Laser Diode
The laser diode design addresses high oscillation threshold currents by optimizing the semiconductor stack and mesa structure to reduce dislocations, achieving efficient continuous oscillation.
Patent Information
- Application Number
- JP2021055272
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-29
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2041-03-29
AI Technical Summary
Conventional ultraviolet laser diodes using nitride semiconductors face challenges with high oscillation threshold currents due to film relaxation and dislocations during the formation and processing of the light-emitting layer, hindering continuous oscillation required for practical applications.
A laser diode design incorporating a nitride semiconductor substrate with a semiconductor stack, including a first conductivity type cladding layer, a light-emitting layer with quantum wells, and a second conductivity type cladding layer, featuring a mesa structure with a first and second ridge region separated by a groove, optimized to reduce dislocations and strain, thereby lowering the oscillation threshold current.
The design effectively suppresses dislocations, reducing the oscillation threshold current and enhancing the efficiency of the laser diode, enabling stable continuous oscillation.
Smart Images

Figure 0007594257000002 
Figure 0007594257000003 
Figure 0007594257000004
Abstract
Description
[Technical field]
[0001] The present disclosure relates to laser diodes. [Background technology]
[0002] Conventionally, nitride semiconductors have been used as materials for forming laser diodes. Nitride semiconductors have a direct transition recombination mode, and therefore are suitable as materials for laser diodes in that they can provide high recombination efficiency and high optical gain. As an example of a laser diode using such a nitride semiconductor, a technology for oscillating a current injection type laser diode in the ultraviolet region has been disclosed (for example, Non-Patent Document 1). [Prior art documents] [Non-patent literature]
[0003] [Non-Patent Document 1] Zhang et al., Applied Physics Express 12, 124003(2019) Summary of the Invention [Problem to be solved by the invention]
[0004] The ultraviolet laser diodes described above are pulse driven, and continuous oscillation is required for practical applications. This continuous oscillation requires a reduction in the oscillation threshold current. The oscillation threshold current is significantly deteriorated (increased) by relaxation of the light emitting layer during the film formation process and processing process of the laser diode. The oscillation threshold current is also deteriorated by the introduction of dislocations into the light emitting layer. An object of the present disclosure is to provide a laser diode with a low lasing threshold current. [Means for solving the problem]
[0005] In order to solve the above-mentioned problems, a laser diode according to an embodiment of the present disclosure includes a nitride semiconductor substrate containing Al, a semiconductor laminate disposed on the nitride semiconductor substrate, and an electrode directly connected to a top of the semiconductor laminate, the semiconductor laminate including: a first-conductivity-type cladding layer including a nitride semiconductor layer of a first conductivity type disposed on the nitride semiconductor substrate; a light-emitting layer formed of a nitride semiconductor including one or more quantum wells disposed on the first-conductivity-type cladding layer; and a second-conductivity-type cladding layer including a nitride semiconductor of a second conductivity type disposed on the light-emitting layer, a part of the semiconductor laminate having a mesa structure protruding beyond a surface of a part of the first-conductivity-type cladding layer, and a region of the mesa structure farthest from the nitride semiconductor substrate includes the second-conductivity-type cladding layer, the laser diode including: a first ridge region having a long side and a short side in a plan view; and a second ridge region having a long side and a short side disposed at a position facing each of the long sides of the first ridge region across a separation groove, the length of the short side of the second ridge region in a plan view being 5 μm or more and 12 μm or less. It should be noted that the above summary of the invention does not list all of the features of the present disclosure. Effect of the Invention
[0006] According to one aspect of the present disclosure, a laser diode with a low lasing threshold current can be provided. [Brief description of the drawings]
[0007] [Figure 1] 1 is a schematic plan view illustrating a configuration example of a laser diode according to an embodiment of the present disclosure. [Diagram 2] 1 is a schematic cross-sectional view illustrating a configuration example of a laser diode according to an embodiment of the present disclosure. [Diagram 3] 10 is a schematic cross-sectional view illustrating another configuration example of a laser diode according to an embodiment of the present disclosure. FIG. [Figure 4] 10 is a schematic plan view illustrating another configuration example of a laser diode according to an embodiment of the present disclosure. FIG. [Diagram 5] 10 is a schematic cross-sectional view illustrating another configuration example of a laser diode according to an embodiment of the present disclosure. FIG. [Figure 6] 10 is a schematic cross-sectional view illustrating another configuration example of a laser diode according to an embodiment of the present disclosure. FIG. [Figure 7] 10 is a schematic cross-sectional view illustrating another configuration example of a laser diode according to an embodiment of the present disclosure. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] The laser diode according to the present disclosure will be described below through embodiments, but the following embodiments do not limit the invention according to the claims. Also, not all of the combinations of features described in the embodiments are necessarily essential to the solution of the invention.
[0009] 1. Embodiment A laser diode according to an embodiment of the present disclosure will be described. (1.1) Structure of a laser diode The laser diode according to this embodiment includes a nitride semiconductor substrate including Al, a semiconductor laminate disposed on the nitride semiconductor substrate, and an electrode directly connected to the top of the semiconductor laminate. The semiconductor laminate includes a first conductive type cladding layer including a first conductive type nitride semiconductor layer disposed on the nitride semiconductor substrate, a light emitting layer formed of a nitride semiconductor including one or more quantum wells disposed on the first conductive type cladding layer, and a second conductive type cladding layer including a second conductive type nitride semiconductor disposed on the light emitting layer. A part of the semiconductor laminate is a mesa structure protruding from a part of the surface of the first conductive type cladding layer. The region of the mesa structure farthest from the nitride semiconductor substrate includes the second conductive type cladding layer, and includes a rectangular first ridge region having long sides and short sides in a plan view, and a rectangular second ridge region having long sides and short sides disposed at positions facing each of the long sides of the first ridge region across a separation groove. The length of the short side of the second ridge region in a plan view is 5 μm or more and 12 μm or less. Each layer of the laser diode will now be described in detail.
[0010] (Nitride semiconductor substrate) The nitride semiconductor substrate (hereinafter sometimes referred to as substrate) contains a nitride semiconductor containing Al. The nitride semiconductor containing Al is, for example, AlN. That is, the substrate is preferably an AlN single crystal substrate. The nitride semiconductor containing Al is not limited to AlN, and may be, for example, AlGaN. For example, when the substrate is a nitride semiconductor single crystal substrate such as AlN or AlGaN, the difference in lattice constant with the nitride semiconductor layer formed on the substrate becomes small, and the nitride semiconductor layer is grown in a lattice-matched system, thereby reducing threading dislocations. The threading dislocation density of the substrate is 5×10 4 cm -2 In particular, from the viewpoint of reducing the oscillation threshold current, the threading dislocation density is preferably 1×10 3 More than 1×10 4 cm -2 It is more preferable that:
[0011] Here, the wording "comprises" in the expression "comprises a nitride semiconductor" means that the layer mainly contains a nitride semiconductor, but this expression also includes cases where other elements are included. Specifically, this expression also includes cases where the composition of this layer is slightly changed by adding a small amount of an element other than the nitride semiconductor (for example, elements such as Ga (when Ga is not the main element), In, As, P, or Sb, at a few percent or less). In expressions of the composition of other layers, the wording "comprises" has a similar meaning. Also, the small amount of elements contained is not limited to the above.
[0012] The substrate may be doped n-type or p-type with donor or acceptor impurities, and may be a mixed crystal of a nitride semiconductor such as AlN and sapphire (Al2O3), Si, SiC, MgO, Ga2O3, ZnO, GaN, or InN.
[0013] As an example, the substrate preferably has a layer thickness of 100 μm or more and 600 μm or less. In addition, examples of the plane orientation include the c-plane (0001), a-plane (11-20), m-plane (10-10), etc., but a c-plane (0001) substrate is more preferable. Furthermore, it can be formed on a plane inclined by a certain angle (for example, -4° to 4°, preferably -0.4° to 0.4°) from the normal direction of the c-plane (0001), but it is not limited thereto.
[0014] (First conductive type cladding layer) The first conductive type cladding layer is formed on the substrate. Here, for example, in the expression "the first conductive type cladding layer is formed on the substrate", the word "on" means that the first conductive type cladding layer is formed on one surface of the substrate. Also, the above expression includes the case where another layer further exists between the substrate and the first conductive type cladding layer. In the relationship between other layers as well, the word "on" has the same meaning. For example, when the second conductive type cladding layer is formed on the first conductive type waveguide layer via an electron blocking layer as described later, it is also included in the expression "the second conductive type cladding layer is formed on the first conductive type waveguide layer". In the description of this embodiment, "the first conductive type" and "the second conductive type" each mean a semiconductor having a different conductive type. For example, when one is n-type conductivity, the other is p-type conductivity.
[0015] The first conductive type cladding layer is a layer of a nitride semiconductor containing Al and Ga. The first conductive type cladding layer is, for example, Al a Ga (1-a) formed by N (0 < a < 1). Thereby, when a material corresponding to the bandgap energy in the deep ultraviolet region is formed as the light-emitting layer, it is possible to enhance the crystallinity of the light-emitting layer and improve the light-emitting efficiency. From the viewpoint of realizing high light-emitting efficiency, the nitride semiconductor constituting the first conductive type cladding layer is preferably a mixed crystal of AlN and GaN. Also, from the viewpoint of growing with complete strain with respect to the substrate, the first conductive type cladding layer is more preferably formed by Al a Ga (1-a) N (0.6 < a ≦ 0.8). The first-conductivity-type clad layer may be a gradient layer in which the Al composition increases as the distance from the substrate increases for the purpose of controlling the longitudinal conductivity. In this case, the limitation on the Al composition described above can be the Al composition averaged over the film thickness of the first-conductivity-type clad layer with respect to the Al composition at the position in the film thickness direction within the first-conductivity-type clad layer.
[0016] When the first-conductivity-type clad layer is an n-type conductive semiconductor layer, it may contain impurities such as group V elements other than N such as In, P, As, Sb, and impurities such as C, H, F, O, Mg, Si, etc., but the types of impurity elements are not limited to this. From the viewpoints of reducing electrical resistance and the availability of raw materials, the impurity contained in the first-conductivity-type clad layer is preferably Si, and the impurity concentration is 5×10 18 cm -3 or more and 5×10 19 cm -3 or less.
[0017] The first-conductivity-type clad layer preferably has a layer thickness of 200 nm or more and 800 nm or less, more preferably has a layer thickness of 300 nm or more and 750 nm or less, and even more preferably has a layer thickness of 300 nm or more and 500 nm or less, from the viewpoints of lattice relaxation within the first-conductivity-type clad layer and film resistance.
[0018] (Light-emitting layer) The light-emitting layer is a layer of a nitride semiconductor containing Al and Ga. The nitride semiconductor contained in the light-emitting layer is preferably a mixed crystal of, for example, AlN and GaN from the viewpoint of realizing high luminous efficiency, for example, Al b Ga (1-b) N (0 < b < 1). In addition to N, the light-emitting layer may contain impurities such as group V elements other than N such as P, As, Sb, and impurities such as C, H, F, O, Mg, Si, etc., but it is not limited to this.
[0019] Also, the light-emitting layer can take either a multiple quantum well structure or a single quantum well structure. Although it depends on the longitudinal conductivity of the first-conductivity-type clad layer and the second-conductivity-type clad layer, the number of quantum well structures is preferably any one of 1 to 3. Also, for the purpose of reducing the influence of crystal defects in the light-emitting layer, etc., elements such as Si, Sb, P, etc. may be contained in part or all of the light-emitting layer at 1×10 15 cm -3 or more.
[0020] (Waveguide layer) From the viewpoint of light confinement, the laser diode of this embodiment may be provided with a waveguide layer that is formed above and below the light-emitting layer so as to sandwich the light-emitting layer and has the effect of confining the light emitted from the light-emitting layer within the light-emitting layer. The waveguide layer is preferably composed of two layers: a first-conductivity-type waveguide layer disposed on the first-conductivity-type clad layer side with respect to the light-emitting layer and a second-conductivity-type waveguide layer disposed on the second-conductivity-type clad layer side with respect to the light-emitting layer. That is, the laser diode of this embodiment may include, for example, a first-conductivity-type waveguide layer disposed between the first-conductivity-type clad layer and the light-emitting layer to confine light to the light-emitting layer, and a second-conductivity-type waveguide layer disposed between the second-conductivity-type clad layer and the light-emitting layer to confine light to the light-emitting layer.
[0021] From the viewpoint of light confinement, the waveguide layer is preferably a nitride semiconductor containing Al and Ga having a bandgap higher in energy than the light-emitting layer. The waveguide layer preferably has an Al composition and a film thickness that increase the overlap of the electric field intensity distribution of the light standing in the device and the light-emitting layer. From the viewpoint of carrier confinement in the light-emitting layer, when the light-emitting layer is Al b Ga (1-b) N (0 < b < 1) and the waveguide layer is Al c Ga (1-c) N (0 < c < 1), it is more preferable that b < c and c ≧ b + 0.05. For example, when taking a light-emitting layer with an emission wavelength of 265 nm as an example, b = 0.52, and c is preferably 0.57 or more. Also, from the viewpoints of light confinement and sheet resistance, the total film thickness of the first-conductivity-type waveguide layer and the second-conductivity-type waveguide layer is preferably 70 nm or more and 150 nm or less.
[0022] Although it is preferable that the Al compositions of the first conductivity type waveguide layer and the second conductivity type waveguide layer are each uniform in the film thickness direction, this is not always the case. In order to avoid light absorption by a metal (for example, the second electrode) present above the second conductivity type cladding layer described later, the Al composition of the second conductivity type waveguide layer may be higher than the Al composition of the first conductivity type waveguide layer. For the same purpose, the film thickness of the second conductivity type waveguide layer may be thicker than the film thickness of the first conductivity type waveguide.
[0023] When the first conductivity type waveguide layer is an n-type conductive semiconductor layer, in order to obtain the same conductivity type as the first conductivity type cladding layer, impurities other than N such as group V elements other than N such as P, As, Sb, and impurities such as H, C, O, F, Mg, Si may be mixed, but this is not always the case.
[0024] (Second conductivity type cladding layer) The second conductivity type cladding layer is a nitride semiconductor layer containing Al and Ga having second conductivity type conductivity, formed on the light emitting layer. The second conductivity type cladding layer is formed, for example, by Al d Ga (1-d) N (0 < d < 1). When a waveguide layer (second conductivity type waveguide layer) is provided on the light emitting layer, the second conductivity type cladding layer is formed on the waveguide layer (second conductivity type waveguide layer). Thereby, the second conductivity type cladding layer is easily lattice-matched to the light emitting layer or the waveguide layer, and it is possible to suppress the threading dislocation density.
[0025] The second conductivity type cladding layer has conductivity sufficient to inject carriers (electrons or holes) into the light emitting layer, and if it is possible to increase the overlap between the electric field strength distribution of the standing light mode in the device and the light emitting layer (that is, increase the light confinement), the conductivity type is not particularly limited. The second conductivity type cladding layer may be, for example, p-type AlGaN doped with Mg. Also, when the second conductivity type cladding layer is a p-type conductive semiconductor layer, impurities such as group V elements other than N such as P, As, Sb, and impurities such as C, H, F, O, Mg, Si may be mixed, but the types of impurity elements are not limited to this.
[0026] From the perspective of more efficiently injecting carriers into the light-emitting layer, the p-type clad layer is Al with an Al composition e that decreases in the direction away from the upper surface of the substrate, e Ga (1-e) a compositionally graded layer (p-type vertical conduction layer) formed of N, and Al f Ga (1-f) preferably includes a p-type lateral conduction layer containing N (0 < f ≦ 1). Hereinafter, the p-type vertical conduction layer and the p-type lateral conduction layer will be described.
[0027] (p-type vertical conduction layer) The p-type vertical conduction layer is a layer that constitutes the region on the light-emitting layer side of the p-type clad layer. The p-type vertical conduction layer is a layer containing Al e Ga (1-e) N. The profile (gradient) of the Al composition e in the p-type vertical conduction layer may decrease continuously or discontinuously. Here, "decreasing discontinuously" means including a portion where the Al composition e is the same (constant in the film thickness direction) in a part of the film of the p-type vertical conduction layer. That is, the p-type vertical conduction layer may include a portion where the Al composition e does not decrease in the direction away from the substrate, but does not include an increasing portion.
[0028] From the perspective of lattice matching, the film thickness of the p-type vertical conduction layer is preferably 500 nm or less. Further, from the perspectives of light confinement in the light-emitting layer and carrier injection, the film thickness of the p-type vertical conduction layer is more preferably 250 nm or more and 450 nm or less, and even more preferably 300 nm or more and 400 nm or less.
[0029] For the purpose of suppressing impurity diffusion and the like, in the region of the second-conductivity-type vertical conduction layer close to the light-emitting layer, impurities such as H, Mg, Be, Zn, Si, and B are not doped (not intentionally mixed in), that is, it is preferably in an undoped state. Here, "undoped" means that the above-mentioned impurities are not intentionally supplied as elements in the process of forming the target layer. However, when elements derived from raw materials and manufacturing equipment are mixed in the following range of 1×10 16 cm -3 or less, this is not the case. Also, the undoped region of the second-conductivity-type vertical conduction layer includes at least the boundary with the light-emitting layer (the second-conductivity-type waveguide layer when the second-conductivity-type waveguide layer is provided), but its size is not limited. For example, all regions of the second-conductivity-type vertical conduction layer may be in an undoped state. Also, as another example, 50% of the region of the second-conductivity-type vertical conduction layer close to the light-emitting layer may be in an undoped state. Also, as another example, about 10% of the region of the second-conductivity-type vertical conduction layer close to the light-emitting layer may be in an undoped state.
[0030] (Second-conductivity-type lateral conduction layer) The second-conductivity-type lateral conduction layer is a layer that constitutes the region of the second-conductivity-type cladding layer on the side opposite to the light-emitting layer, and is formed on the second-conductivity-type vertical conduction layer. The second-conductivity-type lateral conduction layer is a layer containing Al f Ga (1-f) N (0 < f ≦ 1). Here, the Al composition f on the surface of the second-conductivity-type lateral conduction layer facing the second-conductivity-type vertical conduction layer is preferably greater than the minimum value of the Al composition e of the second-conductivity-type vertical conduction layer. For the purpose of controlling the longitudinal resistivity of the second-conductivity-type lateral conduction layer and the like, impurities such as H, Mg, Be, Zn, Si, and B may be intentionally mixed in. The amount of impurities mixed in may be, for example, 1×10 19 cm -3 or more and 5×10 21 cm -3 or less.
[0031] The thickness of the second conductivity type lateral conduction layer is preferably 20 nm or less, more preferably 10 nm or less, and further preferably 5 nm or less, from the viewpoint of facilitating quantum transmission of carriers through the second conductivity type lateral conduction layer.
[0032] When a second-conductivity-type contact layer (described later) is provided on the second-conductivity-type lateral conduction layer, the Al composition at the interface between the second-conductivity-type lateral conduction layer and the second-conductivity-type contact layer is preferably smaller than the Al composition in the second-conductivity-type contact layer and is completely distorted with respect to the substrate. Such a second-conductivity-type lateral conduction layer can improve the lateral conductivity by guiding carriers at the interface as the net internal electric field accumulated on the surface and inside near the surface of the second-conductivity-type lateral conduction layer becomes negative.
[0033] In this way, the second conductive type vertical conductive layer generates carriers (for example, holes when the second conductive type vertical conductive layer is formed of a p-type semiconductor) by the polarization doping effect, and has the effect of efficiently injecting the carriers into the active layer in the light emitting layer. Therefore, by providing the second conductive type vertical conductive layer on the light emitting layer, the carrier injection efficiency of the laser diode can be increased and the threshold voltage can be reduced. In addition, the second-conductivity-type lateral conduction layer has the effect of spreading the carrier distribution, which is narrowed by the electric field concentrated under the electrode, in the lateral direction (within the plane of the second-conductivity-type lateral conduction layer). Due to this effect, the second-conductivity-type lateral conduction layer can increase the efficiency of carrier injection into the light-emitting layer, just like the second-conductivity-type vertical conduction layer.
[0034] (Middle class) Between the second conductive cladding layer and the waveguide, i.e., between the second conductive vertical conductive layer and the second conductive waveguide layer, an Al composition g increases in a direction away from the top surface of the substrate from the viewpoint of improving the carrier conductivity and / or from the viewpoint of forming the second conductive lateral conductive layer and the second conductive contact layer with perfect distortion. g Ga (1-g)An intermediate layer composed of N(0 < g ≦ 1.0) can be provided. The intermediate layer may be a mixed crystal that is not a bandgap that does not absorb light of a desired emission wavelength, and preferably has a film thickness of 50 nm or less, and may be an undoped layer containing no impurities.
[0035] (Second conductive type contact layer) The semiconductor laminate portion of the laser diode of this embodiment may further include a second conductive type contact layer disposed on the second conductive type clad layer. The nitride semiconductor constituting the second conductive type contact layer is preferably formed of, for example, GaN, AlN, or InN and a mixed crystal containing them, and more preferably a nitride semiconductor containing GaN.
[0036] The second conductive type contact layer may be mixed with impurities other than N such as P, As, Sb, and impurities such as C, H, F, O, Mg, Si, Be. From the versatility of the source gas, the impurity contained in the second conductive type contact layer is preferably Mg. From the viewpoint of reducing contact resistance, the concentration of Mg is 8×10 19 cm -3 or more and 5×10 21 cm -3 or less, and preferably 5×10 20 cm -3 or more and 5×10 21 cm -3 or less is more preferable.
[0037] Also, the layer thickness of the second conductive type contact layer is preferably 1 nm or more and 20 nm or less. The thinner the layer thickness of the second conductive type contact layer, the higher the carrier injection efficiency of the laser diode, and the thicker the layer thickness, the lower the carrier injection efficiency.
[0038] (Electron blocking layer) The semiconductor laminate of the laser diode of this embodiment may further include an electron blocking layer above the light emitting layer, the electron blocking layer having a band gap larger than that of the second conductive type waveguide layer. The electron blocking layer may be provided, for example, inside the second conductive type waveguide layer, between the second conductive type waveguide layer and the light emitting layer, or between the second conductive type waveguide layer and the second conductive type vertical conductive layer. The thickness of the electron blocking layer is preferably 30 nm or less, more preferably 20 nm or less, and even more preferably 15 nm or less, so that carriers (holes) can easily quantum-transport through the electron blocking layer.
[0039] (Mesa and ridge structures) The mesa structure is formed to electrically separate the second conductive type layer from the first conductive type layer. The mesa structure is a structure in which a part of the semiconductor laminate is removed. Here, the "semiconductor laminate" refers to at least the first conductive type cladding layer, the light emitting layer, and the second conductive type cladding layer, and also includes the above-mentioned waveguide layers (the first conductive type waveguide layer and the second conductive type waveguide layer), the intermediate layer, and the second conductive type contact layer, if these layers are provided.
[0040] From the viewpoint of current confinement of the laser and amplification by reflection at the end facets, it is preferable that the mesa structure is rectangular in plan view with long and short sides, with the long sides extending in the <1-100> direction. This is because when obtaining the resonator mirror end faces of the laser resonator by various methods such as cleavage and etching, the atomically flat (1-100) surface is the easiest to form the resonator mirror end faces. Here, the direction of the long sides can also be interpreted as the laser resonance direction. In other words, the mesa structure has a resonator in which the end faces parallel to the (1-100) crystal plane of the nitride semiconductor substrate serve as resonator mirror end faces. As a result, the laser diode according to this embodiment is an edge-emitting laser diode in which the mesa structure emits light in the <1-100> direction.
[0041] The ridge structure is formed to further confine the current in the mesa structure. The ridge structure can efficiently increase the current density by confining the current. For this reason, like the mesa structure, the ridge structure is preferably rectangular in plan view having long and short sides, with the long sides extending in the <1-100> direction.
[0042] When forming multiple ridge structures in a mesa structure, the region that will become the ridge structure can be protected with a mask and etched with inductively coupled plasma (ICP) or the like to form a separation groove outside the region that will become the ridge structure. This makes it possible to form a first ridge region and a second ridge region that are separated by the separation groove. In this case, the width (length of the short side) of the second ridge region is 5 μm or more and 12 μm or less, and preferably 5 μm or more and 7 μm or less.
[0043] In this case, from the viewpoint of confining the current, it is preferable that the separation groove is formed at least up to the second cladding layer and has a depth that exposes the second cladding layer. Also, the position and shape of the second ridge region are not limited as long as it is disposed in a position facing the first ridge region across the separation groove, but from the viewpoint of process such as mask alignment, it is preferable that an end of the second ridge region substantially overlaps with any of the ends of the region directly below the second ridge region in the semiconductor laminate.
[0044] For example, the first ridge region may be formed at the center of the width direction of the mesa structure (the direction of the short side of the mesa structure in a plan view). Two or more second ridge regions may be formed parallel to the first ridge region in the width direction of the mesa structure, or only one second ridge region may be formed on a side facing one of the long sides of the first ridge region in the width direction of the mesa structure in parallel to the first ridge region. When only one second ridge region is formed on a side facing one of the long sides of the first ridge region in the width direction of the mesa structure in parallel to the first ridge region, the first electrode may be formed on the side where the second ridge region is formed as viewed from the first ridge region in a plan view. The following description is based on the premise that two or more second ridge regions are formed parallel to the first ridge region in the width direction of the mesa structure, but is not limited thereto. The first ridge region is in direct contact with the second electrode and has the functions of confining the current and oscillating the laser, while the second ridge region has the functions of relieving distortion induced in the mesa structure and preventing dislocations from extending inward from the edge of the mesa structure.
[0045] The mesa structure can be formed by etching the semiconductor laminate. Depending on the etching conditions at this time, strain is introduced into the end face of the mesa structure. This is because the semiconductor laminate grows in a pseudomorphic manner in which it is lattice-matched to the substrate, and strain is accumulated in the semiconductor laminate. When heat treatment is performed in the manufacturing process of the laser diode, this strain is released and dislocations are introduced into the entire semiconductor laminate. In this case, dislocations are also introduced into the light-emitting layer formed above the semiconductor laminate. At this time, if dislocations are introduced into the first ridge region, the oscillation threshold current of the laser diode is significantly deteriorated. For this reason, by forming the second ridge region at the end of the mesa structure, strain relaxation occurs only in the second ridge region, and dislocation introduction into the first ridge region can be avoided.
[0046] From the viewpoint of strain relaxation, the width (length in the short side direction) of the second ridge region is preferably shorter than the length in the short side direction of the separation groove, and is preferably 20% to 60% of the entire width (length in the short side direction) of the mesa structure, and more preferably 20% to 35%. The width (length in the short side direction) of the separation groove is preferably 9 μm to 23 μm, and more preferably 19 μm to 23 μm. As described above, it is important from the viewpoint of the oscillation threshold current to stop dislocations in the second ridge region. Therefore, it is preferable that only the region directly under the second ridge region has a plurality of dislocation lines extending in the crystal orientation <1-100> direction, and it is preferable that no dislocation lines extending in the <1-100> direction exist in the region directly under the first ridge region. More preferably, no dislocation lines extending in the <1-100> direction exist in the region directly under the first ridge region and the separation groove. Furthermore, it is preferable that the number of dislocation lines extending in the <1-100> direction in the region directly under the second ridge region is greater than the number of dislocation lines extending in directions other than the <1-100> direction. In this case, from the viewpoint of preventing the extension of dislocations into the inside of the first ridge region, it is preferable that the Burgers vector of the dislocation line in the region directly under the second ridge region has a component in the <11-20> direction.
[0047] (electrode) The laser diode can be formed by a second electrode disposed on the second conductivity type cladding layer and a first electrode disposed on the first conductivity type cladding layer, where the first electrode is formed in electrical contact with the first conductivity type cladding layer and the second electrode is formed in electrical contact with the second conductivity type cladding layer. The first electrode can be disposed, for example, on the back side of the substrate, and is disposed on the first conductive clad layer exposed by removing layers above the first conductive clad layer of the semiconductor laminate by, for example, chemical etching or dry etching.
[0048] When the first conductive type cladding layer is an n-type cladding layer, the first electrode is formed of a metal such as Al, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Co, Rh, Ir, Ni, Pd, Pt, Cu, Ag, Au, Zr, or a mixed crystal of these metals, or a conductive oxide such as ITO or Ga2O3. When the first conductive type cladding layer is a p-type cladding layer, the first electrode is formed of a metal such as Ni, Au, Pt, Ag, Rh, Pd, Pt, Cu, Al, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Co, Ir, Zr, or a mixed crystal of these metals, or a conductive oxide such as ITO or Ga2O3.
[0049] When the second conductive type cladding layer is an n-type cladding layer, the second electrode is formed of a metal such as Al, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Co, Rh, Ir, Ni, Pd, Pt, Cu, Ag, Au, Zr, or a mixed crystal of these metals, or a conductive oxide such as ITO or Ga2O3. When the second conductive type cladding layer is a p-type cladding layer, the second electrode is formed of a metal such as Ni, Au, Pt, Ag, Rh, Pd, Pt, Cu, Al, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Co, Ir, Zr, or a mixed crystal of these metals, or a conductive oxide such as ITO or Ga2O3.
[0050] The arrangement area and shape of the first electrode and the second electrode are not limited as long as electrical contact is obtained with each of the first conductivity type cladding layer and the second conductivity type cladding layer (the second conductivity type contact layer if a second conductivity type contact layer is provided).
[0051] (Buffer layer) The buffer layer is formed between the substrate and the first-conductivity-type cladding layer, and is preferably formed on the entire surface of the substrate. By providing the buffer layer, a nitride semiconductor layer having a small lattice constant difference and a small thermal expansion coefficient difference and a small number of defects is formed on the buffer layer. Furthermore, by providing the buffer layer, the first-conductivity-type cladding layer can be grown under compressive stress, and the occurrence of cracks in the first-conductivity-type cladding layer can be suppressed. Therefore, even if the substrate is formed of a nitride semiconductor such as AlN or AlGaN, a nitride semiconductor layer having a small number of defects can be formed above the buffer layer.
[0052] The buffer layer is made of a nitride semiconductor such as AlN or AlGaN, etc. The buffer layer may contain impurities such as C, Si, Fe, Mg, etc.
[0053] The buffer layer has a thickness of, for example, several μm. Specifically, the thickness of the buffer layer is preferably thicker than 10 nm and thinner than 10 μm. When the thickness of the buffer layer is thicker than 10 nm, the crystallinity of the nitride semiconductor such as AlN is high. When the thickness of the buffer layer is thinner than 10 μm, cracks are less likely to occur in the buffer layer formed by crystal growth on the entire surface of the wafer. Moreover, the buffer layer is more preferably thicker than 50 nm and thinner than 5 μm. When the thickness of the buffer layer is thicker than 50 nm, a layer with high crystallinity can be formed. When the thickness of the buffer layer is thinner than 5 μm, cracks are less likely to occur in the buffer layer.
[0054] (1.2) Manufacturing method of ultraviolet light emitting element The laser diode of this embodiment is manufactured through a process of forming each layer on a substrate.
[0055] (Formation of the substrate) The substrate is formed by a general substrate growth method such as a vapor phase growth method, such as a sublimation method or a hydride vapor phase epitaxy (HVPE) method, or a liquid phase growth method.
[0056] (Formation of semiconductor laminate) Each layer of the semiconductor laminate formed on the substrate can be formed by, for example, molecular beam epitaxy (MBE), hydride vapor phase epitaxy (HVPE), or metal organic chemical vapor deposition (MOCVD). Here, among the layers formed on the substrate, the nitride semiconductor layer can be formed using, for example, an Al source containing trimethylaluminum (TMAl), a Ga source containing trimethylgallium (TMGa) or triethylgallium (TEGa), or an N source containing ammonia (NH3). Laser diodes are manufactured through a process of removing unnecessary portions of each layer of a semiconductor laminate formed on a substrate by etching. The unnecessary portions of each layer of the semiconductor laminate can be removed by, for example, inductively coupled plasma (ICP) etching.
[0057] (Electrode formation) The laser diode may also be manufactured through a process of forming electrodes. The electrodes, such as the first electrode and the second electrode, may be formed by, for example, resistance heating deposition, electron gun deposition, or sputtering, but are not limited to these methods. Each electrode may be formed as a single layer, or may be formed by laminating multiple layers. Each electrode may also be heat-treated in an oxygen, nitrogen, or air atmosphere after the layers are formed. Finally, the substrate on which the layers have been formed through the above-mentioned steps is divided into individual pieces by dicing to manufacture the laser diodes.
[0058] 2. Measurement methods for the physical properties of ultraviolet light-emitting devices The physical properties of the laser diode described above can be measured as follows.
[0059] (Measurement of impurity and doping concentrations) The concentrations of dopants and impurities contained in the substrate and each layer of the semiconductor laminate that constitutes the laser diode can be measured by secondary ion mass spectrometry (SIMS). When measuring the concentration of dopants and impurities in each layer of the semiconductor laminate by SIMS after processing into a device, the measurement can be performed after removing the electrodes by chemical etching or physical polishing. The concentration of dopants and impurities in each layer of the semiconductor laminate can also be measured by sputtering from the substrate side where no electrodes are formed. Specifically, SIMS measurements are performed under the measurement conditions provided by Evans Analytical Group (EAG), Inc. A cesium (Cs) ion beam with an energy of 14.5 keV is used to sputter the sample during the measurements.
[0060] (Layer thickness measurement method) The thickness of each layer constituting the laser diode can be measured by cutting out a predetermined cross section perpendicular to the substrate, observing this cross section with a transmission electron microscope (TEM), and using the length measurement function of the TEM. As a measurement method, first, a cross section perpendicular to the main surface of the substrate of the laser diode is observed using a TEM. Specifically, for example, in a TEM image showing a cross section perpendicular to the main surface of the substrate of the laser diode, a range of 2 μm or more in a direction parallel to the main surface of the substrate is set as the observation width. Since contrast is observed at the interface between two layers with different compositions within this observation width, the thickness up to this interface is observed in a continuous observation region with a width of 200 nm. The average value of the thickness of each layer included in this 200 nm wide observation region can be calculated from five points arbitrarily extracted from the above-mentioned observation width of 2 μm or more, thereby obtaining the layer thickness of each layer.
[0061] (Method of measuring shape) The length of each part constituting the laser diode can be measured by cutting out a predetermined cross section perpendicular to the substrate, observing this cross section with a scanning electron microscope (SEM), and using the length measurement function of the SEM. As a measurement method, first, a cross section perpendicular to the main surface of the substrate of the laser diode is observed using the SEM. Specifically, for example, the observation width is set to a range of 100 μm or more in a direction parallel to the main surface of the substrate in an SEM image showing a cross section perpendicular to the main surface of the substrate of the laser diode. Within this observation width, the length of each part can be obtained.
[0062] (Method of measuring relaxation) The presence or absence of relaxation can be obtained from the lattice constant calculated from the TEM lattice diffraction image. Distortion can be expressed as the amount by which the lattice constant in the in-plane direction of the a-axis of each layer of the laser diode has changed from the original lattice constant. If the lattice constant is the same as that of the substrate, it is strained, and if there is a difference, it can be said to be relaxed. Here, relaxation calculated from calculations is defined as 20% or more. The difference in lattice constant can be measured by automatic mapping measurement of the lattice diffraction image at each spot, and displayed as a mapping using analysis software. Specifically, measurements can be performed using the conditions of the Toray Research Center.
[0063] (Method of measuring atomic concentration of each layer) One method for measuring the atomic concentration in each layer that constitutes a laser diode is reciprocal space mapping (RSM) using the X-ray diffraction (XRD) method. Specifically, the lattice relaxation rate and Al composition relative to the substrate can be obtained by analyzing reciprocal space mapping data in the vicinity of the diffraction peak obtained using an asymmetric plane as the diffraction plane. Examples of the diffraction plane include the (10-15) plane and the (20-24) plane. In addition, layers and regions that do not provide sufficient reflection intensity by XRD, such as the light-emitting layer, the gradient layer, and hillocks formed in each layer, can be measured by X-ray photoelectron spectroscopy (XPS), energy dispersive X-ray spectroscopy (EDX), and electron energy-loss spectroscopy (EELS).
[0064] In EELS, the composition of a sample is analyzed by measuring the energy lost when an electron beam passes through the sample. Specifically, for example, the energy loss spectrum of the intensity of the transmitted electron beam is measured and analyzed for a thin-sectioned sample used in TEM observation. The position of the peak that appears around 20 eV of energy loss changes depending on the composition of each layer, and the composition can be determined from the peak position. In the same manner as in the method for calculating layer thickness by TEM observation described above, the Al composition of each layer is obtained by calculating the average value of the Al composition in an observation width of 200 nm from five points arbitrarily selected from an observation region of 2 μm or more.
[0065] In EDX, characteristic X-rays generated by an electron beam in a thin-sectioned sample used in the above-mentioned TEM observation, etc. are measured and analyzed. In the same manner as the method for calculating layer thickness using TEM observation described above, the Al composition of each layer is obtained by calculating the average value of the Al composition in an observation width of 200 nm from five points arbitrarily selected from an observation region of 2 μm or more.
[0066] In XPS, the evaluation of the depth direction is possible by performing XPS measurement while performing sputter etching using an ion beam. Although Ar+ is generally used as the ion beam, other ion species such as Ar cluster ions can be used as long as they can be irradiated with the etching ion gun mounted on the XPS device. The XPS peak intensities of Al, Ga, and N are measured and analyzed to obtain the depth direction distribution of the Al composition of each layer. Instead of sputter etching, the laser diode may be polished obliquely so that the cross section perpendicular to the main surface of the substrate is enlarged and exposed, and the exposed cross section may be measured by XPS.
[0067] The composition of each layer can be measured not only by XPS but also by Auger Electron Spectroscopy (AES). In this case, the composition can be measured by Auger Electron Spectroscopy on a cross section exposed by sputter etching or oblique polishing. The composition of each layer can also be measured by SEM-EDX measurement of a cross section exposed by oblique polishing.
[0068] (Method of measuring dislocation lines in the second ridge region) The dislocation lines formed in the second ridge region can be measured by cutting out a predetermined cross section parallel to the surface of the substrate and observing it with a transmission electron microscope (TEM). As an example, a primary sample with an observation area of 20 μm square or more, including the first ridge region including the first conductivity type cladding layer, is prepared by cutting out the primary sample from the substrate using a focused ion beam method. Next, a secondary sample is prepared by thinning the primary sample to a thickness of 0.5 μm using polishing or a focused ion beam method. For the secondary sample, <0001> A planar TEM image is obtained using an electron beam incident on the zone axis. During this process, cross-sectional TEM images can be simultaneously obtained using the primary sample or a sample obtained using a similar method to the primary sample.
[0069] Observed at magnifications of 10k to 20k with an applied voltage of 200kV. <0001> Dislocations are counted using a planar TEM image with the zone axis incidence. The observation area is moved from the edge of the second ridge region toward the first ridge region to a region of 20 μm, and dislocation lines are observed. The extension direction of the obtained dislocation lines does not extend completely in the <1-100> direction throughout the entire field of view, and the number of lines may increase or decrease by meeting other dislocation lines. Therefore, the number of dislocation lines is counted by imagining a sampling line extending in the <1-100> direction parallel to the direction extending from the side of the mesa structure into the mesa, and the number of intersections between the sampling line and the dislocation line is determined by the statistical average value of multiple sampling lines. Specifically, measurements are taken more than 20 times by moving the measurement point within a 20 μm field of view with sampling lines spaced 1 μm or less apart. The average value of these more than 20 measurements is taken as the number of dislocations. Hereinafter, this measurement is called a planar TEM measurement.
[0070] Burgers spectrum analysis of dislocation lines further involves acquiring planar TEM dark-field images under systematic reflection conditions of reciprocal lattice vectors <-1100> and <11-20>, and identifying the direction of the Burgers vector from the disappearance of the contrast of the dislocation lines. For example, if the Burgers vector has a component in the <11-20> direction, the contrast of the dislocation lines disappears in the planar TEM dark-field image under systematic reflection conditions of <11-20>.
[0071] (Applications of ultraviolet light emitting devices) The laser diode according to the present disclosure can be applied to devices in, for example, the medical and life science fields, the environmental field, the industrial and manufacturing fields, the lifestyle and home appliances field, the agricultural field, and other fields. The laser diode can be applied to a drug or chemical synthesis and decomposition device, a liquid, gas, and solid (container, food, medical equipment, etc.) sterilization device, a semiconductor cleaning device, etc., a surface modification device for film, glass, metal, etc., an exposure device for manufacturing semiconductors, FPD (Flat Panel Display), PCB (Printed Wiring Board), and other electronic products, a printing and coating device, an adhesive and sealing device, a transfer and molding device for film, pattern, mockup, etc., and a measurement and inspection device for banknotes, wounds, blood, chemical substances, etc.
[0072] Examples of liquid sterilization equipment include, but are not limited to, automatic ice makers, ice trays and ice storage containers in refrigerators, water tanks for ice makers, freezers, ice makers, humidifiers, dehumidifiers, cold water tanks, hot water tanks and flow piping for water servers, freezer-type water purifiers, portable water purifiers, water supply units, hot water heaters, wastewater treatment equipment, garbage disposers, toilet drain traps, washing machines, water sterilization modules for dialysis, connector sterilizers for peritoneal dialysis, and disaster water storage systems.
[0073] Examples of gas sterilization devices include, but are not limited to, air purifiers, air conditioners, ceiling fans, floor or bedding vacuum cleaners, futon dryers, shoe dryers, washing machines, clothes dryers, indoor germicidal lamps, storage ventilation systems, shoe boxes, chests of drawers, etc. Examples of solid sterilization equipment (including surface sterilization equipment) include, but are not limited to, vacuum packing machines, belt conveyors, hand tool sterilization equipment for medical, dental, barber, and beauty salon use, toothbrushes, toothbrush holders, chopstick cases, cosmetic pouches, drain covers, toilet spot cleaners, and toilet lids.
[0074] 3. Examples of UV light-emitting elements The laser diode of this embodiment will be described in more detail below with reference to Figures 1 and 2. The detailed configuration of each layer in each of the following embodiments is as described above.
[0075] (3.1) First embodiment 1 and 2 are schematic diagrams for explaining a laser diode 1 according to a first embodiment. Fig. 1 is a schematic plan view of the laser diode 1, and Fig. 2 is a schematic cross-sectional view of the laser diode 1. In Fig. 1, <1-100><11-20> <0001> Each of the arrows indicates a crystal orientation. FIG. 2 is a schematic cross-sectional view of the laser diode 1. As shown in FIG. 2, the laser diode 1 includes a substrate 10, a semiconductor laminate 20 disposed on the substrate 10, a first electrode 31, and a second electrode 32. The semiconductor laminate 20 includes a first conductive type cladding layer 21, a light emitting layer 22, and a second conductive type cladding layer 23. A part of the semiconductor laminate 20 is a mesa structure 201, a first ridge region 202, and a second ridge region 203, and a separation groove G is formed between the first ridge region 202 and the second ridge region 203. The first ridge region 202 and the second ridge region 203 are formed in the second conductive type cladding layer 23. An end surface ES (see FIG. 1) of the mesa structure 201 is a resonator structure for optical resonance and emission, and laser light is emitted in a direction perpendicular to the end surface ES (the direction of the arrow in FIG. 1). The laser diode 1 includes: Region directly below the second ridge region 203 Only in the upper portion of the substrate 10 are there a plurality of dislocation lines extending in the <1-100> crystal orientation of the substrate 10.
[0076] (3.2) Second embodiment Fig. 3 is a schematic diagram for explaining a laser diode 2 according to the second embodiment. Fig. 3 is a schematic cross-sectional view of the laser diode 2. The laser diode 2 differs from the laser diode 1 according to the first embodiment in that the laser diode 2 has a semiconductor laminate portion 20A further including a waveguide layer 24 of a first conductivity type and a waveguide layer 25 of a second conductivity type. In such a laser diode 2, the effect of confining light in the light emitting layer 22 is improved, and the emission intensity of the laser diode 2 is improved.
[0077] (3.3) Third embodiment 4 and 5 are schematic diagrams for explaining a laser diode 3 according to a third embodiment. Fig. 4 is a schematic plan view of the laser diode 3, and Fig. 5 is a schematic cross-sectional view of the laser diode 3. The laser diode 3 differs from the laser diode 2 according to the second embodiment in that it has a semiconductor laminate portion 20B including a second-conductivity-type contact layer 26 disposed on a second-conductivity-type cladding layer 23. In the laser diode 3, a first ridge region 202 and a second ridge region 203 are formed in the second-conductivity-type cladding layer 23 and the second-conductivity-type contact layer 26, and a separation groove G is formed between the first ridge region 202 and the second ridge region 203. In such a laser diode 3, the efficiency of carrier injection into the light emitting layer 22 is improved, and the light emission efficiency of the laser diode 3 is improved.
[0078] The second conductive type contact layer 26 may be combined with, for example, the laser diode 2 according to the second embodiment. That is, the laser diode may have the second conductive type contact layer 26 disposed on the second conductive type cladding layer 23 of the laser diode 2 (not shown).
[0079] (3.4) Fourth embodiment Fig. 6 is a schematic diagram for explaining a laser diode 4 according to the fourth embodiment. Fig. 6 is a schematic cross-sectional view of the laser diode 4. The laser diode 4 differs from the laser diode 1 according to the first embodiment in that it has a semiconductor laminate 20C including a second-conductivity-type cladding layer 23 composed of a second-conductivity-type vertical conductive layer 23A and a second-conductivity-type lateral conductive layer 23B, and a second-conductivity-type contact layer 26. In the laser diode 4, a first ridge region 202 and a second ridge region 203 are formed in the second-conductivity-type vertical conductive layer 23A and the second-conductivity-type lateral conductive layer 23B, and the second-conductivity-type contact layer 26. A separation groove G is formed between the first ridge region 202 and the second ridge region 203. In such a laser diode 4, the efficiency of carrier injection into the light emitting layer 22 is improved, and the light emission efficiency of the laser diode 4 is improved.
[0080] (3.5) Fifth embodiment Fig. 6 is a schematic diagram for explaining a laser diode 5 according to the fifth embodiment. Fig. 6 is a schematic cross-sectional view of the laser diode 5. The laser diode 5 differs from the laser diode 1 according to the first embodiment in that it has a semiconductor laminate 20D including a first-conductivity-type waveguide layer 24 and a second-conductivity-type waveguide layer 25, a second-conductivity-type cladding layer composed of a second-conductivity-type vertical conductive layer 23A and a second-conductivity-type lateral conductive layer 23B, and an intermediate layer 27 provided between the second-conductivity-type vertical conductive layer 23A and the second-conductivity-type waveguide layer 25. In the laser diode 5, the first ridge region 202 and the second ridge region 203 are formed in the second-conductivity-type vertical conductive layer 23A and the second-conductivity-type lateral conductive layer 23B, and a separation groove G is formed between the first ridge region 202 and the second ridge region 203. Such a laser diode 5 can improve the lateral conductivity of carriers by forming the second conductive type lateral conduction layer 23B and the second conductive type contact layer 26 with perfect strain while improving the conductivity of carriers in the intermediate layer 27.
[0081] 4.Effects The above-mentioned laser diode has the following advantages. (1) The laser diode has an electrode directly connected to the top of a mesa structure, and has a rectangular first ridge region having long and short sides in a planar view in a region of the mesa structure farthest from the nitride semiconductor substrate, and a rectangular second ridge region having long and short sides arranged in positions facing each of the long sides of the first ridge region across an isolation groove, the length of the short side of the second ridge region in a planar view being equal to or greater than 5 μm and equal to or less than 12 μm. This makes it possible to suppress the extension of dislocations into the first ridge region and into the isolation groove in the laser diode, and to avoid the introduction of dislocations into the light-emitting layer, which would significantly deteriorate the current, thereby lowering the oscillation threshold current.
[0082] (2) The width (length of the short side) of the second ridge region of the laser diode is preferably 20% to 60% of the entire width (length in the short side direction) of the mesa structure. This makes it possible to avoid the introduction of dislocations into the light-emitting layer, which would otherwise significantly deteriorate the lasing threshold current, and therefore to reduce the lasing threshold current.
[0083] (3) The separation grooves of the laser diode preferably have a depth that exposes at least the second conductivity type cladding layer. This allows efficient current confinement and reduces the oscillation threshold current.
[0084] (4) The width (length in the short side direction) of the separation groove of the laser diode is preferably 9 μm or more and 23 μm or less. This makes it possible to avoid the introduction of dislocations into the light-emitting layer, which would otherwise significantly deteriorate the lasing threshold current, and therefore to reduce the lasing threshold current.
[0085] (5) It is preferable that the width (length of the short side) of the short side of the second ridge region of the laser diode is shorter than the width (length of the short side) of the separation groove. This makes it possible to avoid the introduction of dislocations into the light-emitting layer, which would otherwise significantly deteriorate the lasing threshold current, and therefore to reduce the lasing threshold current.
[0086] (6) In plan view of the laser diode, an edge of the second ridge region preferably substantially overlaps with any edge of the region of the semiconductor laminate directly below the second ridge region. This allows the laser diode to be formed through a simple manufacturing process.
[0087] (7) The semiconductor laminate portion of the laser diode preferably has a resonator in which end faces parallel to the (1-100) crystal plane of the nitride semiconductor substrate serve as resonator mirror end faces, and is an edge-emitting laser diode that emits light in the <1-100> direction. This allows the resonator mirror end faces of the laser resonator to be formed into atomically flat (1-100) faces, which makes it easy to form the resonator mirror end faces.
[0088] (8) It is preferable that the longer sides of the second ridge region of the laser diode extend in the <1-100> direction, and that the semiconductor laminate has a plurality of dislocation lines extending in the <1-100> crystal orientation only in the region directly below the second ridge region. This makes it possible to avoid the introduction of dislocations into the light-emitting layer, which would otherwise significantly deteriorate the lasing threshold current, and therefore to reduce the lasing threshold current.
[0089] (9) In the semiconductor laminate of the laser diode, it is preferable that the Burgers vector of the dislocation line in the region immediately below the second ridge region has a component in the <11-20> direction. This makes it possible to avoid the introduction of dislocations into the light-emitting layer, which would otherwise significantly deteriorate the lasing threshold current, and therefore to reduce the lasing threshold current.
[0090] (10) In the semiconductor laminate of the laser diode, the number of dislocation lines extending in the <1-100> direction in the region immediately below the second ridge region is preferably greater than the number of dislocation lines extending in directions other than the <1-100> direction. This makes it possible to avoid the introduction of dislocations into the light-emitting layer, which would otherwise significantly deteriorate the lasing threshold current, and therefore to reduce the lasing threshold current.
[0091] (11) In the semiconductor laminate of the laser diode, there are no dislocation lines extending in the <1-100> direction in the region immediately below the first ridge region. This makes it possible to avoid the introduction of dislocations into the light-emitting layer, which would otherwise significantly deteriorate the lasing threshold current, and therefore to reduce the lasing threshold current.
[0092] (12) In the semiconductor laminate of the laser diode, it is preferable that no dislocation lines extending in the <1-100> direction are present in the first ridge region and the region immediately below the isolation trench. This makes it possible to avoid the introduction of dislocations into the light-emitting layer, which would otherwise significantly deteriorate the lasing threshold current, and therefore to reduce the lasing threshold current.
[0093] (13) The nitride semiconductor substrate of the laser diode is preferably an AlN single crystal substrate. This reduces the difference in lattice constant between the substrate and the nitride semiconductor layer formed on the substrate, and by growing the nitride semiconductor layer in a lattice-matched system, threading dislocations can be reduced, making it possible to form a highly stable nitride semiconductor layer. (14) The laser diode may have an electrode directly connected to the top of a mesa structure, and may have a rectangular first ridge region having long and short sides in a planar view in a region of the mesa structure farthest from a nitride semiconductor substrate, and a rectangular second ridge region having long and short sides arranged in a position facing one of the long sides of the first ridge region across an isolation groove, and the length of the short side of the second ridge region in a planar view may be greater than or equal to 5 μm and less than 12 μm. This makes it possible to suppress the extension of dislocations into the first ridge region and into the isolation groove in the laser diode, and to avoid the introduction of dislocations into the light-emitting layer, which would significantly deteriorate the current, thereby lowering the oscillation threshold current. In this case, the second ridge region is preferably disposed at a position sandwiched between an electrode disposed on the first ridge region and an electrode disposed on the first conductivity type cladding layer in a plan view. This makes it possible to efficiently reduce the oscillation threshold current. EXAMPLES
[0094] Examples and comparative examples of the present disclosure will be described below.
[0095] [Example 1] A 550μm thick (0001) AlN single crystal substrate was used as the substrate, and annealing was performed on this substrate using a metal organic chemical vapor deposition (MOCVD) device. The annealing process was performed in two sets of annealing at 1300℃, one set being annealing for 5 minutes in an NH3 atmosphere and the other being annealing for 5 minutes in an H2 atmosphere.
[0096] Next, an AlN layer, which is a homoepitaxial layer, was formed on the substrate as a buffer layer. The AlN layer was formed to a thickness of 500 nm in an environment at 1200°C. At this time, the ratio (V / III ratio) of the supply rate of the group III element source gas to the supply rate of the nitrogen source gas was set to 50. The degree of vacuum of the chamber in which the annealing was performed was set to 50 mbar. The growth rate of the AlN layer at this time was 0.5 μm / hr. Trimethylaluminum (TMAl) was used as the Al source, and ammonia (NH3) was used as the N source.
[0097] A first conductive cladding layer was formed on the AlN layer formed as described above. The first conductive cladding layer was an n-type AlGaN layer (Al: 70%, i.e., Al 0.70 Ga 0.30 The first conductive type cladding layer was formed to a thickness of 350 nm under the conditions of a temperature of 1080°C, a degree of vacuum of 50 mbar, and a V / III ratio of 4000. The growth rate of the first conductive type cladding layer was 0.4 μm / hr. Trimethylaluminum (TMAl) was used as the Al raw material. Triethylgallium (TEGa) was used as the Ga raw material. Ammonia (NH3) was used as the N raw material. Monosilane (SiH4) was used as the Si raw material.
[0098] Next, an n-type waveguide layer, which is a first conductive type waveguide layer, was formed on the first conductive type cladding layer. The n-type waveguide layer was an n-type AlGaN layer (Al: 63%, i.e., Al 0.63 Ga 0.37 The n-type waveguide layer was formed to a thickness of 60 nm under the conditions of a temperature of 1080°C, a degree of vacuum of 50 mbar, and a V / III ratio of 4000. The growth rate of the n-type waveguide layer was 0.35 μm / hr. Trimethylaluminum (TMAl) was used as the Al raw material, triethylgallium (TEGa) was used as the Ga raw material, and ammonia (NH3) was used as the N raw material.
[0099] Next, a light emitting layer was formed on the n-type waveguide layer. The light emitting layer was formed to have a multiple quantum well structure in which quantum well layers and barrier layers were stacked three times. Here, the quantum well layer was an AlGaN layer (Al: 52%, i.e., Al 0.52 Ga 0.48 The barrier layer having a thickness of 6.0 nm was an AlGaN layer (Al: 63%, i.e., Al 0.63 Ga 0.37 N layer). The light-emitting layer was formed under conditions of a vacuum degree of 50 mbar and a V / III ratio of 4000. The growth rate of the quantum well layer was 0.18 μm / hr, and the growth rate of the barrier layer was 0.15 μm / hr.
[0100] Next, a p-type waveguide layer, which is a second conductive type waveguide layer, was formed on the light emitting layer. The p-type waveguide layer was an AlGaN layer containing no dopant (Al: 63%, i.e., Al 0.63 Ga 0.37 The p-type waveguide layer was formed to a thickness of 60 nm under the conditions of a temperature of 1080°C, a degree of vacuum of 50 mbar, and a V / III ratio of 4000. The growth rate of the p-type waveguide layer was 0.35 μm / hr. Trimethylaluminum (TMAl) was used as the Al raw material, and triethylgallium (TEGa) was used as the Ga raw material.
[0101] Next, a second conductive cladding layer was formed on the p-type waveguide layer. The second conductive cladding layer has a laminated structure including a second conductive vertical conductive layer and a second conductive horizontal conductive layer, and is a graded layer with a gradient Al composition ratio. The second conductive vertical conductive layer was an AlGaN layer with a thickness of 320 nm, in which the Al composition is distributed in the direction away from the substrate and changes from Al=1.0 to 0.7. The second conductive horizontal conductive layer was a p-type AlGaN layer with a thickness of 2 nm and Al=0.9. The second conductive cladding layer was formed under the conditions of a temperature of 1080° C., a degree of vacuum of 50 mbar, and a V / III ratio of 4000. The growth rate of the second conductive cladding layer at this time was 0.3 to 0.5 μm / hr. Trimethylaluminum (TMAl) was used as the Al raw material. Triethylgallium (TEGa) was used as the Ga raw material.
[0102] Next, a p-type contact layer, which is a second conductive type contact layer, was formed on the second conductive type cladding layer. Here, the p-type contact layer was formed of an AlGaN layer and a GaN layer. The AlGaN layer was a p-type nitride semiconductor layer with a layer thickness of 30 nm, using Mg as a dopant impurity and with an Al composition distribution in the direction away from the substrate, varying from Al=0.7 to 0.4. The GaN layer was formed of GaN (i.e. Al:0%) with a thickness of 10 nm.
[0103] The p-type contact layer was formed under the conditions of a temperature of 950° C., a degree of vacuum of 150 mbar, and a V / III ratio of 3650. The growth rate of the p-type contact layer at this time was 0.2 μm / hr.
[0104] In this way, a semiconductor laminate was formed on an AlN substrate. When reciprocal lattice mapping measurement was performed on this semiconductor laminate by XRD, it was found that the semiconductor laminate had grown pseudomorphically without relaxation up to the p-type contact layer.
[0105] The semiconductor laminate formed as described above was annealed in an N2 atmosphere at 700°C for 10 minutes or more to further reduce the resistance of the p-type contact layer. The n-type cladding layer was exposed by dry etching using a gas containing Cl2 and BCl3 using an ICP. The n-type cladding layer was formed in a rectangular region long in the <1-100> direction in plan view. The ICP conditions were: antenna power 320W, bias power 30W, automatic pressure regulation (APC: Adaptive Pressure Control valve) 2Pa, process pressure 600Pa, and gas flow rates of Cl2 gas 20sccm and BCl3 gas 5sccm.
[0106] The formed mesa structure had a length of 700 μm in the <1-100> direction and a length of 40 μm in the <11-20> direction, where the length of the mesa structure in the <1-100> direction is the distance between the end faces of the cavity mirror in a plan view, and the length in the <11-20> direction is the distance between the side faces of the mesa structure.
[0107] A first ridge region and a second ridge region separated by a separation groove were formed by dry etching using gas containing Cl2 and BCl3 using ICP. The separation groove was etched to a depth that exposed the second conductive cladding layer. The ICP conditions were antenna power of 320 W, bias power of 30 W, automatic pressure regulation (APC: Adaptive Pressure Control valve) of 2 Pa, process pressure of 600 Pa, and gas flow rates of Cl2 gas at 20 sccm and BCl3 gas at 5 sccm.
[0108] The first ridge region and the second ridge region thus formed had a length of 700 μm in the <1-100> direction. The first ridge region had a length of 7 μm in the <11-20> direction, and the second ridge region had a length of 5 μm in the <11-20> direction. The end of the second ridge region nearly overlapped the end of the mesa structure. Here, the length of the first ridge region and the second ridge region in the <1-100> direction is the distance between the end faces of the resonator mirror in a plan view. The length of the first ridge region and the second ridge region in the <11-20> direction is the distance between the side faces of the ridge structure. In this case, the width of the separation groove was 23 μm, and the ratio of the second ridge region to the width of the mesa structure was 25%.
[0109] On the p-type contact layer in the first ridge region, Ni and Au were sequentially deposited in a rectangular shape elongated in the <1-100> direction to form multiple electrode metal regions as second electrodes. At this time, the width of the second electrode was 5 μm and the length was 700 μm. In addition, in the region where the n-type cladding layer of the mesa structure was exposed, V, Al, Ni, Ti, and Au were sequentially deposited in a rectangular shape elongated in the <1-100> direction to form multiple electrode metal regions as first electrodes. Furthermore, the substrate was divided into stripes by cleaving multiple times in the <11-20> direction within the electrode metal regions to form individual laser diodes. The final length of the mesa structure in the <1-100> direction was 600 μm.
[0110] The laser diode thus obtained was subjected to current injection and edge emission intensity measurements. The threshold voltage was 9.0 V and the oscillation threshold current was 10 kA / cm. 2 It was. Plane-view TEM measurements of this laser diode revealed that dislocation lines extending in the <1-100> direction were observed in the second ridge region, but no dislocations were observed in the first ridge region or the separation groove. Furthermore, the number of dislocation lines extending in the <1-100> direction in the second ridge region was greater than the number of dislocation lines extending in directions other than the <1-100> direction. The Burgers vectors of the dislocation lines also had a component in the <11-20> direction.
[0111] [Example 2] A laser diode of Example 2 was formed in the same manner as in Example 1, except that the width of the second ridge region was 7 μm, the width of the separation groove was 19 μm, and the ratio of the second region to the width of the mesa structure was 35%. The laser diode thus obtained was subjected to current injection and edge emission intensity measurements. The threshold voltage was 9.2 V and the oscillation threshold current was 10.5 kA / cm. 2 It was.
[0112] Plane-view TEM measurements of this laser diode revealed that dislocation lines extending in the <1-100> direction were observed in the second ridge region, but no dislocation lines were observed in the first ridge region or separation groove. Furthermore, the number of dislocation lines extending in the <1-100> direction in the second ridge region was greater than the number of dislocation lines extending in directions other than the <1-100> direction. The Burgers vector of the dislocation lines also had a component in the <11-20> direction.
[0113] [Example 3] A laser diode of Example 3 was formed in the same manner as in Example 1, except that the width of the second ridge region was 9 μm, the width of the separation groove was 15 μm, and the ratio of the width of the second region to the width of the mesa structure was 45%. The laser diode thus obtained was subjected to current injection and edge emission intensity measurements. The threshold voltage was 9.5 V and the oscillation threshold current was 11.2 kA / cm. 2 It was.
[0114] Plane-view TEM measurements of this laser diode revealed that dislocation lines extending in the <1-100> direction were observed in the second ridge region, but no dislocations were observed in the first ridge region or the separation groove. Furthermore, the number of dislocation lines extending in the <1-100> direction in the second ridge region was greater than the number of dislocation lines extending in directions other than the <1-100> direction. The Burgers vectors of the dislocation lines also had a component in the <11-20> direction.
[0115] [Example 4] The laser diode of Example 4 was formed in the same manner as in Example 1, except that the width of the second ridge region was 12 μm, the width of the separation groove was 9 μm, and the ratio of the second region to the width of the mesa structure was 60%. The laser diode thus obtained was subjected to current injection and edge emission intensity measurements. The threshold voltage was 9.7 V and the oscillation threshold current was 12.5 kA / cm. 2 It was.
[0116] Plane-view TEM measurements of this laser diode revealed that dislocation lines extending in the <1-100> direction were observed in the second ridge region, but no dislocations were observed in the first ridge region or the separation groove. Furthermore, the number of dislocation lines extending in the <1-100> direction in the second ridge region was greater than the number of dislocation lines extending in directions other than the <1-100> direction. The Burgers vectors of the dislocation lines also had a component in the <11-20> direction.
[0117] [Example 5] The laser diode of Example 5 was formed in the same manner as Example 1, except that the width of the first ridge was 5 μm, the width of the second ridge region was 7 μm, the width of the separation groove was 21 μm, and the ratio of the second region to the width of the mesa structure was 35%. The laser diode thus obtained was subjected to current injection and edge emission intensity measurements. The threshold voltage was 9.3 V and the oscillation threshold current was 10.4 kA / cm. 2 It was.
[0118] Plane-view TEM measurements of this laser diode revealed that dislocation lines extending in the <1-100> direction were observed in the second ridge region, but no dislocations were observed in the first ridge region or the separation groove. Furthermore, the number of dislocation lines extending in the <1-100> direction in the second ridge region was greater than the number of dislocation lines extending in directions other than the <1-100> direction. The Burgers vectors of the dislocation lines also had a component in the <11-20> direction.
[0119] [Example 6] The laser diode of Example 6 was formed in the same manner as Example 1, except that the width of the first ridge was 5 μm, the width of the second ridge region was 10 μm, the width of the separation groove was 15 μm, and the ratio of the second region to the width of the mesa structure was 50%. The laser diode thus obtained was subjected to current injection and edge emission intensity measurements. The threshold voltage was 9.6 V and the oscillation threshold current was 11.5 kA / cm. 2 It was.
[0120] Plane-view TEM measurements of this laser diode revealed that dislocation lines extending in the <1-100> direction were observed in the second ridge region, but no dislocations were observed in the first ridge region or the separation groove. Furthermore, the number of dislocation lines extending in the <1-100> direction in the second ridge region was greater than the number of dislocation lines extending in directions other than the <1-100> direction. The Burgers vectors of the dislocation lines also had a component in the <11-20> direction.
[0121] [Comparative Example 1] A laser diode of Comparative Example 1 was formed in the same manner as in Example 1, except that the width of the second ridge region was 3 μm, the width of the separation groove was 27 μm, and the ratio of the second region to the width of the mesa structure was 15%. The laser diode thus obtained was subjected to current injection and edge emission intensity measurements. The threshold voltage was 10.5 V and the oscillation threshold current was 18.0 kA / cm. 2 It was.
[0122] Plane-view TEM measurements of this laser diode revealed that dislocation lines extending in the <1-100> direction were observed not only in the second ridge region, but also in the first ridge region and the separation groove. Furthermore, the number of dislocation lines extending in the <1-100> direction in the second ridge region was greater than the number of dislocation lines extending in directions other than the <1-100> direction. Furthermore, the Burgers vectors of the dislocation lines had a component in the <11-20> direction.
[0123] [Comparative Example 2] A laser diode of Comparative Example 1 was formed in the same manner as in Example 1, except that the width of the second ridge region was 15 μm, the width of the separation groove was 3 μm, and the ratio of the second region to the width of the mesa structure was 75%. The laser diode thus obtained was subjected to current injection and edge emission intensity measurements. The threshold voltage was 10.4 V and the oscillation threshold current was 15.0 kA / cm 2 It was.
[0124] Plane-view TEM measurements of this laser diode revealed that dislocation lines extending in the <1-100> direction were observed in the second ridge region, but no dislocations were observed in the first ridge region or the separation groove. Furthermore, the number of dislocation lines extending in the <1-100> direction in the second ridge region was greater than the number of dislocation lines extending in directions other than the <1-100> direction. The Burgers vectors of the dislocation lines also had a component in the <11-20> direction.
[0125] [Comparative Example 3] A laser diode of Comparative Example 3 was formed in the same manner as in Example 1, except that the second ridge region and the separation groove were not present. The laser diode thus obtained was subjected to current injection and edge emission intensity measurements. The threshold voltage was 10.7 V and the oscillation threshold current was 20.0 kA / cm. 2 It was.
[0126] Plane-view TEM measurements of this laser diode revealed dislocation lines extending in the <1-100> direction from the edge of the mesa structure to the first ridge region, and the Burgers vector of the dislocation lines had a component in the <11-20> direction.
[0127] Table 1 below shows the evaluation results of each of the examples and comparative examples.
[0128] [Table 1]
[0129] As shown in Table 1, the laser diodes of each embodiment in which the short side length of the second ridge region was 5 μm or more and 12 μm or less had significantly lower threshold currents and oscillation thresholds than the laser diode of Comparative Example 3 in which no second ridge region was provided. Furthermore, the laser diodes of each example in which the short side length of the second ridge region was 5 μm or more and 12 μm or less had lower threshold currents and oscillation thresholds than the laser diodes of Comparative Examples 1 and 2 in which the short side length of the second ridge region was outside this range. In this case, the length of the short side of the separation groove was 9 μm or more and 23 μm or less, and the length of the short side of the second ridge region was 20% to 60% of the length in the short side direction of the mesa structure.
[0130] Furthermore, in the laser diodes of Examples 1, 2 and 5, in which the short side length of the second ridge region is 5 μm or more and 7 μm or less (i.e. the short side length of the separation groove is 19 μm or more and 23 μm or less and the short side length of the second ridge region is 20% or more and 35% or less of the length in the short side direction of the mesa structure), the threshold current and oscillation threshold were further reduced, and the laser diode characteristics were significantly improved. From the above, it was found that in order to obtain a laser diode with a low oscillation threshold current, it is necessary to provide a second ridge region arranged across a separation groove in the short side direction of the first ridge region, and to appropriately set the length of the short side of the second ridge region.
[0131] Although the embodiments of the present disclosure have been described above, the technical scope of the present disclosure is not limited to the technical scope described in the above-mentioned embodiments. Various modifications or improvements can be made to the above-mentioned embodiments, and it is clear from the claims that the forms to which such modifications or improvements are made are also included in the technical scope of the present disclosure. [Explanation of symbols]
[0132] 10 Substrate 20 Semiconductor laminate 21 First conductive type cladding layer 22 Light-emitting layer 23 Second conductive type cladding layer 23A Second conductive type vertical conductive layer 23B Second conductive type lateral conductive layer 24 First conductive type waveguide layer 25 Second conductive type waveguide layer 26 Second conductive type contact layer 27 Middle Class 31 1st electrode 32 2nd electrode 201 Mesa structure including first conductive type cladding layer 202 First ridge region of the mesa structure not including the first conductive type cladding layer 203 Second ridge region of mesa structure not including first conductive type cladding layer Side of SS mesa structure End face of ES mesa structure
Claims
1. a nitride semiconductor substrate containing Al; a semiconductor laminate portion disposed on the nitride semiconductor substrate; an electrode directly connected to the top of the semiconductor stack; Equipped with The semiconductor laminate portion is a first conductivity type cladding layer including a first conductivity type nitride semiconductor layer disposed on the nitride semiconductor substrate; a light emitting layer formed of a nitride semiconductor including one or more quantum wells and disposed on the first conductive type cladding layer; a second conductivity type cladding layer including a second conductivity type nitride semiconductor disposed on the light emitting layer; having a portion of the semiconductor laminate has a mesa structure protruding from a surface of a portion of the first conductive type cladding layer, a region of the mesa structure farthest from the nitride semiconductor substrate includes the second conductivity type cladding layer, and has a first ridge region that is rectangular in shape and has long sides and short sides in a plan view, and a second ridge region that is rectangular in shape and has long sides and short sides and is disposed at positions facing each of the long sides of the first ridge region across an isolation trench, a length of a short side of the second ridge region in a plan view is not less than 5 μm and not more than 12 μm; The electrode is directly connected to the top of the first ridge region. Laser diode.
2. The length of the short side of the second ridge region is 20% to 60% of the length of the mesa structure in the direction of the short side.
2. The laser diode of claim 1.
3. The separation groove has a depth that exposes at least the second conductive type cladding layer.
3. The laser diode according to claim 1 or 2.
4. The length of the separation groove in the direction of the short side is 9 μm or more and 23 μm or less.
4. A laser diode according to claim 1.
5. The length of the short side of the second ridge region is shorter than the length of the separation groove in the short side direction.
5. A laser diode according to claim 1.
6. In a plan view, an end of the second ridge region overlaps with any one of ends of a region of the semiconductor laminate directly below the second ridge region.
6. A laser diode according to claim 1.
7. The semiconductor laminate portion has a resonator in which an end face parallel to a crystal plane (1-100) of the nitride semiconductor substrate is a resonator mirror end face, and is an edge-emitting laser diode that emits light in the <1-100> direction.
7. A laser diode according to claim 1.
8. the long side of the second ridge region extends in a <1-100> direction, The semiconductor laminate has a plurality of dislocation lines extending in a crystal orientation <1-100> only in a region directly below the second ridge region.
8. A laser diode according to claim 1.
9. In the semiconductor laminate, the Burgers vector of the dislocation line in the region immediately below the second ridge region has a component in the <11-20> direction.
9. The laser diode of claim 8.
10. In the semiconductor laminate, the number of dislocation lines extending in the <1-100> direction in a region immediately below the second ridge region is greater than the number of dislocation lines extending in a direction other than the <1-100> direction.
10. The laser diode according to claim 8 or 9.
11. In the semiconductor laminate, in a region immediately below the first ridge region, there are no dislocation lines extending in the <1-100> direction.
11. A laser diode according to any one of claims 8 to 10.
12. In the semiconductor laminate, no dislocation lines extending in the <1-100> direction exist in the first ridge region and in the region immediately below the separation groove.
12. A laser diode according to any one of claims 8 to 11.
13. The nitride semiconductor substrate is an AlN single crystal substrate.
13. A laser diode according to any one of claims 1 to 12.
14. The semiconductor laminate portion is pseudomorphically grown to be lattice-matched to the substrate.
14. A laser diode according to any one of claims 1 to 13.
Citation Information
Patent Citations
Ridge wave guiding type semiconductor laser device
JP2003273464A
Method for manufacturing nitride semiconductor wafer of element of group iii
JP2003300800A
Semiconductor device and manufacturing method therefor
JP2004260152A
Semiconductor laser device
JP2004363582A
Semiconductor laser device
JP2005019679A