Etching method, substrate processing apparatus, and substrate processing system
By forming a protective film with tin atoms on the substrate and using specific gas combinations, the method addresses the challenge of protecting the mask during plasma etching, achieving enhanced selectivity and control in the etching process.
Patent Information
- Application Number
- JP2021036107
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-06-19
- Filing Date
- 2021-03-08
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2041-03-08
AI Technical Summary
Existing plasma etching methods for silicon-containing films face challenges in effectively protecting the mask during the etching process, leading to potential damage and reduced selectivity and control over the etching process.
A protective film containing tin atoms is formed on the substrate surface, which is then etched using a combination of gases to protect the mask and selectively etch the desired regions, allowing for controlled etching while maintaining the integrity of the mask.
The method enhances the selectivity and control of the etching process, protecting the mask and sidewalls, and allows for precise adjustment of mask dimensions and shape, while also being easily removable without causing contamination.
Smart Images

Figure 0007594943000001 
Figure 0007594943000002 
Figure 0007594943000003
Abstract
Description
[Technical field]
[0001] SUMMARY Exemplary embodiments of the present disclosure relate to an etching method, a substrate processing apparatus, and a substrate processing system. [Background technology]
[0002] In the manufacture of electronic devices, plasma etching is performed on a film on a substrate. Plasma etching is applied to, for example, a silicon-containing film. In the plasma etching of a silicon-containing film, a process gas containing a fluorocarbon gas is used. Such plasma etching is described in the following Patent Document 1. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] US Patent Application Publication No. 2018 / 0286707 Summary of the Invention [Problem to be solved by the invention]
[0004] The present disclosure provides techniques for forming a protective film for etching a substrate. [Means for solving the problem]
[0005] In one exemplary embodiment, an etching method is provided that includes forming a protective film on a surface of a substrate, the substrate having an area to be etched and a mask disposed over the area, the protective film including tin atoms, and the etching method further includes etching an area in the substrate. Effect of the Invention
[0006] According to one exemplary embodiment, a protective film can be formed for etching a substrate. [Brief description of the drawings]
[0007] [Figure 1] 1 is a flow diagram of an etching method according to an exemplary embodiment. [Diagram 2] FIG. 2 is a partially enlarged cross-sectional view of an example substrate. [Diagram 3] 1 is a schematic diagram of a substrate processing apparatus according to an exemplary embodiment; [Figure 4] FIG. 2 is an enlarged cross-sectional view of an electrostatic chuck in a substrate processing apparatus according to an exemplary embodiment. [Diagram 5] FIG. 5(a) is a diagram for explaining an example of step STa of the etching method shown in FIG. 1, and FIG. 5(b) is a partially enlarged cross-sectional view of the example substrate in a state after step STa has been performed. [Figure 6] 1 is a flow diagram of a deposition method that may be used in an etching method according to an example embodiment. [Figure 7] FIG. 7(a) is a partially enlarged cross-sectional view of an example substrate after a precursor layer has been formed, and FIG. 7(b) is a partially enlarged cross-sectional view of an example substrate after a protective film has been formed. [Figure 8] FIG. 8(a) is a diagram for explaining an example of step ST2 of the etching method shown in FIG. 1, and FIG. 8(b) is a partially enlarged cross-sectional view of the example substrate in a state after step ST2 has been performed. [Figure 9] FIG. 9(a) is a partially enlarged cross-sectional view of an example substrate after a precursor layer has been formed, and FIG. 9(b) is a partially enlarged cross-sectional view of an example substrate after a protective film has been formed. [Figure 10] FIG. 1 illustrates a substrate processing system according to an exemplary embodiment. [Figure 11] 4 is a flow diagram of an etching method according to another exemplary embodiment. [Figure 12] 4 is a flow diagram of an etching method according to yet another illustrative embodiment. [Figure 13] 4 is a flow diagram of an etching method according to yet another illustrative embodiment. [Figure 14] Each of (a) and (b) of FIG. 14 is a partially enlarged cross-sectional view of an example of the substrate in a state after step ST31 of FIG. 12 is performed. [Figure 15] 15(a) is a partially enlarged cross-sectional view of an example substrate after step ST2 of FIG. 12 or step ST22 of FIG. 13, and FIG. 15(b) is a partially enlarged cross-sectional view of an example substrate after step ST32 of FIG. 12 or step ST42 of FIG. 13. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Various exemplary embodiments are described below.
[0009] In one exemplary embodiment, an etching method is provided that includes the steps of: a) forming a protective film on a surface of a substrate, the substrate having an area to be etched and a mask disposed over the area, the protective film including tin atoms, and b) etching an area in the substrate.
[0010] In the above embodiment, a protective film containing tin (Sn) atoms is formed on the surface of the substrate. In the above embodiment, a region in the substrate is etched. Therefore, according to the above embodiment, it is possible to etch the region in the substrate while protecting the surface and / or sidewall surface provided by the region of the mask. The etching of the film may be plasma etching.
[0011] In one exemplary embodiment, step b) may be performed after step a), while in another exemplary embodiment, steps a) and b) may be performed at least partially simultaneously.
[0012] In one exemplary embodiment, the step a) may include a-1) supplying a first gas to the substrate, and a-2) supplying a second gas to the substrate, wherein at least one of the first gas and the second gas may include a tin-containing material.
[0013] In one exemplary embodiment, a precursor layer may be formed on the surface of the substrate using a first gas in step a-1), and a protective film may be formed from the precursor layer using a second gas in step a-2).
[0014] In one exemplary embodiment, the first gas may include a tin-containing material, and in step a-2), the protective film may be formed by oxidizing, nitriding, sulfiding, reducing, or halogenating the precursor layer using the second gas.
[0015] In one exemplary embodiment, in the step a-2), a plasma of the second gas may be generated. In the step b), during the execution of the step a-2), a region in the substrate may be etched by chemical species from the plasma of the second gas. According to this exemplary embodiment, the steps a-2) and b) are performed simultaneously, thereby achieving high throughput.
[0016] In one exemplary embodiment, one of the first gas and the second gas may include a tin-containing material, and the other of the first gas and the second gas may include H 2 O, H 2 O 2 , O 2 , O 3 , N 2 O 4 , a nitrogen-containing inorganic compound, a sulfur-containing inorganic compound, a halogen compound, a carbon-containing material, a silicon-containing material, or a tin-containing material. Alternatively, the other of the first gas and the second gas may include N 2and an oxygen-containing material. In this case, a chemical species from a plasma generated from the other of the first gas and the second gas may be supplied to the precursor layer containing tin atoms formed on the surface of the substrate. At least one of the first gas and the second gas may be supplied to the precursor layer without generating a plasma therefrom.
[0017] In one exemplary embodiment, in the step a), a plurality of deposition cycles each including the step a-1) and the step a-2) may be sequentially performed. Between the step a-1) and the step a-2), and between the step a-2) and the step a-1), purging of the inner space of the chamber housing the substrate therein may be performed.
[0018] In one exemplary embodiment, the conditions for forming the precursor layer in at least one deposition cycle of the plurality of deposition cycles may be different from the conditions for forming the precursor layer in at least one other deposition cycle of the plurality of deposition cycles.
[0019] In one exemplary embodiment, the conditions for forming a protective film from the precursor layer in at least one deposition cycle of the plurality of deposition cycles may be different from the conditions for forming a protective film from the precursor layer in at least one other deposition cycle of the plurality of deposition cycles.
[0020] In one exemplary embodiment, in step a), the protective film may be formed by chemical vapor deposition using a deposition gas containing a tin-containing material.
[0021] In one exemplary embodiment, the deposition gas is N 2 , H 2 O, H 2 O 2 , O 2 , O 3 , N 2 O 4The gas may further include at least one of an oxygen-containing substance, an inorganic compound containing nitrogen, an inorganic compound containing sulfur, a halogen compound, a carbon-containing substance, a silicon-containing substance, and a rare gas.
[0022] In one exemplary embodiment, the etching method may further include a step of etching a region in the substrate prior to step a) ("step c") The protective film may be formed in step a) on a sidewall surface that defines the opening formed in the region in the substrate in step c).
[0023] In one exemplary embodiment, the thickness of the protective film may vary depending on the depth position within the opening.
[0024] In one exemplary embodiment, multiple cycles each including steps a) and b) may be performed in sequence.
[0025] In one exemplary embodiment, the conditions for forming the overcoat in at least one cycle of the plurality of cycles may be different than the conditions for forming the overcoat in at least one other cycle of the plurality of cycles.
[0026] In one exemplary embodiment, conditions for etching the film in at least one cycle of the plurality of cycles may differ from conditions for etching the film in at least one other cycle of the plurality of cycles.
[0027] In one exemplary embodiment, the film to be etched may be a silicon-containing film or an organic film.
[0028] In another exemplary embodiment, a substrate processing apparatus is provided. The substrate processing apparatus includes a chamber, a substrate support, a gas supply, and a controller. The substrate support is configured to support a substrate in the chamber. The gas supply is configured to supply gas into the chamber. The controller is configured to control the gas supply. The controller controls the gas supply to supply gas into the chamber to form a protective film including tin atoms on a surface of a substrate supported by the substrate support. The controller controls the gas supply to supply gas into the chamber to etch a region in the substrate.
[0029] In yet another exemplary embodiment, a substrate processing system is provided that includes a deposition apparatus and a substrate processing apparatus, the deposition apparatus configured to form a protective film comprising tin atoms on a surface of a substrate, and the substrate processing apparatus configured to etch a region within the substrate.
[0030] Various exemplary embodiments will now be described in detail with reference to the drawings, in which the same or corresponding parts are designated by the same reference numerals.
[0031] Fig. 1 is a flow diagram of an etching method according to an example embodiment. The etching method shown in Fig. 1 (hereinafter referred to as "method MT") is applied to a substrate. Fig. 2 is a partially enlarged cross-sectional view of an example substrate. The substrate W shown in Fig. 2 has a region RE. The region RE is the region to be etched. The substrate W further has a mask MK. The substrate W may further have an undercoat region UR.
[0032] The region RE is provided on the underlayer region UR. The mask MK is provided on the region RE. The mask MK is patterned. That is, the mask MK provides one or more openings. The substrate W has sidewall surfaces and a bottom surface that define each of the one or more openings. In the substrate W shown in FIG. 2, the sidewall surfaces are provided by the mask MK, and the bottom surface is provided by the region RE. The region RE is partially exposed from the opening of the mask MK. The region RE may be formed of any material. The region RE is, for example, a silicon-containing film or an organic film. The region RE may be formed of a dielectric material. The mask MK may be formed of any material as long as the region RE is selectively etched with respect to the mask MK. The mask MK may be a hard mask or a mask formed of a photoresist. The mask MK formed of a photoresist may or may not contain tin atoms. The photoresist may be a photoresist for extreme ultraviolet light.
[0033] Below, some examples of combinations of the region RE and the mask MK are shown.
[0034] In the first example of the substrate W, the region RE is an organic film. In the first example of the substrate W, the mask MK is formed of a silicon-containing film. The silicon-containing film is, for example, an anti-reflective film containing silicon.
[0035] In the second example of the substrate W, the region RE is a low dielectric constant film and contains silicon, carbon, oxygen, and hydrogen. That is, in the second example of the substrate W, the region RE is a SiCOH film. In the second example of the substrate W, the mask MK is formed of a metal-containing film such as a tungsten-containing film or a titanium-containing film. In the second example of the substrate W, the mask MK may be formed of an organic film such as a photoresist film, a silicon nitride film, or a polycrystalline silicon film.
[0036] In the third example of the substrate W, the region RE is a polycrystalline silicon film. In the third example of the substrate W, the mask MK is formed of a metal-containing film such as a tungsten-containing film or a titanium-containing film. In the third example of the substrate W, the mask MK may be formed of an organic film such as a photoresist film, a silicon oxide film, or a silicon nitride film.
[0037] In a fourth example of the substrate W, the region RE is a silicon-containing film. The silicon-containing film may be a silicon-containing dielectric film. The silicon-containing film may be a single layer film. The silicon-containing film may be a multilayer film, at least one of which is formed from a silicon-containing dielectric film. The silicon-containing film is, for example, a silicon oxide film, a silicon nitride film, a multilayer film including an alternating silicon oxide film and a silicon nitride film, or a multilayer film including an alternating silicon oxide film and a polycrystalline silicon film. In a fourth example of the substrate W, the mask MK is formed from an organic film, a metal-containing film, or a polycrystalline silicon film. The organic film is, for example, an amorphous carbon film, a spin-on carbon film, or a photoresist film. The metal-containing film is, for example, formed from tungsten or tungsten carbide.
[0038] In one embodiment, the method MT is performed using a substrate processing apparatus. Figure 3 is a schematic diagram of a substrate processing apparatus according to an exemplary embodiment. The substrate processing apparatus shown in Figure 3 is a capacitively coupled plasma processing apparatus 1.
[0039] The plasma processing apparatus 1 includes a chamber 10. The chamber 10 provides an internal space 10s therein. The chamber 10 may include a chamber body 12. The chamber body 12 has a substantially cylindrical shape. The internal space 10s is provided inside the chamber body 12. The chamber body 12 is made of, for example, aluminum. A corrosion-resistant film may be provided on the inner wall surface of the chamber body 12. The corrosion-resistant film may be a film made of a ceramic such as aluminum oxide or yttrium oxide.
[0040] The sidewall of the chamber body 12 may provide a passage 12p. The substrate W passes through the passage 12p when being transferred between the internal space 10s and the outside of the chamber 10. The passage 12p can be opened and closed by a gate valve 12g. The gate valve 12g is provided along the sidewall of the chamber body 12.
[0041] The plasma processing apparatus 1 further includes a substrate support 14. The substrate support 14 is configured to support the substrate W in the chamber 10, i.e., in the internal space 10s. The substrate support 14 may be supported by a support portion 13. The support portion 13 is made of an insulating material. The support portion 13 has a substantially cylindrical shape. The support portion 13 extends upward from the bottom of the chamber body 12 in the internal space 10s.
[0042] The substrate support 14 may include a lower electrode 18 and an electrostatic chuck 20. The lower electrode 18 and the electrostatic chuck 20 are provided in the chamber 10. The substrate support 14 may further include an electrode plate 16. The electrode plate 16 is provided in the chamber 10. The electrode plate 16 is made of a conductor such as aluminum and has a substantially disk-like shape. The lower electrode 18 is provided on the electrode plate 16. The lower electrode 18 is made of a conductor such as aluminum and has a substantially disk-like shape. The lower electrode 18 is electrically connected to the electrode plate 16.
[0043] FIG. 4 is an enlarged cross-sectional view of an electrostatic chuck in a substrate processing apparatus according to an exemplary embodiment. Hereinafter, reference will be made to FIGS. 3 and 4. The electrostatic chuck 20 is provided on the lower electrode 18. The substrate W is placed on the upper surface of the electrostatic chuck 20. The electrostatic chuck 20 has a main body 20m and an electrode 20e. The main body 20m has a substantially disk shape and is made of a dielectric material. The electrode 20e is a film-like electrode and is provided in the main body 20m. The electrode 20e is connected to a DC power supply 20p via a switch 20s. When a voltage is applied to the electrode 20e from the DC power supply 20p, an electrostatic attractive force is generated between the electrostatic chuck 20 and the substrate W. Due to the generated electrostatic attractive force, the substrate W is attracted to the electrostatic chuck 20 and held by the electrostatic chuck 20.
[0044] The substrate support 14 may have one or more heaters HT. Each of the one or more heaters HT may be a resistive heating element. The plasma processing apparatus 1 may further include a heater controller HC. Each of the one or more heaters HT generates heat in response to power individually provided from the heater controller HC. As a result, the temperature of the substrate W on the substrate support 14 is adjusted. The one or more heaters HT constitute a temperature adjustment mechanism of the plasma processing apparatus 1. In one embodiment, the substrate support 14 has a plurality of heaters HT. The plurality of heaters HT are provided in the electrostatic chuck 20.
[0045] An edge ring ER is disposed on the periphery of the substrate support 14. The substrate W is disposed on the electrostatic chuck 20 within a region surrounded by the edge ring ER. The edge ring ER is used to improve the in-plane uniformity of the plasma processing on the substrate W. The edge ring ER may be formed of, but is not limited to, silicon, silicon carbide, or quartz.
[0046] The lower electrode 18 may provide a flow path 18f for a heat exchange medium (e.g., a coolant) therein. The heat exchange medium is supplied to the flow path 18f from a chiller unit 22 provided outside the chamber 10 via a pipe 22a. The heat exchange medium supplied to the flow path 18f is returned to the chiller unit 22 via a pipe 22b. In the plasma processing apparatus 1, the temperature of the substrate W placed on the electrostatic chuck 20 is adjusted by heat exchange between the heat exchange medium and the lower electrode 18. The chiller unit 22 may also constitute a temperature adjustment mechanism of the plasma processing apparatus 1.
[0047] The plasma processing apparatus 1 may be provided with a gas supply line 24. The gas supply line 24 supplies a heat transfer gas (e.g., He gas) from a heat transfer gas supply mechanism to a gap between the upper surface of the electrostatic chuck 20 and the back surface of the substrate W.
[0048] The plasma processing apparatus 1 further includes an upper electrode 30. The upper electrode 30 is provided above the substrate support 14. The upper electrode 30 is supported on the upper part of the chamber body 12 via a member 32. The member 32 is made of an insulating material. The upper electrode 30 and the member 32 close the upper opening of the chamber body 12.
[0049] The upper electrode 30 may include a top plate 34 and a support 36. The bottom surface of the top plate 34 is the bottom surface on the side of the internal space 10s and defines the internal space 10s. The top plate 34 may be formed of a low-resistance conductor or semiconductor with little Joule heat. The top plate 34 is provided with a plurality of gas discharge holes 34a. The plurality of gas discharge holes 34a penetrate the top plate 34 in the plate thickness direction.
[0050] The support 36 detachably supports the top plate 34. The support 36 is made of a conductive material such as aluminum. The support 36 provides a gas diffusion chamber 36a therein. The support 36 further provides a plurality of gas holes 36b. The plurality of gas holes 36b extend downward from the gas diffusion chamber 36a. The plurality of gas holes 36b communicate with the plurality of gas discharge holes 34a, respectively. The support 36 further provides a gas inlet 36c. The gas inlet 36c is connected to the gas diffusion chamber 36a. A gas supply pipe 38 is connected to the gas inlet 36c.
[0051] A gas source group 40 is connected to the gas supply pipe 38 via a valve group 41, a flow rate controller group 42, and a valve group 43. The gas source group 40, the valve group 41, the flow rate controller group 42, and the valve group 43 constitute a gas supply unit GS. The gas source group 40 includes a plurality of gas sources. The gas sources of the gas source group 40 include a plurality of gas sources used in the method MT. When one or more gases used in the method MT are formed from liquid, the multiple gas sources include one or more gas sources each having a liquid source and a vaporizer. Each of the valve group 41 and the valve group 43 includes a plurality of opening and closing valves. The flow rate controller group 42 includes a plurality of flow rate controllers. Each of the multiple flow rate controllers of the flow rate controller group 42 is a mass flow controller or a pressure-controlled flow rate controller. Each of the multiple gas sources in the gas source group 40 is connected to the gas supply pipe 38 via a corresponding on-off valve in the valve group 41, a corresponding flow rate controller in the flow rate controller group 42, and a corresponding on-off valve in the valve group 43.
[0052] The plasma processing apparatus 1 may further include a shield 46. The shield 46 is detachably provided along the inner wall surface of the chamber body 12. The shield 46 is also provided on the outer periphery of the support portion 13. The shield 46 prevents etching by-products from adhering to the chamber body 12. The shield 46 is formed, for example, by forming a corrosion-resistant film on the surface of a member made of aluminum. The corrosion-resistant film may be a film made of a ceramic such as yttrium oxide.
[0053] The plasma processing apparatus 1 may further include a baffle plate 48. The baffle plate 48 is provided between the support 13 and the side wall of the chamber body 12. The baffle plate 48 is formed by forming a corrosion-resistant film on the surface of a member made of, for example, aluminum. The corrosion-resistant film may be a film made of ceramic such as yttrium oxide. The baffle plate 48 has a plurality of through holes. An exhaust port 12e is provided below the baffle plate 48 and at the bottom of the chamber body 12. An exhaust device 50 is connected to the exhaust port 12e via an exhaust pipe 52. The exhaust device 50 has a pressure adjustment valve and a vacuum pump such as a turbo molecular pump.
[0054] The plasma processing apparatus 1 further includes a first high frequency power supply 62 and a second high frequency power supply 64. The first high frequency power supply 62 is a power supply that generates a first high frequency power. The first high frequency power has a frequency suitable for generating plasma. The frequency of the first high frequency power is, for example, within a range of 27 MHz to 100 MHz. The first high frequency power supply 62 is connected to the upper electrode 30 via a matching device 66. The matching device 66 has a circuit for matching the impedance of the load side (upper electrode 30 side) of the first high frequency power supply 62 to the output impedance of the first high frequency power supply 62. The first high frequency power supply 62 may be connected to the lower electrode 18 via the matching device 66. The first high frequency power supply 62 constitutes an example of a plasma generating unit.
[0055] The second high frequency power supply 64 is a power supply that generates a second high frequency power. The second high frequency power has a frequency lower than that of the first high frequency power. When the second high frequency power is used together with the first high frequency power, the second high frequency power is used as a bias high frequency power for attracting ions to the substrate W. The frequency of the second high frequency power is, for example, within a range of 400 kHz to 13.56 MHz. The second high frequency power supply 64 is connected to the lower electrode 18 via a matching device 68 and the electrode plate 16. The matching device 68 has a circuit for matching the impedance of the load side (lower electrode 18 side) of the second high frequency power supply 64 to the output impedance of the second high frequency power supply 64.
[0056] It is also possible to generate plasma by using the second high frequency power without using the first high frequency power, that is, by using only a single high frequency power. In this case, the frequency of the second high frequency power may be a frequency higher than 13.56 MHz, for example, 40 MHz. In this case, the plasma processing apparatus 1 does not need to include the first high frequency power supply 62 and the matching device 66. In this case, the second high frequency power supply 64 constitutes an example of a plasma generating unit.
[0057] When plasma is generated in the plasma processing apparatus 1, a gas is supplied from the gas supply unit GS to the internal space 10s. A high-frequency electric field is generated between the upper electrode 30 and the lower electrode 18 by supplying a first high-frequency power and / or a second high-frequency power. The gas is excited by the generated high-frequency electric field. As a result, plasma is generated.
[0058] The plasma processing apparatus 1 may further include a control unit 80. The control unit 80 may be a computer including a processor, a storage unit such as a memory, an input device, a display device, a signal input / output interface, and the like. The control unit 80 controls each unit of the plasma processing apparatus 1. In the control unit 80, an operator can use the input device to input commands and the like to manage the plasma processing apparatus 1. In addition, the control unit 80 can visualize and display the operating status of the plasma processing apparatus 1 using the display device. Furthermore, a control program and recipe data are stored in the storage unit of the control unit 80. The control program is executed by the processor of the control unit 80 to execute various processes in the plasma processing apparatus 1. The processor of the control unit 80 executes the control program and controls each unit of the plasma processing apparatus 1 according to the recipe data, whereby the method MT is executed in the plasma processing apparatus 1.
[0059] The method MT will be described in detail with reference to Fig. 1 again. In the following description, the method MT will be described by taking as an example a case where the substrate W shown in Fig. 2 is processed using the plasma processing apparatus 1. Note that the method MT may use other substrate processing apparatuses. The method MT may also process other substrates.
[0060] The method MT is performed with the substrate W placed on the substrate support 14. The method MT may be performed while maintaining a reduced pressure environment in the internal space 10s of the chamber 10 and without removing the substrate W from the internal space 10s. In one embodiment, the method MT may start with step STa. In step STa, the region RE is etched. The region RE may be etched using plasma.
[0061] In step STa, plasma Pa is generated from the processing gas in the chamber 10. When the first example of the substrate W described above is processed, i.e., when the region RE of the substrate W is an organic film, the processing gas used in step STa may contain an oxygen-containing gas. The oxygen-containing gas contains, for example, oxygen gas, carbon monoxide gas, or carbon dioxide gas. Alternatively, when the first example of the substrate W is processed, the processing gas used in step STa may contain nitrogen gas and / or hydrogen gas.
[0062] When the second example of the substrate W described above is processed, that is, when the region RE of the substrate W is a low dielectric constant film, the process gas used in the step STa may contain a gas containing fluorine. The gas containing fluorine is, for example, a fluorocarbon gas. The fluorocarbon gas is, for example, C 4 F 8 It's gas.
[0063] When the third example of the substrate W described above is processed, that is, when the region RE of the substrate W is a polycrystalline silicon film, the processing gas used in the step STa may contain a halogen-containing gas. The halogen-containing gas may be, for example, HBr gas, Cl 2 Gas or SF 6 It's gas.
[0064] In the fourth example of the substrate W described above, when the region RE is a silicon oxide film, the process gas used in the process STa may include a fluorocarbon gas. In the fourth example of the substrate W, when the region RE is a silicon nitride film, the process gas used in the process STa may include a hydrofluorocarbon gas. In the fourth example of the substrate W, when the region RE is a multilayer film including alternately stacked silicon oxide films and silicon nitride films, the process gas used in the process STa may include a fluorocarbon gas and a hydrofluorocarbon gas. In the fourth example of the substrate W, when the region RE is a multilayer film including alternately stacked silicon oxide films and polycrystalline silicon films, the process gas used in the process STa may include a fluorocarbon gas and a halogen-containing gas. The fluorocarbon gas may be, for example, CF 4 Gas, C. 4 F6 Gas or C 4 F 8 Hydrofluorocarbon gases are, for example, CH 3 F gas. The halogen-containing gas is, for example, HBr gas or Cl 2 It's gas.
[0065] FIG. 5(a) is a diagram for explaining an example of step STa of the etching method shown in FIG. 1, and FIG. 5(b) is a partially enlarged cross-sectional view of an example of a substrate in a state after the step STa is performed. In the step STa, as shown in FIG. 5(a), chemical species from plasma Pa are supplied to the region RE, and the region RE is etched by the chemical species. In the step STa, the region RE is etched to a position between the lower surface of the region RE and the upper surface of the region RE. This position is determined so that the region RE is not substantially etched in the lateral direction even if the region RE is etched to that position in the step STa. The lower surface of the region RE is the surface of the region RE that contacts the base region UR. The upper surface of the region RE is the surface of the region RE exposed from the opening of the mask MK. When the step STa is performed, an opening OP that is continuous with the mask MK is formed in the region RE as shown in FIG. 5(b). The opening OP is defined by a side wall surface SS and a bottom surface BS. The side wall surface SS is provided by the mask MK and the region RE. The bottom surface BS is provided by the region RE. After performing the step STa, the mask MK may be thinned.
[0066] In step STa, the control unit 80 controls the gas supply unit GS to supply a processing gas into the chamber 10. In step STa, the control unit 80 controls the exhaust device 50 to set the pressure of the gas in the chamber 10 to a designated pressure. In step STa, the control unit 80 controls the plasma generating unit to generate plasma from the processing gas. In step STa in one embodiment, the control unit 80 controls the first high frequency power supply 62 and / or the second high frequency power supply 64 to supply a first high frequency power and / or a second high frequency power.
[0067] The method MT may not include step STa. In this case, an opening OP is provided in advance in the region RE of the substrate to which the method MT is applied. Alternatively, when the method MT does not include step STa, steps ST1 and ST2 are applied to the substrate W shown in FIG. 2.
[0068] In step ST1, a protective film PF is formed on the surface of the substrate W. The protective film PF contains tin (Sn) atoms. The protective film PF may be, for example, a film containing metal tin as a main component, a film containing tin oxide (SnO x ), a film containing tin hydroxide (Sn(OH) x ), tin nitride (Sn x N y ), a film containing tin sulfide (SnS x ) as a main component, or a film containing a tin halide as a main component. Here, each of "x" and "y" is an integer of 1 or more. The oxide of tin is, for example, SnO 2 , SnO, etc. Tin hydroxides are, for example, Sn(OH) 2 , Sn(OH) 4 Nitrides of tin include, for example, SnN and Sn 3 N 4 Tin sulfides include, for example, SnS, SnS 2 Tin halides include, for example, SnF 4 , SnCl 2 , SnBr 2 , SnI 2 The compounds constituting the protective film may be composited and / or mixed in any ratio.
[0069] In one embodiment, the step ST1 may be formed by a film formation method shown in the flowchart of Fig. 6. Fig. 6 is a flowchart of a film formation method that may be used in the etching method according to one example embodiment.
[0070] In one embodiment, step ST1 includes step ST11 and step ST13. Step ST1 may further include step ST12 and step ST14. Step ST12 is performed between step ST11 and step ST13. Step ST14 is performed between step ST13 and step ST11.
[0071] In step ST11, a first gas is supplied to the substrate W. That is, in step ST11, the first gas is supplied into the chamber 10. In step ST11, plasma may be generated from the first gas in the chamber 10. Alternatively, in step ST11, plasma may not be generated from the first gas. In step ST11, the control unit 80 controls the gas supply unit GS to supply the first gas into the chamber 10. In step ST11, the control unit 80 controls the exhaust device 50 to set the pressure of the gas in the chamber 10 to a designated pressure. When plasma is generated in step ST11, the control unit 80 controls the plasma generation unit to generate plasma from the first gas in the chamber 10. In one embodiment, in order to generate plasma from the first gas, the control unit 80 controls the first high frequency power supply 62 and / or the second high frequency power supply 64 to supply a first high frequency power and / or a second high frequency power.
[0072] In step ST12, the internal space 10s is purged. In step ST12, the control unit 80 controls the exhaust device 50 to exhaust the internal space 10s. In step ST12, the control unit 80 may control the gas supply unit GS to supply an inert gas into the chamber 10. By performing step ST12, the first gas in the chamber 10 may be replaced with the inert gas. By performing step ST12, excess substances adsorbed on the substrate W may be removed.
[0073] In step ST13, a second gas is supplied to the substrate W. That is, in step ST13, the second gas is supplied into the chamber 10. In step ST13, plasma may be generated from the second gas in the chamber 10. Alternatively, in step ST13, plasma may not be generated from the second gas. In step ST13, the control unit 80 controls the gas supply unit GS to supply the second gas into the chamber 10. In step ST13, the control unit 80 controls the exhaust device 50 to set the pressure of the gas in the chamber 10 to a designated pressure. When plasma is generated in step ST13, the control unit 80 controls the plasma generation unit to generate plasma from the second gas in the chamber 10. In one embodiment, in order to generate plasma from the second gas, the control unit 80 controls the first high frequency power supply 62 and / or the second high frequency power supply 64 to supply a first high frequency power and / or a second high frequency power. A protective film PF is formed on the surface of the substrate W by steps ST11 and ST13.
[0074] In step ST14, the internal space 10s is purged. Step ST14 is the same as step ST12. By performing step ST14, the second gas in the chamber 10 can be replaced with an inert gas.
[0075] In step ST1, a plurality of film formation cycles CY1 each including step ST11 and step ST13 may be repeated in sequence. Each of the plurality of film formation cycles CY1 may further include step ST12 and step ST14. The thickness of the protective film PF may be adjusted by the number of times the film formation cycle CY1 is repeated. When the film formation cycle CY1 is repeated, it is determined in step ST15 whether or not a stop condition is satisfied. The stop condition is satisfied when the number of times the film formation cycle CY1 is performed reaches a predetermined number. When it is determined in step ST15 that the stop condition is not satisfied, the film formation cycle CY1 is performed again. When it is determined in step ST15 that the stop condition is satisfied, the execution of step ST1 is terminated, and the process proceeds to step ST2.
[0076] In one embodiment, one of the first gas and the second gas includes a tin-containing material, and the other of the first gas and the second gas includes H 2 O, H 2 O 2 , O 2 , O 3 , N 2 O 4 , a nitrogen-containing inorganic compound, a sulfur-containing inorganic compound, a halogen compound, a carbon-containing substance, a silicon-containing substance, or a tin-containing substance. In this case, the other of the first gas and the second gas may be used without generating a plasma thereof, or a plasma may be generated from the other of the first gas and the second gas. Alternatively, the other of the first gas and the second gas may be N 2 and an oxygen-containing substance. In this case, a chemical species from a plasma generated from the other of the first gas and the second gas may be supplied to the precursor layer containing tin atoms formed on the surface of the substrate W. Alternatively, at least one of the first gas and the second gas may be supplied to the precursor layer containing tin atoms formed on the surface of the substrate W without generating plasma therefrom. The oxygen-containing substance may be NO or CO 2 It could be.
[0077] The tin-containing material may be, for example, a stannane compound, an oxygen-containing tin compound, a nitrogen-containing tin compound, or a tin halide compound.
[0078] Examples of the stannane compound include stannane, tetramethylstannane, tributylstannane, phenyltrimethylstannane, tetravinylstannane, dimethyldichlorostannane, butyltrichlorostannane, and trichlorophenylstannane.
[0079] Examples of oxygen-containing tin compounds include tributyltin methoxide, tin tert-butoxide, dibutyltin diacetate, triphenyltin acetate, tributyltin oxide, triphenyltin acetate, triphenyltin hydroxide, butylchlorotin dihydroxide, and tin acetylacetonate.
[0080] Examples of nitrogen-containing tin compounds include dimethylaminotrimethyltin, tris(dimethylamino)tert-butyltin, azidotrimethyltin, tetrakis(dimethylamino)tin, and N,N'-di-tert-butyl-2,3-diamidinobutanetin(II).
[0081] Examples of the tin halide compound include tin chloride, tin bromide, tin iodide, dimethyltin dichloride, butyltin trichloride, phenyltin trichloride, etc. The tin halide compound may be tetravalent tin chloride, tin bromide, or tin iodide. Tetravalent tin chloride, tin bromide, and tin iodide have low melting points, and therefore may be used to form a precursor layer from which the protective film PF is formed. On the other hand, tetravalent tin fluoride and divalent tin halide have high melting points, and therefore may be used as materials for forming the protective film PF.
[0082] An example of a nitrogen-containing inorganic compound that may be contained in the other of the first gas and the second gas is NH 3 , N 2 O 4 The sulfur-containing inorganic compound that may be contained in the other of the first gas and the second gas is, for example, H 2 S, SO 2 , COS, or CS 2 The halogen compound that may be contained in the other of the first gas and the second gas is CF 4 , F 2 , CCl 4 The carbon-containing substance that may be contained in the other of the first gas and the second gas is a hydrocarbon, a fluorocarbon, an organic compound having a hydroxyl group, a carboxylic acid, a carboxylic acid anhydride, or a carboxylic acid halide. The hydrocarbon is, for example, methane or propylene. The fluorocarbon is, for example, CF 4 Or C 4 F 6The organic compound having a hydroxyl group is, for example, an alcohol such as methanol or ethylene glycol, or a phenol. The carboxylic acid is, for example, acetic acid or oxalic acid. The silicon-containing material that may be contained in the other of the first gas and the second gas is, for example, silicon chloride or aminosilane.
[0083] Hereinafter, reference will be made to FIG. 6 as well as FIG. 7(a) and FIG. 7(b). FIG. 7(a) is a partially enlarged cross-sectional view of an example substrate after a precursor layer is formed. FIG. 7(b) is a partially enlarged cross-sectional view of an example substrate after a protective film is formed. In one embodiment, in step ST11, a precursor layer PC may be formed on the surface of the substrate W using a first gas. In this embodiment, the first gas contains the above-mentioned tin-containing material. The first gas may further contain a carrier gas. The carrier gas is an inert gas. The inert gas is, for example, a rare gas or nitrogen gas. In step ST11, as shown in FIG. 7(a), a precursor layer PC is formed on the substrate W from a material contained in the first gas. Note that the precursor layer PC may be formed as a monolayer on the substrate W by performing steps ST11 and ST12.
[0084] In one embodiment, in step ST13, as shown in FIG. 7(b), a protective film PF may be formed from the precursor layer PC. In step ST13, a second gas is used to form the protective film PF. The second gas contains a reactive species that reacts with a substance constituting the precursor layer PC to form the protective film PF from the precursor layer PC. The second gas may further contain a carrier gas. The carrier gas is an inert gas. In step ST13, the protective film PF may be formed by oxidizing, nitriding, sulfiding, reducing, or halogenating the precursor layer PC using the second gas. The second gas for oxidizing the precursor layer PC is, for example, H 2 O, H 2 O 2 , O 3 , O 2 , and N 2 O 4The second gas for nitriding the precursor layer PC includes at least one of the above-mentioned nitrogen-containing inorganic compounds, N 2 , and N 2 O 4 The second gas for sulfurizing the precursor layer PC includes, for example, the above-mentioned inorganic compound containing sulfur. The second gas for reducing the precursor layer PC includes, for example, CO or 1,4-bis(trimethylsilyl)-1,4-dihydropyrazine. The second gas for halogenating the precursor layer PC includes, for example, the above-mentioned halogen compound.
[0085] Referring again to FIG. 1, in one embodiment, step ST2 is performed after step ST1 as shown in FIG. The method MT may further include a step (breakthrough step) of generating plasma from a processing gas and etching the protective film PF on the bottom surface BS before step ST2. The processing gas used in the breakthrough step may include a hydrogen-containing gas. The hydrogen-containing gas may be H 2 , hydrocarbons, and hydrogen halides. The hydrocarbons include, for example, CH 4 The hydrogen halide is, for example, HBr. The process gas used in the breakthrough step may further contain a rare gas (for example, Ar gas).
[0086] In step ST2, the region RE is etched. In one embodiment, the region RE is etched by chemical species from plasma. In step ST2, a plasma P2 is generated from a processing gas in the chamber 10. The processing gas used in step ST2 for the processing of each of the above-mentioned examples of the substrate W may be the same as the processing gas used in step STa.
[0087] Fig. 8(a) is a diagram for explaining an example of step ST2 of the etching method shown in Fig. 1, and Fig. 8(b) is a partially enlarged cross-sectional view of an example of a substrate in a state after performing step ST2. In step ST2, as shown in Fig. 8(a), chemical species from plasma P2 are irradiated onto region RE, and region RE is etched by the chemical species. As a result of performing step ST2, the depth of opening OP is increased as shown in Fig. 8(b).
[0088] In step ST2, the control unit 80 controls the gas supply unit GS to supply a processing gas into the chamber 10. In step ST2, the control unit 80 controls the exhaust device 50 to set the pressure of the gas in the chamber 10 to a designated pressure. In step ST2, the control unit 80 controls the plasma generating unit to generate plasma from the processing gas. In step ST2 in one embodiment, the control unit 80 controls the first high frequency power supply 62 and / or the second high frequency power supply 64 to supply a first high frequency power and / or a second high frequency power.
[0089] In the method MT, multiple cycles CY each including a step ST1 and a step ST2 may be executed in sequence. When multiple cycles CY are executed in sequence, it is determined whether or not a stop condition is satisfied in step ST3. The stop condition is satisfied when the number of times the cycle CY has been executed reaches a predetermined number of times. When it is determined that the stop condition is not satisfied in step ST3, the cycle CY is executed again. When it is determined that the stop condition is satisfied in step ST3, step ST4 may then be executed.
[0090] In step ST4, the protective film PF is removed. In step ST4, the protective film PF is etched using a removal gas. In step ST4, the protective film may be etched by chemical species from plasma generated from the removal gas. Alternatively, the protective film may be etched without generating plasma using the removal gas. The removal gas may include a hydrogen-containing gas. The hydrogen-containing gas may be H 2 , hydrocarbons, and hydrogen halides. The hydrocarbons include, for example, CH4 The hydrogen halide is, for example, HBr. The removal gas may further include a rare gas (for example, Ar gas). The removal gas may include Cl 2 The gas may contain halogen gas such as:
[0091] In step ST4, the control unit 80 controls the gas supply unit GS to supply a removal gas into the chamber 10. In step ST4, the control unit 80 controls the exhaust device 50 to set the pressure of the gas in the chamber 10 to a designated pressure. In step ST4, the control unit 80 controls the plasma generation unit to generate plasma from the removal gas. In step ST4 in one embodiment, the control unit 80 controls the first high frequency power supply 62 and / or the second high frequency power supply 64 to supply a first high frequency power and / or a second high frequency power.
[0092] As described above, in the method MT, a protective film PF containing tin (Sn) is formed on the surface of the substrate. In the method MT, the region RE in the substrate W is etched. Therefore, the method MT makes it possible to etch the region RE while the surface of the mask MK and / or the side wall surface SS provided by the region RE are protected. Therefore, the method MT makes it possible to increase the selectivity of etching the region RE relative to etching the mask MK. In addition, the method MT makes it possible to adjust the dimensions of the mask MK by the protective film PF. In addition, the method MT makes it possible to correct the shape of the mask MK by the protective film PF. In addition, the method MT makes it possible to protect the side wall surface SS during etching of the region RE. Since the protective film PF contains tin atoms, it has a high etching resistance compared to organic films and silicon-containing films. In addition, the protective film PF is easier to remove compared to protective films containing other metals. The protective film PF can be easily removed using, for example, a plasma of a hydrogen-containing gas. Therefore, the protective film PF is less likely to be a source of contamination in the chamber 10.
[0093] In one embodiment, the conditions of step ST1 for forming the protective film PF in at least one of the multiple cycles CY may be different from the conditions of step ST1 for forming the protective film PF in at least one other cycle of the multiple cycles CY. The conditions of step ST1 in all the cycles CY may be different from each other. In this case, the protective film PF in each cycle may be formed so that its thickness or coverage is different from the thickness or coverage of the protective film PF formed in the other cycles.
[0094] In one embodiment, the conditions of step ST2 in at least one of the multiple cycles CY may be different from the conditions of step ST2 in at least one other cycle of the multiple cycles CY. The conditions of step ST2 in all the cycles CY may be different from each other. In this case, the region RE is etched in each cycle such that the etching amount of the region RE is different from the etching amount of the region RE in the other cycles.
[0095] In one embodiment, in each of the multiple cycles CY, the conditions for forming the protective film PF in one of the multiple film formation cycles CY1 may be different from the conditions for forming the protective film PF in at least one other film formation cycle among the multiple film formation cycles CY1. That is, in each of the multiple cycles CY, the conditions for step ST11 and / or step ST13 in one film formation cycle may be different from the conditions for step ST11 and / or step ST13 in at least one other film formation cycle. In each of the multiple cycles CY, the conditions for forming the protective film PF in all the film formation cycles CY1 may be different from each other. In this case, the distribution of the thickness of the protective film PF can be controlled in each of the multiple film formation cycles CY1 included in each of the multiple cycles CY.
[0096] Hereinafter, reference will be made to (a) and (b) of FIG. 9. (a) of FIG. 9 is a partially enlarged cross-sectional view of an example substrate after a precursor layer is formed, and (b) of FIG. 9 is a partially enlarged cross-sectional view of an example substrate after a protective film is formed. As shown in (b) of FIG. 9, the protective film PF only needs to cover a part of the side wall surface SS that would otherwise be etched laterally, and does not need to cover the entire surface of the substrate W. For example, the protective film PF does not need to cover the bottom surface BS. Alternatively, the thickness of the protective film PF may vary depending on the position in the depth direction in the opening OP. That is, the thickness of the protective film PF may have a distribution that changes depending on the position in the depth direction in the opening OP. For example, the thickness of the protective film PF may be large near the upper end of the opening OP and small or zero near the deep part of the opening OP. The protective film PF having such a thickness distribution can be formed by a protective film PF formation process or chemical vapor deposition (CVD) method described below with reference to (a) and (b) of FIG. 9.
[0097] In order to form the protective film PF shown in FIG. 9B, in step ST11, the precursor layer PC may be formed to cover a part of the side wall surface SS but not the entire surface of the substrate W, as shown in FIG. 9A. In order to form the precursor layer PC in this way, at least one of the conditions (1) to (5) is satisfied in step ST11. In the condition (1), the gas pressure in the chamber 10 during the execution of step ST11 is set to a pressure lower than the pressure at which the substance forming the precursor layer PC is adsorbed on the entire surface of the substrate W when other processing conditions are the same. In the condition (2), the processing time of step ST11 is set to a time shorter than the processing time at which the substance forming the precursor layer PC is adsorbed on the entire surface of the substrate W when other processing conditions are the same. In the condition (3), the dilution degree of the substance forming the precursor layer PC in the first gas is set to a value higher than the dilution degree at which the substance forming the precursor layer PC is adsorbed on the entire surface of the substrate W when other processing conditions are the same. Under condition (4), the temperature of the substrate support 14 during step ST11 is set to a temperature lower than the temperature at which the substance that forms the precursor layer PC is adsorbed onto the entire surface of the substrate W when other processing conditions are the same. Condition (5) can be applied when plasma is generated in step ST11. Under condition (5), the absolute value of the high-frequency power (the first high-frequency power and / or the second high-frequency power) is set to a value smaller than the absolute value at which the substance that forms the precursor layer PC is adsorbed onto the entire surface of the substrate W when other processing conditions are the same.
[0098] In order to form the protective film PF shown in FIG. 9B, at least one of the conditions (1) to (5) may be satisfied in step ST13. In the condition (1), the pressure of the gas in the chamber 10 during the execution of step ST13 is set to a pressure lower than the pressure at which the reaction between the substance in the second gas and the substance forming the precursor layer PC is completed over the entire precursor layer PC when other processing conditions are the same. In the condition (2), the processing time of step ST13 is set to a time shorter than the processing time at which the reaction between the substance in the second gas and the substance forming the precursor layer PC is completed over the entire precursor layer PC when other processing conditions are the same. In the condition (3), the dilution degree of the substance forming the protective film PF in the second gas is set to a value higher than the dilution degree at which the reaction between the substance in the second gas and the substance forming the precursor layer PC is completed over the entire precursor layer PC when other processing conditions are the same. Under condition (4), the temperature of the substrate support 14 during step ST13 is set to a temperature lower than the temperature at which the reaction between the substance in the second gas and the substance that forms the precursor layer PC is completed throughout the entire precursor layer PC when other processing conditions are the same. Condition (5) can be applied when plasma is generated in step ST13. Under condition (5), the absolute value of the high-frequency power (the first high-frequency power and / or the second high-frequency power) is set to a value smaller than the absolute value at which the reaction between the substance in the second gas and the substance that forms the precursor layer PC is completed throughout the entire precursor layer PC when other processing conditions are the same.
[0099] In another embodiment, a chemical vapor deposition method (CVD method) may be used as the film formation method in step ST1 of the method MT. The CVD method used in step ST1 may be a plasma CVD method or a thermal CVD method. When the CVD method is used as the film formation method in step ST1, the film formation gas supplied to the chamber 10 contains the above-mentioned tin-containing substance. The film formation gas may further contain an additive gas. The additive gas may be an inorganic compound containing nitrogen, an inorganic compound containing sulfur, a halogen compound, a carbon-containing substance, a silicon-containing substance, a N-containing substance, or a tin-containing substance, as described above in relation to the first gas and the second gas. 2 , H 2 O, H 2 O2 , O 2 , O 3 , N 2 O 4 , an oxygen-containing material, and / or a rare gas.
[0100] Reference is now made to Fig. 10. Method MT may be performed using a substrate processing system including a film forming apparatus and a plasma processing apparatus. Fig. 10 is a diagram showing a substrate processing system according to an exemplary embodiment. The substrate processing system PS shown in Fig. 10 may be used to perform method MT.
[0101] The substrate processing system PS includes stages 2a-2d, containers 4a-4d, a loader module LM, an aligner AN, load lock modules LL1, LL2, process modules PM1-PM6, a transfer module TF, and a controller MC. The number of stages, containers, and load lock modules in the substrate processing system PS may be any number equal to or greater than one. The number of process modules in the substrate processing system PS may be any number equal to or greater than two.
[0102] The stages 2a to 2d are arranged along one edge of the loader module LM. The containers 4a to 4d are mounted on the stages 2a to 2d, respectively. Each of the containers 4a to 4d is, for example, a container called a FOUP (Front Opening Unified Pod). Each of the containers 4a to 4d is configured to accommodate a substrate W therein.
[0103] The loader module LM has a chamber. The pressure in the chamber of the loader module LM is set to atmospheric pressure. The loader module LM has a transport device TU1. The transport device TU1 is, for example, an articulated robot, and is controlled by the controller MC. The transport device TU1 is configured to transport the substrate W through the chamber of the loader module LM. The transport device TU1 can transport the substrate W between each of the containers 4a to 4d and the aligner AN, between the aligner AN and each of the load lock modules LL1 to LL2, and between each of the load lock modules LL1 to LL2 and each of the containers 4a to 4d. The aligner AN is connected to the loader module LM. The aligner AN is configured to adjust the position of the substrate W (calibrate the position).
[0104] Each of the load lock modules LL1 and LL2 is provided between the loader module LM and the transfer module TF. Each of the load lock modules LL1 and LL2 provides a preliminary reduced pressure chamber.
[0105] The transfer module TF is connected to each of the load lock modules LL1 and LL2 via gate valves. The transfer module TF has a transfer chamber TC that can be depressurized. The transfer module TF has a transfer apparatus TU2. The transfer apparatus TU2 is, for example, an articulated robot, and is controlled by a controller MC. The transfer apparatus TU2 is configured to transfer the substrate W via the transfer chamber TC. The transfer apparatus TU2 can transfer the substrate W between each of the load lock modules LL1 to LL2 and each of the process modules PM1 to PM6, and between any two of the process modules PM1 to PM6.
[0106] Each of the process modules PM1 to PM6 is a processing apparatus configured to perform a dedicated substrate processing. One of the process modules PM1 to PM6 is a film forming apparatus. This film forming apparatus is used to form a protective film PF in step ST1. When plasma is generated in step ST1, this film forming apparatus is a plasma processing apparatus such as the plasma processing apparatus 1 or another plasma processing apparatus. When the protective film PF is formed without generating plasma in step ST1, this film forming apparatus does not need to have a configuration for generating plasma.
[0107] Another process module among the process modules PM1 to PM6 is a substrate processing apparatus such as the plasma processing apparatus 1 or another plasma processing apparatus. This substrate processing apparatus is used to etch the region RE in step ST2. This substrate processing apparatus may be used for the etching in step STa and the removal of the protective film PF in step ST4. Alternatively, the etching in step STa may be performed using a substrate processing apparatus that is yet another process module among the process modules PM1 to PM6. Also, the removal of the protective film PF in step ST4 may be performed using a substrate processing apparatus that is yet another process module among the process modules PM1 to PM6.
[0108] In the substrate processing system PS, a control unit MC is configured to control each unit of the substrate processing system PS. The control unit MC controls a film forming apparatus to form a protective film PF in step ST1. After forming the protective film PF, the control unit MC controls the substrate processing apparatus to etch the region RE to increase the depth of the opening OP. This substrate processing system PS can transport the substrate W between process modules without exposing it to the atmosphere.
[0109] Reference is now made to FIG. 11. FIG. 11 is a flow chart of an etching method according to another exemplary embodiment. The etching method shown in FIG. 11 (hereinafter referred to as "method MT2") is applied to a substrate. Method MT2 may be applied to, for example, substrate W shown in FIG. 2. Method MT2 will be described below using, as an example, a case in which substrate W shown in FIG. 2 is processed using plasma processing apparatus 1. Note that other substrate processing apparatuses may be used in method MT2. Other substrates may be processed in method MT2.
[0110] The method MT2 is performed with the substrate W placed on the substrate support 14. The method MT2 may start with step STa. Step STa in the method MT2 is the same as step STa in the method MT. The method MT2 may not include step STa. In this case, an opening OP is provided in advance in the region RE of the substrate to which the method MT2 is applied. Alternatively, when the method MT2 does not include step STa, steps ST21 and ST22 in the method MT2 are applied to the substrate W shown in FIG. 2.
[0111] In step ST21, a protective film PF is formed on the surface of the substrate W. Step ST21 includes steps ST211 and ST212. In step ST211, a precursor layer PC is formed on the surface of the substrate W. The precursor layer PC includes tin atoms. In step ST211, a first gas is used to form the precursor layer PC. The first gas includes the tin-containing material described above in relation to the method MT. The first gas used in step ST211 may further include a carrier gas. The carrier gas is an inert gas. The inert gas is, for example, a rare gas or nitrogen gas. In step ST211, as shown in (a) of FIG. 7, a precursor layer PC is formed on the substrate W from a material contained in the first gas. In step ST211, the precursor layer PC may be formed without generating plasma from the first gas. Alternatively, in step ST211, the precursor layer PC may be formed using chemical species from the plasma generated from the first gas.
[0112] In step ST211, the control unit 80 controls the gas supply unit GS to supply a first gas into the chamber 10. In step ST211, the control unit 80 controls the exhaust device 50 to set the pressure of the gas in the chamber 10 to a designated pressure. When plasma is generated in step ST211, the control unit 80 controls the plasma generating unit to generate plasma from the film formation gas in the chamber 10. In one embodiment, in order to generate plasma from the film formation gas, the control unit 80 controls the first high frequency power supply 62 and / or the second high frequency power supply 64 to supply a first high frequency power and / or a second high frequency power.
[0113] Step ST212 is performed after step ST211. In step ST212, a protective film PF is formed from the precursor layer PC using chemical species from the plasma of the second gas. The substance contained in the second gas for forming the protective film PF from the precursor layer PC may be the same as the substance in the second gas used in step ST13 of the method MT.
[0114] In the method MT2, step ST22 is performed during the execution of step ST212. In other words, step ST212 and step ST22 are performed simultaneously. In step ST22, the region RE is etched by chemical species from the plasma of the second gas during the execution of step ST212. The chemical species from the plasma that changes the precursor layer PC into a protective film PF and the chemical species from the plasma that etches the region RE may be the same as or different from each other. By simultaneously performing step ST212 and step ST22, as shown in (b) of FIG. 8, the protective film PF is formed from the precursor layer PC, and at the same time, the region RE is etched, increasing the depth of the opening OP.
[0115] When the first example of the substrate W described above is processed in the method MT2, i.e., when the region RE of the substrate W is an organic film, the second gas may include an oxygen-containing gas. The oxygen-containing gas may be, for example, oxygen gas (O 2 gas), carbon monoxide gas (CO gas), or carbon dioxide gas (CO 2In this case, the second gas may further include carbonyl sulfide gas. When the first example of the substrate W is processed in the method MT2, the second gas includes O 2 , CO 2 , N 2 , H 2 , H 2 The inorganic compound having an NH bond may include at least one of the following: 3 , N 2 H 2 When the first example of the substrate W is processed in the method MT2, a protective film PF is formed from the precursor layer PC by chemical species from the plasma formed from the second gas, and a region RE is etched by chemical species from the plasma formed from the second gas.
[0116] When the second example of the substrate W described above is processed in the method MT2, i.e., when the region RE of the substrate W is a low dielectric constant film, the second gas contains fluorine and nitrogen. For example, the second gas contains a fluorocarbon gas and a nitrogen-containing gas. The fluorocarbon gas is, for example, C 4 F 8 The nitrogen-containing gas is, for example, nitrogen gas (N 2 In this case, the second gas may further include a rare gas (e.g., Ar gas) and / or an oxygen-containing gas. The oxygen-containing gas is oxygen gas (O 2 ), carbon dioxide gas (CO 2 In this case, a protective film PF is formed from the precursor layer PC by at least one of halogen species, nitrogen species, and oxygen species from the plasma formed from the second gas. Also, the region RE is etched by fluorine species from the plasma formed from the second gas.
[0117] When the third example of the substrate W described above is processed in the method MT2, that is, when the region RE of the substrate W is a polycrystalline silicon film, the second gas may include a halogen-containing gas and / or an oxygen-containing gas. The halogen-containing gas may be, for example, HBr gas, Cl 2 Gas or SF6 The second gas is a gas. The oxygen-containing gas includes, for example, oxygen gas, carbon monoxide gas, or carbon dioxide gas. In this case, the second gas may further include a rare gas (for example, Ar gas). In this case, the protective film PF is formed from the precursor layer PC by oxygen species from the plasma formed from the second gas. Also, the region RE is etched by halogen species from the plasma formed from the second gas.
[0118] When a fourth example of the substrate W in which the region RE is a silicon oxide film is processed in the method MT2, the second gas includes a fluorocarbon gas. In this case, the second gas further includes an oxygen-containing and / or nitrogen-containing gas. The fluorocarbon gas is, for example, CF 4 Gas, C. 4 F 6 Gas or C 4 F 8 The oxygen-containing gas is, for example, oxygen gas (O 2 gas), carbon monoxide gas (CO gas), or carbon dioxide gas (CO 2 The nitrogen-containing gas includes, for example, nitrogen gas (N 2 In this case, the second gas may further include a rare gas (e.g., Ar gas). In this case, a protective film PF is formed from the precursor layer PC by oxygen species and / or nitrogen species from the plasma formed from the second gas. In addition, the region RE is etched by fluorine species from the plasma formed from the second gas.
[0119] When a fourth example of the substrate W in which the region RE is a silicon nitride film is processed in the method MT2, the second gas includes a hydrofluorocarbon gas and / or an oxygen-containing gas. The hydrofluorocarbon gas is, for example, CH 3 The oxygen-containing gas is, for example, oxygen gas (O 2 gas), carbon monoxide gas (CO gas), or carbon dioxide gas (CO 2In this case, the second gas may further include a rare gas (e.g., Ar gas). In this case, the protective film PF is formed from the precursor layer PC by oxygen species from the plasma formed from the second gas. Also, the region RE is etched by fluorine species from the plasma formed from the second gas.
[0120] When a fourth example of the substrate W in which the region RE is a multilayer film including alternately stacked silicon oxide films and silicon nitride films is processed by the method MT2, the second gas includes a fluorocarbon gas and a hydrofluorocarbon gas. In this case, the second gas further includes an oxygen-containing and / or nitrogen-containing gas. In this case, the second gas may further include a rare gas (e.g., Ar gas). In this case, the protective film PF is formed from the precursor layer PC by oxygen species or nitrogen species from the plasma formed from the second gas. Also, the region RE is etched by fluorine species from the plasma formed from the second gas.
[0121] When a fourth example of the substrate W in which the region RE is a multilayer film including alternating silicon oxide films and polycrystalline silicon films is processed in the method MT2, the second gas includes a fluorocarbon gas and a halogen-containing gas. The fluorocarbon gas is, for example, CF 4 Gas, C. 4 F 6 Gas or C 4 F 8 The halogen-containing gas is, for example, HBr gas or Cl 2 In this case, the second gas further includes an oxygen-containing and / or nitrogen-containing gas. In this case, the second gas may further include a rare gas (e.g., Ar gas). In this case, the protective film PF is formed from the precursor layer PC by oxygen species or nitrogen species from the plasma formed from the second gas. In addition, the region RE is etched by fluorine species and halogen species from the plasma formed from the second gas.
[0122] In steps ST212 and ST22, the control unit 80 controls the gas supply unit GS to supply the second gas into the chamber 10. In steps ST212 and ST22, the control unit 80 controls the exhaust device 50 to set the pressure of the gas in the chamber 10 to a designated pressure. In steps ST212 and ST22, the control unit 80 controls the plasma generating unit to generate plasma from the second gas. In steps ST212 and ST22, the control unit 80 controls the first high frequency power supply 62 and / or the second high frequency power supply 64 to supply the first high frequency power and / or the second high frequency power.
[0123] In the method MT2, multiple cycles each including step ST21 and step ST22 may be executed in sequence. When multiple cycles are executed in sequence, it is determined whether or not a stop condition is satisfied in step ST23. The stop condition is satisfied when the number of times the cycle has been executed reaches a predetermined number. When it is determined in step ST23 that the stop condition is not satisfied, the cycle is executed again. When it is determined in step ST23 that the stop condition is satisfied, step ST24 may then be executed. Step ST24 is a step similar to step ST4.
[0124] Method MT2 may be performed using a substrate processing system PS. In this case, step ST211 is performed using one of the process modules PM1 to PM6, which is a film forming apparatus. Step ST212 and step ST22 are performed using another of the process modules PM1 to PM6, which is the plasma processing apparatus 1 or another plasma processing apparatus. Step ST24 is performed using one of the process modules PM1 to PM6, which is the plasma processing apparatus 1 or another plasma processing apparatus. The process module used in step ST24 may be the process module used in step ST212 and step ST22, or may be another process module.
[0125] As described above, in the method MT2, the step ST212 and the step ST22 are performed simultaneously. That is, the generation of the chemical species that changes the precursor layer PC into the protective film PF and the generation of the chemical species that etches the region RE are performed simultaneously. Therefore, the method MT2 has a high throughput. In this manner, the step ST21 and the step ST22 may be performed at least partially simultaneously.
[0126] Hereinafter, reference will be made to FIG. 12, FIG. 13, FIG. 14(a), FIG. 14(b), FIG. 15(a), and FIG. 15(b). Each of FIG. 12 and FIG. 13 is a flow chart of an etching method according to yet another exemplary embodiment. Each of FIG. 14(a) and FIG. 14(b) is a partially enlarged cross-sectional view of an example substrate in a state after performing step ST31 of FIG. 12. FIG. 15(a) is a partially enlarged cross-sectional view of an example substrate in a state after performing step ST2 of FIG. 12 or step ST22 of FIG. 13. FIG. 15(b) is a partially enlarged cross-sectional view of an example substrate in a state after performing step ST32 of FIG. 12 or step ST42 of FIG. 13.
[0127] 12 (hereinafter referred to as "method MT3") differs from method MT in that it includes step ST31 and / or step ST32. One or more cycles out of all the cycles CY of method MT3 may include step ST31 and / or step ST32. Alternatively, all the cycles CY of method MT3 may include step ST31 and / or step ST32.
[0128] 13 (hereinafter referred to as "method MT4") differs from method MT2 in that it includes step ST42. In method MT4, one or more cycles among a plurality of cycles each including step ST21 and step ST22 may include step ST42. Alternatively, in method MT4, all of a plurality of cycles each including step ST21 and step ST22 may include step ST42.
[0129] Step ST31 of method MT3 is performed between step ST1 and step ST2. In step ST31, the protective film PF is partially removed. When step ST31 is applied to the substrate shown in FIG. 7(b), a portion of the protective film PF covering the mask MK is removed as shown in FIG. 14(a). When step ST31 is applied to the substrate shown in FIG. 9(b), a portion of the protective film PF covering the mask MK is removed as shown in FIG. 14(b). According to step ST31, the width of the opening of the mask MK is adjusted before the etching in step ST2. The process for partially removing the protective film PF in step ST31 is the same as the process in step ST4.
[0130] Step ST32 of the method MT3 is performed after step ST2 in the cycle CY. Step ST42 of the method MT4 is performed after step ST22 in the cycle including steps ST21 and ST22. After the etching in each of steps ST2 and ST22, the protective film PF may narrow the width of the opening in the mask MK near the upper end of the opening, as shown in FIG. 15(a). This is because the protective film PF is deformed by the etching in each of steps ST2 and ST22, or the constituent material of the protective film PF etched in each of steps ST2 and ST22 is redeposited on the substrate. In each of steps ST32 and ST42, the protective film PF is removed, as shown in FIG. 15(b). As a result, blocking of the opening of the mask MK by the protective film PF is suppressed. Note that the process for removing the protective film PF in each of steps ST32 and ST42 is the same as the process in step ST4 or step ST24. In each of steps ST32 and ST42, the protective film PF may be completely removed, or may be partially removed so as to prevent blocking of the openings of the mask MK.
[0131] Although various exemplary embodiments have been described above, the present invention is not limited to the above-described exemplary embodiments, and various additions, omissions, substitutions, and modifications may be made. In addition, elements in different embodiments can be combined to form other embodiments.
[0132] For example, the substrate processing apparatus used in performing each of the methods MT and MT2 may be any type of plasma processing apparatus. For example, the substrate processing apparatus used in performing each of the methods MT and MT2 may be a capacitively coupled plasma processing apparatus other than the plasma processing apparatus 1. The substrate processing apparatus used in performing each of the methods MT and MT2 may be an inductively coupled plasma processing apparatus, an ECR (electron cyclotron resonance) plasma processing apparatus, or a plasma processing apparatus that uses surface waves such as microwaves to generate plasma. In addition, when plasma is not used in the method MT, the substrate processing apparatus does not need to have a plasma generation unit.
[0133] The region RE may be formed of a metal, a metal oxide, or a chalcogenide. Such a region RE may be etched in steps STa, ST2, and ST22 by plasma formed from a gas containing, for example, a halogen-containing gas.
[0134] From the foregoing, it will be understood that various embodiments of the present disclosure have been described herein for purposes of illustration, and that various modifications may be made without departing from the scope and spirit of the present disclosure. Accordingly, the various embodiments disclosed herein are not intended to be limiting, with the true scope and spirit being indicated by the appended claims. [Explanation of symbols]
[0135] 1...plasma processing apparatus, PS...substrate processing system, W...substrate, RE...region, PF...protective film.
Claims
1. a) forming a protective film on a surface of a substrate, the substrate having a region to be etched and a mask provided on the region, the protective film being formed on and in contact with a sidewall surface defining an opening of the mask or the region, the protective film including tin atoms; b) etching said area; An etching method comprising:
2. 2. The etching method of claim 1, wherein a) is performed before the opening is formed in the region.
3. 2. The etching method of claim 1, wherein a) and b) occur at least partially simultaneously.
4. a) is a-1) forming a precursor layer on the sidewall surface by a first gas containing a tin-containing substance; a-2) generating a plasma from a second gas and forming the protective film from the precursor layer by a first chemical species from the plasma; Including, In the step b), during the step a-2), the region is etched with a second chemical species from the plasma that is different from the first chemical species. The etching method according to claim 3.
5. The a) is a-1) supplying a first gas to the substrate; a-2) supplying a second gas to the substrate; Including, At least one of the first gas and the second gas includes a tin-containing material. The etching method according to any one of claims 1 to 3.
6. In the step a-1), a precursor layer is formed on the surface of the substrate using the first gas; In the step a-2), the protective film is formed from the precursor layer by using the second gas. The etching method according to claim 5 .
7. the first gas comprises a tin-containing material; In the step a-2), the precursor layer is oxidized, nitrided, sulfurized, reduced, or halogenated using the second gas to form the protective film. The etching method according to claim 6.
8. In the step a-2), plasma of the second gas is generated; In the step b), during the step a-2), the region is etched by chemical species from the plasma of the second gas. The etching method according to claim 6 or 7.
9. one of the first gas and the second gas includes a tin-containing material; The other of the first gas and the second gas is H 2 O, H 2 O 2 , O 2 , O 3 , N 2 O 4 , nitrogen-containing inorganic compounds, sulfur-containing inorganic compounds, halogen compounds, carbon-containing materials, silicon-containing materials, or tin-containing materials; The etching method according to claim 5 .
10. one of the first gas and the second gas includes a tin-containing material; The other of the first gas and the second gas is N 2 and an oxygen-containing material, The etching method according to claim 5 .
11. 11. The etching method according to claim 4, wherein in the step a), a plurality of film formation cycles each including the steps a-1) and a-2) are sequentially performed.
12. 3. The etching method according to claim 1, wherein in the step a), the protective film is formed by chemical vapor deposition using a film-forming gas containing a tin-containing substance.
13. The deposition gas is N 2 , H 2 O, H 2 O 2 , O 2 , O 3 , N 2 O 4 13. The etching method of claim 12, further comprising at least one of an oxygen-containing material, an inorganic compound containing nitrogen, an inorganic compound containing sulfur, a halogen compound, a carbon-containing material, a silicon-containing material, and a rare gas.
14. c) further comprising the step of etching said region prior to a); The etching method according to any one of claims 1 to 13, wherein in step a), the protective film is formed on a sidewall surface that defines an opening formed in the region in step c).
15. 15. The etching method according to claim 14, wherein the thickness of the protective film varies depending on the position in the depth direction within the opening.
16. The etching method according to any one of claims 1 to 15, wherein a plurality of cycles each including a) and b) are carried out in sequence.
17. 7. The etching method according to claim 1, wherein the protective film contains at least one of metallic tin, an oxide of tin, a nitride of tin, a sulfide of tin, and a halide of tin.
18. The etching method according to any one of claims 1 to 17, wherein the mask is a hard mask, a photoresist, or a mask formed from a photoresist containing tin atoms.
19. The etching method according to any one of claims 1 to 18, further comprising the step of removing the protective film.
20. A chamber; a substrate support configured to support a substrate within the chamber; a gas supply configured to supply a gas into the chamber; A controller configured to control the gas supply unit; Equipped with The control unit is controlling the gas supply unit to supply a gas into the chamber to form a protective film on a sidewall surface that defines a region to be etched of the substrate supported by the substrate support or a sidewall surface that defines an opening of a mask on the region, the protective film including tin atoms; controlling the gas supply to supply gas into the chamber to etch a region in the substrate; Substrate processing equipment.
21. a film forming apparatus configured to form a protective film on a sidewall surface that defines a region of a substrate to be etched or an opening of a mask on the region, the protective film including tin atoms; a substrate processing apparatus configured to etch regions within the substrate; A substrate processing system comprising:
Citation Information
Patent Citations
Method of etching film and plasma processing apparatus
JP2019207911A
Eliminating stochastic yield effects in lithography
KR1020190142426A
Gas additives for sidewall passivation during high aspect ratio cryogenic etch
US20180286707A1
Metal-containing passivation for high aspect ratio etch
WO2020041213A1