Suppression of neck-in in tubular LDPE-based polymers for extrusion coating at medium and high line speeds.

A polymer blend of LDPE and ethylene acrylate copolymer addresses the challenge of high neck-in and low drawdown in extrusion coating, enabling efficient production with reduced material waste and increased throughput.

JP7593991B2Active Publication Date: 2024-12-03DOW GLOBAL TECHNOLOGIES LLC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022504158
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-31
Filing Date
2020-07-24
Publication Date
2024-12-03
Estimated Expiration
2040-07-24

AI Technical Summary

Technical Problem

Existing extrusion coating processes face challenges in achieving low neck-in values and high drawdown at medium to high linear speeds, particularly with tubular LDPE polymers, leading to material waste and limited throughput.

Method used

A polymer blend comprising at least 90% by weight low density polyethylene (LDPE) and 1% to 10% by weight ethylene acrylate copolymer, with specific monomer compositions, is developed to enhance processability and reduce neck-in while maintaining high drawdown.

Benefits of technology

The polymer blend achieves neck-in values of less than 100 mm at linear speeds up to 500 m/min, improving dimensional stability and allowing high throughput in extrusion coating applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593991000001
    Figure 0007593991000001
  • Figure 0007593991000002
    Figure 0007593991000002
  • Figure 0007593991000003
    Figure 0007593991000003
Patent Text Reader

Abstract

An embodiment of the present disclosure includes a polymer blend comprising at least 90% by weight of a low-density polyethylene (LDPE) polymer and 1% to 10% by weight of an ethylene acrylate copolymer, the ethylene acrylate copolymer being the polymerization reaction product of at least 50% by weight of ethylene, based on the total weight of monomers present in the ethylene acrylate copolymer, 2 to 40% by weight of an alkyl acrylate, based on the total weight of monomers present in the ethylene acrylate copolymer, and 0 to 20% by weight of a monocarboxylic acid monomer, based on the total weight of monomers present in the ethylene acrylate copolymer.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to U.S. Provisional Patent Application No. 62 / 880,832, filed July 31, 2019, the entire disclosure of which is incorporated herein by reference.

[0002] Embodiments of the present disclosure relate generally to extrusion coating applications, where the extrusion coating comprises a polymer blend having low neck-in values ​​at low to high line speeds. [Background technology]

[0003] Extrusion coating is a continuous manufacturing process in which a polymer is melt processed and extruded through a die to form a thin film that is coated onto a substrate or as a tie layer between two substrates. Processability is important for extrusion coating, and there are two important parameters in extrusion coating: neck-in and draw-down. Neck-in is the contraction of the polymer film between the die exit and the coating substrate (i.e. during the air gap) and is considered a source of material waste. Draw-down refers to how fast the coating line can be run and how thin the polymer film can be stretched. A suitable polymer for extrusion coating must have low neck-in (to minimize polymer waste) and high / sufficient draw-down (to obtain thin coatings and high throughput).

[0004] Low density polyethylene (LDPE) polymers are branched polyethylenes with high melt strength. The high melt strength of the polymer provides good processability for extrusion coating. Neck-in and draw-down depend on the properties of the polymer. For example, LDPE polymers with higher melt indexes generally have more neck-in but higher draw-down. LDPEs with lower melt indexes tend to have lower neck-in and lower draw-down. For a given equipment, a lower neck-in and sufficient / higher draw-down is usually preferred.

[0005] The melt index and melt strength of LDPE polymers can be affected by the reactor used to produce the polymer. Polymerization conditions such as temperature, pressure, and polymer concentration vary widely in tubular reactor systems, but tend to be more uniform than autoclave reactor systems. Polymerization conditions in tubular reactors result in polymer compositions with lower molecular weights and / or increased short chain branching levels in the low molecular weight fraction, which can make the polymer more processable. Tubular LDPE polymers tend to have higher drawdowns due to faster line speeds and thinner coating thicknesses. In contrast, autoclave processes typically produce polymers with higher molecular weight fractions. In general, autoclave LDPE has lower neck-in values ​​because the polymers are more branched and have a broader molecular weight distribution (MWD). This allows autoclave LDPE polymers to have more entanglements of the polymer to "resist" shrinkage. Autoclave LDPE tends to have lower neck-in than tubular LDPE. Generally, tubular LDPE has a low melt index (4-5 MI) and autoclave LDPE has a high melt index (7-8 MI). Lower melt index tubular LDPE usually has greater neck-in values ​​and faster drawdown than the higher melt index autoclave LDPE polymers.

[0006] Polyethylene resins for extrusion coating on paper, board, aluminum, and a variety of other materials are typically processed at elevated temperature conditions, e.g., 270°C to 350°C, and medium to high extrusion line speeds (e.g., 300 m / min to 800 m / min). These resins may be low density polyethylene (LDPE) polymers. In general, however, autoclaved LDPE polymers tend to have lower neck-in, while tubular LDPE tends to be more shear thinning and can be processed at higher line speeds and thinner coating thicknesses. Summary of the Invention

[0007] There is a continuing need to create polymer blends that have low neck-in and are processable at high extrusion line speeds. An embodiment of the present disclosure includes a polymer blend comprising at least 90% by weight of a low density polyethylene (LDPE) polymer and 1% to 10% by weight of an ethylene acrylate copolymer. The ethylene acrylate copolymer is the polymerization reaction product of at least 50% by weight of ethylene, based on the total weight of monomers present in the ethylene acrylate copolymer, 2 to 40% by weight of an alkyl acrylate, based on the total weight of monomers present in the ethylene acrylate copolymer, and 0 to 20% by weight of a monocarboxylic acid monomer, based on the total weight of monomers present in the ethylene acrylate copolymer.

[0008] An embodiment of the present disclosure includes a coated polymeric substrate comprising a polymeric substrate, a coating comprising a polymer blend of the present disclosure, and a tie layer disposed between the polymeric substrate and the coating. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] In one or more embodiments of the present disclosure, the polymer blend comprises at least 90% by weight of a low density polyethylene (LDPE) polymer and 1% to 10% by weight of an ethylene acrylate copolymer. The polymer blend comprises at least 90% by weight of a low density polyethylene (LDPE) polymer and an ethylene acrylate copolymer in an amount of 1% to 8%, 1% to 5%, or 1% to 3% by weight.

[0010] In some embodiments of the polymer blend, the LDPE polymer is a tubular reactor produced polymer. The LDPE polymer can have a density of 0.910 g / cc to 0.930 g / cc. In some embodiments, the LDPE polymer can have a density of 0.910 g / cc to 0.920 g / cc, 0.916 g / cc to 0.930 g / cc, 0.918 g / cc to 0.926 g / cc, or 0.915 g / cc to 0.920 g / cc.

[0011] In some embodiments of the polymer blend, the LDPE polymer has a melt index (I2) of 2 g / 10 min to 8 g / 10 min as determined according to ASTM D 1238 (190° C., 2.16 kg). In various embodiments, the LDPE polymer has a melt index (I2) of 2 g / 10 min to 7.7 g / 10 min, 2 g / 10 min to 6 g / 10 min, 2 g / 10 min to 5 g / 10 min, or 2 g / 10 min to 4.5 g / 10 min.

[0012] In one or more embodiments of the polymer blend, the LDPE polymer has a molecular weight distribution (MWD=Mw / Mn) of 5 to 11, 8 to 10.5, or 8.5 to 11, as determined by conventional gel permeation chromatography (GPC) methods.

[0013] In one or more embodiments of the polymer blend, the ethylene acrylate copolymer is the polymerization reaction product of at least 50 weight percent ethylene, based on the total weight of monomers present in the ethylene acrylate copolymer, from 2 to 40 weight percent alkyl acrylate, based on the total weight of monomers present in the ethylene acrylate copolymer, and from 0 to 20 weight percent monocarboxylic acid monomer, based on the total weight of monomers present in the ethylene acrylate copolymer.

[0014] In various embodiments of the polymer blend, the ethylene acrylate copolymer comprises at least 50% by weight ethylene, based on the total weight of monomers present in the ethylene acrylate copolymer, and 10% to 30% by weight alkyl acrylate, based on the total weight of monomers present in the ethylene acrylate copolymer. In one or more embodiments, the ethylene acrylate copolymer comprises 15% to 30% by weight alkyl acrylate, based on the total weight of monomers present in the ethylene acrylate copolymer. In some embodiments, the ethylene acrylate copolymer comprises at least 75% by weight ethylene and 12% to 25% by weight alkyl acrylate, based on the total weight of monomers present in the ethylene acrylate copolymer.

[0015] In some embodiments of the polymer blend, the alkyl acrylate of the acrylate copolymer can be, by way of example and not limitation, acrylate, ethyl acrylate, n-butyl acrylate, isobutyl acrylate, or combinations thereof. In various embodiments, the alkyl acrylate is a C2-C8-alkyl acrylate, i.e., an alkyl acrylate having an alkyl group having 1-8 carbons.

[0016] In various embodiments of the polymer blend, the monocarboxylic acid monomer comprises acrylic acid, methacrylic acid, or a combination thereof.

[0017] In one or more embodiments of the polymer blend, the ethylene acrylate copolymer has a melt index (I2) of 2 g / 10 min to 12 g / 10 min, as determined according to ASTM D 1238 (190° C., 2.16 kg). In some embodiments, the ethylene acrylate copolymer has a melt index (I2) of 4 g / 10 min to 10 g / 10 min.

[0018] One or more embodiments of the present disclosure include a film comprising a polymer blend according to any embodiment previously described in this disclosure.

[0019] In various embodiments, a film comprising the polymer blend has a hardness of 8 g / m at temperatures between 290° C. and 320° C. 2 ~30g / m 2 or 12 g / m 2 ~25g / m 2 and at a line speed of 300 m / min to 800 m / min, or 300 m / min to 500 m / min, has a neck-in value of 140 mm or less, or 120 mm or less, or 100 mm or less.

[0020] In one embodiment, a film produced from the polymer blend has a neck-in value of less than 100 mm, while it has a linear speed of 500 m / min and a temperature of 320° C. of 12 g / m 2 In another embodiment, the film is coated on the substrate at a coating weight of 24 g / m at a line speed of 500 m / min and a temperature of 320° C. 2 In another embodiment, the film has a neck-in value of less than 100 mm when coated on paper at a coating weight of 24 g / m at a line speed of 300 m / min and a temperature of 320° C. 2 When coated on paper at a coating weight of 0.1 g / m2, the film has a neck-in value of less than 100 mm.

[0021] The neck-in value refers to the difference between the die width and the final width of the extruded polymer blend of the manufactured article. The neck-in value is influenced by the swelling of the extrudate and, to a lesser extent, by surface tension effects. It is well known that for conventional ethylene polymers, increasing the melt index tends to increase the neck-in value, and decreasing the molecular weight increases the melt index.

[0022] An embodiment of the present disclosure includes a coated polymeric substrate comprising a polymeric substrate, a coating on the polymeric substrate comprising any of the polymeric blends of the present disclosure, and a tie layer disposed between the polymeric substrate and the coating.

[0023] In one or more embodiments of the coated polymeric substrate, the polymeric substrate comprises polyethylene, polypropylene, polyethylene terephthalate, or polyamide. In some embodiments, the polymeric substrate is uniaxially or biaxially oriented.

[0024] The polymer blends of the present disclosure can be extrusion coated onto a variety of polymer substrates at medium to high extrusion line speeds (e.g., 300 m / min to 800 m / min). Films produced from the polymer blends have low neck-in values ​​at medium to high extrusion line speeds, allowing for high throughput at the coating line.

[0025] polymerization In some embodiments, the LDPE polymer of the polymer blend is produced in a high pressure free radical initiated polymerization process. In high pressure free radical initiated polymerization processes, two basic types of reactors are known. The first type is a stirred autoclave vessel (autoclave reactor) with one or more reaction zones. The second type is a jacketed tube (tubular reactor) with one or more reaction zones.

[0026] The pressure in each autoclave and tubular reactor zone of the process is typically from 100 MPa to 400 MPa, more typically from 120 MPa to 360 MPa, and even more typically from 150 MPa to 320 MPa.

[0027] Polymerization temperatures in each tubular reactor zone of the process are typically from 100°C to 400°C, more typically from 130°C to 360°C, and even more typically from 140°C to 330°C.

[0028] The polymerization temperature in each autoclave reactor zone of the process is typically from 150 to 300°C, more typically from 165 to 290°C, and even more typically from 180 to 280°C.

[0029] In some embodiments, a tubular reactor having at least three reaction zones may be used to produce the LDPE polymer of the polymer blend of the present disclosure.

[0030] Initiator The process for producing the LDPE polymer of the polymer blend of the present disclosure is a free radical polymerization process. The type of free radical initiator used in the process is not critical, but preferably one of the initiators applied should allow high temperature operation in the range of 300°C to 350°C. Examples of suitable free radical initiators include organic peroxides such as peresters, perketals, peroxyketones, percarbonates, and cyclic multifunctional peroxides. These organic peroxy initiators are added to the reactor at 0.005% to 0.2% by weight, based on the total weight of polymerizable monomers in the reactor. The peroxide is typically injected as a dilute solution in a suitable solvent, such as a hydrocarbon solvent.

[0031] Other suitable initiators include azodicarboxylic acid esters, azodicarboxylic acid dinitriles, and 1,1,2,2-tetramethylethane derivatives, as well as other components capable of forming free radicals in the desired operating temperature range.

[0032] In one embodiment, the initiator is added to at least one reaction zone of the polymerization reactor. In a further embodiment, the initiator is added to the reactor or polymerization process at a peak polymerization temperature of 320° C. to 350° C. In a further embodiment, the initiator includes at least one peroxide group incorporated into a cyclic structure.

[0033] Examples of suitable initiators for polymerizing polyethylene include, but are not limited to, TRIGONOX 301 (3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxonane) and TRIGONOX 311 (3,3,5,7,7-pentamethyl-1,2,4-trioxepane), both available from Akzo Nobel, and HMCH-4-AL (3,3,6,6,9,9-hexamethyl-1,2,4,5-tetroxonane), available from United Initiators. Additional initiators are disclosed in WO 02 / 14379 and WO 01 / 68723, which are incorporated herein by reference.

[0034] Additives One or more additives may be added to the polymer blend.Suitable additives include, but are not limited to, stabilizers, fillers (such as clay, talc, titanium dioxide, zeolite, organic or inorganic particles including powdered metals, etc.), organic or inorganic fibers (including carbon fibers, silicon nitride fibers, steel wire or mesh, and nylon or polyester coatings), nanoparticles, clays, tackifiers, and oil extenders (including paraffinic or naphthenic oils).

[0035] Polymer Manufacturing The polymer blends of the present disclosure may be utilized in a variety of thermoplastic manufacturing processes to produce useful articles, including extrusion coatings and extrusion laminates.

[0036] definition Unless stated to the contrary, implicit from the context, or customary in the art, all parts and percentages are by weight and all test methods are as of the filing date of this disclosure.

[0037] The term "blend" or "polymer blend" as used in this disclosure means an intimate physical mixture of two or more polymers without physical or chemical reaction between the polymers. A blend may be miscible and free of phase separation at the molecular level, or it may be immiscible and demonstrate some degree of phase separation at the molecular level. A blend may, but need not, include one or more domain configurations, which may be determined from transmission electron spectroscopy, light scattering, x-ray scattering, and other methods known in the art. A blend may be achieved by physically mixing two or more polymers at the macro or micro level. Examples of physical mixing at the macro level include melt blending or compounding of resins. Examples of physical mixing at the micro level include the simultaneous formation of two or more polymers in the same reactor.

[0038] The term "polymer" refers to a compound prepared by polymerizing monomers, whether of the same or different types. Polymers include homopolymers, which are prepared from only one type of monomer, with the understanding that trace amounts of impurities may be incorporated into the polymer structure.

[0039] The terms "ethylene-based polymer" or "ethylene polymer" refer to a polymer that contains at least 50 weight percent polymerized ethylene, based on the total weight of the polymer. Ethylene-based polymers and ethylene polymers can be ethylene homopolymers or can contain one or more comonomers, provided that ethylene has the largest weight fraction of the polymer among all monomers in the polymer.

[0040] Test Method Density: Samples for density measurement are prepared according to ASTM D 1928. The polymer sample is compressed at 190° C. and 30,000 psi for 3 minutes, then at 21° C. and 207 MPa for 1 minute. Measurements are taken within 1 hour of pressing the sample using ASTM D 792, Method B.

[0041] Melt Index: Melt index, or I2, (grams / 10 minutes or dg / min), is measured in accordance with ASTM D 1238, condition 190°C / 2.16 kg.

[0042] Triple detector gel permeation chromatography (3D-GPC) The chromatography system includes a PolymerChar GPC-IR (Valencia, Spain) high temperature GPC chromatograph with an internal IR5 infrared detector (IR5) coupled to a Precision Detectors (now Agilent Technologies) two-angle laser light scattering (LS) detector model 2040. For all light scattering measurements, a 15 degree angle is used for measurement purposes. The autosampler oven compartment is set to 160°C and the column compartment is set to 150°C. Columns that may be used include four Agilent "Mixed A" 30 cm, 20 micron linear mixed bed columns. Chromatography solvents that may be used include 1,2,4 trichlorobenzene, containing 200 ppm butylated hydroxytoluene (BHT). The solvent source is nitrogen injected. Injection volumes that may be used include 200 microliters (μL) and the flow rate was 1.0 milliliters / min.

[0043] The GPC column set is calibrated with at least 20 narrow molecular weight distribution polystyrene standards with molecular weights ranging from 580 to 8,400,000 g / mol, arranged in six "cocktail" mixtures with at least 10 intervals between each molecular weight (meaning that there is approximately a 10-fold difference in order of magnitude). Standards are purchased from Agilent Technologies. Polystyrene standards are prepared at 0.025 grams in 50 milliliters of solvent for molecular weights of 1,000,000 and above, and 0.05 grams in 50 milliliters of solvent for molecular weights below 1,000,000. The polystyrene standards are dissolved at 80° C. with gentle agitation for 30 minutes. The polystyrene standard peak molecular weights are converted to polyethylene molecular weights using Equation 1 (as described in Williams and Ward, J. Polym. Sci., Polym. Let., 6, 621 (1968)). M ポリエチレン =A×(M ポリスチレン ) B (Formula 1) where M is the molecular weight, A has a value of 0.4315, and B is equal to 1.0.

[0044] A fifth order polynomial is used to fit each of the polyethylene equivalent calibration points. A small adjustment is made to A (approximately 0.415 to 0.44) to correct for column resolution and band broadening effects, such that the NIST standard NBS1475 is obtained at 52,000 MW.

[0045] A total plate count for the GPC column set is performed with Eicosane (prepared at 0.04 g in 50 milliliters of TCB and dissolved for 20 minutes with gentle agitation). Plate count (Equation 2) and symmetry (Equation 3) are measured with a 200 microliter injection according to the following formula:

number

number

[0046] Samples are prepared semi-automatically using PolymerChar "Instrument Control" software. Samples were targeted to a weight of 2 mg / mL and the solvent (containing 200 ppm BHT) was added via the PolymerChar high temperature autosampler to a septa-capped vial that had been pre-flushed with nitrogen. Samples were dissolved at 160 degrees Celsius with "slow" shaking for 2 hours.

[0047] Mn (GPC) , Mw (GPC)、 and Mz (GPC) The calculation was based on GPC results using PolymerChar GPCOne™ software, the internal IR5 detector (measurement channel) of the PolymerChar GPC-IR chromatograph according to Equations 4-6 using baseline-subtracted IR chromatograms at each equally spaced data collection point (i), and the polyethylene equivalent molecular weights obtained from a narrow standard calibration curve at point (i) from Equation 1.

number

number

number

[0048] To monitor deviations over time, a flow marker (decane) is introduced into each sample via a micropump controlled by the PolymerChar GPC-IR system. This flow marker (FM) was used to linearly calibrate the pump flow rate (Flow (apparent)) of each sample by RV matching the respective decane peak in the sample (RV (FM sample)) with the decane peak in the narrow standard calibration (RV (FM calibrated)). Any change in time of the decane marker peak is assumed to be related to a linear shift in flow rate (Flow (effective)). To facilitate the highest accuracy of the RV measurement of the flow marker peak, a least squares fitting routine is used to fit the peaks of the flow marker concentration chromatogram to a quadratic equation. The first derivative of the quadratic equation is used to determine the true peak position. After calibrating the system based on the flow marker peaks, the effective flow rate (relative to the narrow standard calibration) is calculated as in Equation 7. Processing of the flow marker peaks was performed by PolymerChar GPCOne™ software. An acceptable flow correction is that the effective flow rate should be within + / - 2% of the apparent flow rate. Flow (effective) = Flow (apparent) * (RV(FM calibrated) / RV(FM sampled)) (Equation 7)

[0049] A systematic approach for the determination of multiple detector offsets was performed in a manner consistent with that published by Balke, Mourey, et. al. (Mourey and Balke, Chromatography Polym. Chpt 12, (1992)) (Balke, Thitiratsakul, Lew, Cheung, Mourey, Chromatography Polym. Chpt 13, (1992)) using PolymerChar GPCOne™ software to optimize triple detector log (MW and IV) results from broad homopolymer polyethylene standards (Mw / Mn>3) to narrow standard column calibration results from narrow standard calibration curves.

[0050] Absolute molecular weight data are obtained using PolymerChar GPCOne™ software in a manner consistent with that published by Zimm (Zimm, BH, J. Chem. Phys., 16, 1099 (1948)) and Kratochvil (Kratochvil, P., Classical Light Scattering from Polymer Solutions, Elsevier, Oxford, NY (1987)). The overall injected concentration used in determining the molecular weight is obtained from the mass detector area and mass detector constant derived from a suitable linear polyethylene homopolymer or one of the polyethylene standards of known weight average molecular weight. The calculated molecular weight (using GPCOne™) was obtained using the light scattering constant and refractive index concentration coefficient, dn / dc, of 0.104 derived from one or more of the polyethylene standards described below. In general, the mass detector response (IR5) and light scattering constant (determined using GPCOne™) should be determined from a linear standard with a molecular weight greater than about 50,000 g / mol. Viscometer calibration (determined using GPCOne™) can be accomplished using the method described by the manufacturer, or alternatively, by using the published values ​​of a suitable linear standard, such as Standard Reference Material (SRM) 1475a (available from the National Institute of Standards and Technology (NIST)). A viscometer constant (obtained using GPCOne™) is calculated that relates the specific viscosity area (DV) and injected mass for the calibration standard to its intrinsic viscosity. The chromatographic concentration is assumed to be low enough to preclude addressing the second viral coefficient effect (concentration effect on molecular weight).

[0051] The other moments Mn (Abs) and Mz (Abs) is calculated according to the following equations 8 and 9.

number

number

[0052] Extrusion Coating: To produce the extrusion coated substrates, a Davis Standard ER-WE-PA, Maschinenfabrik Erkrath Nr. 7237 (construction year: 1990, with flat EBR (edge ​​bead reduction)) is used. The Davis Standard ER-WE-PA, Maschinenfabrik Erkrath Nr. has a 1050 mm wide slit die (maximum substrate width: 800 mm) and is equipped with a feedblock coextrusion system, the extruder has an output of up to 350 kg / h of polymer. The molten polymer leaves the die at a temperature of 260-340 °C. The air gap was set at 250 mm and the nip-off was set at -15 mm. These rated as single slot feedblock, and the largest extruder "A" (with ET Barr 3.5 inch double flight compression screw L / D 32). This Davis Standard ER-WE-PA line is part of Pack Studio in Horgen. The molten polymer is coated onto a paper substrate and cooled by a chill roll with a chill roll temperature of 15°C. Air gap: 250mm Nip offset: -15mm Extrusion temperature setting: 320℃ Base material: 60g / m 2 Kraft paper EXAMPLES

[0053] Six exemplary compositions were prepared and the polymer characteristics of each were measured.

[0054] Example 1 was a polymer blend prepared from 97% by weight of AGILITY™ EC7000 manufactured by Dow Inc. as the LDPE component and 3% of ELVALOY™ AC 2618 manufactured by Dow Inc. as the acrylate copolymer.

[0055] Example 2 was a polymer blend prepared from 97% by weight of AGILITY™ EC7000 manufactured by Dow Inc. as the LDPE component and 3% of ELVALOY™ AC 3427 manufactured by Dow Inc. as the acrylate copolymer.

[0056] Example 3 was a polymer blend prepared from 97% by weight of AGILITY™ EC7000 manufactured by Dow Inc. as the LDPE component and 3% of ELVALOY™ AC 3717 manufactured by Dow Inc. as the acrylate copolymer.

[0057] Example 4 was a polymer blend prepared from 97% by weight of AGILITY™ EC7000 manufactured by Dow Inc. as the LDPE component and 3% of ELVALOY™ AC 1820 manufactured by Dow Inc. as the acrylate copolymer.

[0058] Comparative Example C1 was 100 wt. % AGILITY™ EC7000 manufactured by Dow Inc. as an example of LDPE produced in a tubular reactor.

[0059] Comparative Example C2 was 100 wt. % LDPE PT7007 manufactured by Dow Inc. and was an example of LDPE produced in an autoclave reactor.

[0060] The characteristics of each of the polymer blends and the comparative polymers are summarized in Table 1. [Table 1]

[0061] Each of the present invention and comparative examples was 2 The amount of coating is 70g / m 2The melt was extruded on a 3.5 inch diameter screw with a length to diameter ratio (L / D) of 32 on kraft paper. Melt pressure and melt temperature were recorded using a thermocouple placed in the adapter. The melt was delivered through a Davis Standard / Er-We-Pa Flex Lip Edge Bead Reduction Die, Series 510A, set at a nominal die gap of 0.7 mm. Melt drawing and application (vertical of the melt onto the moving substrate) was performed with an air gap of 250 mm and a nip offset of 15 mm towards the pressure roll. The melt was applied onto the moving substrate in the laminator nip (the point of contact between the pressure roll and the substrate) with a rubber surface layer in contact with a "water cooled" chill roll with a matte surface finish, maintained at a temperature of 15°C to 20°C. The air gap is defined as the vertical distance between the die lip and the laminator nip. The nip offset is defined as the horizontal offset of the die lip position relative to the laminator nip.

[0062] Table 2 summarizes the results of the neck-in determination for Comparative Example C1, Comparative Example C2, and Examples 1-4. To determine the neck-in values ​​of the polymer blends (specifically for Examples 1-4), each polymer blend and comparative example was coated onto a substrate, specifically paper, as described above. The conditions listed in Table 1 include a line speed of 300 m / min or 500 m / min. The polymer substrate was coated with a 12 g / m 2 or 24 g / m 2 The mixture was coated to a coating weight of 1000g. [Table 2]

[0063] When evaluating the performance of each of the polymer blends of Examples 1-4 and the polymer of the comparative example, a smaller neck-in value is more desirable. A suitable neck-in value for extrusion coating is about 100 mm or less. A lower neck-in value indicates greater dimensional stability of the web (polymer after being extruded through the die). If the web is more dimensionally stable, the coating of the substrate can be more tightly controlled, allowing the polymer to be smoothly applied to the substrate.

[0064] Comparative C1 was an ethylene polymer produced in a tubular reactor. Comparative C2 was an ethylene polymer produced in an autoclave reactor. Comparative C1 had a neck-in value of over 100 mm at linear speeds of 300 m / min and 500 m / min. Comparative C2 had a neck-in value of 103 mm at a medium speed of 300 m / min, but could not be extruded at all onto a substrate at 500 m / min. Examples of the invention of this application include the following: [1] A polymer blend comprising: at least 90% by weight of a low density polyethylene (LDPE) polymer; 1% to 10% by weight of an ethylene acrylate copolymer, the ethylene acrylate copolymer comprising: at least 50 weight percent ethylene, based on the total weight percent of monomers present in the ethylene acrylate copolymer; 2 to 40 weight percent of an alkyl acrylate, based on the total weight percent of the monomers present in the ethylene acrylate copolymer; and 0 to 20 weight percent of a monocarboxylic acid monomer, based on the total weight percent of said monomers present in said ethylene acrylate copolymer. [2] The LDPE has a density of 0.910 g / cc to 0.930 g / cc and an ASTM Melt index (I) between 2 g / 10 min and 5 g / 10 min, as determined in accordance with D 1238 (190 °C, 2.16 kg) 2 The polymer blend according to the above [1], [3] The ethylene acrylate copolymer has a melt index (I) of 4 g / 10 min to 10 g / 10 min, as determined in accordance with ASTM D 1238 (190° C., 2.16 kg). 2 2. The polymer blend of claim 1, wherein [4] The polymer blend of any one of the preceding claims, wherein the polymer blend comprises 1% by weight to 5% by weight of the ethylene acrylate copolymer. [5] The polymer blend of any one of the preceding claims, wherein the ethylene acrylate copolymer comprises at least 75% by weight ethylene, and 12% to 25% by weight alkyl acrylate. [6] The polymer blend of any one of the preceding claims, wherein the alkyl acrylate comprises methyl acrylate, ethyl acrylate, n-butyl acrylate, or isobutyl acrylate, or a combination thereof, and the monocarboxylic acid monomer comprises one or more of acrylic acid, methacrylic acid, or a combination thereof. [7] The polymer blend of any one of the preceding claims, wherein the LDPE polymer is a tubular polymer. [8] A film comprising a polymer blend according to any one of the preceding claims. [9] 12 g / m at a line speed of 500 m / min and a temperature of 320 °C 2 The film according to [8] above, wherein when coated on paper at a coating weight of 100 μm, the film has a neck-in of less than 100 mm.

[10] A coated polymer substrate comprising: A polymer substrate; A coating comprising the polymer blend according to any one of [1] to [6] above; a tie layer disposed between the polymeric substrate and the coating.

[11] The coated polymer substrate of

[10] above, wherein the polymer substrate comprises polyethylene, polypropylene, polyethylene terephthalate, or polyamide.

[12] The coated polymer substrate according to

[10] or

[11] above, wherein the polymer substrate is uniaxially or biaxially oriented.

Claims

1. 1. A polymer blend comprising: at least 90% by weight of a low density polyethylene (LDPE) polymer; 1% to 10% by weight of an ethylene acrylate copolymer, The ethylene acrylate copolymer is at least 50 weight percent ethylene, based on the total weight percent of monomers present in the ethylene acrylate copolymer; 2 to 40 weight percent of an alkyl acrylate, based on the total weight percent of the monomers present in the ethylene acrylate copolymer; 0 to 20 weight percent of a monocarboxylic acid monomer, based on the total weight percent of said monomers present in said ethylene acrylate copolymer; and having a melt index (I 2 ) of 4 g / 10 min to 10 g / 10 min as determined according to ASTM D1238 (190° C., 2.16 kg); A polymer blend comprising:

2. The LDPE polymer has a density of 0.910 g / cc to 0.930 g / cc, and a melt index (I) of 2 g / 10 min to 5 g / 10 min, as determined according to ASTM D1238 (190° C., 2.16 kg). 2 2. The polymer blend of claim 1 having a molecular weight of 1:1 or more.

3. 10. The polymer blend of claim 1, wherein the polymer blend comprises from 1% to 5% by weight of the ethylene acrylate copolymer.

4. 10. The polymer blend of claim 1, wherein the ethylene acrylate copolymer comprises at least 75% by weight ethylene and from 12% to 25% by weight alkyl acrylate.

5. 2. The polymer blend of claim 1, wherein the alkyl acrylate comprises methyl acrylate, ethyl acrylate, n-butyl acrylate, or isobutyl acrylate, or a combination thereof, and the monocarboxylic acid monomer comprises one or more of acrylic acid, methacrylic acid, or a combination thereof.

6. A film comprising a polymer blend according to any one of claims 1 to 5.

7. 12 g / m at a line speed of 500 m / min and a temperature of 320° C. 2 7. The film of claim 6, wherein when coated onto paper at a coating weight of 0.15 wt. %, the film has a neck-in of less than 100 mm.

8. 1. A coated polymeric substrate comprising: A polymer substrate; A coating comprising the polymer blend of any one of claims 1 to 5; a tie layer disposed between the polymeric substrate and the coating.

9. The coated polymeric substrate of claim 8 , wherein the polymeric substrate comprises polyethylene, polypropylene, polyethylene terephthalate, or polyamide.

10. The coated polymeric substrate of claim 8 , wherein the polymeric substrate is uniaxially or biaxially oriented.

Citation Information

Patent Citations

  • Manufacture of composite material for high foam polyethylene for insulation and high foam body coated insulation cable

    JP1991192607A

  • Polyethylene composition and cable for direct current prepared using the same

    JP2015000883A

  • Low-density ethylene polymers with high melt strength

    JP2015535035A

  • Polymer blends for use in multilayer structures and multilayer structures containing them

    JP2019537655A

  • Blends of an olefin high polymer with an ethylene / acrylic acid copolymer

    US3410928A