Aluminum alloy clad material for heat exchangers and heat exchangers

The aluminum alloy cladding material balances strength, corrosion resistance, and brazing properties by optimizing compositions and particle dispersion, resulting in a heat exchanger with enhanced durability and brazing performance.

JP7594467B2Active Publication Date: 2024-12-04MA ALUMINUM CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021035088
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-05
Publication Date
2024-12-04
Estimated Expiration
2041-03-05

AI Technical Summary

Technical Problem

Existing aluminum alloy cladding materials for heat exchangers face challenges in achieving a balance between high strength, corrosion resistance, and brazing properties due to the inclusion of elements like Si or Cu, which can improve some properties but degrade others.

Method used

The aluminum alloy cladding material is formulated with specific compositions of Mn, Si, Fe, and Cu in the core material, and Zn, Mn, Si, and Fe in the sacrificial material, with controlled dispersion of second-phase particles, and optimized homogenization and rolling processes to enhance strength, corrosion resistance, and brazing properties.

Benefits of technology

The solution results in a heat exchanger with improved corrosion resistance and durability, achieving a tensile strength of 140 MPa or more, while maintaining excellent brazing properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594467000003
    Figure 0007594467000003
  • Figure 0007594467000004
    Figure 0007594467000004
  • Figure 0007594467000005
    Figure 0007594467000005
Patent Text Reader

Abstract

To provide an aluminum alloy-clad material for heat exchangers having excellent strength, brazing suitability, and corrosion resistance.SOLUTION: An aluminum alloy-clad material for heat exchangers has: a core containing Mn: 1.0-1.5 mass%, Si: 0.5-0.9 mass%, and Fe: 0.3-0.6 mass% with the balance being Al and unavoidable impurities; a sacrificial material that contains Zn: 2.5-4.0 mass%, Mn: 0.7-1.3 mass%, Si: 0.3-0.7 mass%, and Fe: 0.3-0.7 mass% with the balance being Al and unavoidable impurities; and a solder material composed of an Al-Si alloy. In the core before brazing, in-core second phase particles with a circle equivalent diameter of 50-200 nm are dispersed. The in-core second phase particles have a number density of 1000000 / mm2 or less. In the sacrificial material before brazing, in-sacrificial material second phase particles with a circle equivalent diameter of 50-200 nm are dispersed and the in-sacrificial material second phase particles have a number density of 320000-440000 / mm2.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an aluminum alloy clad material for heat exchangers used in automobiles and the like, and to such heat exchangers. [Background technology]

[0002] Heat exchangers are generally made of various aluminum alloy clad materials with brazing material or sacrificial material on one or both sides of the core material. Currently, aluminum alloy clad materials for heat exchangers are required to be thin and strong in order to reduce the weight of automobiles. In particular, automotive heat exchangers that cool fluids such as engines and engine oil require high corrosion resistance on the cooling water channel side. Furthermore, since automotive heat exchangers require joining of various components by brazing heat treatment, brazeability is also important. For example, in Patent Document 1, Si or Cu is contained in the core material to improve strength. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2014-31588 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, although the inclusion of Si or Cu in the core material improves strength, it also has trade-offs, such as a decrease in corrosion resistance or brazing ability, making it difficult to satisfy all of these properties. The present invention has been made in light of the above circumstances, and has an object to provide an aluminum alloy clad material for heat exchangers, and a heat exchanger, which have excellent strength, corrosion resistance and brazing properties. [Means for solving the problem]

[0005] In the invention of the aluminum alloy clad material for heat exchangers of the present invention, a first embodiment of the present invention comprises a core material containing 1.0-1.5 mass% Mn, 0.5-0.9 mass% Si, 0.3-0.6 mass% Fe, with the balance being Al and unavoidable impurities, a sacrificial material containing 2.5-4.0 mass% Zn, 0.7-1.3 mass% Mn, 0.3-0.7 mass% Si, 0.3-0.7 mass% Fe, with the balance being Al and unavoidable impurities, and a brazing material made of an Al-Si based alloy, In the core material before brazing, second phase particles having a circle equivalent diameter of 50 to 200 nm are dispersed, and the number density of the second phase particles in the core material is 1,000,000 particles / mm 2 is equal to or less than the above, and In the sacrificial material before brazing, second phase particles having a circle equivalent diameter of 50 to 200 nm are dispersed, and the number density of the second phase particles in the sacrificial material is 320,000 to 440,000 particles / mm 2 It is.

[0006] A second aspect of the invention of the aluminum alloy clad material for heat exchangers is characterized in that, in the above-mentioned aspect of the invention, the core material further contains Cu: 0.1 to 0.6 mass %.

[0007] The invention of a third aspect of the aluminum alloy clad material for heat exchangers is the invention of the above aspect, in which the tensile strength after heat treatment equivalent to brazing at 600°C for 3 minutes is 140 MPa or more.

[0008] The heat exchanger of the present invention is such that the laminated material made of the core material and the sacrificial material in the aluminum alloy clad material for heat exchangers of the above-mentioned embodiment is brazed to another member.

[0009] The items defined in the present invention will be described below. <Core composition> Mn: 1.0-1.5% Mn forms fine Al-Mn-Si, Al-Mn-Fe, and Al-Mn-Fe-Si intermetallic compounds in the matrix, improving the material strength of the core material. However, if the content is below the lower limit, the effect is not fully obtained. On the other hand, if the content exceeds the upper limit, giant intermetallic compounds are generated during casting, and castability and rollability are reduced. For this reason, the Mn content is set to 1.0 to 1.5%. For the same reason, it is preferable to set the lower limit to 1.1% and the upper limit to 1.4%.

[0010] Silicon: 0.5 to 0.9% Silicon forms fine Al-Mn-Si and Al-Mn-Fe-Si intermetallic compounds in the matrix, improving the strength of the material. However, if the content is below the lower limit, the desired effect cannot be obtained sufficiently. On the other hand, if the content exceeds the upper limit, the melting point of the material decreases and the brazing property decreases. For this reason, the content of silicon is set to 0.5 to 0.9%. For the same reason, it is preferable to set the lower limit to 0.6% and the upper limit to 0.8%.

[0011] Fe: 0.3 to 0.6% Fe forms fine Al-Mn-Fe and Al-Mn-Fe-Si intermetallic compounds in the matrix, enhancing the material strength of the core material. However, if the content is below the lower limit, the desired effect cannot be sufficiently obtained. On the other hand, if the content exceeds the upper limit, giant intermetallic compounds are generated during casting, which reduces castability and rollability, and further reduces corrosion resistance. For this reason, the Fe content is set to 0.3 to 0.6%. For the same reason, it is preferable to set the lower limit to 0.35% and the upper limit to 0.55%.

[0012] Cu: 0.1-0.6% Cu dissolves in the matrix and improves the material strength, so it is included as desired. However, if the content is less than the lower limit, the desired effect cannot be obtained sufficiently. On the other hand, if the content exceeds the upper limit, the potential becomes nobler and the corrosion resistance decreases. In addition, the melting point decreases and the brazing property decreases. For this reason, the Cu content is set to 0.1 to 0.6%. For the same reason, it is preferable to set the lower limit to 0.2% and the upper limit to 0.5%. In addition, when Cu is not intentionally included, Cu may be included as an impurity in an amount of 0.1% or less.

[0013] <Sacrificial material> Zn: 2.5-4.0% Zn makes the potential more base and improves the corrosion resistance of the sacrificial material. However, if the content is less than the lower limit, the effect is not fully exerted because the content is too low. On the other hand, if the content exceeds the upper limit, the corrosion rate increases too much, the sacrificial anode effect cannot be obtained, and the corrosion resistance decreases. For this reason, the Zn content is set to 2.5 to 4.0%. For the same reason, it is preferable to set the lower limit to 2.7% and the upper limit to 3.8%.

[0014] Mn: 0.7-1.3%, Mn has the effect of improving the strength of the sacrificial material and improving the corrosion resistance. In addition, Mn has the effect of improving the corrosion resistance by controlling the number and size of dispersed particles of Al-Mn-based second phase particles and dispersing the corrosion points by particle dispersion by containing an appropriate amount of Mn. However, if the content is below the lower limit, the desired effect cannot be obtained. On the other hand, if the content exceeds the upper limit, the sacrificial anode effect due to the potential ennoblement cannot be obtained, and local corrosion occurs. For this reason, the Mn content is set to the range of 0.7 to 1.3%. For the same reason, it is preferable to set the lower limit to 0.8% and the upper limit to 1.2%.

[0015] Silicon: 0.3 to 0.7% Silicon improves corrosion resistance. In addition, when an appropriate amount of silicon is contained together with manganese, it has the effect of controlling the dispersed particle size and improving corrosion resistance. However, if the content is below the lower limit, localized corrosion occurs. On the other hand, if the content exceeds the upper limit, the sacrificial anode effect due to the potential ennoblement cannot be obtained, and localized corrosion occurs. For this reason, the Si content is set in the range of 0.3 to 0.7%. For the same reason, it is preferable to set the lower limit at 0.4% and the upper limit at 0.6%.

[0016] Fe: 0.3 to 0.7% Fe generates Al-Mn-based second phase particles in the matrix, improving corrosion resistance. However, if the content is below the lower limit, the desired effect cannot be obtained sufficiently. On the other hand, if the content exceeds the upper limit, the particle density becomes too high and uniform dispersion is not possible, causing local corrosion in which the dense particle areas corrode locally, resulting in a decrease in corrosion resistance. For this reason, the Fe content is set to a range of 0.3 to 0.7%. For the same reason, it is preferable to set the lower limit to 0.35% and the upper limit to 0.65%.

[0017] <Brazing material> The brazing filler metal is generally an Al-Si alloy (Si: 3-12%, etc.) for brazing to the joined object. In some cases, an Al-Si alloy containing an appropriate amount of Zn is used to improve the corrosion resistance of the outer surface. The present invention does not specify the composition of the brazing filler metal, but any of the above brazing filler metals can be used.

[0018] <Second-phase particles in the core material before brazing: 50 to 200 nm, number density 1,000,000 particles / mm 2 Below> The second phase particles in the core material before brazing affect the recrystallization rate during brazing. If there are many second phase particles of the above sizes, recrystallization is delayed and erosion increases. For this reason, the number density of the above sizes is set to 1,000,000 particles / mm 2 It is preferable to do the following: The control of the number density can be achieved by optimizing the composition and performing homogenization at high temperature for a long time. The homogenization conditions are preferably 560°C to 620°C for 6 to 12 hours. If the temperature is too high, the slab may partially melt and it may be uneconomical in terms of energy costs.

[0019] <Second-phase particles in the sacrificial material before brazing: 50-200 nm, number density 320,000-440,000 particles / mm 2 Corrosion points are dispersed by particle dispersion. If the number of particles is small, the dispersion effect is insufficient, and localized corrosion occurs. On the other hand, if the particle density is too high, the second phase particles are not dispersed uniformly, and the dense particle areas corrode locally. For this reason, the number density of second phase particles of the above size in the sacrificial material before brazing is set to 320,000 to 440,000 pieces / mm2 It is preferable to do so. The control of the number density can be achieved by controlling the appropriate composition, homogenization treatment, and the reduction rate and number of passes in cold rolling.

[0020] <Strength after brazing: 140MPa or more> If the strength is low, the durability of the heat exchanger after brazing and assembly will decrease. Considering the durability as a heat exchanger, it is desirable for the strength after brazing to be 140 MPa or more. Effect of the Invention

[0021] According to the present invention, the corrosion resistance of an aluminum alloy clad material for heat exchangers after brazing can be improved, and the durability of the heat exchanger can be improved. [Brief description of the drawings]

[0022] [Figure 1] 1 is a cross-sectional view of an aluminum alloy clad material for heat exchangers according to one embodiment of the present invention in a state before brazing. [Diagram 2] FIG. 2 is a perspective view showing a portion of a heat exchanger according to an embodiment of the present invention. [Diagram 3] 1 shows a photograph, used as a substitute for a drawing, of a cross section of a test material in an embodiment, observed by a microscope. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In the drawings used in the following description, the characteristic parts may be enlarged for the purpose of emphasizing the characteristic parts, and the dimensional ratios of each component may not be the same as in reality. Also, for the same purpose, non-characteristic parts may be omitted.

[0024] Fig. 1 shows a cross-sectional view of an aluminum alloy clad material 1 used in an automotive heat exchanger of this embodiment. The aluminum alloy clad material 1 is mainly composed of a core material 1a made of an aluminum alloy, a layered sacrificial material 1b clad on one side of the core material 1a, and a layered brazing material 1c clad on the other side of the core material 1a. Although this embodiment is described as being for a heat exchanger for an automobile, the present invention is not limited to use in an automobile.

[0025] The manufacturing process will be described below. An aluminum alloy for a sacrificial material and an aluminum alloy for a core material, each of which is within the composition range of the present invention, and an Al-Si-based (including those containing Zn) brazing material alloy are prepared. These alloys can be melted by a conventional method. The aluminum alloy for the brazing material is not particularly limited in the present invention as long as it is an Al-Si-based alloy, and for example, a JIS 4343 alloy, a 4045 alloy, or a 4047 alloy can be used. A brazing material without Zn or a brazing material with an increased amount of Zn can also be used. Furthermore, an Al-Si alloy or an Al-Si-Zn alloy containing Mn, Fe, Zr, Ti, Cu, Li, etc. can also be used.

[0026] After being melted, these alloys may be subjected to a homogenization treatment, if desired. The core material is homogenized after slab casting in order to remove inhomogeneous structures such as segregation. In this invention, the high-temperature, long-term homogenization promotes the re-dissolution of second-phase particles in the core material, and reduces the particle dispersion density that causes delayed recrystallization during subsequent brazing, thereby suppressing erosion. The preferred homogenization conditions are 560°C or higher. The aluminum alloy for brazing material may also be subjected to homogenization treatment if desired. For example, homogenization treatment may be performed at 560° C. to 620° C. for 6 to 12 hours.

[0027] The purpose of the sacrificial material is to disperse corrosion sites by dispersing second-phase particles (inhibiting local corrosion). Therefore, if homogenization treatment is performed after slab casting to remove inhomogeneous structures such as segregation and to round off coarse intermetallic compounds to improve surface machinability, the second-phase particles cannot be reduced and the coarse intermetallic compounds cannot be dispersed by crushing during rolling (rounded particles make them difficult to crush), which reduces the dispersion effect of the second-phase particles. Therefore, the preferable condition for performing homogenization treatment is 300°C or less, and it does not have to be performed.

[0028] The ingot is then hot-rolled into a plate material, or may be continuously cast and rolled into a plate material. These plate materials are clad with an appropriate cladding ratio in a stacked state with a sacrificial material placed on one side of a core material and a brazing material placed on the other side. The cladding ratio of each member is not particularly limited, but for example, the core material is 60% to 90%, the sacrificial material is 5% to 30%, and the brazing material is 5% to 30%. In the manufacture of clad materials, hot rolling is generally performed, followed by further cold rolling to obtain an aluminum alloy brazing sheet of the desired thickness. Next, cold rolling is performed to obtain the specified thickness, and the coarse intermetallic compounds in the sacrificial material are crushed and dispersed by cold rolling, with the aim of dispersing second phase particles as well. The preferred conditions for cold rolling are that if the reduction is small, the coarse intermetallic compounds cannot be crushed, and if it is large, they are crushed too much, so it is desirable to perform 5 passes or more with a reduction of 10 to 35%.

[0029] By carrying out final cold rolling, the sheet thickness is desirably adjusted to 0.1 to 1.0 mm, although the present invention is not limited to a specific final sheet thickness. By the above steps, an aluminum alloy clad material for heat exchangers can be obtained.

[0030] In the clad material, before brazing, second phase particles having a circle equivalent diameter of 50 to 200 nm are dispersed in the core material, and the number density of the second phase particles is 1,000,000 particles / mm 2or less, second-phase particles having a circle equivalent diameter of 50 to 200 nm are dispersed in the sacrificial material before brazing, and the number density of the second-phase particles in the sacrificial material is 320,000 to 440,000 particles / mm 2 It is.

[0031] The obtained clad material can be combined with aluminum materials for heat exchangers, such as fins, headers, side plates, etc., which have been processed into tubes and corrugated, and brazed to manufacture a heat exchanger. Thus, the heat exchanger includes a laminate of a core material and a sacrificial material. For example, the above-mentioned clad material 1 can be formed into a pipe with the sacrificial material 1b on the inner surface side. The pipe is then flattened into a flat tube, which is then machined into a desired shape such as the header plate 11 shown in Fig. 2. The header plate 11 is assembled with a number of tubes 12, fins 13, and side supports 14, and is then brazed. Resin (not shown) is placed on the header plate 11 so as to cover the protruding portions of the tubes 11, and the gap between the resin tank and the header plate 11 is sealed by a rubber packing (O-ring) (not shown).

[0032] The assembled body 10 can be brazed by a conventional method. The brazing conditions are not particularly limited, but for example, the brazing can be performed under the following conditions: after heating from room temperature to 550°C, heating at a heating rate such that it takes 1 to 10 minutes to reach the target temperature from 550°C, holding the target temperature of 590 to 615°C for 1 to 20 minutes, thereafter cooling to 300°C at a rate of 50 to 100°C / min, and then air-cooling to room temperature.

[0033] The composition of the other member to be brazed is not particularly limited, and an aluminum material of an appropriate composition can be used, etc. The aluminum material includes pure aluminum as well as an aluminum alloy material. In the present invention, the heat treatment conditions and method for brazing (brazing temperature, atmosphere, presence or absence of flux, type of brazing material, etc.) are not particularly limited, and brazing can be performed by any desired method.

[0034] The clad material has a tensile strength of 145 MPa or more after brazing. The brazing conditions assumed for these characteristics are a heat treatment at 600°C for 3 minutes. Note that the brazing conditions of the present invention are not limited to specific conditions and can be set appropriately.

[0035] The resulting heat exchanger has good brazing properties and is excellent in strength and corrosion resistance.

[0036] In this embodiment, the sacrificial material is provided with an effect of preventing localized corrosion by adding an appropriate amount of Mn, Si, and Fe, and with an appropriate amount of Zn, it is provided with an effect of sacrificial corrosion protection, and the core material is provided with an appropriate amount of Si, Mn, Fe, and Cu to improve its strength, and the core material is subjected to an appropriate heat treatment and rolling to promote recrystallization during brazing, thereby obtaining good brazing properties, making it possible to achieve both post-braze strength and brazing properties, which are in a contradictory relationship. That is, according to this embodiment, a heat exchanger excellent in strength, corrosion resistance, and brazing properties can be obtained. EXAMPLES

[0037] The aluminum alloys for the sacrificial material, core material, and brazing material were cast by semi-continuous casting. The aluminum alloys for the sacrificial material and core material were shown in Table 1 (balance: Al and unavoidable impurities). The brazing material was an alloy with an Al-Si composition (Al-7.8%Si-0.2%Mn-2.0%Zn). The core material was subjected to the homogenization treatment shown in Table 2, and then hot-rolled and cold-rolled to a specified thickness. The core material was then laminated with a liner (side material) and subjected to the clad rolling described below. Next, hot rolling was performed, and further cold rolling was performed to a plate thickness of 0.5 mm. After that, annealing was performed for 3 hours at a temperature condition of 360°C to produce a plate material with temper O. In each pass of cold rolling after cladding, the reduction ratio was 10 to 35%. In the present invention, the cladding ratio of the sacrificial material was set to 14%, and the cladding ratio of the brazing material was set to 10%. Furthermore, the clad material was subjected to a heat treatment at 600°C for 3 minutes in anticipation of brazing treatment. Each test material was subjected to evaluation tests for the following properties, and the results are shown in Table 2.

[0038] [Table 1]

[0039] ○Particle distribution After tempering, the test material before brazing heat treatment was subjected to the measurement of the circle equivalent diameter and number density (pieces / mm 2 ) was measured by image analysis using composition images observed with a field emission scanning electron microscope (FE-SEM). The measurement method was as follows: before brazing heat treatment, the test material was mechanically polished and processed with a cross-section polisher (CP) to expose the cross-section (cross-section parallel to the rolling direction) of the plate to prepare a sample; the sample was then photographed at 10,000 to 50,000 magnifications using an FE-SEM. Photographs were taken of the core material and the sacrificial material from 10 different fields of view, and the circular equivalent diameter and number density of the dispersed particles were measured by image analysis.

[0040] Corrosion resistance (OY water immersion test) After brazing heat treatment, the test material was subjected to OY water (Cl-: 195 ppm, SO4 2- :60ppm, Cu 2+ :1ppm, Fe 3+ The immersion test was carried out using a test solution prepared by adjusting the pH of the test solution (pH 11 with 0.1% NaOH solution) to pH 11 using a 0.1% NaOH aqueous solution. The test conditions were room temperature x 16 hours + 88°C x 8 hours (without stirring) in a daily cycle, and the evaluation was carried out for up to 12 weeks. The pH adjustment was carried out with the test solution at 88°C. After the immersion test, the corrosion depth was measured. [Evaluation Criteria] × The corrosion depth reaches the core material. The corrosion rate is too fast and large pitting occurs. △The corrosion depth in the sacrificial material shows pitting. · No pitting due to corrosion within the sacrificial material

[0041] Mechanical properties (tensile strength after brazing) Tensile tests were conducted on JIS No. 5 or No. 13B test pieces that had been heat treated at 600°C for several minutes. [Evaluation Criteria] × Tensile strength less than 140MPa ·〇Tensile strength 140MPa~144MPa Tensile strength: over 144MPa

[0042] Brazing: Erosion evaluation (drop type fluidity test) To evaluate brazeability, the test material was subjected to 0% to 10% strain in a tensile tester, hung vertically, and heat-treated at 600°C for 3 minutes. The cross section of the material that melted and flowed down was observed to determine the erosion depth (corrosion) of the core material. The evaluation results are shown as O to × based on the brazeability evaluation in Table 2. [Evaluation Criteria] ×Erosion depth to core material exceeds 100μm ·△Erosion depth to core material: 80~100μm · Erosion depth to the core material is less than 80μm

[0043] Figure 3 shows optical microscope images of the material before the erosion evaluation (left) and after the erosion evaluation in which erosion has occurred. In the material where erosion has occurred, erosion has occurred deep within the core material.

[0044] [Table 2] [Explanation of symbols]

[0045] 1. Aluminum alloy clad material 1a Core material 1b Sacrificial material 1c Brazing material 10 Assembly 11 Header Plate 12 Tubes 13. Finn 14 Side Support

Claims

1. The present invention comprises a core material containing 1.0 to 1.5 mass% Mn, 0.5 to 0.9 mass% Si, 0.3 to 0.6 mass% Fe, with the remainder being Al and unavoidable impurities, a sacrificial material containing 2.5 to 4.0 mass% Zn, 0.7 to 1.3 mass% Mn, 0.3 to 0.7 mass% Si, 0.3 to 0.7 mass% Fe, with the remainder being Al and unavoidable impurities, and a brazing material made of an Al-Si alloy, In the core material before brazing, second phase particles having a circle equivalent diameter of 50 to 200 nm are dispersed, and the number density of the second phase particles in the core material is 1,000,000 particles / mm 2 and In the sacrificial material before brazing, second phase particles having a circle equivalent diameter of 50 to 200 nm are dispersed, and the number density of the second phase particles in the sacrificial material is 320,000 to 440,000 particles / mm 2 This is an aluminum alloy clad material for heat exchangers.

2. 2. The aluminum alloy clad material for heat exchangers according to claim 1, characterized in that the core material further contains Cu: 0.1 to 0.6 mass %.

3. 3. The aluminum alloy clad material for heat exchangers according to claim 1, which has a tensile strength of 140 MPa or more after a heat treatment at 600° C. for 3 minutes equivalent to brazing.

4. 4. The aluminum alloy clad material for heat exchangers according to claim 1, wherein the laminated material made of the core material and the sacrificial material is brazed to another member.

Citation Information

Patent Citations

  • Production of aluminum brazing sheet

    JP1991268893A

  • Aluminum alloy-clad material for heat exchanger having excellent erosion-corrosion resistance and general corrosion resistance

    JP2006152380A

  • Brazing sheet for automotive heat exchanger for brazed tube making

    JP2010095758A

  • Aluminum alloy clad sheet for heat exchanger

    JP2010168622A

  • Aluminum alloy brazing sheet and method for manufacturing the same

    JP2013023748A