Laminated film and method for producing same

The laminated film with a gas barrier layer and smooth release layer addresses the issue of insufficient oxygen barrier performance in release films, ensuring effective protection and ease of use.

JP7594775B2Active Publication Date: 2024-12-05UNITIKA LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020165071
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-02-28
Filing Date
2020-09-30
Publication Date
2024-12-05
Estimated Expiration
2040-09-30

AI Technical Summary

Technical Problem

Existing release films fail to provide sufficient oxygen barrier performance, leading to deterioration of adherends and difficulty in maintaining quality and functionality.

Method used

A laminated film comprising a gas barrier layer with a specific surface roughness and containing an organic compound, along with a release layer formed from acid-modified polyolefin resin and a crosslinking agent, ensuring a smooth surface and improved adhesion properties.

Benefits of technology

The laminated film maintains excellent oxygen barrier properties and bending resistance, preventing cracking and facilitating easy bonding and release, even after repeated use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594775000001
    Figure 0007594775000001
Patent Text Reader

Abstract

To provide a release film having releasability and having sufficient oxygen barrier properties in a state of being stuck to an adherend.SOLUTION: A laminate film has a release layer, a base material, and a gas barrier layer. At least one outermost surface layer of the laminate film is the release layer, the release layer has a surface roughness parameter Sa (an arithmetical average height) of 0.05 μm or less, and the gas barrier layer contains an organic compound.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminated film and a method for producing the same. [Background technology]

[0002] Release films are widely used in the medical and industrial fields, including as process materials for the manufacture of printed wiring boards, flexible printed wiring boards, multilayer printed wiring boards, etc., as well as protective materials for protecting medical tapes, poultices, adhesive materials, liquid crystal display components, etc.

[0003] For example, Patent Document 1 discloses a release film having an acid-modified polyolefin resin layer as a release layer, which has good releasability with respect to various adherends. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2009 / 025063 Summary of the Invention [Problem to be solved by the invention]

[0005] In recent years, for adherends that are susceptible to deterioration due to oxygen, which can result in a decrease in yield and quality, there has been a demand for release films to be endowed with sufficient oxygen barrier performance so that the release film also functions as a protective film to prevent the oxidative deterioration of the adherend. However, even with the release film disclosed in Patent Document 1, even if a gas barrier layer is provided, it is difficult to obtain high enough gas barrier performance to maintain the quality of an adherend having high performance or functionality.

[0006] In view of this problem, an object of the present invention is to provide a release film that has releasability and also has sufficient oxygen barrier performance when attached to an adherend. [Means for solving the problem]

[0007] As a result of intensive research to solve the above-mentioned problems, the inventors discovered that the above-mentioned problems can be solved by a laminate film that includes a gas barrier layer containing an organic compound and in which a release layer constituting at least one of the outermost layers has a specific surface shape, thereby arriving at the present invention.

[0008] That is, the gist of the present invention is as follows. (1) A laminate film including a release layer, a substrate, and a gas barrier layer, wherein at least one outermost layer of the laminate film is a release layer; The surface roughness parameter Sa (arithmetic mean height) of the release layer surface is 0.05 μm or less, Gas barrier layer , polycarboxylic acids and compounds that form crosslinked structures with polycarboxylic acids Contains A cross-linked structure is formed, The content of polycarboxylic acids in the gas barrier layer is 40 to 90 mass %. A laminated film characterized by: (2) The laminate film according to (1), wherein the release layer contains an acid-modified polyolefin resin and a crosslinking agent. (3) Compounds that form crosslinked structures with polycarboxylic acids But, rear L'Colle and / or cross-linking agent The laminate film according to (1) or (2), (4) A method for producing the laminated film described above in (2), comprising the step of applying a liquid for forming a release layer, the liquid containing an acid-modified polyolefin resin, a crosslinking agent and an aqueous medium, to one side of a substrate. (5) The method for producing a laminated film according to (4) above, further comprising the step of drying and stretching the substrate coated with the release layer-forming liquid material. (6) The above ( 1 A method for producing the laminated film according to any one of the preceding claims, comprising: Polycarboxylic acids and compounds that form crosslinked structures with polycarboxylic acids Contains The content of polycarboxylic acids is 40 to 90% by mass. a liquid material for forming a gas barrier layer on the substrate, drying the substrate on which the liquid material for forming a gas barrier layer has been applied, and stretching the substrate. Effect of the Invention

[0009] The laminated film of the present invention has a gas barrier layer laminated thereon, and the surface of the laminated release layer has a smooth shape, so that even when the laminated film is attached to an adherend and heat-treated in an environment in which oxygen is present, the laminated film of the present invention has excellent oxygen barrier properties as a protective film for the adherend. In addition, the laminated film of the present invention has excellent flex resistance because the gas barrier layer contains an organic compound, and even when the laminated film is released from the adherend, cracks are unlikely to occur in the gas barrier layer, so that the laminated film can be suitably used in a process in which lamination and release are repeated. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention will be described in detail below. The laminate film of the present invention is a laminate film comprising a release layer, a substrate, and a gas barrier layer, at least one outermost layer of the laminate film is a release layer, the surface of the release layer has a specific smoothness, and the gas barrier layer contains an organic compound.

[0011] <Base material> Examples of the substrate constituting the laminated film of the present invention include polyester films such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyethylene naphthalate (PEN), poly(1,4-cyclohexylene dimethylene terephthalate), and polylactic acid (PLA), polyolefin films such as polypropylene, polystyrene films, polyamide 6, poly-p-xylylene adipamide (MXD6 nylon), polyamide 66, polyamide 46, polyamide 4T, polyamide 6T, polyamide 9T, polyamide 10T, polyamide 11T, polyamide 12T, and polyamide 6I, polycarbonate films, polyacrylonitrile films, polyimide films, and laminates thereof (e.g., polyamide 6 / MXD6 nylon / polyamide 6, polyamide 6 / ethylene-vinyl alcohol copolymer / polyamide 6, polyamide 6 / 6T, polyamide 6 / 6I, and polyamide 6 / 6T / 6I) or mixtures thereof. Polyester films and polyamide films having mechanical strength and dimensional stability are preferred. Here, T represents terephthalic acid, and I represents isophthalic acid. Among them, the substrate is preferably a polyethylene terephthalate film from the viewpoints of flex resistance and adhesion to the release layer and gas barrier layer, and is preferably a semi-aromatic polyamide film from the viewpoints of heat resistance, flex resistance, and adhesion to the gas barrier layer, and is particularly preferably a polyamide 9T film or a polyamide 10T film.

[0012] (polyester resin) The polymerization method of the polyester resin constituting the polyester film substrate is not particularly limited, and examples thereof include transesterification and direct polymerization. Examples of transesterification catalysts include compounds such as oxides and acetates of Mg, Mn, Zn, Ca, Li, Ti, etc. Examples of polycondensation catalysts include compounds such as oxides and acetates of Sb, Ti, Ge, etc. Since the polyester after polymerization contains monomers, oligomers, and by-products such as acetaldehyde, it may be subjected to solid-phase polymerization at a temperature of 200° C. or higher under reduced pressure or in an inert gas stream.

[0013] The intrinsic viscosity of the polyester resin is preferably 0.55 to 0.80, more preferably 0.60 to 0.75. If the intrinsic viscosity is less than the above range, the film is easily cut during film formation, making it difficult to produce stably, and the strength of the obtained film is low. On the other hand, if the intrinsic viscosity exceeds the above range, shear heat is generated during melt extrusion of the resin in the film production process, the load on the extruder is increased, the production speed has to be sacrificed, and it becomes difficult to control the thickness of the film, so that the productivity of the film decreases. In addition, the obtained film has an increased amount of thermal decomposition and gelation, and surface defects, foreign matter, and surface coarse protrusions. In addition, if the intrinsic viscosity is too high, the polymerization time and polymerization process are long, which is also a factor that increases costs.

[0014] (Semi-aromatic polyamide resin) The semi-aromatic polyamide resin constituting the semi-aromatic polyamide film substrate is composed of a dicarboxylic acid component and a diamine component, and has an aromatic component in the dicarboxylic acid component or the diamine component, and is preferably composed of an aromatic dicarboxylic acid component and an aliphatic diamine component.

[0015] The aromatic dicarboxylic acid component is preferably mainly composed of terephthalic acid, more preferably contains 60 mol% or more, further preferably contains 70 mol% or more, and particularly preferably contains 85 mol% or more. If the content of terephthalic acid is less than 60 mol%, the heat resistance and low water absorbency of the obtained film are reduced. Examples of aromatic dicarboxylic acid components other than terephthalic acid include isophthalic acid and naphthalenedicarboxylic acid (1,2-, 1,3-, 1,4-, 1,5-, 1,6-, 1,7-, 1,8-, 2,3-, 2,6-, and 2,7-forms). The aromatic dicarboxylic acid component may contain other dicarboxylic acids as long as the effects of the present invention are not impaired. Examples of other dicarboxylic acids include aliphatic dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, sebacic acid, dodecanedioic acid, tetradecanedioic acid, and octadecanedioic acid.

[0016] The aliphatic diamine component preferably contains an aliphatic diamine having 4 to 15 carbon atoms as a main component, more preferably contains an aliphatic diamine having 6 to 12 carbon atoms as a main component, even more preferably contains an aliphatic diamine having 9 to 12 carbon atoms as a main component, and particularly preferably contains an aliphatic diamine having 9 to 10 carbon atoms as a main component. The aliphatic diamine component preferably contains 60 mol % or more of aliphatic diamines having 4 to 15 carbon atoms, more preferably 75 mol % or more, and even more preferably 90 mol % or more. By making the content of the aliphatic diamines having 4 to 15 carbon atoms 60 mol % or more, the obtained film can achieve both heat resistance and productivity. The aliphatic diamines having 4 to 15 carbon atoms may be used alone or in combination of two or more. When two or more types are used in combination, the content is the total of the two or more.

[0017] Examples of aliphatic diamines having 4 to 15 carbon atoms include 1,4-butanediamine, 1,5-pentanediamine, 1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 1,9-nonanediamine, 1,10-decanediamine, 1,11-undecanediamine, 1,12-dodecanediamine, 1,13-tridecanediamine, 1,14-tetradecanediamine, and 1,15-pentadecaamine. and branched chain aliphatic diamines such as 2-methyl-1,8-octanediamine, 4-methyl-1,8-octanediamine, 5-methyl-1,9-nonanediamine, 2,2,4- / 2,4,4-trimethylhexamethylenediamine, 2-methyl-1,5-pentanediamine, 2-methyl-1,6-hexanediamine, and 2-methyl-1,7-heptanediamine.

[0018] The aliphatic diamine component may contain other diamines as long as the effects of the present invention are not impaired. Examples of other diamines include alicyclic diamines such as isophorone diamine, norbornane dimethylamine, and tricyclodecane dimethylamine, and aromatic diamines such as metaxylylene diamine, paraxylylene diamine, metaphenylene diamine, and paraphenylene diamine.

[0019] The semi-aromatic polyamide resin may be copolymerized with lactams such as ε-caprolactam, ζ-enantholactam, η-capryllactam, and ω-laurolactam, as long as the effects of the present invention are not impaired.

[0020] Specific examples of semi-aromatic polyamide resins include polyamide 4T, polyamide 6T, polyamide 9T, polyamide 10T, polyamide 11T, polyamide 12T, polyamide 6I, polyamide 6 / 6T, polyamide 6 / 6I, and polyamide 6 / 6T / 6I. Here, T represents terephthalic acid, and I represents isophthalic acid. Among these, polyamide 9T and polyamide 10T are preferred from the viewpoint of adhesion to the gas barrier layer.

[0021] The semi-aromatic polyamide resin may contain a polymerization catalyst and an end-capping agent. Examples of the end-capping agent include acetic acid, lauric acid, benzoic acid, octylamine, cyclohexylamine, and aniline. Examples of the polymerization catalyst include phosphoric acid, phosphorous acid, hypophosphorous acid, and salts thereof.

[0022] The melting point (Tm) of the semi-aromatic polyamide resin is preferably 260° C. or higher, and more preferably 270 to 350° C. When the Tm of the semi-aromatic polyamide resin is in this range, the semi-aromatic polyamide film obtained is inhibited from thermal decomposition (thermal deterioration), and the obtained laminate film can be easily released even after a reflow soldering process when used as a processing material for a printed circuit board. The melting point of the semi-aromatic polyamide resin can be adjusted to the above range by selecting the raw materials and composition.

[0023] The semi-aromatic polyamide resin preferably has an intrinsic viscosity of 0.8 to 2.0 dL / g, more preferably 0.9 to 1.8 dL / g. When the semi-aromatic polyamide resin has an intrinsic viscosity of 0.8 dL / g or more, a film having excellent mechanical strength can be produced, but when the intrinsic viscosity exceeds 2.0 dL / g, it may be difficult to produce the film.

[0024] The semi-aromatic polyamide resin can be produced by any method known as a method for producing crystalline polyamide. For example, there can be mentioned a solution polymerization method or an interfacial polymerization method (Method A) using an acid chloride and a diamine component as raw materials, a method of preparing a low polymer using a dicarboxylic acid component and a diamine component as raw materials and polymerizing the low polymer by melt polymerization or solid-phase polymerization (Method B), a method of producing a crushed mixture of salt and low polymer using a dicarboxylic acid component and a diamine component as raw materials and solid-phase polymerizing the mixture (Method C), and a method of producing a salt using a dicarboxylic acid component and a diamine component as raw materials and solid-phase polymerizing the mixture (Method D). Among them, Methods C and D are preferred, and Method D is more preferred. Methods C and D can produce a crushed mixture of salt and low polymer or salt at a lower temperature than Method B, and do not require a large amount of water when producing a crushed mixture of salt and low polymer or salt. Therefore, the generation of gel-like bodies can be reduced, and fish eyes can be reduced.

[0025] As the semi-aromatic polyamide resin, commercially available products can be suitably used, such as "Genesta (registered trademark)" manufactured by Kuraray Co., Ltd., "Zecot (registered trademark)" manufactured by Unitika Ltd., "Reny (registered trademark)" manufactured by Mitsubishi Engineering Plastics Corporation, "Arlen (registered trademark)" manufactured by Mitsui Chemicals, Inc., "Ultramid (registered trademark)" manufactured by BASF, and "Rilsan HT (registered trademark)" manufactured by Arkema.

[0026] (Production of base film) Next, a method for producing the base film will be described. First, a sufficiently dried resin is fed into an extruder, where it is sufficiently plasticized and melted at a temperature above the temperature at which it exhibits fluidity, passed through a filter selected as necessary, and then the molten polymer is discharged in sheet form from a flat die such as a T-die or I-die, and brought into contact with the cooling surface of a moving cooling body such as a cooling roll or steel belt whose temperature is adjusted to below the glass transition temperature (Tg) to obtain an unstretched film. Methods that can be used to cool and solidify the molten polymer discharged in sheet form by bringing it into contact with the moving cooling body include the air knife casting method, electrostatic application method, and vacuum chamber method. The obtained unstretched film is preferably stretched from the viewpoint of improving mechanical properties and heat resistance, that is, uniaxial orientation is performed by a uniaxial stretching method, or biaxial orientation is performed by a biaxial stretching method. The biaxial stretching method is not particularly limited, but flat-type sequential biaxial stretching method, flat-type simultaneous biaxial stretching method, tubular method, etc. can be used. Among these, the polyester film used as the substrate constituting the laminated film of the present invention is best suited for the flat type successive biaxial stretching method, while the semi-aromatic polyamide film is best suited for the flat type simultaneous biaxial stretching method.

[0027] In the uniaxial stretching method for polyester films, an unstretched film is stretched in the longitudinal or transverse direction at a stretch ratio of about 2 to 6 times in the temperature range of the Tg of the resin to 50° C. higher than the Tg. In the simultaneous biaxial stretching method, an unstretched film is biaxially stretched to a stretch ratio of about 2 to 4 times in both the longitudinal and transverse directions in a temperature range of from the Tg of the resin to 50° C. higher than the Tg. Before being introduced into the simultaneous biaxial stretching machine, the unstretched film may be subjected to preliminary longitudinal stretching up to about 1.2 times. In the sequential biaxial stretching method, an unstretched film is heated with a heating roll or infrared rays and stretched in the longitudinal direction to obtain a longitudinally stretched film. The longitudinal stretching is preferably performed at a stretching ratio of 2.5 to 4.0 times in a temperature range of Tg to 40°C higher than Tg of the polyester by utilizing the peripheral speed difference between two or more rolls. The longitudinally stretched film is then continuously subjected to transverse stretching in the width direction, heat setting, and heat relaxation in sequence to obtain a biaxially oriented film. The transverse stretching is started at a temperature of Tg to 40°C higher than Tg of the resin, and the maximum temperature is preferably a temperature (100 to 40)°C lower than the melting point (Tm) of the resin. The transverse stretching ratio is adjusted depending on the required physical properties of the final film, but is preferably 3.5 times or more, further preferably 3.8 times or more, and more preferably 4.0 times or more. After stretching in the longitudinal direction and the width direction, the film can be further stretched again in the longitudinal direction and / or the width direction to increase the elastic modulus and dimensional stability of the film. Following the stretching, it is preferable to heat set the film for several seconds at a temperature (50-10)°C lower than the Tm of the resin, and simultaneously relax the film by 1-10% in the width direction. After the heat setting, the film is cooled to below Tg to obtain a biaxially stretched film.

[0028] In stretching the semi-aromatic polyamide film, the flat-type simultaneous biaxial stretching method is optimal because it has good film thickness accuracy and uniform physical properties in the film width direction as described above. As a stretching device for the flat-type simultaneous biaxial stretching method, a screw-type tenter, a pantograph-type tenter, a linear motor-driven clip-type tenter, etc. can be used. The stretching ratio is preferably in the range of 1.5 to 10 times in both the machine direction (MD) and the transverse direction (TD), and more preferably 2 to 5 times, in order to provide the final semi-aromatic polyamide film with excellent heat resistance and mechanical strength. The stretching speed is preferably such that both the MD and TD stretching strain rates exceed 400% / min, more preferably 800 to 12000% / min, and even more preferably 1200 to 6000% / min. If the strain rate is 400% / min or less, crystals grow during stretching and the film breaks, while if the strain rate is too fast, the unstretched sheet may be unable to keep up with the deformation and break. The stretching temperature is preferably equal to or higher than the Tg of the semi-aromatic polyamide resin, and more preferably exceeds Tg and is equal to or lower than (Tg+50)° C. If the stretching temperature is lower than Tg, the film is likely to break and stable production cannot be performed, whereas if the temperature exceeds (Tg+50)° C., uneven stretching may occur. After the semi-aromatic polyamide film is stretched as described above, it is preferable to perform a heat setting treatment as necessary while the film is held by the clips used during stretching. The heat setting temperature is preferably 250 to (Tm-5)°C, more preferably 280 to (Tm-10)°C. If the heat setting temperature is less than 250°C, the resin layer containing the acid-modified olefin resin provided on the semi-aromatic polyamide film before stretching will undergo an insufficient curing reaction, resulting in reduced releasability. Furthermore, after the heat setting treatment, the film is preferably subjected to a relaxation treatment of 1 to 10%, more preferably 3 to 7%, as necessary while still being held by the clips. By performing the relaxation treatment, the film can obtain sufficient dimensional stability. After optionally performing heat setting or relaxation treatment, the film is cooled and wound on a take-up roll to obtain a semi-aromatic polyamide resin stretched film roll. The obtained semi-aromatic polyamide resin stretched film roll can be slit to a desired width.

[0029] (Multi-layer film substrate) Although a single-layer film can be obtained by the above-mentioned production method, the substrate constituting the laminated film may be a multilayer film having two or more kinds of layers laminated together. The multilayer film can be produced by the above-mentioned production method, in which the resins constituting each layer are melted separately, extruded using a multilayer die, laminated and fused before solidification, and then biaxially stretched and heat-set, or by a method in which two or more resins are melted separately, extruded to form films, and laminated and fused in an unstretched state or after stretching, etc. From the viewpoint of process simplicity, it is preferable to use a multilayer die and laminate and fused before solidification.

[0030] The substrate constituting the laminated film of the present invention may be a single layer structure or a multilayer structure (e.g., two-type two-layer, two-type three-layer, three-type three-layer, four-layer or more multilayer, etc.), but it is preferable to have a multilayer structure from the viewpoint of being able to control the surface roughness for each side and improving handling properties such as winding properties. Two-type two-layer and two-type three-layer structures are more preferable, and two-type two-layer is even more preferable. The two-type two-layer structure refers to a two-layer structure manufactured using two types of layer-forming materials, and these two layers have different compositions (e.g., particle content). The two-type three-layer structure refers to a three-layer structure manufactured using two types of layer-forming materials, and the two outermost layers and the middle layer have different compositions (e.g., particle content). The three-type three-layer structure refers to a three-layer structure manufactured using three types of layer-forming materials, and these three layers have different compositions (e.g., particle content).

[0031] (particle) The substrate may contain particles for the main purpose of imparting easy slippage and preventing scratches in each process. However, if the substrate contains particles on the side on which the release layer is laminated, the release layer may have a rough surface, and the oxygen barrier performance when laminated to an adherend may be reduced. Therefore, it is preferable that the substrate on the side on which the release layer is laminated does not contain particles.

[0032] The type of particles contained is not particularly limited as long as they are particles capable of imparting lubricity, and specific examples include inorganic particles such as silica, calcium carbonate, magnesium carbonate, barium carbonate, calcium sulfate, calcium phosphate, magnesium phosphate, kaolin, aluminum oxide, and titanium oxide, and organic particles such as acrylic resin, styrene resin, urea resin, phenolic resin, epoxy resin, and benzoguanamine resin. Furthermore, precipitated particles obtained by precipitating and finely dispersing a part of a metal compound such as a catalyst during the manufacturing process of the resin constituting the base material can also be used.

[0033] On the other hand, the shape of the particles contained is not particularly limited, and any of spherical, blocky, rod-like, flat, etc. may be used. In addition, there is no particular limit to the hardness, specific gravity, color, etc. of the particles. Two or more kinds of these series of particles may be used in combination as necessary.

[0034] The average particle size of the particles is usually 5 μm or less, preferably in the range of 0.1 to 3 μm. If the average particle size exceeds 5 μm, the surface roughness of the film becomes too high, and for example, when used for transfer, the surface shape of the molded surface to be transferred may be affected.

[0035] The particle content is usually 5% by mass or less, and preferably in the range of 0.0003 to 3% by mass. If the particle content exceeds 5% by mass, the transparency of the film may become insufficient.

[0036] The method of adding the particles is not particularly limited, and a conventionally known method can be adopted. For example, the particles can be added at any stage of producing the resin constituting each layer. In the case of the process of producing a polyester, it is preferable to add the particles after the completion of the esterification or transesterification reaction.

[0037] (Additives) The substrate may contain additives, as necessary, such as antioxidants, heat stabilizers, ultraviolet absorbers, antistatic agents, pinning agents, etc. Examples of antioxidants include hindered phenol compounds and hindered amine compounds, examples of heat stabilizers include phosphorus compounds, and examples of ultraviolet absorbers include benzophenone compounds and benzotriazole compounds.

[0038] The thickness of the substrate is not particularly limited as long as it can be formed into a film, but from the standpoints of mechanical strength, handling properties, productivity, etc., it is usually 5 to 300 μm, and preferably 10 to 150 μm.

[0039] <Release layer> The laminated film of the present invention has a release layer provided on at least one outermost layer of the laminated film.

[0040] The components constituting the release layer include silicone compounds, fluorine-containing copolymers, polyolefin resins, acid-modified polyolefin resins, polyester resins, epoxy resins, cyanate resins, polyether resins, polystyrene resins, urethane resins, polyamide resins, polyimide resins, long-chain alkyl group-containing compounds, acrylic resins, polyalkylene glycols, polyalkyleneimines, methyl cellulose, hydroxycellulose, starches, and mixtures thereof. From the viewpoint of releasability, the components constituting the release layer are preferably polyolefin resins, acid-modified polyolefin resins, silicone compounds, fluorine compounds, long-chain alkyl group-containing compounds, acrylic resins, or mixtures thereof, and further preferably contain an acid-modified polyolefin resin and a crosslinking agent, or a long-chain alkyl group-containing compound, polyvinyl alcohol, and a crosslinking agent.

[0041] (Acid-modified polyolefin resin) The acid-modified polyolefin resin is a resin that contains an olefin component as a main component and is modified with an acid-modifying component. The olefin component constituting the acid-modified polyolefin resin preferably contains at least one selected from ethylene, propylene, and butene. From the viewpoint of releasability from the acrylic adhesive, it is more preferable that the olefin component contains ethylene. From the viewpoint of further improving the releasability from the acrylic adhesive, the ethylene content in the olefin component is preferably 50% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more. From the viewpoint of releasability from the epoxy prepreg, it is more preferable that the olefin component contains propylene. From the viewpoint of further improving the releasability from the epoxy prepreg, the propylene content in the olefin component is preferably 50% by mass or more, more preferably 80% by mass or more, even more preferably 95% by mass or more, and particularly preferably 99% by mass or more.

[0042] The acid-modified component constituting the acid-modified polyolefin resin includes unsaturated carboxylic acid components, specifically acrylic acid, methacrylic acid, maleic acid, maleic anhydride, itaconic acid, itaconic anhydride, fumaric acid, crotonic acid, etc., as well as half esters and half amides of unsaturated dicarboxylic acids. Among them, in order to stably disperse the resin in the aqueous dispersion of the resin described later, acrylic acid, methacrylic acid, maleic acid, and maleic anhydride are preferred, and acrylic acid, methacrylic acid, and maleic anhydride are particularly preferred. Two or more of these acid-modified components may be contained in the acid-modified polyolefin resin.

[0043] The ratio of the acid-modified component in the acid-modified polyolefin resin is preferably 1 to 10% by mass, more preferably 2 to 9% by mass. When the acid-modified component is less than 1% by mass, the ratio of polar groups in the acid-modified polyolefin resin contained in the release layer is reduced, so the release layer tends not to have sufficient adhesion to the substrate, and may contaminate the adherend released from the release layer. Furthermore, in the aqueous dispersion of the resin described below, it tends to be difficult to stably disperse the resin. On the other hand, when the ratio of the acid-modified component exceeds 10% by mass, the ratio of polar groups is increased, so that the adhesion between the release layer and the substrate is sufficient, but the adhesion between the release layer and the adherend is also increased at the same time, so that the releasability from the adherend tends to decrease.

[0044] In order to further improve the adhesion to the substrate, the acid-modified polyolefin resin may contain an ethylenically unsaturated component containing an oxygen atom in the side chain. Examples of ethylenically unsaturated components containing oxygen atoms in the side chain include esters of (meth)acrylic acid and alcohols having 1 to 30 carbon atoms, and among these, from the viewpoint of availability, esters of (meth)acrylic acid and alcohols having 1 to 20 carbon atoms are preferred. Specific examples of such compounds include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, hexyl (meth)acrylate, octyl (meth)acrylate, decyl (meth)acrylate, lauryl (meth)acrylate, dodecyl (meth)acrylate, and stearyl (meth)acrylate. A mixture of these may be used. Among these, from the viewpoint of adhesion to polyester film, methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, hexyl acrylate, and octyl acrylate are more preferred, ethyl acrylate and butyl acrylate are even more preferred, and ethyl acrylate is particularly preferred. "(meth)acrylic acid" means "acrylic acid or methacrylic acid". The ethylenically unsaturated component containing an oxygen atom in the side chain has a polar group in the molecule, similar to the acid-modified component. Therefore, by including an ethylenically unsaturated component containing an oxygen atom in the side chain in the acid-modified polyolefin resin, the release layer has high adhesion to the substrate. However, if the amount of the ethylenically unsaturated component containing an oxygen atom in the side chain is too large, the properties of the olefin-derived resin are lost, and the release layer may have low releasability from the adherend. The ratio of the ethylenically unsaturated component containing an oxygen atom in the side chain in the acid-modified polyolefin resin is preferably 1 to 40% by mass, more preferably 2 to 35% by mass, even more preferably 3 to 30% by mass, and particularly preferably 6 to 18% by mass. Even if an acid-modified polyolefin resin containing an ethylenically unsaturated component containing an oxygen atom in the side chain is used, the releasability of the release layer is not impaired other than the adhesion to the substrate.

[0045] The acid-modified polyolefin resin may be copolymerized with a small amount of other monomers, such as dienes, (meth)acrylonitrile, vinyl halides, vinylidene halides, carbon monoxide, and sulfur dioxide.

[0046] The components constituting the acid-modified polyolefin resin may be copolymerized in the acid-modified polyolefin resin in any form, and examples of the copolymerization state include random copolymerization, block copolymerization, and graft copolymerization (graft modification).

[0047] The melting point of the acid-modified polyolefin resin is preferably 80 to 200° C., more preferably 90 to 150° C. If the melting point exceeds 200° C., high-temperature treatment may be required when forming a release layer on the substrate surface. On the other hand, if the melting point is less than 80° C., the release layer has poor releasability.

[0048] Examples of acid-modified polyolefin resins that can be used in the present invention include the Bondine series manufactured by Arkema, the Nucrel series manufactured by Mitsui DuPont Polychemicals, the Rexpearl series manufactured by Japan Polyethylene Corporation, the Umex series manufactured by Sanyo Chemical Industries, Ltd., the Bestplast series manufactured by Evonik, the Primacol series manufactured by Dow Chemical Company, the Admar series manufactured by Mitsui Chemicals, Inc., and the Toyotack series manufactured by Toyobo Co., Ltd.

[0049] (Long-chain alkyl group-containing compounds) The long-chain alkyl group-containing compound is a compound having a straight-chain or branched alkyl group having a carbon number of usually 6 or more, preferably 8 or more, more preferably 12 or more. Examples of the alkyl group include a hexyl group, an octyl group, a decyl group, a lauryl group, an octadecyl group, and a behenyl group. The upper limit of the carbon number of the alkyl group is usually 30. Examples of the long-chain alkyl group-containing compound include various polymeric compounds having a long-chain alkyl group on the side chain, amine compounds having a long-chain alkyl group, ether compounds having a long-chain alkyl group, and quaternary ammonium salts having a long-chain alkyl group. Considering heat resistance and staining, a polymeric compound is preferable. In addition, from the viewpoint of effectively obtaining releasability, a polymeric compound having a long-chain alkyl group on the side chain is more preferable.

[0050] The polymer compound having a long-chain alkyl group in the side chain can be obtained by reacting a polymer compound having a reactive group with a compound having a long-chain alkyl group capable of reacting with the reactive group. Examples of the reactive group include hydroxyl group, amino group, carboxyl group, acid anhydride, etc. Examples of the polymer compound having these reactive groups include polyvinyl alcohol, polyethyleneimine, polyethyleneamine, reactive group-containing polyester resin, reactive group-containing poly(meth)acrylic resin, etc. Among these, polyvinyl alcohol is preferred in consideration of releasability and ease of handling.

[0051] Examples of compounds having a long-chain alkyl group capable of reacting with the reactive group include long-chain alkyl group-containing isocyanates such as hexyl isocyanate, octyl isocyanate, decyl isocyanate, lauryl isocyanate, octadecyl isocyanate, behenyl isocyanate, etc., long-chain alkyl group-containing acid chlorides such as hexyl chloride, octyl chloride, decyl chloride, lauryl chloride, octadecyl chloride, behenyl chloride, etc., long-chain alkyl group-containing amines, long-chain alkyl group-containing alcohols, etc. Among these, in consideration of releasability and ease of handling, long-chain alkyl group-containing isocyanates are preferred, and octadecyl isocyanate is particularly preferred.

[0052] Furthermore, polymeric compounds having a long-chain alkyl group in the side chain can also be obtained by polymerization of a long-chain alkyl (meth)acrylate or copolymerization of a long-chain alkyl (meth)acrylate with another vinyl group-containing monomer. Examples of long-chain alkyl (meth)acrylates include hexyl (meth)acrylate, octyl (meth)acrylate, decyl (meth)acrylate, lauryl (meth)acrylate, octadecyl (meth)acrylate, and behenyl (meth)acrylate.

[0053] (Polyvinyl alcohol) In the present invention, the release layer preferably contains polyvinyl alcohol from the viewpoint of improving releasability. The polyvinyl alcohol is not particularly limited, but examples thereof include a polymer of vinyl ester completely or partially saponified. By containing polyvinyl alcohol in the release layer, it is possible to improve the adhesion between the release layer and the substrate, and also to improve the releasability between the release layer and the adherend. The polyvinyl alcohol in the present invention is preferably water-soluble in order to be used as a liquid material as described later.

[0054] From the viewpoint of the surface smoothness of the release layer and releasability in a high temperature range, the polyvinyl alcohol preferably has a saponification degree of 99% or less, more preferably 98% or less, and even more preferably 95% or less.

[0055] The content of polyvinyl alcohol is preferably 10 to 1000 parts by mass, more preferably 100 to 1000 parts by mass, even more preferably 210 to 800 parts by mass, and particularly preferably 300 to 600 parts by mass, relative to 100 parts by mass of the above resin, from the viewpoints of improving the smoothness of the surface roughness of the release layer, improving the adhesion between the release layer and the substrate, and improving the releasability between the release layer and the adherend.

[0056] In the present invention, commercially available polyvinyl alcohols can be used. For example, "JP-15", "JT-05", "JL-05E", "JM-33", "JM-17", "JF-05", and "JF-10" of "J-Poval" manufactured by Japan Vinyl Acetate & Poval Corporation, and "PVA-CST", "PVA-624", "PVA-203", "PVA-220", and "PVA-405" of "Kuraray Poval" manufactured by Kuraray Co., Ltd. can be used.

[0057] (Crosslinking agent) In the present invention, the release layer preferably contains a crosslinking agent together with the above resin and polyvinyl alcohol. By containing a crosslinking agent, the components of the release layer are crosslinked to improve the release properties, and the cohesive force of the release layer is improved to make it difficult to transfer to the adherend, and the water resistance can be improved.

[0058] The content of the crosslinking agent is preferably 1 to 20 parts by mass, more preferably 2 to 15 parts by mass, and even more preferably 2 to 10 parts by mass, relative to 100 parts by mass of the resin. If the content of the crosslinking agent is less than 1 part by mass, the release layer tends to have a weak cohesive force, poor adhesion to the substrate, and easily transfer to the adherend. On the other hand, if the content exceeds 20 parts by mass, the release layer may react with the adherend and have poor releasability, or the liquid material for forming the release layer may thicken, decreasing stability.

[0059] As the crosslinking agent, a compound having a plurality of functional groups in the molecule that react with a carboxyl group can be used, and examples thereof include polyfunctional epoxy compounds; polyfunctional isocyanate compounds; polyfunctional aziridine compounds; carbodiimide group-containing compounds; oxazoline group-containing compounds; phenolic resins; and amino resins such as urea compounds, melamine resins, and benzoguanamine resins. One of these may be used, or two or more may be used in combination. Among these, polyfunctional isocyanate compounds, melamine compounds, urea compounds, polyfunctional epoxy compounds, carbodiimide group-containing compounds, and oxazoline group-containing compounds are preferred, carbodiimide group-containing compounds and oxazoline group-containing compounds are more preferred, and oxazoline group-containing compounds are even more preferred. By using an oxazoline group-containing compound, it is possible to obtain a laminated film that is excellent in releasability from the adherend and adhesion to the substrate. These crosslinking agents may also be used in combination.

[0060] Specifically, polyepoxy compounds, diepoxy compounds, etc. can be used as the polyfunctional epoxy compounds. For example, sorbitol polyglycidyl ether, polyglycerol polyglycidyl ether, pentaerythritol polyglycidyl ether, diglycerol polyglycidyl ether, triglycidyl tris(2-hydroxyethyl)isocyanate, glycerol polyglycidyl ether, and trimethylolpropane polyglycidyl ether can be used as the polyepoxy compounds. For example, neopentyl glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, resorcinol diglycidyl ether, ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, and polytetramethylene glycol diglycidyl ether can be used as the diepoxy compounds.

[0061] Examples of polyfunctional isocyanate compounds that can be used include tolylene diisocyanate, diphenylmethane-4,4'-diisocyanate, metaxylylene diisocyanate, hexamethylene-1,6-diisocyanate, 1,6-diisocyanatehexane, an adduct of tolylene diisocyanate and hexanetriol, an adduct of tolylene diisocyanate and trimethylolpropane, polyol-modified diphenylmethane-4,4'-diisocyanate, carbodiimide-modified diphenylmethane-4,4'-diisocyanate, isophorone diisocyanate, 1,5-naphthalene diisocyanate, 3,3'-bitrylene-4,4'-diisocyanate, 3,3'-dimethyldiphenylmethane-4,4'-diisocyanate, and metaphenylene diisocyanate. Blocked isocyanate compounds in which the isocyanate groups are blocked with bisulfites and sulfonic acid group-containing phenols, alcohols, lactams, oximes, active methylene compounds, and the like may also be used. An example of a commercially available polyfunctional isocyanate compound is "Basonate HW-100" manufactured by BASF.

[0062] As the polyfunctional aziridine compound, for example, N,N'-hexamethylene-1,6-bis-(1-aziridinecarboxamide), trimethylolpropane-tri-β-aziridinylpropionate, etc. can be used.

[0063] The carbodiimide group-containing compound is not particularly limited as long as it has one or more carbodiimide groups in the molecule. The carbodiimide compound forms an ester with two carboxyl groups in the acid-modified portion of the acid-modified polyolefin resin at one carbodiimide portion to achieve crosslinking. For example, compounds having carbodiimide groups such as p-phenylene-bis(2,6-xylylcarbodiimide), tetramethylene-bis(t-butylcarbodiimide), and cyclohexane-1,4-bis(methylene-t-butylcarbodiimide), and polycarbodiimide, which is a polymer having a carbodiimide group, can be used. One or more of these can be used. Among these, polycarbodiimide is preferred because of its ease of handling. Commercially available polycarbodiimide products include the Carbodilite series manufactured by Nisshinbo Corporation, specifically water-soluble types "SV-02", "V-02", "V-02-L2", and "V-04"; emulsion types "E-01" and "E-02"; organic solution types "V-01", "V-03", "V-07", and "V-09"; and solvent-free type "V-05".

[0064] The oxazoline group-containing compound is not particularly limited as long as it has two or more oxazoline groups in the molecule. In the oxazoline compound, each of the two oxazoline moieties forms an amide ester with one carboxyl group in the acid-modified portion of the acid-modified polyolefin resin to achieve crosslinking. Such a polymer can be prepared by polymerization of an addition-polymerizable oxazoline group-containing monomer alone or with other monomers. Examples of the addition-polymerizable oxazoline group-containing monomer include 2-vinyl-2-oxazoline, 2-vinyl-4-methyl-2-oxazoline, 2-vinyl-5-methyl-2-oxazoline, 2-isopropenyl-2-oxazoline, 2-isopropenyl-4-methyl-2-oxazoline, and 2-isopropenyl-5-ethyl-2-oxazoline. The addition-polymerizable oxazoline group-containing monomer can be one of these or a mixture of two or more of them. Among these, 2-isopropenyl-2-oxazoline is industrially easily available and is suitable.The other monomer is not limited as long as it is a monomer copolymerizable with the addition-polymerizable oxazoline group-containing monomer, and examples thereof include (meth)acrylic acid esters such as alkyl acrylate and alkyl methacrylate (alkyl groups include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, t-butyl, 2-ethylhexyl, and cyclohexyl groups); unsaturated carboxylic acids such as acrylic acid, methacrylic acid, itaconic acid, maleic acid, fumaric acid, crotonic acid, styrenesulfonic acid, and salts thereof (sodium salt, potassium salt, ammonium salt, tertiary amine salt, and the like); unsaturated nitriles such as acrylonitrile and methacrylonitrile; acrylamide, methacrylamide, N-alkane, etc. Examples of the monomer include unsaturated amides such as alkyl acrylamide, N-alkyl methacrylamide, N,N-dialkyl acrylamide, and N,N-dialkyl methacrylate (the alkyl group is a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a t-butyl group, a 2-ethylhexyl group, and a cyclohexyl group); vinyl esters such as vinyl acetate and vinyl propionate; vinyl ethers such as methyl vinyl ether and ethyl vinyl ether; α-olefins such as ethylene and propylene; halogen-containing α,β-unsaturated aliphatic monomers such as vinyl chloride, vinylidene chloride, and vinyl fluoride; and α,β-unsaturated aromatic monomers such as styrene and α-methylstyrene. As the other monomer, one or more of these monomers can be used. Among these, oxazoline group-containing polymers are preferred from the viewpoint of ease of handling. Commercially available oxazoline group-containing polymers include the Epocross series manufactured by Nippon Shokubai Co., Ltd., specifically water-soluble types "WS-500" and "WS-700"; emulsion types "K-1010E", "K-1020E", "K-1030E", "K-2010E", "K-2020E", and "K-2030E".

[0065] As the phenolic resin, for example, resol type phenolic resins and / or novolac type phenolic resins prepared using phenol, bisphenol A, alkylphenols such as pt-butylphenol, octylphenol, and p-cumylphenol, p-phenylphenol, cresol, and the like as raw materials can be used.

[0066] As the urea resin, for example, dimethylol urea, dimethylol ethylene urea, dimethylol propylene urea, tetramethylol acetylene urea, 4-methoxy 5-dimethyl propylene urea dimethylol can be used.

[0067] The melamine resin is, for example, a compound having an imino group, a methylol group, and / or an alkoxymethyl group (e.g., a methoxymethyl group, a butoxymethyl group) as a functional group in one molecule. As the melamine resin, imino group-type methylated melamine resin, methylol group-type methylated melamine resin, methylol group-type methylated melamine resin, fully alkylated methylated melamine resin, etc. can be used. Among them, methylolated melamine resin is most preferable. Furthermore, in order to promote the thermal curing of the melamine resin, it is preferable to use an acid catalyst such as p-toluenesulfonic acid.

[0068] As the benzoguanamine resin, for example, trimethylolbenzoguanamine, hexamethylolbenzoguanamine, trismethoxymethylbenzoguanamine, hexakismethoxymethylbenzoguanamine, etc. can be used.

[0069] (Characteristics of the release layer) In the present invention, the surface of the release layer constituting the outermost surface of the laminate film must have a surface roughness parameter Sa (arithmetic mean height) of 0.05 μm or less from the viewpoint of improving gas barrier properties, and is preferably 0.001 to 0.050 μm, more preferably 0.001 to 0.030 μm, and even more preferably 0.001 to 0.010 μm. By having the surface roughness of the release layer within the above range, even when the laminate film of the present invention is bonded to an adherend and heat-treated in an environment where oxygen is present, the laminate film of the present invention can protect the bonded adherend from oxygen without decreasing the oxygen barrier performance.

[0070] In the laminated film of the present invention, when an acrylic adherend as a pressure-sensitive adhesive material is attached to the release layer and measured, the peel strength between the release layer and the adherend is preferably 3.0 N / cm or less, more preferably 2.8 N / cm or less, and even more preferably 2.6 N / cm or less. If the peel strength exceeds 3.0 N / cm, the peel strength is heavy and it becomes difficult to practically use the film as a release film.

[0071] In the laminated film of the present invention, the peel strength between the release layer and the epoxy prepreg, measured by attaching the epoxy prepreg to the release layer, is preferably 1.5 N / cm or less, more preferably 0.01 to 1.0 N / cm, and even more preferably 0.02 to 0.8 N / cm. If the peel strength exceeds 1.5 N / cm, it becomes difficult to peel from the epoxy prepreg, and handling properties are reduced. The peel strength from the epoxy prepreg described above is measured by sandwiching the epoxy prepreg between a pair of release sheets and applying a pressure of 15 kg / cm. 2 The epoxy prepreg is cured by holding it at 190°C or 230°C for 70 minutes under a pressure of 1.0 mmHg, and then the measurement is performed.

[0072] In the present invention, the thickness of the release layer is preferably 0.01 to 1 μm, more preferably 0.03 to 0.7 μm, and further preferably 0.05 to 0.5 μm. If the thickness of the release layer is less than 0.01 μm, sufficient releasability cannot be obtained, and if it exceeds 1 μm, it is likely to transfer to the adherend and costs will increase, which is not preferable.

[0073] <Gas barrier layer> The laminate film of the present invention must have a gas barrier layer laminated thereon. The gas barrier layer needs to contain an organic compound from the viewpoints of adhesion to the substrate and resistance to breakage or cracking in the gas barrier layer even when the laminate film is used repeatedly.

[0074] The organic compound constituting the gas barrier layer is not particularly limited, and examples thereof include polyvinylidene chloride (PVDC), polyvinyl alcohol, copolymers of vinyl alcohol and ethylene (EVOH), polycarboxylic acids, etc. When a crosslinked structure is formed in the organic compound constituting the gas barrier layer, the gas barrier performance can be maintained even when used in a high temperature environment. Examples of organic compounds capable of forming a crosslinked structure include those containing polycarboxylic acid or anhydrides thereof.

[0075] (Polycarboxylic acids) Polycarboxylic acids are compounds having two or more carboxyl groups in the molecule, or anhydrides thereof. In the case of anhydrides, all carboxyl groups may have an anhydride structure, or some of the carboxyl groups may have an anhydride structure. Polycarboxylic acids may be in the form of either a monomer or a polymer.

[0076] Specific examples of polycarboxylic acids include a) monomer compounds such as 1,2,3,4-butanetetracarboxylic acid, b) homopolymers or copolymers of (meth)acrylic acid such as polyacrylic acid, polymethacrylic acid, acrylic acid-methacrylic acid copolymer, acrylic acid-maleic acid copolymer, and acrylic acid-maleic anhydride copolymer, c) olefin-maleic acid copolymers such as polymaleic acid, ethylene-maleic acid copolymer, and ethylene-maleic anhydride copolymer, d) polysaccharides having a carboxyl group in the side chain such as alginic acid, and e) polyamides or polyesters having a carboxyl group. These polycarboxylic acids can be used alone or in combination of two or more.

[0077] When the polycarboxylic acid is a polymer, its weight average molecular weight is not particularly limited, but is generally preferably 1,000 to 1,000,000, more preferably 10,000 to 150,000, and most preferably 15,000 to 110,000. If the weight average molecular weight of the polycarboxylic acid is too low, the resulting gas barrier layer will be fragile, while if the molecular weight is too high, handling properties will be impaired and, in some cases, the polycarboxylic acid may aggregate in a coating liquid for forming the gas barrier layer described below, impairing the gas barrier properties of the resulting gas barrier layer.

[0078] In the present invention, it is preferable to use an olefin-maleic acid copolymer as the polycarboxylic acid, and it is more preferable to use an ethylene-maleic acid copolymer (EMA). By using EMA, better gas barrier properties can be obtained. As EMA, known or commercially available EMA can be used. Also, EMA obtained by a known production method can be used, for example, a copolymer obtained by polymerizing maleic anhydride and ethylene by a method such as solution radical polymerization can be used.

[0079] The maleic acid unit in EMA is preferably 5 mol% or more, more preferably 20 mol% or more, even more preferably 30 mol% or more, and most preferably 35 mol% or more. In a dry state, the maleic acid unit in the olefin-maleic acid copolymer is likely to become a maleic anhydride structure in which adjacent carboxyl groups are dehydrated and cyclized, and when wet or in an aqueous solution, the ring opens to become a maleic acid structure. Therefore, in the present invention, unless otherwise specified, maleic acid units and maleic anhydride units are collectively referred to as maleic acid units.

[0080] The weight average molecular weight of EMA is usually about 1,000 to 1,000,000, preferably 3,000 to 500,000, more preferably 7,000 to 300,000, and most preferably 10,000 to 200,000.

[0081] The content of polycarboxylic acids in the gas barrier layer is not particularly limited and can be appropriately set depending on the type of polycarboxylic acid used, and is usually about 40 to 90 mass %, and preferably 50 to 80 mass %.

[0082] (Polyalcohol) The gas barrier layer in the laminated film of the present invention may contain other components (particularly, components that react with polycarboxylic acids to crosslink the polycarboxylic acids) together with the polycarboxylic acids. For example, in the laminated film of the present invention, the gas barrier layer preferably contains a polyalcohol or the like. The gas barrier layer can obtain higher gas barrier properties by containing a polyalcohol together with the polycarboxylic acids.

[0083] A polyalcohol is a compound having two or more hydroxyl groups in a molecule, and may be either a low molecular weight compound or a high molecular weight compound (polymer). Examples of the polyalcohol include sugar alcohols such as glycerin and pentaerythritol, monosaccharides such as glucose, disaccharides such as maltose, and oligosaccharides such as galactooligosaccharides. Examples of the high molecular weight compound include polyvinyl alcohol, ethylene-vinyl alcohol copolymer, and polysaccharides such as starch. The above polyalcohols can be used alone or in combination of two or more kinds.

[0084] When the polyalcohol is polyvinyl alcohol, ethylene-vinyl alcohol copolymer, etc., the saponification degree is not limited, but is usually preferably 95 mol% or more, more preferably 98 mol% or more. The average polymerization degree is preferably 50 to 2,000, more preferably 200 to 1,000. This allows for better gas barrier properties to be obtained.

[0085] The content of polyalcohol is not limited, but the molar ratio (OH group / COOH group) of the OH group contained in the polyalcohol to the COOH group contained in the polycarboxylic acid (in the case of anhydride, the anhydride group is calculated as two COOH groups) is preferably set to 0.01 to 20, more preferably set to 0.01 to 10, even more preferably set to 0.02 to 5, and most preferably set to 0.04 to 2. This allows for better gas barrier properties to be obtained.

[0086] (Crosslinking agent) The gas barrier layer in the present invention may contain a crosslinking agent. By containing a crosslinking agent, the gas barrier properties can be improved. The content of the crosslinking agent in the gas barrier layer is preferably 0.1 to 30 parts by mass, and more preferably 1 to 20 parts by mass, based on 100 parts by mass of the polycarboxylic acid. Examples of the crosslinking agent include a compound having self-crosslinking properties and a compound having multiple functional groups in the molecule that react with a carboxyl group, and when the gas barrier layer contains a polyalcohol, a compound having multiple functional groups in the molecule that react with a hydroxyl group may be used.Specific examples of the crosslinking agent include isocyanate compounds, melamine compounds, urea compounds, epoxy compounds, carbodiimide compounds, zirconium salt compounds such as ammonium zirconium carbonate, metal alkoxides, etc.These crosslinking agents may be used in combination.

[0087] Furthermore, by subjecting the polycarboxylic acids in the gas barrier layer to an ion crosslinking reaction with a metal compound (metal ion), it is possible to obtain better gas barrier properties.

[0088] The metal compound may be contained in the substrate or in an overcoat layer laminated on the gas barrier layer, but by containing the metal compound in the substrate, excellent barrier properties can be obtained. When the metal compound is contained in the substrate, it is necessary to ionically crosslink the polycarboxylic acid in the gas barrier layer with the metal compound, so that it is preferable that the gas barrier layer is laminated on the substrate.

[0089] The metal constituting the metal compound is not particularly limited, and examples thereof include monovalent metals such as lithium, sodium, potassium, rubidium, and cesium, and divalent or higher metals such as magnesium, calcium, zirconium, zinc, copper, cobalt, iron, nickel, and aluminum. The type of metal is not limited to one type, and may be two or more types.

[0090] Among these, metals with high ionization tendency are preferred because they react easily with polycarboxylic acids constituting the gas barrier layer, and divalent metals are preferred from the viewpoint of gas barrier properties. Therefore, for example, at least one of lithium, sodium, potassium, magnesium, calcium, and zinc is preferred, and at least one of magnesium, calcium, and zinc is more preferred.

[0091] In the present invention, the metal compound is not particularly limited as long as it is a compound containing the above-mentioned metal. Examples include oxides, hydroxides, halides, inorganic acid salts (carbonates, hydrogencarbonates, phosphates, sulfates, etc.), and organic acid salts (carboxylates (acetates, formates, stearates, citrates, malates, maleates), sulfonates, etc.). In the present invention, oxides or carbonates are particularly preferred in terms of exhibiting excellent gas barrier properties.

[0092] Among the above metal compounds, preferred examples include at least one of lithium carbonate, sodium hydrogen carbonate, magnesium oxide, magnesium carbonate, magnesium hydroxide, magnesium acetate, calcium oxide, calcium carbonate, calcium hydroxide, calcium chloride, calcium phosphate, calcium sulfate, calcium acetate, zinc acetate, zinc oxide, and zinc carbonate.

[0093] From the viewpoint of gas barrier properties, divalent metal compounds are preferred, and it is more preferred to use at least one of magnesium compounds, calcium compounds, and zinc compounds.Therefore, for example, at least one of magnesium oxide, magnesium carbonate, magnesium hydroxide, magnesium acetate, calcium oxide, calcium carbonate, calcium acetate, zinc oxide, and zinc acetate can be preferably used.In addition, from the viewpoint of the transparency of the substrate, at least one of monovalent metal compounds and divalent metal compounds is preferred, and at least one of alkali metal compounds and alkaline earth metal compounds is more preferred.Therefore, for example, at least one of lithium carbonate, sodium bicarbonate, magnesium oxide, magnesium carbonate, and magnesium hydroxide can be preferably used.

[0094] The metal compound may be subjected to a surface treatment (surface film formation treatment) as necessary. This can improve dispersibility, weather resistance, wettability with thermoplastic resin, heat resistance, transparency, etc. The surface treatment may be a known inorganic or organic treatment. Examples of the inorganic treatment include a treatment in which alumina, silica, titania, zirconia, tin oxide, antimony oxide, zinc oxide, etc. are formed on the particle surface of the metal compound. Examples of the organic treatment include a treatment in which a fatty acid compound, a polyol compound such as pentaerythritol, trimethylolpropane, etc., an amine compound such as triethanolamine, trimethylolamine, etc., a silicone resin, a silicone-based compound such as alkylchlorosilane, etc. are formed on the particle surface of the metal compound.

[0095] The content of the metal compound in the substrate is usually 0.1 to 20% by mass, preferably 0.1 to 18% by mass, more preferably 0.2 to 15% by mass, and even more preferably 0.3 to 10% by mass, and from the viewpoint of haze, it is preferably 5% by mass or less. When the content of the metal compound is 0.1 to 20% by mass, excellent gas barrier properties and mechanical properties can be obtained. On the other hand, when the content of the metal compound is less than 0.1% by mass, the ion crosslinked structure formed by reaction with the polycarboxylic acid in the gas barrier layer is reduced, and the desired gas barrier properties cannot be obtained. On the other hand, when the content exceeds 20% by mass, the frequency of breakage during stretching during film formation increases, the productivity is likely to decrease, and the mechanical properties are also likely to decrease.

[0096] (Additives) The gas barrier layer may contain, for example, a heat stabilizer, an antioxidant, a reinforcing agent, a pigment, an anti-deterioration agent, a weather resistance agent, a flame retardant, a plasticizer, a release agent, a lubricant, a preservative, an antifoaming agent, a wetting agent, a viscosity adjuster, and the like, as long as the gas barrier property, adhesion to the substrate, and the like are not significantly impaired.

[0097] Examples of the heat stabilizer, antioxidant, and deterioration inhibitor include hindered phenols, phosphorus compounds, hindered amines, sulfur compounds, copper compounds, and alkali metal halides, and these may be used in combination.

[0098] Examples of reinforcing materials include clay, talc, wollastonite, silica, alumina, calcium silicate, sodium aluminate, sodium aluminosilicate, magnesium silicate, glass balloons, carbon black, zeolite, montmorillonite, hydrotalcite, fluorine mica, metal fibers, metal whiskers, ceramic whiskers, potassium titanate whiskers, boron nitride, graphite, glass fibers, carbon fibers, fullerenes (C60, C70, etc.), and carbon nanotubes.

[0099] The thickness of the gas barrier layer is preferably 0.05 μm or more in order to more reliably obtain the gas barrier properties of the laminated film. The upper limit of the thickness is not particularly limited, but is preferably about 5 μm from the standpoint of economy and the like.

[0100] <Laminated film> The laminated film of the present invention includes a release layer, a substrate, and a gas barrier layer, and at least one of the outermost layers is a release layer. As long as the effects of the present invention are not impaired, other layers may be laminated between the release layer and the substrate layer, between the release layer and the gas barrier layer, between the substrate and the gas barrier layer, or on the surface of the laminated film on which the release layer is not laminated. Examples of layers laminated between the layers include an easy-adhesion layer, and examples of layers laminated on the surface include an antistatic layer.

[0101] The laminated film of the present invention can maintain its oxygen barrier performance even when it is attached to an adherend and heat-treated (for example, at 180°C for 30 minutes) in an environment where oxygen is present. When the surface roughness parameter Sa (arithmetic mean height) of the release layer surface of a release film laminated with a gas barrier layer exceeds 0.05 μm, the transparency of the adherend may decrease during heat treatment in an environment where oxygen is present. The laminated film of the present invention maintains its oxygen barrier performance even when it is attached to an adherend and heat-treated at 180°C for 30 minutes in an environment where oxygen is present, and therefore can suppress an increase in the haze of the adherend.

[0102] Since the gas barrier layer of the laminated film of the present invention contains an organic compound, the gas barrier layer is less likely to break or crack, and the laminated film exhibits good oxygen barrier properties even when repeatedly used as a release film. Specifically, the oxygen permeability of the laminated film in an atmosphere of 20°C and 85% RH after 300,000 times of folding and bending tests using a durability tester is 50 cc / (m 2 ·atm·day) or less, and more preferably 20cc / (m 2 ·atm·day) or less is preferable, and 10cc / (m 2 ·atm·day) or less is even more preferable.

[0103] <Laminated film manufacturing method> As an example of the laminate film of the present invention, a laminate film having a structure of a release layer / substrate / gas barrier layer will be given and its production method will be described below. The method for producing a laminated film of the present invention includes a step of applying a release layer-forming liquid material to one side of a substrate, a step of drying and stretching the substrate coated with the release layer-forming liquid material, and a step of applying a gas barrier layer-forming liquid material to one side of a substrate, and drying and stretching the substrate coated with the gas barrier layer-forming liquid material.

[0104] In the present invention, the liquid medium constituting the liquid material for forming the release layer or the liquid material for forming the gas barrier layer is preferably an aqueous medium. The aqueous medium means a solvent containing water and an amphipathic organic solvent and having a water content of 2% by mass or more, or may be water alone. An amphipathic organic solvent refers to an organic solvent in which the solubility of water in the organic solvent at 20°C is 5 mass% or more (the solubility of water in organic solvents at 20°C is described in literature such as "Solvent Handbook" (Kodansha Scientific, 10th edition, 1990)). Specific examples of amphipathic organic solvents include alcohols such as methanol, ethanol, n-propanol, and isopropanol; ethers such as tetrahydrofuran and 1,4-dioxane; ketones such as acetone and methyl ethyl ketone; esters such as methyl acetate, n-propyl acetate, isopropyl acetate, methyl propionate, ethyl propionate, and dimethyl carbonate; ethylene glycol derivatives such as ethylene glycol n-butyl ether; organic amine compounds containing ammonia such as diethylamine, triethylamine, diethanolamine, triethanolamine, N,N-dimethylethanolamine, and N,N-diethylethanolamine; and lactams such as 2-pyrrolidone and N-methyl-2-pyrrolidone.

[0105] The liquid material for forming the release layer can be prepared, for example, by adding polyvinyl alcohol and a crosslinking agent to a liquid material of an acid-modified polyolefin resin, although the method is not limited to this. The liquid of the acid-modified polyolefin resin may be an aqueous dispersion of the acid-modified polyolefin resin. The method for dispersing the acid-modified polyolefin resin in water is not particularly limited, but may be, for example, the method described in International Publication No. 02 / 055598. The particle size of the acid-modified polyolefin resin dispersed in the aqueous medium is preferably 1 μm or less, more preferably 0.8 μm or less, in terms of stability when mixed with other components and storage stability after mixing. Such a particle size can be achieved by the manufacturing method described in International Publication No. 02 / 055598. The number average particle size of the acid-modified polyolefin resin is measured by dynamic light scattering. The solids concentration of the aqueous dispersion of the acid-modified polyolefin resin is not particularly limited, but in order to maintain the viscosity of the aqueous dispersion at an appropriate level, it is preferably 1 to 60% by mass, and more preferably 5 to 30% by mass.

[0106] The solid content concentration of the liquid material for forming the release layer is not particularly limited and can be appropriately selected depending on lamination conditions, the desired thickness and performance, etc. However, in order to maintain the viscosity of the liquid material at an appropriate level and form a uniform release layer, the solid content is preferably 2 to 30% by mass, more preferably 3 to 20% by mass. The release layer-forming liquid may contain additives such as antioxidants, ultraviolet absorbers, lubricants, and colorants, provided that the properties of the liquid are not impaired.

[0107] In the present invention, the method for applying the release layer-forming liquid material or the gas barrier layer-forming liquid material to the substrate may be a known method, such as gravure roll coating, reverse roll coating, wire bar coating, lip coating, air knife coating, curtain flow coating, spray coating, dip coating, brush coating, etc. In applying the release layer-forming liquid material, gravure roll coating is particularly effective because it can suppress the occurrence of minute non-planar shapes in the coating film.

[0108] Known methods for applying a liquid include an offline method in which a liquid is applied to a previously stretched film, and an in-line method in which a substrate film coated with the liquid is dried and stretched. In the present invention, the liquid is preferably applied by the in-line method from the viewpoint of reducing the surface roughness parameter Sa of the release layer surface and improving the barrier properties. When the liquid is applied by the in-line method, the dispersed particles dispersed in the liquid can form a film simultaneously with the stretching of the coating applied to the substrate film due to the heat during stretching, and the particles fuse together, thereby reducing the surface roughness parameter Sa.

[0109] The laminated film of the present invention can be suitably used for applications such as protective films for double-sided tapes and adhesive materials, protective materials and process materials when producing liquid crystal display components, printed wiring boards, and the like, and for forming sheet-like structures such as ion exchange membranes, ceramic green sheets, and heat dissipation sheets. EXAMPLES

[0110] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these. The properties of the raw materials and the laminated film were measured by the following methods.

[0111] (1) Saponification rate of polyvinyl alcohol The saponification rate of polyvinyl alcohol was measured in accordance with JIS K-6726.

[0112] (2) Surface roughness parameter Sa (arithmetic mean height) Using a Talysurf CCI6000 manufactured by Taylor / Hobson, the surface roughness parameter Sa (arithmetic mean height, μm) was measured at 10 points on the surface of the release layer of the laminated film under the following conditions, and the average was calculated. Measurement length: 0.66mm x 0.66mm Cutoff: Robust Gaussian filter, 0.25mm

[0113] (3) Releasability for acrylic adhesives A 50 mm wide, 150 mm long acrylic adhesive tape (Nitto Denko No. 31B / acrylic adhesive) was pressed with a rubber roll onto the release layer side of the obtained laminated film to prepare a sample. The sample was sandwiched in the form of metal plate / rubber plate / sample / rubber plate / metal plate and left under a load of 2 kPa in an atmosphere of 70°C for 20 hours, and then cooled for 30 minutes or more to return to room temperature to obtain a sample for peel strength measurement. The peel strength between the acrylic adhesive tape and the laminated film of the peel strength measurement sample was measured in a thermostatic chamber at 23°C using a tensile tester (Shimadzu Corporation Autograph AGS-100B) at a peel angle of 180 degrees and a peel speed of 300 mm / min.

[0114] (4) Releasability to epoxy prepreg Both sides of an epoxy prepreg (EI-6765, manufactured by Sumitomo Bakelite Co., Ltd.) measuring 60 mm x 100 mm were sandwiched between the release layer side of the laminated film obtained, and the temperature was raised from 30°C to 150°C at a rate of 15°C / min in a vacuum press at 1.07 kPa (8 Torr), and after holding at 150°C for 22 minutes, the temperature was further raised to 190°C at a rate of 5°C / min and then compressed under a pressure of 5 kg / cm. 2 After applying a pressure of 15kg / cm for 10 minutes, 2 The sample was then cooled to room temperature and held at 190°C for 70 minutes while applying a pressure of 1.0 MPa. The peel strength between the cured epoxy prepreg and the laminated film of the obtained sample was measured using a tensile tester (Shimadzu Corporation Autograph AGS-100B) in a thermostatic room at 23° C. The peel angle was 180 degrees and the peel speed was 300 mm / min.

[0115] (5) Releasability of epoxy prepreg after high-temperature treatment In the above (4), the specimen was prepared at a pressure of 15 kg / cm 2 The condition of "holding at 190°C for 70 minutes while applying a pressure of 15 kg / cm 2 A sample was prepared in the same manner, except that the conditions were changed to "hold at 230°C for 70 minutes while applying a pressure of 100 MPa." The peel strength was measured.

[0116] (6) Oxygen permeability The oxygen permeability of the obtained laminated film was measured in an atmosphere of a temperature of 20° C. and a relative humidity of 0% according to the JIS K7126-2 method using an oxygen barrier measuring device (OX-TRAN 2 / 20MH) manufactured by Mocon.

[0117] (7) Bending resistance of the gas barrier layer The obtained laminated film was cut into a rectangle of 80 mm x 100 mm to prepare a test piece. The prepared test specimens were thoroughly conditioned at a temperature of 20°C and a humidity of 65% RH, and then attached to a durability testing machine (Yuasa System Co., Ltd., DLDMLH-FU type) with a bending radius of 3.0 mm. A bending test was then performed in the same atmosphere, in which the entire surface was folded 180° 300,000 times. Thereafter, the oxygen permeability was measured under the same conditions as in (6) using an oxygen barrier measuring device (OX-TRAN2 / 20, manufactured by Mocon).

[0118] (8) Oxygen permeability after high-temperature treatment The obtained laminated film was placed in an oven at 230° C. and subjected to a heat treatment for 30 minutes, after which the oxygen permeability was measured under the same conditions as in (6) using an oxygen barrier measuring device (OX-TRAN 2 / 20MH) manufactured by Mocon.

[0119] (9) Gas barrier performance (haze change) Based on JIS-K7136:2000, the haze values ​​before and after the heat treatment were measured using a haze meter NDH4000 (manufactured by Nippon Denshoku Industries Co., Ltd.) in the following manner, and the difference therebetween was taken as the amount of haze change. Both sides of a heat-resistant transparent adhesive sheet (LUCIACS CS9621T manufactured by Nitto Denko) (200 mm x 200 mm) were sandwiched between the release layer side of the obtained laminated film (200 mm x 200 mm) and pressed with a rubber roll to attach the laminated film. The haze value of the transparent adhesive sheet with the laminated film attached was measured. Next, the transparent adhesive sheet with the laminated film attached was placed in an oven and heated for 30 minutes at 180°C in Examples 1 to 12 and Comparative Examples 1 to 9, and heated for 30 minutes at 230°C in Examples 13 to 17 and Comparative Examples 10 to 11. After the heat treatment, the haze value was measured for the central part (50 mm x 100 mm) of the transparent adhesive sheet with the laminated film attached. The difference in the haze value before and after the heat treatment was calculated as the amount of change in haze, and the gas barrier performance of the laminated film was evaluated. The heat treatment was performed in an atmosphere containing oxygen. The amount of change in haze before and after the heat treatment is preferably 2.0% or less, more preferably 1.0% or less, and most preferably 0.5% or less.

[0120] A material for preparing a liquid for forming a release layer was produced by the following method.

[0121] <Production of Acid-Modified Polyolefin Resin A-1> 280 g of propylene-butene-ethylene terpolymer (propylene / butene / ethylene=68.0 / 16.0 / 16.0 (mass ratio)) was heated and melted in a four-neck flask under a nitrogen atmosphere, and then 32.0 g of maleic anhydride as an unsaturated carboxylic acid and 6.0 g of dicumyl peroxide as a radical generator were added over 1 hour while stirring while maintaining the temperature in the system at 170°C, and then reacted for 1 hour. After the reaction was completed, the reaction product obtained was poured into a large amount of acetone to precipitate a resin. This resin was further washed several times with acetone to remove unreacted maleic anhydride, and then dried under reduced pressure in a vacuum dryer to obtain an acid-modified polyolefin resin A-1 (acid modification amount 7.0%, melting point 135°C).

[0122] <Production of Acid-Modified Polyolefin Resins A-2 and A-3> In the production of the above acid-modified polyolefin resin A-1, except that the propylene-butene-ethylene terpolymer (propylene / butene / ethylene = 68.0 / 16.0 / 16.0 (mass ratio)) was changed to a propylene-ethylene copolymer (propylene / ethylene = 99 / 1 (mass ratio)), the same procedure was used to obtain acid-modified polyolefin resin A-2 (acid modification amount 2.3%, melting point 145°C). Also, acid-modified polyolefin resin A-3 (acid modification amount 2.0%, melting point 105° C.) was obtained in the same manner, except that the copolymer was changed to an ethylene-ethyl acrylate copolymer (ethylene / ethyl acrylate=93 / 7 (mass ratio)).

[0123] <Production of Aqueous Dispersion of Acid-Modified Polyolefin Resin A-1> Using a stirrer equipped with a sealable pressure-resistant 1-liter glass container with a heater, 60.0 g of the acid-modified polyolefin resin A-1 produced by the above method, 45.0 g of ethylene glycol-n-butyl ether (boiling point 171 ° C), 6.9 g of N,N-dimethylethanolamine (boiling point 134 ° C, 1.0 times equivalent to the carboxyl group of the maleic anhydride unit in the resin), and 188.1 g of distilled water were charged into the above glass container, and the stirring blade rotation speed was set to 300 rpm and stirred. As a result, no resin precipitation was observed at the bottom of the container, and it was confirmed that the resin was in a floating state. Therefore, while maintaining this state, the heater was turned on after 10 minutes and heated. Then, the temperature inside the system was kept at 140 ° C and stirred for another 60 minutes. After that, the mixture was cooled to room temperature (about 25 ° C) by air cooling while stirring at a rotation speed of 300 rpm. Further, pressure filtration (air pressure 0.2 MPa) was performed using a 300 mesh stainless steel filter (wire diameter 0.035 mm, plain weave) to obtain a uniform aqueous dispersion of acid-modified polyolefin resin A-1 (solid content concentration 25% by mass). There was almost no residual resin on the filter.

[0124] <Production of Aqueous Dispersions of Acid-Modified Polyolefin Resins A-2 and A-3> Except for changing the acid-modified polyolefin resins used to A-2 and A-3, aqueous dispersions of acid-modified polyolefin resins A-2 and A-3 (solid content concentration 25% by mass) were obtained in the same manner as described above.

[0125] <Production of long-chain alkyl group-containing compound A-4> 200 parts of xylene and 600 parts of octadecyl isocyanate were added to a four-neck flask and heated under stirring. From the point when xylene started to reflux, 100 parts of polyvinyl alcohol with an average degree of polymerization of 500 and a degree of saponification of 88 mol% were added little by little at 10-minute intervals over about 2 hours. After the addition of polyvinyl alcohol was completed, the mixture was refluxed for another 2 hours to terminate the reaction. The reaction mixture was cooled to about 80°C and then added to methanol, whereupon the reaction product precipitated as a white precipitate. The precipitate was filtered off, 140 parts of xylene was added, heated to completely dissolve the product, and then methanol was added again to cause precipitation. This operation was repeated several times, and the precipitate was washed with methanol, dried, and pulverized to obtain polymer compound A-4 having a long-chain alkyl group on the side chain.

[0126] As polyvinyl alcohol for preparing the liquid material for forming the release layer, the following aqueous solution was used. JT-05: JT-05 manufactured by Japan Vinyl Acetate & Poval, saponification rate 94.5%, polymerization degree 500, solid content concentration 8% by mass VC-10: VC-10 manufactured by Japan Vinyl Acetate & Poval, saponification rate 99.3%, polymerization degree 1,000, solids concentration 8% by mass

[0127] The following crosslinking agents were used: WS-700: Nippon Shokubai Epocross WS-700, an aqueous solution of an oxazoline group-containing compound, solids concentration 25% by mass

[0128] A liquid material for forming a gas barrier layer was produced by the following method.

[0129] <Production of Liquid Material B-1 for Forming Gas Barrier Layer> A 20% by mass aqueous solution of polyvinyl alcohol was prepared using polyvinyl alcohol (VC-10 manufactured by Nippon Vinyl Acetate & Poval Co., Ltd.) with a degree of polymerization of 1000 and a saponification rate of 99.3% as a solution containing compound (A). Also, a 1,2,3,4-butanetetracarboxylic acid (Rikacid BTW manufactured by New Japan Chemical Co., Ltd.) was used as a solution containing compound (B), and an aqueous solution containing 10 mol % sodium hydroxide based on the carboxyl groups of compound (B) was prepared. Then, the aqueous solutions of compound (A) and compound (B) were mixed and stirred so that the mass ratio of compound (A) / compound (B) was 30 / 70, thereby producing liquid material B-1 for forming a gas barrier layer having a solid content of 20 mass%.

[0130] <Production of Liquid Material B-2 for Forming Gas Barrier Layer> An ethylene-maleic acid copolymer (weight average molecular weight 60,000) and polyvinyl alcohol ("Poval 105" manufactured by Kuraray Co., Ltd., saponification degree 98-99%, average polymerization degree approximately 500) were mixed at a mass ratio (solid content) of 70 / 30 to produce liquid material B-2 for forming a gas barrier layer with a solid content of 10 mass %.

[0131] The semi-aromatic polyamide resin constituting the substrate was produced by the following method. <Production of Polyamide 9T> 3289 parts by mass of terephthalic acid (TA), 2533 parts by mass of 1,9-nonanediamine (NDA), 633 parts by mass of 2-methyl-1,8-octanediamine (MODA), 48.9 parts by mass of benzoic acid (BA), 6.5 parts by mass of sodium hypophosphite monohydrate (0.1% by mass relative to the total of the four polyamide raw materials) and 2200 parts by mass of distilled water were placed in a reactor and substituted with nitrogen. The molar ratio of these raw materials (TA / BA / NDA / MODA) was 99 / 2 / 80 / 20. The contents of the reactor were stirred at 100°C for 30 minutes, and then the internal temperature was raised to 210°C over 2 hours. At this time, the internal pressure of the reactor was 2.12 MPa (22 kg / cm 2 The reaction was continued for 1 hour, after which the temperature was raised to 230°C and kept at 230°C for another 2 hours. The steam was gradually released and the pressure was reduced to 2.12MPa (22kg / cm 2 The reaction was carried out while maintaining the pressure at 0.98 MPa (10 kg / cm) for 30 minutes. 2 ) and reacted for another hour to obtain a prepolymer, which was then dried at 100°C under reduced pressure for 12 hours and then crushed to a size of 2 mm or less. The pulverized prepolymer was then subjected to solid-phase polymerization for 10 hours at a temperature of 230°C and a pressure of 13.3 Pa (0.1 mmHg) to obtain a polymer. This was fed to a twin-screw extruder ("TEX44C" manufactured by Japan Steel Works, Ltd.), melt-kneaded and extruded at a cylinder temperature of 320°C, cooled, and cut to produce pellets of polyamide 9T.

[0132] <Polyamide 10T> 489 parts by mass of terephthalic acid (TA), 507 parts by mass of 1,10-decanediamine (DDA), 2.8 parts by mass of benzoic acid (BA), 1.0 part by mass of sodium hypophosphite monohydrate (0.1% by mass relative to the total of the three polyamide raw materials) and 1000 parts by mass of distilled water were placed in a reactor and substituted with nitrogen. The molar ratio of these raw materials (TA / BA / DDA) was 99 / 2 / 100. The contents of the reaction vessel were stirred at 28 revolutions per minute at 80° C. for 0.5 hours, and then heated to 230° C. Then, the contents were heated at 230° C. for 3 hours. After that, the contents were cooled and the reaction product was taken out. The reaction product was pulverized and then heated in a dryer under a nitrogen stream at 220°C for 5 hours to obtain a polymer by solid-state polymerization. The polymer was fed to a twin-screw extruder (TEX44C, manufactured by Japan Steel Works, Ltd.), melt-kneaded and extruded under a cylinder temperature of 320°C, cooled, and cut to produce pellets of polyamide 10T.

[0133] Example 1 <Preparation of liquid for forming release layer> An aqueous dispersion of acid-modified polyolefin resin A-1, an aqueous polyvinyl alcohol solution "JT-05", and an aqueous solution of an oxazoline group-containing compound as a crosslinking agent "WS-700" were mixed to solid contents of 100 parts by mass, 500 parts by mass, and 7 parts by mass, respectively, and the final solid concentration was adjusted with water to 6.5% by mass, thereby obtaining a liquid for forming a release layer. <Manufacturing of laminated film> As the polyethylene terephthalate (A), a polyethylene terephthalate resin was used in which 0.07 mass % of silica particles having a particle diameter of 2.3 μm was added to the polyethylene terephthalate (B) described below. As the polyethylene terephthalate (B), a polyethylene terephthalate resin having a polymerization catalyst of antimony trioxide, an intrinsic viscosity of 0.67, a glass transition temperature of 78°C, and a melting point of 253°C was used. Polyethylene terephthalate (B) was fed into extruder I (screw diameter: 50 mm), and polyethylene terephthalate (A) was fed into extruder II (screw diameter: 65 mm), respectively, and melted at 280°C. Before reaching the outlet of the T-die, the two melts were joined and laminated in two layers so that the layer thickness ratio (I / II) was 33 / 5 and the total thickness was 600 μm. The laminated melt was extruded from the outlet of the T-die of the multi-layer die, and was rapidly cooled in close contact with a casting drum by the T-die method-electrostatic pinning method, forming an unstretched film with a thickness of 600 μm. Then, this unstretched film was stretched 3.5 times with longitudinal stretching rolls heated to 90°C. On one side of the longitudinally stretched film (the side of the layer made of polyethylene terephthalate (A)), the gas barrier layer-forming liquid material B-1 was applied at a rate of 5 g / m using a reverse gravure coater. 2 (wet equivalent), and then apply the release layer forming liquid to the opposite side (the side of the layer made of polyethylene terephthalate (B)) using a reverse gravure coater at a rate of 5 g / m 2 The longitudinally stretched film coated with the gas barrier layer forming liquid and the release layer forming liquid was stretched 4.5 times at 120°C in a transverse stretching tenter, then heat-treated at 230°C for 10 seconds, cooled and wound up. The thickness of the obtained laminated film was 38 μm, and the thicknesses of the release layer and gas barrier layer on both sides were approximately 0.08 μm.

[0134] Examples 2 to 6 A laminated film was obtained in the same manner as in Example 1, except that the release layer-forming liquid material was changed to one having the composition shown in Table 1.

[0135] Example 7 A laminated film was obtained in the same manner as in Example 3, except that polyethylene terephthalate (A) was a polyethylene terephthalate resin obtained by adding 0.07 mass% of silica particles having a particle diameter of 2.3 μm and 0.5 mass% of magnesium oxide to polyethylene terephthalate (B) and that aqueous dispersion B-2 for forming a gas barrier layer was used.

[0136] Examples 8 to 10 A laminated film was obtained in the same manner as in Example 7, except that the release layer-forming liquid material was changed to one having the composition shown in Table 1.

[0137] Examples 11-12 In the same manner as in Example 1, an unstretched film was obtained. The unstretched film was stretched 3.5 times at 90° C. using a roll-type longitudinal stretching machine to obtain a stretched film. The longitudinally stretched film was stretched 4.5 times at 120° C. in a transverse stretching tenter, then heat-treated at 230° C. for 10 seconds, cooled, and wound up. The thickness of the obtained biaxially stretched film was 38 μm. A release layer-forming liquid having the composition shown in Table 1 was applied to one side (the side of the layer made of polyethylene terephthalate (B)) of the obtained biaxially stretched film using a Mayer bar, and dried for 90 seconds at 150° C. Thereafter, a gas barrier layer-forming liquid B-1 was applied to one side (the side of the layer made of polyethylene terephthalate (A)) of the biaxially stretched film using a Mayer bar, and dried for 90 seconds at 150° C. Thereafter, aging was carried out at 50° C. for 2 days to obtain a laminated film in which a 0.6 μm-thick release layer and a 0.6 μm-thick gas barrier layer were provided on both sides of a 38 μm-thick polyester film.

[0138] Example 13 Polyamide 9T was put into extruder I (screw diameter: 50 mm), and polyamide 9T (A) containing 0.07% by mass of silica particles having a particle diameter of 2.3 μm was put into extruder II (screw diameter: 65 mm), and melted by setting the cylinder temperature to 295 ° C (front stage), 320 ° C (middle stage), and 320 ° C (rear stage). After melting at 320 ° C, each melt was merged and laminated in two layers before reaching the outlet of the T-die so that the layer thickness ratio (I / II) was 33 / 5 and the total thickness was 600 μm. The laminated melt was extruded from the T-die outlet of a multi-layer die set at 320 ° C, pressed against a cooling roll with a circulating oil temperature set at 50 ° C by electrostatic application, and cooled to form an unstretched film with a thickness of 600 μm. The cooling roll used had its surface coated with ceramic (Al2O3) to a thickness of 0.15 mm. Two carbon brushes were placed in line upstream of the contact point between the roll surface and the film and brought into contact with the cooling roll, and the holders of the carbon brushes were grounded to remove static electricity from the surface of the ceramic coating layer. Tungsten wires with a diameter of 0.2 mm were used as electrodes, and a voltage of 6.5 kV was applied using a 300 W (15 kV x 20 mA) DC high voltage generator. Next, the gas barrier layer-forming liquid material B-1 was applied at a rate of 10 g / m2 to one side of the film (the side of the layer made of polyamide 9T(A)) using a reverse gravure coater. 2 (wet equivalent), and then, using a reverse gravure coater, 10 g / m of a release layer-forming liquid having the composition shown in Table 1 was applied to the opposite side (the side of the layer made of polyamide 9T). 2After coating to a coating amount of 1000 g (WET equivalent), the unstretched film coated with the liquid for forming the gas barrier layer and the liquid for forming the release layer was introduced into a tenter-type simultaneous biaxial stretching machine (manufactured by Hitachi, Ltd.) while holding both ends with clips, and simultaneously biaxially stretched at a preheating section temperature of 120°C, a stretching section temperature of 130°C, a longitudinal stretching strain rate of 2400% / min, a transverse stretching strain rate of 2760% / min, a longitudinal stretching ratio of 3.0 times, and a transverse stretching ratio of 3.3 times. Then, heat fixing was performed at 285°C in the tenter, and a 5% relaxation treatment was performed in the width direction of the film, followed by uniform gradual cooling, both ends of the film were released from the clips, the ears were trimmed, and the film was wound up to a width of 0.5 m and a length of 500 m. The thickness of the obtained laminated film was 38 μm, and the thicknesses of the release layer and gas barrier layer on both sides were approximately 0.08 μm.

[0139] Example 14 A laminated film was obtained in the same manner as in Example 13, except that the release layer-forming liquid material was changed to the composition shown in Table 1.

[0140] Example 15 A laminated film was obtained in the same manner as in Example 13, except that polyamide 9T (A) was a polyamide 9T resin containing 0.07 mass% silica particles having a particle diameter of 2.3 μm and 0.5 mass% magnesium oxide, and that aqueous dispersion B-2 for forming a gas barrier layer was used.

[0141] Examples 16-17 A laminated film was obtained in the same manner as in Example 13, except that the resin constituting the substrate was changed from polyamide 9T to polyamide 10T in Example 16 and to polyamide 6T (Arlen, manufactured by Mitsui Chemicals, Inc.) in Example 17.

[0142] Comparative Examples 1 to 4 and 7 In the same manner as in Example 1, an unstretched film was obtained. The unstretched film was stretched 3.5 times at 90° C. using a roll-type longitudinal stretching machine to obtain a stretched film. In Comparative Examples 1 to 4, the stretched film was coated with only the release layer-forming liquid material having the composition shown in Table 1, stretched 4.5 times at 120°C in a transverse stretching tenter, heat-treated at 230°C for 10 seconds, cooled, and wound up. The thickness of the obtained laminated film was 38 μm, and the thickness of the release layer was approximately 0.08 μm. In Comparative Example 7, a laminate film having a thickness of 38 μm and having only a gas barrier layer without a release layer was obtained in the same manner except that only the liquid material for forming a barrier layer was applied. The thickness of the gas barrier layer was about 0.08 μm.

[0143] Comparative Example 5 In Example 2, polyethylene terephthalate (B) was fed into extruder I, and polyethylene terephthalate (A) containing 0.07% by mass of silica particles having a particle diameter of 2.3 μm was fed into extruder II, respectively, and melted at 280°C. Then, before reaching the outlet of the T-die of the multilayer die, the layers were laminated together in three layers so that the layer thickness ratio (II / I / II) was 5 / 28 / 5 and the total thickness was 600 μm. The laminated melt was extruded from the T-die outlet of the multilayer die, and was rapidly cooled in close contact with a casting drum by the T-die method-electrostatic pinning method, to form an unstretched film having a thickness of 600 μm. Then, this unstretched film was stretched 3.5 times with longitudinal stretching rolls heated to 90°C. Thus, a longitudinally stretched film was obtained. A laminated film was obtained in the same manner as in Example 2, except that the aqueous dispersion for forming a gas barrier layer and the liquid material for forming a release layer were applied to one side of the longitudinally stretched film.

[0144] Comparative Example 6 A laminated film was obtained in the same manner as in Comparative Example 5, except that a polyethylene terephthalate resin containing 0.07 mass% silica particles having a particle diameter of 2.3 μm and 0.5 mass% magnesium oxide in polyethylene terephthalate (B) was used as polyethylene terephthalate (A).

[0145] Comparative Example 8 Using the laminate film produced in Comparative Example 3, which had only the release layer laminated thereon, a 6 nm-thick aluminum oxide thin film layer was laminated on the opposite side of the release layer as a gas barrier layer made of metal oxide by vacuum deposition while introducing oxygen gas using a vacuum deposition machine. Next, a mixed resin obtained by mixing 100 parts by mass of a water-based urethane resin (Takelac WPB341 manufactured by Mitsui Chemicals) and 10 parts by mass of an isocyanate-based silane coupling agent (KBE9007 manufactured by Shin-Etsu Chemical Co., Ltd.) was applied onto the aluminum oxide thin film layer by gravure coating to laminate a top coat layer having a thickness of 0.2 μm, thereby obtaining a laminated film.

[0146] Comparative Example 9 A release layer-forming liquid having the composition shown in Table 1 was applied to one side of a biaxially stretched polyester resin film (Unitika Ltd. "Emblett PET-12", thickness 12 μm) using a Mayer bar, and dried at 150° C. for 90 seconds. Thereafter, gas barrier layer-forming liquid B-1 was applied to one side of the biaxially stretched film using a Mayer bar, and dried at 150° C. for 90 seconds. Thereafter, aging was performed at 50° C. for 2 days to obtain a release film in which a 0.6 μm-thick release layer and a 0.6 μm-thick gas barrier layer were provided on both sides of a 12 μm-thick polyester film.

[0147] Comparative Examples 10 to 11 In Examples 13 and 16, a laminate film was prepared by stretching an unstretched film to which only the liquid for forming a release layer had been applied, without applying any liquid for forming a gas barrier layer. A 6 nm-thick thin aluminum oxide layer was laminated on the opposite side of the release layer as a gas barrier layer made of metal oxide by vacuum deposition of aluminum using a vacuum deposition machine while introducing oxygen gas. Next, a mixed resin obtained by mixing 100 parts by mass of a water-based urethane resin (Takelac WPB341 manufactured by Mitsui Chemicals) and 10 parts by mass of an isocyanate-based silane coupling agent (KBE9007 manufactured by Shin-Etsu Chemical Co., Ltd.) was applied onto the aluminum oxide thin film layer by gravure coating to laminate a top coat layer having a thickness of 0.2 μm, thereby obtaining a laminated film.

[0148] The laminated films obtained in the examples and comparative examples were subjected to various evaluations, and the results are shown in Table 1.

[0149] [Table 1]

[0150] The laminate films of Examples 1 to 17 had a gas barrier layer laminated thereon and a small surface roughness parameter Sa value of the release layer, and therefore had excellent oxygen barrier properties, and the adherends to which the laminate films were bonded had small changes in haze value before and after heat treatment in air, and oxidation degradation was suppressed. Among them, the laminate films of Examples 2, 5, 6, 13, and 16 had particularly excellent oxygen barrier properties, since they had small surface roughness parameter Sa values. The laminate films of Examples 3 and 7 had a high ethylene ratio in the olefin component of the acid-modified polyolefin resin constituting the release layer, and therefore had excellent releasability against acrylic pressure-sensitive adhesives. Moreover, the laminate films of Examples 13 to 17 had excellent oxygen barrier properties after heat treatment at 230°C because the base films were polyamide 9T, polyamide 10T, and polyamide 6T.

[0151] The laminated films of Comparative Examples 1 to 4, which did not have a gas barrier layer, had high oxygen permeability and were poor in oxygen barrier properties. The laminate films of Comparative Examples 5, 6, and 9 had poor oxygen barrier properties due to the large values ​​of the surface roughness parameter Sa of the release layer, and the adherends to which the laminate films were bonded showed a large change in haze value before and after heat treatment in air, indicating oxidative degradation. The laminated film of Comparative Example 7, which did not have a release layer, had poor releasability against acrylic pressure sensitive adhesives and epoxy prepregs. The laminated film of Comparative Example 8, which had a metal film-based gas barrier layer, had poor oxygen barrier properties after the bending resistance test. In the laminate films of Comparative Examples 10 and 11, the gas barrier layer was a metal vapor deposition film that did not contain organic compounds, so the oxygen permeability was high after the bending test and high-temperature treatment, and the oxygen barrier properties were poor.

Claims

1. A laminate film including a release layer, a substrate, and a gas barrier layer, wherein at least one outermost layer of the laminate film is the release layer, The surface roughness parameter Sa (arithmetic mean height) of the release layer surface is 0.05 μm or less, the gas barrier layer contains a polycarboxylic acid and a compound that forms a crosslinked structure with the polycarboxylic acid, and a crosslinked structure is formed; A laminated film, characterized in that the content of polycarboxylic acids in the gas barrier layer is 40 to 90 mass %.

2. 2. The laminated film according to claim 1, wherein the release layer contains an acid-modified polyolefin resin and a crosslinking agent.

3. A laminated film as described in claim 1 or 2, characterized in that the compound that forms a cross-linked structure with the polycarboxylic acids is a polyalcohol and / or a cross-linking agent.

4. A method for producing the laminated film described in claim 2, comprising a step of applying a liquid material for forming a release layer, the liquid material containing an acid-modified polyolefin resin, a crosslinking agent, and an aqueous medium, to one side of a substrate.

5. 5. The method for producing a laminated film according to claim 4, further comprising the step of drying and stretching the substrate on which the release layer-forming liquid has been applied.

6. 2. A method for producing the laminated film according to claim 1, comprising the steps of: applying, to one side of a substrate, a liquid material for forming a gas barrier layer, the liquid material containing polycarboxylic acids and a compound that forms a crosslinked structure with the polycarboxylic acids, and the polycarboxylic acid content being 40 to 90% by mass; drying the substrate to which the liquid material for forming a gas barrier layer has been applied; and stretching the substrate.

Citation Information

Patent Citations

  • Gas-barrier laminate

    JP2007112114A

  • Release film for medical application

    JP2009248453A

  • Release film for molding molding and method for producing the same

    JP2011230320A

  • Slippery polyester film and method of manufacturing the same

    JP2012020429A

  • Release sheet

    JP2016175322A