Composite material, manufacturing method for composite material and terminal

A composite material with a surface-treated carbon particle-containing silver layer addresses copper diffusion issues, ensuring reliability and conductivity in sliding electrical contact parts, particularly in high-temperature environments, while maintaining cost-effectiveness.

JP7595042B2Active Publication Date: 2024-12-05DOWA METALTECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022078052
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-05-11
Publication Date
2024-12-05
Estimated Expiration
2042-05-11

AI Technical Summary

Technical Problem

Existing composite materials for sliding electrical contact parts in automotive and electronic devices suffer from insufficient reliability due to copper diffusion and oxidation, leading to increased resistance, especially in high-temperature environments, and conventional methods to enhance reliability increase manufacturing costs.

Method used

A composite material is developed with a silver layer containing carbon particles, where the carbon particles are surface-treated with specific benzoic acid compounds and electroplated, resulting in a composite film with predetermined convex portions that inhibit copper diffusion, enhancing reliability while maintaining thinness.

Benefits of technology

The composite material exhibits excellent reliability and conductivity, with minimal resistance changes even after exposure to high temperatures, and reduces manufacturing costs by preventing copper diffusion and oxidation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007595042000010
    Figure 0007595042000010
  • Figure 0007595042000001
    Figure 0007595042000001
  • Figure 0007595042000002
    Figure 0007595042000002
Patent Text Reader

Abstract

To provide a composite material that comprises a composite film, composed of a silver layer including carbon particles, formed on a base material and exhibits excellent reliability even when the composite film is thin, a method of producing the same, and a terminal for an electric contact using the composite material.SOLUTION: A composite material comprises a composite film, composed of a silver layer including carbon particles, formed on a base material, with the ratio of specified protrusions observed in an observation field being at least 12 area% when the composite film is observed with a laser microscope.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composite material in which a predetermined composite coating is formed on a base material, and a manufacturing method thereof, and in particular to a composite material used as a material for sliding electrical contact parts such as switches and connectors, and a manufacturing method thereof. [Background technology]

[0002] Conventionally, silver (Ag)-plated materials have been used as materials for sliding electrical contact parts such as switches and connectors to prevent oxidation of conductor materials such as copper (Cu) and copper alloys due to heating during the sliding process.

[0003] However, silver plating is soft and easily worn, and generally has a high coefficient of friction, which means that it is prone to peeling off due to sliding.To solve this problem, a method has been proposed in which a composite coating made of carbon particles such as graphite and carbon black, which have excellent wear resistance and lubricity, is dispersed in a silver matrix and formed on a conductor material by electroplating to improve wear resistance (see, for example, Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 3054628 [Patent Document 2] Patent No. 4806808 Summary of the Invention [Problem to be solved by the invention]

[0005] For example, in the automotive industry, as autonomous driving advances, sliding electrical contact parts such as in-vehicle switches and connectors are required to have excellent electrical conductivity as well as higher reliability than ever before (low deterioration of electrical conductivity even after exposure to high temperature environments). The same is true for sliding electrical contact parts used in other electronic devices.

[0006] Given such increasingly stringent requirements, the composite materials of Patent Documents 1 and 2 are insufficiently reliable.

[0007] In the composite materials disclosed in Patent Documents 1 and 2, in a composite coating (AgC coating) containing carbon particles, copper diffuses from the copper base material, which is the material, using the grain boundaries between the crystals that make up the silver matrix as a diffusion path. In particular, when the composite coating is thin, copper easily diffuses in the composite coating when heated, reaches the surface of the composite coating and is oxidized, causing an increase in resistance. In other words, reliability is insufficient. Reliability can be improved by thickening the composite coating and increasing the distance to the coating surface, but in that case, the manufacturing cost of the composite material will increase.

[0008] The present invention has been made under the above circumstances, and the problem to be solved by the present invention is to provide a composite material in which a composite coating containing carbon particles in a silver layer is formed on a base material, the composite coating being highly reliable even though it is thin, a manufacturing method thereof, and a terminal for electrical contacts using the composite material. [Means for solving the problem]

[0009] As a result of intensive research to solve the above problems, the inventors have found that when carbon particles are subjected to a specific surface treatment with a specific benzoic acid compound and then electroplated with a silver plating solution containing the carbon particles, the composite film has a specific number of protrusions. They also found that such a composite film has excellent reliability even though it is thin. Based on the above, the inventors have completed the present invention.

[0010] That is, the present invention is as follows.

[0011] [1] A composite material in which a composite coating made of a silver layer containing carbon particles is formed on a base material, When the composite coating is observed with a laser microscope, a pixel height is determined, which is a height difference between each pixel constituting an observation field of view and the lowest pixel in the observation field of view. When the pixel heights of the pixels are arranged in ascending order, the pixel height of the pixel at which the cumulative number ratio is 10% is defined as a reference height H0, and a pixel in the observation field of view whose pixel height is 1 μm or more higher than the reference height H0 is defined as a convex portion, the proportion of the convex portions in the observation field of view is 12 area % or more. Composite material.

[0012] [2] The composite material described in [1], wherein the material is composed of Cu or a Cu alloy.

[0013] [3] The composite material according to [1] or [2], wherein the silver crystallite size of the composite coating is 40 nm or less.

[0014] [4] The composite material according to any one of [1] to [3], wherein the protrusions account for 15 to 75% by area.

[0015] [5] The composite material according to any one of [1] to [4], wherein the proportion of carbon particles on the surface of the composite coating is 10 to 80 area %.

[0016] [6] The composite material according to any one of [1] to [5], wherein the thickness of the composite coating is 1.5 to 25 μm.

[0017] [7] The composite material according to any one of [1] to [6], wherein the surface of the composite coating has a Vickers hardness of 100 or more.

[0018] [8] The composite material according to any one of [1] to [7], wherein the composite coating has an arithmetic mean roughness Ra of 0.6 μm or more.

[0019] [9] The composite material according to any one of [1] to [8], wherein a base layer made of at least one material selected from the group consisting of Cu, Ni, Sn, and Ag is formed between the material and the composite coating.

[0020]

[10] A method for producing a composite material, comprising the steps of: forming a composite coating made of a silver layer containing carbon particles on a material by electroplating in a silver plating solution containing carbon particles, the carbon particles are surface-treated carbon particles that have been treated in an aqueous liquid with a compound A represented by the following general formula (1) for 30 minutes or more; [ka] (In formula (1), m is an integer of 1 to 5, Ra is a carboxyl group, Rb is an aldehyde group, a carboxyl group, an amino group, a hydroxyl group or a sulfonic acid group; Rc is hydrogen or an optional substituent; When m is 2 or more, a plurality of Rb's may be the same or different, When m is 3 or less, a plurality of Rc's may be the same or different. Ra and Rb may each independently be bonded to the benzene ring via a divalent group consisting of at least one group selected from the group consisting of -O- and -CH2-.

[0021]

[11] The method for producing a composite material according to

[10] , wherein the silver plating solution contains the surface-treated carbon particles and a compound B represented by the following general formula (2): [ka] In formula (2), p is an integer of 1 to 5, Rd is a carboxyl group; Re is an aldehyde group, a carboxyl group, an amino group, a hydroxyl group, or a sulfonic acid group; Rf is hydrogen or an optional substituent; When p is 2 or more, a plurality of Re may be the same or different, When p is 3 or less, a plurality of Rf's may be the same or different. Rd and Re may each independently be bonded to the benzene ring via a divalent group consisting of at least one group selected from the group consisting of -O- and -CH2-.

[0022]

[12] The method for producing a composite material according to

[10] or

[11] , wherein the material is composed of Cu or a Cu alloy.

[0023]

[13] The method for producing a composite material according to any one of

[10] to

[12] , wherein the treatment of the carbon particles with compound A is carried out by stirring an aqueous liquid containing the carbon particles and compound A for 30 minutes or more.

[0024]

[14] The method for producing a composite material according to any one of

[10] to

[13] , wherein the concentration of compound B in the silver plating solution is 2 to 250 g / L.

[15] The composite material according to any one of

[10] to

[14] , wherein the silver plating solution contains silver ions at a concentration of 5 to 150 g / L. Manufacturing method .

[0025]

[16] The method for producing a composite material according to any one of

[10] to

[15] , wherein the concentration of the surface-treated carbon particles in the silver plating solution is 10 to 150 g / L.

[0026]

[17] A terminal for electrical contacts, the terminal using the composite material according to any one of [1] to [9] as a constituent material. Effect of the Invention

[0027] According to the present invention, there is provided a composite material in which a composite coating containing carbon particles in a silver layer is formed on a base material, the composite material having excellent reliability even though the composite coating is thin, a manufacturing method thereof, and a terminal for electrical contacts using the composite material. [Brief description of the drawings]

[0028] [Figure 1]1 shows frequency distribution diagrams of pixel heights of pixels constituting images observed by a laser microscope, which were created in order to calculate the convexity area ratio in the examples, (a) being a frequency distribution diagram for Example 6, and (b) being a frequency distribution diagram for Comparative Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0029] Hereinafter, an embodiment of the present invention will be described. [Manufacturing method of composite materials] The embodiment of the method for producing a composite material of the present invention is a method for producing a composite material, which comprises forming a composite coating containing carbon particles in a silver layer on a base material by electroplating in a silver plating solution containing carbon particles that have been subjected to a predetermined surface treatment. Each component of the method for producing a composite material will be described below.

[0030] <<Material>> As the constituent material of the material on which the composite coating is formed, it is preferable to use a material that can be plated with silver and has the conductivity required for materials such as sliding electrical contact parts such as switches and connectors, and furthermore, from the viewpoint of cost, Cu (copper) and Cu alloys are preferable as the constituent material. As the Cu alloy, from the viewpoint of conductivity and strength, an alloy composed of Cu, at least one selected from the group consisting of Si (silicon), Fe (iron), Mg (magnesium), P (phosphorus), Ni (nickel), Sn (tin), Co (cobalt), Zn (zinc), Be (beryllium), Pb (lead), Te (tellurium), Ag (silver), Zr (zirconium), Cr (chromium), Al (aluminum) and Ti (titanium), and inevitable impurities is preferable. The amount of Cu in the Cu alloy is preferably 85% by mass or more, more preferably 92% by mass or more (the amount of Cu is preferably 99.95% by mass or less).

[0031] As described below, the material is preferably used for terminal applications (as a composite material with a composite coating formed thereon), but the material itself may have a shape for such applications, or the material may be flat (such as a flat plate) and then molded into the shape for application after becoming a composite material.

[0032] << Formation of base layer >> In the method for producing a composite material of the present invention, a base layer may be formed on the material, and the base layer may be electroplated as described below. The base layer is formed for the purpose of preventing copper of the material from diffusing to the plating surface and oxidizing, which may cause the composite material to lose its electrical conductivity, and for the purpose of improving the adhesion of the composite coating. The constituent metal of the base layer may be at least one metal or alloy selected from the group consisting of Cu, Ni, Sn, and Ag. The base layer may be a single layer of Cu, Ni, Sn, Ag, or an alloy thereof, or a layer of a combination of these (laminate structure), and the base layer may be formed on the entire surface layer of the material or on only a part of it, depending on the application of the composite material to be produced.

[0033] The method for forming the underlayer is not particularly limited, and the underlayer can be formed by electroplating using a plating solution containing ions of the above-mentioned constituent metals by a known method, or by laminating layers made of the metals that constitute the desired alloy layer in order and then reflowing (heat treating). From the viewpoint of wastewater treatment costs, it is preferable that the plating solution does not substantially contain cyanide compounds.

[0034] <<Agストライクめっき> > Before forming the composite coating on the material, it is preferable to form a very thin intermediate layer by Ag strike plating to improve the adhesion between the material and the composite coating. When a base layer is formed on the material, Ag strike plating is performed on the base layer (thereby improving the adhesion between the base layer and the composite coating). As a method for implementing Ag strike plating, any conventionally known method can be adopted without particular limitation as long as it does not impair the effects of the present invention. It is preferable that the plating solution used for Ag strike plating does not substantially contain cyanide compounds in terms of wastewater treatment costs.

[0035] <<Electroplating>> In the method for producing a composite material of the present invention, the above-described material is subjected to electroplating in a specific silver plating solution, after which a base layer and / or an intermediate layer is formed by Ag strike plating as necessary, to form a composite coating containing carbon particles in a silver layer on the material.

[0036] <Silver plating solution> The silver plating solution contains silver ions and carbon particles that have been subjected to a specific surface treatment, and preferably contains a specific compound B.

[0037] {Silver ions} The silver plating solution contains silver ions. From the viewpoints of the rate at which the composite film is formed and of preventing unevenness in the appearance of the composite film, the silver concentration in the silver plating solution is preferably 5 to 150 g / L, more preferably 10 to 120 g / L, and most preferably 20 to 100 g / L.

[0038] {Surface-treated carbon particles} The silver plating solution contains surface-treated carbon particles that have been subjected to a surface treatment described below. From the viewpoint of the abrasion resistance of a composite material obtained by forming a composite coating on a substrate using the silver plating solution, and because there is a limit to the amount of carbon particles that can be introduced into the composite coating, the amount of the surface-treated carbon particles in the silver plating solution is preferably 10 to 150 g / L, more preferably 15 to 120 g / L, and particularly preferably 30 to 100 g / L.

[0039] The surface-treated carbon particles, like conventionally used carbon particles, are rolled into the silver matrix when a composite coating (silver plating film) is formed on a material by electroplating, and thus enhance the wear resistance of the composite material. From the viewpoint of exerting such a function, the carbon particles constituting the surface-treated carbon particles are preferably graphite particles. The volume-based cumulative 50% particle size (D50) of the carbon particles measured by a laser diffraction / scattering type particle size distribution measuring device is preferably 0.5 to 15 μm, more preferably 1 to 10 μm, from the viewpoint of ease of roll-in into the silver matrix. Furthermore, the shape of the carbon particles is not particularly limited, such as substantially spherical, flaky, or amorphous, but is preferably flaky, since the wear resistance of the composite material can be enhanced by smoothing the surface of the composite coating.

[0040] (Oxidation treatment of carbon particles) In addition, it is preferable to oxidize the carbon particles (before the surface treatment) to remove lipophilic organic matter adsorbed on the surface of the carbon particles, thereby increasing the dispersibility of the carbon particles in the silver plating solution. Examples of such lipophilic organic matter include aliphatic hydrocarbons such as alkanes and alkenes, and aromatic hydrocarbons such as alkylbenzenes. As the oxidation treatment of the carbon particles, in addition to wet oxidation treatment, dry oxidation treatment using O2 gas or the like can be used, but wet oxidation treatment is preferable from the viewpoint of mass production, and carbon particles with a large surface area can be uniformly treated by wet oxidation treatment. As a method of wet oxidation treatment, a method of adding an appropriate amount of oxidizing agent after suspending carbon particles in water can be used. As the oxidizing agent, nitric acid, hydrogen peroxide, potassium permanganate, potassium persulfate (potassium peroxodisulfate), sodium perchlorate, or the like can be used. It is considered that the lipophilic organic matter attached to the carbon particles is oxidized by the added oxidizing agent to a form that is easily soluble in water, and is appropriately removed from the surface of the carbon particles. In addition, by filtering and washing the carbon particles with water after the wet oxidation treatment, the effect of removing lipophilic organic matter from the surface of the carbon particles can be further enhanced. Lipophilic organic matter such as aliphatic hydrocarbons and aromatic hydrocarbons can be removed from the surface of the carbon particles by the oxidation treatment of the carbon particles, and according to an analysis of the 300°C heated gas, the gas generated by heating the carbon particles after the oxidation treatment at 300°C contains almost no lipophilic aliphatic hydrocarbons such as alkanes and alkenes, or lipophilic aromatic hydrocarbons such as alkylbenzenes. Even if the carbon particles after the oxidation treatment contain a small amount of aliphatic hydrocarbons or aromatic hydrocarbons, the carbon particles can be uniformly dispersed in the silver plating solution used in the present invention. However, it is preferable that the carbon particles do not contain any hydrocarbons with a molecular weight of 160 or more, and that the 300°C heating generated gas intensity (purge and trap gas chromatograph mass spectrometry intensity) of the hydrocarbons with a molecular weight of less than 160 in the carbon particles is 5,000,000 or less.

[0041] (Surface treatment of carbon particles) In the present invention, the carbon particles that have been subjected to the above-mentioned oxidation treatment are preferably treated with a specific compound A in an aqueous liquid for 30 minutes or more. When electroplating is performed using a silver plating solution containing carbon particles that have been subjected to such treatment, a composite coating having a predetermined amount of protrusions (a plating layer made of a silver layer containing carbon particles) is formed. A composite material in which such a composite coating having protrusions is formed on a base material has excellent reliability.

[0042] The compound A is represented by the following general formula (1). [ka]

[0043] In formula (1), m is an integer of 1 to 5, Ra is a carboxyl group, Rb is an aldehyde group, a carboxyl group, an amino group, a hydroxyl group or a sulfonic acid group, Rc is hydrogen or an arbitrary substituent, and Ra and Rb may each independently be bonded to the benzene ring via at least one divalent group selected from the group consisting of -O- and -CH2-. Examples of the divalent group include -CH2-CH2-O-, -CH2-CH2-CH2-O-, (-CH2-CH2-O-) n (n is an integer of 2 or more).

[0044] In formula (1), when m is 2 or more, the multiple Rb's may be the same or different from each other, and when m is 3 or less, the multiple Rc's may be the same or different from each other. With respect to Rc, examples of the "optional substituent" include an alkyl group having 1 to 10 carbon atoms, an alkylaryl group, an acetyl group, a nitro group, a halogen group, and an alkoxyl group having 1 to 10 carbon atoms.

[0045] From the viewpoint of forming sufficient convex portions and obtaining a composite material with excellent reliability, Rb is preferably a carboxyl group, m is preferably 1, and Rc is preferably hydrogen.

[0046] Specifically, such treatment of carbon particles with compound A (hereinafter also simply referred to as surface treatment) can be carried out, for example, as follows.

[0047] The aqueous liquid containing the carbon particles and compound A is stirred for 30 minutes or more. It is believed that compound A is thereby adsorbed to the surface of the carbon particles. When electroplating is performed on a material with a silver plating solution containing such surface-treated carbon particles, a silver matrix is ​​formed, and the surface-treated carbon particles are caught in it to form a composite film, as in the case of electroplating with a silver plating solution containing carbon particles that are not surface-treated. During the formation of the composite film, surface-treated carbon particles that are caught in the silver matrix but are partially exposed are present on the surface, and silver (Ag) is precipitated (usually silver is precipitated on silver) at the exposed part of the particle where compound A is adsorbed, and it is believed that this grows to become a convex part. That is, it is believed that compound A is the starting point for the precipitation of silver. From the viewpoint of the reliability and manufacturing cost of the obtained composite material, the time for stirring the aqueous liquid containing carbon particles and compound A (surface treatment time) is preferably 45 minutes to 300 hours, more preferably 55 minutes to 250 hours. It should be noted that compound A is the same compound as compound B described later, and when carbon particles that have not been surface-treated as described in this section and compound B are added to a silver plating solution to prepare a plating solution containing carbon particles and the like, it can be considered that the carbon particles have been surface-treated with compound B for several seconds to several minutes. However, such a short-term treatment does not provide the effects of the present invention (see Comparative Example 2 described later).

[0048] The aqueous liquid used in the surface treatment may be pure water or a mixed solvent of water and an organic solvent. In the case of a mixed solvent, the content of water in the solvent is preferably 60% by mass or more, more preferably 80% by mass or more, from the viewpoint of the reliability of the composite material obtained. In addition, taking into consideration the environmental load, pure water is particularly preferable as the aqueous liquid.

[0049] From the viewpoint of efficiency of the surface treatment, the amount of carbon particles used per 100 parts by mass of the aqueous liquid is preferably 2 to 15 parts by mass, and more preferably 3 to 10 parts by mass.

[0050] The amount of compound A used per 100 parts by mass of carbon particles is preferably 0.8 to 10 parts by mass, and more preferably 1.5 to 5 parts by mass, from the viewpoints of the reliability of the resulting composite material and production costs.

[0051] The temperature of the aqueous liquid during the surface treatment is preferably from 10 to 50°C, and more preferably from 20 to 35°C, from the viewpoint of surface treatment efficiency.

[0052] Stirring during the surface treatment can be performed with a stirrer or stirring blade, and the rotation speed is preferably 250 to 600 rpm, more preferably 300 to 500 rpm, from the viewpoints of the efficiency of the surface treatment and the reliability of the resulting composite material.

[0053] After the surface treatment with compound A has been carried out as described above, the aqueous liquid containing the surface-treated carbon particles may be filtered, and the filtered product may be washed with water to recover the surface-treated carbon particles.

[0054] {Compound B} Next, the silver plating solution preferably contains compound B. Compound B is represented by the following general formula (2).

[0055] [ka]

[0056] In formula (2), p is an integer of 1 to 5, Rd is a carboxyl group, Re is an aldehyde group, a carboxyl group, an amino group, a hydroxyl group or a sulfonic acid group, Rf is hydrogen or an arbitrary substituent, and Rd and Re may each independently be bonded to the benzene ring via a divalent group consisting of at least one selected from the group consisting of -O- and -CH2-. Examples of the divalent group include -CH2-CH2-O-, -CH2-CH2-CH2-O-, (-CH2-CH2-O-) q Examples include ( q is an integer greater than or equal to 2).

[0057] It is believed that compound B adsorbs to the surface of the deposited silver and inhibits the growth of silver crystals, thereby reducing the crystallite size of silver in the composite coating formed by electroplating, resulting in a composite material with excellent hardness and therefore excellent wear resistance.

[0058] In the above general formula (2), when p is 2 or more, the multiple Re present may be the same or different, and when p is 3 or less, the multiple Rf present may be the same or different, and examples of the "optional substituent" for Rf include an alkyl group having 1 to 10 carbon atoms, an alkylaryl group, an acetyl group, a nitro group, a halogen group, and an alkoxyl group having 1 to 10 carbon atoms.

[0059] The concentration of compound B in the silver plating solution is preferably 2 to 250 g / L, and more preferably 3 to 200 g / L, from the viewpoints of suppressing unevenness in the appearance of the composite coating and appropriately controlling the silver crystallite size in the composite coating that is formed.

[0060] {Complexing agent} The silver plating solution used in the present invention preferably contains a complexing agent. The complexing agent complexes the silver ions in the silver plating solution, enhancing the stability of the ions. This action increases the solubility of silver in the solvent that constitutes the plating solution.

[0061] Complexing agents having the above-mentioned functions can be widely used, but from the viewpoint of the stability of the complex formed, compounds having a sulfonic acid group are preferred. Examples of compounds having a sulfonic acid group include alkylsulfonic acids having 1 to 12 carbon atoms, alkanolsulfonic acids having 1 to 12 carbon atoms, and hydroxyarylsulfonic acids. Specific examples of these compounds include methanesulfonic acid, 2-propanolsulfonic acid, and phenolsulfonic acid.

[0062] From the viewpoint of stabilizing silver ions, the amount of the complexing agent in the silver plating solution is preferably 30 to 200 g / L, and more preferably 50 to 120 g / L.

[0063] {Other additives} As other additives, for example, the silver plating solution used in the present invention may contain brighteners, hardeners, and conductive salts. The hardeners include carbon sulfide compounds (e.g., carbon disulfide), inorganic sulfur compounds (e.g., sodium thiosulfate), organic compounds (sulfonates), selenium compounds, tellurium compounds, metals in Group 4B or 5B of the periodic table, and the like. The conductive salts include potassium hydroxide, and the like.

[0064] {solvent} The solvent constituting the silver plating solution is mainly water. Water is preferred because of its solubility in (complexed) silver ions and other components contained in the plating solution, and because water has a small environmental impact. A mixed solvent of water and alcohol may also be used as the solvent.

[0065] {Cyanide compounds} The main components of the silver plating solution used in the present invention are as described above, and this silver plating solution typically does not substantially contain cyanide compounds (specifically, the content of cyanide compounds in the silver plating solution is 1 mg / L or less). A cyanide compound is a compound containing a cyano group (-CN), and the amount of cyanide compounds can be quantified according to JIS K 0102:2019. Cyanide compounds are subject to the Water Pollution Control Act (Effluent Standards) and the PRTR (Pollutant Release and Transfer Register) system, and the wastewater treatment costs are high. As described above, the silver plating solution used in the present invention typically does not substantially contain cyanide compounds, and therefore the wastewater treatment costs are low.

[0066] <Electroplating conditions> Next, various conditions for electroplating using the silver plating solution described above will be described. For example, by electroplating described below, metallic silver is deposited on a material, and at the same time, surface-treated carbon particles are caught in the silver matrix to form a composite film. It is considered that silver is deposited and grows at the compound A portion of the surface-treated carbon particles exposed from the silver matrix being formed, forming a predetermined amount of convex portions. In addition, when the silver plating solution contains compound B, the function of compound B keeps the silver crystallite size in the composite film small.

[0067] (Cathode and Anode) The material to be electroplated is the cathode. The anode is what dissolves to provide silver ions, e.g. a silver electrode plate.

[0068] (current density) The cathode and anode are immersed in a silver plating solution (plating bath) and a current is passed through them to perform silver plating. The current density here is set to 0.5 to 10 A / dm from the viewpoints of the speed at which the composite film is formed and the suppression of unevenness in the appearance of the composite film. 2 is preferable, and 1 to 8 A / dm 2 More preferably, 1 to 5 A / dm 2 is more preferred.

[0069] (Temperature, stirring, plating time, plating area) The temperature (plating temperature) of the plating bath (silver plating solution) during electroplating is preferably 15 to 50°C, more preferably 20 to 45°C, from the viewpoint of plating production efficiency and preventing excessive evaporation of the solution. The stirring speed of the plating bath by a stirrer or stirring blade is preferably 200 to 550 rpm, more preferably 350 to 500 rpm, from the viewpoint of uniform plating. The silver plating time (time to apply electric current) can be appropriately adjusted depending on the thickness of the desired composite coating, but is typically in the range of 25 to 1800 seconds. The area to be plated may be the entire surface layer of the material or a part of the surface layer of the material, depending on the application of the composite material to be manufactured.

[0070] <<Partial removal of carbon particles from the surface of the composite coating>> A composite film is formed on a material by the electroplating described above. On the surface of this composite film, there are carbon particles that are caught (embedded) in the silver matrix and are difficult to fall off, and carbon particles that are attached to the surface rather than caught and are easy to fall off. The latter may contaminate equipment during bending processing of the composite material. Therefore, it is preferable to remove such carbon particles by cleaning. One cleaning method is a treatment of ultrasonically cleaning the surface of the composite film. The ultrasonic cleaning is preferably performed at 20 to 100 kHz for 1 to 300 seconds. Another cleaning method is electrolytic cleaning. In this case, the electrolytic cleaning is performed at 1 to 30 A / dm 2 It is preferable that the heating is performed at 10 to 300 seconds.

[0071] [Composite material] Hereinafter, an embodiment of the composite material of the present invention will be described. The composite material is a composite material in which a composite coating made of a silver layer containing carbon particles is formed on a base material, and when the surface of the composite coating is observed with a laser microscope, the proportion of predetermined convex parts in the observation field is 12 area % or more. This composite material can be manufactured, for example, by an embodiment of the manufacturing method for the composite material of the present invention. Hereinafter, each component of this composite material will be described.

[0072] <<Material>> The material is the same as the material described above for the manufacturing method of the composite material of the present invention. That is, Cu (copper) and Cu alloys are suitable as constituent materials of the material, and as the Cu alloy, from the viewpoint of electrical conductivity and strength, an alloy composed of Cu, Si (silicon), Fe (iron), Mg (magnesium), P (phosphorus), Ni (nickel), Sn (tin), Co (cobalt), Zn (zinc), and at least one selected from the group consisting of Be (beryllium), Pb (lead), Te (tellurium), Ag (silver), Zr (zirconium), Cr (chromium), Al (aluminum) and Ti (titanium), and inevitable impurities is preferable.

[0073] <<Composite coating>> The composite coating formed on the base material is composed of a silver layer containing carbon particles. In this silver layer, the carbon particles are (preferably substantially uniformly) dispersed in a matrix made of silver. If Ag strike plating is performed before forming the composite coating, an intermediate layer formed by this strike plating exists between the base material (or the undercoat layer described later) and the composite coating, but in many cases this is very thin and cannot be distinguished from the composite coating. The composite coating may be formed on the entire surface layer of the base material, or on only a part of the surface layer.

[0074] <Carbon particles> The carbon particles are the same as the surface-treated carbon particles described above in the manufacturing method for the composite material of the present invention. That is, the carbon particles are preferably graphite particles, and the shape is not particularly limited, such as substantially spherical, flaky, or amorphous, but is preferably flaky because the wear resistance of the composite material can be improved by smoothing the surface of the composite coating. When the composite material of the present invention is described in the manufacturing method for the composite material of the present invention, it is considered that compound A is adsorbed on the surface of the carbon particles.

[0075] From the viewpoint of the abrasion resistance of the composite material, the average primary particle diameter of the carbon particles is preferably 0.5 to 15 μm, and more preferably 1 to 10 μm. The average primary particle diameter is the average value of the major axis of the particles, and the major axis is the length of the longest line that can be drawn within the particle in an image (plane) of the carbon particles in the composite coating of the composite material observed at an appropriate observation magnification. The major axis is determined for 50 or more particles.

[0076] <Specified convexity and arithmetic mean roughness Ra> The composite coating in the embodiment of the composite material of the present invention has a predetermined convex portion, which exhibits excellent reliability. In this specification, the convex portion is defined as follows.

[0077] The composite coating of the composite material is observed with a laser microscope at a magnification of 1000 times, and the height of each pixel (pixel height) in the obtained image of the observation field (143 μm × 107.2 μm, composed of 1024 × 768 pixels) is obtained. This pixel height is obtained as the height difference with respect to the lowest pixel in the observation field (height X of any pixel - height Y of the lowest pixel). The pixel height of the pixel (10th percentile value) at which the cumulative number ratio when the pixel heights of each pixel obtained are arranged in ascending order is 10% is set as the reference height H0. The total number of pixels in the observation field is 786432, and the pixel height of the pixel at which the cumulative number ratio exceeds 10% for the first time is set as the reference height H0 (10th percentile value). The reference height H0 is, for example, 0.1 to 10 μm, and preferably 0.3 to 5 μm.

[0078] A portion (pixel) in the observation field of view where the pixel height is 1 μm or more higher than H0 is defined as a convex portion. The composite film can be formed by a technique such as electroplating, and the above 10th percentile value can be approximated to the height of a portion of the composite film (plated film) where a flat film is formed, i.e., the flat portion. In the present invention, a portion that is a predetermined height (1 μm or more) higher than this flat portion is defined as the convex portion.

[0079] As explained in the section [Problems to be Solved by the Invention], when a composite material is heated, copper diffuses from the material toward the composite coating, reaches the surface of the coating and is oxidized, increasing the resistance of the composite material. On the other hand, in the present invention, although the mechanism is unclear, it is believed that copper is less likely to diffuse into the protruding parts that make up the composite coating. And, as described above, the protruding parts have a height of 1 μm or more from the reference height H0, which is a certain level or more.

[0080] In the embodiment of the composite material of the present invention, when the composite coating is observed with the laser microscope, it is considered that copper is unlikely to diffuse within the observation field as described above, and the proportion of tall convex parts is 12 area % or more, thereby achieving excellent reliability. The above-mentioned area proportion (convex part area ratio) can be calculated as the proportion of pixels having a pixel height 1 μm or more higher than H0 to the total number of pixels among all pixels constituting the observation field. From the viewpoint of the reliability of the composite material and the difficulty in manufacturing to make the proportion of convex parts very large, the convex part area ratio is preferably 15 to 75 area %, and further from the viewpoint of electrical conductivity, the proportion is particularly preferably 18 to 70%.

[0081] There is no particular upper limit on the height of the convex part, but the pixel height of the highest pixel among the pixels constituting the above observation field (height of the highest pixel x T The height Y of the lowest pixel is, for example, 1.8 to 25 μm, and preferably 2.4 to 20 μm.

[0082] The arithmetic mean roughness Ra of the surface of the composite coating of the composite material of the present invention having such protrusions exhibits a certain degree or more of value, specifically, for example, 0.6 μm or more (usually 7.0 μm or less).

[0083] <Crystallite size and Vickers hardness> The crystallite size of silver in the composite coating in the embodiment of the composite material of the present invention is preferably small, 40 nm or less. With such a small crystallite size, the hardness of the composite coating is high due to the Hall-Petch relationship (generally, the smaller the crystal grains of a metal material, the stronger it is), and the high hardness makes the composite coating less likely to be scraped, and the wear resistance of the composite material is high. From the viewpoint of increasing the hardness and improving the wear resistance, and because it is difficult to make the crystallite size very fine in manufacturing, the crystallite size is preferably 2 to 35 nm, more preferably 2 to 30 nm.

[0084] In the present invention, the silver crystallite size is determined by averaging (adding and dividing by 2) the crystallite sizes of the silver (111) and (222) faces in order to reduce bias due to the crystal plane. A more detailed method for measuring the crystallite size will be described in the Examples.

[0085] As described above, the composite coating of the preferred embodiment has a small crystallite size and therefore a high hardness, specifically, its Vickers hardness Hv is preferably 100 or more, and more preferably 120 to 230. Details of the method for measuring the Vickers hardness Hv will be described in the Examples.

[0086] <Carbon content and area ratio> The composite coating in the embodiment of the composite material of the present invention contains carbon particles as described above, and the carbon content in the composite coating is preferably 1 to 50 mass %, more preferably 1.5 to 40 mass %, and even more preferably 2 to 35 mass %, from the viewpoints of the wear resistance and electrical conductivity of the composite material.

[0087] The ratio (area ratio) of the carbon particles on the surface of the composite coating containing the carbon particles is an index of wear resistance, and is preferably 10 to 80 area %, more preferably 12 to 50 area %, from the viewpoint of the balance between wear resistance and electrical conductivity. As explained in the explanation of the manufacturing method of the composite material of the present invention, there are cases where carbon particles that are merely attached and easily fall off are present on the surface of the composite coating. In this case, the area ratio of carbon on the surface of the composite coating is obtained after performing ultrasonic cleaning treatment similar to that explained in the section <<Partial removal treatment of carbon particles on the surface of the composite coating>>. Details of the method for measuring the area ratio will be explained in the examples.

[0088] <Total silver and carbon content> Regarding elemental composition, the composite coating in the composite embodiment of the present invention typically consists essentially of silver and carbon.

[0089] <Thickness of composite film> The thickness of the composite coating is not particularly limited, but it is preferable that the composite coating has a minimum thickness in terms of wear resistance, reliability, and conductivity. If the thickness is too large, the effect of the composite coating is saturated and the raw material cost increases. From the above viewpoints, the thickness of the composite coating is preferably 0.5 to 45 μm, more preferably 1 to 35 μm, and even more preferably 1.5 to 25 μm. Since the composite coating of the present invention has a predetermined amount of protrusions, the composite coating exhibits excellent reliability even if the thickness of the composite coating is thin. The thickness of the composite coating is measured with a fluorescent X-ray thickness meter, and the details of the measurement method will be described in the examples.

[0090] <<Underlayer>> A base layer may be formed between the material and the composite coating for various purposes. The constituent metal of the base layer may be at least one metal or alloy selected from the group consisting of Cu, Ni, Sn, and Ag. For example, in order to prevent copper in the material from diffusing to the surface of the composite coating and deteriorating the electrical conductivity, it is preferable to form a base layer made of Ni. In order to prevent zinc in the material from diffusing to the surface of the composite coating when the material is a copper alloy containing zinc such as brass, it is preferable to form a base layer made of Cu. In order to improve the adhesion of the composite coating to the material, it is preferable to form a base layer made of Ag. The thickness of the base layer is not particularly limited, but from the viewpoint of its function and cost, it is preferably 0.1 to 2 μm, and more preferably 0.2 to 1.5 μm. In addition, materials that are Sn-plated or reflow-plated with Cu or Ni base (a laminated structure of Cu base, Ni base, and Sn base from the material side) are often used for the terminals of electric and electronic components, and a base layer with such a laminated structure may be formed in the present invention. Therefore, in the present invention, the base of the composite coating may be a single layer made of Cu, Ni, Sn, Ag or an alloy of these, or a layer combining these (laminate structure). Also, different layers may be formed depending on the location, for example, a composite coating as defined in the present invention may be formed on the electrical contact portion of the material (a base layer may or may not be formed) and a reflow Sn-plated base layer may be formed on the wire crimping portion (no composite coating is formed).

[0091] <<Reliability of composite materials>> The composite material according to the embodiment of the present invention has a composite coating having a predetermined number of the above-mentioned protrusions, and is therefore highly reliable. It also has excellent electrical conductivity equivalent to that of the prior art.

[0092] Specifically, the contact resistance measured by the method (four-terminal method) in the examples described later is preferably 0.6 to 3.0 mΩ at a load of 0.5 N, 0.4 to 2.5 mΩ at a load of 1.0 N, and 0.3 to 2.0 mΩ at a load of 2.0 N, and more preferably 0.6 to 2.8 mΩ at a load of 0.5 N, 0.4 to 2.3 mΩ at a load of 1.0 N, and 0.3 to 1.8 mΩ at a load of 2.0 N.

[0093] The contact resistance of the composite material measured by a method (four-terminal method) described in the Examples below after storing the composite material in an air atmosphere at 200°C for 120 hours is preferably 0.6 to 3.0 mΩ at a load of 0.5 N, 0.5 to 2.5 mΩ at a load of 1.0 N, and 0.4 to 2.0 mΩ at a load of 2.0 N; More preferably, the resistance is 0.6 to 2.8 mΩ at a load of 0.5N, 0.5 to 2.3 mΩ at a load of 1.0N, and 0.4 to 1.8 mΩ at a load of 2.0N.

[0094] From the viewpoint of reliability, the ratio of the contact resistance before and after storing the composite material in an air atmosphere at 200°C for 120 hours (contact resistance after heated storage / contact resistance before heated storage) is preferably 0.6 to 2.0, more preferably 0.7 to 1.5, and even more preferably 0.75 to 1.4 at any of 0.5 N, 1.0 N, and 2.0 N.

[0095] As described above, the composite material according to the embodiment of the present invention has excellent reliability, with almost no change in contact resistance before and after heating. Furthermore, since it shows sufficiently low resistance even at a low load of 1.0 N, for example, in mating parts such as terminals of connectors (terminals can be manufactured, for example, by bending the composite material according to the present invention), the terminals are designed to be subjected to a certain stress (a force greater than the above 1.0 N, etc.), but even if the stress applied to the terminals decreases to about 1.0 N due to the phenomenon of stress relaxation after long-term use, sufficient conductivity can be ensured.

[0096] From the viewpoints of electrical conductivity as well as reliability, it is preferable that the convex area ratio is 30 area % or more and the thickness of the composite coating is 2.8 μm or more, and it is more preferable that the convex area ratio is 35 to 62 area % and the thickness of the composite coating is 3.0 μm or more.

[0097] [Terminal] The composite material according to the embodiment of the present invention has excellent reliability, and the preferred composite material has excellent hardness (and therefore excellent wear resistance), and is therefore suitable as a constituent material for terminals for electrical contacts, particularly terminals in electrical contact parts such as switches and connectors that undergo sliding during use. EXAMPLES

[0098] Hereinafter, examples of the composite material and the manufacturing method thereof according to the present invention will be described in detail.

[0099] [Example 1] <Preparation of carbon particles: oxidation treatment> 80 g of scaly graphite particles (PAG-3000 manufactured by Nippon Graphite Industries Co., Ltd.) having an average particle size of 4.8 μm was added to 1.4 L of pure water, and the mixture was heated to 50° C. while being stirred. The average particle size is a particle size at which the cumulative value based on volume is 50%, measured using a laser diffraction / scattering particle size distribution measuring device (MT3300 (LOW-WET MT3000II Mode) manufactured by Microtrack Bell Co., Ltd.). Next, 0.6 L of a 0.1 mol / L aqueous potassium peroxodisulfate solution was gradually dropped into the mixture as an oxidizing agent, and the mixture was stirred for 2 hours to perform an oxidation treatment, after which the mixture was filtered through a filter paper, and the obtained solid matter was washed with water.

[0100] The carbon particles before and after this oxidation treatment were analyzed using a purge-and-trap gas chromatograph mass spectrometer (a combination of a JHS-100 thermal desorption device manufactured by Japan Analytical Industry Co., Ltd. and a GCMS QP-5050A gas chromatograph mass spectrometer manufactured by Shimadzu Corporation) to analyze the gas generated by heating at 300°C. It was found that the oxidation treatment described above removed lipophilic aliphatic hydrocarbons (such as nonane, decane, and 3-methyl-2-heptene) and lipophilic aromatic hydrocarbons (such as xylene) that had adhered to the carbon particles.

[0101] <Preparation of carbon particles and surface treatment> After adding 50 g of the carbon particles after the oxidation treatment to 1 L of pure water, 1 g of 2,4-dihydroxybenzoic acid (compound A) was added and the surface treatment was performed on the carbon particles by stirring at 400 rpm for 1 hour with a stirrer at a liquid temperature of 25° C. Then, the carbon particles were filtered through filter paper, and the obtained solid matter (carbon particles) was washed with water.

[0102] <Agストライクめっき> A plate material made of a Cu-Ni-Sn-P alloy (copper alloy plate material containing 1.0 mass% Ni, 0.9 mass% Sn, 0.05 mass% P, with the remainder being Cu and unavoidable impurities) (NB-109EH manufactured by DOWA Metaltech Co., Ltd.) measuring 5.0 cm in length, 5.0 cm in width, and 0.2 mm in thickness was prepared. Using this plate material as the cathode and an iridium oxide mesh electrode plate (a titanium mesh material coated with iridium oxide) as the anode, plating was performed in a sulfonic acid-based silver strike plating solution containing methanesulfonic acid as a complexing agent (Dynesilver GPE-ST manufactured by Daiwa Kasei Co., Ltd., substantially free of cyanide compounds, silver concentration 3 g / L, methanesulfonic acid concentration 42 g / L) at a liquid temperature of 25°C and a current density of 5 A / dm 2 The material was electroplated (silver strike plating) for 60 seconds. The silver strike plating was performed on the entire surface of the material.

[0103] <AgCめっき> The carbon particles (graphite particles) that had been subjected to the above-mentioned oxidation treatment and surface treatment were added to a sulfonic acid-based silver plating solution containing methanesulfonic acid as a complexing agent, with a silver concentration of 30 g / L and a methanesulfonic acid concentration of 60 g / L (Dynesilver GPE-HB (containing compound B corresponding to general formula (2) at a concentration of 4.2 g / L, and the solvent is mainly water) manufactured by Daiwa Kasei Co., Ltd.) to prepare a carbon particle-containing sulfonic acid-based silver plating solution containing surface-treated carbon particles at a concentration of 50 g / L, silver at a concentration of 30 g / L, and methanesulfonic acid at a concentration of 60 g / L. This silver plating solution does not substantially contain Sb or cyanide compounds.

[0104] Next, the above Ag strike-plated material was used as the cathode and the silver electrode plate was used as the anode, and the plating was performed in the above carbon particle-containing sulfonic acid-based silver plating solution at a temperature of 25°C and a current density of 3 A / dm while stirring at 400 rpm with a stirrer. 2 The composite film (AgC plating film) containing carbon particles in the silver layer was formed on the base material. The composite film was formed on the entire surface of the base material.

[0105] <Ultrasonic cleaning treatment> The surface of the composite coating of the obtained composite material was subjected to ultrasonic cleaning treatment at 28 kHz for 4 minutes using an ultrasonic cleaner (VS-100III manufactured by AS ONE, output 100 W, tank dimensions: length 140 mm x width 240 mm x depth 100 mm) with water as the liquid medium.

[0106] The manufacturing conditions of the above composite materials are summarized in Tables 1 and 2 below, along with the manufacturing conditions of Examples 2 to 7 and Comparative Examples 1 to 5, which will be described later.

[0107] The obtained composite material was evaluated as follows.

[0108] <Silver crystallite size of composite film> The surface of the composite coating was subjected to X-ray diffraction measurement (Cu Kα ray tube, tube voltage: 30 kV, tube current: 10 mA, step width: 0.02°, scanning range: 2θ = 10° to 154°, scanning speed: 10° / min, measurement time: about 15 min, (111) plane peak: 2θ = 37.9 to 38.7°, (222) plane peak: 2θ = 79 to 82.2°) using an X-ray diffraction apparatus (Rigaku Corporation, RINT-2000) in accordance with JIS H 7805:2005. From the peaks of the detected silver (111) and (222) planes, the full width at half maximum (FWHM: Full Width at Half Maximum) was obtained using X-ray analysis software (Rigaku Corporation, PDXL), and the crystallite size of each silver crystal plane was calculated using the Scherrer formula. In order to reduce bias due to the crystal plane, the average crystallite size of the (111) and (222) planes of silver was used as the silver crystallite size. The crystallite size was 26.3 nm.

[0109] The Scherrer formula is as follows: D = K λ / (β cosθ) D: Crystallite size K: Scherrer constant, set to 0.9 λ: wavelength of X-rays, 1.54 Å for CuKα rays β: Full width at half maximum (FWHM) (rad) θ: Measurement angle (deg)

[0110] <Carbon area ratio on composite coating surface> The composite coating surface was observed using a tabletop microscope (Hitachi High-Tech TM4000 Plus) at an accelerating voltage of 5 kV and magnified 1000 times. The composite coating surface was binarized with GIMP 2.10.10 (image analysis software) to calculate the carbon area ratio. Specifically, the highest brightness of all pixels was set to 255 and the lowest brightness was set to 0, and the gradation was binarized so that pixels with a brightness of 127 or less were black and pixels with a brightness of more than 127 were white. The silver part (white part) and the carbon particle part (black part) were separated, and the ratio Y / X of the number of pixels Y of the carbon particle part to the number of pixels X of the entire image was calculated as the carbon area ratio (%) of the surface. The carbon area ratio was 26.2%.

[0111] <Vickers hardness Hv of composite coating surface> The Vickers hardness Hv of the composite coating surface was measured using a microhardness tester (HM221 manufactured by Mitutoyo Corporation) by applying a load of 0.01 N to the flat part of the composite material for 15 seconds, according to JIS Z 2244, and the average value of three measurements was used. The resulting Vickers hardness Hv was 174.

[0112] <Thickness of composite film> The thickness of this composite coating (a circular area with a diameter of 0.2 mm at the center of a surface of 5.0 cm long and 5.0 cm wide) was measured with a fluorescent X-ray thickness gauge (FT9450 manufactured by Hitachi High-Tech Science Corporation) and was found to be 3.3 μm. Note that it is difficult to detect C atoms (of carbon particles) with a fluorescent X-ray thickness gauge, so the thickness was determined by detecting Ag atoms, but in the present invention, the thickness determined in this manner is regarded as the thickness of the composite coating.

[0113] <Arithmetic mean roughness of composite coating> For the surface of the above-mentioned composite coating, images of the composite coating surface were taken at 1000x magnification using a laser microscope (VKX-110, manufactured by Keyence Corporation). The arithmetic mean roughness Ra, a parameter that represents the surface roughness (over the entire observation surface of the composite coating), was calculated using an analysis application (VK-HIXA version 3.8.0.0, manufactured by Keyence Corporation) based on JIS B 0601 (2001), and was found to be 2.6 μm.

[0114] <Reference height H0 and maximum height> In order to obtain the arithmetic mean roughness Ra, the observation field (143 μm × 107.2 μm, composed of 1024 × 768 pixels) obtained by observation with a laser microscope was subjected to "surface tilt correction (automatic)" of an analysis application (VK-HIXA version 3.8.0.0 manufactured by Keyence Corporation) for an image including height data of each pixel constituting the observation field, and a frequency distribution diagram was created for the height (pixel height) of each pixel constituting the image of the observation field using the application. The pixel height of each pixel was calculated by setting the pixel height of the lowest pixel in the observation field to 0 and calculating the height (height difference) relative to this. The statistical software Rstudio (Version 1.4.1103 free software) was used to calculate the 10th percentile value of the frequency distribution diagram created. This is the reference height H0 in the present invention, which was specifically 1.6 μm. In addition, the height (maximum height) of the highest pixel was 17.1 μm.

[0115] <Protruding area ratio> In the image of the above observation field where the reference height H0 was calculated, the ratio of the number of pixels with a pixel height of (H0+1) μm or more to the total number of pixels constituting the observation field, that is, the area ratio of the convex parts, was calculated. As a result, the area ratio of the convex parts was 67.8%.

[0116] <Reliability evaluation> (Initial resistance value) A material measuring 2.0 cm wide x 3.0 cm long was cut out from the same Cu-Ni-Sn-P alloy plate material used in Example 1, and Ag strike plating and AgC plating were carried out under the same conditions as in Example 1 to obtain a composite material (flat test piece).

[0117] The same Cu-Ni-Sn-P alloy plate material as used in Example 1 was cut to a length of 4.0 cm and a width of 1.0 cm, and an indent (extrusion into a hemispherical shape) with an inner diameter of 1.0 mm was applied to the center. The surface of the protruding convex part of the indent (the surface to be pressed against the flat test piece described below) was plated (AgSb plated) in the same manner as in Comparative Example 4 described later to obtain an indent test piece.

[0118] This flat test piece was placed in a sliding wear testing machine (CRS-G2050-DWA, manufactured by Yamazaki Seiki Laboratory Co., Ltd.), and the contact resistance was measured using the four-terminal method when the convex part of the indented test piece was pressed against it with a constant load (0.5, 1.0, 2.0 N). The results were 1.5 mΩ at 0.5 N, 1.3 mΩ at 1.0 N, and 1.0 mΩ at 2.0 N.

[0119] (Evaluation of resistance value after heating storage) The flat test pieces were stored in air at 200°C for 120 hours (test pieces with indents were not stored under heat). After that, the contact resistance was measured by the four-terminal method in the same manner as above, and the results were 1.8 mΩ at 0.5 N, 1.2 mΩ at 1.0 N, and 0.9 mΩ at 2.0 N.

[0120] The above evaluation results are summarized in Tables 3 and 4 below, together with the evaluation results of Examples 2 to 7 and Comparative Examples 1 to 5, which will be described later.

[0121] [Example 2] A composite material was prepared in the same manner as in Example 1, except that the plating time for AgC plating was 120 seconds.

[0122] The thickness, Vickers hardness Hv, convex area ratio, maximum height, arithmetic mean roughness Ra, carbon area ratio of the composite coating surface, and reliability of the obtained composite material were evaluated in the same manner as in Example 1. The reference height H0 was 2.9 μm.

[0123] [Example 3] A composite material was prepared in the same manner as in Example 1, except that the plating time for AgC plating was 300 seconds.

[0124] The thickness, Vickers hardness Hv, convex area ratio, maximum height, arithmetic mean roughness Ra, carbon area ratio of the composite coating surface, and reliability of the obtained composite material were evaluated in the same manner as in Example 1. The reference height H0 was 2.5 μm.

[0125] [Example 4] A composite material was prepared in the same manner as in Example 1, except that the plating time for AgC plating was 600 seconds.

[0126] The thickness, Vickers hardness Hv, convex area ratio, maximum height, arithmetic mean roughness Ra, carbon area ratio of the composite coating surface, and reliability of the obtained composite material were evaluated in the same manner as in Example 1. The reference height H0 was 0.3 μm.

[0127] [Example 5] A composite material was prepared in the same manner as in Example 1, except that the plating time for AgC plating was 1200 seconds.

[0128] The thickness, Vickers hardness Hv, convex area ratio, maximum height, arithmetic mean roughness Ra, carbon area ratio of the composite coating surface, and reliability of the obtained composite material were evaluated in the same manner as in Example 1. The reference height H0 was 1.3 μm.

[0129] [Example 6] A composite material was prepared in the same manner as in Example 1, except that the time for surface treatment of the carbon particles was 180 hours.

[0130] The thickness of the composite coating, Vickers hardness Hv, convex area ratio, maximum height, arithmetic mean roughness Ra, carbon area ratio of the composite coating surface, and reliability were evaluated for the obtained composite material in the same manner as in Example 1. The reference height H0 was 2.6 μm. Note that a frequency distribution diagram, which was created to determine the convex area ratio, is shown in FIG. 1(a), with the pixel height of each pixel constituting the laser microscope observation image on the horizontal axis and the frequency (number) of each pixel on the vertical axis.

[0131] [Example 7] Using the same material as in Example 1 as the cathode and a Ni electrode plate as the anode, the plating was performed in a nickel plating bath (aqueous solution) consisting of nickel sulfamate with a concentration of 342 g / L (Ni concentration of 80 g / L) and boric acid with a concentration of 45 g / L, at a liquid temperature of 55°C and a current density of 4 A / dm 2 The material was electroplated (Ni plating) for 40 seconds while stirring at 40°C to form a Ni coating (Ni undercoat) with a thickness of 0.3 μm on the material. The thickness of the undercoat was measured in the same manner as that for determining the thickness of the composite coating.

[0132] A composite material was produced in the same manner as in Example 1, except that Ag strike plating was applied to a material having a Ni undercoat.

[0133] The thickness, Vickers hardness Hv, convex area ratio, maximum height, arithmetic mean roughness Ra, carbon area ratio of the composite coating surface, and reliability of the obtained composite material were evaluated in the same manner as in Example 1. The reference height H0 was 3.1 μm.

[0134] [Comparative Example 1] A silver-plated material having a silver plating film formed on a base material was produced in the same manner as in Example 1, except that Ag plating was performed using a sulfonic acid-based silver plating solution with an Ag concentration of 30 g / L containing methanesulfonic acid at a concentration of 60 g / L as a complexing agent (Dynesilver GPE-HB (containing a compound corresponding to general formula (2) and mainly composed of water as a solvent) manufactured by Daiwa Kasei Co., Ltd.) instead of the carbon particle-containing sulfonic acid-based silver plating solution.

[0135] The thickness of the silver plating film, Vickers hardness Hv, convex area ratio, maximum height, arithmetic mean roughness Ra, carbon area ratio of the composite film surface, and reliability of the obtained composite material were evaluated in the same manner as in Example 1. The reference height H0 was 2.5 μm.

[0136] [Comparative Example 2] Except for not carrying out surface treatment on the carbon particles, a composite material was produced in the same manner as in Example 1. The time from preparation of the carbon particle-containing sulfonic acid-based silver plating solution to carrying out electroplating was about 10 minutes.

[0137] The thickness, Vickers hardness Hv, convex area ratio, maximum height, arithmetic mean roughness Ra, carbon area ratio of the composite coating surface, and reliability of the obtained composite material were evaluated in the same manner as in Example 1. The reference height H0 was 2.4 μm.

[0138] [Comparative Example 3] For the composite material prepared in Example 3, three drops of an abrasive (DP Lubricant Red, Model No. 40700070, Emulsion Base (containing diamond abrasive grains with a particle size of 3 μm or less) manufactured by Struers Co., Ltd.) were dropped onto a polishing cloth (MD-Mol manufactured by Struers Co., Ltd., Model No. 40500220, 100% taffeta woven wool manufactured by Struers Co., Ltd.) set on a tabletop sample polishing machine (LaboPol 20 manufactured by Struers Co., Ltd.), and the composite coating was pressed against the polishing cloth for 5 seconds while rotating the polishing cloth at 100 rpm, thereby performing buff polishing. After polishing, the arithmetic mean roughness of the composite coating was calculated using a laser microscope as in Example 1. In addition, when the thickness of the composite coating was measured as in Example 1, it was found to have decreased by 0.2 μm. This operation was repeated, and polishing was terminated when the surface roughness Ra became 1.0 μm or less for the first time.

[0139] The thickness of the composite coating, Vickers hardness Hv, convex area ratio, arithmetic mean roughness Ra, carbon area ratio of the composite coating surface, and reliability were evaluated for the obtained (polished) composite material in the same manner as in Example 1. The reference height H0 was 2.9 μm. Note that a frequency distribution diagram was created to determine the convex area ratio, with the horizontal axis representing the pixel height of each pixel constituting the laser microscope observation image and the vertical axis representing the frequency (number) of each pixel, as shown in FIG. 1(b).

[0140] [Comparative Example 4] <Agストライクめっき> A material similar to that in Example 1 was prepared, and this material was used as the cathode and a titanium platinum mesh electrode plate (a titanium mesh material plated with platinum) as the anode. The plating was performed at 25°C in a cyanide-based Ag strike plating solution (prepared from general reagents, silver cyanide concentration 3 g / L, potassium cyanide concentration 90 g / L, solvent water) containing a cyanide compound as a complexing agent, at a current density of 5 A / dm 2 Electroplating (Ag strike plating) was performed for 30 seconds.

[0141] <AgSbめっき> A cyanide-based Ag-Sb alloy plating solution (solvent: water) containing a cyanide compound as a complexing agent and having a silver concentration of 60 g / L and an antimony (Sb) concentration of 2.5 g / L was prepared. The cyanide-based Ag-Sb alloy plating solution contains 10 mass% silver cyanide, 30 mass% sodium cyanide, and Nissin Bright N (manufactured by Nissin Chemical Industries, Ltd.), and the concentration of Nissin Bright N in the plating solution is 50 mL / L. Nissin Bright N contains a brightener and diantimony trioxide, and the concentration of diantimony trioxide in Nissin Bright N is 6 mass%.

[0142] Next, the above Ag strike plated material was used as the cathode and the silver electrode plate as the anode, and the plating was performed in the above cyan-based Ag-Sb alloy plating solution at a temperature of 18°C ​​and a current density of 3 A / dm while stirring at 400 rpm with a stirrer. 2 The material was electroplated at 0.05 V for 300 seconds to obtain a composite material in which a composite coating (silver-antimony coating) was formed on the material.

[0143] The thickness, Vickers hardness Hv, convex area ratio, maximum height, arithmetic mean roughness Ra, carbon area ratio of the composite coating surface, and reliability of the obtained composite material were evaluated in the same manner as in Example 1. The reference height H0 was 2.2 μm.

[0144] [Comparative Example 5] Instead of the sulfonic acid-based silver plating solution of Example 1, a sulfonic acid-based silver plating solution with a silver concentration of 30 g / L containing methanesulfonic acid at a concentration of 60 g / L as a complexing agent (Dainsilver GPE-PL (containing no compound corresponding to general formula (2) and using water as the solvent) manufactured by Daiwa Kasei Co., Ltd.) was used, to which carbon particles (graphite particles) that had been subjected to the same oxidation treatment as in Example 1 were added. The resulting carbon particle-containing sulfonic acid-based silver plating solution was used to perform AgC plating for a plating time of 300 seconds, and a composite material in which a composite coating was formed on a material was produced in the same manner as in Example 1.

[0145] The thickness of the composite coating, Vickers hardness Hv, convex area ratio, maximum height, arithmetic mean roughness Ra, carbon area ratio of the composite coating surface, and silver crystallite size of the composite coating were evaluated for the obtained composite material in the same manner as in Example 1. The reference height H0 was 3.2 μm. Note that the reliability of Comparative Example 5 was not evaluated.

[0146] The production conditions and the like for the above-mentioned Examples 1 to 7 and Comparative Examples 1 to 5 are summarized in Tables 1 and 2, and various evaluation results are summarized in Tables 3 and 4.

[0147] [Table 1]

[0148] [Table 2]

[0149] [Table 3]

[0150] [Table 4]

[0151] Comparative Example 2 shows that unless the carbon particles are treated (surface treated) with Compound A, the projections are not sufficiently formed, and the reliability is reduced. Comparative Example 3 shows that even in the case of a composite coating that has been subjected to the above-mentioned surface treatment, the reliability is reduced if the projections are removed.

Claims

1. A composite material comprising a composite coating formed on a base material and made of a silver layer containing carbon particles, When the composite coating is observed with a laser microscope, the pixel height of each pixel constituting the observation field of view is calculated as the height difference with respect to the lowest pixel in the observation field of view. When the pixel heights of each pixel are arranged in ascending order, the pixel height of the pixel at which the cumulative number ratio is 10% is defined as the reference height H. 0 The pixel height in the observation field of view is the reference height H 0 When a pixel having a height of 1 μm or more is defined as a convex portion, the proportion of the convex portions in the observation field of view is 12 area % or more. Composite material.

2. The composite of claim 1 , wherein the material comprises Cu or a Cu alloy.

3. 3. The composite material of claim 1 or 2, wherein the composite coating has a silver crystallite size of 40 nm or less.

4. 3. The composite material according to claim 1, wherein the protrusions account for 15 to 75% by area.

5. 3. The composite material according to claim 1, wherein the proportion of the carbon particles on the surface of the composite coating is 10 to 80 area %.

6. The composite material according to claim 1 or 2, wherein the thickness of the composite coating is 1.5 to 25 μm.

7. 3. The composite material according to claim 1, wherein the surface of the composite coating has a Vickers hardness of 100 or more.

8. The composite material according to claim 1 or 2, wherein the composite coating has an arithmetic mean roughness Ra of 0.6 μm or more.

9. 3. The composite material according to claim 1, further comprising an underlayer made of at least one material selected from the group consisting of Cu, Ni, Sn, and Ag, formed between the base material and the composite coating.

10. A method for producing a composite material, comprising the steps of: forming a composite coating made of a silver layer containing carbon particles on a material by electroplating in a silver plating solution containing carbon particles, the carbon particles are surface-treated carbon particles that have been treated with 2,4-dihydroxybenzoic acid in an aqueous liquid for 30 minutes or more; the silver plating solution contains the surface-treated carbon particles and a compound B represented by the following general formula (2), The silver plating solution contains silver ions at a concentration of 5 to 150 g / L, the concentration of the surface-treated carbon particles in the silver plating solution is 10 to 150 g / L; The concentration of compound B in the silver plating solution is 2 to 250 g / L; a concentration of the complexing agent in the silver plating solution is 30 to 200 g / L; 【Chemistry 1】 In formula (2), p is an integer of 1 to 5, Rd is a carboxyl group; Re is an aldehyde group, a carboxyl group, an amino group, a hydroxyl group, or a sulfonic acid group; Rf is hydrogen or an optional substituent; When p is 2 or more, a plurality of Re may be the same or different, When p is 3 or less, a plurality of Rf's may be the same or different, Rd and Re may each independently be bonded to the benzene ring via a divalent group consisting of at least one group selected from the group consisting of -O- and -CH 2 -.

11. The method for producing a composite material according to claim 10, wherein the material is composed of Cu or a Cu alloy.

12. The method for producing a composite material according to claim 10 or 11, wherein the treatment of the carbon particles with 2,4-dihydroxybenzoic acid is carried out by stirring the carbon particles and an aqueous liquid containing 2,4-dihydroxybenzoic acid for 30 minutes or more.

13. 3. A terminal for electrical contacts, the terminal comprising the composite material according to claim 1 or 2 as a constituent material.

Citation Information

Patent Citations

  • Electric contact material manufacturing method and electric contact material

    JP2007042391A

  • Graphene powder, graphene powder / organic solvent dispersion, graphene-electrode active material composite particle, electrode paste, and electrode

    JP2019052083A

  • Ag-GRAPHENE COMPOSITE PLATING FILM METAL TERMINAL AND MANUFACTURING METHOD THEREOF

    JP2021072185A

  • Composite plated material, and method of producing the same

    JP2021109981A

  • Sliding contacts for electrical equipment

    JP3054628B2