Pressure wave generating element and its manufacturing method
The pressure wave generating element with an oriented fiber layer and metal coating addresses the inefficiencies of existing thermophones by enhancing sound pressure and reducing electrical resistance, enabling efficient energy conversion and improved sound output.
Patent Information
- Application Number
- JP2023500712
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-02-19
- Filing Date
- 2022-02-03
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-02-03
AI Technical Summary
Existing pressure wave generating elements, such as thermophones, face challenges in improving energy conversion efficiency and sound pressure due to high cost, handling difficulties, and the need for higher voltages to drive carbon nanotubes, which also have high resistivity.
A pressure wave generating element with a fiber layer composed of oriented fibers partially coated with metal, where the fibers are oriented along a predetermined direction and supported by a substrate, and electrodes are applied along this orientation to minimize electrical resistance and increase surface area for air contact.
The solution enhances sound pressure per unit input power by increasing air contact surface area and allowing for optimized electrical resistance, enabling higher input power without excessive heat conduction, thus improving energy conversion efficiency.
Smart Images

Figure 0007593470000007 
Figure 0007593470000008 
Figure 0007593470000009
Abstract
Description
[Technical field]
[0001] The present invention relates to a pressure wave generating element that generates pressure waves by periodically heating air, and also to a method for manufacturing the pressure wave generating element. [Background technology]
[0002] The pressure wave generating element is also called a thermophone, and as an example, a resistor layer is provided on a support. When a current flows through this resistor, the resistor heats up, and the air in contact with the resistor expands thermally. When the current is then stopped, the expanded air contracts. This periodic heating generates sound waves. When the drive signal is set to an audio frequency, it can be used as an audio speaker. When the drive signal is set to an ultrasonic frequency, it can be used as an ultrasonic source. Since such a thermophone does not use a resonance mechanism, it is possible to generate wideband and short-pulse sound waves. Since a thermophone converts electrical energy into thermal energy before generating sound waves, there is a demand for improvements in energy conversion efficiency and sound pressure.
[0003] In Patent Document 1, a carbon nanotube structure in which multiple carbon nanotubes are arranged in parallel with each other is provided as a resistor, thereby increasing the surface area in contact with air and reducing the heat capacity per unit area. In Patent Document 2, a silicon substrate is used as a heat dissipation layer, and porous silicon with low thermal conductivity is used as a heat insulating layer to improve the heat insulating properties. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2009-296591 A [Patent Document 2] Japanese Patent Application Publication No. 11-300274 Summary of the Invention [Problem to be solved by the invention]
[0005] In Patent Document 1, the reduction of heat capacity is considered by using carbon nanotubes in the heat generating layer. Although carbon nanotubes have been put to practical use, they are expensive and difficult to handle during production, so there is a high possibility that problems will arise when they are put to practical use. In addition, the resistivity (10 -5 ~10 -2 Ωcm) is the resistance of metal materials (10 -6 Since the resistivity is higher than that of the resistivity of the dielectric constant (Ωcm), it is necessary to operate the element at a higher voltage in order to input the same amount of power.
[0006] It is an object of the present invention to provide a pressure wave generating element having improved sound pressure and suitable electrical resistance, and also to provide a method for manufacturing such a pressure wave generating element. [Means for solving the problem]
[0007] A pressure wave generating element according to one aspect of the present invention includes: A support; a fiber layer provided on the support and configured to generate heat when an electric current is applied thereto; the fiber layer includes fibers having a surface at least partially provided with a metal coating; the fibers are oriented along a predetermined direction; The sensor further includes a pair of electrodes for applying a voltage along the orientation direction of the fibers.
[0008] A method for manufacturing a pressure wave generating element according to another aspect of the present invention includes the steps of: Providing a support; forming a fiber membrane on a rotating drum using fibers spun by an electrospinning method; mounting the fibrous membrane on the support and applying a metal coating onto the fibrous membrane to form a fibrous layer. Effect of the Invention
[0009] According to the pressure wave generating element of the present invention, the fiber layer contains fibers at least partially coated with a metal coating on the surface, which increases the surface area in contact with the air, thereby improving the sound pressure. Furthermore, the use of a metal material allows the electrical resistance of the fiber layer to be set to an appropriate value. Furthermore, the orientation of the fibers allows the electrical resistance of the fiber layer to be reduced. Therefore, the input power to the element can be set high, improving the sound pressure.
[0010] Furthermore, the method for manufacturing a pressure wave generating element according to the present invention can realize a fiber layer with a large surface area in contact with air and appropriate electrical resistance. Furthermore, the rotation of the drum can increase the degree of fiber orientation by spinning. [Brief description of the drawings]
[0011] [Figure 1] 1 is a cross-sectional view showing an example of a pressure wave generating element according to a first embodiment of the present invention. [Diagram 2] 1 is an electron microscope photograph showing the surface of a fiber layer 20, in which the fibers are randomly oriented. [Diagram 3] 1 is an electron microscope photograph showing the surface of a fiber layer 20, in which the fibers are oriented along a predetermined direction. [Figure 4] FIG. 2 is a cross-sectional view showing the thickness distribution of a metal coating. [Diagram 5] Fig. 5A is a plan view showing an example of a pressure wave generating element, Fig. 5B is a schematic view showing the orientation state of the fibers fb in the fiber layer 20. [Figure 6] 1 is a graph showing the relationship between the diameter of fibers used in a fiber layer and the estimated specific surface area. [Figure 7] 10 is a flowchart showing an example of a method for manufacturing a pressure wave generating element. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] A pressure wave generating element according to one aspect of the present invention includes: A support; a fiber layer provided on the support and configured to generate heat when an electric current is applied thereto; the fiber layer includes fibers having a surface at least partially provided with a metal coating; the metal coating has an increasing thickness away from the substrate; the fibers are oriented along a predetermined direction; The optical fiber further includes a pair of electrodes for applying a voltage along the orientation direction of the fibers, where "oriented" means that the extension direction of the fibers is not completely random.
[0013] According to this configuration, the fiber layer includes fibers having a metal coating at least partially provided on the surface thereof. This increases the surface area in contact with the air, improving the sound pressure per unit input power. The fibers can be arranged in the form of a nonwoven fabric, a woven fabric, a knitted fabric, or a mixture thereof, and the cavities around the fibers are connected to each other to ensure air permeability between the internal cavities and the external space. Thus, the contact area between the porous structure formed by the fibers and the air is significantly increased compared to a non-porous smooth surface. This increases the efficiency of heat transfer from the fiber layer to the air, improving the sound pressure. In addition, the metal coating is thicker as it gets farther from the support, so that it can suppress heat generation on the support side inside the fiber layer while increasing heat generation on the opposite side to the support, thereby suppressing heat conduction from the fiber layer to the support and improving the efficiency of heating the air, thereby improving the sound pressure per unit input power.
[0014] Furthermore, by applying a metal coating to at least a portion of the fiber, the electrical resistance of the fiber layer can be easily set to an appropriate value by adjusting the coating thickness and selecting the coating material, thus obtaining the desired electrical resistance and optimizing the drive voltage.
[0015] In addition, when a low thermal conductive material is used as the fiber, for example, the thermal conduction from the fiber layer to the support can be suppressed. This increases the temperature change on the surface of the fiber layer, improving the sound pressure per unit input power. Since the fiber layer containing such fibers has a porous structure, it is not necessary to introduce a heat insulating layer to improve the sound pressure as in Patent Document 2.
[0016] In addition, the orientation of the fibers can reduce the electrical resistance of the fiber layer, allowing the input power to be set higher, improving sound pressure.
[0017] Furthermore, by providing a pair of electrodes for applying a voltage in the direction of fiber orientation, electricity can be passed through the fiber layer in a state where the electrical resistance is minimized, allowing the input power to the element to be set high, improving sound pressure.
[0018] In the present invention, the degree of orientation of the fibers is preferably −0.6 or more.
[0019] According to this configuration, the degree of fiber orientation is -0.6 or more, so that the electrical resistance of the fiber layer can be reduced, and therefore the input power to the element can be set high, thereby improving the sound pressure.
[0020] In the present invention, the diameter of the fibers is preferably within the range of 20 nm to 1000 nm.
[0021] According to this configuration, the fiber diameter is reduced, which makes it possible to increase the specific surface area of the fiber layer and increase the sound pressure per unit input power. On the other hand, if the fiber diameter is less than 20 nm, the strength of the fiber itself decreases, which affects the durability and lifespan of the element.
[0022] In the present invention, the fibers are preferably polymer fibers. Specific examples of materials for forming the polymer fibers include polyimide, polyamide, polyamideimide, polyethylene, polypropylene, acrylic resin, polyvinyl chloride, polystyrene, polyvinyl acetate, polytetrafluoroethylene, liquid crystal polymer, polyphenylene sulfide, polyether ether ketone, polyarylate, polysulfone, polyether sulfone, polyetherimide, polycarbonate, modified polyphenylene ether, polybutylene terephthalate, polyethylene terephthalate, polyacetal, polylactic acid, polyvinyl alcohol, ABS resin, polyvinylidene fluoride, cellulose, polyethylene oxide, polyethylene glycol, and polyurethane.
[0023] This configuration enables spinning using the electrospinning method, which makes it possible to realize fibers with diameters in the range of 1 nm to 2000 nm, such as nanofibers, submicron fibers, and micron fibers.
[0024] In the present invention, the polymer fibers are preferably polyimide fibers.
[0025] This configuration can increase the heat resistance of the fiber layer, making it possible to apply a heat treatment process in a later step, such as reflow soldering.
[0028] A method for manufacturing a pressure wave generating element according to another aspect of the present invention includes the steps of: Providing a support; forming a fiber membrane on a rotating drum using fibers spun by an electrospinning method; The fiber membrane is bonded to the support, and the fiber membrane is placed on the support. The thickness increases with distance from the support. and applying a metal coating to form a fibrous layer.
[0029] According to this configuration, the fiber layer includes fibers having a metal coating at least partially formed on the surface thereof, and functions as a heater. This increases the surface area in contact with the air, improving the sound pressure per unit input power. In addition, a fiber layer having an appropriate electrical resistance can be easily realized. In addition, the metal coating is thicker as it gets farther from the support, so that it can suppress heat generation on the support side inside the fiber layer while increasing heat generation on the opposite side to the support, thereby suppressing heat conduction from the fiber layer to the support and improving the efficiency of heating the air, thereby improving the sound pressure per unit input power.
[0030] Furthermore, by using the electrospinning method, it is possible to realize fibers having diameters in the range of 1 nm to 2000 nm, such as nanofibers, submicron fibers, and micron fibers.
[0031] In addition, the degree of fiber orientation can be increased by utilizing the rotation of the drum during spinning.
[0032] In the present invention, the peripheral speed of the rotating drum is set in the range of 10472 mm / s to 31416 mm / s.
[0033] This configuration allows for spinning of fibers having an appropriate degree of orientation.
[0034] (Embodiment 1) FIG. 1 is a cross-sectional view showing an example of a pressure wave generating element 1 according to a first embodiment of the present invention.
[0035] The pressure wave generating element 1 includes a support 10, a fiber layer 20, and a pair of electrodes D1, D2. The support 10 is formed of an electrical insulator such as a semiconductor such as silicon, glass, a ceramic substrate such as alumina, zirconia, magnesium oxide, aluminum nitride, boron nitride, silicon nitride, or a flexible substrate such as a PET film or a polyimide film. A thermal insulation layer having a lower thermal conductivity than the support 10 may be provided on the support 10, thereby suppressing the dissipation of heat from the fiber layer 20 to the support 10. As described later, when the fiber layer 20 has a thermal insulation function, the above-mentioned thermal insulation layer may be omitted.
[0036] A fiber layer 20 is provided on the support 10. The fiber layer 20 is made of a conductive material and is electrically driven to generate heat when an electric current flows through it, and to emit pressure waves caused by the periodic expansion and contraction of air. A pair of electrodes D1, D2 are provided on both sides of the fiber layer 20. The electrodes D1, D2 have a single-layer structure or a multi-layer structure made of a conductive material.
[0037] In this embodiment, the fiber layer 20 includes fibers having a metal coating at least partially formed on the surface thereof. This increases the surface area in contact with the air, improving the sound pressure. Furthermore, by applying a metal coating to the fibers, the electrical resistance of the fiber layer 20 can be set to an appropriate value depending on the adjustment of the coating thickness and the selection of the coating material.
[0038] The fibers may be placed directly on the support 10 or may be placed via an adhesive layer, such as a polymeric material.
[0039] 2 and 3 are electron microscope photographs showing the surface of the fiber layer 20. Fig. 2 shows a case where the fibers are randomly oriented and bonded or entangled by thermal, mechanical or chemical action to form a sheet. Fig. 3 shows a case where the fibers are oriented along a predetermined direction and bonded or entangled by thermal, mechanical or chemical action to form a sheet. A metal coating is applied to the surface of the fibers.
[0040] The fibers can be selected from the group consisting of polymer fibers, glass fibers, carbon fibers, carbon nanotubes, metal fibers, and ceramic fibers. When low thermal conductive materials such as polymers, glass, and ceramics are used as the fibers, the fibers themselves have a thermal insulation function, so that the thermal conduction from the fiber layer to the support can be suppressed. This increases the temperature change on the surface of the fiber layer, and improves the sound pressure per unit input power.
[0041] The metal coating is preferably formed of a metal material such as Au, Ag, Cu, Pt, Rh, Pd, Ru, Ni, Ir, Cr, Mo, W, Ti, Al, etc., or an alloy containing two or more of these metals. The metal coating may have a single layer structure or a multi-layer structure made of multiple materials.
[0042] (Embodiment 2) 7 is a flow chart showing an example of a method for manufacturing a pressure wave generating element. First, in step S1, a support 10 is prepared.
[0043] Next, in step S2, a fiber membrane is formed on the circumferential surface of the rotating drum collector using the spun fibers. As the spinning method, a melt blowing method, a flash spinning method, a centrifugal spinning method, a melt spinning method, etc. can be used. In addition, a method in which pulp is crushed and processed into a sheet, such as cellulose nanofiber, can be used. In particular, when the electrospinning method is used, nanofibers, submicron fibers, micron fibers, etc. can be realized.
[0044] By spinning with the rotation of the drum, the spun fibers are oriented in a predetermined direction (see FIG. 3). For example, when a drum collector with a diameter of 200 mm is rotated at about 50 rpm to about 3000 rpm, the drum peripheral speed is about 524 mm / s to about 31400 mm / s.
[0045] Next, in step S3, the obtained fiber membrane is peeled off and bonded onto the support 10, and then a metal coating is applied onto the fiber membrane to form a fiber layer 20. The coating method may be vapor deposition, sputtering, electrolytic plating, electroless plating, ion plating, atomic layer deposition, or the like. The metal material may be any of those generally mentioned above.
[0046] Next, in step S4, a pair of electrodes D1, D2 are formed on the obtained fiber layer 20. The electrode film formation method may be vapor deposition, sputtering, electrolytic plating, electroless plating, ion plating, atomic layer deposition, printing, spray coating, dip coating, or the like. The electrode material is preferably a metal material such as Au, Ag, Cu, Pt, Rh, Pd, Ru, Ni, Ir, Cr, Mo, W, Ti, Al, Sn, or an alloy containing two or more of these metals. The electrode structure may be a single layer structure or a multi-layer structure made of multiple materials. EXAMPLES
[0047] Example 1 (Sample preparation method) The pressure wave generating elements were produced by the following method (Comparative Sample 1, Samples 1 to 4).
[0048] A polyimide (PI) solution prepared using N,N-dimethylformamide (DMF) as a solvent was used as the spinning solution. The solution concentration was adjusted to 8 wt%, and 0.1 wt% lithium chloride was added to the solution. Other additives that can be used include tetrabutylammonium chloride and potassium trifluoromethanesulfonate.
[0049] Using this solution, PI fibers were spun onto the aluminum foil attached to the circumferential surface of the drum collector by the electrospinning method. The drum collector used had a diameter of 200 mm and was spun while rotating at 50 rpm to 3000 rpm. By increasing the rotation speed, for example, oriented fibers as shown in Fig. 3 could be produced.
[0050] The conditions for electrospinning were an applied voltage of 23 kV and a nozzle-to-collector distance of 14 cm, and the film formation time was adjusted so that the thickness of the fiber film was about 1 to 80 μm. The produced fiber film was peeled off from the aluminum foil and adhered onto a Si substrate (support). Adhesion to the substrate can be carried out by previously applying an adhesive such as epoxy to the substrate or using a double-sided tape or the like. Also, as the substrate, a glass, a ceramic substrate such as alumina, zirconia, magnesium oxide, aluminum nitride, boron nitride, silicon nitride, or a flexible substrate such as a PET film or a polyimide film can be used.
[0051] Au with a thickness distributed in the range of 1 to 40 nm was formed on the fiber film formed on the substrate by sputtering. As the method for metal coating on the fibers, techniques such as vapor deposition, ion plating, atomic layer deposition, electroless plating, etc. may be used. Also, as the metal species, Au, Ag, Cu, Pt, Rh, Pd, Ru, Ni, Ir, Cr, Mo, W, Ti, Al, etc. can be used.
[0052] The thickness of the metal coating may be uniform or non-uniform in the circumferential direction of the fiber. For example, the thickness may increase as the distance from the support increases. The metal coating has a thickness T1 at the position closest to the support side and a thickness T2 at the position farthest from the support side, and it may satisfy T1 < T2. The form of the metal coating on the fiber may be such that, for example, as shown in Fig. 4, there may be a portion where the metal coating 22 is not applied at the lower part close to the support 10 on the circumferential surface of the fiber 21. Thereby, while suppressing heat generation on the support side inside the fiber layer, heat generation on the side opposite to the support can be enhanced.
[0053] The coating state (cross-sectional image) of metal-coated fibers can be analyzed as follows: For example, the coating state on the fiber can be analyzed by processing the sample with a focused ion beam (FIB), observing it with a transmission electron microscope (JEOL JEM-F200), and performing element mapping analysis by energy dispersive X-ray spectroscopy.
[0054] The fabricated element was processed to have a size of 5 mm x 6 mm. A pair of electrodes D1 and D2 were formed on both sides of the sample with dimensions of 0.8 mm x 4 mm and an electrode distance of 3.4 mm. The electrode layer structure was Ti (10 nm thick), Cu (500 nm thick), and Au (100 nm thick) from the support side.
[0055] Methods for forming electrodes include vapor deposition, sputtering, ion plating, atomic layer deposition, electrolytic plating, electroless plating, coating, spray coating, dip coating, etc. Materials for electrodes include Au, Ag, Cu, Pt, Rh, Pd, Ru, Ni, Ir, Cr, Mo, W, Ti, Al, etc.
[0056] Fig. 5A is a plan view showing an example of a pressure wave generating element. Fig. 5B is a schematic diagram showing the orientation state of the fibers fb in the fiber layer 20. The x direction corresponds to the rotation direction of the drum collector, and the fibers fb are oriented along the x direction. The electrodes D1 and D2 have an elongated shape along the y direction and are installed near both ends of the fibers fb. When a voltage is applied between the electrodes D1 and D2 along the x direction, a current I flows along the x direction.
[0057] In this way, when the current flows along the orientation direction of the fibers fb (x direction in the figure), the electrical resistance of the fiber layer is small. On the other hand, when the current flows along a direction perpendicular to the orientation direction of the fibers fb (y direction in the figure), the electrical resistance of the fiber layer is large. Therefore, in order to increase the power input to the element and improve the sound pressure, it is preferable that the direction of the current I and the orientation direction of the fibers fb coincide.
[0058] (Evaluation method) 1) Electrical characteristics (sound pressure, resistance) The sound pressure of the pressure wave generating element was measured using a MEMS microphone (Knowles SPU0410LR5H). The distance between the pressure wave generating element and the microphone was 6 cm, and the evaluation was performed by reading the microphone output voltage when the driving signal frequency was 60 kHz. The input voltage to the pressure wave generating element was 18 V. The resistance of the element was measured by the four-terminal method using a digital multimeter (Agilent 34410A).
[0059] 2) Fiber diameter The diameter of the metal-coated fibers was observed with a scanning electron microscope (Hitachi S-4800, accelerating voltage 5 kV, magnification 3k to 120k) to obtain SEM images, and the average fiber diameter was calculated by measuring the fiber diameter from the obtained images. Specifically, 10 fibers per field of view were randomly extracted from the multiple fibers contained in the obtained images, excluding abnormal ones, and this was repeated for 5 fields of view to sample a total of 50 fibers, whose diameters were measured, and the average fiber diameter was calculated.
[0060] 3) Degree of orientation The degree of fiber orientation was calculated as follows. The degree of fiber orientation was measured by observing with a scanning electron microscope (Hitachi S-4800, accelerating voltage 5 kV, magnification 1 k to 20 k times) to obtain an SEM image, measuring the direction (angle) of the fiber in the SEM image by needle analysis using the analysis software "A-zo-kun (Asahi Kasei Engineering Co., Ltd.)", and evaluating the kurtosis to calculate the degree of orientation. Specifically, in FIG. 5B, an image is obtained so that the y direction is 0° (180°) and the x direction is 90°. 30 to 100 fibers were randomly selected from the image, the angle of each fiber was measured, and the kurtosis was calculated. For example, the KURT function of the spreadsheet software EXCEL can be used to calculate the kurtosis.
[0061] Kurtosis is defined by the following formula (1), and is a statistic that indicates how much a distribution deviates from a normal distribution, showing the sharpness of the peak and the spread of the tail. In a normal distribution, kurtosis is 0, and when it is less than 0, the peak is gentle and the tail is short, and when it is greater than 0, the peak is steep and the tail is long. In the formula, n is the sample size, x iis each data value, the x bar is the mean, and s is the standard deviation.
[0062]
number
[0063] [Table 1]
[0064] (How to make Comparative Sample 2) As a comparative sample 2, an element using CNTs (carbon nanotubes) was produced.
[0065] A film with a thickness of about 500 nm to 1000 nm was formed on a Si substrate by spin coating using multi-walled CNT ink (MW-I) manufactured by Meijo Nano Carbon Co., Ltd. The spin coating was performed at a rotation speed of 5000 rpm for 15 seconds and dried at 120°C.
[0066] In order to decompose the dispersant contained in the solution, the element was subjected to heat treatment at 400℃ for 2 hours to obtain a CNT thin film. Electrodes were formed on both sides of the sample, measuring 0.8mm x 4mm and with an electrode separation distance of 3.4mm. The layered structure of the electrodes was Ti (10nm thick), Cu (500nm thick), and Au (100nm thick) from the substrate side.
[0067] When the characteristics of the pressure wave generating element using the CNTs produced by the above process were evaluated (using the same evaluation method as above), the resistance was 140 Ω and the sound pressure was 0.01 Pa.
[0068] [Table 2]
[0069] The results in Tables 1 and 2 show that compared to the case where a CNT film was formed by spin coating, the element obtained by applying Au coating to polyimide fibers oriented in a specific direction has lower electrical resistance and improved sound pressure. It is also clear that the greater the degree of fiber orientation, the lower the electrical resistance becomes and the further the sound pressure improves.
[0070] By forming the fibers coated with a metal material in this way, it is possible to realize a pressure wave generating element that has low element resistance and high sound pressure. By further reducing the element resistance, it is possible to realize a pressure wave generating element that can be driven at a low voltage.
[0071] Furthermore, by orienting the fibers, the packing and density of the fibers are increased, making it possible to realize a pressure wave generating element with low element resistance and high sound pressure.
[0072] In addition, since the metal film is formed using fibers with a diameter of 1 μm or less as a mold, it is possible to increase the specific surface area of the fiber layer, thereby increasing the sound pressure.
[0073] Furthermore, if a low thermal conductive material such as a polymer is used for the fibers, there is an insulating effect toward the substrate, and the temperature change on the surface of the heating element increases, which can lead to a higher sound pressure. As an example, the thermal conductivity of polyimide is approximately 0.28 W / m·K, while that of SiO2 (the oxide layer on the surface of a silicon substrate) is approximately 1.3 W / m·K. Polyimide has a lower thermal conductivity and a higher insulating effect toward the substrate, which results in a higher sound pressure.
[0074] Furthermore, when the fibers are made of polyimide having heat resistance (300° C. or higher), a post-processing heat treatment such as reflow soldering can be applied.
[0075] Example 2 (Sample preparation method) The pressure wave generating elements were produced by the following method (Comparative Sample 3, Samples 5 to 7).
[0076] A polyimide (PI) solution prepared using N,N-dimethylformamide (DMF) as a solvent was used as the spinning solution. The solution concentration was adjusted to 6 wt%, and 0.1 wt% lithium chloride was added to the solution. Other additives that can be used include tetrabutylammonium chloride and potassium trifluoromethanesulfonate.
[0077] Using this solution, PI fibers were spun onto an aluminum foil attached to the periphery of a drum collector by electrospinning. The drum collector used had a diameter of 200 mm, and spinning was performed while rotating at 50 rpm to 3000 rpm. By increasing the rotation speed, it was possible to produce oriented fibers, such as those shown in Figure 3.
[0078] The electrospinning conditions were an applied voltage of 29 kV, a nozzle-to-collector distance of 14 cm, and the deposition time was adjusted so that the fiber membrane had a thickness of about 1 to 80 μm. The fabricated fiber membrane was peeled off from the aluminum foil and attached to a Si substrate (support). The attachment to the substrate can be performed by applying an adhesive such as epoxy to the substrate in advance, or by using double-sided tape. The substrate can be made of glass, ceramic substrates such as alumina, zirconia, magnesium oxide, aluminum nitride, boron nitride, silicon nitride, or flexible substrates such as PET film or polyimide film.
[0079] A gold film with a thickness ranging from 1 to 40 nm was formed on the fiber membrane formed on the substrate by sputtering. Methods for metal coating on the fiber may include vapor deposition, ion plating, atomic layer deposition, and electroless plating. Metal species that can be used include Au, Ag, Cu, Pt, Rh, Pd, Ru, Ni, Ir, Cr, Mo, W, Ti, and Al.
[0080] The form of the metal coating (FIG. 4), element size, electrode formation method, electrode structure and fiber orientation (FIGS. 5A and 5B), and evaluation method are the same as those described in (Example 1).
[0081] In Example 2, the solution concentration was reduced from 8 wt% to 6 wt%, and the electrospinning applied voltage was increased from 23 kV to 29 kV, compared to Example 1. As a result, the fibers spun were thinner, the fiber diameter after metal coating was also thinner, and the density of the fiber membrane was increased.
[0082] [Table 3]
[0083] The results in Table 3 show that even when the fibers are thin, the greater the degree of fiber orientation, the smaller the electrical resistance becomes, and the further the sound pressure is improved.
[0084] Example 3 (Sample preparation method) The pressure wave generating elements were produced by the following method (Comparative Sample 4, Sample 8).
[0085] A polyimide (PI) solution prepared using N,N-dimethylformamide (DMF) as a solvent was used as the spinning solution. The solution concentration was adjusted to 10 wt%.
[0086] Using this solution, PI fibers were spun onto an aluminum foil attached to the periphery of a drum collector by electrospinning. The drum collector used had a diameter of 200 mm, and spinning was performed while rotating at 50 rpm and 3000 rpm. By increasing the rotation speed, it was possible to produce oriented fibers, such as those shown in Figure 3.
[0087] The electrospinning conditions were an applied voltage of 29 kV, a nozzle-to-collector distance of 14 cm, and the deposition time was adjusted so that the fiber membrane had a thickness of about 1 to 80 μm. The fabricated fiber membrane was peeled off from the aluminum foil and attached to a Si substrate (support). The attachment to the substrate can be performed by applying an adhesive such as epoxy to the substrate in advance, or by using double-sided tape. The substrate can be made of glass, ceramic substrates such as alumina, zirconia, magnesium oxide, aluminum nitride, boron nitride, silicon nitride, or flexible substrates such as PET film or polyimide film.
[0088] A gold film with a thickness ranging from 1 to 40 nm was formed on the fiber membrane formed on the substrate by sputtering. Methods for metal coating on the fiber may include vapor deposition, ion plating, atomic layer deposition, and electroless plating. Metal species that can be used include Au, Ag, Cu, Pt, Rh, Pd, Ru, Ni, Ir, Cr, Mo, W, Ti, and Al.
[0089] The form of the metal coating (FIG. 4), element size, electrode formation method, electrode structure and fiber orientation (FIGS. 5A and 5B), and evaluation method are the same as those described in (Example 1).
[0090] In Example 3, the solution concentration was increased from 8 wt% to 10 wt%, and the electrospinning applied voltage was increased from 23 kV to 29 kV, compared to Example 1. As a result, the spun fibers were thicker, the fiber diameter after metal coating was also thicker, and the density of the fiber membrane was reduced.
[0091] [Table 4]
[0092] The results in Table 4 show that even when the fibers are thick, the greater the degree of fiber orientation, the smaller the electrical resistance becomes, and the further the sound pressure is improved.
[0093] Example 4 (Sample preparation method) Pressure wave generating elements were produced by the following method (Comparative Sample 5, Sample 9).
[0094] A polyamic acid solution prepared using N,N-dimethylacetamide (DMAc) as a solvent was used as the spinning solution. The solution concentration was adjusted to 25 wt%.
[0095] Using this solution, polyamic acid fibers were spun onto an aluminum foil attached to the periphery of a drum collector by electrospinning. The drum collector used had a diameter of 200 mm, and spinning was performed while rotating at 50 rpm and 3000 rpm. By increasing the rotation speed, it was possible to produce oriented fibers, such as those shown in Figure 3.
[0096] The electrospinning conditions were an applied voltage of 23 kV, a nozzle-to-collector distance of 14 cm, and the film formation time was adjusted so that the fiber membrane was about 1 to 80 μm thick. The obtained polyamic acid fiber was heat-treated (imidized) at 300°C for 1 hour to obtain polyimide fiber. In the case of polymer materials with low thermal decomposition temperatures or melting points, a fiber membrane cannot be obtained by applying a heat treatment process, but polyimide materials are heat-resistant, so a heat treatment process can be applied.
[0097] The fabricated fiber membrane was peeled off from the aluminum foil and attached to a Si substrate (support). Attachment to the substrate can be achieved by applying an adhesive such as epoxy to the substrate beforehand, or by using double-sided tape. The substrate can be made of glass, ceramic substrates such as alumina, zirconia, magnesium oxide, aluminum nitride, boron nitride, silicon nitride, or flexible substrates such as PET film or polyimide film.
[0098] A gold film with a thickness ranging from 1 to 100 nm was formed on the fiber membrane formed on the substrate by sputtering. Methods for metal coating on the fiber may include vapor deposition, ion plating, atomic layer deposition, and electroless plating. Metal species that can be used include Au, Ag, Cu, Pt, Rh, Pd, Ru, Ni, Ir, Cr, Mo, W, Ti, and Al.
[0099] The form of the metal coating (FIG. 4), element size, electrode formation method, electrode structure and fiber orientation (FIGS. 5A and 5B), and evaluation method are the same as those described in Example 1. In this example, the input voltage to the pressure wave generating element in the sound pressure measurement was 8 V.
[0100] [Table 5]
[0101] The results in Table 4 show that even when the fibers are thick, the greater the degree of fiber orientation, the smaller the electrical resistance becomes, and the further the sound pressure is improved.
[0102] Figure 6 is a graph showing the relationship between the diameter of the fibers used in the fiber layer and the estimated specific surface area. When the fiber diameter is 1 μm or less, the specific surface area of the fiber layer increases rapidly (super specific surface area effect). For example, when the specific surface area is 200 μm -1 In this case, the fiber diameter is 20 nm. The diameter of the fiber used in the fiber layer is preferably within the range of 20 nm to 1000 nm. By reducing the fiber diameter, it is possible to increase the specific surface area of the fiber layer, and the sound pressure per unit input power can be increased. On the other hand, if the fiber diameter is less than 20 nm, the strength of the fiber itself decreases, which affects the durability and lifespan of the element.
[0103] As described above, the fiber layer contains fibers having a metal coating at least partially on the surface thereof, which increases the surface area in contact with the air, thereby improving the sound pressure. Furthermore, the use of a metal material allows the electrical resistance of the fiber layer to be set to an appropriate value. Furthermore, the orientation of the fibers allows the electrical resistance of the fiber layer to be reduced. This allows the input power to the element to be set high, improving the sound pressure.
[0104] The present invention will now be fully described in connection with preferred embodiments with reference to the accompanying drawings. However, various variations and modifications will be apparent to those skilled in the art. and modifications therein without departing from the scope of the present invention as defined by the appended claims. It should be understood to be included. [Industrial Applicability]
[0105] INDUSTRIAL APPLICABILITY The present invention is extremely useful industrially in that it can realize a pressure wave generating element having improved sound pressure and appropriate electrical resistance. [Explanation of symbols]
[0106] 1 Pressure wave generating element 10 Support 20 Fiber layer 21 Textiles 22 Metal Coating D1,D2 electrode
Claims
1. A support; a fiber layer provided on the support and configured to generate heat when an electric current is applied thereto; the fiber layer includes fibers having a surface at least partially provided with a metal coating; the metal coating has an increasing thickness away from the substrate; the fibers are oriented along a predetermined direction; A pressure wave generating element further comprising a pair of electrodes for applying a voltage along the orientation direction of the fibers.
2. 2. The pressure wave generating element according to claim 1, wherein the degree of orientation of the fibers is -0.6 or more.
3. The pressure wave generating element according to claim 2 , wherein the diameter of the fibers is within a range of 20 nm to 1000 nm.
4. The pressure wave generating element according to any one of claims 1 to 3, wherein the fibers are polymeric fibers.
5. The pressure wave generating element according to claim 4 , wherein the polymer fiber is a polyimide fiber.
6. Providing a support; forming a fiber membrane on a rotating drum using fibers spun by an electrospinning method; and bonding the fiber membrane to the support and applying a metal coating on the fiber membrane, the thickness of which increases as it moves away from the support, to form a fiber layer.
7. The method for manufacturing a pressure wave generating element according to claim 6, wherein the peripheral speed of the rotating drum is set in the range of 10472 mm / s to 31416 mm / s.
Citation Information
Patent Citations
Pressure wave generation device
JP1999300274A
Electrically-conductive fiber
JP2005256215A
Thermoacoustic device
JP2009296591A