Zeolite dense body and method for producing same

The hydrothermal hot press method transforms zeolite powder into a dense bulk body with high ionic conductivity, addressing sintering challenges and environmental concerns, suitable for advanced batteries and sensors.

JP7595263B2Active Publication Date: 2024-12-06NAT UNIV CORP KUMAMOTO UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020213207
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-27
Filing Date
2020-12-23
Publication Date
2024-12-06
Estimated Expiration
2040-12-23

AI Technical Summary

Technical Problem

Existing zeolite powders are difficult to sinter into dense bulk bodies, limiting their ionic conductivity and requiring costly, environmentally harmful materials, and existing solid electrolytes have insufficient conductivity for advanced batteries.

Method used

A hydrothermal hot press method is used to solidify zeolite powder, creating a dense zeolite bulk body with high ionic conductivity using abundant and inexpensive elements, maintaining the zeolite skeleton structure and forming a good ion conduction path.

Benefits of technology

The method produces a zeolite dense body with ionic conductivity of 1.0×10^-3 S cm^-1, reducing environmental impact and manufacturing costs, suitable for next-generation batteries and chemical sensors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007595263000007
    Figure 0007595263000007
  • Figure 0007595263000008
    Figure 0007595263000008
  • Figure 0007595263000009
    Figure 0007595263000009
Patent Text Reader

Abstract

To provide a zeolite dense body that achieves high ion conductivity, a low environment load, and a low production cost.SOLUTION: A zeolite dense body has an ion conductivity of 1.0×10-3S cm-1 or higher and is represented by the following general formula (1) (M1 / n)x(AlxSiyO2(x+y)) zH2O, where M is one or two or more kinds of metal elements selected from Na, Li, K, Ca, Mg, Ba, and Ag, 0≤x≤y, 0≤z≤216, and n is a valence.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a zeolite dense body and a method for producing the same, and more particularly to a zeolite dense body having high ionic conductivity in the form of a bulk body. [Background technology]

[0002] Zeolites are generally used in catalysts, adsorbents, etc. for the purposes of petroleum reforming, purification of exhaust gas generated from internal combustion engines, synthesis of hydrocarbons, etc. Zeolites are often used in the form of powder in catalysts and adsorbents, and many patent applications also contain descriptions of zeolites in the form of powder and their chemical properties.

[0003] For example, a catalyst for purifying exhaust gas has been proposed (Patent Document 1), which contains a zeolite powder containing an 8-membered ring zeolite carrying a transition metal, and in which the molar ratio of the amount of Al constituting the zeolite skeleton to the amount of Al in the zeolite powder (hereinafter also referred to as the Al ratio) is 0.70 or more. In the examples of Patent Document 1, it is said that when the Al ratio of the zeolite powder is 1.06, the purification rate of nitrogen oxides (NO) is high, and high initial catalytic activity and high catalytic activity retention rate can be achieved.

[0004] On the other hand, ion-conducting materials play an important role in electrochemical devices such as various batteries and chemical sensors. For example, a lithium-ion secondary battery is composed of a solid electrolyte material that exhibits lithium ion conductivity and a pair of electrodes. Therefore, the performance of a lithium-ion secondary battery is strongly governed by the ion conductivity of the solid electrolyte material.

[0005] Solid electrolytes used in various batteries and chemical sensors have an average capacitance of 1.0×10 -3 S cm -1 ~1.0×10 -2 S cm -1 However, for example, in a lithium-ion solid-state battery, the ionic conductivity is about one order of magnitude lower than the above range, at 10 -5 ~10-3 At present, applied research is being conducted on ion conductivity on the order of 100 nm. For example, as a solid electrolyte membrane for a conventional lithium-ion secondary battery, a solid electrolyte membrane made of zeolite in which the total content of carbon and nitrogen elements in the zeolite is less than 1 mass % has been proposed (Patent Document 2). In an example of Patent Document 2, AC impedance was measured at 27°C, and the lithium ion conductivity calculated from the resistance value obtained by Cole-Cole plotting was 7.0×10 -4 S cm -1 (Patent Document 2). In addition, as a solid electrolyte for conventional lithium-ion all-solid-state batteries, a sulfide-based inorganic solid electrolyte material containing Li, P, S, and M as constituent elements, where M is one or more elements selected from Fe, Co, and Zn, has been proposed (Patent Document 3). In an example of this Patent Document 3, the lithium ion conductivity of the inorganic solid electrolyte material measured by an AC impedance method under measurement conditions of 27.0°C, an applied voltage of 10 mV, and a measurement frequency range of 0.1 Hz to 7 MHz is 1.4 × 10 -3 S cm -1 It is said to be the case. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2019-171243 A [Patent Document 2] JP 2018-198128 A [Patent Document 3] JP 2019-071235 A Summary of the Invention [Problem to be solved by the invention]

[0007] However, in the above Patent Document 1, zeolite is a powder, and unlike general ceramics, it cannot be sintered, so it is extremely difficult to prepare a dense bulk body. In addition, there is no disclosure or suggestion about the electrical properties of zeolite powder, especially the ionic conductivity of zeolite powder. In addition, several research examples that have examined the ionic conductivity of zeolite have been reported, but in these research examples, a compact of zeolite powder is actually used. In the case of a compact, the bonding between the zeolite powder particles is weak, making it difficult to form a good ionic conduction path, so that even if the zeolite powder itself is a substance that exhibits high ionic conductivity, it is not possible to exhibit high ionic conductivity.

[0008] In Patent Document 2, the lithium ion conductivity is 10 -4 However, the value of the ion conductivity is not sufficient, and there is room for improvement. In addition, in the example of Patent Document 3, the lithium ion conductivity is 10 -3 Although it is disclosed that the order is 100%, the constituent elements of the inorganic solid electrolyte material, Li, P, S, Fe, Co, and Zn, are all metal species with small Clarke numbers, and obtaining the metal species that are the materials for the solid electrolyte imposes a large environmental burden and increases the manufacturing cost. With the further development of the automobile industry, communication equipment industry, and other industries that require batteries, there is a demand for inorganic solid electrolyte materials with higher ionic conductivity and less environmental burden.

[0009] An object of the present invention is to provide a dense zeolite body which exhibits high ionic conductivity, has a small environmental impact, and can reduce production costs, and a method for producing the same. [Means for solving the problem]

[0010] As a result of intensive research, the inventors of the present invention have found that by using zeolite powder, which is composed of inexpensive and abundant elements, and by hydrothermally solidifying the zeolite powder using a hydrothermal hot pressing method in which a hydrothermal reaction process and a pressurization process are performed simultaneously, a very dense zeolite bulk body with very few gaps between particles while maintaining the zeolite framework structure can be obtained. As a result, -2It was found that the zeolite exhibits extremely high ionic conductivity of the order of 100 nm. In addition, the zeolite framework is composed of elements with extremely large Clarke numbers, such as silicon (Si), aluminum (Al), and oxygen (O) (O, Si, and Al are the top three elements with Clarke numbers), and is therefore abundant as a resource, making it extremely inexpensive and environmentally friendly. By applying the zeolite dense body of the present invention to devices in various industrial fields, it is possible to reduce the environmental load and also reduce manufacturing costs.

[0011] In particular, if zeolites, whose main application areas have previously been thought of as catalysts and adsorbents, are applied as dense zeolite bodies to batteries and other electrochemical devices, the impact on industry will be enormous.

[0012] In addition, from the viewpoint of energy diversification, many companies, including automobile companies, are competing to develop next-generation batteries such as metal-air batteries in addition to lithium-ion secondary batteries. These include sodium metal-air batteries and magnesium metal-air batteries. One of the major features of zeolite is that it can incorporate various mobile metal elements (cation species) into its structure through ion exchange reactions. Usually, when introducing a different element into a base material such as a metal, the element species that can be introduced are limited. In contrast, zeolite exhibits unique chemical properties such as ion exchangeability, so that various mobile metal elements can be introduced into its framework structure. This ion exchangeability property is a great attraction in the development of metal-air batteries. In other words, it becomes possible to appropriately control the mobile metal species in accordance with the reaction of the metal-air battery, making it possible to provide a metal-air battery with a high degree of design freedom. In addition, zeolite has the electrical insulation required for a solid electrolyte due to its structure. Therefore, the zeolite dense body of the present invention, which has extremely high ionic conductivity, is also very useful as a solid electrolyte for next-generation batteries such as metal-air batteries.

[0013] That is, the gist and configuration of the present invention are as follows.

[0014] [1] Represented by the following general formula (1), the ionic conductivity is 1.0 × 10 -3 S cm -1 That is all of the zeolite dense body. (M 1 / n ) x (Al x S y O 2(x+y) )·zH2O···(1) Here, M is one or more metal elements selected from Na, Li, K, Ca, Mg, Ba, and Ag, 0≦x≦y, 0≦z≦216, and n is a valence number.

[0015] [2] The zeolite dense body according to the above [1], having a relative density measured based on theoretical density and bulk density of 80% or more.

[0016] [3] Bulk density: 1.7 g / cm 3 More than 2.0g / cm 3 The zeolite dense body according to the above [1] or [2], which is:

[0017] [4] Log(σ / S cm) calculated from ionic conductivity at room temperature or higher and 150°C or lower -1 ) is -3 or more.

[0018] [5] The zeolite dense body according to any one of the above [1] to [4], which has an A-type or X-type framework structure.

[0019] [6] The zeolite dense body according to the above [1], wherein M is Na or Li.

[0020] [7] A method for producing a zeolite dense body, comprising introducing a mixture of water or an alkaline aqueous solution and zeolite powder into an enclosed space configured to be capable of being heated and pressurized, and producing a zeolite dense body by a hydrothermal hot pressing method.

[0021] [8] The method for producing a zeolite dense body according to the above [7], wherein the zeolite powder is pulverized by a ball mill method before being mixed with the water or alkaline aqueous solution.

[0022] [9] The method for producing a zeolite dense body according to the above [7] or [8], wherein after producing the zeolite dense body by the hydrothermal hot pressing method, the zeolite dense body is dehydrated.

[0023]

[10] The method for producing a dense zeolite body according to the above [7], wherein the mixture is heated and pressurized at a temperature of 100°C or more and 200°C or less, at a pressure of 50 MPa or more and 300 MPa or less, and for a holding time of 0.5 hours or more and 24 hours or less.

[0024]

[11] The method for producing a dense zeolite body according to the above [7], wherein the concentration of the alkaline aqueous solution in the mixture is 0.1 mol / L or more and 1.8 mol / L or less. Effect of the Invention

[0025] According to the present invention, high ionic conductivity is exhibited, while the environmental load is small and the production cost can be reduced. [Brief description of the drawings]

[0026] [Figure 1] 1(a) to 1(c) are schematic diagrams illustrating an example of a method for producing a dense zeolite body according to this embodiment. [Diagram 2] FIG. 2(a) and FIG. 2(b) are electron microscope images showing the A-type zeolite dense body obtained in the examples. [Diagram 3] FIG. 3 is an electron microscope image showing the A-type zeolite powder compact obtained in the comparative example. [Figure 4] FIG. 4 is a graph showing the temperature dependence of ionic conductivity of a dense A-type zeolite body and a compact A-type zeolite powder body. [Diagram 5] FIG. 5 is an electron microscope image showing the dense zeolite X body obtained in the example. [Figure 6]FIG. 6 is an electron microscope image showing the zeolite X compact obtained in the comparative example. [Figure 7] FIG. 7 is a graph showing the temperature dependence of ionic conductivity of a zeolite X dense body and a zeolite X compact. [Figure 8] FIG. 8 is a graph showing the relationship between the ionic conductivity of the A-type zeolite dense bodies obtained in the examples and the relative humidity of the atmosphere during measurement of the ionic conductivity. [Figure 9] FIG. 9 is a graph showing the relationship between the ionic conductivity of the zeolite X dense bodies obtained in the examples and the relative humidity of the atmosphere during the measurement of the ionic conductivity. [Figure 10] FIG. 10 is a graph showing the correlation between the concentration of the aqueous sodium hydroxide solution during hydrothermal hot pressing of the zeolite X dense body obtained in the examples, and the bulk density, relative density, and ionic conductivity. [Figure 11] FIG. 11 is a graph showing the correlation between the relative density and ionic conductivity of the zeolite X dense bodies obtained in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. Note that the drawings used in the following description may show characteristic parts in an enlarged scale for the sake of convenience in order to make the characteristics of the present invention easier to understand. For this reason, the dimensional ratios of each component may differ from the actual ones.

[0028] [Composition of zeolite dense bodies] The zeolite dense body according to the present embodiment is represented by the following general formula (1) and has an ionic conductivity of 1.0×10 -3 S cm -1 That's all. (M 1 / n ) x (Al x S y O 2(x+y) )·zH2O···(1) Here, M is one or more metal elements selected from Na, Li, K, Ca, Mg, Ba, and Ag, 0≦x≦y, 0≦z≦216, and n is a valence number.

[0029] The zeolite dense body of the present embodiment forms a dense assembly of crystal grains, unlike conventional zeolite molded bodies such as zeolite powder compacts, due to the formation of bonds between the particles constituting the zeolite powder. This three-dimensional structure of the dense assembly makes it possible to form a good ion conduction path. For this reason, the ion conductivity of the zeolite dense body is 1.0×10 -3 S cm -1 More preferably, it is 0.5×10 -2 S cm -1 More preferably, it is 1.0×10 -2 S cm -1 The relative humidity of the atmosphere during use of the zeolite dense body is preferably 30% or more, more preferably 50% or more, and even more preferably 70% or more. By using the zeolite dense body of the present embodiment in an environment in which the relative humidity can be maintained within the above range, higher ionic conductivity can be achieved.

[0030] The dense zeolite body is composed of a framework of anionic crystalline aluminosilicate and a cationic metal element M supported on the framework. The metal element M is preferably Na or Li, from the viewpoint that cationic species having a smaller ionic radius exhibit higher ionic conductivity.

[0031] In this zeolite dense body, the relative density measured by the theoretical density and the bulk density is preferably 80% or more, more preferably 85% or more, and even more preferably 90% or more. By having the relative density within the above range, more bonds are formed between the particles, and a zeolite bulk body having a relative density close to the theoretical density can be obtained. In addition, a dense crystal structure without impurities, voids, pinholes, etc. at the crystal grain boundaries can be obtained.

[0032] The bulk density of the zeolite compact is 1.7 g / cm3 More than 2.0g / cm 3 It is preferable that the density is 1.8 g / cm or less. 3 More than 2.0g / cm 3 The bulk density of the compact made of zeolite powder is preferably 0.9 g / cm or less. 3 More than 1.1g / cm 3 Since the bulk density of the zeolite dense body of the present embodiment is larger than those of the above, a denser zeolite bulk body can be obtained. The bulk density can be measured from the shape and mass of the sample.

[0033] The dense zeolite body has the same skeletal structure as the zeolite powder used as the raw material. Examples of the skeletal structure of the dense zeolite body include A-type (LTA), X-type or Y-type (FAU), L-type (LTL), ZSM-5 (MFI), beta (BEA), ferrierite (FER), and mordenite (MOR). From the viewpoint that the more cations there are, the more cations that contribute to ion conduction and the higher the ion conductivity, the dense zeolite body preferably has a skeletal structure with a low silica / alumina ratio, and is preferably A-type or X-type.

[0034] In the dense zeolite body, a plurality of pores having a pore size corresponding to each skeletal structure are formed. For example, when the dense zeolite body has an A-type skeletal structure, the pore size is 0.42 nm (4.2 Å), and when the dense zeolite body has an X-type skeletal structure, the pore size is 0.74 nm (7.4 Å). In the above skeletal structures, the pore sizes are largest in the order of X-type or Y-type, L-type, mordenite, beta, ZSM-5, ferrierite, and A-type.

[0035] The shape of the zeolite dense body is not particularly limited and may take various shapes, but examples thereof include layer shapes, sheet shapes, and membrane shapes from the viewpoint of miniaturization and low height of the device. When the zeolite dense body is in the form of a layer, sheet, or membrane, the thickness is preferably 10 μm or more and 2000 μm or less, and more preferably 50 μm or more and 1000 μm or less. By making the thickness of the zeolite dense body 50 μm or more, it is possible to prevent the dense body from being broken or short-circuited. In addition, by making the zeolite dense body thin, the resistance of ion conduction can be reduced, and high ion conduction properties can be obtained.

[0036] In addition, for dense zeolite, the log(σ / S cm) calculated from the ionic conductivity (σ) is -1 ) is greater than or equal to -3. In the fields of batteries and chemical sensors, log(σ / S cm -1 ) is -3 or more, which is called the superionic conduction region, and is one of the indices that govern the electrical performance of each device. By expressing the ionic conductivity contained in this superionic conduction region in a relatively low temperature range, such as from room temperature to 150°C, it is possible to maintain significantly higher ionic conductivity within the allowable temperature range within the device, for example, the allowable temperature range of a lithium-ion secondary battery in a vehicle, and to obtain excellent charge / discharge characteristics of the lithium-ion secondary battery.

[0037] This zeolite dense body may be used as a zeolite dense layer or zeolite dense film formed on an electrode layer such as a positive electrode layer or a negative electrode layer, or may be used as a zeolite dense layer formed on a substrate. When the zeolite dense body is used as a solid electrolyte layer or solid electrolyte film, the zeolite dense body can constitute a zeolite dense layer or zeolite dense film formed between a positive electrode active material layer of a positive electrode layer and a negative electrode active material layer of a negative electrode layer. When the zeolite dense body is used as a chemical sensor, it can constitute a zeolite dense layer formed on a ceramic substrate or a metal substrate.

[0038] [Method of manufacturing zeolite dense body] The method for producing a zeolite dense body according to this embodiment involves introducing a mixture of water or an alkaline aqueous solution and zeolite powder into an enclosed space configured to be capable of being heated and pressurized, and producing a zeolite dense body by the HHP method.

[0039] 1(a) to 1(c) are schematic diagrams for explaining an example of a method for producing a zeolite dense body according to the present embodiment. A hydrothermal hot press apparatus 10 (hereinafter also referred to as an HHP apparatus) used in this production method includes a reaction vessel body 11 having a through hole 12 with a substantially circular cross section at the center, a lower rod 13A inserted into the through hole 12 from below the reaction vessel body 11 and arranged so as to be movable in the vertical direction, an upper rod 13B inserted into the through hole 12 from above the reaction vessel body 11 and arranged so as to be movable in the vertical direction, and an enclosed space 14 provided between the lower rod 13A and the upper rod 13B inside the through hole 12. The enclosed space 14 is defined by the upper surface 13a of the lower rod 13A, the lower surface 13b of the upper rod 13B, and the inner peripheral surface 12a of the through hole 12, and functions as a mold when producing a zeolite dense body. Further, the hydrothermal hot press apparatus 10 is provided with a heating unit (not shown), such as a heater, that is arranged so as to surround the reaction vessel body 11 .

[0040] First, a mixture P is prepared by mixing water or an aqueous alkali solution of a predetermined concentration with zeolite powder as a raw material. The type of zeolite powder used as the raw material is not particularly limited. Examples of the zeolite powder framework structure include A-type (LTA), X-type or Y-type (FAU), L-type (LTL), ZSM-5 (MFI), beta (BEA), ferrierite (FER), and mordenite (MOR), and A-type or X-type is preferable.

[0041] The alkaline aqueous solution may be, for example, an aqueous solution containing one or more selected from sodium hydroxide, sodium carbonate, sodium bicarbonate, potassium hydroxide, potassium carbonate, potassium bicarbonate, calcium hydroxide, lithium hydroxide, sodium silicate (water glass), natural soda, etc.

[0042] The concentration of the alkaline aqueous solution can be appropriately selected depending on the type of alkali, the type of zeolite, etc., but is preferably from 0.1 mol / L to 10 mol / L, more preferably from 0.1 mol / L to 5.0 mol / L, even more preferably from 0.1 mol / L to 2.0 mol / L, and particularly preferably from 0.1 mol / L to 1.8 mol / L.

[0043] The blending ratio of water or an alkaline aqueous solution in the mixture can be appropriately selected depending on the type of zeolite, the type and concentration of the alkaline aqueous solution, etc., but the mass of water or an alkaline aqueous solution relative to the mass of the mixture is preferably 5 mass% or more and 30 mass% or less, and more preferably 10 mass% or more and 20 mass% or less.

[0044] The zeolite powder may be pulverized by a ball mill method before mixing the zeolite powder with water or an alkaline aqueous solution. By pulverizing the zeolite powder in advance by a ball mill method and mixing the pulverized zeolite powder with water or an alkaline aqueous solution to prepare a mixture, the relative density of the zeolite dense body is increased, and higher ionic conductivity can be obtained.

[0045] The particle size of the zeolite powder after ball mill pulverization is preferably 0.1 μm or more and 10 μm or less, more preferably 0.5 μm or more and 5.0 μm or less, and even more preferably 0.8 μm or more and 3.0 μm or less.

[0046] Then, the lower rod 13A is inserted from above into the through hole 12 of the reaction vessel body 11, and the obtained mixture P is placed on the upper surface 13a of the lower rod 13A (FIG. 1(a)). After that, the upper rod 13B is inserted from above into the through hole 12 of the reaction vessel body 11, and an enclosed space 14 is formed in the through hole 12 (FIG. 1(b)). Then, the lower rod 13A and the upper rod 13B are moved close to each other to set the inside of the enclosed space 14 to a predetermined pressure, and the inside of the enclosed space 14 is heated by a heating unit (not shown) (FIG. 1(c)). As a result, the mixture P in the enclosed space 14 is heated to a predetermined temperature and pressurized to a predetermined pressure by a hydrothermal hot pressing method (hereinafter also referred to as a HHP method). Then, the lower rod 13A and the upper rod 13B are pulled out from the through hole 12, and a zeolite dense body M is obtained. Conventional production methods require a substrate to support the zeolite powder, and it is difficult to obtain a membrane with high ionic conductivity unless an appropriate substrate is selected. On the other hand, the production method of the present embodiment does not require a substrate to support the zeolite powder, and a zeolite dense body M with high ionic conductivity can be stably produced.

[0047] The heating and pressurizing conditions of the HHP method are not particularly limited, but for example, the mixture is preferably heated and pressurized at a temperature of 100° C. to 200° C., a pressure of 50 MPa to 300 MPa, and a holding time of 0.5 hours to 24 hours. It is more preferable to heat and pressurize the mixture at a temperature of 100° C. to 150° C., a pressure of 100 MPa to 300 MPa, and a holding time of 1 hour to 5 hours.

[0048] After producing the dense zeolite body M by the HHP method, the dense zeolite body M may be dehydrated as necessary. From the viewpoint of electrical insulation, it is preferable that the dense zeolite body M has a low water content, but if the dense zeolite body M has an excessively low water content, there is a risk of the ion conductivity decreasing. From the above viewpoint, the water content of the dense zeolite body M is preferably 0% by mass or more and 25% by mass or less, and more preferably 10% by mass or more and 25% by mass or less, based on the total mass of the dense zeolite body M.

[0049] A material such as carbon graphite powder may be applied to the upper surface 13a of the lower rod 13A, the lower surface 13b of the upper rod 13B, and / or the inner peripheral surface 12a of the through-hole 12 in the reaction vessel body 11. Also, an inclined surface may be provided by chamfering or the like at the portion of the through-hole 12 that serves as the outlet for the dense zeolite body M. This makes it possible to prevent the dense zeolite body M from sticking to the reaction vessel body 11 and to suppress damage to the dense zeolite body M when the sample is taken out. Furthermore, a surface treatment such as carburization may be applied to the upper surface 13a of the lower rod 13A, the lower surface 13b of the upper rod 13B, and / or the inner surface 12a of the through hole 12 in the reaction vessel body 11. This makes it possible to suppress deformation and wear of the upper surface 13a of the lower rod 13A, the lower surface 13b of the upper rod 13B, and / or the inner surface 12a of the through hole 12 in the reaction vessel body 11 during the production of the zeolite dense body M. EXAMPLES

[0050] EXAMPLES Examples of the present invention will be described below, but the present invention is not limited to the following examples.

[0051] Example 1 A type (LTA) zeolite powder (manufactured by Tosoh Corporation) was pulverized in a ball mill (manufactured by Irie Shokai, device name "Desktop Ball Mill"). The zeolite powder after pulverization and water were adjusted so that the mass of water relative to the mass of the mixture was 17 mass%, and this was mixed uniformly to obtain a mixture. As shown in Table 1, a dense A type zeolite body was produced by the HHP method at a heating temperature of 150°C and a pressure of 150 MPa.

[0052] Example 2 A dense body of A-type zeolite was produced in the same manner as in Example 1, except that the dense body of A-type zeolite obtained by the HHP method was dehydrated by ordinary heating.

[0053] Example 3 A type zeolite dense body was produced in the same manner as in Example 1, except that the crushed zeolite powder and a 5.0 mol / L aqueous sodium hydroxide solution were adjusted so that the mass of the aqueous sodium hydroxide solution relative to the mass of the mixture was 17 mass%, and then the mixture was uniformly mixed to obtain a mixture.

[0054] Comparative Example 1 A type A zeolite powder compact was produced in the same manner as in Example 1, except that unpulverized type A (LTA) zeolite powder was mixed with water and a pellet-shaped powder compact was produced at a pressure of 100 MPa instead of the HPP method.

[0055] Comparative Example 2 A type A zeolite compact was produced in the same manner as in Comparative Example 1, except that the obtained type A zeolite compact was dehydrated by ordinary heating.

[0056] [Table 1]

[0057] Next, the characteristics of the A-type zeolite dense bodies of Examples 1 to 3 and the A-type zeolite compact powder bodies of Comparative Examples 1 and 2 were observed, measured and evaluated by the methods described below.

[0058] [Appearance of zeolite dense body and zeolite powder compact] As representative examples, the appearances of the A-type zeolite dense bodies of Examples 1 and 3 and the A-type zeolite compact of Comparative Example 1 were confirmed by electron microscope images (manufactured by JEOL Ltd., device name "JSM-6510A") The results are shown in Figures 2(a), 2(b) and 3.

[0059] It was found that the zeolite dense body of Example 1 (FIGS. 2(a) and 2(b)) had very few gaps between crystal grains, compared with the zeolite compact of Comparative Example 1 (FIG. 3). In addition, when comparing the A-type zeolite dense bodies of Example 1 and Example 3, it was found that the use of a 5.0 mol / L aqueous sodium hydroxide solution as a mixture resulted in fewer gaps between crystal grains than the use of water.

[0060] [Evaluation of ionic conductivity] (Measurement of ionic conductivity) The impedance of the obtained zeolite dense body was measured by an AC two-terminal method, and the ion conductivity at each temperature was calculated. In Examples 1 to 3 and Comparative Examples 1 and 2, humidity control was not performed, and the ion conductivity was measured in the outside air humidity environment on the measurement day.

[0061] From the ionic conductivity obtained above, log(σ / S cm -1 ) was calculated to evaluate the ionic conductivity. The results are shown in FIG. 4 and Table 1. In Table 1, "*" indicates that the sample contained impurities. The ionic conductivity in Table 1 indicates, as an example, the ionic conductivity measured at the temperature shown in the table for each of the examples and comparative examples.

[0062] As shown in FIG. 4, in Example 1, the log(σ / S cm -1 It was found that the value of log(σ / S·cm) was larger than -3, and high ionic conductivity was obtained. This is presumably because the gaps between the crystals are very small and good ionic conduction paths are formed between the crystal grains. Also, in Example 2, the log(σ / S·cm) was larger than -3 over the entire range from room temperature to around 400°C. -1 ) is -3 or more, and it is found that high ion conductivity equivalent to that of Example 1 can be obtained. In addition, when compared with the reference data obtained for the solid electrolyte having β-alumina and Nasicon type crystal structures, it is found that the A-type zeolite compact bodies of Examples 1 and 2 have high ion conductivity equivalent to that of β-alumina and Nasicon type solid electrolytes. In particular, it is found that Example 1 shows higher ion conductivity than the Nasicon type crystal structure in a relatively low temperature range from room temperature to around 150°C.

[0063] On the other hand, in Comparative Example 1 and Comparative Example 2, the log(σ / S cm -1 ) was approximately -4 or less, and the ionic conductivity was poor.

[0064] Example 4 Commercially available X-type (FAU) zeolite powder was used. The zeolite powder and 1.0 mol / L aqueous sodium hydroxide solution were adjusted so that the mass of the aqueous sodium hydroxide solution was 17 mass% relative to the mass of the mixture, and then mixed uniformly to obtain a mixture. A dense body of X-type zeolite was produced by the HHP method at a heating temperature of 150°C and a pressure of 150 MPa.

[0065] Example 5 A dense zeolite X body was produced in the same manner as in Example 4, except that the dense zeolite X body obtained by the HHP method was dehydrated by ordinary heating.

[0066] Comparative Example 3 A zeolite X compact was produced in the same manner as in Example 4, except that the X-type (FAU) zeolite powder was used to produce a pellet-shaped compact at a pressure of 100 MPa instead of the HPP method, and dehydrated by normal heating.

[0067] Next, the characteristics of the zeolite X-type dense bodies of Examples 4 to 5 and the zeolite X-type compact powder body of Comparative Example 3 were observed, measured, and evaluated in the same manner as above. The results are shown in Figures 5 to 7. In Examples 4 to 5 and Comparative Example 3, humidity control was not performed, and ionic conductivity was measured in the outdoor humidity environment on the measurement day.

[0068] As shown in Figs. 5 and 6, it was found that the zeolite dense body of Example 4 (Fig. 5) had much fewer gaps between crystal grains than the zeolite compact of Comparative Example 3 (Fig. 6).

[0069] As shown in FIG. 7, in Example 4, the log(σ / S cm -1 ) was greater than -3, and it was found that high ionic conductivity was obtained. In Example 5, the log(σ / S cm -1) is greater than -4, which is inferior to Example 4, but it is found that it has a higher ion conductivity than Comparative Example 3. In addition, when compared with the reference data obtained for the solid electrolyte having β-alumina and Nasicon type crystal structures, it is found that the A-type zeolite compact bodies of Examples 4 and 5 have a high ion conductivity equivalent to that of β-alumina and Nasicon type solid electrolytes. In particular, it is found that Example 4 shows a higher ion conductivity than the Nasicon type crystal structure in a relatively low temperature range from room temperature to around 150°C.

[0070] Example 6 The ionic conductivity of the A-type zeolite dense body was measured in the same manner as in Example 1, except that the relative humidity of the atmosphere during the measurement of the ionic conductivity of the A-type zeolite dense body was maintained at 30%.

[0071] Example 7 The ionic conductivity of the A-type zeolite dense body was measured in the same manner as in Example 1, except that the relative humidity of the atmosphere during the measurement of the ionic conductivity of the A-type zeolite dense body was maintained at 90%.

[0072] Comparative Example 4 The ionic conductivity of the A-type zeolite compact was measured in the same manner as in Comparative Example 1, except that the relative humidity of the atmosphere during the measurement of the ionic conductivity of the A-type zeolite compact was maintained at 30%.

[0073] Comparative Example 5 The ionic conductivity of the A-type zeolite compact was measured in the same manner as in Comparative Example 1, except that the relative humidity of the atmosphere during the measurement of the ionic conductivity of the A-type zeolite compact was maintained at 90%.

[0074] Next, in the same manner as above, the properties of the A-type zeolite dense bodies of Examples 6 to 7 and the A-type zeolite compacts of Comparative Examples 4 to 5 were measured and evaluated. The results are shown in FIG.

[0075] As shown in FIG. 8, Example 6, which was measured in an environment of relative humidity 30%, had a lower log(σ / S cm) value than Comparative Example 4, which was measured in an environment of relative humidity 30%, in a relatively low temperature range from room temperature to about 150°C. -1 ) was larger, and it was found that high ionic conductivity was obtained. Similarly, Example 7 measured in a 90% relative humidity environment had a log(σ / S cm -1 ) value was large, indicating that high ionic conductivity could be obtained. In addition, in Example 7, in the relatively low temperature range from room temperature to around 150°C, the log(σ / S cm -1 ) was large, and it was found that higher ionic conductivity could be obtained. In other words, it was found that in the dense A-type zeolite body produced by the HHP method, the ionic conductivity measured in an environment with a relative humidity of 90% was about twice as high as the ionic conductivity measured in an environment with a relative humidity of 30%. Furthermore, it was found that in Examples 6 and 7, in the relatively low temperature range from room temperature to around 150°C, higher ionic conductivity was exhibited than in the Nasicon-type crystal structure.

[0076] On the other hand, in Comparative Example 4, which was measured under a relative humidity of 30%, log(σ / S cm -1 ) was equivalent to that of Comparative Example 1, and was inferior in ionic conductivity to that of Example 6 measured in a relative humidity of 30%. Similarly, in Comparative Example 5 measured in a relative humidity of 90%, the log(σ / S cm -1 ) was larger than that of Comparative Example 1, but the ion conductivity was inferior to that of Example 7 measured in an environment of a relative humidity of 90%.

[0077] Example 8 The ionic conductivity of the dense zeolite X was measured in the same manner as in Example 4, except that the relative humidity of the atmosphere during the measurement was maintained at 30%.

[0078] Example 9 The ionic conductivity of the dense zeolite X body was measured in the same manner as in Example 4, except that the relative humidity of the atmosphere during the measurement was maintained at 80%.

[0079] Comparative Example 6 A zeolite X compact was produced in the same manner as in Comparative Example 3, except that the obtained zeolite X compact was not dehydrated, and the ionic conductivity was measured.

[0080] Comparative Example 7 The ionic conductivity of the zeolite X compact was measured in the same manner as in Comparative Example 6, except that the relative humidity of the atmosphere during the measurement of the ionic conductivity of the zeolite compact was maintained at 30%.

[0081] Comparative Example 8 The ionic conductivity of the zeolite X dense body was measured in the same manner as in Comparative Example 6, except that the relative humidity of the atmosphere during the measurement of the ionic conductivity of the zeolite compact was maintained at 80%.

[0082] In the same manner as above, the properties of the zeolite X dense bodies of Examples 8 to 9 and the zeolite X compacts of Comparative Examples 6 to 8 were measured and evaluated. The results are shown in FIG.

[0083] As shown in FIG. 9, Example 8, which was measured in an environment of relative humidity 30%, had a lower log(σ / S cm) value than Comparative Example 7, which was measured in an environment of relative humidity 30%, in a relatively low temperature range from room temperature (approximately 27°C) to approximately 100°C. -1 ) was larger, and it was found that high ionic conductivity was obtained. Similarly, Example 9 measured in an environment of 80% relative humidity had a log(σ / S cm -1 ) value was large, indicating that high ionic conductivity could be obtained.

[0084] In addition, in Example 9, in the relatively low temperature range from room temperature to around 100°C, the log(σ / S cm -1) was large, and it was found that higher ionic conductivity could be obtained. In other words, it was found that in the dense X-type zeolite body produced by the HHP method, the ionic conductivity measured in an environment with a relative humidity of 80% was higher than that measured in an environment with a relative humidity of 30%. Furthermore, it was found that in Examples 8 and 9, in the relatively low temperature range from room temperature to around 100°C, higher ionic conductivity was exhibited than in the Nasicon-type crystal structure.

[0085] On the other hand, in Comparative Example 7, which was measured under a relative humidity of 30%, log(σ / S cm -1 ) was equivalent to that of Comparative Example 6, and was inferior in ionic conductivity to that of Example 8 measured in a relative humidity of 30%. Similarly, in Comparative Example 8 measured in a relative humidity of 80%, the log(σ / S cm -1 ) was larger than those of Comparative Examples 6 and 7, but the ion conductivity was inferior to that of Example 9 measured in an environment of a relative humidity of 80%.

[0086] [Correlation between crushing and relative density] Using the above-mentioned A-type zeolite powder that was not ground by a ball mill, the amount of water or sodium hydroxide solution added to the mixture was kept constant at 100 μL, and the concentration of the sodium hydroxide solution was changed. A-type zeolite dense bodies were prepared at HHP temperatures of 100°C and 150°C, with a holding time of 2 hours and a pressure of 150 MPa. The relative density of the obtained A-type zeolite dense bodies is shown in Table 2, and the ionic conductivity at room temperature and 450°C is shown in Table 3. In Tables 2 and 3, "0 mol / L" indicates that water was used instead of sodium hydroxide solution. The values ​​in the upper row of Table 3 indicate the ionic conductivity at room temperature, and the values ​​in the lower row indicate the ionic conductivity at 450°C. In Table 2, "*" indicates that the sample contained impurities.

[0087] For comparison, when uncrushed A-type zeolite powder was compressed at a pressure of 100 MPa to produce A-type zeolite powder, the relative density was 52% and the ionic conductivity at room temperature was 6.0 × 10 -6 S cm-1 , and the ionic conductivity at 450°C is 9.6×10 -5 S cm -1 It was.

[0088] [Table 2]

[0089] [Table 3]

[0090] The results in Table 2 show that the relative density of the A-type zeolite dense body is greater than that of the A-type zeolite compact regardless of whether the heating temperature during HHP is 100°C or 150°C, and that the relative density tends to increase as the concentration of the aqueous sodium hydroxide solution increases. However, when the heating temperature during HHP is 150°C and the concentration of the aqueous sodium hydroxide solution is 3.0 mol / L or 5.0 mol / L, impurities are generated in the obtained A-type zeolite dense body.

[0091] Furthermore, the results in Table 3 show that when the heating temperature during HHP was 100° C., the ionic conductivity of the A-type zeolite dense body was greater than that of the A-type zeolite compact both at room temperature and 450° C. When the heating temperature during HHP was 150° C., the ionic conductivity of the A-type zeolite dense body was greater than that of the A-type zeolite compact both at room temperature and 450° C.

[0092] Next, the A-type zeolite powder was pulverized in a ball mill under wet conditions using ethanol. The particle size of the A-type zeolite powder after pulverization was 0.5 μm to 3.0 μm. A dense A-type zeolite body was produced under the same conditions as above except that the A-type zeolite powder after pulverization was used, and the concentration of the sodium hydroxide aqueous solution in the mixture was changed at heating temperatures of 100°C and 150°C during HHP and a pressure of 150 MPa. The relative density of the obtained A-type zeolite dense body is shown in Table 4, and the ionic conductivity at room temperature and 450°C is shown in Table 5. The upper value in Table 5 indicates the ionic conductivity at room temperature, and the lower value indicates the ionic conductivity at 450°C. In addition, "*" in Table 4 indicates that the sample contained impurities.

[0093] For comparison, when the A-type zeolite powder after the crushing process was compressed under a pressure of 150 MPa to produce an A-type zeolite powder compact, the relative density was 61% and the ionic conductivity at room temperature was 9.3 × 10 -7 S cm -1 , and the ionic conductivity at 450°C is 1.6×10 -4 S cm -1 It was.

[0094] [Table 4]

[0095] [Table 5]

[0096] From the results in Table 4, it was found that the relative density of the A-type zeolite dense body was greater than that of the A-type zeolite compact, regardless of whether the heating temperature during HHP was 60°C, 80°C, 100°C, or 150°C. It was also found that the relative density tended to increase as the concentration of the aqueous sodium hydroxide solution increased, regardless of whether the heating temperature during HHP was 80°C, 100°C, or 150°C. However, when the heating temperature during HHP was 150°C and the concentration of the aqueous sodium hydroxide solution was 5.0 mol / L, impurities were generated in the obtained A-type zeolite dense body.

[0097] Furthermore, the results in Table 5 show that when the heating temperature during HHP was 80° C., the ionic conductivity of the A-type zeolite dense body at both room temperature and 450° C. was greater than that of the A-type zeolite compact. Furthermore, when the heating temperature during HHP was 150° C., the ionic conductivity of the A-type zeolite dense body at both room temperature and 450° C. was greater than that of the A-type zeolite compact.

[0098] Furthermore, it was found that when the heating temperature during HHP and the amount of water or sodium hydroxide added were the same, the ionic conductivity of the crushed dense body of zeolite A was greater than that of the uncrushed dense body of zeolite A.

[0099] [Correlation between solution concentration and ionic conductivity]

[0100] Using the above-mentioned zeolite X powder, the amount of water or sodium hydroxide solution added to the mixture was kept constant at 100 μL, and the concentration of the sodium hydroxide solution was changed, and the zeolite X dense body was prepared at a heating temperature of 150°C, a holding time of 2 hours, and a pressure of 150 MPa during HHP. The bulk density and relative density of the obtained zeolite X dense body, as well as the ionic conductivity measured at 300°C, are shown in Table 6. Graphs plotting the obtained measured values ​​are shown in Figures 10 and 11.

[0101] [Table 6]

[0102] From the results in Table 6 and Figure 10, it can be seen that the bulk density and relative density of the dense zeolite X increase with increasing concentration of the sodium hydroxide solution during HHP. However, the log(σ / S cm -1 ) does not increase with increasing sodium hydroxide concentration during HHP. Up to a sodium hydroxide concentration of 1.5 mol / L, the log(σ / S cm -1) is greater than -2.7, but when the concentration of the sodium hydroxide solution exceeds 1.8 mol / L, the log(σ / S cm -1 ) was less than -3.0. When the concentration of the sodium hydroxide solution exceeded 5.0 mol / L, the log(σ / S cm -1 ) is less than -3.7, and when the concentration of the sodium hydroxide solution exceeds 5.5 mol / L, the log(σ / S cm -1 ) value.

[0103] In addition, the relative density and log(σ / S cm -1 ) is shown in Figure 11. As shown in the figure, the dotted region in the figure is the region where the relative density of the dense zeolite X is 80% or more. However, even if the dense zeolite X has a relative density within this region, it does not necessarily have high ionic conductivity. In particular, even if the relative density of the dense zeolite X is 90% or more, the log(σ / S cm -1 ) was less than -3. This result indicates that high ionic conductivity cannot be obtained simply by increasing the concentration of the aqueous sodium hydroxide solution during HHP, but that there is an optimal range for the concentration of the aqueous sodium hydroxide solution during HHP in order to obtain high ionic conductivity at each temperature. [Industrial Applicability]

[0104] Since the zeolite dense body of the present invention has extremely high ionic conductivity, it is useful as a solid electrolyte material for next-generation batteries such as all-solid-state batteries and metal-air batteries, and can also be used as a material in technical fields to which conventional zeolites have not been applied, as a material for chemical sensors, and as a material for thermoelectric conversion. [Explanation of symbols]

[0105] 10. Hydrothermal hot press equipment 11 Reaction vessel body 12 Through hole 12a Inner surface 13A Lower Rod 13a Top side Upper rod of 13B Lower surface of 13b Sealed space 14

Claims

1. Represented by the following general formula (1), the ionic conductivity is 1.0×10 -3 S. cm -1 That's all. A zeolite dense body having a relative density, as measured by theoretical density and bulk density, of 80% or more. (M) 1/n ) x (Al) x Yes y O 2(x+y) )・vH 2 O ・・・(1) Here, M is one or more metal elements selected from Na, Li, K, Ca, Mg, Ba, and Ag, 0<x≦y, 0≦z≦216, and n is a valence number.

2. Bulk density: 1.7 g / cm 3 2.0g / cm or more 3 2. The zeolite dense body according to claim 1, wherein:

3. Log (σ / S cm) calculated from ionic conductivity at room temperature or higher and 150°C or lower -1 3. The zeolite dense body according to claim 1, wherein the zeolite density is -3 or more.

4. The zeolite dense body according to any one of claims 1 to 3, having an A-type or X-type framework structure.

5. The zeolite dense body according to claim 1 , wherein M is Na or Li.

6. A method for producing the zeolite dense body according to claim 1, comprising the steps of: A method for producing a zeolite dense body, comprising introducing a mixture of water or an alkaline aqueous solution and zeolite powder into an enclosed space configured to be capable of being heated and pressurized, and producing a zeolite dense body by a hydrothermal hot pressing method.

7. The method for producing a zeolite dense body according to claim 6, wherein the zeolite powder is pulverized by a ball mill method before the water or the alkaline aqueous solution and the zeolite powder are mixed.

8. The method for producing a zeolite dense body according to claim 6 or 7, wherein after the zeolite dense body is produced by the hydrothermal hot pressing method, the zeolite dense body is dehydrated.

9. The method for producing a dense zeolite body according to claim 6, wherein the mixture is heated and pressurized at a temperature of 100° C. to 200° C., a pressure of 50 MPa to 300 MPa, and a holding time of 0.5 hours to 24 hours.

10. The method for producing a dense zeolite body according to claim 6, wherein the concentration of the aqueous alkaline solution in the mixture is from 0.1 mol / L to 1.8 mol / L.

Citation Information

Patent Citations

  • Zeolite shaped article and its manufacture method

    JP2005306725A

  • Proton conductive solid electrolyte

    JP2007200601A

  • Solid electrolyte

    JP2016219134A

  • Solid electrolyte film

    JP2018198128A

  • Sulfide-based inorganic solid electrolyte material, solid electrolyte, solid electrolyte membrane, and lithium ion battery

    JP2019071235A