Positive electrode for lithium secondary battery and lithium secondary battery including the same
The positive electrode composite layer with a dense and acicular crack structure addresses structural instability in lithium secondary batteries, enhancing safety and performance by reducing gas generation and maintaining stable lithium ion transfer.
Patent Information
- Application Number
- JP2023515362
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-02-09
- Filing Date
- 2022-04-05
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-04-05
AI Technical Summary
Conventional lithium secondary battery additives are structurally unstable, leading to oxygen gas generation, electrode expansion, and side reactions, which deteriorate battery performance and safety.
A positive electrode composite layer with a dense structure and acicular crack structure is designed, incorporating a positive electrode additive with a specific chemical formula (Li p Co (1-q) M 1 q O 4) and a lithium metal composite oxide (Li x [Ni y Co z Mn w M 2 v ]O u), which reduces gas generation and provides a path for lithium ion and electron movement.
The design enhances battery safety and electrical performance by minimizing gas production and maintaining stable lithium ion transfer, improving charge/discharge capacity and cycle life.
Smart Images

Figure 0007594096000004 
Figure 0007594096000005 
Figure 0007594096000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a positive electrode for a lithium secondary battery and a lithium secondary battery including the same.
[0002] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0064296 filed on May 18, 2021, and Korean Patent Application No. 10-2022-0016953 filed on February 9, 2022, and all contents disclosed in the documents of said Korean patent applications are incorporated herein by reference. [Background technology]
[0003] With the development of technology and increasing demand for mobile devices, the demand for secondary batteries as an energy source is rapidly increasing. Among such secondary batteries, lithium secondary batteries, which have high energy density and working potential, long cycle life, and low self-discharge rate, have been commercialized and are widely used.
[0004] Recently, as lithium secondary batteries are used as power sources for medium- to large-sized devices such as electric vehicles, there is an increasing demand for high capacity, high energy density, and low cost of lithium secondary batteries, and the irreversible additives used in electrodes are also required to have higher irreversible capacity. However, it is true that there has been a limit to the development of positive electrode additives with such high irreversible capacity.
[0005] Meanwhile, conventional irreversible additives such as Li6CoO4 are generally manufactured by reacting excess lithium oxide with metal oxides such as cobalt oxide. The irreversible additives manufactured in this way are structurally unstable and generate large amounts of oxygen gas (O2) as charging proceeds, as described below. If the irreversible additives do not completely react during initial charging of the secondary battery, i.e., during activation of the battery, they may react during subsequent charging and discharging processes to generate side reactions and large amounts of oxygen gas inside the battery. The oxygen gas thus generated may induce volume expansion of the electrode assembly, and act as one of the main factors causing deterioration of battery performance.
[0006] [ka]
[0007] In addition, the by-products such as lithium oxide may react with binder components during preparation of a slurry composition for manufacturing an electrode, causing an increase in viscosity or gelation of the composition, which may result in difficulty in uniform application of the electrode composition for forming an active material layer, resulting in a problem of deterioration of battery characteristics.
[0008] Therefore, in order to improve the safety and electrical performance of lithium secondary batteries, there is a demand for the development of technology that can reduce side reactions caused by irreversible additives and the generation of gases such as oxygen (O2) during charging and discharging. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Korean Patent Publication No. 10-2019-0078392 Summary of the Invention [Problem to be solved by the invention]
[0010] Therefore, an object of the present invention is to provide a positive electrode for a lithium secondary battery and a lithium secondary battery that can realize excellent battery safety and high charge / discharge capacity by improving side reactions caused by irreversible additives and reducing the amount of gas such as oxygen (O2) generated during charge / discharge. [Means for solving the problem]
[0011] To solve the above problems, In one embodiment, the present invention comprises: A positive electrode current collector; A positive electrode mixture layer is formed on at least one surface of the positive electrode current collector and contains a positive electrode active material and a positive electrode additive represented by the following chemical formula 1: After the initial charge, the cross-sectional structure of the positive electrode mixture layer is as follows: a first region having a dense structure filled with first metal oxide particles; and a second region having an acicular crack structure inside and outside the second metal oxide particle:
[0012] [Chemical formula 1] Li p Co (1-q) M 1 q O4
[0013] In the above chemical formula 1, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; p and q are 5≦p≦7 and 0≦q≦0.5, respectively.
[0014] Here, the second region may have a structure in which it is dispersed in an island form within the first region.
[0015] The second region may occupy 0.001 to 10% of the entire cross-sectional area of the positive electrode mixture layer.
[0016] The needle-like crack structure contained in the second region may include cracks having an average thickness of 5 nm to 800 nm and an average length of 50 nm to 10 μm.
[0017] The positive electrode additive may have a tetragonal structure with a space group of P42 / nmc.
[0018] In addition, the positive electrode active material may be a lithium metal composite oxide represented by the following Chemical Formula 2:
[0019] [Chemical formula 2] Li x [Ni y Co z Mn w M 2 v ]O u
[0020] In the above chemical formula 2, M 2 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; x, y, z, w, v, and u are within the range of 1.0≦x≦1.30, 0.1≦y<0.95, and 0.01, respectively. <z≦0.5、0.01<w≦0.5、0≦v≦0.2、1.5≦u≦4.5である。
[0021] The positive electrode mixture layer may further contain one or more conductive materials selected from the group consisting of natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, and carbon fiber.
[0022] Moreover, in one embodiment, the present invention provides There is provided a lithium secondary battery comprising the above-mentioned positive electrode of the present invention, a negative electrode, and a separator located between the positive electrode and the negative electrode.
[0023] In this case, the negative electrode may include a negative electrode current collector and a negative electrode mixture layer that is located on at least one surface of the negative electrode current collector and contains a negative electrode active material.
[0024] The negative electrode active material may contain a carbon material and a silicon material. The carbon material may include at least one selected from the group consisting of natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, carbon fiber, graphene, and carbon nanotubes. The silicon material may include silicon (Si) particles and silicon oxide (SiO X , 1≦X≦2) particles.
[0025] The silicon material may be included in an amount of 1 to 20 parts by weight per 100 parts by weight of the negative electrode mixture layer. Effect of the Invention
[0026] The positive electrode for a lithium secondary battery according to the present invention contains a positive electrode additive represented by Chemical Formula 1 in a positive electrode mixture layer, and has a region having a needle-shaped crack structure in a cross section of the positive electrode mixture layer after initial charging (activation). This reduces the amount of gas generation, such as oxygen, caused by the positive electrode additive, which is an irreversible additive, during subsequent charging and discharging processes, and ensures a path for the movement of lithium ions and / or electrons, thereby providing an excellent effect of improving the battery safety and electrical performance of the lithium secondary battery. [Brief description of the drawings]
[0027] [Figure 1] 1A and 1B are images obtained by analyzing cross-sectional structures of a positive electrode for a lithium secondary battery according to the present invention before and after initial charging (activation) using a scanning electron microscope (SEM), in which (a) shows the cross-sectional structure before initial charging (activation), and (b) shows the cross-sectional structure after initial charging (activation). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] Although the present invention can be modified in various ways and can have a variety of embodiments, a specific embodiment will be described in detail.
[0029] However, this is not intended to limit the invention to the particular embodiment, but should be understood to include all modifications, equivalents, or alternatives falling within the spirit and scope of the invention.
[0030] In the present invention, the terms "comprise" and "have" are intended to specify the presence of features, numbers, steps, operations, components, parts, or combinations thereof described in the specification, and should be understood as not precluding the presence or additional possibility of one or more other features, numbers, steps, operations, components, parts, or combinations thereof.
[0031] In addition, in the present invention, when a layer, film, region, plate, or other portion is described as being "on" another portion, this includes not only the case where it is "directly on" the other portion, but also the case where there is another portion in between. Conversely, when a layer, film, region, plate, or other portion is described as being "under" the other portion, this includes not only the case where it is "directly under" the other portion, but also the case where there is another portion in between. In addition, in the present application, being "located on" can include not only the case where it is located at the top, but also the case where it is located at the bottom.
[0032] In addition, in the present invention, a "major component" means 50% by weight or more, 60% by weight or more, 70% by weight or more, 80% by weight or more, 90% by weight or more, 95% by weight or more, or 97.5% by weight or more of the total weight of the composition or specific component, and in some cases, it may mean 100% by weight when it constitutes the entire composition or specific component.
[0033] In the present invention, "Ah" is a unit of capacity of a lithium secondary battery, and is called "ampere-hour" and means the amount of current per hour. For example, if a battery capacity is "3000mAh", it means that it can be discharged at a current of 3000mA for one hour.
[0034] The present invention will now be described in more detail.
[0035] <Positive electrodes for lithium secondary batteries> In one embodiment, the present invention comprises: A positive electrode current collector; A positive electrode mixture layer is formed on at least one surface of the positive electrode current collector and contains a positive electrode active material and a positive electrode additive represented by the following chemical formula 1: After the initial charge, the cross-sectional structure of the positive electrode mixture layer is as follows: a first region having a dense structure filled with first metal oxide particles; and a second region having an acicular crack structure inside and outside the second metal oxide particle:
[0036] [Chemical formula 1] Li p Co (1-q) M 1 q O4
[0037] In the above chemical formula 1, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; p and q are 5≦p≦7 and 0≦q≦0.5, respectively.
[0038] The positive electrode for a lithium secondary battery according to the present invention has a structure in which a mixture layer is formed on a positive electrode current collector, and the positive electrode mixture layer has a configuration containing a positive electrode active material and a positive electrode additive.
[0039] In this case, the positive electrode active material may be a lithium composite transition metal oxide containing two or more elements selected from the group consisting of nickel (Ni), cobalt (Co), manganese (Mn), aluminum (Al), zinc (Zn), titanium (Ti), magnesium (Mg), chromium (Cr) and zirconium (Zr). For example, the positive electrode active material may be a lithium metal composite oxide capable of reversible intercalation and deintercalation, as shown in the following chemical formula 2:
[0040] [Chemical formula 2] Li x [Ni y Co z Mn w M 2 v ]O u
[0041] In the above chemical formula 2, M 2 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; x, y, z, w, v, and u are within the range of 1.0≦x≦1.30, 0.1≦y<0.95, and 0.01, respectively. <z≦0.5、0.01<w≦0.5、0≦v≦0.2、1.5≦u≦4.5である。
[0042] The lithium metal composite oxide represented by the above chemical formula 2 is a metal oxide containing lithium, nickel, cobalt and manganese, and in some cases, other transition metals (M 2 For example, the positive electrode active material may be doped with LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.9 Co 0.05 Mn 0.05 O2, LiNi0.8 Co 0.1 Mn 0.05 Al 0.05 O2 and LiNi 0.7 Co 0.1 Mn 0.1 Al 0.1 O2. As an example, the positive electrode active material may contain one or more compounds selected from the group consisting of LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.8 Co 0.1 Mn 0.05 Al 0.05 O2 and LiNi 0.7 Co 0.1 Mn 0.1 Al 0.1 O2, etc. can be used alone or in combination.
[0043] The content of the positive electrode active material may be 85 to 95 parts by weight, specifically 88 to 95 parts by weight, 90 to 95 parts by weight, 86 to 90 parts by weight, or 92 to 95 parts by weight, relative to 100 parts by weight of the positive electrode mixture layer.
[0044] The positive electrode mixture layer includes a positive electrode additive that provides irreversible capacity together with a positive electrode active material that exhibits electrical activity, and the positive electrode additive may include lithium cobalt oxide represented by the following Chemical Formula 1:
[0045] [Chemical formula 1] Li p Co (1-q) M 1 q O4
[0046] In the above chemical formula 1, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; p and q are 5≦p≦7 and 0≦q≦0.5, respectively.
[0047] The positive electrode additive contains an excess of lithium and can provide lithium to replace lithium consumption that occurs due to irreversible chemical and physical reactions at the negative electrode during initial charging, i.e., activation, thereby increasing the charge capacity of the battery and reducing the irreversible capacity, thereby improving the life characteristics.
[0048] Among them, the positive electrode additive represented by the above formula 1 has a higher lithium ion content than nickel-containing oxides commonly used in the industry, and therefore can replenish lithium ions lost in irreversible reactions during initial charging (activation) of the battery, thereby significantly improving the charge / discharge capacity of the battery. Also, compared to iron- and / or manganese-containing oxides commonly used in the industry, there is no side reaction caused by the elution of transition metals during charging / discharging of the battery, and therefore has the advantage of excellent battery stability.
[0049] Examples of lithium cobalt oxides represented by the chemical formula 1 include Li6CoO4, Li6Co 0.5 Zinc 0.5 O4, Li6Co 0.7 Zinc 0.3 It may also include O4.
[0050] The average particle size of the lithium cobalt oxide represented by the above chemical formula 1 may be 0.1 to 10 μm, specifically, 0.1 to 8 μm, 0.1 to 5 μm, 0.1 to 3 μm, 0.5 to 2 μm, 0.1 to 0.9 μm, 0.1 to 0.5 μm, 0.6 to 0.9 μm, 1 to 4 μm, 1.5 to 3.5 μm, 4 to 6 μm, 5 to 10 μm, or 6 to 9 μm. By controlling the average particle size of the lithium cobalt oxide to the above range, the present invention can enhance the irreversible activity of the lithium cobalt oxide and prevent the powder electrical conductivity of the lithium cobalt oxide from being reduced.
[0051] The positive electrode additive may be included in an amount of 0.01 to 5 parts by weight relative to 100 parts by weight of each positive electrode mixture layer, specifically, 0.01 to 4 parts by weight; 0.01 to 3 parts by weight; 0.01 to 2 parts by weight; 0.1 to 1 parts by weight; 0.5 to 2 parts by weight; 1 to 3 parts by weight; 2 to 4 parts by weight; 1.5 to 3.5 parts by weight; 0.5 to 1.5 parts by weight; 1 to 2 parts by weight; 0.1 to 0.9 parts by weight; or 0.3 to 1.2 parts by weight.
[0052] In addition, the lithium cobalt oxide represented by the above formula 1 may have a tetragonal crystal structure, and may be included in the space group P42 / nmc having a distorted tetrahedral structure formed by cobalt and oxygen atoms. The positive electrode additive having a distorted tetrahedral structure has a distorted tetrahedral structure formed by cobalt and oxygen atoms, and is structurally unstable, so that it may generate side reactions and / or a large amount of oxygen gas inside the battery during initial charge / discharge as well as subsequent charge / discharge. However, the present invention can reduce the amount of gas generation such as oxygen generated by the positive electrode additive, which is an irreversible additive, by partially introducing a region having a needle-shaped crack structure into the positive electrode mixture layer during initial charge (activation), and at the same time, it is possible to secure a migration path for lithium ions and / or electrons, thereby improving the battery safety and electrical performance of the lithium secondary battery.
[0053] Specifically, the positive electrode for a lithium secondary battery according to the present invention may have a cross-sectional structure of a positive electrode composite layer after initial charging (activation) including a first region having a dense structure filled with first metal oxide particles and a second region having needle-shaped crack structures inside and outside the second metal oxide particles. More specifically, the first region means a region including a lithium metal composite oxide represented by Chemical Formula 2 as the first metal oxide. Since the first metal oxide can be reversibly intercalated and deintercalated during charging and discharging of a lithium secondary battery, the first metal oxide included in this region does not induce lithium loss due to charging and discharging of the lithium secondary battery, and even if lithium loss occurs, the degree of loss is small. Therefore, the first region may have a dense structure densely filled with first metal oxide particles and has no cracks or cracks, or may have microcracks or cracks of less than 5 nm, as analyzed by a scanning electron microscope (SEM). The second region means a region including a lithium cobalt oxide represented by Chemical Formula 1 as the second metal oxide. The second metal oxide loses lithium through an irreversible electrochemical reaction during initial charging of the lithium secondary battery, and the second metal oxide contained in this region induces loss due to charging and discharging of the lithium secondary battery. Therefore, the second region may have a structure in which needle-shaped cracks due to lithium loss are formed inside and outside (specifically, inside and on the surface of the second metal oxide particles) of a plurality of densely packed second metal oxide particles, or at the boundaries of the second metal oxide particles.
[0054] The first and second regions may form a positive electrode mixture layer, and the first region may have a structure in which the second region, which acts as a continuous phase and is a dispersed phase, is uniformly dispersed in the first region in an island form. In this case, the area ratio of the second region may be 0.001 to 10% with respect to the total cross-sectional area of the positive electrode mixture layer, and more specifically, it may be 0.001 to 8%, 0.001 to 6%, 0.001 to 5%, 0.001 to 3%, 0.001 to 2%, 0.05 to 2%, 0.1 to 2%, or 0.1 to 0.9% with respect to the total cross-sectional area of the positive electrode mixture layer. In the present invention, after initial charging (activation), the cross section of the positive electrode mixture layer has a structure in which the second region is uniformly dispersed in the first region at a specific area ratio, thereby minimizing or preventing side reactions and / or gas generation such as oxygen (O2) caused by the positive electrode additive during charging and discharging after activation.
[0055] The crack structure formed in the second region may have a needle-like shape with an average thickness of 5 nm to 800 nm and an average length of 50 nm to 10 μm.
[0056] Specifically, the needle-like cracks may have an average thickness of 5nm to 700nm; 5nm to 250nm; 5nm to 100nm; 5nm to 50nm; 5nm to 25nm; 10nm to 30nm; 15nm to 60nm; 50nm to 200nm; 80nm to 250nm; 100nm to 300nm; 150nm to 300nm; 200nm to 400nm; 250nm to 500nm; or 500nm to 800nm.
[0057] In addition, the needle-like cracks may have an average length of 50 nm to 8 μm; 50 nm to 6 μm; 50 nm to 5 μm; 50 nm to 3 μm; 50 nm to 2 μm; 50 nm to 1 μm; 50 nm to 900 nm; 50 nm to 750 nm; 50 nm to 500 nm; 50 nm to 250 nm; 100 nm to 500 nm; 100 nm to 900 nm; 200 nm to 400 nm; 500 nm to 900 nm; 900 nm to 2 μm; 1 μm to 10 μm; 1 μm to 8 μm; 1 μm to 5 μm; 1 μm to 3 μm; 5 μm to 10 μm; 2 μm to 6 μm; 4 μm to 7 μm; 1 μm to 3 μm; 2 μm to 4 μm; or 0.8 μm to 1.2 μm.
[0058] Here, the average length may refer to the length of the major axis, which is the longest line segment among the line segments that intersect the center of the crack with the center. The average thickness refers to the length of the minor axis, which is the shortest line segment among the line segments that intersect the center of the crack with the center, perpendicular to the major axis. In addition, the needle-like cracks may be connected to adjacent needle-like cracks to form a line shape (e.g., a straight line, a curve, etc.), and such line shapes may be repeated to randomly form crack structures such as ridges and valleys.
[0059] As an example, the second region may include needle-like cracks having an average thickness of 10 nm to 100 nm and an average length of 300 nm to 1 μm.
[0060] As another example, the second region may include needle-like cracks having an average thickness of 400 nm to 700 nm and an average length of 2 μm to 7 μm.
[0061] As another example, the second region may have a structure that is a mixture of first needle-shaped cracks having an average thickness of 10 nm to 100 nm and an average length of 300 nm to 1 μm, and second needle-shaped cracks having an average thickness of 400 nm to 700 nm and an average length of 2 nm to 7 μm.
[0062] As another example, the second region may include a needle-like structure having an average thickness and an average length of 50 to 90 nm and 500 to 1,500 nm, respectively. The needle-like structure has an irregularly positioned and connected morphology.
[0063] The crack structure formed in the second region may include a plurality of needle-like cracks, and the needle-like cracks may be formed irregularly. In some cases, the cracks may be oriented in any one direction, or oriented around any one point to form a radial shape, or the cracks may be connected to each other to form an irregular network structure, but is not limited thereto.
[0064] By controlling the shape and size of the cracks formed in the second region as described above, the present invention can improve side reactions and / or gases such as oxygen (O2) that are generated due to the positive electrode additive represented by Chemical Formula 1 during charging and discharging after the initial charging (activation).
[0065] Furthermore, the shape and size of the crack structure formed in the second region can control the initial charging conditions, i.e., the activation conditions, of the lithium secondary battery. Specifically, the crack structure in the second region can be formed by activating the lithium secondary battery under a constant current condition of 0.6 to 50 mA, or, in some cases, under a constant current-constant voltage condition of 1.0 C or less and an end-of-charge voltage of 4.2 V or less. The activation can be performed stepwise depending on the SOC.
[0066] For example, the crack structure of the second region may be realized by successively performing a three-step charging process, i.e., activation steps 1 to 3, during initial charging of the positive electrode for a lithium secondary battery. Specifically, the initial charging step may be performed as an activation step 1 in which a current of 0.05C to 0.3C is applied to the lithium secondary battery to charge it at an SOC of 30% to less than 40%, an activation step 2 in which a current of 0.3C to 0.5C is applied to the lithium secondary battery that has undergone the activation step 1 to charge it at an SOC of 40% to less than 50%, and an activation step 3 in which a current of 0.6C to 0.9C is applied to the lithium secondary battery that has undergone the activation step 2 to charge it at an SOC of 50% to less than 60%.
[0067] As an example, the crack structure of the second region may be formed by performing an activation stage 1 in which a current of 0.08C to 0.15C is applied to the lithium secondary battery during initial charging to charge the battery to an SOC of 30 to 39%, an activation stage 2 in which a current of 0.35C to 0.45C is applied to the lithium secondary battery that has undergone the activation stage 1 to charge the battery to an SOC of 40 to 49%, and an activation stage 3 in which a current of 0.65C to 0.8C is applied to the lithium secondary battery that has undergone the activation stage 2 to charge the battery to an SOC of 50 to 59%.
[0068] Meanwhile, the positive electrode mixture layer may further contain a conductive material, a binder, an additive, and the like in addition to the positive electrode active material and the positive electrode additive.
[0069] In this case, the conductive material can be used to improve the performance of the positive electrode, such as the electrical conductivity, and may include one or more selected from the group consisting of natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, carbon nanotubes, graphene, and carbon fibers. For example, the conductive material may include acetylene black.
[0070] The conductive material may be 0.5 to 5 parts by weight relative to 100 parts by weight of the positive electrode mixture layer, specifically, 0.5 to 4 parts by weight; 0.5 to 3 parts by weight; 0.5 to 1 part by weight; 0.5 to 2 parts by weight; 1 to 3 parts by weight; 2 to 4 parts by weight; 1.5 to 3.5 parts by weight; 0.5 to 1.5 parts by weight; or 1 to 2 parts by weight.
[0071] The binder may include one or more resins selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethylmethacrylate, and copolymers thereof. As an example, the binder may include polyvinylidene fluoride.
[0072] The binder may be contained in an amount of 1 to 10 parts by weight, specifically 2 to 8 parts by weight, or 1 to 5 parts by weight, relative to 100 parts by weight of the entire positive electrode mixture layer.
[0073] Additionally, the average thickness of the positive electrode composite layer is not particularly limited, but may be specifically 50 μm to 300 μm, and more specifically 100 μm to 200 μm; 80 μm to 150 μm; 120 μm to 170 μm; 150 μm to 300 μm; 200 μm to 300 μm; or 150 μm to 190 μm.
[0074] In addition, the positive electrode can be a positive electrode current collector having high conductivity without inducing chemical changes in the battery. For example, stainless steel, aluminum, nickel, titanium, calcined carbon, etc. can be used, and in the case of aluminum or stainless steel, those surface-treated with carbon, nickel, titanium, silver, etc. can be used. In addition, the positive electrode current collector can be formed with fine irregularities on the surface to increase the adhesive force of the positive electrode active material, and can be in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc. In addition, the average thickness of the current collector can be appropriately applied to 3 to 500 μm in consideration of the conductivity and total thickness of the positive electrode to be manufactured.
[0075] <Lithium secondary battery> Moreover, in one embodiment, the present invention provides There is provided a lithium secondary battery including the above-described positive electrode according to the present invention, a negative electrode, and a separator interposed between the positive electrode and the negative electrode.
[0076] The lithium secondary battery according to the present invention includes the above-mentioned positive electrode of the present invention, and has excellent characteristics in terms of battery safety and electrical performance. The lithium secondary battery according to the present invention has a structure including the above-mentioned positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode.
[0077] Here, the negative electrode is prepared by applying a negative electrode active material onto a negative electrode current collector, followed by drying and pressing to prepare a negative electrode composite layer, and may further selectively contain the same conductive material, organic binder polymer, additives, etc. as those of the positive electrode, as necessary.
[0078] The negative electrode active material may include, for example, a carbon material and a silicon material. The carbon material means a carbon material mainly composed of carbon atoms, and examples of such carbon materials include graphite having a perfect layered crystal structure like natural graphite, soft carbon having a low crystalline layered crystal structure (graphene structure; a structure in which hexagonal honeycomb-shaped carbon planes are arranged in layers), and hard carbon in which such a structure is mixed with a non-crystalline portion, artificial graphite, expanded graphite, carbon fiber, non-graphitizable carbon, carbon black, acetylene black, ketjen black, carbon nanotubes, fullerene, activated carbon, graphene, carbon nanotubes, etc., and preferably, may include one or more selected from the group consisting of natural graphite, artificial graphite, graphene, and carbon nanotubes. More preferably, the carbon material may include natural graphite and / or artificial graphite, and may include at least one of graphene and carbon nanotubes together with the natural graphite and / or artificial graphite. In this case, the carbon substance may contain 50 to 95 parts by weight of graphene and / or carbon nanotubes relative to 100 parts by weight of the total carbon substance, and more specifically, may contain 60 to 90 parts by weight; or 70 to 80 parts by weight of graphene and / or carbon nanotubes relative to 100 parts by weight of the total carbon substance.
[0079] The silicon substance is a particle containing silicon (Si) as a metal component as a main component, and is a silicon (Si) particle and a silicon oxide (SiO X , 1≦X≦2) particles. As an example, the silicon material may include silicon (Si) particles, silicon monoxide (SiO) particles, silicon dioxide (SiO2) particles, or a mixture of these particles.
[0080] In addition, the silicon material may have a mixed form of crystalline particles and amorphous particles, and the ratio of the amorphous particles may be 50 to 100 parts by weight, specifically 50 to 90 parts by weight, 60 to 80 parts by weight, or 85 to 100 parts by weight, based on 100 parts by weight of the total silicon material. By controlling the ratio of the amorphous particles contained in the silicon material within the above range, the present invention can improve thermal stability and flexibility without deteriorating the electrical properties of the electrode.
[0081] In addition, the silicon material may include a carbon material and a silicon material, and may be included in an amount of 1 to 20 parts by weight relative to 100 parts by weight of the negative electrode composite layer. Specifically, the silicon material may be included in an amount of 5 to 20 parts by weight, 3 to 10 parts by weight, 8 to 15 parts by weight, 13 to 18 parts by weight, or 2 to 7 parts by weight relative to 100 parts by weight of the negative electrode composite layer.
[0082] By adjusting the contents of the carbon material and silicon material contained in the negative active material within the above ranges, the present invention can reduce the lithium consumption and irreversible capacity loss during the initial charge and discharge of the battery, and improve the charge capacity per unit mass.
[0083] For example, the negative electrode active material may include 95±2 parts by weight of graphite and 5±2 parts by weight of a mixture of silicon monoxide (SiO) particles and silicon dioxide (SiO2) particles uniformly mixed, relative to 100 parts by weight of the negative electrode composite layer. By adjusting the contents of the carbon material and silicon material contained in the negative electrode active material within the above ranges, the present invention can reduce the lithium consumption and irreversible capacity loss during initial charging and discharging of the battery, and improve the charging capacity per unit mass.
[0084] The negative electrode mixture layer may have an average thickness of 100 μm to 200 μm, specifically, 100 μm to 180 μm, 100 μm to 150 μm, 120 μm to 200 μm, 140 μm to 200 μm, or 140 μm to 160 μm.
[0085] In addition, the negative electrode current collector is not particularly limited as long as it has high conductivity without inducing chemical changes in the battery, and for example, copper, stainless steel, nickel, titanium, calcined carbon, etc. can be used. In the case of copper or stainless steel, it is also possible to use a material that has been surface-treated with carbon, nickel, titanium, silver, etc. In addition, the negative electrode current collector can be formed with fine irregularities on the surface to strengthen the binding force with the negative electrode active material, as with the positive electrode current collector, and can be in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc. In addition, the average thickness of the negative electrode current collector can be appropriately applied to 3 to 500 μm in consideration of the conductivity and total thickness of the negative electrode to be manufactured.
[0086] The separator is a thin insulating membrane having high ion permeability and mechanical strength, which is interposed between the positive and negative electrodes. The separator is not particularly limited as long as it is one commonly used in the industry. Specifically, a sheet or nonwoven fabric made of chemically resistant and hydrophobic polypropylene, glass fiber, or polyethylene may be used. In some cases, a composite separator in which inorganic particles / organic particles are coated with an organic binder polymer on a porous polymer substrate such as the sheet or nonwoven fabric may be used. When a solid electrolyte such as a polymer is used as the electrolyte, the solid electrolyte may also serve as the separator. The pore diameter of the separator may be an average of 0.01 to 10 μm, and the thickness may be an average of 5 to 300 μm.
[0087] Meanwhile, the positive and negative electrodes may be wound in a jelly roll form and housed in a cylindrical battery, a prismatic battery, or a pouch battery, or may be housed in a pouch battery in a folded or stack-and-folded form, but is not limited thereto.
[0088] The lithium salt-containing electrolyte according to the present invention may be composed of an electrolyte and a lithium salt. The electrolyte may be a non-aqueous organic solvent, an organic solid electrolyte, or an inorganic solid electrolyte.
[0089] Examples of the non-aqueous organic solvent that can be used include aprotic organic solvents such as N-methyl-2-pyrrolidinone, ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, gamma-butyrolactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphoric acid triester, trimethoxymethane, dioxolane derivatives, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, and ethyl propionate.
[0090] Examples of the organic solid electrolyte that can be used include polyethylene derivatives, polyethylene oxide derivatives, polypropylene oxide derivatives, phosphate polymers, polyagitation lysine, polyester sulfide, polyvinyl alcohol, polyvinylidene fluoride, and polymeric materials containing ionic dissociation groups.
[0091] Examples of the inorganic solid electrolyte that can be used include nitrides, halides, and sulfates of Li, such as Li3N, LiI, Li5NI2, Li3N-LiI-LiOH, LiSiO4, LiSiO4-LiI-LiOH, Li2SiS3, Li4SiO4, Li4SiO4-LiI-LiOH, and Li3PO4-Li2S-SiS2.
[0092] The lithium salt is a substance that is easily dissolved in a non-aqueous electrolyte, and examples of the lithium salt include LiCl, LiBr, LiI, LiClO4, LiBF4, and LiB 10 Cl 10 , LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li, (CF3SO2)2NLi, lithium chloroborane, lithium lower aliphatic carboxylates, lithium tetraphenylboronate, imides, etc. can be used.
[0093] In addition, for the purpose of improving charge / discharge characteristics, flame retardancy, etc., the electrolyte may contain, for example, pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, n-glyme, hexamethylphosphoric triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, aluminum trichloride, etc. In some cases, in order to impart non-flammability, a halogen-containing solvent such as carbon tetrachloride or trifluoroethylene may be further contained, and in order to improve high-temperature storage characteristics, carbon dioxide gas may be further contained, and fluoroethylene carbonate (FEC), propene sultone (PRS), etc. may be further contained.
[0094] The present invention will now be described in more detail with reference to examples and experimental examples.
[0095] However, the following examples and experimental examples are merely illustrative of the present invention, and the content of the present invention is not limited to the following examples and experimental examples.
[0096] <Examples 1 to 3 and Comparative Examples 1 to 4. Production of Lithium Secondary Batteries> a) Manufacturing of positive electrodes for lithium secondary batteries N-methylpyrrolidone was poured into a homo mixer, and LiNi as a positive electrode active material was mixed with 100 parts by weight of the positive electrode slurry solids. 0.6 Co 0.2 Mn 0.2 97 parts by weight of O2 and Li6CoO4 or Li6Co as a positive electrode additive 0.7 Zinc 0.30.8 parts by weight of O4; 0.7 parts by weight of a mixture (75:25 wt. / wt.) of carbon nanotubes (average size: 60±10 nm) and denka black (average size: 2±0.5 μm) as a conductive material; and 1.5 parts by weight of PVDF as a binder were weighed and added, and mixed at 2,000 rpm for 60 minutes to prepare a positive electrode slurry for a lithium secondary battery. The prepared positive electrode slurry was applied to one side of an aluminum current collector, dried at 100° C., and rolled to prepare a positive electrode. At this time, the total thickness of the positive electrode composite layer was 130 μm, and the total thickness of the prepared positive electrode was about 200 μm.
[0097] b) Manufacture of lithium secondary batteries A negative electrode slurry was prepared by preparing 84 parts by weight of natural graphite and 14 parts by weight of silicon (SiOx, where 1≦x≦2) particles as a negative electrode active material and 2 parts by weight of styrene butadiene rubber (SBR) as a binder, relative to 100 parts by weight of the negative electrode slurry solid content, in the same manner as in the method for producing the positive electrode slurry. At this time, the graphite used in the production of the negative electrode mixture layer was natural graphite (average particle size: 0.01 to 0.5 μm), and the silicon (SiOx) particles had an average particle size of 0.9 to 1.1 μm. The prepared negative electrode slurry was applied to one side of a copper current collector, dried at 100 ° C., and rolled to produce a negative electrode. At this time, the total thickness of the negative electrode mixture layer was 150 μm, and the total thickness of the produced negative electrode was about 250 μm.
[0098] The prepared positive and negative electrodes were laminated with a separator (thickness: about 16 μm) made of a porous polyethylene (PE) film between them, and E2DVC was injected as an electrolyte to assemble a full cell battery. Here, "E2DVC" refers to a type of carbonate-based electrolyte, a solution in which lithium hexafluorophosphate (LiPF6, 1.0M) and vinyl carbonate (VC, 2% by weight) are mixed with a mixture of ethylene carbonate (EC): dimethyl carbonate (DMC): diethyl carbonate (DEC) = 1:1:1 (volume ratio).
[0099] The fabricated full cell was initially charged at 22±2° C. under the conditions shown in Table 1 below to fabricate a lithium secondary battery.
[0100] [Table 1]
[0101] <Experimental Example> In order to evaluate the performance of the positive electrode for a lithium secondary battery according to the present invention, the following experiment was carried out.
[0102] a) Analysis of the cross-sectional structure of the positive electrode composite layer after initial charging In Examples 1 to 3 and Comparative Examples 1 to 4, the positive electrodes were separated from the initially charged lithium secondary batteries, and the positive electrode composite layers were peeled off from the separated positive electrodes to prepare test pieces. The cross sections of the prepared test pieces were analyzed using a scanning electron microscope (SEM). The results are shown in FIG.
[0103] As a result, as shown in FIG. 1, the positive electrode composite layer separated from the lithium secondary batteries of Examples 1 to 3 was found to have a structure in which the positive electrode active material particles, identified as white, were densely packed, and had no cracks and / or cracks, and fine needle-like cracks were formed in an island shape at the inside and surface of some metal oxide, specifically, positive electrode additive particles, identified as gray, and at the boundaries between the positive electrode additive particles. At this time, the needle-like cracks had a structure in which first cracks having an average thickness of 10 nm to 100 nm and an average length of 150 nm to 400 nm and second cracks having an average thickness of 500 nm to 750 nm and an average length of 5.5 μm to 7.3 μm were mixed, and it was confirmed that the first cracks and the second cracks were partially irregularly connected to form a line shape (e.g., a straight line, a curve, etc.). In addition, it was shown that the crack structure occupies 0.5 to 5% of the entire cross-sectional area.
[0104] In contrast, the positive electrode composite layers separated from the lithium secondary batteries of Comparative Examples 1 to 4 had a crack structure formed across the entire cross section of the composite layer, or had a structure in which regions having crack structures in the positive electrode additive particles were formed in the form of islands, as in the positive electrode composite layers of the Examples, but it was confirmed that the average thickness and average length of the formed cracks were significantly larger than those of the Examples and accounted for 10% or more of the area of the entire cross section of the composite layer.
[0105] From these results, it can be seen that in the positive electrode for a lithium secondary battery according to the present invention, cracks formed in the positive electrode mixture layer can be controlled during the activation step.
[0106] B) Evaluation of the cumulative amount of gas generated during charging and discharging after the initial charge The lithium secondary batteries initially charged in Examples 1 to 3 and Comparative Examples 1 to 4 were subjected to a degassing process, and then discharged to a cut-off voltage of 2 V at a discharge current of 0.1 C. After that, the secondary batteries from which the internal gas had been removed were repeatedly charged and discharged 50 times at 45° C., 4.5 V and 1.0 C. In this case, the amount of gas generated during each charge and discharge was measured, and the cumulative amount of gas generated after the initial charge and discharge was calculated. The results are shown in Table 2 below.
[0107] C) Evaluation of cycle life performance The lithium secondary batteries initially charged in Examples 1 to 3 and Comparative Examples 1 to 4 were subjected to a degassing process, and then discharged to an end voltage of 2 V at a discharge current of 0.1 C. Then, 100 charge / discharge cycles (n=100) were performed at 25° C. under the conditions of a charge end voltage of 4.25 V, a discharge end voltage of 2.5 V, and 0.5 C / 0.5 C, to measure the capacity retention (Capacity Retention [%]). The capacity retention was calculated using the following formula 1, and the results are shown in Table 2 below:
[0108] [Formula 1] Capacity retention rate (%) = (discharge capacity after 100 charge / discharge cycles / discharge capacity after 1 charge / discharge cycle) x 100
[0109] [Table 2]
[0110] As shown in Table 2, the positive electrode for a lithium secondary battery according to the present invention contains the positive electrode additive represented by Chemical Formula 1, and at the same time, has a specific crack structure introduced into the cross section of the positive electrode mixture layer after initial charging, thereby showing excellent safety and electrical performance of the lithium secondary battery.
[0111] Specifically, it was confirmed that the amount of gas generated during charging and discharging was significantly reduced after degassing of the gas generated during initial charging and discharging of the lithium secondary battery prepared in the examples. In addition, it was confirmed that the lithium secondary battery had a high initial charging capacity of 103 mAh or more and a high capacity retention rate of 95% or more.
[0112] On the other hand, the lithium secondary battery manufactured in the comparative example was shown to generate a large amount of gas due to accelerated decomposition of the electrolyte during charging and discharging after the initial charging (activation). In addition, it was confirmed that the lithium secondary battery in the comparative example had a low initial charging capacity of less than 102 mAh, and the capacity retention rate after 100 charge / discharge cycles was less than 94% due to the decomposition of the electrolyte.
[0113] From these results, the positive electrode for a lithium secondary battery according to the present invention contains a positive electrode additive represented by Chemical Formula 1, and has a positive electrode composite layer including a region having an acicular crack structure in its cross section after initial charging (activation). This reduces the amount of gas generation, such as oxygen, that is generated by the positive electrode additive, which is an irreversible additive, during the charge / discharge process after initial charging, and ensures a path for the movement of lithium ions and / or electrons, thereby providing an excellent effect of improving the battery safety and electrical performance of the lithium secondary battery.
[0114] Although the present invention has been described above with reference to preferred embodiments, it will be understood that a person skilled in the art or having ordinary knowledge in the art can make various modifications and variations to the present invention without departing from the spirit and technical scope of the present invention as described in the claims below.
[0115] Therefore, the technical scope of the present invention should not be limited to the contents described in the detailed description of the specification, but should be defined by the claims.
Claims
1. A positive electrode current collector; A positive electrode mixture layer is formed on at least one surface of the positive electrode current collector and contains a positive electrode active material and a positive electrode additive represented by the following chemical formula 1: After the initial charge, the cross-sectional structure of the positive electrode mixture layer is as follows: a first region having a dense structure filled with first metal oxide particles; a second region having an acicular crack structure inside and outside the second metal oxide particle; The second region occupies 0.001 to 10% of the total cross-sectional area of the positive electrode mixture layer. [Chemical formula 1] Li p Co (1-q) M 1 q O 4 In the above Chemical Formula 1, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; p and q are 5≦p≦7 and 0≦q≦0.5, respectively.
2. A positive electrode current collector, A positive electrode mixture layer is formed on at least one surface of the positive electrode current collector and contains a positive electrode active material and a positive electrode additive represented by the following chemical formula 1: After the initial charge, the cross-sectional structure of the positive electrode mixture layer is as follows: a first region having a dense structure filled with first metal oxide particles; a second region having an acicular crack structure inside and outside the second metal oxide particle; The needle-like crack structure has a structure in which first cracks having an average thickness of 10 nm to 100 nm and an average length of 150 nm to 400 nm are mixed with second cracks having an average thickness of 500 nm to 750 nm and an average length of 5.5 μm to 7.3 μm; The first cracks and the second cracks are partially irregularly connected to form a line shape. [Chemical formula 1] Li p Co (1-q) M 1 q O 4 In the above Chemical Formula 1, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; p and q are 5≦p≦7 and 0≦q≦0.5, respectively.
3. The positive electrode for a lithium secondary battery according to claim 1 , wherein the second region has a structure in which the second region is dispersed in an island form within the first region.
4. The positive electrode additive has a space group of P4 2 3. The positive electrode for a lithium secondary battery according to claim 1 or 2, having a tetragonal structure in which N is a cubic lattice constant.
5. The positive electrode for a lithium secondary battery according to claim 1 or 2, wherein the positive electrode active material is a lithium metal composite oxide represented by the following chemical formula 2: [Chemical formula 2] Li x [Ni y Co z Mn w M 2 v ]O u In the above Chemical Formula 2, M 2 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; x, y, z, w, v, and u are within the ranges of 1.0≦x≦1.30, 0.1≦y<0.95, 0.01<z≦0.5, 0.01<w≦0.5, 0≦v≦0.2, and 1.5≦u≦4.5, respectively.
6. 3. The positive electrode for a lithium secondary battery according to claim 1, wherein the positive electrode mixture layer further contains one or more conductive materials selected from the group consisting of natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, and carbon fiber.
7. A lithium secondary battery comprising the positive electrode according to claim 1 or 2, a negative electrode, and a separator located between the positive electrode and the negative electrode.
8. The negative electrode includes a negative electrode current collector and a negative electrode mixture layer located on at least one surface of the negative electrode current collector and containing a negative electrode active material, The lithium secondary battery according to claim 7 , wherein the negative electrode active material contains a carbon material and a silicon material.
9. The silicon material is composed of silicon (Si) particles and silicon oxide (SiO X 9. The lithium secondary battery according to claim 8, comprising one or more of the following particles:
10. The lithium secondary battery according to claim 8, wherein the silicon material is contained in an amount of 1 to 20 parts by weight per 100 parts by weight of the negative electrode mixture layer.
11. 9. The lithium secondary battery according to claim 8, wherein the carbon material comprises at least one selected from the group consisting of natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, carbon fiber, graphene, and carbon nanotubes.
Citation Information
Patent Citations
Lithium battery and manufacturing method
JP2004207055A
Lithium ion secondary battery
JP2007287446A
Cathode active material for non-aqueous electrolyte secondary battery, its manufacturing method, and nonaqueous secondary battery using this cathode active material
JP2008152923A
Power storage device
JP2015088268A
Positive electrode additive, method for producing the same, positive electrode and lithium secondary battery containing the same