Reduced graphene oxide

The method of suspending GO in a liquid medium with iodide and UV irradiation addresses the limitations of existing GO reduction techniques, enabling efficient and scalable production of reduced graphene oxide with improved conductivity for use in electrical devices.

JP7594792B2Active Publication Date: 2024-12-05MONASH UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2021569357
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-05-24
Filing Date
2020-05-22
Publication Date
2024-12-05
Estimated Expiration
2040-05-22

AI Technical Summary

Technical Problem

Existing methods for reducing graphene oxide (GO) face limitations such as energy demand, safety concerns, environmental issues, high cost, and limited scalability due to the use of toxic reducing agents and harsh conditions, making large-scale production of reduced GO unsustainable.

Method used

A method involving suspending GO in a liquid medium with iodide, partially reducing GO, forming a graphite layer, and then irradiating it with ultraviolet light to further reduce GO, eliminating the need for toxic reagents and harsh conditions.

Benefits of technology

This method enables efficient and controllable reduction of GO, producing reduced graphene oxide with higher conductivity, allowing for large-scale production and stable liquid compositions suitable for electrodes in electrical devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594792000002
    Figure 0007594792000002
  • Figure 0007594792000003
    Figure 0007594792000003
  • Figure 0007594792000004
    Figure 0007594792000004
Patent Text Reader

Abstract

Provided is a method for reducing graphene oxide (GO), comprising: suspending GO in a liquid medium and dissolving iodide, whereby the dissolved iodide partially reduces the GO to obtain a liquid composition comprising partially reduced GO (prGO) and dissolved iodide; removing the liquid medium from the liquid composition to form a graphite layer comprising prGO and iodide; and irradiating the graphite layer with ultraviolet light to further reduce the prGO and provide reduced graphene oxide.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for reducing graphene oxide (GO), in particular to a method for providing reduced GO, and to the corresponding reduced GO. [Background technology]

[0002] Graphene oxide (GO) is an oxidized form of graphene in which oxygen-containing groups are attached to the graphite basal planes forming the graphene structure. Compared to graphene, GO has poor electrical conductivity. However, the electrical conductivity properties of GO can be improved by reducing GO to remove the oxygen-containing groups from its structure. Reducing GO restores the π-conjugation, which results in improved thermal and electrical conductivity. Currently, there are a number of methods for reducing GO available, including thermal, chemical, or photochemical methods for reducing GO.

[0003] Thermal reduction of GO requires exposure of GO to heat. Although the procedure is simple, thermal reduction of GO promotes unwanted re-stacking of graphene sheets due to the formation of strong π-π interactions within the structure of reduced GO. Although various countermeasures have been proposed to prevent re-stacking, this problem remains unsolved. Furthermore, the production of thermally reduced GO requires energy, and large-scale production of reduced GO may be unsustainable.

[0004] In chemical reduction methods, GO is exposed to a solution of a strong reducing agent. Traditionally, such reducing agents include NaBH4, hydroiodic acid (HI), hydroquinone, sulfur compounds, hydrazine, and hydrazine derivatives. However, the toxicity and explosiveness of these reducing agents limits the chemical reduction of GO to small-scale laboratory use.

[0005] In addition, both thermal and chemical reduction methods are inherently unsuitable for mass-supplying reduced GO in a dry state onto a substrate, and the substrate materials that can withstand high temperatures and reactive chemicals are very limited in the conventional methods.

[0006] In photochemical reduction, GO is exposed to radiation. Generally, photocatalytic additives must be added to GO as photoelectron sources and reduction promoters to promote the removal of oxygen-containing groups by radiation. However, these additives tend to remain as contaminants in the reduced GO, significantly reducing its applicability in electrical and electronic devices.

[0007] In summary, existing methods for reducing GO have limitations in energy demand, safety, applicability, etc., and as a result suffer from environmental concerns, high cost, limited scalability, and inefficiency. Therefore, there is an opportunity to address or ameliorate one or more of the shortcomings or limitations of the prior art, or at least provide a useful alternative. Summary of the Invention

[0008] The present invention provides a method for reducing graphene oxide (GO), the method comprising the steps of: (i) suspending GO in a liquid medium and dissolving iodide, whereby the dissolved iodide partially reduces the GO to obtain a liquid composition comprising partially reduced GO (prGO) and dissolved iodide; (ii) removing the liquid medium from the liquid composition to form a graphitic layer comprising prGO and iodide; and (iii) irradiating the graphite layer with ultraviolet light to further reduce the prGO and provide reduced graphene oxide.

[0009] The specific sequence of chemical and photoreduction steps in the present method can provide an efficient and highly controllable reduction of GO. Advantageously, the use of iodide and UV light does not require harmful or toxic reagents or harsh experimental conditions. As a result, the proposed method can advantageously realize the mass production of reduced GO.

[0010] The use of iodide promotes the overall reduction of GO in both steps (i) and (iii) of the method. Also, in liquid media, dissolved iodide promotes the partial reduction of GO. During UV irradiation, the presence of iodide is believed to accelerate the reduction rate of prGO resulting in reduced GO with higher electrical conductivity compared to that obtained by conventional methods.

[0011] Liquid compositions containing prGO and iodide are advantageously stable. In particular, the liquid compositions do not exhibit phase separation of prGO over extended periods of time. As a result, the liquid compositions can be advantageously stored for extended periods of time without the need for stabilization with dispersing agents such as surfactants. This is particularly advantageous when the liquid medium is water; unless a surfactant is also mixed in the water, suspensions of prGO are generally unstable and tend to settle after a short period of time.

[0012] In some embodiments, GO and iodide are provided in a liquid medium in a weight ratio of GO:iodide of about 1:2 to about 4:1. Those particular ratios advantageously allow for partial reduction of GO while providing a liquid composition of prGO and iodide that is particularly stable over long periods of time without the aid of added surfactants. In other words, the use of iodide in these weight ratios provides an advantageous compromise between the degree of reduction and the reduction of the zeta potential of the suspension, resulting in improved stability.

[0013] In some embodiments, the method includes depositing a liquid composition containing PrGO and dissolved iodide on a substrate prior to removing the liquid medium from the liquid composition. The liquid medium can then be removed from the liquid composition, consolidating a graphitic layer containing prGO and iodide on the substrate. By irradiating the solidified layer with UV light, the method of the present invention is thus capable of providing graphitic layers of reduced GO in bulk on a wide range of substrates for devices.

[0014] In some embodiments, the substrate is a current collector for an electrode. Thus, the method of the present invention is particularly advantageous for large-scale production of graphitic layers of reduced GO for use in electrodes in a wide range of electrical devices. The resulting electrodes exhibit superior ion transport properties over conventional reduced GO-based electrodes, making them particularly suitable for use in supercapacitors.

[0015] Aspects of the invention also relate to reduced GO obtained by the method of the invention, and to electrodes comprising reduced graphene oxide obtained by the method of the invention.

[0016] The reduced graphene oxide obtained by the methods described herein is believed to be unique in itself.

[0017] Thus, the present invention also provides a graphitic material consisting of sheets of reduced graphene oxide intercalated with iodide.

[0018] In some aspects, the invention also relates to electrodes comprising such graphitic materials, and to supercapacitors comprising the electrodes.

[0019] The graphitic materials of the present invention, having iodide-intercalated reduced GO sheets, advantageously exhibit superior ion transport properties compared to conventional reduced GO, making them particularly suitable for use in electrodes. Moreover, supercapacitors made with these electrodes advantageously have larger gravimetric capacitance and significantly improved rating capability than supercapacitors made with conventional reduced GO. The specific structure of the composites facilitates providing low equivalent series resistance (ESR) in the devices, resulting in superior supercapacitive performance and rating capacity.

[0020] Further aspects and embodiments of the invention are described in more detail below. [Brief description of the drawings]

[0021] Embodiments will now be described with reference to the following non-limiting drawings. [Figure 1] Figure 1 shows a Fourier transform infrared (FTIR) spectrum of partially reduced GO / KI graphitic layers obtained by drop-casting an aqueous suspension of partially reduced GO and KI onto a glass slide and then drying. [Diagram 2] Raman spectra and corresponding ID / IG ratios of (i) dried GO, (ii) partially reduced GO / KI graphitic layers obtained by drop-casting a 1:2 (by weight) aqueous suspension of partially reduced GO and KI onto a glass slide and drying (denoted as GO:KI (1:2)), and (iii) reduced GO layers obtained after UV irradiation (denoted as UV(GO:KI) (1:2)). [Diagram 3] High-resolution C1s X-ray photoelectron spectroscopy (XPS) spectra of (a) KI powder and (b) dried GO and the corresponding O / C ratios are shown. [Figure 4] High-resolution C1s X-ray photoelectron spectroscopy (XPS) spectra and the corresponding O / C ratios of (a) GO:KI (1:2) graphite layer, (b) UV(GO:KI) (1:2) graphite layer, and (c) dried GO layer after UV light irradiation (UV(GO)). [Diagram 5] X-ray diffraction (XRD) patterns of GO, GO:KI (1:2) graphitic layers formed on a glass slide, and the corresponding graphitic layers UV(GO:KI) (1:2) after UV irradiation are shown. [Figure 6] Zeta potential values ​​of aqueous suspensions of GO and partially reduced GO suspensions obtained by combining GO and KI in water at GO:KI weight ratios of 4:1, 2:1, 1:1, and 1:2 are shown. [Figure 7] High-resolution I3d-XPS spectra of KI powder, GO:KI (1:2) graphite layer, and UV(GO:KI) (1:2) graphite layer are shown. [Figure 8] A scanning electron microscope (SEM) micrograph showing the cross section of an electrode obtained by forming a UV(GO:KI) (1:2) graphite layer on a metal current collector is shown. [Figure 9] (a) Cyclic voltammograms of a supercapacitor with a UV(GO:KI) (1:2) electrode measured at different scan rates, (b) the scan rate dependence of the specific capacitance of the UV(GO:KI) (1:2) electrode, and (c) Nyquist diagram showing the electrical impedance behavior of the electrode. [Figure 10] The galvanostatic charge-discharge curves of the supercapacitor with UV(GO:KI) (1:2) electrodes measured at different current densities are shown. [Figure 11] (a) Cyclic voltammogram of a 2 V supercapacitor with UV(GO:KI) (1:2) electrode and (b) galvanostatic charge-discharge curves of the 2 V supercapacitor and comparison with the corresponding 1 V supercapacitor measured at a current of 28.8 mA. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] The present invention provides a method for reducing graphene oxide (GO).

[0023] As used herein, the term "graphene oxide" (or "GO") refers to a compound formed from carbon, oxygen, and hydrogen obtained by the oxidation of graphite, in which oxygen-containing groups are attached to the basal planes of stacked graphene sheets.

[0024] As used herein, "graphene" refers to a typical sp 2 Graphene is an allotrope of carbon that consists of planar sheets of covalently bonded carbon atoms packed into a honeycomb-like two-dimensional crystal lattice, one atom thick. The covalently bonded carbon atoms form repeating units that typically consist of six-membered rings, but can also form five- and seven-membered rings. Such layers of covalently bonded carbon atoms are commonly referred to as graphene "sheets."

[0025] Due to its chemical properties, graphene has a very stable structure, high electrical conductivity, high toughness, high strength, and large specific surface area, which are desirable properties for a supercapacitor electrode material. However, there are challenges and limitations in making electrodes directly from graphene. Despite its large surface area, supercapacitors formed with a single layer of graphene may have limited volumetric capacitance. Also, stacking graphene sheets can provide high volumetric capacitance, but the small space between the sheets can lead to poor ionic access to the surface. Furthermore, aqueous graphene suspensions (i.e., graphene "inks") are only stable if stabilized with surfactants, which can act as contaminants and affect the conductivity of the resulting graphene-based electrodes. Similarly, organic-based graphene inks are typically stabilized with surfactants and provided suspended in harmful solvents such as toluene, N-methyl-2-pyrrolidone (NMP), etc. Furthermore, conventional graphene manufacturing methods are energy intensive and costly, making them unsuitable for mass production.

[0026] Therefore, in practice, it is preferable to reduce GO to produce a conductive layer with a graphene-like structure rather than forming electrodes directly from native graphene. GO is easy to process as it is easily suspended in polar solvents such as water, and relatively stable inks can be obtained, which can be used in various film formation techniques such as die casting and tape casting. Furthermore, reduction of GO can provide a conductive graphene-like structure, which has conductive properties that are not affected by the limited volumetric capacity that limits the direct applicability of native graphene.

[0027] From a structural point of view, typically sp 2 The planar sheets of bonded carbon atoms packed into a honeycomb-like two-dimensional crystal lattice are referred to herein as the "graphitic" structure, and it is therefore understood that graphene, GO, and all forms of reduced GO, including partially reduced GO, share the "graphitic" structure.

[0028] GO is an electrically insulating graphitic material consisting of one or more graphene carbon sheets bearing oxygen-containing functional groups attached perpendicularly to the basal plane of the graphene. As used herein, the expression "oxygen-containing functional groups" refers to functional groups such as epoxides, carbonyls, hydroxyls, and phenols that are covalently bonded to the carbon atoms of the graphene oxide sheets. Typically, such oxygen-containing functional groups result from oxidation reactions carried out on the graphite.

[0029] A typical FTIR spectrum of GO shows the presence of peaks associated with carboxylic acid and carbonyl sites C-O, C-OH, C=C, C=O. These peaks are detected primarily along the edges of the graphene sheets, but also on the basal planes. The oxygen content of GO can be measured by any suitable technique. For example, the oxygen content and degree of oxidation of GO can be measured by X-ray photoelectron spectroscopy (XPS). Typically, GO has a carbon to oxygen (C:O) ratio determined by XPS that ranges from about 2:1 to about 4:1, preferably from about 2.5:1 to 3:1.

[0030] GO suitable for use in the present invention may be obtained by any means known to those skilled in the art. For example, GO may be obtained by performing an oxidation reaction on graphite. One example of a procedure available in this regard is known as the modified Hummer's method, which involves chemically oxidizing graphite powder by sequentially exposing the graphite to strong oxidizing agents such as H2SO4, KMnO4, H2O2, and HCl. A detailed description of those procedures is provided in Hummers, WS et al., "Preparation of Graphitic Oxide," J. Am. Chem. Soc. 1958, Volume 80, p. 1339, and Stankovich, S. et al., "Synthesis of Graphene-Based Nanosheets via Chemical Reduction of Exfoliated Graphite Oxide," Carbon 2007, Volume 45, p. 1558-1565, the contents of which are incorporated herein in their entirety.

[0031] GO may be provided in any form that is reducible. In some embodiments, GO is provided in the form of multi-sheet GO, in which the graphitic basal planes of GO are stacked in a multi-sheet arrangement. In other embodiments, GO is provided in the form of single-sheet (or monolayer) GO, in which the graphitic basal planes of GO are provided as a single, discrete sheet.

[0032] The method of the present invention involves suspending GO and dissolving iodide in a liquid medium.

[0033] "Suspending" GO in a liquid medium means that GO is provided in the liquid medium as a dispersed phase; that is, GO suspended in a liquid medium does not appreciably sink or float in the liquid medium. "Iodide" means a compound in which iodine is in the formal oxidation state -1, typically provided in the form of a salt. Thus, "dissolving" iodide in a liquid medium means that iodide is dissolved in the medium in the form of an ion.

[0034] As used herein, the liquid medium may be any medium capable of suspending GO and dissolving iodide. Typically, the liquid medium has sufficient polarity to ensure homogeneous suspension of GO and dissolution of iodide. For example, the liquid medium may include water in an amount of at least about 50% by weight, based on the total weight of the liquid medium. In some embodiments, the liquid medium includes water in an amount of 50% to 100% by weight, 75% to 100% by weight, or 90% to 100% by weight, based on the total weight of the liquid medium. In some embodiments, the liquid medium is water.

[0035] GO may be suspended in a liquid medium and iodide may be dissolved according to any procedure known to one skilled in the art. For example, GO may be suspended in a liquid medium in the form of particles or flakes and combined with iodide by dissolving iodide in the medium. This can be accomplished by any method that results in the combination of the two components.

[0036] In some embodiments, GO is first suspended in a liquid medium and then iodide is dissolved in the suspension. In some alternative embodiments, iodide is first dissolved in a liquid medium to form an iodide solution and then GO is suspended in the iodide solution. In yet some alternative embodiments, GO and iodide are suspended / dissolved in two separate aliquots of a liquid medium and the two aliquots are then combined.

[0037] GO may be suspended in the liquid medium in any amount, provided that it is suspended in the liquid medium without visible settling or floating. In some embodiments, GO is suspended in the liquid medium according to a concentration of at least 0.1 g / L. For example, GO is suspended in the liquid medium at a concentration of at least about 1 g / L, at least about 10 g / L, at least about 20 g / L, at least about 50 g / L, at least about 100 g / L, or at least about 500 g / L. In some embodiments, GO is suspended in the liquid medium according to a concentration of about 0.1 g / L to about 500 g / L, about 1 g / L to about 500 g / L, about 10 g / L to about 100 g / L, or about 10 g / L to about 50 g / L. For example, GO may be suspended in the liquid medium according to a concentration of about 20 g / L.

[0038] Additionally, iodide can be used in any amount relative to the suspended GO that ensures dissolution of iodide in the medium and partial reduction of GO. For example, GO and iodide can be provided in a liquid medium such that the weight ratio of GO to iodide is about 1:50 to about 50:1, e.g., about 1:25 to about 25:1, about 10:1 to about 1:10, or about 5:1 to about 1:5.

[0039] In some embodiments, GO and iodide are provided in a liquid medium such that the weight ratio of GO:iodide is about 1:2 to about 4:1, such as about 2:1 to about 4:1. In particular, GO and iodide may be provided in a liquid medium such that the weight ratio of GO:iodide is about 2:1 or about 4:1. In some embodiments, GO and iodide are provided in a liquid medium such that the weight ratio of GO:iodide is about 1:2. The particular ratios of these embodiments advantageously allow for partial reduction of GO while providing a particularly stable GO / iodide suspension for extended periods of time without the aid of added surfactants. In particular, the weight ratios in these embodiments provide a slight reduction of GO while decreasing the zeta potential of the suspension, resulting in improved stability, as shown in the data set forth in the Examples, particularly Example 3.

[0040] The iodide can be any iodide compound capable of chemically reducing GO. In some embodiments, the iodide is an anion I - Suitable examples of such salts include alkali metal iodides. Thus, in some embodiments, the iodide is an alkali metal iodide, such as an alkali metal iodide selected from lithium iodide, potassium iodide, sodium iodide, and combinations thereof.

[0041] By suspending GO in a liquid medium and dissolving iodide, GO and iodide combine, and iodide partially reduces GO. Iodide "partially" reduces GO (GO is "partially" reduced by iodide) means that iodide acts to remove some of the oxygen-containing functional groups of GO. In other words, the mere combination of GO and iodide does not induce complete deoxidation of GO. Thus, iodide can partially reduce GO by removing less than about 100%, less than about 75%, less than about 50%, or less than about 25% of the oxygen-containing functional groups of GO.

[0042] The majority of oxygen-containing functional groups in GO are hydroxyl and epoxy groups. Thus, the key to an effective partial reduction of GO is the removal of hydroxyl and epoxy groups from the GO structure. Without being bound by theory, it is believed that iodide ions in solution catalyze the ring-opening reaction of epoxides to form hydroxyl groups, which then undergo dehydration to the corresponding olefins, leaving the graphitic basal plane of GO. It is also not excluded that iodide ions directly replace hydroxyl groups that are directly bonded to the carbons that form the GO structure.

[0043] In particular, it is believed that the iodide ion acts as a good nucleophile, attacking the carbon atom attached to both the hydroxyl group and the epoxy group. Further iodide ions attack the positively charged iodine atom of the C-I bond of GO, acting as a good leaving group and forming sp 3 Carbon atom is sp 2Thus, the reduction of GO promoted by dissolved iodide is believed to proceed according to a three-step mechanism: (a) ring-opening of the epoxide to give hydroxyl groups, (b) replacement of the hydroxyl groups by iodide ions, and (c) elimination of the iodine atom to give reduced GO.

[0044] Raman spectroscopy can be used to assess the extent to which GO is partially reduced by iodide. This is seen at approximately 1600 cm -1 and about 1350 cm -1 This can be done by considering the ratio of the intensities of the G band (IG) and D band (ID) in the Raman spectrum of GO at a wave number of 1600 cm -1 The G band near the junction of all pairs of sp in the carbon rings and carbon chains is typical of graphene-like arrays. 2 Possibly related to atomic bond stretching, at about 1350 cm -1 The D band is particularly related to the presence of defects involving oxygen-containing functional groups, such as sp 2 This is due to the breathing mode of atoms.

[0045] In this context, iodide is a Raman spectrophotometer for GO. D / I G The ratio is I for pristine GO (i.e., before contact with dissolved iodide). D / I G GO can be said to be "partially" reduced when the ratio is reduced by less than 50%, less than 25%, less than 10%, or less than 5%. D / I G The decrease in the ratio is believed to be due to the removal of oxygen-containing functional groups and restoration of C=C bonds in honeycomb structures such as graphene. Thus, in some embodiments, the method includes suspending GO and dissolving iodide in a liquid medium, where iodide is the I of GO. D / I G The ratio is primitive GO I D / I G The GO is partially reduced such that the ratio is reduced by less than 25%, for example less than 10%.

[0046] The iodide may partially reduce GO for a reaction time effective to ensure partial reduction of GO. Although it is believed that the iodide effectively partially reduces GO within seconds of the two components coming into contact, the liquid composition may be stirred for any period of time compatible with the practical application of the procedure. For example, the liquid composition may be stirred for about 10 seconds to about 24 hours. In some embodiments, the liquid composition is stirred for about 30 minutes to about 6 hours.

[0047] The method also includes removing the liquid medium to form a graphitic layer consisting of partially reduced GO (prGO) and iodides.

[0048] The liquid medium can be removed by any means known to those skilled in the art. For example, the liquid medium can be removed by thermal evaporation. By "removing" the liquid medium, it is meant that at least 75% of the liquid medium is removed. In some embodiments, the liquid medium removal eliminates at least 80%, at least 90%, or about 100% of the liquid medium.

[0049] Upon removal of the liquid medium, a graphitic layer is formed that contains prGO and iodide. By "graphitic layer" is meant a layer of material having a graphitic structure. The "graphitic" nature of the layer is due to the presence of prGO in the layer, which has an inherent graphitic structure. In this specification, this expression is used to indicate any consolidated mass containing prGO and iodide that results from removal of the liquid medium. In solid form, such consolidated mass exists as a three-dimensional structure formed from graphitic sheets of prGO and iodide, with the iodide usually existing as crystalline iodide intercalated within the sheets. Such a structure has separate and independent thickness, length, and width dimensions.

[0050] In some embodiments, the method includes depositing a liquid composition comprising prGO and dissolved iodide on a substrate prior to removing the liquid medium. Deposition can be performed according to any means known to one skilled in the art, provided that upon removal of the liquid medium, a graphitic layer comprising prGO and iodide is formed on the surface of the substrate. In some embodiments, depositing the liquid composition on the substrate comprises drop casting, spin coating, dip coating, spray coating, inkjet printing, gravure printing, screen printing, rod coating, tape casting, or slot die casting the liquid composition on the surface of the substrate. Thereafter, the formation of a graphitic layer comprising prGO and iodide is achieved by removing the liquid medium as described herein.

[0051] After depositing the liquid composition on the substrate, the liquid medium can be removed to provide a thin graphitic layer on the substrate that includes prGO and iodide. By "thin" it is meant that the graphitic layer has a thickness that is significantly less than both its length and width dimensions such that dimensional properties like a conventional film are obtained. Thus, the layer formed on the substrate can have any thickness that is compatible with the structural integrity of the layer. For example, the layer may have a thickness of at least about 10 nm, at least about 50 nm, at least about 100 nm, at least about 500 nm, at least about 1 μm, at least about 10 μm, or at least about 100 μm. In some embodiments, the layer has a thickness ranging from about 10 nm to about 10 μm.

[0052] The substrate to which the liquid composition is applied may be any substrate compatible with the liquid composition. In that regard, there is no particular limit to the type of surface of the substrate with which the liquid composition is contacted. For example, the surface may form part of a substrate made of metal, glass, ceramic, composite, paper, polymer, fabric, or combinations thereof. The surface may be flat, curved, undulating, or may have a defined shape that is intended to be imparted to the graphite layer resulting from removal of the liquid medium. In this way, the surface of the substrate may effectively function as a mold to impart shape and configuration features to the resulting graphite layer.

[0053] In some examples, the substrate may be an electrode component, such as a current collector. As will be appreciated by those skilled in the art, a "current collector" is a conductive component that facilitates the flow of electrons to and from an electrical device, such as a supercapacitor, connected to an external electrical circuit. Suitable current collectors are comprised of metal structures, such as metal foils or metal grids. Typically, current collectors are present in the form of sheets or thin layers and may be formed of any material suitable for conducting electricity.

[0054] In some embodiments, the substrate is a current collector formed from a conductive material selected from nickel, aluminum, steel, copper, gold, silver, and the like. In some embodiments, the current collector is a transparent current collector. For example, the current collector may be formed from a transparent conductive polymer or a transparent ceramic conductor. In some embodiments, the current collector is formed from a transparent conductive polymer selected from poly(3,4-ethylenedioxythiophene) (PEDOT), poly(3,4-ethylenedioxythiophene)-poly(styrenesulfonic acid) (PEDOT-PSS) copolymer, poly(4,4-dioctylcyclopentadithiophene), poly(3-hexylthiophene) (P3HT), and combinations thereof. In some embodiments, the current collector is formed from a transparent ceramic conductor selected from indium tin oxide (ITO), fluorine doped tin oxide (FTO), lanthanum strontium manganites (LSMO), aluminum doped zinc oxide (AZO), and combinations thereof. In some embodiments, the current collector is formed from a layer of conductive carbon paper, carbon cloth, carbon felt, or carbon nanotubes (CNTs).

[0055] The method of the present invention also includes irradiating the prGO and iodide-containing graphite layers with ultraviolet light to further reduce the prGO and provide a reduced form of graphene oxide.

[0056] Irradiating the layer containing prGO and iodide with UV light can be accomplished by any means known to one of skill in the art, but typically this step involves exposing the layer to UV light emitted from a suitable UV light source.

[0057] Without wishing to be bound by theory, it is believed that UV irradiation of the layer can facilitate the photochemical reduction of residual oxygen-containing functional groups present in prGO. In particular, during UV irradiation, the layer is irradiated with photons having energies higher than the energy boundary characteristic of the chemical bonds between the oxygen-containing functional groups and the graphitic basal plane of prGO. This can remove the oxygen-containing functional groups from prGO and also restore the aromatic double-bonded carbons.

[0058] Thus, by "ultraviolet radiation" herein is meant radiation with wavelengths within the UV range (i.e., 10 nm to 400 nm) suitable for further reducing prGO. Raman spectroscopy can be used to assess whether prGO is "further reduced" upon exposure to ultraviolet radiation. This occurs at approximately 1600 cm -1 and about 1350 cm -1 This can be done by considering the ratio between the intensities of the G band (IG) and the D band (ID) in the Raman spectrum of prGO at wavenumbers of 1600 cm to 1600 cm. As described herein, -1 The G band near the center of the graphene-like array is characterized by all pairs of sp 2 can be related to the bond stretching of the atoms, approximately 1350 cm -1 The D band of the 1,2-dichlorophenyl ether is particularly related to the presence of defects involving oxygen-containing functional groups, particularly sp 2 This is due to the breathing mode of atoms.

[0059] In this respect, irradiating a layer with ultraviolet light produces Raman scattering of the irradiated layer. D / I G The ratio is I of the layer before irradiation. D / I G The prGO may be said to be "further reduced" if the Raman I D / I G The ratio is I of the layer before irradiation. D / I GThe ratio may be decreased by at least about 1%, at least about 5%, at least about 25%, at least about 50%, at least about 75%, or about 100%. D / I G The decrease in the ratio can be attributed to the further removal of oxygen-containing functional groups in the graphene-like honeycomb structure and the restoration of C=C bonds.

[0060] Thus, in some embodiments, irradiating a layer comprising prGO and iodide with UV light can result in an I-type photocatalytic reaction of the irradiated layer. D / I G The ratio is I of the layer before irradiation. D / I G The prGO is further reduced to a ratio of about 1% to about 10%.

[0061] Parameters such as the wavelength of the UV light, the intensity of the UV light, and the duration of exposure can affect the extent to which prGO is further reduced.

[0062] The UV irradiation may be at any UV wavelength that promotes further reduction of prGO. In some embodiments, the UV irradiation includes wavelengths in the UVC range. By "UVC range" is meant one or more wavelengths within the range of about 100 nm to about 280 nm.

[0063] In some embodiments, the ultraviolet light is monochromatic ultraviolet light with a wavelength in the UVC range. For example, the ultraviolet light may be monochromatic ultraviolet light with a wavelength of about 254 nm. When ultraviolet light is "monochromatic" at a particular wavelength, it means that the radiant intensity peaks at that wavelength with an intensity distribution of less than 10% around the peak value.

[0064] A suitable degree of further reduction of prGO can be selected based on, for example, the radiant energy characteristic of the UV source. In this regard, the UV source can be selected to provide a radiant flux (power) at the layer unit surface sufficient to promote further reduction of prGO. Such radiant flux is expressed as "irradiance" and is measured in milliwatts per square centimeter (mW / cm2). 2 In some embodiments, the ultraviolet light may be measured at about 1 to about 100 mW / cm. 2 For example, ultraviolet light has an intensity of about 10 to about 50 mW / cm 2 In some embodiments, the UV radiation may have an intensity of about 20 to about 25 mW / cm. 2 It has a strength of.

[0065] The UV irradiation may be performed for a time sufficient to promote further reduction of the prGO, for example, the layer including prGO and iodide may be irradiated for an irradiation time of from about 10 minutes to about 24 hours, such as from about 2 hours to about 17 hours.

[0066] The step of irradiating the layer with UV light may be carried out according to any setup known to those skilled in the art. For example, the layer may be placed in a chamber that can be sealed from external radiation sources and includes a UV source as the only radiation source in the chamber. The inner wall of the chamber may be made to reflect UV light itself to ensure uniform distribution of UV light in the chamber. During irradiation, the layer containing prGO and iodide may be placed at any distance from the UV source that promotes further reduction of prGO. For example, the layer may be placed at a distance of about 1 cm to about 25 cm from the UV source. In one embodiment, the irradiation of the layer containing prGO and iodide is carried out in a substantially oxygen-free environment, such as a vacuum or an inert atmosphere, such as a nitrogen or argon atmosphere.

[0067] The methods of the present invention provide reduced forms of GO. Due to the specific nature of the method steps, the "reduced form" of GO is understood to encompass GO reduced to any degree between that of prGO and that of fully reduced GO in the liquid composition. Thus, in some embodiments, reduced GO consists of fully reduced GO. The degree of reduction of reduced GO can be measured by the intensity ratio of the D band to the G band (I) that characterizes the Raman spectrum of a given sample relative to the corresponding non-reduced GO. D / I G Specifically, the term "reduced" GO herein refers to the intensity ratio I of the corresponding unreduced GO. D / I G Intensity ratio I at least 5% smaller than D / I G The graphite material is characterized by:

[0068] Thus, the present invention also relates to reduced GO obtained according to the methods described herein.

[0069] The reduced forms of GO described herein are believed to be unique in themselves. Thus, the present invention also relates to graphitic materials comprising sheets of reduced graphene oxide (GO) intercalated with iodide. The iodide may be present in any form as described herein. For example, the iodide may be an alkali metal iodide of the type described herein.

[0070] The reduced GO sheets may be characterized by any packing density with intercalated iodide that is compatible with the structural integrity of the material. Generally, the packing density of reduced GO sheets is between about 0.05 and about 10 g / cm. 3 In some embodiments, the graphite material has a density in the range of about 0.1 μg / cm 2 ~about 50mg / cm 2 of reduced GO sheets, or ca. 10 μg / cm 2 ~about 50mg / cm 2 , or about 100 μg / cm 2~about 50mg / cm 2 , or about 1 mg / cm 2 ~about 50mg / cm 2 , or about 1 mg / cm 2 ~about 10mg / cm 2 , or about 7 mg / cm 2 It is composed of reduced GO sheets.

[0071] By "intercalating" iodide into the reduced GO sheets, we mean that the iodide is spatially disposed between at least two adjacent graphite sheets of the reduced GO. The iodide may be provided in any form that allows at least two sheets to be intercalated. For example, the reduced GO sheets may be intercalated with iodide in ionic form or iodide in salt form. In some embodiments, iodide intercalates the partially reduced GO sheets in its crystalline salt form.

[0072] The reduced GO sheets may be intercalated with any amount of iodide compatible with the structural integrity of the resulting graphitic material. For example, the graphitic material may contain at least about 5 wt.%, at least about 10 wt.%, at least about 25 wt.%, at least about 50 wt.%, or at least about 75 wt.% iodide, based on the total weight of the material.

[0073] In terms of functionality, the specific structure of graphite materials makes them suitable for use as electrode materials in supercapacitors: the presence of intercalated iodide can significantly reduce the resistance of the resulting electrodes and increase their rated capacity.

[0074] Thus, the graphitic materials described herein may find useful application as electrode materials in a variety of electrical devices, particularly energy storage devices such as supercapacitors.

[0075] The present invention therefore also relates to an electrode made of a graphitic material of the type described herein, and to a supercapacitor comprising such an electrode, which can be obtained, for example, by providing reduced GO on a suitable current collector, as described herein.

[0076] The term "supercapacitor" is used herein to mean an electrical energy storage device that can store some or all of its energy as a double layer of charge (one layer composed of a charged electrode material and the other layer composed of an adjacent layer of ions from the electrolyte). Typically, supercapacitors have an energy density of 0.05 Wh / kg or greater and can provide a power density of 10 W / kg or greater.

[0077] Supercapacitors have attracted attention because they have higher power density and a longer life cycle than secondary batteries, making them a viable alternative to conventional secondary batteries in applications that require rapid power supply and charging, such as regenerative braking, short-term energy storage, hybrid electric vehicles, large industrial equipment, and portable devices.

[0078] In its most basic configuration, a supercapacitor consists of an electrode that functions as a cathode, an electrode that functions as an anode, an ion-permeable separator between the electrodes, and an electrolyte that is in contact with the electrodes. The separator and electrolyte ensure electrical insulation between the electrodes while allowing the diffusion of ions between each electrode. As a result, electrons can only flow between the electrodes and the external electrical load (circuit) to which they are connected. The electrode that functions as the "cathode," or "positive electrode," is the electrode into which electrons enter the supercapacitor when it is discharged. Conversely, the electrode that functions as the "anode" is the electrode from which electrons leave the supercapacitor when it is discharged.

[0079] Advantageously, electrodes comprising reduced GO as described herein can function as both negative and positive electrodes. Thus, a supercapacitor comprising electrodes of the type described herein can be a hybrid supercapacitor or a symmetric supercapacitor. A hybrid supercapacitor has one electrode of the type described herein, and a symmetric supercapacitor has two identical electrodes of the type described herein.

[0080] In some embodiments, the supercapacitor is a symmetric supercapacitor having a sandwich structure. In this configuration, the supercapacitor consists of two identical electrodes and a separator sandwiched between the electrodes. Such supercapacitors can be fabricated according to any procedure known to those skilled in the art. Typically, supercapacitors are fabricated by (i) providing an electrode having a layer of reduced GO of the type described herein formed on a suitable current collector, and (ii) assembling the electrodes in a sandwich structure by interposing a suitable electrolyte and a separator.

[0081] As used herein, "electrolyte" refers to a material that is electronically insulating but ionically conducting. Suitable electrolytes are known to those skilled in the art. Typically, an electrolyte contains mobile ions and is in intimate contact with the electrodes, thereby providing individual, separated paths of the ions for the electrons. Typically, requirements for a good electrolyte include a wide voltage window, high electrochemical stability, high ion concentration and low solvated ionic radius, low resistivity, low viscosity, low volatility, low toxicity, low cost, and availability in high purity.

[0082] Examples of suitable electrolytes include electrolyte solutions obtained by combining a metal salt with a solvent. The term "metal salt" refers to a compound consisting of a metal ion (cation) and a counter anion capable of providing the metal ion in solution. In this regard, the term "counter anion" refers to a negatively charged ion associated with the cation to provide charge neutrality of the resulting lithium salt.

[0083] As long as the requirements of the present invention are met, there is no particular restriction on the type of counter anion that can be used. Examples of suitable counter anions include BF4 - , PF6 - , N(CN)2 - , (CF3SO2)2N - , (FSO2)2N - , OCN - , SCN - , dicyanomethanide, carbamoylcyano(nitroso)methanide, (C2F5SO2)2N - , (CF3SO2)3C - , C(CN)3 - , B(CN)4 - , (C2F5)3PF3 - , alkyl-SO3 - , Perfluoroalkyl-SO3 - , Aryl-SO3 - , I - , H2PO4 - , HPO4 2- , sulfate, sulfite, nitrate, trifluoromethanesulfonate, p-toluenesulfonate, bis(oxalate)borate, acetate, formate, gallate, glycolate, BF3(CN) - , BF2(CN)2 - , BF(CN)3 - , BF3(R) - , BF2(R)2 - , BF(R)3 - (R is an alkyl group (e.g., methyl, ethyl, propyl), cyclic sulfonyl amide, bis(salicylate)borate, perfluoroalkyl trifluoroborate, chloride, bromide, transition metal complex anion (e.g., [Tb(hexafluoroacetylacetonate)4]).

[0084] The cations may be lithium ions. Thus, in some embodiments, the electrolyte is a solution of a salt selected from a lithium salt, a sodium salt, a potassium salt, and combinations thereof.

[0085] Examples of suitable lithium salts include Li2SO4, Li[PF2(C2O4)2], Li[SO3CF3], Li[N(CF3SO2)2], Li[C(CF3SO2)3], Li[N(SO2C2F5)2]. LiClO4, LiPF6, LiAsF6, LiBF4, LiB(C6F5)4, LiB(C6H5)4, Li[B(C2O4)2], Li[BF2(C2O4)], or a mixture of any two or more thereof. In some embodiments, the electrolyte is a Li2SO4 electrolyte.

[0086] Examples of suitable sodium salts include Na2SO4, NaClO4, NaBF4, NaPF6, sodium bis(fluorosulfonyl)imide (NaTFSI), sodium bis(fluorosulfonyl)imide (NaFSI), sodium bis(oxalato)borate (NaBOB), NaSCN, NaSbF6, NaAsF6, NaAlCl4, NaSiF6, NaSO3, CF3, and mixtures thereof.

[0087] Examples of suitable potassium salts include K2SO4, KClO4, KBF4, KPF6, potassium bis(trifluoromethanesulfonyl)imide (KTFSI), potassium bis(fluorosulfonyl)imide (KFSI), potassium bis(oxalato)borate (KBOB), KSCN, KSbF6, KAsF6, KAlCl4, KSiF6, KSO3CF3, and mixtures thereof.

[0088] The solvent used to obtain the electrolyte may be any solvent capable of dissolving the metal salt. Depending on the salt, the solvent used for the electrolyte may therefore be an organic solvent or an inorganic solvent. Examples of suitable inorganic electrolyte solvents include SO2, SOCl2, SO2Cl2, and the like, including mixtures of any two or more thereof. Organic electrolytes include dimethyl carbonate (DMC), ethyl carbonate (EMC), diethyl carbonate (DEC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), ethylene carbonate (EC), propylene carbonate (PC), dipropyl carbonate (DPC), bis(trifluoroethyl)carbonate, bis(pentafluoropropyl)carbonate, and the like. Bis(pentafluoropropyl) carbonate, trifluoroethyl methyl carbonate, pentafluoroethyl methyl carbonate, heptafluoropropyl methyl carbonate, perfluorobutyl methyl carbonate, trifluoroethyl ethyl carbonate, pentafluoroethyl ethyl carbonate, heptafluoropropyl ethyl carbonate, perfluorobutyl ethyl carbonate, fluorine-based oligomers. Methyl propionate, butyl propionate, ethyl propionate, sulfolane, 1,2-dimethoxyethane, 1,2-diethoxyethane, tetrahydrofuran, 1,3-dioxolane, 4-methyl-1,3-dioxolane dimethoxyethane, triglyme, dimethylvinylene carbonate, tetraethylene glycol, dimethyl ether, polyethylene glycols, sulfones, gamma-butyrolactone (GBL), etc. Examples of suitable solvents include vinylene carbonate, chloroethylene carbonate, methyl butyrate, ethyl butyrate, ethyl acetate, gamma valerolactone, ethyl valerate, 2-methyltetrahydrofuran, 3-methyl-2-oxazolidinone, 1,3-dioxolane, 4-methyl-1,3-dioxolane, vinyl ethylene carbonate, 2-methyl-1,3-dioxolane, acetonitrile (ACN), and mixtures of any two or more thereof. In some embodiments, the solvent is water.

[0089] The electrolyte may include any amount of metal ions that facilitates the functionality of the supercapacitor. For example, the electrolyte may include a concentration of metal ions of at least about 1 mol%, at least about 10 mol%, at least about 15 mol%, at least about 20 mol%, at least about 25 mol%, at least about 30 mol%, at least about 35 mol%, at least about 40 mol%, at least about 45 mol%, at least about 50 mol%, at least about 55 mol%, at least about 60 mol%, at least about 65 mol%, at least about 70 mol%, at least about 75 mol%, at least about 80 mol%, at least about 85 mol%, at least about 90 mol%, or at least about 95 mol%.

[0090] Suitable separators for use in supercapacitors are known to those skilled in the art and may be provided in the form of an ion-permeable layer interposed between the electrodes. The function of such an ion-permeable layer is to provide electrical insulation between the electrodes while allowing the diffusion of ions between them. The separator may therefore be any material that ensures (i) electrical insulation and (ii) ionic conductivity between the electrodes. For example, the separator may be formed from a polymeric material or a ceramic-polymer composite material, such as Celgard membrane or glass fiber. The latter composite separators have the advantage of ensuring thermal stability while significantly reducing the risk of fire. Thus, examples of suitable separators include layers made of non-woven fibers (e.g. cotton, nylon, polyester, glass) or polymeric films (e.g. poly, polyvinyl chloride, such as polyethylene, polypropylene, tetrafluoroethylene, etc.).

[0091] The supercapacitors described herein can operate over a wide range of voltages, in some embodiments, the supercapacitors can operate at voltages from about 0.01 V to about 9 V, from about 0.01 V to about 4.5 V, from about 0.01 V to about 3 V, or from about 0.01 V to about 2.5 V.

[0092] Furthermore, supercapacitors can exhibit significant energy and power densities over conventional devices.

[0093] In some embodiments, the supercapacitor has an energy density of at least about 1 Wh / kg, at least about 10 Wh / kg, or at least about 50 Wh / kg. For example, the supercapacitor may have an energy density of about 1 Wh / kg to about 400 Wh / kg, or an energy density of about 1 Wh / kg to about 50 Wh / kg.

[0094] The supercapacitor may also have a power density of at least about 100 W / kg. In some embodiments, the supercapacitor has a power density of about 100 W / kg to about 15,000 W / kg, about 250 W / kg to about 15,000 W / kg, about 500 W / kg to about 15,000 W / kg, about 500 W / kg to about 10,000 W / kg, or about 750 W / kg to about 10,000 W / kg. For example, the supercapacitor may have a power density of about 1,500 W / kg to about 3,500 W / kg. EXAMPLES

[0095] Specific embodiments of the present invention will now be described with reference to the following non-limiting examples.

[0096] Example 1 Preparation of prGO suspension in water First, a graphene oxide (GO) suspension with a concentration of approximately 20 g / liter was prepared by exfoliating desalted graphite oxide (GtO) powder (supplied by Sixth Element) in reverse osmosis water (RO water). An appropriate amount of potassium iodide (KI) was then added to the suspended GO to achieve a GO:KI weight ratio of 1:2 to 4:1. The mixture was rigorously stirred at room temperature to obtain a homogeneous and stable liquid composition consisting of prGO suspended in water.

[0097] The effect of the addition of KI on the oxygen-containing functional groups of GO was investigated by Fourier transform infrared spectroscopy (FTIR). For this purpose, aliquots of suspensions with different weight ratios of GO and KI were coated on glass slides and dried in a vacuum oven to remove the water. FTIR spectra of the dried layers were then measured using an attenuated total reflectance Fourier transform infrared spectrometer (ATR-FTIR) (PerkinElmer, USA) from 950 to 4000 cm -1 Wave number range, 2cm -1 A resolution of 100 s was used for recording, with an average of 32 scans.

[0098] Example 2 FTIR spectrum As shown in Figure 1, the FTIR spectrum of GO films contains peaks associated with the carboxylic acid and carbonyl moieties C-O, C-OH, C=C, and C=O. These peaks are mainly present along the sheet edges, but also on the basal planes of the graphene sheets, as well as a broad O-H peak. Interestingly, the peaks corresponding to the C-O, C-O-H, and C=O functional groups were significantly reduced with increasing amounts of KI and almost completely disappeared at a GO to KI weight ratio of 1:2. This indicates that the simple combination of suspended GO and dissolved KI in water is sufficient to promote the chemical reduction of GO, with the resulting suspension consisting mainly of prGO.

[0099] Raman spectroscopy To further understand the interaction between KI and GO, Raman spectroscopy measurements were performed. A Renishaw Confocal micro‐Raman Spectrometer equipped with a HeNe (632.8 nm) laser at 10% power was used to obtain Raman spectra of the dried layers obtained from the liquid compositions of prGO and KI films obtained by removing the water. The laser spot size was 1 μm, and extended scans of 10 s duration were performed at wavenumbers between 100 and 3200. After background removal, the intensity of the spectra was normalized by dividing the data by the maximum intensity. Peak fitting was performed using the PeakFit software package, and the fitted curve was used to calculate the intensity ratio of the main G band to the D band (ID / I G The results are summarized in Figure 2.

[0100] Each spectrum contains a peak at 1600 cm -1 Near the center of the graphitized GO structure are the sp of all pairs of carbon rings and carbon chains, which is an indication of the graphitization of the GO structure. 2 The G band, which corresponds to atomic bond stretching, and the 1350 cm -1 Nearby, there is a carbon ring sp that requires defects / disorder for activation. 2 The D band was due to the atomic breathing mode. By combining KI and GO, D / I G The ratio (measured and averaged over at least five different regions of the sample) decreased from 1.21 to 1.13. This decrease in ratio is attributed to the removal of functional groups and the restoration of C=C bonds. These results are consistent with the FTIR analysis, which suggests that GO was partially reduced to prGO by KI.

[0101] X-ray photoelectron spectroscopy (XPS) XPS confirms the observations from FTIR and Raman spectroscopy. The O / C ratios of the samples were determined from survey spectra. To separate the signals of GO, prGO, and the reduced form of GO produced by UV irradiation, the samples containing KI were thoroughly washed before XPS analysis. Figures 3 and 4 show the high-resolution C1s spectra of each sample.

[0102] Due to the close proximity of the peaks, the C1s spectrum of KI also contains the K2p doublet. The removal of this doublet after washing indicates the effectiveness of the washing process and the removal of K ions. The O / C ratio of the GO layer was 0.407 and its C1s spectrum contained peaks belonging to C=O, C‐O, and C‐C / C=C groups as shown in the graph. It was found that the O / C ratio was reduced to 0.341 by simply combining dissolved KI with suspended GO, indicating that the process reduced GO mainly by removing C‐O groups such as epoxy and hydroxyl groups.

[0103] X-ray diffraction (XRD) The reduction of GO by KI was further confirmed by X-ray diffraction (XRD) analysis of the dried layer using a Bruker D2 phaser diffractometer with Cu-Kα radiation at a voltage of 30 kV and 10 mA, a scan rate of 2° / min, and a step size of 0.02°. Pristine GO showed only one peak at 2θ of about 10.7°, which was attributed to the (001) plane of GO (Figure 5). This was due to the presence of K between the (001) planes of GO. + or I - This is believed to be due to the intercalation of ions, which increases the interlayer distance. Furthermore, a small hump appears at about 24-25°, which is believed to be the characteristic rGO(002) peak. The remaining peaks are found to belong to unreacted KI crystals.

[0104] Electrical Sheet Resistance Electrical sheet resistance measurements were performed with a Keithley electrometer (Model 2400, USA) using a 1 mm wide four-point probe. The results showed that the addition of KI significantly reduced the sheet resistance. The sheet resistance of the dried GO layer was about 1.4 GΩ / sq., while that of the GO:KI (1:2) was reduced to about 24.7 MΩ / sq. To eliminate the influence of residual KI on the measurements, the films were extensively washed with RO water and dried in a vacuum oven. The sheet resistance value of the washed film was about 25.5 MΩ / sq., very close to that of the unwashed film. These results are further evidence of the formation of prGO and the restoration of C=C bonds upon combination with KI.

[0105] Example 3 Polarized light microscopy of liquid compositions Liquid compositions containing prGO and iodide show optical properties of liquid crystals. To prove the liquid crustal nature of the suspensions, polarized light microscopy was performed using an inverted Leica DM IRB microscope fitted with a CRI Abrio polarized imaging system. Images were taken in a birefringence setup mode consisting of a linear polarizer, an analyzer, and two variable electro-optical retarder plates instead of a conventional compensator. Polarized light transmitted through the sample, set on a conventional microscope slide, is captured by a highly sensitive CCD camera after passing through an analyzer. The captured signals were sequentially processed using a digital image processing system to produce optical retardation and retarded axial images of the anisotropic material. rGO suspensions with a GO:KI ratio of 1:2 were used for this purpose.

[0106] As seen from polarized light microscopy micrographs (not shown), the liquid composition containing prGO and iodide exhibits optical retardation. This retardation arises from the in-plane and out-of-plane optical retardation characteristic of anisotropic materials. Furthermore, the prGO platelets align in a preferred direction that varies spatially throughout the sample, forming typical nematic liquid crystal domains. This analysis indicates the liquid crystalline nature of the liquid composition.

[0107] Example 4 Stability of the liquid composition Although GO forms very stable suspensions in water, it is difficult to obtain stable aqueous prGO suspensions. Therefore, it is important to investigate the stability of liquid compositions containing prGO. As an indicator of stability, the zeta potential of the liquid compositions was measured using a Brookhaven Nanobrook Omni Zeta Potential Analyzer. Each measurement was taken at 25°C and consisted of 20 phase cycles, with the average value from five measurements for each sample. For the measurements, a palladium electrode was immersed in a polystyrene cuvette to avoid air bubbles. The path length of the polystyrene cuvette was set to 1.0 cm, and the Smoluchowski approximation method was used: TIFF0007594792000001.tif10150(in the formula, uE is the electrophoretic mobility, θ E is the electrophoretic velocity, E is the electric field strength, ε is the dielectric constant, and η is the viscosity of the medium.) The zeta potential ζ was calculated using

[0108] The addition of KI to GO initially increased the zeta potential (Figure 6). This can be attributed to the formation of some prGO that initially reduced the stability of the suspension. With further addition of KI, the zeta potential began to decrease and became lower than that of the pure GO suspension, indicating improved stability. With the addition of KI and further removal of functional groups, the high electrostatic negative charge was reduced by the K + It may be shielded by the net positive charge due to the presence of ions. On the other hand, I - The electrostatic repulsion by the ions is believed to aid in the effective dispersion of prGO in the aqueous phase, leading to a lower zeta potential and improved suspension stability.

[0109] The stability of the suspension was further physically evaluated by long-term storage. The prGO liquid composition with a GO:KI weight ratio of 1:2 was diluted with an appropriate amount of RO water for 10 min. -2 The suspension was diluted in different ranges to give a concentration of 1000 g / liter. The suspension was stable for 4 months and showed no visible floating or settling of prGO.

[0110] Example 5 UV exposure To further reduce the prGO (GO:KI 1:2) layer, the dried coating was exposed to 254 nm UV light at 22.4 mW / cm using a UV lamp (55 W, Philips, TUV PL-L 55W / 4P). 2 The irradiation was carried out for 17 hours at an intensity of 1.

[0111] After reduction by UV irradiation, the GO peaks in the XRD patterns completely disappeared (Figure 5), and the characteristic I peaks in the Raman spectra were D / I GThe ratio further decreased to 1.07 (Fig. 2). Furthermore, XPS analysis confirmed the UV reduction of GO by removing the C-O groups and decreasing the O / C ratio to 0.177 (Fig. 4(b)). Of note, the XPS analysis showed that the pure GO film reduced by UVC light showed a larger O / C ratio (0.233) (Fig. 4(c)). These results indicate that the addition of KI to GO partially reduced GO and improved the reduction efficiency by UV irradiation. Furthermore, the high-resolution I 3d XPS scan of the sample (Fig. 7) revealed that I formed bonds with prGO especially during UV reduction to form I-doped prGO. In Fig. 7a, the full width at half maximum (FWHM) of the right peak is 1.0983 eV. In Fig. 7b, the right peak can be resolved into two peaks with FWHMs of 1.3262 (area 77.03%) and 1.4 (area 22.97%). In Figure 7c, the peak on the right side is resolved into two peaks with FWHMs of 1.2408 (89.04% area) and 1.3861 (10.96% area). The x-axis in Figures 7a, 7b, and 7c is binding energy (eV).

[0112] In addition, the sheet resistance of the UV-treated rGO film was significantly reduced by a factor of about 22, from ~24.7 MΩ / sq. to ~1.1 MΩ / sq.

[0113] Example 6 Fabrication of supercapacitors The reduced GO form obtained by the procedure described in the above examples was used to fabricate a double-layer supercapacitor device. The initial reduced GO was rod-coated onto a metal current collector to fabricate an electrode. The surface load of the fabricated electrode was approximately 7 mg / cm, as measured using a microbalance with a load accuracy of 10 μg. 2 which is 2.3 mg / cm 2 This corresponds to a graphite surface loading of 1. The electrode was further reduced by UV irradiation for 17 hours and packaged in a typical pouch cell configuration, in which a pair of folded electrodes are separated by a separator immersed in Li2SO4 electrolyte at ambient conditions.

[0114] Scanning electron microscopy (SEM, FEI Nova NanoSEM 450 FEG) was used to study the electrode morphology and the distribution of residual KI crystals in the rGO. Cross-sectional SEM micrographs revealed that KI crystals (round particles) were distributed between the graphite layers of rGO forming a lasagna-type structure (Fig. 8). Such a distribution of iodide between the graphite sheets is expected to significantly reduce the electrode resistance and improve the rated capacity.

[0115] Example 7 The performance of the supercapacitor device was evaluated with a BioLogic potentiostat. The open circuit potential (OCP) was monitored for at least 1 h to check the stability over time. A stable potential was considered before electrochemical measurements were performed if the OCP fluctuated within 10 mV for 1000 s. Cyclic voltammograms (CV curves) of the electrodes were recorded at various scan rates (5 mV / s-100 mV / s) within the test potential range. The measurements were repeated for 50 cycles at each scan rate. The CV voltammograms of the supercapacitor device at different scan rates are shown in Figure 9.

[0116] The voltammogram exhibits a rectangular shape up to a scan rate of 100 mV / s, indicating the typical double-layer capacitance behavior of the electrode and its excellent characterization capability (Figure 9(a)). The relative dielectric constant of the electrode at 5 mV / s was about 83 F / g. Figure 9(b) summarizes the scan rate-dependent specific capacitance of the electrode. The electrode exhibited good capacity retention with increasing scan rate, with the capacity retention being about 70%. Furthermore, the electrode exhibited a high energy density of 11.5 Wh / kg and a large power density of 2800 W / kg in a pouch cell configuration.

[0117] Electrochemical impedance spectroscopy (EIS) tests were performed by applying a sinusoidal potential perturbation with an amplitude of 10 mV to the open circuit potential. The impedance response was measured at frequencies between 1 MHz and 10 MHz, and six points were recorded for each decade of frequency. All electrochemical experiments were repeated at least three times to check the reproducibility of the electrochemical data. Figure 9(c) shows the Nyquist plot of the electrode. The plot consists of a small semicircle at high frequency and a straight line with a high slope in the low frequency region. The small semicircle at high frequency represents the very small charge transfer resistance, while the straight line with a high slope in the low frequency region represents the capacitive nature of the electrode. The resistance of the electrode, estimated from the intersection of the Nyquist plot with the real part of the impedance (x-axis), was found to be very small, about 60 MΩ.

[0118] The galvanostatic charge-discharge curves of the electrode measured at various current densities (0.2 A / g, 0.5 A / g, 1 A / g, 2 A / g) are shown in Figure 10. At all current densities, symmetrical and linear charge-discharge profiles with a constant slope over the entire potential range were obtained, indicating a nearly perfect double-layer capacitive behavior. Furthermore, a very small IR drop was observed in the charge-discharge curves, indicating that the equivalent series resistance (ESR) of the device was small (~400 MΩ), consistent with the impedance measurements (~300 MΩ, estimated from the intersection of the tangent line in the low-frequency region of the Nyquist plot with the real part of the impedance (x-axis)).

[0119] Example 8 We fabricated 1 V and 2 V supercapacitor devices, the latter obtained by connecting two 1 V devices in series. Figure 11 summarizes the CV curves and charge / discharge behavior of the 2 V device and compares it with the CV curve of the 1 V supercapacitor measured at the same current of 28.8 mA. The 2 V supercapacitor showed similar characteristics to the 1 V supercapacitor, i.e., a rectangular CV curve and a symmetrical linear charge / discharge profile.

[0120] In this specification and claims, unless the context requires otherwise, the word "comprise" and variations such as "comprises" and "comprising" are understood to mean the inclusion of a stated integer or step, or group of integers or steps, but not the exclusion of other integers or steps, or group of integers or steps.

[0121] Any reference in this specification to a prior publication (or information derived therefrom) or known matter is not, and should not be, an acknowledgement, admission or in any way suggest that the prior publication (or information derived therefrom) or known matter forms part of the common general knowledge in the art to which this specification pertains.

Claims

1. 1. A method for reducing graphene oxide (GO), comprising: suspending GO in a liquid medium and dissolving iodide, whereby the dissolved iodide partially reduces the GO to obtain a liquid composition comprising partially reduced GO (prGO) and dissolved iodide; removing the liquid medium from the liquid composition to form a graphite layer comprising prGO and iodides; and Irradiating the graphite layer with UV light to further reduce the prGO and provide reduced graphene oxide. A method comprising:

2. 10. The method of claim 1, wherein the GO and the iodide are provided to the liquid medium in a weight ratio of GO:iodide of about 1:2 to about 4:

1.

3. 3. The method of claim 1 or 2, wherein the GO is suspended in the liquid medium at a concentration of about 0.1 g / L to about 500 g / L.

4. The method of any one of claims 1 to 3, wherein the liquid medium comprises water.

5. The method of any one of claims 1 to 4, comprising the step of applying the liquid composition to a substrate prior to removing the liquid medium from the liquid composition.

6. 6. The method of claim 5, wherein applying the liquid composition to a substrate comprises drop casting, spin coating, dip coating, spray coating, ink jet printing, gravure printing, screen printing, rod coating, tape casting, or slot die casting the liquid composition onto a surface of the substrate.

7. The method of claim 5 or 6, wherein the substrate is selected from a polymeric substrate, a ceramic substrate, and a metallic substrate.

8. The method according to any one of claims 5 to 7, wherein the substrate is a current collector for an electrode.

9. The method according to any one of claims 1 to 8, wherein the ultraviolet light has a wavelength in the UVC range.

10. The method of claim 9 , wherein the ultraviolet light is monochromatic ultraviolet light.

11. The method of claim 10, wherein the monochromatic ultraviolet light has a wavelength of about 254 nm.

12. The ultraviolet light is about 1 to about 100 mW / cm 2 The method according to any one of claims 1 to 11, wherein the strength of the

13. 13. The method of any one of claims 1 to 12, wherein the graphite layer comprising prGO and iodide is irradiated for about 10 minutes to about 24 hours.

14. The method of any one of claims 1 to 13, wherein the iodide is an alkali metal iodide selected from lithium iodide, potassium iodide, sodium iodide, and combinations thereof.

15. A graphite material comprising stacked sheets of iodide-intercalated reduced graphene oxide, the stacked sheets having a packing density of 0.05 to 10 g / cm 3 .

16. 16. An electrode comprising the graphite material of claim 15.

17. 17. A supercapacitor comprising the electrode of claim 16.

18. 20. The supercapacitor of claim 17 having an electrolyte comprising a salt selected from a lithium salt, a sodium salt, a potassium salt, and combinations thereof.

Citation Information

Patent Citations

  • Graphene-dispersed liquid and preparation method thereof

    JP2014009104A

  • Film formation method and element

    JP2016222526A

  • High-quality graphene and method of producing same via microwave reduction of graphene oxide

    WO2018044762A1