Polymer-coated wire manufacturing method and polymer-coated wire manufacturing device
The electrospinning method efficiently forms a polymer layer on wire surfaces by controlling thickness through rotational and movement speeds, addressing the inefficiencies of existing coating methods and enhancing the wire's durability.
Patent Information
- Application Number
- JP2021002588
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-12
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-01-12
AI Technical Summary
Existing coating methods struggle to efficiently and stably form a polymer layer on wire surfaces with a thickness of several μm to several tens of μm.
A method involving electrospinning, where a spinning solution is discharged from a nozzle perpendicular to a rotating electrode, winding polymer fibers around the wire while controlling the thickness by adjusting the rotational speed and movement speed, followed by heat treatment and cooling.
Enables efficient and stable formation of a polymer layer on the wire surface, allowing precise thickness control and improved durability of the polymer-coated wire.
Smart Images

Figure 0007595341000002 
Figure 0007595341000003 
Figure 0007595341000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a polymer-coated wire. and Polymer-coated wire manufacturing equipment Place Regarding. [Background technology]
[0002] A coating method has been proposed for forming a coating layer on the surface of a thin wire made of an inorganic or organic material (see, for example, Patent Document 1). In this coating method, a coating solution used to form a coating layer is spotted on the tip of a jig for holding droplets or on a substrate, and the thin wire is passed through the droplets that are held to coat the surface of the thin wire with the coating solution, and then drying, heating, light irradiation, and other processes are performed to form a coating layer on the surface of the thin wire. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2013-233520 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, with the coating method described in Patent Document 1, it is difficult to coat efficiently and stably, for example, when the thickness of the polymer coated on the surface of the wire needs to be controlled to a thickness of several μm to several tens of μm.
[0005] The present invention has been made in consideration of the above-mentioned circumstances, and provides a method for producing a polymer-coated wire that can efficiently and stably form a polymer layer that coats a wire. and Polymer-coated wire manufacturing equipment Place The purpose is to provide. [Means for solving the problem]
[0006] The method for producing a polymer-coated wire according to the present invention includes the steps of: The method includes a polymer winding process in which an electrode arranged to surround a wire is rotated around the wire at a preset rotational speed, and the wire is moved relative to the electrode in the direction of the rotation axis of the electrode at a preset moving speed, while a nozzle that ejects a spinning solution in which at least one type of polymer is dissolved in at least one type of solvent is maintained at a higher potential than the electrode, and the spinning solution is ejected from the nozzle toward a portion of the wire that faces the electrode in a direction perpendicular to the rotation axis direction, thereby winding a polymer fiber generated from the spinning solution around the wire.
[0007] From another viewpoint, the polymer-coated wire manufacturing apparatus according to the present invention comprises: An electrode disposed so as to surround the wire; a rotation drive unit that rotates the electrode around the wire at a preset rotation speed; a take-up reel for taking up the wire; a reel drive unit that rotates the take-up reel to move the wire relative to the electrode in a direction of a rotation axis of the electrode at a preset moving speed; The spinning solution ejection unit has a nozzle that ejects a spinning solution in which at least one type of polymer is dissolved in at least one type of solvent, and a voltage application unit that applies a DC voltage between the nozzle and the electrode, and ejects the spinning solution from the nozzle toward a portion of the wire facing the electrode in a direction perpendicular to the direction of the rotation axis while maintaining the nozzle at a higher potential than the electrode. Effect of the Invention
[0011] According to the method and apparatus for producing a polymer-coated wire of the present invention, a spinning solution is discharged from a nozzle toward a portion of the wire facing the electrode while the nozzle is maintained at a higher potential than the electrode, and polymer fibers produced from the spinning solution are wound around the wire. This makes it possible to control the thickness of the polymer layer formed on the surface of the wire by adjusting the amount of polymer fiber wound around the wire, thereby enabling the efficient and stable formation of a polymer layer that coats the wire. [Brief description of the drawings]
[0012] [Figure 1] 1 is a schematic diagram of a polymer-coated wire manufacturing apparatus according to an embodiment of the present invention; [Diagram 2] 1A is a schematic diagram for explaining the operation of a polymer-coated wire manufacturing apparatus according to an embodiment, and FIG. 1B is an optical microscope photograph of an example of a polymer-coated wire. [Diagram 3] FIG. 1 is a diagram showing an example of a stent according to an embodiment. [Figure 4] 1A is a SEM photograph of the wire, and FIG. 1B is a SEM photograph of the polymer-coated wire according to Example 1. [Diagram 5] 1A is a SEM photograph of the polymer-coated wire according to Example 2, and FIG. 1B is a SEM photograph of the polymer-coated wire according to Example 3. [Figure 6] 1 is a SEM photograph of a polymer-coated wire according to Example 4. [Figure 7] 1A is a SEM photograph of the polymer-coated wire according to Example 5, and FIG. 1B is a SEM photograph of the polymer-coated wire according to Example 6. [Figure 8] 1A is an optical microscope photograph of the polymer-coated wire according to Comparative Example 1, and FIG. 1B is an optical microscope photograph of the polymer-coated wire according to Comparative Example 2. [Figure 9] 1A is an optical microscope photograph of the polymer-coated wire according to Comparative Example 3, and FIG. 1B is an optical microscope photograph of the polymer-coated wire according to Example 7. [Figure 10]13A is an SEM photograph of the polymer-coated wire according to Example 7, and FIG. 13B is an SEM photograph of another portion of the polymer-coated wire according to Example 7. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, a method for manufacturing a polymer-coated wire, an apparatus for manufacturing a polymer-coated wire, and a polymer-coated wire according to an embodiment of the present invention will be described with reference to the drawings. In the method for manufacturing a polymer-coated wire according to the present embodiment, a polymer layer is formed on the surface of the wire by winding a polymer fiber around the wire by electrospinning. The method for manufacturing a polymer-coated wire according to the present embodiment can be applied to all metal wires that require a polymer coating on the surface.
[0014] For example, as shown in FIG. 1, the polymer-coated wire manufacturing apparatus 1 according to the present embodiment includes a supply reel 21 for unwinding the wire W, a recovery unit 24 for recovering the wire W around which the polymer fiber is wound, and guide rollers 22 and 23 for guiding the wire W. Here, the wire W is made of a known metal such as stainless steel, Ni-Ti alloy, Ta, Co-Cr alloy, or a known metal alloy or a known polymer. The diameter of the wire W is set to, for example, 10 μm or more and 50 μm or less. The recovery unit 24 includes a take-up reel 241 for winding the wire W, and a reel drive unit 242 for rotating the take-up reel 241. The reel drive unit 242 rotates the take-up reel 241 in the direction indicated by the arrow AR1, thereby moving the wire W relative to the electrode 14 in the direction of the rotation axis of the electrode 14, i.e., in the direction indicated by the arrow AR4, at a preset moving speed.
[0015] The polymer-coated wire manufacturing apparatus 1 also includes an electrode 14 arranged to surround the wire W, a support section 13 supporting the electrode 14, a rotary drive section 16 for rotating the electrode 14 and the support section 13 around the wire W at a preset rotation speed, and a spinning solution discharge section 11 for discharging the spinning solution. The support section 13 has a funnel shape made of resin, metal, or the like, and includes a main section 131 formed in a bowl shape with an opening 131a at the bottom, and a cylindrical section 132 whose inside is in communication with the inside of the main section 131 through the opening 131a of the main section 131. The electrode 14 is formed in a bowl shape from metal, and is arranged to cover the inner wall of the main section 131 of the support section 13. The electrode 14 is also grounded via a ground wire (not shown).
[0016] The rotation drive unit 16 has a first friction wheel 164 in an annular shape fixed to the cylindrical portion 132 of the support unit 13, a second friction wheel 161, a motor 162 that rotates the second friction wheel 161, and a rubber timing belt 163 that is stretched between the first friction wheel 164 and the second friction wheel 161. The motor 162 rotates the second friction wheel 161 as indicated by an arrow AR21, thereby rotating the first friction wheel 164 via the timing belt 163 as indicated by an arrow AR22. This causes the electrode 14 and the support unit 13 to rotate as indicated by an arrow AR3.
[0017] The spinning solution discharge part 11 has a cylindrical syringe 111 in which the spinning solution is stored, a nozzle 112 attached to the tip of the syringe 111, a plunger 113 inserted on the opposite side of the syringe 111 from the nozzle 112 side, and a voltage application part 114 that applies a DC voltage to the nozzle 112. Here, the voltage application part 114 is a DC voltage source that applies a DC voltage of 5 kV to 20 kV to the nozzle 112. The spinning solution discharge part 11 also has a pressing mechanism (not shown) that pushes the plunger 113 into the syringe 111 by air pressure. The spinning solution discharge part 11 discharges the spinning solution from the nozzle 112 toward a part of the wire W that faces the electrode 14 while maintaining the nozzle 112 at a higher potential than the electrode 14. At this time, the pressing mechanism pushes the plunger 113 into the syringe 111 with an air pressure of, for example, 20 MPa. Here, the distance between the tip of the nozzle 112 and the part of the wire W facing the electrode 14 is set to 5 cm or more and 10 cm or less, and is preferably set to 5 cm. In addition, the tip 112a where the nozzle 112 is provided is preferably located within a projection area A1 of the electrode 14 in the direction of the rotation axis of the electrode 14. Furthermore, the acute angle formed by the ejection direction of the spinning solution from the nozzle 112 and the direction of the rotation axis of the electrode 14 is preferably set to 20 degrees or more and 90 degrees or less.
[0018] Next, a method for manufacturing a polymer-coated wire using the polymer-coated wire manufacturing apparatus 1 according to the present embodiment will be described. First, a spinning solution preparation step is performed in which at least one type of polymer is dissolved in an organic solvent to prepare a spinning solution. Here, as the polymer, a highly bioabsorbable polymer having a shape memory function can be adopted, and for example, it is selected from polyglycolic acid (PGA), copolymer of glycolic acid and L-lactic acid (PGLA), copolymer of glycolic acid and DL-lactic acid (PGDLLA), poly-L-lactic acid (PLLA), poly-D-lactic acid (PDLA), poly-DL-lactic acid (PDLLA), copolymer of L-lactic acid and ε-caprolactone (LCL), and poly-p-dioxanone (PDO). Examples of the organic solvent include dichloromethane, trichloromethane (CHCl3), dichloroethane, N,N-dimethylformamide, tetrahydrofuran, toluene, pyridine, acetonitrile, formamide, benzene, dimethylacetamide, N-methylpyrrolidone, hexane, 1,4-dioxane, acetone, methanol, ethanol, etc. The concentration of the polymer contained in the spinning solution may be 5 wt% or more and 15 wt% or less, and is preferably 6 wt% or more and 8 wt% or less.
[0019] Next, a spinning solution supplying step is performed in which the spinning solution is supplied into the syringe 111 of the spinning solution discharge part 11. As a result, the spinning solution is stored in the syringe 111.
[0020] Next, as shown in FIG. 2(A), a polymer winding process is performed in which the spinning solution is discharged from the nozzle 112 of the spinning solution discharge unit 11 toward a portion of the wire W facing the electrode 14, thereby winding the polymer fiber FB generated from the spinning solution around the wire W. Here, the electrode 14 and the support unit 13 are rotated around the wire W at a preset rotation speed, and the wire W is moved in the direction indicated by the arrow AR4 at a preset moving speed, while the spinning solution is discharged from the nozzle 112. Here, the nozzle 112 is maintained at a higher potential than the electrode 14. Here, the rotation speed of the electrode 14 and the support unit 13 may be 100 rpm or more and 2000 rpm or less. The moving speed of the wire W may be 25 cm / min or more and 570 cm / min or less. By carrying out this polymer winding process, a polymer-coated wire is formed, for example as shown in Fig. 2(B), which has a wire W and a polymer layer made of a polymer fiber wound around the wire W on the surface of the wire W. Here, the diameter of the polymer fiber is 0.1 μm or more and 10 μm or less.
[0021] Thereafter, a heat treatment process is performed in which the wire W on which the polymer layer made of the polymer fiber is formed is heated to melt the polymer fiber. In this heat treatment process, the treatment temperature may be 200°C or more, and the treatment time may be 10 seconds or more. Next, a cooling process is performed in which the wire W is cooled to form a polymer coating on the surface of the wire W. In this cooling process, for example, the wire W on which the polymer coating is formed on the surface is left in an environment of room temperature (e.g., 25°C) to slowly cool the wire W.
[0022] By carrying out the above series of steps, it is possible to manufacture a polymer-coated wire comprising a wire W and a polymer coating formed on the surface of the wire W. The thickness of the polymer coating of this polymer-coated wire can be 0.5 μm or more and 10 μm or less. Furthermore, when the polymer coating of the polymer-coated wire is formed from polylactic acid, the crystallinity thereof can be 40% or more and 75% or less.
[0023] Moreover, by using the polymer-coated wire according to the present embodiment, a stent 100, which is a so-called braided stent (braided stent) consisting of a mesh-like tube as shown in FIG. 3, can be formed. Here, the stent 100 is formed by folding the polymer-coated wire 101 in a zigzag shape to form a continuous V-shape and then spirally winding it so as to form a tube as a whole. In addition, the polymer-coated wire 101 has tops of two adjacent folded parts in the axial direction of the tube of the stent 100 in contact with each other. These tops in contact with each other may be fused together by, for example, heat melting. Here, the polymer-coated wire may be in a state before heat treatment, i.e., a state in which a polymer fiber is wound around the wire W, or in a state after heat treatment, i.e., a state in which a polymer coating is formed on the surface of the wire W.
[0024] As described above, according to the polymer-coated wire manufacturing method and polymer-coated wire manufacturing apparatus 1 of this embodiment, while the nozzle 112 of the spinning solution discharge unit 11 is maintained at a higher potential than the electrode 14, the spinning solution is discharged from the nozzle 112 toward the portion of the wire W facing the electrode 14, thereby winding the polymer fiber generated from the spinning solution around the wire W. This makes it possible to control the thickness of the polymer layer formed on the surface of the wire W by adjusting the amount of polymer fiber wound around the wire W, and therefore the polymer layer that covers the wire W can be formed efficiently and stably.
[0025] In addition, in the method for producing a polymer-coated wire according to the present embodiment, after the polymer winding step, a heat treatment step of heating the wire W on which a polymer layer made of polymer fibers is formed to melt the polymer fibers, and after the heat treatment step, a cooling step of cooling the wire W to form a polymer coating on the surface of the wire W may be performed. In this case, a polymer-coated wire can be produced that includes the wire W and the polymer coating formed on the surface of the wire W, and the thickness of the polymer coating is 0.5 μm to 10 μm. A stent 100 produced using this polymer-coated wire has the advantage that it can be placed in a living body for a long period of time, such as about 12 months, by suppressing corrosion of the wire W.
[0026] Although the embodiment of the present invention has been described above, the present invention is not limited to the configuration of the above-mentioned embodiment. However, the electrode 14 may be cylindrical and supported by a cylindrical support portion 13. In this case, the wire W may be arranged along the cylindrical axis of the electrode 14, and the electrode 14 and the support portion 13 may be rotated around the cylindrical axis. The electrode 14 may be disk-shaped.
[0027] The stent 100 made using the polymer-coated wire according to the embodiment is not limited to the braided stent having the shape shown in Fig. 3, and may be, for example, a tubular stent by braiding or weaving the polymer-coated wire according to the present embodiment in a mesh shape. Also, although a braided stent has been described as an example of the stent 100 here, the stent is not limited thereto, and may be, for example, a knitted stent made using the polymer-coated wire.
[0028] In the embodiment, the stent 100 may be formed of a polymer-coated wire having a polymer fiber containing a drug. That is, the stent 100 may function as a drug-eluting stent (DES). In this case, a drug may be added to the spinning solution in the above-mentioned spinning solution preparation process. Here, the polymer concentration of the spinning solution is preferably 5 wt% or more and 10 wt% or less, more preferably 8 wt%. In addition, the direct current voltage applied to the nozzle 112 by the voltage application unit 114 is preferably 8 kV to 12 kV or less, more preferably 10 kV. In addition, when polylactic acid is adopted as the polymer contained in the spinning solution, the weight average molecular weight of polylactic acid may be appropriately selected within the range of 10,000 to 300,000 depending on the amount and period of sustained release of the drug. Here, the smaller the molecular weight, the faster the decomposition and the greater the sustained release rate. In addition, the amount of drug added may be set so that an appropriate amount can be sustainedly released within a period required for treatment at each application site in the body. As the drug, at least one selected from the group consisting of limus drugs such as sirolimus, pimecrolimus, tacrolimus, everolimus, zotarolimus, novolimus, myolimus, temsirolimus, deforolimus, or biolimus, and taxane drugs such as paclitaxel can be used. Alternatively, as the drug, for example, anticancer drugs, immunosuppressants, antibiotics, antirheumatic drugs, antithrombotic drugs, HMG-CoA reductase inhibitors, insulin resistance improving drugs, ACE inhibitors, calcium antagonists, antihyperlipidemic drugs, integrin inhibitors, antiallergic drugs, antioxidants, GPIIb / IIIa antagonists, retinoids, flavonoids, carotenoids, lipid improving drugs, DNA synthesis inhibitors, tyrosine kinase inhibitors, antiplatelet drugs, anti-inflammatory drugs, biological materials, interferons, nitric oxide production promoters, etc. may be used.
[0029] In an embodiment, after preparing the stent 100 from a polymer-coated wire having drug-containing polymer fibers, a drug-containing layer forming step may be performed in which a drug is applied to the surface of the polymer coating of the polymer-coated wire constituting the stent 100 by a coating method such as dipping or spraying to form a drug-containing layer that supports the drug. In this case, the drug supported in the drug-containing layer is rapidly introduced into the affected tissue in the early stage after the stent 100 is placed in the body cavity, and the drug contained in the polymer fiber is gradually released as the polymer fiber decomposes. Here, when a limus drug is supported on the surface of the polymer-coated wire, the surface density is 1 μg / mm 2 More than 10μg / mm 2 It is preferable that: EXAMPLES
[0030] The polymer-coated wire manufacturing method and the polymer-coated wire according to the present invention will be described based on the examples. The wires according to Examples 1 to 6 were all made of a Co-Cr alloy with a diameter of 30 μm. The spinning solutions according to Examples 1 to 6 were all made by dissolving poly-L-lactic acid (PLLA) in CHCl3, using trichloromethane (CHCl3) as an organic solvent. The concentration of PLLA was 5% to 7.5% in all cases. The voltage applied to the nozzle 112 of the spinning solution discharge unit 11 was 10 kV, and the distance between the tip of the nozzle 112 and the part of the wire W facing the electrode 14 was set to 5 cm. Furthermore, the acute angle between the discharge direction of the spinning solution from the nozzle 112 and the rotation axis direction of the electrode 14 was set to 45 degrees. The rotation speeds of the electrode 14 and the support unit 13 and the movement speed of the wire W during the production of the polymer-coated wires according to Examples 1 to 6 are as shown in Table 1 below.
[0031] [Table 1]
[0032] Fig. 4(A) is an SEM photograph of the wire before the polymer fiber is wound around it, and Fig. 4(B), Fig. 5(A), Fig. 5(B) and Fig. 6 are SEM photographs of the polymer-coated wires according to Examples 1 to 4, respectively. From the SEM photographs shown in Fig. 4(B) to Fig. 6, it was found that the acute angle between the extension direction of the polymer fiber wound around the wire W and the central axis direction of the wire W becomes smaller as the rotation speed of the electrode 14 increases and the moving speed of the wire W increases.
[0033] 7(A) and (B) show SEM photographs of the polymer-coated wires according to Examples 5 and 6, respectively. From the SEM photographs shown in Figs. 7(A) and (B), it was found that when the rotation speed of the electrode 14 was 1500 rpm and the moving speed of the wire W was 226 cm / min, the winding direction of the polymer fiber wound around the wire W was relatively uniform. On the other hand, it was found that when the rotation speed of the electrode 14 was reduced to 1000 rpm and the moving speed of the wire W was reduced to 28.3 cm / min, the winding direction of the polymer fiber wound around the wire W became non-uniform.
[0034] The polymer-coated wire according to Example 2 was subjected to the above-mentioned heat treatment and cooling processes to produce the polymer-coated wire according to Comparative Examples 1 to 3 and Example 7. The heat treatment process was performed for a period of 10 seconds. The heat treatment process was performed at temperatures of 170°C, 175°C, 180°C, and 200°C in Comparative Examples 1 to 3 and Example 7, respectively. Figures 8(A), 8(B), 9(A), and 9(B) show SEM photographs of the polymer-coated wire according to Comparative Examples 1 to 3 and Example 7, respectively. From the SEM photographs shown in Figures 8(A) to 9(B), it was found that at a treatment temperature of 180°C or less, some of the polymer fibers remained unmelted, whereas at a treatment temperature of 200°C, the polymer fibers were all melted and only the polymer coating was formed. This shows that a treatment temperature of 200°C or more is sufficient to form a good polymer coating. Figures 10(A) and (B) are SEM photographs of the polymer-coated wire of Example 7. Figures 10(A) and (B) show that the polymer-coated wire of Example 7 has a good polymer coating formed on the surface of the wire W. From these results, when producing a polymer-coated wire having a polymer coating, the treatment temperature in the heat treatment step is preferably 200°C or higher. [Industrial Applicability]
[0035] The present invention is suitable as a wire material for a stent. [Explanation of symbols]
[0036] 1: polymer-coated wire manufacturing apparatus, 11: spinning solution discharge section, 13: support section, 14: electrode, 16: rotation drive section, 21: supply reel, 22, 23: guide rollers, 24: recovery section, 100: stent, 101: polymer-coated wire, 111: syringe, 112: nozzle, 112a: tip section, 113: plunger, 114: voltage application section, 131: main section, 131a: opening, 132: cylindrical section, 161: second friction wheel, 162: motor, 163: timing belt, 164: first friction wheel, 241: take-up reel, 242: reel drive section, FB: polymer fiber, A1: projection area, W: wire
Claims
1. a polymer winding step of rotating an electrode disposed so as to surround a wire at a preset rotation speed around the wire and moving the wire relative to the electrode in a direction of a rotation axis of the electrode at a preset moving speed, while discharging a spinning solution in which at least one type of polymer is dissolved in at least one type of solvent from the nozzle while maintaining the nozzle at a higher potential than the electrode, thereby discharging the spinning solution from the nozzle toward a portion of the wire facing the electrode in a direction perpendicular to the direction of the rotation axis, thereby winding a polymer fiber generated from the spinning solution around the wire. Polymer-coated wire manufacturing method.
2. a heat treatment step of heating the wire having the polymer layer made of the polymer fiber formed thereon after the polymer winding step to melt the polymer fiber; and a cooling step of cooling the wire after the heat treatment step to form a polymer coating on the surface of the wire.
2. The method for producing a polymer-coated wire according to claim 1.
3. The rotation speed is 100 rpm or more and 2000 rpm or less.
3. A method for producing a polymer-coated wire according to claim 1 or 2.
4. The moving speed is 25 cm / min or more and 120 cm / min or less. The method for producing a polymer-coated wire according to any one of claims 1 to 3.
5. The spinning solution is prepared by dissolving at least one polymer selected from polyglycolic acid, a copolymer of glycolic acid and L-lactic acid, a copolymer of glycolic acid and DL-lactic acid, poly-L-lactic acid, poly-D-lactic acid, poly-DL-lactic acid, a copolymer of L-lactic acid and ε-caprolactone, and poly-p-dioxanone in an organic solvent. The method for producing a polymer-coated wire according to any one of claims 1 to 4.
6. The wire is made of metal. The method for producing a polymer-coated wire according to any one of claims 1 to 5.
7. The spinning solution contains at least one drug selected from a limus drug and a taxane drug, or a drug selected from an anticancer drug, an immunosuppressant, an antibiotic, an antirheumatic drug, an antithrombotic drug, an HMG-CoA reductase inhibitor, an insulin sensitizer, an ACE inhibitor, a calcium antagonist, an antihyperlipidemic drug, an integrin inhibitor, an antiallergic drug, an antioxidant, a GPIIb / IIIa antagonist, a retinoid, a flavonoid, a carotenoid, a lipid improving drug, a DNA synthesis inhibitor, a tyrosine kinase inhibitor, an antiplatelet drug, an anti-inflammatory drug, a biomaterial, an interferon, and a nitric oxide production promoter. The method for producing a polymer-coated wire according to any one of claims 1 to 6.
8. The method further includes a drug-containing layer forming step of forming a drug-containing layer covering the polymer coating by applying a drug solution containing the drug to the surface of the polymer coating after a cooling step of forming a polymer coating on the surface of the wire by cooling the wire. The method for producing a polymer-coated wire according to claim 7.
9. An electrode disposed so as to surround the wire; a rotation drive unit that rotates the electrode around the wire at a preset rotation speed; a take-up reel for taking up the wire; a reel drive unit that rotates the take-up reel to move the wire relative to the electrode in a direction of a rotation axis of the electrode at a preset moving speed; The present invention is provided with a spinning solution discharge unit having a nozzle for discharging a spinning solution in which at least one type of polymer is dissolved in at least one type of solvent, and a voltage application unit for applying a DC voltage between the nozzle and the electrode, and discharging the spinning solution from the nozzle toward a portion of the wire facing the electrode in a direction perpendicular to the direction of the rotation axis while the nozzle is maintained at a higher potential than the electrode. Polymer-coated wire manufacturing equipment.
Citation Information
Patent Citations
stent with collagen
JP1998503663A
Method and apparatus for producing polymeric fiber shells by electrospinning
JP2005507464A
Method and apparatus for doubling nanofiber
JP2010031412A
Method for coating thin wire and coated thin wire produced by the method for coating
JP2013233520A
Spunbond web containing polylactic acid fiber
JP2017527706A