Printing ink composition, laminate, packaging material, and building material
The printing ink composition with a binder resin, aluminum fine particles, and rosin derivative addresses redispersibility and adhesion issues, enhancing heat resistance and hiding properties for laminates and packaging materials.
Patent Information
- Application Number
- JP2024097601
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2044-06-17
AI Technical Summary
Existing printing inks containing aluminum fine particles face issues with redispersibility, adhesion to substrates, hiding properties, and heat resistance, particularly due to the high specific gravity of aluminum particles leading to sedimentation and poor viscosity stability.
A printing ink composition comprising a binder resin, aluminum fine particles, a rosin derivative, and a solvent, with specific mass ratios and surface treatments, enhances redispersibility, adhesion, and heat resistance by using a rosin derivative with an acid value of 20 mgKOH/g or more and aluminum particles with an average diameter of 5 to 20 μm, treated with (meth)acrylic resin, fatty acid, or silica.
The composition achieves excellent redispersibility, adhesion to substrates, and heat resistance, improving the hiding properties of printed layers, suitable for use in laminates, packaging materials, and construction materials.
Smart Images

Figure 0007594706000005 
Figure 0007594706000006 
Figure 0007594706000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a printing ink composition, a laminate, a packaging material, and a building decoration material. [Background technology]
[0002] Substrates such as films used for packaging materials and building materials are printed with the purpose of conveying information and imparting design and function. In addition, printing inks with dispersed glittering pigments may be printed to provide further design and a sense of luxury. Flat aluminum particles, which are inexpensive and easy to process, are generally used as glittering pigments. In addition, printing inks with dispersed aluminum particles have excellent light-shielding properties and are sometimes used not only for design but also for protecting the contents and blocking light. Printing inks contain solvents to provide a viscosity suitable for methods such as gravure printing and flexographic printing, but aluminum particles have a high specific gravity and therefore tend to settle in the printing ink.
[0003] In addition, the so-called residual printing ink remaining after use as printing ink is sometimes discarded, but there is a demand for reuse in order to reduce costs and waste. Printing inks containing aluminum fine particles have a problem that the aluminum fine particles have a high specific gravity, and the viscosity of the residual ink remaining after use is reduced, which makes the aluminum fine particles more likely to settle. Although it is possible to redisperse the aluminum fine particles that have settled in the residual ink by mechanical stirring using a gyro mixer or the like, this is not efficient in terms of time and cost, and there is a demand for printing inks that can be redispersed by, for example, only relatively weak shaking by hand.
[0004] Patent Document 1 discloses a gravure ink for surface printing that contains aluminum particles, an organic solvent, and a specific ratio of polyamide resin and cellulose resin as binder resins, and discloses that the gravure ink suppresses the settling of aluminum particles. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2020-59806 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, the redispersibility of the aluminum fine particles in the gravure ink described in Patent Document 1 is insufficient. Moreover, there has been no sufficient study yet on achieving a balance between redispersibility and the adhesion to the substrate, hiding power, and heat resistance of the resulting printed layer. The present invention aims to provide a printing ink composition which has excellent redispersibility of aluminum microparticles and which provides a printed layer having excellent adhesion to a substrate, hiding power, and heat resistance; a printing ink containing the printing ink composition; a laminate having a printed layer formed using the printing ink; and a packaging material and a building material which contain the laminate. [Means for solving the problem]
[0007] The present invention has the following aspects. [1] A printing ink composition comprising a binder resin (A), aluminum fine particles (B), a rosin derivative (C), and a solvent (D), wherein the content of the aluminum fine particles (B) relative to the total mass of solids in the printing ink composition is 9 to 29 mass%, the average particle diameter of the aluminum fine particles (B) is 5 to 20 μm, the acid value of the rosin derivative (C) is 20 mg KOH / g or more, the mass ratio of the binder resin (A) to the aluminum fine particles (B) is 2 to 9, and the mass ratio of the aluminum fine particles (B) to the rosin derivative (C) is 1.43 to 10. [2] The printing ink composition according to [1], wherein the surfaces of the aluminum fine particles (B) are treated with at least one selected from the group consisting of (meth)acrylic resins, fatty acids, and silica. [3] The printing ink composition according to [1] or [2], wherein the binder resin (A) comprises at least one selected from the group consisting of (meth)acrylic resins, polyamide resins, cellulose-based resins, and fluorine-modified polyolefin resins. [4] The printing ink composition according to any one of [1] to [3], wherein the rosin derivative (C) contains at least one selected from the group consisting of rosin-modified fumaric acid resins, rosin-modified maleic acid resins, and terpene phenol resins, and the acid value of the rosin derivative (C) is 250 mg KOH / g or less. [5] The printing ink composition according to any one of [1] to [4], wherein the optical density of the printed layer before storage (OD value before storage) and the optical density of the printed layer after storage (OD value after storage), measured by the following measurement method, satisfy the following formula 1. OD value before storage - OD value after storage ≦ 0.25 Equation 1 [Measurement method] The printing ink composition was adjusted to have a viscosity of 16 seconds at 25° C. using a Zahn cup #3. The viscosity-adjusted printing ink composition was then dried to a mass of 2 g / m 2 The optical density of a printed matter coated on a transparent PET film having a thickness of 20 μm so as to obtain a print having an OD value before storage is taken as the OD value before storage. The viscosity-adjusted printing ink composition is placed in a container, and the container is stored in a thermostatic chamber at 20° C. for one month. The container is then shaken, and the viscosity-adjusted printing ink composition after storage is adjusted to a dry mass of 2 g / m 2 The optical density of the print coated on a 20 μm thick transparent PET film is taken as the OD value after storage. [6] A printing ink comprising the printing ink composition according to any one of [1] to [5]. [7] A laminate comprising a substrate and a printed layer formed on at least one surface of the substrate using the printing ink described in [6]. [8] A packaging material comprising the laminate described in [7]. [9] A building material comprising the laminate described in [7]. Effect of the Invention
[0008] According to the present invention, it is possible to provide a printing ink composition which has excellent redispersibility of aluminum microparticles and which provides a printed layer having excellent adhesion to a substrate, hiding power, and heat resistance; a printing ink containing the printing ink composition; a laminate having a printed layer formed using the printing ink; and a packaging material and a building material which contain the laminate. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a cross-sectional view illustrating a schematic example of a laminate of the present invention. [Diagram 2] FIG. 1 is a cross-sectional view illustrating a schematic example of a laminate of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present invention will be described in detail below. The following embodiments are merely examples for explaining the present invention, and are not intended to limit the present invention to these embodiments. The present invention can be implemented in various forms without departing from the spirit of the present invention. "Solid content" refers to the components contained in the printing ink composition (printing ink), excluding volatile media such as water and organic solvents, and is the component that will ultimately form the printed layer, and is specifically measured in accordance with JIS K 5601-1-2:2008. In this specification, "(meth)acrylic resin" is a general term for "acrylic resin" and "methacrylic resin". "(meth)acrylate" is a general term for "acrylate" and "methacrylate". "(meth)acrylic acid" is a general term for "acrylic acid" and "methacrylic acid". "(meth)acrylamide" is a general term for "acrylamide" and "methacrylamide". The weight average molecular weight of the resin is a weight average molecular weight converted into a standard polystyrene molecular weight and is measured by gel permeation chromatography (GPC). The glass transition temperature of a resin is measured in accordance with JIS K 7121:2012 as follows: Using a differential scanning calorimeter, 10 mg of resin is heated from -100°C to 160°C at a rate of 20°C / min to obtain a curve (DSC curve), and the glass transition temperature is determined from the intersection point between the baseline and the tangent to the endothermic curve. The softening point of the resin can be measured by the ring and ball method in accordance with JIS K 5601-2-2:1999. The acid value of the resin can be measured by a neutralization titration method in accordance with JIS K 0070:1992. The amine value of a resin is the amount of potassium hydroxide (mg) equivalent to the amount of hydrochloric acid required to neutralize the primary, secondary, and tertiary amines contained in 1 g of the sample. It can be measured in accordance with ASTM D2074.
[0011] <Printing ink composition> A printing ink composition according to one embodiment of the present invention contains a binder resin (A), aluminum fine particles (B), a rosin derivative (C), and a solvent (D). The printing ink composition may further contain components (optional components) other than the binder resin (A), the aluminum fine particles (B), the rosin derivative (C), and the solvent (D) as necessary, within a range that does not impair the effects of the present invention.
[0012] <Binder resin (A)> The binder resin (A) used in the present invention preferably contains at least one selected from the group consisting of (meth)acrylic resins, polyamide resins, cellulose-based resins, and fluorine-modified polyolefin resins. Among these, polyamide resins and cellulose-based resins are more preferred, and both polyamide resins and cellulose-based resins are even more preferred.
[0013] ((Meth)acrylic resin) The (meth)acrylic resin is a resin that contains (meth)acrylate units. Examples of the (meth)acrylic resin include a homopolymer of (meth)acrylate, a copolymer of two or more kinds of (meth)acrylate, and a copolymer of (meth)acrylate and a monomer other than (meth)acrylate. Examples of the (meth)acrylic resin include a urethane-modified (meth)acrylic resin and a silicone-modified (meth)acrylic resin. Examples of the urethane-modified (meth)acrylic resin include a reaction product of a polyvalent isocyanate compound, a polyol compound, and a hydroxyl group-containing (meth)acrylate, or a reaction product of a polyvalent isocyanate compound and a hydroxyl group-containing (meth)acrylate. The ratio of the (meth)acrylate unit to the total mass of all monomer units constituting the (meth)acrylic resin is preferably from 10 to 100% by mass, more preferably from 20 to 100% by mass. These (meth)acrylic resins may be used alone or in combination of two or more kinds.
[0014] Examples of the (meth)acrylate include alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, isobutyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and lauryl (meth)acrylate; cycloalkyl (meth)acrylates such as cyclohexyl (meth)acrylate; aryl (meth)acrylates such as phenyl (meth)acrylate; aralkyl (meth)acrylates such as benzyl (meth)acrylate; and hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate. These (meth)acrylates may be used alone or in combination of two or more.
[0015] Examples of monomers other than (meth)acrylates include conjugated diene compounds such as 1,3-butadiene, isoprene, and chloroprene; aromatic vinyl compounds such as styrene, α-methylstyrene, halogenated styrene, divinylbenzene, and vinyl toluene; vinyl cyanide compounds such as acrylonitrile and methacrylonitrile; acrylamides such as N,N-dimethyl(meth)acrylamide and N,N-diethyl(meth)acrylamide; unsaturated carboxylic acids such as (meth)acrylic acid, itaconic acid, maleic acid, fumaric acid, and croton; and unsaturated carboxylic acid esters such as diethyl maleate, dibutyl maleate, dibutyl fumarate, diethyl itaconate, and dibutyl itaconate. These monomers may be used alone or in combination of two or more.
[0016] The glass transition temperature (hereinafter also referred to as "Tg") of the acrylic resin is preferably 5 to 105°C, more preferably 10 to 80°C, and even more preferably 15 to 60°C. When the Tg of the (meth)acrylic resin is equal to or higher than the above lower limit, the blocking resistance of the resulting printed layer is likely to be improved. When the Tg of the (meth)acrylic resin is equal to or lower than the above upper limit, the adhesion of the resulting printed layer to the substrate is likely to be improved.
[0017] The weight average molecular weight (hereinafter also referred to as "Mw") of the (meth)acrylic resin is preferably 10,000 to 200,000, more preferably 20,000 to 150,000, and even more preferably 30,000 to 120,000. When the Mw of the (meth)acrylic resin is equal to or greater than the above lower limit, the blocking resistance of the resulting printed layer is likely to be improved. When the Mw of the (meth)acrylic resin is equal to or less than the above upper limit, the adhesion of the resulting printed layer to the substrate is likely to be improved.
[0018] As the (meth)acrylic resin, a commercially available product may be used. Commercially available (meth)acrylic resins include, for example, the "Acrit" series manufactured by Taisei Fine Chemical Co., Ltd. and the "Dianal" series manufactured by Mitsubishi Chemical Corporation.
[0019] (Polyamide resin) The polyamide resin may be a thermoplastic polyamide which is a polycondensation product of a polybasic acid and a polyamine and is soluble in an organic solvent. Examples of polybasic acids include adipic acid, sebacic acid, azelaic acid, phthalic anhydride, isophthalic acid, suberic acid, glutaric acid, fumaric acid, pimelic acid, oxalic acid, malonic acid, succinic acid, maleic acid, terephthalic acid, 1,4-cyclohexyldicarboxylic acid, trimellitic acid, dimer acid, hydrogenated dimer acid, etc. In addition to these polybasic acids, monocarboxylic acids such as acetic acid, propionic acid, lauric acid, palmitic acid, benzoic acid, and cyclohexanecarboxylic acid can also be used in combination. Examples of the polyamine include polyamines. Examples of the polyamine include aliphatic diamines such as ethylenediamine, propylenediamine, hexamethylenediamine, and methylaminopropylamine; aliphatic polyamines such as diethylenetriamine and triethylenetetramine; alicyclic polyamines such as cyclohexylenediamine and isophoronediamine; and aromatic polyamines such as xylylenediamine, phenylenediamine, and diaminodiphenylmethane. In addition to these polyamines, primary or secondary monoamines such as n-butylamine, octylamine, dielamine, monoethanolamine, monopropanolamine, diethanolamine, and dipropanolamine can also be used in combination.
[0020] Specific examples of polyamide resins include thermoplastic polyamide resins using fatty acids made from vegetable materials and polymerized fatty acids made from them. Representative examples of fatty acids made from vegetable materials include tall oil, soybean oil, coconut oil, palm oil, cashew nut oil, rice bran, and cacao beans. On the other hand, examples of polymerized fatty acids include dimer acids and hydrogenated dimer acids obtained by reducing dimer acids with hydrogen. These polyamide resins may be used alone or in combination of two or more.
[0021] The Mw of the polyamide resin is preferably 2,000 to 50,000, more preferably 2,500 to 30,000, and even more preferably 3,000 to 10,000. When the Mw of the polyamide resin is equal to or greater than the lower limit, the abrasion resistance and heat resistance of the resulting printed layer are likely to be improved. When the Mw of the polyamide resin is equal to or less than the upper limit, the solubility in the solvent (D) is likely to be improved.
[0022] The acid value of the polyamide resin is preferably 30 mgKOH / g or less, more preferably 20 mgKOH / g or less, and even more preferably 15 mgKOH / g or less. When the acid value of the polyamide resin is the above upper limit or less, the stability of the printing ink is likely to be improved. The amine value of the polyamide resin is preferably 30 mgKOH / g or less, more preferably 20 mgKOH / g or less, and even more preferably 15 mgKOH / g or less.
[0023] The softening point of the polyamide resin is preferably 80 to 140° C., more preferably 90 to 135° C., and even more preferably 95 to 130° C. When the softening point of the polyamide resin is equal to or higher than the lower limit, the heat resistance and blocking resistance of the resulting printed layer are likely to be improved. When the softening point of the polyamide resin is equal to or lower than the upper limit, the adhesion to the substrate is likely to be improved.
[0024] As the polyamide resin, commercially available products may be used. Commercially available examples of polyamide resins include the "Leomaid" series manufactured by Kao Corporation, the "Newmide" series manufactured by Harima Chemicals, the "Tomide" series manufactured by T&K Toka, the "Sunmide" series manufactured by Air Products Japan, and the "Vegichem Green" series manufactured by Tsuno Foods Industries.
[0025] (Cellulosic resin) The cellulose resin includes cellulose and cellulose derivatives in which at least a part of the hydroxyl groups of cellulose is replaced by other groups, and the cellulose derivatives are preferred.The cellulose derivatives include, for example, nitrocellulose (nitro group-substituted product); cellulose acetate, cellulose acetate propionate, cellulose acetate butyrate, and other lower acyl group-substituted products; methylcellulose, ethylcellulose, and other lower alkyl group-substituted products; benzylcellulose, and other aralkyl group-substituted products; and hydroxyethylcellulose, hydroxypropylcellulose, hydroxymethylpropylcellulose, and other hydroxyalkyl group-substituted cellulose derivatives, and the nitrocellulose is preferred. These cellulose-based resins may be used alone or in combination of two or more kinds.
[0026] The type and viscosity symbol of nitrocellulose, as defined by viscosity measurement according to JIS K 6703:1995, are preferably H1 / 8, H1 / 4, H1 / 2, H1, H2 or H20, more preferably H1 / 4, H1 / 2, H1, H2 or H20, and even more preferably H1 / 2, H1, H2 or H20. When the type and viscosity symbol of nitrocellulose (nitrocellulose) is higher than H1 / 8, the abrasion resistance, heat resistance and blocking resistance of the printed layer formed from the printing ink composition are likely to be improved. When the type and viscosity symbol of nitrocellulose is lower than H20, the stability of the printing ink composition, the adhesion of the printed layer to the substrate and the kneading resistance are likely to be improved. Note that when the type of nitrocellulose is L, the compatibility with the printing ink composition may decrease. That is, when the type of nitrocellulose is H, the compatibility with the printing ink composition is likely to be improved.
[0027] The types are defined according to the nitrogen content in the nitrocellulose. Nitrocellulose with a nitrogen content of 10.7% or more but less than 11.5% is classified as type L. Nitrocellulose, which has a nitrogen content between 11.5% and 12.2%, is classified as type H. The types and viscosity symbols are defined according to the time (fall time) it takes for a specified steel ball to fall between the marked lines in a nitrocellulose solution having a specified solid content concentration. In the case of nitrocellulose of the above type and viscosity symbol H1 / 8, the falling time of a steel ball in a nitrocellulose solution having a solid content concentration of 25 mass % is 1.6 to 2.9 seconds. In the case of nitrocellulose of the above type and viscosity symbol H1 / 4, the falling time of a steel ball in a nitrocellulose solution having a solid content concentration of 25 mass % is 3.0 to 8.9 seconds. In the case of nitrocellulose of the above type and viscosity symbol H1 / 2, the time it takes for a steel ball to fall into a nitrocellulose solution with a solid content of 20% by mass is 3.0 to 4.9 seconds, or the time it takes for a steel ball to fall into a nitrocellulose solution with a solid content of 25% by mass is 9.0 to 22.0 seconds. In the case of nitrocellulose of the above type and viscosity symbol H1, the falling time of a steel ball in a nitrocellulose solution having a solid content concentration of 20 mass % is 5.1 to 9.0 seconds. In the case of nitrocellulose of the above type and viscosity symbol H2, the time it takes for a steel ball to fall into a nitrocellulose solution with a solid content of 12.2% by mass is 1.5 to 2.5 seconds, or the time it takes for a steel ball to fall into a nitrocellulose solution with a solid content of 20% by mass is 15.0 to 40.0 seconds. In the case of nitrocellulose of the above type and viscosity symbol H20, the falling time of a steel ball in a nitrocellulose solution having a solid content concentration of 12.2 mass % is 16.0 to 24.0 seconds. These nitrocelluloses may be used alone or in combination of two or more kinds.
[0028] As the nitrocellulose, a commercially available product may be used. Commercially available nitrocellulose products include, for example, the "RS" series manufactured by Kimia.
[0029] (Fluorine-modified polyolefin resin) Examples of fluorine-modified polyolefin resins include resins obtained by polymerization of hydrocarbon monomers having ethylenic unsaturated bonds, in which at least a portion of hydrogen atoms are replaced with fluorine atoms. That is, examples of monomers for fluorine-modified polyolefin resins include fluorinated olefins and fluorinated compounds other than olefins having ethylenic unsaturated bonds. Examples of fluorinated olefins include, but are not limited to, tetrafluoroethylene, trifluoroethylene, 1,1-difluoroethylene, chlorotrifluoroethylene, and hexafluoropropylene. Examples of fluorinated compounds having ethylenic unsaturated bonds include resins in which at least a portion of hydrogen atoms are replaced with fluorine atoms in ethylenic hydrocarbons, vinyl ethers, and vinyl esters. Furthermore, in addition to these monomers, non-fluorine olefins and compounds other than olefins having ethylenic unsaturated bonds may be copolymerized.
[0030] The above-mentioned fluorinated olefins and fluorinated compounds other than the olefins having an ethylenically unsaturated bond may be used alone or in combination of two or more kinds. These fluorine-modified polyolefin resins may be used alone or in combination of two or more kinds.
[0031] As the fluorine-modified polyolefin resin, a commercially available product may be used. Commercially available fluorine-modified polyolefin resins include, for example, the "Lumiflon" series manufactured by AGC and the "Zeffle" series manufactured by Daikin Industries, Ltd.
[0032] <Aluminum fine particles (B)> The aluminum fine particles (B) function as a glittering pigment. The average particle diameter of the aluminum fine particles (B) is 5 to 20 μm, preferably 5.5 to 19 μm, and more preferably 6 to 18 μm. When the average particle diameter of the aluminum fine particles (B) is equal to or greater than the above lower limit, the transmission density of the resulting printed matter increases, and the hiding power tends to improve. When the average particle diameter of the aluminum fine particles (B) is equal to or less than the above upper limit, the adhesion of the resulting printed layer to the substrate tends to improve. The average particle size of the aluminum fine particles (B) is a cumulative 50% particle size on a volume basis measured by a laser diffraction / light scattering method.
[0033] The surface of the aluminum fine particles (B) is preferably treated with at least one selected from the group consisting of (meth)acrylic resin, fatty acid, and silica. That is, the surface of the aluminum fine particles (B) is preferably provided with a coating layer made of at least one selected from the group consisting of (meth)acrylic resin, fatty acid, and silica. By using such aluminum fine particles (B), a printing ink composition having excellent color development stability over time can be obtained. These aluminum fine particles (B) may be used alone or in combination of two or more.
[0034] The (meth)acrylic resin used for the surface treatment of the aluminum fine particles (B) is the same as the (meth)acrylic resin described above for the binder (A). These (meth)acrylic resins may be used alone or in combination of two or more.
[0035] The fatty acid used for the surface treatment of the aluminum fine particles (B) may be either a saturated fatty acid or an unsaturated fatty acid, and preferably has a carbon number of 12 to 22. Examples of the saturated fatty acid include lauric acid, myristic acid, palmitic acid, stearic acid, and arachidic acid. Examples of the unsaturated fatty acid include oleic acid, elaidic acid, linoleic acid, erucic acid, and ricinoleic acid. These fatty acids may be used alone or in combination of two or more.
[0036] The silica used for the surface treatment of the aluminum fine particles (B) may be either a natural product or a synthetic product, and the synthesis method may be either a dry method or a wet method. Examples of the dry method include the combustion method and the arc method, and examples of the wet method include the precipitation method and the gel method. In addition, the silica may be either crystalline or non-crystalline, and may be either hydrophobic or hydrophilic. These silicas may be used alone or in combination of two or more types.
[0037] <Rosin derivatives (C)> The inclusion of the rosin derivative (C) in the printing ink composition of the present embodiment tends to improve the redispersibility of the aluminum fine particles (B) in the printing ink composition, and also tends to promote detachment of the printed layer when the printed layer is detached with an alkaline solution or the like and the substrate is reused. Examples of the rosin derivative (C) include rosin-modified fumaric acid resin, rosin-modified maleic acid resin, rosin-modified phenolic resin, rosin ester, hydrogenated rosin, polymerized rosin, and terpene phenolic resin, and rosin-modified fumaric acid resin, rosin-modified maleic acid resin, and terpene phenolic resin are preferred. These rosin derivatives (C) may be used alone or in combination of two or more.
[0038] The acid value of the rosin derivative (C) is 20 mgKOH / g or more, preferably 20 to 330 mgKOH / g, more preferably 20 to 300 mgKOH / g, further preferably 22 to 250 mgKOH / g, and particularly preferably 25 to 220 mgKOH / g. When the acid value of the rosin derivative is equal to or more than the lower limit, the redispersibility of the aluminum fine particles (B) in the printing ink composition is likely to be improved. When the acid value of the rosin derivative is equal to or less than the upper limit, the stability of the printing ink composition is likely to be improved.
[0039] The softening point of the rosin derivative (C) is preferably 80 to 200° C., more preferably 85 to 190° C., and even more preferably 90 to 180° C. When the softening point of the rosin derivative (C) is equal to or higher than the above lower limit, the blocking resistance and heat resistance of the resulting printed layer are likely to be improved. When the softening point of the rosin derivative (C) is equal to or lower than the above upper limit, the adhesion of the resulting printed layer to the substrate is likely to be improved.
[0040] As the rosin derivative (C), a commercially available product may be used. Commercially available rosin derivatives (C) include, for example, the "Harimac" series, the "Hariphenol" series, the "Hariestar" series, and the "Haritac" series manufactured by Harima Chemical Industries, Ltd., the "Pine Crystal" series, the "Marquid" series, and the "Tamanol" series manufactured by Arakawa Chemical Industries, Ltd., and the "Foral" series manufactured by Eastman Chemical Company.
[0041] <Solvent (D)> The solvent may be one that dissolves or disperses each component contained in the printing ink composition. Examples of the solvent include ketone-based solvents, hydrocarbon-based solvents, ester-based solvents, ether-based solvents, glycol ether-based solvents, alcohol-based solvents, and water, and these may be used alone or in combination of two or more.
[0042] Examples of ketone-based solvents include acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone. Examples of hydrocarbon-based solvents include aromatic hydrocarbon-based solvents such as toluene and xylene; aliphatic hydrocarbon-based solvents such as n-hexane, n-heptane, and n-octane; and alicyclic hydrocarbon-based solvents such as cyclohexane, methylcyclohexane, and cyclooctane. Examples of ester-based solvents include methyl acetate, ethyl acetate, n-propyl acetate, n-butyl acetate, and isobutyl acetate. Examples of ether-based solvents include tetrahydrofuran, dioxane, diethyl ether, and methyl ethyl ether. Examples of glycol ether-based solvents include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, and propylene glycol monomethyl ether. Examples of alcohol-based solvents include monohydric alcohols such as methanol, ethanol, n-propanol, isopropanol, and n-butanol; and polyhydric alcohols such as ethylene glycol, propylene glycol, and glycerin.
[0043] <Optional ingredients> Examples of optional components include pigments, pigment derivatives, extender pigments, waxes, antiblocking agents, chlorinated polyolefins, fatty acid amides, chelating agents, curing agents, antisettling agents, UV absorbers, antioxidants, antistatic agents, leveling agents, thickeners, defoamers, plasticizers, dispersants, flame retardants, stabilizers, etc. These optional components may be used alone or in combination of two or more.
[0044] <Content of each ingredient> The solid content of the binder resin (A) is preferably from 55 to 82 mass %, more preferably from 56 to 82 mass %, and even more preferably from 57 to 82 mass %, based on the total mass of the solid contents of the printing ink composition. When the content of the binder resin (A) is equal to or more than the lower limit, the adhesion of the resulting printed layer to the substrate is likely to be improved. When the content of the binder resin (A) is equal to or less than the upper limit, the transmission density of the resulting printed matter is increased, and the hiding power is likely to be improved.
[0045] The solid content of the aluminum fine particles (B) is preferably 2 to 10 mass %, more preferably 2 to 9 mass %, further preferably 2 to 8 mass %, particularly preferably 3 to 8 mass %, based on the total mass of the printing ink composition. The solid content of the aluminum fine particles (B) is from 9 to 29 mass %, preferably from 10 to 25 mass %, and more preferably from 11 to 22 mass %, based on the total mass of the solid contents of the printing ink composition. When the content of the aluminum fine particles (B) is equal to or more than the lower limit, the transmission density of the resulting printed matter increases, and the hiding power is likely to be improved.When the content of the aluminum fine particles (B) is equal to or less than the upper limit, the adhesion of the resulting printed layer to the substrate is likely to be improved.
[0046] The solid content of the rosin derivative (C) is preferably from 1.5 to 10 mass %, more preferably from 2 to 9 mass %, and even more preferably from 3 to 8 mass %, based on the total mass of the solid contents of the printing ink composition. When the content of the rosin derivative is equal to or more than the above lower limit, the redispersibility is likely to be improved.When the content of the rosin derivative is equal to or less than the above upper limit, the blocking resistance and heat resistance of the resulting printed layer are likely to be improved.
[0047] The mass ratio of the solid content of the aluminum fine particles (B) to the solid content of the rosin derivative (C) is 1.43-10, preferably 1.59-10, more preferably 1.67-5, and even more preferably 1.82-5. When the mass ratio is equal to or greater than the above lower limit, the heat resistance of the resulting printed layer is likely to be improved.When the mass ratio is equal to or less than the above upper limit, the redispersibility of the aluminum fine particles (B) is likely to be improved.
[0048] The mass ratio of the solid content of the binder resin (A) to the solid content of the aluminum fine particles (B) is 2-9, preferably 2.5-8, and more preferably 3-7. When the mass ratio is equal to or greater than the lower limit, the adhesion of the resulting printed layer to the substrate is likely to be improved, whereas when the mass ratio is equal to or less than the upper limit, the transmission density of the resulting printed layer is increased, and the hiding power is likely to be improved.
[0049] The mass ratio of the solid content of the binder resin (A) to the solid content of the rosin derivative (C) is preferably 6-36, more preferably 6-33, and even more preferably 6-30.
[0050] The content of the solvent (D) is preferably 10 to 80 mass %, more preferably 15 to 70 mass %, and even more preferably 20 to 60 mass %, based on the total mass of the printing ink composition. When the content of the solvent (D) is equal to or more than the lower limit, the flowability of the printing ink composition is likely to be improved. When the content of the solvent (D) is equal to or less than the upper limit, the printability is likely to be improved.
[0051] The content of the optional components is not particularly limited as long as it is within a range that does not impair the effects of the present invention, but for example, it is preferably 0 to 10 mass % and more preferably 0 to 5 mass % relative to the total mass of the solid contents of the printing ink composition.
[0052] <Method for producing printing ink composition> The printing ink composition of this embodiment can be obtained, for example, by dissolving or dispersing the binder resin (A), aluminum fine particles (B), the rosin derivative (C), and optional components as necessary in the solvent (D). The method for mixing the components is not particularly limited, and the components can be mixed by various methods.
[0053] <Printing ink> The printing ink of the present embodiment contains the printing ink composition. It is preferable to appropriately add a solvent (D) and adjust the concentration of the binder resin (A), the aluminum fine particles (B), and the rosin derivative (C) according to the printing method used. The printing method is not particularly limited, and examples thereof include gravure printing, flexographic printing, offset printing, letterpress printing, and screen printing, and gravure printing is preferred.
[0054] <Uses of printing ink composition (printing ink)> The printing ink of this embodiment is suitable as a printing ink for printing on the surface of a substrate or on the surface of a color ink layer formed on the surface of a substrate by gravure printing, flexographic printing, offset printing, letterpress printing, screen printing, etc. In particular, it is suitable as a glitter ink for printing on the surface of a substrate or on the surface of a color ink layer formed on the surface of a substrate by gravure printing. That is, the printing ink composition of this embodiment is suitable for gravure printing.
[0055] When performing gravure printing, the printing ink is adjusted to an appropriate viscosity, and a measurement method using a Zahn cup is widely used for viscosity measurement. In general, the viscosity when performing gravure printing is preferably 10 to 25 seconds, more preferably 14 to 22 seconds, as measured with a Zahn cup #3 at 20°C. If the concentration is equal to or higher than the lower limit, swimming is unlikely to occur, whereas if the concentration is equal to or lower than the upper limit, transfer failure and leveling failure are unlikely to occur.
[0056] In this embodiment, the redispersibility of the aluminum fine particles (B) can be evaluated by the optical density (OD value) of a printed matter using the printing ink. The evaluation method can be the difference between the optical density of the printed layer before storage (OD value before storage) and the optical density of the printed layer after storage (OD value after storage), which is measured by the following measurement method.
[0057] The measurement method is explained below. A printing ink composition having a viscosity adjusted to 16 seconds at 25°C using a Zahn cup #3 was used as a dry mass of 2 g / m 2The optical density of a printed matter coated on a transparent PET film having a thickness of 20 μm so as to obtain a print having an OD value before storage is taken as the OD value before storage. The viscosity-adjusted printing ink composition is placed in a container, and the container is stored in a thermostatic chamber at 20° C. for one month. The container is then shaken, and the viscosity-adjusted printing ink composition after storage is adjusted to a dry mass of 2 g / m 2 The optical density of the printed matter coated on a 20 μm thick transparent PET film is taken as the OD value after storage. As an example of the shaking method, a method of shaking 20 times at a speed of 3 times / second with a shaking width of 20 cm is exemplified. Then, ΔOD=OD value before storage−OD value after storage is calculated.
[0058] ΔOD is preferably 0.40 or less, more preferably 0.25 or less, and even more preferably 0.20 or less. When ΔOD exceeds 0.40, it means that the hiding power is reduced. In other words, it means that the aluminum fine particles (B) are not well redispersed in the printing ink due to the occurrence of sedimentation or aggregation. In other words, when ΔOD is equal to or less than the upper limit, it means that the hiding power is improved. In other words, it means that the occurrence of sedimentation or aggregation is suppressed, and the aluminum fine particles (B) are well redispersed in the printing ink.
[0059] <Mechanism of action> The printing ink composition of the present invention contains a rosin derivative (C). The rosin derivative (C) having an oxidation rate of 20 mgKOH / g or more interacts with the surface of the aluminum fine particles (B), making the aluminum fine particles (B) less likely to aggregate. As a result, it is believed that the redispersibility of the aluminum fine particles (B) is improved. The printing ink composition of the present invention also contains aluminum fine particles (B) having an average particle size of 5 to 20 μm. It is believed that the inclusion of such aluminum fine particles increases the transmission density of the resulting printed matter and improves the hiding power. The printing ink composition of the present invention also contains the aluminum fine particles (B) in a content of 9 to 29 mass% relative to the total mass of the solid content of the printing ink composition, and the mass ratio of the binder resin (A) to the aluminum fine particles (B) is 2 to 9. By setting the content and mass ratio as described above, both the adhesion of the resulting printed layer to the substrate and the hiding power are improved ...1.43 to 10 to the rosin derivative (C). By using such a mass ratio, it is possible to improve both the heat resistance of the resulting printed layer and the redispersibility of the aluminum fine particles (B). From the above, it is considered that a printing ink composition can be obtained that has excellent redispersibility of the aluminum fine particles, and that has excellent adhesion to the substrate, hiding power, and heat resistance of the resulting printed layer.
[0060] <Laminate> An example of a laminate according to an embodiment of the present invention is shown in Figures 1 and 2. Note that the dimensional ratios in Figures 1 and 2 are different from the actual ones for the sake of convenience of explanation. The laminate 10 in FIG. 1 is a printed matter including a substrate 11 and a printed layer 12 provided on one surface of the substrate 11. The laminate 20 in Figure 2 is a printed matter comprising a substrate 21, a first printed layer 22 provided on one side of the substrate 21, and a second printed layer 23 provided on the side of the first printed layer opposite the substrate. When the laminate is attached to a packaging container as a label, it is preferable that the base materials 11, 21 are attached on the inside (the side in contact with the packaging container) of the printed layer 12 and the second printed layer 23, i.e., the printed layer 12 and the second printed layer 23 are attached on the outside.
[0061] <Base material> The type of the substrate 11, 21 can be appropriately selected according to the type of the laminate 10, 20, etc., and is not particularly limited, but is preferably a plastic substrate or a paper substrate. Examples of the plastic substrate include plastic substrates of polyolefin (e.g., polyethylene (PE), polypropylene (PP), etc.), polyester (e.g., polyethylene terephthalate (PET), etc.), polystyrene (PS), biaxially oriented polypropylene (OPP), unoriented polypropylene (CPP), polycarbonate (PC), polymethylmethacrylate (PMMA), polyamide (PA), polyimide (PI), cellophane, and fluorine-modified olefin (e.g., ethylene tetrafluoroethylene copolymer (ETFE), etc.). Substrates made of these materials may be used alone or in combination of two or more. At least one of the front surface (front side) and the back surface (back side) of the plastic substrate may be subjected to a surface treatment such as corona discharge treatment, plasma treatment, flame treatment, solvent treatment or the like, if necessary.
[0062] The substrates 11 and 21 may have a single layer structure or a laminated structure. That is, the substrates 11 and 21 may be a single layer film or a laminated film. When the substrates 11 and 21 are laminated films, they may be configured by laminating two or more films of the same type, or may be configured by laminating two or more films of different types. Examples of preferred film combinations include a combination in which a polyester film is on the front side of the substrates 11 and 21 and a polystyrene film or a polyolefin film is on the back side of the substrates 11 and 21, a cyclic polyolefin film is on the front side of the substrates 11 and 21, and a polyethylene film or a polypropylene film is on the back side of the substrates 11 and 21, and the like.
[0063] The thickness of the substrates 11 and 21 is preferably from 5 to 100 μm, more preferably from 12 to 60 μm, and further preferably from 12 to 50 μm.
[0064] <Printed layer, second printed layer> In the laminate 10, the printed layer 12 is provided on one surface of the substrate 11. In the laminate 20, the second printed layer 23 is provided on the surface opposite to the substrate 21 of the first printed layer 22 provided on one surface of the substrate 21. The printed layer 12 and the second printed layer 23 are printed layers (W) formed using the printing ink of the present embodiment described above. In the present invention, the printed layer 12, which is a printed layer (W) formed using a printing ink, is also referred to as the "printed layer (W)" and the second printed layer 23 is also referred to as the "second printed layer (W)." The thickness of the printed layer 12 and the second printed layer 23 is preferably 0.2 to 3.0 μm, more preferably 0.3 to 2.0 μm, and further preferably 0.3 to 1.5 μm.
[0065] <First printing layer> In the laminate 20 , the first printed layer 22 is provided on one surface of the substrate 21 . The first printed layer 22 is a printed layer (C) (hereinafter also referred to as "color printed layer (C)") formed using an ink composition for the purpose of imparting design, functionality, etc. to the laminate 20. The first printed layer 22 may have a single-layer structure or a laminated structure. The total thickness of the first printed layer 22 is preferably from 0.2 to 15 μm, more preferably from 0.3 to 10 μm, and even more preferably from 0.3 to 8 μm.
[0066] The ink composition used to form the first printed layer 22 contains a color pigment. The ink composition is preferably a printing ink composition. The printing ink composition is not particularly limited, and any known composition can be used. For example, the printing ink composition may include a composition containing a binder resin, a solvent, a coloring pigment, and, if necessary, other components. As the binder resin, any binder resin known in the art can be used. Examples of the solvent include the solvents exemplified above in the description of the printing ink composition of the present invention. Examples of color pigments include organic pigments such as azo pigments (monoazo, condensed azo, etc.), threne pigments (anthraquinone, perinone, perylene, thioindigo, etc.), phthalocyanine pigments (phthalocyanine blue, phthalocyanine green, etc.), quinacridone pigments, dioxazine pigments, isoindolinone pigments, pyrrolopyrrole pigments, aniline black, and organic fluorescent pigments; and inorganic pigments such as natural products (clay, etc.), ferrocyanides (princess blue, etc.), sulfides (zinc sulfide, etc.), sulfates, oxides (chromium oxide, zinc oxide, iron oxide, etc.), hydroxides (aluminum hydroxide, etc.), silicates (ultramarine, etc.), carbonates, carbon (carbon black, graphite, etc.), metal powders (aluminum powder, bronze powder, zinc powder, etc.), and calcined pigments. Examples of color pigments include the above-mentioned titanium oxide and precipitated barium sulfate. Examples of other components include waxes, dispersants, antifoaming agents, lubricants, pH adjusters, and thickeners.
[0067] <Method of manufacturing laminate> The method for producing the laminate 10 in FIG. 1 includes a step of forming a printed layer 12 on one surface of a substrate 11 using the printing ink of this embodiment. The manufacturing method of the laminate 20 in Figure 2 includes a step (1) of forming a first printed layer 22 on one side of a substrate 21 using an ink composition, and a step (2) of forming a second printed layer 23 on the side of the first printed layer 22 opposite the substrate 21 using the printing ink of this embodiment.
[0068] In the method for producing the laminate 10 in FIG. 1, for example, the printing ink of the present embodiment is applied onto one surface of the substrate 11 and dried to form the printed layer 12. Incidentally, after printing ink is applied onto one surface of the substrate 11 and dried to form the printed layer 12, further printing ink may be applied (overcoated).
[0069] The method for applying the printing ink is not particularly limited, and any known application method can be used, such as gravure printing, flexographic printing, brush coating, gravure coater method, die coater method, bar coater method, spray coating method, flow coating method, dip coating method, spin coating method, curtain coating method, etc. Among these, gravure printing is preferred because of its high quality and productivity.
[0070] The drying method is not particularly limited as long as it can remove the solvent contained in the printing ink applied onto one surface of the substrate 11, and examples thereof include reduced pressure drying, pressure drying, heat drying, and air drying. The heating temperature is preferably from 30 to 150°C, and more preferably from 40 to 120°C.
[0071] The method for producing the laminate 20 in FIG. 2 includes the above-mentioned steps (1) and (2) in this order. In step (1), for example, an ink composition is applied onto one surface of the substrate 21 and dried to form a first printed layer 22. In step (2), for example, the printing ink of the present embodiment is applied onto the surface of the first printed layer 22 opposite the substrate 21 and dried to form a second printed layer 23. The step (1) may be carried out once or twice or more, that is, the ink composition may be applied in multiple layers. Step (2) may be performed once or twice or more, i.e., the printing ink may be applied in multiple coats. As the coating method and drying method in steps (1) and (2), the same methods as those used in the production method of the laminate 10 can be applied.
[0072] <Application> The laminates 10 and 20 are preferably used as packaging materials such as soft packaging, and building materials. "Soft packaging" refers to packaging materials made of flexible materials, i.e., flexible packages, and is used for packaging food, daily necessities, etc. "Building materials" refers to plastic base materials used in the structures that make up buildings, and is used for decorating and protecting buildings (wall materials, roof materials, etc.).
[0073] <Other embodiments> The laminate is not limited to the above-described embodiment. For example, in the case of the laminate 10 shown in Fig. 1, the printed layer 12 is provided over the entirety of one surface of the substrate 11, but the printed layer 12 may be provided over a portion of one surface of the substrate 11. In this case, it is preferable that another printed layer is provided in the region of one surface of the substrate 11 where the printed layer 12 is not provided. Examples of the other printed layer include a layer formed from a varnish composition. Similarly, in the case of the laminate 20 shown in Fig. 2, the second printed layer 23 is provided on the entire one surface of the first printed layer 22, but the second printed layer 23 may be provided on a portion of one surface of the first printed layer 22. In this case, it is preferable that another printed layer is provided in the area on one surface of the first printed layer 22 where the second printed layer 23 is not provided. Examples of the other printed layer include a layer formed from a varnish composition.
[0074] 1, another printed layer may be provided on the surface of the printed layer 12 opposite the substrate 11. The other printed layer may be, for example, a layer formed from a varnish composition. Similarly, in the case of the laminate 20 shown in Fig. 2, another printed layer may be provided on the surface of the second printed layer 23 opposite to the first printed layer 22. The other printed layer may be, for example, a layer formed from a varnish composition. EXAMPLES
[0075] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples as long as it does not depart from the gist of the present invention.
[0076] [Raw materials used] As the binder resin (A), the compound shown below was used. A-1: Acrylic resin (manufactured by Taisei Fine Chemical Co., Ltd., product name "Acrit 1LO-846", weight average molecular weight 37,000, glass transition temperature 60°C). A-2: Polyamide resin (Kao Corporation, product name "Reomaid S-8200", weight average molecular weight 10,000, softening point 115℃, acid value 5mgKOH / g, amine value 3.5mgKOH / g). A-3: Nitrocellulose resin (manufactured by Kimia, product name "RS20", type and viscosity code H20). A-4: Fluorine-modified polyolefin resin (AGC Corporation, product name "Lumiflon LF200"). The above binder resin (A) was used after adjusting the solid content to 30 mass %.
[0077] As the aluminum fine particles (B), the following compound was used. B-1: Acrylic resin-coated aluminum microparticles (manufactured by Asahi Kasei Corporation, product name "TR2100", average particle size: 7 μm). B-2: Stearic acid-coated aluminum microparticles (manufactured by Toyo Aluminum Co., Ltd., product name "0700M", average particle size: 8 μm). B-3: Oleic acid-coated aluminum microparticles (manufactured by Toyo Aluminum Co., Ltd., product name "TD180T", average particle size: 16 μm). B-4: Silica-coated aluminum microparticles (manufactured by Toyo Aluminum, product name "EMR6390", average particle size: 8 μm). B-5: Oleic acid-coated aluminum microparticles (manufactured by Toyo Aluminum Co., Ltd., product name "2173", average particle size: 6 μm). B-6: Oleic acid-coated aluminum microparticles (manufactured by Toyo Aluminum Co., Ltd., product name "7620NS", average particle size: 18 μm). B-7: Oleic acid-coated aluminum microparticles (manufactured by Toyo Aluminum Co., Ltd., product name "HS-2", average particle size: 23 μm). The aluminum fine particles (B) were used after adjusting the solid content to 50% by mass.
[0078] As the rosin derivative (C), the compound shown below was used. C-1: Rosin modified fumaric acid resin (Harima Chemicals, product name "Harima AS-5", acid value 185-210mgKOH / g, softening point 160℃). · C-2: Rosin modified maleic acid resin (Harima Chemicals, product name "Haritac 4740", acid value 28mgKOH / g, softening point 120℃). · C-3: Terpene phenol resin (manufactured by Arakawa Chemical Industries, product name "Tamanol 803L", acid value 45-60 mg KOH / g, softening point 153°C). C-4: Hydrogenated rosin resin (manufactured by Arakawa Chemical Industries, product name "Pine Crystal KR-140", acid value 140 mg KOH / g, softening point 140°C). C-5: Rosin modified maleic acid resin (manufactured by Arakawa Chemical Industries, product name "Marukid NO33", acid value 290-320mgKOH / g, softening point 175℃). C-6: Rosin modified phenolic resin (manufactured by Arakawa Chemical Industries, product name "Tamanol 414", acid value 18 mg KOH / g, softening point 185°C).
[0079] As the solvent (D), the following compound was used. D-1: A mixture of ethyl acetate and isopropyl alcohol in a 1:1 mass ratio. D-2: A mixture of ethyl acetate, methylcyclohexane and isopropyl alcohol in a mass ratio of 2:2:1. ·D-3: Methyl ethyl ketone.
[0080] As optional components, the compounds shown below were used. Anti-blocking agent: Cellulose acetate butyrate (manufactured by Eastman Chemical, product name "CAB-381-0.5"). Wax: Polyolefin wax (manufactured by Polycon, product name "Polycon B-310").
[0081] [Evaluation method] (Evaluation of redispersibility) The optical density (OD value before storage) of the printed matter obtained in the examples and comparative examples was measured using a tabletop transmission densitometer 361T manufactured by X-Rite, Inc. The measurement was performed three times, and the average value was taken as the OD value before storage. In the examples and comparative examples, 100 g of printing ink adjusted to have a viscosity of 16 seconds at 25°C measured using Zahn cup #3 was placed in a cylindrical metal container and left to stand for 30 days in a thermostatic chamber at 20°C. After leaving to stand, the container was shaken back and forth by hand 20 times (shaking width: 20 cm, shaking speed: 3 times / second), and the obtained printing ink was printed on the treated surface of an OPP film (manufactured by Futamura Chemical Co., Ltd., product name "FOR", thickness: 25 μm) whose one side had been corona discharge-treated, using a gravure printing machine (manufactured by Matsuo Sangyo Co., Ltd., product name "K Printing Proofer") equipped with a gravure engraving plate with a mesh of 175 lines / inch (30 μm). The optical density (OD value after storage) of the obtained print was measured using a tabletop transmission densitometer 361T manufactured by X-Rite. The measurement was performed three times, and the average value was taken as the OD value after storage. Using the obtained OD value before storage and the OD value after storage, ΔOD was calculated according to the following formula 2. The smaller this value, the better the redispersibility. ΔOD = OD value before storage - OD value after storage Equation 2 The redispersibility was evaluated according to the following criteria. △ to ⊚ were considered to be acceptable. ◯ or ⊚ was more preferable. ◎: ΔOD is 0.15 or less. ◯: ΔOD is greater than 0.15 and less than 0.25. △: ΔOD is more than 0.25 and 0.40 or less. ×: ΔOD is more than 0.40.
[0082] (Evaluation of Adhesion) Cellophane tape (manufactured by Nichiban Co., Ltd.) was applied to the printed surface of the prints obtained in the Examples and Comparative Examples, and the applied Cellophane tape (registered trademark) was quickly peeled off in a direction that made an angle of 90 degrees with the printed surface. After peeling, the condition of the ink coating film remaining on the film of the prints was visually confirmed, and the adhesion was evaluated according to the following criteria. △ to ◎ were considered to be acceptable. ⊚: The printed layer did not peel off at all (peeling rate: 0%). ○: The peeling rate of the printed layer is more than 0% and less than 10%. △: The peeling rate of the printed layer is 10% or more and less than 20%. ×: The peeling rate of the printed layer is 20% or more.
[0083] (Evaluation of Concealment) The optical density (OD value) of the prints obtained in the examples and comparative examples was measured using a tabletop transmission densitometer 361T manufactured by X-Rite. The measurement was performed three times and the average value was calculated. The higher this value, the higher the hiding power. The hiding power was evaluated according to the following criteria. △ to ◎ were considered to be acceptable. ◎: OD value is 0.8 or more. ○: OD value is 0.6 or more and less than 0.8. △: OD value is 0.5 or more and less than 0.6. ×: Less than 0.5.
[0084] (Evaluation of heat resistance) The printed matter obtained in the Examples and Comparative Examples was dried for 10 seconds with a dryer immediately after printing, and then aluminum foil was placed on the surface of the printed layer (printed surface). A heat seal tester (manufactured by Tester Sangyo Co., Ltd., product name "TP-701-C Heat Seal Tester") was used to apply a pressure of 2 kg / cm 2 Heat sealing was performed for 1 second under a load of 1. The heat sealing temperature was in increments of 20° C. in the range of 80° C. to 160° C. After that, the aluminum foil was peeled off, and the heat resistance of the printed layer was evaluated according to the following evaluation criteria. ⊚: The printing layer did not transfer to the aluminum foil side at all. ◯: The percentage of the area of the printed layer transferred to the aluminum foil is more than 0% and less than 10%. △: The area ratio of the printed layer transferred to the aluminum foil is 10% or more and less than 20%. ×: The area ratio of the printed layer transferred to the aluminum foil is 20% or more.
[0085] <Overall rating> In the evaluations of redispersibility, adhesion, hiding power, and heat resistance, if there was one or more "x" it was judged to be "failed." In other words, if there was no "x" in the evaluations of redispersibility, adhesion, hiding power, and heat resistance, it was judged to be "passed." In addition to the evaluation of redispersibility, adhesion, hiding power, and heat resistance, the following evaluations of water resistance, blocking resistance, and detachment were also carried out. Water resistance, blocking resistance, and detachment are not directly related to the problem of the present application. A printing ink composition that does not receive a single "x" in the evaluations of redispersibility, adhesion, hiding power, and heat resistance and has high evaluation results for water resistance, blocking resistance, and detachment can be judged to be a printing ink composition with higher performance.
[0086] (Water resistance evaluation) The printed matter obtained in the Examples and Comparative Examples was placed in a sealed container together with tap water and left to stand in a thermostatic chamber at 40°C for 24 hours. The appearance of the printed layer was then evaluated by visual inspection, and the water resistance was evaluated according to the criteria shown below. ◎: No change was observed in the printed layer. ◯: Whitening is observed in part of the printed layer. Δ: Whitening or swelling was observed in multiple places on the printed layer.
[0087] (Evaluation of blocking resistance) The printed layer of the printed matter obtained in the examples and comparative examples was superimposed on the untreated side of a biaxially oriented polypropylene film (hereinafter referred to as "OPP film") that had not been printed, and a pressure of 4 kg / cm was applied to the back side of the printed matter. 2 The sample was stored for 24 hours in an environment of 40°C and 80% humidity with a load of 100 g / cm2 applied. After storage, the overlapping printed layers were peeled off, and the blocking resistance was evaluated according to the following criteria. ⊚: The printed layer is not transferred to the OPP film and there is no peeling resistance. ◯: More than 0% but less than 10% of the printed layer is transferred to the OPP film, and there is some peel resistance. △: 10% or more of the printed layer is transferred to the OPP film, and there is peeling resistance.
[0088] (Evaluation of detachment property) The printed matter obtained in the examples and comparative examples was placed in 1.5% by mass sodium hydroxide and stirred at 40° C. for 30 minutes, and the state of detachment of the printed layer was evaluated by visual observation and rated according to the following criteria: Note that releasability refers to the ease with which the printed layer is detached when the printed layer is detached with an alkaline solution and the substrate is reused. ⊚: 80% or more of the printed layer was peeled off. ◯: 50% or more and less than 80% of the printed layer peeled off. △: 10% or more but less than 50% of the printed layer peeled off. ×: Less than 10% of the printed layer was detached.
[0089] [Examples 1 to 19, Comparative Examples 1 to 7] <Preparation of printing ink composition> According to the formulations shown in Tables 1 to 4, the binder resin (A), aluminum fine particles (B), rosin derivative (C), solvent (D), and other optional components were mixed, and the resulting mixture was stirred for 30 minutes with a disperser to obtain a printing ink composition. The numbers in Tables 1 to 4 indicate the blending amounts including the volatile matter. A blank space means that the component was not blended (blended amount 0 parts by mass). "NV" indicates the solid content of each component.
[0090] <Creating printed matter> The prepared ink composition was diluted with the same solvent as used in the ink formulation so that the viscosity at 25°C measured using Zahn cup #3 was 16 seconds, to prepare a printing ink. Using a gravure printing machine (manufactured by Matsuo Sangyo Co., Ltd., product name "K Printing Proofer") equipped with a gravure engraving plate with a mesh of 175 lines / inch (30 μm), the prepared printing ink was applied to the treated surface of an OPP film (manufactured by Futamura Chemical Co., Ltd., product name "FOR", thickness: 25 μm) whose one side had been corona discharge-treated. Thereafter, hot air drying was performed at 80°C for 10 seconds to produce a printed matter. The obtained printed matter was used to evaluate redispersibility, adhesion, hiding power, and heat resistance. In addition, water resistance, blocking resistance, and detachment property were also evaluated. The results are shown in Tables 1 to 4.
[0091] [Table 1]
[0092] [Table 2]
[0093] [Table 3]
[0094] [Table 4]
[0095] As shown in Tables 1 to 3, the printed matter obtained from the printing ink composition of each Example was excellent in redispersibility, adhesion, hiding power, and heat resistance. That is, the printed matter obtained from the printing ink composition obtained in each Example had the four properties of redispersibility, adhesion, hiding power, and heat resistance.
[0096] As shown in Table 4, the printed matter obtained from the printing ink composition of Comparative Example 1, in which the content of aluminum fine particles (B) relative to the total mass of the solids of the printing ink composition was low and the mass ratio of the binder resin (A) to the aluminum fine particles (B) was high, had poor hiding power. On the other hand, the printed matter obtained from the printing ink composition of Comparative Example 2, in which the content of aluminum fine particles (B) relative to the total mass of the solids of the printing ink composition was high and the mass ratio of the binder resin (A) to the aluminum fine particles (B) was low, had poor adhesion.
[0097] The printed matter obtained from the printing ink composition of Comparative Example 3, in which the mass ratio of the aluminum fine particles (B) to the rosin derivative (C) was low, had poor heat resistance. On the other hand, the printed matter obtained from the printing ink composition of Comparative Example 4, in which the mass ratio of the aluminum fine particles (B) to the rosin derivative (C) was high, had poor redispersibility.
[0098] The printed matter obtained from the printing ink composition of Comparative Example 5, which contained aluminum fine particles (B) with a large average particle size, was poor in adhesion. The printed matter obtained from the printing ink composition of Comparative Example 6, which contained the rosin derivative (C) with a low acid value, was poor in redispersibility. Moreover, the printed matter obtained from the printing ink composition of Comparative Example 7, which did not contain the rosin derivative (C), was poor in redispersibility. [Industrial Applicability]
[0099] The printing ink composition of the present invention has excellent redispersibility of fine aluminum particles and is therefore particularly useful as an ink for gravure printing. [Explanation of symbols]
[0100] 10 Laminate 11 Base material 12 Printing layer (Printing layer (W)) 20 Laminate 21 Base material 22 First printing layer (color printing layer (C)) 23 Second printing layer (printing layer (W))
Claims
1. A printing ink composition comprising a binder resin (A) (excluding a rosin derivative (C)), aluminum fine particles (B), the rosin derivative (C), and a solvent (D), the binder resin (A) contains at least one selected from the group consisting of (meth)acrylic resins, polyamide resins, cellulose-based resins, and fluorine-modified polyolefin resins, the rosin derivative (C) comprises at least one selected from the group consisting of rosin-modified fumaric acid resin, rosin-modified maleic acid resin, rosin-modified phenolic resin, rosin ester, hydrogenated rosin, polymerized rosin, and terpene phenolic resin; the content of the aluminum fine particles (B) relative to the total mass of the solid content of the printing ink composition is 9 to 29 mass%, The average particle diameter of the aluminum fine particles (B) is 5 to 20 μm, The rosin derivative (C) has an acid value of 20 mgKOH / g or more, a mass ratio of the binder resin (A) to the aluminum fine particles (B) is 2 to 9; A printing ink composition, wherein a mass ratio of the aluminum fine particles (B) to the rosin derivative (C) is 1.43 to 10.
2. 2. The printing ink composition according to claim 1, wherein the surfaces of the aluminum fine particles (B) are treated with at least one selected from the group consisting of (meth)acrylic resins, fatty acids, and silica.
3. 2. The printing ink composition according to claim 1, wherein the rosin derivative (C) comprises at least one selected from the group consisting of a rosin modified fumaric acid resin, a rosin modified maleic acid resin, and a terpene phenol resin, and the rosin derivative (C) has an acid value of 250 mg KOH / g or less.
4. The printing ink composition according to claim 1, wherein the optical density of the printed layer before storage (OD value before storage) and the optical density of the printed layer after storage (OD value after storage), measured by the following measurement method, satisfy the following formula 1. OD value before storage−OD value after storage≦0.25 Equation 1 [Measurement method] The printing ink composition was adjusted to have a viscosity of 16 seconds at 25° C. using a Zahn cup #3. The viscosity-adjusted printing ink composition was then dried to a mass of 2 g / m 2 The optical density of a print coated on a transparent PET film having a thickness of 20 μm so as to satisfy the above condition is defined as the OD value before storage. The viscosity-adjusted printing ink composition was placed in a container, and the container was stored in a temperature-controlled room at 20° C. for one month. The container was then shaken, and the viscosity-adjusted printing ink composition after storage was adjusted to a dry mass of 2 g / m 2 The optical density of a print coated on a transparent PET film having a thickness of 20 μm so as to satisfy the above condition is taken as the OD value after storage.
5. A printing ink composition described in any one of claims 1 to 4, which is for gravure printing.
6. A laminate comprising a substrate and a printed layer formed on at least one surface of the substrate using the printing ink composition according to claim 5.
7. A packaging material comprising the laminate according to claim 6.
8. A building material comprising the laminate according to claim 6.
Citation Information
Patent Citations
Oil-base ink composition for ballpoint
JP2002309148A
Metallic pigment composition, and UV metallic ink composition or UV metallic coating material composition using the same
JP2005272568A
Water-in-oil type emulsion ink for stencil printing
JP2018162421A
Ink composition for lithographic printing
WO2018139582A1
Rotogravure ink for surface printing, and printed matter using the same
JP2020059806A