Method for producing chlorosilanes
By reacting silicon from solar cell modules with hydrogen chloride or tetrachlorosilane and hydrogen, the method simplifies the purification of recovered silicon for chlorosilanes, addressing the complexity of existing recycling methods and ensuring high-quality chlorosilane production.
Patent Information
- Application Number
- JP2024550847
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-06-09
- Filing Date
- 2024-05-21
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2044-05-21
AI Technical Summary
Existing methods for recycling silicon from solar cell modules require multiple purification steps to remove metal and organic impurities, making the process complex and inefficient.
A method is developed to produce chlorosilanes by reacting silicon sources, including polycrystalline and single crystal silicon recovered from solar cell modules, with hydrogen chloride or tetrachlorosilane and hydrogen, allowing impurities to be removed using conventional chlorosilane purification methods.
This approach enables the efficient reuse of recovered silicon as a raw material for chlorosilanes, simplifying the purification process and maintaining the quality of the produced chlorosilanes.
Smart Images

Figure 0007595232000001 
Figure 0007595232000002 
Figure 0007595232000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing chlorosilanes, and more particularly to a method for producing chlorosilanes including trichlorosilane by reacting a silicon source with hydrogen chloride or tetrachlorosilane and hydrogen. [Background technology]
[0002] Toward the realization of a low-carbon society, the reduction of CO2 emissions through the use of renewable energy sources such as solar power generation is accelerating. A typical solar cell module for solar power generation has a three-layer structure: a reinforced glass surface, a sealing resin layer on the inside, and a backsheet on the back. Solar cells made of single crystal or polycrystalline silicon are arranged inside the sealing resin layer and connected with electric wires (interconnectors). The sealing resin is required to have transparency, flexibility, adhesiveness, tensile strength, and weather resistance, and ethylene vinyl acetate copolymer (hereinafter abbreviated as "EVA") is generally used, which bonds the reinforced glass, cells, and backsheet by heating and pressurizing. While the introduction of solar power generation has progressed significantly, the issue of recycling solar cell modules when they are discarded has been pointed out.
[0003] When this solar cell module is heated in an electric furnace or the like under an oxidizing atmosphere, the EVA melts at 80 to 120° C., a deacetylation reaction of the EVA occurs at around 350° C., and a thermal decomposition reaction of the polyethylene portion of the main chain occurs rapidly at around 450° C. Technologies for recycling solar cell modules by such thermal decomposition have been disclosed (see Patent Documents 1 and 2).
[0004] Furthermore, in order to prevent the EVA contained in solar cell modules from burning too rapidly, a method has been proposed in which the resin components are burned slowly and steadily and removed, rather than lowering the oxygen concentration in the heating furnace, allowing valuable materials to be recovered efficiently and simply (see Patent Document 3).
[0005] By the above-mentioned method, resin components such as the back sheet and sealing resin layer can be removed from the solar cell module, and the glass, cells, aluminum frame, etc. can be separated and recovered. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Publication Publication No. 11-165150 [Patent Document 2] Japanese Patent Publication No. 2007-59793 [Patent Document 3] International Publication No. WO2020 / 031661 [Patent Document 4] Korean Patent Publication No. 20230033968 [Patent Document 5] China Patent Publication No. 115353111 Summary of the Invention [Problem to be solved by the invention]
[0007] The glass, aluminum frames, etc. recovered by the above method can be reused for solar cell modules and other uses. On the other hand, although the cells recovered by the above method are mainly composed of polycrystalline silicon or single crystal silicon, metal components such as wiring materials used to construct the solar cell module and resin components for adhesives are attached to them. Therefore, further purification measures are required to use the recovered cells as they are as materials for cells.
[0008] For example, a method has been proposed that includes a primary acid leaching step in which an acid leaching solution is added to crushed waste solar silicon to leach and stir impurities contained in the waste solar silicon (see Patent Document 4).In addition, a method has been proposed in which recovered solar panels are disassembled, immersed in an FeCl3 solution, pickled with hydrochloric acid, and a portion of the organic material is decomposed by heating at 330°C to 380°C, crushed into powder, purified by melting and refining, and then solidified to obtain regenerated silicon (see Patent Document 5).
[0009] These methods involve purifying silicon cells recovered from solar cell modules and reusing them for use in solar cell modules again, but they require numerous purification steps, and a simpler recycling method has been desired.
[0010] Therefore, an object of the present invention is to provide a simple method for reusing silicon cells recovered from solar cell modules. [Means for solving the problem]
[0011] The present inventors have conducted intensive research into the above-mentioned problem. As a result of analyzing impurities in polycrystalline silicon and single crystal silicon recovered from a solar cell module, metal components derived from wiring materials such as aluminum, and organic matter derived from resin were confirmed. Therefore, a method for reusing such polycrystalline silicon and single crystal silicon was investigated. As a result, it was found that it is possible to efficiently produce the chlorosilanes such as trichlorosilane by using silicon as a silicon source for obtaining chlorosilanes such as trichlorosilane by reacting silicon with hydrogen chloride or tetrachlorosilane with hydrogen. In addition, the obtained chlorosilanes had the same quality as those produced from metal silicon. Therefore, it was found that impurities derived from the polycrystalline silicon and single crystal silicon (metal impurities, carbon derived from resin) can be removed by a conventional method for purifying chlorosilanes, and the present invention was completed.
[0012] That is, a production method according to one aspect of the present invention is a production method for chlorosilanes in which a silicon source is reacted with hydrogen chloride, or with tetrachlorosilane and hydrogen, to produce chlorosilanes, wherein the silicon source contains at least one of monocrystalline silicon and polycrystalline silicon recovered from solar panels. Effect of the Invention
[0013] According to a manufacturing method of one aspect of the present invention, polycrystalline silicon and single crystal silicon recovered from a solar cell module can be efficiently used as a raw material (i.e., silicon source) for manufacturing chlorosilanes. In order to use the polycrystalline silicon and single crystal silicon for cells of a solar cell module, it is required to highly purify and remove metal components derived from wiring materials and organic substances derived from resins. On the other hand, in the present invention, after the chlorosilanes are produced, they can be removed by a known purification method, so that the polycrystalline silicon and single crystal silicon can be used as a silicon source for producing chlorosilanes without being highly purified. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] A manufacturing method according to one aspect of the present invention is a method for producing chlorosilanes by reacting a silicon source with hydrogen chloride or tetrachlorosilane and hydrogen to produce chlorosilanes, characterized in that the silicon source contains at least one of monocrystalline silicon and polycrystalline silicon recovered from a solar panel. As described above, silicon cells recovered from solar cell modules are mainly composed of polycrystalline silicon and monocrystalline silicon. On the other hand, polycrystalline silicon and monocrystalline silicon contain impurities such as metal components such as aluminum and organic components derived from resin materials, which are used as wiring materials. Therefore, when using the silicon cells as silicon for solar cell modules, it is necessary to remove these impurities to a high degree.
[0015] On the other hand, when producing polysilicon for semiconductors or solar cells, metallic silicon is converted to trichlorosilane by reacting it with hydrogen chloride or tetrachlorosilane and hydrogen. The trichlorosilane is then purified, and the purified trichlorosilane is reduced with hydrogen to obtain polysilicon. In addition, since the reaction between metallic silicon and hydrogen chloride produces tetrachlorosilane as a by-product in addition to trichlorosilane, the tetrachlorosilane is recovered and reacted with metallic silicon and hydrogen to produce trichlorosilane. Therefore, by using polycrystalline silicon or single crystal silicon recovered from solar cell modules instead of the metallic silicon, high-purity trichlorosilane can be obtained.
[0016] Metallic silicon contains metals such as iron, aluminum, or calcium, which act catalytically in the reaction of metallic silicon with hydrogen chloride or tetrachlorosilane and hydrogen, and have the effect of promoting the reaction. However, if these catalytic components are present in excess, they accumulate in the reaction vessel during the reaction, causing a decrease in the fluidity of the silicon source in the reaction vessel, or affecting the purification efficiency of chlorosilanes after the reaction. On the other hand, polycrystalline silicon or single crystal silicon recovered from a solar cell module contains aluminum derived from the wiring material on the surface, but does not contain iron or calcium, or the content is very low. Therefore, when polycrystalline silicon or single crystal silicon recovered from a solar cell module is used as a silicon source for producing trichlorosilane or the like without undergoing advanced purification, the accumulation of iron and calcium in the reaction vessel can be suppressed, and chlorosilanes can be produced stably for a long period of time.
[0017] In this specification, unless otherwise specified, the expression "A to B" for the numerical values A and B means "A or more and B or less." In such an expression, when a unit is added only to the numerical value B, the unit is also applied to the numerical value A. Hereinafter, a method for producing chlorosilanes according to one embodiment of the present invention will be described in detail.
[0018] <Method of producing chlorosilanes> In a method for producing chlorosilanes according to one embodiment of the present invention, a silicon source is reacted with hydrogen chloride to produce chlorosilanes. This production reaction is represented by the following formula (1); Si+3HCl → SiHCl3+H2(1) In addition, as a side reaction, the following reaction occurs: Si+4HCl → SiCl4+2H2(2) As shown in the above formula, tetrachlorosilane is produced as a by-product, and further, dichlorosilane is also produced as a by-product, although in a small amount.
[0019] On the other hand, tetrachlorosilane (SiCl4), a by-product of polysilicon production, is converted to trichlorosilane and reused in the production of polysilicon. In this production method, trichlorosilane is produced from metallic silicon, tetrachlorosilane, and hydrogen according to the following reaction formula (3). 3SiCl4+2H2+Si → 4SiHCl3(3) The method for producing chlorosilanes according to one embodiment of the present invention can be used in any of the above production methods.
[0020] <Silicon source> The manufacturing method according to one aspect of the present invention is characterized in that the silicon source contains at least one of monocrystalline silicon and polycrystalline silicon (hereinafter collectively referred to as "recovered silicon") recovered from solar panels. As a method for recovering monocrystalline silicon and polycrystalline silicon from solar panels, monocrystalline silicon and polycrystalline silicon recovered by a known method can be used. Among these, it is preferable to use polycrystalline silicon recovered from solar panels because of the reactivity of the reaction of chlorosilanes. Specific examples of the method for recovering monocrystalline silicon and polycrystalline silicon include the method described in Patent Document 3. The method described in Patent Document 3 is a method in which a waste solar panel containing monocrystalline silicon or polycrystalline silicon is heated to heat and melt the resin in the waste solar panel, the heat-melted resin is burned, and then monocrystalline silicon or polycrystalline silicon is recovered from the waste solar panel.
[0021] In addition, the recovered silicon contains impurities such as metal components such as aluminum, organic components derived from resin materials, etc., but in the manufacturing method according to one embodiment of the present invention, the recovered silicon containing impurities can be used as is. However, if the content of these impurities is too high, there is a risk that they cannot be sufficiently removed during purification operations after the reaction, so the content of at least one impurity in the recovered silicon is preferably any of the following. Note that the content in the following description is the content per 100 parts by mass of at least one of the recovered silicon.
[0022] Aluminum: preferably from 50 to 3,000,000 ppm by mass, more preferably from 50 to 300,000 ppm by mass, even more preferably from 50 to 10,000 ppm by mass, and particularly preferably from 50 to 1,000 ppm by mass. Iron: preferably 100 ppm by mass or less, more preferably 50 to 90 ppm by mass, and particularly preferably 60 to 90 ppm by mass. · Calcium: preferably 100 ppm by mass or less, more preferably 1 to 90 ppm by mass, and particularly preferably 1 to 80 ppm by mass. Carbon: preferably 500 ppm by mass or less, more preferably 1 to 300 ppm by mass, and particularly preferably 1 to 100 ppm by mass.
[0023] The metal components of the silicon source or the recovered silicon, i.e., aluminum, iron, and calcium, can be measured by X-ray fluorescence spectrometry (XRF). In addition, for the low concentration range of the above metal elements (100 mass ppm or less), the silicon source can be dissolved in fluoronitric acid, and the filtrate can be measured by inductively coupled plasma optical emission spectrometry (ICP-OES). The carbon content of the silicon source or the recovered silicon can be determined by measuring CO and CO2 by the combustion-infrared absorption method.
[0024] When the content of the above-mentioned impurities in the recovered silicon is too high, for example, the surface of the recovered silicon recovered from waste solar panels may be washed with an acid such as hydrochloric acid, nitric acid, sulfuric acid, hydrofluoric acid, etc., or an alkali such as sodium hydroxide, potassium hydroxide, etc. After the washing, the impurities can be reduced to a desired range by washing with pure water and drying.
[0025] When the recovered silicon is used as a silicon source, the particle size is not particularly limited. From the viewpoint of reactivity with hydrogen chloride or tetrachlorosilane and hydrogen, the particle size is preferably 30 to 2000 μm, more preferably 50 to 1000 μm, and particularly preferably 50 to 500 μm.
[0026] In the manufacturing method according to one aspect of the present invention, the silicon source may contain at least one of the above recovered silicons, and the entire amount of the silicon source may be the recovered silicon. The recovered silicon may be a combination of the above-mentioned washed recovered silicon and unwashed recovered silicon. Alternatively, the recovered silicon may be mixed with metal silicon described below. As described above, in the reaction between metal silicon and hydrogen chloride, or between tetrachlorosilane and hydrogen, metal components such as iron, aluminum, and calcium act catalytically and have the effect of promoting the reaction. Therefore, when using these as the silicon source, the content of metal components such as iron, aluminum, and calcium in the silicon source may be appropriately adjusted. Specifically, when the recovered silicon is mixed with metal silicon described below and used, the content of recovered silicon in 100 parts by mass of the silicon source is preferably 1 to 99 parts by mass, more preferably 50 to 99 parts by mass, and particularly preferably 80 to 95 parts by mass.
[0027] <Metal silicon> The metal silicon used in the above reaction may be any known metal silicon produced by metallurgy or ferrosilicate, without any restrictions. The metal silicon may also contain impurities such as iron compounds, without any particular restrictions on their content. Such metal silicon is usually used in the form of a fine powder having an average particle size of about 100 to 500 μm.
[0028] <Hydrogen chloride> The hydrogen chloride used in the reaction with the silicon source may be contaminated with hydrogen or the like without any restrictions. However, in general, chlorosilanes such as trichlorosilane, tetrachlorosilane, and dichlorosilane are highly hydrolyzable and react with moisture. Therefore, if the hydrogen chloride contains moisture, the yield of the generated trichlorosilane may decrease. Therefore, it is preferable that the hydrogen chloride is in a dry state.
[0029] <Hydrogen> The hydrogen used in the reaction with the silicon source is not particularly limited, and may be pure hydrogen, or hydrogen recovered after the reaction of the silicon source with hydrogen chloride, or tetrachlorosilane and hydrogen, etc. As with the hydrogen chloride, it is preferable that the hydrogen be in a dry state.
[0030] <Reaction of silicon source with hydrogen chloride or tetrachlorosilane and hydrogen> In order to efficiently produce trichlorosilane, it is preferable to use a catalyst in the reaction between a silicon source and hydrogen chloride or between tetrachlorosilane and hydrogen. As the catalyst, any known catalyst component in the reaction between a silicon source and hydrogen chloride or between tetrachlorosilane and hydrogen can be used without any particular limitation.
[0031] Specific examples of such catalyst components include metals of Groups 8 to 10 such as aluminum, iron, and calcium, or their chlorides, and metals or chlorides such as copper and titanium. These catalysts can be used alone or in combination with one another. The amount of the catalyst components used is not particularly limited as long as it is an amount that efficiently produces trichlorosilane, and may be appropriately determined taking into account the capacity of the production equipment. In general, it is sufficient to use 0.05 to 40% by weight, particularly 0.1 to 5% by weight, calculated as the metal element, based on the metal silicon.
[0032] As described above, the recovered silicon contains aluminum, and when metal silicon is mixed and used, the metal silicon contains aluminum, iron, and calcium. Therefore, in the production method according to one aspect of the present invention, it is preferable to mix and use the catalyst components in the silicon source so that the content of the catalyst components falls within the following range. The content in the following description is the content per 100 parts by mass of the silicon source.
[0033] Aluminum: preferably from 50 to 20,000 ppm by mass, more preferably from 500 to 10,000 ppm by mass, and particularly preferably from 600 to 6,000 ppm by mass. Iron: preferably from 50 to 10,000 ppm by mass, more preferably from 50 to 5,000 ppm by mass, and particularly preferably from 1,000 to 3,000 ppm by mass. · Calcium: preferably from 50 to 5000 ppm, more preferably from 50 to 3000 ppm by mass, and particularly preferably from 50 to 500 ppm by mass.
[0034] As described above, the content of metal components, i.e., aluminum, iron, and calcium, in the silicon source or recovered silicon can be measured by X-ray fluorescence spectrometry (XRF). For the low concentration range of the above metal elements (100 mass ppm or less), the silicon source can be dissolved in fluoronitric acid, and the filtrate can be measured by inductively coupled plasma optical emission spectrometry (ICP-OES). The carbon content of the silicon source or recovered silicon can be determined by measuring CO and CO2 by the combustion-infrared absorption method.
[0035] The above catalyst components may be present in the reaction system by being added thereto, but when the silicon source used contains catalyst components such as aluminum, iron, calcium, etc. as impurities, the impurities can be effectively used as catalyst components. Of course, even when metal silicon containing catalyst components as impurities is used, there is no problem in further adding catalyst components to the reaction system in order to increase the reactivity of the silicon source with hydrogen chloride, or tetrachlorosilane and hydrogen.
[0036] In the reaction of the silicon source with hydrogen chloride or tetrachlorosilane and hydrogen, a known reactor can be used without any particular limitation. Specific examples of such a reactor include a fixed bed reactor and a fluidized bed reactor. Among the above reactors, a fluidized bed reactor is preferred because it is possible to continuously supply the silicon source and hydrogen chloride, or tetrachlorosilane and hydrogen, and continuously produce trichlorosilane. In addition, since the above reaction is an exothermic and endothermic reaction, it is also preferred to use a fluidized bed reactor from the viewpoint of uniform temperature distribution in the reaction region.
[0037] The reaction temperature in the reaction between the silicon source and hydrogen chloride, or between tetrachlorosilane and hydrogen may be appropriately determined taking into consideration the material and capacity of the production equipment. If the reaction temperature is higher than necessary, the selectivity of trichlorosilane decreases, and the amount of by-products of chlorosilanes other than trichlorosilane, such as tetrachlorosilane and dichlorosilane, increases. The reaction between the silicon source and hydrogen chloride is an exothermic reaction, and the reaction temperature is generally set in the range of 250 to 400°C.
[0038] On the other hand, the reaction between the silicon source and tetrachlorosilane and hydrogen is an endothermic reaction, and the reaction temperature is generally set in the range of 400 to 700°C, particularly 450 to 600°C.
[0039] <Condensation separation and distillation of chlorosilanes> The reaction of the silicon source with hydrogen chloride or tetrachlorosilane and hydrogen generates a reaction product gas containing trichlorosilane. This reaction product gas contains by-product chlorosilanes other than trichlorosilane, such as tetrachlorosilane or dichlorosilane, and further contains by-product hydrogen and boron and the like contained as unavoidable impurities in the silicon source.
[0040] Therefore, when recovering trichlorosilane from the reaction product gas, the reaction product gas may first be passed through an appropriate filter to remove solid matter such as silicon source particles, and then subjected to condensation and separation. Chlorosilanes including trichlorosilane are condensed and separated from the reaction product gas after passing through the filter.
[0041] In this condensation separation step, the reaction product gas is cooled, and the cooling temperature may be equal to or lower than the temperature at which various chlorosilanes condense, and may be appropriately determined taking into consideration the cooling capacity of the cooling device, etc. The lower the cooling temperature, the greater the effect of removing chlorosilanes tends to be, but generally, -10°C or lower, and particularly -30°C or lower, is sufficient. The pressure in the condensation separation is also not particularly limited as long as the chlorosilanes can be sufficiently removed, and may be appropriately determined taking into consideration the capacity of the condensation removal device, etc., and generally, 300 kPaG or higher, and particularly 500 kPaG or higher, is sufficient.
[0042] The cooling means for condensation is not particularly limited, and any known cooling means can be used as long as it can cool the reaction product gas to the above-mentioned cooling temperature. Specific examples of such cooling means include cooling means for passing the reaction product gas through a cooled heat exchanger to cool it, or cooling means for cooling the reaction product gas by a condensate that has been condensed and cooled. These methods can be used alone or in combination.
[0043] Furthermore, in order to increase the pressure of the gas, a pressurizer may be installed prior to the condensation and removal of chlorosilanes. In order to protect the pressurizer, a preliminary chlorosilane condenser or filter may be installed upstream of the pressurizer. These points can be adopted as standard practice in industrial process design.
[0044] The condensate obtained from the reaction product gas by the above-mentioned condensation separation is a mixture of various chlorosilanes, and trichlorosilane is isolated by distillation. The recovered trichlorosilane is used as a deposition raw material in the process of producing polysilicon.
[0045] Furthermore, the exhaust gas after condensation and separation of chlorosilanes contains hydrogen gas as a main component and can be used as a hydrogen source for various production processes such as hydrogen production in the production of the above-mentioned chlorosilanes.
[0046] 〔summary〕 A method for producing chlorosilanes according to a first aspect of the present invention is a method for producing chlorosilanes by reacting a silicon source with hydrogen chloride, or tetrachlorosilane and hydrogen, to produce chlorosilanes, wherein the silicon source contains at least one of monocrystalline silicon and polycrystalline silicon recovered from solar panels.
[0047] In the method for producing chlorosilanes according to aspect 2 of the present invention, in the above-mentioned aspect 1, the content of at least one of the monocrystalline silicon and polycrystalline silicon in 100 parts by mass of the silicon source is preferably 1 to 99 parts by mass.
[0048] In the method for producing chlorosilanes according to a third aspect of the present invention, in the above-mentioned first or second aspect, the content of aluminum in 100 parts by mass of the silicon source is preferably 50 to 20,000 ppm by mass.
[0049] In the method for producing chlorosilanes according to a fourth aspect of the present invention, in any one of the first to third aspects, the content of iron in 100 parts by mass of the silicon source is preferably 50 to 10,000 ppm by mass.
[0050] In the method for producing chlorosilanes according to a fifth aspect of the present invention, in any one of the first to fourth aspects, the calcium content in 100 parts by mass of the silicon source is preferably 50 to 5000 ppm by mass.
[0051] A sixth aspect of the present invention relates to a method for producing chlorosilanes, and in any one of the first to fifth aspects, the carbon content in 100 parts by mass of the silicon source is preferably 10 to 10,000 ppm by mass.
[0052] In the method for producing chlorosilanes according to Aspect 7 of the present invention, in any one of Aspects 1 to 6, the silicon source preferably has an aluminum content of 50 to 300,000 ppm by mass per 100 parts by mass of at least one of the monocrystalline silicon and polycrystalline silicon.
[0053] In the method for producing chlorosilanes according to an eighth aspect of the present invention, in any one of the first to seventh aspects, the silicon source preferably has an iron content of 100 ppm by mass or less per 100 parts by mass of at least one of the monocrystalline silicon and polycrystalline silicon.
[0054] A ninth aspect of the present invention relates to the method for producing chlorosilanes, and in any one of the first to eighth aspects, the silicon source preferably has a calcium content of 100 ppm by mass or less per 100 parts by mass of at least one of the monocrystalline silicon and polycrystalline silicon.
[0055] In the method for producing chlorosilanes according to Aspect 10 of the present invention, in any one of Aspects 1 to 9, the carbon content per 100 parts by mass of at least one of the monocrystalline silicon and polycrystalline silicon in the silicon source is preferably 500 ppm by mass or less.
[0056] In the method for producing chlorosilanes according to an eleventh aspect of the present invention, in any one of the first to tenth aspects, the single crystal silicon and polycrystalline silicon recovered from the solar panels preferably include single crystal silicon or polycrystalline silicon recovered from the solar panels, and the surface of the obtained single crystal silicon or polycrystalline silicon washed with an acid. EXAMPLES
[0057] The present invention will be further described below with reference to examples, but the present invention is not limited to these examples in any way.
[0058] <Silicon source> In the following examples, the following silicon sources were used: Unwashed recovered silicon: The resin in a waste solar panel containing single crystal silicon is melted by heating the waste solar panel, and the melted resin is then burned and recovered from the waste solar panel. Washed and recovered silicon: The unwashed recovered silicon was immersed in 35% hydrochloric acid for 1 hour and then dried. Metallic silicon: commercially available Silicon iron: commercially available Silicon copper: A mixture of commercial products and metallic silicon
[0059] The aluminum, iron, calcium, and copper contents in each silicon source were measured by X-ray fluorescence spectrometry (XRF) (ZSX PrimusIV (Rigaku Corporation)). The low concentration range of the above metal elements (100 mass ppm or less) was measured by high-frequency inductively coupled plasma optical emission spectrometry (ICP-OES) (Optima8300 (PerkinElmer Corporation)). The carbon content was determined by measuring CO and CO2 using a combustion-infrared absorption method (EMIA-110 (Horiba, Ltd.)). The contents of each element in each silicon source are shown in Table 1.
[0060] [Table 1]
[0061] <Reaction of silicon source with hydrogen chloride> A SUS reaction tube with an inner diameter of 8 mm was filled with 10 g of silicon source, and the reactor was maintained at 350°C. Hydrogen chloride gas and hydrogen gas were then continuously fed into the reactor at 50 ml / min each for 250 min. The exhaust gas from the reactor was cooled to -70°C to obtain a coolant.
[0062] The supply of hydrogen chloride gas and hydrogen gas was stopped, the temperature was lowered, the reaction residue was removed from the reactor and weighed, and the reaction rate (%) of the silicon source in Table 2 was calculated from the amount of the silicon source charged in the reactor using the following formula. Reaction rate=((amount of silicon source charged)-(amount of reaction residue)) / (amount of silicon source charged)×100
[0063] After the reaction was completed, the reaction residue was visually observed to confirm the presence or absence of silicon lumps with a particle size of 1 mm or more. The methyldichlorosilane (MDCS) content of the above obtained coolant was measured by gas chromatography. The remaining silicon lumps, which are agglomerations of silicon reaction residue, indicate a deterioration in fluidity and reactivity in the reactor during long-term operation.
[0064] <Example 1> The above production was carried out using a mixture of 98 parts by mass of washed recovered silicon and 2 parts by mass of unwashed recovered silicon as the silicon source. As a result, the reaction rate was 16% and almost no silicon lumps were observed. The methyldichlorosilane content was 0.3 ppma. Table 2 shows the iron, calcium, aluminum, and carbon contents of the silicon source used, the reaction rate, the presence or absence of silicon lumps, and the MDCS content.
[0065] <Examples 2 to 5, Comparative Example 1> The production was carried out in the same manner as in Example 1, except that the silicon source shown in the table was used in the amount shown in Table 2. The reaction rate and the MDCS content are shown as relative values, with the result of Example 1 being set at 1. The results are shown in Table 2. Even when recovered silicon was used, the reaction rate could be improved to the same level as when metal silicon was used by adjusting the impurity content. On the other hand, since recovered silicon has a lower calcium content than metal silicon, it is presumed that the amount of silicon chunks that cause poor flow is smaller. Furthermore, recovered silicon also has a lower carbon content than metal silicon, so the amount of carbon-derived MDCS produced is also smaller, and chlorosilanes of higher purity are obtained.
[0066] [Table 2]
[0067] <Reaction of silicon source with tetrachlorosilane and hydrogen> A SUS reaction tube with an inner diameter of 8 mm was filled with 3.0 g of silicon source, and the reactor was maintained at 530°C. Tetrachlorosilane gas and hydrogen gas were then continuously fed into the reactor at 40 ml / min and 110 ml / min, respectively, for 300 min. The exhaust gas from the reactor was cooled to -70°C to obtain a coolant.
[0068] The supply of tetrachlorosilane gas and hydrogen gas was stopped, the temperature was lowered, the reaction residue was removed from the reactor and weighed, and the reaction rate (%) of the silicon source in Table 3 was calculated from the amount of silicon source charged into the reactor using the following formula. Reaction rate=((amount of silicon source charged)-(amount of reaction residue)) / (amount of silicon source charged)×100
[0069] <Example 6> The above production was carried out using a mixture of 98 parts by mass of washed and recovered silicon and 2 parts by mass of unwashed and recovered silicon as the silicon source. As a result, the reaction rate was 0.14%, which was almost no reaction. Table 3 shows the contents and reaction rates of iron, calcium, aluminum, carbon, and copper in the silicon source used.
[0070] <Examples 7 to 8, Comparative Examples 2 to 3> Production was carried out in the same manner as in Example 6, except that the silicon source shown in Table 3 was used in the amount shown in Table 3. The reaction rate is shown as a relative value, with the result of Example 6 taken as 1. The results are shown in Table 3. Even when recovered silicon was used, the reaction rate could be improved to the same level as when metallic silicon was used by adjusting the impurity content.
[0071] [Table 3]
Claims
1. A method for producing chlorosilanes, comprising reacting a silicon source with hydrogen chloride or tetrachlorosilane and hydrogen to produce chlorosilanes, the method comprising the steps of: The method for producing chlorosilanes, wherein the silicon source contains at least one of single crystal silicon and polycrystalline silicon recovered from a solar panel.
2. 2. The method for producing chlorosilanes according to claim 1, wherein the content of at least one of the single crystal silicon and the polycrystalline silicon is 1 to 99 parts by mass per 100 parts by mass of the silicon source.
3. 3. The method for producing chlorosilanes according to claim 1, wherein the content of aluminum in 100 parts by mass of the silicon source is 50 to 20,000 ppm by mass.
4. 3. The method for producing chlorosilanes according to claim 1, wherein the content of iron in 100 parts by mass of the silicon source is 50 to 10,000 ppm by mass.
5. 3. The method for producing chlorosilanes according to claim 1, wherein the calcium content in 100 parts by mass of the silicon source is 50 to 5,000 ppm by mass.
6. 3. The method for producing chlorosilanes according to claim 1, wherein the carbon content in 100 parts by mass of the silicon source is 10 to 10,000 ppm by mass.
7. 3. The method for producing chlorosilanes according to claim 1, wherein the silicon source has an aluminum content of 50 to 300,000 ppm by mass per 100 parts by mass of at least one of the single crystal silicon and polycrystalline silicon.
8. 3. The method for producing chlorosilanes according to claim 1, wherein the silicon source has an iron content of 100 ppm by mass or less per 100 parts by mass of at least one of the single crystal silicon and the polycrystalline silicon.
9. 3. The method for producing chlorosilanes according to claim 1, wherein the silicon source has a calcium content of 100 ppm by mass or less per 100 parts by mass of at least one of the single crystal silicon and the polycrystalline silicon.
10. 3. The method for producing chlorosilanes according to claim 1, wherein the silicon source has a carbon content of 500 ppm by mass or less per 100 parts by mass of at least one of the single crystal silicon and the polycrystalline silicon.
11. The monocrystalline silicon and polycrystalline silicon recovered from the solar panels are Recovering single crystal silicon or polycrystalline silicon from the solar panel; 3. The method for producing chlorosilanes according to claim 1, further comprising washing the surface of the obtained single crystal silicon or polycrystalline silicon with an acid.
Citation Information
Patent Citations
Method for recycling the carbon-chuck for manufacture of polycrystalline silicon
CN103303925A
Method for producing silicon for solar cell
JP2011068520A
Recovery of silicon from KERF silicon waste
US20100032630A1
Method for producing polycrystalline silicon
WO2018131500A1
Silicon granules for the preparation of trichlorosilane and associated production method
WO2019122567A1