Plastic film and laminate tube containers
The laminated tube container design with a specific resin film structure addresses slipperiness and rigidity issues, enhancing productivity and reducing environmental impact through the use of biomass-derived materials.
Patent Information
- Application Number
- JP2023156425
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-09-21
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2039-08-21
AI Technical Summary
Laminated tube containers using biomass-derived resin compositions face issues with slipperiness, rigidity, and productivity due to fluctuations in feed speed and sealing properties, leading to environmental load concerns and surface scratches.
A laminated tube container design with a resin film structure comprising a first layer of fossil fuel-derived polyethylene, a second layer of biomass-derived linear low-density polyethylene, and optionally a third layer of fossil fuel-derived polyethylene, with specific density and thickness ratios to achieve a stiffness parameter between 3.5 and 6.5, enhancing slipperiness and rigidity while reducing environmental impact.
The proposed resin film structure improves slipperiness, rigidity, and productivity of laminated tube containers, while significantly reducing environmental load by utilizing biomass-derived materials effectively.
Smart Images

Figure 0007594745000004 
Figure 0007594745000005 
Figure 0007594745000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin film and a laminated tube container including the same. [Background technology]
[0002] In recent years, with the growing demand for the creation of a recycling-oriented society, there is a desire to move away from fossil fuels in the materials field, just as there is in energy, and the use of biomass has attracted attention. Biomass is an organic compound that is photosynthesized from carbon dioxide and water, and by using it, it becomes carbon dioxide and water again, making it a so-called carbon-neutral renewable energy. Recently, the practical application of biomass plastics made from these biomass raw materials has progressed rapidly, and attempts are being made to produce various resins from biomass raw materials.
[0003] As a biomass-derived resin, polylactic acid (PLA), which is produced via lactic acid fermentation, was the first to be commercially produced, but since its performance as a plastic differs significantly from current general-purpose plastics, including its biodegradability, there are limitations to its product applications and manufacturing methods, and it has not yet become widely used.In addition, a life cycle assessment (LCA) is being conducted on PLA, and discussions are being held on the energy consumption during PLA production and its equivalence when replacing general-purpose plastics.
[0004] Here, various types of general-purpose plastics are used, such as polyethylene, polypropylene, polyvinyl chloride, polystyrene, and polyester. In particular, polyethylene is molded into films, sheets, bottles, and the like, and is used in various applications such as packaging materials, and is used in large quantities around the world. Therefore, using conventional polyethylene derived from fossil fuels places a large burden on the environment. For this reason, it is desirable to use raw materials derived from biomass in the production of polyethylene to reduce the amount of fossil fuel used. For example, research has been conducted to date on the production of ethylene and butylene, which are raw materials for polyolefin resins, from renewable natural raw materials (see Patent Document 1).
[0005] On the other hand, it is known that packaging bags using a biomass-derived resin composition as a raw material are significantly inferior in processability and cannot improve productivity compared to those using a fossil fuel-derived resin composition. To solve this problem, Cited Document 2 proposes a film having a multilayer structure in which a biomass-derived resin composition is used as an intermediate layer and fossil fuel-derived polyethylene resin is used as an outer layer and an inner layer. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Special Publication No. 2011-506628 [Patent Document 2] Patent No. 5799520 Summary of the Invention [Problem to be solved by the invention]
[0007] In the laminated tube container, a sealant layer is provided on both the inside and outside of the laminate constituting the container in order to form a welded part by welding (laminating) the body part and forming a cylindrical container. The present inventors manufactured a laminated tube container using a resin film having an intermediate layer made of a biomass-derived resin and two layers made of a fossil fuel-derived polyethylene resin on both sides of the intermediate layer as a sealant layer of the laminate. When the inventors manufactured a laminated tube container using the resin film as a sealant layer of the laminate, they found that when the laminate was bonded into a cylindrical shape, the slipperiness between the laminate and the metal cylinder (mandrel) along which the laminate was aligned deteriorated, causing the feed speed of the laminate to fluctuate, making the sealing of the welded part unstable, and when the laminated tube containers were fed into the container when filling the contents, the slipperiness between the laminated tube containers deteriorated, causing the container to become clogged, and scratches were generated on the surface of the laminated tube container, resulting in a decrease in productivity. Furthermore, the inventors discovered that when the thickness of the above-mentioned resin film of the laminated tube container was reduced in order to further reduce the environmental impact, the body portion of the laminated tube container bent, making it difficult to hold the laminated tube container upside down. As a result of extensive research, the inventors have found that the above-mentioned problems can be solved by setting the density and stiffness parameter values between each layer within specific ranges. The present invention is based on this finding.
[0008] Therefore, an object of the present invention is to provide a laminated tube container having a resin film that can improve the reduction in environmental impact and can also improve the slipperiness and rigidity. [Means for solving the problem]
[0009] The present invention relates to a head portion including a shoulder portion and a spout portion, a torso portion connected to the shoulder portion of the head; A laminated tube container comprising: The body portion is composed of a laminate having at least an outer sealant layer, a base material layer, and an inner sealant layer in this order; the inner sealant layer comprises a resin film having at least a first layer and a second layer; the first layer constitutes at least one outermost layer of the resin film; The first layer and the second layer are directly laminated to each other, The first layer is made of a polyethylene resin derived from a fossil fuel, The second layer is made of a resin containing linear low-density polyethylene derived from biomass, the density of the second layer is less than the density of the first layer; The density difference between the second layer and the first layer is 0.003 g / cm 3 That's all. The resin film has a stiffness parameter (K) of 3.5 or more and 6.5 or less, as determined by the following formula: K=ρ40 ×t ρ: Density of resin film t: resin film thickness
[0010] In one embodiment, the resin film further comprises a third layer on the opposite side to the first layer, the third layer constitutes the other outermost layer of the resin film, the second layer and the third layer are laminated directly or via a thermoplastic resin layer, The third layer is preferably made of a polyethylene resin derived from fossil fuels.
[0011] In one embodiment, the biomass degree of the resin film is preferably 1% or more and 80% or less.
[0012] In one embodiment, the outer sealant layer comprises the resin film, The first layer of the resin film of the outer sealant layer is preferably located on the outermost surface of the body portion. Effect of the Invention
[0013] According to the present invention, it is possible to provide a laminated tube container having a resin film that can improve the environmental load reduction properties and also improve the slipperiness and rigidity. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a cross-sectional view showing an example of a resin film of the present invention. [Diagram 2] FIG. 1 is a cross-sectional view showing an example of a resin film of the present invention. [Diagram 3] FIG. 1 is a cross-sectional view showing an example of a resin film of the present invention. [Figure 4] FIG. 1 is a diagram showing an example of a laminated tube container of the present invention. [Diagram 5] This is a cross-sectional view taken along line A-A in Figure 4. [Figure 6]FIG. 2 is a partial cross-sectional view showing an example of the configuration of a laminate that forms a body portion of a tube container. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] <Resin film> The resin film of the present invention includes at least a first layer and a second layer, and the first layer and the second layer are directly laminated. The resin film may further include a third layer, and the second layer and the third layer may be laminated directly or via a thermoplastic resin layer. The resin film of the present invention will be described with reference to the drawings.
[0016] 1 is a cross-sectional view showing an example of a resin film 10 of the present invention. The resin film 10 includes a first layer 11 and a second layer 12. The first layer 11 constitutes one of the outermost layers of the resin film 10. The first layer 11 and the second layer 12 are directly laminated together.
[0017] 2 is a cross-sectional view showing another example of the resin film 10 of the present invention. The resin film 10 is provided with a first layer 11, a second layer 12, and a third layer 13, in that order. The first layer 11 constitutes one of the outermost layers of the resin film 10. The third layer 13 constitutes the other outermost layer of the resin film 10. The first layer 11 and the second layer 12 are directly laminated to each other. The second layer 12 and the third layer 13 are directly laminated to each other.
[0018] 3 is a cross-sectional view showing another example of the resin film 10 of the present invention. The resin film 10 is provided with a first layer 11, a second layer 12, a thermoplastic resin layer 14, and a third layer 13, in that order. The first layer 11 constitutes one of the outermost layers of the resin film 10. The third layer 13 constitutes the other outermost layer of the resin film 10. The first layer 11 and the second layer 12 are directly laminated. The second layer 12 and the third layer 13 are laminated with the thermoplastic resin layer 14 interposed therebetween.
[0019] It is also possible to appropriately combine a plurality of layer structures of the resin film 10 shown in the above-mentioned Figs. 1 to 3.
[0020] The resin film of the present invention is characterized in that the stiffness parameter (K) of the resin film is 3.5 or more and 6.5 or less. By setting the stiffness parameter to 3.5 or more, the resin film can have excellent stiffness. By setting the stiffness parameter to 6.5 or less, the resin film can have excellent environmental load reduction properties. The stiffness parameter is more preferably 3.7 or more and 6.2 or less, and even more preferably 4.0 or more and 6.0 or less. In the present invention, the stiffness parameter (K) is defined by the following formula: K=ρ 40 ×t ρ: Density of resin film t: resin film thickness The density (ρ) of the resin film is expressed in units of g / cm 3 The values for the resin film density are rounded off to the fourth decimal place.
[0021] The thickness of the resin film is preferably 15 μm or more and 150 μm or less. By making the thickness of the resin film 15 μm or more, the rigidity and seal strength of the resin film can be further improved, and when a laminate is formed with other layers, interlayer peeling can be further suppressed. By making the thickness of the resin film 150 μm or less, the environmental load reduction and productivity of the resin film can be further improved. It is more preferable that the thickness is 40 μm or more and 140 μm or less, and even more preferable that the thickness is 70 μm or more and 130 μm or less.
[0022] The rigidity of the resin film is preferably 60 mN / 20 mm or more, and more preferably 80 mN / 20 mm or more. The rigidity of the resin film is measured by the following method.
[0023] A test piece is prepared by cutting the specimen into a strip having a long side and a short side. Then, both ends of the long side of the test piece are fixed with a chuck and curved into a loop. The loop is then compressed from the outside so that the distance between the indenter and the chuck is a specified distance. The resistance to the compression is recorded as the loop stiffness. In this embodiment, the length of the short side of the strip is 20 mm, and the length of the long side is 130 mm. The loop length is 60 mm, and the distance between the indenter and the chuck is 15 mm. At this time, the compression speed is 3.3 mm / s, and the holding time is 3 seconds. As a stiffness tester for measuring stiffness, for example, a loop stiffness tester manufactured by Toyo Seiki Seisakusho can be used.
[0024] In the resin film of the present invention, the static friction coefficient (μ S ) is preferably 1.00 or less, more preferably 0.70 or less, and even more preferably 0.40 or less, and the dynamic friction coefficient (μ D ) is preferably 1.00 or less, more preferably 0.70 or less, and even more preferably 0.40 or less. Static friction coefficient between resin films (μ S ) and the dynamic friction coefficient (μ D The measurement of the adhesion strength is performed between the first layer surfaces of two resin films in accordance with JIS K-7125. A TR-2 manufactured by Toyo Seiki Seisakusho Co., Ltd. can be used as the measuring device.
[0025] In the resin film of the present invention, the static friction coefficient (μ S ) is preferably 0.40 or less, more preferably 0.30 or less, and even more preferably 0.25 or less, and the dynamic friction coefficient (μ D ) is preferably 0.40 or less, more preferably 0.30 or less, and even more preferably 0.25 or less. Static friction coefficient of resin film against metal (μ S ) and the dynamic friction coefficient (μ DThe measurement of the adhesion strength is performed on the first layer surface of the resin film and on the metal surface in accordance with JIS K-7125. A TR-2 manufactured by Toyo Seiki Seisakusho Co., Ltd. can be used as the measuring device.
[0026] The density of the resin film is 0.910g / cm 3 More than 0.950g / cm 3 The density of the resin film is preferably 0.910 g / cm or less. 3 By setting the density of the resin film to 0.950 g / cm or more, the rigidity of the resin film can be further improved. 3 By setting the density of the resin film at 0.915 g / cm or more, the seal strength can be further improved. 3 More than 0.945g / cm 3 More preferably, it is 0.920 g / cm or less. 3 More than 0.940g / cm 3 It is even more preferable that: The density of the resin film is a value measured according to the method A of JIS K7112-1980 after annealing as described in JIS K6760-1995.
[0027] The resin film of the present invention preferably has a biomass degree, which will be described below, of 1% or more and 80% or less. By setting the biomass degree to 1% or more, it is possible to improve the reduction of the environmental load. By setting the biomass degree to 80% or less, it is possible to improve the rigidity and productivity of the resin film. The biomass degree is more preferably 5% or more and 70% or less, and even more preferably 10% or more and 60% or less. Unless otherwise specified, the "biomass degree" refers to the weight ratio of biomass-derived components.
[0028] (1st layer) The first layer constitutes at least one of the outermost layers of the resin film and is made of fossil fuel-derived polyethylene resin. This can improve the slipperiness of the resin film surface. Fossil fuel-derived polyethylene resin is a polyethylene resin produced only from raw materials derived from fossil fuel, and the concentration of biomass-derived ethylene in fossil fuel-derived polyethylene resin is 0%. Therefore, the biomass degree of fossil fuel-derived polyethylene resin is 0%.
[0029] The density of the first layer is 0.910g / cm 3 More than 0.960g / cm 3 The density of the first layer is preferably 0.910 g / cm or less. 3 By setting the density of the first layer at 0.960 g / cm or more, the rigidity of the resin film and the slipperiness of the surface of the resin film can be further improved. 3 The seal strength can be further improved by making the density of the first layer 0.915 g / cm 3 More than 0.955g / cm 3 More preferably, it is 0.920 g / cm or less. 3 More than 0.950g / cm 3 It is even more preferable that: The density of the first layer is a value measured according to the method specified in Method A of JIS K7112-1980 after annealing as specified in JIS K6760-1995.
[0030] The thickness of the first layer is preferably 5 μm or more and 100 μm or less. By making the first thickness 5 μm or more, the rigidity and seal strength of the resin film can be further improved, and the slipperiness of the resin film surface can be further improved. By making the first thickness 100 μm or less, the environmental load reduction and the productivity of the resin film can be further improved. The thickness of the first layer is more preferably 10 μm or more and 80 μm or less, and further preferably 15 μm or more and 50 μm or less.
[0031] The thickness ratio of the first layer:the second layer is preferably 1:5 to 2:1, and more preferably 1:4 to 1:1.
[0032] The polyethylene resin constituting the first layer may contain one or more of high density polyethylene (HDPE), medium density polyethylene (MDPE), low density polyethylene (LDPE), and linear low density polyethylene (LLDPE) described later, within the scope of the present invention. 3 Medium density polyethylene means polyethylene having a density of 0.930 g / cm or more. 3 More than 0.942g / cm 3 Low density polyethylene and linear low density polyethylene mean polyethylene having a density of less than 0.930 g / cm 3 By "polyethylene" is meant polyethylene having a density less than 1000 MPa.
[0033] The polyethylene resin constituting the first layer preferably has a melt flow rate (MFR) of 0.1 g / 10 min to 10 g / 10 min, more preferably 0.2 g / 10 min to 5 g / 10 min, and even more preferably 0.5 g / 10 min to 3 g / 10 min. By making the MFR 0.1 g / 10 min or more, the extrusion load during molding can be reduced. By making the MFR 10 g / 10 min or less, the mechanical strength of the resin film can be increased. The melt flow rate is a value measured by Method A under conditions of a temperature of 190° C. and a load of 21.18 N in accordance with the method specified in JIS K7210-1995.
[0034] As long as the properties of the present invention are not impaired, the first layer may contain one or more additives, such as antioxidants, antiblocking agents, lubricants, fillers, plasticizers, antistatic agents, UV absorbers, inorganic particles, organic particles, release agents, and dispersants.
[0035] (2nd layer) The second layer is made of a resin containing linear low-density polyethylene derived from biomass, which can reduce the environmental impact and improve the seal strength and impact resistance, such as drop strength, of the resin film.
[0036] The second layer preferably has a biomass degree of 5% or more and 95% or less, as described below. By making the biomass degree 5% or more, it is possible to improve the reduction of the environmental load. By making the biomass degree 95% or less, it is possible to improve the rigidity and productivity of the resin film. The biomass degree is more preferably 10% or more and 90% or less, and further preferably 15% or more and 80% or less.
[0037] The method for producing biomass-derived ethylene, which is a raw material for biomass-derived polyethylene (hereinafter also referred to as biomass polyethylene), is not particularly limited, and it can be obtained by a conventionally known method. An example of the method for producing biomass-derived ethylene will be described below.
[0038] Biomass-derived ethylene can be produced using biomass-derived ethanol as a raw material. In particular, it is preferable to use biomass-derived fermented ethanol obtained from a plant raw material. The plant raw material is not particularly limited, and any conventionally known plant can be used. Examples of the plant raw material include corn, sugarcane, beet, and manioc.
[0039] Fermented ethanol derived from biomass refers to ethanol produced by contacting a culture solution containing a carbon source obtained from a plant raw material with an ethanol-producing microorganism or a product derived from the crushed microorganism, and then purifying the ethanol. Conventionally known methods such as distillation, membrane separation, and extraction can be applied to purify ethanol from the culture solution. For example, there is a method of adding benzene, cyclohexane, etc., and removing water by azeotropy or membrane separation.
[0040] In order to obtain the above ethylene, the ethanol may be further subjected to advanced purification at this stage, for example, so that the total amount of impurities in the ethanol is reduced to 1 ppm or less.
[0041] A catalyst is usually used when obtaining ethylene by the dehydration reaction of ethanol, but the catalyst is not particularly limited and any conventionally known catalyst can be used. From the viewpoint of the process, a fixed bed flow reaction is advantageous because it is easy to separate the catalyst from the product, and for example, γ-alumina is preferable.
[0042] This dehydration reaction is an endothermic reaction, and is therefore usually carried out under heating conditions. As long as the reaction proceeds at a commercially useful reaction rate, the heating temperature is not limited, but is preferably 100° C. or higher, more preferably 250° C. or higher, and even more preferably 300° C. or higher. There is no particular upper limit, but from the viewpoint of energy balance and equipment, it is preferably 500° C. or lower, more preferably 400° C. or lower.
[0043] In the dehydration reaction of ethanol, the yield of the reaction depends on the amount of water contained in the ethanol supplied as a raw material. In general, when performing a dehydration reaction, it is preferable to have no water in consideration of the efficiency of removing water. However, in the case of the dehydration reaction of ethanol using a solid catalyst, it has been found that the amount of other olefins, especially butene, produced tends to increase if water is not present. It is presumed that this is because ethylene dimerization after dehydration cannot be suppressed if a small amount of water is not present. The lower limit of the allowable water content is 0.1% by mass or more, preferably 0.5% by mass or more. The upper limit is not particularly limited, but from the viewpoint of material balance and heat balance, it is preferably 50% by mass or less, more preferably 30% by mass or less, and even more preferably 20% by mass or less.
[0044] By carrying out the dehydration reaction of ethanol in this manner, a mixture of ethylene, water, and a small amount of unreacted ethanol is obtained, but since ethylene is in a gaseous state at room temperature under about 5 MPa or less, water and ethanol can be removed from the mixture by gas-liquid separation to obtain ethylene. This method may be performed by a known method.
[0045] The ethylene obtained by the gas-liquid separation is further distilled. The distillation method, operation temperature, residence time, etc. are not particularly limited, except that the operation pressure at this time is normal pressure or higher.
[0046] When the raw material is biomass-derived ethanol, the obtained ethylene contains trace amounts of carbonyl compounds such as ketones, aldehydes, and esters, which are impurities mixed in during the ethanol fermentation process, as well as carbon dioxide gas, which is a decomposition product thereof, and nitrogen-containing compounds such as amines and amino acids, which are enzyme decomposition products and impurities, as well as ammonia, which is a decomposition product thereof. Depending on the use of ethylene, these trace amounts of impurities may be problematic, so they may be removed by purification. The purification method is not particularly limited, and can be performed by a conventionally known method. An example of a suitable purification operation is an adsorption purification method. The adsorbent used is not particularly limited, and a conventionally known adsorbent can be used. For example, a material with a high surface area is preferable, and the type of adsorbent is selected according to the type and amount of impurities in the ethylene obtained by the dehydration reaction of biomass-derived ethanol.
[0047] In addition, a caustic water treatment may be used in combination as a method for purifying impurities in ethylene. When caustic water treatment is used, it is preferable to carry out the treatment before adsorption purification. In that case, it is necessary to carry out a water removal treatment after the caustic treatment and before the adsorption purification.
[0048] Biomass polyethylene is obtained by polymerizing monomers containing ethylene derived from biomass. It is preferable to use the ethylene derived from biomass obtained by the above-mentioned production method. Since ethylene derived from biomass is used as the raw material monomer, the polymerized polyethylene is derived from biomass. When the biomass polyethylene is a low-density polyethylene derived from biomass, it is polyethylene polymerized by the above-mentioned polymerization method using ethylene derived from biomass. Note that the raw material monomer for polyethylene does not have to contain 100% by mass of ethylene derived from biomass.
[0049] As long as the object of the present invention is not impaired, the monomer that is the raw material of the biomass polyethylene may further contain ethylene derived from a fossil fuel.
[0050] The biomass-derived ethylene concentration in the polyethylene (hereinafter sometimes referred to as "biomass degree") is a value measured by measuring the amount of biomass-derived carbon by radiocarbon (C14) measurement. Carbon dioxide in the atmosphere contains a certain proportion of C14 (105.5 pMC), and it is known that the C14 content in plants that grow by absorbing carbon dioxide from the atmosphere, such as corn, is also about 105.5 pMC. It is also known that fossil fuels contain very little C14. Therefore, by measuring the proportion of C14 in the total carbon atoms in the polyethylene, the proportion of biomass-derived carbon can be calculated, and the weight ratio of the biomass-derived component can be obtained.
[0051] In the present invention, theoretically, if all ethylene derived from biomass is used as the raw material for polyethylene, the concentration of biomass-derived ethylene will be 100%, and the biomass content of the biomass polyethylene will be 100%.
[0052] In the present invention, the biomass polyethylene or the biomass-derived resin layer does not need to have a biomass content of 100%. This is because if even a part of the resin film is made of biomass-derived raw materials, it is in line with the purpose of the present invention, which is to reduce the amount of fossil fuel used compared to conventional methods.
[0053] Resin film made from fossil fuel-derived polyethylene resin theoretically emits 5.03 kg-CO2e / kg of carbon dioxide per kg during the processes of procuring raw materials, manufacturing the film, and disposing of it. In the case of a film made from biomass-derived polyethylene resin with a biomass content of 100%, it theoretically emits 0.41 kg-CO2e / kg of carbon dioxide. Therefore, theoretically, it is possible to reduce carbon dioxide by 0.46 kg-CO2e / kg per 10% biomass content. Note that "CO2e" stands for CO2 equivalent, and is a value converted into carbon dioxide. Furthermore, film manufacturing was calculated assuming film production using the inflation method, and disposal was calculated assuming 100% incineration.
[0054] Here, linear low-density polyethylene will be described. Linear low-density polyethylene is a copolymer of ethylene and an α-olefin polymerized using a multi-site catalyst such as a Ziegler-Natta catalyst or a single-site catalyst such as a metallocene catalyst. Therefore, it is a high-pressure ethylene homopolymer, and is distinguished from low-density polyethylene that can be obtained by a conventionally known high-pressure radical polymerization method. It has a density of 0.930 g / cm 3 It refers to one having a density of less than 1000 nm. Examples of α-olefins that serve as comonomers for linear low-density polyethylene include α-olefins having 3 to 20 carbon atoms, such as propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-nonene, 4-methylpentene, and mixtures thereof. Here, the density of polyethylene is a value measured according to the method specified in Method A of JIS K7112-1980 after annealing as described in JIS K6760-1995.
[0055] The single-site catalyst is a catalyst capable of forming a uniform active species, and is usually prepared by contacting a metallocene transition metal compound or a nonmetallocene transition metal compound with an activating cocatalyst. Compared with a multi-site catalyst, a single-site catalyst is preferred because it has a uniform active site structure and can polymerize a polymer with a high molecular weight and a highly uniform structure. As the single-site catalyst, it is particularly preferred to use a metallocene catalyst. The metallocene catalyst is a catalyst containing each catalyst component of a transition metal compound of Group IV of the periodic table containing a ligand having a cyclopentadienyl skeleton, a cocatalyst, and if necessary, an organometallic compound and a carrier.
[0056] In the above-mentioned transition metal compound of Group IV of the periodic table containing a ligand having a cyclopentadienyl skeleton, the cyclopentadienyl skeleton is a cyclopentadienyl group, a substituted cyclopentadienyl group, etc. The substituted cyclopentadienyl group has at least one substituent selected from a hydrocarbon group having 1 to 30 carbon atoms, a silyl group, a silyl-substituted alkyl group, a silyl-substituted aryl group, a cyano group, a cyanoalkyl group, a cyanoaryl group, a halogen group, a haloalkyl group, a halosilyl group, etc. The substituted cyclopentadienyl group may have two or more substituents, and the substituents may be bonded to each other to form a ring, such as an indenyl ring, a fluorenyl ring, an azulenyl ring, or a hydrogenated product thereof. The rings formed by bonding the substituents to each other may further have substituents.
[0057] In the transition metal compound of Group IV of the periodic table containing a ligand having a cyclopentadienyl skeleton, the transition metal may be zirconium, titanium, hafnium, etc., and zirconium and hafnium are particularly preferred. The transition metal compound usually has two ligands having a cyclopentadienyl skeleton, and it is preferred that the ligands having each cyclopentadienyl skeleton are bonded to each other by a bridging group. The bridging group may be an alkylene group having 1 to 4 carbon atoms, a silylene group, a substituted silylene group such as a dialkylsilylene group or a diarylsilylene group, or a substituted germylene group such as a dialkylgermylene group or a diarylgermylene group. The substituted silylene group is preferred.
[0058] In the transition metal compound of Group IV of the periodic table, representative ligands other than those having a cyclopentadienyl skeleton include hydrogen, hydrocarbon groups having 1 to 20 carbon atoms (such as alkyl groups, alkenyl groups, aryl groups, alkylaryl groups, aralkyl groups, and polyenyl groups), halogens, metaalkyl groups, and metaaryl groups.
[0059] The above-mentioned compounds of transition metals of Group IV of the periodic table containing a ligand having a cyclopentadienyl skeleton can be used as the catalyst component either alone or in combination of two or more kinds.
[0060] The co-catalyst refers to a catalyst that can effectively use the above-mentioned transition metal compound of Group IV of the periodic table as a polymerization catalyst or balance the ionic charge in a catalytically activated state. Examples of the co-catalyst include benzene-soluble aluminoxanes of organoaluminum oxy compounds and benzene-insoluble organoaluminum oxy compounds, ion-exchangeable layered silicates, boron compounds, ionic compounds consisting of cations containing or not containing active hydrogen groups and non-coordinating anions, lanthanoid salts such as lanthanum oxide, tin oxide, and phenoxy compounds containing a fluoro group.
[0061] The transition metal compound of Group IV of the periodic table containing a ligand having a cyclopentadienyl skeleton may be used supported on an inorganic or organic carrier, preferably an inorganic or organic porous oxide, and specific examples of the carrier include ion-exchangeable layered silicates such as montmorillonite, SiO2, Al2O3, MgO, ZrO2, TiO2, B2O3, CaO, ZnO, BaO, ThO2, and mixtures thereof.
[0062] Furthermore, examples of organometallic compounds that may be used as necessary include organoaluminum compounds, organomagnesium compounds, organozinc compounds, etc. Of these, organoaluminum compounds are preferably used.
[0063] In the resin film of the present invention, the density of the second layer is smaller than that of the first layer. This makes it possible to suppress low molecular weight components contained in the biomass-derived resin of the second layer from precipitating on the surface of the resin film, thereby improving the slipperiness of the resin film surface. The low molecular weight components refer to components having a molecular weight of 30,000 or less.
[0064] In the resin film of the present invention, the density difference between the second layer and the first layer is 0.001 g / cm 3 It is preferable that the density difference between the second layer and the first layer is 0.003 g / cm or more. This can further improve the slipperiness of the resin film surface. 3 More preferably, it is 0.005 g / cm or more. 3 More preferably, it is equal to or greater than this.
[0065] The density of the second layer is 0.901g / cm 3 More than 0.950g / cm 3 It is preferable that the following is true: 2 The layer density is 0.901 g / cm 3 By setting the thickness to the above, the rigidity of the resin film can be further improved. 2 The layer density is 0.950g / cm 3 The seal strength can be further improved by the following. 2The layer density is 0.905g / cm 3 More than 0.945g / cm 3 More preferably, it is 0.910 g / cm or less. 3 More than 0.940g / cm 3 It is even more preferable that:
[0066] No. 2 The thickness of the layer is preferably 10 μm or more and 150 μm or less. 2 layers By making the thickness 10 μm or more, the rigidity and seal strength of the resin film can be further improved, and the slipperiness of the surface of the resin film can be further improved. 2 layers By setting the thickness to 150 μm or less, the productivity of the resin film can be further improved. 2 The thickness of the layer is more preferably 15 μm or more and 120 μm or less, and further preferably 20 μm or more and 100 μm or less.
[0067] The resin constituting the second layer may contain one or more of high density polyethylene (HDPE), medium density polyethylene (MDPE), and low density polyethylene (LDPE) within the scope of the present invention, and these may be derived from fossil fuels or biomass. Furthermore, the resin constituting the second layer may contain linear low density polyethylene derived from fossil fuels within the scope of the present invention.
[0068] As long as the properties of the present invention are not impaired, the second layer may contain one or two types of additives, such as antioxidants, antiblocking agents, lubricants, fillers, plasticizers, antistatic agents, UV absorbers, inorganic particles, organic particles, release agents, and dispersants.
[0069] The resin constituting the second layer preferably has a melt flow rate (MFR) of 0.1 g / 10 min to 10 g / 10 min, more preferably 0.2 g / 10 min to 5 g / 10 min, and even more preferably 0.5 g / 10 min to 3 g / 10 min. By making the MFR 0.1 g / 10 min or more, the extrusion load during molding can be reduced. By making the MFR 10 g / 10 min or less, the mechanical strength of the resin film can be increased.
[0070] (3rd layer) The third layer constitutes the other outermost layer of the resin film and is made of fossil fuel-derived polyethylene resin, which improves adhesion to other layers when forming a laminate with other layers.
[0071] The density of the third layer is 0.910g / cm 3 More than 0.960g / cm 3 The density of the third layer is preferably 0.910 g / cm or less. 3 By setting the density of the third layer at 0.960 g / cm or more, the rigidity of the resin film can be further improved. 3 The seal strength can be further improved by making the density of the third layer 0.915 g / cm 3 More than 0.955g / cm 3 More preferably, it is 0.920 g / cm or less. 3 More than 0.950g / cm 3 It is even more preferable that:
[0072] The thickness of the third layer is preferably 5 μm or more and 100 μm or less. By making the third thickness 5 μm or more, the rigidity and seal strength of the resin film can be further improved. By making the third thickness 100 μm or less, the environmental load reduction and the productivity of the resin film can be further improved. The thickness of the third layer is more preferably 10 μm or more and 80 μm or less, and further preferably 15 μm or more and 50 μm or less.
[0073] The thickness ratio of the third layer:the second layer is preferably 1:5 to 2:1, and more preferably 1:4 to 1:1.
[0074] The polyethylene resin constituting the third layer may contain one or more of high density polyethylene, medium density polyethylene, low density polyethylene, linear low density polyethylene, etc., within the scope of the invention.
[0075] The polyethylene resin constituting the third layer preferably has a melt flow rate (MFR) of 0.1 g / 10 min to 10 g / 10 min, more preferably 0.2 g / 10 min to 5 g / 10 min, and even more preferably 0.5 g / 10 min to 3 g / 10 min. By making the MFR 0.1 g / 10 min or more, the extrusion load during molding can be reduced. By making the MFR 10 g / 10 min or less, the mechanical strength of the resin film can be increased.
[0076] As long as the properties of the present invention are not impaired, the third layer may contain one or more additives, such as antioxidants, antiblocking agents, lubricants, fillers, plasticizers, antistatic agents, UV absorbers, inorganic particles, organic particles, release agents, and dispersants.
[0077] (thermoplastic resin layer) The thermoplastic resin layer is a layer formed to bond any two layers together by lamination. The thermoplastic resin layer can be formed by a conventionally known method, for example, a melt extrusion lamination method or a sand lamination method. The material of the thermoplastic resin layer can be a polyolefin resin such as a polyethylene resin or a polypropylene resin, a cyclic polyolefin resin, or a copolymer resin, a modified resin, or a mixture (including an alloy) containing these resins as the main component. Examples of polyolefin resins include low-density polyethylene, medium-density polyethylene, high-density polyethylene, linear low-density polyethylene, polypropylene (PP), ethylene-α-olefin copolymers polymerized using a metallocene catalyst, random or block copolymers of ethylene-polypropylene, ethylene-vinyl acetate copolymers (EVA), ethylene-acrylic acid copolymers (EAA), ethylene-ethyl acrylate copolymers (EEA), ethylene-methacrylic acid copolymers (EMAA), ethylene-methyl methacrylate copolymers (EMMA), ethylene-maleic acid copolymers, ionomer resins, and acid-modified polyolefin resins obtained by modifying the above-mentioned polyolefin resins with unsaturated carboxylic acids such as acrylic acid, methacrylic acid, maleic acid, maleic anhydride, fumaric acid, and itaconic acid in order to improve adhesion between layers. In addition, resins obtained by graft-polymerizing or copolymerizing unsaturated carboxylic acids, unsaturated carboxylic anhydrides, and ester monomers with polyolefin resins can be used. These materials can be used alone or in combination of two or more. Examples of the cyclic polyolefin resin include cyclic polyolefins such as ethylene-propylene copolymers, polymethylpentene, polybutene, and polynorbornene. These resins can be used alone or in combination of two or more. The thermoplastic resin layer may contain a material derived from biomass or a material derived from fossil fuels.
[0078] <Method of manufacturing resin film> The method for producing the resin film of the present invention is not particularly limited, and can be produced by a conventionally known method. The resin film is preferably produced by co-extrusion molding, and the co-extrusion molding is more preferably carried out by a T-die method or an inflation method. Hereinafter, an example of the method for producing the resin film by the T-die method and the inflation method will be described.
[0079] In the T-die method, the resin constituting the first layer and the resin constituting the second layer are each dried, and then supplied to a melt extruder heated to a temperature (Tm) above their respective melting points to a temperature of Tm+70°C to melt them and co-extrude them into a sheet from a T-die. The co-extruded sheet is then quenched and solidified on a rotating cooling drum or the like to form a resin film. As the melt extruder, a single screw extruder, a twin screw extruder, a vent extruder, a tandem extruder, etc. can be used depending on the purpose.
[0080] In the inflation method, the resin constituting the first layer and the resin constituting the second layer are first dried and then fed to a melt extruder heated to a temperature (Tm) to Tm+70° C. above their melting points, and then co-extruded into a cylindrical shape through an annular die. At this time, air is fed from below into the cylindrical molten resin to expand the diameter of the cylinder to a predetermined size, and cooling air is fed from below to the outside of the cylinder. This expanded cylindrical body is called a bubble. Next, the bubble is folded into a film shape by a guide plate and a pinch roll, and wound up in a winding section. The folded film may be wound up as it is in a cylindrical shape, or both ends of the cylinder may be removed by a slitter or the like, cut into two films, and then each may be wound up. In this way, a resin film can be formed. As the melt extruder, a single screw extruder, a twin screw extruder, a vent extruder, a tandem extruder, etc. can be used depending on the purpose.
[0081] <Laminated tube container> The laminated tube container according to the present invention will be described with reference to the drawings. Fig. 4 is a diagram showing an example of the laminated tube container according to the present invention, and Fig. 5 is a cross-sectional view taken along line A-A in Fig. 4. As shown in Fig. 4, the tube container 20 has a head portion 21 and a body portion 22.
[0082] [head] The head 21 is composed of a shoulder 23 connected to one end of the body and a pouring outlet 24 connected to the shoulder, and can be integrally formed from a resin composition by a molding method such as compression molding or injection molding. The resin composition used for the head 21 of the tube container will be described below.
[0083] (Resin composition) The resin composition used to mold the head may contain polyolefin as a main component. Examples of polyolefin include polyethylene, polypropylene, and copolymers containing these, among which polyethylene is preferred. Examples of polyethylene include high-density polyethylene, medium-density polyethylene, low-density polyethylene, and linear low-density polyethylene described below, among which high-density polyethylene is preferred. In addition, when polyethylene is used as the polyolefin, biomass-derived polyethylene resin may be used instead of fossil fuel-derived polyethylene resin.
[0084] In the above-mentioned resin composition production process or to the produced resin composition, one or more additives may be added in addition to the main component polyolefin, so long as the properties of the composition are not impaired. Examples of additives include plasticizers, ultraviolet stabilizers, color inhibitors, matting agents, deodorants, flame retardants, weather resistance agents, antistatic agents, thread friction reducers, slip agents, mold release agents, antioxidants, ion exchange agents, and color pigments. These additives are added in an amount of preferably 1 to 20% by mass, and preferably 1 to 10% by mass, based on the total resin composition.
[0085] The method for producing the head is not particularly limited, and the head can be produced by a conventionally known method. The head can be molded and joined to the body by a compression molding method, an injection molding method, or the like.
[0086] [Torso] The body 22 is connected to the shoulder 23 of the head 21. The body 22 is formed by rolling the laminate into a cylindrical shape, overlapping both ends, and welding the overlapped parts to form a welded part 26, thereby forming a cylindrical container. Fig. 6 is a partial cross-sectional view of a laminate 30 forming the body 22 of the tube container 20. As shown in Fig. 6, the laminate film 30 forming the body 22 includes an outer sealant layer 31, a base layer 32, and an inner sealant layer 33, and is configured by laminating the outer sealant layer 31, the base layer 32, and the inner sealant layer 33 in this order from the outer surface side to the inner surface side of the body 22.
[0087] (Outer sealant layer, inner sealant layer) 6, the outer sealant layer 31 and the inner sealant layer 33 are provided on both sides of the base layer 32. The outer sealant layer and the inner sealant layer are layers formed of a heat-sealable resin film that can be fused to each other by heat. In the body of the laminated tube container of the present invention, the outer sealant layer or the inner sealant layer comprises the resin film of the present invention. When the outer sealant layer comprises the resin film of the present invention, the first layer of the resin film is located on the outermost surface of the body of the laminated tube container, and when the inner sealant layer comprises the resin film of the present invention, the first layer of the resin film is located on the innermost surface of the body of the laminated tube container. This can improve the environmental load reduction and can provide a laminated tube container with excellent slip properties and rigidity. In addition, the productivity of the laminated tube container can be improved. In the body of the laminated tube container of the present invention, both the outer sealant layer and the inner sealant layer preferably comprise the resin film of the present invention, and the first layer of the resin film of the outer sealant layer is located on the outermost surface of the body, and the first layer of the resin film of the inner sealant layer is located on the innermost surface of the body.
[0088] The outer sealant layer and the inner sealant layer may be layers formed using polyolefin resins such as polyethylene resins and polypropylene resins, or cyclic polyolefin resins, or copolymer resins, modified resins, or mixtures (including alloys) mainly composed of these resins. Examples of polyolefin resins include low-density polyethylene, medium-density polyethylene, high-density polyethylene, linear low-density polyethylene, polypropylene (PP), ethylene-α-olefin copolymers polymerized using a metallocene catalyst, random or block copolymers of ethylene-polypropylene, ethylene-vinyl acetate copolymers (EVA), ethylene-acrylic acid copolymers (EAA), ethylene-ethyl acrylate copolymers (EEA), ethylene-methacrylic acid copolymers (EMAA), ethylene-methyl methacrylate copolymers (EMMA), ethylene-maleic acid copolymers, ionomer resins, and acid-modified polyolefin resins obtained by modifying the above-mentioned polyolefin resins with unsaturated carboxylic acids such as acrylic acid, methacrylic acid, maleic acid, maleic anhydride, fumaric acid, and itaconic acid in order to improve adhesion between layers. In addition, resins obtained by graft-polymerizing or copolymerizing unsaturated carboxylic acids, unsaturated carboxylic anhydrides, and ester monomers with polyolefin resins can be used. These materials can be used alone or in combination of two or more. Examples of cyclic polyolefin resins that can be used include cyclic polyolefins such as ethylene-propylene copolymers, polymethylpentene, polybutene, and polynorbornene. These resins can be used alone or in combination of two or more. The inner sealant layer may contain a material derived from biomass or a material derived from fossil fuels.
[0089] The outer sealant layer and the inner sealant layer may be two or more layers. When the outer sealant layer is two or more layers, each layer may have the same composition or different compositions.
[0090] (base material layer) The base layer has a function of supporting the laminate constituting the body, and can be made of any material capable of supporting the laminate without any particular limitation. For example, polyester-based resins such as polyethylene terephthalate resin and polyethylene naphthalate resin, polyvinyl alcohol-based resins, saponified ethylene-vinyl acetate copolymer (EVOH), polyamide-based resins, polypropylene resins, polyolefin-based resins such as polyethylene resins, and other resins, and paper can be used. In addition, the above-mentioned resins may be not only fossil fuel-derived resins, but also biomass-derived resins. For example, in addition to the above-mentioned biomass-derived polyethylene resins, biomass polyesters using biomass-derived ethylene glycol as a diol component as described in JP 2012-116082 A, polylactic acid resins, starch, cellulose, and the like can be used.
[0091] The substrate layer may be two or more layers. When the substrate layer is two or more layers, each layer may have the same composition or different compositions.
[0092] The base layer may be a film made of the above-mentioned resin, but it is preferable to use a film stretched in a uniaxial or biaxial direction from the viewpoint of strength, etc. Hereinafter, the film made of the resin in the body of the laminated tube container of the present invention is also referred to as the base film.
[0093] The base layer may contain additives such as fillers, plasticizers, antistatic agents, UV absorbers, inorganic particles, organic particles, release agents, and dispersants, as long as the additives do not impair the properties of the present invention.
[0094] (Other layers) The laminate may have at least one other layer in addition to the outer sealant layer, the base layer, and the inner sealant layer. Examples of the other layer include a gas barrier layer, a light-shielding layer, and a print layer. When the laminate has two or more other layers, they may have the same composition or different compositions.
[0095] The gas barrier layer may be made of a resin, and examples of the resins that can be used include polyester resins such as polyethylene terephthalate resin and polyethylene naphthalate resin, polyvinylidene chloride resin, polyvinyl alcohol resin, saponified ethylene-vinyl acetate copolymer, fluorine resin, and polyacrylonitrile resin. Examples of the resins that can be used as water vapor barriers include olefin resins such as low-density polyethylene resin, medium-density polyethylene resin, high-density polyethylene resin, linear low-density polyethylene resin, and polypropylene resin. The gas barrier layer may be made of a film made of the above-mentioned resin, but from the viewpoint of strength, it is preferable to use a film that is oriented in a uniaxial or biaxial direction.
[0096] As the gas barrier layer, a metal foil such as aluminum foil may be provided, or one or more layers of a vapor deposition layer of an inorganic material such as aluminum, or a vapor deposition layer of an inorganic oxide may be provided. When a metal foil or a vapor deposition layer is provided on the surface of the base film, the surface of the base film may be previously subjected to a plasma treatment using an inert gas. Such a surface treatment improves the adhesion between the base film and the metal foil or vapor deposition layer, and prevents delamination.
[0097] The vapor-deposited film may be, for example, a vapor-deposited film of one or more inorganic substances or inorganic oxides such as silicon (Si), aluminum (Al), magnesium (Mg), calcium (Ca), potassium (K), tin (Sn), sodium (Na), boron (B), titanium (Ti), lead (Pb), zirconium (Zr), and yttrium (Y).
[0098] The method for forming a vapor-deposited layer of the inorganic substance or inorganic oxide on one side of the resin film may be a known method such as vacuum deposition, sputtering, or chemical vapor deposition.
[0099] The thickness of the vapor-deposited layer of the inorganic substance or inorganic oxide is about 100 Å to 2000 Å, preferably about 200 Å to 1000 Å.
[0100] In order to improve the gas barrier properties of the gas barrier layer, a vapor deposition layer of an inorganic substance or an inorganic oxide as described above may be provided on the base film, and then a gas barrier coating film may be provided on the vapor deposition layer. 1 n M(OR 2 ) m (In the formula, R 1 , R 2 represents an organic group having 1 to 8 carbon atoms, M represents a metal atom, n represents an integer of 0 or more, m represents an integer of 1 or more, and n+m represents the valence of M. and a polyvinyl alcohol resin and / or an ethylene-vinyl alcohol copolymer, and further comprising a step of preparing a gas barrier composition which is polycondensed by a sol-gel method in the presence of a sol-gel catalyst, an acid, water, and an organic solvent; a step of applying the gas barrier composition which is polycondensed by a sol-gel method onto a vapor deposition layer provided on one side of a base film, via a plasma-treated surface with oxygen gas, to provide a coating film; and a step of heat-treating the base film provided with the coating film at 20°C to 180°C and at a temperature not higher than the melting point of the base film for 10 seconds to 10 minutes to form a gas barrier coating film of the gas barrier composition onto the vapor deposition layer provided on one side of the base film, via a plasma-treated surface with oxygen gas, if necessary.
[0101] The general formula R for forming a gas barrier coating film 1 n M(OR 2 ) mAs the alkoxide represented by the formula (I), at least one of a partial hydrolyzate of an alkoxide and a hydrolysis condensate of an alkoxide can be used. In addition, as the partial hydrolyzate of an alkoxide, it is not necessary that all of the alkoxy groups are hydrolyzed, and one in which one or more alkoxy groups are hydrolyzed, or a mixture thereof may be used. Furthermore, as the hydrolysis condensate, a dimer or more of a partially hydrolyzed alkoxide, specifically a dimer to hexamer, is used.
[0102] The above general formula R 1 n M(OR 2 ) m In the alkoxide represented by the formula (I), silicon, zirconium, titanium, aluminum, and the like can be used as the metal atom represented by M. In the present invention, preferred metals include, for example, silicon and titanium. In the present invention, the alkoxide can be used alone or in the form of a mixture of two or more different metal atoms in the same solution.
[0103] In addition, the above general formula R 1 n M(OR 2 ) m In the alkoxide represented by the formula: 1 Specific examples of the organic group represented by the general formula R include alkyl groups such as methyl, ethyl, n-propyl, i-propyl, n-butyl, i-butyl, sec-butyl, t-butyl, n-hexyl, and n-octyl. 1 n M(OR 2 ) m In the alkoxide represented by the formula: 2 Specific examples of the organic group represented by the formula (I) include a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, a sec-butyl group, etc. In the present invention, these alkyl groups may be the same or different in the same molecule.
[0104] As the polyvinyl alcohol resin and / or ethylene-vinyl alcohol copolymer forming the above-mentioned gas barrier coating film, a polyvinyl alcohol resin or an ethylene-vinyl alcohol copolymer can be used alone, or a polyvinyl alcohol resin and an ethylene-vinyl alcohol copolymer can be used in combination. In the present invention, by using a polyvinyl alcohol resin and / or an ethylene-vinyl alcohol copolymer, the gas barrier coating film can be significantly improved in physical properties such as gas barrier properties, water resistance, weather resistance, etc. In particular, by using a polyvinyl alcohol resin and an ethylene-vinyl alcohol copolymer in combination in the present invention, a laminate film can be formed that is significantly excellent in hot water resistance and gas barrier properties after hot water treatment in addition to the above-mentioned gas barrier properties.
[0105] The light-shielding layer can be formed from a resin composition in which a black pigment, a white pigment, etc. are added to a base resin. As the base resin, an olefin resin such as a low-density polyethylene resin, a medium-density polyethylene resin, a high-density polyethylene resin, a linear low-density polyethylene resin, or a polypropylene resin can be used.
[0106] The black pigment used is a black pigment that absorbs light mainly in the near ultraviolet to visible range. Specifically, in addition to carbon black, graphite, iron black, and electrically conductive materials (polyaniline, polypyrrole) can be used.
[0107] As the white pigment, a white pigment that is beautiful and easy to design is added, taking into consideration the appearance design. Specifically, in addition to titanium oxide, calcium carbonate, zinc oxide, barium sulfate, etc. can be used.
[0108] The printed layer may be provided, for example, on the outer sealant layer, the base layer, and / or the gas barrier layer. The printed layer may be a layer on which any desired printed pattern such as letters, pictures, figures, symbols, patterns, etc. is formed for decoration, display of contents, display of expiration date, display of manufacturer, distributor, etc., etc. The printed layer may also be a layer that is given glossiness using gloss varnish (OP varnish) or the like. As the gloss varnish, poly(meth)acrylic resin, (meth)acrylic-styrene copolymer, polyurethane resin, vinyl chloride-vinyl acetate copolymer, chlorinated polypropylene resin, etc. can be used. The printed layer may be provided over the entire surface or only part of the surface, and may be two or more layers. The printing layer can be formed by, for example, gravure printing, offset printing, letterpress printing, flexographic printing, or silk screen printing.
[0109] The outer sealant layer, the base material layer, the inner sealant layer and other layers can be laminated to one another via an adhesive layer by dry lamination, or via an adhesive resin layer by melt extrusion lamination or sand lamination.
[0110] The adhesive layer can be formed by applying an adhesive used for lamination (laminating adhesive) to the surface of the layer to be laminated and drying it. As the laminating adhesive, for example, one-component or two-component curing or non-curing type vinyl, (meth)acrylic, polyamide, polyester, polyether, polyurethane, epoxy, rubber, and other solvent-based, water-based, or emulsion-based adhesives can be used. As a coating method for the laminating adhesive, for example, the direct gravure roll coating method, gravure roll coating method, kiss coating method, reverse roll coating method, Fountain method, transfer roll coating method, and other methods can be used to apply the adhesive to the coating surface of the layer constituting the laminated film. The amount of application is 0.1 g / m 2 ~10g / m 2 (dry state) is preferred, 1 g / m 2 ~5g / m2 (Dry state) is more preferred.
[0111] The adhesive resin layer is formed by a melt extrusion lamination method using a thermoplastic resin. The thermoplastic resin usable for the adhesive resin layer may be a polyolefin resin such as a polyethylene resin or a polypropylene resin, a cyclic polyolefin resin, or a copolymer resin, modified resin, or mixture (including alloy) containing these resins as main components. Examples of polyolefin resins include low-density polyethylene, medium-density polyethylene, high-density polyethylene, linear low-density polyethylene, polypropylene (PP), ethylene-α-olefin copolymers polymerized using a metallocene catalyst, random or block copolymers of ethylene-polypropylene, ethylene-vinyl acetate copolymers (EVA), ethylene-acrylic acid copolymers (EAA), ethylene-ethyl acrylate copolymers (EEA), ethylene-methacrylic acid copolymers (EMAA), ethylene-methyl methacrylate copolymers (EMMA), ethylene-maleic acid copolymers, ionomer resins, and acid-modified polyolefin resins obtained by modifying the above-mentioned polyolefin resins with unsaturated carboxylic acids such as acrylic acid, methacrylic acid, maleic acid, maleic anhydride, fumaric acid, and itaconic acid in order to improve adhesion between layers. In addition, resins obtained by graft-polymerizing or copolymerizing unsaturated carboxylic acids, unsaturated carboxylic anhydrides, and ester monomers with polyolefin resins can be used. These materials can be used alone or in combination of two or more. Examples of the cyclic polyolefin resin include cyclic polyolefins such as ethylene-propylene copolymers, polymethylpentene, polybutene, and polynorbornene. These resins can be used alone or in combination of two or more. The adhesive resin layer may contain a material derived from biomass or a material derived from fossil fuels.
[0112] An anchor coat layer may also be formed to improve the adhesion of the adhesive resin layer. The anchor coat layer can be formed by applying an anchor coat agent to the surface of the layer to be laminated and drying it. The anchor coat agent may be any resin having a heat resistance temperature of 135°C or higher, such as a vinyl modified resin, an epoxy resin, a urethane resin, or a polyester resin, and is particularly preferably an anchor coat agent consisting of a polyacrylic or polymethacrylic resin having two or more hydroxyl groups in the structure and an isocyanate compound as a curing agent. A silane coupling agent may also be used as an additive, and nitrocellulose may also be used in combination to improve heat resistance.
[0113] The laminate constituting the body portion can have various layer configurations depending on the type of contents to be filled and packaged, the purpose of packaging, the packaging form, the distribution form, the sales form, and other conditions. Examples of the layer configuration of the laminate include the following. PE film / adhesive layer / PET / printed layer / adhesive layer / PE film PE film / adhesive layer / EVOH / printing layer / adhesive layer / PE film PE film / adhesive layer / PET / vapor deposition layer / gas barrier coating film / printed layer / adhesive layer / PE film PE film / adhesive layer / PET / vapor deposition layer / gas barrier coating film / printed layer / adhesive layer / CPP PE film / adhesive layer / PET / vapor deposition layer / gas barrier coating / printed layer / adhesive layer / milky PE film PE film / adhesive layer / gas barrier coating film / vapor deposition layer / PET / printed layer / adhesive layer / milky PE film PE film / adhesive layer / PET / printed layer / adhesive layer / gas barrier coating / vapor deposition layer / PET / adhesive layer / PE film PE film / adhesive layer / PET / printed layer / adhesive layer / vapor deposition layer / PET / adhesive layer / PE film PE film / adhesive layer / PET / printed layer / adhesive layer / AL / adhesive layer / PE film PE film / adhesive layer / PET / printed layer / adhesive layer / AL / adhesive layer / PET / adhesive layer / PE film PE film / adhesive layer / PET / printed layer / adhesive layer / AL / PE / PE film / PE / adhesive layer / PE film PE film / PE / AC / PET / printed layer / AC / PE / milky PE film / AC / EMAA / AL / EMAA / PE film PE film / adhesive layer / PET / printed layer / adhesive layer / vapor deposition layer / PET / EAA / AL / EAA / PE film PE film / adhesive layer / printing layer / PE / EAA / AL / EAA / PET / adhesive layer / PE film PE film / PE / printed layer / paper / EMAA / vapor deposition layer / PET / AC / PE / PE film PE film / PE / printed layer / paper / EMAA / AL / EMAA / PE film PE / printed layer / paper / EMAA / AL / EMAA / PE film PE / printed layer / paper / EMAA / vapor deposition layer / PET / AC / PE / PE film Printing layer / PE / PE film / EMAA / AL / EMAA / PE film Printing layer / PE / PE film / EAA / AL / EAA / PET / adhesive layer / PE film Printing layer / PE / PE film / PE / AC / PET / printing layer / AC / PE / milky PE film / AC / EMAA / AL / EMAA / PE film Printing layer / PE / PE film / PE / PET / printing layer / adhesive layer / vapor deposition layer / PET / adhesive layer / PE film Printing layer / PE / milky PE film / PE / PE film Printing layer / PE / PE film / adhesive layer / EVOH / adhesive layer / PE film Printing layer / PE film / adhesive layer / PET / vapor deposition layer / gas barrier coating film / adhesive layer / PE film Printing layer / PE / PE film / PE / AC / PET / printing layer / adhesive layer / vapor deposition layer / PET / adhesive layer / PE film Printing layer / PE film / adhesive layer / deposition layer / PE film / PE / EVOH / PE / PE film In the above example of layer structure, the left side means the outside of the body, and the right side means the inside of the body. The symbol " / " indicates the boundary between layers, and each layer can be laminated by dry lamination, sand lamination, or melt extrusion lamination as described above. In the above example of layer structure, the resin film of the present invention can be used for "PE film". The names of other abbreviations are as follows. PE: polyethylene, PET: polyethylene terephthalate, AL: aluminum foil, CPP: unstretched polypropylene, EVOH: saponified ethylene-vinyl acetate copolymer, EMAA: ethylene-methacrylic acid copolymer, EAA: ethylene-acrylic acid copolymer, AC: anchor coat layer.
[0114] The body is produced by rolling the laminate into a cylindrical shape, overlapping the outer sealant layer and the inner sealant layer at both ends of the body, and heat-sealing the overlapped portion to form a welded portion. The head is connected to the top of one of the openings of the body. Alternatively, the laminate may not be overlapped, but the ends of the laminate may be butted together and welded, and at least the inner surface of the butted portion may be covered with a plastic sealing tape to form a cylinder.
[0115] Heat sealing can be performed by a conventional method such as bar sealing, rotary roll sealing, belt sealing, impulse sealing, high frequency sealing, ultrasonic sealing, flame sealing, or the like.
[0116] <Manufacturing method of laminated tube containers> The method for producing the laminated tube container is not particularly limited, and the laminated tube container can be produced by a conventionally known method. An example of a method for producing the laminated tube container 20 will be described with reference to FIG. 4. The resin composition containing the biomass raw material is used as a molding raw material, and a milky white pigment and other desired additives are added to the resin composition and thoroughly kneaded to produce a resin composition. The resin composition is used to form a head 21 at one opening of the cylindrical body 22 by, for example, a compression molding method, an injection molding method, or other ordinary molding method. This allows the laminated tube container 20 consisting of the head 21 and the body 22 to be molded.
[0117] When the laminated tube container 20 is molded using a compression molding method, the body 22 is attached to a male mold having a convex portion at the top, the male mold and the female mold are opposed to each other, molten resin of the resin composition is supplied into the male and female molds, and the head 21 is molded by compression molding and joined to one opening of the body 22, thereby forming the laminated tube container 20 consisting of the head 21 and the body 22. When the laminated tube container 20 is molded using an injection molding method, the body 22 is attached to a male mold having a convex portion at the top, the male mold and the female mold are opposed to each other, molten resin is supplied from a gate, and the head 21 is molded by injection molding and joined to one opening of the body 22, thereby forming the laminated tube container 20 consisting of the head 21 and the body 22.
[0118] After forming the laminated tube container 20, the contents are filled from the other open end connected to the head 21 of the body 22, and the opening is welded to form the bottom seal portion 25. In this way, a laminated tube container 20 filled and packaged with the contents can be obtained. The cap to be attached to the spout portion 24 is attached by various methods, such as by screwing or fitting, depending on the shape of the spout portion 24.
[0119] The laminated tube container 20 may also have a cap on the head 21. The cap is made of a thermoplastic resin, and examples of the thermoplastic resin include polyolefin resins such as polyethylene resin and polypropylene resin. Examples of the cap include a capping type that is fitted to the mouth of the body 22 by plugging it, and a screw type that is screwed into a thread provided on the outer surface of the mouth of the body 22. In either the capping type or the screw type, a hinge cap can be used in which a cap body having an opening and an upper lid that closes the opening are joined via a hinge. In addition, when a hinge cap is used, it is preferable to use polypropylene resin from the viewpoint of the durability of the hinge.
[0120] The laminated tube container of the present invention can be suitably used as a packaging container for products filled with, for example, toothpaste, cosmetics, foodstuffs, medicines, and other conventionally known contents.
[0121] <Other aspects> In another aspect, an object of the present invention is to provide a resin film that can improve the environmental load reducing properties, as well as the slipperiness and rigidity. In another aspect, another object of the present invention is to provide a laminated tube container comprising this resin film. In another aspect, the present invention provides a resin film comprising at least a first layer and a second layer, the first layer constitutes at least one outermost layer of the resin film; The first layer and the second layer are directly laminated to each other, The first layer is made of a polyethylene resin derived from a fossil fuel, The second layer is made of a resin containing linear low-density polyethylene derived from biomass, the density of the second layer is less than the density of the first layer; The resin film has a stiffness parameter (K) of 3.5 or more and 6.5 or less, as determined by the following formula: K=ρ 40×t ρ: Density of resin film t: resin film thickness In one embodiment, the resin film has a density difference between the second layer and the first layer of 0.001 g / cm 3 More preferably, it is equal to or greater than this. In one embodiment, the resin film further comprises a third layer on the opposite side to the first layer, the third layer constitutes the other outermost layer of the resin film, the second layer and the third layer are laminated directly or via a thermoplastic resin layer, The third layer is preferably made of a polyethylene resin derived from fossil fuels. In one embodiment, the resin film preferably has a biomass ratio of 1% or more and 80% or less. In another aspect, the present invention provides a nozzle comprising: a head portion comprising a shoulder portion and a spout portion; a torso portion connected to the shoulder portion of the head; A laminated tube container comprising: The body portion is composed of a laminate having at least an outer sealant layer, a base material layer, and an inner sealant layer in this order; The laminated tube container is one in which the outer sealant layer comprises the above-mentioned resin film, and a first layer of the resin film of the outer sealant layer is located on the outermost surface of the body, or the inner sealant layer comprises the above-mentioned resin film, and a first layer of the resin film of the inner sealant layer is located on the innermost surface of the body. In one embodiment, the outer sealant layer and the inner sealant layer comprise the resin film described above, It is preferable that the first layer of the resin film of the outer sealant layer is located on the outermost surface of the body portion, and the first layer of the resin film of the inner sealant layer is located on the innermost surface of the body portion. In another aspect, the present invention can provide a resin film that can improve the environmental load reduction properties, as well as the slipperiness and rigidity. In another aspect, the present invention can provide a laminated tube container including this resin film. EXAMPLES
[0122] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these.
[0123] [Example 1] The resin constituting the first layer was 100 parts by mass of fossil fuel-derived medium-density polyethylene (manufactured by Prime Polymer Co., Ltd., product name: UZ3520L, density: 0.931 g / cm 3 , MFR: 2.1 g / 10 min, biomass content: 0%) was melted. Next, as the resin constituting the second layer, 70 parts by mass of fossil fuel-derived medium-density polyethylene (manufactured by Prime Polymer Co., Ltd., product name: UZ3520L, density: 0.931 g / cm 3 , MFR: 2.1 g / 10 min, biomass content: 0%), and 30 parts by mass of biomass-derived linear low-density polyethylene (manufactured by Braskem, product name: SLL-118, density: 0.916 g / cm 3 , MFR: 1.0 g / 10 min, biomass content: 87%) were melted separately. Next, as the resin constituting the third layer, 100 parts by mass of fossil fuel-derived medium-density polyethylene (manufactured by Prime Polymer Co., Ltd., product name: UZ3520L, density: 0.931 g / cm 3 , MFR: 2.1 g / 10 min, biomass ratio: 0%) was melted separately.
[0124] These melts were co-extruded by inflation molding so that the first and third layers constituted the outermost layers of the resin film, to produce a resin film with a layer thickness ratio of 1:3:1 (first layer: second layer: third layer). The thickness of the resin film was 120 μm. The average density of the second layer was 0.927 g / cm 3 The average density of the resin film is 0.928 g / cm 3The biomass ratio of the resin film was 16%. The stiffness parameter (K) of the resin film was 6.04. Details of the obtained resin film are summarized in Table 1. In addition, in the following Tables 1 and 2, "Petroleum MDPE_A" is a medium density polyethylene derived from fossil fuels (manufactured by Prime Polymer Co., Ltd., product name: UZ3520L, density: 0.931 g / cm 3 , MFR: 2.1g / 10min, biomass content: 0%), and "bio-LLDPE" refers to a biomass-derived linear low-density polyethylene (manufactured by Braskem, product name: SLL-118, density: 0.916g / cm 3 , MFR: 1.0 g / 10 min, biomass degree: 87%).
[0125] [Examples 2 to 6] [Comparative Examples 1 to 4] Resin films were produced in the same manner as in Example 1, except that the configuration of the resin film was changed as shown in Tables 1 and 2. Note that "Petroleum MDPE_B" is a fossil fuel-derived medium-density polyethylene (manufactured by Prime Polymer Co., Ltd., product name: SP4020, density: 0.937 g / cm 3 , MFR: 1.8g / 10min, biomass content: 0%), and "Petroleum HDPE" refers to high-density polyethylene derived from fossil fuels (manufactured by Prime Polymer Co., Ltd., product name: HZ3300L, density: 0.950g / cm 3 , MFR: 1.1g / 10min, biomass ratio: 0%), and "petroleum-based LLDPE" is (Prime Polymer Co., Ltd., product name: SP2320, density: 0.920 / cm 3 , MFR: 1.9 g / 10 min, biomass ratio: 0%).
[0126] [Table 1]
[0127] [Table 2]
[0128] <Rigidity evaluation> The resin films obtained in the above Examples and Comparative Examples were cut into pieces with a width of 20 mm and a length of 130 mm, and the stiffness (mN) of the films was measured using a stiffness tester (manufactured by Toyo Seiki Seisakusho Co., Ltd., product name: Loop Stiffness Tester). The loop length was 60 mm, the distance between the chuck fixing the loop and the indenter was 15 mm, the compression speed was 3.3 mm / s, and the holding time was 3 seconds. The measurement results are summarized in Table 3.
[0129] <Slipperiness evaluation> (Sealant layer to sealant layer) Two laminates each including a sealant layer and a base layer were prepared. The base layer was a 12 μm PET film, and the sealant layer was the resin film obtained in the above examples and comparative examples. The sealant layer and the base layer were bonded together using an adhesive. The first layer of the resin film of the sealant layer was located on the outermost surface. The static friction coefficient (μ S ) and the coefficient of kinetic friction (μ D ) was measured. The number of tests was n=3, and the average value was calculated. The test speed was 100 mm / min. The measurement results are summarized in Table 3.
[0130] (Sealant layer vs. metal plate) A laminate including a sealant layer and a base layer was prepared. The base layer was a PET film of 12 μm, and the sealant layer was the resin film obtained in the above-mentioned Examples and Comparative Examples. The sealant layer and the base layer were bonded together using an adhesive. The first layer of the resin film of the sealant layer was located on the outermost surface. The static friction coefficient (μ S ) and the coefficient of kinetic friction (μ D ) was measured. The number of tests was n=3, and the average value was calculated. The test speed was 100 mm / min. SUS304 was used as the metal plate. The measurement results are summarized in Table 3.
[0131] <Reduced environmental impact> The CO2 emissions of the resin films obtained in the above examples and comparative examples were calculated. The CO2 emissions of each resin film were calculated by multiplying the CO2 emissions per kg of each resin film by the average density of the resin film and the thickness of the resin film. The calculation results are summarized in Table 3.
[0132] [Table 3]
[0133] As is clear from the above table, the resin film of the present invention has better slip properties than Comparative Examples 1 and 2 in which the density of the second layer is greater than the density of the first layer. It is also clear that the resin film of the present invention has a reduced environmental impact compared to Comparative Example 2 in which the stiffness parameter exceeds the upper limit. Furthermore, it is clear that the resin film of the present invention has superior rigidity to Comparative Examples 3 and 4, whose rigidity parameters are below the lower limit. [Explanation of symbols]
[0134] 10: Resin film 11: 1st layer 12:Second layer 13:Third layer 14:Thermoplastic resin layer 20: Laminated tube container 21:Head 22: Torso 23:Shoulder 24: Outlet part 25: Bottom seal 26: Adhesive part 30: Laminate 31: Outer sealant layer 32: Base material layer 33: Inner sealant layer
Claims
1. A head portion including a shoulder portion and a spout portion; a torso portion connected to the shoulder portion of the head; A laminated tube container comprising: The body portion is composed of a laminate having at least an outer sealant layer, a base material layer, and an inner sealant layer in this order; the outer sealant layer comprises a resin film having at least a first layer and a second layer; the first layer constitutes at least one outermost layer of the resin film; The first layer and the second layer are directly laminated to each other, The first layer is made of a polyethylene resin derived from a fossil fuel, The second layer is made of a resin containing linear low-density polyethylene derived from biomass, The biomass content of the second layer is 95% or less; The first layer has a thickness of 5 μm or more, The second layer has a thickness of 10 μm or more, The density of the first layer is 0.910 g / cm 3 or more; The density of the second layer is 0.901 g / cm 3 or more; the density of the second layer is less than the density of the first layer; The density difference between the second layer and the first layer is 0.003 g / cm 3 That's all. A laminated tube container, wherein the resin film has a stiffness parameter (K) defined by the following formula of 3.5 or more and 6.5 or less. K=r 40 ×t ρ: Density of resin film [g / cm 3 ] t: resin film thickness [μm]
2. the resin film further comprises a third layer on an opposite side to the first layer, the third layer constitutes the other outermost layer of the resin film, the second layer and the third layer are laminated directly or via a thermoplastic resin layer, 2. The laminated tube container according to claim 1, wherein the third layer is made of a polyethylene resin derived from fossil fuels.
3. 3. The laminated tube container according to claim 1, wherein the resin film has a biomass ratio of 1% or more and 80% or less.
4. A laminated tube container described in any one of claims 1 to 3, wherein a first layer of the resin film provided in the outer sealant layer is located on the outermost surface of the body.
Citation Information
Patent Citations
Diabetes remedy
JP1982099520A
Resin laminate and use application thereof
JP1994246886A
Integrated method for the production of ethylene-butylene copolymer, ethylene-butylene copolymer and use of ethylene and 1-butylene as comonomers supplied from renewable natural raw materials.
JP2011506628A
Laminated tube container
JP2013177153A
Sealant film and packaging material and packaging bag using the same
JP2014046674A