Float glass manufacturing apparatus and float glass manufacturing method
The float glass manufacturing apparatus addresses the issue of buffer film hindrance and scratches by using a gas suction nozzle to manage gas flow, enhancing glass ribbon quality and reducing residual stress.
Patent Information
- Application Number
- JP2021102233
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-06-21
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-06-21
AI Technical Summary
The formation of a buffer film on the glass ribbon is hindered due to the disturbance of reducing gas flow from the dross box into the lehr, leading to reduced oxygen concentration and increased likelihood of scratches on the glass ribbon surface.
A float glass manufacturing apparatus with a gas suction nozzle positioned to restrict the flow of reducing gas from the dross box into the lehr, using a gas discharge nozzle to discharge sulfur oxide gas and a gas suction nozzle to suck gas from below or the sides, maintaining optimal gas concentrations and preventing buffer film formation.
The apparatus effectively inhibits buffer film formation and improves glass ribbon quality by maintaining optimal gas concentrations, reducing scratches and residual stress, while preserving heat insulation properties.
Smart Images

Figure 0007593244000002 
Figure 0007593244000003 
Figure 0007593244000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a float glass manufacturing apparatus and a float glass manufacturing method. [Background technology]
[0002] The float glass manufacturing apparatus includes a float bath for forming a glass ribbon on molten metal, a dross box having a plurality of lift-out rolls for lifting the glass ribbon, and an annealing furnace having a plurality of layer rolls for transporting the glass ribbon. The glass ribbon annealed in the annealing furnace is cut into a desired size and shape to obtain float glass.
[0003] The inside of the float bath is filled with a reducing gas to suppress oxidation of the molten metal. The reducing gas flows from the inside of the float bath into the inside of the dross box, and the inside of the dross box is also filled with the reducing gas. Meanwhile, the inside of the annealing furnace is filled with the atmosphere.
[0004] The dross box includes a carbon member that is in contact with the lift-out roll. The carbon member removes dross adhering to the lift-out roll. The dross is an oxide of molten metal that is brought into the dross box together with the glass ribbon.
[0005] If air flows from the inside of the annealing furnace into the inside of the dross box, the carbon members will be oxidized and consumed by oxygen gas in the air, making it difficult to remove the dross, and as a result, scratches will occur on the lower surface of the glass ribbon.
[0006] Patent Document 1 discloses a technique for suppressing the inflow of air from the inside of an annealing furnace into the inside of a dross box by using an atmosphere partition device. The atmosphere partition device separates a space below a conveying path along which a glass ribbon is conveyed in the dross box from a space below the conveying path in the annealing furnace. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2016-050160 A Summary of the Invention [Problem to be solved by the invention]
[0008] The annealing furnace has a gas discharge nozzle that discharges sulfur oxide gas from below the conveying path of the glass ribbon toward the conveying path. The sulfur oxide gas reacts with the lower surface of the glass ribbon to form a buffer film on the lower surface of the glass ribbon. The buffer film reduces collision between the glass ribbon and the ray roll. The buffer film contains sulfate crystals and the like. The sulfate crystals are formed in an oxidizing atmosphere.
[0009] If the gap between the upper surface of the glass ribbon and the drape inside the dross box is narrow, the reducing gas may forcefully flow from inside the dross box into the inside of the annealing furnace. The flowing reducing gas flows from above to below the glass ribbon. As a result, there are problems such as disturbance of the flow of sulfur oxide gas or a decrease in the oxygen concentration around the gas discharge nozzle. Therefore, the formation of a buffer film is hindered, and scratches are likely to occur on the lower surface of the glass ribbon.
[0010] One aspect of the present disclosure provides a technique for suppressing inhibition of formation of a buffer film caused by a reducing gas flowing from inside a dross box into an inside of an annealing furnace, thereby improving the quality of a glass ribbon. [Means for solving the problem]
[0011] A float glass manufacturing apparatus according to an embodiment of the present disclosure includes a float bath for forming a glass ribbon on molten metal, a dross box having a plurality of lift-out rolls for lifting up the glass ribbon, and an annealing furnace having a plurality of lehr rolls for transporting the glass ribbon. The annealing furnace includes a pair of side walls arranged on either side of a transport path for the glass ribbon, a ceiling portion for blocking the upper side of the transport path, a gas discharge nozzle for discharging sulfur oxide gas from below the transport path toward the transport path, and a gas suction nozzle inserted inward from the side walls and for sucking gas below upward or gas on the sides laterally above the transport path. The gas suction nozzle is disposed in the same position as the gas discharge nozzle in the transport direction, or is disposed upstream of the gas discharge nozzle. Effect of the Invention
[0012] According to one aspect of the present disclosure, the gas suction nozzle can restrict the reducing gas that flows from inside the dross box into the inside of the annealing furnace from reaching the periphery of the gas discharge nozzle, thereby suppressing the inhibition of the formation of the buffer film and improving the quality of the glass ribbon. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a side cross-sectional view showing a float glass manufacturing apparatus according to one embodiment. [Diagram 2] FIG. 2 is a front cross-sectional view showing an example of an annealing furnace. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, an embodiment of the present disclosure will be described with reference to the drawings. In each drawing, the same or corresponding configurations are denoted by the same reference numerals, and description thereof may be omitted. In each drawing, the X-axis direction, the Y-axis direction, and the Z-axis direction are mutually perpendicular, the X-axis direction and the Y-axis direction are horizontal directions, and the Z-axis direction is vertical. The X-axis direction is the conveying direction of the glass ribbon G, and the Y-axis direction is the width direction of the glass ribbon G. In the specification, "~" indicating a numerical range means that the numerical values described before and after it are included as the lower limit and upper limit.
[0015] A float glass manufacturing apparatus 1 according to one embodiment will be described with reference to FIG. 1. The float glass manufacturing apparatus 1 includes a float bath 2, a dross box 3, and an annealing furnace 5, arranged from the upstream side to the downstream side in the conveying direction of a glass ribbon G. The float glass manufacturing apparatus 1 forms a glass ribbon G on molten metal M stored in the float bath 2, and pulls out the formed glass ribbon G from the float bath 2 by a plurality of lift-out rolls 31 provided inside the dross box 3, and sends it to the annealing furnace 5. In addition, the float glass manufacturing apparatus 1 anneals the glass ribbon G inside the annealing furnace 5, and then cuts it into a desired size and shape. Float glass is obtained by cutting the glass ribbon G.
[0016] The float glass is, for example, alkali-free glass, aluminosilicate glass, borosilicate glass, or soda-lime glass. 2 OK 2 It means glass that is substantially free of alkali metal oxides such as O. Here, "substantially free of alkali metal oxides" means that the total content of alkali metal oxides is 0.1 mass % or less.
[0017] The use of float glass is not particularly limited, but for example, it is a cover glass for a display (for example, a liquid crystal display or an organic EL display). When the float glass is used as a cover glass, the float glass is a glass for chemical strengthening. Unlike non-alkali glass, the glass for chemical strengthening contains an alkali metal oxide.
[0018] Chemically strengthened glass is, for example, SiO 2 : 62%~68%, Al 2 O 3 : 6%~12%, MgO: 7%~13%, Na 2 O: 9% to 17%, K 2 O: Contains 0% to 7% Na 2 O and K 2 From the total O content to Al 2 O 3 The difference in content is less than 10%, and ZrO 2 If contained, its content is 0.8% or less.
[0019] Another chemically strengthened glass is SiO 2 : 65%~85%, Al 2 O 3 : 3%~15%, Na 2 O: 5% to 15%, K 2 O: 0% to less than 2%, MgO: 0% to 15%, ZrO 2 : Contains 0% to 1% SiO 2 and Al 2 O 3 The total content of SiO 2 +Al 2 O 3 is less than 88%.
[0020] Another chemically strengthened glass is SiO 2 50% to 75%, Al 2 O 3 9% to 20%, Na 2 O 10% to 20%, K 2 O 0%~6%, MgO 0%~15%, CaO, SrO and BaO total amount (CaO+SrO+BaO) 0%~10%, ZrO 2 and TiO 2 The total amount (ZrO 2 +TiO 2 ) at 0% to 5%, B 2 O 3 0% to 10%, Li 2 Contains 0% to 20% O.
[0021] The float glass may be used as a glass substrate for forming a thin film transistor or a color filter of a display. When the float glass is used as a glass substrate, the float glass is an alkali-free glass. Unlike chemically strengthened glass, the alkali-free glass does not substantially contain an alkali metal oxide.
[0022] Non-alkali glass is, for example, SiO 2 : 50%~73%, Al 2 O 3 : 10.5%~24%, B 2 O 3 :0%~12%, MgO:0%~10%, CaO:0%~14.5%, SrO:0%~24%, BaO:0%~13.5%, MgO+CaO+SrO+BaO:8%~29.5%, ZrO 2 :Contains 0% to 5%.
[0023] In the case where the non-alkali glass has both a high strain point and high solubility, it is preferable that the non-alkali glass contains, in mass % based on oxides, SiO 2 : 58%~66%, Al 2 O 3 : 15%~22%, B 2 O 3 : 5% to 12%, MgO: 0% to 8%, CaO: 0% to 9%, SrO: 3% to 12.5%, BaO: 0% to 2%, MgO + CaO + SrO + BaO: 9% to 18%.
[0024] In the case where a high strain point is particularly desired, the alkali-free glass preferably contains, in mass % on an oxide basis, SiO 2 : 54%~73%, Al 2 O 3 : 10.5%~22.5%, B 2 O 3 : 0% to 5.5%, MgO: 0% to 10%, CaO: 0% to 9%, SrO: 0% to 16%, BaO: 0% to 2.5%, MgO+CaO+SrO+BaO: 8% to 26%.
[0025] The thickness of the float glass is selected depending on the application of the float glass. When the float glass is used as a cover glass for a display, the thickness of the float glass is, for example, 0.1 mm to 2.0 mm. On the other hand, when the float glass is used as a glass substrate for a display, the thickness of the float glass is, for example, 0.1 mm to 0.7 mm.
[0026] Next, referring again to FIG. 1, a float bath 2 according to one embodiment will be described. The float bath 2 includes a bath 21. The bath 21 contains a molten metal M. As the molten metal M, for example, molten tin is used. In addition to molten tin, a molten tin alloy can also be used, and the molten metal M may be any metal having a higher density than the molten glass. The molten glass is continuously supplied onto the molten metal M, and is formed into a band-shaped glass ribbon G by utilizing the smooth liquid surface of the molten metal M.
[0027] The float bath 2 has a ceiling 22 that forms a space above the bath 21. The inside of the float bath 2 is filled with reducing gas and maintained at a pressure higher than atmospheric pressure to prevent oxidation of the molten metal M. The reducing gas is, for example, a mixed gas of nitrogen gas and hydrogen gas, containing 85 volume % to 98.5 volume % of nitrogen gas and 1.5 volume % to 15 volume % of hydrogen gas. The reducing gas is supplied from the joints between the bricks of the ceiling 22 and holes in the ceiling 22.
[0028] The float bath 2 includes a heater 23 that heats the glass ribbon G. The heater 23 is suspended from a ceiling 22, for example, and heats the glass ribbon G passing below. The heater 23 is, for example, an electric heater, and is heated by electrical current. A plurality of heaters 23 are arranged in a matrix in the conveying direction and width direction of the glass ribbon G. By controlling the output of the plurality of heaters 23, it is possible to control the temperature distribution of the glass ribbon G and the sheet thickness distribution of the glass ribbon G.
[0029] The dross box 3 includes a lift-out roll 31 that lifts up the glass ribbon G. The lift-out roll 31 is rotationally driven by a driving device (not shown) such as a motor, and conveys the glass ribbon G obliquely upward by the driving force. The driving device is provided outside the dross box 3. Therefore, a hole is formed in the outer wall of the dross box 3 to allow the lift-out roll 31 to pass through.
[0030] A plurality of lift-out rolls 31 are arranged at intervals in the conveying direction (X-axis direction) of the glass ribbon G inside the dross box 3. The number of lift-out rolls 31 is three in Fig. 1, but may be two or more as long as it is more than one. The axial direction of the lift-out rolls 31 is the same as the width direction (Y-axis direction) of the glass ribbon G.
[0031] The dross box 3 includes a carbon member 32 that is in contact with the lift-out roll 31. The carbon member 32 is disposed in the lower space of the dross box 3. The lower space of the dross box 3 is a space below the glass ribbon G. The carbon member 32 is in contact with the outer peripheral surface of the lift-out roll 31, and removes foreign matter adhering to the outer peripheral surface of the lift-out roll 31. The foreign matter includes, for example, oxides formed by oxidation of the molten metal M brought into the inside of the dross box 3 together with the glass ribbon G, that is, so-called dross.
[0032] The carbon member 32 is, for example, a rectangular parallelepiped. The carbon member 32 may be a trapezoid or an inverted trapezoid quadrangular prism when viewed in the X-axis direction. A plurality of carbon members 32 may be provided in the axial direction of the lift-out roll 31. The number of carbon members 32 arranged along each lift-out roll 31 is determined according to the width of the glass ribbon G (dimension in the Y-axis direction) or the axial length of the lift-out roll 31 (dimension in the Y-axis direction).
[0033] The dimension of the carbon member 32 in the Y-axis direction is, for example, 300 mm to 1000 mm, and preferably 400 mm to 800 mm. The dimension of the carbon member 32 in the Z-axis direction is, for example, 50 mm to 200 mm, and preferably 70 mm to 150 mm. The dimension of the carbon member 32 in the X-axis direction is, for example, 20 mm to 100 mm, and preferably 30 mm to 80 mm.
[0034] The carbon member 32 may contain graphite powder. The maximum particle size of the graphite powder is, for example, 0.1 mm to 3 mm, and preferably 0.5 mm to 2.5 mm. When the maximum particle size of the graphite powder is 0.1 mm to 3 mm, the strength of the carbon member 32, which is a compact of the graphite powder, can be ensured.
[0035] The shore hardness of the carbon member 32 is, for example, 20HS to 90HS, and preferably 30HS to 80HS. If the shore hardness of the carbon member 32 is 20HS to 90HS, the abrasion resistance of the carbon member 32 against the lift-out roll 31 can be ensured.
[0036] The dross box 3 may include a biasing member 33 that presses the carbon member 32 against the lift-out roll 31. The biasing member 33 includes, for example, a metal spring. The spring is a leaf spring. Instead of a leaf spring, the biasing member 33 may include a coil spring, a compression coil spring, a disc spring, a volute spring, a ring spring, or the like. The biasing member 33 may include a fluid pressure cylinder such as an air pressure cylinder.
[0037] The dross box 3 may include a support member 34 that supports the carbon member 32 so that it can be raised and lowered. The support member 34 is disposed on a bottom wall 35 of the dross box 3. The support member 34 has a U-shaped cross section perpendicular to the Y-axis direction, and the carbon member 32 and the biasing member 33 are disposed inside the support member 34. The support member 34 prevents the carbon member 32 and the biasing member 33 from shifting in the X-axis direction.
[0038] The dross box 3 may be provided with a heater 37 on the ceiling 36 in order to adjust the temperature of the glass ribbon G. The heater 37 may be provided not only above but also below the glass ribbon G. In the dross box 3, the temperature of the glass ribbon G is preferably (Tg-50°C) to (Tg+30°C) based on the glass transition point Tg of float glass.
[0039] The dross box 3 is provided with a hood 38 above the glass ribbon G, a heat insulating material 39 disposed on the hood 38, and a drape 40 penetrating a part of the heat insulating material 39 and the hood 38 and suspended from the lower surface of the hood 38. The drape 40 is a plate-like member made of a fire-resistant material such as steel or glass.
[0040] The drape 40 divides the upper space of the dross box 3 into a plurality of spaces in the conveying direction (X-axis direction) of the glass ribbon G. The upper space of the dross box 3 is a space above the glass ribbon G. The drape 40 is disposed, for example, directly above the rotation center line of each lift-out roll 31. The drape 40 extends in the axial direction (Y-axis direction) of each lift-out roll 31.
[0041] The annealing furnace 5 anneals the glass ribbon G to a temperature equal to or lower than the strain point of the glass while conveying it by the annealing roll 51. The annealing furnace 5 is provided with heaters (not shown) on the ceiling and bottom wall in order to adjust the temperature of the glass ribbon G. The annealing roll 51 is driven to rotate by a driving device (not shown) such as a motor, and conveys the glass ribbon G in the horizontal direction by the driving force. The annealing furnace 5 is open to the outside at the outlet on the downstream side. Therefore, the air flows into the inside of the annealing furnace 5.
[0042] Next, an example of the annealing furnace 5 will be described with reference to Fig. 1 and Fig. 2. As shown in Fig. 1, the annealing furnace 5 has, for example, a furnace body 52, a first gas discharge nozzle 53, a second gas discharge nozzle 54, a gas concentration meter 55, and a gas suction nozzle 56. Furthermore, as shown in Fig. 2, the annealing furnace 5 may have an ejector 57 and a vertical pipe 58.
[0043] As shown in Fig. 2, the furnace body 52 has, for example, a rectangular shape when viewed in the X-axis direction. The furnace body 52 includes a pair of side wall portions 521, 522, a ceiling portion 523, and a bottom wall portion 524. The pair of side wall portions 521, 522 are provided to sandwich the conveying path of the glass ribbon G in the Y-axis direction. The ceiling portion 523 closes the upper side of the conveying path of the glass ribbon G. The bottom wall portion 524 closes the lower side of the conveying path of the glass ribbon G. The pair of side wall portions 521, 522 are provided vertically so as to be perpendicular to the Y-axis direction, and the ceiling portion 523 and the bottom wall portion 524 are provided horizontally.
[0044] 1, the first gas discharge nozzle 53 discharges sulfur oxide gas from below the transport path of the glass ribbon G toward the transport path. The first gas discharge nozzle 53 extends in the Y-axis direction, for example, and has a plurality of gas discharge ports spaced apart in the Y-axis direction. Each gas discharge port discharges sulfur oxide gas upward.
[0045] The sulfur oxide gas reacts with the lower surface of the glass ribbon G to form a buffer film on the lower surface of the glass ribbon G. The buffer film buffers collisions between the glass ribbon G and the layer roll 51, and suppresses the occurrence of scratches on the lower surface of the glass ribbon G. The buffer film contains sulfate crystals and the like. Sulfate crystals are formed in an oxidizing atmosphere.
[0046] The first gas discharge nozzle 53 discharges sulfur oxide gas, for example, SO 2 The gas is discharged and sulfate crystals are formed.
[0047] The first gas discharge nozzle 53 is disposed, for example, between the first and second layer rolls 51, 51 from the upstream side to the downstream side in the conveying direction of the glass ribbon G. The first (most upstream) layer roll 51 can block the reducing gas that has flowed from inside the dross box 3 into the annealing furnace 5 toward the discharge port of the sulfur oxide gas. This can prevent the flow of the sulfur oxide gas from being disturbed. In addition, a buffer film can be formed relatively upstream of the annealing furnace 5, which can prevent scratches from occurring on the lower surface of the glass ribbon G.
[0048] Although not shown, the first gas discharge nozzle 53 may be disposed upstream of the first (most upstream) layer roll 51. Although not shown, the first gas discharge nozzle 53 may be disposed downstream of the second layer roll 51 in the transport direction.
[0049] The second gas discharge nozzle 54 discharges an oxygen-containing gas from below the transport path of the glass ribbon G toward the transport path. The second gas discharge nozzle 54 extends in the Y-axis direction, for example, and has a plurality of gas discharge ports spaced apart in the Y-axis direction. Each gas discharge port discharges the oxygen-containing gas upward.
[0050] The oxygen-containing gas may be any gas that contains oxygen, and may be pure oxygen gas or air. The oxygen gas concentration around the first gas discharge nozzle 53 can be increased to promote the production of sulfates.
[0051] The second gas discharge nozzle 54 is preferably disposed adjacent to the first gas discharge nozzle 53, and may be disposed, for example, between the first and second layer rolls 51, 51 from the upstream side to the downstream side in the conveying direction of the glass ribbon G. The oxygen gas concentration in the vicinity of the first gas discharge nozzle 53 can be efficiently increased.
[0052] The second gas discharge nozzle 54 may be provided adjacent to the first gas discharge nozzle 53, and like the first gas discharge nozzle 53, may be disposed upstream of the first (most upstream) layer roll 51, or downstream of the second layer roll 51 in the conveying direction.
[0053] Gas concentration meter 55 is O 2 Gas concentration, SO 2 Gas concentration, or H 2The gas concentration meter 55 measures the O gas concentration, etc. Gas concentration meter 55 is provided next to first gas discharge nozzle 53, for example, below first gas discharge nozzle 53. The gas concentration meter 55 can detect a desired gas concentration around first gas discharge nozzle 53, and can adjust the gas flow rate so that the gas concentration falls within an allowable range. Although not shown, a pressure meter may be provided next to gas concentration meter 55. The pressure meter measures the pressure around first gas discharge nozzle 53.
[0054] Incidentally, if the gap between the upper surface of the glass ribbon G and the drape 40 inside the dross box 3 is narrow, the reducing gas may forcefully flow from the inside of the dross box 3 into the inside of the annealing furnace 4. The reducing gas flows along the upper surface of the glass ribbon G.
[0055] Conventionally, the reducing gas that flowed in would flow from above to below the glass ribbon G and reach the periphery of the first gas discharge nozzle 53. As a result, there were problems such as disturbance of the flow of the sulfur oxide gas or a decrease in the oxygen concentration around the gas discharge nozzle. This prevented the formation of a buffer film, and made it easy for scratches to occur on the lower surface of the glass ribbon.
[0056] The gas suction nozzle 56 is inserted inward from the side wall portions 521, 522, and sucks gas above the transport path of the glass ribbon G. In this embodiment, the gas suction nozzle 56 sucks gas upward from below, but may suck gas from the sides to the sides. The gas suction nozzle 56 may be provided on only one of the pair of side wall portions 521, 522.
[0057] The gas suction nozzle 56 is disposed upstream of the first gas discharge nozzle 53 in the transport direction of the glass ribbon G. The gas suction nozzle 56 may be disposed at the same position as the first gas discharge nozzle 53 in the transport direction of the glass ribbon G.
[0058] According to the present embodiment, the gas suction nozzle 56 is disposed upstream of the first gas discharge nozzle 53 in the transport direction of the glass ribbon G, or disposed at the same position as the first gas discharge nozzle 53, and sucks upward the reducing gas flowing along the upper surface of the glass ribbon G. This makes it possible to restrict the reducing gas from reaching the periphery of the first gas discharge nozzle 53, suppress inhibition of the formation of the buffer film, and improve the quality of the glass ribbon.
[0059] As a technique different from the technique of the present disclosure, it is also possible to provide an opening in the ceiling portion 523 of the furnace body 52 and discharge the reducing gas from the opening to the outside of the furnace body 52. However, providing an opening in the ceiling portion 523 reduces the thermal insulation property of the ceiling portion 523. As a result, the glass ribbon G is rapidly cooled below the opening, and large residual stress is generated in the glass ribbon G.
[0060] According to the present embodiment, no opening is provided in the ceiling portion 523, and the gas suction nozzle 56 is inserted through a small opening in the side wall portions 521 and 522. This makes it possible to suppress a decrease in the thermal insulation property of the furnace body 52, to suppress a rapid decrease in the temperature of the glass ribbon G, and to reduce residual stress generated in the glass ribbon G.
[0061] The gas suction nozzle 56 may be disposed directly above a region where the temperature of the glass ribbon G is equal to or higher than the strain point. The reducing gas flowing in from the dross box 3 can be sucked by the gas suction nozzle 56 on a relatively upstream side of the annealing furnace 5. Thus, the reducing gas can be discharged to the outside of the furnace body 52 before it diffuses.
[0062] The gas suction nozzle 56 is disposed, for example, upstream of the first layer roll 51 from the upstream side to the downstream side in the conveying direction of the glass ribbon G. At the most upstream of the annealing furnace 5, the reducing gas flowing in from the dross box 3 can be sucked by the gas suction nozzle 56. Thus, the reducing gas can be discharged to the outside of the furnace body 52 before it diffuses.
[0063] The gas suction nozzle 56 extends in the Y-axis direction from each of the pair of side wall portions 521, 522 to above the transport path of the glass ribbon G, and sucks gas from below upward. The gas suction nozzle 56 sucks gas from below directly upward or obliquely upward. The gas suction nozzle 56 includes a suction port 56a that sucks gas.
[0064] For example, when viewed from above, the suction port 56a of one gas suction nozzle 56 may overlap at least one widthwise end Ga of the glass ribbon G and extend outward in the width direction from the one widthwise end Ga of the glass ribbon G. Furthermore, when viewed from above, the suction port 56a of another gas suction nozzle 56 may overlap at least the other widthwise end Gb of the glass ribbon G and extend outward in the width direction from the other widthwise end Gb of the glass ribbon G.
[0065] The reducing gas inside the dross box 3 passes through a gap between the lift-out roll 31 and the drape 40 and flows into the annealing furnace 5. At this time, since the glass ribbon G is not present on the outer side of the glass ribbon G in the width direction, the size of the gap is large and a flow of reducing gas is easily formed.
[0066] When viewed from above, if the suction port 56a of one gas suction nozzle 56 extends from one widthwise end Ga of the glass ribbon G to the widthwise outer side, it can efficiently suck up the reducing gas flowing on the widthwise outer side of the glass ribbon G. Similarly, when viewed from above, if the suction port 56a of another gas suction nozzle 56 extends from the other widthwise end Gb of the glass ribbon G to the widthwise outer side, it can efficiently suck up the reducing gas flowing on the widthwise outer side of the glass ribbon G.
[0067] When viewed from above, the suction port 56a of one gas suction nozzle 56 may extend from one widthwise end of the glass ribbon G to the widthwise center, and the suction port 56a of another gas suction nozzle 56 may extend from the other widthwise end to the widthwise center of the glass ribbon G. The reducing gas can be sucked over the entire width of the glass ribbon G.
[0068] In this embodiment, the gas suction nozzle 56 sucks the gas from below upward, but the gas from the side may also be sucked laterally. In this case, for example, when viewed from above, the suction port 56a of one gas suction nozzle 56 may be arranged facing one end in the width direction of the glass ribbon G to suck the reducing gas flowing on the outer side in the width direction of the glass ribbon G. Both the gas suction nozzle 56 that sucks the gas from below upward and the gas suction nozzle 56 that sucks the gas from the side laterally may be used.
[0069] The ejector 57 adjusts the suction amount of the gas suction nozzle 56. By adjusting the suction amount of the gas suction nozzle 56, it is possible to keep the concentrations of various gases within an allowable range around the first gas discharge nozzle 53. The suction amount of the gas suction nozzle 56 may be controlled based on the measurement results of the gas concentration meter 55.
[0070] The vertical pipe 58 extends upward from one end of the gas suction nozzle 56 outside the pair of sidewalls 521, 522. The gas sucked by the gas suction nozzle 56 is cooled in the process of rising up the vertical pipe 58. The gas temperature decreases from the bottom to the top of the vertical pipe 58. The gas temperature difference can form an ascending air current inside the vertical pipe 58, and the gas can be efficiently drawn into the gas suction nozzle 56. In addition, it is easier to secure a space for workers to work beside the furnace body 52 compared to the case where the vertical pipe 58 extends from one end of the gas suction nozzle 56 in the X-axis direction.
[0071] The ejector 57 is provided at the lower end of the vertical pipe 58 and includes an ejector nozzle 57a that ejects gas such as compressed air upward. The gas ejected from the ejector nozzle 57a can increase the upward speed of the ascending air current formed inside the vertical pipe 58, and the gas can be drawn into the gas suction nozzle 56 more efficiently. EXAMPLES
[0072] Experimental data will be described below. Example 1 below is a comparative example, and Examples 2 to 4 are working examples. In Examples 1 to 4, float glass was produced under the conditions shown in Table 1 using the float glass production apparatus 1 shown in Figs. 1 and 2. In Examples 1 to 4, the amount of gas suctioned by the gas suction nozzle 56 (unit: Nm 3 For example, the discharge rate (unit: NL / min) of the first gas discharge nozzle 53 and the discharge rate (unit: NL / min) of the second gas discharge nozzle 54 were set to the same in Examples 1 to 4.
[0073] [Table 1] In Table 1, the suction amount of the gas suction nozzle 56, O 2 Gas concentration, SO 2 Gas concentration, H 2 The O gas concentration and pressure are shown as relative values. 2 Gas concentration (unit: volume %), SO 2 Gas concentration (unit: volume ppm), H 2 O gas concentration (unit: g / cm 3 ) was measured by a gas concentration meter 55. Moreover, the pressure (unit: Pa) is the differential pressure from the atmospheric pressure, and was measured by a pressure gauge next to the gas concentration meter 55.
[0074] As shown in Table 1, in Example 1, gas was not sucked by the gas suction nozzle 56, whereas in Examples 2 to 4, gas was sucked by the gas suction nozzle 56. As a result, in Examples 2 to 4, the amount of O was smaller than that in Example 1 around the first gas discharge nozzle 53. 2 Gas concentration, and SO 2 High gas concentration, H 2 The O gas concentration was low.
[0075] Reducing gas flows from the inside of the dross box 3 into the inside of the annealing furnace 5, and H contained in the reducing gas 2 When the gas reaches the periphery of the first gas discharge nozzle 53, H 2 Gas and O 2 The gas reacts to produce H 2As a result, H gas is generated around the first gas discharge nozzle 53. 2 The O gas concentration increases, and O 2 The gas concentration decreases.
[0076] From the results in Table 1, it can be seen that by sucking the gas using the gas suction nozzle 56, the reducing gas that flows from inside the dross box 3 into the annealing furnace 5 can be restricted from reaching the periphery of the first gas discharge nozzle 53.
[0077] In addition, the results of Table 1 show that the more the amount of gas suctioned by the gas suction nozzle 56 is increased, the more the O 2 Gas concentration, and SO 2 The gas concentration can be increased, 2 It can be seen that the O gas concentration can be reduced. In Example 4, the pressure is low because the amount of gas suctioned by the gas suction nozzle 56 was large.
[0078] The float glass manufacturing apparatus and the float glass manufacturing method according to the present disclosure have been described above, but the present disclosure is not limited to the above-mentioned embodiments. Various changes, modifications, substitutions, additions, deletions, and combinations are possible within the scope of the claims. These naturally fall within the technical scope of the present disclosure. [Explanation of symbols]
[0079] 1. Float glass manufacturing equipment 2. Float Bath 3 Dross Box 5 Annealing furnace 51 Layer Roll 521, 522 Side wall 523 Ceiling 53 First gas discharge nozzle (gas discharge nozzle) 56 Gas suction nozzle M Molten metal G Glass ribbon
Claims
1. A float glass manufacturing apparatus comprising: a float bath for forming a glass ribbon on a molten metal; a dross box having a plurality of lift-out rolls for lifting up the glass ribbon; and an annealing furnace having a plurality of layer rolls for transporting the glass ribbon, the annealing furnace includes a pair of side wall portions provided on either side of a transport path for the glass ribbon, a ceiling portion that closes an upper portion of the transport path, a gas discharge nozzle that discharges sulfur oxide gas from below the transport path toward the transport path, and a gas suction nozzle that is inserted inward from the side wall portions and, above the transport path, sucks a gas below upward or sucks a gas on a side laterally, the gas suction nozzle is disposed at the same position as the gas discharge nozzle in a conveying direction of the glass ribbon, or is disposed upstream of the gas discharge nozzle.
2. The float glass manufacturing apparatus according to claim 1 , wherein the gas suction nozzle is disposed directly above a region where the temperature of the glass ribbon is equal to or higher than the strain point.
3. 3. The float glass manufacturing apparatus according to claim 1, wherein the annealing furnace has an ejector for adjusting a suction amount of the gas suction nozzle.
4. 4. The float glass manufacturing apparatus according to claim 1, wherein the annealing furnace has a vertical pipe extending upward from one end of the gas suction nozzle outside the pair of side wall portions.
5. the annealing furnace includes a vertical pipe extending upward from one end of the gas suction nozzle outside the pair of side wall portions, and an ejector that adjusts a suction amount of the gas suction nozzle, 3. The float glass manufacturing apparatus according to claim 1, wherein the ejector includes an ejector nozzle provided at a lower end of the vertical pipe and ejecting gas upward.
6. The float glass manufacturing apparatus according to any one of claims 1 to 5, wherein the gas discharge nozzle is disposed between a first layer roll and a second layer roll from the upstream side to the downstream side in the conveying direction.
7. The float glass manufacturing apparatus according to any one of claims 1 to 6, wherein the gas suction nozzle is disposed upstream of a first layer roll from the upstream side to the downstream side in the conveying direction.
8. the gas suction nozzle includes a suction port for suctioning a gas, 8. The float glass manufacturing apparatus according to claim 1, wherein, when viewed from above, the suction port of the gas suction nozzle overlaps with one end of the glass ribbon in the width direction and extends outward in the width direction from the one end of the glass ribbon in the width direction.
9. A method for producing float glass, comprising the steps of: producing float glass by using the float glass producing apparatus according to any one of claims 1 to 8.
Citation Information
Patent Citations
Atmosphere partitioning device and float glass manufacturing device
JP2016050160A
Plate glass with protective film and method of manufacturing the plate glass
WO2002051767A1
Device for manufacturing float plate glass and method for manufacturing float plate glass
WO2014077286A1
Float glass production device and float glass production method
WO2019221084A1