Release film roll
The release film roll with a specific configuration of non-reactive and reactive polyolefins, crosslinking agents, and antistatic layers addresses blocking and static discharge issues, providing a smooth and antistatic surface for adhesive layers, enhancing film performance in industrial applications.
Patent Information
- Application Number
- JP2021027303
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-24
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-02-24
AI Technical Summary
Existing release films used in industrial applications face issues such as blocking, peeling force irregularities, and static discharge, particularly when used with adhesive layers requiring high smoothness and antistatic properties, leading to potential contamination and damage in electronic components.
A release film roll comprising a base film with a release layer and an antistatic layer, where the release layer includes non-reactive polyolefin, reactive polyolefin, and a crosslinking agent, and the antistatic layer contains a long-chain alkyl or fluorine-based mold release agent and an antistatic agent, ensuring a smooth surface with minimal blocking and effective antistatic properties.
The film roll achieves minimal blocking, good release properties, and effective antistatic performance, preventing contamination and ensuring smooth peeling without residue, suitable for protecting various adhesive layers.
Smart Images

Figure 0007593163000001 
Figure 0007593163000002 
Figure 0007593163000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a release film roll. [Background technology]
[0002] Release films, which have a release layer on at least one side of a base film, are used in various fields such as industrial materials, optical materials, electronic component materials, and battery packaging materials. Polyethylene terephthalate (PET) films, which are representative polyester films, and biaxially oriented PET films in particular, are widely used as base films for release films because of their excellent transparency, mechanical strength, heat resistance, flexibility, and other properties.
[0003] On the other hand, in adhesive layers used in optical materials, etc., in applications where optical properties such as reflection properties are important, adhesive layers having a particularly smooth surface may be required. When a release film roll with a highly smooth release layer surface was used as a release film compatible with such adhesive layers, the release film tended to be easily blocked. Therefore, various proposals have been made to prevent blocking, such as providing a functional layer for preventing blocking on the surface of the release film opposite to the release layer. Release films are widely used to protect adhesive or bonding surfaces. The most commonly used material for the release surface of release films has been silicone-based polymers containing siloxane units. However, since silicone-based polymers contain siloxane-based low molecular weight compounds, when they are applied to precision applications such as electronic components, the siloxane-based low molecular weight compounds may volatilize and oxidize in the air, causing problems by adhering to electronic components. For this reason, there has been a demand for a film that does not contain siloxane-based low molecular weight compounds and has the same release properties as a release film that uses a silicone-based polymer as a release layer. For example, hard disk devices are becoming increasingly high-performance and high-density at a remarkable pace, and it is expected that such high performance and high density will continue to advance in the future. It has been pointed out that as the performance and density of hard disk devices continue to increase, the accumulation of fine siloxane-based low molecular weight compounds as described above may have a negative effect on reading and writing on hard disks.
[0004] As an example of a release layer that does not contain silicon or halogen elements, a release layer using polyolefin or a long-chain alkyl-containing polymer has been known for some time. These release layers may generate a peeling charge when the release film is peeled off from an adherend such as an adhesive, and as a result, serious problems may occur in the manufacturing process of electronic parts, etc., such as defects in nearby electronic elements caused by electrostatic interference, as well as defects in the product, due to adhesion or entrapment of foreign matter. Therefore, antistatic measures taken by equipment in the manufacturing process are not necessarily sufficient, and antistatic treatment of the release film itself is strongly desired.
[0005] Patent documents 1 to 5 are examples of the achievement of easy peeling using polyolefin. Of these, Patent document 1 has a problem in that the adhesion between the polyolefin and the substrate film is insufficient, and when peeling the release layer from the adhesive, the release layer detaches to the adhesive. In addition, although polyolefin has good peeling properties, it does not have high heat resistance, so there is a problem in that the heat peeling force is heavy. Patent documents 2 to 5 improve the adhesion between the polyolefin and the substrate and the heat resistance by dissolving the polyolefin in an organic solvent, and further mixing it with a polyolefin polyol and an isocyanate-based crosslinking agent, and applying and drying it, but neither can be said to be sufficient.
[0006] Patent Documents 6 to 9 are also examples of the antistatic layer. Patent Document 6 proposes providing a release layer made of a mixture of polyolefin and an antistatic agent, but mixing an antistatic agent makes it impossible to avoid a heavy peeling force. Patent Document 7 proposes providing an antistatic layer between the substrate and the release layer, but the release layer is polyolefin, and there is a problem that the heat peeling force is large. Patent Document 8, like Patent Document 7, provides an antistatic layer between the substrate and the release layer, and uses an acid-modified polyolefin for the release layer, and improves the heat peeling force and the adhesion of the coating film, but there is a problem that the peeling force is heavy compared to unmodified polyolefin. Patent Document 9 proposes a release film with a light peeling force and antistatic properties by providing an antistatic layer cured by ultraviolet irradiation between the substrate and the silicone release layer to prevent the silicone from being inhibited from being cured, but the antistatic layer requires ultraviolet irradiation, making it difficult to coat in-line during the film formation of the substrate, and ultraviolet irradiation equipment is required, resulting in poor productivity. In addition, since the release layer is silicone, it is not suitable for electronic component applications such as hard disks. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2001-246697 A [Patent Document 2] JP 2011-52207 A [Patent Document 3] JP 2011-94096 A [Patent Document 4] JP 2012-87210 A [Patent Document 5] JP 2012-87211 A [Patent Document 6] Japanese Patent Application Publication No. 10-86289 [Patent Document 7] International Publication No. 2009 / 069445 [Patent Document 8] JP 2009-101680 A [Patent Document 9] JP 2005-153250 A Summary of the Invention [Problem to be solved by the invention]
[0008] In addition, in the case of a release film roll, when a functional layer containing a silicone resin component is provided on the opposite side of the release layer, the occurrence of blocking is reduced, but the silicone component is transferred from the back side, and the peeling force of the release layer surface may decrease. In addition, when the functional layer surface is moderately roughened, the occurrence of blocking is reduced, but the unevenness of the functional layer surface may be directly transferred to the release layer surface. For this reason, there was a need for a release film roll that has a highly smooth release layer surface, minimizes the occurrence of blocking, and has good releasability and antistatic properties, and is suitable for protecting various adhesive layers.
[0009] In view of the above problems, the present invention aims to provide a release film roll which is highly smooth, yet causes minimal blocking, has good releasability and antistatic properties, and is suitable for protecting various adhesive layers. [Means for solving the problem]
[0010] As a result of extensive investigations, the present inventors have found that the above problems can be solved by using a release film roll having a specific configuration, and have completed the present invention as described below. That is, the present invention provides the following [1] to
[12] . [1] A release film roll having a configuration comprising a release layer, a base film and an antistatic layer in this order, the release layer being a cured layer of an antistatic layer composition containing (A) a non-reactive polyolefin containing 50 to 80 mass% of ethylene units, (B) a reactive polyolefin and (C) a crosslinking agent, the (C) crosslinking agent being an aliphatic isocyanate having two or more isocyanate groups in one molecule, the surface roughness (Sa) of the release layer being 20 nm or less, and the antistatic layer being a cured layer of an antistatic layer composition containing (D) a release agent having a long-chain alkyl group or a fluorine-based release agent and (E) an antistatic agent. [2] The release film roll according to [1], wherein the (B) reactive polyolefin is a polyolefin polyol. [3] The release film roll according to [1] or [2], wherein the (A) non-reactive polyolefin is a copolymer of ethylene and an α-olefin. [4] The release film roll according to any one of [1] to [3], wherein the (D) release agent having a long-chain alkyl group is a release agent having a long-chain alkyl group having 6 or more carbon atoms. [5] The release film roll according to any one of [1] to [4], wherein the (D) release agent having a long-chain alkyl group is a release agent having a long-chain alkyl group having 8 or more carbon atoms. [6] The release film roll according to [5], wherein the (D) release agent having a long-chain alkyl group is a release agent having a long-chain alkyl group having 8 or more carbon atoms and having polyvinyl alcohol as a copolymerization component. [7] The release film roll according to any one of [1] to [6], wherein the (E) antistatic agent is thiophene or a thiophene derivative. [8] The release film roll according to any one of [1] to [7], wherein the antistatic layer is a cured layer of an antistatic layer composition further containing a binder (F). [9] The release film roll according to any one of [1] to [8], wherein the surface roughness (Sa) of the base film surface is 20 nm or less.
[10] The release film roll according to any one of [1] to [9], wherein the base film is a polyester film.
[11] The release layer and the antistatic layer are arranged to face each other, and a pressure of 10 kg / cm is applied. 2 The release film roll according to any one of [1] to
[10] , wherein the release film roll has a peel strength of 120 gf / 125 mm width or less under conditions of a tensile speed of 300 mm / min and 180° peeling after applying pressure for 20 hours in an atmosphere of 40°C and 80% RH.
[12] The release film roll according to any one of [1] to
[11] , which is for protecting an adhesive layer. Effect of the Invention
[0011] In the present invention, by using a release film roll having a base film on which a release layer and an antistatic layer having a specific configuration are provided, The release layer has a highly smooth surface, yet the occurrence of blocking is minimized, and the release properties and antistatic properties are excellent, making it possible to provide a release film roll suitable for protecting various adhesive layers. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Next, an example of an embodiment of the present invention will be described. However, the present invention is not limited to the embodiment described below.
[0013] The release film roll of the present invention has a structure including a release layer, a base film, and an antistatic layer in this order, and the release layer is a cured layer of a release layer composition including (A) a non-reactive polyolefin containing 50 to 80% by mass of an ethylene unit, (B) a reactive polyolefin, and (C) a crosslinking agent; The (C) crosslinking agent is an aliphatic isocyanate having two or more isocyanate groups in one molecule, the surface roughness (Sa) of the release layer is 20 nm or less, and the antistatic layer is a cured layer of an antistatic layer composition containing (D) a release agent having a long-chain alkyl group or a fluorine-based release agent and (E) an antistatic agent.
[0014] Hereinafter, an example of an embodiment of the release film roll of the present invention will be described. However, the present invention is not limited to the following embodiment, and can be modified as desired without departing from the gist of the present invention. In the present invention, the term "film" includes the term "sheet", and the term "sheet" includes the term "film". In the present invention, when it is described as "X to Y" (X and Y are any numbers), unless otherwise specified, it includes the meaning of "X or more and Y or less", as well as the meaning of "preferably larger than X" or "preferably smaller than Y". In addition, when it is stated that the amount is "X or more" (X is any number), it also means that the amount is "preferably greater than X" unless otherwise specified, and when it is stated that the amount is "Y or less" (Y is any number), it also means that the amount is "preferably smaller than Y" unless otherwise specified.
[0015] <Release film roll> The release film roll of the present invention comprises a base film, and a release layer and an antistatic layer formed on at least one surface of the base film. Each member will be described in more detail below, but first, each member constituting the release film roll will be described in more detail.
[0016] [Base film] The material of the base film constituting the release film roll is not particularly limited as long as it has a film shape. For example, it may be made of paper, resin, metal, etc. Among these, it is preferable to use a resin from the viewpoint of mechanical strength and flexibility.
[0017] Examples of the resin substrate film include resin films formed from polymers such as polyethylene, polypropylene, cycloolefin polymer (COP), polyester, polystyrene, acrylic resin, polycarbonate, polyurethane, triacetyl cellulose (TAC), polyvinyl chloride, polyethersulfone, polyamide, polyimide, polyamideimide, etc. Furthermore, as long as it is possible to form a film, it may be a mixture of these materials (polymer blend) or a composite of the structural units (copolymer).
[0018] Among the above-mentioned films, polyester films are particularly preferred because they have excellent physical properties such as heat resistance, flatness, optical properties, and strength. The polyester films may be single-layered or multi-layered films (i.e., laminated films) having two or more layers with different properties. The polyester film is a film containing polyester as a main resin component. The polyester film may be a non-stretched film (sheet) or a stretched film. Of these, a stretched film stretched in a uniaxial or biaxial direction is preferred. Of these, a biaxially stretched film is more preferred from the viewpoint of balance of mechanical properties and flatness. Therefore, a biaxially stretched polyester film is even more preferred.
[0019] The polyester, which is the main component resin of the polyester film, may be a homopolyester or a copolymer polyester. The main component resin means the resin having the largest mass ratio among the resins constituting the polyester film, and may account for 50 mass% or more, 75 mass% or more, 90 mass% or more, or 100 mass% of the resins constituting the polyester film.
[0020] The homopolyester is preferably one obtained by polycondensation of an aromatic dicarboxylic acid and an aliphatic glycol. Examples of the aromatic dicarboxylic acid include terephthalic acid and 2,6-naphthalenedicarboxylic acid, and terephthalic acid is preferred. Examples of the aliphatic glycol include ethylene glycol, diethylene glycol, 1,4-butanediol, and 1,4-cyclohexanedimethanol, and ethylene glycol is preferred. Representative examples of homopolyester include polyethylene terephthalate (PET) and polybutylene terephthalate (PBT).
[0021] On the other hand, when the polyester is a copolymer polyester, it is preferable that the polyester is a copolymer containing 30 mol % or less of a third component. Examples of the dicarboxylic acid component of the copolymer polyester include one or more of isophthalic acid, phthalic acid, terephthalic acid, 2,6-naphthalenedicarboxylic acid, adipic acid, sebacic acid, etc., and examples of the glycol component include one or more of ethylene glycol, diethylene glycol, propylene glycol, 1,4-butanediol, 1,4-cyclohexanedimethanol, neopentyl glycol, etc. It is preferable that the copolymer polyester contains terephthalic acid as the dicarboxylic acid, contains ethylene glycol as the glycol component, and contains a third component other than these. Among these, the base material in the present release film roll is preferably polyethylene terephthalate, which contains 60 mol % or more, preferably 80 mol % or more of ethylene terephthalate units.
[0022] Particles can be blended into the base film in the release film roll of the present invention, mainly for the purpose of imparting easy slippage and preventing scratches in each process. When particles are blended, the type of particles to be blended is not particularly limited as long as they are particles that can impart easy slippage, and specific examples include inorganic particles such as silica, calcium carbonate, magnesium carbonate, barium carbonate, calcium sulfate, calcium phosphate, magnesium phosphate, kaolin, aluminum oxide, and titanium oxide, and organic particles such as acrylic resin, styrene resin, urea resin, phenolic resin, epoxy resin, and benzoguanamine resin. Furthermore, in the case of polyester film, precipitated particles obtained by precipitating and finely dispersing a part of a metal compound such as a catalyst during the polyester production process can also be used.
[0023] On the other hand, the shape of the particles to be used is not particularly limited, and any of spherical, blocky, rod-like, flat, etc. may be used. In addition, there is no particular limit to the hardness, specific gravity, color, etc. Two or more kinds of these particles may be used in combination as necessary. The average particle size of the particles used is preferably 5 μm or less, more preferably in the range of 0.1 to 3 μm. By using particles with an average particle size in the above range, an appropriate surface roughness can be imparted to the film, and good slipperiness and smoothness can be ensured. When particles are blended, for example, it is preferable to provide a surface layer and a base layer on the substrate film and to incorporate the particles in the surface layer. In this case, it is more preferable to use a substrate film having a multi-layer structure having a particle-containing surface layer, a base layer, and a particle-containing surface layer in this order.
[0024] Furthermore, the content of particles in the base film is preferably 5% by mass or less, more preferably in the range of 0.01 to 3% by mass. By setting the content of particles within the above range, the transparency of the base film is ensured, while the slipperiness of the base film is easily imparted. However, the base film does not have to substantially contain particles. In this specification, "substantially free of particles" means that particles are not intentionally contained, and specifically means that the particle content (particle mass concentration) is 200 ppm or less, more preferably 150 ppm or less, relative to the member or layer (here, the base film). Similar terms shown below have the same meaning. In addition, when the substrate film does not substantially contain particles or the content is small, the substrate film has high transparency and a film with good appearance can be obtained. It is also possible to make only the substrate film surface on the side in contact with the release layer particularly smooth. On the other hand, the slipperiness of the release film roll may be insufficient. Therefore, in such a case, the slipperiness may be improved by blending particles into the release layer or the antistatic layer on the opposite side.
[0025] The thickness of the substrate film is preferably 12 to 125 μm, more preferably 25 to 100 μm, and particularly preferably 25 to 75 μm. If the substrate film has a thickness within the above range, it can be suitably used for optical applications.
[0026] (Laminated structure of base film) When the base film has a laminated structure having two or more layers, a three-layer structure can be adopted, such as B / A / C consisting of a base layer A, a surface layer B, and a surface layer C, or B / A / B consisting of a base layer A and a surface layer B. When the base film has a laminated structure having two or more layers, the main component resin constituting each layer is preferably polyester, as described above.
[0027] In the three-layer structure of B / A / C and B / A / B, the surface layer B and the surface layer C preferably contain particles to ensure ease of handling.
[0028] In the above-mentioned three-layer structures of B / A / C and B / A / B, it is particularly preferable that the surface layer B and the surface layer C each contain particles having a narrow particle size distribution and a substantially uniform average particle size (so-called monodispersity).
[0029] Surface layer B contains, for example, particles having an average particle size of 0.1 to 3 μm, and preferably contains particles having an average particle size of 0.1 to 0.5 μm. Surface layer C contains, for example, particles having an average particle size of 0.1 to 3 μm, and preferably contains particles having an average particle size of 0.05 to 0.2 μm, and more preferably contains particles having an average particle size of 0.05 to 0.1 μm.
[0030] The average particle size of particles can be determined by measuring the diameters of 10 or more particles using a scanning electron microscope (SEM) and taking the average value. In this case, in the case of non-spherical particles, the average value of the longest and shortest diameters can be measured as the diameter of each particle.
[0031] The base film contains the particles at a mass ratio of, for example, 900 ppm or more, preferably 2000 to 10000 ppm, more preferably 2500 ppm to 9500 ppm, and even more preferably 3000 ppm to 9000 ppm. The mass ratio here refers to the ratio of the particles in each surface layer.
[0032] Moreover, it is particularly preferable that the surface layer C contains the particles in a mass ratio of 900 ppm or more and 6000 ppm or less. When the surface layer C contains particles in this range, the handling properties of the film can be improved.
[0033] Moreover, it is particularly preferable that the surface layer B contains the particles in a mass ratio of less than 5000 ppm, and it is most preferable that the surface layer B contains the particles in a mass ratio of 2000 ppm or more and 4000 ppm or less.
[0034] The base layer A preferably functions as the thickest main layer, and in order to reduce costs, it preferably does not substantially contain particles or contains particles at a lower concentration than the surface layer B.
[0035] (Surface roughness of base film (Sa)) The surface roughness (Sa) of the surface of the substrate film of the present invention is preferably 20 nm or less, more preferably 15 nm or less, and even more preferably 10 nm or less. By making the surface roughness (Sa) of the substrate film 20 nm or less, it is possible to obtain a release layer and an antistatic layer with smoother surfaces. In addition, the lower limit of the surface roughness (Sa) of the substrate film surface is not particularly limited, but is usually 0.1 nm or more. In this specification, the surface roughness (Sa) refers to the arithmetic mean height measured in accordance with ISO 25178, and can be measured specifically by the method described in the Examples.
[0036] <Method of manufacturing base film> (Polyester film) When a polyester film is used as the base film, the polyester film is preferably produced by extruding pellets obtained by drying the above-mentioned polyester raw material from a die using an extruder as a molten sheet, and then cooling and solidifying the sheet with a cooling roll to obtain an unstretched sheet. In this case, it is preferable to increase the adhesion between the sheet and the rotating cooling drum in order to improve the flatness of the sheet, and an electrostatic application adhesion method and / or a liquid application adhesion method are preferably used. In this way, an unstretched polyester film is obtained.
[0037] (Biaxially oriented polyester film) The unstretched sheet obtained by the above method is then stretched in a biaxial direction. In this case, the unstretched sheet is first stretched in one direction by a roll or tenter type stretching machine. The stretching temperature is usually 70 to 120°C, preferably 80 to 110°C, and the stretching ratio is usually 2.5 to 7 times, preferably 3.0 to 6 times. Next, the sheet is stretched in a direction perpendicular to the first-stage stretching direction, in which the stretching temperature is usually 70 to 170°C, and the stretching ratio is usually 3.0 to 7 times, preferably 3.5 to 6 times. Then, the sheet is subsequently heat-treated under tension or relaxation of 30% or less at a temperature of 180 to 270°C to obtain a biaxially stretched film. In the above stretching, a method of stretching in one direction in two or more stages can also be adopted. In this case, it is preferable to perform the stretching so that the final stretching ratios in both directions are each within the above range.
[0038] In addition, a simultaneous biaxial stretching method can also be adopted for the production of polyester films. The simultaneous biaxial stretching method is a method in which the unstretched sheet is simultaneously stretched and oriented in the machine direction and the width direction under a temperature controlled condition usually at 70 to 120°C, preferably 80 to 110°C, and the stretching ratio is 4 to 50 times, preferably 7 to 35 times, more preferably 10 to 25 times in terms of area ratio. Then, the sheet is subsequently heat-treated under tension or relaxation of 30% or less at a temperature of 170 to 250°C to obtain a stretched and oriented film. As for the simultaneous biaxial stretching device adopting the above-mentioned stretching method, a conventionally known stretching method such as a screw method, a pantograph method, and a linear drive method can be adopted.
[0039] <Release Layer Composition> (A) Non-reactive polyolefin The non-reactive polyolefin is a non-reactive polyolefin that has substantially no reactivity. More specifically, it means a non-reactive polyolefin that has no reactivity with an isocyanate group. The non-reactive polyolefin may be used alone or in combination of two or more kinds. From the viewpoint of releasability and heat resistance, it is preferable to use a polyethylene copolymer.
[0040] When a polyethylene copolymer is used, it is preferable to use one synthesized using a transition metal catalyst such as a Ziegler-Natta catalyst or a metallocene catalyst. Among these, the use of one synthesized using a metallocene catalyst has the advantage that a release film roll excellent in releasability and heat resistance can be obtained. As the polyethylene copolymer, from the viewpoint of obtaining a release film roll having excellent releasability and heat resistance, it is preferable to use a copolymer of ethylene and an α-olefin, specifically, an ethylene-propylene copolymer, an ethylene-hexene copolymer, an ethylene-butene copolymer, an ethylene-octene copolymer, or the like, and it is more preferable to use an ethylene-propylene copolymer.
[0041] The density of the non-reactive polyolefin is not particularly limited, but is preferably 0.92 g / cm3 It is preferable that the density is 0.90 g / cm or less. 3 More preferably, the density of the non-reactive polyolefin is 0.85 g / cm or less. 3 When the density of the non-reactive polyolefin is within the above range, the mold releasability tends to be good.
[0042] The content of ethylene units contained in the non-reactive polyolefin is in the range of 50% by mass or more and 80% by mass or less. If the content of ethylene units exceeds 80% by mass, gel is generated during coating, which causes an increase in filter pressure and a deterioration in the appearance of the release film roll, resulting in a decrease in productivity. If the content of ethylene units is less than 50% by mass, it becomes difficult to obtain sufficient releasability. From the viewpoint of forming a release layer that is excellent in releasability and does not generate gel, the content of ethylene units is preferably 60% by mass or more and 80% by mass or less, more preferably 70% by mass or more and 80% by mass or less.
[0043] In the present invention, when only one type of non-reactive polyolefin is used, from the viewpoint of the coating strength during the formation of the release layer, the non-reactive polyolefin preferably has an MFR (melt flow rate) of 100 g / 10 min or less at 230° C. and a load of 2.16 kg, more preferably an MFR of 70 g / 10 min or less, even more preferably an MFR of 50 g / 10 min or less, and particularly preferably an MFR of 10 g / 10 min or less. The lower limit is not particularly limited, but is usually 0.2 g / 10 min or more.
[0044] In addition, when two or more kinds of non-reactive polyolefins are used, it is preferable that at least one of them has an MFR of 100g / 10min or less at 230°C and a load of 2.16kg, and the proportion of non-reactive polyolefins having an MFR of 100g / 10min or less in the release layer is preferably 10% by mass or more, more preferably 50% by mass or more. If this condition is satisfied, other non-reactive polyolefins having an MFR of more than 100g / 10min at 230°C and a load of 2.16kg may be used.
[0045] The content of the non-reactive polyolefin in the release layer is preferably 60 to 80% by mass, more preferably 70 to 80% by mass. If the content is less than 50% by mass, the peelability decreases and the desired light peel strength cannot be obtained. On the other hand, if the content exceeds 80% by mass, it is difficult to form a crosslinked structure, and therefore sufficient coating strength may not be obtained.
[0046] (B) Reactive polyolefin The reactive polyolefin used in the present invention reacts with an aliphatic isocyanate to form a three-dimensional network. Through such a crosslinking reaction, it is possible to impart heat resistance and chemical resistance to the release layer.
[0047] The reactive polyolefin is not limited as long as it is a non-reactive polyolefin that can react with an aliphatic isocyanate, but specific examples include those obtained by modifying a non-reactive polyolefin using a compound having a functional group in a molten or solution state, and those obtained by a method such as copolymerizing a compound reactive with ethylene or the like in the presence of a catalyst. The reactive group is not particularly limited, but examples include an epoxy group, a hydroxy group, a carboxy group, and an acid anhydride, and a compound having at least one hydroxy group on average in the molecule is preferred.
[0048] In order to achieve both low peel strength and adhesion to the substrate, the amount of reactive functional groups contained in the reactive polyolefin is preferably 0.01 to 5 mass %, more preferably 0.01 to 1 mass %. If the reactive polyolefin contains reactive functional groups in an amount exceeding 5 mass %, the peel strength tends to increase. From the viewpoint of peel strength, the density of reactive polyolefin is 1.2 g / cm 3 The preferred range is 1.0 g / cm or less, particularly 1.0 g / cm 3 The lower limit is not particularly limited, but is usually 0.7 g / cm 3 That's all.
[0049] Specific examples of reactive polyolefins include hydroxy(meth)acrylate modified ethylene-α-olefin copolymers, hydroxy(meth)acrylate modified polyethylene, hydroxy(meth)acrylate modified polypropylene, non-reactive polyolefin polyols, epoxy group-containing (meth)acrylate modified ethylene-α-olefin copolymers, epoxy group-containing (meth)acrylate modified polyethylene, epoxy group-containing (meth)acrylate modified nuclear hydrogenated styrene-diene copolymers, epoxy group-containing (meth)acrylate modified polypropylene, acid-modified ethylene-α-olefin copolymers, etc. Polyolefin polyols are particularly preferred because they are readily available commercially.
[0050] Specific examples of reactive polyolefin polyols include "Polytail H" (hydroxylated polybutadiene) manufactured by Mitsubishi Chemical Corporation, "Poly bd R-45HT" (liquid hydroxyl-terminated polybutadiene) manufactured by Idemitsu Kosan Co., Ltd., "Poly ip" (liquid hydroxyl-terminated polyisoprene) manufactured by Idemitsu Kosan Co., Ltd., "Epole" (liquid hydroxyl-terminated hydrogenated polyisoprene) manufactured by Idemitsu Kosan Co., Ltd., "GI-1000" (liquid hydroxyl-containing hydrogenated polybutadiene) manufactured by Nippon Soda Co., Ltd., "GI-2000" (liquid hydroxyl-containing hydrogenated polybutadiene) manufactured by Nippon Soda Co., Ltd., and "GI-3000" (liquid hydroxyl-containing hydrogenated polybutadiene) manufactured by Nippon Soda Co., Ltd.
[0051] The reactive polyolefin may have different functional groups in the molecule, and may be a composition of a plurality of reactive polyolefins. The content of the reactive polyolefin in the release layer is preferably 0.2 to 20% by mass, more preferably 0.5 to 10% by mass. When the content is 0.2% by mass or more, the heat resistance and solvent resistance are good. When the content is 20% by mass or less, the releasability is good.
[0052] (C) Crosslinking agent The release layer composition in the release film roll of the present invention uses an aliphatic isocyanate containing two or more isocyanate groups in one molecule as a crosslinking agent. By using such an aliphatic isocyanate, a release layer that has both releasability, heat resistance, and chemical resistance can be formed. The number of isocyanate groups in one molecule is preferably three or more, and more preferably three. Examples of the aliphatic isocyanate include polyisocyanate compounds such as aliphatic polyisocyanates and alicyclic polyisocyanates, and among these, diisocyanate compounds are preferred. Examples of the isocyanate compounds include isocyanate compounds having an isocyanurate skeleton obtained by isocyanating a diisocyanate compound. Examples of the aliphatic polyisocyanates include hexamethylene diisocyanate, pentamethylene diisocyanate, trimethylhexamethylene diisocyanate, lysine diisocyanate, and lysine triisocyanate. Examples of the alicyclic polyisocyanate include hydrogenated diphenylmethane diisocyanate, hydrogenated xylylene diisocyanate, isophorone diisocyanate, norbornene diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, and 1,4-bis(isocyanatomethyl)cyclohexane. Among these, aliphatic diisocyanates are preferred because of their excellent resistance to yellowing. In addition, isocyanate-based compounds having an isocyanurate skeleton are also preferred, and from the same viewpoint, isocyanurate-based compounds having an isocyanurate skeleton obtained by isocyanating an aliphatic diisocyanate or an alicyclic diisocyanate are also preferred, and among these, isocyanate-based compounds having an isocyanurate skeleton are more preferred. The isocyanate compounds may be used alone or in combination of two or more kinds.
[0053] A catalyst may be added to the release layer composition to promote the reaction of the release layer. The type of catalyst is not particularly limited, but it is preferable to use a urethane catalyst to promote the reaction between the reactive polyolefin and the aliphatic isocyanate contained in the release layer composition. Examples of the urethane catalyst include tertiary amines, tertiary amine carboxylates, carboxylate metal salts (potassium acetate, potassium octylate, stannous octoate, etc.) and organometallic compounds (dibutyltin dilaurate, etc.), and among these, tertiary amines are particularly preferable because they are easy to control the reaction.
[0054] Examples of tertiary amines include triethylenediamine, N-ethylmorpholine, N-methylpiperidine, pyrrolidine, quinuclidine, 1,4-diazabicyclo[2.2.2]octane, diethylethanolamine, N,N,N',N'-tetramethylhexamethylenediamine, 1,2-dimethylimidazole, 1-isobutyl-2-methylimidazole, 1,8-diazabicyclo-[5.4.0]-undecene-7 (carboxylate) and bis(dimethylaminoethyl)ether (carboxylate), as well as combinations of two or more of these.
[0055] (Release layer thickness) The thickness of the release layer (after drying) is, for example, 0.1 to 5 μm, preferably 0.1 to 3 μm, more preferably 0.1 to 1 μm, and particularly preferably 0.1 to 0.5 μm. When the thickness of the release layer is equal to or greater than these lower limits, good releasability can be achieved. When the thickness of the release layer is equal to or less than these upper limits, the hardening property of the release layer is good.
[0056] (Surface roughness of release layer (Sa)) The surface roughness (Sa) of the surface of the substrate film of the present invention is preferably 20 nm or less, more preferably 15 nm or less, and even more preferably 10 nm or less. By making the surface roughness (Sa) of the substrate film 20 nm or less, the surface of the release layer can be made smoother, and therefore, for example, the uneven shape can be prevented from being transferred to the surface of a highly smooth adhesive layer, and can be preferably used. In addition, the lower limit of the surface roughness (Sa) of the substrate film surface is not particularly limited, but is usually 0.1 nm or more. In this specification, the surface roughness (Sa) refers to the arithmetic mean height measured in accordance with ISO 25178, and can be specifically measured by the method described in the Examples.
[0057] <Method of forming release layer> As described above, the release layer can be obtained by applying a release layer composition to the surface of a substrate film, drying the composition to form a release layer, and curing the release layer. Examples of a method for applying the release layer composition include air doctor coating, blade coating, rod coating, bar coating, knife coating, squeeze coating, impregnation coating, reverse roll coating, transfer roll coating, gravure coating, kiss roll coating, cast coating, spray coating, curtain coating, calendar coating, and extrusion coating. The drying conditions are not particularly limited, and the drying may be performed at about room temperature or by heating, for example, at about 25 to 120° C., preferably 50 to 100° C., and more preferably 60 to 90° C. The drying time is not particularly limited as long as the solvent can be sufficiently evaporated, and is, for example, about 10 seconds to 30 minutes, and preferably about 15 seconds to 10 minutes.
[0058] <Antistatic layer> In the release film roll of the present invention, it is necessary to provide an antistatic layer on the film surface opposite to the surface on which the release layer is provided. By providing an antistatic layer, it becomes possible to smoothly unwind the film from the release film roll having a highly smooth release layer surface.
[0059] (D) Release agent (Long-chain alkyl compounds) The long-chain alkyl compound used in the present invention is a compound having a straight-chain or branched alkyl group having usually 6 or more, preferably 8 or more, and more preferably 12 or more carbon atoms. On the other hand, the upper limit of the carbon number is not particularly limited, but is preferably 60 or less, more preferably 50 or less. Examples of the alkyl group include hexyl, octyl, decyl, lauryl, octadecyl, and behenyl groups. Examples of the compound having an alkyl group include various long-chain alkyl group-containing polymer compounds, long-chain alkyl group-containing amine compounds, long-chain alkyl group-containing ether compounds, and long-chain alkyl group-containing quaternary ammonium salts. Among them, polymer compounds are preferred in consideration of heat resistance and staining resistance. Also, from the viewpoint of improving releasability, polymer compounds having a long-chain alkyl group in the side chain are more preferred.
[0060] A polymer compound having a long-chain alkyl group in a side chain can be obtained by reacting a polymer having a reactive group with a compound having an alkyl group capable of reacting with the reactive group. Examples of the reactive group include hydroxyl group, amino group, carboxyl group, acid anhydride, etc. Examples of compounds having these reactive groups include polyvinyl alcohol, polyethyleneimine, polyethyleneamine, reactive group-containing polyester resin, reactive group-containing poly(meth)acrylic resin, etc. Among these, polyvinyl alcohol is particularly preferred in terms of releasability and ease of handling.
[0061] Examples of compounds having an alkyl group capable of reacting with the reactive group include long-chain alkyl group-containing isocyanates such as hexyl isocyanate, octyl isocyanate, decyl isocyanate, lauryl isocyanate, octadecyl isocyanate, and behenyl isocyanate, long-chain alkyl group-containing acid chlorides such as hexyl chloride, octyl chloride, decyl chloride, lauryl chloride, octadecyl chloride, and behenyl chloride, long-chain alkyl group-containing amines, and long-chain alkyl group-containing alcohols. Among these, taking into consideration releasability and ease of handling, long-chain alkyl group-containing isocyanates are preferred, and octadecyl isocyanate is particularly preferred.
[0062] The polymeric compound having the above-mentioned long-chain alkyl group in the side chain can also be obtained by polymerization of a long-chain alkyl (meth)acrylate or copolymerization of a long-chain alkyl (meth)acrylate with another vinyl group-containing monomer. Examples of the long-chain alkyl (meth)acrylate include hexyl (meth)acrylate, octyl (meth)acrylate, decyl (meth)acrylate, lauryl (meth)acrylate, octadecyl (meth)acrylate, and behenyl (meth)acrylate.
[0063] (Fluorine compounds) The fluorine compound is a compound containing fluorine atoms in the compound. From the viewpoint of the coating appearance by in-line coating, organic fluorine compounds are preferably used, for example, perfluoroalkyl group-containing compounds, polymers of olefin compounds containing fluorine atoms, aromatic fluorine compounds such as fluorobenzene, etc. From the viewpoint of mold releasability, it is preferable to use a compound having a perfluoroalkyl group. Furthermore, the fluorine compound may also be a compound containing a long-chain alkyl compound as described later.
[0064] Examples of the compound having a perfluoroalkyl group include perfluoroalkyl group-containing (meth)acrylates such as perfluoroalkyl (meth)acrylate, perfluoroalkyl methyl (meth)acrylate, 2-perfluoroalkyl ethyl (meth)acrylate, 3-perfluoroalkyl propyl (meth)acrylate, 3-perfluoroalkyl-1-methylpropyl (meth)acrylate, and 3-perfluoroalkyl-2-propenyl (meth)acrylate, and polymers thereof; and perfluoroalkyl group-containing vinyl ethers such as perfluoroalkyl methyl vinyl ether, 2-perfluoroalkyl ethyl vinyl ether, 3-perfluoropropyl vinyl ether, 3-perfluoroalkyl-1-methylpropyl vinyl ether, and 3-perfluoroalkyl-2-propenyl vinyl ether, and polymers thereof. In consideration of heat resistance and contamination, the polymer is preferably a polymer. The polymer may be a single compound or a polymer of multiple compounds. In addition, from the viewpoint of releasability, the perfluoroalkyl group preferably has 3 to 11 carbon atoms. Furthermore, the polymer may be a polymer with a compound containing a long-chain alkyl compound as described below. From the viewpoint of adhesion to the substrate, it is preferably a polymer with vinyl chloride.
[0065] The proportion of the release agent (D) in the total non-volatile components in the antistatic layer composition is usually 2 to 30 mass %, more preferably 3 to 15 mass %, and even more preferably 5 to 12 mass %. When the proportion of the release agent is equal to or less than the upper limit, blocking resistance is good. On the other hand, if the ratio of the release agent is equal to or higher than the lower limit, blocking resistance may become insufficient.
[0066] (E) Antistatic Agent The antistatic agent used in the present invention is a polymer in which a compound made of thiophene or a thiophene derivative is doped with another anionic compound, or a self-doped polymer having an anionic group in a compound made of thiophene or a thiophene derivative. These substances are preferable because they show excellent electrical conductivity. Examples of compound (E) include those obtained by polymerizing a compound of the following formula (1) or (2) in the presence of a polyanion.
[0067] [ka] In the above formula (1), R 1 and R 2 each independently represents a hydrogen atom or an aliphatic hydrocarbon group, an alicyclic hydrocarbon group, an aromatic hydrocarbon group, or the like having 1 to 20 carbon atoms.
[0068] [ka] In the above formula (2), n represents an integer of 1 to 4.
[0069] Examples of polyanions used in polymerization include poly(meth)acrylic acid, polymaleic acid, polystyrene sulfonic acid, polyvinyl sulfonic acid, etc. As a method for producing such a polymer, for example, a method such as that shown in JP-A-7-90060 can be adopted.
[0070] In the present invention, the compound of the above formula (2) in which n is 2 and polystyrene sulfonic acid is used as the polyanion is preferably used.
[0071] When these polyanions are acidic, they may be partially or completely neutralized. The base used for neutralization is preferably ammonia, organic amines, or alkali metal hydroxides.
[0072] The proportion of the antistatic agent (E) in the total non-volatile components in the antistatic layer composition is usually in the range of 5 to 80 mass%, preferably 10 to 50 mass%, more preferably 15 to 40 mass%. When the proportion of the antistatic agent (E) is within the above range, the antistatic properties are good. On the other hand, when the proportion of the antistatic agent (E) is out of the above lower limit, the antistatic agent may be insufficient.
[0073] (F) Binder resin From the viewpoint of improving the durability of the antistatic layer, it is preferable that the antistatic layer of the release film roll in the present invention further contains a binder resin. Examples of the binder resin include polyester resin, acrylic resin, urethane resin, polyvinyl resin such as polyvinyl alcohol, polyalkylene glycol, polyalkyleneimine, methyl cellulose, hydroxycellulose, starch, etc. Among these, from the viewpoint of improving adhesion with the cured resin layer, it is preferable to use polyester resin, acrylic resin, and urethane resin, more preferably polyester resin and acrylic resin, and further preferably polyester resin. These binder resins may be used alone or in combination of two or more. In the easy-adhesion layer composition, the content of the binder resin is, for example, 20 to 90 mass%, preferably 30 to 80 mass%, based on the solid content.
[0074] (G) Other Ingredients In forming the antistatic layer, particles can be used in combination for the purpose of improving blocking resistance and slipping properties, etc., within the scope of the present invention. (Crosslinking agent) The antistatic layer composition according to the present invention may contain a crosslinking agent for the purpose of improving the durability of the antistatic layer, particularly the durability of the antistatic performance. As the crosslinking agent, various known crosslinking agents can be used, for example, melamine compounds, epoxy compounds, isocyanate compounds, carbodiimide compounds, oxazoline compounds, silane coupling compounds, etc. Among these, from the viewpoint of obtaining good antistatic properties, melamine compounds, epoxy compounds, isocyanate compounds, and carbodiimide compounds are preferred.
[0075] The crosslinking agent is usually present in an amount of 2 to 30% by mass, more preferably 3 to 15% by mass, and even more preferably 5 to 12% by mass, based on the total non-volatile components in the antistatic layer composition. When the crosslinking agent content is within the above range, the strength and transparency of the antistatic layer are good. On the other hand, when the crosslinking agent content is outside the lower limit, the coating strength of the antistatic layer may be insufficient.
[0076] (Thickness of antistatic layer) The thickness of the antistatic layer (after drying) is, for example, in the range of 0.01 to 1 μm, preferably 0.03 to 0.5 μm, more preferably 0.03 to 0.3 μm, and even more preferably 0.03 to 0.1 μm.
[0077] <Method of forming antistatic layer> The antistatic layer may be formed by "in-line coating", which treats the surface of the base film during the manufacturing process of the base film, or by "off-line coating", which applies a coating outside the system onto a base film that has already been manufactured.
[0078] In-line coating is a method of coating within the manufacturing process of a substrate film, specifically, a method of coating at any stage from melt extrusion of the substrate to stretching, heat setting and winding up. Usually, coating is performed on any of the following: an unstretched sheet obtained by melting and quenching, a stretched uniaxially stretched film, a biaxially stretched film before heat setting, or a film after heat setting and before winding up.
[0079] As another method for forming the antistatic layer, for example, the antistatic layer can be formed by dispersing or dissolving the particles and any other additives that the antistatic layer may further contain, such as an antistatic agent, a release agent, a binder, and a crosslinking agent, in a solvent to prepare an antistatic layer composition, and then applying the composition to one side of the substrate film.
[0080] The antistatic layer composition is preferably formed by coating one side of the substrate film as an aqueous coating liquid (water-soluble or water-dispersible resin using water as a medium). However, it is also possible to form the antistatic layer by coating an aqueous coating liquid containing a small amount of an organic solvent. Examples of organic solvents include alcohols such as ethanol, isopropanol, ethylene glycol, and glycerin, ethers such as ethyl cellosolve, t-butyl cellosolve, propylene glycol monomethyl ether, and tetrahydrofuran, ketones such as acetone and methyl ethyl ketone, esters such as ethyl acetate, and amines such as dimethylethanolamine. These can be used alone or in combination. By appropriately selecting and adding these organic solvents to the aqueous coating liquid as necessary, the stability, coatability, or coating film properties of the coating liquid can be improved.
[0081] The antistatic layer composition can be applied to the substrate film using a reverse roll coater, gravure coater, rod coater, air doctor coater or other coating device, as shown in, for example, "Coating Method" by Harazaki Yuji, Maki Shoten, published in 1979.
[0082] Regarding the drying and curing conditions when forming an antistatic layer on a substrate film, for example, when a coating layer is provided by off-line coating, it is usually recommended to carry out heat treatment at 80 to 200° C. for 3 to 40 seconds, preferably at 100 to 180° C. for 3 to 40 seconds. On the other hand, when an antistatic layer is provided by in-line coating, it is usually recommended to carry out heat treatment at 70 to 270° C. for 3 to 200 seconds.
[0083] Regardless of whether off-line coating or in-line coating is used, heat treatment and irradiation with active energy rays such as ultraviolet rays may be used in combination, if necessary. The surface of the polyester film may be previously subjected to a surface treatment such as a corona treatment or a plasma treatment.
[0084] (Release film properties) (Mold releasability) In the release film roll of the present invention, the peel strength between the surface of the release layer and the acrylic adhesive tape under the conditions of a tensile speed of 300 mm / min and 180° peeling is preferably 80 mN / cm or less, more preferably 60 mN / cm or less, and even more preferably 40 mN / cm or less. When the peel strength is 80 mN / cm or less, the peelability from the adhesive layer of the adhesive tape or the like is good, and the film can be suitably used as a protective layer of the adhesive tape or the like. The peel strength can be specifically measured by the method described in the Examples.
[0085] (Antistatic) The antistatic properties of a laminate film can be evaluated by measuring the surface resistivity of the antistatic layer surface. The lower the surface resistivity of the antistatic layer, the better the antistatic properties. 12 If the resistance is less than 1×10 Ω / □, it can be said to have antistatic properties. 8 If it is less than Ω / □, it can be said that the antistatic property is good, and if it is less than 1×10 6 If the surface resistivity is less than Ω / □, it is considered to have very good antistatic properties and is therefore preferable. There is no particular lower limit for the surface resistivity, but taking into account the cost of the conductive agent, it is 1×10 4 It is preferable that the surface resistivity is Ω / □ or more. Specifically, the surface resistivity can be measured by the method described in the Examples.
[0086] The various components in the antistatic layer can be analyzed by, for example, TOF-SIMS, ESCA, fluorescent X-ray analysis, or the like.
[0087] (Blocking resistance) The release film roll of the present invention is arranged so that the release layer and the antistatic layer face each other, and is subjected to a pressure of 10 kg / cm2 The peel strength after 20 hours of treatment in an atmosphere of 40°C and 80%RH under the conditions of a pulling speed of 300 mm / min and 180° peeling is preferably 120 gf / 125 mm width or less, more preferably 100 gf / 125 mm width or less, and even more preferably 80 gf / 125 mm width or less. When the peel strength is 120 gf / 125 mm width or less, the blocking resistance is good, and the film can be smoothly unwound from the release film roll. The peel strength can be specifically measured by the method described in the Examples.
[0088] Since the release film roll of the present invention has the above-mentioned release layer, the adhesive layer has excellent releasability, so that when the film roll of the present invention is peeled off from the adhesive layer, it can be peeled off without leaving any adhesive residue on the release film roll side, and can be suitably used as a protective layer for an adhesive. Moreover, since the release film roll of the present invention has a surface roughness (Sa) of the release layer surface of 20 nm or less, it is possible to prevent the formation of unevenness in the adhesive layer. Furthermore, since the release film roll of the present application has the above-mentioned antistatic layer, it is possible to effectively suppress the generation of static electricity when peeling off the release film from the adhesive layer, and therefore it is possible to prevent contamination such as adhesion of dust to the adhesive layer due to static electricity. The adhesive layer may be an adhesive layer formed from a general-purpose adhesive, and examples of the adhesive include known adhesives such as acrylic adhesives, urethane adhesives, silicone adhesives, and rubber adhesives. EXAMPLES
[0089] The present invention will now be described in more detail with reference to examples, although the present invention is not limited to the examples described below.
[0090] <Measurement and evaluation methods> The methods for measuring and evaluating various physical properties and characteristics are as follows. The results of each measurement and evaluation are summarized in Table 1.
[0091] (1) Intrinsic viscosity (IV) 1 g of polyester was precisely weighed, dissolved in 100 mL of a mixed solvent of phenol / tetrachloroethane = 50 / 50 (mass ratio), and the viscosity was measured at 30 °C using a viscosity (IV) measuring device (Rigo Co., Ltd. "VMS-022UPC·F10").
[0092] (2) Average particle size The powder was observed using a scanning electron microscope (SEM) ("S3400N" manufactured by Hitachi High-Tech Corporation). The size of each particle was measured from the obtained image data, and the average value of 10 points was taken as the average particle size.
[0093] (3) Normal peel strength One side of an acrylic double-sided adhesive tape ("No. 502" manufactured by Nitto Denko Corporation) was attached to the release layer surface of the release film of the examples and comparative examples, cut to a size of 50 mm x 300 mm, and then left to stand at 23°C and 50% RH for 1 hour to prepare a sample for measuring normal peel strength. Thereafter, using a small tabletop tester ("EZ Graph" manufactured by Shimadzu Corporation), the 180° peel strength was measured under the condition of a tensile speed of 300 mm / min, and the peel strength at this time was regarded as the normal peel strength.
[0094] (4) Surface roughness (Sa) On the release layer surface of the release films of the examples and comparative examples, an area of 640 μm x 480 μm was measured under the following measurement conditions using a non-contact surface / layer cross-sectional shape measurement system VertScan (registered trademark) R550GML (manufactured by Ryoka Systems Co., Ltd.), and the arithmetic mean roughness (Sa) of the release layer surface was calculated using the output from fourth-order polynomial correction. (Measurement conditions) CCD camera: SONY HR-50 1 / 3' Objective lens: 20x Lens barrel: 1X Body Zoom Lens: No Relay Wavelength filter: 530 white Measurement mode: Under Wave conditions
[0095] (5) Evaluation of blocking resistance The release layer surface and the antistatic layer surface of the release films of the Examples and Comparative Examples were placed facing each other, and pressed with a press at a pressure of 10 kg / cm. 2 The sample was subjected to pressure for 20 hours under an atmosphere of 40°C and 80% RH to obtain a measurement sample for evaluation of blocking resistance. Thereafter, using a peeling device ("AGI" manufactured by Shimadzu Corporation), the peel force was measured under the conditions of a tensile speed of 300 mm / min and 180° peeling, and the peel force at this time was used as an index of blocking resistance. Note that the smaller the peel force, the better the blocking resistance is judged to be.
[0096] (6)Surface resistivity For the release films of the examples and comparative examples, a low resistance resistivity meter "Loresta GP MCP-T600" (manufactured by Nitto Seiko Analytech Co., Ltd.) was used to measure the surface resistivity after conditioning the sample for 30 minutes in a measurement atmosphere of 23°C and 50% RH. If the resistance value exceeded the upper limit of the measurable range, it was deemed unmeasurable.
[0097] The raw materials of the base film in the release film in each of the Examples and Comparative Examples are as follows. (Base film) [Polyester (A)] 100 parts by mass of dimethyl terephthalate, 55 parts by mass of ethylene glycol, and 0.07 parts by mass of calcium acetate monohydrate were placed in a reactor, and the temperature was raised while distilling off methanol to carry out an ester exchange reaction. After the reaction started, the temperature was raised to 230°C over about 4 and a half hours, and the ester exchange reaction was essentially completed. Next, 0.04 parts by mass of phosphoric acid and 0.035 parts by mass of antimony trioxide were added, and polymerization was carried out according to a conventional method. That is, the reaction temperature was gradually increased to a final temperature of 280°C, while the pressure was gradually reduced to a final temperature of 0.05 mmHg. After 4 hours, the reaction was terminated, and the polyester (A) was obtained by chipping according to a conventional method. The obtained intrinsic viscosity was 0.63 dL / g. [Polyester (B)] Silica particles having an average particle size of 2 μm were added to the polyester (A) to obtain polyester (B) containing 0.2% by mass of silica particles. The intrinsic viscosity was 0.65 dL / g.
[0098] [Example 1] The surface layer was made of a mixture of 90 parts by mass of polyester (A) and 10 parts by mass of polyester (B), and the base layer was made of only polyester (A). The mixture was fed to two extruders and melted at 285°C. The mixture was then co-extruded on a cooling roll set at 40°C in a layer structure of two kinds and three layers (surface layer / base layer / surface layer=1 / 8 / 1 discharge amount (mass ratio)) and cooled and solidified to obtain an unstretched sheet. The film was then stretched 3.4 times in the longitudinal direction at a film temperature of 85°C using the roll peripheral speed difference, and the coating solution of the antistatic layer composition 1 described below was applied to one side of the longitudinally stretched film, which was introduced into a tenter and stretched 4.3 times in the transverse direction at 110°C. The film was then heat-treated at 235°C. The film was then relaxed 2% in the transverse direction. A 75μm thick polyester film having an antistatic layer with a film thickness (after drying) of 28nm was obtained as a base film.
[0099] (Antistatic Layer Composition 1) The following (E) , (D1) , (F) and (G) in a mass ratio (E) / (D1) The components were mixed in a ratio of / (F) / (G)=7 / 10 / 68 / 15 to obtain antistatic layer composition 1. (E) Thiophene-based antistatic agents The conductive agent "Orgacon ICP1010" (manufactured by Agfa-Gevaert, an aqueous dispersion of polyethylenedioxythiophene and polystyrene sulfonic acid) was neutralized with concentrated aqueous ammonia to a pH of 9. (D1) Long chain alkyl release agent 200 parts by mass of xylene and 600 parts by mass of octadecyl isocyanate were added to a four-neck flask and heated under stirring. From the point when xylene started to reflux, 100 parts by mass of polyvinyl alcohol with an average degree of polymerization of 500 and a degree of saponification of 88 mol% was added in small portions at 10-minute intervals over about 2 hours. After the addition of polyvinyl alcohol was completed, the mixture was refluxed for another 2 hours to terminate the reaction. The reaction mixture was cooled to about 80°C, and methanol was added to precipitate the reaction product as a white precipitate, which was then recovered by filtration. 140 parts by mass of xylene was added to the recovered reaction product, which was heated to completely dissolve it, and then methanol was added again to precipitate it. This operation was repeated several times, and the reaction product was washed with methanol, dried and crushed, and then collected. (D1) As a result, a long chain alkyl type release agent of (F) Binder resin: Aqueous dispersion of polyester resin having a condensed polycyclic structure copolymerized with the following composition: Monomer composition: (acid component) 2,6-naphthalenedicarboxylic acid / 5-sodium sulfoisophthalic acid / (diol component) ethylene glycol / diethylene glycol = 92 / 8 / / 80 / 20 (molar ratio) (G) Other additives: Polyglycerin with an average degree of polymerization of 4
[0100] Next, the following release layer composition was applied to the side opposite the side of the base film on which the antistatic layer was formed, and heat-treated at 150°C for 30 seconds to obtain the release film of Example 1 having a non-silicone release layer with a thickness (after drying) of 0.2 μm. (Release Layer Composition) (A) 99.0 parts by mass of ethylene-propylene copolymer B1 as a non-reactive polyolefin, (B) 1.0 part by mass of "Polytail H" (manufactured by Mitsubishi Chemical Corporation) as a reactive polyolefin, and toluene were mixed and heated to obtain a toluene solution with a concentration of 2%. Next, (C) "Mytech 718A" (manufactured by Mitsubishi Chemical Corporation) was added as a crosslinking agent so that the amount of isocyanate groups was 1.1 equivalents relative to the amount of hydroxyl groups contained in the reactive polyolefin, and 1 part by mass of 1,4-diazabicyclo[2.2.2]octane was added as a urethane catalyst relative to 100 parts by mass of the total solid content of the non-reactive polyolefin and the reactive polyolefin to obtain a release layer composition.
[0101] (A): Non-reactive polyolefin: Ethylene-propylene copolymer B1 Ethylene-propylene random copolymer obtained by metallocene catalyst ( 1 Composition by H-NMR: ethylene / propylene = 74 / 26, MFR (230°C, load 2.16 kg) 2.0 g / 10 min, density 0.86 g / cm 3 ). (B): Reactive polyolefin: "Polytail H" (manufactured by Mitsubishi Chemical Corporation, hydrogenated polybutadiene having OH groups, number average molecular weight 2700, OH group amount determined by NMR 1.5% by mass, density 0.85 g / cm 3 ) (C): Crosslinking agent: "Mytec 718A" (manufactured by Mitsubishi Chemical Corporation, 76% by mass butyl acetate solution of aliphatic trifunctional isocyanate-triol adduct) Urethane catalyst: 1,4-diazabicyclo[2.2.2]octane (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.)
[0102] [Example 2] A release film of Example 2 was obtained in the same manner as in Example 1, except that the antistatic layer composition 1 in Example 1 was changed to the following antistatic layer composition 2. (Antistatic Layer Composition 2) In the antistatic layer composition 1, (D1) The following (D2)Antistatic layer composition 2 was obtained in the same manner except for changing the above. (D2) Fluorine-based release agent In a glass reaction vessel, CF3 (CF2), a perfluoroalkyl group-containing acrylate, n CH2CH2OCOCH=CH2 (n = 5-11, average of n = 9) 80.0 g, acetoacetoxyethyl methacrylate 20.0 g, dodecyl mercaptan 0.8 g, deoxygenated pure water 354.7 g, acetone 40.0 g, C 16 H 33 1.0g of N(CH3)3Cl and C8H 17 C6H4O(CH2CH2O) n 3.0 g of H (n=8) was added, and 0.5 g of azobisisobutylamidine dihydrochloride was added, and the mixture was subjected to copolymerization reaction at 60° C. for 10 hours with stirring under a nitrogen atmosphere to obtain a copolymer emulsion of a fluorine compound.
[0103] [Comparative Example 1] A release film of Comparative Example 1 was obtained in the same manner as in Example 1, except that the antistatic layer composition 1 in Example 1 was changed to the following antistatic layer composition 3. (Antistatic Layer Composition 3) In the antistatic layer composition 1, (D1) The following (D3) Antistatic layer composition 3 was obtained in the same manner except for changing the above. (D3) Wax-based release agent: Oxidized polyethylene wax (melting point: 129°C)
[0104] [Comparative Example 2] A release film of Comparative Example 2 was obtained in the same manner as in Example 1, except that the antistatic layer composition 1 in Example 1 was changed to the following antistatic layer composition 4. (Antistatic Layer Composition 4) In the antistatic layer composition 1, (D1) Instead of using the above (E) , (F) and (G) in a mass ratio (E) The components were mixed in a ratio of / (F) / (G)=7 / 10 / 83 to obtain antistatic layer composition 4.
[0105] [Comparative Example 3] A release film of Comparative Example 3 was obtained in the same manner as in Example 1, except that the antistatic layer composition was not applied.
[0106] [Table 1]
[0107] (Consideration) From the results of the Examples and Comparative Examples, it was found that according to the present invention, in a roll-type release film having a highly smooth release layer surface, both blocking resistance and antistatic properties can be achieved. In particular, it has been found that good characteristics can be achieved by using a long-chain alkyl-based release agent or a fluorine-based release agent as the antistatic layer composition and by using a thiophene-based antistatic agent in combination as the antistatic agent. Among them, the combination of a long-chain alkyl release agent and a thiophene antistatic agent is the most favorable. Although the mechanism is unclear, it is presumed that when the antistatic layer is formed, the long-chain alkyl group is appropriately oriented on the surface of the antistatic layer, and at the same time, the release agent component is present on the surface and the thiophene antistatic agent is also present on the surface in an appropriate amount, so that the balance between release property and antistatic property can be maintained. On the other hand, in the case of a combination of a wax-based release agent and a thiophene-based antistatic agent, even among the same non-silicone-based release agents, the blocking resistance tends to decrease, possibly because it is difficult to adjust the balance between releasability and antistatic properties.
Claims
1. The film has a release layer, a base film, and an antistatic layer in this order. the release layer is a cured layer of a release layer composition comprising (A) a non-reactive polyolefin containing 50 to 80% by mass of ethylene units, (B) a reactive polyolefin, and (C) a crosslinking agent; the (C) crosslinking agent is an aliphatic isocyanate having two or more isocyanate groups in one molecule, The surface roughness (Sa) of the release layer is 20 nm or less, the antistatic layer is a cured layer of an antistatic layer composition containing (D) a release agent having a long-chain alkyl group or a fluorine-containing release agent and (E) an antistatic agent; Release film roll.
2. The release film roll according to claim 1 , wherein the reactive polyolefin (B) is a polyolefin polyol.
3. 3. The release film roll according to claim 1, wherein the non-reactive polyolefin (A) is a copolymer of ethylene and an α-olefin.
4. The release film roll according to any one of claims 1 to 3, wherein the (D) release agent having a long-chain alkyl group is a release agent having a long-chain alkyl group having 6 or more carbon atoms.
5. The release film roll according to any one of claims 1 to 4, wherein the (D) release agent having a long-chain alkyl group is a release agent having a long-chain alkyl group having 8 or more carbon atoms.
6. 6. The release film roll according to claim 5, wherein the release agent (D) having a long-chain alkyl group is a release agent having a long-chain alkyl group having 8 or more carbon atoms and having polyvinyl alcohol as a copolymerization component.
7. A release film roll described in any one of claims 1 to 6, wherein the content of the (D) release agent having a long-chain alkyl group or a fluorine-based release agent in the antistatic layer composition is 2 to 12 mass %.
8. The release film roll according to any one of claims 1 to 7, wherein the (E) antistatic agent is thiophene or a thiophene derivative.
9. A release film roll described in any one of claims 1 to 8, wherein the content of the antistatic agent (E) in the antistatic layer composition is 5 to 40 mass %.
10. The release film roll according to any one of claims 1 to 9, wherein the antistatic layer is a cured layer of an antistatic layer composition further comprising a binder (F).
11. The release film roll according to any one of claims 1 to 10, wherein the surface roughness (Sa) of the base film surface is 20 nm or less.
12. The release film roll according to any one of claims 1 to 11, wherein the base film is a polyester film.
13. The release layer and the antistatic layer were placed facing each other, and a pressure of 10 kg / cm 2 The release film roll according to any one of claims 1 to 12, wherein the release film roll has a peel force of 120 gf / 125 mm width or less under conditions of a pulling speed of 300 mm / min and 180° peeling after being pressed for 20 hours in an atmosphere of 40° C. and 80% RH.
14. The release film roll according to any one of claims 1 to 13, which is for protecting an adhesive layer.
Citation Information
Patent Citations
Release film
JP1998086289A
Mold release sheet and adhesive material
JP2001246697A
Mold release film having antistatic properties and its manufacturing method
JP2005153250A
Mold release sheet
JP2009101680A
Release agent, release material, and adhesive tape
JP2011052207A