Mortar Composition

By using modified polyvinyl alcohol with triallyl isocyanurate in the mortar composition, the strength loss is minimized, ensuring high compressive and bending strength in lightweight mortars, particularly for tunnel backfilling.

JP7594934B2Active Publication Date: 2024-12-05DENKA CO LTD
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
JP2021026152
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-22
Publication Date
2024-12-05
Estimated Expiration
2041-02-22

AI Technical Summary

Technical Problem

Existing lightweight mortar compositions suffer from a significant decrease in compressive and bending strength when polyvinyl alcohol (PVA) is added, making them unsuitable for applications requiring high strength.

Method used

Incorporating modified polyvinyl alcohol (PVA) modified with triallyl isocyanurate into the mortar composition, maintaining a unit volume mass of 2 kg/L or less, with a content of 0.01 to 3.0 parts by mass based on 100 parts by mass of cement, to reduce the rate of strength decrease to 50% or less for bending strength and 65% or less for compressive strength.

Benefits of technology

The modified PVA composition maintains high compressive and bending strength while keeping the mortar lightweight, suitable for applications like backfilling in tunnels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594934000001
    Figure 0007594934000001
Patent Text Reader

Abstract

To provide a mortar composition having a small unit volume mass and having a small reduction rate of compressive strength and flexural strength of the cured product.SOLUTION: Provided is a mortar composition containing cement, sand, and polyvinyl alcohol, the polyvinyl alcohol being a modified polyvinyl alcohol modified by triallyl isocyanurate.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a mortar composition, and more particularly to a mortar composition suitable for use in repair and reinforcement work of concrete structures in the fields of civil engineering and construction. [Background technology]

[0002] Concrete used in the construction of architectural or civil engineering structures contains cement, water, aggregate, etc., and has the property of hardening through the hydration reaction of cement. After hardening, concrete may crack due to volume changes caused by the action of stress, temperature changes, drying, etc. Cracks in concrete cause water leakage, rebar corrosion, etc., and are the main cause of a significant decrease in durability, so if the cracks are severe, they must be repaired. For example, in concrete structures such as tunnels, cracks that have occurred in the tunnel lining concrete are repaired by injecting repair fillers or repairing the cross section.

[0003] Meanwhile, mortar with small unit mass and excellent fluidity has been proposed as a backfill material for cavities and voids that occur between a tunnel and the natural ground. Specifically, a method of introducing air bubbles into mortar (Patent Document 1) and a method of adding lightweight aggregate to mortar (Patent Document 2) have been proposed. However, the compressive strength of lightweight mortar decreases linearly with the weight reduction, and the bending strength also decreases accordingly. Therefore, there is a demand for a mortar composition that is lightweight yet has high strength. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 9-268043 [Patent Document 2] JP 2009-161388 A Summary of the Invention [Problem to be solved by the invention]

[0005] One method for making a mortar composition lighter is to add polyvinyl alcohol (PVA) to the mortar composition. When PVA is added to a mortar composition, air is entrained during mixing, making the mortar composition lighter. However, the compressive strength and bending strength of the hardened product of a lightweight mortar containing PVA are lower than those of a mortar without PVA. Under these circumstances, an object of the present invention is to provide a mortar composition having a small unit volume mass and a small rate of decrease in compressive strength and flexural strength of the hardened product. [Means for solving the problem]

[0006] The present inventors have conducted intensive research to solve the above problems, and have found that the above problems can be solved by using a specific modified polyvinyl alcohol, thereby completing the present invention. That is, the present invention is as follows. [1] A mortar composition comprising cement, sand, and polyvinyl alcohol, wherein the polyvinyl alcohol is modified with triallyl isocyanurate. [2] The mortar composition according to the above [1], wherein the content of the modified polyvinyl alcohol is 0.01 to 3.0 parts by mass per 100 parts by mass of cement. [3] The mortar composition according to [1] or [2] above, having a unit volume mass of 2 kg / L or less. [4] A mortar composition according to any one of [1] to [3] above, in which the reduction in bending strength due to the addition of modified polyvinyl alcohol after 28 days of age is 50% or less and the reduction in compressive strength is 65% or less. [5] The mortar composition according to any one of [1] to [4] above, which is for backfilling. Effect of the Invention

[0007] According to the present invention, it is possible to provide a lightweight mortar composition having a small unit volume mass and a small rate of decrease in compressive strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] [Mortar composition] The mortar composition of the present invention contains cement, sand, and modified polyvinyl alcohol (hereinafter, may be referred to as "modified PVA"). Each of the constituent elements will be described in detail below.

[0009] <Cement> The cement is not particularly limited, and examples thereof include various Portland cements such as normal, early strength, super early strength, low heat, and moderate heat, various mixed cements obtained by mixing blast furnace slag, fly ash, or silica with these Portland cements, filler cements obtained by mixing limestone powder, gypsum, blast furnace slag powder, etc., and Portland cements such as environmentally friendly cements (ecocement) manufactured using municipal waste incineration ash and sewage sludge incineration ash as raw materials, as well as commercially available cement-based solidification materials used in ground improvement work, commercially available fine particle cements, etc., and one or more of these can be used. Also, cements adjusted by increasing or decreasing the amount of components used in normal cements can be used. In the present invention, it is preferable to select ordinary Portland cement or high-early-strength Portland cement from the viewpoints of high fluidity, carbonation resistance, and the like. The cement content in the mortar composition of the present invention is preferably in the range of 5 to 50% by mass. If the cement content is 5% by mass or more, sufficient strength is obtained. On the other hand, if it is 50% by mass or less, cracks due to excess cement do not occur. From the above viewpoints, the cement content is more preferably in the range of 10 to 40% by mass, and further preferably in the range of 15 to 30% by mass.

[0010] <Sand> The sand used in the mortar composition of the present invention is not particularly limited and may be any sand that is usually mixed into mortar, such as river sand, mountain sand, sea sand, lime sand, and silica sand. The content of sand in the mortar composition of the present invention is not particularly limited as long as it is within a range that does not impair the effects of the present invention. Generally, however, the content of sand is preferably 50 to 500 parts by mass, more preferably 100 to 450 parts by mass, and even more preferably 200 to 400 parts by mass, per 100 parts by mass of cement. When the sand content is equal to or greater than the lower limit, the strength of the hardened product of the mortar composition is sufficient, whereas when the sand content is equal to or less than the upper limit, the cement content becomes relatively large and sufficient adhesiveness is obtained.

[0011] <Modified polyvinyl alcohol> The modified polyvinyl alcohol used in the mortar composition of the present invention is a polymer obtained by saponifying a copolymer of a vinyl ester monomer and triallyl isocyanurate (hereinafter sometimes referred to as "TAIC" (registered trademark)). TAIC has the advantage of being highly reactive with vinyl ester monomers and difficult to decompose in saponification reactions. In addition, the presence of multiple functional groups results in the formation of cross-linked structures, which provide resistance to dissolution at high temperatures. The modified PVA according to the present invention may be copolymerized with other monofunctional monomers and / or polyfunctional monomers together with TAIC, as long as the effects of the present invention are not impaired.

[0012] (Vinyl ester monomer) Examples of the vinyl ester monomer include vinyl acetate, vinyl propionate, vinyl butyrate, vinyl valerate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl benzoate, vinyl pivalate, etc., and mixtures of these may also be used. From the viewpoint of ease of polymerization, vinyl acetate is preferred.

[0013] (Monofunctional Monomer) Examples of monofunctional monomers copolymerizable with vinyl ester monomers together with TAIC include the following compounds: α-olefin monomers such as ethylene and propylene; (meth)acrylic acid alkyl ester monomers such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate; unsaturated amide monomers such as (meth)acrylamide and N-methylolacrylamide; unsaturated carboxylic acid monomers such as (meth)acrylic acid, crotonic acid, maleic acid, itaconic acid, and fumaric acid; alkyl (methyl, ethyl, propyl, and the like) ester monomers of unsaturated carboxylic acids; anhydrides of unsaturated carboxylic acids such as maleic anhydride; sodium, potassium, ammonium, and the like salts of unsaturated carboxylic acids; sulfonic acid group-containing monomers or salts thereof such as 2-acrylamido-2-methylpropanesulfonic acid; and alkyl vinyl ether monomers.

[0014] (Polyfunctional Monomer) As a polyfunctional monomer that can be copolymerized with TAIC and vinyl ester monomers, a compound having two or more polymerizable unsaturated bonds in the molecule can be used. Specifically, divinyl ethers such as ethanediol divinyl ether, propanediol divinyl ether, butanediol divinyl ether, ethylene glycol divinyl ether, diethylene glycol divinyl ether, triethylene glycol divinyl ether, polyethylene glycol divinyl ether, propylene glycol divinyl ether, and polypropylene glycol divinyl ether; divinyl sulfonic acid compounds; diene compounds such as pentadiene, hexadiene, heptadiene, octadiene, nonadiene, and decadiene; glycerin diallyl ether, diethylene glycol diallyl ether, ethylene glycol diallyl ether, triethylene glycol diallyl ether, polyethylene glycol diallyl ether, trimethylolpropane diallyl ether, and pentaerythritol diallyl ether. diallyl ether compounds such as glycerol triallyl ether, trimethylolpropane triallyl ether, pentaerythritol triallyl ether, and other triallyl ether compounds; tetraallyl ether compounds such as pentaerythritol tetraallyl ether; polyfunctional monomers containing an allyl ester group such as diallyl phthalate, diallyl maleate, diallyl itaconate, diallyl terephthalate, diallyl adipate, and other diallyl amine compounds; polyfunctional monomers containing an allylamino group such as triallylamine; polyfunctional monomers containing an allylammonium group such as diallyl ammonium salts such as diallyl dimethyl ammonium chloride, and other polyfunctional monomers containing two or more allyl groups such as 1,3-diallyl urea, triallyl phosphate, and diallyl disulfide;Ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, glycerin di(meth)acrylate, glycerin tri(meth)acrylate, pentaerythritol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, Examples of the monomer include polyfunctional monomers having (meth)acrylic acid, such as pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and isocyanuric acid tri(meth)acrylate; polyfunctional monomers having (meth)acrylamide, such as N,N'-methylenebis(meth)acrylamide and N,N'-ethylenebis(meth)acrylamide; polyfunctional aromatic monomers, such as divinylbenzene and trivinylbenzene; and glycidyl group-containing monomers, such as allyl glycidyl ether and glycidyl (meth)acrylate.

[0015] When a vinyl ester monomer is copolymerized with TAIC, the copolymerization ratio is preferably 0.001 to 1.0 mol %, more preferably 0.005 to 0.5 mol %, and even more preferably 0.01 to 0.2 mol %, of the structural unit derived from TAIC relative to 100 mol % of the structural unit derived from the vinyl alcohol unit in the vinyl alcohol polymer. By adjusting the content of TAIC within this range, the dissolution resistance at high temperatures is improved and the vinyl alcohol polymer is not excessively crosslinked, which is also preferable from the viewpoint of production.

[0016] The content of the modified PVA in the mortar composition of the present invention is preferably in the range of 0.01 to 3.0 parts by mass relative to 100 parts by mass of cement. By setting the content of the modified PVA in the above range, the effect of the modified PVA can be exhibited, and the composition can be lightweight while minimizing the decrease in compressive strength and bending strength. From the above viewpoints, the content of the modified PVA is more preferably in the range of 0.05 to 2.0 parts by mass, and even more preferably in the range of 0.1 to 1.0 parts by mass.

[0017] Generally, when PVA is added to a mortar composition, the bending strength and compressive strength are reduced, but the mortar composition of the present invention can reduce the reduction rate of bending strength and compressive strength by using modified PVA. Specifically, the reduction rate of bending strength due to the addition of modified polyvinyl alcohol after 28 days can be reduced to 50% or less, and the reduction rate of compressive strength can be reduced to 65% or less.

[0018] (Method of producing modified polyvinyl alcohol) Any method can be used as a method for copolymerizing a vinyl ester monomer and TAIC, and for example, a known polymerization method such as solution polymerization, suspension polymerization, bulk polymerization, etc. From the viewpoint of ease of operation and the ability to use a solvent common to the subsequent saponification reaction, it is preferable to use a solution polymerization method in an alcohol, and it is particularly preferable to use methanol as the alcohol.

[0019] The polymer obtained as described above can be saponified by any method to produce a modified PVA. An example of the saponification method is a method in which an alkali catalyst is added to an alcohol solution of a polymer (such as polyvinyl ester). Examples of the alcohol that can be used as a solvent for the polymer include methanol, ethanol, butanol, and preferably methanol. The concentration of the polymer in the alcohol solution can be set arbitrarily and may be, for example, 10% by mass or more and 80% by mass or less.

[0020] Next, an alkali catalyst is added to the above solution to carry out a saponification reaction. Examples of the alkali catalyst include hydroxides and alcoholates of alkali metals such as sodium hydroxide, potassium hydroxide, sodium methylate, sodium ethylate, and potassium methylate. Among these, it is preferable to use sodium hydroxide. The amount of the alkali catalyst to be added is not particularly limited, but is preferably 1.0 to 100.0 millimolar equivalents relative to the polymer, and more preferably 5.0 to 30.0 millimolar equivalents. The reaction temperature during saponification is not particularly limited, but is preferably 10 to 70°C, and more preferably 30 to 55°C. The reaction time is also not particularly limited, and may be, for example, 20 minutes to 2 hours.

[0021] The degree of saponification can be appropriately adjusted depending on the application of the PVA, and may be, for example, 72 to 99 mol %. After the saponification reaction, washing and drying may be carried out to remove impurities such as sodium acetate, if necessary.

[0022] <Water> The mortar composition of the present invention usually contains water. The water is not particularly limited, and for example, tap water, groundwater, recycled water from a ready-mix concrete plant, etc. can be used. The content of water in the mortar composition of the present invention is preferably in the range of 10 to 100 parts by mass, more preferably in the range of 20 to 80 parts by mass, and even more preferably in the range of 30 to 70 parts by mass, relative to 100 parts by mass of cement. When the content of water is equal to or more than the lower limit, the viscosity of the mortar composition is appropriate, and coating becomes easy. On the other hand, when the content of water is equal to or less than the upper limit, the content of components such as cement and sand is ensured, and the effect as a backfilling material is sufficiently obtained.

[0023] <Other added ingredients> The mortar composition of the present invention may contain additives that are usually added to mortar compositions, as long as they do not impair the effects of the present invention. For example, one or more of the following may be used within a range that does not substantially impair the purpose of the present invention: antifoaming agent, water reducing agent, setting retarder, gas foaming material, expanding agent, setting regulator, AE agent, rust inhibitor, water repellent, antibacterial agent, colorant, antifreeze agent, limestone fine powder, slowly cooled blast furnace slag fine powder, sewage sludge incineration ash and its molten slag, urban waste incineration ash and its molten slag, and admixtures such as pulp sludge incineration ash, thickeners, shrinkage reducing agents, clay minerals such as bentonite and sepiolite, and anion exchangers such as hydrotalcite. Among the above-mentioned additive components, examples of the defoaming agent include alkylene oxide adducts of higher fatty acids, silicone-based defoaming agents such as dimethyl silicone, mineral oil-based defoaming agents, etc. By adding a defoaming agent, excessive air entrainment can be suppressed. Examples of the water-reducing agent include naphthalene sulfonic acid-based water-reducing agents, melamine sulfonic acid-based water-reducing agents, lignin sulfonic acid-based water-reducing agents, and polycarboxylic acid-based water-reducing agents. The water-reducing agent can help disperse each material and impart fluidity to the mortar composition.

[0024] <Unit volume mass of mortar composition> The unit volume mass of the mortar composition of the present invention is preferably 2 kg / L or less. If it is 2 kg / L or less, it is relatively light. There is no particular limit to the lower limit, but in order to ensure a certain degree of strength, it is preferably 1.3 kg / L or more, more preferably 1.5 kg / L or more, and even more preferably 1.6 kg / L or more.

[0025] [Method of manufacturing mortar composition] The mortar composition of the present invention can be obtained by kneading the above-mentioned cement, sand, water, and modified PVA. The above materials may be kneaded simultaneously, or the cement, sand, and modified PVA may be kneaded first, and water may be added later. The modified PVA may also be dissolved in water beforehand. The kneading method is not particularly limited, and a conventional method can be used. As a mixing device, an existing stirring device can be used, such as a mortar mixer, a tilting mixer, an omni mixer, a V-type mixer, a Henschel mixer, and a Nauta mixer. The kneading conditions are also not particularly limited, and for example, low-speed or high-speed stirring is performed at a temperature of 10 to 50°C for about 1 to 10 minutes. The method for curing the mortar composition of the present invention is not particularly limited, and may be steam curing, autoclave curing, or in-situ curing in a poured state.

[0026] [Uses of mortar composition] The mortar composition of the present invention is suitable for use in repair and reinforcement work of concrete structures in the fields of civil engineering and construction, and is particularly suitable as a backfill material for cavities and voids that occur between tunnels and the natural ground. EXAMPLES

[0027] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0028] <Evaluation method> (1) Unit volume mass: Measured in accordance with JIS A 1171. (2) Fluidity: The mortar was mixed in accordance with JIS R 5201-2015 "Physical Testing Methods for Cement," and the flow values ​​were measured at 15 points immediately after mixing (0 minutes), 30 minutes after mixing, and 60 minutes after mixing.

[0029] (3) Bending strength (3-1) Preparation of bending strength specimen Bending strength specimens were prepared and cured according to the method described in JIS R 5201-2015. (3-2) Bending strength measurement The specimens prepared in (3-1) above were used to measure bending strength in accordance with the method described in JIS R 5201-2015. The test equipment used was a fully automatic compression tester, Hi-Actis-500, manufactured by Marui Co., Ltd., and a jig for bending strength was used. The rate of decrease in bending strength at 28 days of age was also calculated. The rate of decrease in bending strength was calculated by subtracting the bending strength of each Example or Comparative Example from the bending strength of the blank (Reference Example 1) (decrease in bending strength) and dividing the result by the bending strength of the blank.

[0030] (4) Compressive strength (4-1) Preparation of compressive strength specimen Compressive strength specimens were prepared and cured according to the method described in JIS R 5201-2015. (4-2) Compressive strength measurement The specimens prepared in (4-1) above were used to measure bending strength in accordance with the method described in JIS R 5201-2015. The test equipment used was a fully automatic compression tester, Hi-Actis-500, manufactured by Marui Co., Ltd., and a jig for compressive strength was used. The rate of decrease in compressive strength at 28 days of age was also calculated. The rate of decrease in compressive strength was calculated by subtracting the compressive strength of each Example or Comparative Example from the compressive strength of the blank (Reference Example 1) (decrease in compressive strength), and dividing the result by the compressive strength of the blank.

[0031] Example 1 (Modified PVA) In a polymerization vessel equipped with a reflux condenser, a dropping funnel, and a stirrer, 100 parts by mass of vinyl acetate, 67 parts by mass of methanol, 0.16 parts by mass of triallyl isocyanurate (TAIC) as a polyfunctional monomer, 5.0x10 parts by mass of Peroyl NPP (manufactured by Nippon Oil & Fats Co., Ltd.) as an initiator, -6 The mixture was stirred in a nitrogen atmosphere and polymerized at the boiling point for 5.0 hours. The unreacted vinyl acetate monomer was then removed from the polymerization system to obtain a methanol solution of polyvinyl acetate-TAIC copolymer. A methanol solution of sodium hydroxide was added to the obtained methanol solution of vinyl acetate-TAIC copolymer (0.008 mol% of sodium hydroxide relative to the copolymer). Then, a saponification reaction was carried out at 45°C for 45 minutes to obtain a modified PVA with a saponification degree of 88.2 mol%.

[0032] (Mortar composition) 1350g of standard sand, 225g of water, and 0.9g of the modified PVA (0.2 parts by mass per 100 parts by mass of cement) were added to 450g of normal cement, and mixed at 20°C for 2 minutes and 30 seconds. The mortar composition was evaluated by the above-mentioned evaluation method. The results are shown in Table 1.

[0033] Example 2 A mortar composition was obtained in the same manner as in Example 1, except that the amount of modified PVA in Example 1 was changed as shown in Table 1. The results of evaluation in the same manner as in Example 1 are shown in Table 1.

[0034] Comparative Examples 1 and 2 A mortar composition was obtained in the same manner as in Example 1, except that a commercially available unmodified PVA (Denka Poval B-24, manufactured by Denka Co., Ltd.) was used instead of the modified PVA in Example 1 and was mixed in the amounts shown in Table 1. The results of evaluation in the same manner as in Example 1 are shown in Table 1.

[0035] Reference Example 1 (Blank) Mortar conforming to JIS R 5201 (JIS mortar) was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0036] [Table 1]

[0037] The mortar composition of the present invention has a lower compressive strength by adding modified PVA compared to the blank (Reference Example 1), but the decrease rate of the compressive strength is obviously smaller than that of the case where the same amount of unmodified PVA is added. For example, in a comparison between Example 1 and Comparative Example 1, in which the amount of PVA added is 0.2 parts by mass per 100 parts by mass of cement, the decrease rate of the compressive strength at 28 days is calculated to be about 37% in Example 1 and 68% in Comparative Example 1. Even considering that the unit volume mass of Example 1 is larger than that of Comparative Example 1, the difference in the decrease rate of the compressive strength is obviously significant, and it is understood that the mortar composition of the present invention exhibits a high effect. The same is true when comparing Example 2, in which the PVA content is 0.5 parts by mass per 100 parts by mass of cement, with Comparative Example 2. At an age of 28 days, the compressive strength reduction rate for Example 2 was 63%, while that for Comparative Example 2 was calculated to be 82%, demonstrating that the mortar composition of the present invention exhibits excellent effects in terms of compressive strength. Furthermore, the bending strength showed the same tendency as the compressive strength, and it is clear that the mortar composition of the present invention has excellent effects in both compressive strength and bending strength. [Industrial Applicability]

[0038] The mortar composition of the present invention is a lightweight mortar with a small unit mass, yet the rate of decrease in compressive strength of the hardened product is small, and it is possible to ensure a certain level of compressive strength and bending strength. Therefore, it is effective as a mortar material that requires weight reduction, and is useful, for example, as a backfill material for tunnels.

Claims

1. A mortar composition containing cement, sand, and polyvinyl alcohol, wherein the polyvinyl alcohol is modified with triallyl isocyanurate, and the content of the modified polyvinyl alcohol is 0.2 to 0.5 parts by mass relative to 100 parts by mass of cement.

2. The mortar composition according to claim 1, having a unit volume mass of 2 kg / L or less.

3. 3. The mortar composition according to claim 1, wherein the addition of modified polyvinyl alcohol results in a decrease in bending strength of 50% or less and a decrease in compressive strength of 65% or less after 28 days of age.

4. The mortar composition according to any one of claims 1 to 3, which is for backfilling.

Citation Information

Patent Citations

  • Cement admixing agent

    JP1980047256A

  • Hydrophilic nonionic rigid gel

    JP1980104301A

  • Admixing agent for cement

    JP1985171258A

  • Lightweight bubbled grout material and its application

    JP1997268043A

  • Cement hardening retarder and its production

    JP1998053447A