Rolled material
The use of a rolled material with specific alloys and a defined index value improves durability against bending stress, addressing the durability challenges of bendable or curveable members by increasing fatigue limit and reducing elastic modulus, enabling smaller bending radii without breakage.
Patent Information
- Application Number
- JP2024515960
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-05-02
- Filing Date
- 2023-04-14
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-04-14
AI Technical Summary
Existing bendable or curveable members, such as those described in Japanese Patent Application Publication No. 2016-59030, face challenges with durability due to increased bending stress as the bending radius decreases, leading to potential breakage from repeated bending.
A rolled material made of alloys or pure metals, such as beta titanium alloys, austenitic stainless steel, or beryllium copper, with a thickness of 0.03 mm or less, and an index value of 0.014 HV/GPa or higher, determined by the formula (0.0048 × Vickers hardness + 0.21) ÷ elastic modulus, is used to enhance durability against bending stress.
The solution significantly increases the fatigue limit and reduces elastic modulus, thereby enhancing the rolled material's durability against repeated bending, allowing for a smaller bending radius without breakage, and enabling its use in bendable or curveable devices.
Smart Images

Figure 0007593530000014 
Figure 0007593530000015 
Figure 0007593530000016
Abstract
Description
[Technical field]
[0001] The present invention relates to a rolled material, and more particularly to a rolled material used for a member that can be bent or curved. [Background technology]
[0002] 2. Description of the Related Art Bendable or curved members are known in the art (see Patent Document 1).
[0003] For example, Japanese Patent Application Laid-Open No. 2016-59030 describes a flexible display device including a flexible display and a support member that supports the flexible display. In Japanese Patent Application Laid-Open No. 2016-59030, the support member includes a metal plate-like main body and is configured to be elastically deformable together with the flexible display to bend or curve. The support member including the metal plate-like main body is repeatedly bent together with the flexible display. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2016-59030 A Summary of the Invention [Problem to be solved by the invention]
[0005] Although not disclosed in the above-mentioned JP 2016-59030 A, from the viewpoint of design and space saving, it is desirable to make the bending radius of a member that is configured to be elastically deformed together with a flexible display and bend or curve, such as the metal plate of the main body of the support member, smaller. However, as the bending radius is reduced, the bending stress applied to the member (metal plate) increases. Therefore, there is a demand for a member that is excellent in durability against the bending stress applied to the member (metal plate) due to repeated bending.
[0006] The present invention has been made to solve the above-mentioned problems, and one object of the present invention is to provide a rolled material that has excellent durability against bending stress applied to a metal plate (rolled material) due to repeated bending caused by elastic deformation. [Means for solving the problem]
[0007] As a result of intensive research to solve the above problems, the inventors of the present application have found that in order to improve durability against repeated bending due to elastic deformation, it is effective to increase the fatigue limit at which the material does not break even if stress due to repeated bending is applied many times, and to decrease the elastic modulus, which represents the magnitude of distortion due to stress. Thus, the present invention has been completed.
[0008] That is, a rolled material according to one aspect of the present invention is a rolled material used for a member that can be bent or curved, and is made of an alloy or a pure metal, and when a value obtained by the following formula (1) is used as an index value of durability against repeated bending, the index value is 0.014 HV / GPa or more. The thickness is 0.03 mm or less, and the maximum measured bending radius that can be bent or curved is 2.1 mm or less. .
number
[0009] In the rolled material according to one aspect of the present invention, when the index value is (0.0048×Vickers hardness+0.21)÷elastic modulus, which is the index value of durability against repeated bending, the index value is 0.014HV / GPa or more. Here, the inventors of the present application have found that 0.0048×Vickers hardness+0.21 can be regarded as the value of the fatigue limit. Therefore, when the index value is 0.014HV / GPa or more, the fatigue limit is sufficiently large, and durability against repeated bending can be increased. In addition, since the elastic modulus represents the magnitude of strain due to bending stress, the strain is reduced by reducing the elastic modulus, and the occurrence of breakage due to repeated bending can be suppressed. As a result, a rolled material having excellent durability against bending stress applied to the rolled material by repeated bending can be obtained. In addition, the thickness is 0.03 mm or less, and the maximum measured bending radius that can be bent or curved is 2.1 mm or less. This means that the thickness of the rolled material is sufficiently small, and the bending radius can be made sufficiently small, making it possible to use the rolled material in bent or curved portable devices.
[0010] In the rolled material according to the above aspect, the index value is preferably 0.019 HV / GPa or more. The inventors of the present application have found through experiments described below that such a configuration provides sufficiently high durability against repeated bending, allowing the bending radius to be further reduced.
[0011] In the rolled material according to the above aspect, the pure metal is preferably pure titanium. The inventors of the present application have found through experiments described below that the use of pure titanium in this way makes it possible to achieve an index value of 0.014 HV / GPa or more.
[0012] In the rolled material according to the above aspect, the alloy is preferably a beta-titanium alloy, an austenitic stainless steel, or a beryllium copper alloy. The inventors of the present application have found through experiments described below that the use of a beta-titanium alloy, an austenitic stainless steel, or a beryllium copper alloy makes it possible to achieve an index value of 0.014 HV / GPa or more.
[0013] In this case, preferably, The alloy is a beta titanium alloy, The beta titanium alloy is composed of 14.0% by mass to 16.0% by mass of V, 2.5% by mass to 3.5% by mass of Cr, 2.5% by mass to 3.5% by mass of Sn, and 2.5% by mass to 3.5% by mass of Al. The inventors of the present application have found through experiments described below that this composition makes it possible to make the index value of the rolled material 0.014HV / GPa or more, and to make the bending radius of a rolled material with a thickness of 0.03 mm 3 mm or less.
[0014] In the rolled material according to the above aspect, when a value obtained by the following formula (2) is used as a predicted value of the minimum bending radius at which the rolled material can be bent or curved, preferably, when the thickness of the rolled material is 0.03 mm, the predicted value of the minimum bending radius is 2.14 mm or less. Minimum bending radius = (thickness × elastic modulus) ÷ (0.0048 × Vickers hardness + 0.21) (2)
[0015] With this configuration, it is possible to reduce the bending radius by adjusting the elastic modulus or Vickers hardness so that the predicted value of the minimum bending radius is 2.14 mm or less. Furthermore, by predicting the minimum bending radius, it is possible to obtain the value of the minimum bending radius at which it is thought possible to bend or bend the rolled material without conducting an experiment, so that it is possible to easily design the desired rolled material.
[0016] In the rolled material according to the above aspect, the rolled material is preferably used for a bendable or curved support member that supports a display unit of a display device. With this configuration, it is possible to improve the durability of the support member against repeated bending, which is repeatedly bent or curved in accordance with repeated bending deformation of the display unit.
[0018] In the rolled material according to the above aspect, the index value is preferably 0.014 HV / GPa or more and 0.029 HV / GPa or less. The inventors of the present application have found through experiments described below that if the index value is within this range, the bending radius can be made sufficiently small. Effect of the Invention
[0019] According to the present invention, it is possible to provide a rolled material (metal plate) that is excellent in durability against bending stress applied to the rolled material (metal plate) due to repeated bending caused by elastic deformation. [Brief description of the drawings]
[0020] [Figure 1] FIG. 2 is a diagram showing a rolled material according to an embodiment of the present invention. [Diagram 2] FIG. 1 is a diagram showing an example of a bendable display device. [Diagram 3] FIG. 1 is a diagram showing an example of a bendable display device. [Figure 4] 1 is a graph showing the relationship between Vickers hardness and fatigue limit. [Diagram 5]FIG. 2 is a diagram for explaining a method for manufacturing a rolled material. [Figure 6] FIG. 2 is a diagram for explaining a roll direction and a width direction. [Figure 7] 13 is a graph showing the relationship between the index value and the bending radius. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] Hereinafter, an embodiment of the present invention will be described with reference to the drawings.
[0022] (Composition of rolled material) First, with reference to FIG. 1, a rolled material 100 according to an embodiment of the present invention will be described.
[0023] As shown in Fig. 1, the rolled material 100 is made of an alloy or a pure metal. The alloy is a titanium alloy, a stainless steel, or a copper alloy. The pure metal is pure titanium such as TR270C.
[0024] The titanium alloy is a beta titanium alloy having a body-centered cubic structure. The beta titanium alloy contains at least one of vanadium (V), molybdenum (Mo), and niobium (Nb) in addition to titanium (Ti). The beta titanium alloy is, for example, composed of 14.0% by mass to 16.0% by mass of V, 2.5% by mass to 3.5% by mass of Cr, 2.5% by mass to 3.5% by mass of Sn, and 2.5% by mass to 3.5% by mass of Al, and examples of the beta titanium alloy include Ti-15V-3Cr-3Sn-3Al, in terms of mass%.
[0025] Other beta-type titanium alloys include, for example, in mass%, Ti-15Mo-5Zr, Ti-15Mo-5Zr-3Al, Ti-11.5Mo-6Zr-4.5Sn, Ti-4Mo-8V-6Cr-3Al-4Zr, Ti-13V-11Cr-3Al, Ti-29Nb-13Ta-4.6Zr, Ti-36Nb-2Ta-3Zr-0.3O, and Ti-5Fe-3Nb-3Zr.
[0026] The stainless steel includes austenitic stainless steel. The austenitic stainless steel includes SUS301, SUS316L, and Fe-19Cr-11Mn-6Ni-0.35N-0.09C (YUS130S) by mass %. The copper alloy includes beryllium copper alloy.
[0027] The rolled material 100 is used for a member that can be bent or curved by elastic deformation. The thickness of the rolled material 100 is preferably 0.03 mm or less, and more preferably 0.02 mm or less.
[0028] In the rolled material 100 according to the present embodiment, stress is generated inside due to repeated bending caused by elastic deformation, and it is preferable that the fatigue limit is large so that the number of repetitions (number of bendings) until the stress leads to failure (fatigue failure) is large.
[0029] In this embodiment, the value obtained by the following formula (1) is set as an index value of durability against repeated bending. The index value is 0.014 HV / GPa or more. The index value is preferably 0.019 HV / GPa or more. The index value may be set in the range of 0.014 HV / GPa or more and 0.029 HV / GPa or less. Index value = (0.0048 × Vickers hardness + 0.21) ÷ Elastic modulus (1)
[0030] In this embodiment, the value obtained by the following formula (2) is set as the predicted value of the minimum bending radius at which the rolled material 100 can be bent or curved due to elastic deformation. In the present invention, the elastic modulus and Vickers hardness are adjusted so that the predicted value of the minimum bending radius is 2.14 mm or less when the thickness of the rolled material 100 is 0.03 mm. Minimum bending radius = (thickness × elastic modulus) ÷ (0.0048 × Vickers hardness + 0.21) (2)
[0031] In this embodiment, the minimum bending radius of the rolled material 100 is preferably 2.1 mm or less, and more preferably 1.5 mm or less. The bending direction may be the rolling direction or the width direction. As shown in Fig. 6, the direction in which the rolled material 100 is rolled by the rollers 11 is defined as the rolling direction (RD), and the direction perpendicular to the rolling direction is defined as the width direction (TD).
[0032] In this embodiment, it is preferable that the thickness of the rolled material 100 is 0.03 mm or less, and the maximum measured bending radius that can be bent or curved by elastic deformation is 2.1 mm or less.
[0033] As shown in Figures 2 and 3, the rolled material 100 is used in a display device 200 including a communication device, a television, or a computer. The display device 200 includes a display unit 1 and a support member 2 that supports the display unit 1. The display unit 1 displays an image using organic EL (Electro-Luminescence). The support member 2 is made of the rolled material 100. The display device 200 can be bent or curved by elastic deformation.
[0034] As shown in Fig. 2, a display device 200 that can be bent by elastic deformation can be folded because the display unit 1 and the support member 21 are bent. In the case of Fig. 2, the support member 21 is manufactured by forming the rolled material 100 into a frame shape that surrounds the periphery of the display unit 1.
[0035] As shown in Fig. 3, a display device 200 that can be bent by elastic deformation can be rolled up around a shaft portion 3 because the display unit 1 and the support member 22 are bent. In the case of Fig. 3, the support member 22 is manufactured by forming a rolled material 100 into a sheet shape.
[0036] The above formulas (1) and (2) will be explained with reference to FIG. 4. The inventors prepared a titanium alloy (rolled material) with a thickness of 0.03 mm (30 μm), set the fatigue limit at which the surface stress of the titanium alloy (rolled material) when bent at a bending radius of 1.2 mm is 900 MPa as the fatigue strength at which no fracture occurs, and plotted the relationship between the fatigue limit (GPa) and Vickers hardness (HV). As a result, they found that a proportional relationship exists between the fatigue limit and the Vickers hardness, and that the following relationship holds: fatigue limit σ' = (0.0024 × Vickers hardness + 0.1028) ··· formula (3). The decision coefficient R, which indicates the error of the actual measured value of formula (3), 2 is 0.9818, which is close to 1, so there is little error and it can be said to be a valid formula.
[0037] Here, the maximum bending stress σ is expressed by σ=t×E / 2ρ···Equation (4). In the equation, t is the thickness of the rolled material 100, E is the elastic coefficient of the rolled material 100, and ρ is the bending radius. The inventors of the present application set the bending radius ρ when the maximum bending stress σ and the fatigue limit σ' are equal to be the minimum bending radius ρ that can withstand 200,000 repeated bendings. Then, from equations (3) and (4), the inventors derived equation (5) of t×E / 2ρ=(0.0024×Vickers hardness+0.1028), and transformed equation (5) to derive equation ρ=t×E / (0.0048×Vickers hardness+0.2056). Then, the inventors rounded off 0.2056 to two decimal places to obtain 0.21, and derived equation (2) which is a prediction equation for the minimum bending radius. In addition, the larger the (0.0048 × Vickers hardness + 0.21) value, the higher the durability against repeated bending due to elastic deformation, and the smaller the elastic modulus, the easier it is to deform and bend repeatedly, so (0.0048 × Vickers hardness + 0.21) ÷ elastic modulus was set as the index value.
[0038] (Rolled material manufacturing method) As shown in FIG. 5, the rolled material 100 is an alloy or pure metal that is first rolled by rollers 11, and then subjected to a tempering treatment to adjust the index to 0.014 HV or more. The tempering treatment includes rolling and heat treatment such as annealing and aging treatment, and any of the steps may be performed alone or in combination. For example, only rolling is performed so that the rolling ratio is 90% or more. Annealing may be performed at a temperature of 750° C. to 850° C. for 1 minute. After rolling to a rolling ratio of 60% or more, heat treatment may be performed at 450° C. for 1 minute to 4 hours.
[0039] <Effects of this embodiment> In this embodiment, the following effects can be obtained.
[0040] In this embodiment, the rolled material 100 is made of an alloy or pure metal and is used for components that can be bent or curved, and is made of an alloy or pure metal, and when the value obtained by the following formula (1) is used as an index value for durability against repeated bending, the index value is 0.014 HV / GPa or more. Index value = (0.0048 × Vickers hardness + 0.21) ÷ Elastic modulus (1)
[0041] Here, the inventors of the present application have found that 0.0048 x Vickers hardness + 0.21 can be regarded as the value of the fatigue limit. Therefore, when this index value is 0.014 HV / GPa or more, the fatigue limit is sufficiently large, and durability against repeated bending due to elastic deformation can be increased. In addition, since the elastic modulus represents the magnitude of strain due to bending stress, the strain is reduced by reducing the elastic modulus, and it is possible to suppress the occurrence of breakage due to repeated bending due to elastic deformation. As a result, it is possible to obtain a rolled material 100 that is excellent in durability against bending stress applied to the rolled material 100 due to repeated bending due to elastic deformation.
[0042] In this embodiment, the index value is 0.019 HV / GPa or more, which provides sufficiently high durability against repeated bending due to elastic deformation, and the inventors of the present application have found through experiments described below that the bending radius can be further reduced.
[0043] In this embodiment, the pure metal is pure titanium. The inventors of the present application have found through experiments described below that the use of pure titanium makes it possible to achieve an index value of 0.014 HV / GPa or more.
[0044] In this embodiment, the alloy is a beta-titanium alloy, austenitic stainless steel, or beryllium copper. The inventors of the present application have found through experiments described below that by using a beta-titanium alloy, austenitic stainless steel, or beryllium copper, it is possible to make the index value 0.014HV / GPa or more and to make the bending radius 3mm or less.
[0045] In this embodiment, the beta titanium alloy is composed of 14.0 mass% or more and 16.0 mass% or less of V, 2.5 mass% or more and 3.5 mass% or less of Cr, 2.5 mass% or more and 3.5 mass% or less of Sn, and 2.5 mass% or more and 3.5 mass% or less of Al. The inventors of the present application have found through experiments described below that this makes it possible to make the index value of the rolled material 0.014HV / GPa or more, and for example, the bending radius of a rolled material with a thickness of 0.03 mm can be made 3 mm or less.
[0046] In this embodiment, when the value obtained by the following formula (2) is used as the predicted value of the minimum bending radius at which the rolled material can be bent or curved, when the thickness of the rolled material is 0.03 mm, the predicted value of the minimum bending radius is 2.14 mm or less. Minimum bending radius = (thickness × elastic modulus) ÷ (0.0048 × Vickers hardness + 0.21) (2)
[0047] This makes it possible to reduce the bending radius by adjusting the elastic modulus or Vickers hardness so that the predicted value of the minimum bending radius is 2.14 mm or less. Furthermore, by predicting the minimum bending radius, it is possible to obtain the value of the minimum bending radius at which the rolled material 100 can be folded or bent by elastic deformation without conducting an experiment, so that the desired rolled material 100 can be easily designed.
[0048] In this embodiment, the rolled material 100 is used for a bendable or curved support member 2 that supports a display unit 1 of a display device 200. This makes it possible to improve the durability of the support member 2 against repeated bending, which is repeatedly bent or curved due to elastic deformation in association with repeated bending deformation due to elastic deformation of the display unit 1.
[0049] In this embodiment, the thickness is 0.03 mm or less, and the maximum measured value of the bending radius at which the rolled material 100 can be bent or curved is 2.1 mm or less. This allows the rolled material 100 to be used in a portable device that is bent or curved, since the thickness of the rolled material 100 is sufficiently small and the bending radius can be sufficiently small.
[0050] In this embodiment, the index value is 0.014 HV / GPa or more and 0.029 HV / GPa or less. The inventors of the present application have found through experiments described later that if the index value is set in this range, the bending radius due to elastic deformation can be made sufficiently small.
[0051] [Example] Comparative experiments (Examples and Comparative Examples) based on the above embodiment will be described below.
[0052] As shown in Table 1, for Examples 1 to 27 and Comparative Examples 1 to 4, an index value of durability against repeated bending due to elastic deformation was calculated from the Vickers hardness and the elastic modulus.
[0053] [Table 1]
[0054] Table 1 shows Examples 1 to 10. In Examples 1 to 10, the rolled material 100 is made of a beta-type titanium alloy.
[0055] Specifically, as shown in Table 1, Examples 1 to 8 are rolled materials made of Ti-15V-3Cr-3Sn-3Al by mass%, Example 9 is a rolled material made of Ti-15Mo-5Zr by mass%, and Example 10 is a rolled material made of Ti-15Mo-5Zr-3Al by mass%.
[0056] In addition, in Examples 1 to 10, when the final finish (tempering treatment) is cold rolling (second rolling step), the finish code is indicated by H. When the final finish (tempering treatment) is annealing, the finish code is indicated by O. When the final finish (tempering treatment) is a heat treatment (for example, an aging treatment with a holding time of more than 1 hour) performed after rolling, the finish code is indicated by HT.
[0057] Example 1 is a rolled material (thickness 0.03 mm, finish code: H) made of Ti-15V-3Cr-3Sn-3Al that has been subjected to a tempering treatment (rolling at a rolling ratio of 95%). In Example 1, the elastic modulus in the roll direction (rolling direction) was measured and found to be 72 GPa. In addition, Example 1 had a Vickers hardness of 316 HV. Therefore, the index value of Example 1 is 0.0240 HV / GPa.
[0058] Example 2 is a rolled material (thickness 0.03 mm, finish code: H) made of Ti-15V-3Cr-3Sn-3Al that has been subjected to a tempering treatment (rolling at a rolling ratio of 95%). In Example 2, the elastic modulus in the width direction (direction perpendicular to the rolling direction) was measured and found to be 90 GPa. In addition, Example 2 had a Vickers hardness of 316 HV. Therefore, the index value of Example 2 is 0.0192 HV / GPa.
[0059] Example 3 is a rolled material (thickness 0.02 mm, finish code: H) made of Ti-15V-3Cr-3Sn-3Al that has been subjected to a tempering treatment (rolling at a rolling ratio of 97%). In Example 3, the elastic modulus in the roll direction (rolling direction) was measured and found to be 69 GPa. In addition, Example 3 had a Vickers hardness of 326 HV. Therefore, the index value of Example 3 is 0.0257 HV / GPa.
[0060] Example 4 is a rolled material (thickness 0.02 mm, finish code: H) made of Ti-15V-3Cr-3Sn-3Al after tempering (rolling at a rolling ratio of 97%). In Example 4, the elastic modulus in the width direction (direction perpendicular to the rolling direction) was measured and found to be 84 GPa. In addition, Example 4 had a Vickers hardness of 326 HV. Therefore, the index value of Example 4 is 0.0211 HV / GPa.
[0061] Example 5 is a rolled material (thickness 0.03 mm, finish code: HT) made of Ti-15V-3Cr-3Sn-3Al after tempering treatment. In Example 5, as tempering treatment, rolling was performed at a rolling ratio of 95% and then aging treatment was performed at 450°C for 4 hours. In Example 5, the elastic modulus in the roll direction (rolling direction) was measured and found to be 109 GPa. Furthermore, in Example 5, the Vickers hardness was 480 HV. Therefore, the index value of Example 5 is 0.0231 HV / GPa.
[0062] Example 6 is a rolled material (thickness 0.03 mm, finish code: HT) made of Ti-15V-3Cr-3Sn-3Al after tempering treatment. In Example 6, as tempering treatment, rolling was performed at a rolling ratio of 95% and then aging treatment was performed at 450°C for 4 hours. In Example 6, the elastic modulus in the width direction (direction perpendicular to the rolling direction) was measured and found to be 121 GPa. Furthermore, in Example 6, the Vickers hardness was 480 HV. Therefore, the index value of Example 6 is 0.0208 HV / GPa.
[0063] Example 7 is a rolled material (thickness 0.03 mm, finish code: O) made of Ti-15V-3Cr-3Sn-3Al after annealing (holding at 800°C for 1 minute). In Example 7, the elastic modulus in the roll direction (rolling direction) was measured and found to be 80 GPa. In addition, Example 7 had a Vickers hardness of 262 HV. Therefore, the index value of Example 7 is 0.0183 HV / GPa.
[0064] Example 8 is a rolled material (thickness 0.03 mm, finish code: O) made of Ti-15V-3Cr-3Sn-3Al after annealing (holding at 800°C for 1 minute). In Example 8, the elastic modulus in the width direction (direction perpendicular to the rolling direction) was measured and found to be 94 GPa. In addition, Example 8 had a Vickers hardness of 262 HV. Therefore, the index value of Example 8 is 0.0156 HV / GPa.
[0065] Example 9 is a rolled material (finish code: O) made of Ti-15Mo-5Zr and annealed (held at 850°C for 1 minute). The rolled material of Example 9 has, for example, an elastic modulus of 78 GPa in the roll direction (rolling direction) and a Vickers hardness of 280 HV. Therefore, the index value of Example 9 is 0.0199 HV / GPa.
[0066] Example 10 is a rolled material (finish code: O) made of Ti-15Mo-5Zr-3Al after annealing (holding at 850°C for 1 minute). The rolled material of Example 10 has, for example, an elastic modulus of 100 GPa in the roll direction (rolling direction) and a Vickers hardness of 275 HV. Therefore, the index value of Example 10 is 0.0153 HV / GPa.
[0067] [Table 2]
[0068] Table 2 shows Examples 11 to 20. In Examples 11 to 17, the rolled material 100 is made of a beta-type titanium alloy. In Examples 18 to 20, the rolled material 100 is made of pure Ti.
[0069] Specifically, as shown in Table 2, Example 11 is a rolled material made of Ti-11.5Mo-6Zr-4.5Sn by mass%. Example 12 is a rolled material made of Ti-4Mo-8V-6Cr-3Al-4Zr by mass%. Example 13 is a rolled material made of Ti-13V-11Cr-3Al by mass%. Example 14 is a rolled material made of Ti-29Nb-13Ta-4.6Zr by mass%. Examples 15 and 16 are rolled materials made of Ti-36Nb-2Ta-3Zr-0.3O by mass%. Example 17 is a rolled material made of Ti-5Fe-3Nb-3Zr by mass%. Examples 18 and 19 are rolled materials made of TR270C (JIS H4600:2012). Example 20 is a rolled material made of TR550C (JIS H4600:2012).
[0070] In addition, in Examples 11 to 20, when the final finishing (tempering treatment) is cold rolling (second rolling step), the finish code is indicated by H. When the final finishing (tempering treatment) is annealing, the finish code is indicated by O.
[0071] Example 11 is a rolled material (finish code: O) made of Ti-11.5Mo-6Zr-4.5Sn after annealing (holding at 850°C for 1 minute). The rolled material of Example 11 has, for example, an elastic modulus of 79 GPa in the roll direction (rolling direction) and a Vickers hardness of 240 HV. Therefore, the index value of Example 11 is 0.0172 HV / GPa.
[0072] Example 12 is a rolled material (finish code: O) made of Ti-4Mo-8V-6Cr-3Al-4Zr after annealing (holding at 750°C for 1 minute). The rolled material of Example 12 has, for example, an elastic modulus of 104 GPa in the roll direction (rolling direction) and a Vickers hardness of 367 HV. Therefore, the index value of Example 12 is 0.0190 HV / GPa.
[0073] Example 13 is a rolled material (finish code: O) made of Ti-13V-11Cr-3Al after annealing (holding at 800°C for 1 minute). The rolled material of Example 13 has, for example, an elastic modulus in the roll direction (rolling direction) of 101 GPa and a Vickers hardness of 300 HV. Therefore, the index value of Example 13 is 0.0163 HV / GPa.
[0074] Example 14 is a rolled material (finish code: O) made of Ti-29Nb-13Ta-4.6Zr after annealing (holding at 800°C for 1 minute). The rolled material of Example 14 has, for example, an elastic modulus of 60 GPa in the roll direction (rolling direction) and a Vickers hardness of 280 HV. Therefore, the index value of Example 14 is 0.0259 HV / GPa.
[0075] Example 15 is a rolled material (thickness 0.10 mm, finish code: H) made of Ti-36Nb-2Ta-3Zr-0.3O after tempering (rolling at a rolling ratio of 95%). In Example 15, the elastic modulus in the roll direction (rolling direction) was measured and found to be 75 GPa. In addition, in Example 15, the Vickers hardness was 313 HV. Therefore, the index value of Example 15 is 0.0228 HV / GPa.
[0076] Example 16 is a rolled material (finish code: O) made of Ti-36Nb-2Ta-3Zr-0.3O after annealing (holding at 850°C for 1 minute). The rolled material of Example 16 has, for example, an elastic modulus of 50 GPa in the roll direction (rolling direction) and a Vickers hardness of 250 HV. Therefore, the index value of Example 16 is 0.0282 HV / GPa.
[0077] Example 17 is a rolled material (finish code: O) made of Ti-5Fe-3Nb-3Zr after annealing (holding at 900°C for 1 minute). The rolled material of Example 17 has, for example, an elastic modulus of 82 GPa in the roll direction (rolling direction) and a Vickers hardness of 375 HV. Therefore, the index value of Example 17 is 0.0245 HV / GPa.
[0078] Example 18 is a rolled material (thickness 0.03 mm, finish code: H) made of TR270C (JIS H4600:2012) after tempering (rolling at a rolling ratio of 94%). In Example 18, the elastic modulus in the roll direction (rolling direction) was measured and found to be 93 GPa. In addition, Example 18 had a Vickers hardness of 251 HV. Therefore, the index value of Example 18 is 0.0152 HV / GPa.
[0079] Example 19 is a rolled material (thickness 0.03 mm, finish code: H) made of TR270C (JIS H4600:2012) after tempering (rolling at a rolling ratio of 94%). In Example 19, the elastic modulus in the width direction (direction perpendicular to the rolling direction) was measured and found to be 95 GPa. In addition, Example 19 had a Vickers hardness of 251 HV. Therefore, the index value of Example 19 is 0.0149 HV / GPa.
[0080] Example 20 is a rolled material (thickness 0.10 mm, finish code: H) made of TR550C (JIS H4600:2012) after tempering (rolling at a rolling ratio of 65%). In Example 20, the elastic modulus in the roll direction (rolling direction) was measured and found to be 105 GPa. In addition, in Example 20, the Vickers hardness was 300 HV. Therefore, the index value of Example 20 is 0.0157 HV / GPa.
[0081] [Table 3]
[0082] Table 3 shows Examples 21 to 27 and Comparative Examples 1 to 4. In Examples 21 to 26, the rolled material 100 is made of stainless steel. In Example 27, the rolled material 100 is made of beryllium copper alloy. In Comparative Example 1, the rolled material is made of pure titanium. In Comparative Examples 2 and 3, the rolled material is made of stainless steel. In Comparative Example 4, the rolled material is made of aluminum alloy.
[0083] Specifically, as shown in Table 3, Examples 21 to 23 are rolled materials made of SUS301 (JIS G4313:2011). Example 24 is a rolled material made of SUS316L (JIS G4305:2011). Examples 25 and 26 are rolled materials made of YUS130S (Fe-19Cr-11Mn-6Ni-0.35N-0.09C in mass%). Example 27 is a rolled material made of C1720 (JIS H3130:2018). Comparative Example 1 is a rolled material made of TR550C (JIS H46400:2012). Comparative Example 2 is a rolled material made of SUS301 (JIS G4313:2011). Comparative Example 3 is a rolled material made of SUS316L (JIS G4305:2011). Comparative Example 4 is a rolled material made of A5052 (JIS H4000:2014).
[0084] In addition, in Examples 21 to 26 and Comparative Examples 1 to 4, when the final finish (tempering treatment) is cold rolling (second rolling step), the finish code is represented by H. When the final finish (tempering treatment) is annealing, the finish code is represented by O. When the final finish (tempering treatment) involves heat treatment after rolling (for example, aging treatment with a holding time of 1 hour or less), the finish code is represented by EH-TA. In Example 27, a treatment is carried out in the final finish (tempering treatment) to precipitate beryllium at a low temperature to harden it, and therefore the finish code is represented by XHMS.
[0085] Example 21 is a rolled material (thickness 0.03 mm, finish code: EH-TA) made of SUS301 (JIS G4313:2011) after tempering treatment. In Example 21, as tempering treatment, rolling was performed at a rolling ratio of 69% and then aging treatment was performed by holding at 450°C for 1 minute. In Example 21, the elastic modulus in the roll direction (rolling direction) was measured and found to be 183 GPa. In addition, in Example 21, the Vickers hardness was 600 HV. Therefore, the index value of Example 21 is 0.0169 HV / GPa.
[0086] Example 22 is a rolled material (thickness 0.03 mm, finish code: EH-TA) made of SUS301 (JIS G4313:2011) after tempering treatment. In Example 22, as tempering treatment, rolling was performed at a rolling ratio of 69% and then aging treatment was performed at 450°C for 1 minute. In Example 22, the elastic modulus in the width direction (direction perpendicular to the rolling direction) was measured and found to be 211 GPa. In addition, in Example 22, the Vickers hardness was 600 HV. Therefore, the index value of Example 22 is 0.0146 HV / GPa.
[0087] Example 23 is a rolled material (thickness 0.02 mm, finish code: EH-TA) made of SUS301 (JIS G4313:2011) after tempering treatment. In Example 23, as tempering treatment, rolling was performed at a rolling ratio of 62% and then aging treatment was performed at 450°C for 1 minute. In Example 23, the elastic modulus in the roll direction (rolling direction) was measured and found to be 182 GPa. In addition, in Example 23, the Vickers hardness was 557 HV. Therefore, the index value of Example 23 is 0.0158 HV / GPa.
[0088] Example 24 is a rolled material (thickness 0.03 mm, finish code: H) made of SUS316L (JIS G4305:2021) after tempering (rolling at a rolling ratio of 67%). In Example 24, the elastic modulus in the roll direction (rolling direction) was measured and found to be 155 GPa. In addition, in Example 24, the Vickers hardness was 438 HV. Therefore, the index value of Example 24 is 0.0149 HV / GPa.
[0089] Example 25 is a rolled material (thickness 0.03 mm, finish code: H) made of YUS130S (Fe-19Cr-11Mn-6Ni-0.35N-0.09C) after tempering (rolling at a rolling ratio of 67%). In Example 25, the elastic modulus in the roll direction (rolling direction) was measured and found to be 174 GPa. In addition, in Example 25, the Vickers hardness was 520 HV. Therefore, the index value of Example 25 is 0.0156 HV / GPa.
[0090] Example 26 is a rolled material (thickness 0.03 mm, finish code: H) made of YUS130S (Fe-19Cr-11Mn-6Ni-0.35N-0.09C) after tempering (rolling at a rolling ratio of 67%). In Example 26, the elastic modulus in the width direction (direction perpendicular to the rolling direction) was measured and found to be 193 GPa. In addition, Example 26 had a Vickers hardness of 520 HV. Therefore, the index value of Example 26 is 0.0140 HV / GPa.
[0091] Example 27 is a rolled material (thickness 0.03 mm, finish code: XHMS) made of C1720 (JIS H3130:2018) after tempering treatment. In Example 27, as tempering treatment, rolling was performed at a rolling ratio of 88% and then annealing was performed at 450 ° C for 2 minutes. In Example 27, when the elastic modulus in the roll direction (rolling direction) was measured, the elastic modulus was 127 GPa. In addition, in Example 27, the Vickers hardness was 380 HV. Therefore, the index value of Example 27 is 0.0160 HV / GPa.
[0092] Comparative Example 1 is a rolled material (thickness 0.10 mm, finish code: O) made of TR550C (JIS H4600:2012) after annealing (holding at 800°C for 1 minute). In Comparative Example 1, the elastic modulus in the roll direction (rolling direction) was measured and found to be 105 GPa. In addition, in Comparative Example 1, the Vickers hardness was 230 HV. Therefore, the index value of Comparative Example 1 is 0.0125 HV / GPa.
[0093] Comparative Example 2 is a rolled material (thickness 0.02 mm, finish code: EH-TA) made of SUS301 (JIS H4313:2011) after tempering treatment. In Comparative Example 2, as tempering treatment, rolling was performed at a rolling ratio of 62% and then aging treatment was performed by holding at 450°C for 1 minute. In Comparative Example 2, the elastic modulus in the width direction (direction perpendicular to the rolling direction) was measured and found to be 211 GPa. Furthermore, in Comparative Example 2, the Vickers hardness was 557 HV. The index value of Comparative Example 2 is 0.0137 HV / GPa.
[0094] Comparative Example 3 is a rolled material (thickness 0.03 mm, finish code: H) made of SUS316L (JIS H4305:2021) after tempering (rolling at a rolling ratio of 67%). In Comparative Example 3, the elastic modulus in the width direction (direction perpendicular to the rolling direction) was measured and found to be 185 GPa. In Comparative Example 3, the Vickers hardness was 438 HV. Therefore, the index value of Comparative Example 3 is 0.0125 HV / GPa.
[0095] Comparative Example 4 is a rolled material (thickness 0.03 mm, finish code: H) made of A5052 (JIS H4000:2014) after tempering (rolling at a rolling ratio of 90%). In Comparative Example 4, the elastic modulus in the roll direction (rolling direction) was measured and found to be 68 GPa. In addition, in Comparative Example 4, the Vickers hardness was 120 HV. Therefore, the index value of Comparative Example 4 is 0.0116 HV / GPa.
[0096] From the above results, it was found that even if the rolled material is composed of the same chemical composition, if the final finishing (conditions of the tempering process, etc.) or the measurement direction of the elastic modulus is different, the index value may differ and the target value may not be met.
[0097] Table 4 shows the predicted values of the minimum bending radius of the rolled material 100 of Examples 1 to 8, Example 18, Example 19, and Example 21 that can withstand 200,000 repeated bendings, and the actual values of the minimum bending radius that can withstand 200,000 repeated bendings. The 200,000 repeated bendings are repeated bendings caused by elastic deformation. The predicted values of the minimum bending radius that can withstand 200,000 repeated bendings were calculated by the following formula: minimum bending radius (R) = (thickness x elastic modulus) ÷ (0.0048 x Vickers hardness + 0.21). The actual values of the minimum bending radius that can withstand 200,000 repeated bendings were calculated by reducing the bending radius of the rolled material 100 from 3.0 mm in 0.1 mm increments, and the radius that was 0.1 mm larger than the bending radius that could not withstand 200,000 repeated bendings was used as the actual values of the minimum bending radius that can withstand 200,000 repeated bendings.
[0098] [Table 4]
[0099] In Example 1, when repeatedly bending in the roll direction (rolling direction), the predicted minimum bending radius that could withstand 200,000 repeated bendings was 1.25 mm, whereas the actual measured value was 1.20 mm.
[0100] In Example 2, when repeatedly bending in the width direction (direction perpendicular to the rolling direction), the predicted minimum bending radius that could withstand 200,000 repeated bendings was 1.56 mm, whereas the actual measured value was 1.60 mm.
[0101] In Example 3, when repeatedly bending in the roll direction (rolling direction), the predicted minimum bending radius that could withstand 200,000 repeated bendings was 0.78 mm, whereas the actual measured value was 0.80 mm.
[0102] In Example 4, when repeatedly bending in the width direction (the direction perpendicular to the rolling direction), the predicted minimum bending radius that could withstand 200,000 repeated bendings was 0.95 mm, whereas the actual measured value was 1.00 mm.
[0103] In Example 5, when repeatedly bending in the roll direction (rolling direction), the predicted minimum bending radius that could withstand repeated bending 200,000 times was 1.30 mm, whereas the actual measured value was 1.30 mm.
[0104] In Example 6, when repeatedly bending in the width direction (direction perpendicular to the rolling direction), the predicted minimum bending radius that could withstand 200,000 repeated bendings was 1.44 mm, whereas the actual measured value was 1.50 mm.
[0105] In Example 7, when repeatedly bending in the roll direction (rolling direction), the predicted minimum bending radius that could withstand 200,000 repeated bendings was 1.64 mm, whereas the actual measured value was 1.70 mm.
[0106] In Example 8, when repeatedly bending in the width direction (the direction perpendicular to the rolling direction), the predicted minimum bending radius that could withstand 200,000 repeated bendings was 1.92 mm, whereas the actual measured value was 2.00 mm.
[0107] In Example 18, when repeatedly bending in the roll direction (rolling direction), the predicted minimum bending radius that could withstand 200,000 repeated bendings was 1.97 mm, whereas the actual measured value was 2.00 mm.
[0108] In Example 19, when repeatedly bending in the width direction (direction perpendicular to the rolling direction), the predicted minimum bending radius that could withstand 200,000 repeated bendings was 2.01 mm, whereas the actual measured value was 2.00 mm.
[0109] In Example 21, when repeatedly bending in the roll direction (rolling direction), the predicted minimum bending radius that could withstand 200,000 repeated bendings was 1.78 mm, whereas the actual measured value was 1.80 mm.
[0110] Table 5 shows the predicted values of the minimum bending radius that can withstand 200,000 repeated bendings of the rolled material 100 of Examples 22 to 26, Comparative Example 2, and Comparative Example 3, and the actual values of the minimum bending radius that can withstand 200,000 repeated bendings. The 200,000 repeated bendings are repeated bendings caused by elastic deformation. The predicted values of the minimum bending radius that can withstand 200,000 repeated bendings were calculated by the formula: minimum bending radius (R) = (thickness x elastic modulus) ÷ (0.0048 x Vickers hardness + 0.21). The actual values of the minimum bending radius that can withstand 200,000 repeated bendings were calculated by reducing the bending radius of the rolled material 100 from 3.0 mm in 0.1 mm increments, and the radius that was 0.1 mm larger than the bending radius that could not withstand 200,000 repeated bendings was used as the actual values of the minimum bending radius that can withstand 200,000 repeated bendings.
[0111] [Table 5]
[0112] In Example 22, when repeatedly bending in the width direction (direction perpendicular to the rolling direction), the predicted minimum bending radius capable of withstanding 200,000 repeated bendings was 2.05 mm, and the actual measured value was 2.00 mm.
[0113] In Example 23, when repeatedly bending in the roll direction (rolling direction), the predicted minimum bending radius that could withstand 200,000 repeated bendings was 1.26 mm, whereas the actual measured value was 1.30 mm.
[0114] In Example 24, when repeatedly bending in the roll direction (rolling direction), the predicted minimum bending radius that could withstand 200,000 repeated bendings was 2.01 mm, whereas the actual measured value was 2.10 mm.
[0115] In Example 25, when repeatedly bending in the roll direction (rolling direction), the predicted minimum bending radius that could withstand repeated bending 200,000 times was 1.93 mm, whereas the actual measured value was 2.00 mm.
[0116] In Example 26, when repeatedly bending in the width direction (direction perpendicular to the rolling direction), the predicted minimum bending radius that could withstand 200,000 repeated bendings was 2.14 mm, whereas the actual measured value was 2.10 mm.
[0117] In Comparative Example 2, when repeatedly bending in the width direction (direction perpendicular to the rolling direction), the predicted minimum bending radius that could withstand 200,000 repeated bendings was 1.46 mm, whereas the actual measured value was 1.60 mm.
[0118] In Comparative Example 3, when repeatedly bending in the width direction (direction perpendicular to the rolling direction), the predicted minimum bending radius that could withstand repeated bending 200,000 times was 2.40 mm, whereas the actual measured value was 2.30 mm.
[0119] From the above results, the difference between the predicted value calculated by Minimum bending radius = (Thickness × Elastic modulus) ÷ (0.0048 × Vickers hardness + 0.21) and the actual measured value was a maximum of 0.14 mm (Comparative Example 2). However, it is reasonable to consider that a difference of about 0.14 mm is within the margin of error, and the prediction formula for the minimum bending radius can be said to be an effective formula for designing the actual minimum bending radius.
[0120] Table 6 shows the predicted fatigue limits of rolled material 100 for Examples 1 to 8, 18, and 19, calculated using (0.0021 x Vickers hardness + 0.103), the actual measured values, and the differences between the predicted and actual measured values (actual measured values - predicted values).
[0121] [Table 6]
[0122] In Example 1, the predicted value when bending in the roll direction (rolling direction) was 0.861 GPa, and the actual measured value was 0.900 GPa, the difference being +0.039.
[0123] In Example 2, when bending in the width direction (direction perpendicular to the rolling direction), the predicted value was 0.861 GPa and the measured value was 0.844 GPa, the difference being −0.017.
[0124] In Example 3, the predicted value when bending in the roll direction (rolling direction) was 0.885 GPa, and the actual measured value was 0.863 GPa, the difference being -0.022.
[0125] In Example 4, when bending in the width direction (direction perpendicular to the rolling direction), the predicted value was 0.885 GPa and the measured value was 0.840 GPa, the difference being -0.045.
[0126] In Example 5, the predicted value when bending in the roll direction (rolling direction) was 1.255 GPa, and the actually measured value was 1.258 GPa, the difference being +0.003.
[0127] In Example 6, when bending in the width direction (direction perpendicular to the rolling direction), the predicted value was 1.255 GPa and the measured value was 1.210 GPa, the difference being -0.045.
[0128] In Example 7, the predicted value when bending in the roll direction (rolling direction) was 0.732 GPa, and the actual measured value was 0.706 GPa, the difference being -0.026.
[0129] In Example 8, when bending in the width direction (direction perpendicular to the rolling direction), the predicted value was 0.732 GPa and the actual measured value was 0.705 GPa, the difference being -0.027.
[0130] In Example 18, the predicted value when bending in the roll direction (rolling direction) was 0.705 GPa and the actual measured value was 0.698 GPa, the difference being -0.007.
[0131] In Example 19, when bending in the width direction (direction perpendicular to the rolling direction), the predicted value was 0.705 GPa and the actual measured value was 0.713 GPa, the difference being +0.008.
[0132] Table 7 shows the predicted fatigue limits of rolled material 100 for Examples 21 to 26, Comparative Example 2, and Comparative Example 3, calculated using (0.0024 x Vickers hardness + 0.103), the actual measured values, and the differences between the predicted and actual measured values (actual measured values - predicted values).
[0133] [Table 7]
[0134] In Example 21, the predicted value when bending in the roll direction (rolling direction) was 1.543 GPa, and the actual measured value was 1.525 GPa, the difference being -0.018.
[0135] In Example 22, when bending in the width direction (direction perpendicular to the rolling direction), the predicted value was 1.543 GPa and the actual measured value was 1.583 GPa, the difference being +0.040.
[0136] In Example 23, the predicted value when bending in the roll direction (rolling direction) was 1.440 GPa, and the actual measured value was 1.400 GPa, the difference being -0.040.
[0137] In Example 24, the predicted value when bending in the roll direction (rolling direction) was 1.154 GPa, and the actual value was 1.107 GPa, the difference being -0.047.
[0138] In Example 25, the predicted value when bending in the roll direction (rolling direction) was 1.351 GPa, and the actual measured value was 1.305 GPa, the difference being -0.046.
[0139] In Example 26, when bending in the width direction (direction perpendicular to the rolling direction), the predicted value was 1.351 GPa and the actual measured value was 1.379 GPa, the difference being +0.028.
[0140] In Comparative Example 2, when bending in the width direction (direction perpendicular to the rolling direction), the predicted value was 1.440 GPa and the measured value was 1.319 GPa, the difference being -0.121.
[0141] In Comparative Example 3, when bending in the width direction (direction perpendicular to the rolling direction), the predicted value was 1.154 GPa and the actual measured value was 1.207 GPa, the difference being +0.053.
[0142] From the results in Tables 6 and 7, the average σ of the difference between the predicted value and the actual value (actual value - predicted value) was 0.041, and the variation 3σ was ±0.124. Therefore, it was found that when setting the minimum bending radius, it is more preferable to change the minimum bending radius from minimum bending radius = (thickness × elastic modulus) ÷ (0.0048 × Vickers hardness + 0.21 - 0.124 × 2) to minimum bending radius = (thickness × elastic modulus) ÷ (0.0048 × Vickers hardness + 0.21 - 0.25), that is, to minimum bending radius = (thickness × elastic modulus) ÷ (0.0048 × Vickers hardness - 0.04).
[0143] Table 8 shows the results of measuring the index value of durability against repeated bending, density, relative permeability, fatigue limit, and bending radius of the rolled material 100 of Example 1, Example 15, Example 18, Example 21, Example 24, Example 25, Example 27, and Comparative Examples 2 to 4. Table 8 also shows the level and evaluation of each value. The calculation method of the level and evaluation is as shown in Table 9.
[0144] [Table 8]
[0145] [Table 9]
[0146] The ratings are as follows: level 90 to 100 is rated 1, level 70 to less than 90 is rated 2, level 30 to less than 70 is rated 3, level 10 to less than 30 is rated 4, and level 0 to less than 10 is rated 5. Rating 1 means high (higher than average), rating 2 means slightly above average, rating 3 means average, rating 4 means slightly below average, and rating 5 means low (lower than average).
[0147] As shown in Table 9, the higher the level of the index value, the higher the durability against repeated bending is, so the higher the level is, the more preferable. Therefore, the level of the index value is calculated by subtracting the minimum value from the value to be calculated (the value) (the value-minimum value) ÷ subtracting the minimum value from the maximum value (maximum value-minimum value) × 100. In the case of Table 8, for example, the level of the index value of Example 1 is 0.240, the maximum index value is 0.240 in Example 1, and the minimum index value is 0.0116 in Comparative Example 4, so that (0.240-0.116) ÷ (0.240-0.116) × 100 = 100.
[0148] Also, the smaller the relative permeability value, the greater the non-magnetic property, and the higher the evaluation. Furthermore, the smaller the density value, the higher the evaluation because it allows for lighter weight. Therefore, the relative permeability level and density level are calculated as 100-{(relevant value-minimum value)÷maximum value minus minimum value (maximum value-minimum value)×100} so that the lower the level, the higher the evaluation.
[0149] In Example 1, the index value was 0.0240 HV / GPa, the index value level was 100, and the evaluation was 1. In addition, in Example 1, the density was 4.76 g / cm 3 , the index level was 63, and the evaluation was 3. In Example 1, the relative permeability was 1.00050, the index level was 100, and the evaluation was 1. In Example 1, the fatigue limit was 0.90 GPa, and the bending radius was 1.20 mm.
[0150] In Example 15, the index value was 0.0228 HV / GPa, the index value level was 90, and the evaluation was 1. In addition, in Example 15, the density was 5.60 g / cm 3 The index value level was 48, and the evaluation score was 3. In Example 15, the relative permeability was 1.00030, the index value level was 100, and the evaluation score was 1.
[0151] In Example 18, the index value was 0.0152 HV / GPa, the index value level was 29, and the evaluation was 4. In addition, in Example 18, the density was 4.51 g / cm 3 , the index level was 67, and the evaluation was 3. In Example 18, the relative permeability was 1.00030, the index level was 100, and the evaluation was 1. In Example 18, the fatigue limit was 0.698 GPa, and the bending radius was 2.00 mm.
[0152] In Example 21, the index value was 0.0169 HV / GPa, the index value level was 43, and the evaluation was 3. In addition, in Example 21, the density was 7.93 g / cm 3and the index level was 6 and the evaluation was 5. In Example 21, the relative permeability was 1.60000, the index level was 0 and the evaluation was 5. In Example 21, the fatigue limit was 1.525 GPa and the bending radius was 1.80 mm.
[0153] In Example 24, the index value was 0.0149 HV / GPa, the index value level was 27, and the evaluation was 4. In addition, in Example 24, the density was 7.98 g / cm 3 , the index level was 5, and the evaluation was 5. In Example 24, the relative permeability was 1.02100, the index level was 97, and the evaluation was 1. In Example 24, the fatigue limit was 1.107 GPa, and the bending radius was 2.10 mm.
[0154] In Example 25, the index value was 0.0156 HV / GPa, the index value level was 32, and the evaluation was 3. In addition, in Example 25, the density was 7.80 g / cm 3 , the index level was 8, and the evaluation was 5. In Example 25, the relative permeability was 1.00190, the index level was 100, and the evaluation was 1. In Example 25, the fatigue limit was 1.305 GPa, and the bending radius was 2.00 mm.
[0155] In Example 27, the index value was 0.0160 HV / GPa, the index value level was 35, and the evaluation was 3. In addition, in Example 27, the density was 8.26 g / cm 3 , the index value level was 0, and the evaluation was 5. In Example 27, the relative permeability was 1.00004, the index value level was 100, and the evaluation was 1.
[0156] In Comparative Example 2, the index value was 0.0137 HV / GPa, the index value level was 17, and the evaluation was 4. In Comparative Example 2, the density was 7.93 g / cm 3, the index level was 6, and the evaluation was 5. In Comparative Example 2, the relative permeability was 1.60000, the index level was 0, and the evaluation was 5. In Comparative Example 2, the fatigue limit was 1.319 GPa, and the bending radius was 1.60 mm.
[0157] In Comparative Example 3, the index value was 0.0125 HV / GPa, the index value level was 7, and the evaluation was 5. In Comparative Example 3, the density was 7.98 g / cm 3 The index value level was 5 and the evaluation was 5. In Comparative Example 3, the relative permeability was 1.02100, the index value level was 97 and the evaluation was 1. In Comparative Example 3, the fatigue limit was 1.207 GPa and the bending radius was 2.30 mm.
[0158] In Comparative Example 4, the index value was 0.0116 HV / GPa, the index value level was 0, and the evaluation was 5. In Comparative Example 4, the density was 2.68 g / cm 3 , the index value level was 100, and the evaluation was 1. In Comparative Example 4, the relative permeability was 1.00020, the index value level was 100, and the evaluation was 1.
[0159] Table 10 summarizes the evaluation of the index value of durability against repeated bending, the evaluation of density, and the evaluation of relative magnetic permeability for each material based on the results of Table 8. [Table 10]
[0160] In the case of the titanium alloys of Example 1 and Example 15, the durability index value was evaluated as 1. The density was evaluated as 3. Furthermore, the relative magnetic permeability was evaluated as 1.
[0161] In the case of the stainless steel (SUS) of Example 21, Example 24, and Example 25, the durability index value was evaluated as 3 or 4. The density was evaluated as 5. Furthermore, the relative magnetic permeability was evaluated as 1 or 5.
[0162] In the case of the copper alloy of Example 27, the durability index value was evaluated as 2. The density was evaluated as 5. Furthermore, the relative permeability was evaluated as 1.
[0163] In the case of the stainless steel (SUS) of Comparative Example 2 and Comparative Example 3, the durability index value was evaluated as 4 or 5. The density was evaluated as 5. Furthermore, the relative magnetic permeability was evaluated as 1 or 5.
[0164] In the case of the aluminum alloy of Comparative Example 4, the durability index value was evaluated as 5. The density was evaluated as 1. Furthermore, the relative magnetic permeability was evaluated as 1.
[0165] As shown in Table 10, the index value evaluation of titanium alloys was significantly higher than that of stainless steel. Therefore, in terms of durability against repeated bending, titanium alloys are clearly superior to stainless steel.
[0166] In addition, the density of titanium alloys was evaluated to be significantly higher than that of stainless steel. Therefore, in terms of light weight, titanium alloys are superior to stainless steel.
[0167] In addition, the relative permeability of the titanium alloy was evaluated to be higher than that of stainless steel. Therefore, from the viewpoint of non-magnetic properties, the titanium alloy is superior to stainless steel.
[0168] From the above results, the inventors of the present application have found that it is more preferable to use a titanium alloy than stainless steel.
[0169] Figure 7 is a graph in which the bending radius is plotted on the vertical axis and the index value is plotted on the horizontal axis. The graph in Figure 7 is based on the bending radius and index value listed in Table 8. The graph in Figure 7 is expressed as y = -79.576x + 3.1394. From the results in Figure 7, it was found that the larger the index value, the smaller the bending radius becomes.
[0170] [Variations] The embodiments and examples disclosed herein should be considered to be illustrative and not restrictive in all respects. The scope of the present invention is indicated by the claims, not by the description of the embodiments and examples described above, and further includes all modifications (variations) within the meaning and scope of the claims.
[0171] For example, in the present embodiment, the rolled material is used in a display device, but the present invention is not limited to this. In the present invention, the rolled material may be used in a spring member such as a contact point of a switch.
[0172] In addition, in the present embodiment, the titanium alloy is a beta-type titanium alloy, but the present invention is not limited to this.
Claims
1. A rolled material used for a member that can be bent or curved, It is made of alloys or pure metals, When the value obtained by the following formula (1) is an index value of durability against repeated bending, the index value is 0.014 HV / GPa or more, A rolled material having a thickness of 0.03 mm or less and a maximum measured bending radius that can be bent or curved of 2.1 mm or less. [0010]
2. The rolled material according to claim 1 , wherein the index value is 0.019 HV / GPa or more.
3. The rolled material according to claim 1 , wherein the pure metal is pure titanium.
4. 2. The rolled material according to claim 1, wherein the alloy is a beta-titanium alloy, an austenitic stainless steel, or a beryllium copper alloy.
5. The alloy comprising the beta titanium alloy, The beta-type titanium alloy is composed of 14.0 mass% or more and 16.0 mass% or less of V, 2.5 mass% or more and 3.5 mass% or less of Cr, 2.5 mass% or more and 3.5 mass% or less of Sn, and 2.5 mass% or more and 3.5 mass% or less of Al. The rolled material according to claim 4.
6. 2. The rolled material according to claim 1, wherein, when a value obtained by the following formula (2) is a predicted value of a minimum bending radius at which the rolled material can be bent or curved, when the thickness of the rolled material is 0.03 mm, the predicted value of the minimum bending radius is 2.14 mm or less. [0025]
7. The rolled material according to claim 1, which is used for a bendable or curveable support member for supporting a display unit of a display device.
8. The rolled material according to claim 1, wherein the index value is 0.014 HV / GPa or more and 0.029 HV / GPa or less.
Citation Information
Patent Citations
High strength metastable austenitic stainless steel sheet for blade having high elasticity and its production
JP2000239800A
BETA Ti ALLOY WITH HIGH STRENGTH AND LOW YOUNG'S MODULUS, AND ITS MANUFACTURING METHOD
JP2003055749A
ALPHA PLUS BETA TITANIUM ALLOY MEMBER HAVING >=1,000 MPa GRADE TENSILE STRENGTH, AND ITS MANUFACTURING METHOD
JP2007314834A
Titanium material and method for producing the same
JP2009228053A
Titanium alloy, titanium alloy member and method for producing titanium alloy member
JP2010111928A