Electrolytic copper foil and secondary battery using same

The electrolytic copper foil with controlled TOC and Cl content addresses strength and elongation issues, ensuring high loading and safety in secondary batteries by adhering to specific performance criteria, thus improving battery performance and reliability.

JP7593566B2Active Publication Date: 2024-12-03LOTTE ENERGY MATERIALS CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023078483
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-05-16
Filing Date
2023-05-11
Publication Date
2024-12-03
Estimated Expiration
2039-01-15

AI Technical Summary

Technical Problem

Existing electrolytic copper foils face issues with reduced tensile strength, elongation rate, and curling due to high chlorine content, leading to decreased productivity and safety concerns in secondary batteries, particularly when used as electrode plates.

Method used

The development of an electrolytic copper foil with Total Organic Carbon (TOC) of 4 ppm or less and chlorine (Cl) of 10 ppm or less, adhering to the formula (Thickness (μm)/(Tensile strength (kgf/mm²)*Stretching rate (%))≦0.1, ensuring a fracture height of 3 mm or more in the Ericsson test, and maintaining a tensile strength of 45 kgf/mm² with a stretching ratio of 3% or more, along with a glossiness of 100 or more.

Benefits of technology

The solution provides an electrolytic copper foil with improved strength, elongation rate, and triaxial multidirectional stretching, enhancing the loading level of cathode active material, increasing non-capacity, and improving safety and reliability of secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593566000005
    Figure 0007593566000005
  • Figure 0007593566000006
    Figure 0007593566000006
  • Figure 0007593566000007
    Figure 0007593566000007
Patent Text Reader

Abstract

To provide an electrolytic copper foil having high strength even when it is thin and having an improved drawing ratio.SOLUTION: An electrolytic copper foil comprises TOC (Total Organic Carbon) of 4 ppm or less, and Cl (chlorine) of 10 ppm or less, and is composed of a single layer or two or more laminates satisfying the following formula (1). Thickness (μm) / (Tensile strength (kgf / mm2)*Elongation ratio (%))≤0.1 (1)SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrolytic copper foil and a secondary battery using the same, and more particularly to an electrolytic copper foil having high strength with improved tensile strength and elongation at the same time, and a secondary battery using the same in which the loading level of a negative electrode active material is increased to improve reliability such as capacity efficiency and life characteristics, while at the same time improving safety such as three-dimensional compression characteristics. [Background technology]

[0002] Electrolytic copper foil is made in two processes: a foil manufacturing process in which copper foil is manufactured using electroplating, and a post-processing process in which functionality is added through surface treatment of the copper foil. Electrolytic copper foil has the advantage of being easier to control in thickness and physical properties than conventional copper foil, and is therefore used in a variety of applications, including as a base material for electronic devices such as printed circuit boards, or as a plate for secondary batteries.

[0003] Typically, electrolytic copper foil is produced in an electrolytic cell that contains a cylindrical titanium cathode (also called a drum), a lead alloy or iridium oxide-coated titanium anode that is spaced apart, an electrolyte, and a current source. The electrolyte is made of sulfuric acid and / or copper sulfate, and when a direct current is passed between the cathode and anode while the cylindrical cathode is rotated, copper is electrodeposited on the cathode, producing electrolytic copper foil continuously. This process of reducing copper ions to metal by electrolysis is called the foil-making process.

[0004] The copper foil obtained in the foil manufacturing process can be processed through additional post-treatment processes such as a nodule process to improve adhesion to the insulating substrate, a diffusion prevention process to prevent the diffusion of copper ions, an anti-rust process to prevent oxidation from the outside, and a chemical adhesion improvement process to complement adhesion to the insulating substrate, if necessary. If it goes through these post-treatment processes (surface treatment processes), it becomes copper foil for low-profile printed circuits, and if only the anti-rust treatment is performed during the surface treatment process, it can be used for secondary batteries.

[0005] Meanwhile, the strength of electrolytic copper foil can be controlled by controlling the substances that compose the electrolyte during the manufacturing process of electrolytic copper foil. In Japanese Patent No. 5588607 (August 1, 2014, Mitsui Mining & Smelting Co., Ltd.), the electrolyte contains excessive Cl, which reduces the elongation rate, causing problems. In Japanese Patent No. 5373970 (September 27, 2013, Mitsui Mining & Smelting Co., Ltd.), electrolytic copper foil is manufactured by adding iodine, which causes curling and reduces the elongation rate, causing problems. In Japanese Patent No. 5771392 (July 3, 2015, Nippon Denkai Co., Ltd.) and Japanese Patent No. 5595301 (August 15, 2014, Nippon Petroleum Metals Co., Ltd.), the tensile strength of electrolytic copper foil is improved by the composition of the additives added to the electrolyte, but the elongation rate is reduced and curling occurs, causing problems.

[0006] The electrolytic copper foil manufactured according to the above-mentioned Japanese patent has a Cl content of about 35 ppm or more in the electrolyte additive composition, and if the Cl content is 35 ppm or more, there is a problem that the electrode corrosion during continuous production due to excessive Cl and the physical property change due to it occurs, and continuous productivity decreases. In addition, the above-mentioned additive composition causes curling of the electrolytic copper foil, and when such electrolytic copper foil is used as a secondary battery electrode plate and active material is coated on the electrode plate, process failure occurs. In addition, the electrolytic copper foil has a thickness of 12 μm or more and an elongation rate of 3%, but if it is 10 μm or less, which is the thickness applied to actual secondary batteries, the elongation rate decreases, and when it is used in a secondary battery, the life and safety decrease, and there is a problem that process failure occurs frequently.

[0007] In order to improve this and provide an electrodeposited copper foil having a high elongation ratio and high strength even with a thin thickness, various studies are being conducted. Summary of the Invention [Problem to be solved by the invention]

[0008] An object of the present invention is to provide an electrolytic copper foil having high strength and improved elongation even at a thin thickness, which can overcome various drawbacks of the prior art, and a secondary battery using the same.

[0009] Another object of the present invention is to provide an electrolytic copper foil having an improved triaxial multidirectional elongation rate and a secondary battery using the same.

[0010] Another object of the present invention is to provide an electrolytic copper foil having an increased loading level of anode active material, an increased non-capacity, improved life characteristics, reliability and stability, and a secondary battery using the same.

[0011] Another object of the present invention is to provide an electrolytic copper foil that has high strength even in a thin thickness and is therefore used as wiring for PCBs, and a secondary battery using the same.

[0012] Another object of the present invention is to improve the three-dimensional compression characteristics of an electrolytic copper foil in order to enhance the impact resistance of a secondary battery. [Means for solving the problem]

[0013] According to one aspect of the present invention, there is provided an electrolytic copper foil having a TOC (Total Organic Carbon) of 4 ppm or less, a Cl (Chlorine) of 10 ppm or less, and composed of a single layer or a laminate of two or more layers, which satisfies the following formula (1):

[0014] Thickness (μm) / (tensile strength (kgf / mm 2 )*Stretching rate (%))≦0.1 (1)

[0015] The electrolytic copper foil has a thickness of 35 um or more and a breaking height of 3 mm or more as determined by an Erichsen test.

[0016] The tensile strength of the electrolytic copper foil is 45 kgf / mm 2The elongation ratio is 3% or more.

[0017] The electrolytic copper foil has a gloss (Gs(60°)) of 100 or more.

[0018] According to another aspect of the present invention, the present invention uses the above-mentioned electrolytic copper foil as a cathode current collector and applies a loading level of 1.0 g / cm 3 The present invention also includes a cathode for a lithium secondary battery, which is coated with the above-mentioned cathode active material.

[0019] According to another aspect of the present invention, there is provided a lithium secondary battery comprising: an electrode assembly including a cathode in which the above-mentioned electrolytic copper foil is used as a cathode current collector and a cathode active material is coated on the electrolytic copper foil; an anode electrically connected to the cathode and coated with a cathode active material including a lithium compound; and a separator interposed between the cathode and the anode; and the electrode assembly is housed in a battery case together with an electrolyte to form a lithium secondary battery.

[0020] According to another aspect of the present invention, there is provided a printed circuit board having the above-mentioned electrolytic copper foil on any one surface thereof. Effect of the Invention

[0021] According to the present invention as described above, it is possible to provide an electrolytic copper foil having high strength and improved elongation even at a thin thickness, which can overcome various drawbacks of the prior art, and a secondary battery using the same.

[0022] In addition, the present invention can provide an electrolytic copper foil having an improved triaxial multidirectional elongation rate and a secondary battery using the same.

[0023] In addition, according to the present invention, it is possible to provide an electrolytic copper foil and a secondary battery using the same, which have an increased loading level of a negative electrode active material, an increased non-capacity, improved life characteristics, reliability, and increased stability.

[0024] In addition, according to the present invention, it is possible to provide an electrolytic copper foil used as a PCB wiring having high electrical performance due to its high strength even in a thin thickness, and a secondary battery using the same.

[0025] In addition, the present invention can provide an electrolytic copper foil and a secondary battery using the same, which have improved safety in impact resistance tests of large-capacity secondary batteries. [Brief description of the drawings]

[0026] [Figure 1] FIG. 1 is a diagram showing a schematic diagram of an apparatus for performing a three-axis multi-directional test on a secondary battery. [Diagram 2] FIG. 1 is a diagram showing an outline of an Ericson test for an electrolytic copper foil. [Diagram 3] FIG. 2 is a schematic diagram for explaining TOC according to an embodiment of the present invention. [Figure 4] FIG. 4 is a schematic view illustrating an electrode assembly manufactured using an electrolytic copper foil for a secondary battery as a negative electrode current collector according to another embodiment of the present invention. [Diagram 5] FIG. 1 is a diagram showing an apparatus on which an Ericsson test according to the present embodiment was performed. [Figure 6] FIG. 1 is a diagram showing an apparatus on which an Ericsson test according to the present embodiment was performed. [Figure 7] 1 is a photograph showing the results of an Ericson test performed on an example and a comparative example with different numbers of overlapping (nested) sheets. [Figure 8] 7 is an enlarged photograph of Examples 3 and 4 and Comparative Example 2. It is a schematic diagram showing a state in which a second set of CBN particles is dispersed among a first set of CBN particles according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] Other embodiment details are included in the detailed description and drawings.

[0028] The advantages and features of the present invention, and the methods of achieving them, will become clear with reference to the embodiments described in detail below with the accompanying drawings. However, the present invention is not limited to the embodiments disclosed below, but can be embodied in various different forms, and in the following description, when some parts are connected to other parts, this includes not only the case where they are directly connected, but also the case where they are connected via another medium. In addition, in the drawings, parts that are not related to the present invention are omitted to clarify the description of the present invention, and similar parts are given the same reference numerals throughout the specification.

[0029] The present invention will now be described with reference to the accompanying drawings.

[0030] One embodiment of the present invention includes an electrolytic copper foil having a TOC of 4 ppm or less, a Cl (chlorine) of 10 ppm or less, and composed of a single layer or a laminate of two or more layers that satisfies the following formula (1):

[0031] Thickness (μm) / (tensile strength (kgf / mm 2 )*Stretching rate (%))≦0.1 (1)

[0032] The electrolytic copper foil manufactured by the electrolytic plating is laminated at least one layer to form an electrolytic copper foil assembly so that the electrolytic copper foil has a thickness of 35 μm or more, and the electrolytic copper foil assembly has a breaking height of 3 mm or more as determined by an Ericson test.

[0033] Recently, due to the trend of miniaturization and weight reduction of secondary batteries, the loading level of the negative electrode active material is increased for the high energy density of the secondary battery, while the demand for reducing the thickness of the negative electrode current collector is expanding due to the increase in the loading capacity. Meanwhile, there is a limit to the manufacturing of a high energy density negative electrode depending on the tensile strength, elongation rate, and toughness of the electrolytic copper foil of the existing negative electrode current collector. At this time, the types of negative electrode active materials include natural graphite, artificial graphite, hard carbon, soft carbon, SiAlloy, Sioxide, Si-C, Si, Sn metal layer, Li metal layer, etc.

[0034] In addition, the thickness of the electrolytic copper foil, which is the cathode current collector, is reduced, resulting in a decrease in toughness, which causes problems such as cracks and deformation of the cathode during the rolling process in the process of manufacturing the cathode. In addition, when a cathode manufactured to have excessive energy density is used in a secondary battery, there is a safety problem in that heat is generated due to an increase in internal resistance caused by the cracks and deformation of the cathode during reversible charging and discharging using the cathode manufactured at high density.

[0035] In the case of high energy density secondary batteries for automobiles, there are safety tests for compression and penetration, and such safety tests are greatly affected by the physical properties of the electrodeposited copper foil. Therefore, when measuring the elongation rate of the secondary battery, a safety test is performed in which the secondary battery is pulled in three directions, rather than the conventional uniaxial pulling test, and in the triaxial multidirectional test, the three-dimensional elongation rate acts as an important factor compared to the conventional one.

[0036] In the case of conventional electrolytic copper foil, when the loading level of the negative active material is increased due to its low tensile strength and toughness, deformation defects such as cracks and burrs occur. If the tensile strength is increased to solve this problem, defects occur during the multi-directional triaxial test of the secondary battery, which becomes a problem.

[0037] The electrolytic copper foil can be produced using the following electrolytic solution: The electrolytic solution may have a copper concentration of 60 to 120 g / L, a sulfuric acid concentration of 50 to 200 g / L, a chlorine concentration of 5 to 30 ppm, and a TOC concentration of 10 ppm or more, and further contains one or more additives selected from additive A, additive B, additive C, and additive D.

[0038] The additive A is at least one selected from the group consisting of thiourea compounds and compounds in which a thiol group is connected to a nitrogen-containing heterocycle, and the additive B is a sulfonic acid or a metal salt thereof of a compound containing a sulfur atom, including bis-(3-sulfopropyl)-disulfide disodium salt, 3-mercapto-1-propanesulfonic acid, 3-(N,N-dimethylthiocarbamoyl)-thiopropanesulfonic acid sodium salt, 3-[(amino-iminomethyl)thio]-1-propanesulfonic acid sodium salt, and o-ethyldithiocarbonate-S-(3-sulfopropyl)-ester sodium salt. The additive C is a sulfonic acid or a metal salt thereof of a compound containing a sulfur atom other than additive B, including thiourea and thiourea derivatives, including 2-mercapto-5-benzimidazolesulfonic acid, 3(5-mercapto-1H-tetrazolyl)benzenesulfonic acid, and 3-(benzothiazolyl-2-mercapto)-profile-sulfonic acid sodium salt. The additive D is a non-ionic water-soluble polymer, and examples of the non-ionic water-soluble polymer include adhesives, gelatin, polyethylene glycol, polypropylene glycol, starch, polymeric polysaccharides such as cellulose-based water-soluble polymers (such as carboxymethyl cellulose and hydroxyethyl cellulose), polyethyleneimine, polyacrylamide, and the like.

[0039] Examples of the thiourea and thiourea derivatives include water-soluble thiourea and thiourea derivatives such as thiourea (CH4N2S), N,N'-dimethylthiourea (C3H8N2S), N,N'-diethylthiourea (C5H12N2S), tetramethylthiourea (C5H12N2S), thiosemicaberbicide (CH5N3S), N-allylthiourea (C4H8N2S), and ethylenethiourea (C3H6N2S).

[0040] These additives A, B, C and D are not necessarily limited to these, and any additives that can be used as additives in the art can be used.

[0041] FIG. 1 is a schematic diagram showing an apparatus for carrying out a three-axis multi-directional test on a secondary battery, and FIG. 2 is a schematic diagram showing an Ericsson test on an electrolytic copper foil.

[0042] 1 and 2, the triaxial multi-directional test for the secondary battery can correspond to the Erickson test for the electrolytic copper foil. The electrolytic copper foil according to the embodiment of the present invention has an increased breaking height (breaking height) in the Erickson test corresponding to the triaxial multi-directional test, and the secondary battery to which the electrolytic copper foil according to the embodiment of the present invention is applied has improved strength and triaxial elongation rate in the triaxial multi-directional test, thereby increasing safety. The Ericksen test uses the B test method, which applies a wrinkle prevention force of 0.8066 KN, which is a non-standard test method for materials among the Ericksen tests specified in KSB0812 and ISO1520.

[0043] The electrolytic copper foil according to this embodiment is used as a cathode current collector constituting a cathode for a secondary battery. At this time, if the breaking height in the Erickson test is less than 3 mm, the secondary battery using the electrolytic copper foil as a cathode current collector has low tensile strength and triaxial elongation rate, which causes a problem in safety of the secondary battery. The Erickson test was performed based on KSB0812 and ISO8490.

[0044] 3 is a schematic diagram for explaining TOC described in the embodiment of the present invention. The TOC of the electrolytic copper foil inside the copper foil is 4 ppm or less, and Cl (chlorine) is 10 ppm or less.

[0045] Referring to FIG. 3, TOC is an abbreviation for Total Organic Carbon and is defined in the DIN EN1484 standard.

[0046] This is contained in the copper electrolyte and serves to reduce the size of the internal crystal grains of the electrolytic copper foil. If the copper electrolyte contains dissolved carbon dioxide (not TOC, but TIC (total organic carbon)), or if the battery is left at high temperature for a long time during vacuum drying in the battery manufacturing process, many additives present in the grains will diffuse to the grain boundaries, causing abnormal grain growth and changes in the crystal structure. In addition, the change in the physical properties of the electrolytic copper foil after vacuum drying changes the adhesion and stress with the negative electrode active material, causing detachment of the negative electrode active material and the occurrence of cracks during charging and discharging of the secondary battery.

[0047] Thus, the TOC forms impurities at the grain boundaries, suppressing abnormal grain growth and increasing tensile strength. On the other hand, if the TOC content in the electrolytic copper foil exceeds 4 ppm, the elongation rate decreases, and when a negative electrode active material is coated on the electrolytic copper foil, cracks may occur, or in the worst case, the electrolytic copper foil may break.

[0048] In addition, if the Cl content in the electrolytic copper foil exceeds 10 ppm, the cycle characteristics of the secondary battery using the electrolytic copper foil are deteriorated, and the formability in the Ericson test is deteriorated, causing a problem in the safety of the secondary battery. Preferably, when the TOC is 4 ppm or less and the Cl is 10 ppm or less, the electrolytic copper foil can be used as a negative electrode current collector having a high density, and the life characteristics and stability of the secondary battery are improved.

[0049] The electrolytic copper foil has a thickness of 2 μm to 35 μm, a TOC of 4 ppm or less, and a Cl (chlorine) of 10 ppm or less, and includes an electrolytic copper foil composed of a single layer or a laminate of two or more layers that satisfies the following formula (1):

[0050] Thickness (μm) / (tensile strength (kgf / mm 2 )*Stretching rate (%))≦0.1 (1)

[0051] If the thickness of the electrolytic copper foil is less than 2 μm, problems occur such as cracks or deformation during the process of coating the electrolytic copper foil with a negative electrode active material and rolling it, and problems such as sagging of the electrolytic copper foil occur during the process of coating the electrolytic copper foil with a negative electrode active material using a roll, making mass production difficult. On the other hand, if the thickness of the electrolytic copper foil exceeds 35 μm, when the electrolytic copper foil is used as a negative electrode current collector, the volume of the part not generating electric energy increases, reducing the unit capacity of the secondary battery.

[0052] In addition, the tensile strength and the elongation rate are provided depending on the thickness of the electrodeposited copper foil, but since there is a trade-off between their functions, it is preferable that the tensile strength and the elongation rate follow the formula (1). If the value of the formula (1) exceeds 0.1, the breaking height decreases during the Erickson test, which becomes a problem at the time of elongation rate of triaxial deformation.

[0053] The electrolytic copper foil has a tensile strength of 30 kgf / mm 2 The elongation ratio is 3% or more.

[0054] The tensile strength is 30kgf / mm 2 If the thickness is less than 100 μm, when the loading level of the negative electrode active material on the electrolytic copper foil is increased, problems such as deformation and burrs may occur.

[0055] In addition, if the elongation rate is less than 3%, when the electrolytic copper foil is coated with a negative electrode active material, problems such as cracks occurring in the electrolytic copper foil during rolling after coating the negative electrode active material may occur.

[0056] The electrolytic copper foil has a gloss (Gs(60°)) of 100 or more.

[0057] If the gloss (Gs(60°)) of the electrolytic copper foil is less than 100, the negative electrode active material is not uniformly coated due to the surface roughness of the electrolytic copper foil, which causes a problem.

[0058] The electrolytic copper foil includes a negative electrode current collector of a lithium secondary battery, and the loading level of the negative electrode active material coated on one side of the negative electrode current collector is 1.0 g / cm. 3 The thickness of the electrolytic copper foil excluding the negative electrode active material is 2 μm or more.

[0059] If the thickness of the electrolytic copper foil is less than 2 μm, it is not possible to stably support a high loading level of the negative electrode active material, and if the thickness exceeds 35 μm, the volume of the secondary battery is increased, making it difficult to manufacture a slim and compact secondary battery, and the specific capacity of the secondary battery is low, which is a problem. In addition, the loading level of the negative electrode active material may depend on the thickness of the electrolytic copper foil, and within the above-mentioned thickness range, the loading level of the negative electrode active material is preferably 1.0 g / cm or more. 3 In the above cases, electrical energy is generated efficiently while simultaneously maintaining safety.

[0060] According to another embodiment of the present invention, the present invention includes a secondary battery using the electrolytic copper foil described above. The secondary battery includes a cathode in which the electrolytic copper foil is used as a cathode current collector and an anode active material is coated on the electrolytic copper foil serving as the cathode current collector. The secondary battery is formed by housing an electrode assembly including the cathode, an anode electrically connected to the cathode and coated with an anode active material including a lithium compound, and a separator interposed between the cathode and the anode, and the electrode assembly together with an electrolyte in a battery case.

[0061] The present invention may include an electronic device using the secondary battery, and further includes a vehicle using the secondary battery.

[0062] According to another embodiment of the present invention, the present invention includes the above-mentioned electrolytic copper foil, a printed circuit board provided on one side of the electrolytic copper foil, and an electronic device using the printed circuit board according to the embodiment.

[0063] Hereinafter, another embodiment of the present invention will be described with reference to Fig. 4. Except for the following content, the content is the same as that described in the embodiment described with Figs. 1 to 3, so the details thereof will be omitted.

[0064] FIG. 4 is a schematic diagram illustrating an electrode assembly manufactured using an electrolytic copper foil for a secondary battery according to another embodiment of the present invention as a negative electrode current collector.

[0065] 4, the secondary battery according to the present embodiment is formed by using the above-mentioned electrolytic copper foil for secondary batteries as a cathode current collector, forming an electrode assembly 100 including a cathode 110 in which the electrolytic copper foil is coated with an anode active material, an anode 120 electrically connected to the cathode 110 and coated with an anode active material including a lithium compound, and a separator 130 interposed between the cathode 110 and the anode 120, and housing the electrode assembly 110 together with an electrolyte in a battery case. The loading level of the anode active material in the cathode is 1.0 g / cm. 3 The thickness of the electrolytic copper foil excluding the negative electrode active material is 2 μm or more.

[0066] Electrode tabs 111 and 122 are welded to the cathode 110 and anode 120, respectively, and are connected to electrode terminals provided in a battery case or function as electrode terminals themselves.

[0067] The positive electrode 120 is prepared by mixing a lithium compound, a conductive agent, a binder, and a solvent to prepare a positive electrode active material composition in the form of a slurry. The positive electrode active material composition is directly coated on an aluminum current collector, which is a positive electrode current collector, and dried to manufacture a positive electrode plate having a positive electrode active material formed thereon. In another method, the positive electrode active material composition is cast on a separate support, and a film obtained by peeling it off from the support is laminated on the aluminum current collector to manufacture a positive electrode 120 plate having a positive electrode active material formed thereon.

[0068] The negative electrode 110 is prepared as follows. The negative electrode 110 is prepared in the same manner as the positive electrode 120, except that a negative electrode active material is used. In addition, the conductive agent, binder, and solvent in the negative electrode active material composition may be the same as those in the positive electrode 120.

[0069] For example, a negative electrode active material, a conductive agent, a binder, and a solvent are mixed to prepare a negative electrode active material composition, which is then directly coated onto an electrolytic copper foil to prepare a negative electrode plate 110. In another method, the negative electrode active material composition is cast onto a separate support, and the negative electrode active material film peeled off from the support is laminated onto the electrolytic copper foil to prepare a negative electrode plate.

[0070] Next, a separator 130 is prepared to be inserted between the cathode 110 and the anode 120. Any separator that is generally used in lithium batteries can be used as the separator. A separator that has low resistance to the ion movement of the electrolyte and excellent electrolyte moisture absorption ability is used.

[0071] Next, an electrolyte solution is prepared. For example, the electrolyte solution may further include a small amount of additives in addition to the lithium salt in an organic electrolyte solution.

[0072] The cathode 110 and anode 120 are wound or folded with a separator 130 interposed therebetween, and are housed in a battery case. The battery case may be a rectangular or cylindrical can type, or may be in the form of a pouch.

[0073] The electrode assembly 100 consisting of the cathode 110, anode 120 and separator 130, together with the electrolyte and the battery case, may be any material that can be used as a secondary battery material in the art.

[0074] According to another aspect of the present invention, the present invention further includes an electronic device and an automobile using the above-mentioned secondary battery.

[0075] Hereinafter, examples and comparative examples of the present invention will be described. However, the following examples are only preferred examples of the present invention, and the scope of the present invention is not limited to the following examples.

[0076] 1. Manufacturing of electrolytic copper foil A copper substrate was placed in an electrolytic cell containing a copper sulfate electrolyte having the following composition to produce an electrolytic copper foil having a thickness as shown in Table 1.

[0077] (1)Copper sulfate electrolyte Copper concentration: 60~120g / L Sulfuric acid concentration: 50~200g / L Chlorine concentration: 5-30ppm TOC concentration: 10ppm or more (2) Electrolytic cell conditions Electrolyte temperature: 40℃ to 70℃ Current density: 20A / dm 2 ~100A / dm 2

[0078] [Table 1]

[0079] Additive A: N,N'-diethylthiourea Additive B: 3-mercapto-1-propanesulfonic acid Additive C: 3-(benzothiazolyl-2-mercapto)-propionyl-sulfonic acid sodium salt Additive D: Polyethylene glycol (M.W1000)

[0080] 2. Measurement of TOC and Cl content As shown in Table 1, 2.9 g of the prepared electrolytic copper foil was completely dissolved in a persulfuric acid coating solution, and then TOC and Cl were measured by ICP.

[0081] TOC was measured using a TOC-V instrument manufactured by Shimadzu Corporation, Japan, based on the DIN EN1484:1997 standard, and Cl concentration was measured using an ICS-1000 instrument manufactured by Dionex Corporation, Japan, based on the provisions of IPCTM650.

[0082] [Table 2]

[0083] 3. Ericsson test measurement The Erickson test was carried out using the apparatus shown in Figures 5 and 6. The Erickson test is the oldest and most widely used method for formability testing. The electrodeposited copper foil was prepared into a test piece, and each example was pressed with a punch to measure the breaking height (mm), which is the Erickson value until breakage. The measurement method and standards were performed with reference to KSB0812 and ISO8490.

[0084] (1) Test conditions Load: 10kN Punch movement speed: 10mm / min Spherical size: Φ20 (2) Erichsen test result: Method for measuring the breaking height Measurement of the height at which fracture occurs (see Figure 4)

[0085] 4. Compression test of secondary batteries The compression test of the secondary battery was conducted according to the JISC8714 standard.

[0086] [Table 3]

[0087] [Table 4]

[0088] FIG. 7 is a photograph showing the results of an Ericsson test performed on the examples and comparative examples with different numbers of overlapping (nested) sheets, and FIG. 8 is an enlarged photograph of Examples 3 and 4 and Comparative Example 2 in FIG.

[0089] With reference to the above-mentioned Examples and Comparative Examples, it was confirmed that Comparative Example 1, which has a thickness of 35 μm, had poorer results in the Ericson test than Examples 3 to 5, which have other thicknesses. Also, Comparative Example 2, even when the thickness was as thick as 50 μm, had poor results in the Ericson test, and also showed poor results in the battery compression test.

[0090] Those skilled in the art will understand that the present invention can be implemented in other specific forms without changing the technical idea or essential features of the present invention. Therefore, the above-described embodiments should be understood to be illustrative and not limiting in all respects. The scope of the present invention is defined by the claims below rather than the above detailed description, and all modifications and variations derived from the meaning and scope of the claims and their equivalent concepts should be interpreted as being included in the scope of the present invention.

[0091] Item 1: An electrolytic copper foil consisting of a single layer or a laminate of two or more layers, in which TOC is 4 ppm or less and Cl (chlorine) is 10 ppm or less, and which satisfies the following formula (1): Thickness (μm) / (tensile strength (kgf / mm 2 )*Stretching rate (%))≦0.1 (1) Item 2: The electrolytic copper foil according to item 1, characterized in that the electrolytic copper foil has a thickness of 35 μm or more and a breaking height determined by an Erickson test is 3 mm or more. Item 3: The tensile strength of the electrolytic copper foil is 45 kgf / mm 2 2. The electrolytic copper foil according to item 1, wherein the elongation is 3% or more. Item 4: The electrodeposited copper foil according to item 1, having a gloss (Gs(60 °)) of 100 or more. Item 5: The electrolytic copper foil according to any one of items 1 to 4 is used as a cathode current collector, and a loading level of 1.0 g / cm 3 A cathode for a lithium secondary battery, comprising the above-mentioned coated with an anode active material. Item 6: A cathode in which the electrodeposited copper foil according to any one of items 1 to 4 is used as a cathode current collector and a cathode active material is coated on the electrodeposited copper foil; a positive electrode electrically connected to the negative electrode and coated with a positive electrode active material including a lithium compound; an electrode assembly including a separator interposed between the cathode and the anode, A lithium secondary battery formed by housing a material together with an electrolyte in a battery case. Item 7: A printed circuit board, comprising the electrolytic copper foil according to any one of items 1 to 4 provided on one side thereof. [Explanation of symbols]

[0092] 100: Electrode assembly 110: Cathode 120: Anode 130: Separator

Claims

1. An electrolytic copper foil for a secondary battery, The electrolytic copper foil has a TOC content of 3 ppm or less, a chlorine (Cl) content of 4 ppm or less, a thickness of 2 μm to 35 μm, and a chlorine (Cl) content of 4 ppm or less. The electrolytic copper foil has a TOC content of 3 ppm or less, and a chlorine (Cl) content of 4 ppm or less. The electrolytic copper foil has a thickness of 2 μm to 35 μm, and the electrolytic copper foil has a TOC content of 3 ppm or less, Thickness (μm) / (tensile strength (kgf / mm 2 )*Stretching rate (%))≦0.1 (1) and when the electrodeposited copper foil is tested in an Ericson test, when the electrodeposited copper foil having a thickness of 2 μm to 35 μm is composed of a single layer or a laminate of two or more layers and has a thickness of 35 μm or more, the determined breaking height is 3 mm or more; The tensile strength of the electrolytic copper foil is 45 kgf / mm 2 or more, and the elongation rate of the copper foil is 3% or more, The electrolytic copper foil has a gloss (Gs(60°)) of 100 or more.

2. A negative electrode for a lithium secondary battery comprising a negative electrode current collector, the negative electrode current collector comprising the electrolytic copper foil according to claim 1, and a negative electrode active material having a density of 1.0 g / cm 3 The negative electrode for a lithium secondary battery is characterized in that the electrolytic copper foil is coated with the above loading level.

Citation Information

Patent Citations

  • Electrolytic copper foil, copper foil for current collector of secondary battery, and secondary battery

    JP2000182623A

  • Positive electrode for lithium secondary battery use, and lithium secondary battery

    JP2014093295A

  • Electrolytic copper foil, and electrical component and battery comprising the same

    JP2016160503A

  • Power storage device

    JP2017168302A

  • Method of recovering output of electricity storage element

    JP2017195059A