Current collector, electrochemical device and electronic device including said current collector
The use of a polymer-based current collector with specific resistivity ratios and orientations addresses the energy density limitations of lithium-ion batteries, enhancing electron conductivity and stability for high voltage applications.
Patent Information
- Application Number
- JP2022563959
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-06-30
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2040-06-30
AI Technical Summary
Lithium-ion batteries face limitations in achieving high energy density due to differences in capacity among connected batteries, which restricts their application, especially when used in series connections for high voltage requirements in electric vehicles and energy storage systems.
A current collector with a polymer base material and conductive material, having specific electronic resistivity ratios and orientations, is used to enhance electron conductivity and uniform current distribution, reducing the need for inert materials and improving the energy density of lithium-ion batteries.
The proposed current collector achieves uniform current density distribution, enhances electron conductivity, and reduces the overall weight and cost, leading to improved energy density and stability in lithium-ion batteries, suitable for high voltage applications.
Smart Images

Figure 0007595085000003 
Figure 0007595085000004 
Figure 0007595085000005
Abstract
Description
[Technical field]
[0001] The present invention relates to the technical field of electrochemistry, and in particular to current collectors, electrochemical devices and electronic devices containing said current collectors. [Background technology]
[0002] Lithium ion batteries have the advantages of large specific energy, high operating voltage, low self-discharge rate, small volume, light weight, etc., and are widely used in the field of electronic applications. With the rapid development of electric vehicles and portable electronic devices, the demand for the performance of lithium ion batteries is increasing, for example, lithium ion batteries are required to have high energy density, high safety, excellent cycle performance, etc.
[0003] However, lithium-ion batteries are limited by their inherent electrochemical system, and it is usually difficult for the operating voltage of a single battery to exceed 5 V. However, in practical use, lithium-ion batteries are often used at high voltages, for example in electric vehicles (EVs) and energy storage systems (ESSs).
[0004] In the prior art, in order to improve the output voltage of a lithium-ion battery, it is common to connect multiple lithium-ion batteries in series with external wiring. However, with this series connection method, the energy density (ED) of the entire series-connected lithium-ion batteries is low due to the capacity difference between the individual lithium-ion batteries themselves, limiting the range of application of lithium-ion batteries. Summary of the Invention
[0005] The present invention provides a current collector, an electrochemical device including the current collector, and an electronic device including the current collector, for improving the energy density of a lithium ion battery. The specific technical solutions are as follows:
[0006] A first aspect of the present invention provides a current collector comprising a polymer base material and a conductive material, wherein the current collector has an electronic resistivity of 10 Ω·cm to 1000 Ω·cm in an XY in-plane direction and an electronic resistivity of 0.01 Ω·cm to 30 Ω·cm in a Z direction.
[0007] In one embodiment of the present invention, the mass of the conductive material is 10% to 70% of the mass of the current collector.
[0008] In one embodiment of the present invention, the conductive material includes at least one of a one-dimensional conductive material and a two-dimensional conductive material, and the angle between the length direction of the one-dimensional conductive material or the planar direction of the two-dimensional conductive material and the Z direction of the current collector is 0° to 30°.
[0009] In one embodiment of the present invention, the ratio of the electronic resistivity in the XY in-plane direction of the current collector to the electronic resistivity in the Z direction of the current collector is 5-4,000.
[0010] In one embodiment of the present invention, the current collector has a thickness of 2 μm to 500 μm.
[0011] In one embodiment of the invention, one or both ends of the conductive material are exposed at a surface of the polymeric substrate.
[0012] In one embodiment of the present invention, the one-dimensional conductive material has a length of 0.1 μm to 200 μm, a diameter of 2 nm to 500 nm, and a specific surface area of 5 m. 2 / g~2000m 2 / g.
[0013] In one embodiment of the present invention, the two-dimensional conductive material has a length of 2 μm to 10 μm, a thickness of 6 nm to 20 μm, and a specific surface area of 0.5 m. 2 / g~1000m 2 / g.
[0014] In one embodiment of the present invention, the current collector is (a) the electronic resistivity in the XY in-plane direction of the current collector is 50 Ω cm to 1000 Ω cm; (b) the electronic resistivity in the Z direction of the current collector is 0.01 Ω cm to 1 Ω cm; (c) the ratio of the electronic resistivity in the XY in-plane direction of the current collector to the electronic resistivity in the Z direction of the current collector is 100 to 1000; (d) the angle between the conductive material and the Z direction is 0° to 10°; (e) the thickness of the current collector is 5 μm to 50 μm; (f) the mass of the conductive material is 20% to 60% of the mass of the current collector; Satisfy at least one of the following:
[0015] In one embodiment of the present invention, the current collector is (a) the electronic resistivity in the XY in-plane direction of the current collector is 100 Ω cm to 1000 Ω cm; (b) the electronic resistivity in the Z direction of the current collector is 0.01 Ω cm to 0.05 Ω cm; (c) the ratio of electronic resistivity in the XY in-plane direction of the current collector to electronic resistivity in the Z direction of the current collector is 200 to 600; (d) the thickness of the current collector is 5 μm to 20 μm; (e) the mass of the conductive material is 40% to 50% of the mass of the current collector; (f) the tensile strength of the current collector is 80 MPa to 100 MPa; Satisfy at least one of the following:
[0016] In one embodiment of the present invention, the conductive material includes at least one of a carbon material and a metal material.
[0017] In one embodiment of the present invention, the carbon material includes at least one of single-walled carbon nanotubes, multi-walled carbon nanotubes, conductive carbon fibers, conductive carbon black, fullerenes, conductive graphite, and graphene.
[0018] In one embodiment of the present invention, the metallic material includes at least one of Ni, Ti, Ag, Au, Pt, and stainless steel and its alloys.
[0019] In one embodiment of the present invention, the polymer substrate comprises at least one of polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyether ether ketone, polyimide, polyamide, polyethylene glycol, polyamideimide, polycarbonate, cyclic polyolefin, polyphenylene sulfide, polyvinyl acetate, polytetrafluoroethylene, polymethylene naphthalene, polyvinylidene fluoride, polyethylene naphthalate, polypropylene carbonate, poly(vinylidene fluoride-hexafluoropropylene), poly(vinylidene fluoride-co-chlorotrifluoroethylene), silicone resin, vinylon, polypropylene, polyethylene, polyvinyl chloride, polystyrene, polyether nitrile, polyurethane, polyphenylene ether, polysulfone, and derivatives thereof.
[0020] A second aspect of the present invention provides an electrochemical device comprising at least two electrode assemblies and a current collector according to any one of the above embodiments, the current collector being located between the two electrode assemblies.
[0021] A third aspect of the present invention provides an electronic device comprising the electrochemical device according to the second aspect above.
[0022] In the present invention, the term "degree of orientation" refers to the angle between the length direction of a one-dimensional conductive material or the planar direction of a two-dimensional conductive material and the Z direction of the current collector.
[0023] The “unidirectional conduction ratio” is expressed as ((R2-R1)×H) / (R0×(L2-L1)), where R0 is the impedance between two cylindrical metal electrodes facing each other on both sides of the XY plane of the sample, L1 is the distance between the position of a cylindrical metal electrode after the first translation along the XY plane and its initial position, R1 is the impedance between the two cylindrical metal electrodes after the first translation, L2 is the distance between the position of the same cylindrical metal electrode after the second translation along the XY plane and its initial position, R2 is the impedance between the two cylindrical metal electrodes after the second translation, and H is the thickness of the sample.
[0024] Regarding the current collector provided by the present invention, and the electrochemical device and electronic device including the current collector, on the one hand, the polymer substrate in the current collector has excellent oxidation resistance, reduction resistance, ion insulation, mechanical strength, and thermal stability, and the electronic resistivity of the current collector in the Z direction is 0.01 Ω·cm to 30 Ω·cm, so that the bipolar electrochemical device including the current collector of the present invention has excellent electronic conduction performance in the Z direction, and furthermore, the electronic resistivity of the current collector in the XY plane direction is 10 Ω·cm to 1000 Ω·cm, so that the current density in the entire XY plane is more uniformly distributed, and the electrode sheet has better consistency in charging and discharging at different positions, which is favorable for the long-term stable cycle of the electrochemical device. On the other hand, the density of the polymer substrate is lower, so that the content of inactive materials in the entire bipolar electrochemical device can be reduced, thereby improving the energy density of the bipolar electrochemical device. The current collector of the present invention is lower in cost than conventional metal foil current collectors, and is particularly suitable for mass production. Furthermore, the present invention achieves high voltage output of a single electrochemical device, and saves the volume and weight of some of the exterior materials compared with the conventional method of connecting multiple electrochemical cells in series into one electrochemical device, thereby improving the energy density, and also simplifying the entire manufacturing process of the electrochemical device and reducing the manufacturing cost. [Brief description of the drawings]
[0025] In order to clearly explain the technical solutions of the present invention and the prior art, the drawings used in the embodiments or the prior art will be briefly described below. Obviously, the drawings described below are only a part of the embodiments of the present invention, and those skilled in the art can obtain other technical solutions based on these drawings without making inventive efforts.
[0026] [Figure 1] FIG. 1 is a schematic diagram of a current collector according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram of a current collector according to another embodiment of the present invention. [Diagram 3] FIG. 3 is a schematic diagram of an electrochemical device according to one embodiment of the present invention. [Figure 4] FIG. 4 is a schematic diagram showing how the electronic resistivity of a bipolar current collector in the XY in-plane direction is measured using the four-probe method in the present invention. [Diagram 5] FIG. 5 is a schematic diagram for measuring the unidirectional conductivity ratio of a bipolar current collector in the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] In order to make the objectives, technical solutions and advantages of the present invention clearer, the present invention will be further described in detail with reference to the drawings and embodiments. Obviously, the embodiments described in the present invention are only some of the embodiments of the present invention, not all of the embodiments. Those skilled in the art will understand that all other technical solutions obtained based on the embodiments of the present invention without making inventive efforts are included in the protection scope of the present invention.
[0028] In the specific embodiment of the present invention, the present invention will be described taking a lithium ion battery as an example of an electrochemical device, but the electrochemical device of the present invention is not limited to a lithium ion battery.
[0029] A bipolar lithium-ion battery, a new type of lithium-ion battery, has multiple battery cores connected in series to form one lithium-ion battery, thereby increasing the output voltage of the lithium-ion battery. The current collector used in this lithium-ion battery is a bipolar current collector. Since one side of the bipolar current collector contacts the positive electrode active material and the other side contacts the negative electrode active material, the current collector is required to have oxidation resistance and reduction resistance. The bipolar current collector is usually a metal foil such as an aluminum / copper composite foil. However, conventional bipolar lithium-ion batteries usually have the following problems. On the one hand, the poor interfacial bonding between the metals of the aluminum / copper composite foil is disadvantageous to the cycle stability of the bipolar lithium-ion battery, and on the other hand, the metal foil is more expensive, which increases the manufacturing cost of the bipolar lithium-ion battery.
[0030] In addition, the conventional bipolar current collector may further include a multi-layer metal composite current collector obtained by directly combining Cu foil and Al foil. Although such a current collector has a certain degree of oxidation resistance and reduction resistance, it has problems such as poor interfacial bonding between metals and difficulty in thinning the current collector.
[0031] In view of the above, the present invention provides a current collector comprising a polymer substrate and a conductive material. Here, without being limited by any theory, the electronic resistivity of the current collector in the XY plane direction is 10 Ω·cm to 1000 Ω·cm, so that the current density in the entire XY plane of the current collector is more uniformly distributed, and the charge and discharge at different positions of the electrode sheet have better consistency, which is favorable for the lithium ion battery to be cycled stably for a long time. The electronic resistivity of the current collector in the Z direction is 0.01 Ω·cm to 30 Ω·cm, so that the current collector can have excellent electronic conductivity in the Z direction.
[0032] In the present invention, the polymer substrate may be a film, specifically, a film made of a polymer material. A detailed description of the polymer substrate will be given later. The Z direction refers to the thickness direction of the current collector, the XY plane refers to a plane perpendicular to the Z direction, and the XY in-plane direction refers to any direction perpendicular to the Z direction and parallel to the XY plane.
[0033] In one embodiment of the present invention, the mass of the conductive material is 10% to 70% of the mass of the current collector, preferably 20% to 60% of the mass of the current collector, and more preferably 40% to 50% of the mass of the current collector.
[0034] In one embodiment of the present invention, the conductive material includes at least one of a one-dimensional conductive material and a two-dimensional conductive material, and the angle between the length direction of the one-dimensional conductive material or the planar direction of the two-dimensional conductive material and the Z direction of the current collector is 0° to 30°, i.e., the orientation degree of the conductive material is 0° to 30°.
[0035] In the present invention, the one-dimensional conductive material can be a stripe-shaped or rod-shaped conductive material, and the two-dimensional conductive material can be a sheet-shaped conductive material. When the included angle between the length direction of the one-dimensional conductive material or the plane direction of the two-dimensional conductive material and the Z direction of the current collector is 0°-30°, the current collector can have excellent electronic conductivity in the Z direction, and the current collector can have lower electronic conductivity in the XY plane direction, so that the current density in the entire XY plane of the current collector is more uniformly distributed, and the charge and discharge at different positions of the electrode sheet have better consistency.
[0036] Fig. 1 is a schematic diagram of a current collector according to one embodiment of the present invention. As shown in Fig. 1, a one-dimensional conductive material can be embedded in a polymer substrate, and the included angle between the length direction of the one-dimensional conductive material and the Z direction of the current collector is 0° to 30°, preferably 0° to 10°, and more preferably 3° to 10°.
[0037] Fig. 2 is a schematic diagram of a current collector according to another embodiment of the present invention. As shown in Fig. 2, a two-dimensional conductive material can also be embedded in a polymer substrate, and the included angle between the length direction of the two-dimensional conductive material and the Z direction of the current collector is 0° to 30°, preferably 0° to 10°, and more preferably 3° to 10°.
[0038] Furthermore, one or both ends of the one-dimensional conductive material or two-dimensional conductive material can be exposed on the surface of the polymer substrate. As shown in FIG. 1 and FIG. 2, the current collector has two surfaces, designated as surface A and surface B. At any point M on surface A of the current collector, the conductive material can be exposed from the polymer substrate, and at another point N on surface B of the current collector, the conductive material can be exposed from the polymer substrate in the same manner, and it is considered that points M and N are connected by the conductive material in the polymer substrate to realize electronic conduction between surface A and surface B of the current collector. The conductive material in the polymer substrate may be a one-dimensional conductive material or a two-dimensional conductive material penetrating the polymer substrate, or electronic conduction between surface A and surface B may be formed by a plurality of one-dimensional conductive materials or two-dimensional conductive materials connected to each other.
[0039] In one embodiment of the present invention, the ratio of the electronic resistivity in the XY in-plane direction of the current collector to the electronic resistivity in the Z direction of the current collector is 5 to 4000, so that the current collector has excellent electronic conductivity in the Z direction and can have lower electronic conductivity in the XY in-plane direction of the current collector, and the current density can be uniformly distributed throughout the entire XY plane of the current collector.
[0040] In one embodiment of the present invention, the unidirectional conductivity ratio of the current collector is 5.4 to 4240, so that the current collector has excellent electronic conductivity in the Z direction and has lower electronic conductivity in the XY in-plane direction, and the current density can be uniformly distributed throughout the entire XY plane of the current collector.
[0041] In the present invention, the thickness of the current collector is not particularly limited as long as the object of the present invention can be achieved. In one embodiment of the present invention, the thickness of the current collector is 2 μm to 500 μm, preferably 5 to 50 μm, and more preferably 5 μm to 20 μm.
[0042] In one embodiment of the present invention, the electronic resistivity in the XY plane of the current collector is preferably 50 Ω·cm to 1000 Ω·cm, and more preferably 100 Ω·cm to 1000 Ω·cm, thereby enabling a more uniform distribution of current density throughout the XY plane of the current collector. The electronic resistivity in the Z direction of the current collector is preferably 0.01 Ω·cm to 1 Ω·cm, and more preferably 0.01 Ω·cm to 0.05 Ω·cm, thereby enabling the current collector to have excellent electronic conductivity in the Z direction.
[0043] In one embodiment of the present invention, the ratio of the electronic resistivity in the XY in-plane direction of the current collector to the electronic resistivity in the Z direction of the current collector is preferably 100 to 1000, and more preferably 200 to 600. This allows the current collector to have better electronic conductivity in the Z direction and lower electronic conductivity in the XY in-plane direction of the current collector, and allows the current density to be uniformly distributed throughout the entire XY plane of the current collector.
[0044] In the present invention, the size of the one-dimensional conductive material is not particularly limited as long as the object of the present invention can be achieved. For example, the one-dimensional conductive material has a length of 0.1 μm to 200 μm, a diameter of 2 nm to 500 nm, and a specific surface area of 5 m. 2 / g~2000m 2 / g.
[0045] For example, in one-dimensional conductive materials, carbon nanotubes generally have a diameter of 2 nm to 30 nm, a length of 0.1 nm to 200 μm, and a specific surface area of 100 m 2 / g~2000m 2 / g, and the conductive carbon fiber (VGCF) has a diameter of 30 nm to 500 nm, a length of 0.5 μm to 50 μm, and a specific surface area of 5 m 2 / g~100m 2 / g.
[0046] In the present invention, the size of the two-dimensional conductive material is not particularly limited as long as the object of the present invention can be achieved. For example, the two-dimensional conductive material has a length of 2 μm to 10 μm, a thickness of 6 nm to 20 μm, and a specific surface area of 0.5 m. 2 / g~1000m 2 / g.
[0047] For example, in a two-dimensional conductive material, the average length of graphene is 50 nm to 20 μm, the sheet layer generally has 1 to 15 layers, and when converted into a thickness, the thickness is 0.4 nm to 6 nm, and the specific surface area is 10 m 2 / g~1000m 2 / g, and the conductive graphite sheet has a thickness of 0.3 μm to 20 μm, a diameter of 2 μm to 10 μm, and a specific surface area of 0.5 m 2 / g~10m 2 / g.
[0048] In the present invention, the conductive material is not particularly limited as long as the object of the present invention can be achieved, and for example, the conductive material may include at least one of a carbon material and a metal material. In addition, the conductive material of the present invention has excellent conductivity and its electronic resistivity is generally 10 -4 Less than Ω m.
[0049] In the present invention, the carbon material is not particularly limited as long as the object of the present invention can be achieved. For example, the carbon material may include at least one of single-walled carbon nanotubes, multi-walled carbon nanotubes, conductive carbon fibers, conductive carbon black (e.g., acetylene black), fullerene, conductive graphite, and graphene.
[0050] In the present invention, the metal material is not particularly limited as long as the object of the present invention can be achieved, and for example, the metal material may include at least one of Ni, Ti, Ag, Au, Pt, and stainless steel and its alloy. Furthermore, the metal material may be a one-dimensional material or a two-dimensional material, and the physical shape may be changed. For example, the one-dimensional metal material may be a striped metal such as Ni or Ti, and the two-dimensional metal material may be a sheet-shaped (or planar) metal such as Ni or Ti.
[0051] In the present invention, the polymer substrate is not particularly limited as long as it can achieve the object of the present invention, and for example, the polymer substrate can include at least one of polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyether ether ketone, polyimide, polyamide, polyethylene glycol, polyamideimide, polycarbonate, cyclic polyolefin, polyphenylene sulfide, polyvinyl acetate, polytetrafluoroethylene, polymethylene naphthalene, polyvinylidene fluoride, polyethylene naphthalate, polypropylene carbonate, poly(vinylidene fluoride-hexafluoropropylene), poly(vinylidene fluoride-co-chlorotrifluoroethylene), silicone resin, vinylon, polypropylene, polyethylene, polyvinyl chloride, polystyrene, polyether nitrile, polyurethane, polyphenylene ether, polysulfone, and derivatives thereof. It is understood that the polymer substrate itself has ion inactivity, that is, ions are unlikely to pass through the polymer substrate.
[0052] In one embodiment of the present invention, the tensile strength of the current collector is 80 MPa to 100 MPa, so that the current collector has excellent mechanical strength, and a bipolar lithium ion battery including the current collector has good safety.
[0053] The current collector of the present invention has the following beneficial effects compared to conventional current collectors.
[0054] The electronic resistivity of the current collector in the XY plane of the present invention is 10 Ω·cm to 1000 Ω·cm, and the electronic resistivity of the current collector in the Z direction is 0.01 Ω·cm to 30 Ω·cm. Therefore, a lithium-ion battery including the current collector of the present invention has excellent electronic conductivity in the Z direction, and the current density is more uniformly distributed throughout the XY plane. Furthermore, the electrode sheets have better consistency in charge and discharge at different positions, which is advantageous for the bipolar lithium-ion battery to be cycled stably for a long time.
[0055] The lower density of the polymeric substrate in the current collector of the present invention compared to metal current collectors allows for a reduction in the overall proportion of inactive materials in the bipolar lithium ion battery, thereby improving the energy density of the bipolar electrochemical device.
[0056] The current collector of the present invention is less likely to generate conductive fragments when subjected to mechanical abuse such as nail penetration, impact, and pressure, and has a high coating effect on the mechanically damaged surface, compared to conventional metal current collectors, thereby improving the safety margin in the event of such mechanical abuse and improving the safety of bipolar lithium-ion batteries.
[0057] The current collector of the present invention is less expensive and particularly suitable for mass production as compared to conventional metal current collectors, such as conventional stainless steel or titanium current collectors.
[0058] The present invention further provides an electrochemical device comprising at least two electrode assemblies and a current collector according to any one of the above embodiments, the current collector being located between the two electrode assemblies, whereby the at least two electrode assemblies are connected in series internally via a bipolar electrode comprising the current collector of the present invention to form a bipolar lithium ion battery, which can have a higher operating voltage.
[0059] In one embodiment of the present invention, the electrochemical device includes at least two electrode assemblies and a current collector according to any one of the above embodiments, the current collector being located between the two electrode assemblies, and a tab can be extended from the current collector for monitoring the voltage of the electrochemical device.
[0060] In one embodiment of the present invention, the electrochemical device includes at least two electrode assemblies and a bipolar electrode sheet, the bipolar electrode sheet being located between the two electrode assemblies, and the bipolar electrode sheet includes a current collector according to any one of the above embodiments, and a positive electrode active material layer and a negative electrode active material layer coated on both sides of the current collector.
[0061] As can be seen, since the bipolar electrode sheet is obtained by applying a positive electrode active material and a negative electrode active material to both sides of a current collector, the electrochemical device contains more electrode active material, thereby improving the energy density of the electrochemical device.
[0062] In one embodiment of the present invention, the electrochemical device includes at least two electrode assemblies and a bipolar electrode sheet, the bipolar electrode sheet being located between the two electrode assemblies, and the bipolar electrode sheet includes a current collector according to any one of the above embodiments, an undercoat applied to both sides of the current collector, and a positive electrode active material layer and a negative electrode active material layer applied to both sides of the current collector.
[0063] The undercoat can improve the adhesion between the current collector and the active material, and enhance the electronic conduction performance between the current collector and the active material.
[0064] The undercoat is typically obtained by coating a current collector with a slurry formed by mixing conductive carbon black, styrene butadiene rubber, and deionized water, followed by drying. The undercoats on both sides of the bipolar current collector may be the same or different. The manufacturing processes of the positive electrode active material layer, the negative electrode active material layer, the positive electrode undercoat, and the negative electrode undercoat are described in the following examples.
[0065] Fig. 3 is a schematic diagram of an electrochemical device according to one embodiment of the present invention. As shown in Fig. 3, the electrochemical device is separated into two electrode assemblies, such as a first electrode assembly 100 and a second electrode assembly 200, by a bipolar current collector 300. Here, in Fig. 3, the first electrode assembly 100 includes, from the top, a negative electrode 101, a first negative electrode active material layer 102, a first separator 103, a first positive electrode active material layer 104, and a part of the bipolar current collector 300, and the second electrode assembly 200 includes, from the top, a positive electrode 201, a second positive electrode active material layer 202, a second separator 203, a second negative electrode active material layer 204, and another part of the bipolar current collector 300. In addition, the electrochemical device can be sealed by a sealing member 400, so that the electrochemical device is formed into a two independent chamber structure, and the two chambers correspond to the first electrode assembly 100 and the second electrode assembly 200 respectively.
[0066] The present invention further provides an electronic device comprising an electrochemical device according to an embodiment of the present invention.
[0067] In the electrochemical device provided by the present invention, the current collector provided by the present invention can be used as a separator between the electrode assemblies, and of course, the current collector provided by the present invention can also be used as a current collector in the electrode assembly. The separator described in the present invention can be a separating member between two electrode assemblies.
[0068] The positive electrode sheet of the present invention is not particularly limited as long as it can achieve the object of the present invention. For example, the positive electrode sheet usually includes a positive electrode collector and a positive electrode active material. Here, the positive electrode collector is not particularly limited, and any positive electrode collector known in the art, such as aluminum foil, aluminum alloy foil, or a composite current collector, can be used. The positive electrode active material is not particularly limited, and may be any positive electrode active material in the prior art. The positive electrode active material includes at least one of NCM811, NCM622, NCM523, NCM111, NCA, lithium iron phosphate, lithium cobalt oxide, lithium manganate, lithium manganese iron phosphate, and lithium titanate.
[0069] The negative electrode sheet of the present invention is not particularly limited as long as it can achieve the object of the present invention. For example, the negative electrode sheet usually includes a negative electrode current collector and a negative electrode active material layer. Here, the negative electrode current collector is not particularly limited, and any negative electrode current collector known in the art, such as copper foil, aluminum foil, aluminum alloy foil, and composite current collector, can be used. The negative electrode active material layer includes a negative electrode active material, and the negative electrode active material is not particularly limited, and any negative electrode active material known in the art can be used. The negative electrode active material can include at least one of artificial graphite, natural graphite, mesocarbon microbeads, soft carbon, hard carbon, silicon, silicon carbon, and lithium titanate.
[0070] The electrolyte solution of the present invention is not particularly limited, and any electrolyte solution known in the art can be used. The electrolyte solution may be, for example, any one of a gel, a solid, and a liquid. For example, the liquid electrolyte solution may contain a lithium salt and a non-aqueous solvent.
[0071] The lithium salt is not particularly limited, and any lithium salt known in the art can be used as long as it can achieve the object of the present invention. For example, the lithium salt may include at least one of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium difluorophosphate (LiPO2F2), lithium bis(trifluoromethanesulfonyl)imide LiN(CF3SO2)2 (LiTFSI), lithium bis(fluorosulfonyl)imide Li(N(SO2F)2) (LiFSI), lithium bis(oxalate)borate LiB(C2O4)2 (LiBOB), and lithium difluoro(oxalate)borate LiBF2(C2O4) (LiDFOB). For example, LiPF6 can be selected and used as the lithium salt.
[0072] The non-aqueous solvent is not particularly limited as long as the object of the present invention can be achieved. For example, the non-aqueous solvent may contain at least one of a carbonate ester compound, a carboxylate ester compound, an ether compound, a nitrile compound, and other organic solvents.
[0073] For example, the carbonate ester compounds include diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), ethyl methyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinyl ethylene carbonate (VEC), fluoroethylene carbonate (FEC), 1,2- The fluoroethylene carbonate may include at least one of difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, and trifluoromethylethylene carbonate.
[0074] The separator of the present invention is not particularly limited, but includes, for example, a polymer or an inorganic material made of a material stable to the electrolyte of the present invention.
[0075] The separator may include, for example, a substrate layer and a surface treatment layer. The substrate layer may be a nonwoven fabric, a film, or a composite membrane having a porous structure, and the material of the substrate layer may be at least one selected from the group consisting of polyethylene, polypropylene, polyethylene terephthalate, and polyimide. The separator may optionally use a polypropylene porous membrane, a polyethylene porous membrane, a polypropylene nonwoven fabric, a polyethylene nonwoven fabric, or a polypropylene-polyethylene-polypropylene porous composite membrane. Optionally, a surface treatment layer is provided on at least one surface of the substrate layer, and the surface treatment layer may be a polymer layer or an inorganic layer, or may be a layer formed by mixing a polymer and an inorganic material.
[0076] For example, the inorganic layer includes inorganic particles and an adhesive. The inorganic particles are not particularly limited, and may be, for example, at least one selected from the group consisting of aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide, and barium sulfate. The adhesive is not particularly limited, and may be, for example, one or a combination of a plurality of types selected from the group consisting of polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylate, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene, and polyhexafluoropropylene. The polymer layer includes a polymer, the polymeric material including at least one of polyamide, polyacrylonitrile, acrylate polymer, polyacrylic acid, polyacrylate, polyvinylpyrrolidone, polyvinyl ether, polyvinylidene fluoride, and poly(vinylidene fluoride-hexafluoropropylene).
[0077] The present invention provides a method for producing the current collector according to any one of the above embodiments, the method comprising the steps of: A step of producing a polymer material layer: spraying a polymer material on the surface of the stainless steel substrate by an electrostatic spray method so that the thickness of the polymer material layer is 2 μm to 800 μm, thereby producing a polymer material layer; A step of heating the polymer material layer: heating the obtained polymer material layer to 250°C to 300°C to soften the polymer material layer; Planting a conductive material: Planting a one-dimensional conductive material or a two-dimensional conductive material into the polymer material layer in a direction perpendicular to the surface of the polymer material layer by electrostatic flocking, and maintaining the polymer material layer in a softened state; Roll pressing of the polymeric material layer under the condition of overheating: pressing the obtained polymeric material layer by a roll press under the condition of overheating so that the surface of the polymeric material layer is smooth and the thickness is uniform, where the overheating temperature is a temperature 10°C to 20°C higher than the heating temperature, and the thickness of the polymeric material layer after pressing by the roll press is 2 μm to 500 μm; Fabricating the current collector: removing the resulting polymeric material layer from the stainless steel substrate with a doctor blade and winding it up to obtain the current collector.
[0078] In one embodiment of the present invention, the surface of the polymer layer implanted with the conductive material obtained above can be sprayed with another polymer layer by electrostatic spraying, the polymer layer can be kept in a softened state, and pressed by a roll press under a heated condition. The purpose of spraying another polymer layer is to better embed the conductive material in the polymer layer, and it is natural that the thickness of the polymer layer can be reasonably controlled so that the end of the conductive material is exposed to the polymer layer.
[0079] In the present invention, the electrostatic flocking process is not particularly limited as long as the object of the present invention can be achieved. For example, in the electrostatic flocking process, the speed at which the conductive material is implanted in the polymer material layer can be controlled by setting the external electric field strength to 5 kV to 500 kV (the stronger the external electric field, the greater the speed of the conductive material). As a result, after the conductive material is implanted from one side of the polymer material layer, the "implanted end" is exposed from the other side of the polymer material layer.
[0080] In the present invention, the electrostatic spray process is not particularly limited as long as it can obtain one layer of polymer material. The current collector manufactured in the present invention is used as a bipolar current collector in a bipolar electrode sheet. The electrode assembly of the present invention is not particularly limited, and any electrode assembly in the prior art can be used as long as it can achieve the object of the present invention, for example, a stacked type electrode assembly or a wound type electrode assembly can be used. The electrode assembly usually includes a positive electrode sheet, a negative electrode sheet, and a separator.
[0081] Hereinafter, the embodiments of the present invention will be described in more detail with reference to examples and comparative examples. Each experiment and evaluation is performed in the following manner. Note that, unless otherwise specified, "parts by weight" and "%" are based on weight. Example 1
[0082] <Manufacturing of bipolar electrode sheets> <Manufacturing of bipolar current collectors> Step a: Polyethylene terephthalate (PET) particles are sprayed on the surface of the stainless steel substrate by electrostatic spraying method, and the thickness of the PET layer is 20 μm. Step b: The resulting PET layer is heated to 260° C. to soften it. Step c: A one-dimensional conductive material, multi-walled carbon nanotubes (MWCNTs), is implanted into the PET layer in a direction perpendicular to the surface of the PET layer by electrostatic implantation, and the PET layer is in a softened state by maintaining the temperature at 260° C. Here, the external electric field strength in the electrostatic implantation is 50 kV. Step d: Using electrostatic spraying, spray another layer of PET particles onto the surface of the conductive material implanted PET layer obtained in step c, and maintain the temperature at 260° C. so that the PET layer is in a softened state. Here, the thickness of the PET layer obtained after spraying again is 30 μm. Step e: The PET layer obtained in step d is pressed by a roll press under the condition of heating, in which the heating temperature is 270° C., so as to make the surface of the PET layer smooth and the thickness uniform. Step f: The PET layer obtained in step e was removed from the stainless steel substrate by a doctor blade and wound up to obtain a bipolar current collector, which has a conductive material orientation degree of 5°, a conductive material mass of 30% of the current collector mass, and a thickness of 20 μm.
[0083] <Production of negative electrode active material layer in bipolar electrode sheet> The negative active materials graphite, conductive carbon black (Super P), and styrene butadiene rubber (SBR) were mixed in a weight ratio of 96:1.5:2.5, and deionized water (H2O) was added as a solvent to prepare a slurry with a solid content of 70% and stirred uniformly. The slurry was uniformly applied to one side of a bipolar current collector and dried at 110°C to obtain a negative active material layer with a thickness of 130μm.
[0084] <Production of Positive Electrode Active Material Layer in Bipolar Electrode Sheet> The positive electrode active materials, lithium cobalt oxide (LiCoO2), conductive carbon black (Super P), and polyvinylidene fluoride (PVDF), were mixed in a weight ratio of 97.5:1.0:1.5, and N-methylpyrrolidone (NMP) was added as a solvent to prepare a slurry with a solid content of 75% and stirred uniformly. The slurry was uniformly applied to the other side of the bipolar current collector and dried at 90°C to obtain a positive electrode active material layer with a thickness of 110 μm.
[0085] After the above steps were completed, a bipolar electrode sheet was obtained, and the electrode sheet was cut to a specification of 41 mm x 61 mm.
[0086] <Production of negative electrode sheet> Negative electrode active materials graphite (Graphite), conductive carbon black (Super P), and styrene butadiene rubber (SBR) were mixed in a weight ratio of 96:1.5:2.5, and deionized water was added as a solvent to prepare a slurry with a solid content of 70%, which was then uniformly stirred. The slurry was uniformly applied to one side of a copper foil with a thickness of 10 μm, and dried at 110° C. to obtain a negative electrode sheet with a coating layer of 150 μm on one side coated with a negative electrode active material layer. The above coating step was then repeated on the other side of the negative electrode sheet to obtain a negative electrode sheet with a negative electrode active material layer on both sides. The negative electrode sheet was cut to a size of 41 mm x 61 mm and welded to a tab.
[0087] <Production of positive electrode sheets> The positive electrode active material lithium cobalt oxide (LiCoO2), conductive carbon black (Super P), and PVDF were mixed in a weight ratio of 97.5:1.0:1.5, and NMP was added as a solvent to prepare a slurry with a solid content of 75%, which was then stirred uniformly. The slurry was uniformly applied to one side of an aluminum foil with a thickness of 12 μm, and dried at 90°C to obtain a positive electrode sheet with a coating layer of 100 μm. The above steps were then repeated on the other side of the positive electrode sheet to obtain a positive electrode sheet with positive electrode active material layers applied on both sides. The positive electrode sheet was cut to a size of 38 mm x 58 mm and welded to a tab.
[0088] <Preparation of electrolyte> In a dry argon gas atmosphere, organic solvents ethylene carbonate (EC), methyl ethyl carbonate (EMC) and diethyl carbonate (DEC) were mixed in a mass ratio of 30:50:20, and lithium hexafluorophosphate (LiPF6) was dissolved in the organic solvent and mixed uniformly to obtain an electrolyte solution, where the molar concentration of LiPF6 in the electrolyte solution was 1.15 mol / L.
[0089] <Manufacturing of electrode assembly> <Manufacture of the first electrode assembly> A polyethylene (PE) film with a thickness of 15 μm was used as a separator, and a positive electrode sheet was placed on each side of a negative electrode sheet, with a separator placed between the positive electrode sheet and the negative electrode sheet to form a laminate. After that, the four corners of the entire laminate were fixed to obtain a first electrode assembly.
[0090] <Manufacture of the second electrode assembly> A polyethylene (PE) film with a thickness of 15 μm was used as a separator, and a negative electrode sheet was placed on each side of a positive electrode sheet, with a separator placed between the positive electrode sheet and the negative electrode sheet to form a laminate. After that, the four corners of the entire laminate were fixed to obtain a second electrode assembly.
[0091] <Manufacturing bipolar lithium-ion batteries> <Manufacture of bipolar electrode assembly> A 90 μm thick aluminum plastic film formed by pit punching was placed with the pit side facing up, and the first electrode assembly was placed in the pits of the aluminum plastic film with the positive electrode sheet facing up. Then, a bipolar electrode sheet was placed on top of the first electrode assembly with the negative electrode active material layer facing down, so that the positive electrode sheet of the first electrode assembly was aligned and pressed against the negative electrode active material layer of the bipolar electrode sheet to obtain a first assembly.
[0092] The second electrode assembly is placed on the bipolar electrode sheet with the negative electrode sheet facing down and the positive electrode active material layer of the bipolar electrode sheet of the first assembly facing up, so that the negative electrode sheet of the second electrode assembly is aligned with the positive electrode active material layer of the bipolar electrode sheet, and then another pit-punched aluminum plastic film with a thickness of 90 μm covers the second electrode assembly with the pit surface facing down, and the two aluminum plastic films are heat-sealed by a hot press, so that the first electrode assembly and the second electrode assembly are separated by the bipolar electrode sheet to obtain a bipolar electrode assembly. The bipolar electrode assembly has two independent chambers, where the first electrode assembly corresponds to the first chamber and the second electrode assembly corresponds to the second chamber.
[0093] <Injection and sealing of electrode assembly> The bipolar electrode assembly was sealed after injecting electrolyte into each of the two chambers. The positive electrode tab in the first chamber and the negative electrode tab in the second chamber were connected in series to conduct electricity, resulting in a bipolar lithium-ion battery. No ion exchange occurs between the two chambers of the bipolar lithium-ion battery.
[0094] Examples 2 to 3 The orientation of the conductive material is the same as in Example 1, except that it is 10° and 20°, respectively.
[0095] Example 4 The orientation degree of the conductive material is 30°, and the mass fraction of the conductive material with respect to the current collector is 10%, other than that, the same as in Example 1.
[0096] Example 5 The orientation degree of the conductive material is 3°, and the mass fraction of the conductive material with respect to the current collector is 70%, other than that, the same as in Example 1.
[0097] Example 6 The orientation degree of the conductive material is 3°, and the mass fraction of the conductive material with respect to the current collector is 10%, other than that, the same as in Example 1.
[0098] Example 7 The orientation degree of the conductive material is 30°, and the mass fraction of the conductive material with respect to the current collector is 70%, other than that, the same as in Example 1.
[0099] Example 8 The conductive material is the same as in Example 2, except that it is graphene.
[0100] Example 9 The conductive material is the same as in Example 2, except that it is VGCF.
[0101] Example 10 The polymer material is the same as in Example 2, except that it is polyethylene naphthalate (PEN).
[0102] Example 11 The polymer material is the same as in Example 2, except that it is polybutylene terephthalate (PBT).
[0103] Example 12 The thickness of the bipolar current collector is the same as in Example 2, except that it is 500 μm.
[0104] Example 13 The thickness of the bipolar current collector is the same as in Example 2, except that it is 2 μm.
[0105] Example 14 The thickness of the bipolar current collector is the same as in Example 2, except that it is 10 μm.
[0106] Example 15 The mass fraction of the conductive material relative to the current collector is 50%, but the same as in Example 14.
[0107] Example 16 The same as in Example 15, except that a negative electrode undercoat and a positive electrode undercoat are disposed on the bipolar electrode sheet.
[0108] <Production of negative electrode undercoat in bipolar electrode sheet> Conductive carbon black (Super P) and styrene butadiene rubber (SBR) were mixed in a weight ratio of 95:5, and deionized water (H2O) was added as a solvent to prepare a slurry with a solid content of 80%, which was then stirred uniformly. The slurry was evenly applied to one side of a bipolar current collector and dried at 110°C to obtain a negative electrode undercoat with a thickness of 5 μm.
[0109] <Production of negative electrode active material layer in bipolar electrode sheet> The negative electrode active materials graphite, conductive carbon black (Super P), and styrene butadiene rubber (SBR) were mixed in a weight ratio of 96:1.5:2.5, and deionized water (H2O) was added as a solvent to prepare a slurry with a solid content of 70%. The slurry was uniformly applied to the negative electrode undercoat and dried at 110°C to obtain a negative electrode active material layer with a thickness of 120μm.
[0110] <Production of Positive Electrode Undercoat in Bipolar Electrode Sheet> Conductive carbon black (Super P) and styrene butadiene rubber (SBR) were mixed in a weight ratio of 97:3, and deionized water (H2O) was added as a solvent to prepare a slurry with a solid content of 85%. The slurry was uniformly applied to the other side of the bipolar current collector and dried at 110°C to obtain a positive electrode undercoat.
[0111] <Production of Positive Electrode Active Material Layer in Bipolar Electrode Sheet> The positive electrode active materials, lithium cobalt oxide (LiCoO2), conductive carbon black (Super P), and polyvinylidene fluoride (PVDF), were mixed in a weight ratio of 97.5:1.0:1.5, and N-methylpyrrolidone (NMP) was added as a solvent to prepare a slurry with a solid content of 75%. The slurry was uniformly applied to the positive electrode undercoat and dried at 90°C to obtain a positive electrode active material layer with a thickness of 100 μm.
[0112] After the above steps were completed, a bipolar electrode sheet with a thickness of 245 μm was obtained. The electrode sheet was cut to a specification of 41 mm × 61 mm.
[0113] Example 17 The process was the same as in Example 16 except for the manufacturing process of the negative electrode undercoat and the positive electrode undercoat.
[0114] <Production of negative electrode undercoat in bipolar electrode sheet> Polypyrrole (PPy) and styrene butadiene rubber (SBR) were mixed in a weight ratio of 95:5, and deionized water (H2O) was added as a solvent to prepare a slurry with a solid content of 80%, which was then stirred uniformly. The slurry was uniformly applied to one side of a bipolar current collector and dried at 110°C to obtain a negative electrode undercoat with a thickness of 3 μm.
[0115] <Production of Positive Electrode Undercoat in Bipolar Electrode Sheet> Polypyrrole (PPy) and styrene butadiene rubber (SBR) were mixed in a weight ratio of 97:3, and deionized water (H2O) was added as a solvent to prepare a slurry with a solid content of 85%. The slurry was uniformly applied to the other side of the bipolar current collector and dried at 110°C to obtain a positive electrode undercoat.
[0116] Example 18 The process was the same as in Example 16 except for the manufacturing process of the negative electrode undercoat and the positive electrode undercoat.
[0117] <Production of negative electrode undercoat in bipolar electrode sheet> A single Cu plating layer was formed on one surface of the bipolar current collector by physical vapor deposition (PVD) to obtain a negative electrode undercoat having a thickness of 1 μm.
[0118] <Production of Positive Electrode Active Material Layer in Bipolar Electrode Sheet> A single layer of Al plating was formed on the other surface of the bipolar current collector by PVD to obtain a positive electrode undercoat having a thickness of 1 μm.
[0119] Example 19 The manufacturing process is the same as in Example 17 except for the bipolar lithium ion battery.
[0120] Bipolar Lithium-ion battery manufacturing process: The first bipolar electrode sheet, the first separator, the second bipolar electrode sheet, and the second separator were laminated in this order so that the positive electrode active material layer of the first bipolar electrode sheet was adjacent to the negative electrode active material layer of the second bipolar electrode sheet. Then, a seal adhesive was applied around the electrode sheets and an electrolyte injection port was previously installed. Next, the laminated electrode sheets and separator were wound around the electrode assembly. After the seal adhesive was solidified and the upper side was sealed, the electrolyte was injected into the electrode assembly. After the injection was completed, the previously installed electrolyte injection port was sealed, and a bipolar lithium-ion battery was obtained.
[0121] Comparative Example 1 The same as in Example 1 was used except that a Cu / Al composite current collector was used as the bipolar current collector.
[0122] The thickness of the Cu / Al composite current collector is 20 μm.
[0123] Comparative Example 2 The same as Example 1, except that a stainless steel current collector is used as the bipolar current collector.
[0124] The thickness of the stainless steel current collector is 20 μm.
[0125] Comparative Example 3 The bipolar current collector is the same as that in Example 1, except that it is obtained by compounding the zero-dimensional structure conductive material with the polymer substrate.
[0126] In the bipolar current collector, the conductive material with zero-dimensional structure is dot-shaped carbon black particles, the polymer substrate is a PET substrate, the dot-shaped carbon black particles are uniformly and non-orientedly dispersed on the substrate with a three-dimensional distribution, and the thickness of the bipolar current collector is about 50 μm.
[0127] Comparative Example 4 The bipolar current collector is the same as that in Example 1, except that it is obtained by compounding the conductive material with a one-dimensional structure with the polymer substrate.
[0128] In the bipolar current collector, the conductive material with one-dimensional structure is MWCNT, the polymer substrate is a PET substrate, the MWCNT is uniformly and non-orientedly dispersed in the substrate with a three-dimensional distribution, and the thickness of the bipolar current collector is about 50 μm.
[0129] Comparative Example 5 The bipolar current collector is the same as that in Example 1, except that it is obtained by compounding a two-dimensional conductive material with a polymer substrate.
[0130] In the bipolar current collector, the two-dimensional conductive material is graphene, the polymer substrate is a PET substrate, the graphene is uniformly and non-orientedly dispersed on the substrate with a three-dimensional distribution, and the thickness of the bipolar current collector is about 50 μm.
[0131] <Performance measurement> The bipolar current collectors and bipolar lithium ion batteries manufactured in each of the examples and comparative examples were measured using the following methods.
[0132] Measuring the degree of orientation of conductive materials in bipolar current collectors: A scanning electron microscope (SEM) cross-sectional image of the bipolar current collector was obtained, where the cross-section of the bipolar current collector was obtained by plasma cutting and polishing. Based on the image, the included angle between the fiber (one-dimensional conductive material) or nanosheet (two-dimensional conductive material) and the Z direction was measured, and in any image, at least half of the one-dimensional conductive material or the two-dimensional conductive material should meet the angle requirement.
[0133] Measurement of the electronic resistivity in the Z direction of a bipolar current collector: A bipolar current collector sample of 10 cm × 10 cm was obtained, and the A and B sides of the bipolar current collector were sandwiched between two metal clamps with fixed areas, the area of the clamps being equal to the area of the bipolar current collector, and a voltage of 0.1 V was applied between the two clamps, the current value between the two clamps was measured, the resistance value R was calculated, and the electronic resistivity was calculated according to the following formula ρ = RS / L, where R represents the resistance value, S represents the area of the bipolar current collector, and L represents the thickness of the bipolar current collector.
[0134] Measurement of electronic resistivity in the XY plane of a bipolar current collector: As shown in Figure 4, the electronic resistivity of the bipolar current collector in the XY plane direction was measured using the four-probe method. In the four-probe method, four metal probes are arranged in a line on the surface of the bipolar current collector and pressed against the sample surface with a certain pressure (usually 2N). The current I passing through the probes at two points a and d is measured, and the voltage difference V between probes b and c is measured. The electronic resistivity of the material is It was calculated using the formula ρ = C × V / I. Here, the probe coefficient C is calculated by the following formula: Formula 1
[0135] TIFF0007595085000001.tif52154, where the distances between probe a and probe b, between probe b and probe c, and between probe c and probe d are S1, S2, and S3, respectively. After obtaining the probe coefficient C, the electronic resistivity in the XY in-plane direction of the bipolar current collector can be obtained.
[0136] Measurement of the unidirectional conductance ratio of bipolar current collectors: Step A: As shown in Figure 5, two metal cylindrical electrodes with an area S (electrode 1 in the drawing, S is usually about 1 cm) are placed on opposite positions on both sides of the bipolar current collector sample. 2 ) and measure the impedance between the two electrodes using a multimeter, denoted as R0. Step B: Move one metal cylindrical electrode parallel to the sample by a distance L1 (the position of electrode 2 in the drawing) and use a multimeter to measure the impedance between the two electrodes, denoted as R01, where L1>2000H, H is the thickness of the sample. Step C: Continue translating the metal cylindrical electrode along the same direction as in step B by a distance L2 (the position of electrode 3 in the drawing), and use a multimeter to measure the impedance between the two electrodes, denoted as R2, where L2>4000H, H is the thickness of the sample, and L2-L1>2000H. Step D: The unidirectional conductivity ratio of the bipolar current collector was calculated based on the following formula: ((R2-R1)×H) / (R0×(L2-L1)).
[0137] Bipolar current collector thickness measurement: The thickness of the bipolar current collector was measured using a screw micrometer.
[0138] Measurement of tensile strength of bipolar current collector: The bipolar current collector samples were cut into small pieces of appropriate size (e.g., 100 mm x 10 mm) and the tensile strength of the samples was measured with a tensile tester. Determination of the mass fraction of conductive material in the current collector: The measurement can be carried out by employing Measurement Method 1 or Measurement Method 2.
[0139] Measurement method 1: A 10 cm x 10 cm bipolar current collector sample is weighed, and the weight at this time is M0. An appropriate solvent is selected to dissolve the polymer substrate in the bipolar current collector, and the conductive material particles therein are filtered. The solvent used is not particularly limited as long as it can dissolve the polymer substrate in the bipolar current collector. The filtered conductive material particles are washed, dried, and weighed, and the weight at this time is M1, in which case the mass fraction of the conductive material relative to the current collector is (M1 / M0) x %.
[0140] Measurement method 2: A 10cm x 10cm bipolar current collector sample is weighed, and the weight at this time is designated as M0. The conductive material in the bipolar current collector is dissolved in aqua regia, and the polymer substrate therein is filtered. The polymer substrate is washed, dried, and weighed, and the weight at this time is designated as M2. In this case, the mass fraction of the conductive material relative to the current collector is (M0-M2) / M0×%.
[0141] 02C discharge energy density measurement: The lithium ion battery in Comparative Example 1 was charged at 0.5C up to 4.45V, then charged at a constant voltage up to 0.025C, allowed to stand for 5 minutes, and then discharged at 0.2C down to 3.0V.
[0142] The lithium ion batteries in the other comparative examples and examples other than Comparative Example 1 were charged to 8.90V at 0.5C, then charged at a constant voltage to 0.025C, allowed to stand for 5 minutes, and then discharged to 6.0V at 0.2C.
[0143] The discharge energy density of 02C was calculated based on the following formula: energy density (Wh / kg) = discharge energy (Wh) / weight of electrochemical device (kg).
[0144] Cycle Measurement: For the lithium ion battery in Comparative Example 1, when the measurement temperature was 25°C, it was charged at a constant current of 0.5C up to 4.45V, charged at a constant voltage of 0.025C, allowed to stand for 5 minutes, and then discharged at 0.5C up to 3.0V. The capacity obtained at this stage was regarded as the initial capacity. Then, after 50 cycles of 0.5C charge / 0.5C discharge were performed, the ratio of the capacity of the lithium ion battery to the initial capacity was calculated.
[0145] For the lithium ion batteries in the other comparative examples and examples other than Comparative Example 1, when the measurement temperature was 25° C., they were charged at a constant current of 0.5 C to 8.9 V, charged at a constant voltage of 0.025 C, allowed to stand for 5 minutes, and then discharged at 0.5 C to 6.0 V. The capacity obtained at this stage was regarded as the initial capacity. Then, 50 cycles of 0.5 C charge / 0.5 C discharge were performed, and the ratio of the capacity of the lithium ion battery to the initial capacity was calculated.
[0146] Measurement of discharge energy density of 2C / 02C: First, the discharge energy density of 02C was measured using a method similar to that for measuring the discharge energy density of 02C described above, and then the discharge energy density of 2C was measured, and then the ratio of the discharge energy density of 2C to the discharge energy density of 02C was calculated.
[0147] The method for measuring the 2C discharge energy density is as follows. The lithium ion battery in Comparative Example 1 was charged at 0.5C up to 4.45V, then charged at a constant voltage up to 0.025C, and allowed to stand for 5 minutes, and then discharged at 2C down to 3.0V.
[0148] The lithium ion batteries in the other comparative examples and examples other than Comparative Example 1 were charged to 8.90V at 0.5C, then charged to 0.025C at a constant voltage, left to stand for 5 minutes, and then discharged to 6.0V at 2C.
[0149] The discharge energy density of 02C was calculated based on the following formula: energy density (Wh / kg) = discharge energy (Wh) / weight of electrochemical device (kg).
[0150] Nail penetration test: The lithium ion battery in Comparative Example 1 was charged at a constant current rate of 0.05C until the voltage reached 4.45V, at which point the rated voltage was reached. Thereafter, the battery was charged at a constant voltage until the current reached 0.025C, at which point the cut-off current was reached, indicating that the battery was in a fully charged state. The appearance of the battery before measurement was recorded.
[0151] For the lithium ion batteries in the comparative examples and examples other than Comparative Example 1, the lithium ion batteries to be measured were charged at a constant current rate of 0.05C until the voltage reached 8.90V, and then charged at a constant voltage until the current reached 0.025C, and the cut-off current was reached, which meant that the battery was in a fully charged state. The appearance of the battery before measurement was recorded.
[0152] The nail penetration test was performed on the battery in an environment of 25±3℃. The nail diameter was 4mm, the nail penetration speed was 30mm / s, and the nail penetration positions were 15mm from the edge of the electrochemical cell on the Al tab side and 15mm from the edge of the electrochemical cell on the Ni tab side, respectively. The nail penetration test was performed for 3.5min or when the surface temperature of the battery core dropped to 50℃, and the test was stopped. The condition of the batteries during the test was observed as one group of 10 lithium-ion batteries. The judgment criterion was that the battery did not burn or explode, and a pass rate of 90% or more indicates the pass of the nail penetration test.
[0153] The manufacturing parameters and measurement results for each of the examples and comparative examples are shown in Table 1 below.
[0154] [Table 1]
[0155] It is evident from Examples 1 to 19 and Comparative Examples 1 and 2 that the lithium ion battery including the bipolar current collector of the present invention exhibits a significantly improved 02C discharge energy density.
[0156] It is evident from Examples 1 to 19 and Comparative Examples 1 to 5 that the lithium ion battery including the bipolar current collector of the present invention exhibits a significantly improved cycle capacity retention rate.
[0157] From Examples 1 to 3, 5 to 11, 13 to 19 and Comparative Examples 3 to 5, it can be seen that lithium ion batteries equipped with the bipolar current collector of the present invention have significantly improved discharge energy density compared to lithium ion batteries equipped with conventional polymer bipolar current collectors (e.g., Comparative Examples 3 to 5).
[0158] From Examples 1 to 19 and Comparative Examples 1 and 2, it can be seen that lithium ion batteries equipped with the bipolar current collector of the present invention have significantly improved nail penetration pass rates compared to lithium ion batteries equipped with conventional metal foil bipolar current collectors (e.g., Comparative Examples 1 and 2).
[0159] From Example 4, it can be seen that the degree of orientation of the conductive material, the electronic resistivity in the Z direction of the bipolar current collector, and the mass fraction of the conductive material relative to the current collector together affect the discharge energy density of a lithium-ion battery.
[0160] From Examples 12 to 14, it can be seen that the thickness of the bipolar current collector affects the discharge energy density of the lithium ion battery. However, since the discharge energy density of Example 12 is close to the discharge energy densities of Comparative Examples 1 and 2, it can be seen that the thickness of the bipolar current collector does not have a large effect on the discharge energy density of the lithium ion battery.
[0161] Moreover, Examples 12-14 further show that as the thickness of the bipolar current collector increases, the number of lithium ion batteries that pass the nail penetration test increases.
[0162] As can be seen from Table 1, Example 17 is the optimal example, and Example 19 is designed based on a different electrode assembly structure from Example 17, and can also obtain similarly excellent performance.
[0163] The above is only a preferred embodiment of the present invention, and is not intended to limit the present invention. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principle of the present invention are included within the protection scope of the present invention.
Claims
1. A current collector comprising a polymeric substrate and a conductive material, the electronic resistivity of the current collector in the XY in-plane direction is 10 Ω cm to 1000 Ω cm, and the electronic resistivity of the current collector in the Z direction is 0.01 Ω cm to 30 Ω cm; The conductive material includes at least one of a one-dimensional conductive material and a two-dimensional conductive material, and an included angle between a length direction of the one-dimensional conductive material or a planar direction of the two-dimensional conductive material and a Z direction of a current collector is 0° to 30°; a ratio of electronic resistivity in the XY in-plane direction of the current collector to electronic resistivity in the Z direction of the current collector is 5 to 4000; the conductive material is a carbon material, The current collector, wherein the carbon material includes at least one of a single-walled carbon nanotube, a multi-walled carbon nanotube, a conductive carbon fiber, a conductive carbon black, a fullerene, a conductive graphite, and a graphene.
2. 2. The current collector of claim 1, wherein the weight of the conductive material is 10% to 70% of the weight of the current collector.
3. The current collector according to claim 1 , wherein the current collector has a thickness of 2 μm to 500 μm.
4. The current collector according to claim 1 , wherein one or both ends of the conductive material are exposed on a surface of the polymer substrate.
5. 2. The current collector of claim 1, wherein the one-dimensional conductive material has a length of 0.1 μm to 200 μm, a diameter of 2 nm to 500 nm, and a specific surface area of 5 m2 / g to 2000 m2 / g.
6. 2. The current collector according to claim 1, wherein the two-dimensional conductive material has a length of 2 μm to 10 μm, a thickness of 6 nm to 20 μm, and a specific surface area of 0.5 m2 / g to 1000 m2 / g.
7. The current collector is (a) the electronic resistivity of the current collector in the XY in-plane direction is 50 Ω cm to 1000 Ω cm; (b) the electronic resistivity in the Z direction of the current collector is 0.01 Ω cm to 1 Ω cm; (c) the ratio of the electronic resistivity in the XY in-plane direction of the current collector to the electronic resistivity in the Z direction of the current collector is 100 to 1000; (d) the angle between the conductive material and the Z direction is between 0° and 10°; (e) the thickness of the current collector is 5 μm to 50 μm; (f) the mass of the conductive material is 20% to 60% of the mass of the current collector; The current collector according to claim 1 , which satisfies at least one of the above.
8. The current collector is (a) the electronic resistivity of the current collector in the XY in-plane direction is 100 Ω cm to 1000 Ω cm; (b) the electronic resistivity in the Z direction of the current collector is 0.01 Ω cm to 0.05 Ω cm; (c) the ratio of the electronic resistivity in the XY in-plane direction of the current collector to the electronic resistivity in the Z direction of the current collector is 200 to 600; (d) the thickness of the current collector is 5 μm to 20 μm; (e) the mass of the conductive material is 40% to 50% of the mass of the current collector; (f) the tensile strength of the current collector is 80 MPa to 100 MPa; The current collector according to claim 1 , which satisfies at least one of the above.
9. The current collector according to claim 1, wherein the polymer substrate comprises at least one of polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyether ether ketone, polyimide, polyamide, polyethylene glycol, polyamideimide, polycarbonate, cyclic polyolefin, polyphenylene sulfide, polyvinyl acetate, polytetrafluoroethylene, polymethylene naphthalene, polyvinylidene fluoride, polyethylene naphthalate, polypropylene carbonate, poly(vinylidene fluoride-hexafluoropropylene), poly(vinylidene fluoride-co-chlorotrifluoroethylene), silicone resin, vinylon, polypropylene, polyethylene, polyvinyl chloride, polystyrene, polyether nitrile, polyurethane, polyphenylene ether, polysulfone, and derivatives thereof.
10. An electrochemical device comprising the current collector according to any one of claims 1 to 9.
11. An electronic device comprising the electrochemical device of claim 10.
Citation Information
Patent Citations
Bipolar battery
JP2007335206A
Current collector for bipolar secondary battery
JP2010170833A
Collector for bipolar battery
JP2010257712A
Collector for bipolar battery
JP2010277862A
Method for manufacturing collector
JP2012230916A