Photothermal conversion substrate, its manufacturing method, infrared sensor and reactive substrate using same

A nanostructured photothermal conversion substrate with independently arranged pillars addresses the inefficiencies of existing technologies by enhancing light absorption and heat retention, achieving higher conversion efficiency and temperature increases for infrared sensors and reactive substrates.

JP7593626B2Active Publication Date: 2024-12-03NAT INST FOR MATERIALS SCI
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2021027354
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-24
Publication Date
2024-12-03
Estimated Expiration
2041-02-24

AI Technical Summary

Technical Problem

Existing photothermal conversion technologies, such as those using titanium nitride nanoparticles and solar thermophotovoltaic devices, fail to achieve sufficient temperature increases under light irradiation, and infrared sensors lack structures that reduce thermal conductivity in the light-absorbing portion.

Method used

A photothermal conversion substrate with a nanostructure of independently arranged pillars on its surface, made from materials with a positive imaginary part of the complex dielectric constant, where the period of the pillars is less than twice the wavelength, and the ratio of pillar height to width is 0.5 or more, and the ratio of pillar width to period is 0.1 or more and less than 1, enhancing light absorption and heat retention.

Benefits of technology

The substrate efficiently converts light into heat with increased photothermal conversion efficiency, allowing for effective temperature increases and improved performance in infrared sensors and reactive substrates for thermochemical reactions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593626000004
    Figure 0007593626000004
  • Figure 0007593626000005
    Figure 0007593626000005
  • Figure 0007593626000006
    Figure 0007593626000006
Patent Text Reader

Abstract

To provide a substrate for photothermal conversion the photothermal conversion of which is increased, its manufacturing method, and an application using it.SOLUTION: A substrate for photothermal conversion according to the present invention that generates heat by irradiation of light is made from a material the imaginary part of the complex permittivity of which at a wavelength λ of the light is positive, has a nanostructure made of pillars that are located on the surface in a mutually independent manner, the period of the pillars is more than or equal to twice as much as the wavelength λ, a ratio of height of the pillar to width of the pillar is more than or equal to 0.5, and a ratio of the width of the pillar to a period of the pillar falls within a range between more than or equal to 0.1 and less than 1.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a photothermal conversion substrate, a method for producing the same, and an infrared sensor and a reactive substrate each using the same. [Background technology]

[0002] Solar energy is one of the most promising natural energies, and research into how to utilize it is being conducted around the world. One method of utilizing solar energy is photothermal conversion, which absorbs solar light and converts it into heat.

[0003] For example, titanium nitride (TiN) nanoparticles are used for photothermal conversion (see, for example, Patent Document 1). According to Non-Patent Document 1, because TiN nanoparticles have excellent photothermal conversion properties, it is suggested that adding TiN nanoparticles to wastewater or seawater could enable solar distillation, and adding TiN nanoparticles to water could enable solar water heaters.

[0004] For example, solar thermophotovoltaic (TPV) power generation devices that use sunlight as a heat source are known (see, for example, Patent Documents 2 and 3). In TPV power generation devices, a light-absorbing material with high light-to-heat conversion efficiency is used. Patent Document 2 discloses, as the light-absorbing material, tungsten, a tungsten-based alloy, molybdenum, or a molybdenum-based alloy having a large number of cavities that form a two-dimensionally arranged periodic fine surface unevenness pattern. Patent Document 3 discloses, as the light-absorbing material, a structure having microcavities using two different materials.

[0005] However, in either of the cavity structures of Patent Documents 2 and 3, it cannot be said that a sufficient temperature increase can be obtained by light irradiation, and further improvement is required.

[0006] Photothermal conversion also occurs with infrared light, and in fact, infrared sensors using bolometers, pyroelectrics, and thermopiles detect infrared light by converting it into heat. The light receiving parts of commercially available infrared sensors use materials that absorb infrared light over a wide band. An infrared sensor that combines a wavelength-selective microstructure and an infrared light detection material, as in Patent Document 4, has also been demonstrated as shown in Non-Patent Document 1. In either case, a structure that reduces the thermal conductivity of the light absorbing part has not been considered. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Patent No. 6587170 [Patent Document 2] JP 2003-332607 A [Patent Document 3] JP 2015-230831 A [Patent Document 4] Patent No. 6380899 [Non-patent literature]

[0008] [Non-Patent Document 1] Thang Duy Dao et al.,Adv.Sci.2019,6,1900579 Summary of the Invention [Problem to be solved by the invention]

[0009] In view of the above, an object of the present invention is to provide a photothermal conversion substrate having increased photothermal conversion efficiency, a manufacturing method thereof, and an infrared sensor and a reactive substrate each using the same. [Means for solving the problem]

[0010] The photothermal conversion substrate that generates heat when irradiated with light according to the present invention is made of a material whose imaginary part of complex dielectric constant at the wavelength λ of the light is positive, and has a nanostructure on its surface that is composed of pillars that are independent of each other, the period of the pillars is equal to or less than twice the wavelength λ, and the ratio of the height of the pillar to the width of the pillar is equal to or greater than 0.5; The ratio of the pillar width to the pillar period is in the range of 0.1 or more and less than 1, thereby solving the above problem. The ratio of the height of the pillar to the width of the pillar may be in the range 1.25 to 20 inclusive. The ratio of the height of the pillar to the width of the pillar may be in the range 2 to 20, inclusive. The ratio of the pillar width to the pillar period may be in the range 0.1 to 0.9. The ratio of the pillar width to the pillar period may be in the range 0.3 to 0.7. The period of the pillars may be equal to or less than the wavelength λ×1.1. The pillars may be rectangular or cylindrical. The pillar may be hollow. The material may be selected from the group consisting of semiconductors, transition metal nitrides, transition metal carbides, metal oxides, borides, organics, glasses, and graphite. The method for manufacturing the above-mentioned photothermal conversion substrate according to the present invention includes applying a photoresist to a substrate made of a material whose imaginary part of the complex dielectric constant at the wavelength λ of light is positive, patterning the substrate, and etching the patterned substrate, thereby solving the above-mentioned problem. The method for manufacturing the above-mentioned photothermal conversion substrate according to the present invention comprises applying a photoresist to a silicon substrate, patterning the photoresist, etching the patterned silicon substrate, depositing a material having a positive imaginary part of the complex dielectric constant at the wavelength λ of light on the etched silicon substrate, and etching the silicon substrate on which the material has been deposited, thereby solving the above-mentioned problem. The reactive substrate on the surface of which a thermochemical reaction occurs according to the present invention is the above-mentioned photothermal conversion substrate, thereby solving the above-mentioned problems. The thermochemical reaction may be a reaction selected from the group consisting of carbon monoxide detoxification, steam reforming of methane, and dry reforming. The infrared sensor comprising an infrared absorbing substrate and a temperature-sensitive resistance change film according to the present invention solves the above-mentioned problems, since the infrared absorbing substrate is the above-mentioned photothermal conversion substrate. Effect of the Invention

[0011] The photothermal conversion substrate that generates heat by irradiation with light according to the present invention is made of a material whose imaginary part of the complex dielectric constant at the wavelength λ of light is positive. This allows the light to be absorbed and converted into heat. Furthermore, the surface has a nanostructure consisting of pillars located independently of each other. Because of this nanostructure consisting of pillars, the effective thermal conductivity is low, and the irradiated part can be effectively heated. In particular, the pillar period is designed to be twice the wavelength λ or less, the ratio of the pillar height to the pillar width is 0.5 or more, and the ratio of the pillar width to the pillar period is designed to satisfy the range of 0.1 to less than 1, so that the absorbed light can be efficiently converted into heat, and the effective thermal conductivity is anisotropic, so that the heat retention effect is excellent. As a result, a photothermal conversion substrate with increased photothermal conversion efficiency can be provided.

[0012] By using such a photothermal conversion substrate, a reactive substrate can be provided for thermochemical reactions such as oxidation of carbon monoxide and generation of hydrogen from methane, utilizing the temperature rise caused by light irradiation. In addition, by providing a temperature-sensitive variable resistance film on the surface of the photothermal conversion substrate, a larger-area infrared sensor can be provided. [Brief description of the drawings]

[0013] [Figure 1] Schematic diagram showing a photothermal conversion substrate according to the present invention. [Diagram 2] A flowchart showing the steps of manufacturing the photothermal conversion substrate of the present invention. [Diagram 3]A flowchart showing another process for producing a photothermal conversion substrate of the present invention. [Figure 4] Schematic diagram showing an infrared sensor of the present invention. [Diagram 5] FIG. 1 is a schematic diagram showing a reactive chamber equipped with a reactive substrate of the present invention. [Figure 6] FIG. 1 is a schematic diagram showing a photothermal conversion substrate produced in Example 1. [Figure 7] FIG. 1 shows an SEM image of Sample 1-1 of Example 1. [Figure 8] FIG. 1 shows an SEM image of Sample 1-2 in Example 1. [Figure 9] FIG. 1 shows an SEM image of Sample 1-3 in Example 1. [Figure 10] FIG. 1 shows an SEM image of Sample 1-4 of Example 1. [Figure 11] FIG. 1 shows the relationship between laser intensity and surface temperature for Samples 1-1 to 1-4 in Example 1. [Figure 12] FIG. 1 shows the relationship between laser intensity and surface temperature for Samples 1-5 to 1-12 in Example 1. [Figure 13] FIG. 1 shows the results of various simulations of a silicon substrate having a nanostructure made of pillars according to Example 2. [Figure 14] FIG. 1A is a schematic diagram of a photothermal conversion substrate produced in Example 3, and FIG. 1B is a SEM image of a sample of Example 3. [Figure 15] FIG. 11 shows the relationship between laser intensity and surface temperature of the sample in Example 3. [Figure 16] FIG. 1 is a schematic diagram showing a photothermal conversion substrate produced in Example 4. [Figure 17] FIG. 1 shows an SEM image of Sample 4-1 of Example 4. [Figure 18] FIG. 1 shows an SEM image of Sample 4-2 of Example 4. [Figure 19] FIG. 1 shows an SEM image of Sample 4-3 of Example 4. [Figure 20] FIG. 13 is a diagram showing the relationship between the laser intensity and the surface temperature of Samples 4-1 to 4-3 in Example 4. [Figure 21] FIG. 13 shows the results of various simulations of a silicon substrate having a nanostructure made of holes according to Example 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. Note that like elements are given like reference numerals and their description will be omitted. (Embodiment 1) In the first embodiment, the photothermal conversion substrate and the manufacturing method of the present invention will be described in detail.

[0015] FIG. 1 is a schematic diagram showing a photothermal conversion substrate according to the present invention.

[0016] The photothermal conversion substrate 100 according to the present invention, which generates heat by irradiation with light, is made of a material whose imaginary part of the complex dielectric constant at the wavelength λ of light is positive, and has a nanostructure 120 consisting of pillars 110 positioned independently of each other on the surface, the period of the pillars 110 is not more than twice the wavelength λ, the ratio of the height of the pillars to the width of the pillars 110 is 0.5 or more, and the ratio of the width of the pillars to the period of the pillars is in the range of 0.1 or more and less than 1. The inventors of the present application have discovered that by forming a fine structure with a large aspect ratio (nanostructure 120 consisting of pillars 110), it is possible to achieve both high light absorption and low thermal conductivity, and that by making the pillars 110 satisfy the above-mentioned specific design, it is possible to increase the photothermal conversion efficiency. Each feature will be described in detail.

[0017] The photothermal conversion substrate 100 is made of a material whose complex dielectric constant at the wavelength λ of light has a positive imaginary part. The complex dielectric constant ε is expressed as follows. ε=ε1+iε2 Here, ε1 and ε2 are called the real and imaginary parts of the complex dielectric constant, respectively. In the above formula, the imaginary part ε2 is positive with respect to the wavelength λ of light, so that the material constituting the photothermal conversion substrate 100 can efficiently absorb the wavelength.

[0018] Such materials are preferably selected from the group consisting of semiconductors, transition metal nitrides, transition metal carbides, metal oxides, borides, organics, glasses, and graphite.

[0019] For example, when the incident light is visible light (wavelength 380 nm or more and 780 nm or less), a material that is visually opaque can be selected easily. Examples of such materials include a material selected from the group consisting of semiconductors such as silicon and InGaAs, transition metal nitrides such as titanium nitride, transition metal carbides such as titanium carbide, metal oxides such as iron oxide and copper oxide, borides such as lanthanum hexaboride, and graphite.

[0020] For example, when the incident light is far infrared (wavelength is greater than 5.0 μm and less than 10 μm), there are glasses such as borosilicate glass, fire glass, and quartz glass, or organic materials such as acrylic resins such as polymethyl methacrylate resin (PMMA) and epoxy resins. For example, when the incident light is ultraviolet (wavelength is greater than or equal to 200 nm and less than 380 nm), there are metals such as silver and chromium, semiconductors such as silicon and GaAs, and metal oxides such as titanium oxide and zinc oxide. Such materials can be selected according to the incident light. For reference, Table 1 shows the wavelength dependency of the imaginary part of the complex dielectric constant of various materials. A user can appropriately select a material whose imaginary part of the complex dielectric constant is positive for the desired wavelength λ of incident light. Note that Table 1 shows only an example of materials, and is not limited to this.

[0021] [Table 1]

[0022] The photothermal conversion substrate 100 has a nanostructure 120 consisting of pillars 110 on its surface. In this specification, the nanostructure refers to an assembly of pillars 110 arranged periodically. When the pillars 110 form a nanostructure, the thermal conductivity of the nanostructure becomes lower than the thermal conductivity of the material itself, and the heat generated by the absorption of light can be effectively retained. From this viewpoint, the pillars 110 are independent and do not contact each other. In this specification, the pillars 110 being arranged periodically does not necessarily have to have the same period for all the pillars 110. For example, when five pillars 110 are focused on, they may be periodic and satisfy the above condition.

[0023] The pillar 110 is not limited to the rectangular prism shown in Fig. 1, but may be a prismatic prism such as a triangular prism or a pentagonal prism, or a cylindrical prism such as a circular cylinder, a semi-circular cylinder, an elliptical cylinder, etc. The pillar 110 is not limited to one having no cavity inside as shown in Fig. 1, but may be hollow.

[0024] If the thermal conductivity of the material constituting the nanostructure 120 is k0, the photothermal conversion substrate 100 can be considered to be made of a composite material of a material with thermal conductivity k0 and the air between the pillars 110. In particular, by using the pillars 110, the effective thermal conductivity in the x direction and the y direction in Fig. 1 is the same in the photothermal conversion substrate 100, but only the thermal conductivity in the z direction in Fig. 1 can be made different. As a result, the thermal conductivity of the photothermal conversion substrate 100 has anisotropy, and the effective thermal conductivity in the x direction and the y direction in particular is extremely small compared to k0, so that the heat converted from the absorbed light can be efficiently retained.

[0025] In the photothermal conversion substrate 100, the period P of the pillars 110 satisfies the condition of being equal to or less than twice the wavelength λ (P≦λ×2). If the period P is P>λ×2, the effect of diffraction becomes large, making it difficult to obtain sufficient light absorption by the pillars 110. There is no particular limit to the lower limit of the period P, but if it is 50 nm or more, it is preferable because a pillar structure with a large aspect ratio can be fabricated by microfabrication. For example, when the incident light is visible light and near infrared light (up to 1 μm), the period P can preferably be 300 nm or more and 2 μm or less. Within this range, efficient photothermal conversion can be achieved. More preferably, the period P can be 300 nm or more and 1100 nm or less.

[0026] In the photothermal conversion substrate 100, the period P of the pillars 110 is preferably equal to or less than 1.1 times the wavelength λ (P≦λ×1.1), which increases the light absorptance of the pillars 110 and provides excellent photothermal conversion efficiency.

[0027] The ratio (H / W) of the height H of the pillars 110 to the width W of the pillars 110 is 0.5 or more, and the ratio (W / P) of the width W of the pillars 110 to the period P of the pillars 110 satisfies the range of 0.1 or more and less than 1. By satisfying such a specific design, the effective thermal conductivity of the nanostructure 120, particularly the x component and y component, becomes extremely small compared to the pillar material, and absorbed light can be efficiently converted into heat.

[0028] If the lower limit of the ratio (H / W) is less than 0.5, sufficient photothermal conversion does not occur. There is no upper limit to the ratio (H / W) as long as the nanostructure 120 can be manufactured. For example, when the wavelength λ of the incident light is in the terahertz range (wavelength of several hundred μm to several mm), the period P of the pillars 110 is also sufficiently large, and manufacturing is possible even with a ratio (H / W) of 200. Considering the yield, the upper limit of the ratio (H / W) should be 30 or less.

[0029] The ratio (H / W) preferably satisfies the range of 1.25 or more and 20 or less. Within this range, the light-to-heat conversion efficiency can be increased. The ratio (H / W) more preferably satisfies the range of 2 or more and 20 or less. Within this range, the light-to-heat conversion efficiency can be further increased. The ratio (H / W) even more preferably satisfies the range of 5 or more and 20 or less.

[0030] The ratio (W / P) preferably satisfies the range of 0.1 to 0.9 inclusive. Within this range, the light-to-heat conversion efficiency can be increased. The ratio (W / P) more preferably satisfies the range of 0.3 to 0.7 inclusive. Within this range, the probability of light being irradiated between the pillars 110 is reduced, and the effect of light absorption by the pillars 110 can be sufficiently obtained.

[0031] When the wavelength λ of light is, for example, 500 nm, the period (P) of the pillars 110 preferably satisfies the range of 300 nm or more and 1000 nm or less, and the width (W) of the pillars 110 preferably satisfies the range of 90 nm or more and 900 nm or less. This makes it easy to manufacture a photothermal conversion substrate 100 that satisfies the above ratio (H / W) and ratio (W / P). The width of the pillars 110 more preferably satisfies the range of 150 nm or more and 700 nm or less. This allows for good manufacturing yield while achieving the above effects.

[0032] The height (H) of the pillar 110 preferably falls within the range of 375 nm or more and 5000 nm or less. This makes it easy to manufacture a photothermal conversion substrate 100 that satisfies the above ratio (H / W) and ratio (W / P). The height of the pillar 110 more preferably falls within the range of 1000 nm or more and 3300 nm or less. This allows for good manufacturing yield while achieving the above effects.

[0033] Next, an exemplary process for manufacturing the photothermal conversion substrate 100 of the present invention will be described for silicon. FIG. 2 is a flow chart showing the steps of manufacturing the photothermal conversion substrate of the present invention.

[0034] It is known that the imaginary part of the complex dielectric constant of silicon is positive at wavelengths of approximately 1100 nm or less. Figure 2 shows the manufacturing process for obtaining a photothermal conversion substrate by etching silicon itself, and includes the following processes. Step S210: A resist 220 is applied to a silicon substrate 210, and then patterned. Step S220: Etch the patterned substrate.

[0035] In step S210, resist 220 is applied to substrate 210. Resist 220 is a composition whose solubility in a developer changes with light, electron beams, etc., and is available in negative and positive types. Here, it is assumed that the resist is a positive type electron beam resist, whose solubility in a developer increases with electron beam irradiation, and the irradiated portion is removed by development.

[0036] A pattern of squares arranged in a rectangular lattice is drawn on the resist 220, for example, by an electron beam lithography device, and when developed, only the irradiated parts irradiated with the electron beam are removed. Next, a metal film 230 of chromium, nickel, or the like is evaporated. The remaining resist is removed by ashing or with a remover appropriate for the resist. As a result, an etching mask 240 made of the metal film 230 arranged in a lattice is formed, and a patterned substrate is obtained. The lattice pattern includes polygonal patterns such as triangles and rectangles, and dot patterns, and the arrangement includes a hexagonal close-packed lattice.

[0037] In step S220, the substrate 210 is etched in the vertical (thickness) direction through the etching mask 240. For such etching, the Bosch method (gas chopping method), which is known as anisotropic etching in which etching and sidewall protection processes are alternately repeated, can be used. For the etching process, a sulfur fluoride-based gas such as sulfur hexafluoride (SF6) is used. For the sidewall protection process, a fluorocarbon-based gas such as CHF4 or C4F8 is used. Finally, the etching mask 240 made of the metal film 230 is removed with a stripping solution to obtain the photothermal conversion substrate 100.

[0038] Although an etching mask 240 made of a metal film 230 is used, the developed resist 220 may be used as the etching mask. Although the case of a silicon substrate 210 has been described, a substrate made of a material with a positive imaginary part of a complex dielectric constant that allows anisotropic etching, such as that typified by the Bosch method, may also be used.

[0039] FIG. 3 is a flow chart showing another process for producing a photothermal conversion substrate of the present invention.

[0040] FIG. 3 shows a manufacturing process for obtaining a photothermal conversion substrate by depositing a material whose imaginary part of the complex dielectric constant at wavelength λ is positive using a silicon substrate as a template, and the manufacturing process comprises the following steps. Step S310: A resist 320 is applied to a silicon substrate 310 and patterned. Step S320: Etch the patterned substrate 310. Step S330: Deposit a material 330 having a positive imaginary part of the complex dielectric constant at the wavelength λ on the etched substrate 310. Step S340: Etch the silicon substrate around the material 330.

[0041] Step S310 is the same as step S210 described with reference to FIG. 2, and therefore a description thereof will be omitted.

[0042] In step S320, the silicon substrate 310 is etched in the vertical direction through the etching mask. For such etching, anisotropic etching can be used as in step S220. The remaining photoresist is removed with a stripping solution or by ashing.

[0043] In step S330, a material 330 having a positive imaginary part of the complex dielectric constant at wavelength λ is deposited by physical vapor deposition or chemical vapor deposition using the etched silicon substrate 310 as a template. In FIG. 3, the material 330 is deposited so as to fill the holes (etched away portions) in the silicon substrate 310, but the material 330 can be made hollow by controlling the deposition time of the material 330. After the deposition process is completed, the uppermost surface of the material 330 is removed by etching. For such etching, dry etching using chlorine-based plasma, bromine-based plasma, or the like can be used.

[0044] In step S340, the silicon substrate 310 around the deposited material 330 is etched to obtain the photothermal conversion substrate 100. Again, anisotropic etching can be used for the etching, as in step S220.

[0045] The manufacturing processes in FIGS. 2 and 3 are merely examples, and the photothermal conversion substrate 100 of the present invention may be manufactured by appropriately adopting existing semiconductor manufacturing processes.

[0046] (Embodiment 2) In the second embodiment, applications of the photothermal conversion substrate of the present invention described in the first embodiment will be described.

[0047] FIG. 4 is a schematic diagram showing an infrared sensor of the present invention.

[0048] The bolometer type infrared sensor 400 includes an infrared absorbing substrate 410 and a temperature-sensitive variable resistance film 420. The infrared absorbing substrate 410 is the photothermal conversion substrate 100 described in the first embodiment, so a description thereof will be omitted, but it can convert incident light having a wavelength λ into heat when the light is infrared. The temperature-sensitive variable resistance film 420 is located on the infrared absorbing substrate 410, and is a thin film made of a known temperature-sensitive resistance material such as VO2, Ti, or amorphous silicon. The temperature-sensitive variable resistance film 420 is formed on the infrared absorbing substrate 410 by physical vapor deposition or chemical vapor deposition.

[0049] Although not shown, electrode wiring made of an electrically conductive material such as Ti or Al is provided on at least a part of the temperature-sensitive variable resistance film 420, and is electrically connected to the temperature-sensitive variable resistance film 420. The electrode wiring is connected to an external voltmeter or ammeter (not shown) so that a change in the resistance value of the temperature-sensitive variable resistance film 420 accompanying a change in temperature can be measured. Furthermore, the infrared absorbing substrate 410 may be located on and electrically connected to a semiconductor substrate equipped with an integrated circuit such as a CMOS detection circuit.

[0050] With this structure, when infrared rays are irradiated onto the infrared sensor 400, the infrared absorbing substrate 410 absorbs the infrared rays and converts them into heat. As described with reference to FIG. 1, the infrared absorbing substrate 410 has excellent light-to-heat conversion efficiency, and therefore can detect even a weak signal.

[0051] Conventional bolometer-type infrared sensors have a space between the substrate and the infrared absorbing film for thermal isolation. This makes it difficult to increase the area and vulnerable to external stimuli such as vibration. However, by using the infrared absorbing substrate 410, such a space for thermal isolation is not required, making it possible to increase the area and providing excellent rigidity.

[0052] FIG. 5 is a schematic diagram showing a reactive chamber equipped with a reactive substrate of the present invention.

[0053] The reactive substrate 510 of the present invention is the photothermal conversion substrate 100 described in the first embodiment, and therefore a detailed description is omitted, but here, for example, it is heated to a temperature of 200° C. or higher by irradiation with at least visible light (380 nm to 730 nm) and maintained at that temperature. Note that if the light intensity is weak and the temperature does not rise sufficiently, the light intensity can be increased by concentrating the light.

[0054] 5 shows a reactive substrate 510 placed in a reactive chamber 520 such as a quartz tube, into which carbon monoxide (CO) is introduced. A catalyst 530 such as platinum or nickel is applied to the reactive substrate 510.

[0055] As shown in Fig. 5, sunlight is irradiated onto the reactive substrate 510. When sunlight is irradiated onto the reactive substrate 510 through the reactive chamber 520, the reactive substrate 510 efficiently absorbs the sunlight and converts it into heat. Since the reactive substrate 510 has excellent light-to-heat conversion efficiency, the surface temperature is maintained at 200°C or higher. On the reactive substrate 510, carbon monoxide is converted into carbon dioxide and rendered harmless according to the following formula: CO+O2→CO2 In this way, by employing the reactive substrate 510 of the present invention, it is possible to cause a thermochemical reaction using only clean energy such as sunlight, without the need for external power.

[0056] 5 shows an example in which carbon monoxide is converted into carbon dioxide, but the present invention is not limited to this. For example, it goes without saying that steam reforming or dry reforming of methane is also possible.

[0057] The present invention will now be described in detail with reference to specific examples, but it should be noted that the present invention is not limited to these examples. EXAMPLES

[0058] [Example 1] In Example 1, samples 1-1 to 1-12, which are diagrammatically shown in FIG. 6, were manufactured using silicon substrates, and changes in surface temperature upon irradiation with laser light were examined. FIG. 6 is a diagram showing a schematic diagram of the photothermal conversion substrate produced in Example 1. As shown in FIG.

[0059] A silicon substrate (0.38 mm thick) was coated with a resist for electron beam lithography (ZEP A520, Zeon Corporation) by spin coating (Mikasa Corporation, Spin Coater MS-B100). A pattern in which squares of various sizes and periods were arranged on a square lattice was drawn and developed using an electron beam lithography device (Elionix Corporation, ELS-7500EX). Next, metal films were deposited in the order of chromium (5 nm) and nickel (100 nm) using an electron beam evaporator (ULVAC, Inc., UEP-300-2C). The resist was removed using Remover PG (KAYAKU ADVANCED MATERIALS), and the silicon was excavated to a specified depth using the Bosch process. SF6 gas and CH4 gas were used for the Bosch process. Finally, the silicon substrate was immersed in a chromium etching solution to remove the metal film. Table 2 shows a list of the samples 1-1 to 1-12 that were produced.

[0060] [Table 2]

[0061] The obtained samples were observed with a scanning electron microscope (SEM, Hitachi High-Tech Corporation, SU8230). The observation results are shown in Figures 7 to 10. Using a micro-Raman spectrometer (Photon Design Corporation, Jupiter) with a laser light wavelength of 514 nm, the obtained samples were irradiated with laser light of various intensities, and the Raman spectrum at that time was measured. -1 The surface temperature was calculated from the peak shift of the peak near the center frequency of about 520 cm. The silicon substrate was heated on a temperature-controlled stage, and the Raman spectrum was measured at each temperature. -1 The relationship between the peak shift and temperature was obtained by plotting the peak position against the temperature. The results are shown in Figures 11 and 12.

[0062] FIG. 7 is a diagram showing an SEM image of Sample 1-1 in Example 1. FIG. 8 is a diagram showing an SEM image of Sample 1-2 in Example 1. FIG. 9 is a diagram showing an SEM image of Sample 1-3 in Example 1. FIG. 10 is a diagram showing an SEM image of Sample 1-4 in Example 1.

[0063] 7 to 10, it was confirmed that Samples 1-1 to 1-4 have a nanostructure consisting of rectangular pillars on the surface of a silicon substrate, and have the period P and pillar width D listed in Table 2. In addition, it was confirmed by an SEM image taken from a different angle that the height H of the pillars in Samples 1-1 to 1-4 is the size listed in Table 2. Although not shown, it was also confirmed that Samples 1-5 to 1-12 have a nanostructure consisting of pillars listed in Table 2. It was confirmed that the imaginary part of the complex dielectric constant of silicon is 0.52 at a wavelength of 514 nm, which is a positive value.

[0064] FIG. 11 is a diagram showing the relationship between the laser intensity and the surface temperature for Samples 1-1 to 1-4 in Example 1. As shown in FIG. FIG. 12 is a diagram showing the relationship between the laser intensity and the surface temperature for Samples 1-5 to 1-12 in Example 1.

[0065] Figures 11 and 12 also show the relationship between the laser intensity and the surface temperature of a flat silicon substrate without a nanostructure. Note that the surface temperature values ​​do not match between Figures 11 and 12 because the thickness of the silicon substrate is different. Figures 11 and 12 show that the photothermal conversion efficiency is increased by having a nanostructure made of pillars on the surface of a material whose imaginary part of the complex dielectric constant is positive for the incident wavelength, compared to a flat surface.

[0066] FIG. 12 shows that, if the period P and pillar width W are constant, the light-to-heat conversion efficiency increases when the ratio (P / W) is 1.25 or more, and further increases when it is 5 or more.

[0067] [Example 2] In Example 2, in the photothermal conversion substrate shown in Figure 6 using a silicon substrate, electromagnetic field calculations based on the finite element method were used to investigate the dependence of the light absorptance, the x and z components of the thermal conductivity, and the surface temperature on the pillar width / height.

[0068] First, the light absorption rate of the pillar was calculated by electromagnetic field calculation based on the finite element method. Next, a temperature difference was applied to each of the pillars in the nanostructure in the x, y, and z directions, respectively, and the heat conduction equation was solved by the finite element method to obtain the x, y, and z components of the effective thermal conductivity (k x ,k y ,k z ) was obtained (effective medium approximation). In the structure of Fig. 6, the effective thermal conductivity has uniaxial anisotropy, so k x =k y ≠k z It becomes.

[0069] Here, the wavelength of the incident light was set to 514 nm, and parameters such as the pillar period P (400 nm), height H (3200 nm), and laser light intensity were input, and heat transfer calculations were performed using the optical absorptivity and effective thermal conductivity calculated above to obtain the surface temperature of the pillar when irradiated with laser light. These results are shown in Figure 13.

[0070] FIG. 13 shows the results of various simulations on a silicon substrate having a nanostructure consisting of pillars according to Example 2. 13A to 13C show the results when the pillar pitch P is 400 nm, the pillar height H is 3200 nm, and the pillar width W is changed from 20 nm to 380 nm. Fig. 13D shows the result when the pillar pitch P is 400 nm, the pillar width W is 80 nm, and the pillar height H is changed from 1 μm to 46 μm.

[0071] Figure 13(A) shows that the light absorption rate first decreases or increases sharply as the pillar width increases, and then decreases monotonically. Figure 13(B) shows that the effective thermal conductivity decreases as the pillar width decreases for both the x and z components. Figures 13(C) and (D) show that the surface temperature of the light irradiated area changes dramatically depending on the width and height of the pillar. In detail, the surface temperature of the light irradiated area became higher as the pillar width became smaller and the pillar height became higher.

[0072] This also demonstrated that a substrate made of a material with a positive imaginary part of the complex dielectric constant at the wavelength λ of light, having a nanostructure consisting of pillars on its surface, with a pillar period that is less than twice the wavelength λ, a ratio of the pillar height to the pillar width that is 0.5 or more, and a ratio of the pillar width to the pillar period that is in the range of 0.1 or more and less than 1, can function as a photothermal conversion substrate that absorbs light and efficiently converts it into heat.

[0073] [Example 3] In Example 3, titanium nitride (TiN) was used to manufacture Sample 3, which is diagrammatically shown in FIG. 14(A), and the change in surface temperature when irradiated with laser light was examined.

[0074] FIG. 14 is a diagram (A) showing a schematic diagram of the photothermal conversion substrate produced in Example 3, and a diagram (B) showing an SEM image of the sample in Example 3.

[0075] As deep ultraviolet (DUV) resist, anti-reflective film BARC (DUV42S-6) and positive resist (KRF230Y) were applied to a silicon substrate (600 μm thick) by spin coating. The thicknesses of BARC and resist were 65 nm and 360 nm, respectively.

[0076] A circular pattern (diameter 265 nm) was exposed using a DUV stepper (Canon Inc., FPA-3000EX4) and developed with tetramethylammonium hydroxide (TMAH). The silicon was etched to a depth of 2360 nm using the Bosch process. SF6 gas and CH4 gas were used for the Bosch process. The remaining resist was removed with acetone. In this way, a silicon substrate template with holes was obtained.

[0077] Next, a TiN film was deposited in the holes of the silicon substrate using an atomic layer deposition system (R-200 Advanced Plasma ALD, Picosun). TiCl4 and NH3 were used as precursors, and the film was deposited to a thickness of 90 nm at a film formation temperature of 500°C. The silicon substrate with the TiN film was placed in an annealing furnace (PEO-604, ATV Technologie) and heat-treated at 900°C for 1 hour while flowing N2. This improved the crystallinity of the TiN film. The TiN film on the top surface of the silicon substrate was removed by dry etching using chlorine-based plasma.

[0078] Next, the silicon holes were etched by dry etching using SF6 gas. In this way, a nanostructure consisting of TiN film pillars with a height H of 2360 nm, a period P of 400 nm, and a diameter (width) W of 265 nm was obtained, as shown in Figure 14(B). The pillars were hollow and had a wall thickness of 88 nm. The imaginary part of the complex dielectric constant of TiN was confirmed to be 7.65 at a wavelength of 785 nm, which is a positive value.

[0079] Using a micro-Raman spectrometer (WITec, α300), the sample of Example 3 was irradiated with laser light of various intensities, and the Raman spectrum was measured. -1 The relationship between the laser intensity and the surface temperature was obtained from the peak shift of the peak near the surface. The laser light irradiation conditions were a laser light wavelength of 785 nm and a laser intensity after the objective lens of 0.5 mW to 30 mW. The results are shown in Figure 15.

[0080] FIG. 15 is a diagram showing the relationship between the laser intensity and the surface temperature of the sample of Example 3.

[0081] For comparison, Fig. 15 also shows the relationship between the laser intensity and the surface temperature of a flat silicon substrate without a nanostructure. Fig. 15 shows that by having a nanostructure consisting of hollow pillars on the surface of a material whose imaginary part of the complex dielectric constant is positive for the incident wavelength, the temperature rise due to photothermal conversion is increased by about 100 times compared to a flat surface. Furthermore, Examples 1 to 3 show that the material constituting the photothermal conversion substrate of the present invention only needs to have a positive imaginary part of the complex dielectric constant at the wavelength λ of light.

[0082] [Example 4] In Example 4, samples 4-1 to 4-3, which are diagrammatically shown in FIG. 16, were manufactured using silicon substrates, and changes in surface temperature upon irradiation with laser light were examined. FIG. 16 is a diagram illustrating the photothermal conversion substrate produced in Example 4. As shown in FIG.

[0083] Example 4 is different from Examples 1 to 3 in that it has holes instead of pillars. A resist for electron beam lithography (ZEP A520, manufactured by Zeon Corporation) was applied to a silicon substrate (0.38 mm thick) by spin coating (Mikasa Corporation, spin coater MS-B100XCj). Square lattices of various sizes were drawn and developed using an electron beam lithography device (Elionix, model number ELS-7500EX). Next, metal films were deposited in the order of chromium (5 nm) and nickel (100 nm) using an electron beam evaporator (ULVAC, model number UEP-300-2C). The resist was removed using Remover PG (KAYAKU ADVANCED MATERIALS), and the silicon was excavated to a specified depth by the Bosch process. SF6 gas and CH4 gas were used for the Bosch process. Finally, the silicon substrate was immersed in a chromium etching solution to remove the metal film. In this way, a silicon substrate template having holes was obtained. Table 3 shows a list of the produced samples 4-1 to 4-3.

[0084] [Table 3]

[0085] The obtained sample was observed with an SEM to determine the peak shift of the Raman spectrum, and the relationship between the laser intensity and the surface temperature was examined in the same manner as in Example 1. The results are shown in FIGS.

[0086] FIG. 17 is a diagram showing an SEM image of Sample 4-1 in Example 4. FIG. 18 is a diagram showing an SEM image of Sample 4-2 in Example 4. FIG. 19 is a diagram showing an SEM image of Sample 4-3 in Example 4.

[0087] 17 to 19, it was confirmed that Samples 4-1 to 4-3 had a nanostructure made of holes in a silicon substrate, and had the period P and hole width D listed in Table 3.

[0088] FIG. 20 is a diagram showing the relationship between the laser intensity and the surface temperature for Samples 4-1 to 4-3 in Example 4.

[0089] The relationship between the laser intensity and the surface temperature of a flat silicon substrate without a nanostructure is also shown in Fig. 20. According to Fig. 20, when the nanostructure is a hole, no significant increase in the photothermal conversion efficiency was observed.

[0090] [Example 5] In Example 5, in the photothermal conversion substrate shown in FIG. 16 using a silicon substrate, the optical absorptivity, the x and z components of the thermal conductivity, and the hole width dependency of the surface temperature were investigated using electromagnetic field calculations based on the finite element method.

[0091] As in Example 2, the optical absorption rate of the holes was calculated by electromagnetic field calculation based on the finite element method. Next, a temperature difference was applied in the x, y, and z directions for one period of holes in the nanostructure, and the heat conduction equation was solved by the finite element method to obtain the x, y, and z components of the effective thermal conductivity (k x ,k y ,k z) was obtained (effective medium approximation). In the structure of FIG. 16, the effective thermal conductivity has uniaxial anisotropy, so as in Example 2, k x =k y ≠k z It becomes.

[0092] Here, the wavelength of the incident light was set to 514 nm, and parameters such as the hole period P (400 nm), height H (3200 nm), and laser light intensity were input, and heat transfer calculations were performed using the optical absorptivity and effective thermal conductivity calculated above to determine the surface temperature of the holes when irradiated with laser light. These results are shown in Figure 21.

[0093] FIG. 21 shows the results of various simulations on a silicon substrate having a nanostructure consisting of holes according to Example 5.

[0094] Figures 21(A) to (C) show the results when the hole period P is 400 nm, the hole height H is 3200 nm, and the hole width W is changed from 20 nm to 380 nm. Figure 21(A) shows that the light absorption rate increases as the hole width increases, and decreases when the hole width exceeds 340 nm. Figure 21(B) shows that the effective thermal conductivity decreases as the hole width increases in both x and z components. Figure 21(C) shows that the surface temperature of the light irradiated part increases as the hole width increases, but does not increase as much as the pillar structure with a small pillar width shown in Example 2.

[0095] Examples 2 and 5 show that even when using the same silicon substrate, the characteristics of the light-to-heat conversion efficiency are significantly different between a cavity structure (hole) as typified by Patent Documents 2 and 3 and a nanostructure consisting of pillars. [Industrial Applicability]

[0096] The photothermal conversion substrate of the present invention has high photothermal conversion efficiency, and therefore can provide, for example, an infrared sensor in the infrared region, and a reactive substrate that uses sunlight in the visible / near infrared region. [Explanation of symbols]

[0097] 100 Photothermal conversion substrate 110 Pillar 120 Nanostructures 210 Substrate 220, 320 Photoresist 230 Metal Film 240 Etching Mask 310 Silicon substrate 330 Materials with a positive imaginary part of the complex dielectric constant at wavelength λ 400 Infrared Sensor 410 Infrared absorbing substrate 420 Temperature-sensitive resistance change film 510 Reactive Substrates 520 Reactive Chamber 530 Catalyst

Claims

1. A photothermal conversion substrate that generates heat when irradiated with light, The material is made of a material having a positive imaginary part of a complex dielectric constant at a wavelength λ of the light, The surface has a nanostructure consisting of independent pillars, the period of the pillars is equal to or less than twice the wavelength λ; a ratio of the height of the pillar to the width of the pillar is greater than or equal to 5 and less than or equal to 20; A photothermal conversion substrate, wherein a ratio of the width of the pillars to the period of the pillars is in the range of 0.3 to 0.

7.

2. A photothermal conversion substrate as described in claim 1, wherein the ratio of the height of the pillar to the width of the pillar is 15 or less.

3. A photothermal conversion substrate as described in claim 1 or 2, wherein the ratio of the pillar width to the pillar period is in the range of 0.6 or less.

4. 4. The photothermal conversion substrate according to claim 1, wherein the period of the pillars is equal to or less than the wavelength λ×1.

1.

5. 5. The photothermal conversion substrate according to claim 1, wherein the pillar is a rectangular column or a cylindrical column.

6. The photothermal conversion substrate according to claim 5 , wherein the pillar is hollow.

7. 7. The photothermal conversion substrate according to claim 1, wherein the material is selected from the group consisting of semiconductors, transition metal nitrides, transition metal carbides, metal oxides, borides, organic materials, glass, and graphite.

8. A method for producing the photothermal conversion substrate according to any one of claims 1 to 7, comprising the steps of: Applying a photoresist to a substrate made of a material having a positive imaginary part of a complex dielectric constant at a wavelength λ of light, and patterning the photoresist; Etching the patterned substrate. The method includes:

9. A method for producing the photothermal conversion substrate according to any one of claims 1 to 7, comprising the steps of: Applying a photoresist to a silicon substrate and patterning it; Etching the patterned silicon substrate; depositing a material on the etched silicon substrate, the material having a positive imaginary part of its complex dielectric constant at a wavelength λ of light; Etching the silicon substrate on which the material is deposited; The method includes:

10. A reactive substrate for performing a thermochemical reaction on a surface thereof, comprising: The reactive substrate is a photothermal conversion substrate according to any one of claims 1 to 7.

11. 11. The reactive substrate of claim 10, wherein the thermochemical reaction is a reaction selected from the group consisting of carbon monoxide detoxification, steam reforming of methane, and dry reforming.

12. An infrared sensor including an infrared absorbing substrate and a temperature-sensitive variable resistance film, 8. An infrared sensor, wherein the infrared absorbing substrate is a photothermal conversion substrate according to claim 1.

Citation Information

Patent Citations

  • Treatment of waste water by activated sludge

    JP1988080899A

  • Wavelength selective solar light absorbing material and its manufacturing method

    JP2003332607A

  • Thermal infrared detection element

    JP2006226891A

  • Thermal infrared sensor, and method for manufacturing the same

    JP2010210293A

  • Carbon monoxide oxidation catalyst and method for producing the same

    JP2013208621A