Laminate

The laminate with a phase-separated uneven layer and additional functional layers addresses the lack of multifunctionality in existing laminates, providing matte and antistatic properties through a structured composition.

JP7594352B2Active Publication Date: 2024-12-04MITSUBISHI CHEM CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2019142958
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-08-02
Publication Date
2024-12-04
Estimated Expiration
2039-08-02

AI Technical Summary

Technical Problem

Existing laminates with concavo-convex layers formed by phase separation lack the ability to exhibit multiple functions such as matte properties, antistatic properties, and other surface functionalities.

Method used

A laminate configuration with a base material layer, an uneven layer due to phase separation, a primer layer, and a surface functional layer, which can include antistatic, antifouling, or refractive index adjustment layers, and optionally a back functional layer, where the uneven layer contains specific polar and non-polar compounds with controlled thickness and surface resistance values.

Benefits of technology

The laminate achieves matte properties with enhanced antistatic performance and functional capabilities, such as antifouling and refractive index adjustment, by optimizing the composition and structure of the layers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594352000004
    Figure 0007594352000004
  • Figure 0007594352000005
    Figure 0007594352000005
  • Figure 0007594352000006
    Figure 0007594352000006
Patent Text Reader

Abstract

To provide a laminate capable of exhibiting a plurality of functions including matting properties.SOLUTION: A laminate 10 includes a substrate layer 1 and an irregularity layer 2 disposed on one face 1a of the substrate layer 1 and having irregularities by layer phase separation. The laminate further includes one or more layers selected from a group composed of: a primer layer 3 disposed between the substrate layer 1 and the irregularity layer 2; a surface functional layer disposed on a face opposite to the substrate layer 1 side of the irregularity layer 2; and a rear face functional layer disposed on a face opposite to the irregularity layer 2 side of the substrate layer 1.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate. [Background technology]

[0002] A method is known in which fine irregularities are formed on the surface of a substrate to impart a matte finish. For example, Patent Documents 1 to 4 describe a method for obtaining a cured film having an uneven surface by utilizing the phase separation that occurs during the drying process of a coating film containing two compounds with different solubilities. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 4739720 [Patent Document 2] Patent No. 4901914 [Patent Document 3] JP 2011-2820 A [Patent Document 4] JP 2018-72588 A Summary of the Invention [Problem to be solved by the invention]

[0004] According to the methods described in Patent Documents 1 to 4, a laminate is obtained in which a concave-convex layer made of a cured resin having concave-convex shapes due to phase separation is present on a substrate. However, the concave-convex layer alone may not be sufficient to meet the functions required for various applications.

[0005] An object of the present invention is to provide a laminate that can exhibit multiple functions including a matte finish. [Means for solving the problem]

[0006] The present invention has the following configuration. [1] A substrate having a base layer and an uneven layer having unevenness due to phase separation provided on one surface of the substrate layer, and further having one or more layers selected from the group consisting of a primer layer provided between the substrate layer and the uneven layer, a surface functional layer provided on the surface of the uneven layer opposite to the substrate layer side, and a back functional layer provided on the surface of the substrate layer opposite to the uneven layer side, wherein at least the surface functional layer has an antistatic layer, and the surface resistance of the outermost surface on the side of the substrate layer on which the uneven layer is present is 2×10 10 Ω or less the law of nature, the uneven layer is a cured product of a composition containing a compound (X) containing at least one polar group selected from a hydroxyl group, an amino group, an amide group, a sulfonyl group, a phosphate ester group, and a thiol group, and a compound (Y) not containing the polar group, The compound (X) is a (meth)acrylic polymer, The (meth)acrylic polymer has a (meth)acryloyl equivalent of 1.0 mmol / g or more and 10.0 mmol / g or less. A laminate. [2] The laminate described in [1], wherein the surface functional layer is an antifouling layer, an antistatic layer, a refractive index adjusting layer, an infrared absorbing layer, an ultraviolet absorbing layer, or a color correction layer, and the back functional layer is an adhesive layer, an antistatic layer, a refractive index adjusting layer, or an antiblocking layer. [3] The laminate according to [1] or [2], wherein the surface functional layer has a thickness of 0.001 to 3 μm, and the back functional layer has a thickness of 0.001 to 30 μm. [4] The laminate according to any one of [1] to [3], wherein the haze of the outermost surface on the side of the base layer where the uneven layer is present is 0.5 to 99%. [5] The laminate according to any one of [1] to [4], wherein the 60° specular gloss of the outermost surface on the side of the base layer on which the uneven layer is present is 100 or less. [6] The surface functional layer or the primer layer has an antistatic layer, and the surface resistance of the outermost surface on the side where the uneven layer is present relative to the base layer is 1×10 13 The laminate according to any one of [1] to [5], wherein Ω. [7] The back functional layer has an antistatic layer, and the surface resistance of the outermost surface of the base layer opposite to the side where the uneven layer is present is 1×10 13 The laminate according to any one of [1] to [6], 。 [8]The compound (X) has an SP value of 15.1 or more, and the compound (Y) has an SP value of 15.0 or less, [ 1 ] ~[7] The laminate according to claim 1. [ 9 ] the mass ratio of the compound (X) to the compound (Y) in the concave-convex layer is 10:90 to 80:20, 1 ] ~ [ 8 ] Either The laminate according to claim 1. [ 10 ] The thickness of the uneven layer is 1 to 10 μm, [1] to [ 9 ] The laminate described in any one of the above. [ 11 ] The thickness of the base layer is 2 to 350 μm, [1] to [ 10 ] The laminate described in any one of the above. [ 12 ]The substrate layer is a substrate selected from a polyester film, a polyacrylate film, a polyolefin film, a polycarbonate film, a polyimide film, and a triacetyl cellulose film, [1] to [ 11 ] The laminate described in any one of the above. [ 13 ] The primer layer contains a resin, 12 ] The laminate described in any one of the above. [ 14 ] The primer layer contains a compound derived from a crosslinking agent, 13 ] The laminate described in any one of the above. [ 15 ] The primer layer contains an antistatic agent, 14

[0033] Any of the laminates described in any one of the preceding items. 。

[16] The (meth)acrylic polymer is obtained by reacting an epoxy group with a carboxylic acid, 1 ] ~

[15] The laminate according to claim 1. [ 17 ] The compound (X) contains a carbon-carbon unsaturated bond, 1 ]~[ 16] The laminate described in any one of the above. [ 18 ]The compound (Y) is a (meth)acrylic polymer, [ 1 ]~[ 17 ] The laminate described in any one of the above. [ 19 ] the compound (Y) is a (meth)acrylate, [ 1 ]~[ 18 ] The laminate described in any one of the above. Effect of the Invention

[0007] According to the present invention, a laminate having a matte finish can be provided. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of a laminate of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing another example of the laminate of the present invention. [Diagram 3] FIG. 2 is a schematic cross-sectional view showing another example of the laminate of the present invention. [Figure 4] FIG. 2 is a schematic cross-sectional view showing another example of the laminate of the present invention. [Diagram 5] FIG. 2 is a schematic cross-sectional view showing another example of the laminate of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The present invention will be described in detail below. However, the following description is an example of an embodiment of the present invention, and the present invention is not limited to the contents of the following description as long as it does not exceed the gist of the present invention. The present invention can be modified and implemented as desired without departing from the gist of the present invention.

[0010] In the present invention, "(meth)acrylate" is a general term for acrylate or methacrylate, and "(meth)acrylic" is a general term for acrylic and methacrylic. The symbol "~" indicating a range of values ​​means that the values ​​before and after it are included as the lower and upper limits. The laminate of the present invention will now be described with reference to Figures 1 to 5. The dimensional ratios in Figures 1 to 5 are for the convenience of explanation and differ from the actual ratios.

[0011] [Laminate] The laminate of the present invention (hereinafter also referred to as "the laminate") comprises a base layer and a concave-convex layer provided on one surface of the base layer. The laminate further comprises one or more layers selected from the group consisting of a primer layer provided between the base layer and the concave-convex layer, a surface functional layer provided on the surface of the concave-convex layer opposite to the base layer side, and a back functional layer provided on the surface of the base layer opposite to the concave-convex layer side.

[0012] FIG. 1 is a schematic cross-sectional view showing an example of the present laminate. The laminate 10 has a base layer 1, a concave-convex layer 2 provided on one surface 1a of the base layer 1, and a primer layer 3 provided between the base layer 1 and the concave-convex layer 2.

[0013] FIG. 2 is a schematic cross-sectional view showing another example of the present laminate. The laminate 10 has a base layer 1, an uneven layer 2 provided on one surface 1a of the base layer 1, and a surface functional layer 4 provided on the surface of the uneven layer 2 opposite the base layer 1 side.

[0014] FIG. 3 is a schematic cross-sectional view showing another example of the present laminate. The laminate 10 has a base layer 1, an uneven layer 2 provided on one surface 1a of the base layer 1, a primer layer 3 provided between the base layer 1 and the uneven layer 2, and a surface functional layer 4 provided on the surface of the uneven layer 2 opposite the base layer 1 side.

[0015] FIG. 4 is a schematic cross-sectional view showing another example of the present laminate. The laminate 10 has a base layer 1, an uneven layer 2 provided on one surface 1a of the base layer 1, a primer layer 3 provided between the base layer 1 and the uneven layer 2, and a back surface functional layer 5 provided on the surface 1b of the base layer 1 opposite the uneven layer 2.

[0016] FIG. 5 is a schematic cross-sectional view showing another example of the present laminate. The laminate 10 has a base layer 1, an uneven layer 2 provided on one surface 1a of the base layer 1, a primer layer 3 provided between the base layer 1 and the uneven layer 2, a surface functional layer 4 provided on the surface of the uneven layer 2 opposite the base layer 1 side, and a back functional layer 5 provided on the surface 1b of the base layer 1 opposite the uneven layer 2 side.

[0017] The unevenness layer 2 has unevenness due to phase separation. In detail, the unevenness layer 2 has unevenness 2C consisting of recesses 2A and protrusions 2B on the surface opposite to the base layer 1 side.

[0018] "Base material layer" The substrate layer 1 is made of a substrate film. As the base film, for example, a resin film, a metal film, paper, or other conventionally known film can be used, but a resin film is preferred from the viewpoint of processability. The structure of the base film is not particularly limited, and may be a single layer structure or a multi-layer structure of two or more layers. It is preferable that the base film has a multi-layer structure of two or more layers, each of which has its own characteristics, to provide multi-functionality.

[0019] Examples of the resin film include polyester film, poly(meth)acrylate film, polyolefin film, polycarbonate film, polyimide film, triacetyl cellulose film, polystyrene film, polyvinyl chloride film, polyvinyl alcohol film, and nylon film. In particular, when used for display applications, polyester films, poly(meth)acrylate films, polyolefin films, polycarbonate films, polyimide films, and triacetyl cellulose films are preferred. Among these, polyester films, poly(meth)acrylate films, and polyolefin films are preferably used. Furthermore, in consideration of transparency, moldability, and versatility, polyester films are more preferably used.

[0020] The polyester film may be a non-stretched film (sheet) or a stretched film. Of these, a stretched film stretched in a uniaxial or biaxial direction is preferable. Of these, a biaxially stretched film is preferable in terms of excellent balance of mechanical properties and flatness.

[0021] The polyester used in the polyester film that can be used as the base film may be a homopolyester or a copolymer polyester. When the substrate film is made of a homopolyester, it is preferably one obtained by polycondensation of an aromatic dicarboxylic acid and an aliphatic glycol. Examples of aromatic dicarboxylic acids include terephthalic acid and 2,6-naphthalenedicarboxylic acid. Examples of aliphatic glycols include ethylene glycol, diethylene glycol, and 1,4-cyclohexanedimethanol. The aromatic dicarboxylic acids and aliphatic glycols may each be used alone or in combination of two or more.

[0022] Examples of the dicarboxylic acid component of the copolymer polyester include one or more of isophthalic acid, phthalic acid, terephthalic acid, 2,6-naphthalenedicarboxylic acid, adipic acid, sebacic acid, oxycarboxylic acid, etc., and examples of the glycol component include one or more of ethylene glycol, diethylene glycol, propylene glycol, butanediol, 4-cyclohexanedimethanol, neopentyl glycol, etc.

[0023] Representative examples of polyester include polyethylene terephthalate and polyethylene naphthalate. The intrinsic viscosity of the polyester is preferably 0.5 to 1.0 dL / g, more preferably 0.55 to 0.75 dL / g. The intrinsic viscosity is measured by the method described in the examples below.

[0024] Of the above, a more preferred form of polyester film is a film formed from polyethylene terephthalate or polyethylene naphthalate, taking into consideration mechanical strength and heat resistance, and a film formed from polyethylene terephthalate is more preferred, taking into consideration ease of production and handleability for applications such as a surface protection film.

[0025] The poly(meth)acrylate constituting the poly(meth)acrylate film that can be used as the base film may be any poly(meth)acrylate having a unit based on (meth)acrylate, and various acrylic resins can be used. Examples of (meth)acrylate include alkyl (meth)acrylates having an alkyl group with 1 to 4 carbon atoms, such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, and butyl (meth)acrylate, and alkyl (meth)acrylates having an alkyl group with a larger number of carbon atoms. Among these, in consideration of transparency, processability, and chemical resistance, it is preferable to use a unit based on an alkyl (meth)acrylate having an alkyl group with 1 to 4 carbon atoms as the main component, and it is more preferable to use at least one selected from the group consisting of a unit based on methyl (meth)acrylate and a unit based on ethyl (meth)acrylate as the main component, and it is preferable to use a unit based on methyl (meth)acrylate as the main component.

[0026] It is also possible to impart properties such as flexibility to the poly(meth)acrylate by incorporating units based on (meth)acrylates other than alkyl (meth)acrylates or units based on other monomers. The proportion of units based on alkyl (meth)acrylate having an alkyl group having 1 to 4 carbon atoms relative to the total mass of the poly(meth)acrylate is preferably 50 mass % or more, more preferably 80 mass % or more.

[0027] Particles can be blended in the base film for the purpose of imparting easy slippage, preventing scratches in each process, and improving blocking resistance. When particles are blended, the type of particles to be blended is not particularly limited as long as they are particles that can impart easy slippage, and specific examples include inorganic particles such as silica, calcium carbonate, magnesium carbonate, barium carbonate, calcium sulfate, calcium phosphate, magnesium phosphate, kaolin, aluminum oxide, zirconium oxide, and titanium oxide, and organic particles such as acrylic resin, styrene resin, urea resin, phenol resin, epoxy resin, and benzoguanamine resin. Furthermore, when the base layer includes a polyester film, precipitated particles obtained by precipitating a part of a metal compound such as a catalyst during the polyester production process can also be used. Among these, silica particles and calcium carbonate particles are preferred in that they are particularly effective in small amounts.

[0028] The average particle size of the particles is preferably 10 μm or less, more preferably 0.01 to 5 μm, and further preferably 0.01 to 3 μm. If the average particle size exceeds 10 μm, there is a concern that the transparency of the film may decrease.

[0029] The average particle size of the particles refers to the cumulative 50% (by weight) value in the equivalent sphericity distribution measured using a centrifugal sedimentation type particle size distribution measuring device.

[0030] When the base layer contains particles, the particle content in the base film is not necessarily limited because it depends on the average particle size of the particles, but is preferably 5% by mass or less, more preferably 0.0003 to 3% by mass, and even more preferably 0.0005 to 1% by mass, based on the total mass of the layer containing the particles in the base layer. When the particle content exceeds 5% by mass, the particles are less likely to fall off and the transparency of the film is less likely to decrease.

[0031] The shape of the particles to be used is not particularly limited, and any of spherical, blocky, rod-like, flat, etc. may be used. There are also no particular limitations on the hardness, specific gravity, color, etc. Two or more types of these particles may be used in combination as necessary.

[0032] In addition to the above-mentioned particles, conventionally known ultraviolet absorbers, antioxidants, antistatic agents, heat stabilizers, lubricants, dyes, pigments, etc. may be added to the base film as necessary.

[0033] The thickness of the substrate film is not particularly limited as long as it is within a range that allows formation of a film, but is preferably in the range of 2 to 350 μm, more preferably 5 to 250 μm, and further preferably 10 to 100 μm.

[0034] A specific example of the production of the base film will be described below, but the production method is not limited to the following production example, and a commonly known film-forming method can be used. In general, a resin is melted, formed into a sheet, and stretched to increase strength, etc., to produce a film.

[0035] For example, when producing a biaxially stretched polyester film, first, a polyester raw material is melt-extruded from a die using an extruder, and the molten sheet is cooled and solidified with a cooling roll to obtain an unstretched sheet. In this case, in order to improve the flatness of the sheet, it is preferable to increase the adhesion between the sheet and a rotating cooling drum, and an electrostatic application adhesion method or a liquid application adhesion method is preferably adopted. Next, the obtained unstretched sheet is stretched in one direction by a roll or tenter type stretching machine. The stretching temperature is preferably 70 to 120° C., more preferably 80 to 110° C., and the stretching ratio is preferably 2.5 to 7 times, more preferably 3.0 to 6 times. Next, the film is stretched in a direction perpendicular to the first-stage stretching direction, preferably at a temperature of 70 to 170° C. and at a stretch ratio of preferably 2.5 to 7 times, more preferably 3.0 to 6 times. Subsequently, the film is heat-treated at a temperature of 180 to 270°C under tension or relaxation of 30% or less to obtain a biaxially oriented film. In the above stretching, a method of stretching in one direction in two or more stages can be adopted. In that case, it is preferable to perform the stretching so that the final stretch ratios in both directions are each within the above range.

[0036] In addition, simultaneous biaxial stretching can also be used for film production. For example, in the case of polyester film, the simultaneous biaxial stretching method is a method in which the unstretched sheet is simultaneously stretched and oriented in the machine direction and the width direction under a temperature controlled condition usually at 70 to 120°C, preferably 80 to 110°C. The stretching ratio is 4 to 50 times, preferably 7 to 35 times, more preferably 10 to 25 times in area ratio. Then, the sheet is subsequently heat-treated under tension or relaxation of 30% or less at a temperature of 180 to 270°C to obtain a stretch-oriented film. As for the simultaneous biaxial stretching device employing the above-mentioned stretching method, a conventionally known stretching method such as a screw method, a pantograph method, or a linear drive method can be employed.

[0037] "Uneven layer" The uneven layer 2 formed by phase separation is a composition made of materials with different compatibility, which undergoes phase separation during the process of application, drying, and curing, thereby forming an uneven surface. A conventionally known material can be used as the material that causes phase separation. A composition made of materials with different polarities is preferable, since it is particularly easy to form by a method of coating a film. For example, a combination of a compound (X) containing at least one polar group selected from a hydroxyl group, an amino group, an amide group, a sulfonyl group, a phosphate ester group, and a thiol group and a compound (Y) containing no such polar group can be mentioned. In addition, in order to maintain the formed uneven shape and use it for various applications, it is preferable to use a curable composition for hard coat.

[0038] Compound (X) containing at least one polar group selected from hydroxyl, amino, amide, sulfonyl, phosphate, and thiol groups is characterized by hydrogen bonding, which allows the formation of a concave-convex structure by phase separation. Among these hydrogen-bonding groups, hydroxyl, amino, amide, and glycidyl groups are preferred because they are easy to form a concave-convex structure by phase separation, and hydroxyl, amino, and amide groups are particularly preferred from the viewpoints of stability when materials are mixed and ease of forming concave-convex structures. In addition, it is possible to have multiple types of polar groups in the compound, rather than one type. For example, a compound containing both a hydroxyl and an amide group is preferred because it is easy to form concave-convex structures.

[0039] In addition, in consideration of the ease of forming unevenness due to phase separation, the compound (X) is preferably a polymer compound rather than a low molecular weight compound. As the polymer compound, (meth)acrylic polymers, polyvinyl alcohols, and celluloses are preferred because they can introduce a larger number of polar groups, and in particular, (meth)acrylic polymers are more preferred from the viewpoint of being able to introduce various functional groups and being easy to control the performance.

[0040] Furthermore, in order to increase the hardness of the uneven layer 2 formed by phase separation, it is preferable to include a carbon-carbon unsaturated bond in the compound (X). The hardness of the uneven layer 2 formed by phase separation can be adjusted depending on the content of the carbon-carbon unsaturated bond. The carbon-carbon unsaturated bond means a carbon-carbon double bond or a carbon-carbon triple bond, and is preferably a carbon-carbon double bond, and more preferably the carbon-carbon double bond is a (meth)acryloyl group, and particularly considering the reactivity of the carbon-carbon unsaturated bond, is even more preferably an acryloyl group.

[0041] In the (meth)acrylic polymer, the compound (X) containing at least one polar group selected from hydroxyl group, amino group, amide group, sulfonyl group, phosphate group, and thiol group can be prepared by copolymerizing a (meth)acrylate monomer containing such a polar group with another (meth)acrylate monomer, or by reacting an acid, base, or the like with the epoxy group part of the polymer obtained by copolymerizing an epoxy group-containing (meth)acrylate with another (meth)acrylate monomer to generate a hydroxyl group. In particular, the method of using glycidyl (meth)acrylate is useful because it is easy to control the amount of hydroxyl groups.

[0042] Examples of (meth)acrylates containing an epoxy group include glycidyl (meth)acrylate, 3,4-epoxycyclohexyl (meth)acrylate, 3,4-epoxycyclohexyl (meth)acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, etc. Among these, glycidyl (meth)acrylate is preferred, and glycidyl acrylate is particularly preferred, in consideration of good reactivity and ease of use of the material.

[0043] In the case of introducing a hydroxyl group using a (meth)acrylate containing an epoxy group, the ratio of the (meth)acrylate containing an epoxy group in the (meth)acrylate polymer is preferably 10% by mass or more, more preferably 30% by mass or more, even more preferably 50% by mass or more, and particularly preferably 80% by mass or more, with the upper limit being 100% by mass. By using within this range, it becomes easier to control the polarity of the polymer, and it becomes easier to form an uneven structure due to phase separation.

[0044] Compounds used in the (meth)acrylate polymer containing an epoxy group for forming hydroxyl groups include acids and bases, but in consideration of the stability of the (meth)acrylate polymer, acids are preferred, and among them, carboxylic acids are particularly preferred. Among carboxylic acids, the use of (meth)acrylic acid makes it possible to introduce double bonds, which is a more preferred form. Among (meth)acrylic acids, acrylic acid is optimal in consideration of the reactivity of the epoxy group with the carboxylic acid and the reactivity of the introduced double bond. In addition, it is also a preferred form to use a hydroxycarboxylic acid such as lactic acid in order to introduce more hydroxyl groups. Furthermore, in order to form two or more types of structures, it is also possible to react two or more types of carboxylic acids with the epoxy group.

[0045] The amount of epoxy groups to be reacted is usually 1% by mass or more, preferably 20% by mass or more, more preferably 50% by mass or more, and further preferably 80% by mass or more, and may be up to 100% by mass. By reacting within this range, hydroxyl groups are generated, and the form is one in which unevenness due to phase separation is easily formed.

[0046] Examples of (meth)acrylamide monomers for incorporating an amide group into compound (X) include (meth)acryloylmorpholine, hydroxylmethyl(meth)acrylamide, hydroxylethyl(meth)acrylamide, dimethyl(meth)acrylamide, diethyl(meth)acrylamide, and N-isopropyl(meth)acrylamide. Considering ease of introduction, acrylamide monomers are more preferable than methacrylamide monomers. Among the above, considering the stability of the polymer and the strength of polarity, (meth)acryloylmorpholine is particularly preferable, and acryloylmorpholine is even more preferable. Moreover, these (meth)acrylamide monomers may be used alone or in combination of two or more.

[0047] In addition, when a (meth)acrylic polymer is used as the compound (X), various polymerizable (meth)acrylates can be used in addition to the above-mentioned compound groups. For example, alkyl (meth)acrylate monomers such as (meth)acrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, stearyl (meth)acrylate, phenoxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate, methoxyethyl (meth)acrylate, butoxyethyl (meth)acrylate, benzyl (meth)acrylate, cyclohexyl (meth)acrylate, dicyclopentenyl (meth)acrylate, and dicyclopentenyloxyethyl (meth)acrylate; (meth)acrylate monomers having a fluoroalkyl group, such as perfluorohexylethyl (meth)acrylate, 1H,1H,7H-dodecafluoroheptyl (meth)acrylate, and 1H,1H,9H-hexadecafluorononyl (meth)acrylate; (Meth)acrylate monomers having an amino group, such as N,N-diethylaminoethyl (meth)acrylate and N,N-dimethylaminoethyl (meth)acrylate; (meth)acrylate monomers having a hydroxyl group, such as 2-hydroxypropyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, and 1,6-hexanediol mono(meth)acrylate; Examples of raw materials other than the (meth)acrylic acid derivatives include hydrocarbon monomers having a vinyl group, such as styrene, p-chlorostyrene, p-methoxystyrene, divinylbenzene, N-vinylpyrrolidone, N-vinylcaprolactam, acrylonitrile, ethylene glycol divinyl ether, pentaerythritol divinyl ether, 1,6-hexanediol divinyl ether, trimethylolpropane divinyl ether, ethylene oxide-modified hydroquinone divinyl ether, ethylene oxide-modified bisphenol A divinyl ether, pentaerythritol trivinyl ether, dipentaerythritol hexavinyl ether, and ditrimethylolpropane polyvinyl ether.

[0048] The raw material used is not limited to one type, and two or more types may be used in combination to prepare the (meth)acrylic polymer, and it is preferable to use two or more types in combination to prepare the (meth)acrylic polymer.

[0049] The polymerization conditions for producing the (meth)acrylic polymer are not particularly limited, and a known method can be appropriately selected. Usually, the reaction for obtaining the (meth)acrylic polymer is a radical polymerization reaction, and the (meth)acrylic polymer can be obtained by polymerizing the raw material monomers at a desired polymerization temperature in an organic solvent in the presence of a radical polymerization initiator.

[0050] Examples of the organic solvent include ketone-based solvents such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; alcohol-based solvents such as ethanol, methanol, isopropyl alcohol, and isobutanol; ether-based solvents such as ethylene glycol dimethyl ether and propylene glycol monomethyl ether; ester-based solvents such as ethyl acetate, propylene glycol monomethyl ether acetate, and 2-ethoxyethyl acetate; aromatic hydrocarbon solvents such as toluene, etc. These organic solvents may be used alone or in combination of two or more.

[0051] Examples of the radical polymerization initiator include organic peroxides such as benzoyl peroxide and di-t-butyl peroxide, and azo compounds such as 2,2'-azobisbutyronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile), and 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile). These radical polymerization initiators may be used alone or in combination of two or more.

[0052] The polymerization temperature is usually from 20 to 150° C., and preferably from 50 to 100° C. The polymerization time is usually from 1 to 72 hours, and preferably from 3 to 36 hours.

[0053] In addition, the reaction conditions between the epoxy group and the carboxylic acid compound described above are not particularly limited, and a known method can be appropriately selected. The reaction may be carried out without a catalyst or in the presence of a catalyst, and examples of the catalyst include tertiary amines such as triethylamine and benzyldimethylamine, ammonium salts such as tetraethylammonium chloride and tetrabutylammonium bromide, phosphines such as triphenylphosphine and tributylphosphine, and phosphonium salts such as tetrabutylphosphonium bromide and tetrabutylphosphonium iodide. The amount of the catalyst used is usually 0.5% by mass or more, preferably 1.0% by mass or more, and usually 5.0% by mass or less, preferably 3.5% by mass or less, based on the weight of the polymer.

[0054] The reaction temperature for this reaction is usually 20 to 200° C., and preferably 50 to 150° C. The reaction time is usually 1 to 72 hours, and preferably 3 to 20 hours.

[0055] The weight average molecular weight (Mw) of the (meth)acrylic polymer should be appropriately selected depending on the application of the curable composition, but is usually 5000 or more, preferably 7000 or more, more preferably 9000 or more, and usually 100000 or less, preferably 70000 or less, more preferably 50000 or less, and even more preferably 30000 or less. Within the above range, it is easy to form unevenness due to phase separation on the surface after application. The weight average molecular weight (Mw) of the (meth)acrylic polymer can be determined as a converted value based on polystyrene standard using gel permeation chromatography (GPC). Specific measurement conditions are shown in the examples below.

[0056] From the viewpoint of improving the scratch resistance of the uneven layer 2 due to the phase separation formed, the (meth)acryloyl equivalent (the amount of (meth)acryloyl groups introduced) of the (meth)acrylic polymer of the compound (X) is preferably 1.0 mmol / g or more, more preferably 2.0 mmol / g or more, and particularly preferably 2.5 mmol / g or more. From the viewpoint of preventing gelation, the (meth)acryloyl equivalent is preferably 10.0 mmol / g or less, more preferably 8.0 mmol / g or less, and particularly preferably 6.0 mmol / g or less. The (meth)acryloyl equivalent is calculated based on the raw material used, and it is preferable to select the reaction of the epoxy group and the carboxylic acid such as (meth)acrylic acid so that the (meth)acryloyl equivalent is in the above range.

[0057] As the compound (Y) that does not contain a hydroxyl group, an amino group, an amide group, a sulfonyl group, a phosphate group, or a thiol group, various conventionally known compounds can be used. For example, (meth)acrylic polymers and various (meth)acrylic monomers can be used.

[0058] In the present invention, the term "(meth)acrylic polymer" refers to a polymer synthesized from a raw material containing (meth)acrylic acid and / or a (meth)acrylic acid derivative, and is used to include a polymer obtained by further modifying this polymer. As long as the polymer uses at least one raw material ((meth)acrylic monomer) containing (meth)acrylic acid or a (meth)acrylic acid derivative, the other raw materials are not particularly limited (for example, it may be a copolymer using a known polymerizable monomer such as a hydrocarbon monomer having a vinyl group other than a (meth)acrylic monomer. In addition, the term "(meth)acrylic acid derivative" refers to a compound having a structure similar to that of (meth)acrylic acid, such as a metal salt of (meth)acrylic acid, a (meth)acrylic acid ester, or a (meth)acrylic acid amide).

[0059] Examples of the (meth)acrylic polymer include those formed from the above-mentioned (meth)acrylic monomers that do not contain a hydroxyl group, an amino group, an amide group, a sulfonyl group, a phosphate group, or a thiol group, and monomers that undergo polymerization reaction with these.

[0060] In addition, various conventionally known materials can be used as the (meth)acrylic monomer that does not contain a hydroxyl group, an amino group, an amide group, a sulfonyl group, a phosphate group, or a thiol group. Although a monofunctional compound may be used, from the viewpoint of the strength of the formed uneven layer 2, a polyfunctional (meth)acrylate having two or more functional groups is preferable, and a polyfunctional (meth)acrylate having three or more functional groups is particularly preferable. In addition, since a low polarity is preferable, it is preferable to use a compound having few or no hydrogen bonding groups such as ethers, such as an ethylene oxide structure.

[0061] Examples of bifunctional (meth)acrylates include alkanediol di(meth)acrylates such as 1,4-butanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, and tricyclodecanedimethylol di(meth)acrylate; bisphenol-modified di(meth)acrylates such as bisphenol A ethylene oxide-modified di(meth)acrylate and bisphenol F ethylene oxide-modified di(meth)acrylate; polyethylene glycol di(meth)acrylate; polypropylene glycol di(meth)acrylate; urethane di(meth)acrylate; and epoxy di(meth)acrylate.

[0062] The trifunctional or higher polyfunctional (meth)acrylate is not particularly limited, but examples thereof include dipentaerythritol hexa(meth)acrylate, pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, isocyanuric acid ethylene oxide modified tri(meth)acrylate, ε-caprolactone modified tris(acryloxyethyl)isocyanurate and other isocyanuric acid modified tri(meth)acrylate, pentaerythritol triacrylate hexamethylene diisocyanate urethane prepolymer, pentaerythritol triacrylate toluene diisocyanate urethane prepolymer, dipentaerythritol pentaacrylate hexamethylene diisocyanate urethane prepolymer and other urethane acrylates. Among these, dipentaerythritol hexa(meth)acrylate is particularly preferred.

[0063] The weight average molecular weight (Mw) of the (meth)acrylic monomer of compound (Y) is preferably 60 or more, more preferably 100 or more, and even more preferably 200 or more, and is preferably 8000 or less, more preferably 6000 or less, even more preferably 4000 or less, and particularly preferably 2000 or less. Within the above range, it is preferable because a coating liquid that is easy to handle and exhibits phase separation during the coating process, such as drying and UV irradiation, can be obtained while being uniformly compatible as a coating liquid.

[0064] Compound (X) and compound (Y) are compounds for phase separation, and therefore, from the viewpoint of solubility parameter (SP value), it is preferable that the difference between the two is large.

[0065] The SP value of the compound (X) is preferably 15.1 or more, more preferably 16.0 to 22.0, even more preferably 16.5 to 20.0, and particularly preferably in the range of 17.0 to 19.5. By using the compound (X) in the above range, it becomes possible to achieve both the ease of forming a concave-convex structure by phase separation and coatability.

[0066] The SP value of the compound (Y) is preferably 15.0 or less, more preferably 10.0 to 14.5, further preferably 11.0 to 14.0, and particularly preferably in the range of 12.0 to 13.5. By using the compound (Y) within this range, it becomes easier to form a concave-convex structure due to phase separation with the compound (X).

[0067] The difference in SP value between compound (X) and compound (Y) is preferably 0.5 or more, more preferably 1.0 to 9.0, even more preferably 2.0 to 8.0, and particularly preferably 3.0 to 7.0. If the difference is within this range, a concave-convex structure due to phase separation is easily formed.

[0068] The mass ratio of the total amount of the compound (X) to the total amount of the compound (Y) is preferably in the range of 10:90 to 80:20, more preferably 12:88 to 60:40, particularly preferably 15:85 to 50:50, and most preferably 20:80 to 40:60. By setting it in this range, it becomes easy to form an uneven structure by phase separation.

[0069] The thickness of the uneven layer 2 is not particularly limited, but is preferably in the range of 1 to 10 μm, more preferably 1.5 to 8 μm, and even more preferably 2.0 to 6 μm. The thickness of the uneven layer is measured by observing a cross section with an electron microscope.

[0070] "Primer layer" Next, the formation of the primer layer 3 that can be formed on the substrate film (substrate layer 1) will be described. The primer layer 3 is a layer for the purpose of improving the adhesion between the base layer 1 and the uneven layer 2. If the adhesion between the base layer 1 and the uneven layer 2 is insufficient, the laminate may not be usable for some applications. By having the primer layer 3, the adhesion between the base layer 1 and the uneven layer 2 can be improved, allowing the laminate to be used for various applications.

[0071] The primer layer 3 may be provided with other functions. Examples of other functions include antistatic properties. If the primer layer 3 is an antistatic layer having antistatic properties, adhesion of dust and the like due to peeling electrification or frictional electrification to the outermost surface of the laminate, particularly the outermost surface on the side where the uneven layer 2 is present relative to the base layer 1, can be reduced. To provide the primer layer 3 with antistatic properties, for example, an antistatic agent may be added to the primer layer 3.

[0072] The primer layer 3 can be formed by a conventionally known method, among which, in particular, in consideration of the ease of forming the primer layer 3, it is preferably formed by coating. The coating method may be in-line coating, which is performed during the process of producing the base film, or off-line coating, which is performed outside the system on a base film that has already been produced. In-line coating is more preferred.

[0073] Specifically, in-line coating is a method of coating at any stage from melt extrusion of the resin forming the base film to stretching, heat setting and winding up. Usually, coating is performed on any of the following: an unstretched sheet obtained by melting and quenching, a stretched uniaxially stretched film, a biaxially stretched film before heat setting, and a film after heat setting and before winding up. Although not limited to the following, for example, in sequential biaxial stretching, a method of coating a uniaxially stretched film stretched in the longitudinal direction (longitudinal direction) and then stretching in the transverse direction is particularly excellent. According to this method, film formation and primer layer 3 formation can be performed simultaneously, which is advantageous in terms of production costs, and since stretching is performed after coating, the thickness of the primer layer 3 can also be changed by the stretching ratio, and thin film coating can be performed more easily than offline coating.

[0074] According to the in-line coating process described above, the film thickness does not change significantly whether or not the primer layer 3 is formed, and the risk of scratches or foreign matter adhesion also does not change significantly whether or not the primer layer 3 is formed. This is a major advantage over offline coating, which involves a separate coating process.

[0075] Furthermore, by providing the primer layer 3 by coating on the base film before stretching, the primer layer 3 can be stretched together with the base film, so that the formed primer layer 3 has appropriate adhesion to the base film.

[0076] Furthermore, in the production of biaxially stretched polyester film, the film can be restrained in both the longitudinal and transverse directions by stretching the film while holding the ends with clips or the like, and in the heat setting process, high temperatures can be applied without wrinkles or the like and while maintaining flatness. Therefore, the heat treatment performed after the primer layer 3 is provided by coating can be performed at a high temperature that cannot be achieved by other methods, improving the film-forming properties of the primer layer 3 and forming a strong primer layer 3. This is particularly effective for reacting a crosslinking agent.

[0077] Furthermore, in the case of biaxially oriented polyester film, it was found that in-line coating improves adhesion to the uneven layer caused by phase separation and durability. This is thought to be because in-line coating allows heat treatment at high temperatures that cannot be achieved by offline coating, and the heat treatment makes the primer layer 3 itself stronger, making it more resistant to heat and mechanical action during the formation of the uneven layer 2 by phase separation.

[0078] The material for forming the primer layer 3 preferably contains a resin from the viewpoint of improving adhesion with the uneven layer 2. As the resin, a conventionally known resin can be used. Specific examples of the resin include polyester resin, acrylic resin, urethane resin, polyvinyl resin (polyvinyl alcohol, vinyl chloride-vinyl acetate copolymer, etc.), and among them, polyester resin, acrylic resin, and urethane resin are preferred in consideration of adhesion performance and coating properties. When the base film is a polyester film, polyester resin is more preferred from the viewpoint of adhesion between the primer layer 3 and the base film. When the base film is a poly(meth)acrylate film, the primer layer preferably contains an acrylic resin.

[0079] The polyester resin may be one whose main components are a polyvalent carboxylic acid and a polyvalent hydroxy compound. Examples of polyvalent carboxylic acids include terephthalic acid, isophthalic acid, orthophthalic acid, 4,4'-diphenyldicarboxylic acid, 2,5-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, 2-potassium sulfoterephthalic acid, 5-sodium sulfoisophthalic acid, adipic acid, azelaic acid, sebacic acid, dodecanedicarboxylic acid, glutaric acid, succinic acid, trimellitic acid, trimesic acid, pyromellitic acid, trimellitic anhydride, phthalic anhydride, trimellitic acid monopotassium salt, and ester-forming derivatives thereof. Examples of polyhydric hydroxy compounds include ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, 2-methyl-1,5-pentanediol, neopentyl glycol, 1,4-cyclohexanedimethanol, p-xylylene glycol, bisphenol A-ethylene glycol adduct, diethylene glycol, triethylene glycol, polyethylene glycol, polypropylene glycol, polytetramethylene glycol, polytetramethylene oxide glycol, dimethylolpropionic acid, glycerin, trimethylolpropane, sodium dimethylolethylsulfonate, and potassium dimethylolpropionate. One or more of these compounds may be appropriately selected and subjected to a conventional polycondensation reaction to synthesize a polyester resin.

[0080] The acrylic resin is a polymer of polymerizable monomers including a (meth)acrylic monomer. Examples of the acrylic resin include homopolymers and copolymers of (meth)acrylic monomers, and copolymers of (meth)acrylic monomers and polymerizable monomers other than (meth)acrylic monomers.

[0081] The acrylic resin may be a copolymer of such a polymer with another polymer (e.g., polyester, polyurethane, etc.). Such a copolymer is, for example, a block copolymer or a graft copolymer. Alternatively, it also includes a polymer (or a mixture of polymers, as the case may be) obtained by polymerizing a polymerizable monomer in a polyester solution or polyester dispersion. Similarly, it also includes a polymer (or a mixture of polymers, as the case may be) obtained by polymerizing a polymerizable monomer in a polyurethane solution or polyurethane dispersion. Similarly, it also includes a polymer (or a mixture of polymers, as the case may be) obtained by polymerizing a polymerizable monomer in another polymer solution or dispersion.

[0082] The polymerizable monomer is not particularly limited, but particularly representative compounds include various carboxyl group-containing monomers such as acrylic acid, methacrylic acid, crotonic acid, itaconic acid, fumaric acid, maleic acid, and citraconic acid, and salts thereof; various hydroxyl group-containing monomers such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, monobutyl hydroxyl fumarate, and monobutyl hydroxy itaconate; methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate. Examples of suitable polymerizable monomers include various (meth)acrylic acid esters such as lauryl (meth)acrylate; various nitrogen-containing compounds such as (meth)acrylamide, diacetone acrylamide, N-methylol acrylamide, or (meth)acrylonitrile; various styrene derivatives such as styrene, α-methylstyrene, divinylbenzene, and vinyl toluene; various vinyl esters such as vinyl propionate and vinyl acetate; various silicon-containing polymerizable monomers such as γ-methacryloxypropyltrimethoxysilane and vinyltrimethoxysilane; phosphorus-containing vinyl monomers; various vinyl halides such as vinyl chloride and vinylidene chloride; and various conjugated dienes such as butadiene.

[0083] The urethane resin is a polymeric compound having a urethane bond in the molecule, and is typically synthesized by the reaction of a polyol with a polyisocyanate. Examples of the polyol include polycarbonate polyols, polyether polyols, polyester polyols, polyolefin polyols, and acrylic polyols. These compounds may be used alone or in combination.

[0084] Polycarbonate polyols are obtained by dealcoholization reaction between polyhydric alcohols and carbonate compounds. Examples of polyhydric alcohols include ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, and 3,3-dimethylolheptane. Examples of carbonate compounds include dimethyl carbonate, diethyl carbonate, diphenyl carbonate, ethylene carbonate, etc., and examples of polycarbonate-based polyols obtained by the reaction of these compounds include poly(1,6-hexylene) carbonate, poly(3-methyl-1,5-pentylene) carbonate, etc.

[0085] Examples of polyether polyols include polyethylene glycol, polypropylene glycol, polyethylene propylene glycol, polytetramethylene ether glycol, and polyhexamethylene ether glycol.

[0086] Examples of polyester polyols include polycarboxylic acids (malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, sebacic acid, fumaric acid, maleic acid, terephthalic acid, isophthalic acid, etc.) or their acid anhydrides and polyhydric alcohols (ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, 2-methyl-1,3-propanediol, 1,5-pentanediol, neopentyl glycol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, 2-methyl-2,4-pentanediol, 2 2-methyl-2-propyl-1,3-propanediol, 1,8-octanediol, 2,2,4-trimethyl-1,3-pentanediol, 2-ethyl-1,3-hexanediol, 2,5-dimethyl-2,5-hexanediol, 1,9-nonanediol, 2-methyl-1,8-octanediol, 2-butyl-2-ethyl-1,3-propanediol, 2-butyl-2-hexyl-1,3-propanediol, cyclohexanediol, bishydroxymethylcyclohexane, dimethanolbenzene, bishydroxyethoxybenzene, alkyldialkanolamines, lactonediols, etc.), and those having derivative units of lactone compounds such as polycaprolactone.

[0087] In consideration of adhesion performance, among the above polyols, polyester polyols and polycarbonate polyols are more preferably used, and polyester polyols are particularly preferred.

[0088] Examples of polyisocyanates used to obtain urethane resins include aromatic diisocyanates such as tolylene diisocyanate, xylylene diisocyanate, methylene diphenyl diisocyanate, phenylene diisocyanate, naphthalene diisocyanate, and tolidine diisocyanate, aliphatic diisocyanates having an aromatic ring such as α,α,α',α'-tetramethyl xylylene diisocyanate, aliphatic diisocyanates such as methylene diisocyanate, propylene diisocyanate, lysine diisocyanate, trimethylhexamethylene diisocyanate, and hexamethylene diisocyanate, and alicyclic diisocyanates such as cyclohexane diisocyanate, methylcyclohexane diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, and isopropylidenedicyclohexyl diisocyanate. These compounds may be used alone or in combination.

[0089] A chain extender may be used when synthesizing the urethane resin. The chain extender is not particularly limited as long as it has two or more active groups that react with an isocyanate group, and generally, a chain extender having two hydroxyl groups or two amino groups can be mainly used.

[0090] Examples of chain extenders having two hydroxyl groups include glycols such as aliphatic glycols, such as ethylene glycol, propylene glycol, and butanediol; aromatic glycols, such as xylylene glycol and bishydroxyethoxybenzene; and ester glycols, such as neopentyl glycol hydroxypivalate. Examples of chain extenders having two amino groups include aromatic diamines such as tolylenediamine, xylylenediamine, and diphenylmethanediamine; aliphatic diamines such as ethylenediamine, propylenediamine, hexanediamine, 2,2-dimethyl-1,3-propanediamine, 2-methyl-1,5-pentanediamine, trimethylhexanediamine, 2-butyl-2-ethyl-1,5-pentanediamine, 1,8-octanediamine, 1,9-nonanediamine, and 1,10-decanediamine; and alicyclic diamines such as 1-amino-3-aminomethyl-3,5,5-trimethylcyclohexane, dicyclohexylmethanediamine, isopropylidincyclohexyl-4,4'-diamine, 1,4-diaminocyclohexane, and 1,3-bisaminomethylcyclohexane.

[0091] The urethane resin is typically used in the form of a dispersion or solution. The medium for the dispersion or solution may be a solvent, but is preferably water. The aqueous dispersion or solution of the urethane resin may be a forced emulsification type using an emulsifier, a self-emulsification type in which a hydrophilic group is introduced into the structure of the urethane resin, or a water-soluble type, etc. In particular, a self-emulsification type in which an ionic group is introduced into the structure of the urethane resin to form an ionomer is preferred, since it has excellent storage stability of the liquid and excellent water resistance and transparency of the resulting primer layer 3.

[0092] In addition, the ionic group to be introduced may be various, such as carboxyl group, sulfonic acid, phosphoric acid, phosphonic acid, and quaternary ammonium salt, but carboxyl group is preferred. As a method for introducing carboxyl group into urethane resin, various methods can be taken at each stage of polymerization reaction. For example, there is a method of using a resin having a carboxyl group as a copolymerization component during prepolymer synthesis, or a method of using a component having a carboxyl group as one component of polyol, polyisocyanate, chain extender, etc. In particular, a method of using a carboxyl group-containing diol and introducing a desired amount of carboxyl group depending on the amount of this component is preferred.

[0093] For example, dimethylolpropionic acid, dimethylolbutanoic acid, bis-(2-hydroxyethyl)propionic acid, bis-(2-hydroxyethyl)butanoic acid, etc. can be copolymerized with the polyol used in the polymerization of the urethane resin. In addition, it is preferable that the carboxyl group is neutralized with ammonia, amines, alkali metals, inorganic alkalis, etc. to form a salt. Particularly preferred are ammonia, trimethylamine, and triethylamine. In such a urethane resin, the carboxyl group from which the neutralizing agent is removed in the drying process after application can be used as a crosslinking reaction point with another crosslinking agent. This not only provides excellent stability in the liquid state before coating, but also makes it possible to further improve the durability, solvent resistance, water resistance, blocking resistance, etc. of the obtained primer layer 3.

[0094] In addition, in forming the primer layer 3, it is preferable to use a crosslinking agent in combination in order to make the primer layer 3 stronger and improve performance such as adhesion. As the crosslinking agent, a conventionally known material can be used, and examples thereof include melamine compounds, oxazoline compounds, isocyanate compounds, epoxy compounds, carbodiimide compounds, silane coupling compounds, hydrazide compounds, and aziridine compounds. Among them, melamine compounds, isocyanate compounds, epoxy compounds, oxazoline compounds, carbodiimide compounds, and silane coupling compounds are preferred, and from the viewpoint of improving adhesion and durability, melamine compounds, oxazoline compounds, isocyanate compounds, and epoxy compounds are more preferred, and oxazoline compounds and isocyanate compounds are particularly preferred. In addition, one type of these crosslinking agents may be used, but two or more types may be used in combination to further improve adhesion and durability, resulting in good results.

[0095] The melamine compound is a compound having a melamine skeleton in the compound, and for example, an alkylolated melamine derivative, a compound partially or completely etherified by reacting an alcohol with an alkylolated melamine derivative, and a mixture thereof can be used. As the alcohol used for etherification, methyl alcohol, ethyl alcohol, isopropyl alcohol, n-butanol, isobutanol, etc. are preferably used. In addition, the melamine compound may be either a monomer or a dimer or higher polymer, or a mixture thereof may be used. In consideration of reactivity with various compounds, it is preferable that the melamine compound contains a hydroxyl group. Furthermore, a part of melamine may be co-condensed with urea, etc., and a catalyst may be used to increase the reactivity of the melamine compound.

[0096] The isocyanate compound is a compound having an isocyanate or an isocyanate derivative structure, such as a blocked isocyanate. Examples of the isocyanate include aromatic isocyanates such as tolylene diisocyanate, xylylene diisocyanate, methylene diphenyl diisocyanate, phenylene diisocyanate, and naphthalene diisocyanate, aliphatic isocyanates having an aromatic ring such as α,α,α',α'-tetramethyl xylylene diisocyanate, aliphatic isocyanates such as methylene diisocyanate, propylene diisocyanate, lysine diisocyanate, trimethylhexamethylene diisocyanate, and hexamethylene diisocyanate, and alicyclic isocyanates such as cyclohexane diisocyanate, methylcyclohexane diisocyanate, isophorone diisocyanate, methylene bis(4-cyclohexyl isocyanate), and isopropylidenedicyclohexyl diisocyanate. In addition, polymers and derivatives such as biuretized products, isocyanurate products, uretdione products, and carbodiimide modified products of these isocyanates are also included. These may be used alone or in combination. Among the above isocyanates, aliphatic isocyanates or alicyclic isocyanates are more preferable than aromatic isocyanates in order to prevent yellowing due to ultraviolet rays.

[0097] Examples of the blocked isocyanate include those in which the isocyanate group of the isocyanate compound is blocked with a blocking agent. Examples of the blocking agent include bisulfites, phenolic compounds such as phenol, cresol, and ethylphenol, alcoholic compounds such as propylene glycol monomethyl ether, ethylene glycol, benzyl alcohol, methanol, and ethanol, active methylene compounds such as dimethyl malonate, diethyl malonate, isobutanoyl methyl acetate, methyl acetoacetate, ethyl acetoacetate, and acetylacetone, mercaptan compounds such as butyl mercaptan and dodecyl mercaptan, lactam compounds such as ε-caprolactam and δ-valerolactam, amine compounds such as diphenylaniline, aniline, and ethyleneimine, acid amide compounds such as acetanilide and acetic acid amide, and oxime compounds such as formaldehyde, acetaldoxime, acetoneoxime, methyl ethyl ketoneoxime, and cyclohexanoneoxime. These may be used alone or in combination of two or more. As the blocked isocyanate, an isocyanate blocked with an active methylene compound is preferred from the viewpoint that the primer layer is less likely to be destroyed.

[0098] The isocyanate compound in the present invention may be used alone or as a mixture or bond with various polymers. In terms of improving the dispersibility and crosslinking property of the isocyanate compound, it is preferable to use a mixture or bond with a polyester resin or a urethane resin.

[0099] The oxazoline compound is a compound having an oxazoline group in the molecule, and in particular, a polymer containing an oxazoline group is preferred, and can be prepared by polymerization of an addition polymerizable oxazoline group-containing monomer alone or with other monomers. Examples of the addition polymerizable oxazoline group-containing monomer include 2-vinyl-2-oxazoline, 2-vinyl-4-methyl-2-oxazoline, 2-vinyl-5-methyl-2-oxazoline, 2-isopropenyl-2-oxazoline, 2-isopropenyl-4-methyl-2-oxazoline, and 2-isopropenyl-5-ethyl-2-oxazoline, and one or a mixture of two or more of these can be used. Among these, 2-isopropenyl-2-oxazoline is preferred because it is easily available industrially. The other monomer is not limited as long as it is a monomer that can be copolymerized with the addition-polymerizable oxazoline group-containing monomer, and examples thereof include (meth)acrylic acid esters such as alkyl (meth)acrylates (alkyl groups include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, t-butyl, 2-ethylhexyl, and cyclohexyl groups); unsaturated carboxylic acids such as acrylic acid, methacrylic acid, itaconic acid, maleic acid, fumaric acid, crotonic acid, styrenesulfonic acid, and salts thereof (sodium salts, potassium salts, ammonium salts, tertiary amine salts, and the like); unsaturated nitriles such as acrylonitrile and methacrylonitrile; (meth)acrylamide, N-alkyl (meth)acrylamide, and the like. Examples of the monomers that can be used include unsaturated amides such as N,N-dialkyl(meth)acrylamide (alkyl groups include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, t-butyl, 2-ethylhexyl, and cyclohexyl groups); vinyl esters such as vinyl acetate and vinyl propionate; vinyl ethers such as methyl vinyl ether and ethyl vinyl ether; α-olefins such as ethylene and propylene; halogen-containing α,β-unsaturated monomers such as vinyl chloride, vinylidene chloride, and vinyl fluoride; and α,β-unsaturated aromatic monomers such as styrene and α-methylstyrene. One or more of these monomers can be used.

[0100] The amount of oxazoline groups per 1 g of the oxazoline compound is preferably in the range of 0.5 to 10 mmol / g, more preferably 1 to 9 mmol / g, further preferably 3 to 8 mmol / g, and particularly preferably 4 to 6 mmol / g. By using the compound in the above range, the durability of the coating film is improved and the adhesion can be easily adjusted.

[0101] An epoxy compound is a compound having an epoxy group in the molecule, and examples thereof include condensates of epichlorohydrin and a compound having a hydroxyl group or an amino group (ethylene glycol, polyethylene glycol, glycerin, polyglycerin, bisphenol A, etc.), and examples of the polyepoxy compound include sorbitol polyglycidyl ether, polyglycerol polyglycidyl ether, pentaerythritol polyglycidyl ether, diglycerol polyglycidyl ether, triglycidyl tris(2-hydroxyethyl)isocyanate, glycerol polyglycidyl ether, trimethylolpropane polyglycidyl ether, and examples of the diepoxy compound include neopentyl glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, resorcinol diglycidyl ether, ethylene glycol ... Examples of monoepoxy compounds include allyl glycidyl ether, 2-ethylhexyl glycidyl ether, and phenyl glycidyl ether. Examples of glycidyl amine compounds include N,N,N',N'-tetraglycidyl-m-xylylenediamine and 1,3-bis(N,N-diglycidylamino)cyclohexane.

[0102] The carbodiimide compound is a compound having one or more carbodiimide or carbodiimide derivative structures in the molecule. For better strength of the primer layer 3, a polycarbodiimide compound having two or more in the molecule is more preferable.

[0103] Carbodiimide compounds can be synthesized by conventionally known techniques, and generally, condensation reaction of diisocyanate is used.Diisocyanate is not particularly limited, and both aromatic and aliphatic diisocyanates can be used, and specific examples include tolylene diisocyanate, xylylene diisocyanate, diphenylmethane diisocyanate, phenylene diisocyanate, naphthalene diisocyanate, hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, cyclohexane diisocyanate, methylcyclohexane diisocyanate, isophorone diisocyanate, dicyclohexyl diisocyanate, dicyclohexylmethane diisocyanate, etc.

[0104] In order to improve the water solubility or water dispersibility of the polycarbodiimide compound, a surfactant may be added or a hydrophilic monomer such as a polyalkylene oxide, a quaternary ammonium salt of a dialkylamino alcohol, or a hydroxyalkylsulfonate may be added within a range that does not impair the effects of the present invention.

[0105] A silane coupling compound is an organosilicon compound that has an organic functional group and a hydrolyzable group such as an alkoxy group in one molecule. For example, epoxy group-containing compounds such as 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; vinyl group-containing compounds such as vinyltrimethoxysilane and vinyltriethoxysilane; styryl group-containing compounds such as p-styryltrimethoxysilane and p-styryltriethoxysilane; (meth)acrylic group-containing compounds such as 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 3-(meth)acryloxypropylmethyldimethoxysilane, and 3-(meth)acryloxypropylmethyldiethoxysilane; 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, and N-2-(aminoethyl)-3 -aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltriethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldiethoxysilane, 3-triethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, N-phenyl-3-aminopropyltriethoxysilane and other amino group-containing compounds; isocyanurate group-containing compounds such as tris(trimethoxysilylpropyl)isocyanurate and tris(triethoxysilylpropyl)isocyanurate; and mercapto group-containing compounds such as 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-mercaptopropylmethyldimethoxysilane and 3-mercaptopropylmethyldiethoxysilane.

[0106] Among the above compounds, from the viewpoint of strength of the primer layer 3, epoxy group-containing silane coupling compounds, double bond-containing silane coupling compounds such as vinyl groups and (meth)acrylic groups, and amino group-containing silane coupling compounds are more preferred.

[0107] These crosslinking agents are reacted during the drying process and film-forming process to improve the performance of the primer layer 3. It can be assumed that the completed primer layer 3 contains unreacted crosslinking agents, reacted compounds, or a mixture thereof.

[0108] The antistatic agent contained in the primer layer 3 is not particularly limited, and any conventionally known antistatic agent can be used, but a polymer-type antistatic agent is preferable because it has good heat resistance and moist heat resistance. Examples of the polymer-type antistatic agent include compounds having an ammonium group, polyether compounds, compounds having a sulfonic acid group, betaine compounds, conductive organic polymers, and the like.

[0109] The compound having an ammonium group is a compound having an ammonium group in the molecule, and examples of the compound include ammonium compounds of aliphatic amines, alicyclic amines, and aromatic amines. The compound having an ammonium group is preferably a compound having a polymer type ammonium group, and the ammonium group is preferably a structure that is incorporated in the main chain or side chain of the polymer, not as a counter ion. Such a compound can be, for example, a polymer compound having an ammonium group, which is obtained by polymerizing an addition polymerizable monomer containing an ammonium group or a precursor of an ammonium group such as an amine, and converting the precursor group of the ammonium group to an ammonium group as necessary. The polymer can be a polymer containing an addition polymerizable ammonium group or a precursor of an ammonium group such as an amine, which is polymerized alone, or a copolymer of a monomer containing the addition polymerizable ammonium group or a monomer containing the addition polymerizable ammonium group and another monomer.

[0110] As the compound having an ammonium group, a compound having a pyrrolidinium ring is also preferred in terms of excellent antistatic properties and heat resistance stability. The two substituents bonded to the nitrogen atom of the compound having a pyrrolidinium ring are each independently an alkyl group, a phenyl group, or the like, and these alkyl groups and phenyl groups may be substituted with the groups shown below. Substitutable groups include, for example, a hydroxyl group, an amide group, an ester group, an alkoxy group, a phenoxy group, a naphthoxy group, a thioalkoxy group, a thiophenoxy group, a cycloalkyl group, a trialkylammonium alkyl group, a cyano group, and a halogen. The two substituents bonded to the nitrogen atom may be chemically bonded, and an example of a group in which two substituents are chemically bonded is -(CH2) m -(m = an integer of 2 to 5), -CH(CH3)CH(CH3)-, -CH=CH-CH=CH-, -CH=CH-CH=N-, -CH=CH-N=C-, -CH2OCH2-, -(CH2)2O(CH2)2- and the like.

[0111] The compound having a pyrrolidinium ring is preferably a polymer having a pyrrolidinium ring. The polymer having a pyrrolidinium ring can be obtained, for example, by cyclic polymerization of a diallylamine derivative using a radical polymerization catalyst. The polymerization can be carried out by a known method using a polymerization initiator such as hydrogen peroxide, benzoyl peroxide, or tertiary butyl peroxide in a polar solvent such as water or methanol, ethanol, isopropanol, formamide, dimethylformamide, dioxane, or acetonitrile as a solvent, but is not limited thereto. In the present invention, a compound having a polymerizable carbon-carbon unsaturated bond with the diallylamine derivative may be used as a copolymerization component.

[0112] Examples of anions that serve as a counter ion to the ammonium group of the above-mentioned ammonium group-containing compound include halogen ions, sulfonate, phosphate, nitrate, alkylsulfonate, and carboxylate ions.

[0113] The number average molecular weight (Mn) of the compound having an ammonium group is 1000 to 500000, preferably 2000 to 350000, and more preferably 5000 to 200000. If the molecular weight is less than 1000, the strength of the coating film may be weakened and the heat resistance stability may be poor. If the molecular weight exceeds 500000, the viscosity of the coating liquid may be high, and the handling and coating properties may be deteriorated.

[0114] In the present invention, the number average molecular weight (Mn) of the compound having an ammonium group can be determined as a converted value using polystyrene as a standard by using GPC (gel permeation chromatography).

[0115] Examples of the polyether compound include polyethylene oxide, polyether ester amide, and acrylic resins having polyethylene glycol in the side chain.

[0116] In the compound having a sulfonic acid group, the sulfonic acid group may be neutralized with a neutralizing agent to be in the form of a salt. As the compound having a sulfonic acid group, a compound having a plurality of sulfonic acid groups in a molecule, such as polystyrene sulfonic acid and its salts, is preferable.

[0117] As the conductive organic polymer, a conventionally known material can be used, for example, polythiophene-based, polyaniline-based, polypyrrole-based, polyacetylene-based, polyphenylene sulfide-based, etc. can be mentioned, among which polythiophene-based (polythiophene or polythiophene derivative) is preferred because it has both high transparency and high conductivity, is difficult to color, and is easy to exhibit performance by coating. Among polythiophene-based, a compound obtained by combining poly(3,4-ethylenedioxythiophene) with polystyrene sulfonic acid is particularly preferred from the viewpoint of conductive performance. Conductive organic polymers are preferred in that they exhibit high conductivity, have little humidity dependency, and can be expected to be used in a variety of applications.

[0118] In forming the primer layer 3, particles can also be used in combination to prevent blocking or improve slipperiness.

[0119] In addition, within the scope of the present invention, it is also possible to use, as necessary, an antifoaming agent, a coatability improving agent, a thickener, an organic lubricant, an ultraviolet absorber, an antioxidant, a foaming agent, a dye, a pigment, etc. in combination in forming the primer layer 3.

[0120] The proportion of the resin in the primer layer 3 is usually 5% by mass or more, preferably 10 to 99% by mass, more preferably 20 to 95% by mass, and further preferably 30 to 90% by mass. By using it in the above range, the appearance of the primer layer 3 and the adhesion to the uneven layer 2 can be easily improved.

[0121] The proportion of the crosslinking agent in the primer layer 3 is usually 80% by mass or less, preferably 0.5 to 65% by mass, more preferably 3 to 50% by mass, and further preferably 5 to 40% by mass. By using it in the above range, it becomes easier to improve the strength of the primer layer 3 and the adhesion between the uneven layer 2 and the primer layer 3.

[0122] When providing the primer layer 3 with an antistatic function, the proportion of the antistatic agent in the primer layer 3 is usually 80 mass % or less, preferably 0.5 to 70 mass %, and more preferably 1 to 50 mass %, although this is not generalized as it depends on the type of antistatic agent. By using the antistatic agent in the above range, it becomes easier to provide the primer layer 3 with an antistatic function, and it becomes easier to exhibit antistatic performance even after the uneven layer 2 is formed on the primer layer 3.

[0123] The thickness of the primer layer 3 depends on the material used for the primer layer 3 and the performance to be achieved, so cannot be generalized, but is usually in the range of 0.001 to 10 μm, preferably 0.01 to 4 μm, and more preferably 0.02 to 1 μm.

[0124] Regarding the formation of the primer layer 3, it is preferable to produce a laminate by preparing a solution or dispersion in a solvent of the above-mentioned series of compounds, and coating the liquid adjusted to a solid content concentration of approximately 0.1 to 80 mass % on a substrate film. In particular, when forming by in-line coating, it is more preferable to use an aqueous solution or water dispersion. For the purpose of improving dispersibility in water, improving film-forming properties, etc., the coating liquid may contain a small amount of an organic solvent. In addition, only one type of organic solvent may be used, or two or more types may be used as appropriate.

[0125] The primer layer 3 can be formed by a conventional coating method such as gravure coating, reverse roll coating, die coating, air doctor coating, blade coating, rod coating, bar coating, curtain coating, knife coating, transfer roll coating, squeeze coating, impregnation coating, kiss coating, spray coating, calendar coating, extrusion coating, or the like.

[0126] The drying and curing conditions when forming the primer layer 3 on the substrate film are not particularly limited, but in the case of a coating method, the drying temperature of the solvent such as water used in the coating liquid is usually in the range of 50 to 150°C, preferably 80 to 130°C, and more preferably 90 to 120°C. The drying time is approximately 3 to 200 seconds, preferably 5 to 120 seconds. In addition, in order to improve the strength of the primer layer 3, when it is performed in the film production process, a heat treatment step is usually performed in the range of 150 to 270°C, preferably 170 to 230°C, and more preferably 180 to 210°C. The heat treatment time is approximately 3 to 200 seconds, and preferably 5 to 120 seconds.

[0127] If necessary, the heat treatment may be combined with irradiation with active energy rays such as ultraviolet rays. The substrate film constituting the laminate of the present invention may be previously subjected to a surface treatment such as a corona treatment or a plasma treatment.

[0128] "Surface functional layer" In order to further impart various functions, a surface functional layer 4 can be provided on the uneven layer 2 formed by phase separation. Examples of the surface functional layer 4 include an antifouling layer, an antistatic layer, a refractive index adjusting layer (antireflection layer, low reflection layer, etc.), an infrared absorbing layer, an ultraviolet absorbing layer, and a color correcting layer.

[0129] The antifouling layer is provided to improve the antifouling performance by imparting water repellency and oil repellency to the uneven layer 2 formed by phase separation. As the material used for the antifouling layer 2, conventionally known materials such as silicone compounds, fluorine compounds, and compounds containing a long-chain alkyl group can be used. Among these, silicone compounds and fluorine compounds are preferred for achieving stronger antifouling performance, and fluorine compounds and compounds containing a long-chain alkyl group are preferred from the viewpoint of not contaminating the other object with which the antifouling layer comes into contact.

[0130] Silicone compounds are compounds having a silicone structure in the molecule, and examples thereof include alkyl silicones such as dimethyl silicone and diethyl silicone, and phenyl silicone and methylphenyl silicone having a phenyl group. Silicones having various functional groups can also be used, and examples thereof include ether groups, hydroxyl groups, amino groups, epoxy groups, carboxylic acid groups, halogen groups such as fluorine, perfluoroalkyl groups, various alkyl groups, and various aromatic groups, and other hydrocarbon groups. As other functional groups, silicones having vinyl groups and hydrogen silicones in which hydrogen atoms are directly bonded to silicon atoms are also common, and it is also possible to use both in combination as addition type silicones (types obtained by the addition reaction of vinyl groups and hydrogen silane). In addition, a method of introducing a double bond such as an acryloyl group and reacting at the double bond is also preferred.

[0131] In addition, as the silicone compound, modified silicones such as acrylic grafted silicone, silicone grafted acrylic, amino modified silicone, perfluoroalkyl modified silicone, etc. are also usable. In consideration of heat resistance and contamination, it is preferable to use a curable silicone resin, and as the type of curable type, any curing reaction type such as condensation type, addition type, active energy ray curable type, etc. can be used.

[0132] The fluorine compound is a compound containing fluorine atoms in the compound.As the fluorine compound, an organic fluorine compound is preferably used, for example, a perfluoroalkyl group-containing compound, a polymer of an olefin compound containing a fluorine atom, an aromatic fluorine compound such as fluorobenzene, etc. are listed.From the viewpoint of mold releasability, it is preferable to use a compound having a perfluoroalkyl group.Furthermore, the fluorine compound can also be a compound containing a long chain alkyl compound as described later.

[0133] Examples of the compound having a perfluoroalkyl group include perfluoroalkyl group-containing (meth)acrylates such as perfluoroalkyl (meth)acrylate, perfluoroalkyl methyl (meth)acrylate, 2-perfluoroalkyl ethyl (meth)acrylate, 3-perfluoroalkyl propyl (meth)acrylate, 3-perfluoroalkyl-1-methylpropyl (meth)acrylate, and 3-perfluoroalkyl-2-propenyl (meth)acrylate, and polymers thereof, and perfluoroalkyl group-containing vinyl ethers such as perfluoroalkyl methyl vinyl ether, 2-perfluoroalkyl ethyl vinyl ether, 3-perfluoropropyl vinyl ether, 3-perfluoroalkyl-1-methylpropyl vinyl ether, and 3-perfluoroalkyl-2-propenyl vinyl ether, and polymers thereof. In consideration of heat resistance and staining resistance, it is preferable to use a polymer. The polymer may be a single compound or a polymer of multiple compounds. In addition, from the viewpoint of stain resistance, the perfluoroalkyl group preferably has 3 to 11 carbon atoms. It may also be a polymer with a compound containing a long-chain alkyl compound as described below.

[0134] The long-chain alkyl group-containing compound is a compound having a straight-chain or branched alkyl group having a carbon number of usually 6 or more, preferably 8 or more, and more preferably 12 or more. Examples of the alkyl group include a hexyl group, an octyl group, a decyl group, a lauryl group, an octadecyl group, and a behenyl group. Examples of the compound having an alkyl group include various long-chain alkyl group-containing polymer compounds, long-chain alkyl group-containing amine compounds, long-chain alkyl group-containing ether compounds, and long-chain alkyl group-containing quaternary ammonium salts. Considering heat resistance and stain resistance, a polymer compound is preferable. In addition, from the viewpoint of effectively obtaining antifouling properties, a polymer compound having a long-chain alkyl group in the side chain is more preferable.

[0135] The polymer compound having a long-chain alkyl group in the side chain can be obtained by reacting a polymer having a reactive group with a compound having an alkyl group capable of reacting with the reactive group. Examples of the reactive group include hydroxyl group, amino group, carboxyl group, acid anhydride, etc. Examples of the compound having these reactive groups include polyvinyl alcohol, polyethyleneimine, polyethyleneamine, reactive group-containing polyester resin, reactive group-containing poly(meth)acrylic resin, etc. Among these, polyvinyl alcohol is preferable in consideration of antifouling properties and ease of handling.

[0136] Examples of compounds having an alkyl group capable of reacting with the reactive group include long-chain alkyl group-containing isocyanates such as hexyl isocyanate, octyl isocyanate, decyl isocyanate, lauryl isocyanate, octadecyl isocyanate, behenyl isocyanate, etc., long-chain alkyl group-containing acid chlorides such as hexyl chloride, octyl chloride, decyl chloride, lauryl chloride, octadecyl chloride, behenyl chloride, etc., long-chain alkyl group-containing amines, long-chain alkyl group-containing alcohols, etc. Among these, in consideration of releasability and ease of handling, long-chain alkyl group-containing isocyanates are preferred, and octadecyl isocyanate is particularly preferred.

[0137] Furthermore, polymeric compounds having a long-chain alkyl group in the side chain can also be obtained by polymerization of a long-chain alkyl (meth)acrylate or copolymerization of a long-chain alkyl (meth)acrylate with another vinyl group-containing monomer. Examples of long-chain alkyl (meth)acrylate include hexyl (meth)acrylate, octyl (meth)acrylate, decyl (meth)acrylate, lauryl (meth)acrylate, octadecyl (meth)acrylate, and behenyl (meth)acrylate.

[0138] The content of the antifouling material in the surface functional layer 4 for achieving the above-mentioned antifouling performance depends on the material used and cannot be generally stated, but in the case of silicone compounds and fluorine compounds, it is usually 0.01% by mass or more, more preferably 0.1% by mass or more, and even more preferably 0.2% by mass or more, and the upper limit may be 100% by mass. In addition, in the case of using a long-chain alkyl group-containing compound, it is usually 0.1% by mass or more, preferably 1% by mass or more, and even more preferably 3% by mass or more, and the upper limit may be 100% by mass. By using it in the above range, effective antifouling performance can be obtained.

[0139] As the antistatic agent used in forming the antistatic layer as the surface functional layer 4, various antistatic agents used in the primer layer 3 described above can be used. In addition, a method in which a double bond such as an acryloyl group is introduced into a compound having an ammonium group and reacted at the double bond is also preferred.

[0140] Examples of the refractive index adjusting layer include a high refractive index layer, a low refractive index layer, and a laminate thereof. Materials used in forming the refractive index adjusting layer as the surface functional layer 4, when the purpose is to increase the refractive index, include, for example, aromatic-containing compounds such as benzene structure, bisphenol A structure, melamine structure, and fluorene structure, as well as condensed polycyclic aromatic compounds such as naphthalene, anthracene, phenanthrene, naphthacene, benzo[a]anthracene, benzo[a]phenanthrene, pyrene, benzo[c]phenanthrene, and perylene structures, which are considered to have high refractive indexes among aromatic compounds, metal oxides such as zirconium oxide, titanium oxide, zinc oxide, tin oxide, antimony oxide, yttrium oxide, indium oxide, cerium oxide, ATO (antimony tin oxide), and ITO (indium tin oxide), metal-containing compounds such as metal chelate compounds such as titanium chelate and zirconium chelate, compounds containing a sulfur element, and compounds containing a halogen element.

[0141] Metal oxides are preferably used in the form of particles since there is a concern that their adhesion may decrease depending on the form of use, and the average particle size thereof is preferably 100 nm or less, more preferably 50 nm or less, and even more preferably 25 nm or less, from the viewpoint of the appearance of the coating.

[0142] When the refractive index adjustment layer is formed as the surface functional layer 4, a conventionally known material can be used for the purpose of lowering the refractive index. For example, acrylic resin and urethane resin are generally possible because they have a low refractive index. In addition, compounds in which fluorine atoms are incorporated in the resin, such as fluororesins, compounds containing fluororesins in the main skeleton, and compounds containing perfluoroalkyl groups in the side chains, can be used. In addition, examples of inorganic materials include hollow silica particles, fluorine atom-containing inorganic compounds such as magnesium fluoride and calcium fluoride, and hollow particles and nanoporous particles thereof.

[0143] The thickness of the surface functional layer 4 is preferably smaller than the height of the irregularities formed by the irregularity layer 2 due to phase separation. This is because if the thickness is equal to or greater than the height of the irregularities, the matte performance due to the irregularities will decrease. The thickness of the surface functional layer 4 depends on the height of the irregularities and cannot be generalized, but is usually in the range of 0.001 to 3 μm, preferably 0.005 to 2 μm, more preferably 0.01 to 1 μm, even more preferably 0.02 to 0.5 μm, and particularly preferably 0.03 to 0.2 μm. By using the surface functional layer 4 in the above range, it is possible to achieve both the expression of the function of the surface functional layer 4 and the matte performance due to the irregularities of the irregularity layer 2 due to phase separation.

[0144] Regarding the formation of the surface functional layer 4 and the back functional layer 5 described later, it is preferable to manufacture a laminate in such a manner that the above-mentioned series of compounds are prepared as a solution or a dispersion in a solvent, and the liquid adjusted to a solid content concentration of approximately 0.1 to 80 mass% is coated on the substrate film. In particular, when providing by in-line coating, it is more preferable to use an aqueous solution or water dispersion. For the purpose of improving dispersibility in water, improving film-forming properties, etc., the coating liquid may contain a small amount of an organic solvent. In addition, only one type of organic solvent may be used, or two or more types may be used as appropriate.

[0145] Methods for forming the front surface functional layer 4 and the back surface functional layer 5 can be any conventional coating method, such as gravure coating, reverse roll coating, die coating, air doctor coating, blade coating, rod coating, bar coating, curtain coating, knife coating, transfer roll coating, squeeze coating, impregnation coating, kiss coating, spray coating, calendar coating, and extrusion coating.

[0146] The drying and curing conditions when forming the surface functional layer 4 and the back functional layer 5 on the substrate film are not particularly limited, but in the case of a coating method, the drying temperature of the solvent such as water used in the coating liquid is usually in the range of 50 to 150 ° C, preferably 80 to 130 ° C, and more preferably 90 to 120 ° C. The drying time is, as a guideline, in the range of 3 to 200 seconds, preferably 5 to 120 seconds. In addition, in order to improve the strength of the surface functional layer 4 and the back functional layer 5, when it is performed in the film production process, a heat treatment step is usually performed in the range of 150 to 270 ° C, preferably 170 to 230 ° C, and more preferably 180 to 210 ° C. The time of the heat treatment step is, as a guideline, in the range of 3 to 200 seconds, preferably 5 to 120 seconds.

[0147] "Back functional layer" A back functional layer 5 may be provided on the surface opposite to the uneven layer 2 formed by phase separation in order to impart various functions. Examples of the back functional layer 5 include an adhesive layer for adhering to various adherends, an antistatic layer for preventing defects caused by adhesion of surrounding dirt and the like due to peeling electrification of the film or frictional electrification, an adhesive layer for bonding to other substrates, a refractive index adjustment layer for improving the total light transmittance, and an antiblocking layer for reducing blocking of the film.

[0148] The antistatic layer can be formed using an antistatic agent as described above, and the adhesive layer can be formed using a conventionally known adhesive, such as an acrylic-based, polyester-based, urethane-based, or rubber-based adhesive. Among these, an acrylic-based adhesive is preferred in view of versatility, and the refractive index adjustment layer can be formed using a high refractive index material or a low refractive index material as described above.

[0149] The thickness of the back functional layer 5 depends on the material used in the back functional layer and the performance to be achieved, so it cannot be generally determined, but is, for example, 0.001 to 30 μm. When the back functional layer 5 is an adhesive layer, the thickness is preferably 0.01 to 30 μm, more preferably 0.1 to 20 μm. When the back functional layer 5 is an antistatic layer, the thickness is preferably 0.001 to 10 μm, more preferably 0.01 to 5 μm.

[0150] Analysis of the components in the primer layer 3, the uneven layer 2 formed by phase separation, the surface functional layer 4, and the back functional layer 5 can be performed, for example, by time-of-flight secondary ion mass spectrometry (TOF-SIMS), X-ray photoelectron spectroscopy (ESCA), X-ray fluorescence, infrared spectroscopy (IR), etc.

[0151] The haze of the outermost surface of the laminate 10 on the side of the base layer 1 where the uneven layer 2 is present is not particularly limited as long as the matte finish is exhibited, but is preferably 0.5 to 99%, more preferably 1 to 80%, and even more preferably 2 to 50%. By using within the above range, it is easy to obtain good matte finish. The haze at the outermost surface of the laminate 10 on the side where the uneven layer 2 is present relative to the base layer 1 is the percentage of transmitted light that deviates from the incident light by 0.044 rad (2.5°) or more due to forward scattering (the ratio of diffuse transmittance to total light transmittance), of the transmitted light that is incident from the outermost surface on the side where the uneven layer 2 is present relative to the base layer 1 and passes through the laminate 10, and is measured in accordance with JIS K 7136.

[0152] The 60° specular gloss (60° gloss) of the outermost surface of the laminate 10 on the side where the uneven layer 2 is present relative to the base layer 1 is preferably 100 or less, more preferably 80 or less, and even more preferably 70 or less, in consideration of the matte properties. There is no particular lower limit, but it is preferably 1 or more. By using within the above range, it is easy to achieve good matte properties. The 60° specular gloss is measured in accordance with JIS Z 8741. The principle of measuring specular gloss is to measure the specular reflected light flux φs from the sample surface at a specified angle of incidence θ (60° for 60° specular gloss).

[0153] In the case where an antistatic layer is provided as the surface functional layer 4 or the primer layer 3, the antistatic performance is such that the surface resistance value of the outermost surface of the laminate 10 on the side where the uneven layer 2 is present relative to the base layer 1 is preferably 1×10 13 Ω or less, more preferably 1×10 12 Ω or less, more preferably 5×10 11 Ω or less, more preferably 1×10 11 Ω or less, particularly preferably 5×10 10 Within the above range, adhesion of dust and the like to the outermost surface is easily suppressed. The surface resistance value (also referred to as surface resistivity or sheet resistance) of the outermost surface can be adjusted by the amount of antistatic agent contained in the antistatic layer.

[0154] In the case where the back functional layer 5 has an antistatic layer, the antistatic performance is such that the surface resistance of the outermost surface of the base layer 1 opposite to the side where the uneven layer 2 is present is preferably 1×10 13 Ω or less, more preferably 1×10 12 Ω or less, more preferably 5×10 11 Ω or less, more preferably 1×10 11 Ω or less, particularly preferably 5×10 10 When the surface resistivity is equal to or less than the above upper limit, adhesion of dust and the like to the outermost surface is easily suppressed. EXAMPLES

[0155] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples as long as it does not deviate from the gist of the invention. The measurement and evaluation methods used in the present invention are as follows.

[0156] (1) Intrinsic viscosity of polyester 1 g of polyester from which components incompatible with the polyester had been removed was precisely weighed, dissolved in 100 ml of a mixed solvent of phenol / tetrachloroethane = 50 / 50 (weight ratio), and measured at 30°C.

[0157] (2) Average particle size (d50:μm) The average particle size was determined as the cumulative 50% (by weight) value in the equivalent sphericity distribution measured using a centrifugal sedimentation type particle size distribution analyzer SA-CP3 model manufactured by Shimadzu Corporation.

[0158] (3) Method for measuring SP value The SP value was measured by the following method. Weigh 0.5g of sample into a 100ml beaker, add 10ml of acetone to dissolve the sample. While stirring with a magnetic stirrer, drop hexane into the solution and determine the amount of hexane (vh) added at the point where the solution becomes turbid (cloudy point). Next, determine the amount of deionized water (vd) added at the cloudy point when deionized water is used instead of hexane. From vh and vd, the SP value is calculated using the formula given in Reference: SUH, CLARKE, JPSA-1, 5, 1671-1681 (1967). In addition, if the solubility parameter cannot be calculated by the above method, such as when the sample does not dissolve in acetone, it is estimated by the method proposed by Fedors et al. For details, refer to "POLYMER ENGINEERING AND SCIENCE, FEBRUARY, 1974, Vol. 14, No. 2, ROBERT F. FEDORS. (pages 147-154)" to determine the value.

[0159] (4) Measurement method for weight average molecular weight (Mw) Equipment: Tosoh Corporation "HLC-8120GPC" Column: Tosoh Corporation "TSKgel Super H1000+H2000+H3000" Detector: Differential refractive index detector (RI detector / built-in) Solvent: Tetrahydrofuran Temperature: 40℃ Flow rate: 0.5ml / min Injection volume: 10μl Concentration: 0.2% by mass Calibration sample: Monodisperse polystyrene Calibration method: Polystyrene equivalent

[0160] (5) Viscosity measurement method The measurement was performed at a solid content of 30% by mass and a temperature of 25° C. using an E-type viscometer TV-20 manufactured by Toki Sangyo Co., Ltd.

[0161] (6) Measurement method for acrylic acid consumption rate 0.5 g of the reaction solution was dispensed into an Erlenmeyer flask and diluted to 10 g with propylene glycol monomethyl ether solution. 0.1 g of phenolphthalein in ethanol (10%) was added to this solution as an indicator, and 0.1 N ethanolic potassium hydroxide solution (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added dropwise until the solution turned red. The amount of unreacted acrylic acid was determined from the amount added.

[0162] (7) Thickness of primer layer, surface functional layer, and back functional layer The surfaces of the primer layer, front functional layer, and back functional layer were stained with RuO4 and embedded in epoxy resin. Then, sections prepared by ultra-thin sectioning were stained with RuO4, and the cross sections of the primer layer or functional layer were measured using a transmission electron microscope (Hitachi High-Technologies Corporation H-7650, accelerating voltage 100 kV).

[0163] (8) Haze measurement method Measurements were performed using a haze meter HM-150 manufactured by Murakami Color Research Laboratory Co., Ltd. in accordance with JIS K 7136.

[0164] (9) Gloss measurement method The glossiness (gloss) of the outermost surface of the laminate on the side of the base layer where the uneven layer was present was measured as 60° specular glossiness (60° gloss) in accordance with JIS Z 8741 using a glossmeter VG2000 manufactured by Nippon Denshoku Industries Co., Ltd.

[0165] (10) Measurement method for surface resistance Using a high resistivity meter: Hiresta MCP-HP450 manufactured by Mitsubishi Chemical Analytech Co., Ltd., the surface resistivity of the sample was measured after 30 minutes of humidity conditioning in a measurement atmosphere of applied voltage 100V, 23°C, and 50% RH. If the surface resistance value is OVER, it means that the surface resistance value is too high to measure. If the surface resistance value is UNDER, it was measured using the following method. The surface resistivity of the sample was measured after conditioning it for 30 minutes in a measurement atmosphere of 23°C and 50% RH using a four-point ESP probe (probe spacing: 5 mm, probe tip shape: 2 mm diameter cylinder, probe pressure: 240 g / piece, RCF value was constant at 4.235) on a low resistivity meter: Loresta GP MCP-T610 manufactured by Mitsubishi Chemical Analytech Corporation. The resistance value of the front surface side (surface resistance value) and the resistance value of the back surface side (back surface resistance value) of the laminate were measured.

[0166] (11) Evaluation method for matte finish The laminate was placed in a room illuminated by a linear white fluorescent lamp, and the distance between the fluorescent lamp and the laminate was set at 2.5 m. The matte finish on the uneven layer side (reflection of the fluorescent lamp) was evaluated by visual inspection. Ranks A to C are judgments that show that the matte finish can be confirmed. A: The reflected image of the fluorescent light is very blurry and the outline of the fluorescent light cannot be seen. B: The reflected image of the fluorescent light is blurred, but you can faintly see its outline. C: The reflected image of the fluorescent light is slightly blurred, and although the outline can be seen, it appears wavy and appears dark white. D: The reflected image of the fluorescent light is clear, the contours can be clearly seen, and it appears linear and white.

[0167] (12) Method for evaluating adhesion between base layer and rough layer An 11 x 11 cross cut was made in a 10 mm x 10 mm area of ​​the uneven layer or the surface functional layer placed on top of it, and a 24 mm wide tape (Cellotape (registered trademark) CT-24 made by Nichiban Co., Ltd.) was applied on top of it. The tape was then rapidly peeled off at a peel angle of 180 degrees and the peeled surface was observed. If the peeled area was less than 5%, it was rated A, if it was 5% or more but less than 30%, it was rated B, if it was 30% or more but less than 80%, it was rated C, and if it was 80% or more, it was rated D.

[0168] (13) Evaluation method for pen writability (anti-stain properties) When the uneven layer or surface functional layer was written on with a fine-grained oil-based black marker (Mackie) manufactured by Zebra Corporation and the ink was repelled, it was rated as A. When the ink was not repelled with the oil-based marker mentioned above but was repelled with water-based yellow Keicoat 80 WA-SC-91 manufactured by Tombow Co., Ltd., it was rated as B. When the ink was not repelled with any of the above pens, it was rated as C. The more repelled the more excellent the stain-resistant property is evaluated to be.

[0169] (14) Method for evaluating adhesion When the evaluation surfaces (adhesive layer surfaces) were attached to each other, if they stuck together due to the adhesive strength, it was rated A, and if they did not stick together, it was rated B.

[0170] The polyesters used in the examples and comparative examples are as follows. <Polyester (A)> A polyethylene terephthalate homopolymer with an intrinsic viscosity of 0.63 dl / g obtained using magnesium acetate tetrahydrate and tetrabutyl titanate as polymerization catalysts.

[0171] <Polyester (B)> Polyethylene terephthalate homopolymer with an intrinsic viscosity of 0.64 dl / g obtained using magnesium acetate tetrahydrate, orthophosphoric acid and germanium dioxide as polymerization catalysts.

[0172] <Polyester (C)> Polyethylene terephthalate homopolymer containing 0.3% by mass of silica particles with an average particle size of 2 μm.

[0173] Examples of organic solvent-developing compounds constituting the uneven layer and the functional layer (front functional layer, back functional layer) are as follows. (Compound example) Polymers containing hydroxyl groups and unsaturated double bonds: (A-1) To a flask equipped with a thermometer, a stirrer, and a reflux condenser, propylene glycol monomethyl ether (157 parts by mass), glycidyl methacrylate (98 parts by mass), methyl methacrylate (1.0 part by mass), ethyl acrylate (1.0 part by mass), mercaptopropyltrimethoxysilane (1.9 parts by mass), 2,2'-azobis(2,4-dimethylvaleronitrile) (1.0 part by mass), and 1.9 parts by mass of γ-trimethoxysilylpropanethiol (KBM-803, manufactured by Shin-Etsu Chemical Co., Ltd.) were added, and the mixture was allowed to react at 65°C for 3 hours. Then, 2,2'-azobis(2,4-dimethylvaleronitrile) (0.5 parts by mass) was further added and reacted for 3 hours, after which propylene glycol monomethyl ether (138 parts by mass) and p-methoxyphenol (0.45 parts by mass) were added and heated to 100°C. Next, acrylic acid (51 parts by mass) and triphenylphosphine (3.1 parts by mass) were added and reacted at 110°C for 6 hours to obtain a (meth)acryloyl copolymer (A-1) having an unsaturated double bond amount (acryloyl equivalent (amount of acryloyl group introduced)) of 4.6 mmol / g. The SP value of the obtained (meth)acryloyl copolymer (A-1) was 17.4, and the consumption rate of acrylic acid was 94%. The viscosity of this solution (solid content 30% by mass) at 25°C was 100 mPa s, and the weight average molecular weight (Mw) was 17,700.

[0174] Polymers containing amide groups and unsaturated double bonds: (A-2) Propylene glycol monomethyl ether (360 parts by mass) was added to a 2000 ml separable flask equipped with a thermometer, a stirrer, and a reflux condenser. Meanwhile, glycidyl methacrylate (180 parts by mass), acryloylmorpholine (180 parts by mass), propylene glycol monomethyl ether (180 parts by mass), and 2,2'-azobis(2,4-dimethylvaleronitrile) (1.8 parts by mass) were added to a 1000 ml measuring cylinder to prepare a monomer solution. Thereafter, the stirrer of the separable flask was started, and then nitrogen gas was introduced into the separable flask and the measuring cylinder at a flow rate of 300 ml / min for about 1 hour. Next, the separable flask was immersed in an oil bath and heated to an internal temperature of 65°C. Next, the monomer solution prepared in the measuring cylinder was pumped into the separable flask and dropped over 2 hours to carry out radical polymerization. After completion of the dropwise addition, stirring was continued for another 2 hours at an internal temperature of 65°C, and then 2,2'-azobis(2,4-dimethylvaleronitrile) (0.9 parts by mass) was added and reacted for 3 hours, after which propylene glycol monomethyl ether (259 parts by mass) and p-methoxyphenol (1.6 parts by mass) were added and heated to 100°C. Next, acrylic acid (93 parts by mass) and triphenylphosphine (6.8 parts by mass) were added and reacted at 110°C for 6 hours to obtain a (meth)acryloyl copolymer (A-2) having an amide group and an unsaturated double bond and an unsaturated double bond amount (acryloyl equivalent (amount of acryloyl group introduced)) of 2.8 mmol / g. The SP value of the obtained (meth)acryloyl copolymer (A-2) was 19.1, and the consumption rate of acrylic acid was 93%. The viscosity of this solution (solid content 30% by mass) at 25°C was 1050 mPa s, and the weight average molecular weight (Mw) was 22500.

[0175] (Meth)acrylate: (B-1) Dipentaerythritol hexaacrylate (SP value: 12.1) (Meth)acrylate: (B-2) Urethane acrylate U-15HA (SP value: 13.3) manufactured by Shin-Nakamura Chemical Co., Ltd. (Meth)acrylate: (B-3) Pentaerythritol triacrylate succinic acid monoester

[0176] Acrylic resin: (C) Mitsubishi Chemical Corporation BR-80 (acrylic copolymer) (SP value: 13.4)

[0177] Silicone compounds: (D-1) A reactor equipped with a stirrer, a reflux condenser, and a thermometer was charged with polydimethylsiloxane having a number average molecular weight (Mn) of 5000 and substituted with a methacryloyl group at one end ("Silaplane" manufactured by JNC Corporation). FM0721", silicone-containing (meth)acrylate compound) (20 parts by mass), glycidyl methacrylate (60 parts by mass), methyl methacrylate (10 parts by mass), stearyl methacrylate (10 parts by mass), methyl isobutyl ketone (MIBK) (151 parts by mass) were charged, and after stirring was started, the system was replaced with nitrogen and heated to 55°C. 2,2'-azobis(2,4-dimethylvaleronitrile) (1.2 parts by mass) and 1-dodecanethiol (0.9 parts by mass) were added thereto, and the system was heated to 65°C and stirred for 3 hours, after which 2,2'-azobis(2,4-dimethylvaleronitrile) (0.6 parts by mass) was added and stirred at 65°C for 3 hours. The system was heated to 100°C and stirred for 30 minutes, after which 163 parts by mass of MIBK was added and the system was heated again to 100°C. To this was added p-methoxyphenol (0.5 parts by mass) and triphenylphosphine (2.6 parts by mass), followed by addition of acrylic acid (31 parts by mass), and the mixture was heated to 110° C. and stirred for 6 hours. After cooling, 4.8 parts by mass of MIBK was added to obtain an MIBK solution of copolymer (D-1) having a number average molecular weight (Mn) of 6,500.

[0178] Fluorine compounds: (D-2) SHIN-ETSU SUBELYN (registered trademark) KY-1203 manufactured by Shin-Etsu Chemical Co., Ltd.

[0179] Quaternary ammonium compounds: (E) A reactor equipped with a stirrer, a reflux condenser, and a thermometer was charged with N,N-dimethylaminoethyl methacrylate quaternized product (66 parts by mass), N,N-dimethylaminoethyl methacrylate (20 parts by mass), 2-ethylhexyl methacrylate (30 parts by mass), azobisisobutyronitrile (1 part by mass), isopropyl alcohol (200 parts by mass), and methyl ethyl ketone (100 parts by mass). After stirring was started, the system was replaced with nitrogen, the temperature was raised to 80°C, and the reaction was carried out for 8 hours to obtain a solution of copolymer (E).

[0180] Photopolymerization initiator: (F-1) Omnirad 127 by IGM Resins BV Photopolymerization initiator: (F-2) Omnirad 184 by IGM Resins BV

[0181] Examples of the aqueous development compounds constituting the primer layer and the functional layers (front functional layer, back functional layer) are as follows. (Compound example)

[0182] Polyester resin: (IA) A water dispersion of a polyester resin having the following composition: Monomer composition: (acid component) terephthalic acid / isophthalic acid / 5-sodium sulfoisophthalic acid / / (diol component) ethylene glycol / 1,4-butanediol / diethylene glycol = 56 / 40 / 4 / / 70 / 20 / 10 (mol%)

[0183] Acrylic resin: (IB) A water dispersion of an acrylic resin having the following composition: Ethyl acrylate / normal butyl methacrylate / acrylic acid=25 / 73 / 2 (mass%)

[0184] Polyvinyl alcohol: (IC) Polyvinyl alcohol with a degree of saponification of 88 mol% and a degree of polymerization of 500

[0185] Melamine compounds: (IIA) Hexamethoxymethylolmelamine Oxazoline compounds: (IIB) Acrylic polymer with oxazoline group and polyalkylene oxide chain: EPOCROS (oxazoline group amount = 4.5mmol / g, manufactured by Nippon Shokubai Co., Ltd.) Epoxy compounds: (IIC) Polyglycerol polyglycidyl ether, a multifunctional polyepoxy compound

[0186] Particles: (III) Silica particles with an average particle size of 0.07 μm

[0187] Antistatic agents (compounds with ammonium groups): (IVA) A polymer having a pyrrolidinium ring in the main chain, polymerized with the following composition: Diallyldimethylammonium chloride / dimethylacrylamide / N-methylol acrylamide = 90 / 5 / 5 (mol%), number average molecular weight (Mn) 30,000

[0188] Antistatic agent (conductive organic polymer compound): (IVB) Conductive organic polymer compound made by combining poly(3,4-ethylenedioxythiophene) with polystyrenesulfonic acid

[0189] Acrylic resin: (V) A water dispersion of an acrylic resin having the following composition: 2-Ethylhexyl acrylate / methyl methacrylate / methacrylic acid=85 / 12 / 3 (mass%)

[0190] [Example 1] The raw material for the outermost layer (surface layer) was a mixture of polyesters (A), (B), and (C) in proportions of 91%, 3%, and 6% by mass, respectively, and the raw material for the intermediate layer was a mixture of polyesters (A) and (B) in proportions of 97% and 3% by mass, respectively. Each of these raw materials was supplied to two extruders and melted at 285°C. After that, they were co-extruded onto a cooling roll set at 40°C in a layer structure of two types and three layers (surface layer / intermediate layer / surface layer = extrusion amount 1:8:1), and then cooled and solidified to obtain an unstretched sheet. Next, the film was stretched 3.1 times in the longitudinal direction at a film temperature of 85°C using the difference in roll peripheral speed, and then one side of this longitudinally stretched film was coated with coating solution P1 shown in Table 2 below, introduced into a tenter, dried at 95°C for 10 seconds, stretched 4.2 times in the transverse direction at 120°C, and heat-treated at 230°C for 10 seconds. After that, the film was relaxed by 2% in the transverse direction to obtain a 50 μm-thick polyester film having a primer layer with a thickness (after drying) of 0.1 μm.

[0191] Coating solution S1 shown in Table 1 below was applied onto the primer layer of the obtained polyester film, dried at 70°C for 1 minute, and then exposed to 250 mJ / cm 2 with a high-pressure mercury lamp. 2 The coating film made of the coating liquid S1 was irradiated with this light, causing phase separation of the components of the coating film, and forming a concave-convex layer having a thickness (after drying) of 5 μm.

[0192] Next, the coating solution F1 shown in Table 1 below was applied onto the uneven layer, dried at 80°C for 1 minute, and then exposed to 250 mJ / cm 2 with a high-pressure mercury lamp. 2 A coating film made of the coating liquid F1 was irradiated with this light to form a functional layer having a thickness (after drying) of 0.5 μm.

[0193] The laminate obtained showed good results in the matte property and the stain resistance test based on pen writing. The properties of this laminate are shown in Table 3 below.

[0194] [Examples 2 to 13] A laminate was obtained by manufacturing in the same manner as in Example 1, except that the coating agent composition in Example 1 was changed to the coating agent composition shown in Tables 1 and 2. The properties of the obtained laminate are shown in Table 3 below.

[0195] [Example 14] In Example 1, after obtaining an unstretched sheet, the sheet was stretched 3.1 times in the longitudinal direction at a film temperature of 85°C using the roll peripheral speed difference, and then a polyester film was obtained in the same manner except that the coating solution P4 shown in Table 2 below was applied to both sides of this longitudinally stretched film. Then, a concave-convex layer was formed in the same manner as in Example 1. The obtained laminate exhibited antistatic properties on the back side. The properties of this laminate film are shown in Table 3 below.

[0196] [Example 15] A laminate was obtained by manufacturing in the same manner as in Example 14, except that the coating agent composition in Example 14 was changed to the coating agent composition shown in Tables 1 and 2. The properties of the obtained laminate are shown in Table 3 below.

[0197] [Example 16] On the back surface of the polyester film opposite to the concave-convex layer of the laminate obtained in Example 2, the coating solution F8 shown in Table 2 was applied and dried to provide a functional layer having adhesive properties. The properties of this laminate are shown in Table 3 below.

[0198] [Examples 17 and 18] A coating solution shown in Tables 1 and 2 below was formed on 50 μm of ACRYPLEN HBS manufactured by Mitsubishi Chemical Corporation in the same manner as in Example 1. The properties of this laminate are shown in Table 3 below.

[0199] [Comparative Examples 1 and 2] A laminate having a concave-convex layer formed by phase separation was obtained by manufacturing in the same manner as in Example 1, except that the primer layer and the functional layer were not provided in Example 1. The obtained laminate was evaluated, and as shown in Table 3 below, it had no adhesion to the base layer, no antifouling properties, and no antistatic properties, and no functions other than those of the concave-convex layer were observed.

[0200] [Comparative Example 3] A film was obtained by producing in the same manner as in Example 1, except that the primer layer, the uneven layer, and the functional layer were not provided in Example 1. As shown in Table 3 below, the obtained film did not have a matte finish.

[0201] [Table 1]

[0202] [Table 2]

[0203] [Table 3] [Explanation of symbols]

[0204] 1 Base material layer 2 Uneven layer 3 Primer layer 4 Surface functional layer 5 Back functional layer 10 Laminate

Claims

1. A substrate layer and a concavo-convex layer having concavo-convex portions formed by phase separation and provided on one surface of the substrate layer, The present invention further comprises one or more layers selected from the group consisting of a primer layer provided between the base layer and the uneven layer, a surface functional layer provided on the surface of the uneven layer opposite to the base layer side, and a back functional layer provided on the surface of the base layer opposite to the uneven layer side, the surface functional layer having at least an antistatic layer, and a surface resistance of 2×10 at the outermost surface on the side where the uneven layer is present relative to the base layer. 10 Ω or less, the uneven layer is a cured product of a composition containing a compound (X) containing at least one polar group selected from a hydroxyl group, an amino group, an amide group, a sulfonyl group, a phosphate ester group, and a thiol group, and a compound (Y) not containing the polar group, The compound (X) is a (meth)acrylic polymer, The (meth)acrylic polymer has a (meth)acryloyl equivalent of 1.0 mmol / g or more and 10.0 mmol / g or less, The laminate, wherein the compound (X) has an SP value of 17.0 to 19.5, the compound (Y) has an SP value of 12.0 to 13.5, and a difference in the SP values ​​between the compound (X) and the compound (Y) is 4.1 to 5.

3.

2. The laminate according to claim 1, wherein the surface functional layer is an antifouling layer, an antistatic layer, a refractive index adjusting layer, an infrared absorbing layer, an ultraviolet absorbing layer, or a color correction layer, and the back functional layer is an adhesive layer, an antistatic layer, a refractive index adjusting layer, or an antiblocking layer.

3. 3. The laminate according to claim 1, wherein the thickness of the front surface functional layer is 0.001 to 3 μm, and the thickness of the back surface functional layer is 0.001 to 30 μm.

4. The laminate according to any one of claims 1 to 3, wherein the haze of the outermost surface on the side of the base layer where the uneven layer is present is 0.5 to 99%.

5. The laminate according to any one of claims 1 to 4, wherein the 60° specular gloss of the outermost surface on the side of the base layer where the uneven layer is present is 100 or less.

6. The surface functional layer or the primer layer has an antistatic layer, and the surface resistance of the outermost surface on the side where the uneven layer is present with respect to the base layer is 1×10 13 The laminate according to any one of claims 1 to 5, wherein the elastic modulus is Ω.

7. The back functional layer has an antistatic layer, and the surface resistance of the outermost surface of the base layer opposite to the side where the uneven layer is present is 1×10 13 The laminate according to any one of claims 1 to 6, having a resistance of Ω or less.

8. The laminate according to any one of claims 1 to 7, wherein (X):(Y), which represents a mass ratio of the compound (X) to the compound (Y) in the uneven layer, is 10:90 to 80:

20.

9. The laminate according to any one of claims 1 to 8, wherein the uneven layer has a thickness of 1 to 10 µm.

10. The laminate according to any one of claims 1 to 9, wherein the substrate layer has a thickness of 2 to 350 µm.

11. The laminate according to any one of claims 1 to 10, wherein the substrate layer is a substrate selected from the group consisting of a polyester film, a polyacrylate film, a polyolefin film, a polycarbonate film, a polyimide film, and a triacetyl cellulose film.

12. The laminate according to any one of claims 1 to 11, wherein the primer layer contains a resin.

13. The laminate according to any one of claims 1 to 12, wherein the primer layer contains a compound derived from a crosslinking agent.

14. The laminate according to any one of claims 1 to 13, wherein the primer layer contains an antistatic agent.

15. The laminate according to any one of claims 1 to 14, wherein the (meth)acrylic polymer is obtained by reacting an epoxy group with a carboxylic acid.

16. The laminate according to any one of claims 1 to 15, wherein the compound (X) contains a carbon-carbon unsaturated bond.

17. The laminate according to any one of claims 1 to 16, wherein the compound (Y) is a (meth)acrylic polymer.

18. The laminate according to any one of claims 1 to 17, wherein the compound (Y) is a (meth)acrylate.

Citation Information

Patent Citations

  • JP1974001914A

  • Anti-glare hard coat film and display device using the same

    JP2007058204A

  • Newton ring-preventing film and touch panel

    JP2011002820A

  • Optical laminated body

    JP2011031501A

  • Anti-glare film and method for manufacturing the same

    JP2017146620A