Positive electrodes and lithium-ion batteries

By combining a first active material with Mn and a second active material without Mn in the O2 type structure, the positive electrode's resistance in the Mn redox region is reduced, enhancing its capacity.

JP7593301B2Active Publication Date: 2024-12-03TOYOTA JIDOSHA KK
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021185854
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-11-15
Publication Date
2024-12-03
Estimated Expiration
2041-11-15

AI Technical Summary

Technical Problem

Conventional positive electrodes using a positive electrode active material with an O2 type structure containing Li, Mn, and O exhibit high resistance in the Mn redox region, leading to decreased capacity.

Method used

A positive electrode comprising a first active material with an O2 type structure containing Li, Mn, and O, and a second active material with an O2 type structure not containing Mn, which has low resistance in the Mn redox region, is used to construct the positive electrode.

Benefits of technology

The combination of these materials suppresses the overall resistance increase of the positive electrode, thereby improving its capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593301000001
    Figure 0007593301000001
  • Figure 0007593301000002
    Figure 0007593301000002
  • Figure 0007593301000003
    Figure 0007593301000003
Patent Text Reader

Abstract

To disclose a high capacity positive electrode for a lithium ion battery.SOLUTION: A positive electrode includes a first active material and a second active material, and the first active material contains at least Li, Mn, and O as constituent elements and has an O2 type structure, and the second active material contains at least Li, a transition metal element, and O as constituent elements, does not contain Mn, and has an O2 type structure.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application discloses a positive electrode and a lithium ion battery. [Background technology]

[0002] Patent Document 1 discloses a positive electrode active material that contains at least Li, Co, Ni, Mn, and O as constituent elements and has an O2 type structure. Patent Document 2 discloses a technique for attaching at least one of a predetermined complex oxide and a complex fluoride to the surface of a positive electrode active material having an O2 type structure. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2015-176644 A [Patent Document 2] JP 2016-033887 A Summary of the Invention [Problem to be solved by the invention]

[0004] According to the new findings of the present inventors, a positive electrode active material containing at least Li, Mn, and O as constituent elements and having an O2 type structure has a resistance of 3V (vs. Li / Li + ) The resistance becomes high in the redox region of Mn below. When a positive electrode is constructed using such a positive electrode active material, the resistance of the positive electrode as a whole increases in the redox region of Mn, and as a result, the capacity of the positive electrode may decrease. In this respect, there is room for improvement in the capacity of conventional positive electrodes. [Means for solving the problem]

[0005] As one of the means for solving the above problems, the present application provides: a positive electrode comprising a first active material and a second active material; The first active material contains at least Li, Mn, and O as constituent elements and has an O2 type structure; The second active material contains at least Li, a transition metal element, and O as constituent elements, does not contain Mn, and has an O2 type structure. positive electrode Disclose.

[0006] In the positive electrode of the present disclosure, the first active material may contain at least Li, Mn, at least one of Ni and Co, and O as constituent elements.

[0007] In the positive electrode of the present disclosure, the second active material may contain at least Li, Co, and O as constituent elements.

[0008] The positive electrode of the present disclosure may contain the first active material in an amount of 10% by mass or more and 90% by mass or less, where the total of the first active material and the second active material is 100% by mass.

[0009] As one of the means for solving the above problems, the present application provides: A lithium ion battery comprising the positive electrode of the present disclosure. Disclose. Effect of the Invention

[0010] In the positive electrode of the present disclosure, a first active material containing Mn and a second active material not containing Mn are used together as a positive electrode active material having an O2 type structure. In this case, the resistance of the second active material is small even at a potential in the redox region of Mn, and the increase in the resistance of the positive electrode as a whole is suppressed. As a result, the capacity of the positive electrode is easily improved. [Brief description of the drawings]

[0011] [Figure 1] 1A and 1B are schematic diagrams illustrating a configuration of a positive electrode according to an embodiment and a configuration of a lithium ion battery including the positive electrode. [Diagram 2] 1 shows the relationship between the mixing ratio of two types of O2 type positive electrode active materials (first active material and second active material) and the discharge capacity of the positive electrode. [Diagram 3] 1 shows the relationship between the mixing ratio of the O2 type positive electrode active material (first active material) and the O3 type positive electrode active material (third active material) and the discharge capacity of the positive electrode. [Figure 4] The results of measuring the DCIR resistance of the positive electrode for each of the cases of SOC 40% and SOC 20% are shown. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] 1. Positive electrode The positive electrode of the present disclosure includes a first active material and a second active material. The first active material includes at least Li, Mn, and O as constituent elements, and has an O2 type structure. The second active material includes at least Li, a transition metal element, and O as constituent elements, does not include Mn, and has an O2 type structure. As shown in FIG. 1, a positive electrode 10 according to one embodiment may include a positive electrode active material layer 11 and a positive electrode current collector 12, and in this case, the positive electrode active material layer 11 may include a first active material and a second active material.

[0013] 1.1 Cathode active material layer The positive electrode active material layer 11 includes at least a first active material and a second active material as the positive electrode active material, and may further include an electrolyte, a conductive assistant, a binder, and the like. The contents of the positive electrode active material, the electrolyte, the conductive assistant, the binder, and the like in the positive electrode active material layer 11 may be appropriately determined according to the intended battery performance. For example, the content of the positive electrode active material may be 40 mass% or more, 50 mass% or more, or 60 mass% or more, and may be 100 mass% or less, or 90 mass% or less, with the entire positive electrode active material layer 11 (total solid content) being 100 mass%. The shape of the positive electrode active material layer 11 is not particularly limited, and may be, for example, a sheet-like positive electrode active material layer 11 having a substantially flat surface. The thickness of the positive electrode active material layer 11 is not particularly limited, and may be, for example, 0.1 μm or more or 1 μm or more, and may be 2 mm or less or 1 mm or less.

[0014] 1.1.1 Cathode active material The positive electrode active material layer 11 contains at least a first active material and a second active material as positive electrode active materials. The first active material contains at least Li, Mn, and O as constituent elements, and has an O2 type structure. The second active material contains at least Li, a transition metal element, and O as constituent elements, does not contain Mn, and has an O2 type structure. In this way, in the positive electrode of the present disclosure, the first active material containing Mn and the second active material not containing Mn are used in combination as the positive electrode active material having an O2 type structure, thereby achieving a redox region of Mn at 3V (vs. Li / Li + ) or less, the resistance of the second active material is small, and an increase in the resistance of the positive electrode as a whole is suppressed. In other words, the second active material can compensate for the weaknesses of the first active material, and the capacity of the positive electrode can be easily improved.

[0015] The first active material contains at least Mn as a constituent element, and tends to have high resistance in the redox region of Mn. In this respect, it is difficult to obtain a high positive electrode capacity with the first active material alone. On the other hand, by forming a lithium ion battery using a positive electrode containing the first active material, it is easy to improve the cycle characteristics, etc., of the secondary battery.

[0016] The first active material may contain, as a constituent element, Mn and a transition metal element other than Mn. In particular, when the first active material contains, as constituent elements, at least Li, Mn, at least one of Ni and Co, and O, and especially when the first active material contains, as constituent elements, Li, Mn, Ni, Co, and O, the cycle characteristics and the like of a lithium ion battery are more likely to be improved.

[0017] The first active material is Li x Mn a Ni b Co c O 2±δIt may have the chemical composition represented by. x, a, b, and c are not particularly limited as long as the O2-type structure can be maintained. For example, x satisfies 0 < x < 1. x may be 0.1 or more, 0.2 or more, 0.3 or more, 0.4 or more, 0.5 or more, or 0.6 or more, and may be 0.9 or less or 0.8 or less. Also, for example, a, b, and c each satisfy 0 < a < 1, 0 ≤ b < 1, and 0 ≤ c < 1. a may be more than 0, 0.1 or more, 0.2 or more, 0.3 or more, or 0.4 or more, and may be 0.9 or less, 0.8 or less, 0.7 or less, or 0.6 or less. b may be 0 or more or 0.1 or more, and may be 0.9 or less, 0.8 or less, 0.7 or less, 0.6 or less, 0.5 or less, 0.4 or less, or 0.3 or less. c may be 0 or more, 0.1 or more, or 0.2 or more, and may be 0.9 or less, 0.8 or less, 0.7 or less, 0.6 or less, 0.5 or less, or 0.4 or less. a + b + c may be 0.8 or more or 0.9 or more, and may be 1.2 or less or 1.1 or less.

[0018] The second active material does not contain Mn as a constituent element and has low diffusion resistance even at the redox potential of Mn. On the other hand, the second active material has problems different from those of the first active material, such as Na being likely to remain in the crystal structure. In this regard, it is difficult to improve the cycle characteristics and the like when using the second active material alone as a lithium-ion battery, and it is also difficult to obtain a high positive electrode capacity.

[0019] The transition metal element constituting the second active material may be a transition metal element other than Mn, and its type is not particularly limited as long as the O2-type structure can be maintained. For example, Co, Ni, etc. may be mentioned. In particular, when the second active material contains at least Li, Co, and O as constituent elements, it is easier to further improve the positive electrode capacity by combining with the above-mentioned first active material.

[0020] The second active material is Li x Ni d Co e O 2±δIt may have a chemical composition represented by. x, d, and e are not particularly limited as long as the O2-type structure can be maintained. For example, x satisfies 0 < x < 1. x may be 0.1 or more, 0.2 or more, 0.3 or more, 0.4 or more, 0.5 or more, or 0.6 or more, and may be 0.9 or less or 0.8 or less. Also, for example, d satisfies 0 ≦ d < 1, and e satisfies 0 < e ≦ 1.2. d may be 0 or more or 0.1 or more, and may be 0.9 or less, 0.8 or less, 0.7 or less, 0.6 or less, 0.5 or less, 0.4 or less, or 0.3 or less. e may be more than 0, 0.1 or more, 0.2 or more, 0.3 or more, 0.4 or more, or 0.5 or more, and may be 1.0 or less or 0.9 or less. d + e may be 0.8 or more or 0.9 or more, and may be 1.2 or less or 1.1 or less.

[0021] A protective layer containing a Li-ion conductive oxide may be formed on the surface of the positive electrode active material. That is, the positive electrode active material layer 11 may include a first composite including a first active material and a protective layer provided on the surface thereof, or may include a second composite including a second active material and a protective layer provided on the surface thereof. Thereby, reactions between the positive electrode active material and a sulfide (for example, a sulfide solid electrolyte described later) and the like are likely to be suppressed. Examples of the Li-ion conductive oxide include Li3BO3, LiBO2, Li2CO3, LiAlO2, Li4SiO4, Li2SiO3, Li3PO4, Li2SO4, Li2TiO3, Li4Ti5O 12 , Li2Ti2O5, Li2ZrO3, LiNbO3, Li2MoO4, Li2WO4. The coverage rate (area ratio) of the protective layer may be, for example, 70% or more, 80% or more, or 90% or more. The thickness of the protective layer may be, for example, 0.1 nm or more or 1 nm or more, and may be 100 nm or less or 20 nm or less.

[0022] The shape of the positive electrode active material may be any shape that is common for battery active materials. For example, both the first active material and the second active material may be particulate. The positive electrode active material particles may be solid particles, hollow particles, or particles having voids. The positive electrode active material particles may be primary particles, or secondary particles formed by agglomeration of a plurality of primary particles. The average particle diameter (D50) of the positive electrode active material particles may be, for example, 1 nm or more, 5 nm or more, or 10 nm or more, and may be 500 μm or less, 100 μm or less, 50 μm or less, or 30 μm or less. The average particle diameter D50 in the present application is the particle diameter (median diameter) at an integrated value of 50% in a volume-based particle size distribution obtained by a laser diffraction / scattering method.

[0023] There is no particular limitation on the content ratio of the first active material to the second active material in the positive electrode 10. In particular, when the positive electrode 10 contains 10% by mass or more and 90% by mass or less of the first active material, with the total of the first active material and the second active material being 100% by mass, the capacity is more likely to be improved.

[0024] The positive electrode active material layer 11 may contain only the first active material and the second active material as the positive electrode active material. Alternatively, the positive electrode active material layer 11 may contain, in addition to the first active material and the second active material, a different type of positive electrode active material (another positive electrode active material). From the viewpoint of further enhancing the effect of the technology of the present disclosure, the content of the other positive electrode active material in the positive electrode active material layer 11 may be small. For example, the total of the first active material and the second active material may account for 50 mass% or more, 60 mass% or more, 70 mass% or more, 80 mass% or more, 90 mass% or more, 95 mass% or more, or 99 mass% or more of the total positive electrode active material contained in the positive electrode active material layer 11.

[0025] 1.1.2 Electrolytes The electrolyte may be a solid electrolyte or a liquid electrolyte (electrolytic solution). When the positive electrode 10 is a positive electrode for an all-solid-state battery, the positive electrode active material layer 11 may contain a solid electrolyte as the electrolyte. When the positive electrode 10 is a positive electrode for an electrolyte battery, the positive electrode active material layer 11 may contain an electrolyte as the electrolyte.

[0026] The solid electrolyte may be any known solid electrolyte for batteries. The solid electrolyte may be an inorganic solid electrolyte or an organic polymer electrolyte. In particular, inorganic solid electrolytes have excellent ion conductivity and heat resistance. Examples of inorganic solid electrolytes include lithium lanthanum zirconate, LiPON, and Li 1+X Al X Ge 2-X Examples of the solid electrolyte include oxide solid electrolytes such as (PO4)3, Li-SiO-based glass, and Li-Al-SO-based glass; and sulfide solid electrolytes such as Li2S-P2S5, Li2S-SiS2, LiI-Li2S-SiS2, LiI-Si2S-P2S5, Li2S-P2S5-LiI-LiBr, LiI-Li2S-P2S5, LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, and Li2S-P2S5-GeS2. In particular, the performance of the sulfide solid electrolyte, particularly the sulfide solid electrolyte containing Li2S-P2S5, is high. The solid electrolyte may be amorphous or crystalline. The solid electrolyte may be, for example, particulate. Only one type of solid electrolyte may be used alone, or two or more types may be used in combination.

[0027] The electrolyte may contain, for example, lithium ions as carrier ions. The electrolyte may be an aqueous electrolyte or a non-aqueous electrolyte. The composition of the electrolyte may be the same as that of the electrolyte of a lithium ion battery. For example, the electrolyte may be a carbonate-based solvent in which a lithium salt is dissolved at a predetermined concentration. Examples of the carbonate-based solvent include fluoroethylene carbonate (FEC), ethylene carbonate (EC), and dimethyl carbonate (DMC). Examples of the lithium salt include LiPF6.

[0028] 1.1.3 Conductive additives Examples of the conductive assistant include carbon materials such as vapor grown carbon fiber (VGCF), acetylene black (AB), ketjen black (KB), carbon nanotubes (CNT), and carbon nanofibers (CNF); and metal materials such as nickel, aluminum, and stainless steel. The conductive assistant may be, for example, particulate or fibrous, and the size is not particularly limited. Only one type of conductive assistant may be used alone, or two or more types may be used in combination.

[0029] 1.1.4 Binders Examples of the binder include butadiene rubber (BR)-based binders, butylene rubber (IIR)-based binders, acrylate butadiene rubber (ABR)-based binders, styrene butadiene rubber (SBR)-based binders, polyvinylidene fluoride (PVdF)-based binders, polytetrafluoroethylene (PTFE)-based binders, polyimide (PI)-based binders, etc. Only one type of binder may be used alone, or two or more types may be used in combination.

[0030] 1.2 Positive electrode current collector As shown in FIG. 1, the positive electrode 10 may include a positive electrode collector 12 in contact with the positive electrode active material layer 11. The positive electrode collector 12 may be any of those commonly used as a positive electrode collector for a battery. The positive electrode collector 12 may be in the form of a foil, a plate, a mesh, a punched metal, a foam, or the like. The positive electrode collector 12 may be made of a metal foil or a metal mesh. In particular, a metal foil is excellent in terms of ease of handling. The positive electrode collector 12 may be made of a plurality of foils. Examples of metals constituting the positive electrode collector 12 include Cu, Ni, Cr, Au, Pt, Ag, Al, Fe, Ti, Zn, Co, stainless steel, and the like. In particular, from the viewpoint of ensuring oxidation resistance, the positive electrode collector 12 may contain Al. The positive electrode collector 12 may have some kind of coating layer on its surface for the purpose of adjusting resistance, or the like. The positive electrode current collector 12 may be a metal foil or a substrate plated or vapor-deposited with the above metal. When the positive electrode current collector 12 is made of a plurality of metal foils, some layer may be present between the plurality of metal foils. The thickness of the positive electrode current collector 12 is not particularly limited. For example, it may be 0.1 μm or more or 1 μm or more, and may be 1 mm or less or 100 μm or less.

[0031] 1.3 Other In addition to the above configuration, the positive electrode 10 may have a general configuration as a positive electrode of a battery. For example, a tab, a terminal, etc. The positive electrode 10 can be manufactured by a known method except for using the above-mentioned first active material and the second active material in combination as the positive electrode active material. For example, the positive electrode active material layer 11 can be easily formed by forming a positive electrode mixture containing the above-mentioned various components in a dry or wet manner. The positive electrode active material layer 11 may be formed together with the positive electrode current collector 12 or may be formed separately from the positive electrode current collector 12.

[0032] 2. Lithium-ion battery The lithium ion battery of the present disclosure includes the above-mentioned positive electrode. For example, as shown in Fig. 1, a lithium ion battery 100 according to one embodiment has a positive electrode 10, an electrolyte layer 20, and a negative electrode 30. The positive electrode 10 is as described above.

[0033] 2.1 Electrolyte layer The electrolyte layer 20 contains at least an electrolyte. When the lithium ion battery 100 is a solid-state battery (a battery containing a solid electrolyte, which may be a battery partially using a liquid electrolyte in combination, or an all-solid-state battery not containing a liquid electrolyte), the electrolyte layer 20 contains a solid electrolyte and may further contain a binder or the like. In this case, the content of the solid electrolyte and the binder or the like in the electrolyte layer 20 is not particularly limited. On the other hand, when the lithium ion battery 100 is an electrolyte battery, the electrolyte layer 20 contains an electrolyte solution and may further have a separator or the like for holding the electrolyte solution and preventing contact between the positive electrode active material layer 11 and the negative electrode active material layer 31. The thickness of the electrolyte layer 20 is not particularly limited, and may be, for example, 0.1 μm or more or 1 μm or more, and may be 2 mm or less or 1 mm or less.

[0034] The solid electrolyte, the electrolytic solution, the binder, and the like are as described above. The separator may be any separator that is commonly used in lithium ion batteries, and may be made of resin such as polyethylene (PE), polypropylene (PP), polyester, and polyamide. The separator may have a single layer structure or a multi-layer structure. Examples of the multi-layer structure separator include a separator with a two-layer structure of PE / PP, or a separator with a three-layer structure of PP / PE / PP or PE / PP / PE. The separator may be made of a nonwoven fabric such as a cellulose nonwoven fabric, a resin nonwoven fabric, or a glass fiber nonwoven fabric.

[0035] 2.2 Negative electrode As shown in FIG. 1, the negative electrode 30 may include a negative electrode active material layer 31 and a negative electrode current collector 32.

[0036] 2.2.1 Negative electrode active material layer The negative electrode active material layer 31 contains at least a negative electrode active material, and may further contain an electrolyte, a conductive assistant, a binder, and the like. The contents of the negative electrode active material, electrolyte, conductive assistant, binder, and the like in the negative electrode active material layer 31 may be appropriately determined according to the target battery performance. For example, the content of the negative electrode active material may be 40 mass% or more, 50 mass% or more, or 60 mass% or more, and may be 100 mass% or less, or 90 mass% or less, with the entire negative electrode active material layer 31 (total solid content) being 100 mass%. The shape of the negative electrode active material layer 31 is not particularly limited, and may be, for example, a sheet-like negative electrode active material layer having a substantially flat surface. The thickness of the negative electrode active material layer 31 is not particularly limited, and may be, for example, 0.1 μm or more or 1 μm or more, and may be 2 mm or less or 1 mm or less.

[0037] As the negative electrode active material, various materials having a potential (charge / discharge potential) for absorbing and releasing lithium ions that is lower than that of the positive electrode active material can be used. For example, silicon-based active materials such as Si, Si alloys, and silicon oxide; carbon-based active materials such as graphite and hard carbon; various oxide-based active materials such as lithium titanate; metallic lithium, lithium alloys, and the like can be used. Only one type of negative electrode active material may be used alone, or two or more types may be used in combination.

[0038] The shape of the negative electrode active material may be any shape that is common for a negative electrode active material of a battery. For example, the negative electrode active material may be in a particulate form. The negative electrode active material particles may be primary particles or secondary particles formed by agglomeration of a plurality of primary particles. The average particle diameter (D50) of the negative electrode active material particles may be, for example, 1 nm or more, 5 nm or more, or 10 nm or more, and may be 500 μm or less, 100 μm or less, 50 μm or less, or 30 μm or less. Alternatively, the negative electrode active material may be in a sheet form (foil form, film form) such as lithium foil. That is, the negative electrode active material layer 31 may be made of a sheet of the negative electrode active material.

[0039] Examples of the electrolyte that can be contained in the negative electrode active material layer 31 include the above-mentioned solid electrolyte and electrolytic solution. When the lithium ion battery 100 is a solid-state battery (same as above), the performance of the battery is likely to be improved when the negative electrode active material layer 31 contains a solid electrolyte, particularly a sulfide solid electrolyte, and further, a sulfide solid electrolyte containing Li2S-P2S5. Examples of the conductive assistant that can be contained in the negative electrode active material layer 31 include the above-mentioned carbon material and the above-mentioned metal material. The binder that can be contained in the negative electrode active material layer 31 may be appropriately selected from, for example, those exemplified as the binder that can be contained in the above-mentioned positive electrode active material layer 11.

[0040] 2.2.2 Negative electrode current collector As shown in FIG. 1, the negative electrode 30 may include a negative electrode current collector 32 in contact with the negative electrode active material layer 31. The negative electrode current collector 32 may be any of those commonly used as a negative electrode current collector for a battery. The negative electrode current collector 32 may be in the form of a foil, a plate, a mesh, a punched metal, a foam, or the like. The negative electrode current collector 32 may be a metal foil or a metal mesh, or may be a carbon sheet. In particular, a metal foil is excellent in terms of ease of handling. The negative electrode current collector 32 may be made of a plurality of foils or sheets. Examples of metals constituting the negative electrode current collector 32 include Cu, Ni, Cr, Au, Pt, Ag, Al, Fe, Ti, Zn, Co, stainless steel, and the like. In particular, from the viewpoint of ensuring reduction resistance and being difficult to alloy with lithium, the negative electrode current collector 32 may contain at least one metal selected from Cu, Ni, and stainless steel. The negative electrode current collector 32 may have some kind of coating layer on its surface for the purpose of adjusting the resistance or the like. The negative electrode current collector 32 may be a metal foil or a base material on which the above metal is plated or vapor-deposited. When the negative electrode current collector 32 is made of a plurality of metal foils, some kind of layer may be present between the plurality of metal foils. The thickness of the negative electrode current collector 32 is not particularly limited. For example, it may be 0.1 μm or more or 1 μm or more, and may be 1 mm or less or 100 μm or less.

[0041] 2.3 Other The lithium ion battery 100 may have each of the above components housed inside an exterior body. Any known exterior body for a battery can be used as the exterior body. In addition, a plurality of batteries 100 may be electrically connected and stacked in any manner to form an assembled battery. In this case, the assembled battery may be housed inside a known battery case. The lithium ion battery 100 may also have other obvious components such as necessary terminals. The shape of the lithium ion battery 100 may be, for example, a coin type, a laminate type, a cylindrical type, a square type, or the like.

[0042] The lithium ion battery 100 can be manufactured by applying a known method. For example, it can be manufactured as follows. However, the manufacturing method of the lithium ion battery 100 is not limited to the following method, and each layer may be formed by, for example, dry molding. (1) The negative electrode active material constituting the negative electrode active material layer is dispersed in a solvent to obtain a negative electrode layer slurry. The solvent used in this case is not particularly limited, and water or various organic solvents can be used, and N-methylpyrrolidone (NMP) can also be used. The negative electrode layer slurry is then applied to the surface of a negative electrode current collector using a doctor blade or the like, and then dried to form a negative electrode active material layer on the surface of the negative electrode current collector, forming a negative electrode. (2) The positive electrode active material constituting the positive electrode active material layer is dispersed in a solvent to obtain a positive electrode layer slurry. The solvent used in this case is not particularly limited, and water or various organic solvents can be used, and N-methylpyrrolidone (NMP) can also be used. The positive electrode layer slurry is applied to the surface of a positive electrode current collector using a doctor blade or the like, and then dried to form a positive electrode active material layer on the surface of the positive electrode current collector, which serves as a positive electrode. (3) The layers are laminated so that the electrolyte layer (solid electrolyte layer or separator) is sandwiched between the negative electrode and the positive electrode to obtain a laminate having the negative electrode current collector, the negative electrode active material layer, the electrolyte layer, the positive electrode active material layer, and the positive electrode current collector in this order. Other members such as terminals are attached to the laminate as necessary. (4) The laminate is housed in a battery case, and in the case of an electrolyte battery, the battery case is filled with electrolyte, and the laminate is immersed in the electrolyte and sealed in the battery case to form a secondary battery. In the case of an electrolyte battery, the electrolyte may be impregnated in the negative electrode active material layer, the separator, and the positive electrode active material layer at the above step (3).

[0043] 3. Battery system The technology of the present disclosure also has an aspect of being a system for controlling the charging and discharging of a lithium ion battery. That is, the battery system of the present disclosure includes the above-mentioned lithium ion battery 100 and a control unit (not shown) for controlling the charging and discharging of the lithium ion battery 100, and the control unit controls the positive electrode potential at the discharge end potential to be 3V (vs. Li / Li + As described above, according to the technology of the present disclosure, the discharge of the lithium ion battery 100 may be controlled so that the potential of the lithium ion battery 100 is 3 V (vs. Li / Li), which is the potential in the redox region of Mn. + ) or less, the resistance of the second active material is small, and an increase in the resistance of the positive electrode as a whole is suppressed. In other words, even if the positive electrode potential at the end-of-discharge potential is controlled to be a potential in the redox region of Mn, an increase in the resistance of the positive electrode is suppressed, and a high discharge capacity is easily obtained.

[0044] The control unit may be any unit capable of controlling the charging and discharging of the lithium ion battery 100 as described above. When the control unit controls the charging and discharging of the lithium ion battery 100, the end-of-charge potential of the lithium ion battery 100 is not particularly limited and may be determined according to the desired battery performance. EXAMPLES

[0045] The technology of the present disclosure will be described in more detail below with reference to examples, but the technology of the present disclosure is not limited to the following examples.

[0046] 1. Preparation of Positive Electrode Active Material The first and second active materials were prepared as the positive electrode active materials by the following procedure. Both the first and second active materials have an O2 type structure, the first active material contains Mn, and the second active material does not contain Mn. The third active material was LiNi 0.5 Mn 0.5 O2 was prepared.

[0047] 1.1 First active material (Li 0.7 Mn 0.5 Ni 0.2 Co 0.3 O2) Solution 1A was obtained by dissolving 43.06 g of Mn(NO3)2·6H2O, 17.97 g of Ni(NO3)2·6H2O, and 26.98 g of Co(NO3)2·6H2O in 250 g of pure water. Solution 2A was obtained by dissolving 31.8 g of Na2CO3 and 10.1 mL of ammonia water in 250 g of pure water. Solutions 1A and 2A were simultaneously dropped into a beaker containing 100 mL of pure water to obtain mixed solution 3A. The obtained mixed solution 3A was stirred overnight at 50 °C. After stirring, mixed solution 3A was washed with pure water and then dried at 120 °C for more than 48 hours to obtain intermediate substance 1A ((Mn 0.5 Ni 0.2 Co 0.3 )CO3) was obtained.

[0048] 13.5 g of intermediate material 1A and 4.28 g of Na2CO3 were mixed in a mortar and pressed with a hydrostatic press, then held at 600°C for 6 hours and then held at 900°C for 24 hours for firing to obtain intermediate material 2A (Na 0.7 Mn 0.5 Ni 0.2 Co 0.3 O2) was obtained.

[0049] 3.5 g of intermediate material 2A, 4.77 g of LiCl, and 7.75 g of LiNO3 were mixed and dissolved by holding at 280 °C for 1 hour. After that, the mixture was washed with pure water, filtered, and dried to obtain Li as the first active material. 0.7 Mn 0.5 Ni 0.2 Co 0.3 Got O2.

[0050] 1.2 Second active material Solution 1B was obtained by dissolving 89.93 g of Co(NO3)2·6H2O in 250 g of pure water. Solution 2B was obtained by dissolving 31.8 g of Na2CO3 and 10.1 mL of ammonia water in 250 g of pure water. Solutions 1B and 2B were simultaneously dropped into a beaker containing 100 mL of pure water to obtain mixed solution 3B. The resulting mixed solution 3B was stirred overnight at 50°C. After stirring, mixed solution 3B was washed with pure water and then dried at 120°C for more than 48 hours to obtain intermediate substance 1B (CoCO3).

[0051] 13.5 g of intermediate material 1B and 5.1 g of Na2CO3 were mixed in a mortar and pressed with a hydrostatic press, then held at 600°C for 6 hours and then held at 900°C for 24 hours for firing to obtain intermediate material 2B (Na 0.7 CoO2) was obtained.

[0052] 3.5 g of intermediate material 2B, 4.77 g of LiCl, and 7.75 g of LiNO3 were mixed and dissolved at 280 °C for 1 hour. After that, the mixture was washed with pure water, filtered, and dried to obtain Li as the second active material. 0.7 CoO2 was obtained.

[0053] 2. Preparation of Positive Electrode 85% by mass of the positive electrode active material (the mass ratio of the first active material to the second active material was examined from 100:0 to 0:100, or the mass ratio of the first active material to the third active material was examined from 100:0 to 0:100), 10% by mass of acetylene black (LI400) as a conductive assistant, and 5% by mass of polyvinylidene fluoride as a binder were mixed, and the mixture was made into a slurry using N-methyl-2-pyrrolidone, and then applied onto an Al foil as a positive electrode current collector. After this, the mixture was vacuum dried and molded at 120°C to obtain a positive electrode.

[0054] 2.1 Combination of the first and second active materials In Comparative Example 1, Examples 1 to 6, and Comparative Example 2, when the positive electrodes were produced, at least one of the first active material and the second active material was used as the positive electrode active material.

[0055] 2.1.1 Comparative Example 1 The mass ratio of the first active material to the second active material in the positive electrode active material was set to 100:0.

[0056] 2.1.2 Example 1 The mass ratio of the first active material to the second active material in the positive electrode active material was 90:10.

[0057] 2.1.3 Example 2 The mass ratio of the first active material to the second active material in the positive electrode active material was 80:20.

[0058] 2.1.4 Example 3 The mass ratio of the first active material to the second active material in the positive electrode active material was 70:30.

[0059] 2.1.5 Example 4 The mass ratio of the first active material to the second active material in the positive electrode active material was 50:50.

[0060] 2.1.6 Example 5 The mass ratio of the first active material to the second active material in the positive electrode active material was 30:70.

[0061] 2.1.7 Example 6 The mass ratio of the first active material to the second active material in the positive electrode active material was 10:90.

[0062] 2.1.8 Comparative Example 2 The mass ratio of the first active material to the second active material in the positive electrode active material was 0:100.

[0063] 2.2 Combination of the first and third active materials In Comparative Examples 1 and 3 to 9, at least one of the first active material and the third active material was used as the positive electrode active material when the positive electrode was produced. Comparative Example 1 is as described above.

[0064] 2.2.1 Comparative Example 3 The mass ratio of the first active material to the third active material in the positive electrode active material was 90:10.

[0065] 2.2.2 Comparative Example 4 The mass ratio of the first active material to the third active material in the positive electrode active material was 80:20.

[0066] 2.2.3 Comparative Example 5 The mass ratio of the first active material to the third active material in the positive electrode active material was 70:30.

[0067] 2.2.4 Comparative Example 6 The mass ratio of the first active material to the third active material in the positive electrode active material was 50:50.

[0068] 2.2.5 Comparative Example 7 The mass ratio of the first active material to the third active material in the positive electrode active material was 30:70.

[0069] 2.2.6 Comparative Example 8 The mass ratio of the first active material to the third active material in the positive electrode active material was 10:90.

[0070] 2.2.7 Comparative Example 9 The mass ratio of the first active material to the third active material in the positive electrode active material was 0:100.

[0071] 3. Negative Electrode Preparation For the negative electrode, metallic lithium cut to a specified size was used.

[0072] 4. Electrolyte Preparation The non-aqueous electrolyte used was a Daikin electrolyte (1.0M LiPF6 / TW5(TFPC)+F3(TFEMC) 30:70vol%+ TL16(LiDFOB 0.98wt%)).

[0073] 5. Coin Cell Fabrication In an inert atmosphere, the above electrolyte was poured into a coin-type cell using a positive electrode of any one of Examples 1 to 6 and Comparative Examples 1 to 9 and the above negative electrode, to prepare a coin cell for evaluation.

[0074] 6. Discharge capacity measurement Each coin cell was placed in a thermostatic chamber at 25°C and discharged to a final potential of 2.0 V (vs. Li / Li + ), charge end potential 4.8V (vs.Li / Li + ), CC charge and discharge were performed at a current density of 0.1 C, and the discharge capacity was measured. The results for Examples 1 to 6 and Comparative Examples 1 and 2 are shown in FIG. 2, and the results for Comparative Examples 1, 3 to 9 are shown in FIG. 3. As is clear from the results shown in FIGS. 2 and 3, in the positive electrode, when the first active material and the second active material are combined as the positive electrode active material, the discharge capacity is synergistically higher than when the first active material is used alone, when the second active material is used alone, and when the first active material is used in combination with the third active material.

[0075] 7. Measurement of DCIR resistance of positive electrode The DCIR resistance was measured at SOC 40% or 20% for each of the positive electrodes in the case where the first active material was used alone as the positive active material (positive electrode A), the case where the second active material was used alone as the positive active material (positive electrode B), and the case where the first active material and the second active material were combined as the positive active material (positive electrode C, first active material:second active material=70:30 (mass ratio)). The results are shown in FIG. 4. As shown in FIG. 4, the positive electrode A using only the first active material has a higher DCIR resistance than the positive electrodes B and C. At SOC 40%, the Mn redox region is reached, so the resistance of the first active material increases, and it is considered that the resistance of the positive electrode A as a whole increases. In contrast, the positive electrode B using only the second active material does not have a high DCIR resistance even at the same SOC. The DCIR resistance of the positive electrode C using the first active material and the second active material in combination is not as high as that of the positive electrode A.

[0076] 8. Summary The first active material containing at least Li, Mn, and O as constituent elements and having an O2 type structure has a high resistance in the redox region of Mn. Therefore, when the positive electrode is constructed using only the first active material as the positive electrode active material as in the above Comparative Example 1, the resistance of the positive electrode as a whole increases in the redox region of Mn, and as a result, the capacity of the positive electrode decreases. In contrast, when the first active material containing Mn and the second active material not containing Mn are used in combination as the positive electrode active material having an O2 type structure as in the above Examples 1 to 6, the resistance of the second active material is small even at a potential in the redox region of Mn, and the increase in the resistance of the positive electrode as a whole is suppressed, and as a result, the capacity of the positive electrode is improved. Note that the second active material has a problem different from the first active material, such as Na easily remaining in the crystal structure. In this respect, as in the above Comparative Example 2, the second active material alone does not provide a high positive electrode capacity. Furthermore, when the first active material and the third active material are combined as in Comparative Examples 3 to 9, the advantageous effects of the combination are not easily achieved, and the positive electrode capacity is actually lower than when the first active material is used alone.

[0077] In the above embodiment, the electrolyte battery is used as the lithium ion battery, but the above effect can be achieved regardless of the type of lithium ion battery (electrolytic solution battery, solid-state battery). In addition, the negative electrode is not limited to the form using metallic lithium as in the above embodiment. [Explanation of symbols]

[0078] 10 positive electrode 11 Cathode active material layer 12 Positive electrode current collector 20 Electrolyte layer 30 negative electrode 31 Negative electrode active material layer 32 Negative electrode current collector 100 Lithium-ion batteries

Claims

1. a positive electrode comprising a first active material and a second active material; The first active material contains at least Li, Mn, and O as constituent elements and has an O2 type structure, The second active material contains at least Li, a transition metal element, and O as constituent elements, does not contain Mn, and has an O2 type structure. Positive electrode.

2. The first active material contains at least Li, Mn, at least one of Ni and Co, and O as constituent elements; The positive electrode according to claim 1 .

3. The second active material contains at least Li, Co, and O as constituent elements. The positive electrode according to claim 1 or 2.

4. The first active material is contained in an amount of 10% by mass or more and 90% by mass or less, where the total amount of the first active material and the second active material is 100% by mass. The positive electrode according to any one of claims 1 to 3.

5. The first active material has a chemical composition represented by Li x Mn a Ni b Co c O 2±δ (wherein 0<x<1, 0<a<1, 0≦b<1, 0≦c<1, and a+b+c is 0.8 or more and 1.2 or less), The second active material has a chemical composition represented by Li x Ni d Co e O 2±δ (wherein 0<x<1, 0≦d<1, 0<e≦1.2, and d+e is 0.8 or more and 1.2 or less); The positive electrode according to any one of claims 1 to 4.

6. The positive electrode according to any one of claims 1 to 5 is provided. Lithium-ion battery.

Citation Information

Patent Citations

  • Nonaqueous electrolyte secondary battery

    JP2006222072A

  • Composite metal oxide, positive electrode active material for lithium secondary battery, positive electrode for lithium secondary battery, and lithium secondary battery

    JP2012204281A

  • Composite positive electrode active material with improved output characteristics, and secondary battery, battery module, and battery pack containing the same.

    JP2014517480A

  • Positive electrode active material for nonaqueous electrolyte secondary battery and nonaqueous electrolyte secondary battery

    JP2015176644A

  • Nonaqueous electrolyte secondary battery

    JP2016033887A