer having one polymerizable carbon-carbon double bond in the molecule, or may be a polyfunctional monomer having two or more polymerizable carbon-carbon double bonds in the molecule, but a monofunctional monomer is particularly preferably used. Examples thereof include alkyl acrylates such as methyl acrylate and ethyl acrylate, styrene-based monomers such as styrene and alkylstyrene, and unsaturated nitriles such as acrylonitrile and methacrylonitrile. When an alkyl acrylate is used as a copolymerization component, the alkyl group usually has a carbon number of about 1 to 8. When the total monomers for obtaining the acrylic resin are taken as 100 mol %, the alkyl methacrylate is preferably 70 mol % or more, more preferably 80 mol % or more, further preferably 90 mol % or more, and particularly preferably 99 mol % or less.

[0043] The polyester resin refers to a resin having a structure in which dicarboxylic acid units and diol units are repeatedly linked. Specific examples of polyester resins that can be used for the A layer include polyethylene terephthalate, polyethylene-2,6-naphthalate, polypropylene terephthalate, polybutylene terephthalate, and polylactic acid. The polyester resin may be a homoresin in which both the dicarboxylic acid unit and the diol unit are single, or may be a copolymer in which at least one of the dicarboxylic acid unit and the diol unit is a multiple type in order to enhance amorphousness. Alternatively, it may be a blend of polyester resins in which two or more types are compatible with each other.

[0044] Polyester resins can be obtained by 1) polycondensation of a dicarboxylic acid component or its ester-forming derivative (hereinafter collectively referred to as "dicarboxylic acid component") and a diol component, 2) polycondensation of a compound having a carboxylic acid or carboxylic acid derivative moiety and a hydroxyl group in one molecule, and a combination of 1) and 2). Polymerization of polyester resins can be carried out by a conventional method.

[0045] In 1), examples of the dicarboxylic acid component include aliphatic dicarboxylic acids such as malonic acid, succinic acid, glutaric acid, adipic acid, suberic acid, sebacic acid, dodecanedioic acid, dimer acid, eicosanedioic acid, pimelic acid, azelaic acid, methylmalonic acid, and ethylmalonic acid; alicyclic dicarboxylic acids such as adamantanedicarboxylic acid, norbornenedicarboxylic acid, isosorbide, cyclohexanedicarboxylic acid, and decalindicarboxylic acid; terephthalic acid, isophthalic acid, phthalic acid, 1,4-naphthalenedicarboxylic acid, and 1,5- Representative examples include aromatic dicarboxylic acids such as naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 1,8-naphthalenedicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 4,4'-diphenyletherdicarboxylic acid, 4,4'-diphenylsulfonedicarboxylic acid, 5-sodiumsulfoisophthalic acid, phenylendanedicarboxylic acid, anthracenedicarboxylic acid, phenanthrenedicarboxylic acid, and 9,9'-bis(4-carboxyphenyl)fluorene acid, or ester derivatives thereof. These may be used alone or in combination.

[0046] Representative examples of the diol component include aliphatic diols such as ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,2-butanediol, and 1,3-butanediol, alicyclic diols such as cyclohexanedimethanol, spiroglycol, and isosorbide, and aromatic diols such as bisphenol A, 1,3-benzenedimethanol, 1,4-benzenedimethanol, and 9,9'-bis(4-hydroxyphenyl)fluorene. These may be used alone or in combination as necessary.

[0047] In the present invention, the total light transmittance of the A layer film is preferably 80% or more and 98% or less. When the total light transmittance is in this range, the display on a display or the like becomes brighter and easier to see. In order to set the total light transmittance of the A layer within the above range, it is preferable to use a highly transparent resin, for example, at least one resin selected from the above-mentioned cyclic olefin resins, polystyrene resins, polycarbonate resins, acrylic resins, polyester resins, and polyamide resins.

[0048] From the viewpoint of achieving both heat resistance and mechanical strength, the laminated film of the present invention has a glass transition temperature (Tg A In the present invention, the glass transition temperature (Tg A ) can be measured in accordance with JIS K-7121 (1987 edition) (glass transition temperature (Tg B The same is true for the glass transition temperature (Tg A An example of a method for making the glass transition temperature (Tg) exceed 100°C and not more than 170°C is to use a resin having a glass transition temperature exceeding 100°C and not more than 170°C for layer A. When the glass transition temperature of layer A exceeds 100°C, sufficient heat resistance can be achieved to withstand use at high temperatures. Furthermore, when the glass transition temperature of layer A is 170°C or less, sufficient mechanical strength can be ensured.

[0049] In the laminated film of the present invention, the number of times that the A layer reaches flexure at break is preferably 100 times or more and 10,000 times or less, and more preferably 1,000 times or more and 10,000 times or less. By making the number of times that the A layer reaches flexure at break 100 times or more, the punching processability and repeated bending resistance of the A layer are improved, so that the A layer film can be suitably used for optical applications that require flexibility, such as foldable smartphones. From the above viewpoint, the more the number of times that the A layer reaches flexure at break, the more preferable it is, but increasing the number of times that the A layer reaches flexure at break is accompanied by strong molecular orientation. Therefore, if the number of times that the A layer reaches flexure at break is excessively increased, there is a high possibility that retardation will be impaired, so the upper limit of the number of times that the A layer reaches flexure at break is 10,000 times.

[0050] In the present invention, the bending number of times until the A layer breaks refers to the number of bending times at which the A layer film breaks when a bending test is performed on an A layer film sample cut into a size of 110 mm in length (test direction) and 15 mm in width in accordance with JIS P-8115 (2001 edition) under conditions of a load of 1,000 g, a bending angle of 135° left and right (R: +135°, L: -135°), a bending speed of 175 times / min, and a chuck tip R: 0.38 mm. Note that the test direction at this time is the direction in which the breaking strength is the highest.

[0051] The breaking strength for determining the test direction can be measured as follows: A tensile tester (Orientec Tensilon UCT-100) is used to perform a tensile test under conditions of a temperature of 25°C, 63% Rh, a crosshead speed of 300 mm / min, a width of 10 mm, and a sample length of 50 mm. The strength at which the film sample breaks is read, and the value obtained is taken as the breaking strength (MPa).

[0052] The method of adjusting the number of bending times to break of the layer A to 100 times or more and 10,000 times or less or the above-mentioned preferable range includes, for example, a method of adding a highly flexible resin. As the highly flexible resin, for example, an elastomer can be used, and when the main component of the layer A is a cyclic olefin-based resin, the number of bending times to break can be improved by adding an olefin-based elastomer or the like.

[0053] In the laminate film of the present invention, the surface roughness Ra of one or both sides of the A layer is preferably 1 nm or more and 100 nm or less, more preferably 1 nm or more and 80 nm or less, and even more preferably 1 nm or more and 35 nm or less. By adopting such an embodiment, the A layer film exhibits high smoothness and excellent surface characteristics, and therefore, when used for optical applications such as displays, it is possible to display very high definition images.

[0054] In the present invention, the surface roughness Ra of the A layer can be measured using an AFM (atomic force microscope). The AFM (atomic force microscope) is not particularly limited as long as it is measurable, and for example, a "NanoScope" (registered trademark) V Dimension Icon manufactured by BrukerAXS can be used. The measurement procedure and conditions when using this device are as follows. First, a measurement sample is cut into about 1 cm square, fixed to a silicon wafer with epoxy resin, and pre-treated by dripping silver paste. Then, a silicon cantilever is used as a probe, and the A layer film sample surface is scanned in tapping mode under conditions of a scanning range of 3 μm square and a scanning speed of 0.4 Hz at room temperature (25° C.) in the atmosphere. From the data thus obtained, the three-dimensional average roughness is calculated under a cutoff condition of 3 nm using software (Nanoscope Analysis) attached to the AFM, and this is taken as the surface roughness Ra (nm).

[0055] A method for adjusting the surface roughness Ra of one or both sides of the A layer to 1 nm or more and 100 nm or less or the above-mentioned preferred range can be a method for adjusting the stretching ratio. More specifically, the surface roughness Ra can be controlled to be low by increasing the areal stretching ratio, and from the viewpoint of easily adjusting the surface roughness Ra to a desired range, the stretching ratio is preferably 5 times or more, particularly preferably 9 times or more, calculated as the areal stretching ratio.

[0056] The thickness of Layer A in the laminated film of the present invention is not particularly limited as long as it does not impair the effects of the present invention. From the viewpoint of handleability, however, the thickness is preferably 1 μm or more and 100 μm or less, more preferably 5 μm or more and 80 μm or less, and even more preferably 10 μm or more and 50 μm or less.

[0057] From the viewpoint of realizing a degree of heat resistance sufficient to reduce misalignment and wrinkles when used as an A layer film for optical purposes, the A layer in the laminate film of the present invention preferably has a heat shrinkage rate of −1.0% or more and 1.0% or less at 100° C. An example of a method for adjusting the heat shrinkage rate at 100° C. to the above range is to set the glass transition temperature of the A layer to 110° C. or more.

[0058] In the laminated film of the present invention, it is important that the plane orientation coefficient of the B layer is 0.0300 or more and 0.1700 or less from the viewpoint of making the B layer function as a protective layer. By adopting such an embodiment, the crystallization and orientation of the B layer are sufficiently promoted, and the B layer plays the role of a protective layer. "The plane orientation coefficient of the B layer is 0.0300 or more and 0.1700 or less" means that the plane orientation coefficient of at least one B layer is 0.0300 or more and 0.1700 or less, and more preferably, the plane orientation coefficient of the B layers on both sides of the A layer is 0.0300 or more and 0.1700 or less. Hereinafter, unless otherwise specified, the parameters related to the B layer can be interpreted in the same way. If the plane orientation coefficient of the B layer is less than 0.0300, the film surface is easily scratched, and the protective properties of the laminated film are poor. In addition, if the resin used for the B layer is a resin, it is difficult to make the plane orientation coefficient larger than 0.1700 from the viewpoint of resin properties and technology, so this is set as the upper limit.

[0059] The plane orientation coefficient of layer B can be measured by the following method. First, the refractive indexes in the longitudinal direction, width direction, and thickness direction (nMD, nTD, and nZD, respectively) are determined using an Abbe refractometer at 25° C. using sodium D line (wavelength 589 nm) as a light source and methylene iodide as a mounting liquid. Then, the plane orientation coefficient (fn) is calculated from the determined refractive indexes using the following formula (2). fn=(nMD+nTD) / 2-nZD ···(2).

[0060] As a method for making the plane orientation coefficient fall within the above range, for example, a method of using a crystalline resin as the resin constituting layer B and stretching it can be mentioned. Specific examples of the crystalline resin constituting layer B include polyester resins such as polyethylene terephthalate, polyethylene-2,6-naphthalate, polypropylene terephthalate, polybutylene terephthalate, and polylactic acid, polyamide resins such as nylon 6, and olefin resins such as polypropylene. In addition, the plane orientation coefficient of layer B can usually be increased by increasing the stretching ratio.

[0061] If a polyester resin or a polyamide resin is used as the crystalline resin constituting the B layer, it is preferable to stretch the resin by an area ratio of 3 to 16 in order to set the plane orientation coefficient to 0.0300 to 0.1700. If polypropylene is used as the crystalline resin constituting the B layer, it is preferable to stretch the resin by an area ratio of 10 to 36 in order to set the plane orientation coefficient to 0.0300 to 0.1700.

[0062] In the laminated film of the present invention, from the viewpoint of improving the function of the B layer as a protective layer, it is preferable that the in-plane refractive index of the B layer is 1.6000 or more and 1.6600 or less, and the thickness direction refractive index of the B layer is 1.4800 or more and 1.5700 or less. Here, "the in-plane refractive index of the B layer is 1.6000 or more and 1.6600 or less" means that the refractive indexes in the longitudinal direction and the width direction (nMD, nTD) measured by the above-mentioned method are both 1.6000 or more and 1.6600 or less, and the thickness direction refractive index of the B layer means the refractive index in the thickness direction (nZD) measured by the above-mentioned method. By adopting such an embodiment, the orientation and crystallization of the B layer are promoted, and the function of the B layer as a protective layer is improved.

[0063] An example of a method for adjusting nMD and nTD of layer B to 1.6000 or more and 1.6600 or less, and nZD to 1.4800 or more and 1.5700 or less, is a method for producing a laminated film by biaxial stretching.

[0064] In order to set the refractive index in each direction within the above range, if the above-mentioned polyester resin or polyamide resin is used as the resin constituting the B layer, it is preferable to stretch the film by an area ratio of 5 to 16 times. If polypropylene is used as the crystalline resin constituting the B layer, it is preferable to stretch the film by an area ratio of 10 to 36 times. Alternatively, the refractive index in each direction can be increased by heat treatment after stretching.

[0065] In the laminated film of the present invention, the thickness of the B layer is not particularly limited, but is preferably 1 μm or more from the viewpoint of its function as a protective layer, and is preferably 100 μm or less from the viewpoint of handling. From the above viewpoints, it is preferably 2 μm or more and 50 μm or less, and more preferably 5 μm or more and 25 μm or less. The thickness of the B layer on both sides may be the same or different.

[0066] In the laminated film of the present invention, from the viewpoint of the mechanical strength and dimensional stability of the B layer, it is preferable that the B layer has a small endothermic peak temperature (Tmeta) of 120°C or more and 220°C or less. The peak indicates the thermal history in the manufacturing process, and indicates the temperature in the heat treatment process after the biaxial stretching. By adopting such an embodiment, the B layer is crystallized without melting, and the properties such as mechanical strength and dimensional stability are improved, so that the function of the B layer as a protective layer is improved. Furthermore, when the main component of the A layer is a crystalline resin, the retardation of the A layer can also be reduced. From the above viewpoint, it is preferable that the B layer has a small endothermic peak temperature (Tmeta) of 120°C or more and 220°C or less, and is a melting point Tm-80°C or more and a melting point Tm-5°C or less.

[0067] The Tmeta of layer B can be determined from the heating crystallization peak temperature Tcc (°C) and melting point Tm (°C) of layer B, measured according to the method of JIS K-7121 (1987 edition). Specifically, a 5 mg sample of the layer alone is heated from 25°C to 300°C at 20°C / min. The temperature at the top of the exothermic peak obtained from the DSC curve is taken as Tcc, the temperature at the top of the endothermic peak is taken as the melting point Tm, and the minute endothermic peak seen at the midpoint between Tm and Tcc is taken as Tmeta (°C). Note that ΔTcg, which will be described later, is the temperature at the time from Tcc to Tg B The value is taken as the subtraction value.

[0068] In the laminated film of the present invention, from the viewpoint of suppressing stretching unevenness, the crystallinity parameter (ΔTcg) of the B layer is preferably 10° C. or more and 100° C. or less. The laminated film of the present invention can be suitably produced, for example, by laminating a composition for obtaining an A layer and a composition for obtaining a B layer, cooling and solidifying them, and co-stretching them. When using this method, when a laminate having a layer structure in which an intermediate layer is sandwiched between the same outer layers, such as the laminated film of the present invention, is stretched to form a laminated film, it is usually preferable to set the glass transition temperature of at least the B layer to be equal to or higher than the glass transition temperature of the A layer, from the viewpoint of suppressing lateral unevenness due to adhesion, etc., and stretching unevenness due to a temperature excessively high relative to the glass transition temperature of the B layer. However, in the laminated film of the present invention, it is preferable to use resins with different crystallinity and SP values ​​in the A layer and the B layer, so that the design is inevitably prone to differences in glass transition temperature between the A layer and the B layer, and the degree of freedom in resin selection is low. In view of this, in the laminated film of the present invention, by setting the crystallinity parameter ΔTcg of layer B in the above range, crystallization is promoted in the casting process after extrusion from the T-die, thereby preventing adhesion in the stretching process and suppressing stretching unevenness due to excessive temperature. Therefore, deterioration of quality caused by thickness unevenness and orientation unevenness in particular is suppressed. From the above viewpoint, the crystallinity parameter ΔTcg of layer B is preferably 20°C or more and 70°C or less, more preferably 20°C or more and 60°C or less.

[0069] In the laminated film of the present invention, the crystal melting energy ΔHm of the B layer Bis preferably 15.0 J / g or more and 50.0 J / g or less. B When ΔHm is in the above range, the surface hardness of the layer B is high, and high protective performance can be achieved. B An example of a method for making the crystal melting energy within the above range is to use a resin having a crystal melting energy of 15.0 J / g or more and 50.0 J / g or less as the dendrite constituting layer B.

[0070] In the laminated film of the present invention, in order to improve the film formation stability and reduce the unevenness of stretching, the glass transition temperature (Tg B ) is preferably 30°C or higher and 100°C or lower. Controlling the crystallinity parameter (ΔTcg) of layer B within the above range is also preferable for preventing adhesion, but by bringing the glass transition temperatures of layers A and B closer to each other, film formation stability can be further improved and stretching unevenness can be suppressed. From the above viewpoint, therefore, the glass transition temperature of layer B is preferably 30°C or higher and 100°C or lower.

[0071] In the laminated film of the present invention, it is preferable that the B layer is mainly composed of a crystalline resin. Examples of the crystalline resin include an olefin resin, a polyamide resin, and a polyester resin. In the laminated film of the present invention, it is preferable that the crystalline resin is a polyester resin from the viewpoint of versatility and biaxial stretchability. As the olefin resin, the polyamide resin, and the polyester resin, the above-mentioned resins having crystallinity can be used.

[0072] In the laminated film of the present invention, the B layers located on both surface layers may have different compositions as long as the effects of the present invention are not impaired. The main roles of the B layer in the laminated film of the present invention are to protect the A layer and to impart handleability by thickening the B layer, but, for example, one of the B layers may serve as a base layer to improve handleability, and the other B layer may peel off from the A layer and transfer to another material. For the latter B layer in this embodiment, for example, the resins listed above as constituting the B layer may be used alone or in appropriate combination as long as they satisfy the requirements of the present invention.

[0073] The laminated film of the present invention preferably has a haze of 0.5% or more and 3.0% or less from the viewpoint of brightening the display when used in a display or the like. In the present invention, the haze can be measured based on JIS K-7136 (2000 edition). As a means for making the haze of the laminated film within the above range, a method of using a highly transparent resin in the laminated film (particularly the A layer) can be mentioned. Examples of such resins include polyolefin resins, polyimide resins, polyether ether ketone resins, polypropylene resins, cyclic olefin resins, polystyrene resins, polycarbonate resins, acrylic resins, polyester resins, polyamide resins, cellulose resins, etc. Among them, from the viewpoint of colorless transparency and versatility, it is preferable to use at least one resin selected from polypropylene resins, cyclic olefin resins, polystyrene resins, polycarbonate resins, acrylic resins, polyester resins, and polyamide resins.

[0074] The method for producing the laminated film of the present invention will be described below. The method for producing the laminated film of the present invention includes a co-extrusion lamination step of co-extruding and laminating the molten resin composition A and the molten resin composition B, the casting step of cooling and solidifying the laminate obtained by the co-extrusion lamination step, the stretching step of stretching the sheet obtained by the casting step in at least one direction, and the Tg A Tg over +20℃ A The method is characterized by having, in this order, a heat treatment step of performing heat treatment at a temperature of +120° C. or less.

[0075] In the method for producing the laminated film of the present invention, from the viewpoint of improving lamination accuracy, it is preferable to have a width-widening step of individually widening the molten resin composition A and the molten resin composition B upstream of the co-extrusion lamination step. In the method for producing the laminated film of the present invention, since the molten resin composition A and the molten resin composition B are usually mainly composed of resins with different melt viscosities and SP values, when the molten resin compositions are joined together and then the laminated resin is widened in the same manifold, lamination disturbance (also called flow marks) may occur due to differences in melt viscosity, melt tension, and SP value. For this reason, it is preferable to widen each molten resin composition individually before laminating. To widen each molten resin composition individually, for example, a multi-manifold die can be used.

[0076] It is important that the method for producing the film of the present invention has a co-extrusion lamination step in which the molten resin composition A and the molten resin composition B are co-extruded and laminated when the molten resin composition for obtaining the A layer is the molten resin composition A and the molten resin composition for obtaining the B layer is the molten resin composition B. By adopting such an embodiment, the B layer which becomes the protective layer and the A layer which becomes the optical low retardation layer can be formed at once. The molten resin composition A is preferably mainly composed of an amorphous resin, and the molten resin composition B is preferably mainly composed of a crystalline resin. The resins which can be suitably used for the molten resin compositions A and B are the same as those described above as those which can be suitably used in each layer of the laminate film of the present invention.

[0077] As long as the molten resin composition A and the molten resin composition B are co-extruded and laminated, the lamination structure is not important, but when it is required to have layer B as a protective layer on both sides, it is preferable to laminate the molten resin composition B on both sides of the molten resin composition A. In this embodiment, the compositions of the molten resin compositions B located on each side of the molten resin composition A may be the same or different.

[0078] It is important that the manufacturing method of the laminated film of the present invention has a casting process in which the laminate obtained by the coextrusion lamination process is cooled and solidified. In the casting process, from the viewpoint of reducing roll adhesion and stretching unevenness, it is preferable to control the crystallinity of the B layer to 10% or more and 30% or less. As a method for controlling the crystallinity of the B layer to 10% or more and 30% or less, for example, a method of adjusting the casting temperature (temperature of the casting drum) can be mentioned. More specifically, it is preferable to set the casting temperature to be not less than the glass transition temperature of the resin constituting the B layer minus 50°C or more and not more than the glass transition temperature of the resin constituting the B layer. At this time, by setting the casting temperature higher than the glass transition temperature, the crystallinity of the B layer can be increased, and by setting the temperature at the crystallization peak temperature (Tcc°C) of the B layer, crystallization is most likely to occur. By setting the crystallinity of the B layer within the above range, roll adhesion and stretching unevenness can be suppressed even if the glass transition temperature of the B layer is lower than the glass transition temperature of the A layer.

[0079] It is important that the laminated film manufacturing method of the present invention has a stretching step in which the sheet obtained by the casting step is stretched in at least one direction. Usually, when a resin with low crystallinity is used as the A layer, which is a low retardation layer, the dimensional stability is significantly reduced by stretching, so stretching of an amorphous resin is rarely adopted. However, in the present invention, in consideration of the dimensional stability, which is an issue when stretching an amorphous resin, the glass transition temperature Tg of the A layer is set in a state where the B layer, which is a protective layer, is disposed on both sides. AThe film is stretched at a temperature much higher than the temperature at which the film is stretched. This process not only maintains the dimensional stability of the laminated film, but also reduces surface roughness, improves the uniformity of the physical properties by improving the in-plane uniformity, and facilitates the widening and thinning of the film. At this time, the stretching may be performed in at least one direction, and in the case of biaxial stretching, although there is no particular limitation, sequential biaxial stretching, simultaneous biaxial stretching, and inflation methods can be used. The stretching ratio and temperature in each direction during stretching can be appropriately set depending on the type of resin of each composition, but for example, when the main component of the molten resin composition A is a cyclic olefin and the main component of the molten resin composition B is a crystalline polyester resin, the stretching temperature is preferably 100°C or higher and 160°C or lower, 3 times or higher and 16 times or lower, and more preferably 5 times or higher and 16 times or lower.

[0080] The method for producing the laminated film of the present invention is to determine the glass transition temperature (Tg A Tg over +20℃ A It is important to have a heat treatment step in which heat treatment is performed at a temperature of +120°C or less. In this heat treatment step, the protective function is improved by the progression of orientation crystallization of the B layer, while the orientation relaxation of the A layer is promoted, thereby simultaneously realizing improvement in thermal dimensional stability and reduction in retardation value. The device used in the heat treatment step is not particularly limited, and a known device such as a tenter device can be used.

[0081] The laminated film thus obtained is then cooled during the subsequent transport process, and is once wound up into an intermediate roll on a wide winding machine, after which it is cut to the required width and length by a slitter to become the final product.

[0082] The method for manufacturing the laminated film of the present invention not only allows the formation of layer B, which serves as a protective layer, and layer A, which serves as an optical low retardation layer, in one go, but also improves the quality of layer A while maintaining its low retardation properties, and enhances the function of layer B as a protective layer through oriented crystallization.

[0083] Since the laminated film of the present invention is a low retardation film (A layer film) with an easily peelable protective layer (B layer), the protective layer can be peeled off and the film can be suitably used as various optical films such as a polarizer protective film, a protective film for defect inspection, and a transparent conductive film. EXAMPLES

[0084] The present invention will be described below with reference to examples, but the present invention is not limited to these examples. The various properties were measured by the following methods. In each example and comparative example, the layer structure is B1 layer / A layer / B2 layer, regardless of whether the two outermost layers are the same or different, but in the description of the measurement method and evaluation method of each item, the B1 layer and the B2 layer are not distinguished and are referred to as B layer.

[0085] (1) Laminated film and thickness of each layer The total thickness of the laminated film was measured by measuring the thickness of five arbitrary positions of a sample cut out from the film using a dial gauge and calculating the average value. In addition, when measuring the thickness of each layer of the laminated film, a metallurgical microscope Leica DMLM manufactured by Leica Microsystems was used to observe the cross section of the film at a magnification of 100 times, photograph the transmitted light, and measure the thickness of five arbitrary positions for each layer using the length measuring function of the microscope, and then the average value was calculated to be the layer thickness of each layer.

[0086] (2) Glass transition temperature (Tg A , Tg B ), heating crystallization peak temperature Tcc, melting point Tm, minute endothermic peak temperature Tmeta, ΔTcg, crystal melting energy ΔHm In accordance with JIS K7121 (1999), the glass transition temperature (Tg A , Tg B) [℃], heating crystallization peak temperature Tcc [℃], melting point Tm [℃], minute endothermic peak temperature Tmeta [℃] were measured and analyzed in accordance with JIS K-7121 (1987 edition), and crystal melting energy ΔHm [J / g] was measured and analyzed in accordance with JIS K-7122 (1987 edition). Note that ΔTcg in layer B is calculated by the time from Tcc to Tg B The value was obtained by subtracting the value of the temperature at which the heat was generated. The measurements of each item were carried out individually by peeling off layers A and B from the laminated film. Specifically, 5 mg of a sample of each peeled off layer was heated from 25°C to 300°C at 20°C / min, and the temperature at the top of the exothermic peak obtained from the DSC curve was taken as Tcc, the temperature at the top of the endothermic peak obtained from the DSC curve was taken as the melting point Tm, and the small endothermic peak observed at the midpoint between Tm and Tcc was taken as Tmeta. If no melting point was observed, it was recorded as "ND". In addition, for the measurement of crystalline raw materials, in order to remove the influence of crystallization during pelletizing, the sample was heated from 25°C to 300°C at 20°C / min, and then held at 300°C for 5 minutes, and then rapidly cooled by taking out the sample under a 25°C atmosphere to make it amorphous. After storing at 25°C for 5 minutes, the sample was heated from 25°C to 300°C at 20°C / min for the second run. The temperature at the peak of the exothermic peak was taken as the temperature-rise crystallization temperature (Tcc) of the second run. When there were multiple temperature-rise crystallization peaks or crystal melting peaks, the temperature with the largest absolute value of the heat was used.

[0087] (3) Quality of A-layer film Layer A was peeled off from layer B, and the film was cut to a size of 10 cm x 10 cm and attached to a black backing. The condition of the film was then observed under a fluorescent lamp and evaluated according to the following criteria. A: No gel-like foreign matter, wavy unevenness, or streaks were visually observed on the film. B: Gel-like foreign matter, wavy unevenness, and streaks were visually observed on the film.

[0088] (4) Retardation The retardation value was determined by measuring the phase difference for light with a wavelength of 548.3 nm using an automatic birefringence meter (KOBRA-21ADH) manufactured by Oji Measurement Co., Ltd. The measurement was performed once on a single film consisting of only layer A with layers B on both sides peeled off.

[0089] (5) Interlaminar peel strength between layers A and B The peel strength measured according to JIS K 6854-2 (1999 edition) at 180° was used. The A and B layers were peeled on one side, and peeled on the side where the B and A layers were bonded and on the side of the B layer alone. The width of the test piece for the peel strength test was 50 mm, the tensile test speed was 50 mm / min, and measurements were taken at three different locations. The average of the measured values ​​was taken as the interlayer peel strength.

[0090] (6) Solubility parameter SP value (SP A ,SP B ) In the present invention, the Fedors calculation method was used, which allows for relatively simple calculations based on molecular structural formulas. In the Fedors calculation method, it is considered that the solubility changes depending on the molecular cohesive energy density and molar volume depending on the type and number of substituents, and the solubility parameter value δ (cal / cm) is calculated according to the following formula (1). 3 ) 1 / 2 is estimated, where E coh (cal / mol) is the cohesive energy and V is the molar volume (cm 3 / mol).

[0091]

number

[0092] The solubility parameter SP value of a thermoplastic resin can be estimated using Fedor's formula based on the repeating structural units of the molecular chain, so the solubility parameter SP value of a thermoplastic resin containing structural units derived from copolymer components was calculated based on the ratio of each structural unit. The solubility parameter SP value was calculated by rounding off the estimated value calculated based on Fedor's formula to one decimal place. The solubility parameter SP values ​​of representative thermoplastic resins are as follows: polyethylene: 8.0 (cal / cm 3 ) 1 / 2 , Polyethylene terephthalate: 10.7 (cal / cm 3 ) 1 / 2 , polystyrene: 9.4 (cal / cm 3 ) 1 / 2 , polymethyl methacrylate: 9.3 (cal / cm 3 ) 1 / 2 , Polybutylene terephthalate: 10.0 (cal / cm 3 ) 1 / 2 , Nylon 6: 12.7 (cal / cm 3 ) 1 / 2 , Polycarbonate: 9.9 (cal / cm 3 ) 1 / 2 , COP: 8.6 (cal / cm 3 ) 1 / 2 , COC: 7.8 (cal / cm 3 ) 1 / 2 , ABS resin: 10.0 (cal / cm 3 ) 1 / 2 , Polypropylene: 8.0 (cal / cm 3 ) 1 / 2 When multiple components are included, the mass ratio of each component is multiplied by the SP value of each component, and the sum of the multiplied values ​​is regarded as the SP value of the multiple components.

[0093] (7) Total light transmittance, haze Measurements were made according to JIS K-7136 (2000 edition) using a direct-reading haze computer manufactured by Suga Test Instruments Co., Ltd. Each measurement was carried out three times, and the average value was used as the haze of the laminated film.

[0094] (8) Number of times until breakage occurs The layers B on both sides were peeled off from the laminated film to obtain a film consisting of layer A alone. The breaking strength of the film consisting of layer A alone was measured in one arbitrary direction (0°) and in each direction rotated 15°, 30°, 45°, 60°, 75°, 90°, 105°, 120°, 135°, 150°, and 165° to the right parallel to the film surface from the arbitrary direction, and the direction with the highest breaking strength was determined as the test direction, and a film sample was cut into a rectangle of 110 mm (test direction) x 15 mm width. Then, a MIT folding endurance tester (No. 702 manufactured by Mize Co., Ltd.) was used to perform a bending test on the film sample in accordance with JIS P-8115 (2001 edition) at a load of 1,000 g, a bending angle of 135° left and right (R: +135°, L: -135°), a bending speed of 175 times / min, and a chuck tip R: 0.38 mm. The number of times the film sample was bent at the time it broke was taken as the number of times it broke. The test was performed three times, and the average value was used.

[0095] The breaking strength was measured as follows. A tensile test was performed using a tensile tester (Orientec Tensilon UCT-100) under the conditions of temperature 25°C, 63% Rh, crosshead speed 300 mm / min, width 10 mm, and sample length 50 mm, and the value obtained by reading the strength when the film sample broke was taken as the breaking strength. The same measurement was performed five times, and the average value was taken as the breaking strength (MPa) of the film sample.

[0096] (9) Flexibility Based on the number of bending times until breakage measured by the method in (8), the test specimen was judged as follows. The evaluation results were as follows: ⊚ and ◯ were considered to be acceptable. ◎: The number of bending cycles until fracture was 1,000 or more. ◯: The number of times the specimen broke after bending was 100 or more but less than 1,000. ×: The number of bending cycles until fracture was less than 100.

[0097] (10) Surface roughness Ra The B layers on both sides were peeled off from the laminated film to obtain a film consisting of the A layer alone. The surface roughness Ra of the film consisting of the A layer alone was measured using a BrukerAXS AFM (atomic force microscope) "NanoScope" (registered trademark) V Dimension Icon in the following procedure. First, the measurement sample was cut into about 1 cm square, fixed to a silicon wafer with epoxy resin, and pretreated by dripping silver paste. After that, a silicon cantilever was applied as a probe, and the surface of the film sample consisting of the A layer alone was scanned in tapping mode at room temperature (25 ° C.) and in the atmosphere under the conditions of a scanning range of 3 μm square and a scanning speed of 0.4 Hz. From the data obtained in this way, the three-dimensional average roughness was calculated under the cutoff condition of 3 nm using the software (Nanoscope Analysis Ver. 8.15) attached to the AFM. The same measurement was performed five times, and the average value of the obtained three-dimensional average roughness was calculated, which was taken as Ra (nm).

[0098] (11) Refractive index, plane orientation coefficient fn Using sodium D line (wavelength 589 nm) as a light source and methylene iodide as a mounting liquid, the refractive indices in the longitudinal, transverse and thickness directions of the film (nMD, nTD and nZD, respectively) were determined using an Abbe refractometer at 25° C. The plane orientation coefficient (fn) of layer B was calculated from the determined refractive indices using the following formula (2). fn = (nMD + nTD) / 2 - nZD (2) (12) Film formation stability The film was formed for one hour, and the case where no trouble such as film breakage occurred was evaluated as ◯ (pass), and the case where the trouble occurred was evaluated as × (fail).

[0099] (13) Rainbow unevenness A test piece was prepared by laminating a 10 cm square film made of the A layer alone on one side of a polarizer with a polarization degree of 99.9% prepared by adsorbing and orienting iodine in PVA. A laminator roll set at 85°C was used for lamination. The prepared test piece and a polarizing plate without a film were overlapped in a cross-Nicol arrangement and placed on an LED light source (Tritech A3-101). The visibility was confirmed from an angle of 50° to the normal direction of the test piece plane and evaluated according to the following criteria. In the same manner, a test piece was also prepared by laminating a 30 cm square film made of the A layer alone, and the same evaluation was performed. The evaluation results were S to C, which were considered to be acceptable. S: No interference colors were observed in either the 10cm square or the 30cm square evaluations. A: No interference color was observed in the evaluation of a 10 cm square area, and slight interference color was observed in the evaluation of a 30 cm square area. B: Slight interference colors were observed in both the 10cm square and 30cm square evaluations. C: Slight interference color was observed in the evaluation of a 10 cm square area, and interference color was clearly observed in the evaluation of a 30 cm square area. D: Interference colors were clearly observed in both the 10 cm square and 30 cm square evaluations. (14) Peelability The interlaminar peel strength between layers A and B measured by the method described in (5) was evaluated according to the following criteria. The evaluation results were evaluated as ⊚ and ◯. ◎: The interlayer peel strength between layers A and B was 2.0 g / 50 mm or more and 50 g / 50 mm or less. ◯: The interlayer peel strength between layer A and layer B was 1.0 g / 50 mm or more and less than 2.0 g / mm, or more than 50 g / 50 mm and 100 g / 50 mm or less. ×: Did not fall into either category of ◎ or ○.

[0100] (15) Heat resistance A 100 mm square film consisting of Layer A alone was hung in a tree shape in a hot air oven at 100°C so as not to come into contact with the top, bottom, left and right walls, and stored for 12 hours for heat treatment, after which the flatness of the film was visually evaluated according to the following criteria. ◎: No change from before heat treatment. ◯: The film was slightly wavy and wrinkled, but not at a level that caused any problems. ×: Problematic waviness and wrinkles occurred in the film.

[0101] (16) Brittleness A 300 mm wide, 200 m long laminated film (wound on a 6 inch, 350 mm long core) was prepared and rewound around a 3 inch, 350 mm long core under the conditions below. The conveying speed and tension were changed and evaluated according to the following criteria. A: No tears occurred even when rewinding at a speed of 10 m / min and a conveying tension of 70 N / m. B: No tears occurred when rewinding at a speed of 5 m / min and a conveying tension of 50 N / m, but tears occurred when the speed was changed to 10 m / min and the conveying tension to 70 N / m. C: When rewinding at a speed of 5 m / min and a conveying tension of 50 N / m, tears occurred.

[0102] (17)Heat shrinkage rate at 100℃ A film consisting of Layer A alone was cut into a rectangular sample measuring 150 mm long and 10 mm wide in both the longitudinal and transverse directions. Marked lines were drawn on the sample at intervals of 100 mm (50 mm from the center to both ends), and the sample was heat-treated by hanging a 3 g weight and placing it in a hot air oven heated to 100°C for 30 minutes. The distance between the marks after heat treatment was measured, and the thermal shrinkage was calculated from the change in the distance between the marks before and after heating using the following formula (3).

[0103] Heat shrinkage rate (%) = {(gauge length before heat treatment) – (gauge length after heat treatment)} / (gauge length before heat treatment) × 100 (3).

[0104] (18)Protection First, the laminate film was rubbed under the following conditions using a rubbing tester. Next, after rubbing, both B layers were peeled off from the laminate film, and the appearance of the A layer alone was visually inspected. If no scratches were found, it was rated as ⊚ (pass), if slight scratches were found but no practical problem was found, it was rated as ○ (pass), and if obvious scratches were found, it was rated as × (fail). <Rubbing conditions> Evaluation environment conditions: 25℃, 60% RH Rubbing material: Steel wool (manufactured by Japan Steel Wool Co., Ltd., grade No. 0000), wrapped around the rubbing tip (1 cm x 1 cm) of the tester that comes into contact with the sample and fixed with a band. Travel distance (one way): 13cm Scrub speed: 13cm / sec Load: 500g / cm 2 Tip contact area: 1cm x 1cm Number of rubs: 10 times back and forth (20 times).

[0105] [Resins, additives] The following resins and additives were used in the following examples and comparative examples. Note that, regarding the resins, polyethylene A, polyester C, polyester D, polyester E, polyamide resin A, and polypropylene A are crystalline resins, and the other resins are amorphous resins. (Polystyrene A) Polystyrene resin obtained by polymerizing styrene monomer. MFR 9.0g / 10min at 230℃ (Acrylic resin A) Polymethyl methacrylate resin obtained by polymerizing methyl methacrylate. MFR 5.0g / 10min at 230℃ (Polycarbonate resin A) Polycarbonate resin obtained by polycondensation of bisphenol A and phosgene. MVR 12cm at 300℃ 3 / 10min (Cyclic Olefin Resin A (COP-A)) Cyclic olefin polymer (glass transition temperature Tg = 115°C) obtained by polymerizing ethylene with a polymer obtained by ring-opening polymerization of a cyclic olefin monomer. (Cyclic Olefin Copolymer Resin A (COC-A)) A resin obtained by dry blending 60 mass% of ethylene-norbornene copolymer resin A (norbornene unit content: approximately 76 mol%; glass transition temperature Tg = 140°C) and 40 mass% of ethylene-norbornene copolymer resin B (norbornene unit content: 65 mol%; glass transition temperature Tg = 80°C). (Polyethylene A) LLDPE obtained by polymerizing ethylene. MFR 8.0g / 10min at 190℃ (Polyester A) A polyester resin (intrinsic viscosity 0.72) having, as dicarboxylic acid units, 100 mol % of terephthalic acid units, as glycol units, 21 mol % of ethylene glycol units, 46 mol % of 1,4-cyclohexylene dimethanol units, and 33 mol % of isosorbide units. (Polyester B) Spiroglycol 30 mol% copolymerized polyethylene terephthalate (intrinsic viscosity 0.65). (Polyester C) A polyethylene terephthalate resin (intrinsic viscosity 0.65) having 100 mol % terephthalic acid units as dicarboxylic acid units and 100 mol % ethylene glycol units as glycol units. (Polyester D) Polybutylene terephthalate resin (intrinsic viscosity 1.40) containing 100 mol % terephthalic acid units as dicarboxylic acid units and 100 mol % 1-4 butanediol units as glycol units. (Polyester E) An isophthalic acid copolymerized polyethylene terephthalate resin (intrinsic viscosity 0.70) containing 88 mol % terephthalic acid units and 12 mol % isophthalic acid units as dicarboxylic acid units, and containing 100 mol % ethylene glycol units as glycol units. (Polyester F) A polyethylene terephthalate resin (intrinsic viscosity 0.70) copolymerized with 2,6-naphthalenedicarboxylic acid as the dicarboxylic acid component, polyethylene glycol (average molecular weight 400, m×n is 10 or more) as the diol component at 6 mol% of the total diol component, and ethylene glycol at 94 mol% of the total diol component. (Polyester G) An isophthalic acid copolymerized polyethylene terephthalate resin (intrinsic viscosity 0.70) containing 83 mol % terephthalic acid units and 17 mol % isophthalic acid units as dicarboxylic acid units, and containing 100 mol % ethylene glycol units as glycol units. (Polyester H) A polyester resin (intrinsic viscosity 0.72) containing 95 mol % of terephthalic acid units and 5 mol % of isophthalic acid units as dicarboxylic acid units, and 100 mol % of 1,4-cyclohexylene dimethanol units as glycol units. (Polyamide resin A) Toray Industries, Inc.'s nylon resin "Amilan" (registered trademark) CM1017. (Polypropylene A) Homopolypropylene obtained by polymerizing propylene. MFR 7.0g / 10min at 230℃. (Polypropylene B) Ethylene-propylene copolymer polypropylene resin with 9 mol% ethylene copolymerized. MFR 8.0g / 10min at 230℃. (Particle Master A) Particle master (intrinsic viscosity 0.62) containing wet silica particles with an average particle size of 1.2 μm at a particle concentration of 2 mass% in polyester C. (Particle Master B) Particle master (intrinsic viscosity 1.20) containing wet silica particles with an average particle size of 1.2 μm at a particle concentration of 2 mass% in polyester D. (Particle Master C) Particle master (intrinsic viscosity 0.68) containing wet silica particles with an average particle size of 1.2 μm at a particle concentration of 2 mass% in polyester F.

[0106] (Examples 1 to 15, Comparative Examples 1 to 5) A three-layer structure of B1 layer / A layer / B2 layer was used. The raw material composition of each layer was as shown in Table 1, and each was fed to a separate single-screw extruder (L / D=28) and melted at the temperature listed in Table 2, and then passed through a leaf disk filter with a filtration accuracy of 30 μm. After that, the layers were laminated in a feed block installed above the die to form B1 layer / A layer / B2 layer (see table for lamination thickness ratio), and then extruded in a sheet form from a T-die (lip gap: 0.4 mm) onto a mirror-finished cast roll (surface roughness 0.2s) controlled at the temperature listed in Table 2. At that time, the casting position was set at 10° forward from the top of the cast roll, and electrostatic was applied using a wire-shaped electrode with a diameter of 0.1 mm to adhere the B1 layer side to the cast roll, thereby obtaining a cast film. Thereafter, the film was stretched in the longitudinal direction and the transverse direction at the stretching temperature, stretching ratio, and stretching method listed in Table 2, and finally heat-treated at the temperature listed in Table 2 to obtain a laminated film. Evaluations were performed on each item for the obtained laminated film or each layer obtained by peeling it off. The evaluation results are shown in Tables 3 to 8. Note that for Comparative Example 1, the film was melted and broken during the heat treatment step, making it impossible to collect the film, and therefore evaluation of each item was not performed. (Examples 16 to 22) The film had a three-layer structure of B1 layer / A layer / B2 layer. The raw material composition of each layer was as shown in Table 1, and each layer was fed to a separate single-screw extruder (L / D=28) and melted at the temperature shown in Table 2, and then passed through a leaf disk filter with a filtration accuracy of 30 μm. Then, each layer was led to an individual manifold by a converter installed on the top of the multi-manifold die, and the resin layer was individually expanded. Then, a laminated film was obtained in the same manner as in Example 1, except that the resin layer expanded at the land portion immediately before being discharged from the die was laminated to form B1 layer / A layer / B2 layer (see table for lamination thickness ratio). In addition, the obtained laminated film or each layer obtained by peeling it was evaluated for each item. The evaluation results are shown in Tables 3 to 8.

[0107] [Table 1]

[0108] [Table 2]

[0109] [Table 3]

[0110] [Table 4]

[0111] [Table 5]

[0112] [Table 6]

[0113] [Table 7]

[0114] [Table 8] [Industrial Applicability]

[0115] The laminated film of the present invention is a laminated film having a layer A which is a low retardation layer and a layer B which is a protective layer exhibiting a certain plane orientation coefficient, which are in contact with both layers A and B. Since the laminated film can be easily peeled off from the layers A and B and has excellent optical properties and protective performance, it can be suitably used for optical applications such as optical compensation applications such as polarizer protective films mounted on display devices such as displays, transparent conductive films, and low retardation films for inspection.

Claims

1. The layer A and the layer B have different crystal melting energies ΔHm (J / g), Both surfaces of layer A are in contact with layer B, The retardation of the A layer is 0.0 nm or more and 180 nm or less, the plane orientation coefficient of the B layers on both sides of the A layer is 0.0300 or more and 0.1700 or less; ΔHm of layer A is ΔHm A (J / g), ΔHm of B layer is ΔHm B (J / g), the A layer and the B layers on both sides of the A layer are both ΔHm B -ΔHm A is 5.0 (J / g) or more, and the peel strength between at least one of the B layer and the A layer is 1.0 g / 50 mm or more and 100 g / 50 mm or less, A laminated film having a haze of 0.5% or more and 3.0% or less.

2. The solubility parameter of the A layer is SP A (cal / cm 3 ) 1/2 The solubility parameter of the B layer is SP B (cal / cm 3 ) 1/2 Then, |SP A -SP B The laminated film according to claim 1 , wherein | is 0.5 or more and 4.0 or less.

3. The glass transition temperature (Tg A 3. The laminated film according to claim 1 or 2, wherein the temperature of the laminated film is from more than 100° C. to 170° C. or less.

4. 4. The laminated film according to claim 1, wherein the layer A is mainly composed of an amorphous resin.

5. 5. The laminate film according to claim 4, wherein the amorphous resin is at least one resin selected from the group consisting of polypropylene resins, cyclic olefin resins, polystyrene resins, polycarbonate resins, acrylic resins, polyester resins, and polyamide resins.

6. 6. The laminated film according to claim 1, wherein the number of flexing cycles until breakage of the layer A is 100 or more and 10,000 or less.

7. 7. The laminate film according to claim 1, wherein the surface roughness Ra of one or both sides of the layer A is 1 nm or more and 100 nm or less.

8. 8. The laminated film according to claim 1, wherein the layer B has a minor endothermic peak temperature (Tmeta) of 120° C. or higher and 220° C. or lower.

9. The laminated film according to any one of claims 1 to 8, characterized in that the B layer has a plane refractive index of 1.6000 or more and 1.6600 or less, and a thickness direction refractive index of the B layer is 1.4800 or more and 1.5700 or less.

10. The crystallinity parameter (ΔTcg) of the B layer is 10° C. or more and 100° C. or less, and the ΔHm B The laminated film according to any one of claims 1 to 9, characterized in that the strength is 15.0 J / g or more and 50.0 J / g or less.

11. The glass transition temperature (Tg B 11. The laminated film according to claim 1, wherein the temperature of the laminated film is 30° C. or higher and 100° C. or lower.

12. The laminated film according to any one of claims 1 to 11, wherein the layer B is mainly composed of a crystalline resin.

13. The laminated film according to claim 12, wherein the crystalline resin is a polyester resin.

14. A method for producing the laminated film according to any one of claims 1 to 13, comprising the steps of: When the molten resin composition for obtaining the A layer is a molten resin composition A and the molten resin composition for obtaining the B layer is a molten resin composition B, a co-extrusion lamination step of co-extruding the molten resin composition A and the molten resin composition B to laminate them; A casting process in which the laminate obtained by the co-extrusion lamination process is cooled and solidified; a stretching step of stretching the sheet obtained by the casting step in at least one direction; and the glass transition temperature Tg of the layer A A +20℃ or more Tg A A method for producing a laminated film, comprising the steps of:

15. The method for producing a laminated film according to claim 14, wherein the molten resin composition B is laminated on both sides of the molten resin composition A in the co-extrusion lamination step.

16. The method for producing a laminated film according to claim 15, wherein the molten resin compositions B located on either side of the molten resin composition A have compositions different from each other.

17. The method for producing a film according to any one of claims 14 to 16, further comprising a width-spreading step of separately spreading the molten resin composition A and the molten resin composition B upstream of the co-extrusion lamination step.

Citation Information

Patent Citations

  • Non-crystalline polyolefin laminated sheet for phase difference plate and the same plate

    JP1993064865A

  • Manufacture of thermoplastic resin sheet

    JP2001030351A

  • Cycloolefin-based resin film and production method thereof

    JP2009227932A

  • Optical film and its manufacturing method

    JP2010091646A

  • Biaxially-oriented cyclic olefin film and method of producing the same

    JP2011093285A