Structures and circuit boards

The structure with silicon nitride crystal grains and oxide regions addresses the need for improved reliability by enhancing thermal shock resistance and maintaining structural integrity.

JP7594355B2Active Publication Date: 2024-12-04KK TOSHIBA
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2019168946
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-09-18
Publication Date
2024-12-04
Estimated Expiration
2039-09-18

AI Technical Summary

Technical Problem

There is a demand for improved reliability of structures containing silicon nitride.

Method used

The structure includes first crystal grains of silicon nitride with second crystal grains composed of scandium, yttrium, lanthanum, and other elements, surrounded by a first region of an oxide, which enhances thermal shock resistance and reliability.

Benefits of technology

The structure exhibits improved thermal shock resistance and reliability, maintaining bending strength and thermal conductivity with optimized volume ratios and oxygen concentrations of the crystal grains.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594355000001
    Figure 0007594355000001
  • Figure 0007594355000002
    Figure 0007594355000002
  • Figure 0007594355000003
    Figure 0007594355000003
Patent Text Reader

Abstract

To provide a structure and a circuit board capable of improving reliability.SOLUTION: A structure according to an embodiment comprises a first crystal particle, a second crystal particle, and a first region. The first crystal particle includes silicon nitride. The second crystal particle includes a first element selected from a first group consisting of scandium, yttrium, lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, aluminum, chromium, zirconium, magnesium, zinc, titanium, gallium, beryllium, calcium, strontium, barium, hafnium, vanadium, niobium, tantalum, tungsten, iron, cobalt, nickel, and copper, and oxygen. The first region includes an oxide of the first element.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] SUMMARY OF THE DISCLOSURE The present invention relates to a structure and a circuit board. [Background technology]

[0002] There is a demand for improved reliability for structures containing silicon nitride. [Prior art documents] [Non-patent literature]

[0003] [Non-Patent Document 1] Journal of the Ceramic Society of Japan 104 [1] 63-70 (1996) Summary of the Invention [Problem to be solved by the invention]

[0004] SUMMARY OF THE DISCLOSURE Embodiments of the present invention provide structures and circuit boards that can improve reliability. [Means for solving the problem]

[0005] The structure according to the embodiment includes a first crystal grain, a second crystal grain, and a first region. The first crystal grain includes silicon nitride. The second crystal grain includes a first element selected from a first group consisting of scandium, yttrium, lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, aluminum, chromium, zirconium, magnesium, zinc, titanium, gallium, beryllium, calcium, strontium, barium, hafnium, vanadium, niobium, tantalum, tungsten, iron, cobalt, nickel, and copper, and oxygen. The first region includes an oxide of the first element. [Brief description of the drawings]

[0006] [Figure 1] 1(a) to 1(c) are schematic cross-sectional views illustrating a structure according to an embodiment. [Diagram 2] 2A and 2B are schematic cross-sectional views illustrating another structure according to the embodiment. [Diagram 3] 3A and 3B are schematic cross-sectional views illustrating another structure according to the embodiment. [Figure 4] 4A and 4B are schematic cross-sectional views illustrating other structures according to the embodiment. [Diagram 5] 5(a) and 5(b) are schematic perspective views illustrating the structure according to the embodiment. [Figure 6] FIG. 6 is a schematic cross-sectional view illustrating the circuit board according to the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] Hereinafter, embodiments of the present invention will be described with reference to the drawings. The drawings are schematic or conceptual, and the relationship between the thickness and width of each part, the size ratio between parts, etc. are not necessarily the same as those in reality. Even when the same part is shown, the dimensions and ratios of each part may be different depending on the drawing. In this specification and each drawing, elements similar to those already explained are given the same reference numerals and detailed explanations are omitted as appropriate.

[0008] 1(a) to 1(c) are schematic cross-sectional views illustrating a structure according to an embodiment. A structure 110 according to the embodiment includes first crystal grains 11, second crystal grains 12, and a first region 21, as shown in FIGS.

[0009] The first crystal grains 11 include crystalline silicon nitride. The second crystal grains 12 are provided in the first crystal grains 11. The second crystal grains 12 include a first element selected from a first group consisting of scandium, yttrium, lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, aluminum, chromium, zirconium, magnesium, zinc, titanium, gallium, beryllium, calcium, strontium, barium, hafnium, vanadium, niobium, tantalum, tungsten, iron, cobalt, nickel, and copper, and oxygen. For example, the second crystal grains 12 include crystals of an oxide of the first element.

[0010] A plurality of first crystal grains 11 are provided. The plurality of first crystal grains 11 are provided around the second crystal grains 12. For example, the second crystal grains 12 are surrounded by a plurality of first crystal grains 11. The second crystal grains 12 are located between one first crystal grain 11 and another first crystal grain 11. For example, at least a part of the second crystal grains 12 contacts at least one of the one first crystal grain 11 and the other first crystal grain 11. It is preferable that the second crystal grains 12 are surrounded by or contact the first crystal grains 11, because the second crystal grains 12 can absorb the strain generated in the first crystal grains 11.

[0011] Also, for example, the crystal lattice of at least a part of the second crystal grain 12 is matched with the crystal lattice of at least a part of the one first crystal grain 11 and with the crystal lattice of at least a part of the other one first crystal grain 11. The composition of the first crystal grain 11 is, for example, a general formula of SiN 4±x (0≦x≦0.1) Furthermore, at least one element selected from the group consisting of Al and O may be contained inside the crystal lattice of the first crystal grains 11.

[0012] For example, the crystal structure of the first crystal grains 11 is hexagonal. For example, when the second crystal grains 12 contain yttrium, the crystal structure of the second crystal grains 12 is cubic.

[0013] A first region 21 is provided between the first crystal grains 11. The first region 21 may be provided between at least one of the first crystal grains 11 and the second crystal grain 12. The first region 21 is amorphous. The first region 21 may include a crystalline phase. That is, the first region 21 may be composed of only an amorphous phase, or may include both an amorphous phase and a crystalline phase. When the first region 21 includes a crystalline phase, the composition of the crystalline phase is different from the composition of the second crystal grains. The first region 21 includes an oxide of a first element.

[0014] The shapes of the first crystal grains 11 and the second crystal grains 12 may vary depending on the cross section, as shown in Figures 1(a) to 1(c). The shapes of the first crystal grains 11 and the second crystal grains 12 may be any shape, such as a circle, an ellipse, a substantially square, or a substantially triangular shape.

[0015] The structure 110 including the second crystal grains 12 can improve the resistance to thermal shock of the structure 110. This can improve the reliability of the structure 110.

[0016] For example, the volume fraction of one second crystal grain 12 in the structure 110 is 0.0001 vol% or more and 5 vol% or less. Preferably, the volume fraction is 0.0001 vol% or more and 1 vol% or less. Having the volume fraction within this range is preferable because it is possible to improve thermal shock resistance while maintaining bending strength and thermal conductivity. More preferably, the volume fraction is 0.0001 vol% or more and 0.5 vol% or less. Having the volume fraction within this range is more preferable because it is possible to improve thermal shock resistance while maintaining bending strength and thermal conductivity at a higher level.

[0017] The oxygen concentration in at least one of the plurality of first crystal grains 11 is greater than 0 wt% and equal to or less than 0.1 wt%. Preferably, the oxygen concentration is greater than 0 wt% and equal to or less than 0.01 wt%. With the oxygen concentration in this range, the thermal conductivity can be improved, which is preferable. More preferably, the oxygen concentration is greater than 0 wt% and equal to or less than 0.005 wt%. With the oxygen concentration in this range, the thermal conductivity can be further improved, which is more preferable.

[0018] In one cross section of the structure 110, the ratio of the average of the minimum diameters of the first crystal grains 11 to the average of the maximum diameters of the first crystal grains 11 is greater than 0 and less than 0.1. The ratio of the maximum diameter of the second crystal grains 12 to the average of the maximum diameters of the first crystal grains 11 is greater than 0.001 and less than 0.5. The maximum diameter is the length of the longest line segment among the multiple line segments obtained by connecting any two points on the outer edge of one crystal grain in one cross section. The minimum diameter is the length of a line segment that passes through the center of the longest line segment among the multiple line segments and is perpendicular to the longest line segment. FIG. 1(a) shows, as an example, the maximum diameter L1 of one first crystal grain 11, the minimum diameter L2 of one first crystal grain 11, and the maximum diameter of the second crystal grain 12.

[0019] 2(a), 2(b), 3(a), 3(b), 4(a), and 4(b) are schematic views illustrating other structures according to the embodiment.

[0020] The structure 120 shown in Figures 2(a) and 2(b) further includes a third crystal grain 13. The third crystal grain 13 includes a second element selected from a first group and oxygen. For example, the third crystal grain 13 includes crystals of an oxide of the second element. The second element is different from the first element.

[0021] A part of the first crystal grains 11 is provided around the third crystal grain 13. Another part of the first crystal grains 11 is provided around the second crystal grain 12. For example, the third crystal grain 13 is surrounded by the first crystal grains 11. The third crystal grain 13 is located between one first crystal grain 11 and another first crystal grain 11. For example, at least a part of the third crystal grain 13 contacts the one first crystal grain 11 and the other first crystal grain 11. For example, the crystal lattice of at least a part of the third crystal grain 13 is matched with the crystal lattice of at least a part of the one first crystal grain 11 and the crystal lattice of at least a part of the other first crystal grain 11. The third crystal grain 13 is, for example, away from the second crystal grain 12.

[0022] The shape of the third crystal grains 13 may vary depending on the cross section, as shown in Figures 2(a) and 2(b). The shape of the third crystal grains 13 may be any shape, such as a circle, an ellipse, a substantially square, or a substantially triangular shape.

[0023] The structure 120 includes the second crystal grains 12 and the third crystal grains 13, and thus it is possible to improve the resistance to thermal shock of the structure 120. As a result, it is possible to improve the reliability of the structure 120.

[0024] In a structure 131 shown in FIG. 3(a), a second crystal grain 12 is provided within one first crystal grain 11. A structure 132 shown in FIG. 3(b) includes a plurality of second crystal grains 12. One of the plurality of second crystal grains 12 is surrounded by a plurality of first crystal grains 11. Another of the plurality of second crystal grains 12 is provided within one first crystal grain 11. The first crystal grain 11 in which the second crystal grain 12 is provided may be one of the plurality of first crystal grains 11 surrounding another second crystal grain 12.

[0025] In the structure 141 shown in FIG. 4(a), the third crystal grain 13 is provided within one of the first crystal grains 11. For example, the third crystal grain 13 is provided within one of the plurality of first crystal grains 11. The second crystal grain 12 is surrounded by two or more of the plurality of first crystal grains 11.

[0026] 4(b) includes a plurality of third crystal grains 13. Each of the second crystal grains and one of the plurality of third crystal grains 13 is surrounded by two or more of the plurality of first crystal grains 11. Another of the plurality of third crystal grains 13 is provided within another of the plurality of first crystal grains 11.

[0027] The first crystal grain 11 having the third crystal grain 13 provided therein may be one of a plurality of first crystal grains 11 surrounding another third crystal grain 13. The structure 142 may further include another second crystal grain 12 provided within one first crystal grain 11. It is preferable that the third crystal grain 11 is surrounded by or in contact with the first crystal grain 11, because this allows the third crystal grain 13 to absorb strain generated in the first crystal grain 11.

[0028] Here, a method for manufacturing a structure according to this embodiment will be described. Weigh out 100 mol% Si, 2 mol% Y2O3, and 5 mol% MgO in terms of Si3N4. Y2O3 and MgO are used as auxiliary agents. Another auxiliary agent that can be used is B2O3, which may be used alone or in combination. The ratio of auxiliary agent is preferably 2 mol% to 20 mol% in terms of Si3N4. These materials are crushed and mixed in a planetary ball mill for 0.5 to 10 hours. If the crushing time is too short, the grain size of the material will be too large, which is not preferable because it reduces the strength of the structure. If the crushing time is too long, it is not preferable because the thermal conductivity will decrease due to oxidation of the material. Next, the mixture is dried, and a binder is added to granulate. At this time, polyvinyl butyral, polyvinyl alcohol, ethyl cellulose, etc. can be used as the binder. These binders may be used alone or in combination. It is preferable to add 2 wt% to 20 wt% of the binder to the mixture. If the amount is less than 2 wt%, the materials are less likely to bond together, and the strength of the structure is reduced, which is not preferable. If the amount is more than 20 wt%, the amount of binder in the structure becomes too large, and the density of the structure is reduced, which is not preferable. Then, 0.3t / cm 2 More than 3t / cm2 The following pressure is applied to mold the material. The pressure should be adjusted according to the material. If the pressure is too low, the bond will be weak and the molded product will easily crumble, which is not recommended. If the pressure is too high, the molded product may crack, which is also not recommended. The molded body is degreased in air at 400°C to 700°C, and then treated in a nitrogen atmosphere at 1200°C to 1400°C. If the degreasing temperature is too low, the binder components remain, which is undesirable. If the degreasing temperature is too high, the raw materials are oxidized, which is undesirable. In addition, if the heat treatment temperature for nitriding is too low, the reaction does not occur easily, which is undesirable. If the heat treatment temperature is too high, the Si melts before nitriding, which is undesirable. The treatment time for degreasing and nitriding(*) is adjusted according to the treatment temperature. Then, sintering is performed at 1600°C to 2000°C for 1 hour to 96 hours to obtain the structure according to the embodiment. If the sintering temperature is too low, the structure will not be densified, which is not preferable. If the sintering temperature is too high, grain growth will be excessive. This will result in a decrease in strength and a composition shift due to volatilization of Si, which is not preferable. The same applies to the sintering time.

[0029] An example of a method for manufacturing a structure according to the embodiment will be specifically described. Weigh out 100 mol% Si, 2 mol% Y2O3, and 5 mol% MgO in terms of Si3N4. Y2O3 and MgO are used as auxiliary agents. These materials are crushed and mixed in a planetary ball mill for 1 hour. The mixture is dried and 5 wt% polyvinyl butyral is added as a binder to granulate. Then, 1 t / cm 2 The molded body is degreased in air at 500°C, and then treated in a nitrogen atmosphere at 1400°C for 8 hours. Then, sintering is performed at 1900°C for 24 hours to obtain the structure according to the embodiment. In the manufacturing method of the structure according to the comparative example, 100 mol% Si, calculated as Si3N4, 2 mol% Y2O3, and 5 mol% MgO are weighed out. Y2O3 and MgO are used as auxiliary agents. These materials are crushed and mixed in a planetary ball mill for 1 hour. The mixture is dried and powdered in an isostatic press at 3 t / cm. 2The mixture is molded under a pressure of 100000000. The mixture is then treated in a nitrogen atmosphere at 1400°C for 8 hours. The mixture is then sintered at 1900°C for 24 hours to obtain a structure according to the comparative example.

[0030] The oxygen concentration in the first crystal grains 11 and the volume fraction of the second crystal grains 12 of the obtained structure were measured. In this example, the second crystal grains 12 contain Y2O3 crystals. As a result of the measurements, in the structure according to the embodiment, the volume fraction of the second crystal grains 12 was 0.003 vol%. The oxygen concentration in the first crystal grains 11 was 0.015 wt%. The thermal conductivity of the obtained structure was evaluated and found to be 105 W / (mK). In the structure of the comparative example, no Y2O3 crystals were observed. Therefore, in the comparative example, the volume ratio of the second crystal grains 12 was 0 vol%. In the comparative example, the oxygen concentration of the first crystal grains 11 was 0.01 wt%, and the thermal conductivity was 110 W / (mK).

[0031] Furthermore, a three-point bending strength evaluation (JIS-R-1601 (2008)) was performed, and the bending strength of the structure according to the embodiment was 711 MPa. Furthermore, a thermal shock test was performed as follows. A test in which a test piece heated to 1000°C in an electric furnace was dropped into water was repeated 10 times. After that, the above-mentioned three-point bending test was performed, and the bending strength of the structure according to the embodiment was 723 MPa. This value is almost the same as the value measured before the thermal shock test. In contrast, the three-point bending strength of the structure according to the comparative example was 705 MPa. Furthermore, when a three-point bending test was performed after a similar thermal shock test, the bending strength of the structure according to the comparative example decreased to 598 MPa.

[0032] The volume of the second crystal grains 12 in the structure is measured as follows. A transmission electron microscope (TEM) is used to obtain an image of a portion of the cross section of the structure. The magnification for observing the structure is arbitrary. For example, the magnification is preferably 20,000 times or more. The second crystal grains 12 are found by mapping analysis using energy dispersive X-ray analysis (EDX). For example, the electron diffraction pattern can confirm that the second crystal grains 12 are single crystals. Although the electron diffraction pattern of the second crystal grains 12 is one point of information, since they are single-phase particles, they can be considered as single crystals that remain without dissolving. The area occupied by the second crystal grains 12 in the entire area being observed is calculated. The same process is repeated in multiple fields of view. The areas of the second crystal grains 12 in the entire structure are calculated and averaged, and the average result is raised to the power of 3 / 2 to obtain the volume ratio.

[0033] The maximum and minimum diameters of each of the first crystal grains 11 can be measured using a TEM. For example, ten first crystal grains 11 are arbitrarily selected from the observation field of view. The observation field of view is set to, for example, 3500 nm × 3500 nm. The first crystal grains 11 that are partially cut off at the edge of the observation field of view are excluded from the measurement. Next, the maximum and minimum diameters of each of the selected ten first crystal grains 11 are measured. The first crystal grain 11 with the largest maximum diameter and the first crystal grain 11 with the smallest minimum diameter are excluded from the selected ten. As a result, eight or nine first crystal grains 11 remain. Using the maximum and minimum diameters of each of the remaining first crystal grains 11, the ratio of the average of the minimum diameter to the average of the maximum diameter is calculated. When calculating the ratio of the maximum diameter of the second crystal grains 12 to the average of the maximum diameters of the plurality of first crystal grains, the average of the maximum diameters of the plurality of first crystal grains is calculated in the same manner.

[0034] The method for measuring the oxygen concentration in the first crystal grains 11 is as follows. The resulting structure is crushed using a vibrating mill. After removing most of the grain boundaries, hydrofluoric acid and sulfuric acid are used to remove the grain boundaries and the oxide layer on the surface. After washing with water, the structure is sieved using a 100# sieve. The sample obtained by sieving is heated at 2500°C, and the released gas is analyzed to determine the oxygen concentration. This measurement method is described, for example, in Adv. Mater. 2011, 23, 4563-4567. Alternatively, mapping of elements in the second crystal grains 12 may be obtained using EDX, and the oxygen concentration may be calculated based on the mapping result.

[0035] (Modification) Each of the structures according to the above-described embodiments preferably further contains boron (boron: B). By containing boron, a structure having higher thermal conductivity and excellent resistance to strong thermal shock can be realized. The molar ratio of the boron content contained in the structure to the silicon (Si) content contained in the structure (boron content / silicon content) is 0.00 1% That's all, 1% It is presumed that by keeping the molar ratio within this range, if the surfaces of the first crystal grains 11 are nitrided due to thermal runaway during nitridation, the aggregation of silicon particles can be suppressed even if the silicon melts. As a result, it is presumed that the silicon is suppressed from precipitating as lumps, and nitridation can proceed smoothly. Moreover, the molar concentration of boron contained in the first region 21 is greater than the molar concentration of boron contained in the first crystal grains 11, the molar concentration of boron contained in the second crystal grains 12, and the molar concentration of boron contained in the third crystal grains 13. The molar concentration of boron contained in the first region 21 being greater than the molar concentrations of boron contained in each of the first crystal grains 11 and the second crystal grains 12 is preferable because it allows the nitriding reaction to proceed smoothly. Moreover, the molar concentration of boron contained in the first region 21 is greater than the molar concentration of boron contained in the third crystal grains 13. More preferably, the first region 21 contains boron. For example, the first region 21 contains an oxide of boron. For example, the molar ratio of the number of moles of boron contained in the first region 21 to the number of moles of silicon contained in the first crystal grains 11 (number of moles of boron contained in the first region 21 / number of moles of silicon contained in the first crystal grains 11) is 0.00 1% That's all, 1% Preferably, the molar ratio of the number of moles of boron contained in the first region 21 to the number of moles of silicon contained in the first crystal grains 11 is 0.00 or less. 5% Above, 0. 5%More preferably, the molar ratio of the number of moles of boron contained in the first region 21 to the number of moles of silicon contained in the first crystal grains 11 is 0.0 or less. 1% Above, 0. 5% By having the molar ratio within this range, even if silicon melts due to thermal runaway during nitridation, aggregation of silicon can be suppressed, and precipitation of silicon lumps can be suppressed, allowing nitridation to proceed more smoothly, which is more preferable.

[0036] The manufacturing method for the modified example is similar to the above-mentioned method, except for adding a boron compound. The boron compound is preferably added in an amount of 0.001 mol% to 1 mol% relative to Si. This range prevents silicon from precipitating as agglomerates, and allows nitridation to proceed more smoothly.

[0037] A specific example of a method for manufacturing a structure according to the modified example will be described. Si was weighed out at 100 mol% in terms of Si3N4, Y2O3 at 2 mol%, and MgO at 5 mol%. At this time, B2O3 was added at 0.1 mol% relative to Si. Thereafter, the same process as in the manufacturing method of the structure according to the embodiment was carried out. In the manufactured structure, the volume ratio of Y2O3 crystal grains in the first crystal grains 11 was 0.005 vol%. The oxygen concentration in the first crystal grains 11 was 0.013 wt%. The thermal conductivity of the manufactured structure was 111 W / (mK).

[0038] As a result of producing a structure by the above-mentioned manufacturing method, it was found that the precipitation of silicon in the structure can be suppressed. By suppressing the precipitation of silicon, it is possible to improve the thermal shock resistance, thermal conductivity, or bending strength of the structure.

[0039] It is believed that the silicon nitride sintered body is formed from silicon for the following reasons. When the molded body is heated in a nitrogen atmosphere, silicon nitride (e.g., Si3N4) is formed. After that, the oxide of the element selected from the first group forms a liquid phase. The silicon nitride (e.g., Si3N4) is enveloped in the liquid phase. The liquid phase dissolves the silicon nitride like a flux. As a result, the constituent atoms of the silicon nitride become more mobile, promoting the growth of silicon nitride particles. For this reason, the oxide is also called a sintering aid. The liquid phase is rapidly cooled during the cooling process after sintering is completed, so it does not crystallize but becomes an amorphous phase. The inventors of the present application discovered that by completing the nitriding and then sintering before the sintering aid becomes completely liquid, a portion of the aid is incorporated in the silicon particles as a solid. The incorporated aid does not form a eutectic with other aids, but remains as a crystal. This makes it possible to prevent oxygen from the raw silicon particles from remaining in the silicon nitride particles. Furthermore, the inclusion of boron (especially B2O3) in the structure promotes nitridation. This is thought to be because the oxide layer on the surface of the silicon particles and boron oxide form a eutectic at low temperatures (for example, below 1000°C) and become liquid, allowing nitridation to proceed at low temperatures. If the surface of the silicon particles is nitrided to a certain extent, the silicon particles will not aggregate together even if they melt. This makes it possible to suppress the precipitation of silicon.

[0040] FIG. 5 is a perspective view illustrating a structure according to the embodiment. For example, as shown in Fig. 5(a) and Fig. 5(b), the structure according to the embodiment is a substrate. The shape of the substrate is arbitrary. One cross section of the substrate includes any of the structures shown in Fig. 1(a) to Fig. 1(c), Fig. 2(a), Fig. 2(b), Fig. 3(a), Fig. 3(b), Fig. 4(a), and Fig. 4(b). Alternatively, the structure according to the embodiment may be a bearing or the like.

[0041] FIG. 6 is a schematic cross-sectional view illustrating the circuit board according to the embodiment. As shown in Fig. 6, a circuit board 210 according to the embodiment includes a first metal part 31 and a structure 110. Instead of the structure 110, a structure shown in Fig. 2(a), Fig. 2(b), Fig. 3(a), Fig. 3(b), Fig. 4(a), or Fig. 4(b) may be provided. In this example, the structure 110 is used as a substrate.

[0042] The first metal part 31 is joined to the structure 110. For example, a joint 41 is provided between the first metal part 31 and the structure 110. The first metal part 31 may be joined directly to the structure 110 without the joint 41 being interposed therebetween.

[0043] 6, the circuit board 210 further includes a second metal portion 32 and a semiconductor element 50. The semiconductor element 50 is bonded to the first metal portion 31. The first metal portion 31 is located between the structure 110 and the semiconductor element 50. For example, a joint portion 42 is provided between the semiconductor element 50 and the first metal portion 31. The semiconductor element 50 may be bonded directly to the first metal portion 31 without the joint portion 42 being interposed therebetween.

[0044] The second metal part 32 is joined to the structure 110. The structure 110 is located between the first metal part 31 and the second metal part 32. For example, a joint part 43 is provided between the second metal part 32 and the structure 110. The second metal part 32 may be joined directly to the structure 110 without the joint part 43. The second metal part 32 functions as, for example, a heat sink.

[0045] The first metal portion 31 and the second metal portion 32 include, for example, at least one selected from the group consisting of copper, aluminum, and silver. The bonding portions 41 to 43 include, for example, at least one selected from the group consisting of silver and copper. The bonding portions 41 to 43 may further include at least one selected from the group consisting of titanium, hafnium, zirconium, niobium, indium, tin, and carbon. The semiconductor element 50 includes, for example, a diode, a MOSFET, or an IGBT.

[0046] By using the structure 110, it is possible to improve the resistance of the circuit board 210 to thermal shock, thereby improving the reliability of the circuit board 210.

[0047] According to each of the embodiments described above, it is possible to provide a structure and a circuit board capable of improving heat resistance.

[0048] The above describes the embodiments of the present invention with reference to specific examples. However, the embodiments of the present invention are not limited to these specific examples. For example, the specific configurations of each element, such as the first crystal grain, the second crystal grain, the third crystal grain, the first region, the metal part, the joint part, and the semiconductor element, contained in the structure and the circuit board are included in the scope of the present invention as long as a person skilled in the art can carry out the present invention in a similar manner and obtain the same effect by appropriately selecting them from the known range.

[0049] Furthermore, any combination of two or more elements of each of the specific examples, within the scope of technical feasibility, is also included within the scope of the present invention as long as it includes the gist of the present invention.

[0050] In addition, all structures and circuit boards that can be implemented by a person skilled in the art through appropriate design modifications based on the structures and circuit boards described above as embodiments of the present invention also fall within the scope of the present invention as long as they include the gist of the present invention.

[0051] In addition, within the scope of the concept of the present invention, a person skilled in the art may conceive of various modifications and alterations, and it will be understood that these modifications and alterations also fall within the scope of the present invention.

[0052] Although some embodiments of the present invention have been described, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their modifications are included in the scope and spirit of the invention, and are included in the scope of the invention and its equivalents described in the claims. [Explanation of symbols]

[0053] 11 first crystal grain, 12 second crystal grain, 13 third crystal grain, 21 first region, 31 first metal portion, 32 second metal portion, 41-43 joint portion, 50 semiconductor element, 110, 120, 131, 132, 141, 142 structure, 210 circuit board, L1-L3 length

Claims

1. First crystal grains including silicon nitride; a single-crystalline second crystal grain including a first element selected from a first group consisting of scandium, yttrium, lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, and lutetium, and oxygen; a first region including an oxide of the first element; A structure equipped with:

2. The first crystal grains are provided in plurality, The structure according to claim 1 , wherein the plurality of first crystal grains are disposed around the second crystal grain.

3. The first crystal grains are provided in plurality, the second crystal grain is located between one of the plurality of first crystal grains and another of the plurality of first crystal grains; The structure of claim 1 , wherein at least a portion of the second crystal grain is in contact with at least one of the one of the plurality of first crystal grains and the other one of the plurality of first crystal grains.

4. Further comprising a third crystal grain including a second element selected from the first group and oxygen; The structure of claim 1 , wherein the second element is different from the first element.

5. The first crystal grains are provided in plurality, The second crystal grain is surrounded by a portion of the first crystal grains, The structure according to claim 4 , wherein the third crystal grain is surrounded by another portion of the plurality of first crystal grains.

6. The second crystal grain is in contact with at least one of the portions of the first crystal grains, The structure according to claim 5 , wherein the third crystal grain is in contact with at least one of the other portions of the plurality of first crystal grains.

7. The structure according to claim 4 , wherein the third crystal grains are disposed within the first crystal grains.

8. First crystal grains containing silicon nitride and having an oxygen concentration of more than 0 wt % and not more than 0.1 wt %; second crystal grains including a first element selected from a first group consisting of scandium, yttrium, lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, and lutetium, and oxygen; a first region including an oxide of the first element; A structure equipped with:

9. First crystal grains including silicon nitride; second crystal grains containing a first element selected from a first group consisting of scandium, yttrium, lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, and lutetium, and oxygen, the second crystal grains having a volume fraction of 0.0001 vol % or more and 5 vol % or less; a first region including an oxide of the first element; A structure equipped with:

10. First crystal grains including silicon nitride; second crystal grains including a first element selected from a first group consisting of scandium, yttrium, lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, and lutetium, and oxygen; a first region including an oxide of the first element and boron; A structure equipped with:

11. The structure according to claim 10 , wherein a molar ratio of the number of moles of boron contained in the first region to the number of moles of silicon contained in the first crystal grains is 0.001 or more and 1 or less.

12. 7. The structure according to claim 2, wherein a ratio of an average of a minimum diameter of the plurality of first crystal grains to an average of a maximum diameter of the plurality of first crystal grains is greater than 0 and less than or equal to 0.

1.

13. 13. The structure according to claim 2, wherein a ratio of a maximum diameter of the second crystal grains to an average of a maximum diameter of the plurality of first crystal grains is 0.001 or more and 0.5 or less.

14. First crystal grains including silicon nitride; second crystal grains including a first element selected from a first group consisting of scandium, yttrium, lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, and lutetium, and oxygen; a first region including an oxide of the first element; Equipped with A structure, wherein the molar ratio of the boron content to the silicon content is 0.001% or more and 1% or less.

15. First crystal grains including silicon nitride; second crystal grains including a first element selected from a first group consisting of scandium, yttrium, lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, and lutetium, and oxygen; a first region including an oxide of the first element; Equipped with A structure in which the molar concentration of boron contained in the first region is greater than the molar concentration of boron contained in the first crystal grains and is greater than the molar concentration of boron contained in the second crystal grains.

16. The structure according to any one of claims 1 to 15, wherein the first element is yttrium.

17. The structure according to any one of claims 1 to 16, wherein the second crystal grains are single crystals made of the first element and oxygen.

18. The structure according to any one of claims 1 to 17, A first metal part joined to the structure; A circuit board comprising:

19. Further comprising a semiconductor element joined to the first metal portion, The circuit board according to claim 18 , wherein the first metal portion is located between the structure and the semiconductor element.

Citation Information

Patent Citations

  • Highly thermoconductive silicon nitride sintered compact and its production

    JP2000034172A

  • Ceramic plate and electronic apparatus

    JP2018184337A