Quantum dots, quantum dot layers, light-emitting devices, and solar cells
By ensuring 70% or more of the quantum dot surface is either polar or nonpolar and using a single type of ligand for protection, the method addresses production and luminous efficiency challenges, enhancing reliability and efficiency in quantum dot applications.
Patent Information
- Application Number
- JP2023505040
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-12
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2041-03-12
AI Technical Summary
Existing methods for protecting quantum dots with a mixture of polar and neutral ligands face challenges in production efficiency, luminous efficiency, and reliability due to increased steps and difficulty in controlling ligand amounts.
The quantum dots are designed with 70% or more of the surface area ratio as either a polar or nonpolar surface, using a single type of ligand (polar or neutral) for protection, which simplifies the manufacturing process and enhances surface protection.
This approach improves production efficiency and luminous efficiency while increasing the reliability of quantum dots, with potential luminance half-life times exceeding 10,000 hours, suitable for commercial display applications.
Smart Images

Figure 0007594654000007 
Figure 0007594654000008 
Figure 0007594654000009
Abstract
Description
[Technical field]
[0001] The present invention relates to a quantum dot, a quantum dot layer, a light-emitting device, and a solar cell. [Background technology]
[0002] Techniques are known in which the polar faces of quantum dots are protected with polar ligands and the non-polar faces are protected with neutral ligands.
[0003] For example, Patent Document 1 discloses a structure in which the polar faces of quantum dots are protected by binding with a ligand and the non-polar faces are protected by binding with another ligand. For example, Patent Document 2 discloses a structure in which the polar faces of quantum dots are protected by a halide and the non-polar faces are protected by an alkali metal.
[0004] Non-Patent Documents 1 and 2 each disclose a procedure for producing quantum dots. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Publication CN110305656A [Patent Document 2] WO2019 / 218060A1 publication [Non-patent literature]
[0006] [Non-Patent Document 1] Nat. Mater. 2014, 13, 822 [Non-Patent Document 2] Angew.Chem.Int.Ed.2009,48,6861-6864 Summary of the Invention [Problem to be solved by the invention]
[0007] Methods for realizing conventional technologies such as those described in Patent Documents 1 and 2 above include a method in which quantum dots are protected with a mixture of polar and neutral ligands, and a method in which quantum dots are protected with either a polar or neutral ligand and then ligand exchange is performed.
[0008] However, all of these methods have problems in that the production efficiency of surface-protected quantum dots is low due to an increase in the number of steps and difficulty in controlling the amount of ligand, etc. In addition, there are problems in that the luminescence efficiency and reliability of the quantum dots are low.
[0009] An object of one aspect of the present invention is to improve the production efficiency, luminous efficiency, and reliability of surface-protected quantum dots. [Means for solving the problem]
[0010] In order to solve the above problems, a quantum dot according to one embodiment of the present invention is configured such that 70% or more of its surface area is polar planes, or 70% or more of its surface area is nonpolar planes. Effect of the Invention
[0011] According to one aspect of the present invention, the efficiency of producing surface-protected quantum dots can be improved. [Brief description of the drawings]
[0012] [Figure 1] 1 is a cross-sectional view that diagrammatically illustrates a self-luminous element according to a first embodiment of the present invention. [Diagram 2] FIG. 1 is a perspective view showing a structure of an example of a quantum dot according to a first embodiment of the present invention. [Diagram 3] 3 is a diagram showing the plane orientation of each crystal plane of the quantum dot shown in FIG. 2. [Figure 4] 3 is a diagram showing the plane orientation of each crystal plane of the quantum dot shown in FIG. 2. [Diagram 5] FIG. 3 is a schematic diagram illustrating the surface of the quantum dot shown in FIG. 2 and a polar ligand protecting the surface. [Figure 6]FIG. 2 is a perspective view showing a structure of a modified example of the quantum dot according to the first embodiment of the present invention. [Figure 7] FIG. 2 is a perspective view showing a structure of a modified example of the quantum dot according to the first embodiment of the present invention. [Figure 8] FIG. 1 is a cross-sectional view illustrating a solar cell including a photoelectric conversion layer containing quantum dots according to a first embodiment of the present invention. [Figure 9] FIG. 5 is a perspective view showing the structure of an example of a quantum dot according to a second embodiment of the present invention. [Figure 10] FIG. 11 is a perspective view showing the structure of an example of a quantum dot according to a third embodiment of the present invention. [Figure 11] FIG. 11 is a diagram showing the plane orientation of each crystal plane of the quantum dot shown in FIG. [Figure 12] 11A to 11C are diagrams illustrating an example of a method for producing the quantum dots illustrated in FIG. [Figure 13] 11A to 11C are diagrams illustrating an example of a method for producing the quantum dots illustrated in FIG. [Figure 14] FIG. 11 is a perspective view showing a structure of a modified example of the quantum dot according to the third embodiment of the present invention. [Figure 15] FIG. 11 is a perspective view showing the structure of an example of a quantum dot according to a fourth embodiment of the present invention. [Figure 16] FIG. 16 is a schematic diagram illustrating the surface of the quantum dot shown in FIG. 15 and the polar ligands protecting the surface. [Figure 17] FIG. 11 is a perspective view showing the structure of an example of a quantum dot according to embodiment 5 of the present invention. [Figure 18] FIG. 11 is a perspective view showing the structure of an example of a quantum dot according to a sixth embodiment of the present invention. [Figure 19] FIG. 19 is a diagram showing the plane orientation of each crystal plane of the quantum dot shown in FIG. 18. [Figure 20] FIG. 13 is a perspective view showing a structure of a modified example of the quantum dot according to the sixth embodiment of the present invention. [Figure 21] FIG. 21 is a diagram showing the plane orientation of each crystal plane of the quantum dot shown in FIG. 20. [Figure 22] FIG. 13 is a perspective view showing a structure of a modified example of the quantum dot according to the sixth embodiment of the present invention. [Figure 23] 23 is a cross-sectional view showing the plane orientation of each crystal plane of the quantum dot shown in FIG. 22. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] [Embodiment 1] 1 is a cross-sectional view showing a schematic diagram of a self-luminous element 5 according to embodiment 1 of the present invention. The self-luminous element (light-emitting element) 5 is a top-emission type element having a forward structure, and includes an anode 51, a hole injection layer 52, a hole transport layer 53, a light-emitting layer 54 (quantum dot layer), an electron transport layer 55, and a cathode 56.
[0014] Each layer constituting the self-luminous element 5 can be produced by film formation and patterning such as colloidal solution coating, coating and baking, sputtering using a metal mask, photolithography, resin filling, ashing, and dry / wet etching.
[0015] (anode) The anode 51 is an electrode member containing a material having electrical conductivity. When the self-luminous element 5 is a top emission element with a forward structure, the anode 51 is preferably a reflective electrode from the viewpoint of improving extraction efficiency. When the anode 51 is a reflective electrode, for example, the anode 51 may be made of Al, Ag, or an alloy thereof. However, the anode 51 is not limited to these materials, and may be made of a transparent conductive material. In this case, it is preferable to include ITO (Indium Tin Oxide) in consideration of level matching with the hole injection layer 52 described later. The anode 51 may be fabricated by forming each material into a film by a sputtering method. The layer thickness of the anode 51 is, for example, 100 nm or less. Alternatively, the anode 51 may be formed by providing a reflective layer made of Al or Ag below a conductive layer made of ITO via an insulating layer such as polyimide. In this case, contact holes for connecting the conductive layer ITO to the TFT may be formed in the insulating layer and the reflective layer by photolithography.
[0016] (Hole injection layer) The hole injection layer 52 is a layer containing a hole injection material and having a function of increasing the efficiency of hole injection from the anode to the hole transport layer 53 described later. When an organic material is used for the hole injection layer 52, the organic material is preferably PEDOT having a HOMO level that matches the work function of the anode 51. The hole injection layer 52 may be produced, for example, by applying a coating material containing PEDOT and then curing the PEDOT at about 150°C.
[0017] From the viewpoint of improving the long-term reliability of the self-luminous element 5, the hole injection layer 52 is preferably an inorganic material. The inorganic material of the hole injection layer 52 may be an inorganic material, particularly a metal oxide, generally used for the hole injection layer 52, such as p-type NiO, LaO3, LaNiO, ZnO, MgZnO, n-type MoO3 having a deep CBM, WO3, etc. The film formation of the hole injection layer 52 can be performed by sputtering or vapor deposition. However, if the material of the hole injection layer 52 can be made into nanoparticles, the hole injection layer 52 can also be formed by coating using an appropriate colloidal solution.
[0018] The hole injection layer 52 is not essential and may be omitted depending on the desired element structure and characteristics.
[0019] (Hole transport layer) The hole transport layer 53 contains a hole transport material and has a function of increasing the efficiency of transporting holes to the light emitting layer 54. When an organic material is used for the hole transport layer 53, it is preferable to use an organic material whose HOMO level matches the light emitting layer material, including PVK, TFB, Poly-TPD, etc. O, L Metal residues such as aNiO whose VBM matches the light-emitting layer material, or semiconductor materials such as p-type ZnO may be used. For example, when PVK is used as the material for the hole transport layer 53, the layer may be formed by applying a solution in which PVK is dissolved in a solvent such as toluene. When an inorganic material is used as the material for the hole transport layer 53, the layer may be formed by sputtering or vapor deposition. When the hole transport layer 53 includes a material that can be made into nanoparticles, the hole transport layer 53 may be formed by application.
[0020] (Light Emitting Layer) The light-emitting layer 54 includes quantum dots 100. The structure of the quantum dots 100 will be described in detail below with reference to other drawings. The light-emitting layer 54 further includes polar ligands 2. The polar ligands 2 will also be described below with reference to other drawings. In this specification, the term "ligand" includes not only ligands that are currently bound to the surface of the quantum dot, but also ligands that can bind to the surface but are not bound to it.
[0021] (electron transport layer) The electron transport layer 55 is a layer containing an electron transport material and having a function of increasing the efficiency of transporting electrons to the light emitting layer 54. As a material for the electron transport layer 55, a ZnO-based inorganic material such as ZnO, IZO, ZAO, or ZnMgO, or TiO2 can be used. However, the electron transport layer 55 is not limited to this and may contain an organic material. The electron transport layer 55 is formed by, for example, sputtering or coating of a colloidal solution.
[0022] (Cathode) The cathode 56 is an electrode member containing a conductive material. Like the electron transport layer 55, the cathode 56 is formed by depositing or sputtering a metal having a relatively shallow work function, such as Al or Ag, which has been conventionally used.
[0023] Although the self-luminous element 5 according to this embodiment is a top-emission type element, the structure of the self-luminous element is not limited thereto and may be a bottom-emission type. When the self-luminous element 5 is a bottom-emission type element, the anode 51 may be a transmissive electrode and the cathode 56 may be a reflective electrode. The self-luminous element 5 may have a forward structure or an inverted structure. For example, when the self-luminous element 5 has an inverted structure, the self-luminous element 5 may have a structure in which the layers are stacked in the reverse order to the stacking order shown in FIG. 1.
[0024] If materials having better properties are found, the layers described above can be appropriately replaced to form the element.
[0025] (mirror face and direction indices) In this specification, Miller's plane index is used to specify the crystal plane. That is, for crystals other than hexagonal crystals, a crystal plane passing through three points specified by 1 / h*vector a1, 1 / k*vector a2, and 1 / l×vector a3 using unit lattice vectors a1, a2, and a3 and integers h, k, and l is called an (hkl) plane. For hexagonal crystals, a crystal plane passing through the above three points is called an (hkml) plane using unit lattice vector a4 defined by a4:=-a1-a2 and integer m defined by l:=-hk.
[0026] In this specification, for crystals other than hexagonal crystals, the (hkl) plane and planes equivalent to the (hkl) plane are collectively referred to as (hkl)-equivalent planes. Also, for crystals of the hexagonal crystal system, the (hkml) plane and planes equivalent to the (hkml) plane are collectively referred to as (hkml)-equivalent planes.
[0027] In this specification, Miller's directional index is used to specify the crystal direction. That is, for crystals other than hexagonal crystals, the direction along the composite vector specified by p*vector a1+q*vector a2+r×vector a3 using unit cell vectors a1, a2, a3 and integers p, q, and r is called the [pqr] direction. For hexagonal crystals, the direction along the composite vector is called the [pqsr] direction using unit cell vector a4 defined by a4:=-a1-a2 and integer s defined by s:=-pq.
[0028] (Quantum dot structure) Fig. 2 is a perspective view showing an example of the structure of the quantum dot 100 according to the embodiment 1. Fig. 3 and Fig. 4 are views showing the plane orientations of the crystal faces of the quantum dot 100 shown in Fig. 2. Fig. 5 is a schematic diagram showing the surface of the quantum dot 100 shown in Fig. 2 and the polar ligands protecting the surface.
[0029] The quantum dot 100 according to the first embodiment has a zinc-blende crystal system. The quantum dot 100 preferably includes at least one selected from a group including materials that can spontaneously adopt a zinc-blende crystal system. The material is, for example, a II-VI group compound such as ZnS, CdSe, or ZnSe, and a III-V group compound such as InP. In the present disclosure, a II-VI group compound means a compound including a group II element and a group VI element, and a III-V group compound means a compound including a group III element and a group V element. In addition, a group II element may include a group 2 element and a group 12 element, a group III element may include a group 3 element and a group 13 element, a group V element may include a group 5 element and a group 15 element, and a group VI element may include a group 6 element and a group 16 element. In addition, the groups of elements using Roman numerals are based on the old CAS system, and the groups of elements using Arabic numerals are based on the current IUPAC nomenclature.
[0030] The quantum dot 100 may have any of a core structure, a core-shell structure, or a core-multishell structure. In this specification, the "surface of the quantum dot 100" means the surface of the outermost layer of the quantum dot 100. In this specification, the "crystal plane of the quantum dot 100" means the crystal plane of the outermost layer of the quantum dot 100. In this specification, the "crystal system of the quantum dot 100" means the crystal system of the outermost layer of the quantum dot 100.
[0031] When the quantum dot 100 has a core-shell structure, the crystal system of the core and the crystal system of the shell may be the same or different from each other. Similarly, when the quantum dot 100 has a core-multishell structure, the crystal system of the core and the crystal system of the innermost layer of the multishell may be the same or different from each other, and the crystal systems of adjacent layers of the multishell may be the same or different from each other. When multiple layers are stacked, if a layer is thin (typically, if it is three atomic layers or less), it is known that the crystal system of the layer usually follows the crystal system of the layer below the layer. On the other hand, if a layer is thick, it is known that the crystal system of the layer usually follows one of the crystal systems that the material forming the layer can spontaneously adopt in bulk.
[0032] When the quantum dot 100 has a core-shell structure, the band gap of the core is preferably smaller than the band gap of the shell so that holes and electrons are captured and recombined in the core. Specifically, it is preferable that the electron affinity of the core is larger than the electron affinity of the shell and the ionization energy of the core is smaller than the ionization energy of the shell.
[0033] The quantum dot 100 is a polyhedral crystal having a plurality of crystal faces, and the surfaces thereof are mainly polar faces. The surface of the quantum dot 100 includes, for example, 14 faces, including (a) the (100), (-100), (010), (0-10), (001), and (00-1) faces of a rectangle shown in FIG. 4, and (b) the (111), (-111), (1-11), (-1-11), (11-1), (-11-1), (1-1-1), and (-1-1-1) faces of a hexagon shown in FIG. 3. In this case, the ideal shape of the quantum dot 100 is a tetradecahedron obtained by cutting each vertex of a regular octahedron with a square.
[0034] FIG. 3 is a diagram showing a plane equivalent to the (111) plane in the crystal plane of the quantum dot 100. In FIG. 3, the (111) plane and the plane equivalent to the (111) plane are hatched. Among the crystal planes of the quantum dot 100, the planes equivalent to the (111) plane are the (-111) plane, the (1-11) plane, the (-1-11) plane, the (11-1) plane, the (-11-1) plane, the (1-1-1) plane, and the (-1-1-1) plane. FIG. 4 is a diagram showing a plane equivalent to the (100) plane in the crystal plane of the quantum dot 100. In FIG. 4, the (100) plane and the plane equivalent to the (100) plane are hatched. Among the crystal faces of the quantum dot 100, the faces equivalent to the (100) face are the (-100) face, the (010) face, the (0-10) face, the (001) face, and the (00-1) face.
[0035] The (111)- and (100)-equivalent planes in the zinc blende crystal system are polar planes. A polar plane is a crystal plane in which the valences of the cations and anions exposed on the surface are biased. Specifically, a polar plane is a surface that is positively charged due to the presence of more cations than anions on the surface, and can bind strongly to negatively charged polar ligands. In contrast, a nonpolar plane is a crystal plane in which the valences of the exposed cations and anions are balanced. Specifically, a nonpolar plane is a surface that is electrically neutral and uncharged, and can bind strongly to nonpolar ligands.
[0036] Whether a surface is polar or non-polar can be determined by the method described in "(Quantum dot crystal face analysis method)" below. When the surface of the quantum dot 100 is a polar surface, the surface of the quantum dot 100 can be protected (surface protection) using a polar ligand 2 as shown in Fig. 5. The polar ligand 2 can be coordinate-bonded to the polar surface via an unshared electron pair.
[0037] Regarding the relationship between the ratio of polar faces of quantum dots and the durability of light-emitting devices, quantum dot light-emitting devices were fabricated using quantum dots with 50% of the surface area being polar faces and with only polar ligands coordinated thereto, and the durability was measured. As a result, the operating luminance was 1000 cd / m 2 The half-life of brightness was approximately 6,400 hours. Now, if 50% of the surfaces are polar, the remaining 50% are non-polar. The bonds between polar ligands on these non-polar surfaces are weak, and polar ligands are easily detached from these non-polar surfaces. Ligand detachment generates defect levels on the quantum dot surface, and non-radiative recombination of excitons is induced via these defect levels. Therefore, in this case, assuming that the non-radiative recombination probability is determined by the proportion of defect levels present on the surface, the non-radiative recombination probability can be set to 0.5p a (Because the non-polar planes make up 50%), where p ap is the probability that a defect level is formed due to the polar ligand being removed from the nonpolar surface, and that non-radiative recombination of excitons occurs via this defect level, when a quantum dot with only polar ligands is used with a nonpolar surface that is 100% of the surface area. a (0 <p a <1).
[0038] Non-radiative recombination provides thermal energy to the quantum dot, which deactivates the quantum dot with a certain probability. The probability that a QD is deactivated by non-radiative recombination is p b (0 <p b <1), the probability of a QD being deactivated per average time taken for one exciton recombination is 0.5p a p b It is believed to be the case.
[0039] If we generalize the ratio of nonpolar faces, which was set to 0.5 above, to c, the number of undeactivated quantum dots at time t to N(t), and the average number of exciton recombinations per unit time to f, then the amount of deactivated quantum dots per unit time, dN / dt, is given by dN / dt=-p a p b cfN(t) Since the number of undeactivated quantum dots N(t) is proportional to the luminance L(t) of the quantum dot light-emitting device, if N=kL (k is any positive real number), then dL / dt=-p a p b cfkL(t) (1) The solution of equation (1) can be expressed as follows, assuming the initial condition L(0) = L0: L(t) = L0 exp(-p a p b cfkt) (2) It becomes.
[0040] From equation (2), the brightness half-life time t 1 / 2 teeth, t 1 / 2 =In(2) / p a p b cfk (3) In equation (3), the experimental values c = 0.5, t1 / 2 Substituting =6400 hours, p a p b fk≒2.17×10^-4, and equation (3) becomes t 1 / 2 =3200 / λ (4) Here, if the ratio of polar surfaces is 70%, 80%, and 90%, respectively, the ratio of non-polar surfaces c is 0.3, 0.2, and 0.1, respectively. Substituting these into (4), the luminance half-life time t 1 / 2 are 10,667 hours, 16,000 hours, and 32,000 hours, respectively. Assuming that the light-emitting element containing the quantum dots of this application is used in a television display and the average daily television viewing time is 3 hours, these values become 9.74 years, 14.6 years, and 29.2 years.
[0041] From the above, the durability of the self-luminous element was assumed for a configuration in which the quantum dot light-emitting layer 54 contains only the polar ligand 2 as the ligand for surface protection of the quantum dots 100. For the self-luminous element 5 using the quantum dots 100 in which the proportion of the polar faces on the surface of the quantum dots 100 (hereinafter referred to as the "area ratio of the polar faces") is 70%, 2 The half brightness time is expected to be more than 10,000 hours at 1000cd / m 2 A half-life of luminance of 10,000 hours or more in this case corresponds to a display life of about 10 years. A 10-year life is generally a sufficient durability life for commercialization. In addition, for the blue-emitting self-luminous element 5 using quantum dots 100 with a polar surface area ratio of 80% or more, a result equivalent to a display life of about 15 years is expected. In addition, for the blue-emitting self-luminous element 5 using quantum dots 100 with a polar surface area ratio of 90% or more, a result equivalent to a display life of about 30 years is expected.
[0042] Therefore, when 70% or more of the surface of the quantum dot 100 is a polar surface, the surface of the quantum dot 100 can be sufficiently protected (surface protection) by using only the polar ligand 2.
[0043] The higher the area ratio of the polar faces on the surface of the quantum dot 100, the more effective the surface protection by the polar ligand 2. Therefore, the surface of the quantum dot 100 according to the first embodiment may be polar faces at an area ratio of 70% or more, preferably 80% or more, and more preferably 90% or more. Ideally, the surface of the quantum dot 100 includes only polar faces.
[0044] Here, the effect of protecting the surface of the quantum dot by the polar or neutral ligand is evaluated by evaluating the binding energy of the polar ligand on the polar and non-polar surfaces of the surface of the quantum dot. Specifically, the binding energy per mole of the polar ligand 2 to the surface of the quantum dot 100 was calculated for a case in which the surface of the quantum dot 100 is made of CdSe and the polar ligand 2 is a carboxylic acid ligand. The calculation was performed based on the density functional theory (DFT). In the calculation results, the binding energy to the (100) equivalent surface and the (111) equivalent surface, which are polar surfaces, is about 240 kcal / mol, while the binding energy to the (110) equivalent surface, which is a non-polar surface, is about 16 kcal / mol.
[0045] In this way, since the binding energy differs by one order of magnitude or more, when a conventional quantum dot in which the proportion of polar faces is not controlled is surface-protected only with polar ligand 2, the deterioration of the conventional quantum dot progresses from the non-polar face. Also, when a conventional quantum dot is surface-protected only with neutral ligand 3 described below, the deterioration of the conventional quantum dot progresses from the polar face. For this reason, in the conventional techniques such as Patent Documents 1 and 2, in order to surface-protect a conventional quantum dot using both a polar ligand and a neutral ligand, a step of mixing the polar ligand and the neutral ligand or a step of ligand exchange is required.
[0046] In contrast, in the quantum dot 100 according to the first embodiment, the area ratio of the polar surface is 70% or more. Therefore, the area ratio of the non-polar surface in the quantum dot 100 is small. In addition, the polar ligand 2 bound to the polar surface of the quantum dot 100 inhibits the approach of other quantum dots 100 to the non-polar surface of the quantum dot 100. As a result, even if the quantum dot 100 is surface-protected only with the polar ligand 2, the non-polar surface of the quantum dot 100 is unlikely to deteriorate. Therefore, the manufacturing method of the light-emitting layer 54 according to the first embodiment does not require a step of mixing the polar ligand and the neutral ligand or a step of exchanging the ligand. Therefore, the light-emitting layer 54 according to the first embodiment has high manufacturing efficiency. In addition, the ligand used for surface protection of the quantum dot 100 can be a single type.
[0047] The polar ligand 2 may be organic, and includes at least one selected from the group consisting of organic polar ligands containing at least one of a thiol group, an alkoxyl group, a carboxyl group, a phosphonic acid group, and a phosphinic acid group at the end. The ligand containing one or more thiol groups at the end partially contains a structure represented by the following structural formula (1) or the following structural formula (2) in an ionized state. The ligand containing an alkoxyl group at the end partially contains a structure represented by the following structural formula (3) in an ionized state. The ligand containing a carboxyl group at the end partially contains a structure represented by the following structural formula (4) in an ionized state. The ligand containing a phosphonic acid group at the end partially contains a structure represented by the following structural formula (5) or the following structural formula (6) in an ionized state. The ligand containing a phosphinic acid group at the end partially contains a structure represented by the following structural formula (7) in an ionized state.
[0048] [ka] In the above structural formulas (1) to (7), C represents a carbon atom, O represents an oxygen atom, and O - indicates an oxide ion, S indicates a sulfur atom, and S -represents a sulfide ion, P represents a phosphorus atom, and R1 and R2 each independently represent a hydrogen atom, an alkyl group, an aryl group, an alkoxyl group, or an unsaturated hydrocarbon group.
[0049] The polar ligand 2 is preferably organic. Unlike inorganic ligands, organic ligands can have a long chain-like molecular structure. For this reason, organic ligands can easily maintain a large distance between the quantum dots 100, thereby improving the dispersibility and storage stability of the quantum dots 100 in the solution.
[0050] The polar ligand 2 may be inorganic, for example, in its ionized state, has the ionic formula Cl - , Br - , I - , SCN - , C.N. - , O.H. - , S.H. - , SeH - , TeH - , Se 2- , S 2- , Te 2- , Sn2S6 4- , Sn2Se6 4- , In2Se4 2- , In2Te4 2- , Ga2Se4 2- , Sb2Se4 2- , Sb2Te4 2- The inorganic polar ligand includes at least one selected from the group consisting of inorganic polar ligands represented by the formula:
[0051] It is also preferable that the polar ligand 2 is inorganic. Organic bonds (such as CH and CC) are easily broken by heat and light. When the polar ligand 2 is inorganic, it is difficult to decompose because it does not contain an organic bond, which can improve the reliability of the light-emitting layer 54 and the light-emitting element 5. The polar ligand 2 is preferably Se 2- , S 2- , Te 2- It is more preferable that the compound is any one of the following: 2- , S 2- , Te 2-Since it does not contain a chemical bond, it will not be decomposed, and since it has a negative valence of two, it can bond strongly to the polar surface of the quantum dot 100 .
[0052] When forming a film by coating using a colloidal solution in which quantum dots 100 are dispersed, in order to obtain a uniform thickness everywhere and reduce surface irregularities, it is necessary that (1) the quantum dots 100 do not aggregate in the solution, and (2) the flow of the solvent is not hindered. To satisfy (1), the ligands coordinated to the surface of the quantum dots 100 should be dense relative to the volume of the quantum dots 100 in the coated colloidal solution. To satisfy (2), the inertia of the quantum dots 100 in the colloidal solution should be small relative to the viscosity of the solvent of the coated colloidal solution. Here, the smaller the size of the quantum dots 100 in the colloidal solution, the more likely it is that both (1) and (2) above are satisfied. Therefore, in consideration of the size that does not affect the fluidity of the colloidal solution, it is preferable that the size of the quantum dots 100 is 10 nm or less. In other words, if the size is 10 nm or less, a uniform film can be formed when forming a film by coating or the like for the light-emitting layer 54 (see FIG. 1).
[0053] Here, the size of the quantum dots 100 may be a nominal value, a design value, or a measured value. In the case of a measured value, the size of the quantum dots 100 is, for example, an average value obtained by measuring the particle size of the quantum dots 100 multiple times using a transmission electron microscope (TEM) or the like.
[0054] (Quantum dot manufacturing method) The quantum dots 100 can be produced by, for example, a heating method, a hot injection method, a microwave assisted method, and a continuous flow method. Each of these methods will be described below.
[0055] (heating method) The heating method is a technique in which materials are mixed in an organic solvent and heated to pyrolyze and react the materials to synthesize each layer of the quantum dot 100. In the heating method, TOP (trioctylphosphine) or TOPO (trioctylphosphine oxide) is used as the organic solvent, dimethylcadmium is used as the group II raw material, and a desired element, for example, a TOP complex of S, Se, Te, or the like, or an organometallic compound bonded with a methyl group or ethyl group, is used as the group VI raw material. Group II and VI raw materials are mixed in an organic solvent and heated to about 300°C to pyrolyze the raw materials, and the reaction to the II-VI group compounds is promoted by maintaining a high degree of supersaturation of the group II and VI elements in the organic solvent, thereby synthesizing each layer of the quantum dot 100.
[0056] (Hot Injection) Hot injection is a method to generate uniform crystal growth nuclei at high density by rapidly injecting raw materials into a heated organic solvent and utilizing the supersaturation near the injection area. In hot injection, the raw materials used are TOP or T-TOPO as the organic solvent, which is heated to about 300°C. By rapidly injecting II and VI group raw materials into the organic solvent, the degree of supersaturation is rapidly increased locally around the injection area, and uniform crystal growth nuclei are generated at high density. Since the high degree of supersaturation is localized near the injection area, the raw materials consumed in the growth of the growth nuclei are supplied from the surrounding low supersaturation area by diffusion due to the concentration gradient, and the growth of quantum dots continues. Since this method generates nuclei at high density, surfactants or ligands to prevent the aggregation of quantum dots are added, such as alkyl phosphine and alkyl phosphine oxides such as trioctyl phosphine or trioctyl phosphine oxide, long-chain carboxylic acids such as oleic acid, and long-chain amines such as oleylamine.
[0057] (Microwave assisted method) The microwave-assisted method is a method of selectively heating the growth raw material using microwaves. This method has good reaction controllability because the heating is selective, and it is possible to raise the temperature to the temperature range required for the reaction in a short time. In addition, it is easier than the injection method and quantum dots can be synthesized even in air. Since microwaves are selectively resonantly absorbed by molecules with polarization, for example, if a chalcogenide that matches the microwave wavelength is used as a raw material, it is possible to heat the selective raw material and control the growth of quantum dots. Due to this characteristic, the raw material needs to have polarization, and a different raw material is used from the first and second methods. An example of a raw material is a mixed solution of cadmium stearate, an alkane solvent, and group VI powder.
[0058] (Continuous flow method) The continuous flow method is a method in which the nucleation reaction and the growth reaction are caused in different reactors by reacting the raw materials while flowing an organic solvent mixed with the raw materials. Since the nucleation reaction and the growth reaction are caused in different reactors, the appropriate temperature gradient can be precisely set, and each reaction can be precisely controlled. This method is suitable for mass production because it is relatively easy to control the crystal growth. As explained in the continuous flow method and the three manufacturing methods, the quantum dots 100 can be grown either in an organic solution or in a gas phase containing the vapor of an organic solution. In the continuous flow method, an organic solvent and a group II and group VI raw material are mixed, the raw material is moved along the flow of the liquid phase or the gas phase, and a temperature gradient suitable for the nucleation stage, which is the starting point of the growth of the quantum dots 100, and the crystal growth stage is set, so that the nucleation and growth reactions can be precisely controlled in separate reactors. The nucleation and the crystal growth are separated into separate containers, and the conditions suitable for each stage can be precisely and independently controlled by transporting the raw materials between each container on the flow of the liquid phase or the gas phase.
[0059] In crystal growth, it is important to maintain a high degree of supersaturation in the raw material, which is the driving force for nucleation and crystal growth. The four types of manufacturing methods mentioned above, for example, have been developed based on the differences in the means for achieving and maintaining this condition.
[0060] In order to synthesize the quantum dot 100, it is necessary to control the synthesis conditions when synthesizing each layer of the quantum dot 100. Specifically, it is necessary to control the synthesis conditions of each layer of the quantum dot 100 so that the surface of the quantum dot 100 has a shape that terminates only in the (111) equivalent plane and the (100) equivalent plane as shown in FIG. 2. As a method for selectively appearing a specific crystal plane in this way, the pH of the solvent in which the materials are mixed in the process of synthesizing each layer can be controlled to a specific range. It has been experimentally found that the pH of the solvent should be maintained in the range of 9 to 11 in order to obtain the crystal plane shown in FIG. 2. Since this range of pH is weakly basic with a higher H+ concentration than the neutral condition of PH=7, it is considered that the intermediate reaction between H+ and the raw material species is involved in the mechanism of preferentially forming a specific crystal plane.
[0061] As another method, when using II-VI group crystals such as ZnS or CdS or III-V group crystals such as InP, it is known that the (111) equivalent plane appears by relatively decreasing the amount of group VI or group V raw material. This is because the dangling orbitals of the (111) equivalent plane, which has a high surface density of bonding orbitals, relatively increase as the amount of group V or group VI raw material decreases.
[0062] If the conditions for forming the outermost layer of the quantum dot 100 (and the layer immediately below the outermost layer, if the outermost layer is thin) are any of those described above, then a quantum dot 100 including 14 (111)-equivalent planes and (100)-equivalent planes can be obtained. Here, the temperature may be lowered once to stop the reaction, and then heat may be applied to perform heat treatment. In general, by stopping the reaction and performing heat treatment, surface defects in the outermost layer of the quantum dot 100 can be reduced.
[0063] To coordinate the polar ligand 2 to the quantum dot 100 thus produced, the ligand can be replaced by adding a sufficient amount of polar ligand 2 after the production of the quantum dot 100 and heating at 150° C. for 20 minutes. Also, by adding polar ligand 2 at the end of the crystal growth of the quantum dot 100 or during shell formation, quantum dots 100 having polar faces coordinated with polar ligand 2 can be obtained.
[0064] The particle size of the quantum dot 100, not including the polar ligand 2, may be 3 nm or more and 40 nm or less.
[0065] (Method of analyzing the crystal plane of quantum dots) Next, a method for analyzing the crystal planes of the quantum dots 100 will be described. Simply put, the crystal planes of the quantum dots 100 can be analyzed by observing the quantum dots 100 with a conventional X-ray Diffraction (XRD) measuring device, an Energy Dispersive X-ray Spectroscopy (EDS) measuring device, an X-ray Photoelectron Spectroscopy (XPS) measuring device, a Transmission Electron Microscopy (TEM) or the like.
[0066] The crystal system of the quantum dot 100 can be measured by X-ray diffraction. If the thickness is about 20 nm, the diffraction peaks from each crystal plane of the quantum dot 100 can be detected with sufficient accuracy by a general powder X-ray diffraction method. Therefore, the crystal system of the quantum dot 100 can be measured by comparing the obtained spectrum shape with a database or past literature values.
[0067] Furthermore, the composition of the quantum dot 100 can be determined by EDS or XPS, because peaks specific to the elements contained in the composition and their bonding state appear in the spectroscopic results according to the composition of the quantum dot 100.
[0068] Based on the composition and crystal system of the quantum dot 100, the crystal plane spacing and crystal plane index of the quantum dot 100 can be calculated. These values can then be used in combination with TEM observation to measure the plane index and ratio of the nanoparticle surface. Finally, based on the composition, crystal system, and crystal plane index, the area ratio of the polar planes on the surface of the quantum dot 100 can be calculated.
[0069] Typically, the light-emitting layer 54 has a uniform configuration regardless of location with respect to the shape and face index of the quantum dots 100, the type and ratio of ligands, etc. Therefore, the results of an analysis performed on a portion of the light-emitting layer 54 may be applied to the entire light-emitting layer 54.
[0070] Furthermore, when the outermost layer of the quantum dot 100 is so thin that it is difficult to analyze (typically, three atomic layers or less), the object analyzed by the above analysis method includes the layer below the outermost layer. As described above, if the outermost layer is thin, the crystal system of the outermost layer follows the crystal system of the layer below it. Therefore, regardless of the thickness of the outermost layer of the quantum dot 100, the crystal system and crystal index derived based on the above analysis method may be regarded as the crystal system and crystal index of the outermost layer of the quantum dot 100.
[0071] Usually, even if a quantum dot 100 having a polar surface area ratio of 100% is analyzed, the calculated polar surface area ratio tends to be 90% or more and less than 100% due to analytical accuracy, measurement limits, impurities, etc. Therefore, if the calculated polar surface area ratio is 90% or more, it is considered that there is a high probability that the light-emitting layer 54 has quantum dots whose 100% of the surface is polar. Therefore, if the analysis result shows that the polar surface area ratio is 90% or more, it is considered that the light-emitting layer 54 contains quantum dots whose 100% of the surface is polar.
[0072] As described above, the polar surface may occupy 70% or more of the surface of the quantum dot 100. When using quantum dots 100 with a polar surface area ratio of 70%, the calculated polar surface area ratio tends to be 60% or more and 80% or less. Therefore, when the calculated polar surface area ratio is 60%, it is highly likely that the quantum dots 100 with a polar surface area ratio of 70% or more are included in the entire light-emitting layer 54. As described above, when 70% or more of the surface of the quantum dots 100 is polar surface, the surface of the quantum dots 100 can be sufficiently protected (surface protection) by using only the polar ligand 2. Therefore, when the polar surface area ratio in the analysis result is 60% or more, it is considered that at least a part of the quantum dots 100 included in the light-emitting layer 54 is sufficiently surface-protected by only the polar ligand 2.
[0073] The area ratio of the nonpolar planes can be determined by the same method as described above. If the calculated area ratio of the nonpolar planes is 90% or more, it is considered that the light-emitting layer 54 contains quantum dots 100 whose surfaces are 100% nonpolar.
[0074] (Ligand Analysis Method) The functional groups of the ligands, including the polar ligand 2 and the neutral ligand 3 described below, can be determined using a mass analyzer. If the ligand is organic, it is ionized and cut into multiple fragments, and the m / z value (mass / charge) of each fragment and its intensity ratio in the mass spectrum are obtained. Then, based on the m / z value and the intensity ratio, the structural formula and functional groups of the ligand can be determined by referring to a database.
[0075] Most organic compounds are registered in the database, so it is possible to identify them by referring to the database. Even if the ligand is not registered, it can be searched for by analogy with registered organic compounds.
[0076] In addition, even if the ligand is inorganic, the composition formula of the ligand can be determined using a mass spectrometer or an EDS measurement device. As described above, the analysis results performed on a portion of the light-emitting layer 54 may be applied to the entire light-emitting layer 54.
[0077] The light-emitting layer 54 is analyzed as described above to identify compounds that can function as ligands contained in the light-emitting layer 54. Even if only polar ligand 2 (or only neutral ligand 3) is used as the ligand in the light-emitting layer 54 during manufacture, polar ligand 2 (or neutral ligand 3) tends to account for less than 100% of the identified compounds due to analytical accuracy, measurement limits, etc. For this reason, if the proportion of polar ligand 2 (or neutral ligand 3) in the identified compounds is 90% or more in terms of substance amount ratio, it is considered highly likely that 100% of the ligands contained in the light-emitting layer 54 are polar ligand 2 (or neutral ligand 3).
[0078] (Modification) Fig. 6 and Fig. 7 are perspective views showing the structure of modified examples of the quantum dots 100 according to the embodiment 1. Fig. 8 is a cross-sectional view showing a solar cell 6 including a photoelectric conversion layer 57 including the quantum dots 100 according to the embodiment 1.
[0079] The quantum dot 100 according to the first embodiment is not limited to the above. For example, the surface of the quantum dot 100 may include six (100) equivalent faces as shown in Fig. 6, in which case the ideal shape of the quantum dot 100 is a rectangular parallelepiped. Alternatively, for example, the surface of the quantum dot 100 may include eight (111) equivalent faces as shown in Fig. 7, in which case the ideal shape of the quantum dot 100 is a regular octahedron.
[0080] A hexahedral quantum dot 100 as shown in Fig. 6 can be produced by increasing the reaction temperature. For example, if the quantum dot 100 is made of CdSe, the crystal is grown at 275 degrees Celsius or higher. The high temperature increases the rate of ligand desorption and re-adsorption on the crystal surface, which results in the deposition of atoms on crystal faces with high surface energy. In other words, atoms are preferentially deposited on (111) equivalent faces, which have a high density of dangling bonds. As a result, the surface of the quantum dot 100 is composed of (100) equivalent faces.
[0081] However, as described above, when forming a film by coating using a colloidal solution in which the quantum dots 100 are dispersed, in order to obtain a uniform thickness everywhere and reduce surface irregularities, it is necessary that (1) the quantum dots 100 do not aggregate in the solution, and (2) the flow of the solvent is not hindered. In order to satisfy (2), it is preferable that the quantum dots 100 have a shape that allows them to roll easily, that is, a shape close to a sphere. Furthermore, in order to reduce the driving voltage of the self-luminous element 5, it is necessary that the gaps between the quantum dots 100 in the light-emitting layer 54 are small. For this reason, it is preferable that the quantum dots 100 have a shape that allows them to easily fill small gaps, that is, a shape close to a sphere. Therefore, the shape of the quantum dots 100 is preferably an octahedron rather than a hexahedron, and a tetradecahedron rather than an octahedron.
[0082] 8, the first embodiment is applicable to a solar cell 6. The solar cell 6 includes an anode 51, a hole injection layer 52, a hole transport layer 53, a photoelectric conversion layer 57 (quantum dot layer), an electron transport layer 55, and a cathode 56. The photoelectric conversion layer 57 includes the quantum dots 100 according to the first embodiment and polar ligands 2.
[0083] [Embodiment 2] Other embodiments of the present invention will be described below. For ease of explanation, the same reference numerals are given to members having the same functions as those described in the above embodiment, and the description thereof will not be repeated.
[0084] The light-emitting element 5 of this embodiment 2 (see FIG. 1) differs from the light-emitting element 5 of the aforementioned embodiment 1 only in that the light-emitting layer 54 includes the quantum dots 200 of this embodiment 2 instead of the quantum dots 100 of the aforementioned embodiment 1.
[0085] (Quantum dot structure) FIG. 9 is a perspective view showing an example of the structure of a quantum dot 200 according to the second embodiment.
[0086] The quantum dot 200 according to the second embodiment has a sodium chloride type crystal system. The quantum dot 200 preferably includes at least one selected from a group including materials that can spontaneously adopt a sodium chloride type crystal system. The material is, for example, a IV-VI group compound such as PbTe, PbSe, or PbS. In the present disclosure, the IV-VI group compound means a compound including a group IV element and a group VI element. The group IV element may include a group 4 element and a group 14 element.
[0087] When the quantum dot 200 according to the second embodiment has a core-shell structure, the band gap of the core is preferably smaller than the band gap of the shell, similarly to the first embodiment described above.
[0088] The quantum dot 200 is a polyhedral crystal having multiple crystal faces, and the surfaces are mainly polar faces. The surfaces of the quantum dot 200 include, for example, eight triangular faces shown in FIG. 9, namely, (111) face, (-111) face, (1-11) face, (-1-11) face, (11-1) face, (-11-1) face, (1-1-1) face, and (-1-1-1) face. These eight faces are (111) equivalent faces. In this case, the ideal shape of the quantum dot 200 is a regular octahedron.
[0089] The (111) equivalent plane in sodium chloride crystal is a polar plane. As in the above-described first embodiment, the surface of the quantum dot 200 according to the second embodiment may be polar planes at an area ratio of 70% or more, preferably 80% or more, and more preferably 90% or more. Ideally, the surface of the quantum dot 200 includes only polar planes.
[0090] As in the above-described first embodiment, if the area ratio of polar faces calculated as a result of the crystal face analysis of the quantum dots 200 is 90% or more, it is considered that the light-emitting layer 54 contains quantum dots 200 whose surfaces are 100% polar faces.
[0091] (Quantum dot manufacturing method) The quantum dots 200 according to the second embodiment can be produced by the same method as in the first embodiment, such as a heating method, a hot injection method, a microwave assisted method, or a continuous flow method.
[0092] Octahedral quantum dots 100 as shown in Fig. 7 can be produced by using a polar ligand (e.g., a ligand containing a thiol group) that preferentially bonds to the polar face during synthesis and by lowering the reaction temperature, in addition to the production method described in Non-Patent Document 1. For example, when the quantum dots 100 are made of PbS, the crystals are grown at about 110 degrees Celsius.
[0093] Similar to the above-described first embodiment, the second embodiment can also be applied to solar cells.
[0094] [Embodiment 3] Other embodiments of the present invention will be described below. For ease of explanation, the same reference numerals are given to members having the same functions as those described in the above embodiment, and the description thereof will not be repeated.
[0095] The light-emitting element 5 of this embodiment 3 (see FIG. 1) differs from the light-emitting element 5 of the aforementioned embodiment 1 only in that the light-emitting layer 54 includes quantum dots 300 of this embodiment 3 instead of the quantum dots 100 of the aforementioned embodiment 1.
[0096] (Quantum dot structure) Fig. 10 is a perspective view showing an example of the structure of a quantum dot 300 according to the present embodiment 3. Fig. 11 is a diagram showing the plane orientations of the crystal planes of the quantum dot 300 shown in Fig. 10.
[0097] The quantum dot 300 according to the third embodiment has a wurtzite crystal system. The quantum dot 300 preferably includes at least one material selected from a group including materials that can spontaneously adopt a wurtzite crystal system. The material is, for example, a II-VI compound such as ZnS, CdSe, or ZnSe. Note that the II-VI compound can also adopt a zinc blende crystal system depending on the crystal growth conditions.
[0098] When the quantum dot 300 according to the third embodiment has a core-shell structure, the band gap of the core is preferably smaller than the band gap of the shell, similarly to the first embodiment described above.
[0099] The quantum dot 300 is a polyhedral crystal having multiple crystal faces, and its surfaces are mainly polar faces. The quantum dot 300 has a thin flat plate shape in the
[0001] direction including the two faces of the hexagon shown in FIG. 11, the (0001) face and the (000-1) face, as the top face and the bottom face.
[0100] Fig. 11 is a diagram showing a plane equivalent to the (0001) plane in the crystal plane of the quantum dot 300. In Fig. 11, the (0001) plane and a plane equivalent to the (0001) plane are hatched. Of the crystal planes of the quantum dot 300, the plane equivalent to the (0001) plane is the (000-1) plane opposite to the (0001) plane.
[0101] The (0001) equivalent plane and the (1-101) equivalent plane in the wurtzite crystal are polar planes. In the quantum dot 300, the (1-101) equivalent planes are the (1-101) plane, the (01-11) plane, the (-1011) plane, the (-1101) plane, the (0-111) plane, the (10-11) plane, the (1-10-1) plane, the (01-1-1) plane, the (-101-1) plane, the (-110-1) plane, the (0-11-1) plane, and the (10-1-1) plane. As in the above-mentioned embodiment 1, the surface of the quantum dot 300 according to this embodiment 3 may be polar planes at an area ratio of 70% or more, preferably 80% or more, and more preferably 90% or more. In addition, it is ideal that the quantum dot 300 has a flat plate shape.
[0102] As in the above-described first embodiment, if the area ratio of polar faces calculated as a result of the crystal face analysis of the quantum dots 300 is 90% or more, it is considered that the light-emitting layer 54 contains quantum dots 300 whose surfaces are 100% polar faces.
[0103] The surface between the top and bottom surfaces of the quantum dot 300 may include a non-polar surface, for example, a (1-100) equivalent surface. In the quantum dot 300, the (1-100) equivalent surface is a (1-100) surface, a (01-10) surface, a (-1010) surface, a (-1100) surface, a (0-110) surface, and a (10-10) surface. The surface between the top and bottom surfaces of the quantum dot 300 preferably includes a polar surface, for example, a (1-101) equivalent surface that is inclined with respect to the (0001) equivalent surface. The surface between the top and bottom surfaces of the quantum dot 300 may include both or only one of a non-polar surface and a polar surface.
[0104] As shown in FIG. 10, the quantum dot 300 has a thin flat shape in the
[0001] direction because the ratio of the area of the (0001) equivalent plane on the surface of the quantum dot 300 is large. Therefore, the direction of exciton recombination in the quantum dot 300 is mainly a direction substantially perpendicular to the
[0001] direction. As a result, the light emitted by the recombination of excitons is strongly emitted in a direction substantially parallel to the
[0001] direction. When the light emitting layer 54 is formed, the quantum dot 300 is likely to be deposited such that one of the (0001) equivalent planes of the quantum dot 300 is located on the top surface side or the bottom surface side of the light emitting layer 54 due to its own weight. As a result, in the self-light emitting element 5, the light emitting layer 54 mainly emits light in a direction substantially perpendicular to the top surface and the bottom surface of the light emitting layer 54. For this reason, since the incident angle is small, the emitted light is less likely to be reflected on the boundary surface of the self-light emitting element 5, and the attenuation of light inside the self-light emitting element 5 is reduced. This improves the efficiency of extracting light from the self-light emitting element 5.
[0105] (Quantum dot manufacturing method) The quantum dots 300 according to the third embodiment can be produced by the same method as in the first embodiment, for example, a heating method, a hot injection method, a microwave assisted method, or a continuous flow method.
[0106] 12 and 13 are diagrams each showing an example of a method for manufacturing the quantum dot 300 shown in FIG.
[0107] A planar wurtzite quantum dot 300 as shown in Fig. 10 can be manufactured by forming a sheet of a material having a wurtzite crystal system and replacing ions as necessary. For example, when the quantum dot 300 is made of CdSe, first, oleylamine (shown as OA in Fig. 12) is added to CdCl2 to form a nanosheet-shaped complex of CdCl2. CdCl2 is a material that normally has a wurtzite crystal system.
[0108] Next, the octylamine solution in which Se has been dissolved is mixed with the CdCl2 complex and reacted at 100 degrees Celsius for 24 hours. As a result, two chloride ions, Cl, are generated, as shown in FIG. -One selenide ion, Se - The CdSe nanosheet complex thus formed has a flat shape and a wurtzite crystal system.
[0109] (Modification) FIG. 14 is a perspective view showing the structure of a modified example of the quantum dot 300 according to the third embodiment.
[0110] The surface between the top and bottom surfaces of the quantum dot 300 may include, as a non-polar surface, a (11-20) surface and a surface equivalent to the (11-20) surface, as shown in Fig. 14. The surface between the top and bottom surfaces of the quantum dot 300 may include, as a polar surface, a (11-21) surface and a surface equivalent to the (11-21). Surfaces equivalent to the (11-20) surface include the (-2110) surface, the (1-210) surface, the (-1-120) surface, the (2-1-10) surface, and the (-12-10) surface. The planes equivalent to (11-21) are the (-2111), (1-211), (-1-121), (2-1-11), (-12-11), (-2111), (11-2-1), (1-21-1), (-1-12-1), (2-1-1-1), and (-12-1-1).
[0111] Hereinafter, the (11-20) surface and surfaces equivalent to the (11-20) surface will be collectively referred to as (11-20)-equivalent surfaces, and the (11-21) surface and surfaces equivalent to the (11-21) surface will be collectively referred to as (11-21)-equivalent surfaces.
[0112] Similar to the above-described first embodiment, the third embodiment can also be applied to solar cells.
[0113] [Embodiment 4] Other embodiments of the present invention will be described below. For ease of explanation, the same reference numerals are given to members having the same functions as those described in the above embodiment, and the description thereof will not be repeated.
[0114] The light-emitting layer 54 (see FIG. 1) of this embodiment 4 differs from the self-emitting device 5 of the aforementioned embodiment 1 only in that it contains quantum dots 400 and neutral ligands 3 of this embodiment 4 instead of the quantum dots 100 and polar ligands 2 of the aforementioned embodiment 1.
[0115] (Quantum dot structure) Fig. 15 is a perspective view showing an example of the structure of a quantum dot 400 according to the embodiment 4. Fig. 16 is a schematic diagram showing the surface of the quantum dot 400 shown in Fig. 15 and the neutral ligand 3 protecting the surface.
[0116] The quantum dot 400 according to the fourth embodiment has a zinc-blende crystal system. The quantum dot 400 preferably includes at least one material selected from a group including materials that can spontaneously adopt a zinc-blende crystal system. The material is, for example, a II-VI compound such as ZnS, CdSe, or ZnSe, or a III-V compound such as InP.
[0117] When the quantum dot 400 according to the fourth embodiment has a core-shell structure, the band gap of the core is preferably smaller than the band gap of the shell, similarly to the first embodiment described above.
[0118] The quantum dot 400 is a polyhedral crystal having multiple crystal faces, and the surfaces are mainly non-polar faces. The surface of the quantum dot 400 includes, for example, 12 faces of a rhombus shown in FIG. 15, including (110), (011), (101), (1-10), (01-1), (-101), (-110), (0-11), (10-1), (-1-10), (0-1-1), and (-10-1). In this case, the ideal shape of the quantum dot 400 is a dodecahedron. Among the crystal faces of quantum dot 400, the faces equivalent to the (110) face are the (011) face, the (101) face, the (1-10) face, the (01-1) face, the (-101) face, the (-110) face, the (0-11) face, the (10-1) face, the (-1-10) face, the (0-1-1) face, and the (-10-1) face.
[0119] The (110) equivalent plane in the zinc blende crystal system is a non-polar plane. When the surface of the quantum dot 400 is a non-polar plane, the surface of the quantum dot 400 can be sufficiently protected (surface protection) using only the neutral ligand 3, as shown in Figure 16. The neutral ligand 3 can be bonded to the non-polar surface via an unshared electron pair 3a.
[0120] Quantum dots according to the fourth embodiment 4 When 70% or more of the surface of quantum dot 400 is a non-polar surface, the surface of quantum dot 400 can be sufficiently protected (surface protection) using only neutral ligand 3 for reasons similar to those in the first embodiment described above.
[0121] The higher the area ratio of the non-polar faces on the surface of the quantum dot 400, the more effective the surface protection by the neutral ligand 3. Therefore, in contrast to the above-mentioned embodiment 1, the surface of the quantum dot 400 according to this embodiment 4 only needs to be non-polar at 70% or more of its area ratio, preferably 80% or more of the surface area ratio is non-polar, and more preferably 90% or more of the surface area is non-polar. Also, it is ideal that the surface of the quantum dot 400 includes only non-polar faces.
[0122] As in the above-described first embodiment, if the area ratio of the nonpolar planes calculated in the crystal plane analysis of the quantum dots 400 is 60% or more, it is considered that at least a part of the quantum dots 400 contained in the light-emitting layer 54 is sufficiently surface-protected only by the neutral ligands 3. If it is 90% or more, it is considered that the light-emitting layer 54 contains quantum dots 400 whose surfaces are 100% nonpolar planes.
[0123] The non-polar surface has a smaller surface charge and a smaller dangling bond concentration than the polar surface. Therefore, the non-polar surface tends to have a relatively low reactivity, and when the ligand is desorbed from the surface of the quantum dot, the non-polar surface tends to react less with impurities. Therefore, the quantum dot 400 according to the fourth embodiment is less likely to deteriorate, and the reliability of the light-emitting layer 54 and the self-emitting element 5 can be improved.
[0124] The neutral ligand 3 is organic and includes at least one selected from the group consisting of organic neutral ligands including, for example, one or more phosphine groups, phosphine oxide groups, and amine groups at the terminal. The ligand including a phosphine group at the terminal includes, in part, a structure represented by the following structural formula (8) or the following structural formula (9). The ligand including a phosphine oxide group at the terminal includes, in part, a structure represented by the following structural formula (10). The ligand including an amine group at the terminal includes, in part, a structure represented by any one of the following structural formulas (11) to (15).
[0125] [ka] In the above structural formulas (8) to (15), H represents a hydrogen atom, N represents a nitrogen atom, O represents an oxygen atom, P represents a phosphorus atom, and R1, R2, and R3 each independently represent a hydrogen atom, an alkyl group, an aryl group, an alkoxyl group, or an unsaturated hydrocarbon group.
[0126] (Quantum dot manufacturing method) As in the first embodiment, the quantum dots 400 can be produced by, for example, a heating method, a hot injection method, a microwave assisted method, or a continuous flow method.
[0127] Dodecahedral quantum dots such as those shown in Figure 15 can be produced by using neutral ligands that preferentially bind to non-polar faces during the synthesis of the outermost layer. For example, if the quantum dots 400 are made of CdSe, a large amount of neutral ligands are added and crystals are grown at a reaction temperature of about 250 degrees. The neutral ligand is preferably an amine-based ligand. Amine-based ligands bind strongly to the (110) equivalent faces of CdSe and weakly or not at all to other faces. As a result, crystal growth proceeds on faces other than the (110) equivalent face, and the surface of the quantum dots 400 is composed of (110) equivalent faces.
[0128] Like the above-described first embodiment, the fourth embodiment can also be applied to a solar cell.
[0129] [Embodiment 5] Other embodiments of the present invention will be described below. For ease of explanation, the same reference numerals are given to members having the same functions as those described in the above embodiment, and the description thereof will not be repeated.
[0130] The light-emitting layer 54 (see FIG. 1) of this embodiment 5 differs from the light-emitting device 5 of the previously described embodiment 1 only in that it contains quantum dots 500 and neutral ligands 3 of this embodiment 5 instead of the quantum dots 100 and polar ligands 2 of the previously described embodiment 1.
[0131] (Quantum dot structure) FIG. 17 is a perspective view showing an example of the structure of a quantum dot 500 according to the fifth embodiment.
[0132] The quantum dot 500 according to the fifth embodiment has a sodium chloride type crystal system. 5 It is preferable that 00 includes at least one selected from a group including materials that can spontaneously adopt a sodium chloride type crystal system, such as IV-VI group compounds such as PbTe, PbSe, and PbS.
[0133] When the quantum dot 500 according to the fifth embodiment has a core-shell structure, the band gap of the core is preferably smaller than the band gap of the shell, similarly to the first embodiment described above.
[0134] The quantum dot 500 is a polyhedral crystal having multiple crystal faces, and its surfaces are mainly non-polar faces. The surface of the quantum dot 500 includes, for example, six faces of a quadrangle (100) equivalent face, a (-100) face, a (010) face, a (0-10) face, a (001) face, and a (00-1) face as shown in FIG. 17. These six faces are (100) equivalent faces. In this case, the ideal shape of the quantum dot 500 is a rectangular parallelepiped.
[0135] The (100) equivalent plane in the sodium chloride crystal system is a non-polar plane. As in the above-mentioned embodiment 4, the surface of the quantum dot 500 according to the fifth embodiment may be non-polar in an area ratio of 70% or more, preferably 80% or more, and more preferably 90% or more. Ideally, the surface of the quantum dot 500 includes only non-polar planes.
[0136] As in the above-described first embodiment, if the area ratio of nonpolar faces calculated as a result of the crystal face analysis of the quantum dots 500 is 90% or more, it is considered that the light-emitting layer 54 contains quantum dots 500 whose surfaces are 100% nonpolar faces.
[0137] (Quantum dot manufacturing method) The quantum dots 500 according to the fifth embodiment can be produced by the same method as in the first embodiment, for example, a heating method, a hot injection method, a microwave assisted method, or a continuous flow method.
[0138] 17, a hexahedral quantum dot 500 as shown in Fig. 17 can be produced by using a neutral ligand (amine-based ligand) that preferentially bonds to the non-polar face during synthesis of the outermost layer and by lowering the reaction temperature, in addition to the production method described in Non-Patent Document 1. For example, when the quantum dot 100 is made of PbS, the crystal is grown at about 110 degrees Celsius.
[0139] Like the above-described first embodiment, the fifth embodiment is also applicable to solar cells.
[0140] [Embodiment 6] Other embodiments of the present invention will be described below. For ease of explanation, the same reference numerals are given to members having the same functions as those described in the above embodiment, and the description thereof will not be repeated.
[0141] The light-emitting element 5 of this embodiment 6 (see Figure 1) differs from the light-emitting element 5 of the previously described embodiment 1 only in that the light-emitting layer 54 contains quantum dots 600 and neutral ligands 3 of this embodiment 6 instead of the quantum dots 100 and polar ligands 2 of the previously described embodiment 1.
[0142] (Quantum dot structure) Fig. 18 is a perspective view showing the structure of a quantum dot 600 according to the sixth embodiment. Fig. 19 is a diagram showing the plane orientations of the crystal planes of the quantum dot 600 shown in Fig. 18.
[0143] The quantum dot 600 according to the sixth embodiment has a wurtzite crystal system. The quantum dot 600 preferably includes at least one material selected from a group including materials that can spontaneously adopt a wurtzite crystal system. The material is, for example, a II-VI compound such as ZnS, CdSe, or ZnSe. Note that the II-VI compound can also adopt a zinc blende crystal system depending on the crystal growth conditions.
[0144] The quantum dot 600 is a polyhedral crystal having multiple crystal faces, and the surfaces thereof are mainly polar faces. The quantum dot 600 is, for example, a thin rod shape elongated in the
[0001] direction including six sides of the rectangular (1-100), (0-110), (-1010), (-1100), (01-10), and (10-10) faces shown in Fig. 19. The rod shape includes a hexagonal prism shape and a shape in which one or more corners of a hexagonal prism are cut off.
[0145] Fig. 19 is a diagram showing planes equivalent to the (1-100) plane in the crystal planes of the quantum dot 600. In Fig. 19, the (1-100) plane and planes equivalent to the (1-100) plane are hatched. Among the crystal planes of the quantum dot 600, the planes equivalent to the (1-100) plane are the (0-110) plane, the (-1010) plane, the (-1100) plane, the (01-10) plane, and the (10-10) plane.
[0146] The (-1100) equivalent plane in a wurtzite crystal is a nonpolar plane. As in the above-described embodiment 4, the surface of the quantum dot 600 according to the sixth embodiment may be nonpolar in an area ratio of 70% or more, preferably 80% or more, and more preferably 90% or more. Ideally, the surface of the quantum dot 600 includes only nonpolar planes.
[0147] As in the above-described first embodiment, if the area ratio of nonpolar faces calculated as a result of the crystal face analysis of the quantum dots 600 is 90% or more, it is considered that the light-emitting layer 54 contains quantum dots 600 in which 100% of the surface of the quantum dots 600 is a nonpolar face.
[0148] In quantum dot 600, the plane between one of the side surfaces and the plane between the other of the side surfaces may be polar planes, and may include, for example, (0001) equivalent planes and / or (1-101) equivalent planes.
[0149] As shown in FIG. 18, the quantum dot 600 has a rod-like shape elongated in the
[0001] direction because the ratio of the area of the (-1100) equivalent plane on the surface of the quantum dot 600 is large. Therefore, the direction of exciton recombination in the quantum dot 600 is mainly a direction approximately parallel to the [0001 direction]. As a result, the light emitted by the recombination of excitons is strongly emitted in a direction approximately perpendicular to the
[0001] direction of the quantum dot 600. When the light emitting layer 54 is formed, the quantum dot 600 is likely to be deposited such that one of the (-1100) equivalent planes of the quantum dot 600 is located on the top surface side or the bottom surface side of the light emitting layer 54 due to its own weight. As a result, in the self-light emitting element 5, the light emitting layer 54 mainly emits light in a direction approximately perpendicular to the top surface and the bottom surface of the light emitting layer 54. Therefore, the emitted light is less likely to be reflected by the boundary surface of the self-light emitting element 5, and the attenuation of light inside the self-light emitting element 5 is reduced. This improves the efficiency of extracting light from the self-light emitting element 5.
[0150] (Quantum dot manufacturing method) The quantum dots 600 according to the sixth embodiment can be produced by the same method as in the first embodiment, for example, a heating method, a hot injection method, a microwave assisted method, or a continuous flow method.
[0151] Rod-shaped wurtzite quantum dots as shown in FIG. 18 can be fabricated by forming a wurtzite nanocrystal as a core and epitaxially growing a wurtzite nanocrystal as a shell on the (0001) equivalent plane of the core.
[0152] For example, if the quantum dot 600 consists of a CdSe core and a CdS shell, first prepare a three-neck flask and mix 1.5 mmol of CdO, 6 mmol of n-tetradecylphosphonic acid (TDPA), 24 mmol of oleyl alcohol, and 10 g of TOPO in the three-neck flask. Heat this for 1 hour at 150 degrees Celsius in a nitrogen environment. Then, heat it to 350 degrees Celsius, and the moment the solution becomes transparent, inject 2 ml of TOP into the flask. When the solution reaches 350 degrees Celsius, inject 1.5 ml of a TOP complex (trioctylphosphine selenide: TOP-Se) solution with a volume molar concentration of 1.7 mol / l of Se into the flask. After a few seconds of reaction, the flask is immersed in water at 80 degrees Celsius to cool it down and stop the reaction. Next, add 20 ml of methanol to the solution to precipitate the nanoparticles. These nanoparticles are wurtzite-type crystals of CdSe. The CdSe nanocrystals are dispersed in a sulfide TOP (trioctylphosphine sulfide: TOP-S) solution with a volume concentration of 2.4 mol / l.
[0153] Next, a three-neck flask is prepared, and 5 g of TOPO, an arbitrary amount of octadecylphosphonic acid (ODPA), an arbitrary amount of dodecylphosphonic acid (DDPA), and an arbitrary amount of CdO are mixed in the flask. This is heated at 150 degrees Celsius for 1 hour in a nitrogen environment. Then, the temperature is raised to 350 degrees Celsius, and 1 ml of TOP is injected into the flask the moment the solution becomes transparent. When the solution reaches 350 degrees Celsius, 2 ml of the solution in which the CdSe nanocrystals are dispersed in TOP-S is injected into the flask. Note that the molar ratio of Cd to S is maintained at 1.2:1 so that the CdS crystals can easily expose their cation-rich surfaces. After a sufficient reaction time, the flask is immersed in water at 80 degrees Celsius to lower the temperature and stop the reaction. Next, 5 ml of toluene and 10 ml of methanol are added to the solution to precipitate the nanorods. These nanorods are quantum dots 600.
[0154] (Modification) Fig. 20 and Fig. 22 are perspective views showing the structure of a modified example of the quantum dot 600 according to the sixth embodiment. Fig. 21 is a diagram showing the plane orientation of each crystal plane of the quantum dot 600 shown in Fig. 20. Fig. 23 is a cross-sectional view showing the plane orientation of each crystal plane of the quantum dot 600 shown in Fig. 22.
[0155] The quantum dot 600 according to the sixth embodiment is not limited to the above.
[0156] The quantum dot 600 may be, for example, a long and thin rod-like shape including six rectangular (11-20) faces, (-2110) faces, (1-210) faces, (-1-120) faces, (2-1-10) faces, and (-12-10) faces as side faces as shown in Figures 20 and 21. The faces equivalent to the (11-20) faces are the (-2110) faces, (1-210) faces, (-1-120) faces, (2-1-10) faces, and (-12-10) faces. In this case, the quantum dot 600 may include, for example, a (0001) equivalent face and / or a (11-21) equivalent face in a face between one side of the side faces and a face between the other side of the side faces.
[0157] FIG. 21 is a diagram showing a (11-20) equivalent plane in the crystal plane of the quantum dot 600 shown in FIG.
[0158] In wurtzite crystals, the (11-20) equivalent plane is a nonpolar plane.
[0159] The quantum dot 600 may be, for example, a long rod-like shape including twelve sides, which are (1-100)-equivalent planes and (11-20)-equivalent planes, as shown in FIG. 22. In this case, the shape of the rod includes a dodecagonal prism shape and a dodecagonal prism shape with one or more corners cut off. FIG. 23 is a cross-sectional view of the quantum dot 600 shown in FIG. 22. In this case, the surface between one side of the side surfaces of the quantum dot 600 and the surface between the other side of the side surfaces may include, for example, a (0001)-equivalent plane, and / or may include a (1-101)-equivalent plane and a (11-21)-equivalent plane.
[0160] Like the above-described first embodiment, the sixth embodiment can also be applied to solar cells.
[0161] 〔summary〕 The quantum dot according to the first aspect of the present invention has a structure in which 70% or more of the surface area is polar faces, or 70% or more of the surface area is non-polar faces.
[0162] The "area ratio" in the above-mentioned embodiment 1 is an actual value. As described above, if the ratio of the polar surface (or the non-polar surface) in the analysis result is 60% or more, it is considered that the quantum dots in which the area ratio of the polar surface (or the non-polar surface) is 70% or more are included in the entire light-emitting layer. Therefore, when the area ratio of the polar surface (or the non-polar surface) in the analysis result is 60% or more, it is considered that at least a part of the quantum dots included in the quantum dot layer is sufficiently surface-protected by only the polar ligand (or the neutral ligand).
[0163] The quantum dot according to the second aspect of the present invention may be configured in such a way that, in the first aspect, the surface includes only polar faces or only non-polar faces.
[0164] As described above, if the analysis results show that the proportion of the polar surface (or the nonpolar surface) is 90% or more, it is considered that the quantum dot layer actually contains quantum dots in which 100% of the surface area of the quantum dots is the polar surface (or the nonpolar surface).
[0165] The quantum dot according to the third aspect of the present invention may be the quantum dot according to the first or second aspect, which has a core-shell structure and the band gap of the core is smaller than the band gap of the shell.
[0166] The quantum dot according to aspect 4 of the present invention, in any one of aspects 1 to 3, may have a zinc blende crystal system, and the surface may include 14 faces, namely, the (100) face, the (-100) face, the (010) face, the (0-10) face, the (001) face, the (00-1) face, the (111) face, the (-111) face, the (1-11) face, the (-1-11) face, the (11-1) face, the (-11-1) face, the (1-1-1) face, the (1-1-1) face, and the (-1-1-1) face.
[0167] The quantum dot according to aspect 5 of the present invention, in any one of aspects 1 to 3, may have a zinc blende crystal system, and the surface may include six faces, namely, a (100) face, a (-100) face, a (010) face, a (0-10) face, a (001) face, and a (00-1) face.
[0168] The quantum dot according to aspect 6 of the present invention, in any one of aspects 1 to 3, may have a zinc blende crystal system, and the surface may include eight faces, namely, a (111) face, a (-111) face, a (1-11) face, a (-1-11) face, a (11-1) face, a (-11-1) face, a (1-1-1) face, and a (-1-1-1) face.
[0169] The quantum dot according to aspect 7 of the present invention, in any one of aspects 1 to 3, may have a sodium chloride type crystal system, and the surface may include eight faces, namely, a (111) face, a (-111) face, a (1-11) face, a (-1-11) face, a (11-1) face, a (-11-1) face, a (1-1-1) face, and a (-1-1-1) face.
[0170] The quantum dot according to aspect 8 of the present invention, in any one of aspects 1 to 3, may have a wurtzite crystal system, and the surface may include two faces, a (0001) face and a (000-1) face.
[0171] The quantum dot layer according to a ninth aspect of the present invention includes the quantum dots according to any one of the fourth to eighth aspects and a polar ligand.
[0172] The quantum dot layer according to a tenth aspect of the present invention may be configured in the ninth aspect, in which the polar ligand accounts for 90% or more of the substance amount of the ligand contained in the quantum dot layer.
[0173] The "amount ratio of substance" in the above-mentioned embodiment 10 is an analysis result. As described above, if the proportion of the polar ligand in the analysis result is 90% or more, it is highly likely that the amount of substance of the ligand actually contained in the quantum dot is 100%.
[0174] The quantum dot layer according to an eleventh aspect of the present invention may be configured as in the ninth or tenth aspect, wherein the polar ligand at least partially contains at least one of the structures represented by the following structural formulas (1) to (7).
[0175] [ka] In the formula, C represents a carbon atom, O represents an oxygen atom, and O - indicates an oxide ion, S indicates a sulfur atom, and S -represents a sulfide ion, P represents phosphorus, and R1 and R2 each independently represent a hydrogen atom, an alkyl group, an aryl group, an alkoxyl group, or an unsaturated hydrocarbon group.
[0176] The quantum dot layer according to a twelfth aspect of the present invention is the quantum dot layer according to the ninth or tenth aspect, wherein the polar ligand is represented by the ionic formula Cl - , Br - , I - , SCN - , C.N. - , O.H. - , S.H. - , SeH - , TeH - , Se 2- , S 2- , Te 2- , Sn2S6 4- , Sn2Se6 4- , In2Se4 2- , In2Te4 2- , Ga2Se4 2- , Sb2Se4 2- , Sb2Te4 2- The inorganic polar ligand may include at least one selected from the group consisting of inorganic polar ligands represented by the following formula:
[0177] The quantum dot according to aspect 13 of the present invention, in any one of aspects 1 to 3, may have a zincblende crystal system, and the surface may include 12 faces, namely, a (101) face, a (-101) face, a (011) face, a (0-11) face, a (110) face, a (-110) face, a (1-1-) face, a (-1-10) face, a (10-1) face, a (-10-1) face, a (01-1) face, and a (0-1-1) face.
[0178] The quantum dot according to aspect 14 of the present invention, in any one of aspects 1 to 3, may have a sodium chloride type crystal system, and the surface may include six faces, namely, a (100) face, a (-100) face, a (010) face, a (0-10) face, a (001) face, and a (00-1) face.
[0179] The quantum dot according to aspect 15 of the present invention, in any one of aspects 1 to 3, may have a wurtzite crystal system, and the surface may include 12 planes, namely, the (1-100) plane, the (0-110) plane, the (-1010) plane, the (-1100) plane, the (01-10) plane, the (10-10) plane, the (11-20) plane, the (-2110) plane, the (1-210) plane, the (-1-120) plane, the (2-1-10) plane, and the (-12-10) plane.
[0180] The quantum dot according to aspect 16 of the present invention, in any one of aspects 1 to 3, may have a wurtzite crystal system, and the surface may include six faces, namely, a (1-100) face, a (0-110) face, a (-1010) face, a (-1100) face, a (01-10) face, and a (10-10) face.
[0181] The quantum dot according to aspect 17 of the present invention, in any one of aspects 1 to 3, may have a wurtzite crystal system, and the surface may include six faces, namely, a (11-20) face, a (-2110) face, a (1-210) face, a (-1-120) face, a (2-1-10) face, and a (-12-10) face.
[0182] The quantum dot layer according to the eighteenth aspect of the present invention includes the quantum dots according to any one of the thirteenth to seventeenth aspects and a neutral ligand.
[0183] The quantum dot layer according to Aspect 19 of the present invention may be configured in such a manner that, in Aspect 18, 90% or more of the substance amount of the ligand contained in the quantum dot layer is the neutral ligand.
[0184] The "amount ratio of substance" in the above-mentioned embodiment 19 is an analysis result. As described above, if the proportion of the neutral ligand in the analysis result is 90% or more, it is highly likely that the amount of substance of the ligand actually contained in the quantum dot is 100%.
[0185] The quantum dot layer according to Aspect 20 of the present invention may be configured as in Aspect 18 or Aspect 19, wherein the neutral ligand includes at least one of the structures represented by the following structural formulas (8) to (15) in a part thereof.
[0186] [ka] In the formula, O represents an oxygen atom; - represents an oxide ion, P represents phosphorus, and R1, R2, and R3 each independently represent a hydrogen atom, an alkyl group, an aryl group, an alkoxyl group, or an unsaturated hydrocarbon group.
[0187] A light-emitting device according to a twenty-first aspect of the present invention includes the quantum dot layer according to any one of the ninth to twelfth aspects and the eighteenth to twenty aspects.
[0188] A solar cell according to a twenty-second aspect of the present invention has a configuration including the quantum dot layer according to any one of the ninth to twelfth aspects and the eighteenth to twenty aspects.
[0189] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. The technical scope of the present invention also includes embodiments obtained by appropriately combining the technical means disclosed in the different embodiments. Furthermore, new technical features can be formed by combining the technical means disclosed in the respective embodiments. [Explanation of symbols]
[0190] 2. Polar Ligands 3. Neutral Ligands 5. Self-luminous element (light-emitting element) 6. Solar Cells 54 Light-emitting layer (quantum dot layer) 57 Photoelectric conversion layer (quantum dot layer) 100,200,300,400,500,600 quantum dots
Claims
1. 70% or more of the surface area is polar, or 70% or more of the surface area is non-polar, It has a zinc blende crystal system, The quantum dot includes 14 surfaces, namely, a (100) surface, a (-100) surface, a (010) surface, a (0-10) surface, a (001) surface, a (00-1) surface, a (111) surface, a (-111) surface, a (1-11) surface, a (-1-11) surface, a (11-1) surface, a (-11-1) surface, a (1-1-1) surface, and a (-1-1-1) surface.
2. 70% or more of the surface area is polar, or 70% or more of the surface area is non-polar, It has a zinc blende crystal system, The quantum dot has six surfaces, namely, a (100) surface, a (-100) surface, a (010) surface, a (0-10) surface, a (001) surface, and a (00-1) surface.
3. 70% or more of the surface area is polar, or 70% or more of the surface area is non-polar, It has a zinc blende crystal system, The quantum dot, wherein the surface includes eight faces, namely, a (111) face, a (-111) face, a (1-11) face, a (-1-11) face, a (11-1) face, a (-11-1) face, a (1-1-1) face, and a (-1-1-1) face.
4. 70% or more of the surface area is polar, or 70% or more of the surface area is non-polar, It has a sodium chloride type crystal system, The quantum dot, wherein the surface includes eight faces, namely, a (111) face, a (-111) face, a (1-11) face, a (-1-11) face, a (11-1) face, a (-11-1) face, a (1-1-1) face, and a (-1-1-1) face.
5. A quantum dot layer comprising the quantum dot according to any one of claims 1 to 4 and a polar ligand.
6. 6. The quantum dot layer according to claim 5, wherein the polar ligand accounts for 90% or more of the substance amount of the ligand contained in the quantum dot layer.
7. The polar ligand is represented by the following structural formulas (1) to (7): 【Chemistry 1】 (In the formula, C represents a carbon atom, O represents an oxygen atom, and O - represents an oxide ion, S represents a sulfur atom, and S - represents a sulfide ion, P represents phosphorus, and R 1 and R 2 each independently represents a hydrogen atom, an alkyl group, an aryl group, an alkoxyl group, or an unsaturated hydrocarbon group. The quantum dot layer according to claim 5 or 6, which partially contains at least one of the structures represented by the following formula:
8. The polar ligand has the ionic formula Cl - , B - , I - , S.C.N. - , C.N. - , O.H. - , S.H. - , SeH - , TeH - , Se 2- , S 2- , Te 2- , Sn 2 S 6 4- , Sn 2 Se 6 4- , In 2 Se 4 2- , In 2 Te 4 2- , Ga 2 Se 4 2- , Sb 2 Se 4 2- , Sb 2 Te 4 2- The quantum dot layer according to claim 5 or 6, comprising at least one inorganic polar ligand selected from the group consisting of inorganic polar ligands represented by the formula:
9. 70% or more of the surface area is polar, or 70% or more of the surface area is non-polar, It has a zinc blende crystal system, The quantum dot includes 12 surfaces, namely, a (101) surface, a (-101) surface, a (011) surface, a (0-11) surface, a (110) surface, a (-110) surface, a (1-10) surface, a (-1-10) surface, a (10-1) surface, a (-10-1) surface, a (01-1) surface, and a (0-1-1) surface.
10. 70% or more of the surface area is polar, or 70% or more of the surface area is non-polar, It has a sodium chloride type crystal system, The quantum dot has six surfaces, namely, a (100) surface, a (-100) surface, a (010) surface, a (0-10) surface, a (001) surface, and a (00-1) surface.
11. 70% or more of the surface area is polar, or 70% or more of the surface area is non-polar, It has a wurtzite crystal system, The quantum dot includes 12 surfaces, namely, a (1-100) surface, a (0-110) surface, a (-1010) surface, a (-1100) surface, a (01-10) surface, a (10-10) surface, a (11-20) surface, a (-2110) surface, a (1-210) surface, a (-1-120) surface, a (2-1-10) surface, and a (-12-10) surface.
12. 70% or more of the surface area is polar, or 70% or more of the surface area is non-polar, It has a wurtzite crystal system, The quantum dot has six surfaces, namely, a (1-100) surface, a (0-110) surface, a (-1010) surface, a (-1100) surface, a (01-10) surface, and a (10-10) surface.
13. 70% or more of the surface area is polar, or 70% or more of the surface area is non-polar, It has a wurtzite crystal system, The quantum dot, wherein the surface includes six surfaces, namely, a (11-20) surface, a (-2110) surface, a (1-210) surface, a (-1-120) surface, a (2-1-10) surface, and a (-12-10) surface.
14. A quantum dot layer comprising the quantum dot according to any one of claims 9 to 13 and a neutral ligand.
15. 15. The quantum dot layer according to claim 14, wherein the neutral ligand accounts for 90% or more of the substance amount of the ligand contained in the quantum dot layer.
16. The neutral ligand is represented by the following structural formulas (8) to (15): 【Chemistry 2】 (In the formula, O represents an oxygen atom; O - represents an oxide ion, P represents phosphorus, and R 1 and R 2 and R 3 each independently represents a hydrogen atom, an alkyl group, an aryl group, an alkoxyl group, or an unsaturated hydrocarbon group. The quantum dot layer according to claim 14 or 15, comprising at least one of the structures represented by the following formula:
17. A self-luminous device comprising the quantum dot layer according to any one of claims 5 to 8 and claims 14 to 16.
18. A solar cell comprising the quantum dot layer according to any one of claims 5 to 8 and claims 14 to 16.
19. The quantum dot according to any one of claims 1 to 16, wherein the surface comprises only polar faces or only non-polar faces.
20. It has a core-shell structure, 20. The quantum dot according to any one of claims 1 to 16 or claim 19, wherein the band gap of the core is smaller than the band gap of the shell.
Citation Information
Patent Citations
Nanoparticles, preparation method thereof and quantum dot photoelectric device
CN110305656A
Quantun dot light emitting device
KR1020120029174A
Targeted nanoclusters and methods of their use
US20120269721A1
Polymer-encapsulated nanoparticle systems
US20130095239A1
Semiconductor optical element array and manufacturing method therefore
WO2010023921A1