Liquid crystal alignment agent, liquid crystal alignment film and liquid crystal element

The use of polymers [A], [B], and [C] in a liquid crystal aligning agent addresses peeling and adhesion issues, enhancing the reliability and reducing afterimages in liquid crystal elements by improving adhesion to both sealant and base material.

JP7593242B2Active Publication Date: 2024-12-03JSR CORPORATION
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021098776
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-07-29
Filing Date
2021-06-14
Publication Date
2024-12-03
Estimated Expiration
2041-06-14

AI Technical Summary

Technical Problem

Existing liquid crystal alignment films face issues with peeling off at the sealant portion, reduced adhesion to the base material, and increased brittleness due to the introduction of meta-arylene structures, which affect the reliability and afterimage performance of liquid crystal elements.

Method used

A liquid crystal aligning agent comprising polymers with specific structural units, including polymers [A], [B], and [C], which provide enhanced adhesion to both the sealant and base material while reducing afterimages, particularly through the use of polymers with partial structures represented by formulas (1) and (2) and a nitrogen-containing non-aromatic heterocyclic group.

Benefits of technology

The solution results in a liquid crystal alignment film with improved adhesion to the sealant and base material, reducing afterimages and enhancing the reliability of liquid crystal elements, particularly in areas with spacers, while maintaining film strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593242000001
    Figure 0007593242000001
  • Figure 0007593242000002
    Figure 0007593242000002
  • Figure 0007593242000003
    Figure 0007593242000003
Patent Text Reader

Abstract

To provide a liquid crystal alignment agent capable of forming a liquid crystal alignment film excellent in adhesion property between a sealant and a substrate and providing a liquid crystal element hardly generating afterimage.SOLUTION: Liquid crystal alignment agent contains a polymer [A] with partial structure represented by formula (1), a polymer [B] with partial structure represented by formula (2), and a polymer [C] with partial structure X as main chain. In the structure represented by partial structure X:-(CH2)a- or the structure represented by -(CH2)a-, any methylene group is substituted by groups such as -NR7-. In the formula (1), R1 represents protective group. In the formula (2), A1 and A4 each independently represents divalent aromatic ring group. R2 and R3 each independently represents hydrogen atom or monovalent organic group. B1 represents single bond, -NR4-, -O- or divalent aromatic heterocyclic group.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a liquid crystal aligning agent, a liquid crystal alignment film, and a liquid crystal device. [Background technology]

[0002] As the liquid crystal material for liquid crystal elements, negative type liquid crystal is used in liquid crystal elements of the VA driving system, MVA driving system, etc., while positive type liquid crystal is used in liquid crystal elements of the TN type, IPS (In-Plane Switching) driving system, FFS (Fringe Field Switching) driving system, etc. In recent years, it has also been proposed to use negative type liquid crystal in liquid crystal elements of the IPS driving system or FFS driving system in order to achieve even higher resolution of liquid crystal elements (for example, see Patent Document 1).

[0003] In recent years, liquid crystal elements have been applied to a wide range of applications, from relatively large display devices such as liquid crystal televisions and information displays to small display devices such as smartphones. As liquid crystal elements are used in a wider variety of applications, there is a demand for even higher quality liquid crystal elements. In light of this, it has been proposed to incorporate a polymer having a nitrogen-containing metharylene structure into a liquid crystal alignment agent, thereby obtaining a liquid crystal alignment film with low resistance and high transparency, and to obtain a liquid crystal element with little burn-in (DC afterimage) caused by accumulated charges (see, for example, Patent Document 2).

[0004] In touch panel display devices such as smartphones and tablet PCs, efforts are being made to narrow the frame in order to achieve both a larger operating area for the touch panel and a smaller display device. One method for narrowing the frame is known in which a liquid crystal alignment film is formed over the entire surface of a substrate, and then a sealant is applied onto the liquid crystal alignment film to bond the substrates together (see, for example, Patent Document 3). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2016 / 152928 [Patent Document 2] International Publication No. 2019 / 093037 [Patent Document 3] JP 2013-109154 A Summary of the Invention [Problem to be solved by the invention]

[0006] When a sealant is placed on the liquid crystal alignment film for the purpose of narrowing the frame of the liquid crystal element, the liquid crystal alignment film tends to peel off from the substrate at the sealant portion, which may reduce the reliability of the liquid crystal element.

[0007] In addition, when attempting to reduce image retention in liquid crystal elements by introducing a methaarylene structure into a polymer, as in the technology of Patent Document 2, there is a concern that the liquid crystal alignment film will become hard and brittle due to the structure containing many aromatic rings derived from the methaarylene structure, and the adhesion between the liquid crystal alignment film and the substrate (particularly, the adhesion to the substrate at the spacer site) will decrease. On the other hand, it is difficult to simultaneously satisfy multiple characteristics such as reduction of image retention, adhesion to the substrate, and adhesion to the sealant, and there is room for further improvement in the liquid crystal alignment agent.

[0008] The present invention has been made in consideration of the above problems, and has as its main object to provide a liquid crystal alignment agent that can form a liquid crystal alignment film that has excellent adhesion to a sealant and a substrate, and can obtain a liquid crystal element that is less likely to produce an afterimage. [Means for solving the problem]

[0009] The present inventors have conducted extensive research to solve the above problems, and have found that the above problems can be solved by using a plurality of polymers having different structures, thereby completing the present invention. Specifically, the present invention provides the following means.

[0010] <1> A liquid crystal aligning agent comprising: a polymer [A] having a partial structure represented by the following formula (1) and not having a partial structure represented by the following formula (2); a polymer [B] having a partial structure represented by the following formula (2); and a polymer [C] having the following partial structure X in its main chain and not having the partial structure represented by the following formula (1) and not having the partial structure represented by the following formula (2). Substructure X:-(CH 2 ) a - (wherein a is an integer of 2 to 20), or -(CH 2 ) a In the structure represented by -, any methylene group is -NR 7 -, -O-, -COO-, -NR 7 -CO-, -NR 7 -COO-, -NR 8 -CO-NR 9 - and a nitrogen-containing non-aromatic heterocyclic group (wherein R 7 is a hydrogen atom or an alkyl group. 8 and R 9 are each independently a hydrogen atom or an alkyl group, or R 8 and R 9 and are combined together to form R 8 The nitrogen atom to which R is bonded 9 represents a ring structure formed together with the nitrogen atom to which -NR is bonded and -CO-. 7 -, -O-, -COO-, -NR 7 -CO-, -NR 7 -COO-, -NR 8 -CO-NR 9 - and the nitrogen-containing non-aromatic heterocyclic groups are not adjacent to one another). [ka] (In formula (1), R 1 is a protecting group. "*" represents a bond.) [ka] (In formula (2), A 1 and A 4R is each independently a divalent aromatic ring group. 2 and R 3 are each independently a hydrogen atom or a monovalent organic group. 1 is a single bond, -NR 4 R is -, -O- or a divalent aromatic heterocyclic group. 4 is a hydrogen atom or a monovalent organic group. 1 If is a single bond, A 2 is a divalent aromatic ring group, A 3 is a single bond or a divalent aromatic ring group. 1 When A is a divalent aromatic heterocyclic group, 2 and A 3 are each independently a single bond or a divalent aromatic ring group. 1 Ga-NR 4 - or -O-, then A 2 and A 3 are each independently a divalent aromatic ring group, or A 2 The aromatic ring of A 3 is linked to an aromatic ring by a single bond or a chain structure, 4 It represents a nitrogen- or oxygen-containing condensed ring structure formed together with - or -O-. "*" represents a bond.)

[0011] <2> the above <1> A liquid crystal alignment film formed by the liquid crystal alignment agent. <3> A liquid crystal alignment film comprising: a polymer having a structural unit including a partial structure represented by the following formula (1A) in a part other than a group involved in polymerization and not having a partial structure represented by the following formula (2); a polymer having a partial structure represented by the following formula (2); and a polymer having the following partial structure X in its main chain and not having the partial structure represented by the following formula (2). [ka] (In formula (1A), "*" represents a bond.) <4> the above <2> or <3> A liquid crystal element comprising the liquid crystal alignment film. Effect of the Invention

[0012] According to the liquid crystal aligning agent of the present invention, a liquid crystal alignment film having excellent adhesion to a sealant and a substrate can be formed, and a liquid crystal element in which image retention is unlikely to occur can be obtained. In particular, according to the liquid crystal aligning agent of the present invention, the adhesion between the substrate and the liquid crystal alignment film in the spacer arrangement portion can be improved. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The liquid crystal aligning agent of the present disclosure contains three types of polymers having different monomer compositions, namely, polymer [A], polymer [B], and polymer [C]. Each component contained in the liquid crystal aligning agent of the present disclosure and other components that are optionally blended as necessary will be described below.

[0014] In this specification, the term "hydrocarbon group" includes chain-shaped hydrocarbon groups, alicyclic hydrocarbon groups, and aromatic hydrocarbon groups. The term "chain-shaped hydrocarbon group" means a straight-chain hydrocarbon group and a branched hydrocarbon group that do not include a cyclic structure in the main chain and are composed only of a chain structure. However, they may be saturated or unsaturated. The term "alicyclic hydrocarbon group" means a hydrocarbon group that includes only an alicyclic hydrocarbon structure as a ring structure and does not include an aromatic ring structure. However, it is not necessary to be composed only of an alicyclic hydrocarbon structure, and it also includes those that have a chain structure as a part. The term "aromatic hydrocarbon group" means a hydrocarbon group that includes an aromatic ring structure as a ring structure. However, it is not necessary to be composed only of an aromatic ring structure, and it may include a chain structure or an alicyclic hydrocarbon structure as a part. The term "aromatic ring" includes aromatic hydrocarbon rings and aromatic heterocycles. The term "structural unit" means a unit that mainly constitutes the main chain structure, and at least two or more units are included in the main chain structure. Unless otherwise specified, each component and compound may be used alone or in combination of two or more. The term "protecting group" refers to an atomic group that temporarily converts a highly reactive characteristic group (-NH- in the following formula (1)) into an inactive functional group.

[0015] <Polymer [A]> The polymer [A] is a polymer having a partial structure represented by the following formula (1). [ka] (In formula (1), R 1 is a protecting group. "*" represents a bond.)

[0016] In the above formula (1), R 1 The protecting group of R is preferably a monovalent group which is detached by heat, and examples thereof include carbamate-based protecting groups, amide-based protecting groups, imide-based protecting groups, and sulfonamide-based protecting groups. Among these, R 1 is preferably a carbamate-based protecting group. Specific examples of the protecting group include a tert-butoxycarbonyl group (Boc group), a benzyloxycarbonyl group, a 1,1-dimethyl-2-haloethyloxycarbonyl group, an allyloxycarbonyl group (Alloc group), a 2-(trimethylsilyl)ethoxycarbonyl group, and a 9-fluoronylmethyloxycarbonyl group (F-moc group). Among these, the tert-butoxycarbonyl group is particularly preferred because it has excellent thermal detachment properties, can enhance the effect of improving adhesion to a sealing agent, and can reduce the amount of the deprotected portion remaining in the film.

[0017] In addition, in the above formula (1), one of the two "*"s may be bonded to a hydrogen atom. In other words, one of the two "*"s in the above formula (1) may be bonded to a hydrogen atom and the other may be bonded to a carbon atom. Alternatively, both of the two "*"s may be bonded to carbon atoms.

[0018] The polymer [A] preferably has the following partial structure Y in addition to the partial structure represented by the above formula (1). When the polymer [A] further has the partial structure Y, it is preferable in that it can suppress not only DC image retention but also AC image retention caused by deviation of the alignment direction of the liquid crystal from the initial alignment. Substructure Y:-(CH 2 ) b - (wherein b is an integer of 2 to 20), or -(CH 2 ) bIn the structure represented by -, any methylene group is -NR 10 -, -O-, -COO-, -NR 10 -CO-, -NR 10 -COO-, -NR 10 -CO-NR 11 - and a nitrogen-containing non-aromatic heterocyclic group (wherein R 10 and R 11 are each independently a hydrogen atom or a monovalent organic group. 10 -, -O-, -COO-, -NR 10 -CO-, -NR 10 -COO-, -NR 10 -CO-NR 11 - and the nitrogen-containing aromatic heterocyclic groups are not adjacent to one another).

[0019] From the viewpoint of enhancing the effect of improving AC image retention in a liquid crystal element, b in the partial structure Y is preferably 2 or more, and it is more preferable that the partial structure Y contains a linear alkanediyl group having 2 or more carbon atoms. Moreover, from the viewpoint of suppressing a decrease in film strength, b is preferably 12 or less, and more preferably 10 or less. R 10 , R 11 When R is a monovalent organic group, the monovalent organic group is preferably a monovalent hydrocarbon group or a protecting group having 1 to 10 carbon atoms. The monovalent hydrocarbon group is preferably an alkyl group or a phenyl group having 1 to 3 carbon atoms, more preferably an alkyl group having 1 to 3 carbon atoms. Illustrative and preferred examples of the protecting group include R 1 The above description of the above can be used. Of the above, R 10 , R 11 is preferably a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or a tert-butoxycarbonyl group. Examples of the nitrogen-containing non-aromatic heterocyclic group include a piperidine-1,4-diyl group and a piperazine-1,4-diyl group.

[0020] The polymer [A] may have a partial structure represented by the above formula (1) separately from the partial structure Y, or may have the partial structure represented by the above formula (1) in the partial structure Y. When the partial structure Y has the partial structure represented by the above formula (1), the polymer [A] may have a partial structure Y represented by -(CH 2 ) b In the structure represented by -, any methylene group is -NR 10 -, -NR 10 -CO-, -NR 10 -COO- and -NR 10 -CO-NR 11 -, and R 10 and R 11 At least one of the partial structure Y is a protecting group. When the partial structure Y is a protecting group, it is preferable to use a monomer having the partial structure Y in the production of the polymer [A], since it is possible to improve adhesion to a sealant and reduce AC image retention at the same time. It is preferable that the polymer [A] has the partial structure Y in the main chain, since it is possible to enhance the effect of improving the reduction of AC image retention in a liquid crystal element. The polymer [A] does not have the partial structure represented by the following formula (2) that the polymer [B] has.

[0021] In this specification, the phrase "not having" a partial structure (hereinafter referred to as "specific structure") that at least one of the multiple polymers contained in the liquid crystal alignment agent has means that it is acceptable for the other polymer to have the specific structure within a range that does not impair the effects of the present invention. When the other polymer does not have a specific structure, the content of the specific structure in the other polymer is preferably 1 mol % or less, more preferably 0.5 mol % or less, and even more preferably 0.1 mol or less, based on the total structural units of the other polymer (the same applies to polymer [B] and polymer [C]).

[0022] The main chain of the polymer [A] is not particularly limited, but from the viewpoints of forming a liquid crystal alignment film having high affinity with liquid crystals and mechanical strength and high reliability, and of facilitating the introduction of the partial structure represented by the above formula (1) into the polymer, it is preferable that the polymer [A] be at least one selected from the group consisting of polyamic acid, polyamic acid ester, and polyimide.

[0023] The method for producing the polymer [A] is not particularly limited, and can be carried out according to a standard method of organic chemistry. Specifically, for example, a method of polymerization using a monomer having a partial structure represented by the above formula (1); a method of reacting a polymer end with a compound having a partial structure represented by the above formula (1) to introduce the partial structure represented by the above formula (1) into the polymer end, etc. can be mentioned. Among these, it is preferable to produce the polymer [A] by polymerization using a monomer having a partial structure represented by the above formula (1) in terms of being able to enhance the effect of improving the adhesion between the liquid crystal alignment film and the sealant. That is, it is preferable that the polymer [A] is a polymer having a structural unit derived from a monomer having a partial structure represented by the above formula (1).

[0024] The term "main chain" refers to the "trunk" portion of a polymer, which is the longest chain of atoms. It is permissible for this "trunk" portion to contain a ring structure. For example, "having a specific structure in the main chain" means that the specific structure constitutes a part of the main chain. The term "side chain" refers to a portion branched off from the "trunk" of a polymer.

[0025] (Polyamic acid) When the polymer [A] is a polyamic acid, the polyamic acid (hereinafter also referred to as "polyamic acid [A]") is preferably produced by a method of reacting a tetracarboxylic dianhydride with a diamine compound containing a diamine having a partial structure represented by the above formula (1) (hereinafter also referred to as "specific diamine (A)"), in terms of high freedom in monomer selection and ease of introducing the partial structure represented by the above formula (1).

[0026] Tetracarboxylic acid dianhydride Examples of the tetracarboxylic dianhydride used in the synthesis of the polyamic acid [A] include aliphatic tetracarboxylic dianhydrides, alicyclic tetracarboxylic dianhydrides, and aromatic tetracarboxylic dianhydrides. Specific examples of these include aliphatic tetracarboxylic dianhydrides such as 1,2,3,4-butanetetracarboxylic dianhydride and ethylenediaminetetraacetic dianhydride; alicyclic tetracarboxylic dianhydrides such as 1,2,3,4-cyclobutanetetracarboxylic dianhydride, 1,3-dimethyl-1,2,3,4-cyclobutanetetracarboxylic dianhydride, 2,3,5-tricarboxycyclopentylacetic dianhydride, 5-(2,5-dioxotetrahydrofuran-3-yl)-3a,4,5,9b-tetrahydronaphtho[1,2-c]furan-1,3-dione, 5-(2,5-dioxotetrahydrofuran-3-yl)-8-methyl-3a,4,5,9b-tetrahydronaphtho[1,2-c]furan-1,3-dione, and the like. -dione, 2,4,6,8-tetracarboxybicyclo[3.3.0]octane-2:4,6:8-dianhydride, cyclopentane tetracarboxylic dianhydride, cyclohexane tetracarboxylic dianhydride, and the like; as aromatic tetracarboxylic dianhydrides, pyromellitic dianhydride, 3,3',4,4'-biphenyl tetracarboxylic dianhydride, 4,4'-(hexafluoroisopropylidene)diphthalic anhydride, ethylene glycol bisanhydrotrimate, 4,4'-(hexafluoroisopropylidene)diphthalic anhydride, 4,4'-carbonyldiphthalic anhydride, and the like can be mentioned; and in addition, the tetracarboxylic dianhydrides described in JP-A-2010-97188 can be used.

[0027] The tetracarboxylic dianhydride used in the synthesis of the polyamic acid [A] preferably contains an alicyclic tetracarboxylic dianhydride, since it has high solubility in a solvent and can provide a liquid crystal alignment film exhibiting low image retention. The proportion of the alicyclic tetracarboxylic dianhydride used is preferably 20 mol % or more, more preferably 40 mol % or more, and even more preferably 50 mol % or more, based on the total amount of the tetracarboxylic dianhydride used in the synthesis of the polyamic acid [A].

[0028] Diamine compounds The specific diamine (A) used in the synthesis of the polymer [A] is preferably a compound represented by the following formula (1-1). [ka] (In formula (1-1), A 7 and A 8 Each of Y is independently a divalent aromatic ring group. 1 is a divalent organic group. r is 0 or 1. However, when r is 1, A 7 , A 8 and Y 1 At least one of A has a partial structure represented by the above formula (1). 7 has a partial structure represented by the above formula (1).

[0029] In the above formula (1-1), A 7 and A 8 Examples of the divalent aromatic ring group include a divalent aromatic hydrocarbon group and a divalent aromatic heterocyclic group. 7 and A 8 may have a substituent in the aromatic ring portion. Examples of the substituent include an alkyl group having 1 to 5 carbon atoms, a halogen atom, and a monovalent group having a partial structure represented by the above formula (1).

[0030] A 7 , A 8 Specific preferred examples of the divalent aromatic hydrocarbon group include a group obtained by removing any two hydrogen atoms bonded to carbon atoms constituting a benzene ring, a naphthalene ring, or an anthracene ring; and a divalent aromatic heterocyclic group include a group obtained by removing any two hydrogen atoms bonded to carbon atoms constituting a pyridine ring, a pyrimidine ring, a pyridazine ring, or a pyrazine ring. 7 , A 8 is preferably a substituted or unsubstituted phenylene group, biphenylene group or pyridinylene group.

[0031] Y 1As a divalent organic group, -(CH 2 ) b -, -(CH 2 ) b In the structure represented by -, any methylene group is -NR 10 -, -O-, -COO-, -NR 10 -CO-, -NR 10 -COO-, -NR 10 -CO-NR 11 - and a nitrogen-containing non-aromatic heterocyclic group; 10 -, -NR 10 -CO-, -NR 10 -COO-, -NR 10 -CO-NR 11 Among these, Y 1 is -(CH 2 ) b In the structure represented by -, any methylene group is -NR 10 -, -NR 10 -CO-, -NR 10 -COO- and -NR 10 -CO-NR 11 - is preferably a structure in which R 10 and R 11 When both are groups different from the protecting group, A 7 and A 8 At least one of Y has a partial structure represented by the above formula (1) as a substituent introduced into the aromatic ring. 1 does not have an aromatic ring group. r is 0 or 1, with 1 being more preferred.

[0032] Specific examples of the specific diamine (A) include compounds represented by the following formulas (DA-1) to (DA-12). [ka] [ka] (In the formula, "Boc" represents a tert-butoxycarbonyl group, "Alloc" represents an allyloxycarbonyl group, and "F-moc" represents a 9-fluoronylmethyloxycarbonyl group.)

[0033] Of the above, the specific diamine (A) is preferably a compound represented by each of the above formulas (DA-1) to (DA-10), and more preferably a compound represented by each of the above formulas (DA-1), (DA-3) to (DA-6), and (DA-8).

[0034] The diamine compound used in the synthesis of the polyamic acid [A] may be the specific diamine (A) alone, but may also be used together with the specific diamine (A) and a diamine different from the specific diamine (A) (hereinafter also referred to as "other diamine (A)"). Examples of the other diamine (A) include aliphatic diamines, alicyclic diamines, aromatic diamines, and diaminoorganosiloxanes. Specific examples of other diamines (A) include diamine compounds having a partial structure Y in the main chain, such as 4,4'-diaminodiphenylethane, 4,4'-diaminodiphenylpropane, 1,5-bis(4-aminophenoxy)pentane, 1,2-bis(4-aminophenoxy)ethane, 1,3-bis(4-aminophenoxy)propane, 1,6-bis(4-aminophenoxy)hexane, 6,6'-(pentamethylenedioxy)bis(3-aminopyridine), 4'-(2-(4-aminophenoxy)ethoxy)-[1,1'-biphenyl]-4-amine, and 1,3-bis(3-aminopropyl)-tetramethyldisiloxane; Examples of the diamine compound include diamine compounds that do not have a partial structure Y in the main chain, such as o-phenylenediamine, m-phenylenediamine, p-phenylenediamine, 4,4'-diaminodiphenylmethane, 4-aminophenyl-4-aminobenzoate, 2,5-diaminobenzoic acid, 3,5-diaminobenzoic acid, 4,4'-diaminodiphenyl ether, 2,2'-dimethyl-4,4'-diaminobiphenyl, and 3,5-diamino-N,N-bis(pyridin-3-ylmethyl)benzamide.

[0035] In the synthesis of the polyamic acid [A], the amount of the specific diamine (A) used is preferably 10 mol % or more, more preferably 20 mol % or more, even more preferably 25 mol % or more, and particularly preferably 35 mol % or more, based on the total amount of the diamine compounds used in the synthesis of the polyamic acid [A], from the viewpoint of obtaining a sufficient effect of improving adhesion to a sealing agent. In addition, the amount of the diamine having the partial structure Y used (however, when the specific diamine (A) has the partial structure Y, the total amount of the specific diamine (A) and the diamine compounds having the partial structure Y in the main chain among the other diamines (A)) is, from the viewpoint of obtaining a sufficient improvement effect in reducing AC image retention, preferably 10 mol % or more, more preferably 20 mol % or more, even more preferably 30 mol % or more, and particularly preferably 40 mol % or more, based on the total amount of the diamine compounds used in the synthesis of the polyamic acid [A].

[0036] Synthesis of polyamic acid The polyamic acid [A] can be obtained by reacting a tetracarboxylic dianhydride with a diamine compound, optionally together with a molecular weight modifier. In the synthesis reaction of the polyamic acid, the ratio of the tetracarboxylic dianhydride to the diamine compound is preferably such that the acid anhydride group of the tetracarboxylic dianhydride is 0.2 to 2 equivalents per equivalent of the amino group of the diamine compound. Examples of the molecular weight modifier include acid monoanhydrides such as maleic anhydride, phthalic anhydride, and itaconic anhydride, monoamine compounds such as aniline, cyclohexylamine, and n-butylamine, and monoisocyanate compounds such as phenyl isocyanate and naphthyl isocyanate. The ratio of the molecular weight modifier to be used is preferably 20 parts by mass or less per 100 parts by mass of the total of the tetracarboxylic dianhydride and diamine compound used.

[0037] The synthesis reaction of polyamic acid is preferably carried out in an organic solvent. The reaction temperature is preferably -20°C to 150°C, and the reaction time is preferably 0.1 to 24 hours. Examples of organic solvents used in the reaction include aprotic polar solvents, phenolic solvents, alcoholic solvents, ketone solvents, ester solvents, ether solvents, halogenated hydrocarbons, and hydrocarbons. Specific examples of these include one or more selected from the group consisting of N-methyl-2-pyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, dimethylsulfoxide, γ-butyrolactone, tetramethylurea, hexamethylphosphortriamide, m-cresol, xylenol, and halogenated phenols, or a mixture of one or more of these with other organic solvents (e.g., butyl cellosolve, diethylene glycol diethyl ether, etc.). The amount of the organic solvent (a) used is preferably an amount such that the total amount (b) of the tetracarboxylic dianhydride and the diamine is 0.1 to 50% by mass based on the total amount (a+b) of the reaction solution.

[0038] In this manner, a polymer solution in which the polyamic acid [A] is dissolved is obtained. This polymer solution may be used as it is for the preparation of a liquid crystal alignment agent, or the polyamic acid [A] contained in the polymer solution may be isolated and then used for the preparation of a liquid crystal alignment agent.

[0039] (Polyamic acid ester) When the polymer [A] is a polyamic acid ester, the polyamic acid ester can be obtained, for example, by a method of reacting a polyamic acid [A] with an esterifying agent, a method of reacting a tetracarboxylic acid diester with a diamine compound containing a specific diamine (A), or a method of reacting a tetracarboxylic acid diester dihalide with a diamine compound containing a specific diamine (A). The polyamic acid ester may have only an amic acid ester structure, or may be a partially esterified product in which an amic acid structure and an amic acid ester structure coexist. The reaction solution in which the polyamic acid ester is dissolved may be used for preparing a liquid crystal alignment agent as it is, or the polyamic acid ester contained in the reaction solution may be isolated and then used for preparing a liquid crystal alignment agent. In this specification, the term "tetracarboxylic acid derivative" includes tetracarboxylic acid dianhydride, tetracarboxylic acid diester, and tetracarboxylic acid diester dihalide.

[0040] (Polyimide) When the polymer [A] is a polyimide, the polyimide can be obtained, for example, by dehydrating and cyclizing the polyamic acid [A] synthesized as described above to convert it into an imidized product. The polyimide may be a complete imidized product in which all amic acid structures of the polyamic acid precursor are dehydrated and cyclized, or a partial imidized product in which only a part of the amic acid structures are dehydrated and cyclized, and an amic acid structure and an imide ring structure coexist. The imidization rate of the polyimide is preferably 20 to 99%, more preferably 30 to 90%. The imidization rate is the ratio of the number of imide ring structures to the total number of amic acid structures and the number of imide ring structures of the polyimide, expressed as a percentage. Here, a part of the imide rings may be isoimide rings.

[0041] The dehydration ring-closing of polyamic acid is preferably carried out by dissolving polyamic acid in an organic solvent, adding a dehydrating agent and a dehydration ring-closing catalyst to the solution, and heating as necessary. In this method, the dehydrating agent may be, for example, an acid anhydride such as acetic anhydride, propionic anhydride, or trifluoroacetic anhydride. The amount of the dehydrating agent used is preferably 0.01 to 20 moles per mole of the amic acid structure of the polyamic acid. The dehydration ring-closing catalyst may be, for example, a tertiary amine such as pyridine, collidine, lutidine, or triethylamine. The amount of the dehydration ring-closing catalyst used is preferably 0.01 to 10 moles per mole of the dehydrating agent used. Examples of organic solvents used in the dehydration ring-closing reaction include the organic solvents exemplified as those used in the synthesis of polyamic acid. The reaction temperature of the dehydration ring-closing reaction is preferably 0 to 180° C. The reaction time is preferably 1.0 to 120 hours. The reaction solution containing the polyimide may be used for the preparation of a liquid crystal aligning agent as it is, or the polyimide may be isolated and then used for the preparation of a liquid crystal aligning agent.

[0042] <Polymer [B]> The polymer [B] is a polymer having a partial structure represented by the following formula (2). [ka] (In formula (2), A 1 and A 4 R is each independently a divalent aromatic ring group. 2 and R 3 are each independently a hydrogen atom or a monovalent organic group. 1 is a single bond, -NR 4 R is -, -O- or a divalent aromatic heterocyclic group. 4 is a hydrogen atom or a monovalent organic group. 1 If is a single bond, A 2 is a divalent aromatic ring group, A 3 is a single bond or a divalent aromatic ring group. 1 When A is a divalent aromatic heterocyclic group, 2 and A 3are each independently a single bond or a divalent aromatic ring group. 1 Ga-NR 4 - or -O-, then A 2 and A 3 are each independently a divalent aromatic ring group, or A 2 The aromatic ring of A 3 is linked to an aromatic ring by a single bond or a chain structure, 4 It represents a nitrogen- or oxygen-containing condensed ring structure formed together with - or -O-. "*" represents a bond.)

[0043] In the above formula (2), A 1 and A 4 Examples of the divalent aromatic ring group include a divalent aromatic hydrocarbon group and a divalent aromatic heterocyclic group. 1 and A 4 A may have a substituent in the aromatic ring portion. Examples of the substituent include an alkyl group having 1 to 5 carbon atoms and a halogen atom. 1 , A 4 Specific preferred examples of the divalent aromatic hydrocarbon group include a group obtained by removing any two hydrogen atoms bonded to carbon atoms constituting a benzene ring, a naphthalene ring, or an anthracene ring; and a divalent aromatic heterocyclic group include a group obtained by removing any two hydrogen atoms bonded to carbon atoms constituting a pyridine ring, a pyrimidine ring, a pyridazine ring, or a pyrazine ring. 1 and A 4 Of these, a phenylene group, a biphenylene group or a pyridinylene group is preferred, and a phenylene group is particularly preferred.

[0044] R 2 and R 3 In the above, the monovalent organic group is preferably a monovalent hydrocarbon group or a protecting group having 1 to 10 carbon atoms. The monovalent hydrocarbon group is preferably an alkyl group or a phenyl group having 1 to 3 carbon atoms, and more preferably an alkyl group having 1 to 3 carbon atoms. Illustrative and preferred examples of the protecting group include R 1 The above description of the above can be used. R 2 and R3 Of these, is preferably a hydrogen atom or a monovalent hydrocarbon group having 1 to 10 carbon atoms, and more preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms.

[0045] B 1 is a single bond, -NR 4 -, -O-, or a divalent aromatic heterocyclic group. Examples of the divalent aromatic heterocyclic group include a group obtained by removing any two hydrogen atoms from a pyridine ring, a pyrimidine ring, a pyridazine ring, or a pyrazine ring; a group obtained by removing any two hydrogen atoms from a furan ring; and a group obtained by removing any two hydrogen atoms from a thiophene ring. Among these, a group obtained by removing any two hydrogen atoms from a pyrrole ring, a furan ring, or a thiophene ring is preferred, and a group obtained by removing any two hydrogen atoms from a pyrrole ring is more preferred.

[0046] R 4 The monovalent organic group is preferably an alkyl group having 1 to 3 carbon atoms or a phenyl group, and more preferably an alkyl group having 1 to 3 carbon atoms.

[0047] B 1 When A is a single bond or a divalent aromatic heterocyclic group, 2 , A 3 Each of A and B is a divalent aromatic ring group. Examples and preferred examples of the divalent aromatic ring group are shown in 1 and A 4 The explanation of the divalent aromatic ring group above can be used.

[0048] B 1 Ga-NR 4 - or -O-, then A 2 and A 3 As the divalent aromatic ring group, A 1 and A 4 The explanation of the divalent aromatic ring group of A can be used. 2 and A 3 But, A 2 The aromatic ring of A 3 is linked to an aromatic ring by a single bond or a chain structure (e.g., an ethylene group),4 When the nitrogen-containing condensed ring structure formed together with - is represented, the condensed ring structure includes a carbazole structure, a 9-methylcarbazole structure, a 9-ethylcarbazole structure, etc. 2 and A 3 But, A 2 The aromatic ring of A 3 and an aromatic ring contained in the ring having a single bond or a chain structure (for example, an ethylene group) to form an oxygen-containing condensed ring structure together with -O-, examples of the condensed ring structure include a dibenzofuran structure.

[0049] The partial structure represented by the above formula (2) has a total of 3 or more aromatic rings (including aromatic hydrocarbon rings and aromatic heterocycles), and more preferably has 4 or more aromatic rings. When the partial structure represented by the above formula (2) has a total of 4 or more aromatic rings, the conjugated structure becomes longer, which is preferable in that the residual charge is relaxed more quickly and the residual image (especially DC residual image) can be sufficiently reduced. Among these, it is particularly preferable that the partial structure represented by the above formula (2) has a biphenyl structure.

[0050] The main chain of the polymer [B] is not particularly limited and can be appropriately selected depending on the main chain of the polymer [A], etc. When the polymer [A] is at least one selected from the group consisting of polyamic acid, polyamic acid ester, and polyimide, the polymer [B] is preferably at least one selected from the group consisting of polyamic acid, polyamic acid ester, and polyimide, in terms of increasing the affinity with the polymer [A].

[0051] (Polyamic acid) When the polymer [B] is a polyamic acid, the polyamic acid (hereinafter also referred to as "polyamic acid [B]") is preferably a polymer obtained by reacting a tetracarboxylic dianhydride with a diamine compound containing a diamine having a partial structure represented by the above formula (2) (hereinafter also referred to as "specific diamine (B)"), in that the partial structure represented by the above formula (2) can be easily introduced into the polymer. Examples of the tetracarboxylic dianhydride used in the synthesis of the polyamic acid [B] include the compounds exemplified as anhydrides for the tetracarboxylic acid used in the synthesis of the polyamic acid [A]. The tetracarboxylic dianhydride used in the synthesis of the polyamic acid [B] preferably contains an alicyclic tetracarboxylic dianhydride. The explanation of the amount of the alicyclic tetracarboxylic dianhydride used can be cited from the explanation of the polyamic acid [A].

[0052] The specific diamine (B) used in the synthesis of the polymer [B] is preferably a compound represented by the following formula (2-1). [ka] (In formula (2-1), A 1 ~A 4 , B 1 , R 2 and R 3 are the same as those in formula (2) above.)

[0053] Specific examples of the specific diamine (B) include compounds represented by the following formulae (DA-19) to (DA-27), (DA-42) and (DA-43). [ka]

[0054] [ka]

[0055] Of the above, the specific diamine (B) is preferably a compound represented by each of the above formulas (DA-19) to (DA-25) and (DA-42), more preferably a compound represented by each of the above formulas (DA-19) to (DA-23) and (DA-42), and even more preferably a compound represented by each of the above formulas (DA-19) to (DA-21).

[0056] The diamine compound used in the synthesis of the polyamic acid [B] may be only the specific diamine (B), but a diamine different from the specific diamine (B) (hereinafter also referred to as "other diamine (B)") may be used together with the specific diamine (B). Examples of the other diamine (B) include aliphatic diamines, alicyclic diamines, and aromatic diamines. Specific examples of the other diamine (B) include diamine compounds not having the partial structure Y in the main chain, as exemplified in the description of the polymer [A]. It is preferable that the polymer [B] does not have either the partial structure Y or the partial structure X described below.

[0057] In the synthesis of the polymer [B], the amount of the specific diamine (B) used is preferably 2 mol% or more, more preferably 5 mol% or more, and even more preferably 10 mol% or more, based on the total amount of the diamine compounds used in the synthesis of the polymer [B], in order to sufficiently reduce residual images (especially DC residual images). The amount of the specific diamine (B) used can be arbitrarily set within a range of 100 mol% or less, based on the total amount of the diamine compounds used in the synthesis of the polymer [B]. In order to improve the coatability of the liquid crystal alignment agent to the substrate, the amount is preferably 95 mol% or less, more preferably 90 mol% or less, and even more preferably 80 mol% or less.

[0058] The polyamic acid [B], polyamic acid ester, and polyimide as the polymer [B] can be produced in the same manner as the polymer [A]. The above-mentioned explanation of the polymer [A] can be applied to various conditions in the synthesis method of each polymer such as the polyamic acid [B].

[0059] <Polymer [C]> The polymer [C] is a polymer having the following partial structure X in its main chain. By incorporating the polymer [C] having the partial structure X in the liquid crystal alignment agent together with the polymer [A] and the polymer [B], it is advantageous in that it can improve the adhesion between the liquid crystal alignment film and the substrate (particularly, the adhesion to the substrate at the spacer portion) while improving the adhesion to the sealant and reducing the afterimage (AC afterimage and DC afterimage). Substructure X:-(CH 2 ) a - (wherein a is an integer of 2 to 20), or -(CH 2 ) a In the structure represented by -, any methylene group is -NR 7 -, -O-, -COO-, -NR 7 -CO-, -NR 7 -COO-, -NR 8 -CO-NR 9 - and a nitrogen-containing non-aromatic heterocyclic group (wherein R 7 is a hydrogen atom or an alkyl group. 8 and R 9 are each independently a hydrogen atom or an alkyl group, or R 8 and R 9 and are combined together to form R 8 The nitrogen atom to which R is bonded 9 represents a ring structure formed together with the nitrogen atom to which -NR is bonded and -CO-. 7 -, -O-, -COO-, -NR 7 -CO-, -NR 7 -COO-, -NR 8 -CO-NR 9 - and the nitrogen-containing non-aromatic heterocyclic groups are not adjacent to one another).

[0060] In the partial structure X, it is preferable that the partial structure X contains a linear alkanediyl group having 2 or more carbon atoms, since this has a high effect of improving the adhesion between the substrate and the liquid crystal alignment film at the spacer arrangement portion. In addition, from the viewpoint of suppressing a decrease in film strength, a is preferably 12 or less, and more preferably 10 or less.

[0061] R 7 , R 8 , R 9 R is preferably a hydrogen atom or a methyl group, more preferably a hydrogen atom. 8 and R 9 Examples of the ring structure formed by combining these groups include a 2-oxo-4-imidazolidinone-1,3-diyl group. Examples of the nitrogen-containing non-aromatic heterocyclic group include a piperidine-1,4-diyl group and a piperazine-1,4-diyl group. The polymer [C] does not have the partial structure represented by the above formula (1) or the partial structure represented by the above formula (2).

[0062] The partial structure X is, among the above, -COO-, -NR 7 -CO-, -NR 7 -COO- and -NR 8 -CO-NR 9 It is preferable that the partial structure X has at least one group selected from the group consisting of -COO-, -NR 7 -CO-, -NR 7 -COO- and -NR 8 -CO-NR 9 It is preferable that the compound contains at least one group selected from the group consisting of - and a linear alkanediyl group having 2 or more carbon atoms, since this can enhance the effect of improving the adhesion to the substrate.

[0063] The main chain of the polymer [C] is not particularly limited. However, when the polymer [A] is at least one selected from the group consisting of polyamic acid, polyamic acid ester, and polyimide, it is preferable that the polymer [C] is also at least one selected from the group consisting of polyamic acid, polyamic acid ester, and polyimide, in terms of increasing the affinity with the polymer [A] and facilitating the introduction of the partial structure X into the main chain of the polymer.

[0064] When the polymer [C] is a polyamic acid, the polyamic acid (hereinafter also referred to as "polyamic acid [C]") is preferably a polymer obtained by reacting a tetracarboxylic dianhydride with a diamine compound containing a diamine having a partial structure X (hereinafter also referred to as "specific diamine (C)"), in that the partial structure X can be easily introduced into the main chain of the polymer. Examples of the tetracarboxylic dianhydride used in the synthesis of the polyamic acid [C] include the compounds exemplified as anhydrides for the tetracarboxylic acid used in the synthesis of the polyamic acid [A]. The tetracarboxylic dianhydride used in the synthesis of the polyamic acid [C] preferably contains an alicyclic tetracarboxylic dianhydride. The explanation of the polyamic acid [A] can be used to explain the amount of the alicyclic tetracarboxylic dianhydride used.

[0065] The specific diamine (C) is not particularly limited as long as it is a diamine compound having a partial structure X, and examples thereof include aliphatic diamines, alicyclic diamines, aromatic diamines, etc. The specific diamine (C) is preferably a compound represented by the following formula (3-1). [ka] (In formula (3-1), A 5 is a divalent aromatic ring group. 6 Y is a single bond or a divalent aromatic ring group. 2 is a divalent group having a partial structure X. 5 is a hydrogen atom or a monovalent organic group.

[0066] In the above formula (3-1), A5 , A 6 Examples of the divalent aromatic ring group include a divalent aromatic hydrocarbon group and a divalent aromatic heterocyclic group. 5 , A 6 Specific and preferred examples of the divalent aromatic ring group are given below. 1 and A 4 The explanation of the divalent aromatic ring group above can be used.

[0067] R 5 Examples of the monovalent organic group include monovalent hydrocarbon groups having 1 to 10 carbon atoms. 5 is preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and more preferably a hydrogen atom or a methyl group.

[0068] Y 2 is a divalent group having a partial structure X, for example, -(CH 2 ) a - and -(CH 2 ) a In the structure represented by the formula -, any methylene group is -NR 7 -, -O-, -COO-, -NR 7 -CO-, -NR 7 -COO-, -NR 8 -CO-NR 9 - and a divalent group substituted with at least one selected from the group consisting of a nitrogen-containing non-aromatic heterocyclic group (hereinafter also referred to as "heteroatom-containing group (c)"); -(CH 2 ) a and a divalent group formed by bonding at least one of the heteroatom-containing groups (c) to a cycloalkylene group (preferably a cyclohexylene group). 2 does not have an aromatic ring group.

[0069] Specific examples of the specific diamine (C) include aliphatic diamines such as metaxylylenediamine, pentamethylenediamine, and hexamethylenediamine; alicyclic diamines such as 4,4'-methylenebis(cyclohexylamine); and aromatic diamines such as 4,4'-diaminodiphenylethane, 4,4'-diaminodiphenylpropane, 1,3-bis(4-aminophenethyl)urea, 1,3-bis(4-aminobenzyl)urea, 1,5-bis(4-aminophenoxy)pentane, 1,4-bis(4-aminofuran), and the like. Examples of the bis(4-aminophenoxy)butane, 1,3-bis(4-aminophenoxy)propane, 1,6-bis(4-aminophenoxy)hexane, bis[2-(4-aminophenyl)ethyl]hexanedioic acid, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 4,4'-[4,4'-propane-1,3-diylbis(piperidine-1,4-diyl)]dianiline, diethylene glycol bis(4-aminophenyl)ether, and the compounds represented by each of the following formulas (DA-32) to (DA-40). [ka]

[0070] As the specific diamine (C), among the compounds represented by the above formulas (DA-32) to (DA-40), the compounds represented by the above formulas (DA-32) to (DA-35) are preferred, and the compounds represented by the above formulas (DA-32) to (DA-34) are more preferred.

[0071] The diamine compound used in the synthesis of the polyamic acid [C] may be only the specific diamine (C), but a diamine different from the specific diamine (C) (hereinafter also referred to as "other diamine (C)") may be used together with the specific diamine (C). Examples of the other diamine (C) include diamines different from the specific diamines (A) to (C), such as the diamine compounds not having the partial structure Y in the main chain exemplified in the description of the polymer [A].

[0072] In the synthesis of the polymer [C], the amount of the specific diamine (C) used is preferably 10 mol% or more, more preferably 20 mol% or more, and even more preferably 30 mol% or more, based on the total amount of the diamine compounds used in the synthesis of the polymer [C], from the viewpoint of sufficiently increasing the adhesion to the substrate. The amount of the specific diamine (C) used can be arbitrarily set within the range of 100 mol% or less, based on the total amount of the diamine compounds used in the synthesis of the polymer [C].

[0073] The polyamic acid [C], polyamic acid ester and polyimide as the polymer [C] can be produced in the same manner as the polymer [A]. The above explanation of the polymer [A] can be applied to various conditions in the synthesis method of each polymer such as the polyamic acid [C].

[0074] For each of the polymers [A], [B], and [C] used in the preparation of the liquid crystal alignment agent, the solution viscosity of the polymer is preferably 10 to 800 mPa·s when the polymer is made into a 10% by mass solution, and more preferably 15 to 500 mPa·s. The solution viscosity (mPa·s) is a value measured at 25°C using an E-type rotational viscometer for a 10% by mass polymer solution prepared using a good solvent for the polymer (e.g., γ-butyrolactone, N-methyl-2-pyrrolidone, etc.).

[0075] The weight average molecular weight (Mw) of each of the polymers [A], [B] and [C] measured by gel permeation chromatography (GPC) in terms of polystyrene is preferably 1,000 to 500,000, more preferably 2,000 to 300,000. The molecular weight distribution (Mw / Mn) represented by the ratio of Mw to the number average molecular weight (Mn) measured by GPC in terms of polystyrene is preferably 7 or less, more preferably 5 or less.

[0076] In the liquid crystal alignment agent, the content of the polymer [A] is preferably 1% by mass or more, more preferably 2% by mass or more, even more preferably 5% by mass or more, and even more preferably 10% by mass or more, based on the total amount of the polymer components contained in the liquid crystal alignment agent, from the viewpoint of obtaining a sufficient effect of improving adhesion to the sealant. Also, the content of the polymer [A] is preferably 70% by mass or less, more preferably 60% by mass or less, and even more preferably 50% by mass or less, based on the total amount of the polymer components contained in the liquid crystal alignment agent.

[0077] The content of the polymer [B] is preferably 2% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more, based on the total amount of the polymer components contained in the liquid crystal alignment agent, from the viewpoint of increasing the effect of reducing the residual image (especially DC residual image). Also, the content of the polymer [B] is preferably 90% by mass or less, more preferably 80% by mass or less, and even more preferably 70% by mass or less, based on the total amount of the polymer components contained in the liquid crystal alignment agent, from the viewpoint of increasing the coatability of the liquid crystal alignment agent.

[0078] The content of the polymer [C] is preferably 2% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more, based on the total amount of the polymer components contained in the liquid crystal alignment agent, from the viewpoint of enhancing the effect of improving adhesion to the substrate. Also, the content of the polymer [B] is preferably 80% by mass or less, more preferably 70% by mass or less, and even more preferably 60% by mass or less, based on the total amount of the polymer components contained in the liquid crystal alignment agent, from the viewpoint of improving the coatability of the liquid crystal alignment agent.

[0079] Here, it is considered that the polymer [A] is hydrophobized by protecting the -NH- group, and therefore tends to be unevenly distributed on the film surface when the liquid crystal alignment agent is applied onto a substrate. 1 Regarding -, for example, the protecting group (R 1) is eliminated and replaced with a hydrogen atom, which is believed to result in the appearance of a polar functional group. For this reason, the liquid crystal alignment agent containing the polymer [A] is highly soluble in a solvent during film formation, and the polymer [A] is likely to be unevenly distributed on the surface layer, and after film formation, the elimination of the protective group improves adhesion to the sealant, and peeling is unlikely to occur even when a sealant is formed on the surface of the liquid crystal alignment film, which is believed to result in a highly reliable liquid crystal element.

[0080] In addition, in order to further improve the performance of liquid crystal elements, it is considered that the effect of reducing DC afterimages can be achieved by blending polymer [B] having a specific nitrogen-containing conjugated structure represented by the above formula (2) with polymer [A] in a liquid crystal alignment agent. However, the partial structure represented by the above formula (2) has many aromatic rings, and the toughness of the liquid crystal alignment film (especially the lower layer portion) formed is reduced, so that the liquid crystal alignment film is likely to peel off from the substrate when an external force is applied, and the adhesion between the liquid crystal alignment film and the substrate, particularly the adhesion between the substrate and the liquid crystal alignment film in the spacer arrangement portion, is considered to be poor.

[0081] In contrast, it is presumed that by using a liquid crystal alignment agent containing polymer [C] in addition to polymer [A] and polymer [B], it is possible to form a liquid crystal alignment film that has excellent adhesion to the substrate (especially the spacer portion) while maintaining excellent adhesion to the sealant and reducing DC afterimages.

[0082] <Other ingredients> The liquid crystal alignment agent may contain, in addition to the polymer [A], the polymer [B], and the polymer [C], if necessary, components different from the polymer [A], the polymer [B], and the polymer [C] (hereinafter also referred to as "other components").

[0083] (Other polymers) The liquid crystal alignment agent of the present disclosure may contain a polymer (hereinafter also referred to as "other polymer") different from the polymer [A], polymer [B] and polymer [C] as a polymer component. The main skeleton of the other polymer is not particularly limited. Examples of the other polymer include polyamic acid, polyamic acid ester, polyimide, polyorganosiloxane, polyester, polyenamine, polyurea, polyamide, polyamideimide, polybenzoxazole precursor, polybenzoxazole, cellulose derivative, polyacetal, (meth)acrylic polymer, styrene polymer, maleimide polymer, or styrene-maleimide polymer. From the viewpoint of high affinity with liquid crystal when used in combination with the polymer [A], polymer [B] and polymer [C], and high reliability of the liquid crystal element, the other polymer is preferably at least one selected from the group consisting of polyamic acid, polyamic acid ester and polyimide.

[0084] When the liquid crystal alignment agent contains other polymers, the content of the other polymers can be appropriately set within a range that does not impair the effects of the present invention. Specifically, the content of the other polymers is more preferably 5% by mass or less, even more preferably 3% by mass or less, and even more preferably 1% by mass or less, based on the total amount of the polymer components contained in the liquid crystal alignment agent.

[0085] (solvent) The liquid crystal aligning agent of the present disclosure is prepared as a liquid composition in which the polymer [A], the polymer [B], the polymer [C], and other components used as necessary are preferably dispersed or dissolved in a suitable solvent.

[0086] As the solvent, an organic solvent is preferably used.Specific examples thereof include N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, 1,2-dimethyl-2-imidazolidinone, 1,3-dimethyl-2-imidazolidinone, phenol, γ-butyrolactone, γ-butyrolactam, N,N-dimethylformamide, N,N-dimethylacetamide, 4-hydroxy-4-methyl-2-pentanone, diacetone alcohol, 1-hexanol, 2-hexanol, propane-1,2-diol, 3-methoxy-1-butanol, ethylene glycol monomethyl ether, methyl lactate, ethyl lactate, butyl lactate, methyl acetate, ethyl acetate, butyl acetate, methyl acetoacetate, ethyl acetoacetate, ethyl propionate, methyl methoxypropionate, ethyl ethoxypropionate, ethylene glycol methyl ether, ethylene glycol ethyl ether, ethylene glycol-n-propyl ether, and ethylene glycol-i-propyl ether. ether, ethylene glycol-n-butyl ether (butyl cellosolve), ethylene glycol dimethyl ether, ethylene glycol ethyl ether acetate, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, diisobutyl ketone, isoamyl propionate, isoamyl isobutyrate, diisopentyl ether, ethylene carbonate, propylene carbonate, propylene glycol monomethyl ether (PGME), diethylene glycol diethyl ether acetate, propylene glycol monomethyl ether acetate (PGMEA), propylene glycol diacetate, cyclopentanone, cyclohexanone, and the like.

[0087] Other components contained in the liquid crystal alignment agent include, in addition to the above, for example, antioxidants, metal chelate compounds, curing accelerators, surfactants, fillers, dispersants, photosensitizers, etc. The blending ratio of other components can be appropriately selected according to each compound within a range that does not impair the effects of the present disclosure.

[0088] The solid content concentration in the liquid crystal alignment agent (the ratio of the total mass of the components other than the solvent of the liquid crystal alignment agent to the total mass of the liquid crystal alignment agent) is appropriately selected in consideration of viscosity, volatility, etc., and is preferably in the range of 1 to 10 mass %. When the solid content concentration is 1 mass % or more, the thickness of the coating film can be sufficiently ensured, and a liquid crystal alignment film exhibiting good liquid crystal alignment properties is easily obtained. On the other hand, when the solid content concentration is 10 mass % or less, the coating film can be made to have an appropriate thickness, and a liquid crystal alignment film exhibiting good liquid crystal alignment properties is easily obtained, and the viscosity of the liquid crystal alignment agent becomes appropriate, tending to improve the coatability.

[0089] <Liquid crystal alignment film and liquid crystal element> The liquid crystal alignment film of the present disclosure is manufactured by the liquid crystal alignment agent prepared as described above. The liquid crystal element of the present disclosure includes a liquid crystal alignment film formed by using the liquid crystal alignment agent described above. The driving method of the liquid crystal in the liquid crystal element is not particularly limited, and can be applied to various modes such as TN type, STN type, VA type (including VA-MVA type, VA-PVA type, etc.), IPS type, FFS type, OCB (Optically Compensated Bend) type, PSA (Polymer Sustained Alignment) type, etc. The liquid crystal element can be manufactured by a method including, for example, the following steps 1 to 3. In step 1, the substrate used differs depending on the desired operation mode. Steps 2 and 3 are common to each operation mode.

[0090] <Step 1: Formation of coating film> First, a liquid crystal alignment agent is applied onto a substrate, and the applied surface is preferably heated to form a coating film on the substrate. As the substrate, for example, a transparent substrate made of glass such as float glass or soda glass, or a plastic such as polyethylene terephthalate, polybutylene terephthalate, polyethersulfone, polycarbonate, or poly(alicyclic olefin) can be used. As the transparent conductive film provided on one surface of the substrate, a transparent substrate made of tin oxide (SnO 2 NESA membrane (registered trademark of PPG, USA) made of indium oxide-tin oxide (In 2 O 3 -SnO2 Examples of suitable ITO films include an ITO film made of a transparent conductive film. When manufacturing a TN-type, STN-type, or VA-type liquid crystal element, two substrates with patterned transparent conductive films are used. On the other hand, when manufacturing an IPS-type or FFS-type liquid crystal element, a substrate with an electrode patterned into a comb-tooth shape and an opposing substrate with no electrode are used.

[0091] The method of applying the liquid crystal alignment agent to the substrate is not particularly limited, and can be, for example, a spin coat method, a printing method (e.g., offset printing method, flexographic printing method, etc.), an inkjet method, a slit coat method, a bar coater method, an extrusion die method, a direct gravure coater method, a chamber doctor coater method, an offset gravure coater method, an impregnation coater method, an MB coater method, or the like.

[0092] After the liquid crystal alignment agent is applied, preheating (pre-baking) is preferably performed for the purpose of preventing dripping of the applied liquid crystal alignment agent. The pre-baking temperature is preferably 30 to 200°C, and the pre-baking time is preferably 0.25 to 10 minutes. Thereafter, the solvent is completely removed, and a baking (post-baking) step is performed, if necessary, for the purpose of thermally imidizing the amic acid structure present in the polymer. The baking temperature (post-baking temperature) at this time is preferably 80 to 280°C, more preferably 80 to 250°C. The post-baking time is preferably 5 to 200 minutes. The thickness of the film formed is preferably 0.001 to 1 μm. This allows the formation of a film on the substrate that includes the polymer [A'], the polymer [B], and the polymer [C], which are obtained by removing the protective group from the partial structure represented by the above formula (1) of the polymer [A]. The polymer [A'] has a structural unit containing an -NH- group in a portion different from the group involved in polymerization.

[0093] <Step 2: Alignment Treatment> When manufacturing a TN-type, STN-type, IPS-type or FFS-type liquid crystal element, the coating film formed in the above step 1 is subjected to a treatment (alignment treatment) for imparting liquid crystal alignment ability. This imparts the alignment ability of liquid crystal molecules to the coating film, forming a liquid crystal alignment film. As the alignment treatment, it is preferable to use a rubbing treatment in which the surface of the coating film formed on the substrate is rubbed with cotton or the like, or a photo-alignment treatment in which the coating film is irradiated with light to impart liquid crystal alignment ability. When manufacturing a vertical alignment type liquid crystal element, the coating film formed in the above step 1 may be used as it is as a liquid crystal alignment film, or the coating film may be subjected to an alignment treatment in order to further enhance the liquid crystal alignment ability.

[0094] The light irradiation for photo-alignment can be performed by a method of irradiating the coating film after the post-bake step, a method of irradiating the coating film after the pre-bake step but before the post-bake step, or a method of irradiating the coating film during heating in at least one of the pre-bake step and the post-bake step. For example, ultraviolet light and visible light containing light with a wavelength of 150 to 800 nm can be used as the radiation to be irradiated to the coating film. Preferably, ultraviolet light containing light with a wavelength of 200 to 400 nm is used. When the radiation is polarized, it may be linearly polarized or partially polarized. When the radiation used is linearly polarized or partially polarized, the radiation may be performed from a direction perpendicular to the substrate surface, from an oblique direction, or a combination of these. When the radiation is non-polarized, the radiation is irradiated in an oblique direction.

[0095] Examples of the light source used include a low pressure mercury lamp, a high pressure mercury lamp, a deuterium lamp, a metal halide lamp, an argon resonance lamp, a xenon lamp, an excimer laser, etc. The radiation dose is preferably 200 to 30,000 J / m 2 and more preferably 500 to 10,000 J / m 2 After the light irradiation for imparting the alignment ability, the surface of the substrate may be washed with, for example, water, an organic solvent (e.g., methanol, isopropyl alcohol, 1-methoxy-2-propanol acetate, butyl cellosolve, ethyl lactate, etc.) or a mixture thereof, or the substrate may be heated.

[0096] <Step 3: Construction of liquid crystal cell> Two substrates on which the liquid crystal alignment film is formed are prepared as described above, and a liquid crystal is disposed between the two substrates arranged opposite to each other to manufacture a liquid crystal cell. For example, the two substrates are arranged opposite to each other with a gap therebetween so that the liquid crystal alignment film faces each other, the peripheries of the two substrates are bonded together with a sealant, and the liquid crystal is injected and filled into the cell gap surrounded by the substrate surfaces and the sealant, and then the injection hole is sealed, or a method using the ODF method can be mentioned. A bead spacer or a columnar spacer is disposed between the two substrates as an in-plane spacer, thereby forming a cell gap. For example, an epoxy resin containing a hardener and aluminum oxide spheres as a spacer can be used as the sealant. When applying the sealant to the substrate, the sealant can be applied, for example, by a screen printing method, on the surface of the liquid crystal alignment film of at least one of the two substrates on which the liquid crystal alignment film is formed.

[0097] The liquid crystal may be either positive or negative, but is preferably negative. Examples of negative liquid crystal include Merck's "MLC-6608", "MLC-6609", "MLC-6610", and "MLC-7026-100". In particular, when negative liquid crystal is used in IPS and FFS liquid crystal elements, it is preferable because it can reduce the transmission loss above the electrode and improve the contrast. In addition, examples of liquid crystal include nematic liquid crystal and smectic liquid crystal, and among them, nematic liquid crystal is preferable.

[0098] When manufacturing a liquid crystal display device, a polarizing plate is subsequently attached to the outer surface of the liquid crystal cell to obtain a liquid crystal display element. Examples of the polarizing plate include a polarizing film called an "H film" made by absorbing iodine while stretching and aligning polyvinyl alcohol, sandwiched between cellulose acetate protective films, and a polarizing plate made of the H film itself.

[0099] The liquid crystal element of the present invention can be effectively applied to various applications, specifically, for example, it can be used as various display devices such as clocks, portable game machines, word processors, notebook computers, car navigation systems, camcorders, PDAs, digital cameras, mobile phones, smartphones, various monitors, liquid crystal televisions, and information displays, as well as light control devices, retardation films, and the like. EXAMPLES

[0100] Hereinafter, the embodiments will be described in more detail with reference to examples, but the present invention should not be construed as being limited to the following examples.

[0101] In the following examples, the weight average molecular weight (Mw) of the polymer, the imidization ratio of the polyimide in the polymer solution, and the solution viscosity of the polymer solution were measured by the following methods. The required amounts of the raw material compounds and polymers used in the following examples were ensured by repeating the synthesis on a synthesis scale shown in the following synthesis examples as necessary. [Weight average molecular weight of polymer (Mw)] The weight average molecular weight (Mw) is a polystyrene equivalent value measured by GPC under the following conditions. Column: TSKgelGRCXLII, manufactured by Tosoh Corporation Solvent: Lithium bromide and phosphoric acid in N,N-dimethylformamide Temperature: 40℃ Pressure: 68kgf / cm 2 [Imidization rate of polyimide] The polyimide solution was poured into pure water, and the resulting precipitate was thoroughly dried under reduced pressure at room temperature. It was then dissolved in deuterated dimethyl sulfoxide and measured at room temperature using tetramethylsilane as a standard substance. 1 H-NMR was measured. 1 The imidization rate [%] was calculated from the H-NMR spectrum using the following formula (1). Imidization rate [%] = (1-(β 1 / (β 2 ×α)))×100 …(1) (In formula (1), β1 is the peak area due to the proton of the NH group that appears at a chemical shift of around 10 ppm, and β 2 is the peak area due to other protons, and α is the ratio of the number of other protons to one proton of the NH group in the polymer precursor (polyamic acid). [Solution viscosity of polymer solution] The solution viscosity (mPa·s) of the polymer solution was measured at 25°C using an E-type rotational viscometer.

[0102] The abbreviations for the compounds used in the examples are as follows. (Tetracarboxylic acid derivatives) Compound (AN-1) to Compound (AN-8): Compounds represented by the following formulas (AN-1) to (AN-8), respectively. [ka]

[0103] (Diamine compounds) Compound (DA-1) to Compound (DA-12): Compounds represented by the above formulas (DA-1) to (DA-12), respectively Compound (DA-19) to Compound (DA-27), Compound (DA-42): Compounds represented by the above formulas (DA-19) to (DA-27) and (DA-42), respectively Compound (DA-32) to Compound (DA-40): Compounds represented by the above formulas (DA-32) to (DA-40), respectively Compound (DA-13) to Compound (DA-18), Compound (DA-28) to Compound (DA-31), and Compound (DA-41): Compounds represented by the following formulae (DA-13) to (DA-18), (DA-28) to (DA-31), and (DA-41), respectively. [ka]

[0104] <Polymer synthesis> 1. Synthesis of polyamic acid [Synthesis Example 1] Compound (DA-1) was dissolved in N-methyl-2-pyrrolidone (NMP), 0.95 equivalents (molar ratio) of compound (AN-1) was added, and the reaction was carried out at 60°C for 6 hours to obtain a solution containing 15% by mass of polyamic acid. A small amount of the obtained polyamic acid solution was taken, and NMP was added to make a solution with a polyamic acid concentration of 10% by mass. The solution viscosity was measured and found to be 128 mPa·s. Next, this polyamic acid solution was poured into a large excess of methanol to precipitate the reaction product. The precipitate was washed with methanol and dried under reduced pressure at 40°C for 15 hours to obtain polyamic acid (referred to as "Polymer (A-1)"). The weight average molecular weight (Mw) of the obtained polymer was 27,000.

[0105] [Synthesis Examples 2 to 8, 11 to 16, 18 to 53: Synthesis of Polymers (A-2) to (A-8), (A-11) to (A-16), (A-18), (A-19), (B-1) to (B-20), and (C-1) to (C-14)] Polymers (A-2) to (A-8), (A-11) to (A-16), (A-18), (A-19), (B-1) to (B-20), and (C-1) to (C-14) were obtained in the same manner as in Synthesis Example 1, except that the types and molar ratios of the tetracarboxylic dianhydride and diamine compound were changed as shown in Tables 1 to 4 below. The values ​​in Tables 1 to 4 indicate the ratio (parts by mole) of each compound used relative to 100 parts by mole of the total amount of the acid derivatives used in the synthesis for the acid derivatives (tetracarboxylic dianhydride in the synthesis of polyamic acid), and the values ​​in Tables 1 to 4 indicate the ratio (parts by mole) of each compound used relative to 100 parts by mole of the total amount of the diamine compounds used in the synthesis for the diamine compounds.

[0106] [Synthesis Example 17: Synthesis of Polymer (A-17)] Compound (DA-13) was dissolved in N-methyl-2-pyrrolidone (NMP), 0.95 equivalents (molar ratio) of compound (AN-1) was added, and the mixture was reacted at 60°C for 6 hours to obtain a solution containing 15% by mass of polyamic acid. 0.05 equivalents (molar ratio) of di-tert-butyl dicarbonate was added to this polyamic acid solution, and the mixture was stirred at room temperature for 15 hours. Next, this polyamic acid solution was poured into a large excess of methanol to precipitate the reaction product. The resulting precipitate was washed with methanol and dried under reduced pressure at 40°C for 15 hours to obtain a polyamic acid (referred to as "polymer (A-17)") having a Boc group introduced at the polymerization terminal. The weight average molecular weight (Mw) of the obtained polymer was 25,000.

[0107] 2. Synthesis of Polyimide [Synthesis Example 9: Synthesis of Polymer (A-9)] Polymerization was performed in the same manner as in Synthesis Example 1, except that the types and molar ratios of the tetracarboxylic dianhydride and diamine compound were changed as shown in Table 1 below, to obtain a solution containing 15% by mass of polyamic acid. Next, NMP was added to the obtained polyamic acid solution to obtain a solution with a polyamic acid concentration of 10% by mass, and pyridine and acetic anhydride were added to perform a dehydration ring-closing reaction at 60° C. for 4 hours. After the dehydration ring-closing reaction, the solvent in the system was replaced with fresh NMP to obtain a solution containing 15% by mass of polyimide with an imidization rate of about 85%. Next, this polyimide solution was poured into a large excess of methanol to precipitate the reaction product. The precipitate was washed with methanol and dried under reduced pressure at 40° C. for 15 hours to obtain a polyimide (referred to as "Polymer (A-9)"). The weight average molecular weight (Mw) of the obtained polymer was 33,000.

[0108] 3. Synthesis of polyamic acid ester [Synthesis Example 10: Synthesis of Polymer (A-10)] Compound (DA-5) 70 mol parts, compound (DA-6) 15 mol parts, and compound (DA-3) 15 mol parts as diamine compounds, pyridine of 2.5 equivalents (molar ratio) relative to the total amount of diamine compounds as a base, and N-methyl-2-pyrrolidone (NMP) as a solvent were added and dissolved. While stirring this solution with water cooling, dimethyl-1,3-bis(chlorocarbonyl)cyclobutane-2,4-carboxylate 97 mol parts as an acid derivative were added, and NMP was further added so that the solid content concentration was 5% by mass, and the mixture was stirred for 4 hours while cooling with water. This solution was poured into water to precipitate a polymer, and the polymer was filtered by suction filtration, washed with water again, washed with methanol three times, and dried under reduced pressure at 40°C to obtain a polyamic acid ester (referred to as "polymer (A-10)"). The weight average molecular weight (Mw) of polymer (A-10) was 29,000.

[0109] [Table 1]

[0110] [Table 2]

[0111] [Table 3]

[0112] [Table 4]

[0113] [Example 1] 1. Preparation of Liquid Crystal Alignment Agent 20 parts by mass of the polymer (A-1) obtained in Synthesis Example 1, 40 parts by mass of the polymer (B-7) obtained in Synthesis Example 26, and 40 parts by mass of the polymer (C-3) obtained in Synthesis Example 40 were diluted with NMP, γ-butyrolactone (GBL), ethylene glycol monobutyl ether (BC), diacetone alcohol (DAA), and diethylene glycol diethyl ether (DEDG) to obtain a solution with a solid content concentration of 4.0% by mass and a solvent composition ratio of NMP:GBL:BC:DAA:DEDG=30:30:20:10:10 (mass ratio). The liquid crystal alignment agent (R-1) was prepared by filtering this solution through a filter with a pore size of 0.2 μm.

[0114] 2. Formation of liquid crystal alignment film by rubbing method A glass substrate having a flat electrode (bottom electrode), an insulating layer, and a comb-shaped electrode (top electrode) laminated in this order on one side, and having a columnar spacer on the electrode formation surface, and an opposing glass substrate having no electrode were prepared. The liquid crystal alignment agent (R-1) prepared in 1 above was applied to each surface of the pair of substrates using a spinner, heated (pre-baked) on a hot plate at 80°C for 1 minute, and then dried (post-baked) for 30 minutes in an oven at 230°C with the interior replaced with nitrogen, to form a coating film with an average thickness of 0.1 μm. A rubbing treatment was performed on the surface of the coating film using a rubbing machine having a roll wrapped with nylon cloth at a roll rotation speed of 1000 rpm, a stage movement speed of 3 cm / sec, and a pile indentation length of 0.3 mm. The coating film subjected to the rubbing alignment treatment was ultrasonically cleaned in ultrapure water for 1 minute, and then dried in an oven at 100°C for 10 minutes to form a liquid crystal alignment film.

[0115] 3. Manufacturing of FFS type liquid crystal display elements Of the pair of substrates having the liquid crystal alignment film prepared in 2 above, an epoxy resin adhesive containing aluminum oxide spheres with a diameter of 5.5 μm was screen-printed on the edge of the surface on which the liquid crystal alignment film was formed on one substrate, leaving a liquid crystal injection port, and then the substrates were stacked and pressed together so that the rubbing directions of the substrates were antiparallel, and the adhesive was thermally cured at 150°C for 1 hour. Next, negative nematic liquid crystal (MLC-6608, manufactured by Merck) was filled between the pair of substrates through the liquid crystal injection port, and the liquid crystal injection port was sealed with an epoxy adhesive. Furthermore, in order to remove the flow alignment during the liquid crystal injection, the substrate was heated at 120°C and then slowly cooled to room temperature. Next, polarizing plates were attached to both outer surfaces of the substrate to produce an FFS type liquid crystal display element.

[0116] 4. Evaluation of adhesion to sealant (seal adhesion) In the same manner as in 2. above, a pair of substrates having a liquid crystal alignment film was prepared using the liquid crystal alignment agent (R-1). Next, an epoxy resin adhesive containing aluminum oxide spheres having a diameter of 5.5 μm was applied to the center of each of the alignment film-forming surfaces of the pair of substrates, and the substrates were then stacked and pressed so that the alignment film-forming surfaces faced each other, and the adhesive was cured to form a sealant. The pressure at which the sealant peeled off was measured using a tensile tester. Those that peeled off when a pressure of 2.0 kgf or more was applied were rated as "excellent," those that peeled off when a pressure of 1.0 kgf or more but less than 2.0 kgf was applied were rated as "good," and those that peeled off when a pressure of less than 1.0 kgf was applied were rated as "poor." As a result, this example was rated as "excellent."

[0117] 5. Evaluation of AC image retention characteristics An FFS-type liquid crystal cell was fabricated in the same manner as in 3 above, except that no polarizing plates were attached to either outer surface of the substrate. After driving this FFS-type liquid crystal cell for 72 hours at an AC voltage of 10 V, the minimum relative transmittance (%), expressed by the following formula (2), was measured using an apparatus in which a polarizer and an analyzer were placed between a light source and a light quantity detector. Minimum relative transmittance (%) = [(β-B0) / (B100-B0)] × 100 … (2) (In formula (2), B0 is the amount of light transmitted in a blank under crossed Nicols. B100 is the amount of light transmitted in a blank under paranicols. β is the minimum amount of light transmitted when a liquid crystal cell is sandwiched between a polarizer and an analyzer under crossed Nicols.) The black level in the dark state is expressed by the minimum relative transmittance of the liquid crystal cell, and in the case of an FFS type liquid crystal cell, the smaller the black level in the dark state, the better the contrast. A minimum relative transmittance of less than 0.3% was rated as "excellent," 0.3% or more and less than 2.0% was rated as "good," and 2.0% or more was rated as "poor." As a result, this example was rated as "excellent."

[0118] 6. Evaluation of DC image retention characteristics The liquid crystal display element manufactured in 3 above was driven at AC2.5V to set the luminance difference between any two pixels to 0, and then DC1V was applied to only one of the pixels for 20 minutes while driving at AC2.5V to accumulate charge. When the application of DC1V was stopped and the driving was returned to AC2.5V only, a luminance difference occurred between the two pixels due to the accumulated charge. By observing the change over time in this luminance difference, the relaxation time in the process of the residual DC value attenuating was calculated. A relaxation time of less than 10 seconds was judged to be "excellent," a relaxation time of 10 to 20 seconds was judged to be "good," and a relaxation time of 20 seconds or more was judged to be "poor." As a result, this example was rated as "excellent."

[0119] 7. Evaluation of adhesion to substrate (spacer adhesion) The liquid crystal display element manufactured in the above 3. was observed for alignment defects after applying external stress. Specifically, after pressing a rod-shaped indenter with a diameter of 5 mm against the liquid crystal display element for 10 minutes at a load of 2.0 kgf and a rotation speed of 200 rpm, the number of alignment defects in which light leakage occurs in the pixel under crossed Nicols was counted. If the liquid crystal alignment film has high toughness, when the liquid crystal display element is pressed in the thickness direction from above, the liquid crystal alignment film is deformed by following the movement of the spacer in the thickness direction and returns to its original shape, so that the liquid crystal alignment film is not easily peeled off from the substrate. In this case, the adhesion of the liquid crystal alignment film to the substrate can be said to be good. On the other hand, if the liquid crystal alignment film has insufficient toughness, when the liquid crystal display element is pressed in the thickness direction from above, the liquid crystal alignment film cannot follow the movement of the spacer, and the liquid crystal alignment film cracks due to the pressure, and is easily peeled off from the substrate. In this case, the adhesion of the liquid crystal alignment film to the substrate can be said to be poor. Therefore, in this example, the alignment defects after applying external stress to the liquid crystal display element were observed to evaluate the adhesion of the liquid crystal alignment film to the substrate (particularly the adhesion at the spacer portion). The evaluation criteria were "excellent" if the alignment defect location was 0 points, "good" if the alignment defect location was 1 point or more but less than 5 points, and "poor" if the alignment defect location was 5 points or more. As a result, this example was rated as "excellent."

[0120] 8. Evaluation of inkjet coating properties As the substrate to which the liquid crystal alignment agent (R-1) was applied, a glass substrate with a transparent electrode made of ITO was used, which had been heated on a hot plate at 200°C for 1 minute, and then subjected to ultraviolet / ozone cleaning to reduce the water contact angle of the transparent electrode surface to 10° or less. The liquid crystal alignment agent (R-1) prepared above was applied to the transparent electrode surface of the glass substrate with the transparent electrode using an inkjet coater (manufactured by Shibaura Mechatronics Co., Ltd.). The application conditions at this time were 2,500 times / (nozzle·min), discharge amount of 250 mg / 10 seconds, and two round trips (total of four times). After application, the substrate was left to stand for 1 minute, and then heated at 80°C to form a coating film with an average thickness of 0.1 μm. The obtained coating film was observed with the naked eye for unevenness and the number of repellings under irradiation with an interference fringe measurement lamp (sodium lamp). The case where the number of unevenness and cissing spots was 0 in total was judged as "excellent", the case where the number of unevenness and cissing spots was 1 or more and less than 3 in total was judged as "good", and the case where the number of unevenness and cissing spots was 3 or more in total was judged as "poor". As a result, the inkjet coatability of the liquid crystal alignment agent of this example was evaluated as "excellent".

[0121] [Examples 2 to 9, 11 to 19 and Comparative Examples 1 to 9] A liquid crystal alignment agent was prepared in the same manner as in Example 1, except that the composition of the liquid crystal alignment agent was changed as shown in Table 5 below. In addition, a liquid crystal display element was produced using the obtained liquid crystal alignment agent in the same manner as in Example 1, and various evaluations were performed. The results are shown in Table 5 below. In Table 5, the numerical value in parentheses for each polymer indicates the blending ratio (parts by mass) of the solid content of each polymer relative to 100 parts by mass of the total amount of the polymer components used in the preparation of the liquid crystal alignment agent.

[0122] [Example 10] Except for changing the composition of the liquid crystal alignment agent as shown in Table 5 below and using a photo-alignment method instead of a rubbing method for the liquid crystal alignment film, the liquid crystal alignment agent was prepared in the same manner as in Example 1, and a liquid crystal display element and a liquid crystal cell were manufactured and various evaluations were performed. The liquid crystal alignment film was formed by the photo-alignment method as follows. (Formation of liquid crystal alignment film by photoalignment method) A flat electrode (bottom electrode), an insulating layer, and a comb-shaped electrode (top electrode) were laminated in this order on one side of the glass substrate, which had columnar spacers on the electrode-forming surface, and an opposing glass substrate on which no electrode was provided. A liquid crystal alignment agent was applied using a spinner and heated (pre-baked) on a hot plate at 80°C for 1 minute. The substrate was then dried (post-baked) for 30 minutes in an oven at 230°C with the interior replaced with nitrogen, forming a coating film with an average thickness of 0.1 μm. The resulting coating film was irradiated with 1,000 J / m2 of linearly polarized ultraviolet light containing a 254 nm emission line using an Hg-Xe lamp. 2 The coating film was irradiated with light from the normal direction of the substrate to perform a photo-alignment treatment. The amount of irradiation was measured using an actinometer that measures at a wavelength of 254 nm. Next, the coating film that had been subjected to the photo-alignment treatment was heated in a clean oven at 230°C for 30 minutes to perform a heat treatment, thereby forming a liquid crystal alignment film. In addition, the above series of operations is performed with a UV irradiation dose of 100 to 10,000 J / m after post-baking. 2 By varying the exposure dose within the range of 100%, three or more liquid crystal cells with different UV exposure doses were manufactured, and various evaluations were performed in the same manner as in Example 1 using the liquid crystal cell with the exposure dose (optimum exposure dose) that showed the best alignment characteristics.

[0123] [Table 5]

[0124] As shown in Table 5, Examples 1 to 19 had a well-balanced improvement in various properties, such as seal adhesion, AC image retention characteristics, DC image retention characteristics, spacer adhesion, and coatability, compared with Comparative Examples 1 to 9. In contrast, Comparative Examples 1 to 9, which did not contain any of the polymer [A], the polymer [B], and the polymer [C], were evaluated as "poor" in any of the seal adhesion, the DC image retention characteristics, and the spacer adhesion.

Claims

1. A polymer [A] having a partial structure represented by the following formula (1) and not having a partial structure represented by the following formula (2), A polymer [B] having a partial structure represented by the following formula (2), A polymer [C] having the following partial structure X in its main chain and not having a partial structure represented by the following formula (1) or a partial structure represented by the following formula (2), A liquid crystal aligning agent containing at least one polymer selected from the group consisting of polyamic acid, polyamic acid ester, and polyimide obtained by using a diamine component containing at least one diamine selected from the group consisting of a compound represented by the following formula (DA-2R), a compound represented by the following formula (DA-3R), and a compound represented by the following formula (DA-4R), and at least one polymer selected from the group consisting of polyamic acid, polyamic acid ester, and polyimide obtained by using a diamine component containing a diamine represented by the following formula (DA-9R), and a polyamic acid obtained by using a diamine component containing at least one diamine selected from the group consisting of a compound represented by the following formula (DA-10R) and a compound represented by the following formula (DA-11R). Partial structure X: -(CH 2 ) a - (wherein a is an integer of 2 to 20), or -(CH 2 ) a In the structure represented by -, any methylene group is -NR 7 -, -O-, -COO-, -NR 7 —CO—, —NR 7 -COO-, -NR 8 -CO-NR 9 - and a nitrogen-containing non-aromatic heterocyclic group (wherein R 7 is a hydrogen atom or an alkyl group. 8 and R 9 are each independently a hydrogen atom or an alkyl group, or R 8 and R 9 and are combined together to form R 8 A nitrogen atom to which R is bonded. 9 In the partial structure X, -NR represents a ring structure formed together with the nitrogen atom to which -NR is bonded and -CO-. 7 -, -O-, -COO-, -NR 7 —CO—, —NR 7 -COO-, -NR 8 -CO-NR 9 - and the nitrogen-containing non-aromatic heterocyclic groups are not adjacent to each other. 【Chemistry 1】 (In formula (1), R 1 is a protecting group. "*" represents a bond.) 【Chemistry 2】 (In formula (2), A 1 and A 4 R is each independently a divalent aromatic ring group. 2 and R 3 are each independently a hydrogen atom or a monovalent organic group. 1 is a single bond, -NR 4 R is -, -O- or a divalent aromatic heterocyclic group. 4 is a hydrogen atom or a monovalent organic group. 1 When A is a single bond, 2 is a divalent aromatic ring group, A 3 is a single bond or a divalent aromatic ring group. 1 When A is a divalent aromatic heterocyclic group, 2 and A 3 are each independently a single bond or a divalent aromatic ring group. 1 -NR 4 - or -O-, then A 2 and A 3 are each independently a divalent aromatic ring group, or A 2 The aromatic ring of A 3 is linked to an aromatic ring by a single bond or a chain structure, 4 It represents a nitrogen- or oxygen-containing condensed ring structure formed together with - or -O-. "*" represents a bond.) 【Chemistry 8】

2. The liquid crystal aligning agent according to claim 1 , wherein the polymer [A], the polymer [B] and the polymer [C] are at least one selected from the group consisting of polyamic acid, polyamic acid ester and polyimide.

3. The liquid crystal aligning agent according to claim 1 or 2, wherein the polymer [C] contains a structural unit derived from a diamine represented by the following formula (3-1): 【Chemistry 3】 (In formula (3-1), A 5 is a divalent aromatic ring group. 6 Y is a single bond or a divalent aromatic ring group. 2 is a divalent group having the partial structure X. 5 is a hydrogen atom or a monovalent organic group.

4. The partial structure X is -COO-, -NR 7 —CO—, —NR 7 -COO- and -NR 8 -CO-NR 9 The liquid crystal aligning agent according to any one of claims 1 to 3, which has at least one group selected from the group consisting of:

5. The liquid crystal aligning agent according to any one of claims 1 to 4, wherein the polymer [A] contains a structural unit derived from a diamine represented by the following formula (1-1): 【Chemistry 4】 (In formula (1-1), A 7 and A 8 Each of Y is independently a divalent aromatic ring group. 1 is a divalent organic group. r is 0 or 1. However, when r is 1, A 7 , A 8 and Y 1 At least one of A has a partial structure represented by the above formula (1). 7 has a partial structure represented by the above formula (1).

6. The liquid crystal aligning agent according to any one of claims 1 to 5, wherein the polymer [A] has the following partial structure Y in its main chain: Partial structure Y:-(CH 2 ) b - (wherein b is an integer of 2 to 20), or -(CH 2 ) b In the structure represented by -, any methylene group is -NR 10 -, -O-, -COO-, -NR 10 —CO—, —NR 10 -COO-, -NR 10 -CO-NR 11 - and a nitrogen-containing non-aromatic heterocyclic group (wherein R 10 and R 11 are each independently a hydrogen atom or a monovalent organic group. 10 -, -O-, -COO-, -NR 10 —CO—, —NR 10 -COO-, -NR 10 -CO-NR 11 - and the nitrogen-containing non-aromatic heterocyclic groups are not adjacent to each other.

7. The liquid crystal aligning agent according to any one of claims 1 to 6, wherein the polymer [B] contains a structural unit derived from a diamine represented by the following formula (2-1): 【Chemistry 5】 (In formula (2-1), A 1 ~A 4 , B 1 , R 2 and R 3 are the same as those in the above formula (2).

8. A liquid crystal alignment film formed by the liquid crystal aligning agent according to any one of claims 1 to 7.

9. A polymer having a structural unit including a partial structure represented by the following formula (1A) in a portion other than a group involved in polymerization, and not having a partial structure represented by the following formula (2); A polymer having a partial structure represented by the following formula (2): A polymer having the following partial structure X in its main chain and not having a partial structure represented by the following formula (2), A liquid crystal alignment film comprising: (however, excluding those containing at least one polymer selected from the group consisting of polyamic acid, polyamic acid ester, and polyimide obtained by using a diamine component containing at least one diamine selected from the group consisting of a compound represented by the following formula (DA-2R), a compound represented by the following formula (DA-3R), and a compound represented by the following formula (DA-4R); at least one polymer selected from the group consisting of polyamic acid, polyamic acid ester, and polyimide obtained by using a diamine component containing a diamine represented by the following formula (DA-9R); and a polyamic acid obtained by using a diamine component containing at least one diamine selected from the group consisting of a compound represented by the following formula (DA-10R) and a compound represented by the following formula (DA-11R). Partial structure X: -(CH 2 ) a - (wherein a is an integer of 2 to 20), or -(CH 2 ) a In the structure represented by -, any methylene group is -NR 7 -, -O-, -COO-, -NR 7 —CO—, —NR 7 -COO-, -NR 8 -CO-NR 9 - and a nitrogen-containing non-aromatic heterocyclic group (wherein R 7 is a hydrogen atom or an alkyl group. 8 and R 9 are each independently a hydrogen atom or an alkyl group, or R 8 and R 9 and are combined together to form R 8 A nitrogen atom to which R is bonded. 9 In the partial structure X, -NR represents a ring structure formed together with the nitrogen atom to which -NR is bonded and -CO-. 7 -, -O-, -COO-, -NR 7 —CO—, —NR 7 -COO-, -NR 8 -CO-NR 9 - and the nitrogen-containing non-aromatic heterocyclic groups are not adjacent to each other. 【Chemistry 6】 (In formula (1A), "*" represents a bond.) 【Chemistry 7】 (In formula (2), A 1 and A 4 R is each independently a divalent aromatic ring group. 2 and R 3 are each independently a hydrogen atom or a monovalent organic group. 1 is a single bond, -NR 4 R is -, -O- or a divalent aromatic heterocyclic group. 4 is a hydrogen atom or a monovalent organic group. 1 When A is a single bond, 2 is a divalent aromatic ring group, A 3 is a single bond or a divalent aromatic ring group. 1 When A is a divalent aromatic heterocyclic group, 2 and A 3 are each independently a single bond or a divalent aromatic ring group. 1 -NR 4 - or -O-, then A 2 and A 3 are each independently a divalent aromatic ring group, or A 2 The aromatic ring of A 3 is linked to an aromatic ring by a single bond or a chain structure, 4 It represents a nitrogen- or oxygen-containing condensed ring structure formed together with - or -O-. "*" represents a bond.) 【Chemistry 9】

10. A liquid crystal element comprising the liquid crystal alignment film according to claim 8 or 9.

Citation Information

Patent Citations

  • Liquid crystal display device

    JP2013109154A

  • Liquid crystal aligning agent, liquid crystal alignment film and liquid crystal display element

    WO2016152928A1

  • Liquid crystal aligning agent, liquid crystal alignment film, and liquid crystal element

    WO2019093037A1

  • Liquid crystal aligning agent, liquid crystal alignment film, and liquid crystal display device using same

    WO2020158818A1

  • Liquid crystal aligning agent, liquid crystal alignment layer, and liquid crystal display element

    WO2021206003A1