Austenitic stainless steel sheet, manufacturing method thereof and automobile exhaust system part

An austenitic stainless steel sheet with controlled component balances and segregation levels addresses the issue of σ phase precipitation, enhancing heat and corrosion resistance for automobile exhaust system components by optimizing composition and reducing Ni segregation.

JP7595454B2Active Publication Date: 2024-12-06NIPPON STEEL CORPORATION
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020212134
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-22
Publication Date
2024-12-06
Estimated Expiration
2040-12-22

AI Technical Summary

Technical Problem

Existing austenitic stainless steels face challenges in maintaining heat resistance and corrosion resistance due to σ phase precipitation during long-term aging at elevated temperatures, which deteriorates creep properties and localizes Cr concentration, affecting performance in automobile exhaust system components.

Method used

The development of an austenitic stainless steel sheet with controlled component balances and segregation levels, specifically through limiting Ni segregation and optimizing the composition to satisfy specific formulae, thereby reducing σ phase precipitation and enhancing heat and corrosion resistance.

Benefits of technology

The solution provides an austenitic stainless steel sheet with improved heat resistance and corrosion resistance after long-term aging, suitable for automobile exhaust system components, particularly turbochargers, by minimizing σ phase precipitation and maintaining optimal element segregation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007595454000001
    Figure 0007595454000001
  • Figure 0007595454000002
    Figure 0007595454000002
  • Figure 0007595454000003
    Figure 0007595454000003
Patent Text Reader

Abstract

To provide an austenitic stainless steel sheet having excellent heat resistance and corrosion resistance after long-aging in a σ phase precipitation temperature area.SOLUTION: An austenitic stainless steel sheet is adopted that has a predetermined chemical composition and satisfies formula (i): 5[Cr]+6[Si]+9[Mo]-2[Ni]-30[C]-70[N]-100[*Ni] / [Ni]≤0 and formula (ii): 0.80≤[*Ni] / [Ni]<1.00, where, [element symbol] in the formulae each denotes the content (mass%) of the element in steel and [*Ni] denotes an average content of Ni (mass%) in the Ni negative-segregated portion.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an austenitic stainless steel sheet, a method for producing an austenitic stainless steel sheet, and an automobile exhaust system part. [Background technology]

[0002] Exhaust system components such as exhaust manifolds, converters, front pipes, and center pipes of automobiles pass high-temperature exhaust gas discharged from the engine, so the materials that make up the exhaust system components are required to have various properties such as oxidation resistance, high-temperature strength, and thermal fatigue properties. In addition, exhaust system components are required to have excellent corrosion resistance because they are in a condensed water corrosive environment. In addition, stainless steels are often used for these exhaust system components from the perspective of strengthening exhaust gas regulations, improving engine performance, and reducing the weight of the vehicle body. In recent years, exhaust gas regulations have been further strengthened, and exhaust gas temperatures have been increasing due to improvements in fuel efficiency and downsizing. In addition, there are more and more cases where superchargers such as turbochargers are installed, so stainless steels used in exhaust manifolds and turbochargers are required to have even higher heat resistance. The maximum temperature of exhaust gas was previously around 900°C, but it is expected to rise to around 1000°C in the future, and there is a possibility that it will rise to around 1050°C.

[0003] On the other hand, the internal structure of a turbocharger is complex, and it is important to improve the charging efficiency while ensuring heat-resistant reliability, so Ni-based alloys and heat-resistant austenitic stainless steel are mainly used. A typical heat-resistant austenitic stainless steel is SUS310S (25%Cr-20%Ni). In addition, while castings are used for the housing of a turbocharger, there is a demand for thinner heat-resistant austenitic stainless steel sheet metal from the perspective of reducing the weight of the vehicle body.

[0004] From the viewpoint of such an increase in exhaust gas temperature and thinning of parts, it is necessary to further improve the heat resistance of heat-resistant austenitic stainless steel. For example, when the maximum temperature of exhaust gas rises to about 1050°C, the maximum temperature of the exhaust system members and the parts constituting the supercharger will be about 950 to 1000°C, and heat resistance such as creep properties in that temperature range is required. However, the temperature of the parts does not always reach the maximum temperature, and in many cases the time when it is about 900°C, which is lower than the maximum temperature, is long. However, when austenitic stainless steel is aged for a long time at about 900°C, the σ phase precipitates. When the σ phase precipitates, there is a concern that the creep properties will decrease. In addition, since the σ phase is a phase with a high Cr concentration, there is a concern that the Cr concentration in the steel in the vicinity of the σ phase will locally decrease, resulting in a decrease in corrosion resistance. In other words, when developing heat-resistant austenitic stainless steel, it has become necessary to take into account the creep properties and corrosion resistance at around 950 to 1000°C after long-term aging at around 900°C. This means that it is necessary not only to simply improve the heat resistance and corrosion resistance of heat-resistant austenitic stainless steel, but also to develop technology that suppresses the precipitation of σ-phase during long-term aging at around 900°C.

[0005] Patent Document 1 describes how the creep properties of heat-resistant austenitic stainless steel are improved by determining the optimum ranges for the contents of Nb, V, C, N, Al, and Ti and optimizing the manufacturing process. However, the technology described in Patent Document 1 is related to improving creep properties at 800°C, and does not take into account heat resistance in the range above 900°C.

[0006] Patent Document 2 describes a technique for improving creep properties by controlling the characteristics of grain boundaries in the metal structure of heat-resistant austenitic stainless steel. However, the technique described in Patent Document 2 relates to creep properties at 900°C and 950°C, and creep properties at 1000°C are not considered. In addition, creep properties and corrosion resistance that take into account σ precipitation due to long-term aging at around 900°C are not considered.

[0007] Patent Document 3 describes that the high-temperature strength at 1000°C of heat-resistant austenitic stainless steel after aging at 1000°C is improved by controlling the component balance of N and Nb. However, since the σ phase is difficult to precipitate at 1000°C, Patent Document 3 does not take into consideration the precipitation of the σ phase. In addition, the corrosion resistance taking into consideration the precipitation of the σ phase is not examined. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2013-209730 A [Patent Document 2] JP 2019-218588 A [Patent Document 3] Patent No. 5605996 Summary of the Invention [Problem to be solved by the invention]

[0009] An object of the present invention is to provide an austenitic stainless steel sheet having excellent heat resistance and corrosion resistance after long-term aging in the σ-phase precipitation temperature range, a method for producing an austenitic stainless steel sheet, and an automobile exhaust system part. [Means for solving the problem]

[0010] In order to solve the above problems, the present inventors have intensively studied the effects of various components and component segregation inside the base material on the creep properties and corrosion resistance of austenitic stainless steel sheets after aging. As a result, they have found that σ-phase precipitation after aging reduces creep properties and corrosion resistance. They have also found that the σ-phase precipitation after aging is influenced by the component balance of the steel, and that when Ni segregation is large, the σ-phase precipitation increases. When Ni segregation is large, especially in the Ni negative segregation part, which is a region in the steel sheet cross section where the Ni concentration is lower than the Ni content in the steel, σ-precipitation is more likely to occur because the Ni concentration is lower than the Ni content in the steel, and further, in the Ni negative segregation part, other elements are further micro-segregated, causing micro-segregation that is more likely to cause local σ-precipitation, making it more likely to cause σ-precipitation. Based on these findings, they have invented an austenitic stainless steel sheet that has excellent heat resistance and corrosion resistance after long-term aging in the σ-phase precipitation temperature range.

[0011] That is, the gist of the present invention, which aims to solve the above problems, is as follows. (1) In mass percent, C: 0.001% or more, 0.300% or less, N: 0.001% or more, 0.45% or less, Si: 0.10% or more, 5.00% or less, Mn: 0.10% or more, 12.00% or less, P:0.060% or less, S: 0.0200% or less, Cr: 15.0% or more, 35.0% or less, Ni: 2.0% or more, 35.0% or less, Cu: 0.001% or more, 5.00% or less, Mo: 0.001% or more, 5.00% or less, Al: 0.001% or more, 1.000% or less, V: 0.01% or more, 1.00% or less, B: 0.0001% or more, 0.0100% or less, Ca: 0.0001% or more, 0.0200% or less, O: 0.0150% or less, and the balance being Fe and impurities, and satisfying the following formulas (i) and (ii): 5[Cr]+6[Si]+9[Mo]-2[Ni]-30[C]-70[N]-100[*Ni] / [Ni]≦0 Formula (i) 0.80≦[*Ni] / [Ni]<1.00 formula (ii) In the formulas (i) and (ii), the [element symbol] means the content (mass%) of the corresponding element in the steel, and [*Ni] means the average Ni content (mass%) in the Ni-negative segregation portion. (2) In mass percent, C: 0.001% or more, less than 0.080%, N: more than 0.20%, less than 0.39%, Si: more than 1.00%, less than 3.00%, Mn: 0.80% or more, 3.00% or less, P: 0.050% or less, S: 0.0018% or less, Cr:20.0% or more, 35.0% or less, Ni: more than 8.0%, less than 25.0%, Cu: 0.001% or more, 3.40% or less, Mo: 0.001% or more, less than 0.50% Al: more than 0.005%, less than 0.130%, V: 0.01% or more, 1.00% or less, B: 0.0001% or more, 0.0100% or less, Ca: 0.0001% or more, 0.0200% or less, O: 0.0150% or less, and the balance being Fe and impurities, and satisfying the following formulas (iii) and (iv): 5[Cr]+6[Si]+9[Mo]-2[Ni]-30[C]-70[N]-100[*Ni] / [Ni]≦0...Formula (iii) 0.80≦[*Ni] / [Ni]<1.00 Equation (iv) In the formulas (iii) and (iv), the [element symbol] means the content (mass%) of the corresponding element in the steel, and [*Ni] means the average Ni content (mass%) in the Ni-negative segregation portion. (3) Part of Fe is replaced by, in mass%, Ti: 0.001% or more, 1.00% or less, Nb: 0.001% or more, 1.00% or less, W: 0.01% or more, 3.00% or less, Y: 0.001% or more, 0.50% or less, REM: 0.001% or more, 0.50% or less, Zr: 0.01% or more, 0.50% or less, Hf: 0.001% or more, 1.0% or less, Sn: 0.001% or more, 1.0% or less, Mg: 0.0001% or more, 0.0100% or less, Co: 0.01% or more, 1.00% or less, Sb: 0.001% or more, 0.50% or less, Bi: 0.001% or more, 1.0% or less, Ta: 0.001% or more, 1.0% or less, Ga: 0.0001% or more, 0.50% or less, The present invention is characterized in that it contains one or more of the following: (2) 2. The austenitic stainless steel sheet according to claim 1 . (4) In mass percent, C: 0.001% or more, 0.300% or less, N: 0.001% or more, 0.45% or less, Si: 0.10% or more, 5.00% or less, Mn: 0.10% or more, 12.00% or less, P:0.060% or less, S: 0.0200% or less, Cr: 15.0% or more, 35.0% or less, Ni: 2.0% or more, 35.0% or less, Cu: 0.001% or more, 5.00% or less, Mo: 0.001% or more, 1.50% or less, Al: 0.001% or more, 1.000% or less, V: 0.01% or more, 1.00% or less, B: 0.0001% or more, 0.0100% or less, Ca: 0.0001% or more, 0.0200% or less, O: 0.0150% or less, Contains Furthermore, Ti: 0.001% or more, 1.00% or less, Nb: 0.001% or more, 1.00% or less, W: 0.01% or more, 3.00% or less, Y: 0.001% or more, 0.50% or less, REM: 0.001% or more, 0.50% or less, Zr: 0.01% or more, 0.50% or less, Hf: 0.001% or more, 1.0% or less, Sn: 0.0001% or more, 1.0% or less, Mg: 0.0001% or more, 0.0100% or less, Co: 0.01% or more, 1.00% or less, Sb: 0.001% or more, 0.50% or less, Bi: 0.001% or more, 1.0% or less, Ta: 0.001% or more, 1.0% or less, Ga: 0.0001% or more, 0.50% or less, Contains one or more of the following: An austenitic stainless steel sheet, the balance of which is Fe and impurities, and which satisfies the following formulas (i) and (ii): 5[Cr]+6[Si]+9[Mo]-2[Ni]-30[C]-70[N]-100[*Ni] / [Ni]≦0 Formula (i) 0.80≦[*Ni] / [Ni]<1.00 formula (ii) In the formulas (i) and (ii), the [element symbol] means the content (mass%) of the corresponding element in the steel, and [*Ni] means the average Ni content (mass%) in the Ni-negative segregation portion. ( 5 ) Used in automobile exhaust system components, (1)~( 4 ) The austenitic stainless steel sheet according to any one of claims 1 to 4. ( 6 ) (1) ~ ( 5 2. A method for producing an austenitic stainless steel sheet according to claim 1, wherein the thickness A (mm) of the slab during casting, the thickness B (mm) of the final product, the final annealing temperature C (°C), and the final annealing time D (seconds) satisfy the following formula (v): 50≦(C×D) / (A×B)≦700...Formula (v) ( 7 ) (1) ~ ( 52. An automobile exhaust system part comprising an automobile exhaust system member made of the austenitic stainless steel sheet according to any one of claims 1 to 11. Effect of the Invention

[0012] According to the present invention, it is possible to provide an austenitic stainless steel sheet having excellent heat resistance and corrosion resistance after long-term aging in the σ-phase precipitation temperature range, a method for producing an austenitic stainless steel sheet, and an automobile exhaust system part.

[0013] The austenitic stainless steel sheet according to the present invention can be applied to automobile exhaust system members such as turbocharger parts, exhaust manifolds, and converters. In particular, it can be suitably applied to turbochargers mounted on gasoline and diesel vehicles. In the case of turbochargers, it can be applied to a housing constituting the exterior. It can also be suitably applied to precision parts inside nozzle vane type turbochargers, such as back plates, oil deflectors, compressor wheels, nozzle mounts, nozzle plates, nozzle vanes, drive rings, and drive levers. However, the uses of the austenitic stainless steel sheet according to the present invention are not limited to these uses. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The present invention will be described in detail below. In the following description, "X negative segregation portion" refers to a region in the steel sheet cross section where the average content of element X is less than the content of element X in the steel. Also, "X positive segregation portion" refers to a region in the steel sheet cross section where the average content of element X exceeds the content of X in the steel. For example, Ni negative segregation portion refers to a region in the steel sheet cross section where the average Ni content is less than the Ni content in the steel. Also, Cr positive segregation portion refers to a region in the steel sheet cross section where the average Cr content exceeds the Cr content in the steel.

[0015] First, the reasons for limiting the steel composition of the austenitic stainless steel sheet of the present invention will be described. Here, "%" in the steel composition means mass %.

[0016] (C: 0.001% or more, 0.300% or less) Since C is an element that improves high-temperature strength and creep properties, the C content is set to 0.001% or more. In addition, in consideration of manufacturing costs, the C content is preferably set to 0.010% or more. The C content is more preferably set to 0.020% or more. However, since an excessive C content reduces oxidation resistance and intergranular corrosion resistance, the C content is set to 0.300% or less. In addition, in consideration of further improvement of corrosion resistance after aging in the σ precipitation temperature range, the C content is preferably set to less than 0.080%. More preferably, it is set to 0.075% or less.

[0017] (N: 0.001% or more, 0.45% or less) Since N is an element that improves high-temperature strength and creep properties, the N content is set to 0.001% or more. In consideration of manufacturing costs, the N content is preferably set to 0.030% or more. In consideration of further improvement of creep properties after aging in the σ precipitation temperature range, the N content is more preferably set to more than 0.20%. However, since excessive N content causes void defects, the N content is set to 0.45% or less. In consideration of high-temperature fatigue properties, the N content is preferably set to 0.39% or less. In consideration of workability, the N content is more preferably set to 0.32% or less. Even more preferably, the N content is set to 0.28% or less.

[0018] (Si: 0.10% or more, 5.00% or less) Since Si is an element contained as a deoxidizer and also improves oxidation resistance, the Si content is set to 0.10% or more. Since Si is also an element that improves workability, it is preferable that the Si content is set to 0.40% or more. Furthermore, in consideration of scale spalling resistance, the Si content is more preferably set to more than 1.00%. Even more preferably, it is set to 1.50% or more. However, since excessive Si content reduces hot workability and pickling property during manufacturing, the Si content is set to 5.00% or less. Furthermore, Si is an element that promotes σ precipitation, and in consideration of further improvement of creep properties after aging in the σ precipitation temperature range, the Si content is preferably set to 3.00% or less. Furthermore, in consideration of solidification cracking property during welding, the Si content is more preferably set to 2.50% or less. Even more preferably, it is set to 2.20% or less.

[0019] (Mn: 0.10% or more, 12.00% or less) Mn is an element contained as a deoxidizer, and the Mn content is set to 0.10% or more. In consideration of refining costs, the Mn content is more preferably set to 0.40% or more. Furthermore, Mn is an element that improves the solid solubility limit of N, and in consideration of increasing the N content to further improve creep properties after aging in the σ precipitation temperature range, the Mn content is more preferably set to 0.80% or more. Even more preferably, it is set to 1.00% or more. However, since excessive Mn content reduces oxidation resistance, the Mn content is set to 12.00% or less. In consideration of scale peeling resistance, the Mn content is preferably set to 3.00% or less. In consideration of pickling property and workability during manufacturing, the Mn content is more preferably set to 2.30% or less. Even more preferably, it is set to 1.80% or less.

[0020] (P:0.060% or less) P is an impurity that is mainly mixed in from raw materials during steel refining, and is an element that reduces toughness and weldability, so the P content is set to 0.060% or less. In consideration of high-temperature fatigue properties, the P content is preferably set to 0.050% or less. In consideration of manufacturability, the P content is more preferably set to 0.040% or less. Even more preferably, the P content is set to 0.035% or less. However, since an excessive reduction leads to an increase in refining costs, the P content may be set to 0.001% or more. The P content may be set to 0.010% or more.

[0021] (S:0.200% or less) S is an impurity that is mainly mixed in from raw materials during steel refining, and is an element that reduces hot workability and corrosion resistance during manufacturing, so the S content is set to 0.200% or less. In addition, in consideration of scale spalling resistance, the S content is preferably set to 0.0018% or less. More preferably, it is set to 0.0014% or less. Even more preferably, it is set to 0.0012% or less. However, since an excessive reduction leads to an increase in refining costs, the S content may be set to 0.0001% or more. Furthermore, the S content may be set to 0.0003% or more.

[0022] (Cr:15.0% or more, 35.0% or less) Since Cr is an element that improves corrosion resistance, the Cr content is set to 15.0% or more. In addition, in consideration of oxidation resistance, the Cr content is preferably set to 18.0% or more. Furthermore, Cr is an element that improves the solid solubility limit of N, and in consideration of increasing the N content to further improve creep properties after aging in the σ precipitation temperature range, the Cr content is more preferably set to 20.0% or more. However, since excessive Cr content reduces hot workability and pickling property during manufacturing, the Cr content is set to 35.0% or less. In consideration of workability and raw material cost, the Cr content is preferably set to 30.0% or less. More preferably, it is set to 26.0% or less.

[0023] (Ni: 2.0% or more, 35.0% or less) Since Ni is an element that improves corrosion resistance, the Ni content is set to 2.0% or more. In addition, in consideration of further improvement of creep properties after aging in the σ precipitation temperature range, the Ni content is preferably more than 8.0%. More preferably, it is 10.0% or more. However, since excessive Ni content reduces formability, the Ni content is set to 35.0% or less. In addition, Ni is an element that easily segregates, and if the Ni content is high, Ni segregation expands, and σ precipitation is promoted in the Ni negative segregation part where the Ni concentration is lower than the surroundings. Therefore, in consideration of further improvement of creep properties after aging in the σ precipitation temperature range, the Ni content is preferably set to 25.0% or less. In addition, in consideration of raw material costs, the Ni content is more preferably 20.0% or less. Even more preferably, it is 15.0% or less.

[0024] (Cu: 0.001% or more, 5.00% or less) Since Cu is an element that improves corrosion resistance, the Cu content is set to 0.001% or more. Furthermore, in consideration of manufacturability, the Cu content is preferably set to 0.05% or more. However, since an excessive Cu content reduces hot workability during manufacturing, the Cu content is set to 5.00% or less. Furthermore, in consideration of scale spalling resistance, the Cu content is preferably set to 3.40% or less. Furthermore, in consideration of raw material costs, the Cu content is more preferably set to 2.00% or less. Furthermore, in consideration of oxidation resistance, the Cu content is even more preferably set to 1.00% or less. Even more preferably, the Cu content is 0.40% or less.

[0025] (Mo: 0.001% or more, 5.00% or less) Mo is an element that improves corrosion resistance, so the Mo content is set to 0.001% or more. In consideration of manufacturability, the Mo content is preferably set to 0.01% or more, and more preferably 0.05% or more. However, since an excessive Mo content reduces workability, the Mo content is set to 5.00% or less. In consideration of raw material costs, the Mo content is preferably set to 1.50% or less. Furthermore, Mo is an element that promotes σ precipitation, and in consideration of further improvement of creep properties after aging in the σ precipitation temperature range, the Mo content is more preferably set to less than 0.50%.

[0026] (Al: 0.001% or more, 1.000% or less) Since Al is an element contained as a deoxidizing element, the Al content is set to 0.001% or more. Furthermore, in consideration of oxidation resistance and refining costs, the Al content is preferably more than 0.005%, and more preferably 0.010% or more. However, since an excessive Al content deteriorates surface quality, the Al content is set to 1.000% or less. Furthermore, in consideration of high-temperature fatigue properties, the Al content is preferably set to 0.130% or less. Furthermore, in consideration of manufacturability, the Al content is more preferably set to 0.080% or less, and even more preferably 0.070% or less.

[0027] (V: 0.01% or more, 1.00% or less) Since V is an element that improves corrosion resistance and high-temperature strength, the V content is set to 0.01% or more. Furthermore, in consideration of refining costs, the V content is preferably set to 0.03% or more, and more preferably 0.05% or more. However, since an excessive V content reduces manufacturability, the V content is set to 1.00% or less. Furthermore, in consideration of surface quality, the V content is preferably set to 0.20% or less, and more preferably less than 0.15%.

[0028] (B: 0.0001% or more, 0.0100% or less) Since B is an element that improves corrosion resistance and high-temperature strength, the B content is set to 0.0001% or more. In addition, in consideration of hot workability during manufacturing, the B content is preferably set to 0.0002% or more. More preferably, it is set to 0.0003% or more. However, since an excessive B content deteriorates the surface properties of the steel surface, the B content is set to 0.0100% or less. In consideration of manufacturability, the B content is preferably set to 0.0050% or less. In consideration of formability, the B content is more preferably set to 0.0030% or less. Even more preferably, it is set to 0.0015% or less.

[0029] (Ca: 0.0001% or more, 0.0200% or less) Since Ca is an element that promotes desulfurization, the Ca content is set to 0.0001% or more. Furthermore, in consideration of scale spalling resistance, the Ca content is preferably set to 0.0002% or more. However, since excessive Ca content may lead to a decrease in corrosion resistance due to the formation of CaS, a water-soluble inclusion, the Ca content is set to 0.0200% or less. Furthermore, in consideration of manufacturability, the Ca content is more preferably set to 0.0050% or less. Even more preferably, it is set to 0.0030% or less.

[0030] (O:0.0150% or less) O is an unavoidably contained impurity that causes surface defects due to bubbles and inclusions, and also reduces corrosion resistance and oxidation resistance, so the O content is set to 0.0150% or less. In addition, in consideration of manufacturability, the O content is preferably set to 0.0050% or less, and more preferably 0.0035% or less. However, since excessive reduction of O increases refining costs, the O content may be set to 0.0001% or more. The O content may be 0.0003% or more. Here, the O content means the total content including oxygen dissolved in the steel and oxygen in oxides present in the steel.

[0031] In the austenitic stainless steel sheet according to this embodiment, the balance other than the above-mentioned elements is Fe and impurities. However, elements other than the above-mentioned elements may also be contained within a range that does not impair the effects of this embodiment. Note that the impurities referred to here refer to components that are mixed in due to various factors in raw materials such as ores and scraps and manufacturing processes when the austenitic stainless steel according to the present invention is industrially manufactured, and are permissible within a range that does not adversely affect the present invention.

[0032] Next, the formulas (i) to (iv) will be described.

[0033] The present inventors, while examining various influences on creep properties and corrosion resistance after aging of austenitic stainless steel sheets, found that in addition to Cr, Si, Mo, Ni, C, and N, Ni segregation in the base material has a large influence, and that the balance of these is important. Therefore, in this embodiment, it is necessary to satisfy formulas (i) to (iv). However, in the present invention, formulas (i) and (iii) are the same formula, and formulas (ii) and (iv) are the same formula, so here we will explain formulas (i) and (ii), and then we will also explain formulas (ii) and (iv).

[0034] 5[Cr]+6[Si]+9[Mo]-2[Ni]-30[C]-70[N]-100[*Ni] / [Ni]≦0 Formula (i)

[0035] 0.80≦[*Ni] / [Ni]<1.00 formula (ii)

[0036] In the formulas (i) and (ii), the symbol of an element means the content (% by mass) of the element in the steel, and *Ni means the average content (% by mass) of Ni in the Ni-negative segregation region.

[0037] If the value of the left side of formula (i) is more than 0, the steel's composition balance is favorable for σ precipitation, and Ni segregation is large. If the Ni negative segregation is large, the Ni content in the Ni negative segregation portion is low, making σ precipitation more likely, and other elements further micro-segregate in the Ni negative segregation portion, causing micro-segregation that is favorable for local σ precipitation, making σ precipitation more likely. Therefore, formula (i) must be satisfied. More preferably, the value of the left side of formula (i) is -65 or more and -1 or less.

[0038] Moreover, if the value of the middle part of formula (ii) is less than 0.80, the Ni negative segregation is large. Moreover, if the value of the middle part of formula (ii) is 1.00 or more, it means that there is no Ni segregation. However, eliminating Ni segregation completely requires a large amount of heat treatment cost and time, which greatly impairs the economic efficiency. Therefore, it is necessary to satisfy formula (ii). The value of the middle part of formula (ii) is more preferably 0.85 or more and 0.98 or less.

[0039] In addition, when the negative segregation of Ni is large, the positive segregation of Cr, Mo, and Si is also large, and it is considered that σ is easily precipitated in the positive segregation parts of these elements. It is considered that the balance of these Cr, Mo, and Si also has an effect, and it is preferable to satisfy conditions 1 to 3 as preferable conditions. Note that, in condition 2, it is sufficient to satisfy either formula (B) or formula (C), and in condition 3, it is sufficient to satisfy either formula (D) or formula (E).

[0040] (Condition 1) 1.00<[**Cr] / [Cr]≦1.30...Formula (A)

[0041] (Condition 2) [**Mo]≦0.80 (B) or 1.00<[**Mo] / [Mo]≦1.30...Formula (C)

[0042] (Condition 3) [**Si]≦0.80 Formula (D) or 1.00<[**Si] / [Si]≦1.30...Equation (E)

[0043] In the formulas (A) to (E), the [element symbol] means the content (mass%) of the corresponding element in the steel, and the [**element symbol] means the average content (mass%) of the corresponding element in the positive segregation portion of the corresponding element.

[0044] The identification of the Ni-negative segregation part of the austenitic stainless steel sheet according to this embodiment (hereinafter, sometimes referred to as the test material) and the average Ni content in the Ni-negative segregation part are calculated by analyzing the steel sheet cross section with an electron probe microanalyzer (EPMA) as follows. For the EPMA, for example, a JXA-8230 model manufactured by JEOL Ltd. is used. The electron gun is LaB6, and the analysis conditions are set to an acceleration voltage of 15 kV, an irradiation current of 325 nA, and a beam diameter of 5 μm. For the spectrometer, for example, an XM-86030 model manufactured by JEOL Ltd. is used. LiF is used as the analyzing crystal, and the relative intensity of NiKα rays is obtained as the characteristic X-rays, and converted to concentration using a calibration curve.

[0045] For the calibration curve samples for Ni concentration measurement, austenitic stainless steel samples are prepared with the Ni content varied by mass% to 8%, 12%, 20%, and 30% based on SUS304. The Ni content in the calibration curve samples and test steel is analyzed to two decimal places using the ICP atomic emission spectrometry method specified in JIS G 1258, and the positive value is used.

[0046] The positions to be analyzed by EPMA are as follows. In the measurement area of ​​the calibration curve sample or test material, spanning 2 mm in the longitudinal direction of the cross section and the entire thickness, analysis points are set in a grid pattern at 5 μm intervals, and point analysis is performed at each measurement point. This is performed in five measurement areas. The average element content at each measurement point is then taken as the measured value for each element in the steel. A basic calibration curve is created using the content of each element (e.g., Ni content) measured by ICP in the calibration curve sample and the relative intensity of the characteristic X-ray (Kα ray in the case of Ni) measured by EPMA. In addition, the calibration curve is corrected so that the content of each element in the steel measured by ICP (e.g., Ni content) and the content of each element in the steel measured by EPMA (e.g., Ni content) match for each test material.

[0047] The identification of Ni-negative segregation areas and the average Ni content in the Ni-negative segregation areas are determined as follows. If the Ni content at each analysis point at 5 μm intervals measured by EPMA is less than the Ni content in the steel described above, the analysis point is considered to be a Ni-negative segregation area. The average value of the Ni content at each analysis point that is determined to be a Ni-negative segregation area is taken as the average Ni content in the Ni-negative segregation area. The identification and average contents of Cr, Mo and Si positive segregation areas are also determined in the same manner as the identification of Ni-negative segregation areas and the analysis and calculation of the average Ni content. NiKα rays, CrKα rays, MoLα rays and SiKα rays are used as characteristic X-rays, respectively.

[0048] For the calibration curve samples, austenitic stainless steel samples were prepared with varying elemental contents based on SUS304 for each element. The Cr contents of the calibration curve samples for measuring Cr concentration were 10%, 18%, 26%, and 35% by mass, the Mo contents of the calibration curve samples for measuring Mo concentration were 0.5%, 1%, 3%, and 5% by mass, and the Si contents of the calibration curve samples for measuring Si concentration were 0.5%, 1%, 3%, and 5% by mass.

[0049] The austenitic stainless steel plate of the present embodiment contains the above-mentioned X-negative segregation portion and X-positive segregation portion. Specifically, at least Ni-negative segregation portion may be contained, and Cr-positive segregation portion, Mo-positive segregation portion, or Si-positive segregation portion may be contained.

[0050] Furthermore, in the austenitic stainless steel sheet according to this embodiment, the properties can be further improved by selectively containing one or more of Ti, Nb, W, Y, REM, Zr, Hf, Sn, Mg, Co, Sb, Bi, Ta, and Ga as necessary. These elements are described below. Note that these elements do not necessarily have to be contained, so the lower limit of the content of each of these elements is 0%.

[0051] (Ti: 0.001% or more, 1.00% or less) Ti is an element that combines with C, N, and S to improve corrosion resistance, intergranular corrosion resistance, and deep drawability, and is preferably contained at 0.001% or more as necessary. More preferably, it is 0.003% or more, and even more preferably, it is 0.005% or more. However, since excessive Ti content may lead to a decrease in hole expansion workability due to the formation of coarse Ti-based precipitates, it is preferable that the Ti content be 1.00% or less. In addition, in consideration of uniform elongation, it is more preferable that the Ti content be 0.30% or less. In addition, in consideration of the occurrence of surface defects and toughness, it is even more preferable that the Ti content be 0.25% or less.

[0052] (Nb:0.001%, 1.00% or less) Nb is an element that contributes to improving high-temperature strength and intergranular corrosion resistance, and is preferably contained at 0.001% or more as necessary. More preferably, it is 0.005% or more, and even more preferably, it is 0.01% or more. However, since excessive Nb content may lead to an increase in raw material costs and a decrease in manufacturability, it is preferable that the Nb content is 1.00% or less. In addition, in consideration of uniform elongation, hole expandability, and manufacturability, the Nb content is more preferably 0.60% or less. Even more preferably, it is 0.50% or less.

[0053] (W: 0.01% or more, 3.00% or less) W is an element that improves high-temperature strength, and is preferably contained at 0.01% or more as necessary. In addition, W is also an element that improves corrosion resistance, so the W content is more preferably 0.05% or more. However, since excessive W content may lead to a decrease in toughness, the W content is preferably 3.00% or less. In consideration of raw material costs, the W content is more preferably 0.50% or less. In consideration of manufacturability, the W content is even more preferably 0.40% or less.

[0054] (Y: 0.001% or more, 0.50% or less) Y is an element that improves the cleanliness of steel, rust resistance, hot workability, and oxidation resistance, and is preferably contained at 0.001% or more as necessary. More preferably, it is 0.003% or more. However, since an excessive Y content may lead to a decrease in manufacturability, it is preferable that the Y content be 0.50% or less. In addition, taking into consideration the raw material cost, it is more preferable that the Y content be 0.20% or less. Even more preferably, it is 0.10% or less.

[0055] (REM: 0.001% or more, 0.50% or less) REM (rare earth metal) is an element that improves the cleanliness of steel, rust resistance, hot workability, and oxidation resistance, and is preferably contained at 0.001% or more as necessary. More preferably, it is 0.003% or more. However, since excessive REM content may lead to a decrease in manufacturability, it is preferable to set the REM content to 0.50% or less. In addition, considering the raw material cost, it is more preferable to set the REM content to 0.20% or less. Even more preferably, it is 0.10% or less. REM refers to a collective term for 15 elements (lanthanoids) from scandium (Sc) and lanthanum (La) to lutetium (Lu). As REM, one of the above elements may be contained alone, or two or more may be contained. When two or more of the above elements are contained as REM, the REM content is the total content of those elements.

[0056] (Zr: 0.01% or more, 0.50% or less) Zr is an element that improves corrosion resistance, intergranular corrosion resistance, high-temperature strength, and oxidation resistance, and is preferably contained at 0.01% or more as necessary. More preferably, it is 0.03% or more. However, since excessive Zr content may lead to a decrease in manufacturability, it is preferable that the Zr content be 0.50% or less. In addition, taking into consideration the raw material cost, it is more preferable that the Zr content be 0.30% or less. Even more preferably, it is 0.20% or less.

[0057] (Hf: 0.001% or more, 1.0% or less) Hf is an element that improves corrosion resistance, intergranular corrosion resistance, high-temperature strength, and oxidation resistance, and is preferably contained at 0.001% or more as necessary. More preferably, it is contained at 0.003% or more. However, since excessive Hf content may lead to a decrease in manufacturability, it is preferable that the Hf content be 1.0% or less. More preferably, it is 0.5% or less.

[0058] (Sn: 0.0001% or more, 1.0% or less) Sn is an element that improves corrosion resistance and high-temperature strength, and is preferably contained at 0.0001% or more as necessary. More preferably, it is 0.001% or more, or 0.003% or more. However, since an excessive Sn content may cause a decrease in toughness and manufacturability, the Sn content is preferably 1.0% or less. More preferably, it is 0.5% or less.

[0059] (Mg: 0.0001% or more, 0.0100% or less) Mg may be contained as a deoxidizing element, and is also an element that improves formability, so it is preferable that Mg is contained in an amount of 0.0001% or more as necessary. More preferably, it is contained in an amount of 0.0003% or more. However, since an excessive Mg content may lead to a deterioration in surface quality, it is preferable that the Mg content be 0.0100% or less. In addition, in consideration of corrosion resistance and weldability, it is more preferable that the Mg content be 0.0030% or less. Even more preferably, it is 0.0020% or less.

[0060] (Co: 0.01% or more, 1.00% or less) Co is an element that improves high-temperature strength, and is preferably contained at 0.01% or more as necessary. More preferably, it is 0.03% or more. However, since an excessive Co content may cause a decrease in toughness, it is preferable that the Co content be 1.00% or less. In addition, in consideration of manufacturability, it is more preferable that the Co content be 0.50% or less. In consideration of workability, it is even more preferable that the Co content be 0.30% or less.

[0061] (Sb: 0.001% or more, 0.50% or less) Sb is an element that improves high-temperature strength, and is preferably contained at 0.001% or more as necessary. More preferably, it is 0.005% or more. However, since an excessive Sb content may cause a decrease in toughness, it is more preferable that the Sb content be 0.50% or less. Furthermore, in consideration of weldability, it is even more preferable that the Sb content be 0.40% or less.

[0062] (Bi:0.001% or more, 1.0% or less) Bi is an element that suppresses roping that occurs during cold rolling and improves manufacturability, and is preferably contained at 0.001% or more as necessary. More preferably, it is contained at 0.003% or more. However, since an excessive Bi content may cause a decrease in hot workability, the Bi content is preferably 1.0% or less. More preferably, it is 0.5% or less.

[0063] (Ta: 0.001% or more, 1.0% or less) Ta is an element that improves high-temperature strength, and is preferably contained at 0.001% or more as necessary. More preferably, it is contained at 0.003% or more. However, since an excessive Ta content may cause a decrease in toughness, the Ta content is preferably 1.0% or less. In addition, in consideration of manufacturability, the Ta content is more preferably 0.5% or less.

[0064] (Ga: 0.0001% or more, 0.50% or less) Ga is an element that improves corrosion resistance and hydrogen embrittlement resistance, and is preferably contained at 0.0001% or more as necessary. More preferably, it is 0.0003% or more. However, since an excessive Ga content may lead to a decrease in manufacturability, the Ga content is preferably 0.50% or less. More preferably, it is 0.30% or less.

[0065] Next, a method for producing the austenitic stainless steel sheet according to the present invention will be described. The austenitic stainless steel sheet according to the present embodiment may be produced by any method, but can be produced, for example, by the following production method.

[0066] The method for producing the austenitic stainless steel sheet of the present invention can employ a general process for producing austenitic stainless steel. In general, the steel is molten in a converter or electric furnace, refined in an AOD furnace or VOD furnace, or the like, and made into a slab by continuous casting or ingot casting, and then produced through the steps of hot rolling-annealing the hot-rolled sheet-pickling-cold rolling-finish annealing-pickling. If necessary, the annealing of the hot-rolled sheet may be omitted, or the cold rolling-finish annealing-pickling may be repeated.

[0067] The conditions for each of these steps may be general conditions, for example, a hot rolling heating temperature of 1000 to 1300°C, a hot rolled sheet annealing temperature of 900 to 1200°C, and a cold rolled sheet annealing temperature of 800 to 1200°C. However, the present invention is not characterized by the manufacturing conditions, and the manufacturing conditions are not limited. Therefore, the hot rolling conditions, hot rolled sheet thickness, whether or not hot rolled sheet annealing is performed, cold rolling conditions, hot rolled sheet and cold rolled sheet annealing temperatures, atmosphere, etc. can be appropriately selected.

[0068] In addition, the treatment before the final pickling may be a general treatment, for example, a mechanical treatment such as shot blasting or grinding brush, or a chemical treatment such as molten salt treatment or neutral salt electrolysis. In addition, after cold rolling and annealing, temper rolling or tension leveling may be applied. Furthermore, the product plate thickness may be selected according to the required member thickness. In addition, this steel plate may be used as a material to manufacture a welded pipe by a normal manufacturing method for stainless steel pipes for exhaust system components, such as electric resistance welding, TIG welding, or laser welding.

[0069] However, in order to improve the heat resistance and corrosion resistance after long-term aging in the σ-phase precipitation temperature range, it is necessary to further reduce Ni segregation, and to achieve this, the thickness A (mm) of the slab at the time of casting, the thickness B (mm) of the final product, the final annealing temperature C (°C), and the final annealing time D (seconds) should satisfy the following formula (v).

[0070] 50≦(C×D) / (A×B)≦700...Formula (v)

[0071] Ni segregation is reduced as the thickness A (mm) of the slab during casting is smaller, the thickness B (mm) of the final product is smaller, the final annealing temperature C (°C) is higher, and the final annealing time D (seconds) is longer. When the value of the middle part of formula (v) is less than 50, Ni segregation may become large. Also, when the value of the middle part of formula (v) is more than 700, over-annealing may occur, and corrosion resistance may decrease due to consumption of Cr due to oxidation during annealing and promotion of precipitation of carbonitrides. Therefore, formula (v) is satisfied. More preferably, the value of the middle part of formula (v) is 60 to 600.

[0072] According to the austenitic stainless steel sheet of this embodiment, it is possible to provide an austenitic stainless steel sheet having excellent heat resistance and corrosion resistance after long-term aging in the σ-phase precipitation temperature range. Also, according to the manufacturing method of the austenitic stainless steel sheet of this embodiment, it is possible to further reduce Ni segregation, and it is possible to provide an austenitic stainless steel sheet having excellent heat resistance and corrosion resistance after long-term aging in the σ-phase precipitation temperature range.

[0073] Moreover, examples of the automotive exhaust system parts according to this embodiment include automotive turbocharger parts, exhaust manifolds, and converters, and the austenitic stainless steel sheet according to this embodiment can be used as a material for these parts. As automotive turbocharger parts, the austenitic stainless steel sheet can be used for turbocharger parts installed in gasoline and diesel vehicles.

[0074] As a turbocharger part, for example, the austenitic stainless steel sheet of this embodiment can be applied to the material of a housing that constitutes the exterior of a turbocharger.

[0075] The austenitic stainless steel sheet of the present embodiment can also be used as a material for precision parts inside a nozzle vane type turbocharger, such as a back plate, oil deflector, compressor wheel, nozzle mount, nozzle plate, nozzle vane, drive ring, drive lever, etc. However, the uses of the austenitic stainless steel sheet of the present invention are not limited to these uses. EXAMPLES

[0076] The effects of the present invention will be made clearer by the following examples. Note that the present invention is not limited to the following examples, and can be appropriately modified and implemented without departing from the gist of the present invention.

[0077] Test materials (Invention Examples A to S, Comparative Examples a to q) having the composition shown in Tables 1 and 2 were melted in a vacuum melting furnace and cast into 150 kg ingots. These ingots were hot-rolled to obtain hot-rolled steel sheets with a thickness of 5.0 mm. The hot-rolled steel sheets were then annealed and pickled, cold-rolled to a thickness of 2 mm, and finally annealed and pickled at 1000 to 1200°C to give a recrystallized structure to obtain product sheets.

[0078] The various manufacturing conditions were set within the scope of the present invention. That is, the ingot thickness A (mm), final product thickness B (2 mm), final annealing temperature C (°C), and final annealing time D (sec) were set to satisfy the following formula (v). However, steels l to q in Tables 2 and 4 were manufactured under conditions outside the following formula (v).

[0079] 50≦(C×D) / (A×B)≦700 …(v)

[0080] The product sheet was also held at 900°C, which is the σ precipitation temperature range, for 400 hours to be used as an aged material.

[0081] [Table 1]

[0082] [Table 2]

[0083] For the obtained product sheets, the average Ni content in the Ni negative segregation parts and the average contents of each element in the positive segregation parts of Cr, Mo, and Si were calculated by performing EPMA analysis of the sheet cross section as described above.

[0084] To evaluate creep properties, aged materials with a plate thickness of 2 mm were used, and tests were conducted under two conditions: 950°C with a load stress of 20 MPa, and 1000°C with a load stress of 10 MPa. Tests in which the rupture time was 100 hours or more under the conditions of 950°C and a load stress of 20 MPa were rated "Good (◯)", and those in which the rupture time was less than 100 hours were rated "Poor (×)". Tests in which the rupture time was 100 hours or more under the conditions of 100°C and a load stress of 10 MPa were rated "Excellent (◎)".

[0085] The corrosion resistance was evaluated by measuring the pitting potential of finished sheets and aged materials of various thicknesses. The pitting potential was evaluated by measuring the pitting initiation potential V'C100 in a 1 mol / L sodium chloride aqueous solution at 30°C under Ar degassing, according to the method for measuring the pitting potential of stainless steel specified in JIS G 0577. The surface treatment of the test materials included polishing, passivation treatment, and immediate polishing. Materials with a pitting potential of 0.7 times or more that of the finished sheet were rated as "Good", and materials with a drop to less than 0.7 times were rated as "Poor". Materials with a pitting potential of 0.60V or more were rated as "Excellent".

[0086] Tables 3 and 4 show the evaluation results of [*Ni], [**Cr], [**Mo], [**Si], the value of the left side of formula (i), [*Ni] / [Ni], [**Cr] / [Cr], [**Mo] / [Mo], [**Si] / [Si], and creep properties and corrosion resistance for invention examples A to S and comparative examples a to q. Here, [element symbol] means the content (mass%) of the element in the steel, [*element symbol] means the average content (mass%) of the element in the negative segregation part of the element, and [**element symbol] means the average content (mass%) of the element in the positive segregation part of the element.

[0087] [Table 3]

[0088] [Table 4]

[0089] As is clear from Tables 1 to 4, the examples of the present invention, which have the composition specified in the present invention and satisfy formulas (i) and (ii), are superior in creep properties and corrosion resistance to the comparative examples. The examples of the present invention also satisfy conditions 1 to 3.

[0090] Furthermore, as mentioned above, in order to further improve creep properties and corrosion resistance, there are preferred or more preferred ranges for C, N, Si, Mn, Cr, Ni, and Mo. It can be seen that the examples of the present invention falling within these ranges have better evaluations of creep properties and corrosion resistance.

[0091] In addition, steel plates were manufactured under various manufacturing conditions for the base steels B, D, and E, which have compositions within the range of the present invention. Table 5 shows the base steel, the thickness A (mm) of the cast piece, the thickness B (mm) of the product plate, the final annealing temperature C (°C), the final annealing time D (seconds), the value of the middle part of formula (v), the average Ni content of the Ni negative segregation part, the value of the left side of formula (i), the value of the middle part of formula (ii), and the evaluation results of the creep properties and corrosion resistance. Note that the creep properties were evaluated only for the product plate with a thickness B (mm) of 2.0 mm.

[0092] [Table 5]

[0093] As is clear from Table 5, by satisfying formula (v), the negative Ni segregation is reduced, formulas (i) and (ii) are satisfied, and the creep properties and corrosion resistance are improved.

[0094] For No. 5 in Table 5, the final annealing was over-annealed, so the value of formula (v) exceeded 700, and the corrosion resistance was clearly reduced due to consumption of Cr by oxidation during annealing and promotion of precipitation of carbonitrides, etc., and the product was not usable. Therefore, the average Ni content in the Ni segregation parts and formulas (i) and (ii) were not measured or calculated. In Nos. 2, 3, 6, 7, 9 and 10, the value of formula (v) was less than 50, and therefore one or both of formulas (i) and (ii) were not satisfied, and the corrosion resistance was reduced.

[0095] As is clear from these, it is understood that a steel sheet having the individual component compositions specified in the present invention and satisfying the formulas (i) to (ii) has excellent creep properties and corrosion resistance. Furthermore, it is understood that a steel having individual component compositions satisfying various preferred or more preferred ranges has further improved creep properties and corrosion resistance. [Industrial Applicability]

[0096] According to the present invention, it is possible to provide an austenitic stainless steel sheet having excellent creep properties and corrosion resistance for use in heat-resistant parts such as exhaust members for transportation such as automobiles and motorcycles, and plant members. Specific examples of heat-resistant parts for automobiles include exhaust system parts such as exhaust manifolds, converters, front pipes, and flexible pipes, and turbocharger parts such as housings constituting the exterior and precision parts inside nozzle vane turbochargers (e.g., back plates, oil deflectors, compressor wheels, nozzle mounts, nozzle plates, nozzle vanes, drive rings, and drive levers). These applications can contribute to reducing the environmental load by purifying automobile exhaust gases and improving fuel efficiency.

Claims

1. In mass percent, C: 0.001% or more, 0.300% or less, N: 0.001% or more, 0.45% or less, Si: 0.10% or more, 5.00% or less, Mn: 0.10% or more, 12.00% or less, P: 0.060% or less, S: 0.0200% or less, Cr: 15.0% or more, 35.0% or less, Ni: 2.0% or more, 35.0% or less, Cu: 0.001% or more, 5.00% or less, Mo: 0.001% or more, 5.00% or less, Al: 0.001% or more, 1.000% or less, V: 0.01% or more, 1.00% or less, B: 0.0001% or more, 0.0100% or less, Ca: 0.0001% or more, 0.0200% or less, O: 0.0150% or less, and the balance consisting of Fe and impurities, and satisfying the following formulas (i) and (ii): 5[Cr]+6[Si]+9[Mo]-2[Ni]-30[C]-70[N]-100[*Ni] / [Ni]≦0 ... formula (i) 0.80≦[*Ni] / [Ni]<1.00... formula (ii) In the formulas (i) and (ii), the [element symbol] means the content (mass%) of the corresponding element in the steel, and [*Ni] means the average Ni content (mass%) in the Ni-negative segregation portion.

2. In mass percent, C: 0.001% or more and less than 0.080%; N: more than 0.20%, less than 0.39%, Si: more than 1.00%, 3.00% or less, Mn: 0.80% or more, 3.00% or less, P: 0.050% or less, S: 0.0018% or less, Cr: 20.0% or more, 35.0% or less, Ni: more than 8.0%, less than 25.0%, Cu: 0.001% or more, 3.40% or less, Mo: 0.001% or more, less than 0.50% Al: more than 0.005%, less than 0.130%, V: 0.01% or more, 1.00% or less, B: 0.0001% or more, 0.0100% or less, Ca: 0.0001% or more, 0.0200% or less, O: 0.0150% or less, and the balance consisting of Fe and impurities, and satisfying the following formulas (iii) and (iv): 5[Cr]+6[Si]+9[Mo]-2[Ni]-30[C]-70[N]-100[*Ni] / [Ni]≦0...Formula (iii) 0.80≦[*Ni] / [Ni]<1.00... formula (iv) However, in formula (iii) and formula (iv), the [element symbol] means the content (mass%) of the corresponding element in the steel, and [*Ni] means the average Ni content (mass%) in the Ni-negative segregation portion.

3. In place of a part of Fe, further Ti: 0.001% or more, 1.00% or less, Nb: 0.001% or more, 1.00% or less, W: 0.01% or more, 3.00% or less, Y: 0.001% or more, 0.50% or less, REM: 0.001% or more, 0.50% or less, Zr: 0.01% or more, 0.50% or less, Hf: 0.001% or more, 1.0% or less, Sn: 0.0001% or more, 1.0% or less, Mg: 0.0001% or more, 0.0100% or less, Co: 0.01% or more, 1.00% or less, Sb: 0.001% or more, 0.50% or less, Bi: 0.001% or more, 1.0% or less, Ta: 0.001% or more, 1.0% or less, Ga: 0.0001% or more, 0.50% or less, 3. The austenitic stainless steel sheet according to claim 2, further comprising one or more of the following:

4. In mass percent, C: 0.001% or more, 0.300% or less, N: 0.001% or more, 0.45% or less, Si: 0.10% or more, 5.00% or less, Mn: 0.10% or more, 12.00% or less, P: 0.060% or less, S: 0.0200% or less, Cr: 15.0% or more, 35.0% or less, Ni: 2.0% or more, 35.0% or less, Cu: 0.001% or more, 5.00% or less, Mo: 0.001% or more, 1.50% or less, Al: 0.001% or more, 1.000% or less, V: 0.01% or more, 1.00% or less, B: 0.0001% or more, 0.0100% or less, Ca: 0.0001% or more, 0.0200% or less, O: 0.0150% or less, Contains Furthermore, Ti: 0.001% or more, 1.00% or less, Nb: 0.001% or more, 1.00% or less, W: 0.01% or more, 3.00% or less, Y: 0.001% or more, 0.50% or less, REM: 0.001% or more, 0.50% or less, Zr: 0.01% or more, 0.50% or less, Hf: 0.001% or more, 1.0% or less, Sn: 0.0001% or more, 1.0% or less, Mg: 0.0001% or more, 0.0100% or less, Co: 0.01% or more, 1.00% or less, Sb: 0.001% or more, 0.50% or less, Bi: 0.001% or more, 1.0% or less, Ta: 0.001% or more, 1.0% or less, Ga: 0.0001% or more, 0.50% or less, Contains one or more of the following: An austenitic stainless steel sheet, the balance of which consists of Fe and impurities, and which satisfies the following formulas (i) and (ii): 5[Cr]+6[Si]+9[Mo]-2[Ni]-30[C]-70[N]-100[*Ni] / [Ni]≦0 ... formula (i) 0.80≦[*Ni] / [Ni]<1.00... formula (ii) In the formulas (i) and (ii), the [element symbol] means the content (mass%) of the corresponding element in the steel, and [*Ni] means the average Ni content (mass%) in the Ni-negative segregation portion.

5. The austenitic stainless steel sheet according to any one of claims 1 to 4, which is used as an automobile exhaust system member.

6. 6. The method for producing an austenitic stainless steel sheet according to any one of claims 1 to 5, characterized in that the thickness A (mm) of the slab during casting, the thickness B (mm) of the final product, the final annealing temperature C (°C), and the final annealing time D (seconds) satisfy the following formula (v): 50≦(C×D) / (A×B)≦700...Formula (v)

7. 6. An automobile exhaust system part comprising an automobile exhaust system member made of the austenitic stainless steel sheet according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Surface treatment by anticorrosive metal coating

    JP1981005996A

  • Heat-resistant austenitic stainless steel sheet

    JP2013209730A

  • Austenitic stainless steel plate having excellent heat resistance and method for producing the same

    JP2019059995A

  • Austenite stainless steel sheet and manufacturing method therefor

    JP2019218588A

  • Austenitic stainless steel

    WO2018043565A1